Strengthened glass and method for producing same
By creating a tempered glass with a compressive stress layer and controlled hydrogen concentration gradients through ion exchange and water treatment, the impact resistance of tempered glass is significantly enhanced, addressing the limitations of existing technologies in achieving high impact strength.
Patent Information
- Application Number
- PCT/JP2024/018453
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-01
- Filing Date
- 2024-05-20
- Publication Date
- 2024-12-05
AI Technical Summary
Tempered glass used for cover glasses lacks sufficient impact resistance, and existing methods to enhance strength are limited, particularly in the compressive stress characteristics and surface hydrogen concentration.
The development of tempered glass with a compressive stress layer and controlled hydrogen concentration gradients, achieved through ion exchange treatment and water treatment, to increase surface hydrogen concentration and improve impact resistance.
The approach results in tempered glass with enhanced impact strength, characterized by higher surface hydrogen concentration and optimized compressive stress profiles, leading to improved mechanical properties and resistance to scratches and fractures.
Smart Images

Figure JP2024018453_05122024_PF_FP_ABST
Abstract
Description
Tempered glass and its manufacturing method
[0001] The present invention relates to tempered glass, and more particularly to tempered glass suitable for use as a cover glass for a display or the like.
[0002] Chemically strengthened glass is often used as cover glass for devices such as various electronic terminals and display devices.
[0003] Chemically strengthened glass has a compressive stress layer formed on its surface by ion exchange treatment, which suppresses the formation and propagation of cracks on the surface and provides high strength. It is believed that the strength of strengthened glass can be improved by adjusting stress characteristics such as the formation mode of such a compressive stress layer (for example, Patent Document 1).
[0004] International Publication No. 2013 / 088856
[0005] However, in order to obtain higher impact resistance in tempered glass used for cover glass and the like, there are other aspects that need to be adjusted in addition to the stress characteristics, and there is still room for improvement.
[0006] An object of the present invention is to provide a tempered glass having high impact resistance.
[0007] As a result of extensive research, the present inventors have found that the higher the hydrogen concentration at the surface of tempered glass, particularly in an extremely shallow region on the order of nanometers from the surface, is compared to the hydrogen concentration in a region deep inside the glass, the higher the impact resistance of the tempered glass.
[0008] First aspect of the present invention: The tempered glass of the present invention is characterized in that, in the tempered glass having a compressive stress layer on the surface, the ratio of the hydrogen concentration at a depth of 5 nm from the surface to the hydrogen concentration at a depth of 30 nm from the surface is 20 or more.
[0009] Second aspect of the present invention: In any of the above aspects, the tempered glass of the present invention preferably has a K concentration ratio at a depth of 5 nm from the surface to the K concentration at a depth of 30 nm from the surface of 0.85 or less.
[0010] Third aspect of the present invention: In any of the above aspects, the tempered glass of the present invention preferably has a ratio of the Na concentration at a depth of 5 nm from the surface to the Na concentration at a depth of 30 nm from the surface of 0.5 or less.
[0011] Fourth aspect of the present invention: In any of the above aspects, the tempered glass of the present invention preferably has a Li concentration ratio at a depth of 5 nm from the surface to the Li concentration at a depth of 30 nm from the surface of 0.5 or less.
[0012] Fifth aspect of the present invention: In any of the above aspects, in the tempered glass of the present invention, the compressive stress value of the outermost surface of the compressive stress layer is preferably 200 to 1500 MPa.
[0013] Sixth aspect of the present invention: In any of the above aspects, the tempered glass of the present invention preferably has a plate thickness of 1000 μm or less.
[0014] Seventh aspect of the present invention: In any of the above aspects, the tempered glass of the present invention preferably contains, as a glass composition, by mol %, 40 to 80% of SiO, 5 to 25% of AlO, 0 to 30% of BO, 0.1 to 25% of LiO, 0 to 25% of NaO, 0 to 25% of KO, 0 to 20% of MgO, 0 to 10% of ZnO, 0 to 15% of PO, and 0 to 1% of SnO.
[0015] Eighth aspect of the present invention: In any of the above aspects, in the tempered glass of the present invention, it is preferable that the stress depth of the compressive stress layer is 10 to 30% of the plate thickness.
[0016] A ninth aspect of the present invention: A method for producing tempered glass of the present invention includes the steps of: preparing tempered glass having a compressive stress layer on a surface thereof and containing, in mole percent, 40 to 80% SiO, 5 to 25% AlO, 0 to 30% BO, 0.5 to 25% LiO, 0 to 25% NaO, 0 to 25% KO, 0 to 25% MgO, 0 to 10% ZnO, 0 to 15% PO, and 0 to 1% SnO; and a water treatment step of contacting the tempered glass with treatment water at 10 to 100°C for 3 minutes or more.
[0017] According to the tempered glass and the manufacturing method thereof of the present invention, tempered glass having high impact resistance can be obtained.
[0018] 1 is a graph showing an example of hydrogen concentration distribution in a tempered glass according to an embodiment of the present invention.
[0019] In the tempered glass of the present invention having a compressive stress layer on the surface, the ratio of the hydrogen concentration at a depth of 5 nm from the surface to the hydrogen concentration at a depth of 30 nm from the surface is preferably at least 20, at least 25, at least 30, at least 35, at least 40, at least 45, particularly at least 50. The greater the ratio of the hydrogen concentration at the surface to the hydrogen concentration inside the glass, the higher the impact resistance strength that can be obtained.
