Composite particles for negative electrode material, and secondary battery
The use of composite particles with controlled aspect ratio silicon particles coated in a dense carbon phase addresses the efficiency challenges in lithium-ion batteries by reducing side reactions and expansion, resulting in improved battery performance.
Patent Information
- Application Number
- PCT/JP2024/018753
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-21
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional lithium-ion batteries using silicon-carbon composite materials face challenges in improving initial charging and discharging efficiency due to side reactions and silicon particle expansion, which lead to cracks and reduced performance.
The development of composite particles with crystalline silicon particles dispersed in a carbon phase, where the silicon particles have a controlled aspect ratio and are coated with a dense carbon material to reduce pore volume and enhance electrical stability, thereby suppressing side reactions and silicon expansion.
This configuration improves the initial charging and discharging efficiency of lithium-ion batteries by reducing side reactions and silicon particle expansion, leading to enhanced battery performance and stability.
Smart Images

Figure JP2024018753_05122024_PF_FP_ABST
Abstract
Description
Composite particles for negative electrode material and secondary battery
[0001] The present disclosure relates to composite particles for negative electrode materials and secondary batteries.
[0002] Composite materials containing silicon and carbon materials are being investigated as a negative electrode material for increasing the capacity of lithium-ion batteries. Patent Document 1 discloses a negative electrode active material for lithium secondary batteries that is a porous silicon-carbon composite containing a large number of pores and in which multiple nanosilicon particles are embedded in a carbon-based substance.
[0003] Special Publication No. 2022-501787
[0004] In the prior art, it is desirable to improve the initial charge-discharge efficiency of a battery that uses a composite material containing silicon and a carbon material as an active material.
[0005] The composite particles for a negative electrode material of the present disclosure include: a carbon phase; and silicon particles dispersed in the carbon phase; in an X-ray diffraction pattern obtained by X-ray diffraction measurement using Cu-Kα radiation, the half-width of the X-ray diffraction peak derived from the Si (111) plane is 0.1° or more and less than 0.75°; and the average aspect ratio of the silicon particles is 1.0 or more and 1.6 or less.
[0006] According to the technique of the present disclosure, composite particles for a negative electrode material that can improve the initial charge / discharge efficiency of a battery can be provided.
[0007] Fig. 1 is a cross-sectional view showing a schematic configuration of an example of a composite particle for a negative electrode material according to embodiment 1. Fig. 2 is a cross-sectional view showing a schematic configuration of a secondary battery according to embodiment 2.
[0008] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings. The present disclosure is not limited to the following embodiments.
[0009] (Embodiment 1) Figure 1 is a cross-sectional view showing a schematic configuration of one example of a composite particle for a negative electrode material according to embodiment 1. Composite particle 10 includes a carbon phase 1 and silicon particles 2. The silicon particles 2 are dispersed in the carbon phase 1. In an X-ray diffraction pattern obtained by X-ray diffraction measurement of composite particle 10 using Cu-Kα radiation, the half-width of the X-ray diffraction peak derived from the Si (111) plane is 0.1° or more and less than 0.75°. The average aspect ratio of the silicon particles 2 is 1.0 or more and 1.6 or less.
[0010] In the present disclosure, the aspect ratio of a silicon particle 2 is the ratio of the longest diameter (i.e., the length of the major axis) of the silicon particle 2 to the shortest diameter (i.e., the length of the minor axis) of the silicon particle 2 (length of the major axis / length of the minor axis).
[0011] The aspect ratio of the silicon particles 2 can be determined from an SEM image of the composite particle 10 obtained by a scanning electron microscope (SEM). That is, the aspect ratio is calculated by identifying the shortest and longest diameters of the silicon particles 2 from an SEM image of the cross section of the composite particle 10 where the silicon particles 2 are exposed. The average aspect ratio can be determined by determining the aspect ratios of 500 silicon particles 2 randomly extracted from the SEM image of the composite particle 10 and calculating the median value based on their number.
[0012] The X-ray diffraction pattern of the composite particle 10 can be obtained by X-ray diffraction measurement by the θ-2θ method using Cu-Kα rays with wavelengths of 1.5405 Å and 1.5444 Å, that is, wavelengths of 0.15405 nm and 0.15444 nm.
[0013] The diffraction angle of a peak in an X-ray diffraction pattern is defined as the angle at which the signal-to-noise ratio (i.e., the ratio of signal S to background noise N) is 1.3 or more and the peak width at half maximum is 10° or less. MAX When the intensity is I MAX The width is the difference between the two diffraction angles that are half the value of the square root of the diffraction angle.
[0014] The X-ray diffraction peak derived from the (111) plane of Si is, for example, an X-ray diffraction peak having the highest intensity within a diffraction angle 2θ range of 28.1° or more and 28.7° or less, and is, for example, an X-ray diffraction peak located at a diffraction angle 2θ of 28.4°.
[0015] In the composite particle 10, crystalline silicon particles 2 with a small aspect ratio are dispersed in a carbon phase 1. In other words, the carbon phase 1 containing a carbonaceous material coats the crystalline silicon particles 2 with a small aspect ratio. The small aspect ratio of the silicon particles 2 improves the coverage by the carbon phase 1, allowing the pore volume of the composite particle 10 to be reduced. Therefore, in a battery using the composite particle 10, side reactions between the electrolyte and the composite particle 10 can be suppressed, thereby improving the initial charge / discharge efficiency. Furthermore, the small aspect ratio of the silicon particles 2 also reduces the amount of expansion of the silicon particles 2 during battery charge / discharge, thereby suppressing the occurrence of cracks in the composite particle 10, which can cause side reactions with the electrolyte. Therefore, with the above configuration, the initial charge / discharge efficiency of a battery using the composite particle 10 can be improved.
