Positive electrode for power storage elements, power storage element, and power storage device
The direct lamination of high-strength, large-particle-size positive electrode active material layers on a metal aluminum base material with a non-aqueous binder in power storage devices addresses the high resistance and cost issues of existing technologies, achieving improved electrical performance and cost-effectiveness.
Patent Information
- Application Number
- PCT/JP2024/018571
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2024-05-21
- Publication Date
- 2024-12-05
AI Technical Summary
Existing positive electrodes for power storage devices, such as lithium ion batteries, have high electrical resistance due to the use of conductive layers which increase costs and reduce strength, and alternative methods like surface roughening treatments are expensive and may compromise manufacturing.
A positive electrode structure with a positive electrode active material layer directly laminated on a metal aluminum base material, where the active material particles have a breaking strength of 30 MPa or more and an average size of 3 μm or more, and a non-aqueous binder, with a high area ratio of recessed regions for improved contact and reduced resistance.
This configuration reduces electrical resistance while maintaining strength and reducing costs by ensuring sufficient sinking of active material particles into the base material, enhancing the performance and efficiency of power storage devices.
Smart Images

Figure JP2024018571_05122024_PF_FP_ABST
Abstract
Description
Positive electrode for energy storage element, energy storage element, and energy storage device
[0001] The present invention relates to a positive electrode for an energy storage element, an energy storage element, and an energy storage device.
[0002] Non-aqueous electrolyte secondary batteries, typified by lithium-ion non-aqueous electrolyte secondary batteries, are widely used in electronic devices such as personal computers and communication terminals, automobiles, etc., due to their high energy density. Non-aqueous electrolyte secondary batteries generally include an electrode assembly having a pair of electrodes electrically isolated by a separator, and a non-aqueous electrolyte interposed between the electrodes, and are configured to charge and discharge by transferring charge-transporting ions between the electrodes. Furthermore, capacitors such as lithium-ion capacitors and electric double layer capacitors are also widely used as energy storage elements other than non-aqueous electrolyte secondary batteries.
[0003] In general, the positive electrode of an energy storage device has a layer containing a positive electrode active material capable of absorbing and releasing charge-transporting ions. Patent Document 1 describes an invention of a positive electrode for a non-aqueous electrolyte secondary battery having a structure in which a conductive base layer is provided between a positive electrode current collector sheet and a positive electrode active material layer.
[0004] International Publication No. 2017 / 195332
[0005] Providing a conductive layer between a positive electrode current collector sheet (also referred to as a positive electrode substrate, etc.) and a positive electrode active material layer, as in the positive electrode described in Patent Document 1, has the advantage of reducing electrical resistance, but has the disadvantage of being expensive.
[0006] An object of the present invention is to provide a positive electrode for an electric storage element having a structure in which a positive electrode active material layer is directly laminated on a positive electrode substrate, and which has reduced electrical resistance, and to provide an electric storage element and an electric storage device in which such a positive electrode for an electric storage element is used.
[0007] A positive electrode for a storage element according to one aspect of the present invention includes a positive electrode substrate containing metallic aluminum and having a surface on which the metallic aluminum is exposed, and a positive electrode active material layer directly laminated on the surface on which the metallic aluminum is exposed and containing positive electrode active material particles, wherein the positive electrode active material particles have a breaking strength of 30 MPa or more, the positive electrode active material particles have an average particle size of 3 μm or more, the positive electrode active material layer contains a non-aqueous binder, and the proportion of an area of recesses in the region on the surface on which the metallic aluminum is exposed, where the positive electrode active material layer is laminated, is 5% or more.
[0008] An energy storage element according to another aspect of the present invention includes the energy storage element electrode.
[0009] According to another aspect of the present invention, there is provided an electric storage device including two or more electric storage elements, and including one or more of the electric storage elements.
[0010] According to any one aspect of the present invention, it is possible to provide a positive electrode for an energy storage element having a structure in which a positive electrode active material layer is directly laminated on a positive electrode substrate, the positive electrode having reduced electrical resistance, and an energy storage element and an energy storage device in which such a positive electrode for an energy storage element is used.
[0011] Fig. 1 is a schematic cross-sectional view showing one embodiment of a positive electrode for an energy storage element. Fig. 2 is a see-through perspective view showing one embodiment of an energy storage element. Fig. 3 is a schematic view showing one embodiment of an energy storage device formed by assembling a plurality of energy storage elements.
[0012] First, an outline of the energy storage element electrode, the energy storage element, and the energy storage device disclosed in this specification will be described.
[0013] [1] A positive electrode for a storage element according to one aspect of the present invention includes a positive electrode substrate containing metallic aluminum and having a surface on which the metallic aluminum is exposed, and a positive electrode active material layer directly laminated on the surface on which the metallic aluminum is exposed and containing positive electrode active material particles, wherein the positive electrode active material particles have a breaking strength of 30 MPa or more, the positive electrode active material particles have an average particle size of 3 μm or more, the positive electrode active material layer contains a non-aqueous binder, and a proportion of an area of recesses in a region on the surface on which the metallic aluminum is exposed, where the positive electrode active material layer is laminated, is 5% or more.
[0014] The positive electrode for a storage element described in [1] above (hereinafter also simply referred to as "positive electrode") has a structure in which a positive electrode active material layer is directly laminated on a positive electrode substrate, and has reduced electrical resistance. The reason for this is unclear, but the following reason is presumed. The positive electrode active material particles used in the positive electrode described in [1] above are hard, with a breaking strength of 30 MPa or more, and have a sufficient size, with an average particle size of 3 μm or more. During the manufacturing process of the positive electrode, a positive electrode active material layer containing such positive electrode active material particles is laminated on a positive electrode substrate and pressed, causing at least a portion of the positive electrode active material particles to sink into the positive electrode substrate. Here, in the positive electrode described in [1] above, the "proportion of the area of the recesses in the region where the positive electrode active material layer is laminated on the surface where the metal aluminum is exposed" represents the degree to which the positive electrode active material particles have sink into the positive electrode substrate. In other words, a proportion of the area of the recesses of 5% or more indicates that a large number of positive electrode active material particles are sufficiently embedded in the positive electrode substrate. In the positive electrode described in [1] above, since a large number of positive electrode active material particles are sufficiently embedded in the positive electrode substrate, the contact area between the positive electrode active material particles and the positive electrode substrate is large, and it is presumed that the electrical resistance is reduced. Note that, when the breaking strength of the positive electrode active material particles is less than 30 MPa, and when the average particle size of the positive electrode active material particles is less than 3 μm, even if pressing is performed during the positive electrode manufacturing process, the positive electrode active material particles do not sufficiently embed into the positive electrode substrate, and the effect of reducing electrical resistance is not achieved. In addition, since the non-aqueous binder is softer than the aqueous binder, the positive electrode active material particles do not embed too much into the positive electrode substrate, and the strength of the positive electrode substrate can be maintained.
[0015] When the positive electrode is incorporated into an energy storage device, the fracture strength and average particle size of the positive electrode active material particles are measured in a fully discharged state using the following method. First, the energy storage device is charged at a constant current of 0.1 C until the end-of-charge voltage in normal use is reached, and then fully charged. After a 10-minute rest, the device is discharged at a constant current of 0.1 C until the end-of-charge voltage in normal use (lower limit voltage) is reached. The energy storage device is disassembled, the positive electrode is removed, and a test battery is assembled using a metallic lithium electrode as the counter electrode. A current of 10 mA per gram of positive electrode active material layer is applied until the positive electrode potential reaches 2.0 V vs. Li / Li. +The positive electrode is adjusted to a fully discharged state by constant current discharge until the positive electrode reaches a fully discharged state. The test battery is disassembled again and the positive electrode is removed. The electrolyte and other materials adhering to the removed positive electrode are thoroughly washed using dimethyl carbonate, and the electrode is dried overnight at room temperature before the positive electrode active material particles are collected. The collected positive electrode active material particles are then subjected to measurement. The operations from disassembling the energy storage element to collecting the positive electrode active material particles are carried out in an argon atmosphere with a dew point of -60°C or lower. "Normal use" refers to the case where the energy storage element is used under the charging and discharging conditions recommended or specified for the energy storage element. Regarding charging conditions, for example, if a charger for the energy storage element is provided, the energy storage element may be used using that charger.
