Substrate processing method and substrate processing system
The substrate processing method and system efficiently remove the peripheral edge of bonded semiconductor wafers by forming a bonding force reduced region, addressing the inefficiencies of conventional methods like laser ablation.
Patent Information
- Application Number
- PCT/JP2024/018100
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2024-05-16
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional edge trim methods for semiconductor wafers, particularly laser ablation, are time-consuming and inefficient in removing the peripheral edge of bonded substrates.
A substrate processing method and system that forms a bonding force reduced region between the substrates by creating a first and second peripheral edge modified region using a laser, allowing for efficient removal of the peripheral edge without the need for two-step processes like laser ablation.
Enables efficient and appropriate edge trimming of semiconductor wafers by forming a bonding force reduced region, eliminating the need for two-step processes and reducing processing time.
Smart Images

Figure JP2024018100_05122024_PF_FP_ABST
Abstract
Description
Substrate processing method and substrate processing system
[0001] The present disclosure relates to a substrate processing method and a substrate processing system.
[0002] Patent Document 1 discloses a method for treating a laminated substrate in which a first substrate and a second substrate are bonded together. The method includes cutting a peripheral portion of the first substrate from above to a thickness less than the total thickness of the first substrate so as to leave a cutting remainder of a desired thickness, and irradiating the cutting remainder at the peripheral portion of the first substrate with laser light to remove the cutting remainder.
[0003] JP 2022-71480 A
[0004] The technology according to the present disclosure appropriately removes the peripheral edge portion of the first substrate to be removed in a laminated substrate in which a first substrate and a second substrate are bonded together.
[0005] One aspect of the present disclosure is a substrate processing method for processing an overlapped substrate in which a first substrate and a second substrate are bonded, the method including: forming a first peripheral modified region inside the first substrate along the boundary between a peripheral portion and a central portion of the first substrate to be removed; forming a second peripheral modified portion radially inside the first substrate, at least radially outward from the first peripheral modified region; forming a reduced bonding strength region in which bonding strength is reduced, radially outward from the first peripheral modified region, in the bonding region between the first substrate and the second substrate, by forming the second peripheral modified region; and removing the peripheral portion based on the first peripheral modified region and the reduced bonding strength region.
[0006] According to the present disclosure, in a laminated substrate in which a first substrate and a second substrate are bonded together, the peripheral edge portion of the first substrate to be removed can be appropriately removed.
[0007] FIG. 1 is an explanatory diagram of overlapping wafers to be processed; FIG. 2 is a plan view showing an outline of the configuration of a wafer processing system; FIG. 3 is a plan view showing an outline of the configuration of a modification device; FIG. 4 is a side view showing an outline of the configuration of a modification device; FIG. 5 is an explanatory diagram showing how a first peripheral modified region and a second peripheral modified portion are formed in wafer processing; FIG. 6 is an explanatory diagram showing how a second peripheral modified portion is formed in wafer processing; FIG. 7 is an explanatory diagram showing how a first peripheral modified region is formed in wafer processing; FIG. 8 is an explanatory diagram showing how a peripheral portion is removed in wafer processing; and FIG. 9 is an explanatory diagram showing how a first peripheral modified region is formed in another embodiment.
[0008] In the manufacturing process of semiconductor devices, a first wafer, which is a semiconductor substrate (hereinafter referred to as "wafer") having a plurality of devices such as electronic circuits formed on its surface, is bonded to a second wafer to form a laminated wafer, and the first wafer is thinned. Before the thinning process of the first wafer, a process called edge trimming is performed to remove the peripheral portion of the first wafer.
[0009] The edge trimming of the first wafer is performed, for example, by the processing method disclosed in Patent Document 1. As described above, in this processing method, the peripheral edge of the first substrate is cut from above, and then the remaining portion of the peripheral edge of the first substrate is irradiated with laser light to remove the remaining portion by laser ablation. However, removing the peripheral edge in two steps like this, especially laser ablation, is time-consuming, and conventional edge trimming has room for improvement.
