Plated steel sheet and member for automobile

The use of a Zn-Al-Mg alloy layer with an Fe-Al interfacial layer and uneven surface topography in plated steel sheets addresses the challenges of paint adhesion and corrosion resistance, ensuring robust performance in automotive parts by preventing eutectic structure detachment and maintaining coating integrity.

WO2024247816A1PCT designated stage expired Publication Date: 2024-12-05NIPPON STEEL CORPORATION
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018655
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-05-21
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Plated steel sheets used in automotive parts face challenges in achieving both excellent paint adhesion and end-face corrosion resistance, particularly due to the hardness of Zn-Al-Mg-based hot-dip plating layers which can lead to cracking and powdering, impairing paint adhesion.

Method used

A plated steel sheet with a Zn-Al-Mg alloy layer having a specific chemical composition and structure, including an Fe-Al-based interfacial alloy layer, and a surface with uneven topography, where binary or ternary eutectic structures extend to at least half the thickness of the plating layer, enhancing paint adhesion and corrosion resistance.

Benefits of technology

The solution provides improved paint adhesion and end-face corrosion resistance by preventing eutectic structures from falling off, maintaining coating integrity even after processing, and enhancing the overall performance of plated steel sheets in automotive applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018655_05122024_PF_FP_ABST
    Figure JP2024018655_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention uses a plated steel sheet equipped with a plating layer disposed on at least part of the surface of a steel sheet, wherein: the plating layer comprises Al in the amount of 10.00-30.00%, Mg in the amount of 1.00-15.00%, and Fe in the amount of 0.01-15.00%, with the remainder being Zn and impurities; the surface of the plating layer is an uneven surface; a cross-section of the plating layer reveals that the relationship between the length Lo of the plating layer in the longitudinal direction of the cross-section in an observed region and the total length Lr of a contour line on the surface of the plating layer in the observed region satisfies the following formula (1); the plating layer includes a plurality of mass-like binary eutectic structures and / or a plurality of mass-like ternary eutectic structures; and at least some of the plurality of mass-like binary eutectic structures or the plurality of mass-like ternary eutectic structures are continuously present from the surface of the plating layer to a location equal to 1 / 2 of the average thickness of the plating layer. Formula (1): (Lr-Lo) / Lo×100≥2.0 (%)
Need to check novelty before this filing date? Find Prior Art

Description

Plated steel sheets and automotive components

[0001] This application claims priority to Japanese Patent Application No. 2023-087179, filed on May 26, 2023, the contents of which are incorporated herein by reference.

[0002] Zn-Al-Mg hot-dip plated steel sheets having a hot-dip Zn coating layer containing Al and Mg have excellent corrosion resistance. Therefore, Zn-Al-Mg hot-dip plated steel sheets are widely used as materials for structural members that require corrosion resistance, such as building materials. Recently, because Zn-Al-Mg hot-dip coatings have high corrosion resistance, the use of Zn-Al-Mg hot-dip plated steel sheets, in which high-strength steel sheets such as high-tensile steel sheets are coated with Zn-Al-Mg hot-dip coatings, for automotive components has been considered.

[0003] Patent Document 1 describes a plated steel material having a steel material and a plating layer including a Zn—Al—Mg alloy layer disposed on the surface of the steel material, wherein the Zn—Al—Mg alloy layer has a Zn phase and an Mg—Sn intermetallic compound phase is contained in the Zn phase, and the plating layer contains, in mass %, more than 65.0% Zn, more than 5.0% but less than 25.0% Al, more than 3.0% but less than 12.5% ​​Mg, 0.1% to 20.0% Sn, and impurities, and has a chemical composition that satisfies the following formulas 1 to 5: Formula 1: Bi + In < Sn Formula 2: Y + La + Ce ≦ Ca Formula 3: Si < Sn Formula 4: O ≦ Cr + Ti + Ni + Co + V + Nb + Cu + Mn < 0.25 Formula 5: O ≦ Sr + Sb + Pb + B < 0.5

[0004] Patent Document 2 discloses a plated steel material having a steel material and a plating layer including a Zn—Al—Mg alloy layer disposed on the surface of the steel material, in which the cross section of the Zn—Al—Mg alloy layer is 2 Phase area fraction is 45-75%, MgZn 2 The total area fraction of the Zn-Al-MgZn phase and the Al phase is 70% or more, and 2The area fraction of the ternary eutectic structure is 0 to 5%, and the plating layer is composed of, by mass%, Zn: more than 44.90% to less than 79.90%, Al: more than 15% to less than 35%, Mg: more than 5% to less than 20%, Ca: 0.1% to less than 3.0%, and impurities, and when element group A is Y, La, and Ce, element group B is Cr, Ti, Ni, Co, V, Nb, Cu, and Mn, element group C is Sr, Sb, and Pb, and element group D is Sn, Bi, and In, The document describes a plated steel material having a chemical composition in which the total content of elements selected from element group A is 0% to 0.5%, the total content of Ca and the elements selected from element group A is 0.1% to less than 3.0%, the total content of elements selected from element group B is 0% to 0.25%, the total content of elements selected from element group C is 0% to 0.5%, and the total content of elements selected from element group D is 0% to 20.00%.

[0005] Plated steel sheets for automobiles are required to have not only edge corrosion resistance, which is corrosion resistance at cut edges, but also paint adhesion when the plated surface is painted. However, no technology has been developed to improve the paint adhesion of a plated layer containing a Zn-Al-Mg alloy layer.

[0006] International Publication No. WO 2018 / 139619 International Publication No. WO 2018 / 139620

[0007] The present disclosure has been made in view of the above circumstances, and an object of the present disclosure is to provide a plated steel sheet and an automotive component that are excellent in paint adhesion and edge corrosion resistance.

[0008] In order to solve the above problems, the present disclosure employs the following configuration. [1] A steel sheet comprising: a steel sheet; and a plating layer disposed on at least a portion of a surface of the steel sheet, wherein the plating layer has an average chemical composition, in mass%, of Al: 10.00 to 30.00%, Mg: 1.00 to 15.00%, Sn: 0.00 to 1.00%, Si: 0.00 to 2.00%, Ca: 0.00 to 2.00%, Ni: 0.00 to 1.00%, Fe: 0.01 to 15.00%, Sb: 0.00 to 0.50%, Pb: 0.00 to 0.50%, Cu: 0.00 to 1.00%, Ti: 0.00 to 1.00%, Cr: 0.00 to 1.00%, Nb: 0.00 to 1.00%, Zr: 0.00 to 1.00%, Mn: 0.00-1.00%, Mo: 0.00-1.00%, Ag: 0.00-1.00%, Li: 0.00-1.00%, Bi: 0.00-1.00%, V: 0.00-1.00%, Co: 0.00-1.00%, In: 0.00-1.00%, W: 0.00-1.00%, P: 0.00-1.00%, La: 0.00-0.50%, Ce: 0.00-0.50%, B: 0.00-0.50%, Y: 0.00-0.50%, Sr: 0.00-0.50%, a plated steel sheet comprising: a total of 0.00 to 5.00% of Sb, Pb, Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, Li, Bi, V, Co, P, In, W, La, Ce, B, Y, and Sr, with the balance being Zn and impurities; the surface of the plated layer is uneven; in a cross section of the plated layer, a relationship between a longitudinal length Lo of the plated layer within an observation region of the cross section and a total length Lr of a contour line of the surface of the plated layer within the observation region satisfies the following formula (1); the plated layer contains one or both of a plurality of blocky binary eutectic structures and a plurality of blocky ternary eutectic structures; and at least a portion of the plurality of blocky binary eutectic structures or the plurality of blocky ternary eutectic structures is continuously present from the surface of the plated layer to a position that is half the average thickness of the plated layer.(Lr-Lo) / Lo×100≧2.0(%) ... (1) [2] The plated steel sheet according to [1], wherein the plated layer includes an Fe-Al-based interface alloy layer in contact with the steel sheet, and wherein at least a portion of the binary eutectic structure or the ternary eutectic structure exists continuously from the surface of the plated layer to the Fe-Al-based interface alloy layer. [3] The plated steel sheet according to [1], wherein the number of locations where at least a portion of the binary eutectic structure or the ternary eutectic structure exists continuously from the surface of the plated layer to a position half the average thickness of the plated layer is 1 to 15 per rectangular region on the surface of the plated layer with long sides of 500 μm and short sides of 150 μm. [4] The plated steel sheet according to [1], which satisfies the following formula (2) instead of the formula (1), wherein the number of locations at which at least a portion of a plurality of blocky binary eutectic structures or a plurality of blocky ternary eutectic structures are present continuously from the surface of the plating layer to a position half the average thickness of the plating layer is 3 to 15 locations per rectangular region on the surface of the plating layer having a long side of 500 μm and a short side of 150 μm. (Lr-Lo) / Lo×100≧6.0(%) ... (2) [5] The plated steel sheet according to [1], which satisfies the following formula (3) instead of the formula (1), wherein the number of locations at which at least a portion of a plurality of blocky binary eutectic structures or a plurality of blocky ternary eutectic structures are present continuously from the surface of the plating layer to a position half the average thickness of the plating layer is 5 to 15 locations per rectangular region on the surface of the plating layer having a long side of 500 μm and a short side of 150 μm. (Lr-Lo) / Lo×100≧8.0(%) ... (3) [6] The plated steel sheet according to any one of [1], [3], [4], and [5], wherein a location where at least a portion of the plurality of aggregated binary eutectic structures or a plurality of aggregated ternary eutectic structures exists continuously from the surface of the plated layer to a position that is half the average thickness of the plated layer is located in a recessed portion of the uneven surface of the plated layer. [7] The plated steel sheet according to [2], wherein a location where at least a portion of the plurality of aggregated binary eutectic structures or a plurality of aggregated ternary eutectic structures exists continuously from the surface of the plated layer to the Fe-Al-based interface alloy layer is located in a recessed portion of the uneven surface of the plated layer.[8] The plated steel sheet according to [1], wherein the average chemical composition of the plating layer is such that Al and Mg are Al: 10.00 to 25.00% and Mg: 4.50 to 15.00%. [9] The plated steel sheet according to [1], wherein the average chemical composition of the plating layer is such that Al and Mg are Al: 15.00 to 22.00% and Mg: 5.00 to 15.00%.

