Strain gauge, strain measurement device, and strain measurement method
The strain gauge with a nanogranular structure film of specific metal particles in a fluoride or fluoride-oxide matrix addresses the impracticality of conventional strain gauges by enabling electrical conductivity changes at room temperature, enhancing gauge factor and practicality.
Patent Information
- Application Number
- PCT/JP2024/019294
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2024-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional strain gauges using nanogranular structure films with nanometer-sized metal particles in a fluoride matrix exhibit electrical conductivity changes only at extremely low temperatures, making them impractical for practical use.
A strain gauge comprising a substrate with a nanogranular structure film of non-magnetic or magnetic metal particles in a fluoride or fluoride-oxide matrix, where the metal particles have an average size of 1.0 to 5.0 nm and are spaced 0.2 to 0.6 nm apart, allowing electrical conductivity changes at room temperature due to deformation, enhancing the gauge factor and practicality.
The strain gauge achieves high electrical resistivity and improved gauge factor at room temperature, enabling high-order tunneling and tunnel magnetoresistive effects, significantly improving its practicality and accuracy compared to conventional materials.
Smart Images

Figure JP2024019294_05122024_PF_FP_ABST
Abstract
Description
Strain gauge, strain measuring device and strain measuring method
[0001] The present invention relates to a technique for measuring strain on an object.
[0002] It has been reported that when a nanogranular structure film in which nanometer-sized metal particles are dispersed in a fluoride matrix is deformed, the spacing between the metal particles changes, and the electrical conductivity of the nanogranular structure film changes (see, for example, Non-Patent Document 1).
[0003] S. Kaji, G. Oomi, S. Mitani, S. Takahashi, K. Takanashi, and S. Maekawa. Phys. Rev. B68, 054429 (2003). S. Mitani, S. Takahashi, K. Takanashi, K. Yakushiji, S. Maekawa, and H. Fujimori. Phys. Rev. Lett. 81, 2799 (1998).
[0004] However, since this phenomenon occurs at extremely low temperatures close to the temperature of liquid helium, it is difficult to put this phenomenon into practical use in products.
[0005] Therefore, an object of the present invention is to provide a strain gauge that can improve practicality.
[0006] A strain gauge according to a first aspect of the present invention is a strain gauge comprising a substrate and a resistor formed on a surface of the substrate, wherein the resistor is represented by the general formula L 100-a-b-c M a F b O c (L: one or more non-magnetic metal elements selected from Pt, Au, Ag, and Cu; M: one or more elements selected from Li, Mg, Al, Ca, Sr, Ba, Gd, and Y; F: fluorine; O: oxygen; 12.0≦a≦33.0, 17.0≦b≦70.0, 0≦c≦1.0, 50.0≦a+b+c≦90.0), and is composed of a nanogranular structure film in which metal particles represented by L having an average particle size of 1.0 to 5.0 nm are distributed at an average particle spacing of 0.2 to 0.6 nm in an insulating matrix made of a fluoride or a fluoride and oxide of M.
[0007] A strain gauge according to a second aspect of the present invention is a strain gauge comprising a substrate and a resistor formed on a surface of the substrate, the resistor being represented by the general formula L 100-a-b-c M a F b O c (L: one or more magnetic metal elements selected from Fe, Co, and Ni; M: one or more elements selected from Li, Mg, Al, Ca, Sr, Ba, Gd, and Y; F: fluorine; O: oxygen; 12.0≦a≦33.0, 17.0≦b≦70.0, 0≦c≦1.0, 50.0≦a+b+c≦90.0), and is composed of a nanogranular structure film in which metal particles represented by L having an average particle size of 1.0 to 5.0 nm are distributed in an insulating matrix made of a fluoride or a fluoride and oxide of M, with an average particle spacing of 0.2 to 0.6 nm.
[0008] Effect of the Invention In the strain gauges of the first and second aspects of the present invention, the nano-granular structure film constituting the resistor deforms, changing the spacing between the metal particles constituting the nano-granular structure film. This changes the thickness of the tunnel barrier between the particles, and changes the electrical conductivity. In this case, if the band gap of the matrix material constituting the tunnel barrier is high, the electrical resistivity of the entire film increases, and even at room temperature, the film exhibits a high electrical resistivity comparable to that in the low-temperature region described in Non-Patent Document 1. Even at room temperature, electrical conduction due to high-order tunneling described in Non-Patent Document 2 is realized, thereby improving the gauge factor of the strain gauge and ultimately improving its practicality.
