Positive electrode for secondary battery, and secondary battery

The use of a positive electrode with specific particle size distributions and a nitrile group-containing rubber dispersant in the secondary battery's positive electrode mixture layer addresses the issue of reduced capacity due to poor dispersibility, resulting in improved capacity and resistance characteristics.

WO2024248039A1PCT designated stage expired Publication Date: 2024-12-05PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD

Patent Information

Application Number
PCT/JP2024/019703
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-29
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The existing methods for increasing the capacity of secondary batteries by filling gaps in the positive electrode mixture layer with smaller active material particles often result in reduced dispersibility, leading to poor conductive path formation and decreased capacity due to uneven distribution and increased resistance.

Method used

A positive electrode with a mixture layer containing a first metal composite oxide and a second metal composite oxide, where the volume-based median diameters satisfy D1 > D2, and the compressive strength of the first oxide particles is less than that of the second, using a nitrile group-containing rubber as a dispersant to improve dispersibility and prevent particle crushing during the manufacturing process.

Benefits of technology

This approach enhances the dispersibility of the positive electrode mixture, leading to a high-capacity battery with reduced resistance and suppressed side reactions, maintaining the integrity of active material particles and improving charge/discharge cycle characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024019703_05122024_PF_FP_ABST
    Figure JP2024019703_05122024_PF_FP_ABST
Patent Text Reader

Abstract

This positive electrode for a secondary battery comprises: a positive-electrode current collector; and a positive-electrode mixture layer provided on a surface of the positive-electrode current collector. The positive-electrode mixture layer includes: a positive-electrode active material; a carbon conductive assisting agent; and a dispersant. The positive-electrode active material includes: a first metal composite oxide having a first particle size distribution; and a second metal composite oxide having a second particle size distribution. A volume-basis median diameter D1 of the first metal composite oxide and a volume-basis median diameter D2 of the second metal composite oxide satisfy D1 > D2. The dispersant contains a nitrile group-containing rubber.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode for secondary battery and secondary battery CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This disclosure claims the benefit of priority to Japanese Patent Application No. 2023-090332, filed on May 31, 2023, in the Japan Patent Office, the entire contents of which are incorporated herein by reference.

[0002] The present disclosure relates to a positive electrode for a secondary battery and a secondary battery.

[0003] Patent Document 1 describes a lithium-nickel composite oxide comprising: "a first lithium-nickel composite oxide having a volume particle distribution of 3.0 μm≦D25≦10.0 μm, 5.0 μm≦D50≦20.0 μm, and 10.0 μm≦D75≦25.0 μm as measured by a particle size analyzer; and a second lithium-nickel composite oxide having a volume particle distribution of 0.01 μm≦D25≦5.0 μm, 1.0 μm≦D50≦10.0 μm, and 5.0 μm≦D75≦15.0 μm as measured by a particle size analyzer; the first lithium-nickel composite oxide has a higher nickel atom content, which is the proportion of nickel atoms in the chemical formula, than the second lithium-nickel composite oxide, and a positive electrode active material. The present invention proposes a positive electrode active material for a lithium battery, characterized in that the content of the first lithium nickel composite oxide is 80 to 97 wt % and the content of the second lithium nickel composite oxide is 3 to 20 wt % based on the total weight of the material, the first lithium nickel composite oxide has a volume particle distribution of 5.0 μm≦D25≦9.0 μm, 8.0 μm≦D50≦13.0 μm, and 13.0 μm≦D75≦18.0 μm, and the second lithium nickel composite oxide has a volume particle distribution of 1.0 μm≦D25≦3.0 μm, 2.0 μm≦D50≦7.0 μm, and 6.0 μm≦D75≦10.0 μm.

[0004] Patent No. 5868604

[0005] To increase the capacity of secondary batteries, researchers have investigated filling the gaps between larger active material particles with smaller active material particles in the positive electrode mixture layer to increase the density of the positive electrode mixture layer. However, simply mixing active material particles of different particle sizes can reduce the dispersibility of the positive electrode mixture, leading to poor formation of conductive paths and a decrease in capacity. In particular, when the mass of the positive electrode mixture layer supported per unit area of ​​the positive electrode current collector is large, the distribution of the additive is likely to become non-uniform during drying of the positive electrode slurry in which the positive electrode mixture is dispersed in a liquid component (dispersion medium) during the manufacturing process of the positive electrode mixture layer, resulting in a significant decrease in capacity. Therefore, the dispersibility of the positive electrode mixture is important.

[0006] One aspect of the present disclosure relates to a positive electrode for a secondary battery, including: a positive electrode current collector; and a positive electrode mixture layer provided on a surface of the positive electrode current collector, the positive electrode mixture layer including a positive electrode active material, a carbon conductive additive, and a dispersant, the positive electrode active material including a first metal composite oxide having a first particle size distribution and a second composite metal oxide having a second particle size distribution, a volume-based median diameter D1 of the first metal composite oxide and a volume-based median diameter D2 of the second metal composite oxide satisfying D1 > D2, a compressive strength F1 of particles of the first metal composite oxide and a compressive strength F2 of particles of the second composite oxide satisfying F1 < F2, and the dispersant includes a nitrile group-containing rubber.

[0007] Another aspect of the present disclosure relates to a secondary battery including the above-described positive electrode for secondary batteries, a separator, a negative electrode facing the positive electrode with the separator interposed therebetween, and an electrolyte solution.

[0008] According to the present disclosure, a high-capacity positive electrode for a secondary battery can be obtained by improving the dispersibility of the positive electrode mixture. The novel features of the present invention are set forth in the appended claims, but the present invention, both in terms of structure and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings.

[0009] 1 is a schematic vertical cross-sectional view of a secondary battery according to an embodiment of the present disclosure.

[0010] The following describes embodiments of the present disclosure using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values ​​and materials may be exemplified, but other numerical values ​​and materials may be applied as long as the effects of the present disclosure are obtained. In this specification, the term "numerical value A to numerical value B" includes numerical value A and numerical value B and can be read as "numerical value A or greater and numerical value B or less." In the following description, when lower and upper limits of numerical values ​​related to specific physical properties or conditions are exemplified, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not greater than the upper limit. In the following description, when examples of components or methods are listed, only one of the listed examples may be used, or multiple of the listed examples may be used in combination, unless otherwise specified.

[0011] (Positive electrode for secondary battery) The positive electrode according to this embodiment (hereinafter also referred to as "positive electrode (P)") is a positive electrode used in secondary batteries such as non-aqueous electrolyte secondary batteries. The positive electrode (P) includes a positive electrode current collector and a positive electrode mixture layer. The positive electrode mixture layer is provided on the surface of the positive electrode current collector. The positive electrode mixture layer is composed of a positive electrode mixture containing a positive electrode active material, a carbon conductive additive, and a dispersant.

[0012] The positive electrode active material includes a first metal composite oxide having a first particle size distribution and a second composite metal oxide having a second particle size distribution. The volume-based median diameter D1 of the first metal composite oxide and the volume-based median diameter D2 of the second metal composite oxide satisfy the relationship D1 > D2. That is, the first metal composite oxide constitutes active material particles with a large particle size, and the second metal composite oxide constitutes active material particles with a small particle size.

[0013] Increasing the charging voltage is a known method for increasing the capacity of secondary batteries, but continuous exposure to high charging voltages can cause cracking of active material particles, which can lead to side reactions such as gas generation and metal elution from the grain boundaries, resulting in reduced durability.

[0014] On the other hand, when a mixture of large and small active material particles is filled in the positive electrode mixture layer, the small active material particles fill the gaps between the large active material particles. This reduces the gaps in the positive electrode mixture layer and increases the content of the positive electrode active material. This, in principle, can increase the capacity of the secondary battery.

[0015] However, if the dispersion of the active material particle mixture is uneven, not only will the content of the positive electrode active material in the positive electrode mixture layer not be sufficiently increased, but the conductive path may not be properly formed, resulting in a decrease in capacity. Furthermore, localized regions with different physical properties may form in the positive electrode mixture layer, reducing the performance of the positive electrode. For example, localized regions with high and low reactivity may be formed. This also results in differences in the degree of electrolyte migration. As a result, the resistance of the positive electrode mixture layer increases. Furthermore, the potential of the positive electrode (P) varies depending on the region (potential variation occurs). Potential variation in the positive electrode (P) increases the amount of gas generated by side reactions.

