Austenitic stainless steel and method for producing same

The austenitic stainless steel with a tailored composition and manufacturing process achieves excellent low-temperature toughness in the weld heat-affected zone, addressing the cost inefficiencies of existing methods, and is suitable for extreme low-temperature applications like liquefied gas storage tanks.

WO2024247794A1PCT designated stage expired Publication Date: 2024-12-05JFE STEEL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018564
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-05-20
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Austenitic stainless steel used in storage tanks for liquefied gases like liquid hydrogen and liquid helium requires excellent low-temperature toughness, but existing manufacturing methods involving solution heat treatment are costly and inefficient, particularly in improving the weld heat-affected zone's toughness.

Method used

Austenitic stainless steel with a specific composition (C: 0.050% to 0.100%, Si: 0.05% to 1.00%, Mn: 5.0% to 20.0%, Ni: 5.0% to 10.0%, Cr: 11.0% to 20.0%, N: 0.05% to 0.20%, W: 0.05% to 0.50%, and a microstructure with a high ratio of crystal grains with an aspect ratio of 3.5 or less, produced through a process involving heating to 1000°C to 1350°C, hot rolling with specific pass reductions, and rapid water cooling without solution heat treatment.

Benefits of technology

The method achieves excellent low-temperature toughness in the weld heat-affected zone, reducing manufacturing costs and maintaining high ductility and strength, making it suitable for extreme low-temperature applications like liquefied gas storage tanks without the need for costly solution heat treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided is a low-cost austenitic stainless steel having excellent low-temperature toughness in a welding heat affected portion. An austenitic stainless steel according to the present disclosure has: a component composition containing, in mass%, 0.050-0.100% of C, 0.05-1.00% of Si, 5.0-20.0% of Mn, 0.030% or less of P, 0.0050% or less of S, 0.070% or less of Al, 1.5-3.5% of Cu, 5.0-10.0% of Ni, 11.0-20.0% of Cr, 0.05-0.20% of N, 0.05-0.50% of W, 0.0050% or less of O, 0.005% or less of Ti, and 0.005% or less of Nb, the remaining portion being Fe and unavoidable impurities; a micro-structure in which the number proportion of crystal grains having an aspect ratio (long side / short side) of 3.5 or less is 85% or more, and in which the amount of deposited Cr having a diameter greater than 100 nm is 0.2 mass% or less; and a characteristic regarding having an absorption energy of 55 J or more as determined by a Charpy impact test at -269°C in a coarse grain zone of a welding heat affected portion.
Need to check novelty before this filing date? Find Prior Art

Description

Austenitic stainless steel and its manufacturing method

[0001] The present disclosure relates to austenitic stainless steels and methods for producing the same.

[0002] In order to use hot-rolled steel sheets as materials for storage tank structures for liquefied gases such as liquid hydrogen and liquid helium, the hot-rolled steel sheets are required to have excellent toughness at low temperatures. This is because the materials for such storage tank structures are used in extremely low-temperature environments. For example, when using hot-rolled steel sheets for storage tanks for liquid helium, it is desirable that the hot-rolled steel sheets have excellent toughness at temperatures below −269°C, which is the boiling point of helium. In general, the weld heat-affected zone in the welded portion of a steel sheet has inferior low-temperature toughness compared to the base material. Therefore, it is desirable to improve the low-temperature toughness of the weld heat-affected zone of the steel sheet.

[0003] Patent Document 1 discloses an austenitic stainless steel and a method for producing the same. This austenitic stainless steel has a chemical composition, in mass%, of 0.10% or less C, 1.00% or less Si, 6.0 to 12.0% Mn, 0.050% or less P, 0.0500% or less S, 15.0 to 17.0% Ni, 15.0 to 30.0% Cr, 0.01 to 0.30% V, 0.01 to 0.30% Nb, 0.40 to 0.60% N, 0 to 5.0% Mo, and the balance being Fe and impurities, satisfying a predetermined relationship, with an undissolved V content of 0.20% or less by mass and an undissolved Nb content of 0.20% or less by mass. Patent Document 1 also discloses that this austenitic stainless steel has high strength and excellent low-temperature toughness of welds.

