Magnesium potassium titanate, friction adjusting material, friction material composition, friction material, and friction member
The magnesium potassium titanate-based friction material composition addresses the low friction coefficient in high-load regions and environmental copper concerns by using a pseudo-tunnel crystal structure and minimal copper content, enhancing braking performance and reducing environmental impact.
Patent Information
- Application Number
- PCT/JP2024/017660
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-13
- Publication Date
- 2024-12-05
AI Technical Summary
Friction materials used in vehicle brakes face challenges in maintaining a high coefficient of friction, especially in high-load regions, while also needing to reduce copper content due to environmental regulations, and magnesium potassium titanate has shown excellent wear resistance but inadequate friction coefficient in these regions.
A friction material composition incorporating magnesium potassium titanate with a specific pseudo-tunnel crystal structure, formulated with a binder and minimal copper content, enhances the coefficient of friction in high-load regions and stabilizes it through controlled particle size and surface area, and alkali metal ion elution rates.
The magnesium potassium titanate-based friction material composition effectively increases the coefficient of friction in high-load regions, reduces wear dust generation, and meets environmental copper content regulations, providing improved braking performance and reduced environmental impact.
Smart Images

Figure JP2024017660_05122024_PF_FP_ABST
Abstract
Description
Magnesium potassium titanate, friction modifier, friction material composition, friction material, and friction member
[0001] The present invention relates to magnesium potassium titanate, and to a friction modifier, a friction material composition, a friction material, and a friction member each using the magnesium potassium titanate.
[0002] Friction materials used in brakes such as disc brakes and drum brakes that constitute braking devices for various vehicles, industrial machinery, etc. are required to have a large and stable friction coefficient, excellent wear resistance, and low attack on mating materials. Such friction materials are classified into three types: semi-metallic materials containing steel fibers such as steel fibers or stainless steel fibers as a fiber base material in a proportion of 30% by mass or more but less than 60% by mass; low-steel materials containing steel fibers in a proportion of 10% by mass or more but less than 30% by mass; and NAO (Non-Asbestos-Organic) materials that do not contain steel fibers. However, friction materials containing trace amounts of steel fibers are also classified as NAO materials.
[0003] In Japan and the United States, where comfort is emphasized, NAO materials are mainstream because they are less aggressive to mating materials and have an excellent balance between noise and wear resistance.In Europe, low-steel materials are mainstream because they maintain the friction coefficient during high-speed braking.
[0004] Compositions used in friction materials (hereinafter referred to as "friction material compositions") generally contain copper fibers or copper powder. The primary role of copper is to provide thermal conductivity. Because of its high thermal conductivity, copper diffuses heat generated during braking away from the friction interface, reducing friction material wear due to excessive temperature rise and suppressing vibration during braking. The secondary role of copper is to protect the friction interface during high-temperature braking. Due to its malleability, copper spreads to the surface of the friction material during braking to form a coating. It also migrates to the surface of the mating material to form an adhesive coating (hereinafter referred to as a "transfer film"). These protective films reduce friction material wear during high-temperature braking and enable the development of a stable friction coefficient. However, friction materials containing copper contain copper in the wear debris generated during braking, which may cause pollution of rivers, lakes, and oceans. Therefore, state laws have been enacted in California and Washington, USA, prohibiting the sale and installation of friction materials containing 0.5% by mass or more of copper in new vehicles from 2025 onward.
[0005] Therefore, in NAO materials, titanates have attracted attention as a component other than copper that plays a role in the transfer film. Titanates include titanates with tunnel crystal structures (e.g., potassium hexatitanate) and titanates with layered crystal structures (e.g., magnesium potassium titanate), and these are used alone or in combination depending on the application of the friction material. For example, a friction material composition containing titanate and barium sulfate with an average particle size of 0.1 μm to 20 μm (Patent Document 1) has been proposed.
[0006] International Publication No. 2018 / 164028
[0007] Hybrid and electric vehicles, which have become increasingly popular in recent years, are equipped with regenerative brakes to recover frictional energy during braking. However, this mechanism does not function when the battery is fully charged, and it is anticipated that the load on the brakes will increase due to the increased vehicle weight caused by the battery. Furthermore, with the spread of heavy, large vehicles such as SUVs, it is becoming increasingly important for friction materials to have a high coefficient of friction in high-load areas. Furthermore, in some mountainous regions, there is an issue of insufficient braking force when overloaded vehicles descend steep roads.
[0008] Potassium hexatitanate, which has a thermally stable crystal structure, is a promising titanate that provides a friction coefficient in the high load range, but its use is being discouraged, particularly in Europe, due to concerns about the inclusion of WHO fibers (fibrous particles with a major axis of 5 μm or more, a minor axis of 3 μm or less, and an aspect ratio of 3 or more) that exceed environmental standards.On the other hand, magnesium potassium titanate is known as a titanate that does not involve concerns about the inclusion of WHO fibers, but although it has excellent wear resistance, its friction coefficient in the high load range is an issue.
[0009] An object of the present invention is to provide magnesium potassium titanate, which, when used in a friction material, can increase the friction coefficient in a high load region, a friction modifier using the magnesium potassium titanate, a friction material composition, a friction material, and a friction member.
[0010] The present invention provides the following magnesium potassium titanate, a friction modifier, a friction material composition, a friction material, and a friction member each using the magnesium potassium titanate.
[0011] Item 1 Composition formula K x Mg 0.4 Ti 1.6 O 4-y [wherein x is 0.1≦x≦0.6, y=(0.8−x) / 2], and in the Raman spectroscopy of the magnesium potassium titanate, -1 ~165cm -1 Peak area (Ia) at 215 cm -1 ~325cm -1The ratio (Ia / Ib) of the peak area at 785 cm to the peak area (Ib) at 785 cm is 0.03 or more. -1 ~900cm -1 Peak area (Ic) at 215 cm -1 ~325cm -1 Magnesium potassium titanate, wherein the ratio (Ic / Ib) of the peak area to the peak area (Ib) at
[0012] Item 2. The magnesium potassium titanate according to Item 1, which is substantially free of anatase titanium dioxide.
[0013] Item 3. The magnesium potassium titanate according to Item 1 or 2, wherein the magnesium potassium titanate is in the form of plate-like particles.
[0014] Item 4. The magnesium potassium titanate according to any one of Items 1 to 3, wherein the magnesium potassium titanate has an average particle size of 0.1 μm to 100 μm.
[0015] Item 5. The magnesium potassium titanate has a specific surface area of 0.1 m 2 / g to 10m 2 Item 5. The magnesium potassium titanate according to any one of items 1 to 4, wherein the saturation coefficient is 0.15.
[0016] Item 6. The magnesium potassium titanate according to any one of Items 1 to 5, wherein the magnesium potassium titanate has an alkali metal ion elution rate of 0.01% by mass to 15% by mass.
[0017] Item 7. A friction modifier comprising the magnesium potassium titanate according to any one of items 1 to 6.
[0018] Item 8. A friction material composition comprising the magnesium potassium titanate according to any one of items 1 to 6 and a binder, wherein the copper content is less than 0.5% by mass in terms of elemental copper, relative to 100% by mass of the total amount of the friction material composition.
[0019] Item 9. The friction material composition according to Item 8, wherein the content of the magnesium potassium titanate is 1% by mass to 40% by mass relative to 100% by mass of the total amount of the friction material composition.
[0020] Item 10. The friction material composition according to item 8 or 9, further comprising at least one of a titanate having a layered crystal structure and a titanate having a tunnel crystal structure.
[0021] Item 11. The friction material composition according to any one of Items 8 to 10, which is substantially free of a sulfide-based solid lubricant.
[0022] Item 12. The friction material composition according to any one of Items 8 to 11, wherein the content of steel fibers is less than 10% by mass relative to 100% by mass of the total amount of the friction material composition.
[0023] Item 13. The friction material composition according to any one of Items 8 to 11, wherein the content of the steel fiber is 10% by mass or more relative to 100% by mass of the total amount of the friction material composition.
[0024] Item 14. A friction material, which is a molded product of the friction material composition according to any one of items 8 to 13.
[0025] Item 15. A friction member comprising the friction material according to Item 14.
[0026] According to the present invention, it is possible to provide magnesium potassium titanate, which, when used in a friction material, can increase the friction coefficient in a high load region, a friction modifier using the magnesium potassium titanate, a friction material composition, a friction material, and a friction member.
[0027] Fig. 1 is a scanning transmission electron microscope (STEM) image of the titanate obtained in Example 1. Fig. 2 is a Raman spectroscopy spectrum of the titanate obtained in Example 1 and Comparative Example 1 and potassium hexatitanate. Fig. 3 is a graph showing the relationship between the number of braking cycles and the coefficient of friction during fade in Friction Test 1 for the friction members obtained in Example 7 and Comparative Example 3. Fig. 4 is a graph showing the relationship between the change in friction coefficient (μ) with respect to rotor temperature and the average coefficient of friction (μ) during fade in Friction Test 1 for the friction members obtained in Example 7, Comparative Example 3, and Reference Example 1. Fig. 5 is a scanning transmission electron microscope (STEM) image of the titanate obtained in Comparative Example 1.
[0028] Hereinafter, one example of a preferred embodiment of the present invention will be described. However, the following embodiment is merely an example. The present invention is not limited to the following embodiment. In this specification, the word "to" is used to mean that the numerical values before and after it are included as the lower limit and upper limit.
