Image-carrying laminate, method for manufacturing same, intermediate film for laminated glass, and laminated glass

The image-bearing laminate with surface-treated hydrophilic surfaces and strategically layered resins addresses the issue of interlayer peeling in laminated glass, maintaining image quality and adhesion, thus preventing delamination and ensuring long-term clarity and resolution.

WO2024247770A1PCT designated stage expired Publication Date: 2024-12-05SEKISUI CHEMICAL CO LTD

Patent Information

Application Number
PCT/JP2024/018407
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-05-17
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional laminated glass with image-bearing layers experiences interlayer peeling or delamination due to insufficient adhesion between the image-bearing layer and the intermediate film layer, leading to image quality degradation over time.

Method used

An image-bearing laminate is created with a cured product of curable ink on a first resin sheet, where the second surface is subjected to a surface treatment process to improve hydrophilicity, and optionally a second or third resin sheet is laminated to enhance adhesion, using thermoplastic or thermosetting resins like polyvinyl butyral or ethylene-vinyl acetate copolymer resins.

Benefits of technology

The solution prevents delamination during lamination and use, maintaining image clarity and resolution, and improves adhesion between layers, ensuring the image-bearing laminate does not peel off over time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018407_05122024_PF_FP_ABST
    Figure JP2024018407_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides: an image-carrying laminate in which sharpness and resolution of an image are favorably maintained without causing separation of an image-carrying layer during alignment processing or a long period of use; a method for manufacturing the same; an intermediate film for laminated glass; and a laminated glass. The present invention specifically provides an image-carrying laminate 1A on which an image is carried and which comprises: a first resin sheet 10; and an image-carrying layer 20 that is formed of a cured product of a curable ink. The first resin sheet 10 is superposed on the first surface 20A side of the image-carrying layer 20, and a second surface 20B, which is on the reverse side of the first surface 20A, is subjected to a surface treatment by a surface treatment process.
Need to check novelty before this filing date? Find Prior Art

Description

Image-carrying laminate, its manufacturing method, interlayer film for laminated glass, and laminated glass

[0001] The present invention relates to an image-bearing laminate on which an image is carried, an interlayer film for laminated glass having the image-bearing laminate, and laminated glass.

[0002] Laminated glass is safe because it shatters little if it is broken by an external impact, and is therefore widely used as glass for various vehicles such as automobiles, railway cars, aircraft and ships, as well as for buildings, etc. A widely known type of laminated glass is one in which an interlayer film for laminated glass containing a resin component such as a polyvinyl acetal resin or an ethylene-vinyl acetate copolymer resin is interposed between a pair of panes of glass to integrate them.

[0003] In recent years, market demands for design of glass structures such as laminated glass have become more diverse. For example, in automotive applications, there is a growing need and concept for designing glass parts to match the body design and color. In architectural applications, there is also a continuing need for decorative glass for exterior and interior use.

[0004] It has been known to provide a colored layer or a printed layer (image-carrying layer) to enhance the design of a glass structure such as laminated glass. For example, as described in Patent Document 1, it is known to provide decoration by printing by inkjet printing on a thermoplastic hard intermediate layer that constitutes an interlayer film to provide a printed layer.

[0005] International Publication No. 2004 / 011271

[0006] However, when laminated glass is constructed by laminating an image-carrying layer onto a thermoplastic hard interlayer that constitutes the interlayer, using inkjet printing with a typical ultraviolet-curable ink, or by sandwiching a printed resin image-carrying layer between thermoplastic hard interlayers, the interlayer adhesion between the image-carrying layer and the interlayer is insufficient, which can lead to problems such as delamination during lamination processing or over time.

[0007] Therefore, an object of the present invention is to provide an image-bearing laminate in which the image-bearing layer does not undergo interlayer delamination during lamination processing or use over time, and in which the clarity and resolution of the image are well maintained, a method for producing the same, an interlayer film for laminated glass, and laminated glass.

[0008] The gist of the present invention is as follows. [1] An image-bearing laminate on which an image is carried, comprising a first resin sheet and an image-bearing layer made of a cured product of curable ink, wherein the image-bearing layer has the first resin sheet laminated on a first surface side, and a second surface opposite to the first surface has been subjected to a surface treatment by a surface treatment process. [2] The image-bearing laminate according to [1], wherein the surface treatment by the surface treatment process is a treatment to improve the hydrophilicity of the second surface of the image-bearing layer. [3] An image-bearing laminate on which an image is carried, comprising a first resin sheet and an image-bearing layer made of a cured product of curable ink, wherein the image-bearing layer has the first resin sheet laminated on a first surface side, and wherein the second surface opposite to the first surface has a hydrophilicity of 3,200 to 3,700 cm when measured by a Fourier transform infrared spectrophotometer. -1An image-bearing laminate having an absorption peak at 1000 nm. [4] The image-bearing laminate according to [1] or [3], which comprises a second resin sheet laminated on the second surface side of the image-bearing layer. [5] The image-bearing laminate according to any one of [1] to [4], in which the first resin sheet contains either a thermoplastic resin or a thermosetting resin. [6] The image-bearing laminate according to any one of [1] to [5], in which the first resin sheet contains a thermoplastic resin, and the thermoplastic resin is at least one selected from the group consisting of a polyvinyl butyral resin, an ethylene-vinyl acetate copolymer resin, a polyurethane resin, and a polyolefin resin. [7] The image-bearing laminate according to [4], in which the second resin sheet contains a thermoplastic resin, and the thermoplastic resin is at least one selected from the group consisting of a polyvinyl butyral resin, an ethylene-vinyl acetate copolymer resin, a polyurethane resin, and a polyolefin resin. [8] The image-bearing laminate according to any one of [1] to [7], which comprises a third resin sheet on the surface of the first resin sheet opposite to the surface on which the image-bearing layer is laminated. [9] The image-carrying laminate according to any one of [1] to [8], wherein the first resin sheet is at least one selected from the group consisting of a polyester film, a polyolefin film, a polyimide film, and an epoxy film.

[10] The image-carrying laminate according to [8], wherein the third resin sheet contains either a thermoplastic resin or a thermosetting resin.

[11] The image-carrying laminate according to [8], wherein the third resin sheet contains a thermoplastic resin, and the thermoplastic resin is at least one selected from the group consisting of a polyvinyl butyral resin, an ethylene-vinyl acetate copolymer resin, a polyurethane resin, and a polyolefin resin.

[12] An interlayer film for laminated glass, comprising the image-carrying laminate according to any one of [1] to

[11] .

[13] Laminated glass, comprising the interlayer film for laminated glass according to

[12] .

[14] A method for manufacturing an image-carrying laminate, comprising the steps of: preparing a first resin sheet; printing a curable ink on one side of the first resin sheet; and curing the curable ink to form an image-carrying layer; and performing a surface treatment process on a second surface of the image-carrying layer opposite to the first surface on which the first resin sheet is laminated.

[15] The method for producing an image-bearing laminate according to

[14] , further comprising a step of laminating a second resin sheet on the second surface side of the image-bearing layer.

[0009] The present invention can provide an image-bearing laminate, a method for producing the same, an interlayer film for laminated glass, and laminated glass, in which the image-bearing layer does not undergo interlayer delamination during lamination processing or use over time, and the clarity and resolution of the image are well maintained.

[0010] FIG. 1 is a schematic cross-sectional view (part 1) showing an image-carrying laminate according to a first embodiment. FIG. 2 is a schematic cross-sectional view (part 2) showing an image-carrying laminate according to a first embodiment. FIG. 1 is a schematic cross-sectional view (part 1) showing an image-carrying laminate according to a second embodiment. FIG. 2 is a schematic cross-sectional view (part 2) showing an image-carrying laminate according to a second embodiment. FIG. 1 is a graph showing the results of measuring, with a Fourier transform infrared spectrophotometer, the second surfaces of the image-carrying layers in which cyan ultraviolet-curable ink in the image-carrying laminates of Example 1 and Comparative Example 1 has been cured.

[0011] Hereinafter, the present invention will be described with reference to embodiments.

[0012] First Embodiment [Image-Carrying Laminate] As shown in FIG. 1 , an image-carrying laminate according to a first embodiment of the present invention is an image-carrying laminate 1A carrying an image, and includes a first resin sheet 10 and an image-carrying layer 20 made of a cured product of a curable ink. The image-carrying layer 20 has the first resin sheet 10 laminated on a first surface 20A, which is one surface of the image-carrying layer 20, and a second surface 20B opposite the first surface 20A, which has been subjected to a surface treatment process. In the present invention, by subjecting the second surface 20B of the image-carrying layer 20 to a surface treatment process, the image-carrying layer 20 does not undergo interlayer delamination during lamination processing or over time, and the clarity and resolution of the image are maintained at a high level.