[0004] Patent Document 2 discloses an austenitic stainless steel and a method for manufacturing the same, which has a chemical composition, in mass %, of C: 0.005 to 0.07%, Si: 0.1 to 1.2%, Mn: 3.2 to 6.5%, Ni: 9 to 14%, the total of at least one of Cu and Co: 0.005% or more and less than 3%, Cr: 19 to 24%, Mo: 1 to 4%, Nb: 0.05 to 0.4%, N: 0.15 to 0.50%, The austenitic stainless steel has an Al content of 0.05% or less, P content of 0.03% or less, S content of 0.002% or less, O content of 0.02% or less, V content of 0-0.5%, Ti content of 0-0.5%, B content of 0-0.01%, Ca content of 0-0.05%, Mg content of 0-0.05%, REM content of 0-0.5%, and the balance of Fe and impurities. The Nb content analyzed as an electrolytic extraction residue is 0.01-0.3% by mass. Patent Document 2 discloses that this austenitic stainless steel has excellent strength, ductility, and weldability, and discloses, for example, a tensile strength of 690 MPa or more at room temperature. Patent Document 2 also discloses that the strength and ductility of austenitic stainless steel are related to the Nb content analyzed as an electrolytic extraction residue, i.e., the amount of Nb-containing precipitates.

[0005] JP 2020-132979 A International Publication No. 2017 / 056619

[0006] The austenitic stainless steels described in Patent Documents 1 and 2 have a problem of high costs because their manufacturing process requires a solution heat treatment in addition to a hot working process. Therefore, there is a need for a method of manufacturing austenitic stainless steels that have excellent low-temperature toughness in the weld heat-affected zone without carrying out solution heat treatment.

[0007] The present disclosure has been made in view of the above circumstances, and its object is to provide a low-cost austenitic stainless steel having excellent low-temperature toughness in the heat-affected zone of a weld, and a method for producing the same.

[0008] In order to achieve the above object, the austenitic stainless steel and the method for producing the same according to the present disclosure are as follows.

[0009] [1] A component composition containing, in mass%, C: 0.050% or more and 0.100% or less, Si: 0.05% or more and 1.00% or less, Mn: 5.0% or more and 20.0% or less, P: 0.030% or less, S: 0.0050% or less, Al: 0.070% or less, Cu: 1.5% or more and 3.5% or less, Ni: 5.0% or more and 10.0% or less, Cr: 11.0% or more and 20.0% or less, N: 0.05% or more and 0.20% or less, W: 0.05% or more and 0.50% or less, O: 0.0050% or less, Ti: 0.005% or less, and Nb: 0.005% or less, with the balance being Fe and unavoidable impurities; An austenitic stainless steel having a microstructure in which the proportion of crystal grains having an aspect ratio (long side / short side) of 3.5 or less is 85% or more and the amount of precipitated Cr having a diameter of more than 100 nm is 0.2 mass % or less, and the absorbed energy in a coarse-grained region of a weld heat-affected zone in a Charpy impact test at -269°C is 55 J or more.

[0010] [2] The austenitic stainless steel according to [1] above, wherein the chemical composition further contains, in mass%, one or more elements selected from the group consisting of Mo: 2.0% or less, V: 0.5% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, and REM: 0.0200% or less.

[0011] [3] In mass%, C: 0.050% or more and 0.100% or less, Si: 0.05% or more and 1.00% or less, Mn: 5.0% or more and 20.0% or less, P: 0.030% or less, S: 0.0050% or less, Al: 0.070% or less, Cu: 1.5% or more and 3.5% or less, Ni: 5.0% or more and 10.0% or less, Cr: 11.0% or more and 20.0% or less, N: 0.05% or more and 0.20% or less, W: 0.05% or more and 0.50% or less, O: 0.0050% or less, Ti: 0.005% or less, and Nb: 0.005% or less. and the balance consisting of Fe and unavoidable impurities, to a temperature range of 1000°C or higher and 1350°C or lower; a hot rolling process of hot rolling the steel material after the heating process; and a cooling process of cooling the steel material after the hot rolling, wherein the hot rolling process includes: (i) a first rolling process of hot rolling the steel material at 950°C or higher with an average pass reduction of 5% or higher; and (ii) a second rolling process which is performed after the first rolling process and hot rolling the steel material for 5 passes or less at less than 950°C, wherein a finish rolling end temperature is 900°C or higher; and wherein the cooling process involves water cooling at an average water cooling rate of 10°C / s or higher from a cooling start temperature which is in a temperature range of at least a temperature which is 100°C lower than the finish rolling end temperature, to a cooling stop temperature which is in a temperature range of 600°C or lower.

[0012] [4] The method for producing an austenitic stainless steel according to [3] above, wherein the chemical composition further contains, in mass%, one or more elements selected from the group consisting of Mo: 2.0% or less, V: 0.5% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, and REM: 0.0200% or less.

[0013] According to the present disclosure, it is possible to provide a low-cost austenitic stainless steel having excellent low-temperature toughness in the weld heat-affected zone, and a method for producing the same.

[0014] An austenitic stainless steel and a method for producing the same according to an embodiment of the present disclosure will be described.