[0029] <1. Magnesium potassium titanate> The magnesium potassium titanate of the present invention is represented by the composition formula K x Mg 0.4 Ti 1.6 O 4-y [wherein x is 0.1≦x≦0.6, y=(0.8−x) / 2]. In addition, in the Raman spectroscopy of magnesium potassium titanate, -1 ~165cm -1 Peak area (Ia) at 215 cm -1 ~325cm -1 The ratio (Ia / Ib) of the peak area at 785 cm to the peak area (Ib) at 785 cm is 0.03 or more. -1 ~900cm -1 Peak area (Ic) at 215 cm -1 ~325cm -1 The ratio (Ic / Ib) of the peak area of the sample to the peak area (Ib) of the sample is 0.40 or less.
[0030] The present inventors have found that the compound of formula K x Mg 0.4 Ti 1.6 O 4-y [wherein x is 0.1≦x≦0.6, y=(0.8−x) / 2], and in the Raman spectroscopy of magnesium potassium titanate, -1 ~165cm -1 Peak area (Ia) at 215 cm -1 ~325cm -1 The ratio (Ia / Ib) of the peak area at 785 cm to the peak area (Ib) at 785 cm is 0.03 or more. -1 ~900cm -1 Peak area (Ic) at 215 cm -1 ~325cm -1It has been found that magnesium potassium titanate having a ratio (Ic / Ib) of 0.40 or less to the peak area (Ib) in the graph can increase the friction coefficient in a high load region when used in a friction material.
[0031] Raman spectroscopy is a technique in which, due to the fact that each crystal lattice has its own unique lattice vibration, when laser light of a specific wavelength is irradiated onto a crystal, light that has lost energy equal to the phonon energy is scattered (this is called Raman scattering).By detecting this with a spectroscope, it is possible to gain insight into phonon energy.
[0032] Here, the composition formula K, which is known to have a layered crystal structure, 0.8 Mg 0.4 Ti 1.6 O 4 In the Raman spectrum of conventional lepidocrocite-type magnesium potassium titanate, -1 Since a peak is observed around this point, this peak is thought to be a peak derived from the layered crystal structure.
[0033] In addition, the composition formula K is known to have a tunnel-shaped crystal structure. 2 Ti 6 O 13 In the Raman spectrum of potassium hexatitanate, -1 Nearby and 140 cm -1 Nearby and 860 cm -1 Since peaks are observed around , these peaks are thought to be peaks derived from the tunnel-shaped crystal structure of potassium hexatitanate.
[0034] The scanning transmission electron microscope (STEM) image of the magnesium potassium titanate of the present invention suggests that it has a tunnel crystal structure. In addition, the Raman spectrum of the magnesium potassium titanate of the present invention shows a peak at 835 cm that is thought to be derived from a layered crystal structure. -1 No peak was observed near 140 cm, which is thought to be a peak derived from a tunnel-shaped crystal structure. -1 Nearby and 860 cm -1Since peaks are observed around , it can be said that the spectrum is close to that of a tunnel-shaped crystal structure.
[0035] Therefore, it can be seen that the magnesium potassium titanate of the present invention, although it is magnesium potassium titanate, does not have a layered crystal structure but has a crystal structure close to a tunnel-shaped crystal structure (hereinafter referred to as a "pseudo-tunnel-shaped crystal structure"). From these viewpoints, it is clear that the magnesium potassium titanate of the present invention and conventional magnesium potassium titanate are different inorganic substances.
[0036] Since the magnesium potassium titanate of the present invention has a pseudo-tunnel-shaped crystal structure, it is believed that it can increase the friction coefficient when used as a friction modifier for friction materials.Furthermore, it is presumed that the magnesium potassium titanate of the present invention is in a distorted state compared to the tunnel-shaped structure of potassium hexatitanate.Therefore, when the magnesium potassium titanate of the present invention is used as a friction modifier for friction materials with a small amount of steel-based fibers, the crystals collapse under high load, and it is believed that it can chemically act on the metal of the mating material to increase the stability of the friction coefficient.
[0037] In the present invention, the Raman spectrum of magnesium potassium titanate is measured, for example, using a Raman spectrometer at an excitation wavelength of 785 nm and a wave number of 100 cm. -1 ~3200cm -1 The measurement can be performed under the conditions of 1000 s, 1 exposure time, and 10 scans. The peak area in each wavelength range can be calculated by, for example, removing the background of the Raman spectrum using the asymmetric least squares method (ASLS method) and then performing numerical integration using the Simpson method.
[0038] In the present invention, the ratio (Ia / Ib) in the Raman spectrum of magnesium potassium titanate is 0.03 or more, preferably 0.10 or more, more preferably 0.15 or more, and preferably 2.00 or less, more preferably 1.00 or less, and even more preferably 0.40 or less. By setting the ratio (Ia / Ib) in the above range, the coefficient of friction can be further increased.
[0039] In the present invention, the ratio (Ic / Ib) in the Raman spectrum of magnesium potassium titanate is 0.40 or less, preferably 0.35 or less, more preferably 0.26 or less, and preferably 0.20 or more, more preferably 0.22 or more. By setting the ratio (Ic / Ib) in the above range, the coefficient of friction can be further stabilized.
[0040] The composition formula of magnesium potassium titanate of the present invention is K x Mg 0.4 Ti 1.6 O 4-y [wherein x is 0.1≦x≦0.6, y=(0.8−x) / 2], and from the viewpoint of making it easier to form a pseudo-tunnel crystal structure, x is preferably 0.2 or more, more preferably 0.25 or more, and is preferably 0.5 or less, more preferably 0.35 or less.
[0041] From the viewpoint of further improving the stability of the friction coefficient, the magnesium potassium titanate of the present invention preferably contains 5.0% by mass or less of anatase titanium dioxide, more preferably 3.0% by mass or less, and even more preferably contains substantially no anatase titanium dioxide. In this specification, "substantially no anatase titanium dioxide" means that the content is less than 1.0% by mass, which is the detection limit of the XRD method described below. Of course, the content of anatase titanium dioxide may be 0% by mass.
[0042] The crystallite size of the magnesium potassium titanate of the present invention is preferably 20 Å to 200 Å, more preferably 30 Å to 150 Å, and even more preferably 35 Å to 100 Å. When the crystallite size of the magnesium potassium titanate is within the above range, the friction coefficient can be more efficiently stabilized at a high level. The crystallite size can be determined by the Halder-Wagner method using an X-ray diffractometer.
[0043] The magnesium potassium titanate of the present invention is preferably non-fibrous particles from the viewpoint of working environment. Examples of non-fibrous particles include spherical particles (including those with slight surface irregularities and those with a substantially spherical cross section, such as an elliptical cross section), columnar particles (including those with a substantially columnar overall shape, such as rod-shaped, cylindrical, prismatic, rectangular, rectangular, substantially cylindrical, or substantially rectangular), plate-shaped particles, block-shaped particles, particles with multiple protrusions (e.g., amoeba-shaped, boomerang-shaped, cross-shaped, or confetti-shaped), and irregular shapes. Among these, the magnesium potassium titanate is preferably plate-shaped particles. The magnesium potassium titanate may also be porous particles. These various particle shapes can be arbitrarily controlled by the production conditions, particularly the raw material composition and firing conditions. Furthermore, various particle shapes can be analyzed, for example, by scanning electron microscope (SEM) observation.
[0044] As used herein, "non-fibrous particles" refers to particles in which, when the longest side of the rectangular parallelepiped having the smallest volume among the rectangular parallelepipeds circumscribing the particle (circumscribing rectangular parallelepiped) is the major axis L, the next longest side is the minor axis B, and the shortest side is the thickness T (B > T), the ratio L / B is 5 or less. Furthermore, "having multiple convex portions" refers to particles whose projected shape on a plane is different from at least a normal polygon, circle, ellipse, etc., and can have a shape with convex portions in two or more directions. Specifically, these convex portions refer to the portions corresponding to the protruding parts when a polygon, circle, ellipse, etc. (basic shape) is fitted to a photograph (projection drawing) taken by a scanning electron microscope (SEM).
[0045] The average particle size of the magnesium potassium titanate of the present invention is preferably 0.1 μm to 100 μm, more preferably 1 μm to 50 μm, and even more preferably 3 μm to 30 μm. When the average particle size of magnesium potassium titanate is within the above range, the friction characteristics can be further improved when a friction material is produced. In this specification, the "average particle size" refers to the particle size at 50% cumulative volume in the particle size distribution measured by laser diffraction. This particle size D at 50% cumulative volume 50is the particle size at which the cumulative value reaches 50% when the particle size distribution is calculated on a volume basis and the number of particles is counted from the smallest particle size on a cumulative curve with the total volume set to 100%.
[0046] The specific surface area of the magnesium potassium titanate of the present invention is preferably 0.1 m 2 / g to 10m 2 / g, more preferably 0.3m 2 / g to 6m 2 / g, more preferably 0.4m 2 / g to 5m 2 When the specific surface area is within the above range, the friction characteristics of the produced friction material can be further improved. The specific surface area can be measured in accordance with JIS Z8830.
[0047] The alkali metal ion elution rate of the magnesium potassium titanate of the present invention is preferably 0.01 to 15% by mass, more preferably 0.05 to 6% by mass, and even more preferably 0.1 to 3% by mass.
[0048] In the curing reaction of novolac phenolic resin, an example of a thermosetting resin used in a friction material composition, the curing agent (or curing accelerator), for example, hexamethylenetetramine, undergoes ring-opening and bonds with hydroxyl groups in the novolac phenolic resin, initiating the curing reaction. However, if alkali metal ions are present during this process, they undergo an ion exchange reaction with the hydrogen ions in the hydroxyl groups in the novolac phenolic resin, which is thought to inhibit the bond between hexamethylenetetramine (the curing agent (or curing accelerator)) and the novolac phenolic resin (thermosetting resin) (curing inhibition). On the other hand, it is thought that the wear and tear of the friction material caused by braking causes alkali components derived from magnesium potassium titanate to leach out onto the friction surface.