[0016] The "breaking strength" of the positive electrode active material particles is measured by a microcompression test using a microcompression tester (Shimadzu Corporation's "MCT-511"). Specifically, in compression test mode, the breaking test force is measured under the conditions of indenter type: FLAT50, load rate: 0.1340 mN / sec, and test force: 1.0 mN to 30.0 mN, and the breaking strength of the positive electrode active material is determined in accordance with JIS-R-1639-5 (2007). In addition, the breaking strength is measured for five positive electrode active material particles, and the average value is used.
[0017] The "average particle size" of the positive electrode active material particles means the value at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50% based on the particle size distribution measured by a laser diffraction / scattering method for a diluted solution obtained by diluting the particles with a solvent in accordance with JIS-Z-8825 (2013). The same applies to the average particle sizes of other particles.
[0018] The "recess" in the positive electrode substrate refers to a recess having a diameter of 1 μm or more. The "area ratio of the recess in the region where the positive electrode active material layer is laminated on the surface where the metallic aluminum is exposed" is determined by immersing the positive electrode in a solvent capable of dissolving the nonaqueous binder contained in the positive electrode, subjecting it to ultrasonic cleaning at a temperature of 80°C to peel off the positive electrode active material layer from the positive electrode, and observing the resulting positive electrode substrate with a scanning electron microscope (SEM). Specifically, a JSM-7001F (manufactured by JEOL Ltd.) is used as the SEM. The SEM image is a secondary electron image. The acceleration voltage is 15 kV. The observation magnification is set to 20,000x. Other conditions, such as spot diameter, working distance, irradiation current, brightness, and focus, are appropriately set so that the contours of the recess are clearly visible. The surface of the positive electrode substrate in the region where the positive electrode active material layer was laminated on the surface where the metallic aluminum was exposed is observed with an SEM, and the obtained SEM image is saved as an image file. Using image analysis software, 2.88 mm 2 The area of each recess having a diameter of 1 μm or more in the observed area range was added up, and the area of the region where the positive electrode active material layer was laminated on the surface where the metallic aluminum was exposed (2.88 mm 2 ) is calculated as a ratio of the total area of the recesses to the total area of the positive electrode active material layer. If the recesses have a shape other than a perfect circle, the longest diameter is taken as the diameter. The "ratio of the area of the recesses in the region where the positive electrode active material layer is not laminated (on the surface where the metallic aluminum is exposed)" described below is also measured and calculated in the same manner.
[0019] [2] In the positive electrode according to the above [1], a region where the positive electrode active material layer is not stacked may exist on the surface where the metallic aluminum is exposed, and the ratio of an area of recesses in the region where the positive electrode active material layer is not stacked may be 0.5% or less.
[0020] To reduce the electrical resistance of the positive electrode, it is also possible to use a surface-roughened positive electrode substrate. A positive electrode using a surface-roughened positive electrode substrate also reduces electrical resistance due to the increased contact area between the positive electrode substrate and the positive electrode active material particles. However, surface-roughened positive electrode substrates are expensive. Furthermore, the strength of a surface-roughened positive electrode substrate may be reduced due to the sinking of the positive electrode active material particles, which may cause manufacturing problems. In the case of a surface-roughened positive electrode substrate, the entire surface is generally uniformly roughened. That is, when the proportion of the area of recesses in the region where the positive electrode active material layer is not stacked exceeds 0.5%, it is generally assumed that a surface-roughened positive electrode substrate is used. In contrast, in the positive electrode described in [2] above, the proportion of the area of recesses in the region where the positive electrode active material layer is not stacked is 0.5% or less, i.e., a positive electrode substrate that is not surface-roughened is used, which can reduce costs and improve strength.
[0021] [3] In the positive electrode according to the above [1] or [2], the positive electrode active material particles may contain a lithium transition metal compound having a polyanion structure.
[0022] Lithium transition metal compounds having a polyanion structure usually have lower electronic conductivity than other positive electrode active materials, and therefore, in the case of the positive electrode described in [3] above, in which the positive electrode active material particles contain a lithium transition metal compound having a polyanion structure, the advantage of reduced electrical resistance is significant.
[0023] [4] In the positive electrode according to any one of [1] to [3] above, the density of the positive electrode active material layer is 1.5 g / cm 3 It may be more than that.
[0024] The positive electrode described in the above [4] has a further reduced electrical resistance.
[0025] The "density" of the positive electrode active material layer is a value calculated from the mass per area of the positive electrode active material layer and the average thickness of one layer of the positive electrode active material layer. That is, the "density" of the positive electrode active material layer is the apparent density. In the case where positive electrode active material layers are provided on both sides of the positive electrode substrate, the "density" is the average thickness of one positive electrode active material layer provided on one side of the positive electrode substrate. The average thickness of the positive electrode active material layer is the average value of thicknesses measured at any five positions.
[0026] [5] In the positive electrode according to any one of [1] to [4] above, the positive electrode active material layer may further contain a conductive agent, and the content of the conductive agent in the positive electrode active material layer may be 0.5 mass% or more.
[0027] The positive electrode described in the above [5] has a further reduced electrical resistance.
[0028] [6] An energy storage device according to another aspect of the present invention includes the positive electrode according to any one of [1] to [5] above.
[0029] The energy storage element according to the above [6] includes the positive electrode according to any one of the above [1] to [5], and therefore has reduced electrical resistance.
[0030] [7] A power storage device according to another aspect of the present invention includes two or more power storage elements, and includes one or more of the power storage elements described in [6] above.
[0031] The electricity storage device according to the above [7] includes one or more electricity storage elements according to the above [6], and therefore has reduced electrical resistance.
[0032] A positive electrode, a manufacturing method of a positive electrode, an energy storage element, an energy storage device, a manufacturing method of an energy storage element, and other embodiments according to one embodiment of the present invention will be described in detail. Note that the names of the components (elementary components) used in each embodiment may differ from the names of the components (elementary components) used in the background art.
[0033] 1 according to one embodiment of the present invention includes a positive electrode substrate 2 and a positive electrode active material layer 3 laminated directly on the positive electrode substrate 2. The positive electrode 1 is a positive electrode for an electricity storage element, and is preferably a positive electrode for a non-aqueous electrolyte electricity storage element.
[0034] The positive electrode substrate 2 has electrical conductivity. Whether or not the positive electrode substrate 2 has electrical conductivity is determined by determining whether or not the volume resistivity measured in accordance with JIS-H-0505 (1975) is 10 -2 The judgment is made using Ω·cm as a threshold value.
[0035] The positive electrode substrate 2 contains metallic aluminum. Metallic aluminum is a substance containing aluminum element and having metallic properties. The metallic aluminum may be pure aluminum or an aluminum alloy. The positive electrode substrate 2 may consist essentially of pure aluminum or an aluminum alloy, or may consist of pure aluminum or an aluminum alloy. The aluminum element content in the positive electrode substrate 2 may be 80% by mass or more and 100% by mass or less, or 95% by mass or more and 100% by mass or less. Examples of pure aluminum or aluminum alloys include A1085, A3003, and A1N30 specified in JIS-H-4000 (2014) or JIS-H-4160 (2006).
[0036] The positive electrode substrate 2 shown in Fig. 1 has a plate shape. The positive electrode substrate 2 may be, for example, a substrate made of a material other than metallic aluminum, on which a metallic aluminum layer is provided by vapor deposition or the like, but is preferably a metallic aluminum foil. That is, the positive electrode substrate 2 is preferably a pure aluminum foil or an aluminum alloy foil. Hereinafter, pure aluminum foil and aluminum alloy foil will also be collectively referred to as aluminum foil.
[0037] The positive electrode substrate 2 has a surface on which metallic aluminum is exposed. In one embodiment of the present invention, the positive electrode substrate 2 may have metallic aluminum exposed over the entire surface. When the positive electrode substrate 2 is an aluminum foil, metallic aluminum is usually exposed over the entire surface of the positive electrode substrate 2. Note that a positive electrode substrate 2 containing metallic aluminum, on the surface of which a coating such as a coating made of aluminum oxide or a coating containing aluminum fluoride is formed, is also included in those having a surface on which metallic aluminum is exposed.