[0010] The technology disclosed herein appropriately removes a peripheral portion of a first substrate to be removed in a laminated substrate formed by bonding a first substrate and a second substrate. Hereinafter, a wafer processing system as a substrate processing system and a wafer processing method as a substrate processing method according to the present embodiment will be described with reference to the drawings. Note that in this specification and the drawings, elements having substantially the same functional configurations are designated by the same reference numerals, and redundant description will be omitted.
[0011] 1 , a wafer processing system 1 according to this embodiment, which will be described later, processes a laminated wafer T as a laminated substrate in which a first wafer W as a first substrate and a second wafer S as a second substrate are bonded together. Hereinafter, the surface of the first wafer W that is bonded to the second wafer S will be referred to as the front surface Wa, and the surface opposite the front surface Wa will be referred to as the back surface Wb. Similarly, the surface of the second wafer S that is bonded to the first wafer W will be referred to as the front surface Sa, and the surface opposite the front surface Sa will be referred to as the back surface Sb.
[0012] The first wafer W is a semiconductor wafer such as a silicon substrate, and at least one film is laminated on the front surface Wa side. Hereinafter, the film formed on the front surface Wa side will be referred to as the "first laminated film." In this embodiment, the first laminated film includes a device layer Dw and a bonding film Fw. The device layer Dw includes a plurality of devices. The bonding film Fw may include, for example, an oxide film (THOX film, SiO 2 A bonding film Fw, such as a TEOS film, a SiC film, a SiCN film, or an adhesive, is used. The first wafer W is bonded to the second wafer S via the bonding film Fw. The peripheral edge We of the first wafer W is chamfered, and the thickness of the cross section of the peripheral edge We decreases toward its tip. The peripheral edge We is a portion to be removed in the edge trimming process described below, and is, for example, in a range of 0.5 mm to 3 mm in the radial direction from the outer edge of the first wafer W. In the following description, the region of the first wafer W that is radially inward of the peripheral edge We to be removed may be referred to as the central portion Wc.
[0013] The second wafer S has, for example, the same configuration as the first wafer W. That is, a device layer Ds and a bonding film Fs are formed as a second laminated film on the surface Sa side, and the peripheral portion is chamfered. Note that the second wafer S does not necessarily have to be a device wafer on which the device layer Ds is formed, and may be, for example, a support wafer that supports the first wafer W. In such a case, the second wafer S functions as a protective material that protects the device layer Dw of the first wafer W.
[0014] In the following description, the bonding region refers to each interlayer between the first wafer W and the second wafer S. That is, in this embodiment, the bonding region refers to the surface Wa, the area between the device layer Dw and the bonding film Fw, the area between the bonding film Fw and the bonding film Fs, the area between the bonding film Fs and the device layer Ds, and the surface Sa.
[0015] 1 illustrates an example in which device layers Dw, Ds and bonding films Fw, Fs are formed as first and second laminated films on the surfaces Wa, Sa of the first wafer W and the second wafer S. However, the types and numbers of layers of the first and second laminated films are not limited to this.
[0016] 2 , wafer processing system 1 has a configuration in which a load / unload station 2 and a processing station 3 are integrally connected. In load / unload station 2, for example, a cassette C capable of accommodating a plurality of overlapped wafers T is loaded and unloaded between the load / unload station 2 and the outside. Processing station 3 is equipped with various processing devices that perform desired processing on overlapped wafers T.
[0017] The carry-in / out station 2 is provided with a cassette mounting table 10 on which a cassette C capable of accommodating a plurality of overlapped wafers T is mounted. A wafer transfer device 20 is provided adjacent to the cassette mounting table 10 on the positive side of the X-axis of the cassette mounting table 10. The wafer transfer device 20 moves on a transfer path 21 extending in the Y-axis direction, and is configured to be able to transfer the overlapped wafers T between the cassette C on the cassette mounting table 10 and a transition device 30, which will be described later.
[0018] In the loading / unloading station 2 , a transition device 30 for transferring the overlapped wafer T between the processing station 3 and the wafer transfer device 20 is provided adjacent to the wafer transfer device 20 on the positive side of the X axis of the wafer transfer device 20 .
[0019] The processing station 3 is provided with a wafer transfer device 40, a modifying device 50, a peripheral edge removing device 60, and a cleaning device .
