Reflective mask blank, reflective mask, reflective mask blank manufacturing method, and reflective mask manufacturing method
The use of a CrN compound in the reflective mask blank's absorbing film addresses the high relative reflectance issue in conventional EUV lithography masks, enhancing EUV light absorption and phase shifting for improved image contrast and precision.
Patent Information
- Application Number
- PCT/JP2024/017857
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-14
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional reflective masks for EUV lithography face challenges in achieving optimal absorption and phase shifting with materials containing Cr, as they often have high relative reflectance, affecting image contrast and precision in semiconductor manufacturing.
A reflective mask blank comprising a substrate, a multilayer reflective film, a protective film, and an absorbing film with a Cr-containing layer made of a CrN compound, where the CrN compound has a refractive index of 0.920 to 0.940 and an extinction coefficient of 0.032 to 0.044, ensuring good amorphous properties and a relative reflectance of less than 5%, thereby improving EUV light absorption and phase shifting.
The CrN compound-based absorbing film enhances EUV light absorption and phase shifting, reducing shadowing effects and improving image contrast, leading to more precise pattern transfer in EUV lithography.
Smart Images

Figure JP2024017857_05122024_PF_FP_ABST
Abstract
Description
Reflective mask blank, reflective mask, method for manufacturing a reflective mask blank, and method for manufacturing a reflective mask
[0001] The present disclosure relates to a reflective mask blank, a reflective mask, a method for manufacturing a reflective mask blank, and a method for manufacturing a reflective mask.
[0002] In recent years, with the miniaturization of semiconductor devices, EUV lithography (EUVL), an exposure technology using extreme ultraviolet (EUV) light, has been developed. EUV includes soft X-rays and vacuum ultraviolet light, and specifically refers to light with a wavelength of approximately 0.2 nm to 100 nm. At present, EUV light with a wavelength of approximately 13.5 nm is mainly being considered.
[0003] In EUVL, a reflective mask is used. The reflective mask has, in this order, a substrate such as a glass substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and an absorbing film that absorbs EUV light. The absorbing film may not only absorb EUV light, but also shift the phase of the EUV light. In other words, the absorbing film may be a phase shift film. An opening pattern is formed in the absorbing film. In EUVL, the opening pattern in the absorbing film is transferred to a target substrate such as a semiconductor substrate. Transferring includes transferring after reducing the size.
[0004] The reflective mask blank described in Patent Document 1 comprises a substrate, a multilayer reflective film, a protective film, and an absorbing film in this order. Examples of Patent Document 1 disclose the following absorbing films: MoCrRu film (Mo: 20 at%, Cr: 46 at%, Ru: 34 at%), MoWRu film (Mo: 34 at%, W: 15 at%, Ru: 51 at%), MoAuRu film (Mo: 13 at%, Au: 12 at%, Ru: 75 at%), MoWRu film (Mo: 29 at%, W: 6 at%, Ru: 65 at%), MoWV film (Mo: 46 at%, W: 25 at%, V: 29 at%), etc. These absorbing films have a ratio (R A / R B ) is 0.05 to 0.25. A is the reflectance of EUV light reflected by the multilayer reflective film and the protective film to the opposite side of the substrate via the absorbing film. Bis the reflectance of EUV light reflected by the multilayer reflective film and the protective film toward the opposite side of the substrate without passing through the absorbing film.
[0005] The reflective mask blank described in Patent Document 2 includes a substrate, a multilayer reflective film, a protective film, and a phase shift film, in this order. The phase shift film includes a lower layer and a top layer. In Example 1 of Patent Document 2, the lower layer of the phase shift film is a RuCrN film (Ru: 79.4 at %, Cr: 13.6 at %, N: 7.0 at %, refractive index: 0.900, extinction coefficient: 0.023), and the top layer of the phase shift film is a RuCrO film (Ru: 18.1 at %, Cr: 29.5 at %, O: 52.4 at %, refractive index: 0.931, extinction coefficient: 0.027).
[0006] The reflective mask blank described in Patent Document 3 includes a substrate, a multilayer reflective film, a protective film, and a phase shift film, in this order. In Example 1 of Patent Document 3, the phase shift film is a RuCr film (Ru: 7 at %, Cr: 93 at %, refractive index: 0.929, extinction coefficient: 0.037, relative reflectance: 6%). In Example 4 of Patent Document 3, the phase shift film is a RuCr film (Ru: 39 at %, Cr: 61 at %, refractive index: 0.913, extinction coefficient: 0.030, relative reflectance: 15%).
[0007] Japanese Patent Publication No. 2022-135928 Japanese Patent Publication No. 2021-081644 International Publication No. 2019 / 225736
[0008] Various materials have been investigated as materials for the absorbing film. Materials containing Cr as a main component are considered to have a refractive index of 0.920 to 0.940 and an extinction coefficient of 0.032 to 0.044.
[0009] One aspect of the present disclosure provides an absorbing film that is mainly composed of Cr, has good amorphous properties, and has a relative reflectance of less than 5%.