[0038] The average thickness of the positive electrode substrate 2 is preferably 3 μm to 50 μm, more preferably 5 μm to 40 μm, even more preferably 8 μm to 30 μm, and particularly preferably 10 μm to 25 μm. By setting the average thickness of the positive electrode substrate 2 within the above range, the strength of the positive electrode substrate 2 can be increased while increasing the energy density per volume of the energy storage element.
[0039] The positive electrode active material layer 3 is laminated directly on the surface of the positive electrode substrate 2 where the metallic aluminum is exposed. In the positive electrode 1 of FIG. 1 , the positive electrode active material layer 3 is laminated on each of both surfaces of the positive electrode substrate 2 (the upper and lower surfaces of the positive electrode substrate 2 in FIG. 1 ). However, the positive electrode active material layer 3 is not laminated entirely on both surfaces of the positive electrode substrate 2. That is, on the surfaces of the positive electrode substrate 2 where the metallic aluminum is exposed (the upper and lower surfaces of the positive electrode substrate 2 in FIG. 1 ), there are a region 4 where the positive electrode active material layer 3 is laminated and a region 5 where the positive electrode active material layer 3 is not laminated. Note that the terms "upper surface" and "lower surface" merely refer to the two main surfaces of the plate-shaped positive electrode substrate 2, respectively, and do not limit the orientation of the positive electrode 1 when in use. The region 5 where the positive electrode active material layer 3 is not laminated is the portion that will be connected to the positive electrode lead 14 in the energy storage element 10 of FIG. 2 , which will be described later.
[0040] A recess 6 is formed in a region 4 where the cathode active material layer 3 is laminated on the surface of the cathode substrate 2 where the metallic aluminum is exposed. The recess 6 is formed when cathode active material particles (not shown) contained in the cathode active material layer 3, which will be described later, sink into the cathode substrate 2. The lower limit of the area ratio of the recess 6 in the region 4 where the cathode active material layer 3 is laminated is 5%, preferably 8%, more preferably 10%, and even more preferably 12%, 15%, or 20%. When the area ratio of the recess 6 in the region 4 where the cathode active material layer 3 is laminated is equal to or greater than the above-mentioned lower limit, the contact area between the cathode active material particles and the cathode substrate 2 is increased, thereby reducing electrical resistance. The upper limit of the area ratio of the recess 6 in the region 4 where the cathode active material layer 3 is laminated may be, for example, 60%, 50%, or 40%. The area ratio of the recess 6 in the region 4 where the cathode active material layer 3 is laminated may be equal to or greater than any of the above-mentioned lower limits and equal to or less than any of the above-mentioned upper limits.
[0041] The upper limit of the area ratio of the recesses 6 in the region 5 where the positive electrode active material layer 3 is not stacked on the surface where the metallic aluminum of the positive electrode substrate 2 is exposed is preferably 0.5%, more preferably 0.1%. The lower limit of the area ratio of the recesses 6 in the region 5 where the positive electrode active material layer 3 is not stacked may be 0% or even 0.01%. As such, it is preferable that the recesses 6 are not substantially formed in the region 5 where the positive electrode active material layer 3 is not stacked. In a positive electrode 1 according to one embodiment of the present invention, a positive electrode substrate 2 in which the recesses 6 are not substantially formed in the region 5 where the positive electrode active material layer 3 is not stacked, typically a positive electrode substrate 2 that has not been subjected to a surface roughening treatment, can be used. Even when such a positive electrode substrate 2 is used, the electrical resistance is reduced. The area ratio of the recesses 6 in the region 5 where the positive electrode active material layer 3 is not stacked can be equal to or greater than any of the above-mentioned lower limits and equal to or less than any of the above-mentioned upper limits.
[0042] The positive electrode active material layer 3 contains positive electrode active material particles and a non-aqueous binder. The positive electrode active material layer 3 may also contain optional components such as a conductive agent, a thickener, and a filler, as needed.
[0043] The positive electrode active material particles are particles of a positive electrode active material. The positive electrode active material can be appropriately selected from known positive electrode active materials. As the positive electrode active material for a lithium ion secondary battery, a material capable of absorbing and releasing lithium ions is usually used. As the positive electrode active material, for example, α-NaFeO 2 Examples of suitable lithium transition metal composite oxides include those having a α-type crystal structure, those having a spinel-type crystal structure, those having a polyanion structure (hereinafter also referred to as "polyanion compounds"), chalcogen compounds, and sulfur. 2 As the lithium transition metal composite oxide having a crystalline structure, for example, Li[Li x Ni (1-x) ]O 2 (0≦x<0.5), Li[Li x Ni γ Co (1-x-γ) ]O 2(0≦x<0.5, 0<γ<1, 0<1-x-γ), Li[Li x Co (1-x) ]O 2 (0≦x<0.5), Li[Li x Ni γ Mn (1-x-γ) ]O 2 (0≦x<0.5, 0<γ<1, 0<1-x-γ), Li[Li x Ni γ Mn β Co (1-x-γ-β) ]O 2 (0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1, 0<1−x−γ−β), Li[Li x Ni γ Co β Al (1-x-γ-β) ]O 2 (0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1, 0<1−x−γ−β), etc. Examples of lithium transition metal composite oxides having a spinel crystal structure include Li x Mn 2 O 4 , Li x Ni γ Mn (2-γ) O 4 Examples of chalcogen compounds include titanium disulfide, molybdenum disulfide, and molybdenum dioxide. Polyanion compounds will be described in detail later. Atoms or polyanions in these materials may be partially substituted with atoms or anion species of other elements. The surfaces of these materials may be coated with other materials. In the positive electrode active material layer 3, one of these materials may be used alone, or two or more may be used in combination.
[0044] Among the positive electrode active materials, polyanion compounds are preferred. That is, the positive electrode active material particles preferably contain a polyanion compound. Examples of the polyanion compound include oxo acid anions (PO 4 3- , S.O. 4 2- , SiO 4 4- , B.O. 3 3- , V.O. 4 3-The oxo acid anion may be a compound containing a condensed anion (P 2 O 7 4- , P 3 O 10 5- The polyanion compound may have an olivine-type crystal structure. The polyanion compound is typically a polyanion compound containing a lithium element and a transition metal element, and may further contain other elements (e.g., halogen elements, etc.). The transition metal element contained in the polyanion compound is preferably an iron element, a manganese element, a nickel element, or a cobalt element, and more preferably an iron element. The oxo acid anion contained in the polyanion compound may be a phosphate anion (PO 4 3- ) is preferred.
[0045] The polyanion compound is preferably a compound represented by the following formula (1): Li a M b (A.O. c ) d X e ... (1) In formula (1), M is at least one transition metal element. A is at least one selected from B, Al, Si, P, S, Cl, Ti, V, Cr, Mo, and W. X is at least one halogen element. a, b, c, d, and e are numbers satisfying 0<a≦3, 0<b≦2, 2≦c≦4, 1≦d≦3, and 0≦e≦1. a, b, c, d, and e may all be integers or decimals.
[0046] As M in formula (1), any one of Fe, Mn, Ni, and Co, or a combination of any two or more of these, is preferable. As M, Fe, Mn, or a combination thereof is more preferable, and Fe is more preferable. Furthermore, the content of Fe in M is preferably 50 mol% or more, more preferably 70 mol% or more, 90 mol% or more, or 99 mol% or more. As A, P is preferable. As X, F is preferable. In one embodiment, a = 1, b = 1, c = 4, d = 1, and e = 0 may be preferable.
[0047] Specific examples of polyanion compounds include LiFePO 4 , LiCoPO 4 , LiFe 0.5 Co 0.5 P.O. 4 , LiMnPO 4 , LiNiPO 4 , LiMn 0.5 Fe 0.5 P.O. 4 , LiCrPO 4 , LiFeVO 4 , Li 2 FeSiO 4 , Li 2 Fe 2 (SO 4 ) 3 , LiFeBO 3 , LiFePO 3.9 F 0.2 , Li 3 V 2 (P.O. 4 ) 3 , Li 2 MnSiO 4 , Li 2 CoPO 4 F. Atoms or polyanions in these polyanion compounds may be partially substituted with other atoms or anion species. The polyanion compounds may be used singly or in combination of two or more.