[0015] The austenitic stainless steel according to this embodiment has a component composition containing, in mass%, C: 0.050% or more and 0.100% or less, Si: 0.05% or more and 1.00% or less, Mn: 5.0% or more and 20.0% or less, P: 0.030% or less, S: 0.0050% or less, Al: 0.070% or less, Cu: 1.5% or more and 3.5% or less, Ni: 5.0% or more and 10.0% or less, Cr: 11.0% or more and 20.0% or less, N: 0.05% or more and 0.20% or less, W: 0.05% or more and 0.50% or less, O: 0.0050% or less, Ti: 0.005% or less, and Nb: 0.005% or less, with the balance being Fe and unavoidable impurities. The austenitic stainless steel according to this embodiment has a microstructure in which the proportion of crystal grains with an aspect ratio (long side / short side) of 3.5 or less is 85% or more and the amount of precipitated Cr with a diameter of more than 100 nm is 0.2 mass % or less, and the absorbed energy in a Charpy impact test at −269°C in the coarse grain region of the weld heat affected zone is 55 J or more.

[0016] The method for producing an austenitic stainless steel according to this embodiment includes a heating step of heating a steel material having the chemical composition described in the previous paragraph to a temperature range of 1000°C to 1350°C, a hot rolling step of hot-rolling the steel material after the heating step, and a cooling step of cooling the hot-rolled steel material. The hot rolling step includes (i) a first rolling step of hot-rolling the steel material at 950°C or higher with an average pass reduction of 5% or more, and (ii) a second rolling step, which is performed after the first rolling step, of hot-rolling the steel material at less than 950°C for five or fewer passes, and the finish rolling end temperature is 900°C or higher. The cooling step involves water cooling at an average water cooling rate of 10°C / s or higher from a cooling start temperature that is 100°C or higher than the finish rolling end temperature to a cooling stop temperature that is 600°C or lower.

[0017] The austenitic stainless steel according to this embodiment does not require a solution heat treatment step in its manufacturing process, so it can be manufactured at low cost. Furthermore, the austenitic stainless steel according to this embodiment has excellent low-temperature toughness in the weld heat-affected zone.

[0018] The austenitic stainless steel and the method for producing the same according to this embodiment will be described in detail below.

[0019] The austenitic stainless steel according to this embodiment is particularly suitable as a structural steel for use in extremely low temperature environments, such as tanks for storing liquid hydrogen, liquid helium, liquefied gases, and the like.

[0020] The chemical composition of the austenitic stainless steel according to this embodiment will be described. The austenitic stainless steel according to this embodiment has the chemical composition described above. As described above, the steel material used to manufacture the austenitic stainless steel according to this embodiment also has the same chemical composition as the austenitic stainless steel according to this embodiment.

[0021] In the following description, the designation "%" regarding the chemical composition means "mass %" unless otherwise specified. Hereinafter, austenitic stainless steels and steel materials used in the production thereof will be collectively referred to simply as steel materials.

[0022] The C content in the steel material is 0.050% or more and 0.100% or less. C is an inexpensive austenite stabilizing element and is an important element for obtaining austenite. C also dissolves in steel to increase the strength of the steel material through solid solution strengthening and has the effect of improving the low-temperature toughness of the weld heat affected zone. In order to fully obtain these effects, the steel material contains 0.050% or more of C. If the steel material contains more than 0.100% of C, coarse Cr precipitates are excessively formed, and the low-temperature toughness of the weld heat affected zone when the steel material is welded is reduced. The C content in the steel material is preferably 0.060% or more and preferably 0.090% or less.

[0023] The Si content in the steel material is 0.05% or more and 1.00% or less. Si not only acts as a deoxidizer and is necessary for steelmaking, but also has the effect of dissolving in steel to strengthen the steel material through solid solution strengthening. To achieve this effect, the steel material contains 0.05% or more Si. If the steel material contains more than 1.00% Si, non-thermal stress increases excessively, thereby deteriorating the low-temperature toughness of the weld heat-affected zone. The Si content in the steel material is preferably 0.07% or more and preferably 0.80% or less.

[0024] The Mn content in the steel material is 5.0% or more and 20.0% or less. Mn is an inexpensive austenite stabilizing element and is an important element for obtaining austenite. It also has the effect of dissolving in steel and strengthening the steel material through solid solution strengthening. Mn also has the effect of improving the low-temperature toughness of the weld heat-affected zone. To fully obtain these effects, the steel material contains 5.0% or more Mn. If the steel material contains more than 20.0% Mn, manufacturability and cuttability may deteriorate. The Mn content in the steel material is preferably 6.0% or more and preferably 19.0% or less.

[0025] The P content in the steel material is 0.030% or less. If the P content in the steel material exceeds 0.030%, the hot ductility of the steel material may decrease, which may result in an increase in intergranular cracking. For this reason, it is desirable to reduce the P content in the steel material as much as possible. The P content in the steel material is preferably 0.028% or less. Note that an excessive reduction in P content increases refining costs and is economically disadvantageous, so the P content in the steel material is preferably 0.002% or more.

