Non-aqueous electrolyte secondary battery

The non-aqueous electrolyte secondary battery's use of a lithium transition metal composite oxide with high Ni content and a sulfonic acid compound in the positive electrode, along with S in the negative electrode, addresses capacity and output challenges, enhancing performance and stability.

WO2024247772A1PCT designated stage expired Publication Date: 2024-12-05PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018426
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-05-20
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Current non-aqueous electrolyte secondary batteries face challenges in enhancing battery capacity and output characteristics, with existing technologies like those described in Patent Document 1 not adequately addressing these issues.

Method used

A non-aqueous electrolyte secondary battery configuration featuring a positive electrode with a lithium transition metal composite oxide containing 50 mol% or more Ni and a sulfonic acid compound, and a negative electrode with 200 mass ppm or more of S, which improves battery capacity and output characteristics by reducing direct current resistance.

Benefits of technology

The configuration effectively enhances battery capacity and output characteristics, suppressing discharge capacity decrease even at increased discharge rates, and improves the battery's overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018426_05122024_PF_FP_ABST
    Figure JP2024018426_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a positive electrode active material capable of improving battery capacity and output characteristics of a non-aqueous electrolyte secondary battery. This non-aqueous electrolyte secondary battery comprises a positive electrode, a negative electrode, and a non-aqueous electrolyte. The positive electrode contains a lithium transition metal composite oxide as a positive electrode active material, and a sulfonic acid compound represented by general formula I. The lithium transition metal composite oxide contains 50 mol% or more of Ni with respect to the total number of moles of metal elements excluding Li. The negative electrode contains a negative electrode active material and contains 200 ppm by mass or more of S with respect to the total mass of the negative electrode active material. (In the formula, A represents a group 1 element or a group 2 element, R represents a hydrocarbon group, and n is 1 or 2.)
Need to check novelty before this filing date? Find Prior Art

Description

Non-aqueous electrolyte secondary battery

[0001] The present disclosure relates to a non-aqueous electrolyte secondary battery.

[0002] In recent years, the applications of non-aqueous electrolyte secondary batteries have expanded to include power sources for electric vehicles and power storage devices for utilizing natural energy. The characteristics required of the positive electrode active material used in non-aqueous electrolyte secondary batteries also vary depending on the application. For example, Patent Document 1 discloses a non-aqueous electrolyte secondary battery that uses, as a positive electrode active material, a lithium transition metal composite oxide having a low-solubility Li salt scattered on its surface, with the aim of reducing reaction resistance during storage at high temperatures.

[0003] Japanese Patent Application Laid-Open No. 2019-169286

[0004] In non-aqueous electrolyte secondary batteries, it is important to improve output characteristics while maintaining high capacity. The technology described in Patent Document 1 does not adequately address this issue, and there is still room for improvement.

[0005] An object of the present disclosure is to provide a positive electrode active material that enables improvement in the battery capacity and output characteristics of a non-aqueous electrolyte secondary battery.

[0006] A non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a positive electrode, a negative electrode, and a non-aqueous electrolyte. The positive electrode includes a lithium transition metal composite oxide as a positive electrode active material and a sulfonic acid compound represented by general formula I. The lithium transition metal composite oxide contains 50 mol % or more of Ni relative to the total number of moles of metal elements excluding Li. The negative electrode includes a negative electrode active material and contains 200 mass ppm or more of S relative to the total mass of the negative electrode active material. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)

[0007] According to the positive electrode active material for a non-aqueous electrolyte secondary battery according to one aspect of the present disclosure, the battery capacity and output characteristics of the non-aqueous electrolyte secondary battery can be improved.

[0008] 1 is a longitudinal cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment of the present invention;

[0009] In general, lithium transition metal composite oxides containing Ni as a major component are known as high-capacity positive electrode active materials. From the viewpoint of increasing the battery capacity, the Ni content in the lithium transition metal composite oxide is preferably 50 mol% or more relative to the total number of moles of metal elements excluding Li. Furthermore, as a result of the inventors' studies, it has become clear that by incorporating a specific sulfonic acid compound into the positive electrode, a nonaqueous electrolyte secondary battery with improved output characteristics can be realized. This is believed to be due to the reduction in DC resistance in the positive electrode caused by the function of the sulfonic acid compound. After further intensive studies, the inventors have found that by incorporating a specific sulfonic acid compound into the positive electrode and a specific amount of S into the negative electrode as described above, the output characteristics of a nonaqueous electrolyte secondary battery can be further improved. By configuring the positive electrode and negative electrode as described above, a decrease in discharge capacity can be suppressed even when the discharge rate is increased.

[0010] An example of an embodiment of a nonaqueous electrolyte secondary battery according to the present disclosure will be described in detail below. Hereinafter, a cylindrical battery in which a wound electrode assembly is housed in a cylindrical exterior body will be exemplified. However, the electrode assembly is not limited to the wound type and may be a laminated type in which multiple positive electrodes and multiple negative electrodes are alternately stacked one by one with separators interposed therebetween. Furthermore, the exterior body is not limited to a cylindrical shape and may be, for example, prismatic or coin-shaped, or may be a battery case made of a laminate sheet including a metal layer and a resin layer.

[0011] FIG. 1 is an axial cross-sectional view of a cylindrical secondary battery 10 according to an embodiment. As shown in FIG. 1 , the secondary battery 10 includes a wound electrode assembly 14, an electrolyte, and an exterior body 16 that accommodates the electrode assembly 14 and the electrolyte. The electrode assembly 14 includes a positive electrode 11, a negative electrode 12, and a separator 13, and has a wound structure in which the positive electrode 11 and the negative electrode 12 are spirally wound with the separator 13 interposed therebetween. The exterior body 16 is a cylindrical metal container with a bottom and an opening on one axial side, and the opening of the exterior body 16 is closed by a sealing body 17. Hereinafter, for convenience of explanation, the sealing body 17 side of the battery will be referred to as the top, and the bottom side of the exterior body 16 will be referred to as the bottom.