[0048] The lower limit of the content of the polyanion compound in the positive electrode active material particles may be 60 mass%, 80 mass%, 90 mass%, 95 mass%, or 99 mass%, and the upper limit of the content of the polyanion compound in the positive electrode active material particles may be 100 mass% or 99.9 mass%.
[0049] At least a portion of the surface of the positive electrode active material particles containing a polyanion compound may be coated with a carbon material. When at least a portion of the surface of the positive electrode active material particles is coated with a carbon material, electronic conductivity between the positive electrode active material particles and between the positive electrode active material particles and the positive electrode substrate 2 can be improved. The carbon material is, for example, a material having a carbon element content of 80% by mass or more and 100% by mass or less. The carbon element content in the carbon material may be 90% by mass or more, or even 95% by mass. Elements other than carbon that may be contained in the carbon material include oxygen, hydrogen, and nitrogen. Examples of carbon materials include graphite and non-graphitic carbon. The carbon material content in the positive electrode active material particles may be, for example, 0.1% by mass or more and 20% by mass or less, 0.2% by mass or more and 10% by mass or less, or 0.3% by mass or more and 5% by mass or less.
[0050] The positive electrode active material particles may be single particles in which a plurality of primary particles are not aggregated, but are preferably secondary particles formed by aggregation of a plurality of primary particles. As the positive electrode active material particles, secondary particles of a polyanion compound are preferably used.
[0051] The lower limit of the breaking strength of the positive electrode active material particles is 30 MPa, preferably 40 MPa, and more preferably 50 MPa. When the breaking strength of the positive electrode active material particles is equal to or greater than the lower limit, the positive electrode active material particles can be sufficiently embedded into the positive electrode substrate 2 by pressing or the like during the positive electrode manufacturing process, thereby reducing the electrical resistance. When the breaking strength of the positive electrode active material particles is less than the lower limit, the positive electrode active material particles are likely to crack or deform during pressing or the like, and the positive electrode active material particles do not sufficiently embed into the positive electrode substrate 2, thereby not sufficiently reducing the electrical resistance. The upper limit of the breaking strength of the positive electrode active material particles may be, for example, 200 MPa, or may be 150 MPa, 100 MPa, or 80 MPa. The breaking strength of the positive electrode active material particles can be equal to or greater than any of the above-mentioned lower limits and equal to or less than any of the above-mentioned upper limits. The breaking strength of the positive electrode active material particles can be controlled by the types of positive electrode active material and the carbon material coating the surface, as well as by manufacturing conditions such as the method for producing the positive electrode active material (hydrothermal method, solid-phase method, etc.), firing conditions, and conditions for the method for forming the positive electrode active material particles (spray-drying method, etc.). Positive electrode active material particles having a breaking strength within the above range can be selected and used from commercially available known positive electrode active material particles after measuring their breaking strength.
[0052] The lower limit of the average particle size of the positive electrode active material particles is 3 μm, preferably 4 μm, and more preferably 5 μm. When the average particle size of the positive electrode active material particles is equal to or greater than the above lower limit, the positive electrode active material particles can be sufficiently embedded into the positive electrode substrate 2 by pressing or the like during the positive electrode manufacturing process, thereby reducing electrical resistance. On the other hand, the upper limit of the average particle size of the positive electrode active material particles is preferably 30 μm, more preferably 20 μm, even more preferably 15 μm, and even more preferably 10 μm. When the average particle size of the positive electrode active material particles is equal to or less than the above upper limit, pressability is improved and a high-density positive electrode active material layer 3 can be formed, thereby increasing the energy density per volume of the positive electrode 1 and the energy storage device including this positive electrode 1. Furthermore, when the average particle size of the positive electrode active material particles is equal to or less than the above upper limit, the number of contact points between the positive electrode active material particles and between the positive electrode active material and the positive electrode substrate 2 increases, thereby further reducing electrical resistance. The average particle size of the positive electrode active material particles can be equal to or greater than any of the above lower limits and equal to or less than any of the above upper limits. To obtain positive electrode active material particles with a predetermined average particle size, a pulverizer, a classifier, or the like is used. Examples of pulverization methods include methods using a mortar, a ball mill, a sand mill, a vibration ball mill, a planetary ball mill, a jet mill, a counter jet mill, a swirling airflow jet mill, or a sieve. Wet pulverization in the presence of water or an organic solvent such as hexane can also be used. As a classification method, a sieve, an air classifier, or the like is used as needed for both dry and wet methods.
[0053] The content of the positive electrode active material particles in the positive electrode active material layer 3 is preferably 70% by mass or more and 99% by mass or less, more preferably 80% by mass or more and 98% by mass or less, even more preferably 85% by mass or more and 97% by mass or less, and even more preferably 90% by mass or more and 95% by mass or less. By setting the content of the positive electrode active material particles within the above range, both a high energy density and manufacturability of the positive electrode active material layer 3 can be achieved.
[0054] The non-aqueous binder refers to a binder that can be dissolved or dispersed in a non-aqueous solvent when preparing a positive electrode mixture paste. Examples of non-aqueous binders include polyvinylidene fluoride (PVDF), a copolymer of vinylidene fluoride and hexafluoropropylene, a copolymer of ethylene and vinyl alcohol, polyacrylonitrile, polyphosphazene, polysiloxane, polyvinyl acetate, polymethyl methacrylate, polystyrene, polycarbonate, polyamide, polyimide, polyamideimide, a crosslinked polymer of cellulose and chitosan pyrrolidone carboxylate, a chitin or chitosan derivative, and the like. Examples of non-aqueous solvents include N-methylpyrrolidone (NMP).
[0055] The content of the non-aqueous binder in the positive electrode active material layer 3 is preferably 1% by mass to 10% by mass, and more preferably 3% by mass to 6% by mass. By setting the content of the non-aqueous binder within the above range, the positive electrode active material particles can be stably held.
[0056] The conductive agent is not particularly limited as long as it is a material having electrical conductivity. Examples of such conductive agents include carbon materials, metals, conductive ceramics, etc. Examples of carbon materials include graphite, non-graphitic carbon, graphene-based carbon, etc. Examples of non-graphitic carbon include carbon nanofiber, pitch-based carbon fiber, carbon black, etc. Examples of carbon black include furnace black, acetylene black, ketjen black, etc. Examples of graphene-based carbon include graphene, carbon nanotubes (CNT), fullerene, etc. The conductive agent may be in the form of powder, fiber, etc. As the conductive agent, one of these materials may be used alone, or two or more may be mixed and used. These materials may also be used in combination. For example, a composite material of carbon black and CNT may be used. Among these, carbon black is preferred from the viewpoints of electronic conductivity and coatability, and acetylene black is particularly preferred.
[0057] The lower limit of the content of the conductive agent in the positive electrode active material layer 3 is preferably 0.5 mass%, more preferably 1 mass%, even more preferably 2 mass%, even more preferably 3 mass%, and even more preferably 4 mass% in some cases. When the content of the conductive agent in the positive electrode active material layer 3 is equal to or greater than the above-mentioned lower limit, the electrical resistance of the positive electrode 1 is further reduced. On the other hand, the upper limit of the content of the conductive agent in the positive electrode active material layer 3 is preferably 10 mass%, more preferably 9 mass%, even more preferably 8 mass%, and even more preferably 7 mass%, 6 mass%, or 5 mass% in some cases. When the content of the conductive agent in the positive electrode active material layer 3 is equal to or less than the above-mentioned upper limit, the content of the positive electrode active material particles can be increased, and the energy density of the energy storage device can be increased. The content of the conductive agent in the positive electrode active material layer 3 can be equal to or greater than any of the above-mentioned lower limits and equal to or less than any of the above-mentioned upper limits. When the positive electrode active material layer 3 contains positive electrode active material particles at least part of the surface of which is coated with a carbon material, the carbon material coating the positive electrode active material particles is not included in the conductive agent.