[0016] In the manufacturing process of the positive electrode mixture layer, a positive electrode mixture is dispersed in a liquid component (dispersion medium) to prepare a positive electrode slurry. To improve the dispersibility of the active material particles in the positive electrode mixture layer, it is important to improve the dispersibility of the positive electrode mixture in the liquid component (dispersion medium) in the positive electrode slurry. In this regard, the positive electrode mixture layer of the positive electrode (P) is composed of a positive electrode mixture with improved dispersibility.

[0017] (Positive electrode active material) The first metal composite oxide having a first particle size distribution (hereinafter also referred to as "first particle group") and the second composite metal oxide having a second particle size distribution (hereinafter also referred to as "second particle group") contained in the positive electrode active material may have volume-based median diameters D1 and D2 that satisfy D1 > D2, but preferably have the following configuration.

[0018] First, the volume-based median diameter (D) may be measured by separating the positive electrode active material from the positive electrode mixture layer, or may be determined by image analysis of a cross-sectional SEM image of the positive electrode mixture layer. Either method for determining the median diameter (D) will result in approximately the same (no significant difference) median diameter.

[0019] When separating the positive electrode active material from the positive electrode mixture layer, the positive electrode mixture layer may be peeled off from the positive electrode (P), immersed in an appropriate solvent to dissolve or swell components other than the active material particles, such as dispersants, and then separated by centrifugation. This procedure may be repeated one or more times. When a sample of the separated positive electrode active material is analyzed using a laser diffraction / scattering particle size distribution analyzer, a volume-based particle size distribution is obtained. The particle diameter of the peak with the largest area in the obtained particle size distribution is the median diameter of either the first particle group or the second particle group, and the particle diameter of the peak with the second largest area is the median diameter of the other. The larger median diameter is D1, and the smaller median diameter is D2. If the peaks overlap, peak separation can be performed using image analysis. Furthermore, the volume V1 of the first particle group and the volume V2 of the second particle group can be calculated from the area of ​​each peak.

[0020] When analyzing a cross-sectional SEM image of the positive electrode mixture layer, first, the positive electrode mixture layer and the positive electrode current collector are simultaneously cut along the width direction of the positive electrode to obtain a cross-sectional sample of the positive electrode in the thickness direction. At this time, the cross-section may be processed using a cross-section polisher (CP) to obtain the cross-sectional sample. Next, the cross-section of the positive electrode mixture layer in the cross-sectional sample is observed using a scanning electron microscope (SEM).

[0021] The area enclosed by the outline is determined from the outline image of the active material particle in the SEM image. The diameter of a circle (equivalent circle) having the same area as the area enclosed by the outline of the active material particle is determined and used as the particle size of each particle i. The volume of a sphere having the same diameter as the equivalent circle is then considered to be the volume Vi of each particle i. A volume-based particle size distribution can be obtained by determining the diameter and volume of the equivalent circle of any 100 or more particles (preferably 1000 or more). From the obtained particle size distribution, the median diameters D1 and D2, the volume V1 of the first particle group, and the volume V2 of the second particle group can be calculated, similar to the case of separating the positive electrode active material from the positive electrode mixture layer.

[0022] The D1 and D2 that satisfy D1>D2 may have a D1 / D2 ratio of, for example, 2 or more and 6 or less, or 3 or more and 5 or less.

[0023] D1 is, for example, 8 μm or more, or may be 10 μm or more, 11 μm or more, 12 μm or more, or 15 μm or more. D1 may also be 30 μm or less, 25 μm or less, or 20 μm or less. As described above, D1 is preferably in the range of 8≦D1 (μm)≦30.

[0024] D2 may be 10 μm or less, 8 μm or less, 6 μm or less, or 5 μm or less. From the viewpoint of improving charge / discharge cycle characteristics, D2 may be 1 μm or more, or 3 μm or more. As described above, D2 is preferably in the range of 1≦D2(μm)≦10.

[0025] The active material particles are usually, but not limited to, mainly composed of aggregates of primary particles. The particle size of the primary particles is, for example, 0.2 μm to 5 μm. The positive electrode may contain only aggregates of primary particles, but may also be partially or entirely composed of primary particles.

[0026] Here, in the positive electrode (P), the compressive strength (single particle breaking strength) F1 of the first metal composite oxide particles and the compressive strength F2 of the second composite oxide particles satisfy the relationship F1<F2. Generally, F1≧F2 is often the case. Active material particles with a small particle size have a large BET specific surface area, which makes it easy for side reactions to increase on the surface of the active material particles. In addition, in the manufacturing process of the positive electrode mixture layer, a positive electrode slurry is applied to the surface of the positive electrode current collector, the coating is dried, and then the coating is rolled. During rolling, small active material particles are crushed and filled to fill the gaps between large active material particles. This blocks the electrolyte flow path, which tends to reduce the capacity retention rate during charge / discharge cycles, including rapid charging.

[0027] On the other hand, when F1<F2 is satisfied, crushing of small-sized active material particles is suppressed when the coating film is rolled, the overall BET specific surface area of ​​the positive electrode active material is less likely to increase, the degree to which gaps between large-sized active material particles are blocked is also mitigated, and side reactions are suppressed. Furthermore, suppressing crushing of small-sized active material particles makes it less likely that regions with different physical properties will be formed locally in the positive electrode mixture layer, and fluctuations in the potential of the positive electrode (P) are also suppressed.

[0028] F1 / F2 may be less than 1, may be 0.96 or less, preferably 0.6 or less, or may be 0.2 or less, may be 0.1 or more and 0.96 or less, or may be 0.1 or more and 0.9 or less.

[0029] The compressive strength (single particle breaking strength) can be measured using a commercially available measuring device (for example, a microcompression tester (MCT-W201) manufactured by Shimadzu Corporation) according to the following procedure.

[0030] (1) Particles of the positive electrode active material are spread on the lower pressure plate (SKS flat plate) of the measuring device. (2) Particles to be measured are selected using an optical microscope, and the particle diameter is measured. At this time, particles as close as possible to the median diameter D1 or D2 are selected. The particle diameter here is the circle-equivalent diameter (the diameter of a circle having the same area as the particle) determined using an image of the particle taken under an optical microscope.

[0031] (3) A flat diamond indenter having a diameter of 50 μm is used as the upper pressure tool, and only one particle selected as the sample is placed between the upper pressure tool and the lower pressure plate.

[0032] (4) The upper pressure probe is slowly lowered, and from the point where it comes into contact with the sample (the lowering speed changes), a load is applied at a constant acceleration (specifically, a displacement speed of 2.7 mN / sec).

[0033] (5) The relationship between the load and the deformation of the sample is measured, and the point at which the deformation of the sample changes suddenly (the inflection point of the load-deformation profile) is taken as the breaking point, and the breaking strength is calculated from the load and particle diameter at that time using the following formula: Breaking strength is calculated as the average of five measurements.

[0034] St = 2.8P / πd 2 St: Breaking strength [MPa or N / mm 2 ] P: Load [N] d: Particle diameter [mm]

[0035] The ratio of the volume V1 of the first particle group to the sum of the volume V1 of the first particle group and the volume V2 of the second particle group (100 × V1 / (V1 + V2)) may be, for example, 60 vol% or more and 80 vol% or less, or 70 vol% or more and 80 vol% or less.

[0036] The compositions of the first and second metal composite oxides are independent of each other and may be the same or different. Even if the compositions are the same, the volume-based median diameter (D) and compressive strength can be arbitrarily controlled by adjusting the synthesis conditions of the positive electrode active material.

[0037] The first metal composite oxide and the second metal composite oxide each have a composition represented by the general formula: Li y Ni x M (1-x) O 2 In the above general formula, 0.8≦x and 0<y≦1.2 are satisfied, and M is at least one element selected from the group consisting of Co, Mn, Al, Fe, Zr, Ti, Sr, Ca, and B.

[0038] A composite oxide having a composition represented by the above general formula has a high Ni content and is therefore promising as a high-capacity positive electrode active material. More preferably, the above general formula satisfies 0.85≦x.

[0039] Such a composite oxide containing Ni and Li (hereinafter also referred to as "composite oxide (N)") is advantageous in terms of achieving high capacity and low cost. From the viewpoint of obtaining high capacity, the proportion of Ni in the metal elements other than Li contained in the composite oxide (N) is, as described above, preferably 80 atomic % or more, and may be 85 atomic % or more, or may be 90 atomic % or more. The proportion of Ni in the metal elements other than Li is preferably, for example, 95 atomic % or less.