[0013] The image-carrying laminate 1A preferably includes at least a first resin sheet 10 as shown in FIG. 1, but preferably includes a second resin sheet 30 laminated on the second surface 20B side of the image-carrying layer 20 as shown in FIG. 2.

[0014] <Image-bearing layer> The image-bearing layer 20 is a layer (part) in the image-bearing laminate 1A for carrying a formed image. As described above, the image-bearing layer 20 has the second surface 20B subjected to a surface treatment process. This prevents delamination of the image-bearing layer during lamination or over time, and maintains good image clarity and resolution. In this specification, the surface treatment process is preferably a treatment that improves the hydrophilicity of the second surface 20B of the image-bearing layer 20. By improving the hydrophilicity of the second surface 20B of the image-bearing layer 20, the affinity of the image-bearing layer 20 with other layers is improved, improving adhesion, and preventing delamination. For example, when a second resin sheet 30 is provided on the second surface 20B, the affinity with the second resin sheet 30 is improved, improving adhesion between the image-bearing layer 20 and the second resin sheet 30, and preventing delamination. The surface treatment by the surface treatment process may be any treatment that can improve the hydrophilicity of the second surface 20B of the image bearing layer 20, and examples thereof include ozone treatment such as UV ozone treatment, plasma treatment, corona treatment, peroxide treatment, coating treatment, etc. Among these, UV ozone treatment is preferred. UV ozone treatment utilizes the energy of short wavelength ultraviolet light and the ozone (O 3 ) to subject the image bearing layer 20 to hydrophilic treatment.

[0015] The image bearing layer 20 is formed from a cured product of curable ink. The curable ink may be any ink that can be cured by heating or irradiation with active energy rays. Examples of active energy rays include visible light, ultraviolet rays, infrared rays, X-rays, α rays, β rays, and γ rays. The curable ink may also contain a binder resin, and the binder resin may be a curable resin. Of the inks listed above, active energy ray-curable inks are preferred, with ultraviolet-curable inks being particularly preferred.

[0016] When the curable ink is a UV-curable ink, it preferably contains a polymerizable compound that can be cured by active energy rays as a curable resin, as a curable binder resin component. Known polymerizable compounds used in UV-curable inks may be used as the polymerizable compound, but acrylate-based compounds are preferred. The acrylate-based compound is a compound having a (meth)acryloyl group, and may be a monofunctional acrylate compound having one (meth)acryloyl group, but preferably includes a polyfunctional acrylate compound having at least two or more (meth)acryloyl groups. The use of a polyfunctional acrylate compound facilitates proper curing of the image-bearing layer 20.

[0017] The polyfunctional acrylate compound may be either a diacrylate compound having two (meth)acryloyl groups or a polyfunctional acrylate compound having three or more (meth)acryloyl groups, but it is more preferable that the acrylate compound contained in the ink includes a polyfunctional acrylate compound having three or more (meth)acryloyl groups. When a polyfunctional acrylate compound having three or more (meth)acryloyl groups is used, the image-bearing layer 20 can be made into a crosslinked body having a three-dimensional network structure, which increases the mechanical strength and makes it less likely for the material constituting the image-bearing layer 20 to migrate to other layers.

[0018] In addition, a hydroxyl group-containing monomer or a carboxyl group-containing monomer may be used as the polymerizable compound. Examples of the hydroxyl group-containing monomer include hydroxyl-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate. Examples of the carboxyl group-containing monomer include acrylic acid, methacrylic acid, maleic acid, fumaric acid, and itaconic acid. These hydroxyl group-containing monomers and carboxyl group-containing monomers may be used in combination with acrylic compounds other than hydroxyl group-containing monomers and carboxyl group-containing monomers. Using a hydroxyl group-containing monomer or a carboxyl group-containing monomer as the acrylate compound can improve the hydrophilicity of the second surface 20B of the image bearing layer 20 without surface treatment, thereby improving the adhesive strength between the image bearing layer 20 and the second resin sheet 30 and suppressing interlayer delamination.

[0019] The image bearing layer 20 is preferably formed using an ultraviolet-curable ink containing a colorant. The image bearing layer 20 formed using an ultraviolet-curable ink containing a colorant contains a colorant for forming an image. Known pigments and dyes can be used as the colorant used in the image bearing layer 20. Pigments such as blue, yellow, red, green, purple, white, and black can be used as colorants. A single colorant may be used, or two or more colorants may be used in combination. Furthermore, the colorant is preferably one that selectively absorbs visible light, but is not limited to such colorants. A light-emitting material, known as a fluorescent material, that emits visible light when irradiated with excitation light may also be used. The fluorescent material (light-emitting material) may also be a material that emits phosphorescence when irradiated with excitation light. The maximum emission wavelength (maximum excitation wavelength) of the excitation light is not particularly limited, but is preferably 420 nm or less, more preferably 410 nm or less, and even more preferably 408 nm or less. The maximum emission wavelength of the excitation light is preferably equal to or greater than the lower limit and equal to or less than the upper limit, and the light-emitting material can efficiently emit visible light by the excitation light.

[0020] Examples of the luminescent material used in the image-carrying layer 20 include lanthanoid complexes, luminescent materials having a terephthalic acid ester structure, luminescent materials having a naphthalimide skeleton, luminescent materials having a coumarin skeleton, and luminescent materials having a quinoline skeleton. The luminescent materials may be used alone or in combination of two or more. By combining multiple luminescent materials with different emission wavelengths, it is possible to display not only monochromatic images but also images combining various colors. Among the above-mentioned luminescent materials, lanthanoid complexes and luminescent materials having a terephthalic acid ester structure are preferred, and luminescent materials having a terephthalic acid ester structure are more preferred.

[0021] Examples of the compound having a terephthalate skeleton include compounds having a diterephthalate structure, such as a compound having a structure represented by the following formula (1) and a compound having a structure represented by the following formula (2). These may be used alone or in combination of two or more.

[0022]

[0023] In the above formula (1), R 1 represents an organic group, and x is 1, 2, 3, or 4. From the viewpoint of increasing the transparency of the image-bearing layer 20, x is preferably 1 or 2, and it is more preferable that the benzene ring has a hydroxyl group at the 2nd or 5th position, and it is even more preferable that the benzene ring has a hydroxyl group at the 2nd and 5th positions. 1 The organic group is preferably a hydrocarbon group, more preferably a hydrocarbon group having 1 to 10 carbon atoms, even more preferably a hydrocarbon group having 1 to 5 carbon atoms, and particularly preferably a hydrocarbon group having 1 to 3 carbon atoms. When the hydrocarbon group has 10 or less carbon atoms, the fluorescent material having the terephthalate skeleton can be easily dispersed or dissolved in ink. The hydrocarbon group is preferably an alkyl group. In formula (1), two R 1 may be the same as or different from each other.

[0024] Examples of compounds having a structure represented by the above formula (1) include diethyl-2,5-dihydroxyterephthalate, dimethyl-2,5-dihydroxyterephthalate, etc. Among these, the compound having a structure represented by the above general formula (1) is preferably diethyl-2,5-dihydroxyl terephthalate ("diethyl 2,5-dihydroxyterephthalate" manufactured by Aldrich).

[0025] In the above formula (2), R 2 represents an organic group, R 3 and R 4 represents a hydrogen atom or an organic group, and y is 1, 2, 3, or 4. 2 The organic group is preferably a hydrocarbon group, more preferably a hydrocarbon group having 1 to 10 carbon atoms, even more preferably a hydrocarbon group having 1 to 5 carbon atoms, and particularly preferably a hydrocarbon group having 1 to 3 carbon atoms. When the number of carbon atoms in the hydrocarbon group is equal to or less than the upper limit, the fluorescent material having the terephthalate skeleton can be easily dispersed or dissolved in ink. The hydrocarbon group is preferably an alkyl group. In formula (2), two R 1 In the general formula (2), NR may be the same or different. 3 R 4 is an amino group. 3 and R 4 are each independently preferably a hydrocarbon group having 1 to 10 carbon atoms or a hydrogen atom. The hydrocarbon group more preferably has 1 to 5 carbon atoms, and even more preferably has 1 to 3 carbon atoms. 3 and R 4 Preferably, the hydrocarbon groups in R are all alkyl groups. 3 and R 4 may be bonded to form a ring. 3 and R 4 When forming a ring, the total number of carbon atoms is preferably 2 to 6, more preferably 2 to 5. Examples of the ring include azetidine. In the compound having the structure represented by the above general formula (2), y is preferably 2. In formula (2), when two or more NR 3 R4 If there are two or more NR 3 R 4 may be the same or different. Preferred examples of the compound having the structure represented by general formula (2) include diethyl-2,5-diaminoterephthalate (for example, manufactured by Aldrich), dimethyl-2,5-bis(dimethylamino)terephthalate, and diethyl-2,5-bis(azetidin-1-yl)terephthalate.