[0012] The positive electrode 11, negative electrode 12, and separator 13 constituting the electrode assembly 14 are all rectangular, elongated bodies that are spirally wound in the longitudinal direction and alternately stacked in the radial direction of the electrode assembly 14. The separator 13 isolates the positive electrode 11 and the negative electrode 12 from each other. The negative electrode 12 is formed to be slightly larger than the positive electrode 11 to prevent lithium precipitation. That is, the negative electrode 12 is formed to be longer than the positive electrode 11 in the longitudinal and lateral directions. The two separators 13 are formed to be at least slightly larger than the positive electrode 11 and are arranged, for example, to sandwich the positive electrode 11. The electrode assembly 14 includes a positive electrode lead 20 connected to the positive electrode 11 by welding or the like, and a negative electrode lead 21 connected to the negative electrode 12 by welding or the like. In the electrode assembly 14, the longitudinal direction of the positive electrode 11 and the negative electrode 12 is the winding direction, and the lateral direction of the positive electrode 11 and the negative electrode 12 is the axial direction. That is, the end faces in the lateral direction of the positive electrode 11 and the negative electrode 12 form the end faces in the axial direction of the electrode body 14 .

[0013] Insulating plates 18 and 19 are disposed above and below the electrode body 14. In the example shown in Fig. 1 , the positive electrode lead 20 passes through a through hole in the insulating plate 18 and extends toward the sealing body 17, and the negative electrode lead 21 passes outside the insulating plate 19 and extends toward the bottom side of the exterior body 16. The positive electrode lead 20 is connected to the underside of an internal terminal plate 23 of the sealing body 17 by welding or the like, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the internal terminal plate 23, serves as the positive electrode terminal. The negative electrode lead 21 is connected to the inner bottom surface of the exterior body 16 by welding or the like, and the exterior body 16 serves as the negative electrode terminal.

[0014] A gasket 28 is provided between the exterior body 16 and the sealing body 17 to ensure airtightness inside the battery. The exterior body 16 has a grooved portion 22 formed on its side surface that protrudes inward and supports the sealing body 17. The grooved portion 22 is preferably formed in an annular shape along the circumferential direction of the exterior body 16, and supports the sealing body 17 on its top surface. The sealing body 17 is fixed to the top of the exterior body 16 by the grooved portion 22 and the open end of the exterior body 16 that is crimped to the sealing body 17.

[0015] The sealing body 17 has a structure in which, in order from the electrode body 14 side, an internal terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked. Each member constituting the sealing body 17 has, for example, a disk or ring shape, and each member except for the insulating member 25 is electrically connected to one another. The lower valve body 24 and the upper valve body 26 are connected at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, the lower valve body 24 deforms and breaks, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.

[0016] The positive electrode 11, the negative electrode 12, the separator 13, and the non-aqueous electrolyte that constitute the secondary battery 10 will be described in detail below, with the positive electrode 11 being particularly described.

[0017] The positive electrode 11 has, for example, a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core. The positive electrode mixture layer is preferably formed on both sides of the positive electrode core. The positive electrode core can be made of a foil of a metal, such as aluminum or an aluminum alloy, that is stable within the potential range of the positive electrode 11, or a film with such a metal disposed on the surface. The thickness of the positive electrode core is, for example, 10 μm or more and 30 μm or less.

[0018] The positive electrode mixture layer contains, for example, a positive electrode active material, a conductive agent, and a binder. The thickness of the positive electrode mixture layer is, for example, 10 μm to 150 μm on one side of the positive electrode core. The positive electrode 11 can be produced, for example, by applying a positive electrode mixture slurry containing the positive electrode active material, the conductive agent, etc. to the surface of the positive electrode core, drying the coating, and then rolling it to form a positive electrode mixture layer on both sides of the positive electrode core.

[0019] Examples of the conductive agent contained in the positive electrode mixture layer include carbon black (CB) such as acetylene black (AB) and ketjen black, carbon nanotubes (CNT), graphene, and carbon-based particles such as graphite. These may be used alone or in combination of two or more. The content of the conductive agent in the positive electrode mixture layer is, for example, 0.1% by mass or more and 10% by mass or less with respect to the total mass of the positive electrode mixture layer.

[0020] When the solvent of the positive electrode mixture slurry is organic, examples of binders contained in the positive electrode mixture layer include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyimide resins, acrylic resins, polyolefin resins, and polyacrylonitrile (PAN). When the solvent of the positive electrode mixture slurry is aqueous, examples of binders contained in the positive electrode mixture layer include styrene-butadiene rubber (SBR), nitrile-butadiene rubber (NBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc., or a partially neutralized salt), and polyvinyl alcohol (PVA). In either case, one type of binder may be used alone, or two or more types may be used in combination. The content of the binder in the positive electrode mixture layer is, for example, 0.1% by mass or more and 10% by mass or less, relative to the total mass of the positive electrode mixture layer.

[0021] The positive electrode active material contained in the positive electrode mixture layer includes a lithium transition metal composite oxide. The lithium transition metal composite oxide contains 50 mol% or more of Ni relative to the total number of moles of metal elements excluding Li. This improves battery capacity. The Ni content in the lithium transition metal composite oxide is preferably 80 mol% or more, more preferably 90 mol% or more, relative to the total number of moles of metal elements excluding Li. Furthermore, from the viewpoint of structural stabilization, the Ni content is preferably 98 mol% or less.

[0022] The lithium transition metal composite oxide may further contain one or more elements selected from the group consisting of Co, Al, and Mn. The contents of Co, Al, and Mn in the lithium transition metal composite oxide are each, for example, 0 mol % or more and 30 mol % or less relative to the total number of moles of metal elements excluding Li. The total content of Co, Al, and Mn is, for example, 0 mol % or more and 50 mol % or less.

[0023] The lithium transition metal composite oxide is, for example, a compound represented by the general formula Li a Ni x M1 y M2 z O 2-b (wherein 0.8≦a≦1.2, 0.50≦x≦0.98, 0≦y≦0.50, 0≦z≦0.05, 0≦b≦0.05, x+y+z=1, M1 is one or more elements selected from the group consisting of Co, Al, and Mn, and M2 is one or more elements selected from the group consisting of Sr, Ca, Nb, Ti, Zr, and W). The proportion of metal elements contained in the lithium transition metal composite oxide can be measured, for example, by inductively coupled plasma atomic emission spectrometry (ICP-AES).

