Positive electrode for non-aqueous electrolyte secondary batteries, non-aqueous electrolyte secondary battery, and method for manufacturing positive electrode for non-aqueous electrolyte secondary batteries
The positive electrode for non-aqueous electrolyte secondary batteries, featuring a lithium-containing transition metal composite oxide coated with a sulfonic acid compound and containing Ca and Sr or their phosphates, addresses the issue of increased reaction resistance and cycle deterioration by reacting with hydrogen fluoride, enhancing battery performance.
Patent Information
- Application Number
- PCT/JP2024/017608
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2024-05-13
- Publication Date
- 2024-12-05
AI Technical Summary
Lithium-containing transition metal composite oxides with high Ni content in non-aqueous electrolyte secondary batteries experience increased reaction resistance and deteriorated cycle characteristics due to side reactions with the non-aqueous electrolyte, leading to hydrogen fluoride deposition and elution of transition metals, which affects battery performance.
A positive electrode with a lithium-containing transition metal composite oxide having a layered structure, coated with a sulfonic acid compound and containing Ca and Sr, or their phosphates, to reduce reaction resistance and improve cycle characteristics by preferentially reacting with hydrogen fluoride.
The proposed solution effectively reduces reaction resistance and enhances cycle characteristics at high voltages by protecting the lithium-containing transition metal composite oxide from hydrogen fluoride, thereby improving the overall performance of non-aqueous electrolyte secondary batteries.
Smart Images

Figure JP2024017608_05122024_PF_FP_ABST
Abstract
Description
Positive electrode for non-aqueous electrolyte secondary battery, non-aqueous electrolyte secondary battery, and method for manufacturing positive electrode for non-aqueous electrolyte secondary battery
[0001] The present disclosure relates to a positive electrode for a non-aqueous electrolyte secondary battery, a non-aqueous electrolyte secondary battery, and a method for manufacturing a positive electrode for a non-aqueous electrolyte secondary battery.
[0002] In recent years, the applications of non-aqueous electrolyte secondary batteries have expanded to include power sources for electric vehicles and power storage devices for utilizing natural energy. Because the positive electrode significantly affects battery characteristics, including battery capacity, output characteristics, and cycle characteristics, much research has been conducted on the positive electrode. For example, Patent Document 1 discloses a positive electrode for a non-aqueous electrolyte secondary battery that includes a compound containing sulfur (S) and phosphorus (P) in order to suppress gas generation during storage at high temperatures. Patent Document 2 also discloses a positive electrode for a non-aqueous electrolyte secondary battery that uses, as a positive electrode active material, a lithium-containing transition metal composite oxide having a low-solubility Li salt scattered on its surface in order to reduce reaction resistance during storage at high temperatures.
[0003] JP 2009-123463 A JP 2019-169286 A
[0004] In recent years, lithium-containing transition metal composite oxides with a high Ni content have been attracting attention as a positive electrode active material that can realize high battery capacity. However, when a lithium-containing transition metal composite oxide with a high Ni content is used as a positive electrode active material, highly reactive Ni is formed on the particle surface of the composite oxide at a high state of charge (SOC). 4+ Since a large amount of hydrogen fluoride is present, a side reaction between the lithium-containing transition metal composite oxide and the non-aqueous electrolyte is likely to occur. Then, hydrogen fluoride generated by the side reaction reacts with the lithium-containing transition metal composite oxide, and the product deposits on the surface of the lithium-containing transition metal composite oxide, causing the transition metal to leach out from the lithium-containing transition metal composite oxide. As a result, the reaction resistance of the battery increases, and the charge-discharge cycle characteristics deteriorate.
[0005] A positive electrode for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure is a positive electrode for a non-aqueous electrolyte secondary battery having a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core, the positive electrode mixture layer including a lithium-containing transition metal composite oxide having a layered structure as a positive electrode active material, the lithium-containing transition metal composite oxide being represented by the general formula Li x Ni a Co b Mn c M d O 2-y (wherein 0.8<x<1.2, 0.75≦a≦0.98, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, Ca, Sr, and Zr), and the positive electrode mixture layer is characterized in that the positive electrode mixture layer is a secondary particle formed by aggregation of primary particles, a sulfonic acid compound represented by formula (I) is present on the surface of the secondary particle, and the positive electrode mixture layer contains a first compound containing at least one of Ca and Sr, and a second compound containing P, or contains a phosphate containing at least one of Ca and Sr. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)
[0006] A method for manufacturing a positive electrode for a non-aqueous electrolyte secondary battery according to one aspect of the present disclosure includes an active material preparation step of preparing a positive electrode active material, a preparation step of preparing a positive electrode slurry containing the positive electrode active material, a coating step of applying the positive electrode slurry to the surface of a positive electrode core, and a rolling step of rolling the coating film produced in the coating step. The active material preparation step includes a synthesis step of obtaining a lithium-containing transition metal composite oxide, a washing step of washing the lithium-containing transition metal composite oxide with water and dehydrating it to obtain a cake-like composition, a first addition step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition, and a drying step of drying the cake-like composition to obtain a powder-like composition. The method further includes a second addition step of adding a compound containing at least one of Ca and Sr and a compound containing P, or adding a phosphate containing at least one of Ca and Sr, to the positive electrode slurry or the cake-like composition.
[0007] A non-aqueous electrolyte secondary battery according to one aspect of the present disclosure includes the above positive electrode, a negative electrode, and a non-aqueous electrolyte.
[0008] According to the positive electrode for a non-aqueous electrolyte secondary battery of one aspect of the present disclosure, it is possible to provide a non-aqueous electrolyte secondary battery that has improved cycle characteristics at high voltage while reducing the reaction resistance of the battery.
[0009] 1 is a longitudinal cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment of the present invention;
[0010] As described above, lithium-containing transition metal composite oxides with a high Ni content are prone to side reactions with non-aqueous electrolytes, particularly at high SOCs. Therefore, when such composite oxides are used as positive electrode active materials, hydrogen fluoride generated by the side reactions reacts with the lithium-containing transition metal composite oxide, resulting in the deposition of products on the surface of the lithium-containing transition metal composite oxide or the elution of transition metals from the lithium-containing transition metal composite oxide. As a result, the reaction resistance of the battery increases.
[0011] As a result of investigations by the present inventors, it has been found that the reaction resistance of a battery can be reduced by adding a sulfonic acid compound represented by the above formula (I) to the surface of secondary particles of a lithium-containing transition metal composite oxide used as a positive electrode active material. This is thought to be because the function of the sulfonic acid compound makes it easier for Li to be inserted and removed, thereby reducing the reaction resistance at the positive electrode. However, the presence of the sulfonic acid compound has created a new problem: reduced cycle characteristics at high voltages. This is thought to be because, in addition to an increase in the potential of the positive electrode, the reactivity at the positive electrode has increased, resulting in an increase in the amount of hydrogen fluoride generated by a side reaction between the lithium-containing transition metal composite oxide and the non-aqueous electrolyte during repeated charge and discharge.
[0012] The inventors further conducted extensive research and discovered that the presence of a compound containing at least one of Ca and Sr (hereinafter referred to as the first compound) and a compound containing P (hereinafter referred to as the second compound), or a phosphate containing at least one of Ca and Sr (hereinafter simply referred to as the phosphate) in the positive electrode mixture layer constituting the positive electrode, reduces the reaction resistance of the battery while improving cycle characteristics. This is presumably because the sulfonic acid compound reduces the reaction resistance at the positive electrode, while allowing hydrogen fluoride generated by a side reaction to preferentially react with the first compound, the second compound, and the phosphate, thereby protecting the lithium-containing transition metal composite oxide from hydrogen fluoride. The first compound, the second compound, and the phosphate may be present on the surface of the secondary particles, or the effects of the present disclosure can be achieved even if they are present apart from the secondary particles.
[0013] Hereinafter, an example of an embodiment of a nonaqueous electrolyte secondary battery according to the present disclosure will be described in detail with reference to the drawings. Note that configurations obtained by selectively combining the respective components of the multiple embodiments and variations described below are included within the scope of the present disclosure.