[10] The average chemical composition of the plating layer is such that Sn is 0.05 to 0.50%, and Mg is detected in the plating layer by X-ray diffraction measurement. 2The plated steel sheet according to [1], [8] or [9], which has a Sn phase.

[11] The plated steel sheet according to [1], [8] or [9], wherein the average chemical composition of the plated layer contains one or both of La and Ce, and the total amount of La and Ce is 0.05 to 0.50%.

[12] The plated steel sheet according to

[10] , wherein the average chemical composition of the plated layer contains one or both of La and Ce, and the total amount of La and Ce is 0.05 to 0.50%.

[13] A steel sheet comprising: a steel material; a plating layer disposed on at least a portion of a surface of the steel material; and a coating film disposed on a surface of the plating layer, wherein the plating layer has an average chemical composition, in mass%, of Al: 10.00 to 30.00%, Mg: 1.00 to 15.00%, Sn: 0.00 to 1.00%, Si: 0.00 to 2.00%, Ca: 0.00 to 2.00%, Ni: 0.00 to 1.00%, Fe: 0.01 to 15.00%, Sb: 0.00 to 0.50%, Pb: 0.00 to 0.50%, Cu: 0.00 to 1.00%, Ti: 0.00 to 1.00%, Cr: 0.00 to 1.00%, Nb: 0.00 to 1.00%, Zr: 0.00-1.00%, Mn: 0.00-1.00%, Mo: 0.00-1.00%, Ag: 0.00-1.00%, Li: 0.00-1.00%, Bi: 0.00-1.00%, V: 0.00-1.00%, Co: 0.00-1.00%, In: 0.00-1.00%, W: 0.00-1.00%, P: 0.00-1.00%, La: 0.00-0.50%, Ce: 0.00-0.50%, B: 0.00-0.50%, Y :0.00~0.50%, Sr:0.00~0.50%, An automotive member comprising: 0.00 to 5.00% total of Sb, Pb, Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, Li, Bi, V, Co, P, In, W, La, Ce, B, Y, and Sr, with the balance being Zn and impurities; the surface of the plating layer is uneven; in a cross section of the plating layer, the relationship between the longitudinal length Lo of the plating layer within an observation area of ​​the cross section and the total length Lr of the outline of the surface of the plating layer within the observation area satisfies the following formula (4): the plating layer contains one or both of a plurality of blocky binary eutectic structures and a plurality of blocky ternary eutectic structures; and at least a portion of the blocky binary eutectic structures or the blocky ternary eutectic structures exists continuously from the surface of the plating layer to a position half the average thickness of the plating layer. (Lr - Lo) / Lo x 100 ≥ 2.0(%) ... (4).

[0009] According to the present disclosure, it is possible to provide a plated steel sheet and an automotive component that are excellent in both edge corrosion resistance and paint adhesion.

[0010] Fig. 1 is a cross-sectional schematic diagram of a plated steel sheet according to one embodiment of the present disclosure. Fig. 2 is a schematic diagram showing an example of an observation field when a cross-section of a plating layer is observed with a scanning electron microscope. Fig. 3 is a schematic diagram showing an example of an observation field when a cross-section of a plating layer is observed with a scanning electron microscope. Fig. 4 is a schematic diagram showing an example of an observation field when a cross-section of a plating layer of a conventional plated steel material is observed with a scanning electron microscope. Fig. 5 is a flowchart of an example of a method for producing a plated steel sheet according to one embodiment of the present disclosure.

[0011] The present inventors have investigated means for improving the paint adhesion to the plating layer. The metal structure of a Zn-Al-Mg system hot-dip plating layer containing Al, Mg, and Zn contains various phases or structures. For example, in the early solidification stage, Al phase and MgZn phase are formed. 2 It is known that a binary eutectic structure or a ternary eutectic structure crystallizes in the later stage of solidification. The inventors have investigated and found that a binary eutectic structure or a ternary eutectic structure is formed by the Al phase and MgZn 2 It was found that the adhesiveness to the paint film was superior to that of the other phases.

[0012] In conventional Zn-Al-Mg hot-dip coatings, binary or ternary eutectic structures may be exposed on the surface of the coating layer. These binary or ternary eutectic structures are often distributed in the surface of the coating layer, specifically, in a range from the surface of the coating layer to a depth of ¼ to ⅓ of the average thickness of the coating layer. It has been believed that these eutectic structures exposed on the surface of the coating layer improve paint adhesion. However, when manufacturing automotive components from coated steel sheets, the coated steel sheets must be subjected to various processes to obtain automotive components of desired shapes. However, the processed coating layer may develop fine cracks on its surface due to strain during processing. It has been found that when such cracks occur around the eutectic structures exposed on the surface of the coating layer, the eutectic structures surrounded by the cracks may detach from the coating layer, resulting in so-called powdering or flaking, which may not contribute to improving paint adhesion.

[0013] In particular, since a Zn-Al-Mg-based hot-dip plating layer is harder than a conventional Zn-based plating layer, a relatively large number of cracks may occur, increasing the frequency with which the eutectic structure falls off from the plating layer, raising concerns about a decrease in paint adhesion.

[0014] It was also expected that an uneven surface of the plating layer would improve paint adhesion rather than a flat surface.

[0015] The inventors have therefore conducted research and found that, after a hot-dip coating bath is applied to a steel sheet by a hot-dip coating method, by controlling the atmosphere from the time the coating bath is removed until the start of cooling, adjusting the cooling rate during cooling, and selecting a suitable cooling gas, a binary eutectic structure or a ternary eutectic structure can be continuously present to a position deeper than the surface of the coating layer, specifically, at least to a depth of half the average thickness of the coating layer, so that even if cracks occur, the eutectic structure will not fall off from the coating layer, thereby preventing a decrease in paint adhesion. Furthermore, the inventors have found that controlling the atmosphere, adjusting the cooling rate, and selecting a suitable cooling gas can make the surface of the coating layer uneven, thereby further improving paint adhesion.

[0016] Hereinafter, a plated steel sheet and an automotive exterior material according to an embodiment of the present disclosure will be described. The plated steel sheet of this embodiment includes a steel sheet and a plating layer disposed on at least a portion of the surface of the steel sheet, and the plating layer has an average chemical composition, in mass %, of Al: 10.00 to 30.00%, Mg: 1.00 to 15.00%, Sn: 0.00 to 1.00%, Si: 0.00 to 2.00%, Ca: 0.00 to 2.00%, Ni: 0.00 to 1.00%, Fe: 0.01 to 15.00%, Sb: 0.00 to 0.50%, Pb: 0.00 to 0.50%, Cu: 0.00 to 0.50%, and Cr: 0.00 to 0.50%. : 0.00 to 1.00%, Ti: 0.00 to 1.00%, Cr: 0.00 to 1.00%, Nb: 0.00 to 1.00%, Zr: 0.00 to 1.00%, Mn: 0.00 to 1.00%, Mo: 0.00 to 1.00%, Ag : 0.00 to 1.00%, Li: 0.00 to 1.00%, Bi: 0.00 to 1.00%, V: 0.00 to 1.00%, Co: 0.00 to 1.00%, In: 0.00 to 1.00%, W: 0.00 to 1.00%, P: 0. 0.00 to 1.00%, La: 0.00 to 0.50%, Ce: 0.00 to 0.50%, B: 0.00 to 0.50%, Y: 0.00 to 0.50%, Sr: 0.00 to 0.50%, Sb, Pb, Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, Li, Bi, V, Co, P, In, W, La, Ce, B, Y, Sr total: 0.00 to 5.00%, balance: Zn and impurities, and the surface of the plating layer is an uneven surface, and in a cross section of the plating layer, The relationship between the longitudinal length Lo of the coating layer within the observation region and the total length Lr of the contour line of the surface of the coating layer within the observation region satisfies the following formula (1), and the coating layer contains one or both of a plurality of massive binary eutectic structures and a plurality of massive ternary eutectic structures, and at least a portion of the plurality of massive binary eutectic structures or a plurality of massive ternary eutectic structures exists continuously from the surface of the coating layer to a position that is half the average thickness of the coating layer: (Lr - Lo) / Lo x 100 ≥ 2.0 (%) ... (1)

[0017] Furthermore, in the plated steel sheet of the present embodiment, it is preferable that the plating layer contains an Fe-Al-based interface alloy layer in contact with the steel sheet, and that at least a portion of the plurality of massive binary eutectic structures or the plurality of massive ternary eutectic structures is continuously present from the surface of the plating layer to the Fe-Al-based interface alloy layer.