[0016] The average aspect ratio of the silicon particles 2 may be 1.1 or more and 1.6 or less.
[0017] In the X-ray diffraction pattern obtained by X-ray diffraction measurement of the composite particle 10 using Cu-Kα radiation, the half-value width of the X-ray diffraction peak derived from the Si (111) plane may be 0.2° or more and 0.4° or less.
[0018] The carbon phase 1 is a matrix composed of a carbonaceous material. The carbonaceous material is not particularly limited as long as it is a carbonaceous material that can absorb lithium ions. The carbonaceous material may be amorphous. The carbon phase 1 may be composed of an amorphous carbonaceous material. Examples of the carbonaceous material include pitch-derived materials, amorphous carbon, and carbon black. Examples of the pitch include coal pitch and petroleum pitch. This can further stabilize the electrical connection between the silicon particles 2 within the composite particle and the electrical connection between the silicon particles 2 and the carbonaceous material.
[0019] In an X-ray diffraction pattern obtained by X-ray diffraction measurement of composite particle 10 using Cu-Kα radiation, the half-width of the X-ray diffraction peak derived from the (002) plane of C within a diffraction angle 2θ range of 23.0° to 26.0° may be 4.0° to 9.5°. Here, the X-ray diffraction peak derived from the (002) plane of C is, for example, the X-ray diffraction peak having the highest intensity within a diffraction angle 2θ range of 23.0° to 26.0°.
[0020] The silicon particles 2 are, for example, nanosilicon particles. The average particle diameter of the silicon particles 2 may be 10 nm or more and 110 nm or less, or 10 nm or more and 100 nm or less. The average particle diameter of the silicon particles 2 may be 25 nm or more and 65 nm or less. With the above configuration, the initial charge / discharge efficiency of the battery can be improved.
[0021] The average particle diameter of the silicon particles 2 can be determined from an SEM image of the composite particle 10 obtained by SEM. That is, the average particle diameter of the silicon particles 2 can be measured from an SEM image of the cross section of the composite particle 10 in which the cross section of the silicon particles 2 is exposed. The average particle diameter can be determined by measuring the particle diameters of 500 silicon particles 2 randomly extracted from the SEM image of the composite particle 10 and calculating their median diameter (D50). Here, the maximum Feret diameter of the silicon particles 2 in the obtained SEM image can be considered as the particle diameter of the silicon particles 2. The "maximum Feret diameter" is the maximum length of the perpendicular line formed by sandwiching a particle between two parallel lines.
[0022] The median value based on the number of particle diameters of 500 silicon particles 2 measured by SEM observation is regarded as the median diameter of the silicon particles 2.
[0023] The average particle diameter of the composite particles 10 may be 1 μm or more and 10 μm or less. The average particle diameter of the composite particles 10 can be measured in the same manner as the average particle diameter of the silicon particles 2, for example.
[0024] The pore volume of the composite particle 10 may be 0.10 cc / g or less. The pore volume of the composite particle 10 may be 0.01 cc / g or more. The pore volume of the composite particle 10 may be 0.01 cc / g or more and 0.08 cc / g or less, or 0.01 cc / g or more and 0.05 cc / g or less. Since the carbon phase 1 is a dense carbonaceous material and the silicon particles 2 are coated with the dense carbon phase 1, the initial charge / discharge efficiency of the battery can be improved.
[0025] The pore volume of the composite particle 10 can be determined by, for example, the BJH (Barrett-Joyner-Halenda) method using a nitrogen gas adsorption apparatus.
[0026] The specific surface area of the composite particle 10 is 15.0 m 2 / g or less, and 2 / g or less. In the present disclosure, the specific surface area is a BET specific surface area that can be measured by the BET method. The specific surface area of the composite particle 10 is 2.0 m 2 / g or more and 11.0m 2 / g or less, and 2 / g or more 11.0m 2 / g or less, and 6.0m 2 / g or more 11.0m 2 / g or less, and 6.0m 2 / g or more 9.0m 2 / g or less. With the above configuration, the initial charge / discharge efficiency of the battery can be improved.
[0027] The true density of the composite particle 10 may be 2.2 g / cc or less. The true density of the composite particle 10 may be 2.0 g / cc or more and 2.2 g / cc or less. With the above configuration, the silicon particles 2 are coated with the dense carbon phase 1, thereby improving the initial charge / discharge efficiency of the battery. The true density of the composite particle 10 can be measured, for example, by a pycnometer method using He gas.
[0028] The ratio of Si in the composite particle 10 may be 35.0% by mass or more and 60.0% by mass or less. The ratio of Si in the composite particle 10 may be 38.0% by mass or more and 60.0% by mass or less, or 38.9% by mass or more and 50.0% by mass or less. With the above configuration, the initial charge / discharge efficiency of the battery can be improved.