[0049] Therefore, by setting the alkali metal ion elution rate to the above upper limit or less, it is possible to prevent inhibition of curing of the thermosetting resin during hot and pressure molding, and as a result, it is possible to further improve crack resistance under high temperature and high load. Furthermore, by setting the alkali metal ion elution rate to the above lower limit or more, it is possible to suppress rotor rusting even when a friction material using the magnesium potassium titanate of the present invention as a friction modifier is left unused for a long period of time after braking. In other words, by setting the alkali metal ion elution rate of magnesium potassium titanate within the above range, it is possible to achieve both higher levels of crack resistance of the friction material and higher levels of rotor rust suppression.
[0050] In this specification, the term "alkali metal ion elution rate" refers to the mass ratio of alkali metal ions eluted into water at 80°C from a measurement sample such as magnesium potassium titanate.
[0051] In the present invention, in order to further improve adhesion with the binder used in the friction material composition, a treatment layer made of a surface treatment agent may be formed on the surface of the magnesium potassium titanate. Examples of the surface treatment agent include a silane coupling agent and a titanium coupling agent. Among these, a silane coupling agent is preferably used, and an amino-based silane coupling agent, an epoxy-based silane coupling agent, or an alkyl-based silane coupling agent is more preferably used. The above surface treatment agents may be used alone or in combination of two or more.
[0052] Examples of amino-based silane coupling agents include N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-ethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, and N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane.
[0053] Examples of epoxy-based silane coupling agents include 3-glycidyloxypropyl(dimethoxy)methylsilane, 3-glycidyloxypropyltrimethoxysilane, diethoxy(3-glycidyloxypropyl)methylsilane, triethoxy(3-glycidyloxypropyl)silane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.
[0054] Examples of alkyl silane coupling agents include methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, isobutyltrimethoxysilane, isobutyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, cyclohexylmethyldimethoxysilane, n-octyltriethoxysilane, and n-decyltrimethoxysilane.
[0055] A known surface treatment method can be used to form a treatment layer made of a surface treatment agent on the surface of magnesium potassium titanate. For example, a wet method can be used in which the surface treatment agent is dissolved in a solvent that promotes hydrolysis (e.g., water, alcohol, or a mixed solvent thereof) to form a solution, and the solution is sprayed onto magnesium potassium titanate.
[0056] The amount of the surface treatment agent used to treat the surface of the magnesium potassium titanate is not particularly limited. In the case of a wet method, for example, a solution of the surface treatment agent may be sprayed so that the amount of the surface treatment agent is 0.1 to 20 parts by mass per 100 parts by mass of magnesium potassium titanate.
[0057] The magnesium potassium titanate of the present invention may be granulated by treating the magnesium potassium titanate with the surface treatment agent or a binder described below. The average particle size of the granular magnesium potassium titanate is preferably 100 μm to 200 μm.
[0058] (Method for Producing Magnesium Potassium Titanate) The method for producing magnesium potassium titanate of the present invention is not particularly limited, but it can be produced, for example, by the following method.
[0059] First, raw material magnesium potassium titanate (hereinafter sometimes referred to as "raw material KTMO") is prepared. Next, the raw material KTMO is mixed with an acid (acid treatment), and the compound obtained by the acid treatment is calcined, thereby producing the material.
[0060] The raw material KTMO is K 0.8 Mg 0.4 Ti 1.6 O 4 , K. 0.7 Mg 0.4 Ti 1.6 O 3.95 It is preferable to use magnesium potassium titanate having a layered crystal structure such as the above. By forming a pseudo-tunnel crystal structure using a layered crystal structure as a raw material, excellent friction characteristics can be obtained. This also makes it possible to suppress the generation of WHO fibers.
[0061] The raw material KTMO can be obtained, for example, by calcining a mixture of titanium dioxide or a compound that generates titanium dioxide when heated (these are collectively referred to as "titanium compounds"), potassium oxide or a compound that generates potassium oxide when heated (these are collectively referred to as "potassium compounds"), and magnesium oxide or a compound that generates magnesium oxide when heated (these are collectively referred to as "magnesium compounds").
[0062] In conventional methods for producing magnesium potassium titanate, crystals are formed at temperatures lower than the melting point, and as the crystals grow, they take on an idiomorphic shape surrounded by flat crystal faces that reflect the crystal structure, making it easier to specify the crystal orientation. Potassium chloride, potassium fluoride, potassium molybdate, potassium tungstate, etc. are used as fluxes.
[0063] In the production of the raw material KTMO used in the present invention, suppressing crystal growth of the raw material KTMO facilitates the formation of a pseudo-tunnel-shaped crystal structure in a subsequent process. From this perspective, the amount of flux used is preferably less than 10 parts by mass, more preferably 0 parts by mass, per 100 parts by mass of the total amount of titanium compound, potassium compound, and magnesium compound. Furthermore, from the perspective of eluting potassium from between the crystal layers of the raw material KTMO, which has a layered crystal structure, and facilitating the formation of the desired composition and pseudo-tunnel-shaped crystal structure, it is preferable to control the amount of chloride ions on the particle surface or within the crystals of the raw material KTMO to a certain level or less. Specifically, the chloride ion elution rate of the raw material KTMO is preferably 400 ppm or less, more preferably 200 ppm or less.
[0064] In this specification, the term "chlorine ion elution rate" refers to the mass ratio of chloride ions eluted into water at 25°C from a measurement sample such as a titanate or titanium compound.
[0065] Examples of titanium compounds that can be used include low-order titanium dioxide, titanium dioxide hydrate, titanium dioxide hydrate, and titanium hydroxide. Of these, titanium dioxide is preferred as the titanium compound. The crystalline system of titanium dioxide is preferably rutile or anatase. One titanium compound may be used alone, or two or more titanium compounds may be used in combination. From the viewpoint of further reducing the chloride ion elution rate of the raw material KTMO, the chloride ion elution rate of the titanium compound is preferably 100 ppm or less, and more preferably 50 ppm or less.
[0066] Examples of potassium compounds include potassium oxide, potassium carbonate, potassium hydroxide, and potassium nitrate. Of these, potassium carbonate or potassium hydroxide is preferred. One potassium compound may be used alone, or two or more potassium compounds may be used in combination.
[0067] Examples of magnesium compounds include magnesium oxide, magnesium hydroxide, magnesium carbonate, and magnesium fluoride. Among these, magnesium hydroxide is preferred. The magnesium compounds may be used alone or in combination of two or more.
[0068] The mixing ratio of the titanium compound, potassium compound, and magnesium compound can be appropriately adjusted depending on the composition formula of the target raw material KTMO. 0.8 Mg 0.4 Ti 1.6 O 4 In the case of producing the above, the molar ratio of Ti:K:Mg may be set to 1.6:0.8:0.4.
[0069] The calcination during the production of raw material KTMO can be carried out using an electric furnace or the like. The calcination reaction during the production of raw material KTMO can be completed by maintaining the material at a temperature in the range of 800°C to 1100°C for 1 to 24 hours. After calcination, the resulting powder can be crushed to a desired size or sieved to loosen the particles.
[0070] The acid used in the acid treatment is not particularly limited, and known acids can be used. Examples of the acid used in the acid treatment include inorganic acids such as sulfuric acid, hydrochloric acid, and nitric acid, and organic acids such as acetic acid. Two or more acids may be used in combination as needed.
[0071] The acid treatment can be carried out by mixing an acid with an aqueous slurry of the raw KTMO. The concentration of the aqueous slurry is not particularly limited and can be appropriately selected from a wide range. Considering workability, the concentration of the aqueous slurry may be approximately 1% by mass to 30% by mass. Furthermore, since the acid treatment results in a crystalline state in which some potassium is missing, and the resulting product is then fired to form a pseudo-tunnel crystal structure, the amount of acid mixed with the aqueous slurry is preferably 0.10 equivalents to 0.40 equivalents, and more preferably 0.20 equivalents to 0.30 equivalents, relative to the interlayer elements of the raw KTMO. After the acid treatment, the solid content is separated from the aqueous slurry by filtration, centrifugation, or the like. The separated solid content can be washed with water and dried, as necessary.
[0072] The firing can be carried out using an electric furnace or the like. From the viewpoint of forming a pseudo-tunnel-shaped crystal structure while suppressing crystal transition to anatase titanium dioxide or other crystal structures, the firing temperature is preferably in the range of 350°C to 600°C, more preferably 400°C to 550°C, and the temperature is preferably maintained within this range for 0.5 hours to 12 hours, more preferably 0.5 hours to 10 hours, and even more preferably 0.5 hours to 5 hours. After firing, the resulting powder may be pulverized to a desired size or sieved to loosen it. In this manner, the magnesium potassium titanate of the present invention can be obtained.
[0073] In the method for producing magnesium potassium titanate of the present invention, the ratios (Ia / Ib) and (Ic / Ib) of the resulting magnesium potassium titanate can be adjusted to the desired ranges by reducing the amount of flux used in producing the starting KTMO, by lowering the chloride ion elution rate from the starting KTMO, or by applying thermal energy during firing to unstable crystals of the starting KTMO in which some of the potassium has been lost.
[0074] <2. Friction Material Composition> The friction material composition of the present invention contains the magnesium potassium titanate of the present invention and a binder, and is characterized in that the copper content is less than 0.5 mass% in terms of copper element, relative to 100 mass% of the total amount of the friction material composition. In the above friction material composition, the magnesium potassium titanate of the present invention can be used as a friction modifier. Furthermore, the friction material composition of the present invention can further contain steel fibers and other materials, as necessary. In this specification, the term "friction material composition" refers to a composition used in a friction material.