[0040] The composite oxide (N) may be a lithium transition metal composite oxide having a layered rock salt crystal structure. The composite oxide (N) may contain Co, or at least one of Mn and Al. Co, Mn, and Al contribute to stabilizing the crystal structure of the composite oxide (N) having a high Ni content. However, from the viewpoint of reducing production costs, a lower Co content is desirable, and it is preferable that the composite oxide (N) does not contain Co. From the viewpoint of reducing production costs, it is desirable that the proportion of Co in the metal elements other than Li in the composite oxide (N) be kept below 2 atomic %.

[0041] The composite oxide (N) is, for example, a compound represented by the general formula: Li y Ni1-x1-x2-x3-zCo x1 Mnx2 Al x3 Me z O 2+β However, the general formula satisfies 0.9≦y≦1.2, 0≦x1≦0.1, 0≦x2≦0.5, 0≦x3≦0.1, 0≦z≦0.1, 0.8≦1−x1−x2−x3−z, and −0.05≦β≦0.05, and Me is an element other than Li, Ni, Mn, Al, Co, and oxygen.

[0042] As Me, from the viewpoint of stabilizing the crystal structure of the composite oxide (N), at least one selected from the group consisting of Nb, Zr, B, Mg, Fe, Cu, Zn, Sn, Na, K, Ba, Sr, Ca, W, Mo, Si, Ti, Fe, and Cr can be used.

[0043] The contents of the elements constituting the active material particles can be measured using an inductively coupled plasma atomic emission spectroscopy (ICP-AES), an electron probe microanalyzer (EPMA), an energy dispersive X-ray spectroscopy (EDX), or the like.

[0044] The positive electrode current collector may be, for example, in the form of a sheet, and may have a thickness of, for example, 5 μm to 20 μm. Examples of the material for the positive electrode current collector include stainless steel, aluminum, an aluminum alloy, and titanium.

[0045] The first metal composite oxide particles and the second metal composite oxide particles may have a surface modification layer containing a boron compound. When small-sized active material particles (second metal composite oxide particles) are used, forming a surface modification layer on the active material particles makes it possible to more effectively avoid adverse effects caused by their small size (for example, side reactions caused by an increase in specific surface area).

[0046] (Carbon Conductive Aid) The positive electrode mixture of the positive electrode (P) may contain a carbon conductive aid (C) to enhance its electronic conductivity. By containing the carbon conductive aid (C), the electronic conductivity of the positive electrode mixture is improved, and the resistance of the secondary battery is improved.

[0047] (Dispersant) The positive electrode mixture of the positive electrode (P) contains a specific blend of dispersant (hereinafter also referred to as "dispersant (D)") as an auxiliary agent for improving its dispersibility. Specifically, the dispersant (D) contains a nitrile group-containing rubber. The inclusion of the nitrile group-containing rubber in the dispersant (D) significantly improves the dispersibility of the positive electrode mixture in the liquid component. Furthermore, the dispersant (D) is effective even when used in a very small amount relative to the active material particles. Furthermore, the dispersant (D) may further contain at least one of a polyvinylpyrrolidone resin and a cellulose resin. The inclusion of these resins further improves the dispersibility of the positive electrode mixture in the liquid component.

[0048] There are many dispersants for improving the dispersibility of the positive electrode mixture. Therefore, there are countless combinations of dispersants, and the effects of these combinations have not been fully investigated. Furthermore, it is difficult for a person skilled in the art to predict the effects that will be obtained when two or more dispersants are combined. If the effects of these combinations could be predicted, the optimal combination could be determined without experimentation. However, in reality, it is difficult to predict the effects of these combinations. In other words, the composition of dispersant (D) containing a nitrile group-containing rubber, a polyvinylpyrrolidone resin, and a cellulose resin is a combination that even a person skilled in the art would not easily find.

[0049] (Nitrile Group-Containing Rubber) Examples of nitrile group-containing rubbers include copolymers of monomers containing acrylonitrile and diene (e.g., butadiene). Examples of nitrile group-containing rubbers include acrylonitrile-based rubbers such as acrylonitrile-butadiene rubber (NBR) and hydrogenated acrylonitrile-butadiene rubber (H-NBR).

[0050] The weight average molecular weight of the nitrile group-containing rubber may be in the range of 5,000 to 500,000. In terms of enhancing the effects of the configuration of the present disclosure, the weight average molecular weight of the nitrile group-containing rubber may be in the range of 10,000 to 300,000.

[0051] The nitrile group-containing rubber has the effect of suppressing the progression of side reactions that can be increased by using a second particle group that satisfies D1 > D2. Side reactions occur at the interface between the electrolyte and the active material particles, and are particularly pronounced when the active material particles are in a charged state. In a secondary battery during charging, the potential of the positive electrode active material is not necessarily constant, and side reactions are promoted around active material particles that have locally high potentials. The nitrile group-containing rubber has a high effect of improving the dispersibility of the positive electrode mixture and suppressing potential variations. Therefore, the effect of suppressing side reactions becomes apparent when a second particle group with a large specific surface area is used.

[0052] (Polyvinylpyrrolidone Resin) The polyvinylpyrrolidone resin is at least one selected from the group consisting of polyvinylpyrrolidone and polyvinylpyrrolidone derivatives. Examples of polyvinylpyrrolidone derivatives include polymers in which the hydrogen atoms of polyvinylpyrrolidone are substituted with other substituents, such as alkylated polyvinylpyrrolidone. As the polyvinylpyrrolidone resin, polyvinylpyrrolidone alone may be used, or a copolymer of vinylpyrrolidone and other monomolecules may be used. Examples of other monomolecules include styrene-based and vinyl acetate-based monomolecules.

[0053] The weight average molecular weight of the polyvinylpyrrolidone resin may be in the range of 1,000 to 2,000,000. In terms of enhancing the effects of the configuration of the present disclosure, the weight average molecular weight of the polyvinylpyrrolidone resin may be in the range of 5,000 to 1,000,000.

[0054] (Cellulose Resin) The cellulose resin may be a cellulose derivative. Examples of the cellulose derivative include alkyl celluloses such as methyl cellulose and ethyl cellulose, hydroxyalkyl cellulose, and alkali metal salts thereof. Examples of alkali metals that form alkali metal salts include potassium and sodium. Among these, methyl cellulose, ethyl cellulose, and hydroxypropyl methyl cellulose are preferred.

[0055] The weight average molecular weight of the cellulose derivative may be in the range of 1,000 to 1,000,000 (e.g., in the range of 10,000 to 1,000,000). In terms of enhancing the effects of the configuration of the present disclosure, the weight average molecular weight of the cellulose derivative may be in the range of 10,000 to 200,000.

[0056] In the dispersant (D), the amount of the cellulose derivative per 100 parts by mass of the nitrile group-containing rubber is preferably in the range of 10 to 400 parts by mass (for example, in the range of 30 to 400 parts by mass or in the range of 50 to 300 parts by mass). By setting the amount in the range of 10 to 400 parts by mass, particularly high effects can be obtained, as shown in the examples.

[0057] In the dispersant (D), the amount of polyvinylpyrrolidone resin per 100 parts by mass of the nitrile group-containing rubber may be in the range of 10 to 400 parts by mass (for example, in the range of 20 to 200 parts by mass). By setting the amount in the range of 10 to 400 parts by mass, particularly high effects can be obtained, as shown in the examples.

[0058] (Effects of Dispersant (D)) By using the dispersant (D), the dispersibility of the positive electrode mixture is significantly improved, and a positive electrode having a high active material density, low resistance, and suppressed side reactions can be obtained. When a positive electrode active material satisfying F1 < F2 is used, the effect is particularly remarkable. For example, when the active material density of the positive electrode mixture layer is 3.45 g / cm 3 or more, 3.55 g / cm 3 or more, or 3.6 g / cm 3 Even in this case, a positive electrode having low resistance and suppressed side reactions can be obtained.

[0059] Polyvinylpyrrolidone resin has a certain effect in improving dispersibility due to its good wettability with carbon conductive additives, but its electrochemical stability as a single substance is inferior to that of other dispersants, so its use alone tends to result in reduced long-term dispersion stability.On the other hand, the use of a combination of polyvinylpyrrolidone resin, cellulose resin, and nitrile group-containing rubber provides long-term dispersion stability.

[0060] However, since cellulose resin has low affinity to the dispersion medium of the positive electrode mixture (especially aprotic polar solvents), nitrile group-containing rubber and polyvinylpyrrolidone resin work effectively to maximize its effectiveness, thereby achieving both high dispersibility and long-term dispersion stability.

[0061] The cellulose resin and the nitrile group-containing rubber are chemically stable and are less susceptible to denaturation by the lithium component contained in the active material particles. This further improves the long-term dispersion stability of the positive electrode slurry. In particular, positive electrode active materials with a high Ni content are prone to side reactions. Therefore, the effect of the dispersant (D) is particularly significant.