[0010] A reflective mask blank according to one embodiment of the present disclosure has a substrate, a multilayer reflective film, a protective film, and an absorbing film, in this order. The multilayer reflective film reflects EUV light. The protective film protects the multilayer reflective film during processing of the absorbing film. The absorbing film absorbs EUV light. The absorbing film has a Cr-containing layer made of a CrN compound containing 50 at% or more of Cr and 10 at% or more of N. The Cr-containing layer has a full width at half maximum of the most intense peak in the 2θ range of 20° to 50° measured by XRD using CuKα radiation of 1.0° or more, and the ratio of the reflectance of EUV light reflected by the multilayer reflective film and the protective film toward the opposite side of the substrate via the absorbing film to the reflectance of EUV light reflected by the multilayer reflective film and the protective film toward the opposite side of the substrate without via the absorbing film is less than 5%.
[0011] According to one aspect of the present disclosure, it is possible to provide an absorbing film that is mainly composed of Cr, has good amorphous properties, and has a relative reflectance of less than 5%.
[0012] FIG. 1 is a cross-sectional view showing a reflective mask blank according to an embodiment. FIG. 2 is a flowchart showing a method for manufacturing a reflective mask blank according to an embodiment. FIG. 3 is a cross-sectional view showing a reflective mask according to an embodiment. FIG. 4 is a flowchart showing a method for manufacturing a reflective mask according to an embodiment. FIG. 5(A) is a cross-sectional view showing an example of preparation of a reflective mask blank, FIG. 5(B) is a cross-sectional view showing an example of an example at the end of processing a hard mask film, and FIG. 5(C) is a cross-sectional view showing an example of an example at the end of processing an absorbing film. FIG. 6 is a cross-sectional view showing an example of EUV light reflected by the reflective mask of FIG. 3. FIG. 7 is a diagram showing an example of the refractive index and extinction coefficient of each element.
[0013] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In each drawing, the same or corresponding components are denoted by the same reference numerals, and their description may be omitted. In the specification, the symbol "to" indicating a range of values means that the values before and after it are included as the lower and upper limits.
[0014] In each drawing, the X-axis direction, the Y-axis direction, and the Z-axis direction are perpendicular to one another. The Z-axis direction is perpendicular to the first main surface 10a of the substrate 10. The X-axis direction is perpendicular to the plane of incidence of the EUV light (the plane including the incident light beam and the reflected light beam). As shown in Figure 6, the incident light beam is tilted more in the positive Y-axis direction as it moves in the negative Z-axis direction, and the reflected light beam is tilted more in the positive Y-axis direction as it moves in the positive Z-axis direction.
[0015] A reflective mask blank 1 according to one embodiment will be described with reference to FIG. 1 . The reflective mask blank 1 includes, for example, a substrate 10, a multilayer reflective film 11, a protective film 12, an absorbing film 13, and a hard mask film 14, in this order. The multilayer reflective film 11, the protective film 12, the absorbing film 13, and the hard mask film 14 are formed on a first main surface 10a of the substrate 10 in this order. The multilayer reflective film 11 reflects EUV light. The protective film 12 protects the multilayer reflective film 11 from a first etching gas during processing of the absorbing film 13. The absorbing film 13 absorbs EUV light. The absorbing film 13 may not only absorb EUV light but also shift the phase of the EUV light. In other words, the absorbing film 13 may be a phase shift film. The hard mask film 14 protects a portion of the absorbing film 13 from the first etching gas during processing of the absorbing film 13.
[0016] The reflective mask blank 1 may further have a functional film not shown in FIG. 1 . For example, the reflective mask blank 1 may have a conductive film on the opposite side of the substrate 10 from the multilayer reflective film 11. The conductive film is formed on the second main surface 10b of the substrate 10. The second main surface 10b is the surface facing away from the first main surface 10a. The conductive film is used, for example, to attach the reflective mask 2 to an electrostatic chuck of an exposure tool. The reflective mask blank 1 may have a diffusion barrier film (not shown) between the multilayer reflective film 11 and the protective film 12. The diffusion barrier film suppresses diffusion of metal elements contained in the protective film 12 into the multilayer reflective film 11.
[0017] Although not shown, the reflective mask blank 1 may have a buffer film between the protective film 12 and the absorbing film 13. The buffer film protects the protective film 12 from the first etching gas that forms the opening pattern 13a in the absorbing film 13. The buffer film is etched more slowly than the absorbing film 13. Unlike the protective film 12, the buffer film will ultimately have the same opening pattern as the opening pattern 13a in the absorbing film 13.
[0018] Next, a method for manufacturing a reflective mask blank 1 according to one embodiment will be described with reference to Fig. 2. The method for manufacturing the reflective mask blank 1 includes, for example, steps S101 to S105 shown in Fig. 2. In step S101, a substrate 10 is prepared. In step S102, a multilayer reflective film 11 is formed on the first main surface 10a of the substrate 10. In step S103, a protective film 12 is formed on the multilayer reflective film 11. In step S104, an absorbing film 13 is formed on the protective film 12. In step S105, a hard mask film 14 is formed on the absorbing film 13. The method for manufacturing the reflective mask blank 1 may further include a step of forming a functional film not shown in Fig. 2.