[0018] In addition, in the plated steel sheet of this embodiment, it is preferable that the recesses of the uneven surface of the plated layer are located at locations where at least a portion of a plurality of massive binary eutectic structures or a plurality of massive ternary eutectic structures exists continuously from the surface of the plated layer to a position half the average thickness of the plated layer.Furthermore, in the plated steel sheet of this embodiment, it is preferable that the recesses of the uneven surface of the plated layer are located at locations where at least a portion of a plurality of massive binary eutectic structures or a plurality of massive ternary eutectic structures exists continuously from the surface of the plated layer to the Fe-Al-based interface alloy layer.

[0019] Fig. 1 shows a schematic cross-sectional view of a plated steel sheet 1. Fig. 1 is a schematic diagram for explaining the positional relationship between a steel sheet 11 and a plating layer 12. Note that in Fig. 1, the uneven surface of the plating layer 12 is omitted from the illustration.

[0020] As shown in Fig. 1 , the plated steel sheet 1 according to this embodiment has a steel sheet 11. There are no particular limitations on the shape of the steel sheet 11. The steel sheet 11 may also be a base steel sheet that has been formed into, for example, steel pipes, civil engineering and construction materials (fences, corrugated pipes, drainage ditch covers, sand-flying prevention plates, bolts, wire mesh, guardrails, water-blocking walls, etc.), home appliance components (casings for air conditioner outdoor units, etc.), automotive components (suspension components, exterior components, interior components, structural components, etc.), etc. The forming process may be any of various plastic processing techniques, such as pressing, roll forming, and bending.

[0021] The material of the steel plate 11 is not particularly limited. The steel plate 11 can be various steel plates such as general steel, Al-killed steel, ultra-low carbon steel, high carbon steel, various high-tensile steels, and some high-alloy steels (steels containing strengthening elements such as Ni and Cr). The steel plate 11 may also be a hot-rolled steel plate, hot-rolled steel strip, cold-rolled steel plate, or cold-rolled steel strip described in JIS G 3302:2010. There are also no particular limitations on the manufacturing method of the steel plate (hot rolling method, pickling method, cold rolling method, etc.) and the specific manufacturing conditions thereof.

[0022] Furthermore, the steel sheet 11 constituting the plated steel sheet 1 according to this embodiment may be a high-tensile steel sheet for automotive components.

[0023] The plated steel sheet 1 according to this embodiment has a plating layer 12 disposed on at least a portion of the surface of a steel sheet 11. In Fig. 1 , the plating layer 12 is formed on one side of the steel sheet 11, but the plating layer 12 may be formed on both sides of the steel sheet 11. The plating layer 12 is preferably a plating film produced by a so-called hot-dip galvanizing process.

[0024] The plating layer 12 is mainly composed of a Zn—Al—Mg alloy layer due to its chemical composition, which will be described later. Furthermore, the plating layer 12 of the plated steel sheet 1 according to this embodiment may include an Fe—Al-based interfacial alloy layer, mainly composed of Fe and Al, between the steel sheet 11 and the Zn—Al—Mg alloy layer. That is, the plating layer 12 may have a single-layer structure of a Zn—Al—Mg alloy layer, or a multilayer structure including a Zn—Al—Mg alloy layer and an Fe—Al-based interfacial alloy layer.

[0025] The chemical composition of the plating layer will be described below. The "%" designation for the content of each element in the chemical composition means "mass %." The content of an element in the chemical composition may be expressed as an element concentration (e.g., Zn concentration, Mg concentration, etc.).

[0026] "Paint adhesion" refers to the property of a paint film that is resistant to peeling when a paint film is provided on the surface of a plating layer, or when a chemical conversion film and a paint film are provided on the surface of a plating layer. "Plane corrosion resistance" refers to the property of the plating layer (specifically, the Zn-Al-Mg alloy layer) itself that makes it resistant to corrosion. "Edge corrosion resistance" refers to the property of suppressing corrosion of the steel sheet at exposed parts (for example, the cut edge of a plated steel sheet).

[0027] The plating layer according to this embodiment contains Zn and other alloying elements. The chemical composition of the plating layer will be described in detail below. Note that elements whose lower limit concentration is 0.00% are not essential for solving the problems of the plated steel sheet according to this embodiment, but are optional elements that are allowed to be contained in the plating layer for the purpose of improving characteristics, etc.

[0028] <Al: 10.00 to 30.00%> Al contributes to improving planar corrosion resistance and workability. Therefore, the Al concentration is set to 10.00% or more. On the other hand, if Al is excessive, the Mg concentration and Zn concentration decrease relatively, deteriorating edge corrosion resistance. Therefore, the Al concentration is set to 30.00% or less. The Al concentration may be 10.00 to 25.00% or 15.00 to 22.00%. The Al concentration may be 11.00% or more, 13.00% or more, or 16.00% or more. The Al concentration may be 28.00% or less, 24.00% or less, or 20.00% or less.

[0029] <Mg: 1.00 to 15.00%> Mg is an essential element for ensuring flat corrosion resistance. 2 Mg is also necessary to crystallize Sn phases and the like. Therefore, the Mg concentration is set to 1.00% or more. On the other hand, if the Mg concentration is excessive, workability, particularly powdering properties, may deteriorate, and furthermore, flat corrosion resistance may deteriorate. Therefore, the Mg concentration is set to 15.00% or less. The Mg concentration may be 4.50 to 15.00% or 5.00 to 15.00%. The Mg concentration may be 2.00% or more, 3.00% or more, or 4.00% or more. The Mg concentration may be 13.00% or less, 10.00% or less, or 8.00% or less.

[0030] The elements explained below are all optional elements except for Fe and Zn, and therefore the lower limit of each is set to 0%.

[0031] <Sn: 0.00 to 1.00%> The Sn concentration may be 0%. On the other hand, Sn is an element that forms an intermetallic compound with Mg and improves the flat corrosion resistance of the plating layer. Therefore, the Sn concentration may be 0.05% or more, 0.10% or more, or 0.20% or more. However, if the Sn concentration is excessive, flat corrosion resistance will deteriorate. Therefore, the Sn concentration is set to 1.00% or less. The Sn concentration may also be 0.80% or less, 0.60% or less, 0.50% or less, 0.20% or less, or 0.06% or less.

[0032] <Si: 0.00% to 2.00%> The Si concentration may be 0.00%. On the other hand, Si contributes to improving the plane corrosion resistance. 2 Si is an element necessary for crystallizing the Si phase. Therefore, the Si concentration may be greater than 0.00%, 0.01% or more, 0.05% or more, or 0.10% or more. On the other hand, if the Si concentration is excessive, the plane corrosion resistance deteriorates. Therefore, the Si concentration is set to 2.00% or less. The Si concentration may also be set to 1.80% or less, 1.50% or less, 1.20% or less, or 1.00% or less.

[0033] <Ca: 0.00 to 2.00%> The Ca concentration may be 0%. On the other hand, Ca is an element that can adjust the amount of Mg elution that is optimal for imparting flat surface corrosion resistance. Therefore, the Ca concentration may be 0.01% or more, or 0.02% or more. On the other hand, if the Ca concentration is excessive, flat surface corrosion resistance and workability deteriorate. Therefore, the Ca concentration is set to 2.00% or less. The Ca concentration may also be set to 1.00% or less, 0.50% or less, 0.10% or less, or 0.05% or less.

[0034] <Ni: 0.00 to 1.00%> The Ni concentration may be 0.00%. On the other hand, Ni contributes to improving edge corrosion resistance. Therefore, the Ni concentration may be 0.001% or more. On the other hand, if the Ni concentration is excessive, flat surface corrosion resistance deteriorates. Therefore, the Ni concentration is set to 1.00% or less. The Ni concentration may also be 0.50% or less, 0.10% or less, or 0.01% or less.