[0062] (Dispersion) The carbon conductive additive (C) and the dispersant (D) may be used as a dispersion (DL) in combination with a dispersion medium. The dispersion (DL) may contain one or more of the above-mentioned dispersants, or may contain other dispersants. Such other dispersants may be known dispersants. However, the proportion of other dispersants in the total dispersants is small, for example, 30% by mass or less, more preferably 10% by mass or less.

[0063] The amount of the dispersion liquid (DL) used is reflected in the ratio of the components in the positive electrode slurry. The ratios of the components exemplified for the positive electrode mixture can be applied to the ratios of the components in the positive electrode slurry. The content of the dispersant (D) in the positive electrode mixture is, for example, 1.0 mass% or less, and may be 0.01 parts by mass or more and 1 part by mass or less, or 0.05 parts by mass or more and 0.5 parts by mass or less, relative to 100 parts by mass of the positive electrode active material.

[0064] (Binder) The positive electrode mixture layer may further contain a vinylidene fluoride resin. The vinylidene fluoride resin functions as a binder that binds active material particles together or between the active material particles and the positive electrode current collector. The vinylidene fluoride resin contains vinylidene fluoride units as monomer units. The vinylidene fluoride resin may be a copolymer of vinylidene fluoride and other monomers. Examples of vinylidene fluoride resins include polyvinylidene fluoride (PVDF) and polymers of vinylidene fluoride units and other monomer units (such as tetrafluoroethylene and hexafluoropropylene). The content of vinylidene fluoride units in the polymer is, for example, 30 mol% or more.

[0065] The weight-average molecular weight of the vinylidene fluoride resin may be 800,000 or more, 1,000,000 or more, 1,100,000 or more, 1,200,000 or more, or 1,300,000 or more. The weight-average molecular weight of the vinylidene fluoride resin may be 2,000,000 or less, or 1,800,000 or less. By making the weight-average molecular weight 1,000,000 or more, a high effect as a binder can be obtained with a small amount.

[0066] The amount of vinylidene fluoride resin relative to 100 parts by mass of the dispersant (D) may be, for example, in the range of 50 to 2000 parts by mass (e.g., in the range of 100 to 1000 parts by mass).

[0067] In the positive electrode mixture layer, the amount of vinylidene fluoride resin relative to 100 parts by mass of the positive electrode active material may be, for example, 0.1 parts by mass or more, or 0.5 parts by mass or more, and may be 2.0 parts by mass or less, or 1.5 parts by mass or less.

[0068] (Carbon nanotubes) The carbon conductive additive preferably contains carbon nanotubes (hereinafter also referred to as "CNTs"). By using CNTs as the carbon conductive additive, the potential variation in the positive electrode can be further significantly suppressed. Furthermore, by adding only a small amount of CNTs to the positive electrode mixture, the resistance of the positive electrode mixture layer can be significantly reduced.

[0069] The positive electrode mixture layer may contain a carbon conductive additive other than CNT. Examples of such a carbon conductive additive include conductive carbon materials such as graphene and carbon black (acetylene black, ketjen black, furnace black, etc.). The proportion of CNT in all carbon materials (conductive additives) is, for example, 10% by mass or more, preferably in the range of 30 to 100% by mass (e.g., 50 to 100% by mass).

[0070] In the positive electrode mixture layer, the amount of CNTs relative to 100 parts by mass of the positive electrode active material may be 0.01 parts by mass or more, or 0.04 parts by mass or more, or may be 1 part by mass or less, or 0.5 parts by mass or less.

[0071] The length (average length) of the CNTs may be 1 μm or more. In this case, the average aspect ratio of the CNTs (ratio of the fiber length to the diameter) becomes extremely large. CNTs with a large aspect ratio tend to come into contact with the positive electrode active material and the positive electrode current collector. Furthermore, CNTs have excellent electrical conductivity. Therefore, the use of CNTs can significantly reduce the direct current resistance (DCR) of the battery.

[0072] The average length of the CNTs is preferably 1 μm or more from the viewpoint of increasing the conductivity in the positive electrode mixture layer. On the other hand, the upper limit of the length of the CNTs is not particularly limited, but it is preferable that it is not too large compared to the particle size of the positive electrode active material. The average length of the CNTs may be 1 μm or more or 5 μm or more, and may be 20 μm or less or 10 μm or less. The CNTs present in the positive electrode mixture layer may be present in a bundle of multiple CNTs. The length of a single CNT present in the bundle of CNTs is used to calculate the above average length.

[0073] The average length of CNTs is determined by image analysis using a scanning electron microscope (SEM). The average length of CNTs is determined by measuring the lengths of 100 randomly selected CNTs and taking the arithmetic mean. The length refers to the length of the CNTs when stretched linearly.

[0074] The diameter (average diameter) of the CNTs may be 20 nm or less, 15 nm or less, or 1 nm or more. By setting the average diameter to 20 nm or less, a high effect can be obtained with a small amount.

[0075] The average diameter of CNTs is determined by image analysis using a transmission electron microscope (TEM). The average diameter of CNTs can be measured by the following method. First, 100 CNTs are randomly selected, and the diameter (outer diameter) of each is measured at one arbitrary point. The average diameter is then determined by arithmetically averaging the measured diameters.

[0076] The CNTs may be either single-walled CNTs (SWCNTs) or multi-walled CNTs (MWCNTs). Examples of multi-walled CNTs include double-walled CNTs, triple-walled CNTs, and CNTs with four or more walls. The positive electrode mixture layer preferably contains single-walled CNTs and / or multi-walled CNTs. The multi-walled CNTs contained in the positive electrode mixture layer may be one type of multi-walled CNT or multiple types of multi-walled CNTs with different numbers of layers.

[0077] The BET specific surface area of ​​CNT is 200 m 2 / g or more, 250m 2 / g or more, or 300m 2 The upper limit of the BET specific surface area is not particularly limited, but it is preferably 1000 m 2 The BET specific surface area may be 200 m / g or less. 2 By setting the specific surface area of ​​CNT to 1 / g or more, it is possible to suppress the potential variation of the active material in the mixture layer even with a small amount of addition. The BET specific surface area of ​​CNT can be measured by nitrogen adsorption method. However, there is generally a correlation between the BET specific surface area of ​​CNT and the fiber diameter and fiber length. Specifically, if the fiber diameter is 10 nm and the fiber length is 1 μm, the BET specific surface area is 200 m 2 / g or more and 300m 2 / g or less. Therefore, even in the state of a battery, the BET specific surface area of ​​the CNTs can be calculated with high accuracy.

[0078] Although it is usually difficult to highly disperse CNTs, the use of dispersant (D) significantly improves the dispersibility of CNTs. Therefore, even if the amount of CNTs added to the positive electrode mixture is small, the conductivity of the positive electrode mixture layer can be improved and the resistance of the positive electrode mixture layer can be significantly reduced. From the perspective of increasing the capacity of secondary batteries, it is desirable to reduce the amount of conductive additive as much as possible. However, for example, simply reducing the amount of CNT added reduces the dispersibility of the positive electrode mixture, resulting in insufficient formation of conductive paths, resulting in a decrease in the capacity of the positive electrode and aggregation of the CNTs. On the other hand, a positive electrode mixture layer containing dispersant (D) is less likely to suffer from such symptoms and significantly contributes to improving the performance of secondary batteries, including increasing their capacity (density).

[0079] (Method for producing positive electrode active material) An example of a method for producing active material particles is described below. The method for producing active material particles includes, for example, a synthesis step, a washing step, a drying step, and an addition step. Note that the active material particles may be produced by a method other than the following production method.

[0080] In the synthesis step, a metal hydroxide containing the metal elements constituting the first or second metal composite oxide is mixed with a Li compound and calcined to obtain particles of the metal composite oxide (lithium transition metal composite oxide). Instead of the metal hydroxide, a metal oxide obtained by heat-treating the metal hydroxide may be used. The volume-based median diameter of the metal hydroxide is preferably 7 μm or less.

[0081] The metal hydroxide can be obtained, for example, by adding dropwise an alkaline solution such as sodium hydroxide to a stirred solution of a metal salt containing the metal element that constitutes the composite oxide particles, adjusting the pH to the alkaline side (e.g., 8.5 to 12.5), and causing precipitation (coprecipitation).

[0082] Examples of Li compounds include Li 2 CO 3 , LiOH, Li 2 O 2 , Li 2 O, LiNO 3 , LiNO 2 , Li 2 SO 4 , LiOH·H 2Examples of suitable metal hydroxides include O, LiH, and LiF. The mixing ratio of the metal hydroxide (metal oxide) and the Li compound is preferably such that the molar ratio of metal elements excluding Li to Li falls within the range of 1:0.98 to 1:1.1.