[0019] Next, a reflective mask 2 according to one embodiment will be described with reference to FIG. 3. The reflective mask 2 is fabricated using, for example, the reflective mask blank 1 shown in FIG. 1 and includes an opening pattern 13a in an absorbing film 13. In EUVL, the opening pattern 13a in the absorbing film 13 is transferred to a target substrate such as a semiconductor substrate. Transferring includes reducing and transferring. Note that the hard mask film 14 shown in FIG. 1 is not included in the reflective mask 2.
[0020] Next, a method for manufacturing a reflective mask 2 according to one embodiment will be described with reference to Figures 4 and 5. The method for manufacturing a reflective mask 2 includes steps S201 to S204 shown in Figure 4. In step S201, a reflective mask blank 1 is prepared, as shown in Figure 5(A). The reflective mask blank 1 includes a resist film 16, as shown in Figure 5(A). The resist film 16 is formed on a hard mask film 14. An opening pattern to be transferred to the absorption film 13 is formed in the resist film 16.
[0021] 5B, the hard mask film 14 is processed using the resist film 16 having an opening pattern. In the openings in the resist film 16, the hard mask film 14 is exposed to a second etching gas, and the second etching gas etches the hard mask film 14. At the end of step S202, the resist film 16 remains. As a result, the opening pattern of the resist film 16 is transferred to the hard mask film 14.
[0022] The second etching gas is selected depending on the combination of the material of the resist film 16 and the material of the hard mask film 14, and is not particularly limited, but may include, for example, a fluorine-based gas. The fluorine-based gas may be, for example, CF 4 Gas, CHF 3 Gas, C 2 F 6 Gas, C 3 F 6 Gas, C 4 F 6 Gas, C 4 F 8 Gas, CH 2 F 2 Gas, CH 3 F gas, C 3 F 8 Gas, F 2 Gas, SF 6 Gas and NF 3 The second etching gas may contain at least one selected from the group consisting of a fluorine-based gas, an active gas, and an inert gas. The active gas may be, for example, O 2 The inert gas includes, for example, N 2 The second etching gas preferably contains at least one selected from the group consisting of a nitrogen gas, a He gas, and an Ar gas. The second etching gas is preferably a plasma.
[0023] In step S203, as shown in FIG. 5C , the absorber film 13 is processed using the hard mask film 14 having an opening pattern. In the openings in the hard mask film 14, the absorber film 13 is exposed to a first etching gas, and the first etching gas etches the absorber film 13. The hard mask film 14 has higher resistance to the first etching gas than the absorber film 13. At the end of step S203, the hard mask film 14 remains. As a result, the opening pattern of the hard mask film 14 is transferred to the absorber film 13.
[0024] The first etching gas is selected depending on the combination of the material of the hard mask film 14 and the material of the absorption film 13, and is not particularly limited, but includes, for example, a chlorine-based gas and an oxygen-based gas. The chlorine-based gas is, for example, Cl 2 Gas, SiCl 4 Gas, CHCl 3 Gas, CCl 4 Gas and BCl 3 The oxygen-based gas includes at least one selected from the group consisting of O 2 Gas and O 3 The first etching gas may contain at least one selected from the group consisting of a chlorine-based gas, an oxygen-based gas, and an inert gas. The inert gas may be, for example, N 2 The first etching gas preferably contains at least one selected from the group consisting of a nitrogen gas, a He gas, and an Ar gas. The first etching gas is preferably a plasma.
[0025] In step S204, although not shown, the hard mask film 14 is removed. A third etching gas, for example, is used to remove the hard mask film 14. The third etching gas, like the second etching gas, contains, for example, a fluorine-based gas. The third etching gas is preferably a plasma gas. A chemical solution may be used to remove the hard mask film 14.
[0026] Next, referring back to FIG. 1, the substrate 10, the multilayer reflective film 11, the protective film 12, the absorbing film 13, and the hard mask film 14 will be described in this order.
[0027] The substrate 10 is, for example, a glass substrate. The material of the substrate 10 is TiO 2The quartz glass has a smaller coefficient of linear expansion and a smaller change in dimension due to temperature changes than common soda lime glass. 2 80% by mass to 95% by mass of TiO 2 It may contain 4% to 17% by mass of TiO 2 When the content is 4% by mass to 17% by mass, the linear expansion coefficient is approximately zero around room temperature, and there is almost no dimensional change around room temperature. 2 and TiO 2 The substrate 10 may contain a third component or impurities other than the above. The material of the substrate 10 may be crystallized glass in which a β-quartz solid solution is precipitated, silicon, a metal, or the like.