[0035] <Fe: 0.01 to 15.00%> The Fe concentration may be 0%, but since Fe may be mixed into the coating layer from the base steel sheet, the coating layer may contain 0.01% or more. It has been confirmed that an Fe concentration of 15.00% or less does not adversely affect the performance of the coating layer. The Fe concentration may be, for example, 0.01% or more, 0.10% or more, or 0.50% or more. The Fe concentration is set to 15.00% or less. The Fe concentration may also be 10.00% or less, 5.00% or less, 2.00% or less, or 1.00% or less.

[0036] <Sb, Pb: 0.00 to 0.50% each> The concentrations of Sb and Pb may be 0.00%. On the other hand, Sb and Pb contribute to improving edge corrosion resistance. Therefore, the concentrations of Sb and Pb may be 0.01% or more, 0.03% or more, or 0.05% or more. On the other hand, excessive Sb and Pb concentrations deteriorate flat surface corrosion resistance. Therefore, the concentrations of Sb and Pb are set to 0.50% or less. The concentrations of Sb and Pb may also be 0.40% or less, 0.20% or less, or 0.10% or less.

[0037] <Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li: 0.00 to 1.00% each> The concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li may each be 0%. On the other hand, these elements contribute to improving edge corrosion resistance. Therefore, the concentrations of these elements may each be 0.01% or more. On the other hand, excessive concentrations of these elements degrade flat surface corrosion resistance. Therefore, the concentrations of these elements are each set to 1.00% or less. The concentrations of these elements may each be set to 0.50% or less, 0.10% or less, 0.05% or less, or 0.03% or less.

[0038] <Bi, V, Co, In, W: 0.00 to 1.00% each> The concentrations of Bi, V, Co, In, and W may each be 0%. On the other hand, each of these elements contributes to improving edge corrosion resistance. Therefore, the concentrations of these elements may each be 0.001% or more, or 0.01% or more. On the other hand, excessive concentrations of these elements deteriorate planar corrosion resistance. Therefore, the concentrations of Bi, V, Co, In, and W are each set to 1.00% or less. The concentrations of these elements may each be 0.50% or less, 0.10% or less, 0.02% or less, or 0.01% or less.

[0039] <P: 0.00 to 1.00%> The P concentration may be 0%. On the other hand, P contributes to improving edge corrosion resistance. Therefore, the P concentration may be 0.005% or more, or 0.01% or more. On the other hand, if the P concentration is excessive, flat surface corrosion resistance deteriorates. Therefore, the P concentration is set to 1.00% or less. The P concentration may also be 0.05% or less, 0.03% or less, or 0.01% or less.

[0040] <B, Y, and Sr: 0.00 to 0.50% each> The concentrations of B, Y, and Sr may each be 0.00%. On the other hand, B, Y, and Sr contribute to improving edge corrosion resistance. Therefore, the concentrations of these elements may each be 0.001% or more, or 0.01% or more. On the other hand, excessive concentrations of B, Y, and Sr deteriorate planar corrosion resistance. Therefore, the concentrations of these elements are each set to 0.50% or less. The concentrations of these elements may each be set to 0.10% or less, 0.02% or less, or 0.01% or less.

[0041] <La, Ce: 0.00 to 0.50% each> The concentrations of La and Ce may be 0%. On the other hand, La and Ce contribute to improving edge corrosion resistance. Therefore, the concentrations of these elements may each be 0.01% or more. On the other hand, excessive concentrations of La and Ce deteriorate plane corrosion resistance. Therefore, the concentrations of these elements are each set to 0.50% or less. The concentrations of these elements may each be set to 0.10% or less, 0.05% or less, or 0.02% or less. Furthermore, the total amount of La and Ce should be set to 0.05 to 0.50%.

[0042] <Total of Sb, Pb, Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, Li, Bi, V, Co, In, W, P, La, Ce, B, Y, Sr: 0.00 to 5.00%> The total of these elements is set to 0 to 5%. If the total exceeds 5%, flat surface corrosion resistance or edge corrosion resistance may decrease.

[0043] <Remainder: Zn and Impurities> The remainder of the components of the coating layer according to this embodiment is Zn and impurities. Zn is an element that provides the coating layer with flat corrosion resistance and edge corrosion resistance. Impurities refer to components contained in raw materials or components mixed in during the manufacturing process, but not intentionally added. For example, trace amounts of components other than Fe may be mixed into the coating layer as impurities due to mutual atomic diffusion between the base steel sheet and the coating bath.

[0044] Furthermore, in the plating layer according to this embodiment, the total content of Al, Mg, and Zn is preferably 74.00% or more, and may be 80.00% or more, 90.00% or more, 95.00% or more, or 98.00% or more.

[0045] The chemical composition of the plating layer is measured by the following method. First, an acid containing an inhibitor that suppresses corrosion of the steel sheet is used to peel and dissolve the plating layer to obtain an acid solution. Next, the obtained acid solution is subjected to ICP analysis. This allows the chemical composition of the plating layer to be obtained. There are no particular restrictions on the type of acid, as long as it is an acid that can dissolve the plating layer. Note that the chemical composition measured by the above-mentioned means is the average chemical composition of the entire plating layer.

[0046] <Surface of Plated Layer> The surface of the plated layer in this embodiment is an uneven surface. The roughness of the uneven surface is expressed by the relationship between Lo and Lr, as shown in the following formula (1). That is, (Lr - Lo) / Lo x 100 needs to be 2.0(%) or more. If (Lr - Lo) / Lo x 100 is less than 2.0(%), the roughness of the uneven surface is small and it is not possible to improve paint adhesion. (Lr - Lo) / Lo x 100 more preferably satisfies the following formula (2), and even more preferably satisfies the following formula (3). There is no particular upper limit required for (Lr - Lo) / Lo x 100, but if it is too large, the surface smoothness of the plated layer will decrease, and ultimately the surface smoothness of the paint film will also decrease. Therefore, it is preferable that it be 40(%) or less, 20(%) or less, or 12(%) or less.

[0047] (Lr-Lo) / Lo×100≧2.0(%)…(1) (Lr-Lo) / Lo×100≧6.0(%)…(2) (Lr-Lo) / Lo×100≧8.0(%)…(3)

[0048] In Equations (1) to (3), the length Lo is the longitudinal length of the plating layer within the observation area of ​​the cross section of the plating layer, and Lr is the total length of the contour of the surface of the plating layer within the observation area. The observation area is the observation field when the cross section of the plating layer is observed with a scanning electron microscope. The longitudinal length of the plating layer that fits within the observation field is Lo, and the total length of the contour of the surface of the plating layer corresponding to the longitudinal length Lo of the plating layer is Lr. When measuring Lo and Lr, it is desirable to set the observation field when observed with a scanning electron microscope so that the longitudinal length Lo of the plating layer is 500 μm. Furthermore, multiple observation fields may be combined to create an observation field where the longitudinal length Lo of the plating layer is 500 μm. The observation field is positioned at a distance of 5 mm or more from the edge of the plated steel sheet. If the plated steel sheet has a weld, the observation field is positioned at a distance of 1 mm or more from the weld bead. Furthermore, if the plated steel sheet actually has a bent portion, the observation field is positioned at a distance of 2 mm or more from the bent portion. This eliminates the effects of cutting, welding, and bending of the plated steel sheet on the surface quality of the plating layer from the measurement results. The observation field is preferably positioned on a flat area. However, plated steel sheets may not have flat areas. For example, when plated steel sheets are used as exterior components of automobiles, the plated steel sheets may have a gently curved overall shape and may not have flat areas. In this case, it is preferable to position the observation field in an area with a radius of curvature of 5 mm or more. The number of observation fields is five. First, (Lr - Lo) / Lo x 100 is calculated for each of the five observation fields, and then the arithmetic mean of these values ​​is calculated. This arithmetic mean is considered to be (Lr - Lo) / Lo x 100 of the plated steel sheet. Figure 2 shows a schematic diagram of an example of an observation field when observed with a scanning electron microscope. Figure 2 also shows the relationship between Lo and Lr. In Fig. 2, reference numeral 11 denotes a steel sheet, reference numeral 12 denotes a plating layer, and reference numeral 13 denotes an interfacial alloy layer. The double-headed arrows of reference numerals Lo and Lr schematically represent the lengths of Lo and Lr, respectively. Fig. 2 also schematically illustrates the uneven surface of the plating layer.

[0049] <Structure of the plating layer> The plating layer of this embodiment includes one or both of a plurality of massive binary eutectic structures and a plurality of massive ternary eutectic structures. The binary eutectic structure is a eutectic structure of an η-Zn phase and an Al-Zn phase, and the ternary eutectic structure is a eutectic structure of an Al phase, a Zn phase, and an MgZn phase. 2 These eutectic structures may be eutectic structures of the phases. In other words, the binary eutectic structure may have a lamellar structure in which a layered η-Zn phase and a layered Al-Zn phase are superposed. The ternary eutectic structure may have a lamellar structure in which a layered Al phase, a layered Zn phase, and a layered MgZn phase are superposed. 2 It may have a lamellar structure with overlapping phases.