[0009] Furthermore, in the strain gauge of the second aspect of the present invention, the metal particles constituting the nanogranular structure film are magnetic metal particles, and therefore the tunneling magnetoresistance effect (TMR) described in Non-Patent Documents 1 and 2 occurs. Furthermore, when strain is applied to the strain gauge, the spacing between the metal particles changes in response to the deformation of the nanogranular structure film, resulting in different manifestations of TMR. With the conventional materials described in Non-Patent Documents 1 and 2, high-order tunneling only occurs at extremely low temperatures close to the temperature of liquid helium. However, with the strain gauge of the second aspect of the present invention, high-order tunneling occurs at room temperature, thereby further improving the gauge factor based on changes in TMR in the presence of a magnetic field even at room temperature, and thus further improving its practicality.
[0010] 1 is a diagram illustrating the configuration of a strain gauge as an embodiment of the first and second aspects of the present invention; 2 is a diagram illustrating the microstructure of a resistor; 3 is a diagram illustrating the relationship between the atomic ratio a+b+c of the resistor of the first aspect of the present invention and the gauge factor of the strain gauge; 4 is a diagram illustrating the relationship between the atomic ratio a+b+c of the resistor of the second aspect of the present invention and the change in TMR ratio due to strain application;
[0011] First Embodiment A strain gauge according to an embodiment of the present invention shown in FIG. 1 includes a substrate 1 and a resistor 2 .
[0012] The substrate 1 is made of a flexible insulating material such as glass, quartz glass, a surface-oxidized Si wafer, or epoxy resin, and is formed, for example, in the shape of a substantially rectangular plate. Alternatively, the substrate 1 may be made of metal, with an insulating thin film formed on at least one of its main surfaces, such as polyimide, an oxide such as Al2O3, a fluoride such as MgF2, or an epoxy resin. A reference mark 12 (such as a center mark) is provided on one of the main surfaces of the substrate 1, and serves as a target for the position and orientation of the strain gauge (resistor 2).
[0013] The resistor 2 is formed on one main surface of the substrate 1 and is composed of a nanogranular structure film having a predetermined gauge pattern. For example, as shown in Fig. 1, the resistor 2 has a plurality of linear portions 21 that extend substantially linearly in the longitudinal direction of the substrate 1 from one gauge tab 20 to the other gauge tab 20 while folding back at a distal folded tab 22 and a proximal folded tab 24. A pair of gauge leads 4 are connected to each of the pair of gauge tabs 20. The gauge pattern of the resistor 2 may be modified in various ways.
[0014] 2, the resistor 2 is made of a nano-granular structure film in which nanometer-sized metal particles Q1 are dispersed and arranged approximately uniformly in an insulating matrix Q2. The thickness of the nano-granular structure film is, for example, 0.1 to 10.0 μm.
[0015] The nanogranular structure film is a film having a general formula L 100-a-b-c M a F b O c (L: one or more metal elements, M: one or more elements selected from Li, Mg, Al, Ca, Sr, Ba, Gd, and Y, F: fluorine, O: oxygen, 12.0≦a≦33.0, 17.0≦b≦70.0, 0≦c≦1.0, 50.0≦a+b+c≦90.0). The metal particles Q1 have an average particle size of 1.0 to 5.0 nm and are distributed in an insulating matrix Q2 consisting of a fluoride or a fluoride and an oxide of M at an average particle spacing of 0.2 to 0.6 nm.
[0016] In the first embodiment, the metal particles Q1 are particles of one or more types of metal selected from Pt, Au, Ag, and Cu.
[0017] An insulating protective layer or film (e.g., SiO2, Al2O3, etc.) may be provided on one main surface of the substrate 1 so as to cover the resistor element 2.