[0024] The lithium transition metal composite oxide contains, for example, secondary particles formed by aggregation of primary particles. The particle size of the primary particles is, for example, 0.02 μm or more and 2 μm or less. The particle size of the primary particles is measured as the diameter of the circumscribed circle in a particle image observed with a scanning electron microscope (SEM). The average particle size of the secondary particles is, for example, 2 μm or more and 30 μm or less. Here, the average particle size refers to the volume-based median diameter (D50). D50 refers to the particle size at which the cumulative frequency in the volume-based particle size distribution is 50% from the smallest particle size, and is also called the median diameter. The particle size distribution of the secondary particles can be measured using a laser diffraction particle size distribution analyzer (e.g., MT3000II, manufactured by Microtrac-Bell Corporation) using water as a dispersion medium.

[0025] The lithium transition metal composite oxide may have a layered structure. Examples of the layered structure of the lithium transition metal composite oxide include a layered structure belonging to the space group R-3m and a layered structure belonging to the space group C2 / m. From the viewpoints of increasing capacity and stability of the crystal structure, the lithium transition metal composite oxide preferably has a layered structure belonging to the space group R-3m. The layered structure of the lithium transition metal composite oxide may include a transition metal layer, a Li layer, and an oxygen layer.

[0026] A metal compound containing a metal element such as W, Zr, Al, or a rare earth element may be present on the surface of the lithium transition metal composite oxide. Examples of the W-containing compound include WO 3 Examples of the compound containing Al include Al 2 O 3 Examples of compounds containing Zr include ZrO 2 , Zr(OH) 4 , Zr(CO 3 ) 2 and Zr(SO 4 ) 2 ・4H 2 Examples of rare earth-containing compounds include oxides, hydroxides, carbonates, sulfates, nitrates, and phosphates of rare earth elements. The metal compounds may contain these metal elements together with Ca or Sr, and examples thereof include SrAlO 4 , CaAlO 4 The metal compound may further contain Li, and an example thereof is lithium tungstate.

[0027] A nonmetallic compound may be present on the surface of the lithium transition metal composite oxide. The nonmetallic compound contains, for example, one or more nonmetallic elements selected from the group consisting of P and B. Examples of the P-containing compound include Li, 3-x H x P.O. 4 (0≦x≦3) can be exemplified. 3 BO 3 , Li 3 BO 3 , Li 2 B 4 O7 Examples include:

[0028] The positive electrode mixture layer may contain, in addition to the positive electrode active material of the present embodiment, other positive electrode active materials, such as a lithium transition metal composite oxide having a Ni content of less than 50 mol %.

[0029] The positive electrode 11 further contains a sulfonic acid compound represented by the following general formula I. In the positive electrode 11, the positive electrode mixture layer may contain the sulfonic acid compound. When the positive electrode 11 contains the sulfonic acid compound, Li in the positive electrode 11 + This makes insertion / detachment of the ions more likely to occur, reducing the DC resistance and improving the output characteristics. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)

[0030] The sulfonic acid compound is preferably present on the surface of the lithium transition metal composite oxide. By having the sulfonic acid compound present on the surface of the lithium transition metal composite oxide, the Li + This makes it easier for insertion / desorption to occur, and the effect of reducing the DC resistance becomes more pronounced.

[0031] In the above general formula I, A is preferably a Group 1 element, more preferably Li. This can further reduce the DC resistance. Note that when A is a Group 1 element, n=1.

[0032] In general formula I, R is preferably an alkyl group. R is more preferably an alkyl group having 5 or less carbon atoms, further preferably an alkyl group having 3 or less carbon atoms, and particularly preferably a methyl group. In addition, in R, some of the hydrogen atoms bonded to the carbon atoms may be substituted with fluorine. However, in R, not all of the hydrogen atoms bonded to the carbon atoms are substituted with fluorine. The smaller the molecular weight of R, the smaller the DC resistance can be.

[0033] Examples of sulfonic acid compounds include lithium methanesulfonate, lithium ethanesulfonate, lithium propanesulfonate, sodium methanesulfonate, magnesium methanesulfonate, and lithium fluoromethanesulfonate.

[0034] The amount of the sulfonic acid compound contained in the positive electrode 11 is preferably 0.1% by mass or more and 2% by mass or less, and more preferably 0.25% by mass or more and 1.0% by mass or less, relative to the mass of the lithium transition metal composite oxide.

[0035] The presence of the sulfonic acid compound in the positive electrode 11 can be confirmed by Fourier transform infrared spectroscopy (FT-IR). In the infrared absorption spectrum obtained by FT-IR, the positive electrode 11 exhibits a peak at 1238 cm -1 , 1175 cm -1 , 1065 cm -1 , 785 cm -1 It may have an absorption peak at at least one point in the vicinity.

[0036] In the infrared absorption spectrum obtained by FT-IR, for example, the positive electrode 11 containing lithium methanesulfonate has a peak at 1238 cm -1 , 1175 cm -1 , 1065 cm -1 , 785 cm -1 It has an absorption peak around 1238 cm -1 , 1175 cm -1 , 1065 cm -1 The peak around 785 cm is an absorption peak due to the SO stretching vibration of lithium methanesulfonate. -1 The peak in the vicinity is an absorption peak due to the C-S stretching vibration derived from lithium methanesulfonate.

[0037] In the case of the positive electrode 11 containing a sulfonic acid compound other than lithium methanesulfonate, an absorption peak derived from the sulfonic acid compound can be identified, similar to the case of the positive electrode 11 containing lithium methanesulfonate. The presence of the sulfonic acid compound in the positive electrode 11 can also be confirmed by ICP, atomic absorption spectroscopy, X-ray photoelectron spectroscopy (XPS), synchrotron XRD measurement, and TOF-SIMS.

[0038] The presence of the sulfonic acid compound in the positive electrode 11 can be confirmed by proton nuclear magnetic resonance spectroscopy (H-NMR). For example, a positive electrode 11 containing a sulfonic acid compound (methanesulfonic acid compound) in which R in the above general formula I is a methyl group exhibits a single peak in H-NMR analysis at a position chemically shifted by 2.76 ppm to 2.86 ppm relative to the methyl group of tetramethylsilane. The chemical shift may be 2.81 ppm to 2.86 ppm. In a positive electrode 11 containing a sulfonic acid compound other than a methanesulfonic acid compound, the presence of the sulfonic acid compound can be confirmed by observing the peak shift due to the sulfonic acid compound corresponding to the respective compound, as in the case of a positive electrode 11 containing a methanesulfonic acid compound.