[0075] The friction material composition of the present invention contains the magnesium potassium titanate of the present invention as a friction modifier, and therefore the friction coefficient of the friction material in the high load range can be increased.
[0076] Furthermore, by containing less than 0.5 mass % of copper element relative to 100 mass % of the total amount of the friction material composition, or preferably by not containing any copper element, the environmental impact can be reduced compared to conventional friction material compositions. In this specification, "not containing any copper element" means that copper fiber, copper powder, and copper-containing alloys (brass, bronze, etc.) and compounds are not blended as raw materials of the friction material composition.
[0077] According to the friction material composition of the present invention, excellent friction characteristics can be obtained even when no copper component is contained or when the copper component content is reduced.
[0078] (2-1. Binder) The binder integrates the compounding materials contained in the friction material composition and provides strength. There are no particular restrictions on the binder used in the friction material composition of the present invention, and thermosetting resins that are usually used as binders for friction materials can be used.
[0079] Examples of thermosetting resins include phenolic resins; elastomer-dispersed phenolic resins such as acrylic elastomer-dispersed phenolic resins and silicone elastomer-dispersed phenolic resins; modified phenolic resins such as acrylic-modified phenolic resins, silicone-modified phenolic resins, cashew-modified phenolic resins, epoxy-modified phenolic resins, and alkylbenzene-modified phenolic resins; formaldehyde resins; melamine resins; epoxy resins; acrylic resins; aromatic polyester resins; and urea resins. One of these may be used alone, or two or more may be used in combination. Among these, phenolic resins (straight phenolic resins) or modified phenolic resins are preferred as thermosetting resins from the viewpoint of further improving heat resistance, moldability, and friction properties. While both resol-type and novolac-type phenolic resins can be used as phenolic resins, novolac-type phenolic resins are preferred from the viewpoint of production stability and cost. Furthermore, novolac-type phenolic resins may contain additives such as curing agents and curing accelerators (e.g., hexamethylenetetramine) as needed.
[0080] The content of the binder in the friction material composition is preferably 5% by mass to 30% by mass, and more preferably 8% by mass to 20% by mass, based on 100% by mass of the total amount of the friction material composition. By setting the binder content within this range, an appropriate amount of binder is filled into the gaps in the blended materials, resulting in even better friction characteristics.
[0081] (2-2. Magnesium potassium titanate) The magnesium potassium titanate used in the friction material composition of the present invention is the magnesium potassium titanate of the present invention described above. By including the magnesium potassium titanate of the present invention, the friction coefficient of the resulting friction material in the high load range can be increased. In addition, it is expected that the amount of fine wear dust such as PM (particulate matter) 10 and PM 2.5 generated during braking will be reduced.
[0082] The content of the magnesium potassium titanate in the friction material composition is preferably 1% by mass to 40% by mass, more preferably 5% by mass to 35% by mass, and even more preferably 10% by mass to 30% by mass, based on 100% by mass of the total amount of the friction material composition. By setting the content of the magnesium potassium titanate within the above range, even more excellent friction characteristics can be obtained. Furthermore, when the magnesium potassium titanate is used in combination with other titanates described below, the content of the magnesium potassium titanate is preferably 5% by mass to 20% by mass, based on 100% by mass of the total amount of the friction material composition.
[0083] The mass ratio of the magnesium potassium titanate to the binder (magnesium potassium titanate / binder) is preferably 0.1 to 8.0, more preferably 0.5 to 6.0, and even more preferably 1.1 to 4.0. By setting the mass ratio of the magnesium potassium titanate to the binder within the above range, the formability of the friction material can be further improved, and an appropriate transfer film can be formed.
[0084] (2-3. Steel Fibers) In addition to the binder and the magnesium potassium titanate of the present invention, the friction material composition of the present invention may contain steel fibers, which are typically used in friction material compositions, as needed. Examples of steel fibers include steel fibers and stainless steel fibers, with steel fibers being preferred.
[0085] Examples of steel fibers include straight fibers obtained by chatter vibration cutting and curled fibers obtained by cutting long fibers. Straight fibers have a linear fiber shape. Curled fibers, on the other hand, have a shape with curved portions, and include simple arc-shaped fibers, wavy fibers, spiral or vortex-shaped fibers, etc.
[0086] Among these, the steel fibers are preferably curled fibers, from the viewpoint of reducing the amount of shedding from the friction material on the friction surface and more reliably maintaining the friction characteristics during high-temperature braking. Furthermore, it is more preferable that the curled fibers include a portion with a radius of curvature of 100 μm or less. In this case, the fibers are more firmly fixed to the friction material, and the shedding of the friction material from the friction surface is further reduced.
[0087] The average fiber length of the steel-based fibers is preferably 5 mm or less, more preferably 2.5 mm or less, from the viewpoint of further improving abrasion resistance at high temperatures, and is preferably 0.1 mm or more, more preferably 0.5 mm or more, and even more preferably 1.1 mm or more, from the viewpoint of further improving reinforcing properties.
[0088] The average fiber diameter of the steel-based fibers is preferably 300 μm or less, more preferably 100 μm or less, from the viewpoint of further suppressing brake vibration at high temperatures, and is preferably 10 μm or more, more preferably 30 μm or more, from the viewpoint of further preventing the steel-based fibers from falling off.
[0089] The average fiber length and average fiber diameter of the steel-based fibers can be confirmed using a microscope, etc. For example, they can be the average values of 30 steel-based fibers observed under a microscope.
[0090] When the NAO material contains less than 10% by mass (preferably 0% by mass) of steel fibers relative to 100% by mass of the total amount of the friction material composition, the friction coefficient in the high load range can be increased, and the stability of the friction coefficient can also be further improved.
[0091] In the case of a low-steel material in which the content of steel fibers is 10% by mass or more and 30% by mass or less (preferably 13% by mass to 23% by mass) relative to 100% by mass of the total amount of the friction material composition, the friction coefficient can be increased in the high load range.
[0092] When steel fibers are blended into the friction material composition of the present invention, the mass ratio of the magnesium potassium titanate to the steel fibers (magnesium potassium titanate / steel fibers) is preferably 0.1 to 3.0, more preferably 0.6 to 2.5, even more preferably 0.7 to 1.5, and particularly preferably 0.8 to 1.2. By setting the mass ratio of the magnesium potassium titanate to the steel fibers within the above range, detachment of the steel fibers can be further suppressed.
[0093] (2-4. Other Materials) In addition to the binder and the friction modifier of the present invention, other materials typically used in friction material compositions (such as a fibrous base material, an organic friction modifier, an inorganic friction modifier, a lubricant, a pH adjuster, and a filler) may be blended into the friction material composition of the present invention, as needed.
[0094] The content of the other materials in the friction material composition is preferably 20% by mass to 94% by mass relative to 100% by mass of the total amount of the friction material composition.
[0095] (2-4-1. Fibrous base material) The fibrous base material exhibits reinforcing properties in the friction material. Examples of the fibrous base material include inorganic fibers, metal fibers, organic fibers, and carbon-based fibers. As the fibrous base material, one of these may be used alone, or two or more may be used in combination.
[0096] When the friction material composition contains a fibrous base material other than steel fibers, the content thereof is preferably 0.1 to 40% by mass, more preferably 0.1 to 20% by mass, and even more preferably 0.1 to 10% by mass, relative to 100% by mass of the total amount of the friction material composition.
[0097] Examples of inorganic fibers include glass fibers, rock wool, ceramic fibers, biodegradable ceramic fibers, biodegradable mineral fibers, and biosoluble fibers (SiO 2 Examples of the fiber include rock wool, CaO--SrO-based fibers, wollastonite fibers, silicate fibers, and mineral fibers, and among these, rock wool is preferred.
[0098] When the friction material composition contains rock wool, the content thereof is preferably 1 to 10 mass %, more preferably 1 to 7 mass %, relative to 100 mass % of the total amount of the friction material composition. When the rock wool content is within the above range, the coefficient of friction during high-load braking can be increased.
[0099] Examples of metal fibers include straight or curled metal fibers whose main component is a metal such as aluminum, iron, zinc, tin, titanium, nickel, magnesium, silicon, or other metals or alloy fibers (excluding steel-based fibers).
[0100] Examples of organic fibers include aromatic polyamide (aramid) fibers, fibrillated aramid fibers (also called aramid pulp), acrylic fibers (fibers of homopolymers or copolymers whose main raw material is acrylonitrile), fibrillated acrylic fibers, cellulose fibers, fibrillated cellulose fibers, and phenolic resin fibers.
[0101] The organic fibers are preferably aramid fibers or fibrillated aramid fibers, since they provide the friction material with appropriate water absorption, facilitate absorption of atmospheric moisture into the friction material, facilitate elution of the alkali component of the titanate, and are expected to provide rust prevention effects for the rotor and steel fibers. From the viewpoint of further enhancing heat resistance, the organic fibers are preferably para-aramid fibers, typified by poly-p-phenylene terephthalamide. Furthermore, from the viewpoint of further improving the moldability of the friction material and further improving the retention of fillers, the organic fibers are preferably fibrillated aramid fibers. The specific surface area of the fibrillated aramid fibers is preferably 5 m 2 / g~25m 2 / g, more preferably 5m 2 / g~15m 2 The fiber length of the fibrillated aramid fibers is preferably 0.5 mm to 1.2 mm.
[0102] When the friction material composition contains fibrillated aramid fibers, the content thereof is preferably 1 to 10% by mass, more preferably 1 to 8% by mass, and even more preferably 1 to 6% by mass, relative to 100% by mass of the total amount of the friction material composition. When the content of the fibrillated aramid fibers is equal to or greater than the above-mentioned lower limit, crack resistance and wear resistance are improved. On the other hand, when the content of the fibrillated aramid fibers is equal to or less than the above-mentioned upper limit, deterioration of crack resistance and wear resistance due to uneven distribution of the fibrillated aramid fibers and other materials can be more reliably prevented.