[0026] The S content in the steel material is 0.0050% or less. If the S content in the steel material exceeds 0.0050%, the hot ductility of the steel material may decrease, which may result in an increase in intergranular cracking. For this reason, it is desirable to reduce the S content in the steel material as much as possible. The S content in the steel material is preferably 0.0045% or less. Note that excessive reduction of S content increases refining costs and is economically disadvantageous, so the S content in the steel material is preferably 0.0010% or more.

[0027] The Al content in the steel material is 0.070% or less. Al acts as a deoxidizer and is most commonly used in the molten steel deoxidation process. To obtain this effect, the steel material preferably contains 0.010% or more Al. If the steel material contains more than 0.070% Al, the hot ductility of the steel material may decrease, which may increase the occurrence of intergranular cracking. The Al content in the steel material is preferably 0.060% or less.

[0028] The Cu content in the steel material is 1.5% or more and 3.5% or less, and the Ni content is 5.0% or more and 10.0% or less. Cu and Ni are austenite-stabilizing elements and are important elements for obtaining austenite. They also increase the strength of the steel material through solid solution strengthening. Cu and Ni also have the effect of improving the low-temperature toughness of the weld heat-affected zone. To fully achieve these effects, the steel material contains 1.5% or more of Cu and 5.0% or more of Ni. If the steel material contains excessive amounts of these elements, the surface quality may deteriorate during rolling of the steel material and the manufacturing cost may be increased. Therefore, the Cu content in the steel material is 3.5% or less and the Ni content is 10.0% or less. Preferably, the Cu content in the steel material is 2.0% or more and 3.0% or less. Also, preferably, the Ni content in the steel material is 6.0% or more and 9.0% or less.

[0029] The Cr content in the steel material is 11.0% or more and 20.0% or less. Cr is an element necessary for ensuring the corrosion resistance of stainless steel. To achieve this effect, the steel material contains 11.0% or more Cr. If the steel material contains Cr more than 20.0%, coarse Cr precipitates are excessively formed, reducing the low-temperature toughness of the weld heat-affected zone. The Cr content in the steel material is preferably 12.0% or more and preferably 19.0% or less.

[0030] The N content in the steel material is 0.05% or more and 0.20% or less. N is an inexpensive austenite stabilizing element. N is an important element for obtaining austenite, and also has the effect of dissolving in steel to strengthen the steel material through solid solution strengthening. N also has the effect of improving the low-temperature toughness of the weld heat affected zone. To achieve this effect, the steel material contains 0.05% or more of N. If the steel material contains more than 0.20% of N, the nitrides or carbonitrides in the steel material may become coarse, which may reduce the low-temperature toughness of the weld heat affected zone. The N content in the steel material is preferably 0.06% or more and preferably 0.19% or less.

[0031] The W content in the steel material is 0.05% or more and 0.50% or less. W contributes to improving the strength of the steel material and also contributes to improving the corrosion resistance of the steel material. To achieve these effects, the steel material contains 0.05% or more of W. If the steel material contains W in excess of 0.50%, the manufacturing cost of the steel material will be increased. The W content in the steel material is preferably 0.10% or more and preferably 0.40% or less.

[0032] The O content in the steel material is 0.0050% or less. O deteriorates the low-temperature toughness of the weld heat-affected zone by forming oxides. The O content in the steel material is preferably 0.0045% or less. Note that excessive reduction of O increases the refining cost and is economically disadvantageous, so the O content in the steel material is preferably 0.0010% or more.

[0033] The Ti content in the steel material is 0.005% or less, and the Nb content is 0.005% or less. Ti and Nb form high-melting-point carbonitrides in the steel material, which may reduce the low-temperature toughness of the weld heat-affected zone. Ti and Nb are components mixed in from raw materials, etc. Generally, the Ti content in the steel material is more than 0.005% and less than 0.010%, and the Nb content is more than 0.005% and less than 0.010%. Therefore, it is necessary to avoid the mixing of Ti and Nb into the steel material and to limit the Ti and Nb contents to 0.005% or less, respectively, according to the melting method described below. By limiting the Ti and Nb contents in the steel material to 0.005% or less, respectively, the adverse effects of the carbonitrides can be eliminated, and excellent low-temperature toughness and ductility can be ensured in the steel material. The Ti content in the steel material is preferably 0.003% or less. In addition, the Nb content in the steel material is preferably 0.003% or less. Of course, the Ti and Nb contents in the steel material may be 0.000% or 0.001% or more.