[0020] The ratio of the K concentration at a depth of 5 nm from the surface to the K concentration at a depth of 30 nm from the surface is preferably 0.85 or less, 0.5 or less, 0.45 or less, 0.4 or less, 0.35 or less, 0.3 or less, 0.25 or less, 0.2 or less, 0.15 or less, and particularly preferably 0.1 or less. A smaller K concentration ratio means that more K has eluted from the glass surface, and hydrogen instead penetrates the glass surface, increasing the hydrogen concentration ratio on the glass surface, thereby achieving high impact resistance.
[0021] The ratio of the Na concentration at a depth of 5 nm from the surface to the Na concentration at a depth of 30 nm from the surface is preferably 0.5 or less, 0.45 or less, 0.4 or less, 0.35 or less, 0.3 or less, 0.25 or less, 0.2 or less, 0.15 or less, and particularly preferably 0.1 or less. A smaller Na concentration ratio means that more Na is eluted from the glass surface, and hydrogen instead penetrates the glass surface, increasing the hydrogen concentration ratio on the glass surface, thereby achieving high impact strength.
[0022] The ratio of the Li concentration at a depth of 5 nm from the surface to the Li concentration at a depth of 30 nm from the surface is preferably 0.5 or less, 0.45 or less, 0.4 or less, 0.35 or less, 0.3 or less, 0.25 or less, 0.2 or less, 0.15 or less, and particularly preferably 0.1 or less. A smaller Li concentration ratio means that more Li has eluted from the glass surface, and hydrogen instead penetrates the glass surface, increasing the hydrogen concentration ratio on the glass surface, thereby achieving high impact strength.
[0023] The hydrogen concentration, K concentration, Na concentration, and Li concentration can be measured using, for example, D-SIMS (Dynamic SIMS). D-SIMS is a method of generating secondary ions by sputtering the sample surface with a primary ion beam, which makes it possible to perform elemental composition analysis in the depth direction. By using D-SIMS to analyze the distribution of each component in the depth direction from the glass surface, it is possible to measure the concentration of each component at a predetermined depth. The above-mentioned concentration ratios can be obtained by dividing the concentration (atoms / cc) measured in this manner at a depth of 5 nm from the surface by the concentration (atoms / cc) measured in this manner at a depth of 30 nm from the surface.
[0024] The tempered glass of the present invention has a compressive stress layer on its surface. The compressive stress value of the outermost surface is preferably 200 MPa or more, 300 MPa or more, 400 MPa or more, particularly 500 MPa or more. The larger the compressive stress value of the outermost surface, the easier it is to improve the bending strength. On the other hand, if an extremely large compressive stress is formed on the surface, the tensile stress inherent in the tempered glass becomes extremely high, and there is a risk of large dimensional changes before and after the ion exchange treatment. Therefore, the compressive stress value of the outermost surface is preferably 1500 MPa or less, 1200 MPa or less, 1100 MPa or less, 1000 MPa or less, 900 MPa or less, particularly 800 MPa or less.
[0025] The stress depth is preferably 1 μm or more, 2 μm or more, 3 μm or more, 4 μm or more, particularly 5 μm or more, and 5 to 30%, 6 to 25%, 7 to 20%, 8 to 17%, 9 to 16%, 10 to 15%, 11 to 14%, particularly 12 to 13% of the plate thickness. The greater the stress depth, the less likely the tempered glass is to break even if deep scratches are made on the tempered glass, and the smaller the variation in mechanical strength. On the other hand, the greater the stress depth, the greater the dimensional change before and after the ion exchange treatment. Therefore, the stress depth is preferably 20 μm or less, 15 μm or less, 14 μm or less, 13 μm or less, 12 μm or less, 11 μm or less, particularly 10 μm or less.
[0026] The compressive stress value and stress depth can be calculated from the number and spacing of interference fringes observed using, for example, a surface stress meter (FSM-6000 manufactured by Orihara Seisakusho Co., Ltd.).
[0027] The internal tensile stress value is preferably 400 MPa or less, 350 MPa or less, 300 MPa or less, 250 MPa or less, 220 MPa or less, 200 MPa or less, 180 MPa or less, particularly 170 PMa or less. If the internal tensile stress value is too high, the tempered glass is prone to self-destruction due to physical collisions, etc. On the other hand, if the internal tensile stress value is too low, it is difficult to ensure the mechanical strength of the tempered glass. The internal tensile stress value is preferably 20 MPa or more, 30 MPa or more, 40 MPa or more, 50 MPa or more, 60 MPa or more, 80 MPa or more, 100 MPa or more, 125 MPa or more, 140 MPa or more, particularly 150 MPa or more. The internal tensile stress can be calculated using the following formula 1.
[0028] [Equation 1] Internal tensile stress value = (compressive stress value of outermost surface × stress depth) / (plate thickness - 2 × stress depth)
[0029] In the tempered glass of the present invention, the thickness is, for example, 2000 μm or less, 1500 μm or less, 1000 μm or less, 800 μm or less, 750 μm or less, 700 μm or less, 650 μm or less, 600 μm or less, 550 μm or less, 500 μm or less, 400 μm or less, 300 μm or less, or 1 μm or more. From the viewpoint of imparting flexibility to the tempered glass, the thickness is, for example, 200 μm or less, preferably 150 μm or less, 100 μm or less, less than 90 μm, 80 μm or less, 70 μm or less, 60 μm or less, 1 to 50 μm, 5 to 40 μm, particularly 10 to 30 μm.