[0028] The substrate 10 has a first major surface 10a and a second major surface 10b facing opposite to the first major surface 10a. A multilayer reflective film 11 and the like are formed on the first major surface 10a. In plan view (viewed in the Z-axis direction), the substrate 10 measures, for example, 152 mm long and 152 mm wide. The vertical and horizontal dimensions may be 152 mm or greater. The first major surface 10a and the second major surface 10b each have, for example, a square quality assurance area at their centers. The quality assurance area measures, for example, 142 mm long and 142 mm wide. The vertical and horizontal dimensions may be 142 mm or greater. The quality assurance area on the first major surface 10a preferably has a root-mean-square roughness (Rq) of 0.15 nm or less and a flatness of 100 nm or less. Furthermore, the quality assurance area on the first major surface 10a preferably does not have defects that cause phase defects.
[0029] The multilayer reflective film 11 reflects EUV light. The multilayer reflective film 11 is formed by alternately stacking, for example, high-refractive-index layers and low-refractive-index layers. The high-refractive-index layers are made of, for example, silicon (Si), and the low-refractive-index layers are made of, for example, molybdenum (Mo), so that a Mo / Si multilayer reflective film is used. Note that other films that can be used as the multilayer reflective film 11 include a Ru / Si multilayer reflective film, a Mo / Be multilayer reflective film, a Mo compound / Si compound multilayer reflective film, a Si / Mo / Ru multilayer reflective film, a Si / Mo / Ru / Mo multilayer reflective film, a Si / Ru / Mo / Ru multilayer reflective film, and a Si / Ru / Mo multilayer reflective film.
[0030] The thickness of each layer constituting the multilayer reflective film 11 and the number of repeating units of the layers can be appropriately selected depending on the material of each layer and the reflectivity for EUV light. When the multilayer reflective film 11 is a Mo / Si multilayer reflective film, in order to achieve a reflectivity of 60% or more for EUV light at an incident angle θ (see FIG. 6 ) of 6°, Mo layers with a thickness of 2.3±0.1 nm and Si layers with a thickness of 4.5±0.1 nm can be stacked so that the number of repeating units is 30 to 60. The multilayer reflective film 11 preferably has a reflectivity of 60% or more for EUV light at an incident angle θ of 6°. The reflectivity is more preferably 65% or more.
[0031] The method for forming each layer constituting the multilayer reflective film 11 is, for example, DC sputtering, magnetron sputtering, or ion beam sputtering. When the Mo / Si multilayer reflective film is formed using ion beam sputtering, an example of the film formation conditions for the Mo layer and the Si layer is as follows: <Si layer formation conditions> Target: Si target, Sputtering gas: Ar gas, Gas pressure: 1.3×10 -2 Pa ~ 2.7 x 10 -2 Pa, Ion acceleration voltage: 300 V to 1500 V, Film formation rate: 0.030 nm / sec to 0.300 nm / sec, Thickness of Si layer: 4.5±0.1 nm, <Film formation conditions for Mo layer> Target: Mo target, Sputtering gas: Ar gas, Gas pressure: 1.3×10 -2 Pa ~ 2.7 x 10 -2 Pa, ion acceleration voltage: 300 V to 1500 V, film formation rate: 0.030 nm / sec to 0.300 nm / sec, film thickness of Mo layer: 2.3±0.1 nm, <Repeating units of Si layer and Mo layer> Number of repeating units: 30 to 60 (preferably 40 to 50).
[0032] The protective film 12 is formed between the multilayer reflective film 11 and the absorbing film 13 to protect the multilayer reflective film 11. The protective film 12 protects the multilayer reflective film 11 from the first etching gas when processing the absorbing film 13, i.e., in step S203. The protective film 12 is not removed even when exposed to the first etching gas, but remains on the multilayer reflective film 11.
[0033] The protective film 12 contains at least one element selected from, for example, Ru, Rh, and Si. When the protective film 12 contains Rh, the protective film 12 may contain only Rh, or may contain an Rh compound. The Rh compound may contain, in addition to Rh, at least one element Z1 selected from Ru, Nb, Mo, Ta, Ir, Pd, Zr, Y, and Ti.
[0034] Adding Ru, Nb, Mo, Zr, Y, or Ti to Rh can reduce the extinction coefficient while suppressing an increase in the refractive index, and can suppress absorption of EUV light by the protective film 12 (and thus a decrease in reflectance for EUV light). Furthermore, adding Ta, Ir, Pd, or Y to Rh can improve resistance to the first etching gas.
[0035] The Rh compound may contain, in addition to Rh, at least one element Z2 selected from N, O, C, and B. The element Z2 reduces the resistance of the protective film 12 to the first etching gas, but improves the smoothness of the protective film 12 by reducing the crystallinity of the protective film 12. The Rh compound containing the element Z2 has an amorphous structure or a microcrystalline structure. When the Rh compound has an amorphous structure or a microcrystalline structure, the X-ray diffraction profile of the Rh compound does not have a clear peak.
[0036] The protective film 12 may be a film consisting of a single layer, or may be a multi-layer film having a lower layer and an upper layer. The lower layer and upper layer constituting the protective film 12 are formed in this order on the multilayer reflective film 11. The lower layer of the protective film 12 is a layer formed in contact with the uppermost surface of the multilayer reflective film 11. The upper layer of the protective film 12 is in contact with the lowermost surface of the absorbing film 13. By making the protective film 12 have such a multi-layer structure, materials with excellent predetermined functions can be used for each layer, thereby making the entire protective film 12 multifunctional.