[0050] In addition to these eutectic structures, the plating layer also contains massive Al phase, Al-Zn phase, Zn phase, MgZn 2 The plating layer may contain a eutectoid structure containing a lamellar Zn phase and a lamellar Al phase. This eutectoid structure has a lamellar structure, but does not fall under the category of a binary or ternary eutectic structure.

[0051] In the plating layer of this embodiment, at least a portion of a plurality of massive binary or ternary eutectic structures is present continuously from the surface of the plating layer to a position halfway through the average thickness of the plating layer. At least a portion of these massive binary or ternary eutectic structures is exposed on the surface of the plating layer. Compared to other phases such as Al phase and Al-Zn phase, the binary or ternary eutectic structure has superior adhesion to a paint film. Therefore, exposure of the binary or ternary eutectic structure on the surface of the plating layer improves the adhesion of the paint film to the entire plating layer.

[0052] Furthermore, when cracks occur in the coating layer during processing of the plated steel sheet, the cracks often propagate along the boundary between the binary or ternary eutectic structure and other phases or structures. In this embodiment, at least a portion of the binary or ternary eutectic structure exists continuously up to a position half the average thickness of the coating layer. Therefore, cracks that occur during bending tend to propagate from the surface of the coating layer toward the steel sheet and are less likely to propagate in a direction parallel to the surface of the coating layer. Therefore, even if cracks occur, the eutectic structure is less likely to fall off from the coating layer, and powdering or flaking is suppressed. As a result, the coating adhesion of the coating layer is not reduced even when the coating layer is processed.

[0053] More preferably, the plating layer of this embodiment has at least a portion of a plurality of massive binary or ternary eutectic structures present continuously from the surface of the plating layer to the Fe-Al-based interfacial alloy layer, which further suppresses the occurrence of powdering or flaking and further improves the paint adhesion of the plating layer.

[0054] Figure 3 shows an enlarged schematic diagram of an example of a plating layer of this embodiment. It shows the state of existence of a binary eutectic structure or a ternary eutectic structure. Figure 3 also shows a schematic representation of the uneven surface of the plating layer 12, as well as the state of existence of a binary eutectic structure or a ternary eutectic structure. The shaded areas in the figure represent the binary eutectic structure or the ternary eutectic structure. In Figure 3, reference numeral 11 denotes a steel sheet, reference numeral 12 denotes a plating layer, reference numeral 13 denotes an interface alloy layer, and reference numeral 14 denotes a binary eutectic structure or a ternary eutectic structure.

[0055] As shown in Figure 3, it can be seen that the binary or ternary eutectic structure 14 is continuous from the surface of the coating layer 12 toward the steel sheet 11 side. It can also be seen that the binary or ternary eutectic structure 14 exists continuously up to the Fe-Al-based interface alloy layer 13 on the steel sheet 11 side of the coating layer 12. Note that Figure 3 shows an example in which most of the binary or ternary eutectic structure 14 continues up to the Fe-Al-based interface alloy layer 13 on the steel sheet 11 side of the coating layer 12, but the present embodiment is not limited to this, and the coating layer 12 may include a binary or ternary eutectic structure 14 that continues up to a halfway position.

[0056] For reference, a cross-sectional schematic diagram of a conventional plating layer is shown in Figure 4. The conventional plating layer 112 has a flat surface, and the binary or ternary eutectic structure 114 is distributed near the interface alloy layer 113 of the plating layer 112 or near the surface of the plating layer, and no binary or ternary eutectic structure 114 is found that is continuous up to the halfway point of the plating layer 112.

[0057] Furthermore, the surface of the plating layer 12 of this embodiment is an uneven surface as exemplified in Figures 2 and 3, and the binary or ternary eutectic structure 14, which exists continuously to a depth of half the average thickness of the plating layer 12, is present in large amounts in the recesses of the uneven surface, as shown in Figure 3. This is because, as will be described later, the binary or ternary eutectic structure 14 crystallizes in the latter half of the solidification process of the plating layer. The concentration of the binary or ternary eutectic structure 14 in the recesses, combined with the geometric effect of the uneven surface, can improve paint adhesion.

[0058] In this embodiment, a binary eutectic structure or a ternary eutectic structure that exists continuously from the surface of the plating layer to the Fe—Al-based interface alloy layer may be present in large numbers in the recesses of the uneven surface.

[0059] As will be described later in the explanation of the manufacturing method, the binary or ternary eutectic structure begins to crystallize after the Al phase or Al-Zn phase has crystallized. The crystallization of these eutectic structures is thought to begin with nucleation in the region of the coating layer on the steel sheet side, more specifically, on the surface of the Fe-Al-based interface alloy layer. The crystallization of the eutectic structure is thought to progress toward the surface of the coating layer. Therefore, it is thought that most of the binary or ternary eutectic structure according to this embodiment exists continuously from the surface of the coating layer to the Fe-Al-based interface alloy layer.

[0060] However, when the internal structure of the coating layer is observed at any cross section, the entire binary or ternary eutectic structure is not always observed in a continuous form from the surface of the coating layer to the Fe-Al-based interfacial alloy layer. This is because the individual shapes of the blocky binary or ternary eutectic structures are irregular, and the form of the binary or ternary eutectic structure appears different depending on the position of the cross section.

[0061] According to the investigations conducted by the present inventors, if it is observed that at least a portion of a plurality of massive binary or ternary eutectic structures exists continuously from the surface of the plating layer to a position halfway through the average thickness of the plating layer, then it is highly likely that most of the binary or ternary eutectic structures exist in a continuous form from the surface of the plating layer to the Fe-Al-based interface alloy layer, and this is presumed to result in improved paint adhesion.

[0062] In this embodiment, the number of locations where the binary eutectic structure or ternary eutectic structure exists continuously from the surface of the plating layer to a position half the average thickness of the plating layer is preferably 1 to 15 locations per rectangular region on the surface of the plating layer with long sides of 500 μm and short sides of 150 μm. A number of locations less than 1 is not preferred because it results in insufficient paint adhesion. Furthermore, when the above formula (2) is satisfied, the number of such locations is preferably 3 to 15 locations. Furthermore, when the above formula (3) is satisfied, the number of such locations is preferably 5 to 15 locations.

[0063] The presence of a binary or ternary eutectic structure is confirmed as follows. A rectangular region with a long side of 500 μm and a short side of 150 μm is set on the surface of the plating layer. The location of this region is determined by the same means as the observation field for evaluating the roughness of the uneven surface of the plating layer, as described above. Within this region, the number and locations of binary or ternary eutectic structures exposed on the surface of the plating layer are confirmed. Next, the surface of the plating layer including this region is ground sequentially to depths of ¼, ½, ¾, and 9 / 10 of the average thickness of the plating layer, and then mirror-polished to obtain an observation surface. Then, the number and locations of binary or ternary eutectic structures on the observation surface at each of the ¼, ½, ¾, and 9 / 10 depths are confirmed. Then, the number of binary or ternary eutectic structures that appear at the same position is counted on the surface of the plating layer, at the 1 / 4 depth position, and at the 1 / 2 depth position. Whether or not a structure appears at the same position can be determined by counting the number of eutectic structures that appear at the same position if the eutectic structure is within a projection range of a radius of 15 μm from the center of gravity of the eutectic structure on the surface of the plating layer. Binary or ternary eutectic structures that appear at the same position are determined to exist continuously from the surface of the plating layer to a position half the average thickness of the plating layer. There are no particular limitations on the grinding method, but examples include precision machining such as polishing and focused ion beam machining (FIB machining).

[0064] Furthermore, it is confirmed whether a binary eutectic structure or a ternary eutectic structure appears at the same position at all of the plating layer surface, 1 / 4 depth, 1 / 2 depth, 3 / 4 depth, and 9 / 10 depth. As a result, it is determined that a binary eutectic structure or a ternary eutectic structure appearing at the same position exists continuously from the plating layer surface to the Fe-Al-based interface alloy layer.

[0065] The average thickness of the plating layer is defined as the average thickness of the plating layer in a rectangular region with long sides of 500 μm and short sides of 150 μm. The position at a height corresponding to the average thickness of the plating layer from the position of the interface between the steel sheet and the plating layer is estimated as the average surface position of the plating layer, and the ¼, ½, ¾, and 9 / 10 depths of the average thickness of the plating layer are determined based on the estimated surface position.

[0066] In addition, when the plating layer contains 0.05 to 0.5% Sn, the plating layer contains Mg 2 It is preferable that the Sn phase is contained. 2 Since the Sn phase is present in a small amount, its presence can be detected and confirmed by X-ray diffraction measurement using the θ-2θ method. 2 The inclusion of the Sn phase further improves the corrosion resistance of the edge of the plating layer. 2 X-ray diffraction measurement for detecting the Sn phase may be carried out by the θ-2θ measurement method.

[0067] The coating weight of the plating layer per side is, for example, 20 to 200 g / m 2 The amount of adhesion per side should be within the range of 20 g / m 2 By setting the coating weight per side to 200 g / m or more, the flat surface corrosion resistance and edge corrosion resistance of the plated steel sheet can be further improved. 2 By setting the following, the workability of the plated steel sheet can be further improved.