[0018] (Manufacturing Method) The resistor 2 constituting the strain gauge is formed on one main surface of the substrate 1 by sputtering or using an RF sputtering film-forming device. A target of at least one non-magnetic metal element selected from Pt, Au, Ag, and Cu and a target of a fluoride (or a fluoride and an oxide) of one or more elements selected from Li, Mg, Al, Ca, Sr, Ba, Gd, and Y are simultaneously sputtered. The composition of the resistor 2 is adjusted by the area ratio and number of Pt, Au, Ag, or Cu chips placed on the target facing the substrate 1. This results in a nanogranular structure film in which nanometer-sized metal particles are dispersed in a matrix made of fluoride.
[0019] Ar gas or a mixed gas of Ar and O2 (0.1 to 10%) is used for sputtering. The film thickness is controlled by adjusting the film formation time, resulting in a film thickness of approximately 0.3 to 5.0 μm. The substrate is indirectly water-cooled or controlled to a temperature within the range of 100 to 800°C, the sputtering pressure during film formation is controlled to 1 to 60 mTorr, and the sputtering power is adjusted within the range of 50 to 350 W.
[0020] Second Embodiment Similar to the strain gauge according to the first embodiment of the present invention, the strain gauge according to the second embodiment of the present invention includes a substrate 1 and a resistor 2 (see FIG. 1). The resistor 2 is formed of a nano-granular structure film in which nanometer-sized metal particles Q1 are dispersed substantially uniformly in an insulating matrix Q2 (see FIG. 2). The thickness of the nano-granular structure film is, for example, 0.1 to 10.0 μm.
[0021] The nanogranular structure film is a film having a general formula L 100-a-b-c M a F b O c(L: one or more metal elements, M: one or more elements selected from Li, Mg, Al, Ca, Sr, Ba, Gd, and Y, F: fluorine, O: oxygen, 12.0≦a≦33.0, 17.0≦b≦70.0, 0≦c≦1.0, 50.0≦a+b+c≦90.0). The metal particles Q1 have an average particle size of 1.0 to 5.0 nm and are distributed in an insulating matrix Q2 consisting of a fluoride or a fluoride and an oxide of M at an average particle spacing of 0.2 to 0.6 nm.
[0022] The second embodiment differs from the first embodiment in that the metal particles Q1 are magnetic metal particles of one or more types selected from Fe, Co, and Ni.
[0023] The strain gauge of the second embodiment is manufactured in the same manner as the strain gauge of the first embodiment.
[0024] (Example) A SiO2 (synthetic quartz) or non-alkali glass substrate having a length of 10 to 50 mm, a width of 10 to 50 mm, and a thickness of 0.5 to 1.0 mm was used as the substrate 1. 100-a-b-c M a F b O c As the resistor 2 having the composition represented by the formula (1), a nanogranular thin film having a thickness of 1.0 to 3.0 μm was formed in the configuration shown in Fig. 1. In this way, the strain gauge of the example was fabricated.
[0025] Table 1 summarizes the configurations of the nanogranular thin films constituting the strain gauges of Examples 1 to 10, which were fabricated according to the first embodiment, and the gauge factors of the strain gauges. Table 1 also lists the configuration of the nanogranular thin film constituting the strain gauge of Comparative Example 1, and the gauge factor of the strain gauge.
[0026]
[0027] Figure 3 shows the relationship between the a+b+c of resistor 2 and the gauge factor of each strain gauge in Examples 1 to 10 and Comparative Example 1 when no magnetic field is applied, with circled numbers and filled circles corresponding to the corresponding numbers in each Example. Figure 3 shows that the strain gauges in Examples 1 and 2, in which the a+b+c of resistor 2 is near 70.0, exhibit the highest gauge factor. It is preferable that a+b+c is in the range of 60.0 to 80.0 (see Examples 1, 2, 3, 6, 7, and 10). A value of less than 50.0 (see Comparative Example 1) or more than 90.0 is undesirable, as it is equivalent to or lower than the gauge factor of conventional materials such as Cu-Ni alloys.