[0029] The composite particle 10 may further contain N (nitrogen). The above configuration can improve the conductivity of the composite particle 10. Furthermore, silicon oxidation can be suppressed. As a result, the initial charge / discharge efficiency of the battery can be improved. The N ratio in the composite particle 10 may be 0.02% by mass or more and 2.0% by mass or less, or 0.05% by mass or more and 1.0% by mass or less. The N ratio in the composite particle 10 may be 0.05% by mass or more and 0.7% by mass or less, or 0.05% by mass or more and 0.5% by mass or less. The above configuration can improve the initial charge / discharge efficiency of the battery. The N contained in the composite particle 10 is derived from, for example, a binder used in the manufacturing process of the composite particle 10. The above configuration improves the conductivity of the interface between the carbon phase 1 and the silicon particle 2 and suppresses silicon oxidation during manufacturing.
[0030] The composite particle 10 may further contain O (oxygen). The ratio of O in the composite particle 10 may be 7% by mass or less, less than 6.8% by mass, or less than 6.3% by mass. The ratio of O in the composite particle 10 may be 1% by mass or more and 7% by mass or less, 4% by mass or more and less than 6.8% by mass, or 5% by mass or more and 6.25% by mass or less. With the above configuration, the initial charge / discharge efficiency of the battery can be improved.
[0031] The proportion of C in the composite particles 10 may be 35% by mass or more and 60% by mass or less, or 35% by mass or more and 55% by mass or less. According to the above configuration, the initial charge / discharge efficiency of the battery can be improved.
[0032] The mass ratio of Si in the composite particle 10 can be measured using Si-NMR. The mass ratio of C in the composite particle 10 can be measured by combustion-infrared absorption spectroscopy using a carbon / sulfur analyzer. The mass ratio of N in the composite particle 10 can be measured, for example, by inert gas fusion-thermal conductivity spectroscopy (TCD) using an oxygen / nitrogen / hydrogen analyzer. The mass ratio of O in the composite particle 10 can be measured, for example, by inert gas fusion-non-dispersive infrared spectroscopy (NDIR) using an oxygen / nitrogen / hydrogen analyzer.
[0033] In addition to the above-mentioned components, the composite particle 10 may further contain other components. The composite particle 10 may contain the other components in a proportion of more than 0% by mass and not more than 20% by mass, more than 0% by mass and not more than 10% by mass, more than 0% by mass and not more than 5% by mass, or more than 0% by mass and not more than 2% by mass.
[0034] The composite particles 10 are used, for example, as a negative electrode active material.
[0035] (Method for producing composite particles for negative electrode material) An example of a method for producing composite particles for negative electrode material according to embodiment 1 will be described. The method for producing composite particles for negative electrode material according to embodiment 1 includes mixing silicon particles and a carbon source, pressure-molding the resulting mixture, heat-treating the resulting molded body, and coating the heat-treated molded body with carbon.
[0036] When mixing the silicon particles and the carbon source, a binder may be mixed in. That is, the method for producing composite particles for a negative electrode material according to the first embodiment may include mixing the silicon particles, the carbon source, and the binder, pressure-molding the resulting mixture, heat-treating the resulting molded body, and coating the heat-treated molded body with carbon.
[0037] The silicon particles may be the same as the silicon particles 2 described above.
[0038] Examples of carbon sources that can be used include pitch, tar, thermoplastic resins, and thermosetting resins. The carbon source may be pitch, which may be coal pitch or petroleum pitch.
[0039] Examples of binders include ammonium polycarboxylate salts, polyvinylpyrrolidone, ammonium polyacrylate salts, ammonium carboxymethylcellulose salts, polyalkylene polyamines, polyacrylamides, polyethyleneimines, and polyethylene glycols. The binder may be a polymer that undergoes amorphous carbonization under the conditions of heat treatment of the molded body. The above configuration stabilizes the electrical connection between silicon particles or between silicon particles and a carbonaceous material in the composite particles for anode material. The binder may have a structure containing N. The above configuration enables the production of composite particles for anode material that can improve the initial charge / discharge efficiency of a battery. The binder may be polyvinylpyrrolidone.
[0040] The means for mixing the silicon particles, carbon source, and binder is not particularly limited, and they may be mixed using, for example, a rocking mill.
[0041] The mixture is then pressed, for example, using cold isostatic pressing (CIP), or may be pressed using a uniaxial press.
[0042] The resulting molded body is then heat-treated to carbonize the carbon source and binder. The carbon source and binder can be carbonized to amorphous carbon. In this way, composite particles of silicon and carbon are obtained.
[0043] The temperature for the heat treatment of the molded body is, for example, 700° C. or more and 1000° C. or less. The time for the heat treatment is, for example, 1 hour or more and 10 hours or less, and may be 5 hours or less. The heat treatment may be performed in an inert atmosphere.
[0044] The heat-treated molded body may be pulverized, and the particle size may be adjusted to a desired size by pulverization.
[0045] The pulverized molded body is then coated with carbon. For example, the pulverized molded body is coated with a carbon source and then heat-treated under the conditions described above, thereby coating the carbon. The pulverization of the molded body and the coating of carbon may be repeated multiple times. The pulverization may be performed using, for example, a cutter mill.
[0046] In this manner, the composite particles for a negative electrode material according to the first embodiment are obtained.
[0047] (Embodiment 2) A secondary battery according to embodiment 2 includes a negative electrode, a positive electrode, and an electrolyte. The negative electrode contains a negative electrode material including the composite particles for a negative electrode material according to embodiment 1. That is, in the secondary battery according to embodiment 2, the negative electrode contains the composite particles for a negative electrode material according to embodiment 1.