[0039] Measurement by H-NMR can be carried out, for example, as follows. (Pretreatment) 3 mL of heavy water is added to 0.40 g of the positive electrode mixture layer removed from the positive electrode 11, stirred for 1 minute, allowed to stand for 15 hours, and then filtered through a syringe filter to obtain a filtrate. (NMR Measurement) NMR measurement is carried out on the filtrate under the following conditions. Equipment used: ECX-400 manufactured by JEOL Ltd. Measurement solvent: D 2 O Measurement temperature: 25°C Observation nucleus: 1H Observation frequency: 395.884MHz Pulse irradiation power: 2dB Pulse width: 3.6μsec Signal acquisition time: 11.0sec Repetition time: 55sec Number of integrations: 64 Observation width: 7.4kHz Observation center: 5ppm

[0040] The positive electrode 11 containing a lithium transition metal composite oxide and a sulfonic acid compound can be produced, for example, by forming a positive electrode mixture layer using a positive electrode mixture slurry prepared by kneading a sulfonic acid compound with a lithium transition metal composite oxide, a conductive agent, a binder, etc. Alternatively, the positive electrode 11 containing a lithium transition metal composite oxide and a sulfonic acid compound may be produced using a positive electrode active material in which a sulfonic acid compound is attached to the surface of a lithium transition metal composite oxide. Below, an example of a method for producing a positive electrode active material in which a sulfonic acid compound is attached to the surface of a lithium transition metal composite oxide is described. Note that the production method described here is merely an example, and the production of a positive electrode active material is not limited to this method.

[0041] The manufacturing process of the positive electrode active material includes a synthesis step of obtaining a lithium transition metal composite oxide, a washing step of washing the lithium transition metal composite oxide obtained in the synthesis step with water and dehydrating it to obtain a cake-like composition, an adding step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition obtained in the washing step, and a drying step of drying the cake-like composition to obtain a powder-like composition.

[0042] In the synthesis step, a mixture is obtained by mixing a metal oxide with a Li raw material. The metal oxide can be produced by dropping an alkaline solution such as sodium hydroxide into a solution of a metal salt containing Ni, Co, Al, Mn, etc. while stirring it, adjusting the pH to the alkaline side (e.g., 8.5 to 12.5), thereby precipitating (co-precipitating) a composite hydroxide, and then heat-treating the metal hydroxide. The calcination temperature is not particularly limited, but is, for example, in the range of 250°C to 600°C. The Li raw material can be, for example, Li 2 CO 3 , LiOH, Li 2 O 2 , Li 2 O, LiNO 3 , LiNO 2 , Li 2 SO 4 , LiOH·H 2 Examples of the M2 raw material include SrO, CaO, Nb, Ti, Zr, and W. In addition, when mixing, an M2 raw material may be mixed to add M2, which is one or more elements selected from the group consisting of Sr, Ca, Nb, Ti, Zr, and W. Examples of the M2 raw material include SrO, CaO, Nb 2 O 5 , TiO 2 , ZrO 2 , W.O. 3 etc.

[0043] The synthesis step includes a calcination step in which the mixture is calcined to obtain a lithium transition metal composite oxide. The calcination step includes, for example, a first calcination step in which calcination is performed at a first temperature increase rate to a first set temperature of 300°C or higher and 680°C or lower, and a second calcination step in which calcination is performed from the first set temperature to a second set temperature of higher than 680°C and lower than 800°C at a second temperature increase rate. The first temperature increase rate is, for example, in the range of 0.2°C / min to 4.5°C / min, and the second temperature increase rate is, for example, in the range of 0.1°C / min to less than 10°C / min. Note that in each of the first calcination step and the second calcination step, further subdivided temperature ranges may be set to perform multi-stage calcination.

[0044] The holding time of the first set temperature in the first firing step is preferably 5 hours or less, more preferably 3 hours or less. The holding time of the first set temperature is the time during which the first set temperature is maintained after reaching the first set temperature, and the holding time may be zero. The holding time of the second set temperature in the second firing step is preferably 1 hour to 10 hours, more preferably 1 hour to 5 hours. The holding time of the second set temperature is the time during which the second set temperature is maintained after reaching the second set temperature. The firing of the mixture is carried out, for example, in an oxygen stream with an oxygen concentration of 60% or more, and the flow rate of the oxygen stream is set to 10 cm / min. 3 The flow rate shall be 0.2 mL / min to 4 mL / min per kg of the mixture or 0.3 L / min or more per kg of the mixture.

[0045] The synthesis process is not limited to the above process, and a precursor obtained by co-precipitation or mixing of a compound such as a hydroxide, oxide, or carbonate compound containing at least one of Ni, M1, or M2 (M1 is one or more elements selected from the group consisting of Co, Al, and Mn, and M2 is one or more elements selected from the group consisting of Sr, Ca, Nb, Ti, Zr, and W) may be used instead of the metal oxide. If the precursor does not contain compounds such as M1 or M2, the compounds may be added and mixed when mixing the precursor with the Li raw material. Furthermore, these compounds may be pulverized to appropriately change the particle shape or particle size, or may be used after adjusting the water content by including a hydrate.

[0046] In the washing step, the lithium transition metal composite oxide is washed with water and dehydrated to obtain a cake-like composition. The particulate lithium transition metal composite oxide obtained in the synthesis step can be used. By washing with water, unreacted lithium compounds added in the synthesis step and impurities other than the lithium compounds can be removed. When washing with water, for example, 300 g to 5000 g of lithium transition metal composite oxide is added to 1 L of water. The water washing may be repeated multiple times. The dehydration after washing can be performed, for example, using a filter press.

[0047] In the drying step, the cake-like composition obtained in the washing step is dried to obtain a powdery composition. The drying step may be performed in a vacuum atmosphere. The drying conditions are, for example, 150°C to 400°C and 0.5 hours to 15 hours.