[0030] The tempered glass of the present invention preferably has a glass composition containing, in mole percent, 40-80% SiO2, 5-25% Al2O3, 0-30% BO3, 0.1-25% Li2O, 0-25% Na2O, 0-25% KO2O, 0-20% MgO, 0-10% ZnO, 0-15% PO5, and 0-1% SnO2. This composition facilitates increasing the surface hydrogen concentration through the treatment described below. Furthermore, to obtain tempered glass with this composition, the tempering glass prior to ion exchange treatment preferably has a glass composition with a similar content range. The reasons for limiting the content range of each component in the tempered glass of the present invention are explained below. In the description of the content range of each component, percentages refer to mole percent unless otherwise specified.
[0031] SiO2 is a component that forms the glass network. If the SiO2 content is too low, vitrification becomes difficult, and the thermal expansion coefficient becomes too high, which tends to reduce thermal shock resistance. Therefore, the preferred lower limit range of SiO2 is, in mole percent, 40% or more, 45% or more, 50% or more, 55% or more, 57% or more, 59% or more, and particularly 61% or more. On the other hand, if the SiO2 content is too high, meltability and formability tend to decrease, and the thermal expansion coefficient becomes too low, making it difficult to match the thermal expansion coefficient of surrounding materials. Therefore, the preferred upper limit range of SiO2 is 80% or less, 75% or less, 73% or less, 71% or less, 69% or less, and particularly 68.5% or less.
[0032] Al2O3 is a component that enhances ion exchange performance and also increases strain point, Young's modulus, fracture toughness, and Vickers hardness. Therefore, the preferred lower limit of Al2O3 is, in mole percent, 5% or more, 6% or more, 7% or more, 8% or more, 8.5% or more, 9% or more, and particularly 9.2% or more. On the other hand, if the Al2O3 content is too high, the high-temperature viscosity increases, and meltability and formability tend to decrease. Furthermore, devitrification crystals tend to precipitate in the glass, making it difficult to form it into a plate shape by the overflow downdraw method or the like. In particular, when an alumina-based refractory is used as the formed body refractory and a glass plate is formed by the overflow downdraw method, spinel devitrification crystals tend to precipitate at the interface with the alumina-based refractory. Furthermore, acid resistance also decreases, making it difficult to apply to an acid treatment process. Therefore, the preferred upper limit range of Al2O3 is 25% or less, 23% or less, 20% or less, 18% or less, 16% or less, 15% or less, 14% or less, 13% or less, 12.5% or less, 12% or less, 11.5% or less, particularly 11% or less.
[0033] BO reduces high-temperature viscosity and density, stabilizes the glass, and reduces the likelihood of crystal precipitation, lowering the liquidus temperature. It also suppresses Young's modulus and increases bending strength and crack resistance. However, excessive BO content can lead to surface discoloration (known as fading) during ion exchange treatment, reduced water resistance, and a decrease in the compressive stress value of the compressive stress layer. Therefore, the preferred lower limit of BO is, in mole percent, 0% or more, 0.01% or more, 0.02% or more, 0.1% or more, or 0.3% or more. The preferred upper limit is 30% or less, 25% or less, 22% or less, 20% or less, 15% or less, and particularly 10% or less. From the perspective of prioritizing high CS, the BO content can be more preferably 0.2-5% or 0.3-1%. Furthermore, from the viewpoint of improving chemical durability for the purpose of suppressing defects during etching treatment, the upper limit range of the BO content can be preferably 1% or more, 1.5% or more, or 2% or more, and the lower limit range can be preferably 5% or less, 4.5% or less, 4% or less, or 3% or less.
[0034] Li2O is an ion-exchange component, specifically, Li ions contained in glass and K ions in the molten salt are ion-exchanged to obtain a high surface compressive stress. Li2O also reduces high-temperature viscosity and improves meltability and formability. Li2O dissolves in water during water treatment, increasing the hydrogen concentration on the glass surface. Therefore, the preferred lower limit of Li2O, in mole percent, is 0.1% or more, 0.5% or more, 1% or more, 2% or more, 3% or more, 4% or more, 5% or more, 5.5% or more, 6% or more, 6.5% or more, 7% or more, 7.3% or more, 7.5% or more, and particularly 7.8% or more. Therefore, the preferred upper limit of Li2O is 25% or less, 20% or less, 15% or less, 13% or less, 12% or less, 11.5% or less, 11% or less, 10.5% or less, less than 10%, and particularly 9% or less.
[0035] Na2O is an ion exchange component and also a component that reduces high-temperature viscosity and improves meltability and formability. Na2O also improves devitrification resistance and reaction devitrification resistance with refractory molded bodies, particularly alumina-based refractories. Na2O dissolves in water during water treatment and instead increases the hydrogen concentration on the glass surface. If the Na2O content is too low, meltability decreases, the thermal expansion coefficient decreases too much, and the ion exchange rate tends to decrease. Therefore, the preferred lower limit range of Na2O, in mole percent, is 0% or more, 1% or more, 3% or more, 5% or more, 6% or more, 7% or more, 7.5% or more, and particularly 7.8% or more. On the other hand, if the Na2O content is too high, the phase separation viscosity tends to decrease. Furthermore, acid resistance may decrease, and the glass composition may become unbalanced, resulting in decreased devitrification resistance. Therefore, the preferred upper limit range of NaO is 25% or less, 20% or less, 19% or less, 18% or less, 17% or less, 16% or less, 15% or less, 14% or less, 13% or less, 12% or less, 11% or less, 10% or less, 9.5% or less, particularly 9% or less.