[0103] Examples of carbon-based fibers include flame-resistant fibers, PAN-based carbon fibers, pitch-based carbon fibers, and activated carbon fibers.
[0104] (2-4-2. Organic Friction Modifiers) Organic friction modifiers are friction modifiers that are blended with the aim of further improving the noise and vibration performance and wear resistance of friction materials. Examples of organic friction modifiers include unvulcanized or vulcanized rubber powders such as tire rubber, acrylic rubber, isoprene rubber, NBR (nitrile butadiene rubber), SBR (styrene butadiene rubber), chlorinated butyl rubber, butyl rubber, and silicone rubber; cashew dust; rubber-coated cashew dust; melamine dust; and the like. One of these may be used alone, or two or more may be used in combination.
[0105] When the friction material composition contains an organic friction modifier, the content thereof is preferably 0.1 to 30% by mass, more preferably 0.1 to 20% by mass, and even more preferably 0.1 to 10% by mass, relative to 100% by mass of the total amount of the friction material composition.
[0106] (2-4-3. Inorganic Friction Modifiers) Inorganic friction modifiers (excluding magnesium potassium titanate of the present invention) are friction modifiers that are blended with the aim of preventing deterioration in the heat resistance of the friction material, improving the wear resistance, or further improving the coefficient of friction. Examples of inorganic friction modifiers include abrasives, metal powders, and other inorganic fillers.
[0107] The abrasive can be selected appropriately based on the material of the rotor, which is the mating material, so that it acts as an abrasive and improves the coefficient of friction, and can be selected based on the Mohs hardness of the mating material. From the viewpoint of more effectively exhibiting the coefficient of friction due to the abrasive, the Mohs hardness of the abrasive is preferably 6 to 9, more preferably 6 to 8.
[0108] Examples of abrasives include silicon carbide (silicon carbide), titanium dioxide, α-alumina, γ-alumina, silica (silicon dioxide), magnesia (magnesium oxide), zirconia (zirconium oxide), zircon (zirconium silicate), chromium oxide, iron oxide (iron trioxide, etc.), chromite, quartz, and iron sulfide. Among these, the abrasive is preferably zirconia (zirconium oxide) or zircon (zirconium silicate). The average particle size of zirconia (zirconium oxide) is preferably 1 μm to 14 μm. The average particle size of zircon (zirconium silicate) is preferably 0.2 μm to 2 μm.
[0109] Furthermore, abrasives having a large average particle size and abrasives having a small average particle size may be used in combination. Specifically, abrasives having an average particle size of 0.5 μm to 15 μm may be used in combination with abrasives having an average particle size of 20 μm to 200 μm. Furthermore, the mass ratio of the abrasives having a small average particle size to the abrasives having a large average particle size (abrasives having a small average particle size / abrasives having a large average particle size) is preferably 0.1 to 10, more preferably 2 to 8, from the viewpoint of further reducing wear dust. In this case, the coefficient of friction can be increased during heavy-load braking, while the stability of the coefficient of friction during light-load braking can be improved.
[0110] When the friction material composition contains an abrasive, the content thereof is preferably 0.1 to 30% by mass, more preferably 5 to 25% by mass, and even more preferably 5 to 18% by mass, relative to 100% by mass of the total amount of the friction material composition.
[0111] Examples of the metal powder include powders of simple metals or alloys of aluminum, zinc, iron, tin, etc. One of these may be used alone, or two or more may be used in combination.
[0112] Other inorganic fillers include vermiculite, clay, mica, talc, dolomite, chromite, mullite, calcium silicate, titanates other than the magnesium potassium titanate of the present invention (hereinafter referred to as "other titanates"), etc. One of these may be used alone, or two or more may be used in combination.
[0113] Other titanates include potassium hexatitanates such as TERRACESS JSL, TERRACESS JSL-R, TERRACESS DP-R, TERRACESS DP-A, and TERRACESS DP-AS manufactured by Otsuka Chemical Co., Ltd., TXAX-MA and TXAX-A manufactured by Kubota Corporation, and TOFIX-S and TOFIX-SNR manufactured by Toho Titanium Co., Ltd.; sodium hexatitanates such as TERRACESS DSR manufactured by Otsuka Chemical Co., Ltd.; potassium octatitanates such as TERRACESS TF-SS, TERRACESS TF-S, TERRACESS TF-L, and TERRACESS JP manufactured by Otsuka Chemical Co., Ltd.; and TERRACESS PM and TERRACESS Examples of the other titanates that can be used include magnesium potassium titanate such as TERRACESS L, TERRACESS L-SS, and TERRACESS JSM-M manufactured by Otsuka Chemical Co., Ltd. As the other titanate, preferred are sodium hexatitanate and potassium octatitanate having a tunnel-shaped crystal structure; magnesium potassium titanate and lithium potassium titanate having a layered crystal structure, and more preferred is magnesium potassium titanate having a layered crystal structure. As the other titanate, the titanate having a tunnel-shaped crystal structure and the titanate having a layered crystal structure may be used alone, or a titanate having a tunnel-shaped crystal structure and a titanate having a layered crystal structure may be used in combination.
[0114] When the friction material composition contains the other titanate, the mass ratio of the other titanate to the magnesium potassium titanate of the present invention (other titanate / magnesium potassium titanate of the present invention) is preferably 0.1 to 3, more preferably 0.1 to 0.8, from the viewpoint of increasing the friction coefficient in the high load region when used in a friction material.
[0115] (2-4-4. Lubricant) The lubricant is preferably a solid lubricant, and examples thereof include carbon-based solid lubricants, sulfide-based solid lubricants, polytetrafluoroethylene (PTFE), etc., and one of these may be used alone or two or more may be used in combination. The lubricant is preferably one or more selected from the group consisting of carbon-based solid lubricants and sulfide-based solid lubricants, and from the viewpoint of further reducing harmfulness to the human body, a carbon-based solid lubricant is more preferred.
[0116] When the friction material composition contains a lubricant, the content thereof is preferably 0.1 to 20% by mass, more preferably 1 to 10% by mass, and even more preferably 1 to 5% by mass, relative to 100% by mass of the total amount of the friction material composition.
[0117] Examples of the carbon-based solid lubricant include synthetic or natural graphite (graphite), flake graphite, phosphate-coated graphite, carbon black, petroleum coke, coal coke, activated carbon, and elastic graphitized carbon. Synthetic graphite or natural graphite is preferred from the viewpoint of more reliably imparting thermal conductivity. When a carbon-based solid lubricant is contained, its content is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more, relative to 100% by mass of the total amount of the friction material composition. It is preferably less than 15% by mass, more preferably less than 10% by mass, and even more preferably 8% by mass or less. When the content of the carbon-based solid lubricant is equal to or greater than the lower limit, friction material wear at high temperatures tends to be further improved. Furthermore, when the content of the carbon-based solid lubricant is less than or equal to the upper limit, a decrease in the friction coefficient tends to be easily suppressed.
[0118] The average particle size of the carbon-based solid lubricant is not particularly limited, but is preferably 10 μm to 1000 μm. One type of carbon-based solid lubricant may be used alone, or two or more types having different average particle sizes may be used in combination. If the average particle size of the carbon-based solid lubricant is equal to or greater than the above-mentioned lower limit, the thermal conductivity of the resulting frictional material is prevented from increasing excessively, and the transfer of frictional heat to the back plate tends to be suppressed, which can lead to vapor lock. Furthermore, if the average particle size of the carbon-based solid lubricant is equal to or less than the above-mentioned upper limit, the thermal conductivity is improved, which promotes hardening of the binder during frictional material molding, and the strength of the frictional material tends to be improved.
[0119] Examples of the sulfide-based solid lubricant include antimony trisulfide, molybdenum disulfide, tin sulfide, iron sulfide, zinc sulfide, bismuth sulfide, and tungsten disulfide. From the viewpoint of further reducing harmfulness to the human body, the sulfide-based solid lubricant is preferably tin sulfide or molybdenum disulfide. When a sulfide-based solid lubricant is contained, its content is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more, relative to 100% by mass of the total amount of the friction material composition. It is preferably less than 15% by mass, more preferably less than 10% by mass, and even more preferably 8% by mass or less. When the content of the sulfide-based solid lubricant is equal to or greater than the above-mentioned lower limit, rotor wear tends to be further suppressed. Furthermore, when the content of the sulfide-based solid lubricant is less than the above-mentioned upper limit or equal to or less than the above-mentioned upper limit, a decrease in the friction coefficient tends to be easily suppressed.
[0120] The friction material composition of the present invention preferably contains substantially no sulfide-based solid lubricants, such as metal sulfides. "Substantially no sulfide-based solid lubricants" means that no sulfide-based solid lubricants are intentionally blended into the friction material composition, and refers to the absence of sulfide-based solid lubricants in the friction material composition, except in cases where a sulfide-based solid lubricant is mixed into the friction material composition as a trace amount of impurity. In particular, the content of sulfide-based solid lubricants is preferably less than 0.1% by mass relative to 100% by mass of the total amount of the friction material composition, and it is more preferable that the friction material composition does not contain any sulfide-based solid lubricants at all. Substantially no sulfide-based solid lubricants are present, which is expected to be less harmful to humans and to inhibit rotor rusting.
[0121] The friction material composition of the present invention preferably contains the magnesium potassium titanate of the present invention, steel fibers, a carbon-based solid lubricant, and a binder, and the copper content is less than 0.5 mass% in terms of copper element relative to 100 mass% of the total amount of the friction material composition, and the friction material composition is substantially free of a sulfide-based solid lubricant.