[0068] The plated steel sheet of this embodiment may have a coating formed on the plating layer. One or more coatings may be formed. Examples of the coatings that may be formed directly on the plating layer include chromate coatings, phosphate coatings, and chromate-free coatings. These coatings can be formed by known methods such as chromate treatment, phosphate treatment, and chromate-free treatment, as described below.

[0069] The plated steel sheet of the present embodiment described above is excellent in paint adhesion and edge corrosion resistance.

[0070] Furthermore, the automotive member of this embodiment is obtained by cutting the plated steel sheet of this embodiment into a predetermined planar shape by press forming or the like and processing it into a predetermined three-dimensional shape, followed by forming a paint film. That is, the automotive member of this embodiment includes a steel material, a plating layer disposed on at least a portion of the surface of the steel material, and a paint film disposed on the surface of the plating layer, wherein the average chemical composition of the plating layer is as described above, the surface of the plating layer is an uneven surface, the relationship between the longitudinal length Lo of the plating layer within an observation region of the cross section and the total length Lr of the outline of the surface of the plating layer within the observation region in the cross section satisfies the following formula (4), and the plating layer contains one or both of a plurality of massive binary eutectic structures and a plurality of massive ternary eutectic structures, and at least a portion of the plurality of massive binary eutectic structures or the plurality of massive ternary eutectic structures is continuously present from the surface of the plating layer to a position halfway through the thickness of the plating layer.

[0071] (Lr-Lo) / Lo×100≧2.0…(4)

[0072] The automotive member of this embodiment described above is excellent in paint adhesion and edge corrosion resistance.

[0073] Next, a method for manufacturing the plated steel sheet according to this embodiment will be described. The manufacturing method does not need to be limited to a specific method as long as the plated steel sheet according to this embodiment can be manufactured, but the plated steel sheet according to this embodiment can be easily obtained, for example, according to the manufacturing conditions described below.

[0074] In the method for producing a plated steel sheet according to this embodiment, a steel sheet is annealed in a reducing atmosphere, and the steel sheet immediately after annealing is immersed in a hot-dip galvanizing bath and then pulled out, thereby forming a coating layer on the surface of the steel sheet. Next, cooling is performed by spraying a cooling gas onto the steel sheet until the temperature of the coating layer drops from the bath temperature to 260°C. During this process, the oxygen concentration in the atmosphere above the surface of the coating bath and the oxygen concentration in the atmosphere from when the steel sheet is pulled out of the coating bath until cooling is completed are controlled within the range of 100 to 5000 ppm. Furthermore, the average cooling rate during the time the temperature of the coating layer drops from the bath temperature to 260°C is set to 15°C / second or higher. Furthermore, cooling is performed by spraying a cooling gas, the dew point of which is set to 0°C or higher.

[0075] That is, as shown in the flowchart of FIG. 5 , the method for producing a plated steel sheet of this embodiment includes the steps of: (S1) annealing a steel sheet in a reducing atmosphere; (S2) immersing the steel sheet in a hot-dip galvanizing bath; (S3) withdrawing the steel sheet from the hot-dip galvanizing bath; and (S4) spraying cooling gas onto the steel sheet to which the hot-dip galvanizing bath has adhered; (A) in the immersion S2 and withdrawal S3, the oxygen concentration in the atmosphere above the bath surface of the hot-dip galvanizing bath is set to a range of 100 to 5000 ppm; (B) in the spraying S4, the dew point of the cooling gas is set to 0°C or higher; (C) in the spraying S4, the average cooling rate until the temperature of the coating layer is reduced from the temperature of the hot-dip galvanizing bath to 260°C is set to 15°C / second or higher; and (D) in the spraying S4, the oxygen concentration in the atmosphere from when the steel sheet is withdrawn from the coating bath to when cooling is completed is set to a range of 100 to 5000 ppm. The plated steel sheet of this embodiment is obtained by combining all of conditions A, B, C, and D. The details of the manufacturing method will be described below in order.

[0076] (S1 Annealing) Annealing of the steel sheet to be used as the base sheet for plating is carried out in a reducing atmosphere. The reducing atmosphere and annealing conditions are not particularly limited. By this annealing, oxides present on the surface of the steel sheet are removed as much as possible.

[0077] (S2 Immersion) Next, the steel sheet immediately after annealing is immersed in a hot-dip galvanizing bath. The chemical composition of the galvanizing bath may be appropriately adjusted so as to obtain the chemical composition of the coating layer described above. The temperature of the galvanizing bath is not particularly limited, and a temperature at which hot-dip galvanizing can be performed may be appropriately selected. For example, the temperature of the galvanizing bath may be set to a value approximately 20°C or more higher than the melting point of the galvanizing bath.

[0078] (S3 Pulling Up) Next, the steel sheet is pulled up from the coating bath. The coating weight of the coating layer can be controlled by controlling the pulling speed of the steel sheet. If necessary, the coating weight of the coating layer may be controlled by wiping the steel sheet to which the coating layer has been attached. The coating weight of the coating layer is not particularly limited and can be, for example, within the range described above.

[0079] (S4 Spraying) Next, the coating layer is cooled. Cooling is performed by spraying cooling gas onto the steel sheet immediately after it has been pulled out of the hot-dip coating bath. Cooling by spraying cooling gas is performed continuously until the temperature of the steel sheet drops from the bath temperature to 260°C. The cooling conditions below 260°C are not particularly limited, and cooling by spraying cooling gas may be performed subsequently, or the steel sheet may be allowed to cool naturally.

[0080] The oxygen concentration in the atmosphere above the surface of the coating bath and the oxygen concentration in the atmosphere from when the steel sheet is pulled out of the coating bath until cooling is completed are controlled within the range of 100 to 5000 ppm. Preferably, the oxygen concentrations in these atmospheres are within the range of 100 to 1000 ppm. When the molten metal in the coating bath that has adhered to the steel sheet solidifies, an oxide film is formed on the outermost surface of the molten metal in the early stages of solidification, and the thickness of this oxide film is affected by the oxygen concentration in the atmosphere. Once the oxide film has an appropriate thickness, it begins to follow the changes in the surface shape of the coating layer during the subsequent solidification process, forming an uneven surface that satisfies the above formula (1).

[0081] If the oxygen concentration on the surface of the coating bath and in the atmosphere from the time the steel sheet is pulled out of the coating bath until the end of cooling is less than 100 ppm, an oxide film of sufficient thickness will not be formed, making it difficult to create an uneven surface for the coating layer. Furthermore, if the oxygen concentration in the atmosphere exceeds 5000 ppm, a relatively thick and flat oxide film will be formed in the early solidification stage. This oxide film will not follow the changes in the surface shape of the coating layer during the solidification process, resulting in a flat surface for the coating layer after solidification, which will not satisfy the above formula (1). Furthermore, if the oxygen concentration in the atmosphere exceeds 5000 ppm, the oxide film will be prone to cracking, which may make it difficult to maintain the shape of the coating layer during solidification. There are no particular limitations on the means for maintaining the oxygen concentration in the atmosphere above the surface of the coating bath within the range of 100 to 5000 ppm. For example, a cover may be provided to cover the surface of the coating bath, and a gas with an oxygen concentration of 100 to 5000 ppm may be supplied to the interior of the cover. The type of gas supplied to the surface of the coating bath is not particularly limited as long as the oxygen concentration is within the range of 100 to 5000 ppm, and may be a non-oxidizing gas such as nitrogen, an inert gas such as argon, or a mixture of these. In order to maintain the oxygen concentration in the atmosphere from the time the steel sheet is pulled out of the coating bath until cooling is completed within the range of 100 to 5000 ppm, for example, the oxygen concentration of the cooling gas sprayed onto the steel sheet may be set within the range of 100 to 5000 ppm. If air is used as the cooling gas, the cooling gas will have an excessive oxygen concentration, making it impossible to obtain a suitable coating layer.

[0082] Furthermore, by setting the dew point of the cooling gas to 0°C or higher, the shape-maintaining function of the oxide coating can be maintained. If the dew point of the cooling gas is below 0°C, a plating layer whose surface shape satisfies the above formula (1) cannot be obtained. There are no particular restrictions on the type of cooling gas, as long as the oxygen concentration is within the range of 100 to 5000 ppm. The cooling gas may be a non-oxidizing gas such as nitrogen, an inert gas such as argon, or a mixture of these.