[0036] KO is a component that reduces high-temperature viscosity and improves meltability and formability. It also improves devitrification resistance and increases Vickers hardness. KO is also a component that dissolves in water during water treatment and instead increases the hydrogen concentration on the glass surface. However, if the KO content is too high, the phase separation viscosity tends to decrease. Furthermore, acid resistance decreases and the glass composition loses its component balance, which tends to actually decrease devitrification resistance. Therefore, the preferred lower limit range of KO, in mole %, is 0% or more, 0.01% or more, 0.02% or more, 0.05% or more, 0.1% or more, 0.5% or more, 1% or more, 1.5% or more, 2% or more, 2.5% or more, and particularly 2.8% or more, and the preferred upper limit range is 25% or less, 20% or less, 15% or less, 10% or less, 9% or less, 8% or less, 7% or less, 6% or less, 5% or less, 4.5% or less, 4% or less, and particularly 3.5% or less.
[0037] MgO is a component that reduces high-temperature viscosity, improves meltability and formability, and increases the strain point and Young's modulus. Among alkaline earth metal oxides, it is a component that is highly effective in improving ion exchange performance. However, if the MgO content is too high, the density and thermal expansion coefficient tend to increase, and the glass is prone to devitrification. Therefore, the preferred upper limit of MgO is 20% or less, 12% or less, 10% or less, 8% or less, 6% or less, and particularly 5% or less. When MgO is incorporated into the glass composition, the preferred lower limit of MgO is 0.1% or more, 0.5% or more, 1% or more, and particularly 2% or more, in mole percent.
[0038] ZnO is a component that enhances ion exchange performance, and is particularly effective in increasing compressive stress values. It also reduces high-temperature viscosity without reducing low-temperature viscosity. However, if the ZnO content is too high, the glass tends to undergo phase separation, reduce devitrification resistance, increase density, and reduce the stress depth of the compressive stress layer. Therefore, the ZnO content is preferably 0 to 10%, 0 to 6%, 0 to 5%, 0 to 1%, or 0 to 0.5%, particularly preferably 0 to less than 0.1%, in mole percent.
[0039] PO is a component that enhances ion exchange performance, particularly increasing the stress depth of the compressive stress layer. It also suppresses the Young's modulus. However, if the PO content is too high, the glass is prone to phase separation. Therefore, the preferred upper limit of PO is 15% or less, 10% or less, 8% or less, 6% or less, 4% or less, 2% or less, 1% or less, and particularly less than 0.1% by mole.
[0040] SnO2 is a component useful as a fining agent. The preferred content range of SnO2 is 0 to 10,000 ppm (1%), 0 to 7,000 ppm, particularly 50 to 6,000 ppm.
[0041] In addition to the above components, the tempered glass and the glass to be tempered may contain, for example, the following components as part of the glass composition.
[0042] Compared with other components, CaO is highly effective in reducing high-temperature viscosity, improving meltability and formability, and increasing strain point and Young's modulus without reducing devitrification resistance. The CaO content is preferably 0 to 10%. However, if the CaO content is too high, the density and thermal expansion coefficient will increase, and the glass composition will be imbalanced, making the glass more susceptible to devitrification and reducing ion exchange performance. Therefore, the preferred CaO content is, in mole percent, 0 to 5%, 0.01 to 4%, 0.1 to 3%, and particularly 1 to 2.5%.
[0043] SrO is a component that reduces high-temperature viscosity, improves meltability and formability, and increases the strain point and Young's modulus without reducing devitrification resistance. However, if the SrO content is too high, the density and thermal expansion coefficient increase, the ion exchange performance decreases, and the component balance of the glass composition is lost, making the glass more susceptible to devitrification. The preferred range of SrO content is, in mole percent, 0 to 5%, 0 to 3%, 0 to 1%, and particularly 0 to less than 0.1%.
[0044] BaO is a component that reduces high-temperature viscosity, improves meltability and formability, and increases strain point and Young's modulus without reducing devitrification resistance. However, if the BaO content is too high, the density and thermal expansion coefficient increase, the ion exchange performance decreases, and the component balance of the glass composition is lost, making the glass more susceptible to devitrification. The preferred BaO content range, in mole percent, is 0 to 5%, 0 to 3%, 0 to 1%, and particularly 0 to less than 0.1%.
[0045] ZrO2 is a component that significantly enhances ion exchange performance and also increases the viscosity near the liquidus viscosity and the strain point. However, if its content is too high, there is a risk that devitrification resistance will be significantly reduced and the density will be too high. Therefore, the preferred upper limit range of ZrO2 is 10% or less, 8% or less, 6% or less, and particularly 5% or less, in mole percent. Note that, when it is desired to enhance ion exchange performance, it is preferable to incorporate ZrO2 into the glass composition. In this case, the preferred lower limit range of ZrO2 is 0.001% or more, 0.01% or more, 0.5%, and particularly 1% or more.
[0046] As a fining agent, one or more selected from the group consisting of As2O3, Sb2O3, SnO2, F, Cl, and SO3 (preferably the group consisting of SnO2, Cl, and SO3) may be incorporated in an amount of 0 to 30,000 ppm (3%). From the viewpoint of adequately obtaining the fining effect, the content of SnO2 + SO3 + Cl is preferably 0 to 10,000 ppm, 50 to 5,000 ppm, 80 to 4,000 ppm, 100 to 3,000 ppm, and particularly 300 to 3,000 ppm. Here, "SnO2 + SO3 + Cl" refers to the combined amount of SnO2, SO3, and Cl.
[0047] The preferred range of Cl content is 0 to 1500 ppm, 0 to 1200 ppm, 0 to 800 ppm, 0 to 500 ppm, particularly 50 to 300 ppm. The preferred range of SO content is 0 to 1000 ppm, 0 to 800 ppm, particularly 10 to 500 ppm.