[0048] FIG. 2 is a cross-sectional view showing a schematic configuration of a secondary battery according to a second embodiment. The secondary battery 100 includes a positive electrode 23, a negative electrode 26, a separator 27, a non-aqueous electrolyte 29, and an exterior casing 28. The positive electrode 23, the negative electrode 26, the non-aqueous electrolyte 29, and the separator 27 are housed in the exterior casing 28. The separator 27 is disposed between the positive electrode 23 and the negative electrode 26. The positive electrode 23 and the negative electrode 26 face each other with the separator 27 interposed therebetween. The positive electrode 23 includes a positive electrode mixture layer 22 and a positive electrode current collector 21. The positive electrode mixture layer 22 is disposed between the positive electrode current collector 21 and the separator 27. The negative electrode 26 includes a negative electrode mixture layer 25 and a negative electrode current collector 24. The negative electrode mixture layer 25 is disposed between the negative electrode current collector 24 and the separator 27.
[0049] The positive electrode mixture layer 22 includes a positive electrode active material capable of absorbing and releasing lithium ions. Examples of the positive electrode active material include lithium-containing transition metal oxides, lithium-containing transition metal phosphates, transition metal fluorides, polyanionic materials, fluorinated polyanionic materials, transition metal sulfides, transition metal oxysulfides, and transition metal oxynitrides. In particular, using a lithium-containing transition metal oxide or a lithium-containing transition metal phosphate as the positive electrode active material can reduce the manufacturing cost of the battery and increase the average discharge voltage. Examples of lithium-containing transition metal oxides include lithium cobalt oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese oxide, and lithium nickel manganese oxide. Examples of lithium-containing transition metal phosphates include lithium iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, and lithium nickel phosphate. At least one selected from these positive electrode active materials can be used.
[0050] The positive electrode mixture layer 22 may contain a conductive additive, an ion conductor, and a binder as needed.
[0051] Conductive additives and ion conductors are used to reduce the resistance of the electrodes. Examples of conductive additives include carbon materials and conductive polymer compounds. Examples of carbon materials include carbon black, graphite, acetylene black, carbon nanotubes, carbon nanofibers, graphene, fullerene, and graphite oxide. Examples of conductive polymer compounds include polyaniline, polypyrrole, and polythiophene. At least one selected from these conductive additives can be used.
[0052] Binders are used to improve the binding properties of the materials that make up the electrode. Examples of binders include polymeric materials such as polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, polytetrafluoroethylene, carboxymethyl cellulose, polyacrylic acid, styrene-butadiene copolymer rubber, polypropylene, polyethylene, and polyimide. At least one selected from these binders can be used.
[0053] The positive electrode current collector 21 is a sheet or film made of a metal material such as aluminum, an aluminum alloy, stainless steel, titanium, or a titanium alloy. The sheet or film may be porous or non-porous. Examples of the sheet or film include metal foil and metal mesh. A carbon material may be applied to the surface of the positive electrode current collector 21 as a conductive auxiliary material.
[0054] The negative electrode mixture layer 25 includes a negative electrode material. The negative electrode material includes the composite particles for a negative electrode material according to embodiment 1. The negative electrode material (negative electrode mixture layer 25) may include a conductive additive, an ion conductor, and a binder as needed. Materials that can be used for the positive electrode mixture layer 22 can also be used for the negative electrode mixture layer 25 as the conductive additive, ion conductor, and binder.
[0055] The negative electrode current collector 24 is a sheet or film made of a metal material such as stainless steel, nickel, a nickel alloy, copper, or a copper alloy. The sheet or film may be porous or non-porous. Examples of the sheet or film include metal foil and metal mesh. A carbon material may be applied to the surface of the negative electrode current collector 24 as a conductive auxiliary material.
[0056] The separator 27 is an electrolyte layer having lithium ion conductivity. There are no particular limitations on the material of the separator 27 as long as it allows the passage of lithium ions. The material of the separator 27 can be at least one selected from the group consisting of solid electrolytes, gel electrolytes, ion exchange resin membranes, semipermeable membranes, and porous membranes. If the separator 27 is made of these materials, the safety of the secondary battery 100 can be sufficiently ensured. Examples of solid electrolytes include sulfide solid electrolytes such as Li2S-P2S5, Li7La3Zr2O 12 Examples of the electrolyte include oxide solid electrolytes such as LLZ. Examples of the gel electrolyte include gel electrolytes containing fluororesins such as PVdF. Examples of the ion exchange resin membrane include cation exchange membranes and anion exchange membranes. Examples of the porous membrane include porous membranes made of polyolefin resins and porous membranes made of glass paper obtained by weaving glass fibers into nonwoven fabric.
[0057] The non-aqueous electrolyte 29 may be impregnated into the positive electrode 23, the negative electrode 26, and the separator 27. The non-aqueous electrolyte 29 may fill the internal space of the exterior casing 28. The non-aqueous electrolyte 29 functions to allow lithium ions to travel between the positive electrode 23 and the negative electrode 26. The non-aqueous electrolyte 29 may include a non-aqueous electrolyte solution, a gel electrolyte, or an ionic liquid.
[0058] The non-aqueous electrolyte solution contains, for example, a non-aqueous solvent and a lithium salt.