[0014] In the following, a cylindrical battery in which a wound electrode assembly 14 is housed in a cylindrical, bottomed exterior body 16 is exemplified as a nonaqueous electrolyte secondary battery; however, the exterior body of the battery is not limited to a cylindrical exterior body. The nonaqueous electrolyte secondary battery according to the present disclosure may be, for example, a prismatic battery with a prismatic exterior body, a coin-type battery with a coin-type exterior body, or a pouch-type battery with an exterior body composed of a laminate sheet including a metal layer and a resin layer. Furthermore, the electrode assembly is not limited to a wound type, but may also be a stacked type electrode assembly in which multiple positive electrodes and multiple negative electrodes are alternately stacked with separators interposed therebetween. Furthermore, the design of the nonaqueous electrolyte secondary battery according to the present disclosure is not limited to the design of the exemplified nonaqueous electrolyte secondary battery, and known nonaqueous electrolyte secondary battery designs may also be applied.
[0015] FIG. 1 is an axial cross-sectional view of a cylindrical nonaqueous electrolyte secondary battery 10 according to an embodiment. As shown in FIG. 1 , the nonaqueous electrolyte secondary battery 10 includes a wound electrode assembly 14, a nonaqueous electrolyte, and an exterior body 16 that accommodates the electrode assembly 14 and the nonaqueous electrolyte. The electrode assembly 14 includes a positive electrode 11, a negative electrode 12, and a separator 13, and has a wound structure in which the positive electrode 11 and the negative electrode 12 are spirally wound with the separator 13 interposed therebetween. The exterior body 16 is a cylindrical metal container with a bottom that is open on one axial side, and the opening of the exterior body 16 is closed by a sealing body 17. Hereinafter, for convenience of explanation, the sealing body 17 side of the battery will be referred to as the top, and the bottom side of the exterior body 16 will be referred to as the bottom.
[0016] The positive electrode 11, negative electrode 12, and separator 13 that make up the electrode assembly 14 are all rectangular, elongated bodies that are spirally wound in the longitudinal direction and stacked alternately in the radial direction of the electrode assembly 14. The separator 13 isolates the positive electrode 11 and the negative electrode 12 from each other. Two separators 13 are arranged, for example, to sandwich the positive electrode 11. The electrode assembly 14 includes a positive electrode lead 20 connected to the positive electrode 11 by welding or the like, and a negative electrode lead 21 connected to the negative electrode 12 by welding or the like. In the electrode assembly 14, the longitudinal direction of the positive electrode 11 and the negative electrode 12 is the winding direction, and the lateral direction of the positive electrode 11 and the negative electrode 12 is the axial direction. That is, the lateral end faces of the positive electrode 11 and the negative electrode 12 form the axial end faces of the electrode assembly 14.
[0017] Insulating plates 18 and 19 are disposed above and below the electrode body 14. In the example shown in Fig. 1 , the positive electrode lead 20 passes through a through hole in the insulating plate 18 and extends toward the sealing body 17, and the negative electrode lead 21 passes outside the insulating plate 19 and extends toward the bottom side of the exterior body 16. The positive electrode lead 20 is connected to the underside of an internal terminal plate 23 of the sealing body 17 by welding or the like, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the internal terminal plate 23, serves as the positive electrode terminal. The negative electrode lead 21 is connected to the inner bottom surface of the exterior body 16 by welding or the like, and the exterior body 16 serves as the negative electrode terminal.
[0018] A gasket 28 is provided between the exterior body 16 and the sealing body 17 to ensure airtightness inside the battery. The exterior body 16 has a grooved portion 22 formed on its side surface that protrudes inward and supports the sealing body 17. The grooved portion 22 is preferably formed in an annular shape along the circumferential direction of the exterior body 16, and supports the sealing body 17 on its top surface. The sealing body 17 is fixed to the top of the exterior body 16 by the grooved portion 22 and the open end of the exterior body 16 that is crimped to the sealing body 17.
[0019] The sealing body 17 has a structure in which, in order from the electrode body 14 side, an internal terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked. Each member constituting the sealing body 17 has, for example, a disk or ring shape, and each member except for the insulating member 25 is electrically connected to one another. The lower valve body 24 and the upper valve body 26 are connected at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, the lower valve body 24 deforms and breaks, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.
[0020] The positive electrode 11, the negative electrode 12, the separator 13, and the nonaqueous electrolyte that constitute the nonaqueous electrolyte secondary battery 10 will be described in detail below, with the positive electrode 11 being particularly described below.
[0021] [Positive Electrode] The positive electrode 11 has, for example, a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core. The positive electrode mixture layer is preferably formed on both sides of the positive electrode core. The positive electrode core can be made of a foil of a metal, such as aluminum or an aluminum alloy, that is stable within the potential range of the positive electrode 11, or a film with such a metal disposed on the surface. The thickness of the positive electrode core is, for example, 10 μm or more and 30 μm or less.
[0022] The positive electrode mixture layer includes a positive electrode active material, a compound (first compound) containing at least one of Ca and Sr, and a compound (second compound) containing P. The positive electrode mixture layer also includes a phosphate (phosphate) containing at least one of Ca and Sr instead of or in addition to the first compound and the second compound. As will be described in detail later, the first compound, the second compound, and the phosphate may be present on the particle surface of the positive electrode active material, or may be present apart from the particle surface of the positive electrode active material, for example, in the gaps between the positive electrode active material particles. The thickness of the positive electrode mixture layer is, for example, 10 μm or more and 150 μm or less on one side of the positive electrode core.
[0023] The positive electrode active material includes a lithium-containing transition metal composite oxide having a layered structure. The lithium-containing transition metal composite oxide includes secondary particles formed by aggregation of primary particles. The particle size of the primary particles constituting the secondary particles of the lithium-containing transition metal composite oxide is, for example, 0.02 μm or more and 2 μm or less. The particle size of the primary particles is measured as the diameter of a circumscribed circle in a particle image observed with a scanning electron microscope (SEM). The average particle size of the secondary particles of the lithium-containing transition metal composite oxide is, for example, 2 μm or more and 30 μm or less. Here, the average particle size refers to the volume-based median diameter (D50). D50 refers to the particle size at which the cumulative frequency in the volume-based particle size distribution is 50% from the smallest particle size, and is also referred to as the median diameter. The particle size distribution of the secondary particles of the lithium-containing transition metal composite oxide can be measured using a laser diffraction particle size distribution analyzer (e.g., MT3000II, manufactured by Microtrac-Bell Corporation) using water as a dispersion medium.
[0024] Examples of the layered structure of the lithium-containing transition metal composite oxide include a layered structure belonging to the space group R-3m and a layered structure belonging to the space group C2 / m. From the viewpoints of increasing capacity and stabilizing the crystal structure, the lithium-containing transition metal composite oxide preferably has a layered structure belonging to the space group R-3m. The layered structure of the lithium-containing transition metal composite oxide may include a transition metal layer and a Li layer.
[0025] The lithium-containing transition metal composite oxide has the general formula Li x Ni a Co bMn c M d O 2-y (wherein 0.8<x<1.2, 0.75≦a≦0.98, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, Ca, Sr, and Zr.) The content of the elements constituting the lithium-containing transition metal composite oxide can be measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES), an electron probe microanalyzer (EPMA), an energy dispersive X-ray analyzer (EDX), or the like.
[0026] By setting the Ni content in the lithium-containing transition metal composite oxide to 75 mol % or more and 98 mol % or less, a battery with a high capacity can be obtained. The higher the Ni content, the higher the capacity of the battery that can be obtained.
[0027] The content of Co in the lithium-containing transition metal composite oxide is 0 mol % or more and 15 mol % or less, and Co is an optional component. In other words, the lithium-containing transition metal composite oxide does not need to contain Co. By containing Co, the lithium-containing transition metal composite oxide can improve the heat resistance of the battery.
[0028] The content of Mn in the lithium-containing transition metal composite oxide is 0 mol% or less and 25 mol% or more, and Mn is an optional component. In other words, the lithium-containing transition metal composite oxide does not need to contain Mn. By containing Mn, the lithium-containing transition metal composite oxide can stabilize its crystal structure.