[0037] The upper layer of the protective film 12 preferably contains at least one element selected from Ru and Rh, more preferably Rh, and even more preferably a Rh compound. The lower layer of the protective film 12 preferably contains at least one element selected from Ru, Rh, Nb, Mo, Zr, Y, Si, C, N, and B, and more preferably Ru. When the protective film 12 is a multi-layer film, the thickness of the protective film 12 below refers to the total film thickness of the multi-layer film. Note that a mixing layer formed by mixing components contained in the multi-layer reflective film 11 and components contained in the lower layer of the protective film 12 may be formed between the multi-layer reflective film 11 and the lower layer of the protective film 12.
[0038] The thickness of the protective film 12 is preferably 1.0 nm to 4.0 nm, more preferably 2.0 nm to 3.5 nm, and even more preferably 2.5 nm to 3.0 nm. If the thickness of the protective film 12 is 1.0 nm or more, the etching resistance is good. Furthermore, if the thickness of the protective film 12 is 4.0 nm or less, the reflectance to EUV light is good.
[0039] The density of the protective film 12 is preferably 10.0 g / cm 3 ~14.0g / cm 3 The density of the protective film 12 is 10.0 g / cm 3 If the density of the protective film 12 is 14.0 g / cm or more, the etching resistance is good. 3 If it is equal to or less than this, it is possible to suppress a decrease in reflectance for EUV light.
[0040] The upper surface of the protective film 12, i.e., the surface of the protective film 12 on which the absorbing film 13 is formed, preferably has a root-mean-square roughness Rq of 0.20 nm or less, more preferably 0.17 nm or less. If the root-mean-square roughness Rq is 0.20 nm or less, the absorbing film 13 and the like can be formed smoothly on the protective film 12. In addition, scattering of EUV light can be suppressed, and the reflectance for EUV light can be improved. The root-mean-square roughness Rq is preferably 0.05 nm or more.
[0041] The protective film 12 can be formed by, for example, DC sputtering, magnetron sputtering, or ion beam sputtering. When the Rh film is formed by DC sputtering, an example of the film formation conditions is as follows: <Conditions for forming Rh film> Target: Rh target, Sputtering gas: Ar gas, Gas pressure: 1.0×10 -2 Pa ~ 1.0 x 10 0 Pa, target power density: 1.0 W / cm 2 ~8.5 W / cm 2 , Film formation rate: 0.020 nm / sec to 1.000 nm / sec, Film thickness: 1 nm to 10 nm.
[0042] The absorbing film 13 absorbs EUV light. The absorbing film 13 is a film in which an opening pattern 13a is to be formed. The opening pattern 13a is not formed in the manufacturing process of the reflective mask blank 1, but is formed in the manufacturing process of the reflective mask 2. The absorbing film 13 may not only absorb EUV light, but also shift the phase of the EUV light. In other words, the absorbing film 13 may be a phase shift film. The phase shift film shifts the phase of the second EUV light L2 relative to the first EUV light L1 shown in FIG. 6 .
[0043] The first EUV light L1 is light that passes through the opening pattern 13a without passing through the absorbing film 13, is reflected by the multilayer reflective film 11, and passes through the opening pattern 13a without passing through the absorbing film 13 again. The second EUV light L2 is light that passes through the absorbing film 13 while being absorbed by the absorbing film 13, is reflected by the multilayer reflective film 11, and passes through the absorbing film 13 while being absorbed by the absorbing film 13 again.
[0044] The phase difference (≧0) between the first EUV light L1 and the second EUV light L2 is, for example, 170° to 250°. The phase of the first EUV light L1 may be ahead of or behind the phase of the second EUV light L2. The absorbing film 13 improves the contrast of the transferred image by utilizing interference between the first EUV light L1 and the second EUV light L2. The transferred image is an image obtained by transferring the opening pattern 13a of the absorbing film 13 onto the target substrate.
[0045] In EUVL, a so-called shadowing effect occurs. The shadowing effect refers to the occurrence of a region in the vicinity of the sidewall of the opening pattern 13 a where the sidewall blocks the EUV light due to the incident angle θ of the EUV light being not 0° (for example, 6°), resulting in a positional or dimensional deviation of the transferred image. In order to reduce the shadowing effect, it is effective to reduce the height of the sidewall of the opening pattern 13 a, and it is also effective to thin the absorbing film 13.
[0046] The thickness of the absorbing film 13 is, for example, 60 nm or less, and preferably 50 nm or less, in order to reduce the shadowing effect, and is preferably 20 nm or more, and more preferably 30 nm or more, in order to ensure a phase difference between the first EUV light L1 and the second EUV light L2.
[0047] In order to reduce the thickness of the absorbing film 13 so as to reduce the shadowing effect while ensuring the phase difference between the first EUV light L1 and the second EUV light L2, it is effective to reduce the refractive index n of the absorbing film 13. Furthermore, in order to reduce the reflectance for EUV light, it is effective to increase the extinction coefficient k of the absorbing film 13. Thus, the absorbing film 13 is required to have excellent optical properties.