[0059] Examples of non-aqueous solvents that can be used include cyclic carbonates, chain carbonates, cyclic ethers, chain ethers, cyclic esters, chain esters, fluorine-containing solvents, and nitriles. Examples of cyclic carbonates include ethylene carbonate, propylene carbonate, and butylene carbonate. Examples of chain carbonates include dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate. Examples of cyclic ethers include tetrahydrofuran, 1,4-dioxane, and 1,3-dioxolane. Examples of chain ethers include 1,2-dimethoxyethane and 1,2-diethoxyethane. Examples of cyclic esters include γ-butyrolactone. Examples of chain esters include methyl acetate. Examples of fluorine-containing solvents include fluoroethylene carbonate, methyl fluoropropionate, fluorobenzene, fluoroethyl methyl carbonate, and fluorodimethylene carbonate. Examples of nitriles include acetonitrile. At least one selected from these non-aqueous solvents can be used.
[0060] Examples of lithium salts include lithium hexafluorophosphate (LiPF), lithium tetrafluoroborate (LiBF), lithium perchlorate (LiClO), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bisperfluoroethylsulfonylimide (LiN(SO2C2F5)2), LiAsF6, LiCF3SO3, and lithium difluoro(oxalato)borate. At least one selected from these lithium salts can be used.
[0061] The gel electrolyte can be a material obtained by impregnating a polymer material with a non-aqueous electrolyte solution, such as polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polymethyl methacrylate, or a polymer having an ethylene oxide bond.
[0062] Examples of cations constituting ionic liquids include aliphatic chain quaternary cations, aliphatic cyclic ammonium, and nitrogen-containing heterocyclic aromatic cations. Examples of aliphatic chain quaternary cations include tetraalkylammonium and tetraalkylphosphonium. Examples of aliphatic cyclic ammonium include pyrrolidiniums, morpholiniums, imidazoliniums, tetrahydropyrimidiniums, piperaziniums, and piperidiniums. Examples of nitrogen-containing heterocyclic aromatic cations include pyridiniums and imidazoliums. Examples of anions constituting ionic liquids include PF6 - , BF4 - , SbF6 - , AsF6 - , SO3CF3 - , N(SO2F)2 - , N(SO2CF3)2 - , N(SO2C2F5)2 - , N(SO2CF3)(SO2C4F9) - , C(SO2CF3)3 - The ionic liquid may contain a lithium salt.
[0063] The exterior 28 is made of a material obtained by laminating a metal foil such as an aluminum foil with a resin film such as a PET film, for example. The exterior 28 may also be a container made of resin or metal.
[0064] The shape of the secondary battery 100 is not limited to the laminated type. Other shapes of the secondary battery 100 include a coin type, a cylindrical type, a square type, a sheet type, a button type, and a flat type.
[0065] In the secondary battery according to the second embodiment, the negative electrode contains the composite particles for a negative electrode material according to the first embodiment, and therefore the initial charge / discharge efficiency is improved.
[0066] (Other Embodiments) (Additional Notes) The above description of the embodiments discloses the following techniques.
[0067] (Technology 1) Composite particles for a negative electrode material comprising: a carbon phase; and silicon particles dispersed in the carbon phase; wherein, in an X-ray diffraction pattern obtained by X-ray diffraction measurement using Cu-Kα radiation, the half-width of an X-ray diffraction peak derived from a Si (111) plane is 0.1° or more and less than 0.75°; and the average aspect ratio of the silicon particles is 1.0 or more and 1.6 or less.
[0068] This configuration can improve the initial charge / discharge efficiency of the battery.
[0069] (Technology 2) The composite particles for a negative electrode material according to Technology 1, wherein the half width is 0.2° or more and 0.4° or less. With this configuration, the initial charge / discharge efficiency of the battery can be improved.
[0070] (Technology 3) The composite particles for a negative electrode material according to Technology 1 or 2, wherein the silicon particles have an average particle size of 10 nm or more and 100 nm or less. With this configuration, the initial charge / discharge efficiency of the battery can be improved.
[0071] (Technology 4) The composite particles for a negative electrode material according to Technology 3, wherein the average particle diameter is 25 nm or more and 65 nm or less. With this configuration, the initial charge / discharge efficiency of the battery can be improved.
[0072] (Technology 5) Composite particles for a negative electrode material according to any one of Technologies 1 to 4, having a pore volume of 0.10 cc / g or less. With this configuration, the initial charge / discharge efficiency of the battery can be improved.
[0073] (Technology 6) Composite particles for a negative electrode material according to any one of Technologies 1 to 5, having a pore volume of 0.01 cc / g or more and 0.08 cc / g or less. With this configuration, the initial charge / discharge efficiency of the battery can be improved.
[0074] (Technology 7) The composite particles for a negative electrode material according to any one of Technologies 1 to 6, wherein the Si ratio in the composite particles for a negative electrode material is 35.0 mass % or more and 60.0 mass % or less. With this configuration, the initial charge / discharge efficiency of the battery can be improved.
[0075] (Technology 8) The composite particles for a negative electrode material according to any one of Technologies 1 to 7, wherein the N ratio in the composite particles for a negative electrode material is 0.05 mass % or more and 1.0 mass % or less. With this configuration, the charge / discharge efficiency of the battery can be further improved.
[0076] (Technology 9) The composite particles for a negative electrode material according to any one of Technologies 1 to 8, wherein the O ratio in the composite particles for a negative electrode material is less than 6.3 mass %. With this configuration, the initial charge / discharge efficiency of the battery can be further improved.