[0058] The thickener is not particularly limited, and can be one that has the function of adjusting the viscosity of the positive electrode mixture paste containing positive electrode active material particles and a non-aqueous binder to a level suitable for coating by being added to the positive electrode mixture paste. When a thickener is used, the content of the thickener in the positive electrode active material layer 3 can be, for example, 0.1% by mass or more and 8% by mass or less, and can also be 5% by mass or less, or 1% by mass or less. The technology disclosed herein can be preferably implemented in an embodiment in which the positive electrode active material layer 3 does not contain a thickener.
[0059] The filler is not particularly limited. Examples of fillers include polyolefins such as polypropylene and polyethylene; inorganic oxides such as silicon dioxide, alumina, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicates; hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide; carbonates such as calcium carbonate; sparingly soluble ionic crystals such as calcium fluoride, barium fluoride, and barium sulfate; nitrides such as aluminum nitride and silicon nitride; mineral-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica; and artificial products thereof. When a filler is used, the content of the filler in the positive electrode active material layer 3 can be, for example, 0.1% by mass or more and 8% by mass or less, and can also be 5% by mass or less, or 1% by mass or less. The technology disclosed herein can be preferably implemented in an embodiment in which the positive electrode active material layer 3 does not contain a filler.
[0060] The positive electrode active material layer 3 may contain typical non-metallic elements such as B, N, P, F, Cl, Br, and I; typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba; and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material particles, conductive agent, non-aqueous binder, thickener, and filler.
[0061] The lower limit of the density of the positive electrode active material layer 3 is 1.5 g / cm 3 is preferred, and 1.6 g / cm 3 More preferably, 1.7 g / cm 3 is more preferably 1.8 g / cm 3 , 1.9 g / cm 3 , 2.0 g / cm 3 or 2.1 g / cm 3 When the density of the positive electrode active material layer 3 is equal to or higher than the lower limit, the electrical resistance can be further reduced, and the discharge capacity per volume of the positive electrode active material layer 3 can be increased. The upper limit of the density of the positive electrode active material layer 3 is 2.6 g / cm 3 is preferred, and 2.5 g / cm 3, 2.4 g / cm 3 or 2.3 g / cm 3 is more preferable. When the density of the positive electrode active material layer 3 is equal to or less than the above upper limit, the electrolyte can easily impregnate the positive electrode active material layer 3, and cracks in the positive electrode active material layer 3 are less likely to occur. The density of the positive electrode active material layer 3 can be equal to or greater than any of the above lower limits and equal to or less than any of the above upper limits. The density of the positive electrode active material layer 3 can be adjusted by the average particle size of the positive electrode active material particles, the strength of the press in the manufacturing process of the positive electrode, etc.
[0062] The mass per area of one layer of the positive electrode active material layer 3 is 0.5 mg / 100 cm 2 More than 3.0 mg / 100 cm 2 Preferably, 0.7 mg / 100 cm or less 2 More than 2.0 mg / 100 cm 2 The following is more preferable. When the mass per area of one layer of the positive electrode active material layer 3 is within the above range, it is possible to increase the discharge capacity of the energy storage device, etc. Note that the mass per area of one layer of the positive electrode active material layer 3 refers to the mass per area of one positive electrode active material layer 3 provided on one surface of the positive electrode substrate 2 when the positive electrode active material layers 3 are provided on both surfaces of the positive electrode substrate 2, as in the positive electrode 1 in FIG. 1 .
[0063] <Method for Manufacturing Positive Electrode> A positive electrode can be manufactured, for example, by applying a positive electrode mixture paste to a positive electrode substrate having a surface on which metallic aluminum is exposed, drying the paste, and then laminating a positive electrode active material layer on the positive electrode substrate, followed by pressing or the like. The positive electrode mixture paste includes, for example, each component constituting the positive electrode active material layer and a dispersion medium. By pressing, at least a portion of the positive electrode active material particles in the positive electrode active material layer sinks into the positive electrode substrate, forming recesses on the surface (the surface on which metallic aluminum is exposed) of the positive electrode substrate. In addition, the proportion of the area of the recesses in the region on the surface of the positive electrode substrate where the positive electrode active material layer is laminated can be adjusted by the type and average thickness of the positive electrode substrate, the type and breaking strength of the positive electrode active material particles, the average particle size, the strength of the press, and the like.
[0064] <Electricity storage element> An electric storage element according to one embodiment of the present invention includes an electrode assembly having a positive electrode, a negative electrode, and a separator, an electrolyte, and a container that accommodates the electrode assembly and the electrolyte. The electrode assembly is typically a stacked type in which a plurality of positive electrodes and a plurality of negative electrodes are stacked with separators interposed therebetween, or a wound type in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween and wound. The electrolyte is present in a state contained in the positive electrode, the negative electrode, and the separator. The electrolyte may be a nonaqueous electrolyte. As an example of an electric storage element, a nonaqueous electrolyte secondary battery (hereinafter also simply referred to as a "secondary battery") in which the electrolyte is a nonaqueous electrolyte will be described.
[0065] (Positive Electrode) The positive electrode provided in the electricity storage element can be the same as the positive electrode (positive electrode for electricity storage element) according to one embodiment of the present invention.
[0066] (Negative Electrode) The negative electrode has a negative electrode substrate and a negative electrode active material layer disposed on the negative electrode substrate directly or via an intermediate layer.
[0067] The negative electrode substrate is conductive. Metals such as copper, nickel, stainless steel, nickel-plated steel, and aluminum, or alloys thereof, carbon materials, and the like are used as the material for the negative electrode substrate. Among these, copper or copper alloys are preferred. Examples of the negative electrode substrate include foil, vapor-deposited film, mesh, and porous material, with foil being preferred from the viewpoint of cost. Therefore, copper foil or copper alloy foil is preferred as the negative electrode substrate. Examples of copper foil include rolled copper foil and electrolytic copper foil.
[0068] The average thickness of the negative electrode substrate is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, even more preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate within the above range, it is possible to increase the strength of the negative electrode substrate and also increase the energy density per volume of the energy storage element.
[0069] The intermediate layer is a layer disposed between the negative electrode substrate and the negative electrode active material layer. The intermediate layer contains a conductive agent such as carbon particles to reduce the contact resistance between the negative electrode substrate and the negative electrode active material layer. The configuration of the intermediate layer is not particularly limited, and may contain, for example, a binder and a conductive agent.
[0070] The negative electrode active material layer contains a negative electrode active material. The negative electrode active material layer contains optional components such as a conductive agent, a binder, a thickener, and a filler, as needed. The optional components such as the conductive agent and the filler can be selected from the materials exemplified for the positive electrode above.
[0071] The negative electrode active material layer may contain typical non-metallic elements such as B, N, P, F, Cl, Br, and I; typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba; and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than the negative electrode active material, conductive agent, binder, thickener, and filler.
[0072] The negative electrode active material can be appropriately selected from known negative electrode active materials. A material capable of absorbing and releasing lithium ions is usually used as the negative electrode active material for a lithium ion secondary battery. Examples of the negative electrode active material include metal Li; metals or semimetals such as Si and Sn; metal oxides or semimetal oxides such as Si oxide, Ti oxide, and Sn oxide; Li 4 Ti 5 O 12 , LiTiO 2、 TiNb 2 O 7 Examples of the material include titanium-containing oxides such as titanium dioxide, polyphosphate compounds, silicon carbide, and carbon materials such as graphite and non-graphitic carbon (easily graphitizable carbon or non-graphitizable carbon). Among these materials, graphite and non-graphitic carbon are preferred. In the negative electrode active material layer, one of these materials may be used alone, or two or more may be used in combination.
[0073] "Graphite" refers to a graphite material that has an average lattice spacing (d 002 ) is 0.33 nm or more and less than 0.34 nm. Examples of graphite include natural graphite and artificial graphite. Artificial graphite is preferred from the viewpoint of being able to obtain a material with stable physical properties.