[0048] In the addition step, at least one of a sulfonic acid compound and a sulfonic acid solution is added to the cake-like composition obtained in the washing step or the powder-like composition obtained in the drying step. This allows the sulfonic acid compound to adhere to the surface of the lithium transition metal composite oxide. It is preferable to add at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition. The sulfonic acid compound may be in either powder or solution form. The sulfonic acid solution is, for example, a methanesulfonic acid solution obtained by dissolving methanesulfonic acid in water. Li compounds remain in the cake-like composition, and these remaining Li compounds are dissolved in the water contained in the cake-like composition. Therefore, even when a sulfonic acid solution is added, a Li-containing sulfonic acid compound is formed. From the viewpoint of more easily achieving the effects of the present application, a Li compound or a Li compound solution may be added to the cake-like composition or the powder-like composition together with the sulfonic acid solution. Alternatively, a mixed solution in which a sulfonic acid solution and a Li compound or a Li compound solution are premixed may be added to the cake-like composition or the powder-like composition. The Li compound is, for example, LiOH, and the Li compound solution is, for example, a LiOH solution obtained by dissolving LiOH in water. The amounts of the Li compound and sulfonic acid solution added to the cake-like composition preferably satisfy the relationship of 0≦Li compound / sulfonic acid≦1.3 in molar ratio. The amount of sulfonic acid compound or sulfonic acid added is preferably 0.1% by mass or more and 2% by mass or less relative to the mass of the lithium transition metal composite oxide. The concentrations of the sulfonic acid solution and the sulfonic acid compound solution are, for example, 0.5% by mass or more and 40% by mass or less. The addition step may be performed during the washing step, after the washing step, during the drying step, or after the drying step, and the timing of the addition can be changed as appropriate.

[0049] A metal compound containing one or more metal elements selected from the group consisting of W, Zr, Al, and rare earth elements, and a nonmetallic compound containing one or more nonmetallic elements selected from the group consisting of P and B can be attached to the surface of the lithium transition metal composite oxide by adding the raw material of the metal compound or nonmetallic compound during the synthesis process, after the synthesis process, during the washing process, after the washing process, during the drying process, after the drying process, or during the addition process. 4 , ZrO 2 , Zr(CO 3 ) 2 , Zr(SO 4 ) 2 ・4H 2 These metal compounds may be pulverized to appropriately change the particle size, and the amount of water, including hydrates, may be adjusted before use. Examples of rare earth raw materials include oxides, hydroxides, carbonates, etc. of rare earth elements. Examples of W raw materials include tungsten oxide (WO 3 ), lithium tungstate (Li 2 WO 4 , Li 4 WO 5 , Li 6 W 2 O 9 As the W raw material, a solution containing W may be used. As the Al raw material, Al 2 O 3、 Al(OH) 3、 Al 2 (SO 4 ) 3 The P raw material may be Al derived from a lithium transition metal composite oxide. 3-x H x P.O. 4 (0≦x≦3) and the like. 3 BO 3 , Li 3 BO 3 , Li 2 B 4 O 7 , LiBO 2 In addition, when the liquid raw material is added after the drying step, a heat treatment may be carried out to evaporate the water.

[0050] [Negative Electrode] The negative electrode 12 has, for example, a negative electrode current collector and a negative electrode mixture layer formed on the surface of the negative electrode current collector. The negative electrode mixture layer is preferably formed on both sides of the negative electrode current collector. The negative electrode current collector can be a foil of a metal that is stable within the potential range of the negative electrode 12, such as copper or a copper alloy, or a film with such a metal disposed on the surface layer. The negative electrode mixture layer may contain a negative electrode active material and a binder. The thickness of the negative electrode mixture layer is, for example, 10 μm or more and 150 μm or less on one side of the negative electrode current collector.

[0051] The negative electrode active material contained in the negative electrode mixture layer is not particularly limited as long as it can reversibly absorb and release lithium ions, and generally, carbon materials such as graphite are used. Graphite may be any of natural graphite such as flake graphite, lump graphite, and amorphous graphite, or artificial graphite such as lump artificial graphite and graphitized mesophase carbon microbeads. Furthermore, metals that alloy with Li, such as Si and Sn, metal compounds containing Si, Sn, and lithium-titanium composite oxides may also be used as the negative electrode active material. Furthermore, those provided with a carbon coating may also be used. For example, SiO x (0.5≦x≦1.6) or Li 2y SiO (2+y) A Si-containing compound in which fine particles of Si are dispersed in a lithium silicate phase represented by (0<y<2) may be used in combination with graphite.

[0052] Examples of binders contained in the negative electrode mixture layer include styrene butadiene rubber (SBR), nitrile butadiene rubber (NBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc., or a partially neutralized salt), polyvinyl alcohol (PVA), etc. These may be used alone or in combination of two or more.

[0053] The negative electrode 12 further contains 200 ppm by mass or more of S relative to the total mass of the negative electrode active material. The negative electrode mixture layer of the negative electrode 12 may contain S. By incorporating a sulfonic acid compound into the positive electrode 11 and incorporating 200 ppm by mass or more of S relative to the total mass of the negative electrode active material into the negative electrode 12, the output characteristics of the secondary battery 10 are further improved. The S content in the negative electrode 12 can be quantified, for example, using an inductively coupled plasma atomic emission spectrometry (ICP-AES).

[0054] The negative electrode 12 may contain a sulfonic acid compound represented by the following general formula I. That is, the negative electrode 12 may contain the sulfonic acid compound so that the negative electrode 12 contains 200 mass ppm or more of S relative to the total mass of the negative electrode active material. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)

[0055] In the above general formula I, A is preferably a Group 1 element, more preferably Li. This can further reduce the DC resistance. When A is a Group 1 element, n = 1. In the above general formula I, R is preferably an alkyl group. R is more preferably an alkyl group having 5 or less carbon atoms, even more preferably an alkyl group having 3 or less carbon atoms, and particularly preferably a methyl group. In R, some of the hydrogen atoms bonded to the carbon atoms may be substituted with fluorine. However, in R, not all of the hydrogen atoms bonded to the carbon atoms are substituted with fluorine. The smaller the molecular weight of R, the lower the DC resistance can be. Examples of sulfonic acid compounds include lithium methanesulfonate, lithium ethanesulfonate, lithium propanesulfonate, sodium methanesulfonate, magnesium methanesulfonate, and lithium fluoromethanesulfonate.

[0056] The presence of the sulfonic acid compound in the negative electrode 12 can be confirmed by Fourier transform infrared spectroscopy (FT-IR), proton nuclear magnetic resonance spectroscopy (H-NMR), or the like, as in the case of the positive electrode 11.

[0057] The negative electrode 12 can be produced, for example, by applying a negative electrode mixture slurry containing a negative electrode active material, a sulfonic acid compound, a binder, and the like to the surface of a negative electrode current collector, drying the coating, and then rolling the coating to form a negative electrode mixture layer on both sides of the negative electrode current collector.