[0020] The wafer transfer device 40 is provided on the positive X-axis side of the transition device 30. The wafer transfer device 40 is configured to be movable on a transfer path 41 extending in the X-axis direction, and is configured to be able to transfer the overlapped wafer T to the transition device 30, the modification device 50, the edge removal device 60, and the cleaning device 70 in the carry-in / out station 2.
[0021] The modifying device 50 irradiates the inside of the first wafer W with a modifying laser beam (e.g., a YAG laser or a fiber laser) to form a modified peripheral region and a reduced bonding strength region that serve as a base point for peeling off the peripheral edge We. The modifying device 50 also has a control device 51, which will be described later.
[0022] As shown in FIGS. 3 and 4 , the modification apparatus 50 includes a chuck 100 that holds the overlapped wafer T on its upper surface. The chuck 100 suction-holds the back surface Sb of the second wafer S, with the first wafer W on top and the second wafer S on the bottom. The chuck 100 is supported by a slider table 102 via an air bearing 101. A rotation mechanism 103 is provided on the underside of the slider table 102. The rotation mechanism 103 incorporates, for example, a motor as a drive source. The chuck 100 is configured to be rotatable about a vertical axis by the rotation mechanism 103 via the air bearing 101. The slider table 102 is configured to be movable on rails 106 extending in the Y-axis direction on a base 105 via a movement mechanism 104 provided on the underside of the slider table 102. The drive source of the movement mechanism 104 is not particularly limited, but may be, for example, a linear motor.
[0023] A laser head 110 is provided above the chuck 100. The laser head 110 has a lens 111. The lens 111 is a cylindrical member provided on the lower surface of the laser head 110, and irradiates the inside of the overlapped wafer T held by the chuck 100, more specifically, the inside of the first wafer W, with laser light.
[0024] The laser head 110 is supported by a support member 112. The laser head 110 is configured to be able to move up and down by an elevating mechanism 114 along rails 113 extending in the vertical direction. The laser head 110 is also configured to be able to move in the Y-axis direction by a moving mechanism 115. The elevating mechanism 114 and the moving mechanism 115 are each supported by a support column 116.
[0025] An imaging mechanism 120 is provided above the chuck 100 on the Y-axis positive side of the laser head 110. The imaging mechanism 120 includes at least one camera. Images captured by the camera are output to a control device 51 or a control device 80, which will be described later. The modification device 50 determines the position of the overlapped wafer T on the chuck 100 based on the image obtained by the imaging mechanism 120, and then aligns the overlapped wafer T and determines the irradiation position of the laser light based on this. The imaging mechanism 120 is configured to be able to move up and down freely by an elevating mechanism 121, and is further configured to be able to move freely in the Y-axis direction by a moving mechanism 122. The moving mechanism 122 is supported by a support column 116.
[0026] In the illustrated example, the chuck 100 is configured to be rotatable relative to the laser head 110 and movable horizontally by the rotation mechanism 103 and the movement mechanism 104, but the laser head 110 may be configured to be rotatable relative to the chuck 100 and movable horizontally. Alternatively, both the chuck 100 and the laser head 110 may be configured to be rotatable relative to each other and movable horizontally.
[0027] The edge removal device 60 shown in FIG. 2 removes the edge portion We of the first wafer W, i.e., performs edge trimming, using the modified edge region and the reduced bonding strength region formed by the modification device 50 as starting points. The edge trimming method can be selected arbitrarily. In one example, the edge removal device 60 may insert, for example, a wedge-shaped blade between the first wafer W and the second wafer S. Alternatively, for example, an impact may be applied to the edge portion We by spraying air or a water jet toward the edge portion We. Alternatively, for example, an impact may be applied to the edge portion We by applying ultrasonic waves to the edge portion We. Furthermore, for example, the edge portion We may be physically moved in a direction away from the center portion We.
[0028] The cleaning device 70 performs a cleaning process on the first wafer W and the second wafer S after the edge trimming by the edge removal device 60, thereby removing particles from these wafers. Any cleaning method can be selected.