[0074] "Non-graphitic carbon" refers to a carbon having an average lattice spacing (d 002) is 0.34 nm or more and 0.42 nm or less. Examples of non-graphitizable carbon include non-graphitizable carbon and graphitizable carbon. Examples of non-graphitizable carbon include resin-derived materials, petroleum pitch or petroleum pitch-derived materials, petroleum coke or petroleum coke-derived materials, plant-derived materials, and alcohol-derived materials.
[0075] Here, the "discharged state" refers to a state in which the battery is discharged so that lithium ions capable of being absorbed and desorbed during charging and discharging are sufficiently released from the carbon material serving as the negative electrode active material. For example, this refers to a state in which the open circuit voltage of a half cell using a negative electrode containing a carbon material as the negative electrode active material as the working electrode and metallic Li as the counter electrode is 0.7 V or higher.
[0076] "Non-graphitizable carbon" refers to the above-mentioned d 002 The term "carbon material" refers to a carbon material having a particle size of 0.36 nm or more and 0.42 nm or less.
[0077] "Graphitizable carbon" refers to the above-mentioned d 002 The term "carbon material" refers to a carbon material having a particle size of 0.34 nm or more and less than 0.36 nm.
[0078] The negative electrode active material is usually in the form of particles (powder). The average particle size of the negative electrode active material can be, for example, 1 nm or more and 100 μm or less. When the negative electrode active material is a carbon material, a titanium-containing oxide, or a polyphosphate compound, the average particle size may be 1 μm or more and 100 μm or less. When the negative electrode active material is Si, Sn, Si oxide, Sn oxide, or the like, the average particle size may be 1 nm or more and 1 μm or less. By setting the average particle size of the negative electrode active material to be equal to or greater than the above lower limit, the production or handling of the negative electrode active material becomes easy. By setting the average particle size of the negative electrode active material to be equal to or less than the above upper limit, the electronic conductivity of the negative electrode active material layer is improved. A pulverizer, a classifier, or the like is used to obtain powder with a predetermined particle size. When the negative electrode active material is a metal such as metallic Li, the negative electrode active material layer may be in the form of a foil.
[0079] The content of the negative electrode active material in the negative electrode active material layer is preferably 60% by mass to 99% by mass, more preferably 90% by mass to 98% by mass. By setting the content of the negative electrode active material within this range, both high energy density and manufacturability of the negative electrode active material layer can be achieved.
[0080] Examples of the binder in the negative electrode active material layer include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic, and polyimide; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber; and polysaccharide polymers.
[0081] When the negative electrode active material layer contains a binder, the content of the binder in the negative electrode active material layer is preferably 0.1% by mass to 10% by mass, more preferably 1% by mass to 6% by mass.
[0082] Examples of the thickener in the negative electrode active material layer include polysaccharide polymers such as carboxymethyl cellulose (CMC), methyl cellulose, etc. When the thickener has a functional group that reacts with lithium or the like, the functional group may be deactivated in advance by methylation or the like.
[0083] When the negative electrode active material layer contains a thickener, the content of the thickener in the negative electrode active material layer is preferably 0.1% by mass to 10% by mass, more preferably 0.5% by mass to 6% by mass, and the content of the thickener in the positive electrode active material layer may be 4% by mass or less, or may be 2% by mass or less.
[0084] (Separator) The separator can be appropriately selected from known separators. Examples of separators that can be used include separators consisting of only a substrate layer and separators in which a heat-resistant layer containing heat-resistant particles and a binder is formed on one or both surfaces of the substrate layer. Examples of the shape of the substrate layer of the separator include woven fabric, nonwoven fabric, and porous resin film. Among these shapes, porous resin films are preferred from the viewpoint of strength, and nonwoven fabrics are preferred from the viewpoint of non-aqueous electrolyte retention. Materials for the substrate layer of the separator are preferably polyolefins such as polyethylene and polypropylene from the viewpoint of shutdown function, and polyimide and aramid from the viewpoint of oxidative decomposition resistance. A composite material of these resins may also be used for the substrate layer of the separator.
[0085] The heat-resistant particles contained in the heat-resistant layer preferably exhibit a mass loss of 5% or less when heated from room temperature to 500°C under an air atmosphere at 1 atmosphere, and more preferably exhibit a mass loss of 5% or less when heated from room temperature to 800°C. Examples of materials exhibiting a mass loss of a predetermined value or less include inorganic compounds. Examples of inorganic compounds include oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicate; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; sparingly soluble ionic crystals such as calcium fluoride, barium fluoride, and barium titanate; covalently bonded crystals such as silicon and diamond; mineral-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, as well as artificial products thereof. As the inorganic compound, these substances may be used alone or in the form of a complex, or two or more of them may be used in combination. Among these inorganic compounds, silicon oxide, aluminum oxide, or aluminosilicate is preferred from the viewpoint of the safety of the energy storage device.
[0086] The porosity of the separator is preferably 80% by volume or less from the viewpoint of strength, and is preferably 20% by volume or more from the viewpoint of discharge performance. Here, "porosity" refers to a volume-based value measured with a mercury porosimeter.
[0087] The separator may be a polymer gel composed of a polymer and a non-aqueous electrolyte. Examples of polymers include polyacrylonitrile, polyethylene oxide, polypropylene oxide, polymethyl methacrylate, polyvinyl acetate, polyvinylpyrrolidone, and polyvinylidene fluoride. The use of a polymer gel has the effect of suppressing leakage. The separator may be a combination of the porous resin film or nonwoven fabric described above and a polymer gel.
[0088] (Non-aqueous electrolyte) The non-aqueous electrolyte can be appropriately selected from known non-aqueous electrolytes. The non-aqueous electrolyte may be a non-aqueous electrolyte solution. The non-aqueous electrolyte solution contains a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent.
[0089] The non-aqueous solvent can be appropriately selected from known non-aqueous solvents. Examples of non-aqueous solvents include cyclic carbonates, chain carbonates, carboxylic acid esters, phosphate esters, sulfonic acid esters, ethers, amides, and nitriles. Non-aqueous solvents in which some of the hydrogen atoms contained in these compounds have been substituted with halogens may also be used.
[0090] Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), vinylethylene carbonate (VEC), chloroethylene carbonate, fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), styrene carbonate, 1-phenylvinylene carbonate, 1,2-diphenylvinylene carbonate, etc. Of these, EC is preferred.
[0091] Examples of the chain carbonate include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diphenyl carbonate, trifluoroethyl methyl carbonate, bis(trifluoroethyl) carbonate, etc. Among these, DEC and EMC are preferred.
[0092] It is preferable to use a cyclic carbonate or a chain carbonate as the non-aqueous solvent, and it is more preferable to use a cyclic carbonate and a chain carbonate in combination. The use of a cyclic carbonate can promote dissociation of the electrolyte salt and improve the ionic conductivity of the non-aqueous electrolyte. The use of a chain carbonate can reduce the viscosity of the non-aqueous electrolyte. When a cyclic carbonate and a chain carbonate are used in combination, the volume ratio of the cyclic carbonate to the chain carbonate (cyclic carbonate:chain carbonate) is preferably in the range of, for example, 5:95 to 50:50.
[0093] The electrolyte salt can be appropriately selected from known electrolyte salts, such as lithium salts, sodium salts, potassium salts, magnesium salts, and onium salts. Of these, lithium salts are preferred.
[0094] The lithium salt is LiPF 6 , LiPO 2 F 2 , LiBF 4 , LiClO 4 , LiN(SO 2 F) 2 inorganic lithium salts such as lithium oxalate salts, lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP); 3 CF 3 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 C 2 F 5 ) 2 , LiN(SO 2 CF 3 ) (SO 2 C 4 F 9 ), LiC(SO 2 CF 3 ) 3 , LiC(SO 2 C 2 F 5 ) 3 Among these, inorganic lithium salts are preferred, and LiPF 6 is more preferred.
[0095] The content of the electrolyte salt in the non-aqueous electrolyte solution is 0.1 mol / dm at 20°C and 1 atmosphere. 3 2.5mol / dm or more 3 It is preferably 0.3 mol / dm or less. 3 2.0mol / dm or more 3 It is more preferable that it is 0.5 mol / dm or less. 3 More than 1.7mol / dm 3It is more preferable that it is 0.7 mol / dm or less. 3 1.5mol / dm or more 3 By setting the content of the electrolyte salt within the above range, the ionic conductivity of the non-aqueous electrolyte can be increased.