[0034] The steel material in this embodiment is composed of iron (Fe) and inevitable impurities other than the above-mentioned components. Examples of inevitable impurities include H and B, and a total content of each element of 0.01% or less is acceptable. In this embodiment, inevitable impurities refer to impurities that are inevitably mixed in from raw materials, manufacturing processes, manufacturing equipment, etc., and are acceptable to be present within a range that does not impair the objectives of the present invention. Examples of raw materials include iron ore, reduced iron, and scrap.

[0035] The steel material in this embodiment may contain the elements described below as optional components as necessary.

[0036] The Mo content in the steel material may be 2.0% or less. The V content in the steel material may be 0.5% or less. Mo and V contribute to stabilizing austenite and improving the strength of the steel material. To achieve these effects, the steel material preferably contains Mo and V in an amount of 0.1% or more each. If the steel material contains Mo and V in an amount exceeding 2.0% and 0.5%, respectively, the manufacturing cost may be increased.

[0037] The Ca content in the steel material may be 0.0100% or less. The Mg content in the steel material may be 0.0100% or less. The REM (rare earth metal) content in the steel material may be 0.0200% or less. Ca, Mg, and REM are elements useful for controlling the morphology of inclusions. Controlling the morphology of inclusions means converting elongated sulfide-based inclusions into granular inclusions. Through this control of the morphology of inclusions, the ductility, low-temperature toughness, and sulfide stress corrosion cracking resistance of the steel material are improved. To achieve these effects, the steel material preferably contains 0.0005% or more of Ca and Mg and 0.0010% or more of REM. If the steel material contains excessive amounts of these elements, the amount of non-metallic inclusions may increase, which may actually reduce the ductility, low-temperature toughness, or sulfide stress corrosion cracking resistance of the steel material. This may also be economically disadvantageous. It is preferable that the Ca content be 0.0080% or less, the Mg content be 0.0080% or less, and the REM content be 0.0150% or less.

[0038] Next, the microstructure of the austenitic stainless steel according to this embodiment will be described.

[0039] In the austenitic stainless steel according to this embodiment, the proportion of crystal grains with an aspect ratio (longer side / shorter side) of 3.5 or less is 85% or more, and the amount of precipitated Cr with a diameter exceeding 100 nm is 0.2% by mass or less. When the aspect ratio of the crystal grains in austenitic stainless steel is large, stress tends to concentrate at the grain boundaries, and the coarse Cr present at the grain boundaries becomes the origin of fracture, resulting in reduced low-temperature toughness. By setting the proportion of crystal grains with an aspect ratio of 3.5 or less to 85% or more and setting the amount of precipitated Cr with a diameter exceeding 100 nm to 0.2% by mass or less, excellent toughness can be achieved in the coarse-grained region of the weld heat-affected zone when the steel is welded, with an absorbed energy of 55 J or more in a Charpy impact test at −269°C.

[0040] In the austenitic stainless steel according to this embodiment, the proportion of crystal grains having an aspect ratio of 3.5 or less is preferably 87% or more, more preferably 90% or more. In the austenitic stainless steel according to this embodiment, there is no upper limit to the proportion of crystal grains having an aspect ratio of 3.5 or less. To ensure the strength of the austenitic stainless steel according to this embodiment, the proportion of crystal grains having an aspect ratio of 3.5 or less is preferably 97% or less, more preferably 95% or less. In the austenitic stainless steel according to this embodiment, the above aspect ratio is a value measured by the method described in the Examples below. The lower limit of the aspect ratio is 1.0 (when the long side and short side are equal).

[0041] The amount of precipitated Cr having a diameter of more than 100 nm in the austenitic stainless steel according to this embodiment is preferably 0.1 mass % or less. The lower limit of the amount of precipitated Cr having a diameter of more than 100 nm in the austenitic stainless steel according to this embodiment is not particularly specified, and the lower the amount, the more preferable it is, and it may be 0.0 mass %. The amount of precipitated Cr having a diameter of more than 100 nm in the austenitic stainless steel according to this embodiment is a value measured by the method described in the examples below.

[0042] In this embodiment, by performing hot rolling and water cooling under the conditions described below, the ratio of the number of crystal grains having an aspect ratio of 3.5 or less and the amount of precipitated Cr having a diameter of more than 100 nm can be controlled within the above-mentioned numerical ranges. As a result, the austenitic stainless steel according to this embodiment can achieve the low-temperature toughness of the weld heat-affected zone.

[0043] In this embodiment, the austenitic stainless steel may be a steel plate having a thickness of 10 mm or more. When the austenitic stainless steel according to this embodiment is a steel plate, the thickness of the steel plate is preferably 12 mm or more from the viewpoint of suitable use as a structural steel material used in extremely low-temperature environments. The upper limit of the thickness of the steel plate is not particularly limited and can be any thickness, but it is preferably 30 mm or less.