[0026] Furthermore, the ultraviolet-curable ink may contain, in addition to the binder resin and colorant, known components used in inks, such as sensitizers, dispersants, leveling agents, antifoaming agents, surface conditioners, photopolymerization initiators, and other components contained in conventional ultraviolet-curable inks. The ultraviolet-curable ink may be solvent-free, but may contain an organic solvent or the like as necessary.

[0027] The image-bearing layer 20 is preferably a printed layer formed by printing, and more preferably formed by printing on the other surface 10B of the first resin sheet 10. The image-bearing layer 20 may be formed on the entire surface of the image-bearing laminate 1A by so-called solid printing. However, the image-bearing layer 20 is preferably printed in a predetermined image shape, such as a picture, pattern, icon, or other design, text, or a combination thereof, and formed on a partial region of the image-bearing laminate 1A. When the image-bearing layer 20 is printed in a predetermined image shape, a decrease in image resolution and clarity results in a significant deterioration in image quality. However, by performing a surface treatment on the second surface 20B of the image-bearing layer 20 using a surface treatment process as described above, delamination of the image-bearing layer 20 can be suppressed. Therefore, by performing a surface treatment on the second surface 20B of the image-bearing layer 20 using a surface treatment process, delamination of the image can be prevented, and the clarity and resolution of the image can be maintained satisfactorily, thereby appropriately suppressing deterioration in image quality.

[0028] The thickness of the image-bearing layer 20 is not particularly limited, but is preferably 0.5 μm or more and 70 μm or less, more preferably 1 μm or more and 50 μm or less, and even more preferably 5 μm or more and 30 μm or less. By making the thickness of the image-bearing layer 20 equal to or greater than the above-mentioned lower limit, an image can be displayed more appropriately on the image-bearing layer 20. Furthermore, by making the thickness of the image-bearing layer 20 equal to or less than the above-mentioned upper limit, it is possible to prevent the image-bearing layer 20 formed only in a partial region of the image-bearing laminate 1A from creating large irregularities in the image-bearing laminate 1A. It is also possible to prevent the image-bearing laminate 1A from becoming thicker than necessary.

[0029] In one embodiment, the image bearing layer 20 has a wavelength of 3,200 to 3,700 cm when the second surface 20B is measured using a Fourier transform infrared spectrophotometer. -1 The second surface 20B of the image bearing layer 20 has an absorption peak in the above range when measured with a Fourier transform infrared spectrophotometer. When the second surface 20B of the image bearing layer 20 has an absorption peak in the above range, hydroxyl groups are present in the molecular structure constituting the second surface 20B, and the hydrophilicity of the second surface 20B is improved. In other words, when the second surface 20B of the image bearing layer 20 has an absorption peak in the above range when measured with a Fourier transform infrared spectrophotometer, the affinity with the second resin sheet 30 is improved, the adhesive strength between the image bearing layer 20 and the second resin sheet 30 is improved, and interlayer delamination can be suppressed. In order for the second surface 20B of the image bearing layer 20 to have an absorption peak in the above range when measured with a Fourier transform infrared spectrophotometer, methods such as performing surface treatment using the surface treatment process described above and incorporating a component having a hydroxyl group and a carboxyl group into the curable ink used to form the image bearing layer 20 can be used. Since these methods have an absorption peak in the above range when measured with a Fourier transform infrared spectrophotometer, any one of them may be adopted, or two of them may be adopted in combination. Therefore, in one aspect of the present invention, the second surface does not necessarily have to be subjected to a surface treatment by a surface treatment process.

[0030] <First Resin Sheet, Second Resin Sheet> As described above, the image-carrying laminate 1A of the present invention includes at least one resin sheet (first resin sheet 10). However, as shown in FIG. 2, it preferably includes at least two resin sheets (first resin sheet 10 and second resin sheet 30). By including the resin sheets (first resin sheet 10 and second resin sheet 30), the image-carrying layer 20 can be disposed between a pair of substrates, making it easier to properly adhere both sides of the image-carrying laminate 1A to other members via the resin sheets (first resin sheet 10 and second resin sheet 30). Therefore, the image-carrying laminate 1A can be suitably used as an interlayer film for laminated glass.

[0031] The resin sheets (first resin sheet 10 and second resin sheet 30) may be used as substrate layers for holding the image-carrying layer 20. The resin sheets (first resin sheet 10 and second resin sheet 30) may also serve as adhesive layers for adhering the image-carrying laminate 1A to other members, such as glass members. Therefore, the first resin sheet 10 is preferably disposed on one surface of the image-carrying laminate 1A. When the second resin sheet 30 is provided, the second resin sheet 30 is preferably disposed on the other surface (the surface opposite to the one surface) of the image-carrying laminate 1A. By being disposed on the surface of the image-carrying laminate 1A, the resin sheets (first resin sheet 10 and second resin sheet 30) can be appropriately used as adhesive layers for adhering to other members.

[0032] The resin used for the first resin sheet 10 is preferably either a thermoplastic resin or a thermosetting resin, and more preferably a thermoplastic resin. The resin used for the second resin sheet 30 is preferably either a thermoplastic resin or a thermosetting resin, and more preferably a thermoplastic resin. Therefore, it is more preferable that all of the resins used for the resin sheets (first resin sheet 10 and second resin sheet 30) are thermoplastic resins. By including a thermoplastic resin in the resin sheets (first resin sheet 10 and second resin sheet 30), the resin sheets can more easily function as adhesive layers, improving adhesion to glass plates (glass members).

[0033] The thermoplastic resin in each resin sheet (first resin sheet 10 and second resin sheet 30) is not particularly limited, but examples thereof include polyvinyl acetal resin, ethylene-vinyl acetate copolymer resin, ionomer resin, polyurethane resin, thermoplastic elastomer, acrylic resin, acrylic-vinyl acetate copolymer resin, polyvinyl alcohol resin, polyolefin resin, polyvinyl acetate resin, and polystyrene resin. The use of these resins facilitates ensuring adhesion to glass plates. In each resin sheet of the present invention, the thermoplastic resin may be used alone or in combination with two or more. Among the above, at least one selected from the group consisting of polyvinyl acetal resin, ethylene-vinyl acetate copolymer resin, polyurethane resin, and polyolefin resin is preferred. Polyvinyl acetal resin, particularly polyvinyl butyral resin, is more preferred because it exhibits excellent adhesion to glass, especially when used in combination with a plasticizer.

[0034] The thermosetting resin in each resin sheet (first resin sheet 10 and second resin sheet 30) is not particularly limited, but examples thereof include epoxy resin, phenol resin, melamine resin, unsaturated polyester resin, urea resin, silicone resin, etc. Use of these resins makes it easier to ensure adhesion to the glass plate.

[0035] The resins constituting the resin sheets (first resin sheet 10 and second resin sheet 30) may be appropriately selected from the resins listed above. Furthermore, the resins constituting the resin sheets (first resin sheet 10 and second resin sheet 30) may be different from each other, but are preferably the same. When the first resin sheet 10 and the second resin sheet 30 are provided, it is preferable that the resins used in both the first resin sheet 10 and the second resin sheet 30 are at least one selected from the group consisting of polyvinyl acetal resin, ethylene-vinyl acetate copolymer resin, polyurethane resin, and polyolefin resin.

[0036] <Polyvinyl Acetal Resin> The polyvinyl acetal resin is not particularly limited as long as it is a polyvinyl acetal resin obtained by acetalizing polyvinyl alcohol (PVA) with an aldehyde. The aldehyde is not particularly limited, but generally, an aldehyde having 1 to 10 carbon atoms is preferably used. The aldehyde having 1 to 10 carbon atoms is not particularly limited, and examples thereof include n-butyl aldehyde, isobutyraldehyde, n-valeraldehyde, 2-ethylbutyraldehyde, n-hexyl aldehyde, n-octyl aldehyde, n-nonyl aldehyde, n-decyl aldehyde, formaldehyde, acetaldehyde, and benzaldehyde. These aldehydes may be used alone or in combination of two or more. Among the above, n-butylaldehyde, n-hexylaldehyde, and n-valeraldehyde are preferred, and n-butylaldehyde is more preferred. Therefore, the polyvinyl acetal resin is preferably polyvinyl butyral resin (PVB). The polyvinyl butyral resin (PVB) may be modified or unmodified.