[0029] The content of M (M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, Ca, Sr, and Zr) in the lithium-containing transition metal composite oxide is 0 mol % or more and 10 mol % or less, and M is an optional component. In other words, the lithium-containing transition metal composite oxide does not necessarily contain M.
[0030] The sulfonic acid compound represented by formula (I) is present on the surface of the secondary particles of the lithium-containing transition metal composite oxide. In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2. A is preferably a Group 1 element. Among these, Li or Na is more preferred, and Li is particularly preferred. The sulfonic acid compound may be scattered so as to cover at least a portion of the surface of the secondary particles of the lithium-containing transition metal composite oxide, or may be present so as to cover the entire surface of the secondary particles. Furthermore, the sulfonic acid compound may be present on the surface of the primary particles of the lithium-containing transition metal composite oxide.
[0031] In formula (I), R is preferably an alkyl group. The number of carbon atoms in the alkyl group is preferably 5 or less, more preferably 3 or less. From the viewpoint of reducing reaction resistance, a suitable example of R is an alkyl group having 3 or less carbon atoms, and among these, a methyl group is preferred. In R, some of the hydrogen atoms bonded to the carbon may be substituted with fluorine. In formula (I), n is preferably 1.
[0032] Specific examples of the sulfonic acid compound include lithium methanesulfonate, lithium ethanesulfonate, lithium propanesulfonate, sodium methanesulfonate, sodium ethanesulfonate, magnesium methanesulfonate, lithium fluoromethanesulfonate, etc. Among these, at least one selected from the group consisting of lithium methanesulfonate, lithium ethanesulfonate, and sodium methanesulfonate is preferred, with lithium methanesulfonate being particularly preferred.
[0033] The presence of the sulfonic acid compound on the surface of the secondary particles facilitates the insertion and desorption of Li. As a result, the reaction resistance in the positive electrode 11 is reduced, thereby achieving a reduction in the reaction resistance of the battery. Although even a very small amount of the sulfonic acid compound exhibits this effect, it is preferable that the sulfonic acid compound be present on the secondary particle surface of the composite oxide in an amount of 0.05% by mass or more, and more preferably 0.1% by mass or more, relative to the total mass of the lithium-containing transition metal composite oxide. From the viewpoint of cycle characteristics, the upper limit of the sulfonic acid compound content is preferably 1.5% by mass relative to the total mass of the lithium-containing transition metal composite oxide. Therefore, an example of a suitable range of the amount of the sulfonic acid compound is 0.05% by mass or more and 1.5% by mass or less, more preferably 0.1% by mass or more and 1.5% by mass or less, relative to the total mass of the lithium-containing transition metal composite oxide.
[0034] The presence of the sulfonic acid compound on the surface of the secondary particles of the lithium-containing transition metal composite oxide can be confirmed by Fourier transform infrared spectroscopy (FT-IR). In the infrared absorption spectrum obtained by FT-IR, the positive electrode active material containing lithium methanesulfonate exhibits, for example, a peak at 1238 cm -1 , 1175 cm -1 , 1065 cm -1 , 785 cm -1 It has an absorption peak around 1238 cm -1 , 1175 cm -1 , 1065 cm -1 The peak around 785 cm is due to the SO stretching vibration of lithium methanesulfonate. -1 The peak around 1000 nm is a peak due to the C-S stretching vibration derived from lithium methanesulfonate. Note that the presence of a positive electrode active material containing a sulfonic acid compound other than lithium methanesulfonate can also be confirmed from the absorption peak derived from the sulfonic acid compound in the infrared absorption spectrum.
[0035] The presence of the sulfonic acid compound can also be confirmed by X-ray photoelectron spectroscopy (XPS). In the spectrum obtained by XPS, a peak with an intensity (c / s) of 200 or more and 1000 or less is observed in the positive electrode active material containing lithium methanesulfonate, where the binding energy is approximately 165 eV or more and 170 eV or less. The presence of the sulfonic acid compound on the secondary particle surface of the lithium-containing transition metal composite oxide can also be confirmed by ICP, atomic absorption spectroscopy, synchrotron XRD measurement, TOF-SIMS, H-NMR, etc.
[0036] The positive electrode active material, which is one example of the embodiment, can be produced by the following method: Note that the production method described here is only an example, and the method for producing the positive electrode active material is not limited to this method.
[0037] The manufacturing process of the positive electrode active material includes a synthesis step of obtaining a lithium-containing transition metal composite oxide, a washing step of washing and dehydrating the lithium-containing transition metal composite oxide obtained by the synthesis step to obtain a cake-like composition, and a drying step of drying the cake-like composition to obtain a powder-like composition. The manufacturing process of the positive electrode active material also includes a first addition step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition, and a second addition step of adding a compound containing at least one of Ca and Sr and a compound containing P to the cake-like composition. Note that the second addition step is optional and may be performed during the preparation step of the positive electrode 11, which will be described later.
[0038] In the synthesis step, for example, a metal oxide containing 75 mol% to 98 mol% Ni, 0 mol% to 15 mol% Co, 0 mol% to 25 mol% Mn, and 0 mol% to 10 mol% M (M is at least one element selected from W, Mg, Mo, Nb, Ti, Si, Al, Ca, Sr, and Zr) is mixed with a Li compound to obtain a mixture.
[0039] The metal oxide can be obtained, for example, by adding an alkaline solution such as sodium hydroxide dropwise to a stirred solution of a metal salt containing Ni and an arbitrary metal element (Co, Mn, M, etc.) to adjust the pH to the alkaline side (e.g., 8.5 or more and 12.5 or less), thereby precipitating (co-precipitating) a composite hydroxide containing Ni and the arbitrary metal element, and then heat-treating the composite hydroxide. The heat-treatment temperature is not particularly limited, but is, for example, in the range of 250°C or more and 600°C or less.
[0040] Examples of Li compounds include Li 2 CO 3 , LiOH, Li 2 O 2 , Li 2 O, LiNO 3 , LiNO 2 , Li 2 SO 4 , LiOH·H 2 Examples of the metal oxide include O, LiH, and LiF. In order to easily adjust each of the above parameters to the ranges specified above, the mixing ratio of the metal oxide and the Li compound is preferably such that the molar ratio of the total amount of metal elements in the metal oxide to Li is in the range of 1:0.8 or more and 1:1.2 or less, and more preferably in the range of 1:1.0 or more and 1:1.1 or less.
[0041] Next, the synthesis step includes a calcination step in which the resulting mixture is calcined. The calcination step is a multi-stage calcination step that includes at least a first calcination step in which the mixture is calcined at 300°C or higher and 680°C or lower under an oxygen stream, and a second calcination step in which the calcined product obtained by the first calcination step is calcined at a temperature exceeding 680°C under an oxygen stream. In the first calcination step, the temperature is increased to a first set temperature of 680°C or lower at a first temperature increase rate of 0.2°C / min or higher and 4.5°C / min or lower. In the second calcination step, the temperature is increased to a second set temperature of 900°C or lower at a first temperature increase rate of 0.5°C / min or higher and 3.5°C / min or lower. Note that multiple first and second temperature increase rates may be set for each temperature range as long as they are within the above-specified range.
[0042] The holding time of the first set temperature in the first firing step is preferably 5 hours or less, more preferably 3 hours or less. The holding time of the first set temperature is the time during which the first set temperature is maintained after reaching the first set temperature, and the holding time may be zero. The holding time of the second set temperature in the second firing step is preferably 1 hour or more and 10 hours or less, more preferably 1 hour or more and 5 hours or less. The holding time of the second set temperature is the time during which the second set temperature is maintained after reaching the second set temperature. The firing of the mixture is carried out, for example, in an oxygen stream with an oxygen concentration of 60% or more, and the flow rate of the oxygen stream is set to 10 cm / s. 3 The flow rate shall be 0.2 mL / min or more and 4 mL / min or less per kg of the mixture, or 0.3 L / min or more per kg of the mixture.
[0043] The synthesis step is not limited to the above steps, and may include, for example, a known synthesis method in which a precursor obtained by co-precipitating or mixing a compound such as a hydroxide, oxide, or carbonate containing at least one element selected from Ni, Co, Mn, and M (M is at least one element selected from W, Mg, Mo, Nb, Ti, Si, Al, Ca, Sr, and Zr) is mixed with a Li source and fired to obtain a lithium-containing transition metal composite oxide. When the precursor does not contain a compound such as M, these compounds such as M may be mixed and fired when the precursor and Li source are mixed and fired. Furthermore, these compounds may be pulverized to appropriately change the particle shape or particle size, or may be used after adjusting the water content by including a hydrate.