[0077] (Technology 10) The composite particles for a negative electrode material according to any one of Technologies 1 to 9, wherein the carbon phase is composed of an amorphous carbonaceous material. With this configuration, the initial charge / discharge efficiency of the battery can be improved.
[0078] (Technology 11) The composite particles for a negative electrode material according to any one of Techniques 1 to 10, wherein in an X-ray diffraction pattern obtained by X-ray diffraction measurement using Cu-Kα radiation, the half-width of an X-ray diffraction peak derived from the (002) plane of C within a diffraction angle 2θ range of 23.0° to 26.0° is 4.0° to 9.5°. With this configuration, the initial charge-discharge efficiency of the battery can be improved.
[0079] (Technology 12) Composite particles for a negative electrode material according to any one of Technologies 1 to 11, having a true density of 2.0 g / cc or more and 2.2 g / cc or less. With this configuration, the silicon particles are coated with a dense carbon phase, thereby improving the initial charge / discharge efficiency of the battery.
[0080] (Technology 13) Specific surface area is 11.0 m 2 / g or less. This configuration can improve the initial charge / discharge efficiency of the battery.
[0081] (Technology 14) A secondary battery comprising: a negative electrode containing the composite particles for a negative electrode material according to any one of Technologies 1 to 13; a positive electrode; and an electrolyte.
[0082] With this configuration, the effect of improving the initial charge / discharge efficiency can be obtained.
[0083] The present disclosure will be described in more detail below using examples. The following examples are merely examples of embodiments, and are not intended to limit the scope of the present disclosure.
[0084] [Preparation of composite particles for negative electrode material] (Example 1) Silicon particles with an average particle diameter of 40 nm and an aspect ratio of 1.3 were prepared. The average particle diameter and aspect ratio of the silicon particles were calculated from SEM images of the silicon particles taken by a scanning electron microscope. Specifically, the median diameter (D50) and the number-based median value of the aspect ratio calculated from the maximum Feret diameter of 500 particles arbitrarily selected in the SEM images of the silicon particles were calculated as the average particle diameter and the aspect ratio, respectively.
[0085] 50 g of silicon particles, 10 g of polyvinylpyrrolidone as a binder, and 50 g of zirconia balls as a mixing medium were placed in a rocking mill and mixed at 60 Hz for 1 minute. After mixing, 55 g of petroleum pitch was added to the rocking mill and mixed at 60 Hz for 1 minute.
[0086] The mixture was then press-molded by cold isostatic pressing (CIP) at 190 MPa for 5 minutes to obtain a molded body.
[0087] The resulting molded body was heat treated at 800° C. for 5 hours in an argon atmosphere at a temperature increase rate of 100° C. / min to obtain composite particles of silicon and carbon.
[0088] The obtained composite particles were pulverized using a cutter mill at 18,000 rpm for 5 minutes. 3.25 g of petroleum pitch was added to 50 g of the pulverized composite particles, and the mixture was again heat-treated and pulverized under the same conditions.
[0089] The above heat treatment and pulverization were each repeated once more, thereby obtaining composite particles for a negative electrode material of Example 1.
[0090] Example 2 Composite particles for a negative electrode material of Example 2 were obtained in the same manner as in Example 1, except that silicon particles having an average particle size of 25 nm and an aspect ratio of 1.2 were used.
[0091] Example 3 Composite particles for a negative electrode material of Example 3 were obtained in the same manner as in Example 1, except that silicon particles having an average particle size of 50 nm and an aspect ratio of 1.2 were used.
[0092] Example 4 Composite particles for a negative electrode material of Example 4 were obtained in the same manner as in Example 1, except that silicon particles having an average particle size of 65 nm and an aspect ratio of 1.2 were used.
[0093] Example 5 Composite particles for a negative electrode material of Example 5 were obtained in the same manner as in Example 1, except that silicon particles having an average particle size of 110 nm and an aspect ratio of 1.2 were used.
[0094] (Example 6) Composite particles for negative electrode material of Example 6 were obtained in the same manner as in Example 1, except that silicon particles having a different crystallinity from the silicon particles used in Example 1 and an aspect ratio of 1.2 were used.
[0095] (Example 7) Composite particles for negative electrode material of Example 7 were obtained in the same manner as in Example 6, except that silicon particles having a crystallinity different from that of the silicon particles used in Example 1 and the silicon particles used in Example 6 were used.
[0096] Example 8 Composite particles for a negative electrode material of Example 8 were obtained in the same manner as in Example 1, except that silicon particles with an aspect ratio of 1.0 were used.
[0097] Example 9 Composite particles for a negative electrode material of Example 9 were obtained in the same manner as in Example 1, except that silicon particles with an aspect ratio of 1.6 were used.
[0098] Example 10 Composite particles for a negative electrode material of Example 10 were obtained in the same manner as in Example 1, except that the amount of petroleum pitch charged into the rocking mill was 32.5 g.
[0099] Example 11 Composite particles for a negative electrode material of Example 11 were obtained in the same manner as in Example 1, except that the amount of petroleum pitch charged into the rocking mill was 85 g.
[0100] Example 12 Composite particles for a negative electrode material of Example 12 were obtained in the same manner as in Example 1, except that the amount of binder charged into the rocking mill was 16.5 g.
[0101] Example 13 Composite particles for a negative electrode material of Example 13 were obtained in the same manner as in Example 1, except that the amount of binder charged into the rocking mill was 1.65 g.