[0037] Polyvinyl alcohol (PVA) can be obtained, for example, by saponifying a polyvinyl ester such as polyvinyl acetate. The degree of saponification of polyvinyl alcohol is generally 70 to 99.9 mol%. Polyvinyl acetal resins may be used singly or in combination of two or more. The average degree of polymerization of PVA is preferably 200 or more, more preferably 500 or more, even more preferably 1,000 or more, and even more preferably 1,500 or more. Increasing the average degree of polymerization above the lower limit improves the penetration resistance of laminated glass. Furthermore, the average degree of polymerization of PVA is preferably 5,000 or less, more preferably 4,000 or less, even more preferably 3,500 or less, and even more preferably 2,500 or less. The average degree of polymerization of polyvinyl alcohol is determined according to JIS K 6726, "Test Methods for Polyvinyl Alcohol."

[0038] The hydroxyl group content of the polyvinyl acetal resin is preferably 15 to 38 mol%, more preferably 20 to 35 mol%, even more preferably 25 to 33 mol%, and even more preferably 32 to 80 mol%. By ensuring that the hydroxyl group content is equal to or greater than the above-mentioned lower limit, the adhesiveness is likely to be improved, and the penetration resistance of the laminated glass is likely to be improved. Furthermore, by ensuring that the hydroxyl group content is equal to or less than the above-mentioned upper limit, the laminated glass is prevented from becoming too hard. From the same viewpoint, when a polyvinyl butyral resin is used as the polyvinyl acetal resin, the hydroxyl group content of the polyvinyl butyral resin is preferably 15 to 38 mol%, more preferably 20 to 35 mol%, even more preferably 25 to 33 mol%, and even more preferably 32 to 80 mol%. The hydroxyl group content of the polyvinyl acetal resin is the molar fraction calculated by dividing the number of ethylene groups to which hydroxyl groups are bonded by the total number of ethylene groups in the main chain, expressed as a percentage. The amount of ethylene groups to which hydroxyl groups are bonded can be measured, for example, in accordance with JIS K 6728 "Testing methods for polyvinyl butyral."

[0039] The degree of acetalization of the polyvinyl acetal resin is preferably 47 to 85 mol%, more preferably 55 to 80 mol%, and even more preferably 60 to 75 mol%. By setting the degree of acetalization at or above the lower limit, transparency is increased. By setting the degree of acetalization at or below the upper limit, moisture resistance of the image-bearing laminate or laminated glass is increased. Note that the term "degree of acetalization" refers to the degree of butyralization when the acetal group is a butyral group and the polyvinyl acetal resin is a polyvinyl butyral resin. The degree of acetalization is a molar fraction calculated by subtracting the amount of ethylene groups to which hydroxyl groups and the amount of ethylene groups to which acetyl groups are bonded from the total amount of ethylene groups in the main chain, and dividing the result by the total amount of ethylene groups in the main chain, expressed as a percentage. The degree of acetalization (degree of butyralization) may be calculated from the results of measurement according to, for example, JIS K 6728 "Testing methods for polyvinyl butyral."

[0040] The acetylation degree of the polyvinyl acetal resin is preferably 30 mol% or less, more preferably 20 mol% or less, even more preferably 10 mol% or less, and even more preferably 2 mol% or less. When the acetylation degree is below the above upper limit, the moisture resistance of the first resin sheet 10 and the second resin sheet 30 is increased. The acetylation degree is not particularly limited, but is preferably 0.01 mol% or more, more preferably 0.1 mol% or more. The acetylation degree is a molar fraction calculated by dividing the amount of ethylene groups to which acetyl groups are bonded by the total amount of ethylene groups in the main chain, expressed as a percentage. The amount of ethylene groups to which acetyl groups are bonded can be measured, for example, in accordance with JIS K 6728 "Test Methods for Polyvinyl Butyral."

[0041] Ethylene-vinyl acetate copolymer resin: The ethylene-vinyl acetate copolymer resin may be a non-crosslinked ethylene-vinyl acetate copolymer resin or a high-temperature crosslinked ethylene-vinyl acetate copolymer resin. Furthermore, modified ethylene-vinyl acetate resins such as saponified ethylene-vinyl acetate copolymers and hydrolyzed ethylene-vinyl acetate can also be used as the ethylene-vinyl acetate copolymer resin. The ethylene-vinyl acetate copolymer resin preferably has a vinyl acetate content of 10 to 50% by mass, more preferably 20 to 40% by mass, as measured in accordance with JIS K 6730 "Testing Methods for Ethylene-Vinyl Acetate Resins" or JIS K 6924-2:1997. By adjusting the vinyl acetate content to above these lower limits, adhesion to glass is improved and the penetration resistance of laminated glass is likely to be improved. Furthermore, by adjusting the vinyl acetate content to below these upper limits, the breaking strength of the image-bearing laminate is increased and the impact resistance of the laminated glass is improved.

[0042] <Polyurethane Resin> Examples of polyurethane resins include polyurethanes obtained by reacting an isocyanate compound with a diol compound, and polyurethanes obtained by reacting an isocyanate compound with a diol compound and a chain extender such as a polyamine. The polyurethane resin may also contain sulfur atoms. In this case, some or all of the diols may be selected from polythiols and sulfur-containing polyols. Polyurethane resins can improve adhesion to organic glass. Therefore, they are preferably used when the laminated glass member is made of organic glass.

[0043] <Polyolefin Resin> Examples of polyolefin resins include polyethylene resin, polypropylene resin, polybutene resin, poly(4-methylpentene-1) resin, and cycloolefin resin.

[0044] <<Plasticizer>> When each resin sheet (first resin sheet 10 and second resin sheet 30) contains a thermoplastic resin, it is preferable that it further contains a plasticizer. That is, the first resin sheet 10 preferably contains a thermoplastic resin and a plasticizer. Furthermore, when the second resin sheet 30 is provided, the second resin sheet 30 also preferably contains a thermoplastic resin and a plasticizer. The first resin sheet 10 and the second resin sheet 30 become flexible by containing a plasticizer, and as a result, the image-carrying laminate 1A also becomes flexible. Furthermore, when the image-carrying laminate 1A is used as an interlayer film for laminated glass, it improves the flexibility of the laminated glass and also improves its penetration resistance. Furthermore, it is possible to exhibit high adhesion to glass plates.

[0045] When polyvinyl acetal resin is used as the thermoplastic resin, it is particularly effective to include a plasticizer in each resin sheet. Therefore, it is more preferable that the first resin sheet 10 includes a polyvinyl acetal resin and a plasticizer. It is also more preferable that the second resin sheet 30 includes a polyvinyl acetal resin and a plasticizer. Examples of plasticizers include organic ester plasticizers such as monobasic organic acid esters and polybasic organic acid esters, and phosphorus-based plasticizers such as organic phosphate ester plasticizers and organic phosphite ester plasticizers. Among these, organic ester plasticizers are preferred.

[0046] Examples of the organic ester plasticizer include triethylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylhexanoate, triethylene glycol dicaprylate, triethylene glycol di-n-octanoate, triethylene glycol di-n-heptanoate, tetraethylene glycol di-n-heptanoate, tetraethylene glycol di-2-ethylhexanoate, dibutyl sebacate, dioctyl azelate, dibutyl carbitol adipate, ethylene glycol di-2-ethylbutyrate, 1,3-propylene glycol di-2-ethylbutyrate, 1,4-butylene glycol di-2-ethylbutyrate, 1,2-butylene glycol di-2-ethylbutyrate, and diethylene glycol di- Examples of suitable adipates include 2-ethyl butyrate, diethylene glycol di-2-ethylhexanoate, dipropylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylpentanoate, tetraethylene glycol di-2-ethylbutyrate, diethylene glycol dicaprylate, triethylene glycol di-n-heptanoate, tetraethylene glycol di-n-heptanoate, triethylene glycol di-2-ethylbutyrate, dihexyl adipate, dioctyl adipate, hexylcyclohexyl adipate, diisononyl adipate, heptylnonyl adipate, dibutyl sebacate, oil-modified alkyd sebacic acid, a mixture of a phosphate ester and an adipate ester, and mixed adipates. Examples of mixed adipates include adipates prepared from two or more alcohols selected from alkyl alcohols having 4 to 9 carbon atoms and cyclic alcohols having 4 to 9 carbon atoms. Among the above plasticizers, triethylene glycol-di-2-ethylhexanoate (3GO) is particularly suitable.