[0048] Rare earth oxides such as NdO and LaO increase Young's modulus and can control the color of glass by eliminating the color when a complementary color is added. However, the raw materials themselves are expensive, and adding a large amount of these oxides can easily reduce devitrification resistance. Therefore, the content of rare earth oxides is preferably 4% or less, 3% or less, 2% or less, 1% or less, and particularly 0.5% or less.
[0049] From an environmental perspective, it is preferable that the glass composition be substantially free of As2O3, F, PbO, and Bi2O3. Here, "substantially free of As2O3" means that As2O3 is not actively added as a glass component, but is permitted to be present at the impurity level; specifically, the As2O3 content is less than 500 ppm. "Substantially free of F" means that F is not actively added as a glass component, but is permitted to be present at the impurity level; specifically, the F content is less than 500 ppm. "Substantially free of PbO" means that PbO is not actively added as a glass component, but is permitted to be present at the impurity level; specifically, the PbO content is less than 500 ppm. The phrase "substantially free of Bi2O3" means that Bi2O3 is not actively added as a glass component, but is allowed to be mixed in at an impurity level, and specifically means that the Bi2O3 content is less than 500 ppm.
[0050] High temperature viscosity of tempered glass and tempering glass 10 2.5 The temperature at viscosity dPa·s is preferably 1680°C or less, 1670°C or less, 1660°C or less, 1650°C or less, 1640°C or less, 1630°C or less, 1620°C or less, 1600°C or less, 1550°C or less, 1520°C or less, 1500°C or less, particularly 1300 to 1490°C. 2.5 The lower the temperature at dPa·s, the lower the melting temperature becomes, which reduces the burden on glass manufacturing equipment such as a melting furnace and also makes it easier to improve the bubble quality. 2.5 The lower the temperature at viscosity dPa·s, the easier it is to reduce the manufacturing cost of tempered glass.
[0051] The dimensions of the tempered glass are preferably a rectangle or a square with one side measuring 50 mm or more, 60 mm or more, 70 mm or more, 80 mm or more, 90 mm or more, 100 mm or more, 120 mm or more, or 150 mm or more, particularly 200 to 2000 mm. <Method for manufacturing tempered glass>
[0052] The present method for manufacturing tempered glass includes a tempered-glass preparation step and a water treatment step, in this order. In this embodiment, the tempered-glass preparation step further includes a tempering-use glass preparation step, a thinning step, a chemical tempering step, and a surface etching step.
[0053] The tempering glass preparation step is a step of preparing glass to be tempered. Glass to be tempered can be obtained, for example, by blending and melting glass raw materials blended to have the above-described glass composition, and cutting and processing the resulting plate- or sheet-shaped mother glass into small glass pieces using a forming method such as the overflow downdraw method, slot downdraw method, float method, or redraw method. To obtain a smooth surface, the overflow downdraw method is preferably used as the forming method. When formed by the overflow downdraw method, the glass to be tempered has a forming confluence surface inside.
[0054] The edge faces of the glass to be tempered are preferably subjected to treatments such as polishing, heat treatment, etching, etc. to chamfer or improve strength. The main surfaces of the glass to be tempered may be polished, but, for example, when the main surfaces have been formed smooth in advance by the overflow downdraw method or when the glass has been formed to a uniform thickness with high precision, the main surfaces may not be polished, i.e., the unpolished surfaces may be used as they are. Note that when the glass is formed by the overflow downdraw method and not polished, the main surfaces of the glass to be tempered are fire-polished surfaces.
[0055] The thinning process is a process of thinning the thickness of the glass to be tempered to a predetermined range by etching. By performing this thinning process, even if a thick glass to be tempered is prepared in the preparation process, the thickness of the glass to be tempered can be thinned to a range suitable for the intended use.
[0056] In the thinning process, for example, the entire glass to be tempered is immersed in a liquid etching medium, and the entire surface of the glass to be tempered is wet-etched. This process allows the entire glass to be uniformly etched, thereby suppressing thickness variations caused by the etching process. When this etching process is performed, the surface of the glass to be tempered is composed of an etched surface.
[0057] The etching medium can be an acidic or alkaline aqueous solution capable of etching glass.
[0058] As the acidic etching medium, for example, an acidic aqueous solution containing HF can be used. When an aqueous solution containing HF is used, the etching rate for glass is high and production efficiency is good.
[0059] The HF-containing aqueous solution may be, for example, an aqueous solution containing only HF, or a combination of HF and HCl, HF and HNO3, HF and H2SO4, or HF and NH4F. The concentration of each of the HF, HCl, HNO3, H2SO4, and NH4F compounds is preferably 0.1 to 30 mol / L. When etching using an HF-containing aqueous solution, fluorides containing glass components are generated as by-products, which can lead to a decrease in etching rate and defects. However, as described above, by using a mixed acid with other acids such as HCl, HNO3, or H2SO4, the by-products can be decomposed, thereby preventing a decrease in productivity. When etching is performed using an acidic aqueous solution, the temperature of the acidic aqueous solution is preferably, for example, 10 to 30°C, and the time for immersing the glass to be tempered is preferably, for example, 0.1 to 60 minutes.
[0060] The alkaline etching medium may be an alkaline aqueous solution containing NaOH or KOH. The alkaline aqueous solution has a relatively low etching rate for glass compared to the etching medium containing HF, and therefore has the advantage of making it easier to precisely control the etching amount. This is particularly suitable when it is necessary to control the glass thickness or compressive stress layer in units of several micrometers.