[0058] [Separator] A porous sheet having ion permeability and insulating properties is used for the separator 13. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator 13 include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may have a single-layer structure or a multi-layer structure. Furthermore, a highly heat-resistant resin layer such as an aramid resin may be formed on the surface of the separator 13.

[0059] A filler layer containing an inorganic filler may be formed at the interface between the separator 13 and at least one of the positive electrode 11 and the negative electrode 12. Examples of inorganic fillers include oxides and phosphate compounds containing metal elements such as Ti, Al, Si, and Mg. The filler layer can be formed by applying a slurry containing the filler to the surface of the positive electrode 11, the negative electrode 12, or the separator 13.

[0060] [Non-aqueous electrolyte] The non-aqueous electrolyte has, for example, lithium ion conductivity. The non-aqueous electrolyte may be a liquid electrolyte (electrolytic solution) or a solid electrolyte.

[0061] The liquid electrolyte (electrolytic solution) contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent that can be used include esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more of these. The non-aqueous solvent may contain a halogen-substituted compound in which at least a portion of the hydrogen atoms in these solvents are substituted with halogen atoms such as fluorine. Examples of the halogen-substituted compound include fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, and fluorinated chain carboxylic acid esters such as methyl fluoropropionate (FMP).

[0062] Examples of the esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylic acid esters such as γ-butyrolactone (GBL) and γ-valerolactone (GVL); and chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP).

[0063] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ethers, 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, and methyl phenyl ether. and chain ethers such as ethyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.

[0064] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiClO 4 , LiBF 4 , LiPF 6 , LiAlCl 4 , LiSbF 6 , LiSCN, LiCF3 SO 3 , LiCF 3 CO 2 , LiAsF 6 , LiB 10 Cl 10 , lower aliphatic lithium carboxylates, LiCl, LiBr, LiI, phosphates, borates, and imide salts. Examples of phosphates include lithium difluorophosphate (LiPO 2 F 2 Examples of the borate salt include lithium bis(oxalato)borate (LiBOB) and lithium difluoro(oxalato)borate (LiDFFOB). Examples of the imide salt include lithium bisfluorosulfonylimide (LiN(FSO 2 ) 2 ), lithium bistrifluoromethanesulfonyl imide (LiN(CF 3 SO 2 ) 2 ), lithium trifluoromethanesulfonate nonafluorobutanesulfonate imide (LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 )), lithium bispentafluoroethanesulfonyl imide (LiN(C 2 F 5 SO 2 ) 2 Among these, LiPF is preferred from the viewpoint of ionic conductivity, electrochemical stability, etc. 6 The concentration of the lithium salt may be, for example, 4 mol or less, or 3 mol or less, preferably 1.8 mol or less, and more preferably 0.8 mol or more and 1.8 mol or less, per 1 L of the non-aqueous solvent.

[0065] The non-aqueous electrolyte may contain an additive such as an unsaturated carbonate ester, an acid anhydride, a phenol compound, a benzene compound, a nitrile compound, an isocyanate compound, a sultone compound, a sulfate compound, a borate ester compound, a phosphate ester compound, or a phosphite ester compound.

[0066] Examples of unsaturated cyclic carbonates include vinylene carbonate, 4-methylvinylene carbonate, 4,5-dimethylvinylene carbonate, 4-ethylvinylene carbonate, 4,5-diethylvinylene carbonate, 4-propylvinylene carbonate, 4,5-dipropylvinylene carbonate, 4-phenylvinylene carbonate, 4,5-diphenylvinylene carbonate, vinylethylene carbonate, and divinylethylene carbonate. One type of unsaturated cyclic carbonate may be used alone, or two or more types may be used in combination. Some of the hydrogen atoms in the unsaturated cyclic carbonate may be substituted with fluorine atoms. The acid anhydride may be an anhydride formed by intermolecular condensation of multiple carboxylic acid molecules, but is preferably an acid anhydride of a polycarboxylic acid. Examples of polycarboxylic acid anhydrides include succinic anhydride, maleic anhydride, and phthalic anhydride.

[0067] Examples of phenolic compounds include phenol, hydroxytoluene, etc. Examples of benzene compounds include fluorobenzene, hexafluorobenzene, cyclohexylbenzene (CHB), etc.

[0068] Examples of nitrile compounds include adiponitrile, pimelonitrile, propionitrile, and succinonitrile. Examples of isocyanate compounds include methyl isocyanate (MIC), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), and bisisocyanatomethylcyclohexane (BIMCH). Examples of sultone compounds include propane sultone and propene sultone. Examples of sulfate compounds include ethylene sulfate, ethylene sulfite, dimethyl sulfate, and lithium fluorosulfate. Examples of borate ester compounds include trimethyl borate and tris(trimethylsilyl)borate. Examples of phosphate ester compounds include trimethyl phosphate and tris(trimethylsilyl)phosphate. Examples of phosphite ester compounds include trimethyl phosphite and tris(trimethylsilyl)phosphite.

[0069] As the solid electrolyte, for example, a solid or gel-like polymer electrolyte, an inorganic solid electrolyte, etc. can be used. As the inorganic solid electrolyte, a material known in all-solid-state lithium ion secondary batteries, etc. (for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a halogen-based solid electrolyte, etc.) can be used. The polymer electrolyte includes, for example, a lithium salt and a matrix polymer, or a non-aqueous solvent, a lithium salt, and a matrix polymer. As the matrix polymer, for example, a polymer material that absorbs the non-aqueous solvent and gels is used. As the polymer material, for example, a fluororesin, an acrylic resin, a polyether resin, etc. can be used.

[0070] The non-aqueous electrolyte preferably contains 200 mass ppm or less of S relative to the total mass of the non-aqueous electrolyte. This further improves the output characteristics of the secondary battery. The S content in the non-aqueous electrolyte can be quantified, for example, by an inductively coupled plasma atomic emission spectrometer (ICP-AES). The S content in the non-aqueous electrolyte can be determined, for example, by measuring the S content in propane sultone (C 3 H 6 O 3The content of sulfur can be adjusted by adding an additive containing sulfur such as sulfur (S).

[0071] Hereinafter, the present disclosure will be further described with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.