[0102] Example 14 Composite particles for a negative electrode material of Example 14 were obtained in the same manner as in Example 1, except that the binder charged into the rocking mill was changed to 1.65 g of polyethylene glycol.
[0103] (Reference Example 1) 50 g of silicon particles having an average particle size of 10 μm and 2 kg of zirconia beads were pulverized using a ball mill at 1000 rpm for 5 hours. The obtained silicon particles had an average particle size of 150 nm and an aspect ratio of 2. Composite particles for a negative electrode material of Reference Example 1 were obtained in the same manner as in Example 1, except that the silicon particles obtained in this manner were used.
[0104] (Reference Example 2) 50 g of silicon particles having an average particle size of 10 μm and 2 kg of zirconia beads were pulverized using a ball mill at 1000 rpm for 15 hours. The obtained silicon particles had an average particle size of 40 nm and an aspect ratio of 2.5. Composite particles for negative electrode material of Reference Example 2 were obtained in the same manner as in Example 1, except that the silicon particles obtained in this manner were used.
[0105] [Cross-Sectional SEM Observation] The average aspect ratios and average particle diameters of the silicon particles were confirmed using cross-sectional SEM images of the composite particles for negative electrode materials of Examples 1 to 14 and Reference Examples 1 and 2. The results are shown in Table 1.
[0106] [BET Specific Surface Area] The BET specific surface area of the composite particles for negative electrode material of Examples 1 to 14 and Reference Examples 1 and 2 was determined by the BET multipoint method using a nitrogen gas adsorption apparatus (Microtrac-Bel, BEL SOAP Mini X). The value calculated at a relative pressure ratio of 0.1 to 0.3 was taken as the surface area. The measurement results are shown in Table 1.
[0107] [Pore Volume] The pore volumes of the composite particles for negative electrode material of Examples 1 to 14 and Reference Examples 1 and 2 were measured by the BJH method using a nitrogen gas adsorption apparatus (BEL SOAP Mini X, manufactured by Microtrac-Bel). The measurement results are shown in Table 1.
[0108] [X-ray Diffraction] X-ray diffraction patterns of the composite particles for negative electrode material of Examples 1 to 14 and Reference Examples 1 and 2 were obtained by powder X-ray diffraction measurement. An X-ray diffractometer (ENPYREAN, manufactured by Spectris) was used for the measurement. Cu-Kα radiation (wavelengths 1.5405 Å and 1.5444 Å) was used as the X-ray source. The half-widths of the peaks derived from the Si (111) plane in the X-ray diffraction patterns are shown in Table 1.
[0109] [Component Analysis] The mass ratios of Si, C, N, and O in the composite particles for negative electrode material of Examples 1 to 14 and Reference Examples 1 and 2 were measured as follows. The measurement results are shown in Table 1.
[0110] The mass ratio of Si in the composite particles was measured by quantifying Si using Si-NMR under the conditions shown below.
[0111] <Si-NMR measurement conditions> Measurement device: Varian solid-state nuclear magnetic resonance spectrometer (INOVA-400) Probe: Varian 7 mm CPMAS-2 MAS: 4.2 kHz MAS speed: 4 kHz Pulse: DD (45° pulse + signal acquisition time 1H decoupled) Repetition time: 1200 sec to 3000 sec Observation width: 100 kHz Observation center: near -100 ppm Signal acquisition time: 0.05 sec Number of accumulations: 560 Sample amount: 207.6 mg
[0112] The mass ratio of C in the composite particles was measured by a high-frequency induction heating furnace combustion-infrared absorption method using a carbon / sulfur analyzer (Horiba, Ltd., EMIA-520). A sample was weighed onto a magnetic board, a combustion improver was added, and the board was inserted into a combustion furnace (carrier gas: oxygen) heated to 1350°C, and the amount of carbon dioxide gas generated during combustion was detected by infrared absorption. A calibration curve was created using carbon steel (carbon content 0.49%) manufactured by Bureau of Analyzed Samples. Ltd., and the carbon content of the sample was calculated to quantify C.
[0113] The mass ratio of N and the mass ratio of O in the composite particles were measured using an oxygen, nitrogen, and hydrogen analyzer (EGMA-830, manufactured by Horiba, Ltd.). The sample was placed in a Ni capsule and, together with Sn pellets and Ni pellets that served as flux, placed in a carbon crucible heated at 5.75 kW, and the released carbon dioxide gas, carbon monoxide gas, and nitrogen gas were detected. The quantification of O was performed by creating a calibration curve using NS-16-2 (steel standard sample) and calculating the oxygen content of the sample. The quantification of N was performed by creating a calibration curve using SS-2-115 (steel standard sample) and calculating the nitrogen content of the sample.
[0114] [Preparation of Evaluation Cells] Using the composite particles for negative electrode material of Examples 1 to 14 and Reference Examples 1 and 2, evaluation cells of Examples 1 to 14 and Reference Examples 1 and 2 were prepared as follows.
[0115] (Preparation of Negative Electrode) Composite particles for negative electrode material and graphite were mixed in a mass ratio of 5:95 to prepare a negative electrode active material. A negative electrode mixture containing the negative electrode active material, sodium carboxymethyl cellulose (CMC-Na), and styrene-butadiene rubber (SBR) in a mass ratio of negative electrode active material:CMC-Na:SBR=97.5:1:1.5 was added with water and stirred to prepare a negative electrode slurry. Next, a 1 m thick film was applied to both surfaces of a copper foil. 2 The negative electrode slurry was applied to both sides of the copper foil so that the mass of the negative electrode mixture per sheet was 190 g, and the coating was dried and then rolled to form a sheet with a density of 1.5 g / cm 3 A negative electrode having the negative electrode mixture layer formed thereon was fabricated.