[0029] The wafer processing system 1 described above is provided with a control device 51 and at least one control device 80. The control device 51 individually controls the operation of each of the modifying devices 50. The control device 80 comprehensively controls a series of wafer processing operations in the wafer processing system 1.
[0030] Controller 51 and controller 80 each process computer-executable instructions that cause reformer 50 and wafer processing system 1 to perform the various steps described in this disclosure. Controller 51 and controller 80 can be configured to control elements of reformer 50 and wafer processing system 1 to perform the various steps described herein. In one embodiment, some or all of controller 51 can be included in reformer 50, and some or all of controller 80 can be included in wafer processing system 1.
[0031] The control device 51 and the control device 80 may each include a processing unit, a storage unit, and a communication interface. The control device 51 and the control device 80 may each be realized by, for example, a computer. The processing unit may be configured to read a program providing logic or routines that enable various control operations from the storage unit and execute the read program to perform various control operations. This program may be stored in the storage unit in advance or may be acquired via a medium when needed. The acquired program is stored in the storage unit and read from the storage unit and executed by the processing unit. The medium may be various computer-readable storage media or a communication line connected to the communication interface. The storage medium may be temporary or non-temporary. The processing unit may be a CPU (Central Processing Unit) or one or more circuits. The storage unit may include a RAM (Random Access Memory), a ROM (Read Only Memory), a HDD (Hard Disk Drive), a SSD (Solid State Drive), or a combination thereof. The communication interface may communicate between the modifying apparatus 50 and the wafer processing system 1 via a communication line such as a LAN (Local Area Network).
[0032] In this embodiment, the control device 51 is installed separately from the reformer 50, but the control device 51 may be configured integrally with the control device 80. In other words, the operation of the reformer 50 may be controlled by the control device 80.
[0033] Next, wafer processing performed using the wafer processing system 1 configured as above will be described.
[0034] In this embodiment, before being processed in the wafer processing system 1, the first wafer W and the second wafer S are bonded together outside the wafer processing system 1 to form a laminated wafer T in advance.
[0035] In this embodiment, after processing in the wafer processing system 1, a process for thinning the central portion Wc of the first wafer W is performed outside the wafer processing system 1. The process for thinning the first wafer W is optional. Note that a thinning device for thinning the central portion Wc of the first wafer W, such as a grinding device (not shown), may be provided outside the wafer processing system 1 as in this embodiment, or may be installed in the wafer processing system 1.
[0036] First, a cassette C containing a plurality of overlapping wafers T is placed on the cassette mounting table 10 of the carry-in / out station 2. Next, the overlapping wafers T are removed from the cassette C by the wafer transfer device 20 and transferred to the modification device 50 via the transition device 30 and the wafer transfer device 40.
[0037] 5 to 7, the modification device 50 irradiates the interior of the first wafer W with a modification laser beam L to form a first peripheral modified region M1 and a second peripheral modified region M2 in the circumferential direction in a plan view. In this embodiment, the second peripheral modified region M2 is formed, and then the first peripheral modified region M1 is formed.
[0038] 5 and 6, laser light L is irradiated in the surface direction (radial direction) inside the first wafer W at least radially outward from a first peripheral modified region N1 (first peripheral modified portion M1 and first crack C1) described below, i.e., at the peripheral portion We, to form a second peripheral modified portion M2. In this case, the second peripheral modified portion M2 may be formed from the radially outer side to the radially inner side, or from the radially inner side to the radially outer side.
[0039] The second peripheral modified region M2 is formed in the vicinity of the front surface Wa of the first wafer W. Specifically, the distance H in the thickness direction between the second peripheral modified region M2 and the front surface Wa is, for example, within 20 μm.
[0040] Furthermore, adjacent second peripheral modified regions M2 are not connected to each other. In other words, cracks from the second peripheral modified regions M2 do not reach adjacent second peripheral modified regions M2. To prevent the second peripheral modified regions M2 from connecting to each other in this manner, one or both of the spacing of the laser light L irradiated onto the interior of the first wafer W and the intensity of the laser light L are controlled. The lower limit of the spacing of the laser light L, i.e., the spacing P between the second peripheral modified regions M2, is a spacing at which cracks do not connect between adjacent second peripheral modified regions M2, and the upper limit of the spacing P is a spacing at which a bonding strength reduction region R, described below, can be formed. The spacing P is, for example, 30 μm to 80 μm.