[0044] In the washing step, the lithium-containing transition metal composite oxide is washed with water and dehydrated to obtain a cake-like composition. The particulate lithium-containing transition metal composite oxide obtained in the synthesis step can be used. By washing with water, unreacted lithium compounds added in the synthesis step and impurities other than the lithium compounds can be removed. When washing with water, for example, 300 g or more and 5000 g or less of lithium-containing transition metal composite oxide is added to 1 L of water. The water washing may be repeated multiple times. The dehydration after washing with water can be performed, for example, using a filter press.
[0045] In the first addition step, at least one of a sulfonic acid compound and a sulfonic acid solution is added to the cake-like composition obtained in the washing step. This allows the sulfonic acid compound to adhere to the surface of the lithium-containing transition metal composite oxide. The sulfonic acid compound may be in either powder or solution form. The sulfonic acid solution is, for example, a methanesulfonic acid solution obtained by dissolving methanesulfonic acid in water. Li compounds remain in the cake-like composition, and these remaining Li compounds are dissolved in the water contained in the cake-like composition. Therefore, even when a sulfonic acid solution is added, a Li compound or a Li compound solution containing Li is formed. From the viewpoint of more easily achieving the effects of the present application, a Li compound or a Li compound solution may be added to the cake-like composition together with the sulfonic acid solution, or a mixed solution in which the sulfonic acid solution and the Li compound or the Li compound solution are premixed may be added to the cake-like composition. The Li compound is, for example, LiOH, and the Li compound solution is, for example, a LiOH solution obtained by dissolving LiOH in water. The amounts of the Li compound and sulfonic acid solution added to the cake-like composition preferably satisfy the relationship of 0≦Li compound / sulfonic acid≦1.3 in molar ratio. The amount of sulfonic acid compound or sulfonic acid added is preferably 0.05% by mass or more and 1.5% by mass or less, and more preferably 0.1% by mass or more and 1.0% by mass or less, relative to the mass of the lithium-containing transition metal composite oxide. The concentrations of the sulfonic acid solution and the sulfonic acid compound solution are, for example, 0.5% by mass or more and 40% by mass or less.
[0046] In the second addition step, a compound containing at least one of Ca and Sr and a compound containing P are added to the cake-like composition obtained in the washing step. The second addition step may be performed before or after the first addition step. The second addition step may be performed simultaneously with the first addition step. The second addition step may be performed simultaneously with the water washing step.
[0047] The compound containing at least one of Ca and Sr is Ca(OH) 2 , CaO, CaCl 2 , CaCO 3 , CaSO 4, Ca(NO 3 ) 2 , Sr(OH) 2 , Sr(OH) 2 ・8H 2 O, Sr(OH) 2 ・H 2 O, SrO, SrCl 2 , SrCl 2 ・6H 2 O, SrCO 3 , SrSO 4 , Sr(NO 3 ) 2 These compounds may be used after drying and dehydration in order to reduce the amount of water generated in the drying process. These compounds may also be pulverized to have a particle size of 0.1 μm or more and 20 μm or less. Examples of compounds containing P include Li 3-x H x P.O. 4 (0≦x≦3), (NH 4 ) 2 HPO 4 , N.H. 4 H 2 P.O. 4 , P 4 O 10 , H 3 P.O. 3 , Na 2 HPO 4 , NaH 2 P.O. 4 and the like. The compound containing at least one of Ca and Sr and the compound containing P may be added simultaneously or separately. For example, the first addition step may be performed after adding the compound containing at least one of Ca and Sr, and then the compound containing P may be added. Furthermore, a compound in a form different from the compound added in the second addition step may be present on the surface of the secondary particles.
[0048] In the second addition step, a phosphate containing at least one of Ca and Sr may be added instead of or in addition to the compound containing at least one of Ca and Sr and the compound containing P. Examples of the phosphate containing at least one of Ca and Sr include Ca(H 2 P.O.4 ) 2 , Ca(H 2 P.O. 4 ) 2 ・H 2 O, CaHPO 4 , CaHPO 4 (H 2 O), Ca 3 (P.O. 4 ) 2 , Sr(H 2 P.O. 4 ) 2 , SrHPO 4 , Sr 3 (P.O. 4 ) 2 etc.
[0049] Furthermore, in the second addition step, after adding the compound, a heat treatment may be performed. The heating temperature is, for example, 100° C. or higher and 600° C. or lower. The heat treatment may be performed after the drying step.
[0050] In the drying step, the cake-like composition to which the sulfonic acid compound and the like have been added is dried to obtain a powdery composition. The drying step may be performed under a vacuum atmosphere. The drying conditions are, for example, 100°C or higher and 600°C or lower, preferably 150°C or higher and 400°C or lower. The drying time is preferably 0.5 hours or higher and 15 hours or lower.
[0051] As described above, the positive electrode mixture layer contains a compound (first compound) containing at least one of Ca and Sr, and a compound (second compound) containing P. The positive electrode mixture layer may contain a phosphate (phosphate) containing at least one of Ca and Sr instead of or in addition to the first compound and the second compound.
[0052] The first compound, the second compound, and the phosphate are present, for example, on the surface of secondary particles of the lithium-containing transition metal composite oxide. The first compound, the second compound, and the phosphate preferentially react with hydrogen fluoride produced by decomposition of the non-aqueous electrolyte. As a result, the lithium-containing transition metal composite oxide can be protected from hydrogen fluoride. The first compound, the second compound, and the phosphate may be scattered so as to cover at least a portion of the surface of the secondary particles of the lithium-containing transition metal composite oxide, or may be present so as to cover the entire surface of the secondary particles. Furthermore, the first compound, the second compound, and the phosphate may be directly attached to the surface of the secondary particles, or may be attached to the surface of a sulfonic acid compound present on the surface of the secondary particles. Furthermore, one particle of the first compound, the second compound, and the phosphate may be present in contact with both the particle surface of the sulfonic acid compound and the surface of the secondary particles.
[0053] When at least one of the first compound, the second compound, and the phosphate is present on the surface of the secondary particles of the lithium-containing transition metal composite oxide, elution of the transition metal from the lithium-containing transition metal composite oxide at high voltage is further suppressed. Therefore, when at least one of the first compound, the second compound, and the phosphate is present on the surface of the secondary particles of the lithium-containing transition metal composite oxide, the cycle characteristics at high voltage are further improved. Furthermore, this effect may be significantly obtained when at least one of the first compound, the second compound, and the phosphate is present on the surface of the secondary particles of the lithium-containing transition metal composite oxide.
[0054] The first compound, the second compound, and the phosphate may be present in the positive electrode mixture layer without adhering to the surfaces of the secondary particles. The first compound, the second compound, and the phosphate may be present, for example, in the gaps between the positive electrode active materials in particulate form. Even in this case, the first compound, the second compound, and the phosphate preferentially react with hydrogen fluoride produced by decomposition of the non-aqueous electrolyte. As a result, the lithium-containing transition metal composite oxide can be protected from hydrogen fluoride, thereby achieving the effects of the present disclosure.
[0055] The first compound is, for example, a compound containing at least one of sulfate, oxide, hydroxide, and chloride containing at least one of Ca and Sr. An example of the first compound is CaSO 4 , CaO, Ca(OH) 2 , CaCl 2 , SrSO 4 , SrO, Sr(OH) 2 , SrCl 2 An example of the second compound is Li 3-x H x P.O. 4 (0≦x≦3). An example of a phosphate is Ca(H 2 P.O. 4 ) 2 , Ca(H 2 P.O. 4 ) 2 ・H 2 O, CaHPO 4 , CaHPO 4 (H 2 O), Ca 3 (P.O. 4 ) 2 , Sr(H 2 P.O. 4 ) 2 , SrHPO 4 , Sr 3 (P.O. 4 ) 2 The first compound, the second compound, and the phosphate may be used singly or in combination of two or more. The presence of the first compound, the second compound, and the phosphate can be confirmed by synchrotron XRD measurement, X-ray photoelectron spectroscopy (XPS), time-of-flight secondary ion mass spectrometry (TOF-SIMS), or the like.