[0072] Example 1 Preparation of Positive Electrode Active Material [Ni 0.90 Co 0.05 Al 0.05 ](OH) 2 The composite hydroxide represented by the formula (1) was calcined at 500°C for 8 hours to obtain a metal oxide containing Ni, Co, and Al. Next, lithium hydroxide monohydrate (LiOH·H) was added to the composite hydroxide represented by the formula (1) so that the molar ratio of the total amount of Ni, Co, and Al to Li was 1:1.03. 2 This mixture was placed under an oxygen flow (10 cm) with an oxygen concentration of 95%. 3 The mixture was heated from room temperature to 650°C at a heating rate of 2.0°C / min under a temperature of 2 mL / min per 1 kg of the mixture and 5 L / min per 1 kg of the mixture, and then heated from 650°C to 740°C at a heating rate of 0.5°C / min to obtain a lithium transition metal composite oxide (synthesis step).

[0073] Water was added to the lithium transition metal composite oxide obtained in the synthesis step to a slurry concentration of 1500 g / L, followed by stirring for 15 minutes and filtration to obtain a cake-like composition (washing step). Powdered lithium methanesulfonate was added to this cake-like composition (addition step). The amount of lithium methanesulfonate added was 0.3 mass% relative to the total mass of the lithium transition metal composite oxide. After the addition step, a drying step was performed under conditions of 180°C and 2 hours in a vacuum atmosphere to obtain the positive electrode active material of Example 1. Fourier transform infrared spectroscopy (FT-IR) confirmed the presence of lithium methanesulfonate on the surface of the positive electrode active material. Measurement of the positive electrode active material using an inductively coupled plasma (ICP) atomic emission spectrometer (ICP-AES) confirmed the presence of the elements shown in Table 1 below, excluding Li and O.

[0074] [Preparation of Positive Electrode] 92 parts by mass of the above positive electrode active material, 5 parts by mass of acetylene black (AB), and 3 parts by mass of polyvinylidene fluoride (PVDF) were mixed, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to prepare a positive electrode mixture slurry. Next, the positive electrode mixture slurry was applied to both sides of a positive electrode core made of aluminum foil, and after drying the coating, the coating was rolled with a rolling roller and cut to a predetermined electrode size to prepare a positive electrode. In addition, an exposed portion in which the surface of the positive electrode core was exposed was provided in a part of the positive electrode.

[0075] [Preparation of Negative Electrode] Natural graphite was used as the negative electrode active material. The negative electrode active material, sodium carboxymethyl cellulose (CMC-Na), styrene-butadiene rubber (SBR), and lithium methanesulfonate were mixed in an aqueous solution at a solids mass ratio of 100:1:1:0.08 to prepare a negative electrode mixture slurry. Next, the negative electrode mixture slurry was applied to both sides of a negative electrode core made of copper foil, and after drying the coating, the coating was rolled with a rolling roller and cut to a predetermined electrode size to prepare a negative electrode. Note that an exposed portion was provided in part of the negative electrode, exposing the surface of the negative electrode core. The sulfur content of the negative electrode was measured using an inductively coupled plasma (ICP) atomic emission spectrometer (ICP-AES), and was found to be 250 ppm by mass relative to the total mass of the negative electrode active material.

[0076] [Preparation of non-aqueous electrolyte] A mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 3:3:4 was added to a non-aqueous electrolyte solution containing lithium hexafluorophosphate (LiPF 6 ) was dissolved in the solution to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.

[0077] [Preparation of Test Cell] A positive electrode lead was attached to the exposed portion of the positive electrode, and a negative electrode lead was attached to the exposed portion of the negative electrode, and the positive and negative electrodes were spirally wound with a polyolefin separator interposed therebetween to prepare a wound electrode assembly. This electrode assembly was housed in an exterior body made of an aluminum laminate sheet, and the nonaqueous electrolyte was poured into it. The opening of the exterior body was then sealed to obtain a test cell.

[0078] [Evaluation of Output Characteristics] At an ambient temperature of 25°C, the test cell was charged at a constant current of 0.2C to 4.2V, and then charged at a constant voltage of 4.2V to 0.02C. The test cell was then left to stand for 1 hour, and then discharged at a constant current of 0.2C to 2.5V, returning the test cell to its initial state. Next, the test cell in this initial state was again charged at a constant current of 0.2C to 4.2V, then charged at a constant voltage of 4.2V to 0.02C, and then discharged at a constant current of 0.5C to 2.5V, and the discharge capacity at this time was defined as the 0.5C discharge capacity. After a 10-minute break, the test cell was discharged at a constant current of 0.02C to 2.5V, and the discharge capacity at this time was defined as the 0.02C discharge capacity. The output characteristics were calculated using the following formula: Output characteristics = (0.5C discharge capacity) / (0.5C discharge capacity + 0.02C discharge capacity).

[0079] Examples 2 to 5 Test cells were produced and evaluated in the same manner as in Example 1, except that the amount of lithium methanesulfonate added in the preparation of the positive electrode active material and the amount of lithium methanesulfonate added in the preparation of the negative electrode were changed as shown in Table 1, and in Example 5, the nonaqueous electrolyte was prepared as shown below.

[0080] Preparation method of non-aqueous electrolyte in Example 5 A non-aqueous electrolyte was prepared by mixing ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 3:3:4 in 100 parts by mass of a solvent. 3 H 6 O 3 0.4 parts by mass of lithium hexafluorophosphate (LiPF S) was added to the mixed solvent to prepare a mixed solvent. 6 ) was dissolved in the solution to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.

[0081] Example 6 A test cell was prepared and evaluated in the same manner as in Example 1, except that lithium methanesulfonate was not added in the preparation of the positive electrode active material, lithium methanesulfonate was mixed with the positive electrode active material, AB, and PVDF in the preparation of the positive electrode to prepare a positive electrode mixture slurry, and the amount of lithium methanesulfonate added in the preparation of the negative electrode was changed as shown in Table 1. The amount of lithium methanesulfonate added was 0.5% by mass with respect to the total mass of the lithium transition metal composite oxide.

[0082] <Comparative Example 1> A test cell was prepared and evaluated in the same manner as in Example 1, except that the amount of lithium methanesulfonate added in the preparation of the positive electrode active material was changed to 0.5 mass %, and that no lithium methanesulfonate was added in the preparation of the negative electrode.