[0047] The content of the plasticizer in each of the resin sheets (first resin sheet 10 and second resin sheet 30) is not particularly limited, but is preferably 10 parts by mass or more and 100 parts by mass or less relative to 100 parts by mass of the thermoplastic resin. When the content of the plasticizer is 10 parts by mass or more, the image-bearing laminate 1A becomes appropriately flexible. Therefore, when the image-bearing laminate 1A is used as an interlayer film for laminated glass, the penetration resistance of the laminated glass is improved. Furthermore, when the content of the plasticizer is 100 parts by mass or less, separation of the plasticizer from the resin sheets (first resin sheet 10 and second resin sheet 30) is prevented. The content of the plasticizer is more preferably 20 parts by mass or more, even more preferably 30 parts by mass or more, even more preferably 35 parts by mass or more, and more preferably 70 parts by mass or less, even more preferably 63 parts by mass or less.

[0048] The resin sheets (first resin sheet 10 and second resin sheet 30) each mainly contain a resin or a resin and a plasticizer, and the total amount of the thermoplastic resin and the plasticizer in each of the resin sheets (first resin sheet 10 and second resin sheet 30) is typically 70% by mass or more and 100% by mass or less, preferably 80% by mass or more and 100% by mass or less, and more preferably 90% by mass or more and 100% by mass or less, based on the total amount of each resin sheet. However, since the resin sheets (first resin sheet 10 and second resin sheet 30) generally often contain additives as described below, the total amount of the thermoplastic resin and the plasticizer may be less than 100% by mass.

[0049] Each resin sheet (first resin sheet 10 and second resin sheet 30) of the present invention may contain various additives such as heat shielding agents, ultraviolet absorbers, antioxidants, light stabilizers, ultraviolet absorbers, and antioxidants, as appropriate.

[0050] The thickness of each of the resin sheets (first resin sheet 10 and second resin sheet 30) is not particularly limited, but is, for example, 50 μm to 1,000 μm, preferably 100 μm to 800 μm, and more preferably 200 μm to 500 μm. By setting the thickness of the resin sheets (first resin sheet 10 and second resin sheet 30) within the above range, the image-carrying layer 20 can be appropriately supported by the resin sheets (first resin sheet 10 and second resin sheet 30) without increasing the thickness of the image-carrying laminate 1A more than necessary, and the image-carrying laminate 1A can be easily adhered to other members such as laminated glass members.

[0051] [Method for Manufacturing Image-Carrying Laminate] An example of a method for manufacturing the image-carrying laminate 1A according to the first embodiment is described below. In the method for manufacturing the image-carrying laminate 1A according to the first embodiment, first, a first resin sheet 10 is prepared, and a curable ink is printed on the other surface 10B of the first resin sheet 10, and the curable ink is cured to form the image-carrying layer 20. The image-carrying layer 20 may be provided partially on the other surface 10B of the first resin sheet 10, or may be provided entirely on the other surface 10B of the first resin sheet 10. The printing method for the curable ink is not particularly limited, but examples include screen printing, inkjet printing, flexographic printing, and offset printing. Of these, inkjet printing is preferred. When the curable ink is an ultraviolet-curable ink, the printed and applied ultraviolet-curable ink is irradiated with ultraviolet light and cured to form the image-carrying layer 20. Next, the second surface 20B of the image bearing layer 20 opposite to the first surface 20A on which the first resin sheet 10 is laminated is subjected to the surface treatment process as described above.

[0052] When the image-bearing laminate 1A includes a second resin sheet 30 on the second surface 20B of the image-bearing layer 20, the second resin sheet 30 may be laminated on the second surface 20B of the image-bearing layer 20 after the surface treatment by the surface treatment process. The lamination method for the second resin sheet 30 is not particularly limited, and any known method may be used, such as a lamination method. The lamination method may involve extrusion molding a thermoplastic resin onto the second surface 20B of the image-bearing layer 20 that has been surface-treated by the surface treatment process. Alternatively, the second surface 20B may be formed by laminating a thermoplastic resin formed into a film by press molding or the like onto the second surface 20B of the image-bearing layer 20 that has been surface-treated by the surface treatment process, or another known lamination method may be used.

[0053] By going through the above steps, the image-carrying laminate 1A shown in FIGS. 1 and 2 can be obtained. In this manufacturing method, by performing a surface treatment on the surface of the image-carrying layer 20 by a surface treatment process, the image-carrying layer 20 does not undergo delamination, and the image clarity and resolution are maintained at a good level. In this manufacturing method, by forming the image-carrying layer 20 by printing, it becomes easier to express images of various shapes using the image-carrying layer 20, and it becomes easier to obtain an image-carrying laminate 1A with a high design quality. Note that the above manufacturing method is one example for obtaining the image-carrying laminate 1A according to the first embodiment, and is not limited to the above method. Furthermore, in one aspect of the first embodiment, a component having a hydroxyl group and a carboxyl group is contained in the curable ink, and a wavelength of 3,200 to 3,700 cm is obtained on the second surface 20B when measured with a Fourier transform infrared spectrophotometer. -1 When an absorption peak is to be provided at the surface, the surface treatment process may be omitted.

[0054] <Method of using the image-carrying laminate> The image-carrying laminate 1A can be used for various purposes, but is preferably used as an adhesive sheet that is adhered to another member via the first resin sheet 10, or the first resin sheet 10 and the second resin sheet 30. Here, the other member to which the image-carrying laminate 1A of the present invention is adhered is preferably a glass member. As the glass member, a glass plate is preferred. Specific examples of the glass plate are the same as the glass plates used in the laminated glass member described below.

[0055] [Interlayer Film for Laminated Glass] The image-carrying laminate 1A is preferably used as an interlayer film for laminated glass. The image-carrying laminate 1A may be used as an interlayer film for laminated glass as is, or may be used as an interlayer film for laminated glass after being additionally laminated with a substrate layer (also referred to as an "additional substrate layer"). That is, the present invention provides a laminated glass interlayer film having the image-carrying laminate 1A. The laminated glass interlayer film may be made of the image-carrying laminate 1A, or may have other layers such as an additional substrate layer in addition to the image-carrying laminate 1A. Note that the configuration of the additional substrate layer is the same as the configuration of the resin sheet described above, and therefore description thereof will be omitted.

[0056] The image-carrying laminate 1A may be used as an adhesive layer for adhering the first resin sheet 10, or the first resin sheet 10 and the second resin sheet 30, to other members. Therefore, when the image-carrying laminate 1A has the first resin sheet 10 and the second resin sheet 30 as base layers, it may be used as an interlayer film for laminated glass as is. That is, the image-carrying laminate 1A is placed between a pair of laminated glass members, and the first resin sheet 10 is adhered to one of the laminated glass members and the second resin sheet 30 is adhered to the other laminated glass member, thereby joining the pair of laminated glass members via the image-carrying laminate 1A.

[0057] However, even when the image-carrying laminate 1A has the first resin sheet 10 and the second resin sheet 30, a laminate having an additional substrate layer laminated thereon may be used as an interlayer film for laminated glass. For example, an additional substrate layer may be laminated on the outer side of one or both of the first resin sheet 10 and the second resin sheet 30, and used as an interlayer film for laminated glass.

[0058] On the other hand, when the image-carrying laminate 1A has only one resin sheet (first resin sheet 10) as the substrate layer, it is preferable to appropriately laminate an additional substrate layer and use the laminate with the additional substrate layer laminated as an interlayer film for laminated glass. In this case, the additional substrate layer may be laminated on the side of the image-carrying laminate 1A opposite to the side on which the first resin sheet 10 is provided. Specifically, in the first embodiment ( FIG. 1 ), the additional substrate layer may be laminated on the image-carrying layer 20.

[0059] However, even when the image-carrying laminate has only one resin sheet (first resin sheet 10) as the substrate layer, the image-carrying laminate 1A may be used as an interlayer for laminated glass without laminating an additional substrate layer. In this case, for example, the image-carrying layer 20 may be provided on only a portion of one surface of the first resin sheet 10, and the other surface 10B of the first resin sheet 10 may be exposed. By bonding the other surface 10B of the first resin sheet 10 to one laminated glass member and bonding the one surface 10A of the first resin sheet 10 (i.e., the surface opposite to the surface on which the image-carrying layer 20 is provided) to the other laminated glass member, the image-carrying laminate 1A can be used as an interlayer for laminated glass to appropriately bond two laminated glass members.

[0060] [Laminated Glass] Laminated glass contains an interlayer film for laminated glass, and generally comprises a pair of laminated glass components and an interlayer film for laminated glass disposed between the pair of laminated glass components, with the pair of laminated glass components joined together via the interlayer film for laminated glass.