[0122] In the friction material composition of the present invention containing magnesium potassium titanate, steel-based fibers, a carbon-based solid lubricant, and a binder, the content of the sulfide-based solid lubricant is preferably less than 0.1% by mass, based on 100% by mass of the total friction material composition. It is even more preferable that the friction material composition does not contain any sulfide-based solid lubricant. The content of the steel-based fibers is preferably 10% to 30% by mass, more preferably 13% to 23% by mass, based on 100% by mass of the total friction material composition. Furthermore, the mass ratio of the magnesium potassium titanate of the present invention to the carbon-based solid lubricant (magnesium potassium titanate of the present invention / carbon-based solid lubricant) is preferably 2.0 to 6.0, more preferably 3.5 to 5.5, and even more preferably 3.5 to 5.0. By setting the content of each component within the above ranges, a friction material containing steel-based fibers can be formed that has a composition that is less harmful to the environment and human body, yet has a higher friction coefficient in the high-load range, and generates less fine wear dust such as PM10 and PM2.5 during braking.
[0123] (2-4-5. pH Adjuster) Examples of pH adjusters include inorganic bases such as calcium hydroxide (slaked lime), sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, trisodium phosphate, disodium hydrogen phosphate, tripotassium phosphate, and dipotassium hydrogen phosphate, and organic bases such as imidazole, histidine, and hexamethylenediamine. From the viewpoints of cost and hygroscopicity, the pH adjuster is preferably an inorganic base. One of these may be used alone, or two or more may be used in combination. The pH adjuster may also be used to prevent rust adhesion between the friction material and the mating material (rotor).
[0124] When the friction material composition contains a pH adjuster, the content thereof is preferably 0.1 to 8% by mass relative to 100% by mass of the total amount of the friction material composition.
[0125] (2-4-6. Filler) Examples of the filler include barium sulfate and calcium carbonate. Preferably, barium sulfate can be used as the filler. One of these may be used alone, or two or more may be used in combination.
[0126] Barium sulfate comes in two forms: elutriated barium sulfate (baryte powder), which is obtained by crushing a mineral called barite, washing it to remove iron, and elutriating it, and artificially synthesized precipitated barium sulfate. The particle size of precipitated barium sulfate can be controlled by the synthesis conditions, allowing for the production of fine barium sulfate with a low content of the desired coarse particles. It is preferable to use precipitated barium sulfate in order to further reduce impurities and achieve a more uniform particle size distribution of the barium sulfate particles.
[0127] (2-5. Method for Producing Friction Material Composition) The friction material composition of the present invention can be produced by (1) a method of mixing the components using a mixer such as a Loedige mixer ("Loedige" is a registered trademark), a pressure kneader, or an Eirich mixer ("Eirich" is a registered trademark); or (2) a method of preparing granules of the desired components and, if necessary, mixing other components using a mixer such as a Loedige mixer, a pressure kneader, or an Eirich mixer.
[0128] The content of each component in the friction material composition of the present invention can be appropriately selected depending on the desired friction characteristics, and the composition can be produced by the above-mentioned production method.
[0129] The friction material composition of the present invention may also be prepared by preparing a masterbatch containing a specific component at a high concentration, and then adding and mixing a thermosetting resin or the like to this masterbatch.
[0130] <3. Friction Material and Friction Member> In the present invention, the friction material composition is pre-molded at room temperature (20°C), and the resulting pre-molded body is subjected to heat and pressure molding (molding pressure of 10 MPa to 40 MPa, molding temperature of 150°C to 200°C). If necessary, the resulting molded body is subjected to heat treatment in a heating furnace (150°C to 220°C, held for 1 hour to 12 hours), and then the molded body is subjected to machining and polishing, thereby producing a friction material having a predetermined shape.
[0131] The friction material of the present invention is used as a friction member formed from the friction material to form a friction surface. Examples of friction members that can be formed using the friction material include (1) a structure consisting of only the friction material, and (2) a structure having a substrate such as a backing metal and the friction material of the present invention provided on the substrate to provide a friction surface.
[0132] The substrate is used to further improve the mechanical strength of the friction member, and examples of the material for the substrate include metals such as iron and stainless steel, and fiber-reinforced resins such as glass fiber-reinforced resins and carbon fiber-reinforced resins.
[0133] Friction materials usually have many fine pores formed inside, which act as escape routes for decomposition products (gases and liquids) at high temperatures, preventing a decrease in friction characteristics, and also preventing squealing by reducing the rigidity of the friction material and improving damping. In ordinary friction materials, the material blend and molding conditions are controlled so that the porosity is preferably 5% to 30%, and more preferably 10% to 25%.
[0134] The friction member of the present invention is made of the friction material composition of the present invention, and therefore can obtain excellent friction characteristics even when it does not contain a copper component or when the copper component content is reduced. Therefore, the friction member of the present invention can be suitably used in brake systems in general, such as disc pads, brake linings, and clutch facings that constitute braking devices for various vehicles and industrial machines, and can be suitably used particularly as a friction member for regenerative cooperative brakes.
[0135] The present invention will now be described in further detail with reference to specific examples.
[0136] The present invention is not limited to the following examples, and can be practiced with appropriate modifications within the scope of the present invention.
[0137] <Production of Titanate> (Comparative Example 1: Titanate A) 496.9 g of anatase titanium dioxide (chloride ion elution rate: 20 ppm), 213.7 g of potassium carbonate, and 89.4 g of magnesium hydroxide were mixed by a conventional method to obtain a raw material mixture. The raw material mixture was loaded into a vibration mill and milled for 30 minutes under conditions of a vibration frequency of 1200 cpm and an amplitude of 6.0 mm to obtain a milled mixture. 48 ml of water was added to the milled mixture and mixed, and 15 g of the milled mixture was formed into pellets at a pressure of 10 MPa using a hydraulic press. The pellets were fired in an electric furnace at 1000°C for 4 hours, then slowly cooled. The resulting fired product was pulverized and passed through a 20-mesh sieve to obtain the target titanate A.
[0138] Table 1 shows the chemical composition, crystal structure, crystallite size, average particle size, specific surface area, particle shape, alkali metal ion elution rate, and chloride ion elution rate of the obtained titanate A.
[0139] (Comparative Example 2: Titanate B) A 20 mass% aqueous slurry of titanate A produced in Comparative Example 1 was prepared, and 0.27 equivalents of sulfuric acid relative to the potassium in the magnesium potassium titanate was mixed with this aqueous slurry and stirred for 2 hours at room temperature (20° C.). This aqueous slurry was suction filtered and washed with deionized water to separate a cake (solid content). This cake was dried at 110° C. for 12 hours, baked at 300° C. for 1 hour in an electric furnace, and then slowly cooled. The baked product was passed through a 20-mesh sieve to obtain the target titanate B.
[0140] Table 1 shows the chemical composition, crystal structure, crystallite size, average particle size, specific surface area, particle shape, alkali metal ion elution rate, and chloride ion elution rate of the obtained titanate B.
[0141] (Example 1: Titanate 1) A 20 mass% aqueous slurry of titanate A produced in Comparative Example 1 was prepared, and 0.27 equivalents of sulfuric acid relative to the potassium in the magnesium potassium titanate was mixed with this aqueous slurry and stirred for 2 hours at room temperature (20° C.). This aqueous slurry was suction filtered and washed with deionized water to separate the cake (solid content). This cake was dried at 110° C. for 12 hours, calcined at 500° C. for 1 hour in an electric furnace, and then slowly cooled. The calcined product was passed through a 20-mesh sieve to obtain the target titanate 1.
[0142] Table 1 shows the chemical composition, crystal structure, crystallite size, average particle size, specific surface area, particle shape, alkali metal ion elution rate, and chloride ion elution rate of the obtained titanate 1.
[0143] (Example 2: Titanate 2) A 20 mass% aqueous slurry of titanate A produced in Comparative Example 1 was prepared, and 0.27 equivalents of sulfuric acid relative to the potassium in the magnesium potassium titanate was mixed with this aqueous slurry and stirred for 2 hours at room temperature (20° C.). This aqueous slurry was suction filtered and washed with deionized water to separate the cake (solid content). This cake was dried at 110° C. for 12 hours, calcined at 500° C. for 12 hours in an electric furnace, and then slowly cooled. The calcined product was passed through a 20-mesh sieve to obtain the target titanate 2.
[0144] The chemical composition, crystal structure, crystallite size, average particle size, specific surface area, particle shape, alkali metal ion elution rate, and chloride ion elution rate of the obtained titanate 2 are shown in Table 1.
[0145] (Example 3: Titanate 3) A 20 mass% aqueous slurry of titanate A produced in Comparative Example 1 was prepared, and 0.34 equivalents of sulfuric acid relative to the potassium in the magnesium potassium titanate was mixed with this aqueous slurry and stirred for 2 hours at room temperature (20° C.). This aqueous slurry was suction filtered and washed with deionized water to separate the cake (solid content). This cake was dried at 110° C. for 12 hours, calcined at 500° C. for 1 hour in an electric furnace, and then slowly cooled. The calcined product was passed through a 20-mesh sieve to obtain the target titanate 3.
[0146] Table 1 shows the chemical composition, crystal structure, crystallite size, average particle size, specific surface area, particle shape, alkali metal ion elution rate, and chloride ion elution rate of the obtained titanate 3.
[0147] (Example 4: Titanate 4) A 20 mass% aqueous slurry of titanate A produced in Comparative Example 1 was prepared, and 0.27 equivalents of sulfuric acid relative to the potassium in the magnesium potassium titanate was mixed with this aqueous slurry and stirred for 2 hours at room temperature (20° C.). This aqueous slurry was suction filtered and washed with deionized water to separate the cake (solid content). This cake was dried at 110° C. for 12 hours, calcined at 600° C. for 1 hour in an electric furnace, and then slowly cooled. The calcined product was passed through a 20-mesh sieve to obtain the target titanate 4.