[0056] The amounts of P, Ca, and Sr contained in the positive electrode mixture layer are preferably 0.001% by mass or more and 1% by mass or less, and more preferably 0.01% by mass or more and 1% by mass or less, relative to the total mass of the positive electrode active material. In this case, the effects of the present disclosure are more significantly exhibited. Furthermore, the amounts of P, Ca, and Sr contained in the positive electrode mixture layer may vary in the thickness direction of the positive electrode mixture layer, but are preferably approximately the same throughout the thickness direction of the positive electrode mixture layer.
[0057] The positive electrode mixture layer further includes, for example, a conductive agent and a binder. Examples of the conductive agent included in the positive electrode mixture layer include carbon black (CB) such as acetylene black (AB) and ketjen black, carbon nanotubes (CNT), graphene, graphite, and other carbon-based particles. These may be used alone or in combination of two or more.
[0058] Examples of binders contained in the positive electrode mixture layer include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyimide-based resins, acrylic-based resins, polyolefin-based resins, polyacrylonitrile (PAN), etc. These may be used alone or in combination of two or more.
[0059] The positive electrode 11, which is an example of an embodiment, can be produced, for example, through an active material production process for producing a positive electrode active material, a preparation process for preparing a positive electrode slurry containing the positive electrode active material, a conductive agent, and a binder, a coating process for applying the positive electrode slurry to the surface of a positive electrode core and drying it, and a rolling process for rolling the coating film produced in the coating process. Here, a compound containing at least one of Ca and Sr and a compound containing P may be added in the preparation process. This makes it possible to disperse the first compound and the second compound, or a phosphate, in the positive electrode mixture layer. Note that if the second addition process is performed in the production of the above-described positive electrode active material, the compound containing at least one of Ca and Sr and the compound containing P may not be added in the preparation process.
[0060] [Negative Electrode] The negative electrode 12 may have, for example, a negative electrode core and a negative electrode mixture layer formed on the surface of the negative electrode core, or a metal Li foil may be used as the negative electrode 12. Alternatively, the negative electrode 12 may have a negative electrode core, and lithium metal may be deposited on the surface of the negative electrode core upon charging. When the negative electrode 12 has a negative electrode mixture layer, the negative electrode mixture layer is preferably formed on both sides of the negative electrode core. The negative electrode core may be a foil of a metal stable within the potential range of the negative electrode 12, such as copper or a copper alloy, or a film with such a metal disposed on the surface. The thickness of the negative electrode core is, for example, 5 μm or more and 30 μm or less. The negative electrode mixture layer includes, for example, a negative electrode active material and a binder. The thickness of the negative electrode mixture layer is, for example, 10 μm or more and 150 μm or less on one side of the negative electrode core. The negative electrode 12 can be produced, for example, by applying a negative electrode mixture slurry containing a negative electrode active material, a binder, etc. to the surface of a negative electrode core, drying the coating, and then rolling it to form a negative electrode mixture layer on both sides of the negative electrode core.
[0061] The negative electrode active material contained in the negative electrode mixture layer is not particularly limited as long as it can reversibly absorb and release lithium ions, and generally, carbon materials such as graphite are used. Graphite may be any of natural graphite such as flake graphite, lump graphite, and amorphous graphite, or artificial graphite such as lump artificial graphite and graphitized mesophase carbon microbeads. Furthermore, metals that alloy with Li, such as Si and Sn, metal compounds containing Si, Sn, and lithium-titanium composite oxides may also be used as the negative electrode active material. Furthermore, those provided with a carbon coating may also be used. For example, SiO x (0.5≦x≦1.6) or Li 2y SiO (2+y) A Si-containing compound in which fine particles of Si are dispersed in a lithium silicate phase represented by (0<y<2) may be used in combination with graphite.
[0062] Examples of binders contained in the negative electrode mixture layer include styrene butadiene rubber (SBR), nitrile butadiene rubber (NBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc., or a partially neutralized salt), polyvinyl alcohol (PVA), etc. These may be used alone or in combination of two or more.
[0063] [Separator] A porous sheet having ion permeability and insulating properties is used for the separator 13. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator 13 include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may have a single-layer structure or a multi-layer structure. Furthermore, a highly heat-resistant resin layer such as an aramid resin may be formed on the surface of the separator 13.
[0064] A filler layer containing an inorganic filler may be formed at the interface between the separator 13 and at least one of the positive electrode 11 and the negative electrode 12. Examples of inorganic fillers include oxides and phosphate compounds containing metal elements such as Ti, Al, Si, and Mg. The filler layer can be formed by applying a slurry containing the filler to the surface of the positive electrode 11, the negative electrode 12, or the separator 13.
[0065] [Non-aqueous electrolyte] The non-aqueous electrolyte has ion conductivity (for example, lithium ion conductivity). The non-aqueous electrolyte may be a liquid electrolyte (electrolytic solution) or a solid electrolyte.
[0066] The liquid electrolyte (electrolytic solution) contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent that can be used include esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more of these. The non-aqueous solvent may contain a halogen-substituted compound in which at least a portion of the hydrogen atoms in these solvents are substituted with halogen atoms such as fluorine. Examples of the halogen-substituted compound include fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, and fluorinated chain carboxylic acid esters such as methyl fluoropropionate (FMP).
[0067] Examples of the esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylic acid esters such as γ-butyrolactone (GBL) and γ-valerolactone (GVL); and chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP).
[0068] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ethers, 1,2-dimethoxyethane ethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, and methyl phenyl ether. and chain ethers such as ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.
[0069] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiClO 4 , LiBF 4 , LiPF 6 , LiAlCl 4 , LiSbF 6 , LiSCN, LiCF 3 SO 3 , LiCF 3 CO 2 , LiAsF 6 , LiB 10 Cl 10 , lower aliphatic lithium carboxylates, LiCl, LiBr, LiI, phosphates, borates, and imide salts. Examples of phosphates include lithium difluorophosphate (LiPO 2 F 2Examples of the borate salt include lithium bis(oxalato)borate (LiBOB) and lithium difluoro(oxalato)borate (LiDFFOB). Examples of the imide salt include lithium bisfluorosulfonylimide (LiN(FSO 2 ) 2 ), lithium bistrifluoromethanesulfonyl imide (LiN(CF 3 SO 2 ) 2 ), lithium trifluoromethanesulfonate nonafluorobutanesulfonate imide (LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 )), lithium bispentafluoroethanesulfonyl imide (LiN(C 2 F 5 SO 2 ) 2 Among these, LiPF is preferred from the viewpoint of ionic conductivity, electrochemical stability, etc. 6 The concentration of the lithium salt may be, for example, 4 mol or less, or 3 mol or less, preferably 1.8 mol or less, and more preferably 0.8 mol or more and 1.8 mol or less, per 1 L of the non-aqueous solvent.
[0070] The non-aqueous electrolyte may contain an additive such as an unsaturated carbonate ester, an acid anhydride, a phenol compound, a benzene compound, a nitrile compound, an isocyanate compound, a sultone compound, a sulfate compound, a borate ester compound, a phosphate ester compound, or a phosphite ester compound.
[0071] Examples of unsaturated cyclic carbonates include vinylene carbonate, 4-methylvinylene carbonate, 4,5-dimethylvinylene carbonate, 4-ethylvinylene carbonate, 4,5-diethylvinylene carbonate, 4-propylvinylene carbonate, 4,5-dipropylvinylene carbonate, 4-phenylvinylene carbonate, 4,5-diphenylvinylene carbonate, vinylethylene carbonate, and divinylethylene carbonate. One type of unsaturated cyclic carbonate may be used alone, or two or more types may be used in combination. Some of the hydrogen atoms in the unsaturated cyclic carbonate may be substituted with fluorine atoms. The acid anhydride may be an anhydride formed by intermolecular condensation of multiple carboxylic acid molecules, but is preferably an acid anhydride of a polycarboxylic acid. Examples of polycarboxylic acid anhydrides include succinic anhydride, maleic anhydride, and phthalic anhydride.