[0061] As described above, the interlayer film for laminated glass used in laminated glass may be composed of an image-carrying laminate, or may be composed of an image-carrying laminate to which other layers, such as an additional substrate layer, have been laminated. The laminated glass member used in laminated glass may be a glass plate. The glass plate may be either inorganic or organic glass, with inorganic glass being preferred. Examples of inorganic glass include, but are not limited to, clear glass, float glass, polished glass, figured glass, wired glass, striped glass, and green glass. Organic glass generally refers to what is called resin glass, and examples include, but are not limited to, organic glass composed of resins such as polycarbonate, acrylic resin, acrylic copolymer resin, and polyester. The two glass plates may be composed of the same material or different materials. For example, one glass plate may be inorganic glass and the other organic glass. However, it is preferred that both glass plates are inorganic glass or organic glass. The thickness of each glass plate is not particularly limited, but is, for example, approximately 0.1 to 15 mm, preferably 0.5 to 5 mm. The thickness of each glass plate may be the same or different from each other, but it is preferable that the thicknesses are the same.

[0062] The method for producing laminated glass is not particularly limited. For example, an image-bearing laminate is sandwiched between two laminated glass members, and the image-bearing laminate is passed through a pressure roll, or placed in a rubber bag and subjected to vacuum suction to remove any air remaining between the two glass members and the resin film. This is then pre-bonded at approximately 70 to 110°C to obtain a laminate. The laminate is then placed in an autoclave or pressed at approximately 120 to 150°C and a pressure of 1 to 1.5 MPa to obtain a laminated glass.

[0063] Furthermore, when another resin layer such as an additional substrate layer of an image-carrying laminate is laminated, the laminated glass may be produced by first laminating and integrating the other layer such as the additional substrate layer onto the image-carrying laminate, and then sandwiching the integrated product between two laminated glass members in the same manner as above. When another layer such as an additional substrate layer is laminated onto the image-carrying laminate, the laminated glass may be produced by sandwiching a product obtained by superposing the image-carrying laminate and the other resin layer between two laminated glass members without first integrating them in the same manner as above. In this case, an interlayer film for laminated glass, which is formed by laminating the other layer onto the image-carrying laminate, is also produced while producing the laminated glass.

[0064] The interlayer film for laminated glass and laminated glass of the present invention can be used as glass structures such as window glass in a variety of fields, and can be used for vehicles such as automobiles, railway vehicles, aircraft, and ships, as well as for architectural applications, and is particularly preferably used for various vehicle applications such as automobiles. When used in automobiles, it can be used for any of windshields, side windows, and rear windows.

[0065] The interlayer film for laminated glass and laminated glass of the present invention can carry an image in the glass structure, and therefore are preferably used in applications requiring high design quality. For example, when used in automobile window glass, the automobile window glass can be decorated to match the body design or body color. In architectural applications, they are also preferably used as decorative glass for exterior or interior use.

[0066] Furthermore, as described above, when the image-bearing layer contains a light-emitting material, the laminated glass is preferably used together with a light source device that irradiates excitation light. The light source device is not particularly limited, but when the laminated glass is used for vehicles, it is preferably disposed, for example, inside the vehicle. When the laminated glass is used for architectural purposes, the light source device may be disposed inside or outside the building.

[0067] Second Embodiment Next, a second embodiment of the present invention will be described in detail. The second embodiment differs from the first embodiment in that, as shown in FIGS. 3 and 4, a third resin sheet 40 is provided on one side 10A of the first resin sheet 10 opposite the other side 10B on which the image bearing layer 20 is laminated. Hereinafter, the differences between the first embodiment and the second embodiment will be described. Furthermore, parts whose description is omitted are the same as those in the first embodiment. Furthermore, in the following description, components having the same configuration as those in the first embodiment will be denoted by the same reference numerals.

[0068] As shown in FIGS. 3 and 4, the image-carrying laminate 1B according to the second embodiment includes a third resin sheet 40 as an outer layer of the first resin sheet 10. As shown in FIGS.

[0069] <First Resin Sheet> The first resin sheet 10 in the image-carrying laminate 1B according to the second embodiment is preferably made of a material that has good adhesive strength between the third resin sheet 40 and the image-carrying layer 20 and can suppress interlayer delamination. Examples of the first resin sheet 10 in the image-carrying laminate 1B include polyester films, polyolefin films, polyimide films, and epoxy films. Of these, polyester films are preferred, and among polyester films, polyethylene terephthalate (PET) films are more preferred.

[0070] The thickness of the first resin sheet 10 is not particularly limited, but is preferably 0.5 μm to 400 μm, more preferably 10 μm to 300 μm, and particularly preferably 50 μm to 200 μm. When the thickness of the first resin sheet 40 is equal to or greater than the lower limit, the first resin sheet 40 can easily function as an adhesive layer. Furthermore, when the thickness of the first resin sheet 40 is equal to or less than the upper limit, the image-carrying laminate 1B can be prevented from becoming thicker than necessary.

[0071] <Second Resin Sheet> The second resin sheet 30 in the image-carrying laminate 1B according to the second embodiment can have the same configuration as the second resin sheet 30 in the image-carrying laminate 1A according to the first embodiment described above.

[0072] <Third Resin Sheet> The third resin sheet 40 may be used as a base layer for holding the first resin sheet 10 and the image carrying layer 20. The third resin sheet 40 may also serve as an adhesive layer for adhering the image carrying laminate 1B to another member such as a glass member.

[0073] The resin used in the third resin sheet 40 is preferably either a thermoplastic resin or a thermosetting resin, and more preferably a thermoplastic resin. When the third resin sheet 40 contains a thermoplastic resin, it is easier to function as an adhesive layer, and the adhesiveness to the glass plate (glass member) is improved.

[0074] The thermoplastic resin in the third resin sheet 40 is not particularly limited, but examples include polyvinyl acetal resin, ethylene-vinyl acetate copolymer resin, ionomer resin, polyurethane resin, thermoplastic elastomer, acrylic resin, acrylic-vinyl acetate copolymer resin, polyvinyl alcohol resin, polyolefin resin, polyvinyl acetate resin, and polystyrene resin. The use of these resins facilitates ensuring adhesion to the glass plate. In each resin layer of the present invention, the thermoplastic resin may be used alone or in combination with two or more. Among the above, at least one selected from the group consisting of polyvinyl acetal resin, ethylene-vinyl acetate copolymer resin, polyurethane resin, and polyolefin resin is preferred. Polyvinyl acetal resin is more preferred, and polyvinyl butyral resin is particularly preferred, as it exhibits excellent adhesion to glass, especially when used in combination with a plasticizer.

[0075] The thermosetting resin in the third resin sheet 40 is not particularly limited, but examples thereof include epoxy resin, phenol resin, melamine resin, unsaturated polyester resin, urea resin, silicone resin, etc. Use of these resins makes it easier to ensure adhesion to the glass plate.

[0076] <<Plasticizer>> When the third resin sheet 40 contains a thermoplastic resin, it preferably further contains a plasticizer. That is, the third resin sheet 40 preferably contains a thermoplastic resin and a plasticizer. The third resin sheet 40 becomes flexible by containing a plasticizer, and as a result, the image-carrying laminate 1B also becomes flexible. Furthermore, when the image-carrying laminate 1B is used as an interlayer film for laminated glass, it improves the flexibility of the laminated glass and also improves its penetration resistance. Furthermore, it is possible to exhibit high adhesion to glass plates.

[0077] When polyvinyl acetal resin is used as the thermoplastic resin, it is particularly effective to include a plasticizer in the third resin sheet 40. Therefore, it is more preferable that the third resin sheet 40 contain a polyvinyl acetal resin and a plasticizer. Examples of plasticizers include organic ester plasticizers such as monobasic organic acid esters and polybasic organic acid esters, and phosphorus-based plasticizers such as organic phosphate ester plasticizers and organic phosphite ester plasticizers. Of these, organic ester plasticizers are preferred. Details of the plasticizer are as described above, with triethylene glycol-di-2-ethylhexanoate (3GO) being particularly preferred.

[0078] The content of the plasticizer in the third resin sheet 40 is not particularly limited, but is preferably 10 parts by mass or more and 100 parts by mass or less relative to 100 parts by mass of the thermoplastic resin. When the content of the plasticizer is 10 parts by mass or more, the image-bearing laminate 1B becomes appropriately flexible. Therefore, when the image-bearing laminate 1B is used as an interlayer film for laminated glass, the penetration resistance of the laminated glass is improved. Furthermore, when the content of the plasticizer is 100 parts by mass or less, separation of the plasticizer from the third resin sheet 40 is prevented. The content of the plasticizer is more preferably 20 parts by mass or more, even more preferably 30 parts by mass or more, even more preferably 35 parts by mass or more, and more preferably 70 parts by mass or less, even more preferably 63 parts by mass or less.