[0148] Table 1 shows the chemical composition, crystal structure, crystallite size, average particle size, specific surface area, particle shape, alkali metal ion elution rate, and chloride ion elution rate of the obtained titanate 4.
[0149] (Example 5: Titanate 5) A 20 mass% aqueous slurry of titanate A produced in Comparative Example 1 was prepared, and 0.22 equivalents of sulfuric acid relative to the potassium in the magnesium potassium titanate was mixed with this aqueous slurry and stirred for 2 hours at room temperature (20° C.). This aqueous slurry was suction filtered and washed with deionized water to separate the cake (solid content). This cake was dried at 110° C. for 12 hours, calcined at 500° C. for 1 hour in an electric furnace, and then slowly cooled. The calcined product was passed through a 20-mesh sieve to obtain the target titanate 5.
[0150] Table 1 shows the chemical composition, crystal structure, crystallite size, average particle size, specific surface area, particle shape, alkali metal ion elution rate, and chloride ion elution rate of the obtained titanate 5.
[0151] (Example 6: Titanate 6) A 20 mass% aqueous slurry of titanate A produced in Comparative Example 1 was prepared, and 0.14 equivalents of sulfuric acid relative to the potassium in the magnesium potassium titanate was mixed with this aqueous slurry and stirred for 2 hours at room temperature (20° C.). This aqueous slurry was suction filtered and washed with deionized water to separate the cake (solid content). This cake was dried at 110° C. for 12 hours, calcined at 500° C. for 1 hour in an electric furnace, and then slowly cooled. The calcined product was passed through a 20-mesh sieve to obtain the target titanate 6.
[0152] The chemical composition, crystal structure, crystallite size, average particle size, specific surface area, particle shape, alkali metal ion elution rate, and chloride ion elution rate of the obtained titanate 6 are shown in Table 1.
[0153] <Measurement of Physical Properties of Titanates> The physical properties of titanates 1 to 6, titanate A, and titanate B were measured as follows, and the results are shown in Table 1.
[0154] (Chemical Composition) The chemical composition was confirmed using an ICP-AES analyzer (manufactured by SII Nanotechnologies, product number "SPS5100").
[0155] (Crystalline structure) The crystal structure was confirmed using a scanning transmission electron microscope (STEM, manufactured by JEOL Ltd., product number "JEM-ARM200F") and a Raman spectrometer (manufactured by METTLER TOLEDO, product number "React Raman 785"). The observation using the scanning transmission electron microscope (STEM) was carried out by preparing a TEM sample by argon ion milling using an ion slicer. The measurement using the Raman spectrometer was carried out at an excitation wavelength of 785 nm and a wave number of 100 cm. -1 ~3200cm -1 The conditions were: exposure time 1 second, and number of scans 10. Specifically, the crystal structure was confirmed as follows.
[0156] Fig. 1 is a scanning transmission electron microscope (STEM) image of titanate 1 obtained in Example 1. Fig. 5 is a scanning transmission electron microscope (STEM) image of titanate A obtained in Comparative Example 1.
[0157] As shown in Figure 1, titanate 1 obtained in Example 1 had a structure similar to a tunnel-shaped crystal structure. Similarly, titanates 2 to 6 obtained in Examples 2 to 6 also had structures similar to a tunnel-shaped crystal structure. On the other hand, as shown in Figure 5, titanate A obtained in Comparative Example 1 had a layered crystal structure. Similarly, titanate B obtained in Comparative Example 2 also had a layered crystal structure.
[0158] FIG. 2 shows Raman spectra of the titanates obtained in Example 1 and Comparative Example 1, and potassium hexatitanate.
[0159] As shown in FIG. 2, titanate 1 obtained in Example 1 exhibited a peak at 835 cm , which is thought to be derived from a layered crystal structure, as in titanate A in Comparative Example 1. -1 On the other hand, in the titanate 1 obtained in Example 1, a peak was observed around 140 cm, which is thought to be a peak derived from a tunnel-shaped crystal structure like potassium hexatitanate. -1 Nearby and 860 cm -1 Since peaks are observed around 1000 s, it can be said that the spectrum of titanate 1 obtained in Example 1 is close to the spectrum of potassium hexatitanate.
[0160] Thus, from the scanning transmission electron microscope (STEM) image and Raman spectroscopy, it was confirmed that titanate 1 obtained in Example 1 had a pseudo-tunnel crystal structure that was close to a tunnel crystal structure. Similarly, it was confirmed that titanates 2 to 6 obtained in Examples 2 to 6 also had pseudo-tunnel crystal structures.
[0161] Furthermore, from the Raman spectroscopy of titanate 1 to titanate 6, titanate A, and titanate B, -1 ~165cm -1 Peak area (Ia) at 215 cm -1 ~325cm -1 The ratio (Ia / Ib) of the peak area at 785 cm -1 ~900cm -1 Peak area (Ic) at 215 cm -1 ~325cm -1 The ratio (Ic / Ib) of the peak area (Ib) at the peak
[0162] In measuring the peak area in each wavelength range, the background of the Raman spectrum was removed using the asymmetric least squares method (ASLS method), and then the peak area was calculated by performing numerical integration using the Simpson method.
[0163] (Crystallite Size) To determine the crystallite size, X-ray diffraction measurement was performed by wide-angle X-ray diffraction. CuKα rays (wavelength 1.5418 Å) were used as the X-ray source. An X-ray diffraction measurement device manufactured by Rigaku Corporation, product number "Ultima IV" was used. X-ray diffraction measurement was performed in the 2θ range of 5° to 60°, and the crystallite size was calculated using the Halder-Wagner method.
[0164] (Average particle size) Measurement was performed using a laser diffraction particle size distribution analyzer (Shimadzu Corporation, product number "SALD-2300"), and the particle size at 50% cumulative volume in the obtained particle size distribution was taken as the average particle size.
[0165] (Specific Surface Area) Measurement was carried out using an automatic specific surface area measuring device (manufactured by Micromeritics, product number "TriStar II 3020").
[0166] (Particle Shape) The particle shape was confirmed using a field emission scanning electron microscope (manufactured by Hitachi High-Tech Corporation, product number "S-4800").
[0167] (Alkali Metal Ion Elution Rate) The mass (X) of the sample was measured, and then the sample was added to ultrapure water to prepare a 1% by mass slurry. After stirring at 80°C for 4 hours, the solid content was removed using a membrane filter with a pore size of 0.2 µm to obtain an extract. The mass (Y) of the alkali metal ions in the obtained extract was measured using an ion chromatograph (manufactured by Dionex Corporation, product number "ICS-1100"). Next, using the values of the masses (X) and (Y) g, the alkali metal ion elution rate (mass %) was calculated based on the formula [(Y) / (X)] x 100.
[0168] (Chloride ion elution rate) The mass (X) of the sample was measured, and then the sample was added to ultrapure water to prepare a 1% by mass slurry. After stirring at 25°C for 10 minutes, the solid content was removed using a membrane filter with a pore size of 0.2 μm to obtain an extract. The mass (Y) of the chloride ions in the obtained extract was measured using an ion chromatograph (manufactured by Dionex Corporation, product number "ICS-1100"). Next, using the values of the masses (X) and (Y) in the above, the formula [(Y) / (X)]×10 was used. 6 The chloride ion elution rate (ppm) was calculated based on the above.
[0169]
[0170] As shown in Table 1, titanates 1 to 6 obtained in Examples 1 to 6 had a pseudo-tunnel crystal structure, and in their Raman spectra, the ratio (Ia / Ib) was 0.03 or more and the ratio (Ic / Ib) was 0.40 or less. On the other hand, titanates A and B obtained in Comparative Examples 1 and 2 had a layered crystal structure, and in their Raman spectra, the ratio (Ia / Ib) was less than 0.03 and the ratio (Ic / Ib) was greater than 0.40.
[0171] <Production of Friction Member> Titanate 1 to Titanate 6, Titanate A, and the following materials were used to produce the friction member.
[0172] (Binder) Thermosetting resin: Hexamethylenetetramine-blended novolac phenolic resin powder
[0173] (Other titanates) Titanate C: potassium hexatitanate, columnar particles, average major axis 65 μm, average minor axis 13 μm Titanate D: sodium hexatitanate, porous spherical particles, average particle diameter 21.2 μm, manufactured by Otsuka Chemical Co., Ltd. (trade name: TERRACESS DSR) Titanate E: potassium hexatitanate, porous spherical particles, average particle diameter 60.1 μm, manufactured by Otsuka Chemical Co., Ltd. (trade name: TERRACESS DP-AS) Titanate F: potassium hexatitanate, columnar particles, average particle diameter 36 μm, manufactured by Otsuka Chemical Co., Ltd. (trade name: TERRACESS JSL)
[0174] (Steel-based fiber) Steel fiber: manufactured by Bonstar Sales Co., Ltd., trade name "Cut Wool BS-1V", curled fiber, average fiber length (cut length) 1.5 mm, average fiber diameter 50 μm
[0175] (Other materials) Rock wool: average fiber length 125 μm, maximum shot content (125 μm or more) 5.0% Aramid fiber: fibrillated para-aramid fiber (aramid pulp), fiber length 0.89 mm, specific surface area 9.8 m 2 / g Cashew dust: average particle diameter 200 μm Zirconium silicate 1: zirconium silicate powder, average particle diameter 1.1 μm, Mohs hardness 7.5 Zirconium silicate 2: zirconium silicate powder, average particle diameter 1.5 μm, Mohs hardness 7.5 Iron oxide: average particle diameter 0.3 μm, Mohs hardness 6 Alumina: α-alumina, average particle diameter 57 μm, Mohs hardness 9 Mica: natural mica, average particle diameter 180 μm Graphite: synthetic graphite, average particle diameter 730 μm Antimony trisulfide: average particle diameter 1.5 μm Tin sulfide: tin (II) sulfide, average particle diameter 7 μm Slaked lime: average particle diameter 0.2 μm Barium sulfate 1: precipitated barium sulfate powder, average particle diameter 1.6 μm Barium sulfate 2: elutriated barium sulfate powder, average particle diameter 24 μm
[0176] (Examples 7 to 17, Comparative Example 3, and Reference Example 1: Friction Member (NAO Material)) The materials were blended according to the blending ratios shown in Tables 2 and 3, and mixed for 3 minutes using an Eirich mixer. The resulting mixture was pressurized at room temperature (20°C) for 5 seconds at a pressure of 15 MPa to produce a temporary compact. The temporary compact was fitted into the cavity of a heated molding die heated to 150°C, and with a back plate (material: steel) placed on top, the mixture was pressurized at a pressure of 10 MPa to 40 MPa for 300 seconds so that the porosity of the compact was 15%. Five degassing treatments were performed between 5 and 70 seconds measured from the start of pressurization. The resulting compact was placed in a constant temperature dryer heated to 220°C and held there for 2 hours to completely harden, thereby obtaining a friction member (NAO material).