[0041] In this case, the second peripheral modified region M2 expands, causing compressive stress to act, and tensile stress to act in region Q1 above the second peripheral modified region M2 and region Q2 below the second peripheral modified region M2. That is, tensile stress accumulates in these regions Q1 and Q2, and tensile stress acts on the front surface Wa of the first wafer W. As a result, compressive stress acts on the upper portion of the first wafer W (the portion above the second peripheral modified region M2) such that the upper portion of the first wafer W warps obliquely upward so as to peel off the peripheral region We (arrows in FIG. 6 ).
[0042] Here, between the first wafer W and the second wafer S, the bonding region between the first and second stacked films, i.e., the bonding region between the bonding film Fw and the bonding film Fs, is the most susceptible to peeling because an unbonded region is formed radially outside this bonding region. In such a case, tensile stress acts on the bonding region between the bonding film Fw and the bonding film Fs in response to the compressive stress (warpage) in the upper portion of the first wafer W described above, reducing the bonding strength of the bonding region and forming a bonding strength reduced region R. This bonding strength reduced region R extends between the first peripheral modified region N1 (described later) and the outer edge portion.
[0043] If adjacent second peripheral modified regions M2 were connected by a crack, the compressive stress would be released, no tensile stress would act on the surface Wa of the first wafer W, and the bonding strength reduced region R would be unlikely to be formed. The bonding strength would then be reduced in the region formed by the second peripheral modified region M2 and the crack, resulting in removal of the peripheral region We from this region. In this regard, according to the present embodiment, the second peripheral modified regions M2 are not connected to each other, so the bonding strength reduced region R is more likely to be formed outside the first wafer W, and the bonding strength reduced region R is removed from this region.
[0044] Furthermore, in this embodiment, since the second peripheral modification portion M2 is formed near the surface Wa of the first wafer W, the tensile stress acting on the surface Wa of the first wafer W increases, making it even more likely that the bonding strength reduction region R will be formed.
[0045] Note that, if the tensile stress acting on the bonding strength reduced region R becomes large, a part of the bonding region between the bonding film Fw and the bonding film Fs may peel off. Even in such a case, by controlling the laser light L irradiated into the interior of the first wafer W, the bonding strength reduced region R is formed so as to extend radially outward from the first peripheral modified region N1.
[0046] Next, as shown in FIGS. 5 and 7 , laser light L is irradiated into the first wafer W along the boundary between the peripheral edge portion We and the central portion We of the first wafer W to form a first peripheral modified region M1. The boundary between the peripheral edge portion We and the central portion We is, for example, a boundary extending in the thickness direction of the first wafer W. When the first peripheral modified region M1 is formed, a first crack C1 extends from the first peripheral modified region M1 along the boundary between the peripheral edge portion We and the central portion We. The first crack C1 extends to the bonding region between the bonding film Fw and the bonding film Fs. Then, a first peripheral modified region N1 including the first peripheral modified region M1 and the first crack C1 is formed. The first peripheral modified region N1 extends between the back surface Wb of the first wafer W and the bonding region between the bonding film Fw and the bonding film Fs.
[0047] When the first peripheral modified region N1 is formed, the compressive stress in the upper portion of the first wafer W is released, and the tensile stress in the bonding strength reduced region R is released. At this time, in the bonding strength reduced region R, the tensile stress is released, for example, from the radially outer side toward the radially inner side (toward the first peripheral modified region N1). As a result, the bonding film Fw and the bonding film Fs peel off in the bonding strength reduced region R. The peeling in the bonding strength reduced region R progresses to the first peripheral modified region N1, and the bonding strength reduced region R and the first peripheral modified region N1 are connected. The first peripheral modified region N1 and the bonding strength reduced region R then serve as the starting point for removing the peripheral portion We.