[0083] The positive electrode active material is LiOH and Li 2 CO 3 The positive electrode active material may contain LiOH and Li 2 CO 3 For example, the total may be 0.2 mass % or more.

[0084] LiOH and Li 2 CO 3 The higher the total content of the alkali components (in other words, the higher the dispersibility of the cathode mixture in the cathode slurry). Therefore, the importance of using a dispersant (D) increases. The alkali components react with binders such as polyvinylidene fluoride, which tends to cause changes in the state of the cathode slurry and destabilize the state of the cathode slurry. The higher the Ni content of the composite oxide constituting the cathode active material, the more difficult it is to control the dispersibility of the cathode mixture in the cathode slurry. 2 CO 3 The total content of the dispersant (D) can be increased, but is at most 1.0 mass %. By using the dispersant (D), destabilization of the positive electrode slurry due to the alkaline component is significantly restricted.

[0085] When mixing a metal hydroxide (metal oxide) with a Li compound, a Ca compound, a Sr compound, an Fe compound, a Cu compound, a Zr compound, an Mg compound, a Si compound, a Cr compound, a Ti compound, an S compound, a fluoride, etc. Examples of Ca compounds include CaO and Ca(OH). 2 , and CaCO 3 Examples of Sr compounds include SrO and Sr(OH). 2 , and SrCO 3 For other elements, oxides, hydroxides, sulfides, and fluorides can be used. In addition, alkaline earth metals and Zr are useful because they are highly effective in reducing resistance.

[0086] A mixture of a metal hydroxide (metal oxide) and a Li compound, etc., is fired, for example, in an oxygen atmosphere (flowing a gas with an oxygen concentration of 80% or more). The firing conditions may include a temperature rise rate of more than 1.0°C / min and less than 5.5°C / min from 450°C to 680°C, and a maximum temperature of 700°C to 850°C. The temperature rise rate from above 680°C to the maximum temperature may be, for example, 0.1°C / min to 3.5°C / min. The maximum temperature may be maintained for 1 hour to 30 hours. This firing process may be a multi-stage firing, and multiple temperature rise rates may be set for each temperature range as long as they are within the above-specified range. The particle size of the single particles can be adjusted by adjusting the firing conditions. For example, the particle size of the single particles can be increased by increasing the maximum temperature.

[0087] In the washing step, the composite oxide particles obtained in the synthesis step are washed with water and dehydrated to obtain a cake-like composition. The washing and dehydration can be performed using known methods and conditions. These steps may be performed within a range that does not cause lithium to leach out of the composite oxide particles and degrade the battery characteristics. Ca compounds, Sr compounds, Fe compounds, Cu compounds, Zr compounds, Mg compounds, Si compounds, Cr compounds, Ti compounds, S compounds, fluorides, etc. may also be added to the cake-like composition.

[0088] In the drying step, the cake-like composition obtained in the washing step is dried to obtain a powdery composition. The drying step may be performed in a vacuum atmosphere. The drying conditions are, for example, 150°C to 400°C and 0.5 hours to 15 hours.

[0089] In the addition step, for example, boric acid (H 3 BO 3 A boron-containing compound such as LiFePO4, LiO2, or LiO3 is added to the mixture, and the temperature is raised to 200° C. to 400° C. This allows a surface modification layer containing the boron compound to be formed on the surface of the lithium transition metal composite oxide. The amount of the boron-containing compound added is, for example, 0.1 mol % to 7 mol % relative to the total molar amount of metal elements excluding Li in the composite oxide particles.

[0090] In this manner, the positive electrode active material (the first particle group and the second particle group) is obtained. The positive electrode active material may be produced by a method other than the synthesis process described above, or may be produced by a known method.

[0091] The content of the positive electrode active material in the positive electrode mixture layer is determined using a positive electrode mixture sample. The positive electrode mixture sample is obtained by the following procedure. First, a discharged secondary battery is disassembled and the positive electrode is removed. Next, the positive electrode is washed with an organic solvent and vacuum-dried. After that, only the positive electrode mixture layer is removed, and the removed positive electrode mixture layer is used as the mixture sample. By performing analyses such as TG-DTA, NMR, and pyrolysis GC-MS on the mixture sample, the proportions of the dispersant, binder, and carbon conductive additive other than the positive electrode active material can be calculated. When the carbon conductive additive contains multiple types of carbon materials, the proportion of carbon nanotubes in the conductive additive can be calculated by combining thermal analysis such as TG-DTA and microscopic Raman spectroscopy on a cross section of the positive electrode mixture layer.

[0092] 1 m of positive electrode mixture layer (1 layer) 2 The mass per unit area may be 200 g or more, and is preferably 250 g or more. By setting the mass to 250 g or more, it is possible to increase the capacity of the secondary battery. As described above, the positive electrode according to the present disclosure can suppress the adverse effects caused by increasing the mass. The mass can be increased by thickening the positive electrode mixture layer or increasing the density of the positive electrode mixture layer. 2 If the mass per unit area is large, the distribution of the auxiliary agent is likely to become non-uniform during drying of the positive electrode slurry in which the positive electrode mixture is dispersed in a liquid component (dispersion medium) in the manufacturing process of the positive electrode mixture layer, resulting in a significant decrease in capacity. Therefore, it is particularly important to improve the dispersibility of the positive electrode mixture. In the examples described later, the positive electrode mixture layer (1 layer) has a 1 m 2 Mass per unit is 320 g / m 2 In both cases, sufficient battery characteristics are ensured.

[0093] The thickness of the positive electrode mixture layer is not particularly limited, but may be in the range of 50 μm to 250 μm. According to this embodiment, even if the positive electrode mixture layer is made thick, an increase in internal resistance can be suppressed.

[0094] (Positive electrode current collector) The positive electrode current collector is made of a sheet-like conductive material. As the positive electrode current collector, a non-porous conductive substrate (such as a metal foil) or a porous conductive substrate (such as a mesh, net, or punched sheet) is used. The thickness of the positive electrode current collector is not particularly limited, but is, for example, 3 to 50 μm and can be selected depending on the application. Examples of the material of the positive electrode current collector include stainless steel, aluminum, aluminum alloy, and titanium. The positive electrode mixture layer may be formed on only one side of the positive electrode current collector, or may be formed on both sides of the positive electrode current collector.

[0095] (Positive Electrode Slurry and Positive Electrode Manufacturing Method) The positive electrode slurry according to this embodiment includes the above-described components of the positive electrode mixture and a liquid component (dispersion medium) in which they are dispersed. Specifically, the positive electrode mixture includes at least a positive electrode active material, a carbon conductive additive (e.g., CNT), and a dispersant (D). The positive electrode active material includes a first metal composite oxide having a first particle size distribution and a second composite metal oxide having a second particle size distribution. As described above, the volume-based median diameter D1 of the first metal composite oxide and the volume-based median diameter D2 of the second metal composite oxide satisfy the relationship D1 > D2. The dispersant (D) includes a nitrile group-containing rubber and may further include a polyvinylpyrrolidone resin and a cellulose resin. The positive electrode mixture further includes a binder (e.g., polyvinylidene fluoride).

[0096] The liquid component (dispersion medium) is not particularly limited, and may be water, an organic solvent, or a mixture thereof. Examples of the organic solvent include protic solvents such as alcohols (e.g., ethanol), and aprotic solvents such as ethers (e.g., tetrahydrofuran), amides (e.g., dimethylformamide), and N-methyl-2-pyrrolidone (NMP).

[0097] In principle, the ratio of the components contained in the positive electrode slurry is reflected in the ratio of the components in the positive electrode mixture layer. Therefore, by changing the ratio of the components contained in the positive electrode slurry, the ratio of the components in the positive electrode mixture layer can be changed. The ratios of the components exemplified for the positive electrode mixture layer can be applied to the ratios of the components in the positive electrode slurry.

[0098] There are no particular limitations on the method for producing the positive electrode, and known methods may be applied. For example, the positive electrode may be formed by the following method. First, a positive electrode slurry is prepared by dispersing a positive electrode mixture in a liquid component (dispersion medium). Next, the positive electrode slurry is applied to the surface of a positive electrode current collector to form a coating film, and the coating film is then dried to form a positive electrode mixture layer. The dried coating film may be rolled as necessary. The positive electrode mixture layer may be formed on one surface or both surfaces of the positive electrode current collector.