[0116] (Preparation of Positive Electrode) Positive Electrode Active Material LiNi 0.88 Co 0.09 Al 0.03 A positive electrode mixture containing O2, acetylene black (AB), and polyvinylidene fluoride (PVDF) in a mass ratio of positive electrode active material:AB:PVDF = 95:2.5:2.5 was prepared. N-methyl-2-pyrrolidone (NMP) was added to the positive electrode mixture and stirred to prepare a positive electrode slurry. Next, the positive electrode slurry was applied to both surfaces of an aluminum foil, the coating was dried, and then rolled to form a film with a density of 3.6 g / cm3 on both surfaces of the aluminum foil. 3 A positive electrode having the positive electrode mixture layer formed thereon was fabricated.
[0117] (Preparation of Electrolyte Solution) A non-aqueous electrolyte solution was prepared by dissolving LiPF6 at a concentration of 1.0 mol / L in a mixed solvent containing ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of EC:DEC=3:7.
[0118] (Preparation of Secondary Battery) Tabs were attached to the positive and negative electrodes, respectively, and the positive and negative electrodes were spirally wound with a separator interposed therebetween so that the tabs were positioned at the outermost periphery to prepare an electrode assembly. The electrode assembly was inserted into an exterior body made of aluminum laminate film, vacuum dried at 105°C for 2 hours, and then a nonaqueous electrolyte solution was injected. The opening of the exterior body was sealed to obtain a secondary battery as an evaluation cell.
[0119] [Evaluation of charge / discharge efficiency] The evaluation cells of Examples 1 to 14 and Reference Examples 1 and 2 were charged at a constant current of 1 It (800 mA) at an ambient temperature of 25 ° C. until the voltage reached 4.2 V, and then charged at a constant voltage of 4.2 V until the current reached 1 / 20 It (40 mA). A 10-minute rest period was then provided, followed by constant current discharge at a current of 1 It (800 mA) until the voltage reached 2.5 V. This evaluated the initial charge / discharge efficiency of the evaluation cells of Examples 1 to 14 and Reference Examples 1 and 2. Table 1 shows the relative values when the charge / discharge efficiency of Reference Example 2 was taken as 100%.
[0120]
[0121] (Discussion) The batteries using the composite particles for negative electrode material of Examples 1 to 14 had improved initial charge-discharge efficiency compared to Reference Examples 1 and 2.
[0122] The technology of the present disclosure is useful for batteries such as lithium ion secondary batteries.
Claims
1. Composite particles for a negative electrode material comprising: a carbon phase; and silicon particles dispersed in the carbon phase; in an X-ray diffraction pattern obtained by X-ray diffraction measurement using Cu-Kα radiation, the half-width of an X-ray diffraction peak derived from a Si (111) plane is 0.1° or more and less than 0.75°; and the average aspect ratio of the silicon particles is 1.0 or more and 1.6 or less.
2. The composite particle for a negative electrode material according to claim 1, wherein the half width is 0.2° or more and 0.4° or less.
3. The composite particle for a negative electrode material according to claim 1, wherein the average particle size of the silicon particles is 10 nm or more and 100 nm or less.
4. The composite particles for a negative electrode material according to claim 3, wherein the average particle size is 25 nm or more and 65 nm or less.
5. The composite particle for a negative electrode material according to claim 1, having a pore volume of 0.10 cc / g or less.
6. The composite particle for a negative electrode material according to claim 5, wherein the pore volume is 0.01 cc / g or more and 0.08 cc / g or less.
7. The composite particle for a negative electrode material according to claim 1, wherein the Si ratio in said composite particle for a negative electrode material is 35.0 mass % or more and 60.0 mass % or less.
8. The composite particle for a negative electrode material according to claim 1, wherein the N ratio in the composite particle for a negative electrode material is 0.05 mass % or more and 1.0 mass % or less.
9. The composite particle for a negative electrode material according to claim 1, wherein the O ratio in the composite particle for a negative electrode material is less than 6.3 mass %.
10. The composite particle for a negative electrode material according to claim 1, wherein the carbon phase is composed of an amorphous carbonaceous material.
11. The composite particle for a negative electrode material according to claim 1, wherein in an X-ray diffraction pattern obtained by X-ray diffraction measurement using Cu-Kα radiation, the half-width of an X-ray diffraction peak derived from the (002) plane of C within a diffraction angle 2θ range of 23.0° or more and 26.0° or less is 4.0° or more and 9.5° or less.
12. The composite particles for a negative electrode material according to claim 1, having a true density of 2.0 g / cc or more and 2.2 g / cc or less.
13. Specific surface area is 11.0 m 2 The composite particle for a negative electrode material according to claim 1 , wherein the molecular weight of the composite particle is 1 / g or less.
14. A secondary battery comprising: a negative electrode containing the composite particle for a negative electrode material according to any one of claims 1 to 13; a positive electrode; and an electrolyte.
Citation Information
Patent Citations
Negative electrode active material for lithium secondary battery and lithium secondary battery including the same
JP2022501787A
Coated composite particle
JP2021187733A
Lithium ion secondary battery
JP2022126004A
Anode, and electrochemical and electronic devices including the same
JP2022514807A