[0083] The average cooling rate during the time period from the bath temperature until the temperature of the coating layer reaches 260°C is set to 15°C / second or more. There is no particular upper limit to the average cooling rate, but it may be, for example, 200°C / second or less. By setting the average cooling rate to 15°C / second or more, primary Al crystals (Al phase) and Al-Zn phases are sufficiently crystallized in the early stage of the solidification process. The average cooling rate during the time period from the bath temperature until the temperature of the coating layer reaches 260°C is a value calculated by the following formula. The cooling time is the time from when the steel sheet is pulled out of the coating bath until the temperature of the coating layer falls to 260°C. Average cooling rate = (bath temperature - 260) ÷ cooling time

[0084] As primary Al crystals (Al phase) and Al-Zn phases are fully crystallized in the early stages of the solidification process, the amount of molten metal on the steel sheet surface decreases. Then, as the temperature of the molten metal decreases, the crystallization of binary and ternary eutectic structures begins, forming such structures as to fill the periphery of the already crystallized Al phase and Al-Zn phase. Because the crystallization of the eutectic structure begins when the remaining amount of molten metal is low, the binary and ternary eutectic structures form recesses in the coating layer. Furthermore, the crystallization of the eutectic structure primarily begins in the region of the coating layer closer to the steel sheet. More specifically, crystallization begins from nucleation on the surface of the Fe-Al interfacial alloy layer and progresses toward the surface of the coating layer. As a result, the binary and ternary eutectic structures are continuously present from the steel sheet side of the coating layer toward the surface.

[0085] After the plating layer is formed, various chemical conversion treatments and painting treatments may be carried out.

[0086] In the hot-dip plated steel material of this embodiment, a coating may be formed on the plating layer. One or more layers of the coating may be formed. Examples of the type of coating directly on the plating layer include a chromate coating, a phosphate coating, and a chromate-free coating. These coatings can be formed by known methods such as chromate treatment, phosphate treatment, and chromate-free treatment.

[0087] Chromate treatments include electrolytic chromate treatments that form a chromate film by electrolysis, reactive chromate treatments that form a film by utilizing a reaction with the material and then wash away excess treatment solution, and paint-on chromate treatments that apply a treatment solution to the substrate and dry it without rinsing with water to form a film. Any of these treatments may be used.

[0088] Examples of electrolytic chromate treatments include electrolytic chromate treatments using chromic acid, silica sol, resins (phosphoric acid, acrylic resins, vinyl ester resins, vinyl acetate acrylic emulsions, carboxylated styrene butadiene latex, diisopropanolamine-modified epoxy resins, etc.), and hard silica.

[0089] Examples of the phosphate treatment include zinc phosphate treatment, zinc calcium phosphate treatment, and manganese phosphate treatment.

[0090] Chromate-free treatments are particularly suitable because they do not place a burden on the environment. Chromate-free treatments include electrolytic chromate-free treatments that form a chromate-free film by electrolysis, reactive chromate-free treatments that form a film by utilizing a reaction with the material and then wash away excess treatment liquid, and paint-on chromate-free treatments that apply a treatment liquid to the substrate and dry it without rinsing with water to form a film. Any of these treatments may be used.

[0091] Furthermore, one or more organic resin coatings may be provided on the coating directly on the plating layer. The organic resin is not limited to a specific type, and examples thereof include polyester resins, polyurethane resins, epoxy resins, acrylic resins, polyolefin resins, and modified versions of these resins. Here, the term "modified version" refers to a resin obtained by reacting a reactive functional group contained in the structure of these resins with another compound (such as a monomer or a crosslinking agent) containing a functional group capable of reacting with the functional group.

[0092] Such organic resins may be a mixture of one or more unmodified organic resins, or a mixture of one or more organic resins obtained by modifying at least one other organic resin in the presence of at least one organic resin. The organic resin film may also contain any coloring pigment or anti-rust pigment. Water-based organic resins obtained by dissolving or dispersing them in water may also be used.

[0093] As long as the requirements set forth in the present disclosure are met, the method for manufacturing a plated steel sheet is not limited to the above, and electroplating, vapor deposition plating, thermal spraying, cold spraying, etc. may be used instead of hot-dip plating.

[0094] Examples of the present invention will be described below. However, the conditions in the examples are merely examples adopted to confirm the feasibility and effects of the present invention. The present invention is not limited to these examples. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.

[0095] Cold-rolled steel sheets (0.05C-0.1Si-0.2Mn) with a thickness of 1.6 mm were used as the base steel sheets for plating. First, the steel sheets were annealed. The annealed steel sheets were immersed in various hot-dip coating baths and then pulled out, thereby depositing a coating layer on the steel sheet surface. Next, various plated steel sheets were produced by cooling using a cooling gas from immediately after pulling out of the coating bath until the coating layer reached 260°C. The cooling gas was mainly composed of nitrogen gas. The oxygen concentration and dew point of the cooling gas were as shown in Tables 2A and 2B.

[0096] The annealing conditions for annealing the steel sheet in a reducing atmosphere were a soaking temperature of 800°C and a soaking time of 10 seconds. The annealing atmosphere was a reducing atmosphere consisting of a mixed gas of 5% hydrogen and the balance nitrogen. The oxygen concentration in the annealing atmosphere was 20 ppm or less. The annealed steel sheet was then air-cooled with nitrogen gas until the immersion temperature reached the bath temperature + 20°C, after which it was immersed in the hot-dip galvanizing bath for about 3 seconds and then pulled up. The pulling-up speed was 20 to 200 mm / sec. During the pulling-up, N 2 The plating deposition weight was controlled by wiping gas.

[0097] The chemical compositions of the coating layers were as shown in Tables 1A and 1B. The manufacturing conditions were as shown in Tables 2A and 2B. The morphology of the binary or ternary eutectic structure in the coating layers was also evaluated, and the results are shown in Tables 3A and 3B. Furthermore, the coating adhesion and edge corrosion resistance of the coated steel sheets were evaluated, and the results are shown in Tables 3A and 3B.

[0098] The chemical composition of the plating layer, the metal structure of the plating layer, and the unevenness of the surface of the plating layer were evaluated by the above-mentioned methods. The unevenness of the surface of the plating layer was evaluated by setting an observation field in which the longitudinal length Lo of the plating layer was within a range of 500 μm. 2 The presence or absence of Sn phase was determined by X-ray diffraction measurement of the surface of the plating layer. 2 The evaluation was made based on whether or not a diffraction peak of Sn was confirmed.

[0099] Edge corrosion resistance (simulated edge corrosion resistance) was evaluated by cutting the plated steel sheet at any point to expose the cut edge, subjecting the cut edge to a neutral salt spray test as specified in JIS Z 2371, and evaluating the state of red rust on the cut edge. The evaluation criteria for the red rust area ratio are shown below. "AAA," "AA," and "A" were considered to be acceptable. The results are shown in Tables 3A and 3B.

[0100] (Evaluation) AAA: Red rust area ratio 10% or less after 2500 hours AA: Red rust area ratio 10% or less after 2000 hours A: Red rust area ratio 20% or less after 1500 hours B: Red rust area ratio more than 20% after 1500 hours

[0101] To evaluate paint adhesion (adhesion strength), 50 x 100 mm samples were taken from the plated steel sheet and subjected to Zn phosphate treatment (SD5350 system: Nippon Paint Industrial Coating standard). Subsequently, electrodeposition coating (PN110 Powernix® Gray: Nippon Paint Industrial Coating standard) was applied to a thickness of 20 μm and baked at 150°C for 20 minutes. The steel sheet was then bent into a V-shape using a 60° mold with a 10 mm radius of curvature. After unbending, it was further immersed in a 5% NaAl aqueous solution at 50°C for 1,000 hours. A tape peel test was then performed in which adhesive tape was applied only to the V-bent surface and instantly peeled off. The ratio of the area where the paint peeled to the area where the adhesive tape was applied was calculated and rated as follows: "AAA," "AA," and "A" were considered acceptable. The results are shown in Tables 3A and 3B.

[0102] (Evaluation) AAA: Peeled area ratio less than 13% AA: Peeled area ratio 13% or more and less than 25% A: Peeled area ratio 25% or more and less than 35% B: Peeled area ratio 35% or more

[0103] The plated steel sheets of Nos. 1 to 31 had an uneven surface of the plating layer, had a plurality of massive binary eutectic structures or ternary eutectic structures or both in the plating layer, and a portion of the eutectic structure that continuously existed from the surface of the plating layer to half the thickness of the plating layer or to the depth of the Fe—Al-based interfacial alloy layer was located in the concave portions of the uneven surface, the chemical composition of the plating layer and the morphology of the eutectic structure were within the ranges of the present disclosure, and both the edge corrosion resistance and the paint adhesion were excellent.

[0104] In No. 32, the amount of Al in the plating layer was insufficient, resulting in a small (Lr-Lo) / Lo×100 ratio and insufficient paint adhesion.

[0105] In No. 33, the amount of Al in the plating layer was excessive, which resulted in a small (Lr-Lo) / Lo×100 ratio and insufficient paint adhesion.

[0106] In No. 34, the amount of Mg in the plating layer was insufficient. As a result, the (Lr-Lo) / Lo×100 ratio was small, resulting in insufficient paint adhesion. Furthermore, the edge corrosion resistance also deteriorated.

[0107] In No. 35, the amount of Mg in the plating layer was excessive, which resulted in a small (Lr-Lo) / Lo×100 ratio and insufficient paint adhesion.