[0048] 7 is a diagram showing an example of the refractive index n and extinction coefficient k of each element. In this specification, the refractive index n is the refractive index for EUV light (e.g., light with a wavelength of 13.5 nm). Also, in this specification, the extinction coefficient k is the extinction coefficient for EUV light (e.g., light with a wavelength of 13.5 nm).
[0049] 7, A represents a range in which the refractive index n is 0.920 to 0.940 and the extinction coefficient k is 0.032 to 0.044. A material containing Cr as a main component is considered as a material having optical properties in range A. In this embodiment, a CrN compound containing 50 at % or more of Cr and 10 at % or more of N is used as the material having optical properties in range A.
[0050] The optical properties (refractive index n and extinction coefficient k) of CrN compounds are taken from the database of the Center for X-Ray Optics, Lawrence Berkeley National Laboratory, or values calculated from the "incident angle dependence" of reflectance, which will be described later.
[0051] The incident angle θ of the EUV light, the reflectance R for the EUV light, the refractive index n of the absorbing film 13, and the extinction coefficient k of the absorbing film 13 satisfy the following formula (1): R=|(sin θ−((n+ik) 2 -cos 2 θ) 1/2 ) / (sinθ+((n+ik) 2 -cos 2 θ) 1/2 ) | (1) A plurality of combinations of the incident angle θ and the reflectance R are measured, and the refractive index n and the extinction coefficient k are calculated by the least squares method so that the error between the plurality of measurement data and the formula (1) is minimized.
[0052] The refractive index n of the CrN compound is preferably 0.920 to 0.940, more preferably 0.920 to 0.930. The smaller the refractive index n of the absorbing film 13, the thinner the absorbing film 13 can be made.
[0053] The extinction coefficient k of the CrN compound is preferably 0.032 to 0.044, and more preferably 0.034 to 0.044. The greater the extinction coefficient k of the absorbing film 13, the smaller the relative reflectance Ra, which will be described later.
[0054] The relative reflectance Ra is the ratio (%) of the reflectance R2 of the second EUV light L2 to the reflectance R1 of the first EUV light L1. The first EUV light L1 is EUV light that is reflected by the multilayer reflective coating 11 and the protective coating 12 toward the opposite side of the substrate 10 without passing through the absorbing film 13. The reflectance R1 of the first EUV light L1 is measured, for example, before the absorbing film 13 is formed. The reflectance R1 of the first EUV light L1 may also be measured after the absorbing film 13 is formed and then removed. The second EUV light L2 is EUV light that is reflected by the multilayer reflective coating 11 and the protective coating 12 toward the opposite side of the substrate 10 via the absorbing film 13. The reflectance R2 of the second EUV light L2 is measured, for example, after the absorbing film 13 is formed.
[0055] The absorbing film 13 has a Cr-containing layer 13A made of a CrN compound. If the CrN compound has an N content of 10 at% or more, it has good amorphous properties and a relative reflectance Ra of less than 5%. If the relative reflectance Ra is less than 5%, the intensity difference between the first EUV light L1 and the second EUV light L2 can be improved, and the contrast of the transferred image can be improved. The N content of the CrN compound is preferably 10 at% or more, and more preferably 15 at% or more. The N content of the CrN compound is preferably 40 at% or less, more preferably 35 at% or less, and even more preferably 30 at% or less.
[0056] The amorphousness is expressed by the diffraction intensity of XRD using CuKα radiation. For CrN compounds, the full width at half maximum (FWHM) of the most intense peak in the 2θ range of 20° to 50° measured by XRD using CuKα radiation is 1.0° or more. The out-of-plane method is used as the XRD method.
[0057] If the full width at half maximum FWHM is 1.0° or more, the crystallinity of the Cr-containing layer 13A is low, and the roughness of the sidewalls of the opening pattern 13a can be reduced. The full width at half maximum FWHM is preferably 2.0° or more, and more preferably 3.0° or more. The larger the full width at half maximum FWHM, the better, and it is preferable that there is no clear peak.
[0058] As described above, the CrN compound contains 50 at% or more of Cr and 10 at% or more of N. The CrN compound preferably further contains Ru. The Ru content of the CrN compound is preferably 5 at% or more, more preferably 10 at% or more. When the Ru content of the CrN compound is 5 at% or more, the refractive index of the CrN compound is sufficiently small.
[0059] The Ru content of the CrN compound is preferably 25 at% or less. If the Ru content of the CrN compound is 25 at% or less, the extinction coefficient k of the CrN compound becomes 0.032 or more. The Ru content of the CrN compound is more preferably 20 at% or less.
[0060] The ratio of the Ru content to the Cr content of the CrN compound (Ru / Cr) is preferably 0.60 or less. If the ratio of the Ru content to the Cr content of the CrN compound (Ru / Cr) is 0.60 or less, the extinction coefficient k of the CrN compound will be 0.032 or more. The ratio of the Ru content to the Cr content of the CrN compound (Ru / Cr) is more preferably 0.50 or less, even more preferably 0.40 or less, even more preferably 0.30 or less, particularly preferably 0.25 or less, and most preferably 0.22 or less.