[0079] The third resin sheet 40 is mainly composed of a resin or a resin and a plasticizer, and the total amount of the thermoplastic resin and the plasticizer in the third resin sheet 40 is usually 70% by mass or more and 100% by mass or less, preferably 80% by mass or more and 100% by mass or less, and more preferably 90% by mass or more and 100% by mass or less, based on the total amount of the resin sheet. However, since the third resin sheet 40 generally often contains additives as described below, the total amount of the thermoplastic resin and the plasticizer may be less than 100% by mass.

[0080] The third resin sheet 40 of the present invention may contain various additives such as a heat shielding agent, an ultraviolet absorber, an antioxidant, a light stabilizer, an ultraviolet absorber, and an antioxidant, as appropriate.

[0081] The thickness of the third resin sheet 40 is not particularly limited, but is, for example, 50 μm to 1,000 μm, preferably 100 μm to 800 μm, and more preferably 200 μm to 500 μm. By setting the thickness of the third resin sheet 40 within the above range, the first resin sheet 10 and the image-carrying layer 20 can be appropriately supported by the third resin sheet 40 without increasing the thickness of the image-carrying laminate 1B more than necessary, and the image-carrying laminate 1B can be easily adhered to other members such as laminated glass members.

[0082] [Method for Manufacturing Image-Carrying Laminate] An example of a method for manufacturing the image-carrying laminate 1B according to the second embodiment is described below. In the method for manufacturing the image-carrying laminate 1B according to the first embodiment, first, a first resin sheet 10 having a third resin sheet 40 laminated on one surface 10A is prepared. A curable ink is printed on the other surface 10B of the first resin sheet 10, and the curable ink is cured to form the image-carrying layer 20. The image-carrying layer 20 may be provided partially on the other surface 10B of the first resin sheet 10, or may be provided entirely on the other surface 10B of the first resin sheet 10. The printing method for the curable ink is not particularly limited, but examples include screen printing, inkjet printing, flexographic printing, and offset printing. Of these, inkjet printing is preferred. When the curable ink is an ultraviolet-curable ink, the printed and applied ultraviolet-curable ink is irradiated with ultraviolet light and cured to form the image-carrying layer 20. Next, the second surface 20B of the image bearing layer 20 opposite to the first surface 20A on which the first resin sheet 10 is laminated is subjected to the surface treatment process as described above.

[0083] When the image-bearing laminate 1B includes a second resin sheet 30 on the second surface 20B of the image-bearing layer 20, the second resin sheet 30 may be laminated on the second surface 20B of the image-bearing layer 20 after the surface treatment by the surface treatment process. The lamination method for the second resin sheet 30 is not particularly limited, and any known method may be used, such as a lamination method. The lamination method may involve extrusion molding a thermoplastic resin onto the second surface 20B of the image-bearing layer 20 that has been surface-treated by the surface treatment process. Alternatively, the second surface 20B may be formed by laminating a thermoplastic resin formed into a film by press molding or the like onto the second surface 20B of the image-bearing layer 20 that has been surface-treated by the surface treatment process, or another known lamination method may be used.

[0084] 3 and 4 can be obtained through the above steps. In this manufacturing method, by performing a surface treatment process on the surface of the image-bearing layer 20, the image-bearing layer 20 does not undergo delamination, and the image clarity and resolution are maintained at a good level. In this manufacturing method, by forming the image-bearing layer 20 by printing, it becomes easier to express images of various shapes using the image-bearing layer 20, and it becomes easier to obtain an image-bearing laminate 1B with a high level of design.

[0085] The above-described manufacturing method is merely an example for obtaining the image-carrying laminate 1B according to the second embodiment, and is not limited to the above method. For example, first, a first resin sheet 10 is prepared, and a curable ink is printed on the other surface 10B of the first resin sheet 10. The curable ink is then cured to form the image-carrying layer 20. Next, the second surface 20B of the image-carrying layer 20, opposite the first surface 20A on which the first resin sheet 10 is laminated, is subjected to a surface treatment process as described above. Next, a third resin sheet 40 is laminated on one surface 10A of the first resin sheet 10. If the image-carrying laminate 1B includes a second resin sheet 30 on the second surface 20B of the image-carrying layer 20, the second resin sheet 30 may also be laminated on the second surface 20B of the image-carrying layer 20 after the surface treatment process. The image-carrying laminate 1B shown in FIGS. 3 and 4 can also be obtained by going through the above steps.

[0086] In one aspect of the second embodiment, the curable ink contains a component having a hydroxyl group and a carboxyl group, and the second surface (20B) has an intensity of 3,200 to 3,700 cm when measured with a Fourier transform infrared spectrophotometer. -1 When an absorption peak is to be provided at the surface, the surface treatment process may be omitted.

[0087] The present invention will be explained in more detail by way of examples, but the present invention is not limited to these examples in any way.

[0088] [Example 1] (Formation of Image-Carrying Laminate) First, as the first resin sheet 10 and the second resin sheet 30, 100 parts by mass of PVB (polyvinyl butyral resin, average polymerization degree 1,700, hydroxyl group amount 30.5 mol%, acetylation degree 1 mol%, acetalization degree 68.5 mol%) and 30 parts by mass of plasticizer (3GO: triethylene glycol-di-2-ethylhexanoate) were prepared as four resin film substrates (thickness 400 μm). Four colors (cyan, magenta, yellow, black) of ultraviolet-curable ink (manufactured by Mimaki Engineering Co., Ltd., product name "LUS-120") were solidly applied by inkjet printing to the entire surface of one side of the prepared film substrates as the four first resin sheets 10, and ultraviolet light was applied at 3 W / cm. 2 The ultraviolet-curable ink was cured under the conditions of

[0043]

[0044]

[0045]

[0046]

[0047]

[0048]

[0049]

[0050]

[0051]

[0052]

[0053]

[0054]

[0055]

[0056]

[0057]

[0058]

[0059]

[0060]

[0059]

[0061]

[0059]

[0059]

[0062]

[0059]

[0063]

[0059]

[0064]

[0059]

[0065]

[0066]

[0059]

[0066]

[0059]

[0067]

[0068]

[0069]

[0070]

[0071]

[0072]

[0073]

[0074]

[0075]

[0076]

[0077]

[0078]

[0079]

[0080]

[0081]

[0082]

[0083]

[0084]

[0085]

[0086]

[0087]

[0088]

[0089]

[0090]

[0091]

[0092]

[0093]

[0094]

[0095]

[0096]

[0097]

[0098] [009 ...

[0089] (Formation of Laminated Glass) The obtained image-bearing laminate 1A (interlayer film for laminated glass) was sandwiched between two pieces of clear glass (15 cm long x 15 cm wide x 2.5 mm thick) to obtain a laminate. This laminate was placed in a rubber bag and degassed at a vacuum of 2.6 kPa for 20 minutes, and then transferred to an oven in the degassed state, and further held at 90°C for 30 minutes to vacuum press the laminate to pre-pressure bond it. The pre-pressure bonded laminate was then pressed in an autoclave at 135°C and a pressure of 1.2 MPa for 20 minutes to obtain laminated glass.

[0090] [Example 2] The same procedure as in Example 1 was carried out, except that four sheets of resin film substrates (thickness 400 μm) made of EVA (ethylene-vinyl acetate copolymer resin, vinyl acetate content 20% by mass) were prepared and used as the first resin sheet 10 and the second resin sheet 30.

[0091] [Example 3] The same procedure as in Example 1 was carried out, except that four sheets of resin film substrates (thickness 400 μm) made of 100 parts by mass of polyolefin resin (manufactured by STR Corporation, product name "PHOTOCAP 35521P HLT") were prepared and used as the first resin sheet 10 and the second resin sheet 30.

[0092] [Example 4] The same procedure as in Example 1 was carried out, except that four resin film substrates (thickness 400 μm) made of 100 parts by mass of polyurethane resin (Huntsman, product name "IROGRAN A60 E6038") as a thermoplastic resin were prepared and used as the first resin sheet 10 and the second resin sheet 30.