[0028] Table 2 summarizes the configuration of the granular thin films constituting the strain gauges of Examples 11 to 20 fabricated according to the second embodiment, as well as the TMR ratios of the strain gauges when strain is applied and when strain is not applied. The TMR ratios were measured with a 1 T magnetic field applied. Strain was applied by bonding the strain gauge shown in Figure 1 to a stainless steel strain element measuring 50 mm wide, 180 mm long, and 1 mm thick. One end of the long side of the strain element was supported and the other end was pressed 5 mm into the strain gauge, bending it. Although compressive stress was applied to the strain gauge, applying tensile stress resulted in a change in the TMR ratio of the same magnitude as when compressive strain was applied, but the sign was reversed.
[0029]
[0030] In Figure 4, the relationship between a+b+c of resistor 2 and the TMR ratio when no strain is applied to resistor 2 (no strain) in a situation where a magnetic field is applied to each strain gauge of Examples 11 to 20 is shown by the circled numbers corresponding to the corresponding number in each Example. In Figure 4, the relationship between a+b+c of resistor 2 and the TMR ratio when strain is applied to resistor 2 (strain) in a situation where a magnetic field is applied to each strain gauge of Examples 11 to 20 is shown by the "x" plots adjacent to the circled numbers. In Figure 4, some of the "x" plots are hidden by the circled numbers and are not displayed.
[0031] The difference between the TMR ratio without strain and the TMR ratio with strain is 1% or more, and the gauge factor converted from the TMR ratio in an applied magnetic field is 20 or more, which is significantly larger than the gauge factor of conventional materials such as Cu-Ni alloys. The composition range (a + b + c) exhibiting a large TMR ratio is preferably in the range of 50.0 to 90.0 (see Examples 11 to 20), more preferably in the range of 65.0 to 85.0 (see Examples 11, 12, 14, 16, 17, and 18), and even more preferably in the range of 68.0 to 80.0 (see Examples 11, 12, 16, and 17). When (a + b + c) is less than 50.0 or exceeds 90.0, TMR is not exhibited or is very small, which is undesirable.
[0032] 1. Substrate 12. Reference mark 2. Resistor 20. Gauge tab 21. Straight section 22. Distal folded tab 24. Proximal folded tab 4. Gauge lead Q1. Metal particles Q2. Insulating matrix.
Claims
1. A strain gauge comprising a substrate and a resistor formed on the surface of the substrate, the resistor being represented by the general formula L 100-a-b-c M a F b O c A strain gauge having a composition represented by the formula: (L: one or more non-magnetic metal elements selected from Pt, Au, Ag, and Cu, M: one or more elements selected from Li, Mg, Al, Ca, Sr, Ba, Gd, and Y, F: fluorine, O: oxygen, 12.0≦a≦33.0, 17.0≦b≦70.0, 0≦c≦1.0, 50.0≦a+b+c≦90.0), and comprising a nanogranular structure film in which metal particles having an average particle size of 1.0 to 5.0 nm represented by L are distributed at an average particle spacing of 0.2 to 0.6 nm in an insulating matrix made of a fluoride or a fluoride and an oxide of M.
2. A strain gauge comprising a substrate and a resistor formed on the surface of the substrate, the resistor being represented by the general formula L 100-a-b-c M a F b O c A strain gauge having a composition represented by the formula: (L: one or more magnetic metal elements selected from Fe, Co, and Ni, M: one or more elements selected from Li, Mg, Al, Ca, Sr, Ba, Gd, and Y, F: fluorine, O: oxygen, 12.0≦a≦33.0, 17.0≦b≦70.0, 0≦c≦1.0, 50.0≦a+b+c≦90.0), and comprising a nanogranular structure film in which metal particles having an average particle size of 1.0 to 5.0 nm represented by L are distributed at an average particle spacing of 0.2 to 0.6 nm in an insulating matrix made of a fluoride or a fluoride and an oxide of M.
3. A strain measuring device comprising the strain gauge according to claim 1 or 2, circuit components constituting a bridge circuit including said strain gauge, and a magnet for applying a magnetic field to said strain gauge.
4. A strain measurement method comprising the steps of: attaching a strain gauge as defined in claim 1 or 2 to an object; applying a magnetic field to the strain gauge using a magnet; and detecting the strain condition in the object according to changes in the electrical resistance of the strain gauge.
Citation Information
Patent Citations
Deformation measuring device and its manufacturing method
JP2007292618A
Nanogranular structure material and method for producing same
WO2022186177A1