[0108] In No. 36, the oxygen concentration in the atmosphere from above the plating bath to the end of the cooling step exceeded 5,000 ppm. As a result, in No. 36, the (Lr-Lo) / Lo×100 ratio was small, resulting in insufficient coating adhesion.

[0109] In No. 37, the average cooling rate from the coating bath temperature to 260°C was low. As a result, in No. 37, primary Al crystals (Al phase or Al-Zn phase) were not sufficiently crystallized, the (Lr-Lo) / Lo×100 ratio was small, and the coating adhesion was insufficient.

[0110]

[0111]

[0112]

[0113]

[0114]

[0115]

[0116] DESCRIPTION OF SYMBOLS 1... Plated steel sheet 11... Steel sheet 12, 112... Plated layer 13, 113... Interface alloy layer 14, 114... Binary eutectic structure or ternary eutectic structure

Claims

1. A steel sheet having a plating layer disposed on at least a portion of a surface of the steel sheet, the plating layer having an average chemical composition, in mass%, of Al: 10.00-30.00%, Mg: 1.00-15.00%, Sn: 0.00-1.00%, Si: 0.00-2.00%, Ca: 0.00-2.00%, Ni: 0.00-1.00%, Fe: 0.01-15.00%, Sb: 0.00-0.50%, Pb: 0.00-0.50%, Cu: 0.00-1.00%, Ti: 0.00-1.00%, Cr: 0.00-1.00%, Nb: 0.00-1.00%, Zr: 0.00-1.00%, Mn: 0.00-1.00%, Mo: 0.00-1.00%, Ag: 0.00-1.00%, Li: 0.00-1.00%, Bi: 0.00-1.00%, V: 0.00-1.00%, Co: 0.00-1.00%, In: 0.00-1.00%, W: 0.00-1.00%, P: 0.00-1.00%, La: 0.00-0.50%, Ce: 0.00-0.50%, B: 0.00-0.50%, Y: 0.00-0.50%, Sr: 0.00-0.50%, A plated steel sheet comprising: Sb, Pb, Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, Li, Bi, V, Co, P, In, W, La, Ce, B, Y, and Sr: 0.00 to 5.00% in total, with the balance being Zn and impurities; the surface of the plated layer is an uneven surface; in a cross section of the plated layer, the relationship between the longitudinal length Lo of the plated layer within an observation area of ​​the cross section and the total length Lr of the contour line of the surface of the plated layer within the observation area satisfies the following formula (1); the plated layer contains one or both of a plurality of aggregated binary eutectic structures and a plurality of aggregated ternary eutectic structures; and at least a portion of the plurality of aggregated binary eutectic structures or the plurality of aggregated ternary eutectic structures is present continuously from the surface of the plated layer to a position that is 1 / 2 the average thickness of the plated layer. (Lr-Lo) / Lo x 100 ≧ 2.0 (%) ... (1) 2. The plated steel sheet according to claim 1, wherein the plated layer includes an Fe-Al-based interface alloy layer in contact with the steel sheet, and at least a portion of the binary eutectic structure or the ternary eutectic structure in a plurality of clusters is continuously present from the surface of the plated layer to the Fe-Al-based interface alloy layer.

3. The plated steel sheet according to claim 1, wherein the number of locations at which at least a portion of a plurality of aggregates of the binary eutectic structure or a plurality of aggregates of the ternary eutectic structure are continuously present from the surface of the plating layer to a position that is 1 / 2 the average thickness of the plating layer is 1 to 15 locations per rectangular region on the surface of the plating layer with long sides of 500 μm and short sides of 150 μm.

4. The plated steel sheet according to claim 1, which satisfies the following formula (2) instead of the formula (1), and the number of locations where at least a portion of the binary eutectic structure or the ternary eutectic structure is present continuously from the surface of the plating layer to a position that is 1 / 2 the average thickness of the plating layer is 3 to 15 locations per rectangular region on the surface of the plating layer with long sides of 500 μm and short sides of 150 μm: (Lr-Lo) / Lo×100≧6.0(%) ... (2) 5. The plated steel sheet according to claim 1, which satisfies the following formula (3) instead of the formula (1), and the number of locations where at least a portion of the binary eutectic structure or the ternary eutectic structure is continuously present from the surface of the plating layer to a position that is 1 / 2 the average thickness of the plating layer is 5 to 15 locations per rectangular region on the surface of the plating layer with a long side of 500 μm and a short side of 150 μm: (Lr-Lo) / Lo×100≧8.0(%) ... (3) 6. The plated steel sheet according to any one of claims 1, 3, 4 and 5, wherein a location where at least a portion of a plurality of aggregates of the binary eutectic structure or a plurality of aggregates of the ternary eutectic structure are present continuously from the surface of the plating layer to a position that is 1 / 2 of the average thickness of the plating layer is located in a concave portion of the uneven surface of the plating layer.

7. The plated steel sheet according to claim 2, wherein a portion of the binary eutectic structure or the ternary eutectic structure is present continuously from the surface of the plated layer to the Fe-Al-based interface alloy layer, the portion being located in a concave portion of the uneven surface of the plated layer.

8. The plated steel sheet according to claim 1, wherein the average chemical composition of the plating layer is such that Al and Mg are Al: 10.00 to 25.00%, Mg: 4.50 to 15.00%.

9. The plated steel sheet according to claim 1, wherein the average chemical composition of the plating layer is such that Al and Mg are Al: 15.00 to 22.00%, Mg: 5.00 to 15.00%.

10. In the average chemical composition of the plating layer, Sn is 0.05 to 0.50%, and Mg is detected in the plating layer by X-ray diffraction measurement. 2 The plated steel sheet according to claim 1 , claim 8 or claim 9 , which has a Sn phase.

11. The plated steel sheet according to claim 1, claim 8 or claim 9, wherein the average chemical composition of the plating layer contains one or both of La and Ce, the total amount of La and Ce being 0.05 to 0.50%.

12. The plated steel sheet according to claim 10, wherein the average chemical composition of the plating layer contains one or both of La and Ce, the total amount of La and Ce being 0.05 to 0.50%.

13. A steel material, a plating layer disposed on at least a portion of a surface of the steel material, and a coating film disposed on a surface of the plating layer, wherein the average chemical composition of the plating layer is, in mass%, Al: 10.00-30.00%, Mg: 1.00-15.00%, Sn: 0.00-1.00%, Si: 0.00-2.00%, Ca: 0.00-2.00%, Ni: 0.00-1.00%, Fe: 0.01-15.00%, Sb: 0.00-0.50%, Pb: 0.00-0.50%, Cu: 0.00-1.00%, Ti: 0.00-1.00%, Cr: 0.00-1.00%, Nb: 0.00-1.00%, Zr: 0.00-1.00%, Mn: 0.00-1.00%, Mo: 0.00-1.00%, Ag: 0.00-1.00%, Li: 0.00-1.00%, Bi: 0.00-1.00%, V: 0.00-1.00%, Co: 0.00-1.00%, In: 0.00-1.00%, W: 0.00-1.00%, P: 0.00-1.00%, La: 0.00-0.50%, Ce: 0.00-0.50%, B: 0.00-0.50%, Y :0.00~0.50%, Sr:0.00~0.50%, An automotive member comprising: a total of Sb, Pb, Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, Li, Bi, V, Co, P, In, W, La, Ce, B, Y, and Sr: 0.00 to 5.00%, and the balance: Zn and impurities; the surface of the plating layer is an uneven surface; in a cross section of the plating layer, a relationship between a longitudinal length Lo of the plating layer within an observation area of ​​the cross section and a total length Lr of a contour line of the surface of the plating layer within the observation area satisfies the following formula (4); the plating layer contains one or both of a plurality of aggregated binary eutectic structures and a plurality of aggregated ternary eutectic structures; and at least a portion of the plurality of aggregated binary eutectic structures or the plurality of aggregated ternary eutectic structures is continuously present from the surface of the plating layer to a position that is 1 / 2 the average thickness of the plating layer. (Lr-Lo) / Lo×100≧2.0(%) ... (4)

Citation Information

Patent Citations

  • Game machine

    JP2023087179A

  • Plated steel

    WO2018139620A1

  • ROUGHENED HOT DIP Zn-Al-Mg ALLOY PLATED STEEL SHEET, METHOD FOR PRODUCING THE SAME, AND COMPOSITE OBTAINED BY JOINING HOT DIP Zn-Al-Mg ALLOY PLATED STEEL SHEET WITH THERMOPLASTIC RESIN MOLDED BODY, AND METHOD FOR PRODUCING THE SAME

    JP2011157579A

  • HOT-DIP GALVANIZED Zn-Al-Mg BASE PLATED STEEL PLATE AND MANUFACTURING METHOD OF THE SAME

    JP2018188704A

  • High-corrosion-resistance hot-dip galvanized steel plate having highly uniform appearance and manufacturing method therefor

    WO2013002358A1