[0044] Next, an example of a method for producing the austenitic stainless steel according to this embodiment will be described.

[0045] First, molten steel having the above-mentioned composition is obtained by melting using a known melting method such as a converter or an electric furnace, etc. Secondary refining may also be carried out in a vacuum degassing furnace.

[0046] When obtaining the austenitic stainless steel according to this embodiment, in order to limit the contents of Ti and Nb, which hinder structural control, to the above-mentioned numerical ranges, it is necessary to take measures to prevent Ti and Nb from being mixed in raw materials as much as possible and to reduce their contents. For example, the basicity of the slag in the refining stage may be reduced to concentrate these alloys in the slag and discharge them, thereby reducing the concentrations of Ti and Nb in the slab product. Alternatively, oxygen may be blown into the molten steel to oxidize it, and the Ti and Nb alloy may be floated and separated during reflux.

[0047] Thereafter, it is preferable to produce a steel material such as a slab of a predetermined size by a known casting method such as a continuous casting method or an ingot-making and blooming rolling method.

[0048] The method for producing austenitic stainless steel according to this embodiment will be described in detail below.

[0049] In the method for producing austenitic stainless steel according to this embodiment, the heating step, the hot rolling step, and the cooling step are carried out as described above.

[0050] In the following description, unless otherwise specified, the temperature indicated in "°C" refers to the surface temperature of the steel material or steel plate (austenitic stainless steel). In each process described below, the temperature is controlled based on the surface temperature of the steel material or steel plate. The surface temperature can be measured, for example, with a radiation thermometer.

[0051] In the heating step, the steel material is heated to 1000°C or higher and 1350°C or lower. By setting the heating temperature of the steel material to 1000°C or higher, segregation can be reduced in the hot rolling step described below, and an austenite structure can be obtained even in negative segregation areas, ensuring low-temperature toughness in the weld heat-affected zone. If the heating temperature of the steel material exceeds 1350°C, the steel may begin to melt. The heating temperature of the steel material is preferably 1130°C or higher and 1320°C or lower.

[0052] The hot rolling process includes a first rolling process and a second rolling process that is performed after the first rolling process.

[0053] In the first rolling step, the steel material after the heating step is hot-rolled at 950°C or higher. In the first rolling step, the average pass reduction is set to 5% or higher. As described above, in the present disclosure, it is important to ensure that the proportion of crystal grains with an aspect ratio (longer side / shorter side) of 3.5 or less in the microstructure of the austenitic stainless steel is 85% or higher. If mixed grains are formed in the first rolling step, i.e., rolling in the recrystallization region, the aspect ratio of the crystal grains will increase in the subsequent rolling (second rolling step). Therefore, in the first rolling step, it is effective to set the average pass reduction to 5% or higher in order to promote recrystallization in the temperature range of 950°C or higher, which is the recrystallization region. The upper limit of the temperature of the steel material in the first rolling step is not particularly limited, but the temperature can be 1350°C or lower. In the first rolling step, the average pass reduction is preferably 6% or higher. In the first rolling step, the higher the average pass reduction is, the more preferable. However, from the viewpoint of the capacity of the rolling mill, the average pass reduction may be 10% or less.

[0054] In the second rolling step, the steel material is hot-rolled for 5 passes or less at a temperature of less than 950°C. The finish rolling temperature is 900°C or higher. That is, the hot rolling of the steel material in the second rolling step is performed at a temperature of 900°C or higher but lower than 950°C.

[0055] Since the temperature ranges from below 950°C to above 900°C, which is a partial recrystallization region, the aspect ratio of the crystal grains of the steel material increases in the second rolling step. Therefore, it is important to limit the number of hot rolling passes below 950°C in the second rolling step to five or less. The number of hot rolling passes below 950°C in the second rolling step is preferably three or less. The lower limit of the number of hot rolling passes below 950°C is zero.

[0056] If hot rolling is performed at a temperature below 900°C in the second rolling step, the aspect ratio of the crystal grains will increase significantly due to the non-recrystallized region. Therefore, the finish rolling end temperature (the temperature of the steel material at the entry side of the last rolling pass in the second rolling step) is set to 900°C or higher. The finish rolling end temperature is preferably 920°C or higher. The finish rolling end temperature is less than 950°C.

[0057] The cooling step is performed after the second rolling step. In the cooling step, the steel material is water-cooled. In the cooling step, the steel material is water-cooled at an average water-cooling rate of 10°C / s or more from a cooling start temperature in a temperature range equal to or higher than a temperature 100°C lower than the finish rolling end temperature (finish rolling end temperature -100°C) to a cooling stop temperature in a temperature range equal to or lower than 600°C. This suppresses the formation of precipitated Cr and can suppress a decrease in the low-temperature toughness of the weld heat-affected zone of the austenitic stainless steel. The upper limit of the cooling start temperature is not particularly limited, but the cooling start temperature can be 920°C or less. The lower limit of the cooling stop temperature is not particularly limited, but the cooling stop temperature can be 250°C or higher. The upper limit of the average water-cooling rate is not particularly limited, but the average water-cooling rate can be 40°C / s or less.