[0093] Example 5 (Formation of Image-Carrying Laminate) First, four sheets of PET (polyethylene terephthalate, thickness 100 μm) were prepared as the first resin sheet 10. Four colors (cyan, magenta, yellow, black) of ultraviolet-curable ink (manufactured by Mimaki Engineering Co., Ltd., product name "LUS-100") were solidly coated on the entire surface of each of the four prepared PET sheets by inkjet printing, and ultraviolet light was applied at a dose of 3 W / cm. 2The UV-curable ink was cured under these conditions to form an image bearing layer 20 (20 μm thick). Next, a UV ozone treatment (NovaScan, product name "UV Ozone Cleaner") was performed on the second surface 20B of the image bearing layer 20, opposite the first surface 20A on which the first resin sheet 10 was laminated. Four resin film substrates (400 μm thick) each composed of 100 parts by weight of PVB (polyvinyl butyral resin, average degree of polymerization 1,700, hydroxyl group content 30.5 mol%, acetylation degree 1 mol%, acetalization degree 68.5 mol%) and 30 parts by weight of plasticizer (3GO: triethylene glycol-di-2-ethylhexanoate) were prepared as the second resin sheet 30 and the third resin sheet 40. The four prepared second resin sheets 30 were laminated on the second surface 20B side of each image-carrying layer 20 coated in each color, and the four prepared third resin sheets 40 were laminated on one surface 10A side of the first resin sheet 10 to obtain an image-carrying laminate 1B having a thickness of 920 μm and the structure shown in Figure 4.

[0094] (Formation of Laminated Glass) The obtained image-bearing laminate 1B (interlayer film for laminated glass) was sandwiched between two sheets of clear glass (15 cm long x 15 cm wide x 2.5 mm thick) to obtain a laminate. This laminate was placed in a rubber bag and degassed at a vacuum of 2.6 kPa for 20 minutes, and then transferred to an oven in the degassed state, and further held at 90°C for 30 minutes to vacuum press the laminate to pre-pressure bond it. The pre-pressure bonded laminate was then pressed in an autoclave at 135°C and a pressure of 1.2 MPa for 20 minutes to obtain laminated glass.

[0095] Comparative Example 1 The same procedure as in Example 1 was carried out, except that the surface treatment of the second surface 20B of the image bearing layer 20 by the surface treatment process was omitted.

[0096] Comparative Example 2 The same procedure as in Example 5 was carried out, except that the surface treatment of the second surface 20B of the image bearing layer 20 by the surface treatment process was omitted.

[0097] (Peak Evaluation in Measurement with a Fourier Transform Infrared Spectrophotometer (FI-IR)) When the second surface 20B of the image bearing layer 20 of the laminated glass obtained in each Example and Comparative Example was measured with a Fourier Transform Infrared Spectrophotometer, a peak of 3,200 to 3,700 cm -1 The image-carrying laminates 1A of Example 1 and Comparative Example 1 were evaluated according to the following criteria for whether they had an absorption peak at 3,200 to 3,700 cm. The evaluation results are shown in Table 1. The measurement conditions for the Fourier transform infrared spectrophotometer (FI-IR) were as follows. As an example of the measurement results, a graph of the results of measuring the second surface 20B of the image-carrying layer 20 in which the cyan ultraviolet-curable ink in the image-carrying laminates 1A of Example 1 and Comparative Example 1 was cured using the Fourier transform infrared spectrophotometer is shown in FIG. 5. <Evaluation criteria> OK: 3,200 to 3,700 cm -1 Absorption peak at NOK: 3,200 to 3,700 cm -1 No absorption peak was observed. <Measurement conditions> A Perkin-Elmer FI-IR device was attached to a diamond ATR horizontal device and the measurement was performed using the ATR method. -1 The average spectrum was obtained after four scans in the wavenumber range of .

[0098] (Evaluation of Delamination During Lamination) Delamination during lamination of the laminated glass obtained in each Example and Comparative Example was evaluated according to the following evaluation criteria. The evaluation results are shown in Table 1. <Evaluation Criteria> OK: No delamination was observed between the layers of the obtained laminated glass sample. NOK: Air had entered the corners of the obtained laminated glass sample, causing delamination between the layers.

[0099] (Evaluation of Delamination After Pummel Test (Sekisui Method)) The laminated glass obtained in each Example and Comparative Example was conditioned at a temperature of -18°C ± 0.6°C for 16 hours, and the central portion (150 mm long x 150 mm wide) of this laminated glass was hit with a hammer with a head of 0.45 kg to crush the glass until the particle size was 6 mm or less. Delamination was then evaluated according to the following evaluation criteria. The evaluation results are shown in Table 1. <Evaluation Criteria> OK: No delamination was observed between the resin sheet and the image-bearing layer. NOK: Delamination was observed between the image-bearing layer and the second resin sheet of the obtained laminated glass sample.

[0100]

[0101] In each of the above examples, the surface of the image bearing layer was subjected to a surface treatment process, and as a result, the wavelength of the image bearing layer was measured using a Fourier transform infrared spectrophotometer in the range of 3,200 to 3,700 cm -1 In contrast, in each of the comparative examples, the absorption peak was in the range of 3,200 to 3,700 cm when measured with a Fourier transform infrared spectrophotometer. -1 The image-bearing layer exhibited delamination, and the sharpness and resolution of the image were not maintained.

[0102] 1A, 1B Image-carrying laminate 10 First resin sheet 20 Image-carrying layer 30 Second resin sheet 40 Third resin sheet

Claims

1. An image-bearing laminate carrying an image, comprising a first resin sheet and an image-bearing layer made of a cured product of a curable ink, the image-bearing layer having the first resin sheet laminated on a first surface side, and a second surface opposite the first surface having been subjected to a surface treatment by a surface treatment process.

2. The image-bearing laminate according to claim 1, wherein the surface treatment by the surface treatment process is a treatment for improving the hydrophilicity of the second surface of the image-bearing layer.

3. An image-carrying laminate carrying an image, comprising a first resin sheet and an image-carrying layer made of a cured product of a curable ink, the image-carrying layer having the first resin sheet laminated on a first surface side, and a Fourier transform infrared spectrophotometer measuring a second surface opposite to the first surface, the second surface having an intensity of 3,200 to 3,700 cm -1 The image-bearing laminate has an absorption peak at 4. The image-bearing laminate according to claim 1 or 3, further comprising a second resin sheet laminated on the second surface side of the image-bearing layer.

5. The image-bearing laminate according to claim 1 or 3, wherein said first resin sheet contains either a thermoplastic resin or a thermosetting resin.

6. The image-bearing laminate according to claim 1 or 3, wherein the first resin sheet contains a thermoplastic resin, and the thermoplastic resin is at least one selected from the group consisting of polyvinyl butyral resin, ethylene-vinyl acetate copolymer resin, polyurethane resin and polyolefin resin.

7. The image-bearing laminate according to claim 4, wherein the second resin sheet contains a thermoplastic resin, and the thermoplastic resin is at least one selected from the group consisting of polyvinyl butyral resin, ethylene-vinyl acetate copolymer resin, polyurethane resin and polyolefin resin.

8. The image-bearing laminate according to claim 1 or 3, further comprising a third resin sheet on the surface of said first resin sheet opposite to the surface on which said image-bearing layer is laminated.

9. The image-bearing laminate according to claim 1 or 3, wherein the first resin sheet is at least one selected from the group consisting of polyester films, polyolefin films, polyimide films and epoxy films.

10. The image-bearing laminate according to claim 8, wherein said third resin sheet comprises one of a thermoplastic resin and a thermosetting resin.

11. The image-bearing laminate according to claim 8, wherein the third resin sheet contains a thermoplastic resin, and the thermoplastic resin is at least one selected from the group consisting of polyvinyl butyral resin, ethylene-vinyl acetate copolymer resin, polyurethane resin, and polyolefin resin.

12. An interlayer for laminated glass comprising the image-bearing laminate according to claim 1 or 3.

13. A laminated glass comprising the interlayer film for laminated glass according to claim 12.

14. A method for manufacturing an image-bearing laminate, comprising the steps of: preparing a first resin sheet, printing a curable ink on one side of the first resin sheet, and curing the curable ink to form an image-bearing layer; and performing a surface treatment by a surface treatment process on a second surface of the image-bearing layer opposite to the first surface side on which the first resin sheet is laminated.

15. The method for producing an image-bearing laminate according to claim 14, further comprising the step of laminating a second resin sheet on said second surface side of said image-bearing layer.

Citation Information

Patent Citations

  • Ink-jet printed rigid interlayer and a process for preparing same

    WO2004011271A1

  • Laminate and production thereof

    JP2000238195A

  • Decorative laminated glass

    JP2009078962A

  • Interlayer film for decorative laminated glass and decorative laminated glass using the same

    JP2010138008A

  • Decorative laminated glass

    JP2011190133A

Cited By