[0096] The nonaqueous electrolyte may contain additives in addition to the nonaqueous solvent and the electrolyte salt, such as halogenated carbonates such as fluoroethylene carbonate (FEC) and difluoroethylene carbonate (DFEC), unsaturated cyclic carbonates such as vinylene carbonate (VC), methylvinylene carbonate, and ethylvinylene carbonate, oxalates such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP), and lithium bis(fluorosulfonyl)imide. imide salts such as (LiFSI); aromatic compounds such as biphenyl, alkylbiphenyl, terphenyl, partially hydrogenated terphenyl, cyclohexylbenzene, t-butylbenzene, t-amylbenzene, diphenyl ether, and dibenzofuran; partial halides of the above aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, and 3,5-difluoroanisole. Halogenated anisole compounds; succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, cyclohexanedicarboxylic anhydride; ethylene sulfite, propylene sulfite, dimethyl sulfite, methyl methanesulfonate, busulfan, methyl toluenesulfonate, dimethyl sulfate, ethylene sulfate, sulfolane, dimethyl sulfone, diethyl sulfone, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2-diisopropyl methyl ether) 4-methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, 4-methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, thioanisole, diphenyl disulfide, dipyridinium disulfide, 1,3-propene sultone, 1,3-propane sultone, 1,4-butane sultone, 1,4-butene sultone, perfluorooctane, tristrimethylsilyl borate, tristrimethylsilyl phosphate, tetrakistrimethylsilyl titanate, lithium monofluorophosphate, and lithium difluorophosphate.These additives may be used alone or in combination of two or more.
[0097] The content of the additive contained in the non-aqueous electrolyte is preferably 0.01% by mass to 10% by mass, more preferably 0.1% by mass to 7% by mass, even more preferably 0.2% by mass to 5% by mass, and particularly preferably 0.3% by mass to 3% by mass, based on the total mass of the non-aqueous electrolyte. By setting the content of the additive within the above range, it is possible to improve the capacity retention performance or cycle performance after high-temperature storage, and further improve safety.
[0098] The non-aqueous electrolyte may be a solid electrolyte, or a non-aqueous electrolytic solution and a solid electrolyte may be used in combination.
[0099] The solid electrolyte can be selected from any material that has ionic conductivity of lithium, sodium, calcium, etc. and is solid at room temperature (e.g., 15° C. to 25° C.) Examples of the solid electrolyte include sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and polymer solid electrolytes.
[0100] As the sulfide solid electrolyte, in the case of a lithium ion secondary battery, for example, Li 2 S-P 2 S 5 , LiI-Li 2 S-P 2 S 5 , Li 10 Ge-P 2 S 12 etc.
[0101] The shape of the energy storage element of this embodiment is not particularly limited, and examples thereof include a cylindrical battery, a prismatic battery, a flat battery, a coin battery, and a button battery.
[0102] Figure 2 shows an energy storage element 10 as an example of a prismatic battery. Note that this figure is a see-through view of the inside of the container. An electrode assembly 11 having a positive electrode and a negative electrode wound with a separator sandwiched between them is housed in a prismatic container 12. The positive electrode is electrically connected to a positive electrode terminal 13 via a positive electrode lead 14. The negative electrode is electrically connected to a negative electrode terminal 15 via a negative electrode lead 16.
[0103] <Electricity Storage Device> The energy storage element of the present embodiment can be mounted as an energy storage unit (battery module) configured by assembling a plurality of energy storage elements in an automobile power source such as an electric vehicle (EV), a hybrid electric vehicle (HEV), or a plug-in hybrid electric vehicle (PHEV), a power source for electronic devices such as a personal computer or a communication terminal, or a power source for power storage, etc. In this case, it is sufficient that the technology of the present invention is applied to at least one energy storage element included in the energy storage unit.
[0104] An energy storage device according to one embodiment of the present invention includes two or more energy storage elements, and includes one or more energy storage elements according to one embodiment of the present invention described above (hereinafter referred to as the "second embodiment"). It is sufficient that the technology according to one embodiment of the present invention is applied to at least one energy storage element included in the energy storage device according to the second embodiment, and the energy storage device may include one energy storage element according to one embodiment of the present invention described above and one or more energy storage elements not according to one embodiment of the present invention described above, or may include two or more energy storage elements according to one embodiment of the present invention described above.
[0105] 3 shows an example of a power storage device 30 according to a second embodiment in which power storage units 20, each of which is a collection of two or more electrically connected power storage elements 10, are further assembled. The power storage device 30 may include a bus bar (not shown) that electrically connects two or more power storage elements 10, a bus bar (not shown) that electrically connects two or more power storage units 20, etc. The power storage units 20 or the power storage device 30 may include a status monitoring device (not shown) that monitors the status of one or more power storage elements 10.
[0106] <Method for Manufacturing Energy Storage Element> The method for manufacturing the energy storage element of this embodiment can be appropriately selected from known methods. The manufacturing method includes, for example, preparing an electrode assembly, preparing an electrolyte, and housing the electrode assembly and the electrolyte in a container. Preparing the electrode assembly includes preparing a positive electrode and a negative electrode, and forming the electrode assembly by stacking or winding the positive electrode and the negative electrode with a separator interposed therebetween.
[0107] The method for placing the electrolyte in the container can be appropriately selected from known methods. For example, when a non-aqueous electrolyte solution is used as the electrolyte, the non-aqueous electrolyte solution may be poured into the container through an inlet formed in the container, and the inlet may then be sealed.
[0108] <Other Embodiments> The positive electrode for an energy storage element, the energy storage element, and the energy storage device of the present invention are not limited to the above-described embodiments, and various modifications may be made without departing from the spirit of the present invention. For example, the configuration of one embodiment can be added to the configuration of another embodiment, and part of the configuration of one embodiment can be replaced with the configuration of another embodiment or well-known technology. Furthermore, part of the configuration of one embodiment can be deleted. Also, well-known technology can be added to the configuration of one embodiment.
[0109] In the above embodiment, the case where the energy storage element is used as a chargeable and dischargeable non-aqueous electrolyte secondary battery (e.g., a lithium ion secondary battery) has been described, but the type, shape, size, capacity, etc. of the energy storage element are arbitrary. The present invention can also be applied to various secondary batteries and capacitors such as electric double layer capacitors and lithium ion capacitors. The energy storage element of the present invention may be an energy storage element other than a non-aqueous electrolyte energy storage element.
[0110] In the above embodiment, the electrode assembly in which the positive electrode and the negative electrode are stacked with a separator interposed therebetween has been described, but the electrode assembly may not include a separator. For example, the positive electrode and the negative electrode may be in direct contact with each other in a state in which a non-conductive layer is formed on the active material layer of the positive electrode or the negative electrode.
[0111] In the above embodiment, the positive electrode has been described in which the positive electrode active material layer is laminated on both sides of the positive electrode substrate, but the positive electrode active material layer may be laminated on only one side of the positive electrode substrate. Also, the positive electrode substrate may have a shape other than a plate shape.