[0058] In the method for producing austenitic stainless steel according to this embodiment, no solution heat treatment is performed after the cooling step. Solution heat treatment for austenitic stainless steel involves heating the austenitic stainless steel, in which precipitated Cr has formed, to 1000 to 1100°C, maintaining the temperature until a single-phase austenite structure is formed, and then rapidly cooling the stainless steel in water, thereby resolving the precipitated Cr and restoring corrosion resistance.

[0059] In this manner, an austenitic stainless steel and a method for producing the same can be provided.

[0060] The present disclosure will be described below based on examples. Note that the following examples are preferred examples of the present disclosure, and the present disclosure is not limited to these examples.

[0061] Steel slabs (Steel Nos. 1 to 29) with the chemical compositions shown in Table 1 were produced using a converter-ladle refining (secondary refining)-continuous casting process. The symbol "-" in Table 1 indicates that a component is not intentionally added, and includes not only cases where the component is not contained (0%) but also cases where the component is inevitably contained. In Table 1, Steel Nos. 1 to 10 and 23 to 29 have the chemical compositions according to this embodiment. Next, the steel slabs were heated and hot-rolled under the conditions shown in Table 2 (see "Steel Plate Manufacturing Method" in Table 2), followed by water cooling, to produce austenitic stainless steel plates (Sample Nos. 1 to 36) with thicknesses of 10 to 30 mm. Furthermore, rectangular joint test plates (size: 250 mm x 500 mm) were taken from the produced steel plates, and welded joints were produced by MAG welding. This welding involved a square groove, a ceramic backing material, and Ar-30% CO shielding gas. 2 The welding conditions were: 1.5° torch sweepback angle: 5-10°, and average welding heat input: 2.0 kJ / mm. In Table 2, steel plates of Sample Nos. 1-10 and 30-36 are austenitic stainless steels according to the invention that satisfy the range of this embodiment. In Tables 1 and 2, underlined values ​​indicate that the values ​​are outside the range specified in this embodiment.

[0062]

[0063]

[0064] The obtained steel plates and welded joints were evaluated in the following manner.

[0065] (1) The ratio of the number of crystal grains having an aspect ratio of 3.5 or less was determined as follows.

[0066] The cross section of the obtained steel sheet perpendicular to the sheet width direction was polished and etched, and the electron backscatter diffraction (EBSD) pattern was measured in a scanning electron microscope (SEM) at the center position of the sheet thickness. The measurement area was 1 mm × 1 mm. The measured EBSD data was analyzed using OIM-Analysis, and the number ratio of crystal grains having an aspect ratio (long side / short side) of 3.5 or less was calculated. These number ratios are also shown in Table 2.

[0067] (2) The amount of precipitated Cr with a diameter of more than 100 nm was determined as follows.

[0068] For the obtained hot-rolled steel sheets, samples for electrolytic extraction were taken from the center position of the sheet thickness, and the precipitates extracted by electrolytic extraction using a 10% AA (10% acetylacetone-1% tetramethylammonium chloride-methanol) solution were filtered and collected using an alumina filter with a pore size of 100 nm, and the Cr content in the precipitates was measured by ICP atomic emission spectrometry. The amounts of these precipitated Cr with diameters exceeding 100 nm are also shown in Table 2.

[0069] (3) The low temperature toughness of the weld heat affected zone was evaluated as follows.

[0070] For the welded joints produced from each sample, three Charpy V-notch test specimens were taken from each sample in accordance with the provisions of JIS Z 2242 (2023). Using the three Charpy V-notch test specimens, a Charpy impact test was performed at -269°C. The average value of the absorbed energy of the three test specimens was then calculated. Note that the temperature (-269°C) at which the Charpy impact test was performed in this example corresponds to the boiling point of liquid helium.

[0071] The average values ​​thus determined are also shown as absorbed energies at -269°C in Table 2. When the average absorbed energy of the three specimens was 55 J or more, the specimen was judged to have excellent low-temperature toughness, satisfying the target performance. That is, in this embodiment, excellent low-temperature toughness means that the average absorbed energy in a Charpy impact test is 55 J or more in an environment of -269°C, which is the boiling point of liquid helium.

[0072] As shown in Table 2, the austenitic stainless steel according to this embodiment (samples Nos. 1 to 10, 30 to 36) has a microstructure in which the number ratio of crystal grains having an aspect ratio (long side / short side) of 3.5 or less is 85% or more, and the amount of precipitated Cr having a diameter of more than 100 nm is 0.2% by mass or less.