[0061] In the aqueous solution containing NaOH or KOH, the concentration of the alkaline component is preferably 1 to 20 mol / L. When etching is performed using an alkaline aqueous solution, the temperature of the alkaline aqueous solution is, for example, 10 to 130°C, and the time for immersing the processing glass is preferably, for example, 0.5 to 120 minutes. When increasing the etching rate to improve productivity, it is preferable to heat the alkaline aqueous solution to a temperature of 80°C or higher. Conversely, when it is desired to control the etching amount with higher precision, it is preferable to limit the temperature of the alkaline aqueous solution to 70°C or lower. When a high etching rate is more important, it is preferable to use an aqueous solution of NaOH.
[0062] The thickness of the removed surface layer portion of the tempered glass in the thinning step is not particularly limited because it depends on the original thickness (initial thickness) of the tempered glass before the thinning step, but may be larger than the thickness of the removed surface layer portion of the tempered glass in the surface layer etching step.
[0063] In the chemical strengthening step, the glass to be strengthened is subjected to an ion exchange treatment. In this embodiment, the glass to be strengthened is immersed in a molten salt for the ion exchange treatment. By converting the glass to be strengthened through the ion exchange treatment, the bending strength of the glass to be strengthened is improved.
[0064] The molten salt is a salt containing a component that is ion-exchangeable with the components in the glass to be tempered, and is typically an alkali metal nitrate. Examples of alkali metal nitrates include NaNO, KNO, and LiNO. These can be used alone (at 100% by mass) or in combination. When multiple alkali metal nitrates are mixed, the mixing ratio can be determined arbitrarily. For example, the ratio can be, by mass, 5-95% NaNO and 5-95% KNO, preferably 30-80% NaNO and 20-70% KNO, and more preferably 50-70% NaNO and 30-50% KNO.
[0065] The temperature of the molten salt is, for example, 350°C to 500°C, and preferably 355°C to 470°C, 360°C to 450°C, 365°C to 430°C, or 370°C to 410°C. The immersion time is, for example, 3 to 300 minutes, and preferably 5 to 120 minutes, or 7 to 100 minutes. Of course, the conditions such as the temperature of the molten salt and the immersion time can be appropriately changed depending on the composition, etc., within a range in which the above-mentioned stress characteristics can be obtained.
[0066] The surface etching step is a step of etching the tempered glass in a shallower area than the compressive stress layer after the chemical strengthening step and before the water treatment step. By performing this surface etching step, surface defects formed in the tempered glass during the chemical strengthening step or the like can be reduced. As a result, the impact strength and / or bending strength of the tempered glass can be improved.
[0067] In the surface etching step, for example, the entire tempered glass is immersed in a liquid etching medium, and the entire surface of the glass to be treated is wet-etched. This process allows the entire tempered glass to be uniformly etched, thereby suppressing thickness variations caused by the etching process. When this etching process is performed, the surface of the tempered glass is composed of an etched surface.
[0068] As the etching medium, the same etching medium as used in the thinning step can be used.
[0069] The thickness of the surface layer portion of the tempered glass removed in the surface layer etching step is preferably 0.25 μm or more and 3 μm or less. The thickness of the surface layer portion of the tempered glass removed is more preferably 0.3 μm or more and 2.5 μm or less, 0.35 μm or more and 2.3 μm or less, 0.4 μm or more and 2.1 μm or less, particularly preferably 0.45 μm or more and 1.9 μm or less. By setting the etching amount within such a range, the amount of change in the maximum compressive stress and the compressive stress depth before and after etching can be reduced.
[0070] It is preferable that the entire surface of the tempered glass produced through the surface etching step, i.e., both the front and back main surfaces and the end surfaces, are etched. In this way, defects are reduced over the entire surface of the tempered glass, and high strength can be achieved.
[0071] The above steps are merely an example, and if the desired thickness and surface condition can be obtained, the thinning step and surface etching step may be omitted.
[0072] In the water treatment step, the tempered glass is brought into contact with the treatment water for 3 minutes or more. By bringing the tempered glass into contact with the treatment water in this manner, the hydrogen concentration on the surface of the tempered glass increases, improving the impact resistance strength. Note that if the contact time between the tempered glass and the treatment water (hereinafter referred to as the water treatment time) is too short, the hydrogen concentration on the surface of the tempered glass will not be sufficiently high, and the impact resistance strength improvement effect will not be fully achieved. Therefore, it is preferable that the water treatment time be equal to or greater than the above-mentioned lower limit.
[0073] The lower limit of the water treatment time is preferably 3 minutes or more, 5 minutes or more, 10 minutes or more, or 15 minutes or more, and the upper limit of the water treatment time is, for example, 1500 minutes or less, preferably 1000 minutes or less.
[0074] The temperature of the treatment water is, for example, 10 to 100°C. The lower limit range of the temperature of the treatment water is preferably 20°C or higher, 30°C or higher, 40°C or higher, or 45°C or higher. The upper limit range of the temperature of the treatment water is preferably 95°C or lower, 90°C or lower, or 85°C or lower. As the temperature of the treatment water increases, the treatment time required to obtain the desired impact resistance tends to become shorter.
[0075] In one embodiment, the water treatment step can be carried out by immersing the tempered glass in treatment water stored in a container. In the treatment water, multiple sheets of tempered glass are supported by a support stand in a vertical position with a predetermined spacing in the thickness direction. The container containing the tempered glass and the treatment water is then placed in a thermostatic device (temperature control device) maintained at a predetermined temperature for a predetermined time, and the tempered glass is subjected to water treatment. In this case, it is preferable to leave the tempered glass stationary in the treatment water without applying external vibrations such as ultrasonic waves to the treatment water. Immersing the tempered glass in the treatment water in this manner allows the entire tempered glass to efficiently come into contact with the treatment water, making it easier to enjoy the effect of improving impact resistance.