[0072] Examples of phenolic compounds include phenol, hydroxytoluene, etc. Examples of benzene compounds include fluorobenzene, hexafluorobenzene, cyclohexylbenzene (CHB), etc.
[0073] Examples of nitrile compounds include adiponitrile, pimelonitrile, propionitrile, and succinonitrile. Examples of isocyanate compounds include methyl isocyanate (MIC), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), and bisisocyanatomethylcyclohexane (BIMCH). Examples of sultone compounds include propane sultone and propene sultone. Examples of sulfate compounds include ethylene sulfate, ethylene sulfite, dimethyl sulfate, and lithium fluorosulfate. Examples of borate ester compounds include trimethyl borate and tris(trimethylsilyl)borate. Examples of phosphate ester compounds include trimethyl phosphate and tris(trimethylsilyl)phosphate. Examples of phosphite ester compounds include trimethyl phosphite and tris(trimethylsilyl)phosphite.
[0074] As the solid electrolyte, for example, a solid or gel-like polymer electrolyte, an inorganic solid electrolyte, etc. can be used. As the inorganic solid electrolyte, a material known in all-solid-state lithium ion secondary batteries, etc. (for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a halogen-based solid electrolyte, etc.) can be used. The polymer electrolyte includes, for example, a lithium salt and a matrix polymer, or a non-aqueous solvent, a lithium salt, and a matrix polymer. As the matrix polymer, for example, a polymer material that absorbs the non-aqueous solvent and gels is used. As the polymer material, for example, a fluororesin, an acrylic resin, a polyether resin, etc. can be used.
[0075] Hereinafter, the present disclosure will be further described with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.
[0076] Example 1 Preparation of Positive Electrode Active Material [Ni 0.90 Mn 0.10 ](OH) 2The composite hydroxide represented by the formula (1) was calcined at 500°C for 8 hours to obtain a metal oxide containing Ni and Mn. Next, lithium hydroxide monohydrate (LiOH·H) was added to the composite hydroxide represented by the formula (1) so that the molar ratio of Li to the total amount of Ni and Mn was 1:1.03. 2 O) was mixed to obtain a mixture. Then, this mixture was placed under an oxygen flow (10 cm) with an oxygen concentration of 95%. 3 The mixture was heated from room temperature to 650°C at a temperature increase rate of 2.0°C / min under a temperature of 2 mL / min per kg of the mixture and 5 L / min per kg of the mixture, and then heated from 650°C to 740°C at a temperature increase rate of 0.5°C / min to obtain a lithium-containing transition metal composite oxide (synthesis step).
[0077] Water was added to the lithium-containing transition metal composite oxide obtained in the synthesis step so that the slurry concentration was 1500 g / L, and the mixture was stirred for 15 minutes and filtered to obtain a cake-like composition (washing step). 2 and H 3 P.O. 4 were added simultaneously (second addition step). 2 and H 3 P.O. 4 The masses of Ca and P in the positive electrode active material were 0.02 mass % and 0.02 mass %, respectively, relative to the total mass of the positive electrode active material. 2 and H 3 P.O. 4Powdered lithium methanesulfonate was added to the cake-like composition to which the lithium methanesulfonate had been added (first addition step). The amount of lithium methanesulfonate added was 0.3 mass% relative to the total mass of the lithium-containing transition metal composite oxide. The resulting cake-like composition was dried under vacuum at 180°C for 2 hours to obtain the positive electrode active material of Example 1 (drying step). The prepared positive electrode active material was measured by Fourier transform infrared spectroscopy (FT-IR), confirming the presence of lithium methanesulfonate on the secondary particle surface of the lithium-containing transition metal composite oxide. Furthermore, TOF-SIMS confirmed the presence of Ca and P on the secondary particle surface of the lithium-containing transition metal composite oxide. This suggests that a Ca-containing compound (first compound) and a P-containing compound (second compound) or a phosphate containing Ca are present on the secondary particle surface.
[0078] [Preparation of Positive Electrode] The positive electrode active material, acetylene black (AB), and polyvinylidene fluoride were mixed in a mass ratio of 86:10:4, and N-methyl-2-pyrrolidone (NMP) was used as a dispersion medium to prepare a positive electrode mixture slurry. Next, the positive electrode mixture slurry was applied to a positive electrode core made of aluminum foil, the coating was dried and compressed, and then the positive electrode core was cut to a predetermined electrode size to obtain a positive electrode in which a positive electrode mixture layer was disposed on both sides of the positive electrode core. In addition, an exposed portion in which the surface of the positive electrode core was exposed was provided in a part of the positive electrode.
[0079] [Preparation of non-aqueous electrolyte] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF 6 ) was dissolved in the solution to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.
[0080] [Preparation of Test Cell] A positive electrode lead was attached to the exposed portion of the positive electrode, and a negative electrode lead was attached to the lithium metal foil serving as the negative electrode. The positive electrode and the negative electrode were spirally wound with a polyolefin separator interposed therebetween to prepare a wound electrode assembly. This electrode assembly was housed in an exterior body made of an aluminum laminate sheet, and the nonaqueous electrolyte was poured into it. The opening of the exterior body was then sealed to obtain a test cell.
[0081] [Evaluation of Reaction Resistance] The test cell was subjected to constant current charging at 0.2 C in a temperature environment of 25 ° C until the battery voltage reached 4.4 V (vs. Li), and constant voltage charging at 4.4 V until the current value reached 0.02 C. After a 1-hour pause, the cell was discharged at a constant current of 0.2 C until it reached 2.5 V, which was the initial charge / discharge. Next, after a 2-hour pause in a temperature environment of 10 ° C, the cell was subjected to constant voltage charging at 4.4 V with a current value equivalent to 0.01 C using a Solartron 1255B (manufactured by Solartron), and the AC impedance of each cell was measured at an applied voltage of 10 mV and a measurement frequency range of 0.01 to 200 kHz. The value of the reaction resistance was determined from the Nyquist plot (an arc of about 1 Hz to 0.1 Hz).
[0082] [Evaluation of cycle characteristics] The test cell was charged to 4.4 V (vs. Li) at a constant current of 0.2 C in a temperature environment of 25°C, and then charged at a constant voltage of 4.4 V until the current value reached 0.01 C. After a 1-hour rest, the cell was discharged to 2.5 V at a constant current of 0.2 C, which constituted one cycle. The discharge capacity at 0.2 C after 30 cycles was measured. The capacity retention rate was calculated using the following formula: Capacity retention rate = Discharge capacity after 30 cycles / Discharge capacity at first cycle
[0083] Example 2 In the second addition step of preparing a positive electrode active material, CaCl was added so that the masses of Ca and P in the positive electrode active material were 0.02 mass % and 0.04 mass %, respectively, relative to the total mass of the positive electrode active material. 2 and H 3 P.O. 4 A test cell was prepared in the same manner as in Example 1 except that the above was added, and evaluation was carried out.
[0084] Example 3 In the second addition step of preparing a positive electrode active material, CaCl was added so that the masses of Ca and P in the positive electrode active material were 0.04 mass % and 0.02 mass %, respectively, relative to the total mass of the positive electrode active material. 2 and H 3 P.O. 4 A test cell was prepared in the same manner as in Example 1 except that the above was added, and evaluation was carried out.
[0085] Example 4 In the second addition step of preparing a positive electrode active material, CaCl was added so that the masses of Ca and P in the positive electrode active material were 0.04 mass % and 0.01 mass %, respectively, relative to the total mass of the positive electrode active material. 2 and H 3 P.O. 4 A test cell was prepared in the same manner as in Example 1 except that the above was added, and evaluation was carried out.
[0086] Example 5 In the second addition step of preparing a positive electrode active material, CaCl was added so that the masses of Ca and P in the positive electrode active material were 0.01 mass % and 0.04 mass %, respectively, relative to the total mass of the positive electrode active material. 2 and H 3 P.O. 4 A test cell was prepared in the same manner as in Example 1 except that the above was added, and evaluation was carried out.