[0099] (Secondary Battery) The secondary battery includes the above-described positive electrode for secondary batteries, a separator, a negative electrode facing the positive electrode via the separator, and an electrolyte. The secondary battery may include an exterior body. Examples of the secondary battery include lithium ion secondary batteries and lithium metal secondary batteries. Components other than the positive electrode mixture layer are not particularly limited, and known components may be used. Examples of components of the secondary battery other than the positive electrode are described below.

[0100] (Negative electrode) The negative electrode typically includes a negative electrode mixture layer containing a negative electrode active material. The negative electrode may include a negative electrode current collector and a negative electrode mixture layer disposed on the negative electrode current collector. However, in the case of a lithium metal secondary battery, a negative electrode current collector on which lithium metal or a lithium alloy can be deposited may be used as the negative electrode.

[0101] The negative electrode mixture layer is composed of a negative electrode mixture, which contains a negative electrode active material as an essential component. The negative electrode mixture may contain optional components such as a binder, a thickener, and a conductive additive. These optional components may include the components exemplified as the components of the positive electrode.

[0102] The negative electrode mixture layer may be formed by applying a negative electrode slurry, in which the components of the negative electrode mixture are dispersed in a dispersion medium, to the surface of the negative electrode current collector and drying the coating. The dried coating may be rolled as necessary. The dispersion medium may be any of the dispersion mediums exemplified for the positive electrode slurry. The negative electrode mixture layer may be formed on only one surface of the negative electrode current collector, or on both surfaces of the negative electrode current collector.

[0103] (Negative electrode active material) The negative electrode active material is selected depending on the type of secondary battery. An example of the negative electrode active material is a material capable of absorbing and releasing lithium ions. Examples of such materials include carbonaceous materials and Si-containing materials. The negative electrode active material may contain or be a Si-containing material. Metallic lithium, a lithium alloy, or the like may be used as the negative electrode active material. The negative electrode may contain one type of negative electrode active material or a combination of two or more types.

[0104] Examples of carbonaceous materials include graphite, easily graphitizable carbon (soft carbon), and hardly graphitizable carbon (hard carbon). One type of carbonaceous material may be used alone, or two or more types may be used in combination. Graphite is preferred because it has excellent charge / discharge stability and a small irreversible capacity. Examples of graphite include natural graphite, artificial graphite, and graphitized mesophase carbon particles.

[0105] Examples of Si-containing materials include simple Si, silicon alloys, silicon compounds (such as silicon oxides), and composite materials in which a silicon phase is dispersed in a lithium ion conductive phase (matrix). Examples of silicon oxides include SiO x The lithium ion conductive phase may include SiO particles. For example, x is 0.5≦x<2, and may be 0.8≦x≦1.6. 2 At least one selected from the group consisting of a silicate phase, a silicate phase, and a carbon phase may be used.

[0106] The negative electrode current collector may be a metal foil. The negative electrode current collector may be porous. Examples of materials for the negative electrode current collector include stainless steel, nickel, nickel alloy, copper, and copper alloy.

[0107] (Electrolyte) The non-aqueous electrolyte may be a liquid electrolyte (electrolytic solution), a gel electrolyte, or a solid electrolyte.

[0108] The gel electrolyte contains a lithium salt and a matrix polymer, or a lithium salt, a non-aqueous solvent, and a matrix polymer. The matrix polymer is, for example, a polymer material that absorbs the non-aqueous solvent and gels. Examples of the polymer material include fluororesin, acrylic resin, polyether resin, and polyethylene oxide.

[0109] The solid electrolyte may be an inorganic solid electrolyte, such as a material known in all-solid-state lithium ion secondary batteries (e.g., oxide-based solid electrolytes, sulfide-based solid electrolytes, halide-based solid electrolytes, etc.).

[0110] The liquid electrolyte (electrolytic solution) contains a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. The electrolyte salt contains at least a lithium salt. The concentration of the lithium salt in the non-aqueous electrolyte is, for example, 0.5 mol / L or more and 2 mol / L or less.

[0111] Known materials can be used as the nonaqueous solvent. Examples of nonaqueous solvents that can be used include cyclic carbonates, chain carbonates, cyclic carboxylic acid esters, and chain carboxylic acid esters. Examples of cyclic carbonates include propylene carbonate (PC), ethylene carbonate (EC), fluoroethylene carbonate (FEC), and vinylene carbonate (VC). Examples of chain carbonates include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC). Examples of cyclic carboxylic acid esters include γ-butyrolactone (GBL) and γ-valerolactone (GVL). Examples of chain carboxylic acid esters include nonaqueous solvents such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP). One type of nonaqueous solvent may be used alone, or two or more types may be used in combination.

[0112] Examples of lithium salts include lithium salts of chlorine-containing acids (LiClO 4 , LiAlCl 4 , LiB 10 Cl 10 etc.), lithium salts of fluorine-containing acids (LiPF 6, LiPF 2 O 2 , LiBF 4 , LiSbF 6 , LiAsF 6 , LiCF 3 SO 3 , LiCF 3 CO 2 etc.), lithium salt of fluorine-containing acid imide (LiN(FSO 2 ) 2 , LiN(CF 3 SO 2 ) 2 , LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 ), LiN(C 2 F 5 SO 2 ) 2 and lithium halides (LiCl, LiBr, LiI, etc.). The lithium salts may be used alone or in combination of two or more.

[0113] The concentration of the lithium salt in the electrolyte solution may be 1 mol / L or more and 2 mol / L or less, or 1 mol / L or more and 1.5 mol / L or less. By setting the lithium salt concentration within the above range, an electrolyte solution having excellent ionic conductivity and appropriate viscosity can be obtained.

[0114] The electrolyte may contain known additives, examples of which include 1,3-propane sultone, methylbenzenesulfonate, cyclohexylbenzene, biphenyl, diphenyl ether, and fluorobenzene.

[0115] (Separator) The separator is disposed between the positive electrode and the negative electrode. The separator preferably has high ion permeability and adequate mechanical strength and insulating properties. The separator may be made of a microporous thin film, woven fabric, nonwoven fabric, or the like. Examples of separator materials include polyolefins (polypropylene, polyethylene, etc.) and other resins.

[0116] (Exterior Body) The exterior body (battery case) houses the electrode group and the non-aqueous electrolyte. The exterior body is not particularly limited, and a known exterior body may be used. The electrode group is composed of a positive electrode, a negative electrode, and a separator. The configuration of the electrode group is not particularly limited, and may be a wound type or a laminated type. A wound type electrode group is formed by winding a positive electrode and a negative electrode with a separator interposed therebetween. A laminated type electrode group is formed by stacking a positive electrode and a negative electrode with a separator interposed therebetween. The shape of the non-aqueous electrolyte secondary battery is not particularly limited, and may be cylindrical, prismatic, coin-shaped, button-shaped, laminate-shaped, etc.

[0117] 1 is a longitudinal cross-sectional view of a cylindrical secondary battery 10 (hereinafter also simply referred to as "battery 10") according to the present disclosure. However, the present disclosure is not limited to the following configuration.

[0118] In FIG. 1 , the battery 10 includes an electrode group 18, a nonaqueous electrolyte (not shown), and a cylindrical battery case (metal can) 22 with a bottom that accommodates these components. A sealing body 11 is crimped to the opening of the battery case 22 via a gasket 21, thereby sealing the interior of the battery 10. The sealing body 11 includes an internal pressure-activated safety valve that cuts off current and, if necessary, ruptures when the battery's internal pressure increases excessively. Specifically, the sealing body includes a valve body 12 having a thin portion, a metal plate 13, and an annular insulating member 14 interposed between the valve body 12 and the metal plate 13. The valve body 12 and the metal plate 13 are electrically connected to each other at their respective centers. A positive electrode lead 15L extending from the positive electrode 15 is connected to the metal plate 13. Thus, the valve body 12 functions as both an external terminal for the positive electrode 15 and a safety valve. When the internal pressure of the battery increases, the connection between the valve body 12 and the metal plate 13 is severed, interrupting the current. Furthermore, when the thin-walled portion breaks, gas is released to the outside, ensuring safety. The negative electrode lead 16L extending from the negative electrode 16 is connected to the inner bottom surface of the battery case 22. An annular groove 22a is formed near the open end of the battery case 22. A first insulating plate 23 is disposed between one end face of the electrode group 18 and the annular groove 22a. A second insulating plate 24 is disposed between the other end face of the electrode group 18 and the bottom of the battery case 22. The electrode group 18 is formed by winding the positive electrode 15 and the negative electrode 16 together with the separator 17 interposed therebetween into a cylindrical shape. The outermost periphery of the electrode group 18 is located at the end of the winding of the negative electrode 16. In other words, in the electrode group 18, the outermost periphery of the negative electrode 16 is disposed outside the outermost periphery of the positive electrode 15. The outermost periphery of the electrode group 18 is composed of the negative electrode current collector 16b at the end 16D of the negative electrode 16 on the winding end side, which is wound around the outer surface of the negative electrode 16 located further inward without going through the positive electrode 15, but this structure is just one example, and the structure is not limited thereto.