[0048] The overlapped wafer T with the first peripheral modified region N1 and the bonding strength reduced region R formed thereon is then transferred by the wafer transfer device 40 to the peripheral removal device 60. In the peripheral removal device 60, a blade B is inserted between the first wafer W and the second wafer S, as shown in Fig. 8, and the peripheral portion We is removed from the first wafer W. At this time, the peripheral portion We is peeled and removed from the central portion We of the first wafer W, using the first peripheral modified region N1 and the bonding strength reduced region R as base points.
[0049] The overlapped wafer T from which the peripheral edge portion We of the first wafer W has been removed is then transferred by the wafer transfer device 40 to the cleaning device 70. In the cleaning device 70, the first wafer W and / or the second wafer S from which the peripheral edge portion We has been removed are cleaned.
[0050] Thereafter, the overlapped wafer T that has been subjected to all the processes is transferred by the wafer transfer device 20 to the cassette C on the cassette mounting table 10 via the transition device 30. In this way, a series of wafer processes in the wafer processing system 1 is completed.
[0051] According to the above embodiment, a bonding strength reduction region R is formed in the bonding region between the bonding film Fw and the bonding film Fs, and the peripheral portion We is removed starting from the first peripheral modified region N1 and the bonding strength reduction region R. Therefore, no part of the first wafer W remains radially outside the first peripheral modified region N1 (peripheral portion We). Therefore, there is no need to remove the peripheral portion We in two stages as in the conventional method, and in particular, removal by laser ablation is not required. As a result, edge trimming can be performed appropriately and efficiently.
[0052] In the above embodiment, the reforming apparatus 50 forms the second peripheral modified region M2 and then the first peripheral modified region N1 (first peripheral modified region M1). However, the order in which the second peripheral modified region M2 and the first peripheral modified region N1 are formed is not limited to this. For example, the second peripheral modified region M2 may be formed after the first peripheral modified region N1 is formed. Even in such a case, by not connecting adjacent second peripheral modified regions M2, the effect of performing the edge trimming described above appropriately and efficiently can be achieved.
[0053] In the above embodiment, the second peripheral modified region M2 is formed radially outward from the first peripheral modified region N1, but it may also be formed radially inward from the first peripheral modified region N1. Even in this case, the bonding strength reduction region R can be formed to appropriately and efficiently remove the peripheral portion We.
[0054] However, the second peripheral modified region M2 is formed near the front surface Wa of the first wafer W. Therefore, for example, if the second peripheral modified region M2 is formed above the thinning surface (the surface to be thinned) when thinning the central region Wc of the first wafer W, there is a risk that the second peripheral modified region M2 will remain in the central region Wc of the first wafer W after thinning. For this reason, the second peripheral modified region M2 is preferably formed radially outward of the first peripheral modified region N1.
[0055] In the above embodiment, the first peripheral modified region N1 extended from the back surface Wb of the first wafer W to the bonding region between the bonding film Fw and the bonding film Fs. However, the first peripheral modified region N1 may extend from the back surface Wb of the first wafer W to the bonding region (front surface Wa) between the first wafer W and the bonding film Fw. The lower end position to which the first peripheral modified region N1 extends depends on the adhesion between the first wafer W and the bonding film Fw. When the first peripheral modified region M1 is formed inside the first wafer W, the first peripheral modified region M1 expands and compressive stress acts on the first peripheral modified region M1. Then, for example, when the adhesion between the first wafer W and the bonding film Fw is strong, the compressive stress is transmitted to the bonding film Fw, and the first crack C1 extends to the bonding region between the bonding film Fw and the bonding film Fs. On the other hand, for example, when the adhesion between the first wafer W and the bonding film Fw is small, the compressive stress remains inside the first wafer W, and the extension of the first crack C1 stops at the surface Wa of the first wafer W.
[0056] In the above embodiments, the bonding strength reduced region R is formed in the bonding region between the bonding film Fw and the bonding film Fs, but it may also be formed in the bonding region (front surface Wa) between the first wafer W and the bonding film Fw. The position where the bonding strength reduced region R is formed depends on the adhesion between the first wafer W and the bonding film Fw. For example, when the adhesion between the first wafer W and the bonding film Fw is strong, the bonding strength reduced region R is formed in the bonding region between the bonding film Fw and the bonding film Fs. On the other hand, when the adhesion between the first wafer W and the bonding film Fw is weak, the bonding strength reduced region R is formed on the front surface Wa of the first wafer W.