[0073] Furthermore, in these austenitic stainless steels according to this embodiment, the absorbed energy in the coarse grain region of the weld heat affected zone in a Charpy impact test at −269° C. was 55 J or more, satisfying the target performance.

[0074] In contrast, the steel sheets of Samples No. 11 to 29, which are outside the scope of the present disclosure, could not satisfy the target performance, regardless of the ratio of the number of crystal grains having an aspect ratio of 3.5 or less and the amount of precipitated Cr having a diameter of more than 100 nm.

[0075] As shown in the above examples, the austenitic stainless steel according to this embodiment can be produced at low cost because it does not require a heat treatment step in its production process. Furthermore, the austenitic stainless steel according to this embodiment has excellent toughness in low-temperature environments. Therefore, the austenitic stainless steel according to this embodiment can be suitably used as a material for steel structures (such as tanks for liquefied gas storage) used in low-temperature environments. This can significantly contribute to improving the safety and lifespan of such steel structures. Furthermore, the method for producing the austenitic stainless steel according to this embodiment is economical because it does not result in a decrease in productivity or an increase in production costs.

[0076] It should be noted that the embodiments disclosed in this specification are merely examples, and the embodiments of the present disclosure are not limited to these, and can be modified as appropriate within the scope of the purpose of the present disclosure.

[0077] The present disclosure is applicable to austenitic stainless steels and methods for making same.

Claims

1. A component composition containing, by mass%, C: 0.050% to 0.100%, Si: 0.05% to 1.00%, Mn: 5.0% to 20.0%, P: 0.030% or less, S: 0.0050% or less, Al: 0.070% or less, Cu: 1.5% to 3.5%, Ni: 5.0% to 10.0%, Cr: 11.0% to 20.0%, N: 0.05% to 0.20%, W: 0.05% to 0.50%, O: 0.0050% or less, Ti: 0.005% or less, and Nb: 0.005% or less, with the balance being Fe and unavoidable impurities; An austenitic stainless steel having a microstructure in which the ratio of the number of crystal grains having an aspect ratio (long side / short side) of 3.5 or less is 85% or more and the amount of precipitated Cr having a diameter of more than 100 nm is 0.2 mass % or less, and a characteristic in which the absorbed energy in a Charpy impact test at -269°C in a coarse grain region of a weld heat affected zone is 55 J or more.

2. The austenitic stainless steel according to claim 1, wherein the chemical composition further contains, in mass percent, one or more elements selected from the group consisting of Mo: 2.0% or less, V: 0.5% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, and REM: 0.0200% or less.

3. In mass%, C: 0.050% or more and 0.100% or less, Si: 0.05% or more and 1.00% or less, Mn: 5.0% or more and 20.0% or less, P: 0.030% or less, S: 0.0050% or less, Al: 0.070% or less, Cu: 1.5% or more and 3.5% or less, Ni: 5.0% or more and 10.0% or less, Cr: 11.0% or more and 20.0% or less, N: 0.05% or more and 0.20% or less, W: 0.05% or more and 0.50% or less, O: 0.0050% or less, Ti: 0.005% or less, and Nb: 0.005% or less. and the balance being Fe and unavoidable impurities, to a temperature range of 1000°C or higher and 1350°C or lower; a hot rolling process of hot rolling the steel material after the heating process; and a cooling process of cooling the steel material after the hot rolling, wherein the hot rolling process includes: (i) a first rolling process of hot rolling the steel material at 950°C or higher with an average pass reduction of 5% or higher; and (ii) a second rolling process which is performed after the first rolling process and hot rolling the steel material at less than 950°C for 5 passes or less, wherein a finish rolling end temperature is 900°C or higher; and wherein the cooling process includes water cooling at an average water cooling rate of 10°C / s or higher from a cooling start temperature which is in a temperature range of 100°C lower than the finish rolling end temperature to a cooling stop temperature which is in a temperature range of 600°C or lower.

4. A method for producing an austenitic stainless steel as described in claim 3, wherein the chemical composition further contains, in mass percent, one or more selected from the group consisting of Mo: 2.0% or less, V: 0.5% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, and REM: 0.0200% or less.

Citation Information

Patent Citations

  • Austenitic stainless steels plate having high strength and high toughness at very low temperature

    JP1986270356A

  • Production of high mn non-magnetic steel plate excellent in toughness at low temperature

    JP1994293920A

  • HIGH Mn STEEL MATERIAL FOR CRYOGENIC USE

    JP2016196703A

  • Austenitic alloy for cryogenic applications

    WO2010013083A1

  • Steel, and method for producing same

    WO2021033693A1