[0087] Example 6 In the second addition step of the preparation of the positive electrode active material, CaCl 2 and H 3 P.O. 4 Instead of Ca(H 2 P.O. 4 ) 2 ・H 2 A test cell was prepared in the same manner as in Example 1 except for adding O, and evaluation was carried out. 2 P.O. 4 ) 2 ・H 2O was added so that the masses of Ca and P in the positive electrode active material were 0.02 mass % and 0.04 mass %, respectively, relative to the total mass of the positive electrode active material. Furthermore, TOF-SIMS confirmed the presence of Ca and P on the surface of the secondary particles of the lithium-containing transition metal composite oxide. This suggests that a Ca-containing compound (first compound) and a P-containing compound (second compound) or a phosphate containing Ca are present on the surface of the secondary particles.
[0088] Comparative Example 1 A test cell was produced and evaluated in the same manner as in Example 1, except that the first addition step and the second addition step were not performed in the production of the positive electrode active material.
[0089] Comparative Example 2 A test cell was produced and evaluated in the same manner as in Example 1, except that the second addition step was not carried out in the production of the positive electrode active material.
[0090] Comparative Example 3 In the production of a positive electrode, the first addition step was not performed, and CaCl 2 A test cell was prepared and evaluated in the same manner as in Example 1, except that only CaCl was added so that the mass of Ca in the positive electrode active material was 0.01 mass % relative to the total mass of the positive electrode active material. 2 Furthermore, it was confirmed by TOF-SIMS that a Ca-containing compound (first compound) was present on the surface of the secondary particles of the lithium-containing transition metal composite oxide.
[0091] Comparative Example 4 In the production of a positive electrode, the first addition step was not performed, and H 3 P.O. 4 A test cell was prepared and evaluated in the same manner as in Example 1, except that only H was added. 3 P.O. 4 Furthermore, it was confirmed by TOF-SIMS that a P-containing compound (second compound) was present on the surface of the secondary particles of the lithium-containing transition metal composite oxide.
[0092] Comparative Example 5 In the production of a positive electrode, the first addition step was not performed, and H3 P.O. 4 A test cell was prepared and evaluated in the same manner as in Example 1, except that only H was added. 3 P.O. 4 Furthermore, it was confirmed by TOF-SIMS that a P-containing compound (second compound) was present on the surface of the secondary particles of the lithium-containing transition metal composite oxide.
[0093] Comparative Example 6 A test cell was prepared and evaluated in the same manner as in Example 1, except that the first addition step was not performed in the preparation of the positive electrode. CaCl was added so that the masses of Ca and P in the positive electrode active material were 0.01 mass % and 0.04 mass %, respectively, relative to the total mass of the positive electrode active material. 2 and H 3 P.O. 4 was added. Furthermore, it was confirmed by TOF-SIMS that Ca and P were present on the surface of the secondary particles of the lithium-containing transition metal composite oxide. This suggests that a Ca-containing compound (first compound) and a P-containing compound (second compound) or a phosphate containing Ca were present on the surface of the secondary particles.
[0094] Comparative Example 7 In the production of a positive electrode, CaCl 2 A test cell was prepared and evaluated in the same manner as in Example 1, except that only CaCl was added so that the mass of Ca in the positive electrode active material was 0.01 mass % relative to the total mass of the positive electrode active material. 2 Furthermore, it was confirmed by TOF-SIMS that a Ca-containing compound (first compound) was present on the surface of the secondary particles of the lithium-containing transition metal composite oxide.
[0095] Comparative Example 8 In the production of a positive electrode, in the second addition step, H 3 P.O. 4 A test cell was prepared and evaluated in the same manner as in Example 1, except that only H was added. 3 P.O. 4Furthermore, it was confirmed by TOF-SIMS that a P-containing compound (second compound) was present on the surface of the secondary particles of the lithium-containing transition metal composite oxide.
[0096] Comparative Example 9 In the production of a positive electrode, in the second addition step, H 3 P.O. 4 A test cell was prepared and evaluated in the same manner as in Example 1, except that only H was added. 3 P.O. 4 Furthermore, it was confirmed by TOF-SIMS that a P-containing compound (second compound) was present on the surface of the secondary particles of the lithium-containing transition metal composite oxide.
[0097] The reaction resistance and capacity retention rates of the test cells of Examples 1 to 6 and Comparative Examples 1 to 9 are shown in Table 1. Table 1 also shows the composition of the lithium-containing transition metal composite oxide, the type and amount of the sulfonic acid compound added in the first addition step, and the type, amount, and timing of addition of the compound added in the second addition step. The reaction resistance and capacity retention rates of the test cells of Examples 1 to 6 and Comparative Examples 1 to 9 shown in Table 1 are expressed relative to the reaction resistance and capacity retention rate of the test cell of Comparative Example 1, which are set at 100. A smaller value for the reaction resistance means a reduced reaction resistance, and a larger value for the capacity retention rate means better cycle characteristics.
[0098]
[0099] As shown in Table 1, the test cells of the examples exhibited reduced reaction resistance and improved cycle characteristics compared to the test cells of the comparative examples. On the other hand, the test cell of comparative example 2, in which the sulfonic acid compound was present on the surfaces of the secondary particles but the first compound and the second compound were not present on the surfaces of the secondary particles, exhibited reduced reaction resistance compared to the test cell of comparative example 1, but deteriorated cycle characteristics. This is presumably because the function of the sulfonic acid compound increased reactivity at the positive electrode, resulting in an increase in the amount of hydrogen fluoride generated by a side reaction between the positive electrode active material and the non-aqueous electrolyte.
[0100] Furthermore, the test cell of Comparative Example 6, in which the sulfonic acid compound was not present on the surfaces of the secondary particles but the first compound and the second compound, or the phosphate, had improved cycle characteristics but increased reaction resistance compared to the test cell of Comparative Example 1. This is presumably because at least a portion of the surfaces of the secondary particles was covered with the first compound and the second compound, or the phosphate, making it difficult for Li to be inserted and extracted from the surfaces of the secondary particles.
[0101] Furthermore, the test cells of Comparative Examples 7, 8, and 9, in which a sulfonic acid compound was present on the surface of the secondary particles but only one of the first compound and the second compound was present, exhibited reduced reaction resistance and improved cycle characteristics compared to the test cell of Comparative Example 1. However, the improvement effect of the test cells of Comparative Examples 7, 8, and 9 was smaller than that of the test cell of the Example. From these results, it can be said that the effects of the present disclosure are more pronounced when a sulfonic acid compound is present on the surface of the secondary particles while both the first compound and the second compound or a phosphate is present. Furthermore, when comparing the test cell of Comparative Example 8 with the test cell of Comparative Example 9, the test cell of Comparative Example 9 exhibited slightly improved cycle characteristics but actually increased reaction resistance. In other words, when either the first compound or the second compound was present on the surface of the secondary particles, it was difficult to achieve both excellent reaction resistance and cycle characteristics even if the mass of the first compound or the second compound was increased.
[0102] Example 7 In the preparation of the positive electrode active material, the composition of the composite hydroxide was changed to [Ni 0.90 Co 0.05 Al 0.05 ](OH) 2 In more detail, in the preparation of the positive electrode, the positive electrode active material, acetylene black (AB), and polyvinylidene fluoride were mixed in a mass ratio of 86:10:4, and SrCl 2 (first compound) and Li 3 P.O. 4(second compound) was added at the same time, and N-methyl-2-pyrrolidone (NMP) was used as a dispersion medium to prepare a positive electrode mixture slurry. 2 and Li 3 P.O. 4 In the positive electrode active material, Sr and P were added so that their masses were 0.01% by mass and 0.04% by mass, respectively, relative to the total mass of the positive electrode active material. Furthermore, TOF-SIMS confirmed the presence of Sr and P in the positive electrode mixture layer of the lithium-containing transition metal composite oxide. This suggests that at least a Sr-containing compound (first compound) and a P-containing compound (second compound) are present in the positive electrode mixture layer.
[0103] Example 8 In the second addition step of the positive electrode preparation, SrCl 2 and Li 3 P.O. 4 Instead of Ca 3 (P.O. 4 ) 2 A test cell was prepared and evaluated in the same manner as in Example 7, except that Ca was added. 3 (P.O. 4 ) 2 In the present example, the masses of Ca and P in the positive electrode mixture layer were 0.02% by mass and 0.04% by mass, respectively, relative to the total mass of the positive electrode active material. Furthermore, the presence of Ca and P in the positive electrode mixture layer of the lithium-containing transition metal composite oxide was confirmed by TOF-SIMS. From this, it is presumed that a phosphate containing at least Ca is present in the positive electrode mixture layer.