[0177] (Examples 18 to 21, Comparative Examples 4 to 7: Friction Members (Low-Steel Material)) The materials were blended according to the blending ratios shown in Tables 5 and 6, and mixed for 3 minutes using an Eirich mixer. The resulting mixture was placed in the cavity of a hot-molding mold heated to 150°C, and with a back plate (made of steel) still placed on top, the molded body was pressurized at a pressure of 15 MPa to 40 MPa for 240 seconds so that the porosity of the molded body was 15%. The resulting molded body was placed in a constant-temperature dryer heated to 210°C, held there for 2 hours, and completely cured to obtain a friction member (low-steel material).
[0178] <Evaluation of Friction Member> The Rockwell hardness and fade test of the friction members prepared above were evaluated as follows.
[0179] (Rockwell Hardness) The Rockwell hardness of the surface of the friction member was measured according to the method of JIS D 4421. The S scale was used as the hardness scale.
[0180] (Friction Test 1) The surface (friction surface) of the friction member was polished to 1.0 mm, and a braking effectiveness test was performed based on JASO C406. However, the first fade test conditions were changed to a speed of 160 km / h, which is assumed to be a high load, and the braking effectiveness test was performed. The rotor used was a cast iron rotor that conforms to ASTM standard number A48 / A48M.
[0181] FIG. 3 is a graph showing the relationship between the number of braking cycles and the coefficient of friction during fading in friction test 1 for the friction members obtained in Example 7 and Comparative Example 3.
[0182] As can be seen from Figure 3, Example 7, which used magnesium potassium titanate with a pseudo-tunnel crystal structure, had a larger friction coefficient in the high load range and better stability of the friction coefficient than Comparative Example 3, which used magnesium potassium titanate with a layered crystal structure.
[0183] 4 is a graph showing the relationship between the change in friction coefficient (μ) with respect to rotor temperature and the average friction coefficient (μ) during fade in Friction Test 1 for the friction members obtained in Example 7, Comparative Example 3, and Reference Example 1. The average friction coefficient (μ) during fade was determined from the average value (average μ) of 10 braking cycles in the first fade test results.
[0184] From Figure 4, it can be seen that Example 7, which used magnesium potassium titanate with a pseudo-tunnel crystal structure, had a friction coefficient that was equal to or greater than that of Reference Example 1, which used potassium hexatitanate with a tunnel crystal structure, and the stability of the friction coefficient was also improved.
[0185] For Examples 7 to 17, Comparative Example 3, and Reference Example 1, the average value (average μ) of the 10 braking cycles in the first fade test results and Δμ (maximum - minimum) were calculated from the difference between the maximum μ and minimum μ during the first fade. The results are shown in Tables 2 and 3 below.
[0186]
[0187]
[0188] (Friction Test 2) The surface (friction surface) of the friction member (low-steel material) was polished by 1.0 mm to prepare a friction member for a scale dynamo test. The friction member and a rotor (cast iron rotor belonging to type A in the ASTM standard) were used to perform a test at 65 km / h and 3.5 m / s. 2The friction members and rotors that had been previously subjected to the above-mentioned conditions were used to carry out tests under the friction conditions shown in Table 4, and the average friction coefficient, friction material wear amount, and rotor wear amount were measured. The test was carried out twice, and the average values were used as the measurement results. The results are shown in Table 5.
[0189] (Wear dust measurement) The surface (friction surface) of the friction member (low-steel material) was polished by 1.0 mm to prepare a friction member for a scale dynamo test. The friction member and a disc rotor (cast iron rotor belonging to type A in the ASTM standard) were used to measure the friction dust at 65 km / h and 3.5 m / s. 2 The friction test was performed under the conditions of 500 braking cycles, and an abrasion dust collector was connected to a scale dynamometer. An MCI sampler (equipped with a filter to collect PM10-2.5 and PM2.5) manufactured by Tokyo Dylec Co., Ltd. was attached to the abrasion dust collector. Next, using the friction members and disc rotors that had been previously subjected to abrasion testing under the above conditions, a friction test was performed under the friction conditions shown in Table 4, and the mass of particulate matter (amount of PM10-2.5 generated and amount of PM2.5 generated) that was collected by the filter, representing abrasion dust generated during the friction test, was measured. The test was performed twice, and the average value was used as the measurement result. The results are shown in Table 6.
[0190]
[0191]
[0192]
[0193] From Table 5, it was confirmed that the friction members of Examples 18 to 21, which used magnesium potassium titanate (titanate 1) with a pseudo-tunnel crystal structure, could form low-steel materials with small wear amounts of the friction material and rotor and large friction coefficients.
[0194] On the other hand, the friction members of Comparative Examples 4 and 6, which used only titanate A having a layered crystal structure, and the friction members of Comparative Examples 5 and 7, which did not contain titanate, had particularly insufficient friction coefficients.
[0195] From Table 6, it was confirmed that the friction members of Examples 18 and 19, which used magnesium potassium titanate (titanate 1) with a pseudo-tunnel crystal structure, could form low-steel materials that generated little fine dust.
[0196] Furthermore, it was confirmed that the friction members of Examples 20 and 21, which contained magnesium potassium titanate (titanate 1) with a pseudo-tunnel crystal structure but did not contain tin sulfide, were able to form low-steel materials that generated particularly little fine dust.
[0197] On the other hand, the friction member of Comparative Example 5, which did not contain titanate, generated a large amount of fine dust, which was not sufficient.
Claims
1. Composition formula K x Mg 0.4 Ti 1.6 O 4-y [wherein x is 0.1≦x≦0.6, y=(0.8−x) / 2], and in the Raman spectrum of the magnesium potassium titanate, -1 ~165cm -1 Peak area (Ia) at 215 cm -1 ~325cm -1 The ratio (Ia / Ib) of the peak area at 785 cm to the peak area at 785 cm is 0.03 or more. -1 ~900cm -1 Peak area (Ic) at 215 cm -1 ~325cm -1 The ratio (Ic / Ib) of the peak area to the peak area (Ib) in the above formula (Ic / Ib) is 0.40 or less.
2. The magnesium potassium titanate according to claim 1, which is substantially free of anatase titanium dioxide.
3. The magnesium potassium titanate according to claim 1 or 2, wherein the magnesium potassium titanate is in the form of plate-like particles.
4. The magnesium potassium titanate according to claim 1 or 2, wherein the average particle size of the magnesium potassium titanate is 0.1 μm to 100 μm.
5. The specific surface area of the magnesium potassium titanate is 0.1 m 2 / g to 10m 2 The magnesium potassium titanate according to claim 1 or 2, wherein the molecular weight of the magnesium potassium titanate is 1000 or more.
6. The magnesium potassium titanate according to claim 1 or 2, wherein the alkali metal ion elution rate of the magnesium potassium titanate is 0.01% by mass to 15% by mass.
7. A friction modifier comprising the magnesium potassium titanate according to claim 1 or 2.
8. A friction material composition containing magnesium potassium titanate according to claim 1 or 2 and a binder, the friction material composition having a copper content of less than 0.5 mass% in terms of copper element per 100 mass% of the total amount of the friction material composition.
9. The friction material composition according to claim 8, wherein the content of the magnesium potassium titanate is 1% by mass to 40% by mass relative to 100% by mass of the total amount of the friction material composition.
10. The friction material composition according to claim 8, further comprising at least one of a titanate having a layered crystal structure and a titanate having a tunnel-shaped crystal structure.
11. The friction material composition according to claim 8, which is substantially free of a sulfide-based solid lubricant.
12. The friction material composition according to claim 8, wherein the content of steel-based fibers is less than 10 mass % relative to 100 mass % of the total amount of the friction material composition.
13. The friction material composition according to claim 8, wherein the content of the steel fiber is 10 mass % or more relative to 100 mass % of the total amount of the friction material composition.
14. A friction material which is a molded product of the friction material composition according to claim 8.
15. A friction member comprising the friction material according to claim 14.
Citation Information
Patent Citations
Friction material composition, friction material, and friction member
WO2018164028A1
Plate like potassium hexatitanate, plate like potassium tetratitanate, manufacturing method thereof and friction material
JP2001253712A
Friction material composition, and friction material and friction member using the same
JP2015147913A
Friction material
JP2017193612A
Lepidocrosite type potassium magnesium titanate and method for production thereof, and friction material
WO2002010069A1