[0076] The method for bringing the treated water into contact with the tempered glass is not limited to the above-described embodiment, and other embodiments are also possible. For example, the treated water may be brought into contact with the tempered glass by spraying it onto the tempered glass from a nozzle or the like, or by running water over the entire surface of the tempered glass.
[0077] The tempered glass may be moved relative to the treatment water. Specifically, for example, the tempered glass immersed in the treatment water in a container may be moved within the treatment water, or the tempered glass may be moved within an area where the treatment water is sprayed by a nozzle or the like.
[0078] Although the embodiment of the present invention has been described, the embodiment of the present invention is not limited to this, and various modifications can be made without departing from the spirit of the present invention.
[0079] In the above-described embodiment, the shape of the tempered glass is not particularly limited. The shape of the tempered glass may be, for example, a square, a rectangle, a circle, an ellipse, or the like in a plan view.
[0080] In the above-described embodiment, the tempered glass may be subjected to three-dimensional bending as necessary. Specifically, by subjecting the glass to be processed to three-dimensional bending in advance, the tempered glass to be finally produced can be given a three-dimensional curved shape. Furthermore, the tempered glass of the present invention may be spherical.
[0081] In the above embodiment, a case where a single chemical strengthening step (ion exchange treatment) is performed has been exemplified, but two or more chemical strengthening steps may be performed. Heat treatment may also be performed before or after ion exchange. Heat treatment can relieve stress and promote ion diffusion, thereby controlling the depth of the compressive stress layer, etc. When a chemical strengthening step is performed, it is preferable that the tempered glass be washed and dried after the chemical strengthening step and before the water treatment step. When chemical strengthening is performed multiple times as described above, the stress distribution of the tempered glass may have at least one of a bending point, a maximum value, a minimum value, or an inflection point in the compressive stress layer region.
[0082] In the above embodiment, the tensile stress in the tensile stress layer may not be constant in the thickness direction. For example, when the depth of the compressive stress relative to the thickness of the tempered glass is set to be relatively large, the stress distribution in the tensile stress layer may be a distribution shape along a downwardly convex quadratic curve having a minimum value at the center of the thickness of the tempered glass.
[0083] In the above-described embodiment, the stress distribution of the tempered glass may be asymmetric between the front and back surfaces. The asymmetric stress distribution can be obtained by polishing one main surface of the tempered glass more than the other main surface, or by chemically tempering the glass in a state where a film that inhibits ion exchange is applied to one main surface.
[0084] The tempered glass according to the present invention will be described below based on examples. Note that the following examples are merely illustrative and the present invention is not limited to the following examples in any way.
[0085] The samples were prepared as follows: First, a glass plate having the glass composition shown in Table 1 was prepared.
[0086]
[0087] Specifically, glass raw materials were prepared to have the compositions shown in Table 1, and melted in a test melting furnace. Thereafter, the obtained molten glass was formed into a sheet having an initial thickness shown in Tables 2 and 3 by an overflow downdraw method, and cut into a size of 50 mm × 50 mm to obtain glass to be tempered.
[0088] Next, sheet-shaped tempered glass was produced by treating the obtained glass to be tempered under the conditions shown in Tables 2 and 3. That is, the tempered glass was produced by subjecting the glass to be tempered to a thinning step, a chemical tempering step, a surface layer etching step, and a water treatment step in this order.
[0089] The thinning step was carried out by immersing the glass to be tempered in an aqueous HF solution.
[0090] The chemical strengthening step was carried out by immersing the glass to be strengthened in a molten salt of 100% KNO3 under the temperature and time conditions shown in Tables 2 and 3.
[0091] The surface etching step was performed by immersing the tempered glass in an aqueous HF solution.
[0092] The water treatment step was carried out by immersing the chemically strengthened glass in pure water under the temperature and time conditions shown in Tables 2 and 3 and leaving it to stand.
[0093] In Tables 2 and 3, Nos. 1 and 3 are examples of the present invention, and Nos. 2 and 4 are comparative examples.
[0094]
[0095]
[0096] The concentrations of hydrogen, Li, Na, and K in the obtained glass plate were measured from the surface to a depth of 40 nm by the following D-SIMS analysis.
[0097] The detailed measurement conditions for D-SIMS are as follows: Device name: PHI ADEPT-1010 manufactured by Physical Electronics Corporation Primary ion species: Cs + Primary ion acceleration energy: 1 kV Primary ion current: 50 nA Primary ion raster size: 400 x 800 μm Gate size: 16% of primary ion raster size Charge compensation electron gun used: Yes (acceleration energy: 500 eV) Monitored secondary ions Negative ions: X - (X: 1 H. 30 Si) Positive ion: CsX + (X: 7 Li, 23 Na, 28 Si, 41 K) Vacuum degree of measurement chamber: 5.0 x 10 -8 Pa or less Data processing methods were as follows: Concentration conversion: Conversion was performed using the sensitivity in SiO2 (a standard sample prepared by ion implantation was used). Depth conversion: Sputtering time was converted to depth using the sputtering rate in SiO2. Normalization method: After normalization by Si intensity for each point (each depth), each element was normalized by the intensity at a depth of 30 nm from the surface.