[0104] <Comparative Example 10> A test cell was produced and evaluated in the same manner as in Example 7, except that the first addition step was not performed in the production of the positive electrode active material, and the second addition step was not performed in the production of the positive electrode.
[0105] Comparative Example 11 A test cell was produced and evaluated in the same manner as in Example 7, except that the second addition step was not carried out in the production of the positive electrode.
[0106] Comparative Example 12 A test cell was produced and evaluated in the same manner as in Example 7, except that the first addition step was not carried out in the production of the positive electrode active material.
[0107] The reaction resistance and capacity retention rates of the test cells of Examples 7 and 8 and Comparative Examples 10 to 12 are shown in Table 2. Table 2 also shows the composition of the lithium-containing transition metal composite oxide, the type and amount of the sulfonic acid compound added in the first addition step, and the type, amount, and timing of addition of the compound added in the second addition step. The reaction resistance and capacity retention rates of the test cells of Examples 7 and 8 and Comparative Examples 10 to 12 shown in Table 1 are expressed relative to the reaction resistance and capacity retention rate of the test cell of Comparative Example 10, which are set to 100. A smaller value for the reaction resistance indicates a reduced reaction resistance, and a larger value for the capacity retention rate indicates better cycle characteristics.
[0108]
[0109] As shown in Table 2, the test cells of the examples have improved cycle characteristics while reducing reaction resistance compared to the test cells of the comparative examples. In other words, the effects of the present disclosure are exerted even when a sulfonic acid compound is present on the surfaces of the secondary particles and the first compound and the second compound or a phosphate is present in the positive electrode mixture layer.
[0110] The present disclosure will be further described by the following embodiments. Configuration 1: A positive electrode for a non-aqueous electrolyte secondary battery, comprising a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core, wherein the positive electrode mixture layer contains a lithium-containing transition metal composite oxide having a layered structure as a positive electrode active material, and the lithium-containing transition metal composite oxide is represented by the general formula Li x Ni a Co b Mn c M d O 2-y(wherein 0.8<x<1.2, 0.75≦a≦0.98, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, Ca, Sr, and Zr), and the positive electrode for a non-aqueous electrolyte secondary battery is a positive electrode for a non-aqueous electrolyte secondary battery, the positive electrode being represented by formula (I), wherein the positive electrode mixture layer is a first compound containing at least one of Ca and Sr and a second compound containing P, or a phosphate containing at least one of Ca and Sr. (wherein A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) Configuration 2: The positive electrode for a non-aqueous electrolyte secondary battery according to Configuration 1, wherein A is a Group 1 element. Configuration 3: The positive electrode for a non-aqueous electrolyte secondary battery according to Configuration 1 or 2, wherein A is Li. Configuration 4: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 3, wherein R is an alkyl group. Configuration 5: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 4, wherein R is a methyl group. Configuration 6: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 5, wherein the first compound, the second compound, and the phosphate are present on the surfaces of the secondary particles. Configuration 7: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 6, wherein in the positive electrode active material, the amount of the sulfonic acid compound present on the surfaces of the secondary particles is 0.05 mass % or more and 1.5 mass % or less, relative to the total mass of the lithium-containing transition metal composite oxide. Configuration 8: The positive electrode for a nonaqueous electrolyte secondary battery according to any one of Configurations 1 to 7, wherein the amounts of P, Ca, and Sr contained in the first compound, the second compound, and the phosphate are 0.001 mass % or more and 1 mass % or less, relative to the total mass of the positive electrode active material. Configuration 9: A method for manufacturing a positive electrode for a non-aqueous electrolyte secondary battery, the method comprising: an active material preparation step of preparing a positive electrode active material; a preparation step of preparing a positive electrode slurry containing the positive electrode active material; a coating step of applying the positive electrode slurry to a surface of a positive electrode core; and a rolling step of rolling the coating film formed in the coating step, wherein the active material preparation step comprises: a synthesis step of obtaining a lithium-containing transition metal composite oxide; a washing step of washing the lithium-containing transition metal composite oxide with water and dehydrating it to obtain a cake-like composition; a first addition step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition; and a drying step of drying the cake-like composition to obtain a powder-like composition, the method further comprising a second addition step of adding a compound containing at least one of Ca and Sr and a compound containing P, or adding a phosphate containing at least one of Ca and Sr to the positive electrode slurry or the cake-like composition.Configuration 10: A non-aqueous electrolyte secondary battery comprising the positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 8, a negative electrode, and a non-aqueous electrolyte.
[0111] REFERENCE SIGNS LIST 10 non-aqueous electrolyte secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 16 exterior body, 17 sealing body, 18, 19 insulating plate, 20 positive electrode lead, 21 negative electrode lead, 22 grooved portion, 23 internal terminal plate, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cap, 28 gasket
Claims
1. A positive electrode for a non-aqueous electrolyte secondary battery having a positive electrode core and a positive electrode mixture layer formed on a surface of the positive electrode core, the positive electrode mixture layer containing a lithium-containing transition metal composite oxide having a layered structure as a positive electrode active material, the lithium-containing transition metal composite oxide being represented by the general formula Li x Ni a Co b Mn c M d O 2-y (wherein 0.8<x<1.2, 0.75≦a≦0.98, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, Ca, Sr, and Zr), and is a secondary particle formed by aggregation of primary particles, a sulfonic acid compound represented by formula (I) is present on surfaces of the secondary particles, and the positive electrode mixture layer contains a first compound containing at least one of Ca and Sr and a second compound containing P, or contains a phosphate containing at least one of Ca and Sr. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) 2. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein A is a Group 1 element.
3. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein A is Li.
4. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein R is an alkyl group.
5. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein R is a methyl group.
6. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the first compound, the second compound, and the phosphate are present on the surface of the secondary particles.
7. The positive electrode for a nonaqueous electrolyte secondary battery according to claim 1, wherein in the positive electrode active material, the amount of the sulfonic acid compound present on the surfaces of the secondary particles is 0.05 mass % or more and 1.5 mass % or less with respect to the total mass of the lithium-containing transition metal composite oxide.
8. The positive electrode for a nonaqueous electrolyte secondary battery according to claim 1, wherein the amounts of P, Ca, and Sr contained in the first compound, the second compound, and the phosphate are 0.001 mass % or more and 1 mass % or less with respect to the total mass of the positive electrode active material.
9. A method for producing a positive electrode for a non-aqueous electrolyte secondary battery, comprising: an active material preparation step of preparing a positive electrode active material; a preparation step of preparing a positive electrode slurry containing the positive electrode active material; a coating step of applying the positive electrode slurry to a surface of a positive electrode core; and a rolling step of rolling the coating film produced in the coating step, wherein the active material preparation step comprises: a synthesis step of obtaining a lithium-containing transition metal composite oxide; a washing step of washing the lithium-containing transition metal composite oxide with water and dehydrating it to obtain a cake-like composition; a first addition step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition; and a drying step of drying the cake-like composition to obtain a powder-like composition, and further comprising a second addition step of adding a compound containing at least one of Ca and Sr and a compound containing P, or adding a phosphate containing at least one of Ca and Sr to the positive electrode slurry or the cake-like composition.
10. A non-aqueous electrolyte secondary battery comprising the positive electrode for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 8, a negative electrode, and a non-aqueous electrolyte.
Citation Information
Patent Citations
Positive electrode for lithium-ion secondary battery, method of manufacturing the same, and lithium-ion secondary battery
JP2009123463A
Cathode active material, cathode using it and nonaqueous electrolyte secondary battery
JP2009187940A
Nonaqueous electrolyte secondary battery
JP2015090858A
Positive electrode active material for lithium ion secondary battery, and lithium ion secondary battery
JP2019169286A
Salted eggs manufacturing method
KR1020210004417A
Cited By
Positive electrode active material for nonaqueous electrolyte secondary batteries