[0119] (Additional Notes) The above description discloses the following technologies. (Technology 1) A positive electrode for a secondary battery, comprising: a positive electrode current collector; and a positive electrode mixture layer provided on the surface of the positive electrode current collector, wherein the positive electrode mixture layer includes a positive electrode active material, a carbon conductive additive, and a dispersant, wherein the positive electrode active material includes a first metal composite oxide having a first particle size distribution and a second composite metal oxide having a second particle size distribution, wherein a volume-based median diameter D1 of the first metal composite oxide and a volume-based median diameter D2 of the second metal composite oxide satisfy D1 > D2, wherein a compressive strength F1 of the particles of the first metal composite oxide and a compressive strength F2 of the particles of the second composite oxide satisfy F1 < F2, and wherein the dispersant includes a nitrile group-containing rubber. (Technology 2) The first metal composite oxide and the second metal composite oxide are each independent and have the general formula: Li y Ni x M (1-x) O 2The positive electrode for a secondary battery according to Technology 1, wherein the general formula satisfies 0.8≦x and 0<y≦1.2, and M is at least one element selected from the group consisting of Co, Mn, Al, Fe, Zr, Ti, Sr, Ca, and B. (Technology 3) The positive electrode for a secondary battery according to Technology 2, wherein the general formula satisfies 0.85≦x. (Technology 4) The positive electrode for a secondary battery according to any one of Technology 1 to 3, wherein the first particle size distribution satisfies 8≦D1 (μm)≦30, and the second particle size distribution satisfies 1≦D2 (μm)≦10. (Technology 5) The positive electrode for a secondary battery according to any one of Technology 1 to 4, wherein the positive electrode mixture layer further contains a vinylidene fluoride resin. (Technology 6) The positive electrode for a secondary battery according to Technology 5, wherein the vinylidene fluoride resin has a weight-average molecular weight of 1,000,000 or more. (Technology 7) The positive electrode for a secondary battery according to any one of Technologies 1 to 6, wherein the dispersant further contains a polyvinylpyrrolidone resin and a cellulose resin. (Technology 8) The positive electrode for a secondary battery according to any one of Technologies 1 to 7, wherein the carbon conductive assistant contains carbon nanotubes. (Technology 9) The positive electrode for a secondary battery according to Technology 8, wherein the carbon nanotubes have a diameter of 20 nm or less. (Technology 10) A secondary battery comprising: the positive electrode for a secondary battery according to any one of Technologies 1 to 9, a separator, a negative electrode facing the positive electrode with the separator interposed therebetween, and an electrolyte.

[0120] The present disclosure will be specifically described below based on examples, but the present disclosure is not limited to the following examples. In these examples, a plurality of nonaqueous electrolyte secondary batteries with different positive electrodes were fabricated and evaluated.

[0121] <<Fabrication of Battery A1>> Battery A1 was fabricated using the following method. (1) Fabrication of Negative Electrode A silicon composite material and graphite were mixed in a mass ratio of silicon composite material:graphite = 5:95, and used as the negative electrode active material. The negative electrode active material, carboxymethyl cellulose sodium (CMC-Na), styrene-butadiene rubber (SBR), and water were mixed in a predetermined mass ratio to prepare a negative electrode slurry. Next, the negative electrode slurry was applied to the surface of copper foil (negative electrode current collector) to form a laminate including copper foil and a coating film formed on the copper foil. Next, the coating film was dried, and the laminate was rolled. In this way, a negative electrode including copper foil and a negative electrode mixture layer formed on both sides of the copper foil was formed.

[0122] (2) Preparation of Positive Electrode A positive electrode active material, a dispersant (D), MWCNT (carbon conductive additive), polyvinylidene fluoride (binder), and N-methyl-2-pyrrolidone (dispersion medium) were mixed in a predetermined mass ratio to prepare a positive electrode slurry.

[0123] The positive electrode active material has the composition formula LiNi 0.90 Co 0.05 Mn 0.05 O 2 A first metal oxide (NCM) represented by the formula LiNi 0.85 Co 0.10 Mn 0.05 O 2 The particles of the second metal composite oxide (NCM) represented by the formula:

[0124] The first metal oxide particles were a first particle group having a median diameter D1 of 14 μm, and the second metal oxide particles were a second particle group having a median diameter D2 of 4 μm (D1 / D2=3.5), and the first particle group and the second particle group were mixed at a volume ratio of 8:2.

[0125] The compressive strength F1 of the particles of the first metal composite oxide and the compressive strength F2 of the particles of the second composite oxide were 180 MPa and 190 MPa, respectively, and F1 / F2 = 0.95 (F1 < F2).

[0126] The MWCNTs had an average length of 1 to 5 μm and an average diameter of 10 nm, and the amount of CNTs was 0.5 parts by mass relative to 100 parts by mass of the positive electrode active material.

[0127] The weight average molecular weight of polyvinylidene fluoride was 1,300,000, and the amount of polyvinylidene fluoride was 1.0 part by mass relative to 100 parts by mass of the positive electrode active material.

[0128] The amount of the dispersant (D) was 0.2 parts by mass relative to 100 parts by mass of the positive electrode active material. The dispersant (D) contained polyvinylpyrrolidone (PVP), ethyl cellulose (eC), and a nitrile group-containing rubber (hydrogenated nitrile rubber (HNBR)).

[0129] The amount of ethyl cellulose (eC) relative to 100 parts by mass of hydrogenated nitrile rubber (HNBR) is 100 parts by mass.

[0130] The amount of polyvinylpyrrolidone (PVP) relative to 100 parts by mass of hydrogenated nitrile rubber (HNBR) is 100 parts by mass.

[0131] The positive electrode slurry was applied to the surface of an aluminum foil (positive electrode current collector) to form a coating film, and a laminate of the aluminum foil and the coating film was obtained. Next, the coating film was dried, and the laminate was rolled. In this way, a positive electrode including an aluminum foil and a positive electrode mixture layer formed on both sides of the aluminum foil was produced. The active material density in the positive electrode mixture layer was 3.5 g / cm. 3 It was.

[0132] (3) Preparation of electrolyte solution: LiPF in a non-aqueous solvent 6 The electrolyte solution was prepared by adding LiPF (lithium salt). 6 The concentration of was 1.0 mol / L. As the non-aqueous solvent, a mixed solvent containing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of EC:EMC=3:7 was used.

[0133] (4) Fabrication of Secondary Battery Leads were attached to each of the positive and negative electrodes. Next, an electrode group was fabricated by spirally winding the positive and negative electrodes so that the separator was disposed between the positive and negative electrodes. Next, the electrode group was inserted into an exterior body. The exterior body was made of a laminate film including aluminum foil (barrier layer). Next, the exterior body with the electrode group inserted was vacuum dried at 105°C for 2 hours, after which a nonaqueous electrolyte solution was injected into the exterior body and the opening of the exterior body was sealed. In this way, secondary battery A1 was fabricated.

[0134] <<Fabrication of Battery A2>> The active material density in the positive electrode mixture layer was 3.6 g / cm 3 A positive electrode was produced in the same manner and under the same conditions as in Battery A1, except that the laminate of aluminum foil and coating film was rolled until the positive electrode reached a temperature of 1000 .mu.m.sup.2.

[0135] <<Preparation of Battery A3>> A positive electrode was prepared in the same manner and under the same conditions as for Battery A1, except that only 0.2 parts by mass of a nitrile group-containing rubber was used as a dispersant per 100 parts by mass of the positive electrode active material. The active material density in the positive electrode mixture layer was 3.5 g / cm. 3 It was.

[0136] <<Preparation of Battery A4>> A positive electrode was prepared in the same manner and under the same conditions as for Battery A3, except that 1.5 parts by mass of acetylene black (AB) per 100 parts by mass of the positive electrode active material was used instead of MWCNT as the carbon conductive additive, to prepare secondary battery A4. The active material density in the positive electrode mixture layer was 3.5 g / cm 3 It was.