[0112] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0113] [Example 1] (Fabrication of Positive Electrode) As the positive electrode active material particles, LiFePO 4 having a breaking strength of 55.4 MPa and an average particle size of 5.1 μm was used. 4Secondary particles of the above were prepared. The positive electrode active material particles used in the examples and comparative examples were all selected from commonly manufactured particles. Furthermore, an aluminum foil without surface roughening treatment was prepared as the positive electrode substrate. Because this positive electrode substrate was an aluminum foil, the entire surface was an exposed surface of metallic aluminum. A positive electrode mixture paste was prepared using the above positive electrode active material particles, acetylene black (AB) as a conductive agent, polyvinylidene fluoride (PVDF) as a non-aqueous binder, and N-methylpyrrolidone (NMP) as a non-aqueous solvent as a dispersion medium. The mass ratio of the positive electrode active material particles to AB and PVDF was 90.0:5.0:5.0 in terms of solid content. This positive electrode mixture paste was applied to both sides of the aluminum foil serving as the positive electrode substrate, leaving one end region uncovered. The resulting mixture was then dried and roll-pressed to form a positive electrode active material layer, thereby obtaining the positive electrode of Example 1. The coating amount of the positive electrode mixture paste is 1.0 mg / 100 cm in terms of solid content. 2 That is, the mass per area of one layer of the positive electrode active material layer in the obtained positive electrode of Example 1 was 1.0 mg / 100 cm 2 The density of the positive electrode active material layer of the obtained positive electrode of Example 1, measured by the above method, was 2.16 g / cm 3 The area ratio of the recesses in the region where the positive electrode active material layer was laminated on the surface of the positive electrode substrate (the surface where the metallic aluminum was exposed) was 21.6%, and the area ratio of the recesses in the region where the positive electrode active material layer was not laminated was 0.1% or less. Note that in the positive electrodes of other Examples and Comparative Examples, the area ratio of the recesses in the region where the positive electrode active material layer was not laminated was also 0.1% or less.
[0114] (Preparation of Negative Electrode) A negative electrode mixture paste was prepared by mixing graphite (artificial graphite and natural graphite) (Gr) as a negative electrode active material, styrene-butadiene rubber (SBR) as a binder, carboxymethyl cellulose (CMC) as a thickener, and water as a dispersion medium. The mass ratio of graphite to SBR to CMC was 96.7:2.1:1.2 in terms of solid content. This negative electrode mixture paste was applied to both sides of copper foil as a negative electrode substrate, dried, and roll-pressed to form a negative electrode active material layer, thereby obtaining a negative electrode.
[0115] (Non-aqueous electrolyte) A 0.9 mol / dm 3 At a concentration of LiPF 6 The above was dissolved in 0.3 mass % vinylene carbonate (VC) as an additive to prepare a solution. The above solution was used as a non-aqueous electrolyte.
[0116] (Separator) A polyethylene microporous film was used as the separator.
[0117] (Assembly of Energy Storage Element) The positive electrode, negative electrode, and separator were stacked to prepare an electrode body. The obtained electrode body was placed in a container, and the non-aqueous electrolyte was then poured into the container and sealed. The assembled energy storage element was charged at a constant current of 0.2 C to 3.5 V in a temperature environment of 25°C, and then charged at a constant voltage of 3.5 V. The charge was terminated when the charge current reached 0.01 C. After a 10-minute pause, constant current discharge was performed at a discharge current of 0.2 C to 2.0 V. After the initial charge and discharge, the energy storage element of Example 1 was obtained.
[0118] [Examples 2 to 18, Comparative Examples 1 to 5] Positive electrode active material particles (in all cases, LiFePO 4 The positive electrodes and energy storage devices of Examples 2 to 18 and Comparative Examples 1 to 5 were obtained in the same manner as in Example 1, except that the positive electrode active material particles used in Comparative Example 5 were used as secondary particles, the mass ratio of the positive electrode active material particles to AB and PVDF, and the mass per area of one layer of the positive electrode active material layer were set as shown in Table 1, and the linear pressure of the roll press on the positive electrode active material layer was appropriately changed (including cases where roll press was not performed). Note that the breaking strength of the positive electrode active material particles used in Comparative Example 5 could not be measured.
[0119] For each of the obtained positive electrodes, the density of the positive electrode active material layer and the ratio of the area of the recesses in the region where the positive electrode active material layer was laminated on the surface of the positive electrode substrate (the surface where the metallic aluminum was exposed), measured by the above-mentioned method, are shown in Table 1.
[0120] [Comparative Example 6] A positive electrode of Comparative Example 6 was obtained in the same manner as in Example 14, except that an aqueous binder, styrene-butadiene rubber (SBR), a thickener, carboxymethyl cellulose (CMC), and water were used as the dispersion medium, and the mass ratios of the positive electrode active material particles, AB, SBR, and CMC were set as shown in Table 2 in terms of solid content.
[0121] [Evaluation] (Measurement of AC Resistance) For each of the energy storage elements of the examples and comparative examples, the initial AC resistance (ACR) at 1 kHz was determined in an environment of 25° C. Table 1 shows the measurement results.
[0122]
[0123]
[0124] As shown in Table 1, the energy storage devices of Examples 1 to 18, which used positive electrode active material particles having a breaking strength of 30 MPa or more and an average particle size of 3 μm or more, in which the positive electrode active material layer contained a non-aqueous binder PVDF, and in which the proportion of the area of the recesses in the region on the surface of the positive electrode substrate (the surface on which the metallic aluminum was exposed) was 5% or more, had an ACR of 1.0 Ω or less, and thus achieved reduced electrical resistance. On the other hand, the energy storage devices of Comparative Examples 1, 2, and 5, which used positive electrode active material particles having a breaking strength of 30 MPa or more and an average particle size of less than 3 μm, and the energy storage devices of Comparative Examples 3 and 4, which used positive electrode active material particles having a breaking strength of 30 MPa or more and an average particle size of 3 μm or more but in which the proportion of the area of the recesses in the region on the surface of the positive electrode substrate
[0125] As shown in Table 2, in Comparative Example 6, in which SBR, an aqueous binder, was used as the binder, the positive electrode broke during the assembly process of the energy storage element, and it was not possible to produce an energy storage element, so the ACR could not be measured. This is thought to be because aqueous binders are harder than non-aqueous binders, and the positive electrode active material particles were embedded too deeply into the positive electrode substrate, resulting in a decrease in the strength of the positive electrode substrate.
[0126] The present invention is suitably used as an electricity storage element, including a non-aqueous electrolyte secondary battery, which is used as a power source for electronic devices such as personal computers and communication terminals, automobiles, and the like.
[0127] REFERENCE SIGNS LIST 1 positive electrode 2 positive electrode substrate 3 positive electrode active material layer 4 region where positive electrode active material layer is laminated 5 region where positive electrode active material layer is not laminated 6 recess 10 energy storage element 11 electrode body 12 container 13 positive electrode terminal 14 positive electrode lead 15 negative electrode terminal 16 negative electrode lead 20 energy storage unit 30 energy storage device
Claims
1. A positive electrode for a storage element, comprising: a positive electrode substrate containing metallic aluminum and having a surface on which the metallic aluminum is exposed; and a positive electrode active material layer directly laminated on the surface on which the metallic aluminum is exposed, the positive electrode active material layer containing positive electrode active material particles, wherein the breaking strength of the positive electrode active material particles is 30 MPa or more, the average particle size of the positive electrode active material particles is 3 μm or more, the positive electrode active material layer contains a non-aqueous binder, and the area ratio of recesses in the region on the surface on which the metallic aluminum is exposed, where the positive electrode active material layer is laminated, is 5% or more.
2. The positive electrode for a storage element according to claim 1, wherein there is a region on the surface where the metallic aluminum is exposed where the positive electrode active material layer is not laminated, and the proportion of an area of recesses in the region where the positive electrode active material layer is not laminated is 0.5% or less.
3. The positive electrode for a storage element according to claim 1 or 2, wherein the positive electrode active material particles contain a lithium transition metal compound having a polyanion structure.
4. The density of the positive electrode active material layer is 1.5 g / cm 3 The positive electrode for an energy storage element according to claim 1 or 2, wherein 5. The positive electrode for a storage element according to claim 1 or 2, wherein the positive electrode active material layer further contains a conductive agent, and the content of the conductive agent in the positive electrode active material layer is 0.5 mass % or more.
6. An electric storage element comprising the positive electrode for an electric storage element according to claim 1 or 2.
7. A power storage device comprising two or more power storage elements, the power storage device comprising one or more of the power storage elements according to claim 6.
Citation Information
Patent Citations
Positive electrode for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery
WO2017195332A1
Non-aqueous electrolyte secondary battery
JP1995335199A
Electrode and lithium secondary battery using it
JP1997161769A
Manufacturing method for secondary battery and secondary battery
JP2003051313A
Electrode for lithium ion secondary battery
JP2007059387A
Cited By
Positive electrode for nonaqueous electrolyte power storage element, nonaqueous electrolyte power storage element, and power storage device
WO2026155205A1