[0098] The surface concentrations of each component in Tables 2 and 3 indicate the concentration ratio at the surface of the glass, based on the concentration of each component measured as described above, with the concentration inside the glass taken as the reference. Specifically, for each component, the concentration at a depth of 5 nm from the surface was calculated as the surface concentration, assuming that the concentration at a depth of 30 nm from the surface is 1. Figure 1 is a graph showing the concentration distribution of hydrogen. In Figure 1, the horizontal axis represents the depth from the glass surface, and the vertical axis represents the concentration (concentration ratio) at each depth, assuming that the concentration at a depth of 30 nm from the surface is 1.
[0099] The impact strength is shown in the results of measurements performed by the following two types of impact resistance tests 1 and 2. <Impact Resistance Test 1> In Impact Resistance Test 1, the obtained glass sample (planar dimensions: 50 mm × 50 mm) was first placed on a stone surface plate, and the tip of a spherical impactor (tip diameter: 0.7 mm, total mass: 5.4 g) was dropped onto the glass sample. The impactor was dropped onto the glass sample through the inner hole of a vertically held guide tube so that the tip of the impactor fell perpendicularly to the glass sample. The height of the tip of the impactor before the drop was defined as the drop height, and the initial value was set to 1.0 cm. If the glass sample did not break upon the drop, the height was increased by 0.5 cm and the sample was dropped again. In this way, the drop height increase and drop trial were repeated until the glass sample broke, and the drop height at which the glass sample broke was determined as the breaking height for the test. <Impact Resistance Test 2> In impact resistance test 2, first, a polyethylene sheet (thickness 0.25 mm) cut to the same shape was attached to one main surface of the obtained glass sample (planar dimensions 50 mm x 50 mm) via an optical adhesive film (thickness 0.05 mm, PDS1 manufactured by PANAC Corporation) to obtain a laminated sample. The obtained laminated sample was placed on a stone surface plate with the glass side facing up, and the tip of a spherical impactor (tip spherical diameter 0.7 mm, total mass 5.4 g) was dropped onto the glass sample to perform the test. At this time, the impactor was dropped to the glass sample through the inner hole of the guide cylinder held vertically so that the tip of the impactor fell perpendicular to the glass sample. The height of the tip of the impactor before the drop was defined as the drop height, and its initial value was set to 1.0 cm and dropped. If the glass sample did not break due to the drop, the height was raised 0.5 cm and dropped again. In this way, the drop height was increased and the drop trial was repeated until the glass sample broke, and the drop height at which the glass sample broke was determined as the breaking height of the test.
[0100] According to the results of the impact resistance test, it was confirmed that the Examples (Nos. 1 and 3) with high surface hydrogen concentrations had higher breaking heights than the Comparative Examples (Nos. 2 and 4) with low surface hydrogen concentrations.
[0101] The glass article of the present invention can be used, for example, for smartphones, mobile phones, tablet computers, personal computers, digital cameras, touch panel displays, cover glass for other display devices, in-vehicle display devices, in-vehicle panels, etc.
Claims
1. Tempered glass having a compressive stress layer on its surface, characterized in that the ratio of the hydrogen concentration at a depth of 5 nm from the surface to the hydrogen concentration at a depth of 30 nm from the surface is 20 or more.
2. The tempered glass according to claim 1, characterized in that the ratio of the K concentration at a depth of 5 nm from the surface to the K concentration at a depth of 30 nm from the surface is 0.85 or less.
3. The tempered glass according to claim 1 or 2, characterized in that the ratio of the Na concentration at a depth of 5 nm from the surface to the Na concentration at a depth of 30 nm from the surface is 0.5 or less.
4. The tempered glass according to claim 1 or 2, characterized in that the ratio of the Li concentration at a depth of 5 nm from the surface to the Li concentration at a depth of 30 nm from the surface is 0.5 or less.
5. The tempered glass according to claim 1 or 2, wherein the compressive stress value of the outermost surface of the compressive stress layer is 200 to 1500 MPa.
6. The tempered glass according to claim 1 or 2, characterized in that the plate thickness is 1000 μm or less.
7. The glass composition, in mole percent, is SiO 2 40-80%, Al 2 O 3 5-25%, B 2 O 3 0-30%, Li 2 O 0.1-25%, Na 2 O 0-25%, K 2 O 0-25%, MgO 0-20%, ZnO 0-10%, P 2 O 5 0-15%, SnO 2 The tempered glass according to claim 1 or 2, characterized in that it contains 0 to 1% of Cr.
8. The tempered glass according to claim 1 or 2, characterized in that the depth of the compressive stress layer is 10 to 30% of the plate thickness.
9. A glass having a compressive stress layer on the surface, and a glass composition of SiO 2 40-80%, Al 2 O 3 5-25%, B 2 O 3 0-30%, Li 2 O 0.1-25%, Na 2 O 0-25%, K 2 O 0-25%, MgO 0-20%, ZnO 0-10%, P 2 O 5 0-15%, SnO 2 A method for producing tempered glass, comprising: preparing tempered glass containing 0 to 1% of niobium; and treating the tempered glass with treated water at 10 to 100° C. for 3 minutes or more.
Citation Information
Patent Citations
Glass substrate for magnetic recording medium and its production and magnetic recording medium
JP1996180402A
Glass substrate and its production method, and magnetic recording medium and its production method
JP2005187239A
Laminated glass articles comprising a hydrogen-containing glass core layer and methods of forming the same
US20200156997A1
Glass substrate for magnetic disk, process for producing the glass substrate, and magnetic disk
WO2009041618A1
Chemically strengthened glass
WO2018199045A1
Cited By
Glass article, method of producing glass article, and display device
US20250128985A1