[0083] The evaluation results of the test cells of the examples and comparative examples are shown in Table 1. In Table 1, the output characteristics of the test cells of the examples are expressed relative to the output characteristics of the test cell of Comparative Example 1, which is set to 100. Table 1 also shows the amounts of sulfonic acid compound added to the positive electrode and negative electrode, the S content in the negative electrode, and the S content in the non-aqueous electrolyte. The S content in the non-aqueous electrolyte was obtained by ICP-AES analysis of the non-aqueous electrolyte taken out of the test cell after the output characteristics were evaluated.

[0084]

[0085] In Table 1, the test cells of the examples have improved output characteristics compared to the test cells of the comparative examples. This shows that the output characteristics of a nonaqueous electrolyte secondary battery are improved by incorporating a predetermined sulfonic acid compound in the positive electrode and a predetermined amount of S in the negative electrode.

[0086] The present disclosure is further described by the following embodiments: Configuration 1: A non-aqueous electrolyte secondary battery including a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the positive electrode includes a lithium transition metal composite oxide as a positive electrode active material and a sulfonic acid compound represented by general formula I, the lithium transition metal composite oxide contains 50 mol % or more of Ni relative to the total number of moles of metal elements excluding Li, and the negative electrode includes a negative electrode active material and contains 200 mass ppm or more of S relative to the total mass of the negative electrode active material. (wherein A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) Configuration 2: The nonaqueous electrolyte secondary battery according to Configuration 1, wherein the sulfonic acid compound is present on the surface of the lithium transition metal composite oxide. Configuration 3: The nonaqueous electrolyte secondary battery according to Configuration 1 or 2, wherein A is a Group 1 element. Configuration 4: The nonaqueous electrolyte secondary battery according to Configuration 1 or 2, wherein A is Li. Configuration 5: The nonaqueous electrolyte secondary battery according to any one of Configurations 1 to 4, wherein R is an alkyl group. Configuration 6: The nonaqueous electrolyte secondary battery according to any one of Configurations 1 to 4, wherein R is a methyl group. Configuration 7: The positive electrode has a peak at 1238 cm in an infrared absorption spectrum. -1 , 1175 cm -1 , 1065 cm -1 , 785 cm -1 The nonaqueous electrolyte secondary battery according to any one of Configurations 1 to 6, wherein the positive electrode has an absorption peak at at least one position near 1238 cm. Configuration 8: The nonaqueous electrolyte secondary battery according to any one of Configurations 1 to 7, wherein the positive electrode has a single peak in H-NMR analysis at a position chemically shifted by 2.76 ppm or more and 2.86 ppm or less with respect to the methyl group of tetramethylsilane as the reference. Configuration 9: The nonaqueous electrolyte secondary battery according to any one of Configurations 1 to 8, wherein the negative electrode contains the sulfonic acid compound. Configuration 10: The negative electrode has a single peak in an infrared absorption spectrum at 1238 cm -1 , 1175 cm -1 , 1065 cm -1 , 785 cm -1The nonaqueous electrolyte secondary battery of any one of configurations 1 to 11, wherein the negative electrode has an absorption peak at at least one position near the methyl group of tetramethylsilane.

[0087] REFERENCE SIGNS LIST 10 Secondary battery, 11 Positive electrode, 12 Negative electrode, 13 Separator, 14 Electrode body, 16 Exterior body, 17 Sealing body, 18, 19 Insulating plate, 20 Positive electrode lead, 21 Negative electrode lead, 22 Grooved portion, 23 Internal terminal plate, 24 Lower valve body, 25 Insulating member, 26 Upper valve body, 27 Cap, 28 Gasket

Claims

1. A non-aqueous electrolyte secondary battery comprising a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the positive electrode contains a lithium transition metal composite oxide as a positive electrode active material and a sulfonic acid compound represented by general formula I, the lithium transition metal composite oxide contains 50 mol % or more of Ni relative to the total number of moles of metal elements excluding Li, and the negative electrode contains a negative electrode active material and contains 200 mass ppm or more of S relative to the total mass of the negative electrode active material. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the sulfonic acid compound is present on the surface of the lithium transition metal composite oxide.

3. The nonaqueous electrolyte secondary battery according to claim 1, wherein A is a Group 1 element.

4. The nonaqueous electrolyte secondary battery according to claim 1, wherein A is Li.

5. The nonaqueous electrolyte secondary battery according to claim 1, wherein R is an alkyl group.

6. The nonaqueous electrolyte secondary battery according to claim 1, wherein R is a methyl group.

7. The positive electrode has an infrared absorption spectrum of 1238 cm -1 , 1175 cm -1 , 1065cm -1 , 785 cm -1 2. The nonaqueous electrolyte secondary battery according to claim 1, having an absorption peak at at least one position in the vicinity of the nonaqueous electrolyte secondary battery.

8. The nonaqueous electrolyte secondary battery according to claim 1, wherein the positive electrode has a single peak at a position chemically shifted by 2.76 ppm or more and 2.86 ppm or less with respect to a methyl group of tetramethylsilane as the reference in H-NMR analysis.

9. The nonaqueous electrolyte secondary battery according to claim 1, wherein the negative electrode contains the sulfonic acid compound.

10. The negative electrode has a peak at 1238 cm in the infrared absorption spectrum. -1 , 1175 cm -1 , 1065cm -1 , 785 cm -1 10. The nonaqueous electrolyte secondary battery according to claim 9, having an absorption peak at at least one location in the vicinity of the nonaqueous electrolyte secondary battery.

11. The nonaqueous electrolyte secondary battery according to claim 9, wherein the negative electrode has a single peak at a position chemically shifted by 2.76 ppm or more and 2.86 ppm or less with respect to a methyl group of tetramethylsilane as the reference in H-NMR analysis.

12. The nonaqueous electrolyte secondary battery according to claim 1, wherein the nonaqueous electrolyte contains 200 ppm by mass or less of S based on the total mass of the nonaqueous electrolyte.

Citation Information

Patent Citations

  • Lithium titanate powder for power storage device electrode, active substance material, and power storage device using the active substance material

    JP2018006164A

  • Positive electrode active material for lithium ion secondary battery, and lithium ion secondary battery

    JP2019169286A

  • Negative electrode for rechargeable battery, method for producing same, and rechargeable battery using same

    WO2014119375A1