[0061] The absorbing film 13 may have an oxide layer 13B made of an oxide on the opposite side of the Cr-containing layer 13A from the protective film 12. The oxide layer 13B is formed, for example, by natural oxidation of the surface of the Cr-containing layer 13A by the atmosphere. Note that the oxide layer 13B is not necessary, and the absorbing film 13 may be composed of only the Cr-containing layer 13A.
[0062] The thickness of the oxide layer 13B is preferably 5 nm or less. Since the thickness of the oxide layer 13B is sufficiently thin, the physical properties (e.g., optical properties) of the absorbing film 13 are substantially equal to the physical properties of the Cr-containing layer 13A. The thickness of the oxide layer 13B is more preferably 4 nm or less. The thickness of the oxide layer 13B is preferably 0.1 nm or more.
[0063] The method for forming the absorbing film 13 is, for example, a DC sputtering method, a magnetron sputtering method, an ion beam sputtering method, or the like. 2 The nitrogen content of the absorbing film 13 can be controlled by adjusting the gas content. 2 The oxygen content of the absorbing film 13 can be controlled by adjusting the gas content.
[0064] When a RuCrN film is formed by reactive sputtering, an example of the film formation conditions is as follows: <Formation conditions for RuCrN film> Target: Ru target and Cr target, Output density of Ru target: 1.0 W / cm 2 ~8.5 W / cm 2 , Cr target power density: 1.0 W / cm 2 ~8.5 W / cm 2 , Sputtering gas: Ar gas and N2 Gas mixture, N in sputtering gas 2 Gas volume ratio (N 2 / (Ar+N 2 )): 0.01 to 0.25, Film formation rate: 0.020 nm / sec to 0.060 nm / sec, Film thickness: 20 nm to 60 nm.
[0065] The hard mask film 14 is formed on the opposite side of the protective film 12 with respect to the absorbing film 13, and is used to form an opening pattern 13a in the absorbing film 13. The hard mask film 14 enables the resist film 16 to be made thinner.
[0066] The hard mask film 14 preferably contains at least one element selected from Al, Hf, Y, Cr, Nb, Ti, Mo, Ta, and Si. The hard mask film 14 may further contain at least one element selected from O, N, C, and B.
[0067] The thickness of the hard mask film 14 is preferably 2 nm or more and 30 nm or less, more preferably 2 nm or more and 25 nm or less, and even more preferably 2 nm or more and 10 nm or less.
[0068] The hard mask film 14 may be formed by, for example, DC sputtering, magnetron sputtering, or ion beam sputtering.
[0069] The experimental data will be explained below. In Examples 1 to 7, a reflective mask blank 1 was fabricated having a substrate 10, a multilayer reflective film 11, a protective film 12, and an absorbing film 13 in this order. In Examples 1 to 7, reflective mask blanks 1 were fabricated having the same configuration except for the configuration of the absorbing film 13. Examples 1 to 3 are working examples, and Examples 4 to 7 are comparative examples.
[0070] The substrate 10 is made of SiO 2 -TiO 2 A glass substrate (6-inch (152 mm) square outer diameter, 6.3 mm thick) was prepared. This glass substrate had a thermal expansion coefficient of 0.02×10 at 20° C. -7 / °C, Young's modulus is 67 GPa, Poisson's ratio is 0.17, and specific rigidity is 3.07 × 10 7 m 2 / s2 The quality assurance area of the first main surface 10a of the substrate 10 was polished to a root-mean-square roughness (Rq) of 0.15 nm or less and a flatness of 100 nm or less. A 100 nm-thick Cr film was formed on the second main surface 10b of the substrate 10 using magnetron sputtering. The sheet resistance of the Cr film was 100 Ω / □.
[0071] A Mo / Si multilayer reflective film was formed as the multilayer reflective film 11. The Mo / Si multilayer reflective film was formed by repeating the deposition of a Si layer (4.5 nm thick) and a Mo layer (2.3 nm thick) 40 times using an ion beam sputtering method. The total thickness of the Mo / Si multilayer reflective film was 272 nm ((4.5 nm + 2.3 nm) × 40).
[0072] A Rh film (thickness: 5 nm) was formed as the protective film 12. The Rh film was formed by ion beam sputtering.
[0073] The Cr-containing layer shown in Table 1 was formed as the absorbing film 13. The Cr-containing layer was formed using a dual-target sputtering method. The chemical composition of the Cr-containing layer was measured using an X-ray photoelectron spectrometer (PHI 5000 VersaProbe) manufactured by ULVAC-PHI, Inc. The thicknesses of the Cr-containing layer and oxide layer were measured by X-ray reflectivity. The surface of the Cr-containing layer is naturally oxidized in the atmosphere to form an oxide layer, and the thickness of the oxide layer was 5 nm or less.