[0057] 9, the first peripheral modified region N1 may be formed in an oblique direction along the crystal orientation of the silicon of the first wafer W. For example, the 111 crystal orientation of silicon is at an angle of approximately 70 degrees from the horizontal, and the first peripheral modified region N1 is formed along this 111 crystal orientation.
[0058] Here, when inserting blade B into edge removal device 60, if the insertion force or insertion amount of blade B is increased to properly remove edge portion We, a crack may occur from the radially inner tip of second edge modification portion M2, causing separation between the first wafer W and the second wafer S.
[0059] In this regard, by forming the first peripheral modified region N1 along the crystal orientation as in this example, the peripheral portion We can be easily removed in the first peripheral modified region N1. As a result, the insertion force and insertion depth of the blade B when removing the peripheral portion We can be reduced, thereby suppressing the above-mentioned peeling.
[0060] In the above embodiment, the second peripheral modified region M2 is formed in the surface direction of the first wafer W, but the formation direction of the second peripheral modified region M2 is not limited to this. As described above, it is sufficient that adjacent second peripheral modified regions M2 are not connected to each other. For example, the second peripheral modified region M2 may be formed in a direction oblique to the surface direction of the first wafer W. In this case, the second peripheral modified region M2 may be formed, for example, so as to descend from the radially inner side to the radially outer side.
[0061] 9, the second peripheral modified region M2 may be formed in multiple layers by stacking them in the thickness direction of the first wafer W. In this case, the tensile stress in the bonding strength reduction region R can be increased while preventing cracks from connecting between adjacent second peripheral modified regions M2. In this case, the upper and lower second peripheral modified regions M2 may be formed alternately so that they do not overlap in a plan view. In this case, it is possible to further prevent cracks from connecting between adjacent second peripheral modified regions M2 in the thickness direction. Note that, although two layers of the second peripheral modified region M2 are formed in the illustrated example, the number of layers of the second peripheral modified region M2 is not limited to this.
[0062] In the above embodiment, the first peripheral modified region N1 (first peripheral modified portion M1) and the second peripheral modified portion M2 were formed in the reforming device 50, but these first peripheral modified region N1 and second peripheral modified portion M2 may also be formed in a different reforming device.
[0063] In the above embodiment, the modification apparatus 50 forms the first peripheral modified region N1 and the second peripheral modified portion M2. However, it may also form multiple divided modified regions that serve as base points for dividing the peripheral portion We into smaller pieces. Each divided modified region extends in the thickness direction of the first wafer W, radially outward of the first peripheral modified region N1. Specifically, a divided modified region is formed by irradiating the first wafer W with laser light L in the thickness direction, and a crack is then propagated from the divided modified region in the thickness direction of the first wafer W to form a divided modified region including the divided modified region and the crack. By forming multiple divided modified regions in the radial direction, a line of divided modified regions extending radially outward from the first peripheral modified region N1 is formed, and multiple lines of the same line are further formed in the circumferential direction. In such a case, when the peripheral edge removing device 60 removes the peripheral edge We, the peripheral edge We is divided into a plurality of small pieces, starting from the divided modified regions of the plurality of lines.
[0064] The embodiments disclosed herein should be considered to be illustrative in all respects and not restrictive. The above-described embodiments may be omitted, substituted, or modified in various ways without departing from the scope and spirit of the appended claims. For example, the components of the above-described embodiments may be arbitrarily combined. Such an arbitrary combination naturally provides the functions and effects of each of the components involved in the combination, and also provides other functions and effects that are apparent to those skilled in the art from the description of this specification.
[0065] Furthermore, the effects described herein are merely descriptive or exemplary and are not limiting. In other words, the technology according to the present disclosure may achieve other effects that are apparent to those skilled in the art from the description of this specification, in addition to or in place of the above-described effects.