[0137] <<Preparation of Battery A5>> A positive electrode was prepared in the same manner and under the same conditions as those for Battery A4, except that the weight-average molecular weight of polyvinylidene fluoride was 1,000,000, to prepare secondary battery A5. The active material density in the positive electrode mixture layer was 3.5 g / cm 3 It was.

[0138] <<Preparation of Battery B1>> Composition formula: LiNi 0.85 Co 0.10 Al 0.05 O 2and the active material density in the positive electrode mixture layer is 3.6 g / cm 3 A positive electrode was produced in the same manner and under the same conditions as for Battery A1, except that the laminate of aluminum foil and coating was rolled until the thickness reached 100 μm. The second metal oxide particles were a second particle group having a median diameter D2 of 4 μm, and the first particle group and the second particle group were mixed at a volume ratio of 8:2. The compressive strength F2 of the second composite oxide particles was 120 MPa, and F1 / F2 = 1.50 (F1 > F2).

[0139] <<Preparation of Battery B2>> A positive electrode was prepared in the same manner and under the same conditions as those for Battery A1, except that only polyvinylpyrrolidone (PVP) was used as a dispersant in an amount of 0.2 parts by mass per 100 parts by mass of the positive electrode active material. The active material density in the positive electrode mixture layer was 3.5 g / cm. 3 It was.

[0140] <<Preparation of Battery B3>> A positive electrode was prepared in the same manner and under the same conditions as those for Battery A1, except that only ethyl cellulose (eC) was used as a dispersant in an amount of 0.2 parts by mass per 100 parts by mass of the positive electrode active material. The active material density in the positive electrode mixture layer was 3.5 g / cm. 3 Table 1 shows an outline of the configuration of each positive electrode.

[0141]

[0142] [Evaluation] <Liquid absorption (pore diameter)> A 2 g test piece was cut out from the prepared positive electrode, and the pore diameter distribution in the electrode plate (the size of the pores in the electrode plate through which the electrolyte can pass) was measured using an Autopore V9620 model manufactured by Shimadzu Corporation-Micromeritics Co., Ltd. The measurement range was pore diameters of approximately 0.003 μm to 100 μm, and the pore mode diameter was calculated from the entire measurement range.

[0143] <Electrode Plate Resistance> A square test piece of 5 cm × 5 cm was punched out from the prepared positive electrode, and the mixture layer resistance and interface resistance were measured using an electrical resistance measurement system RM2610 manufactured by Hioki Electric Co., Ltd. The mixture layer resistance at this time was defined as the electrode plate resistance.

[0144] <Charge Capacity> The produced batteries were subjected to constant current charging at a constant current of 0.2 It until the voltage reached 4.2 V in a temperature environment of 25°C, constant voltage charging at 4.2 V until the current value reached 1 / 50 It, and then constant current discharging at a constant current of 0.2 It until the voltage reached 2.5 V. This cycle was repeated twice, and the capacity was confirmed.

[0145] <Safety (ARC)> The fabricated batteries were charged at a constant current of 0.2 It in a temperature environment of 25°C until the voltage reached 4.2 V, and then charged at a constant voltage until the current value reached 1 / 50 It at 4.2 V. After that, a nail with a diameter of 0.9 mm was pierced into the secondary battery at a speed of 1 mm / sec to forcibly short-circuit the battery. The reciprocal of the heat generation rate [W] was calculated from the rate of increase in the surface temperature of the battery at this time.

[0146] <Rapid charging cycle characteristics> The produced batteries were subjected to constant current charging at a constant current of 0.7 It until the voltage reached 4.2 V in a temperature environment of 25°C, followed by constant voltage charging at 4.2 V until the current value reached 1 / 50 It, and then constant current discharging at a constant current of 1.0 It until the voltage reached 2.5 V. This cycle was repeated 200 times, and the capacity retention rate relative to the initial capacity was confirmed.

[0147] The results are shown in Table 2. The evaluation results of the batteries (except for the liquid absorption) are relative values, with the result of Battery A1 being set at 100.

[0148]

[0149] The positive electrode of Battery A1 of Example 1 had high liquid absorption (large pore diameter), low plate resistance, and good battery characteristics. This result was due to the improved dispersibility of the positive electrode mixture. Furthermore, suppression of cracking of the active material particles by satisfying F1 < F2 also contributed to this result. Furthermore, Battery A2 of Example 2 had even lower plate resistance and improved rapid charge cycle characteristics, despite the increased active material density.

[0150] The positive electrode of Battery A3 of Example 3 showed a slight increase in plate resistance, but generally showed good results. Battery A4 of Example 4 and Battery A5 of Example 5 showed reduced liquid absorption, increased plate resistance, and deteriorated battery characteristics, but showed better results than Batteries B1 to B3 of Comparative Examples 1 to 3. The results of Battery B1 are related to the requirement of F1 > F2. It is believed that cracks in the active material particles reduced the electrolyte flow paths, resulting in a deterioration in rapid charge cycle characteristics.

[0151] On the other hand, since the dispersant in Battery B2 of Comparative Example 2 was polyvinylpyrrolidone alone, and the dispersant in Battery B3 of Comparative Example 3 was ethyl cellulose alone, it is believed that the dispersibility of the positive electrode mixture was low, the positive electrode plate resistance was high, and the rapid charge cycle characteristics were deteriorated.

[0152] A secondary battery comprising a high-capacity, high-performance secondary battery positive electrode according to the present disclosure is useful as a main power source for mobile communication devices, portable electronic devices, electric vehicles, and the like.

[0153] While the present invention has been described in terms of presently preferred embodiments, such disclosure is not to be interpreted as limiting. Various changes and modifications will no doubt become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. It is therefore intended that the appended claims be interpreted to cover all changes and modifications that do not depart from the true spirit and scope of the invention.

[0154] REFERENCE SIGNS LIST 10 Secondary battery 11 Sealing body 12 Valve body 13 Metal plate 14 Insulating member 15 Positive electrode 15L Positive electrode lead 16 Negative electrode 16b Negative electrode current collector 16D End portion on winding end side 16L Negative electrode lead 17 Separator

Claims

1. A positive electrode for a secondary battery comprising: a positive electrode current collector; and a positive electrode mixture layer provided on a surface of the positive electrode current collector, the positive electrode mixture layer including a positive electrode active material, a carbon conductive assistant, and a dispersant, the positive electrode active material including a first metal composite oxide having a first particle size distribution and a second composite metal oxide having a second particle size distribution, a volume-based median diameter D1 of the first metal composite oxide and a volume-based median diameter D2 of the second metal composite oxide satisfy D1>D2, a compressive strength F1 of particles of the first metal composite oxide and a compressive strength F2 of particles of the second composite oxide satisfy F1<F2, and the dispersant includes a nitrile group-containing rubber.

2. The first metal composite oxide and the second metal composite oxide are each independent and have the general formula: Li y Ni x M (1-x) O 2 wherein the general formula satisfies 0.8≦x and 0<y≦1.2, and M is at least one selected from the group consisting of Co, Mn, Al, Fe, Zr, Ti, Sr, Ca, and B.

3. The positive electrode for a secondary battery according to claim 2, wherein the general formula satisfies 0.85≦x.

4. The positive electrode for a secondary battery according to claim 1, wherein the first particle size distribution satisfies 8≦D1 (μm)≦30, and the second particle size distribution satisfies 1≦D2 (μm)≦10.

5. The positive electrode for a secondary battery according to claim 1, wherein the positive electrode mixture layer further contains a vinylidene fluoride resin.

6. The positive electrode for a secondary battery according to claim 5, wherein the weight average molecular weight of the vinylidene fluoride resin is 1,000,000 or more.

7. The positive electrode for a secondary battery according to claim 1, wherein the dispersant further comprises a polyvinylpyrrolidone resin and a cellulose resin.

8. The positive electrode for a secondary battery according to claim 1, wherein the carbon conductive assistant comprises carbon nanotubes.

9. The positive electrode for a secondary battery according to claim 8, wherein the carbon nanotubes have a diameter of 20 nm or less.

10. A secondary battery comprising: the positive electrode for a secondary battery according to any one of claims 1 to 9; a separator; a negative electrode facing the positive electrode via the separator; and an electrolyte.

Citation Information

Patent Citations

  • Positive electrode active material, and positive electrode and lithium battery employing the same.

    JP5868604B2

  • Positive electrode plate for secondary batteries and secondary battery using the same

    JP2015043257A

  • Speech Training System For Hearing Impaired Person

    KR1020220115409A

  • Positive electrode for secondary battery and secondary battery

    WO2021153397A1

  • Conductive material liquid dispersion, positive electrode slurry for nonaqueous electrolyte secondary battery, positive electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery

    WO2022210902A1