[0074] The experimental conditions and results of Examples 1 to 7 are shown in Table 1. The relative reflectance Ra was determined by calculating the reflectances R1 and R2 using the optical simulation described in "Experimental Approach to EUV Imaging Enhancement by Mask Absorber Height Optimization (2013)" (authors: N. Davydova, R. Kruif, H. Rolff, B. Connolly, E. Setten, A. Lammers, D. Oorschot, N. Fukugami, Y. Kodera). The thickness of the oxide layer is sufficiently small, so the relative reflectance Ra is approximately the same even if the oxide layer is present.
[0075]
[0076] As shown in Table 1, in Examples 1 to 3, unlike Examples 4 to 7, the Cr-containing layer was formed of a CrN compound containing 50 at% or more of Cr and 10 at% or more of N. As a result, in Examples 1 to 3, it was possible to obtain absorbing films having a refractive index of 0.920 to 0.940, an extinction coefficient of 0.032 to 0.044, good amorphousness, and a relative reflectance of less than 5%.
[0077] The reflective mask blank, reflective mask, reflective mask blank manufacturing method, and reflective mask manufacturing method according to the present disclosure have been described above, but the present disclosure is not limited to the above-described embodiments. Various changes, modifications, substitutions, additions, deletions, and combinations are possible within the scope of the claims. These naturally fall within the technical scope of the present disclosure.
[0078] This application claims priority based on Japanese Patent Application No. 2023-090180 filed with the Japan Patent Office on May 31, 2023, the entire contents of which are incorporated herein by reference.
[0079] REFERENCE SIGNS LIST 1 reflective mask blank 2 reflective mask 10 substrate 11 multilayer reflective film 12 protective film 13 absorbing film
Claims
1. A reflective mask blank having a substrate, a multilayer reflective film, a protective film, and an absorbing film in this order, wherein the multilayer reflective film reflects EUV light, the protective film protects the multilayer reflective film during processing of the absorbing film, and the absorbing film absorbs EUV light, the absorbing film has a Cr-containing layer made of a CrN compound containing 50 at% or more of Cr and 10 at% or more of N, and the Cr-containing layer has a full width at half maximum of the highest intensity peak in the 2θ range of 20° to 50° of 1.0° or more as measured by XRD using CuKα radiation, and the ratio of the reflectance of EUV light reflected by the multilayer reflective film and the protective film to the opposite side of the substrate via the absorbing film to the reflectance of EUV light reflected by the multilayer reflective film and the protective film to the opposite side of the substrate without the absorbing film being passed through the absorbing film is less than 5%.
2. The reflective mask blank according to claim 1, wherein the CrN compound further contains Ru, the Ru content of the CrN compound is 25 at % or less, and the extinction coefficient of the Cr-containing layer is 0.032 or more.
3. A reflective mask blank according to claim 1 or 2, wherein the refractive index of the Cr-containing layer is 0.920 or more and 0.940 or less.
4. The reflective mask blank according to claim 1 or 2, wherein the Cr-containing layer has a thickness of 20 nm to 60 nm.
5. A reflective mask blank according to claim 1 or 2, wherein the absorbing film has an oxide layer made of an oxide on the opposite side of the protective film with respect to the Cr-containing layer, and the thickness of the oxide layer is 5 nm or less.
6. The reflective mask blank according to claim 1 or 2, wherein the protective film contains at least one element selected from the group consisting of Ru, Rh and Si.
7. A reflective mask comprising the reflective mask blank according to claim 1 or 2, and comprising an aperture pattern in the absorbing film.
8. A method for manufacturing a reflective mask blank, comprising: forming a multilayer reflective film, a protective film, and an absorbing film in this order on a substrate, wherein the multilayer reflective film reflects EUV light, the protective film protects the multilayer reflective film during processing of the absorbing film, and the absorbing film absorbs EUV light, the absorbing film has a Cr-containing layer made of a CrN compound containing 50 at% or more of Cr and 10 at% or more of N, and the Cr-containing layer has a full width at half maximum of the highest intensity peak in a 2θ range of 20° to 50° of 1.0° or more as measured by XRD using CuKα radiation, and the ratio of the reflectance of EUV light reflected by the multilayer reflective film and the protective film to the opposite side of the substrate via the absorbing film to the reflectance of EUV light reflected by the multilayer reflective film and the protective film to the opposite side of the substrate without the absorbing film is less than 5%.
9. A method for manufacturing a reflective mask, comprising the steps of: preparing a reflective mask blank according to claim 1 or 2; and forming an aperture pattern in the absorbing film, in this order.
Citation Information
Patent Citations
Reflective mask blank and method for manufacturing reflective mask
JP2010206156A
Reflective mask blank for EUV lithography, substrate with function film for the mask blank, and methods for their production
JP2015215602A
Reflective mask blank for EUV lithography, reflective mask for EUV lithography and their manufacturing method
JP2022024617A
Reflective mask blank, reflective mask, method for manufacturing a reflective mask blank, and method for manufacturing a reflective mask
JP7272519B1
Phase shift mask for extreme ultraviolet lithography and a method of manufacturing a semiconductor device using the same
US20210389662A1