[0066] REFERENCE SIGNS LIST 1 wafer processing system 50 modification device 60 edge removal device 80 control device M2 second edge modification section N1 first edge modification region R bonding strength reduction region S second wafer T overlapping wafer W first wafer Wc central portion We edge portion
Claims
1. A substrate processing method for processing an overlapped substrate formed by bonding a first substrate and a second substrate, comprising: forming a first peripheral modified region within the first substrate along a boundary between a peripheral portion and a central portion of the first substrate to be removed; forming a second peripheral modified portion radially within the first substrate, at least radially outward from the first peripheral modified region; forming a reduced bonding strength region in which bonding strength is reduced, radially outward from the first peripheral modified region, in the bonding region between the first substrate and the second substrate by forming the second peripheral modified region; and removing the peripheral portion based on the first peripheral modified region and the reduced bonding strength region.
2. The substrate processing method according to claim 1, wherein when the second peripheral modified regions are formed, adjacent second peripheral modified regions are not connected to each other.
3. The substrate processing method according to claim 2, further comprising controlling at least the interval or intensity of laser light irradiated radially inside the first substrate when forming the second peripheral modified portion.
4. The substrate processing method according to claim 1, wherein the second peripheral modification portion is formed by laminating in a thickness direction of the first substrate.
5. The substrate processing method according to claim 4, wherein when the second peripheral modification portion is formed, the second peripheral modification portion of the upper layer and the second peripheral modification portion of the lower layer do not overlap in a planar view.
6. The substrate processing method according to claim 1, wherein the reduced bonding strength region is formed in a bonding region between a first laminate film formed on the surface of the first substrate and a second laminate film formed on the surface of the second substrate.
7. A substrate processing method as described in claim 6, wherein the first peripheral modified region includes a first peripheral modified portion and a first crack extending from the first peripheral modified portion, and the first peripheral modified region extends to a junction region between the first stack film and the second stack film.
8. The substrate processing method according to claim 1, wherein the first peripheral modified region and the region of reduced adhesion are connected, and the region of reduced adhesion is formed by peeling off the bonding region.
9. A substrate processing system for processing an overlapped substrate formed by bonding a first substrate and a second substrate, comprising: a modification device that forms a first peripheral modified region inside the first substrate along a boundary between a peripheral portion and a central portion of the first substrate to be removed, and forms a second peripheral modified portion radially inside the first substrate at least radially outside the first peripheral modified region; a peripheral removal device that removes the peripheral portion based on the first peripheral modified region and a region of reduced bonding strength; and a control device, wherein the control device executes control to form the bonding strength reduced region in which bonding strength is reduced, in the bonding region between the first substrate and the second substrate radially outside the first peripheral modified region, by forming the second peripheral modified portion.
10. The substrate processing system according to claim 9, wherein the control device executes control such that, when forming the second peripheral modified regions, adjacent second peripheral modified regions are not connected to each other.
11. The substrate processing system of claim 10, wherein the control device controls at least the interval or intensity of laser light irradiated radially inside the first substrate when forming the second peripheral modification portion.
12. The substrate processing system according to claim 9, wherein the control device executes control to form the second peripheral modified portion by lamination in a thickness direction of the first substrate.
13. The substrate processing system of claim 12, wherein the control device performs control such that, when forming the second peripheral modification portion, the second peripheral modification portion of an upper layer and the second peripheral modification portion of a lower layer do not overlap in a planar view.
14. The substrate processing system of claim 9, wherein the control device executes control to form the reduced bonding strength region in a bonding region between a first laminate film formed on the surface of the first substrate and a second laminate film formed on the surface of the second substrate.
15. A substrate processing system as described in claim 14, wherein the first peripheral modified region includes a first peripheral modified portion and a first crack extending from the first peripheral modified portion, and the control device performs control to extend the first peripheral modified region to a bonding region between the first stack film and the second stack film.
16. The substrate processing system of claim 9, wherein the control device executes control to connect the first peripheral modified region and the reduced bonding strength region, and control to form the reduced bonding strength region by peeling off the bonding region.
Citation Information
Patent Citations
Manufacture method of semiconductor device
CN108231646A
Laminated wafer grinding method
JP2022165203A
Processing method and processing system
JP2023003476A
Substrate processing system, substrate processing method, and computer storage medium
WO2019176589A1
Substrate processing device and substrate processing method
WO2020129732A1