Immobilizing method for carbon dioxide, carbon dioxide-immobilized cement hardened body, and production method for same
The method of using a high-concentration potassium carbonate solution for CO2 fixation in hardened cement bodies efficiently captures and stabilizes CO2, addressing the inefficiencies and leakage risks of existing methods, achieving high CO2 immobilization rates for construction applications.
Patent Information
- Application Number
- PCT/JP2024/020028
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-31
- Publication Date
- 2024-12-05
AI Technical Summary
Current methods for carbon dioxide fixation in concrete, such as neutralization/carbonation reactions and liquid-phase carbonation, face challenges like long immobilization times and low efficiency, especially when CO2 concentration is low, and risk of CO2 leakage when increasing concentration.
A method involving the use of an aqueous solution of potassium carbonate with a concentration of 15% or more, applied to a hardened cement body through immersion or sprinkling, which includes a carbon dioxide gas absorption step to create a potassium carbonate solution, facilitating efficient CO2 fixation into calcium carbonate.
This method significantly reduces the CO2 fixation time and increases the immobilization efficiency, allowing for substantial CO2 capture, up to 30 kg or more per ton, while minimizing the risk of CO2 leakage, and produces a stable carbon dioxide-fixed cement hardened body suitable for construction materials.
Smart Images

Figure JP2024020028_05122024_PF_FP_ABST
Abstract
Description
Method for fixing carbon dioxide, hardened cement body with fixed carbon dioxide and method for manufacturing the same
[0001] The present invention relates to a method for immobilizing carbon dioxide, a hardened cement product having carbon dioxide immobilized therein by the method, and a method for producing the same.
[0002] In order to curb global warming, there is a growing call for decarbonization, which aims to virtually eliminate emissions of carbon dioxide, a greenhouse gas. In order to achieve the goal of decarbonization, in addition to reducing carbon dioxide emissions, attention is also being paid to carbon dioxide fixation technology, which fixes emitted carbon dioxide in a solid or liquid form (carbon fixation).
[0003] At construction sites, attempts are being made to fix carbon dioxide in concrete, which is used in buildings and civil engineering structures. To fix carbon dioxide in concrete, a conventional technology is used that utilizes the carbonation / carbonation reaction in which carbon dioxide is supplied to hardened cement paste and calcium carbonate is produced from cement hydrates such as calcium hydroxide.
[0004] However, when the carbon dioxide concentration is low, it takes a long time to fix the carbon dioxide. If the carbon dioxide concentration is increased to shorten the fixation time, there is a risk that the carbon dioxide will leak into the atmosphere, and therefore a sealed curing facility or the like is required (see Patent Document 1). For this reason, carbon dioxide fixation has not yet been widely put to practical use.
[0005] Meanwhile, liquid-phase carbonation technology is also being investigated, in which carbon dioxide is immobilized by supplying water containing carbon dioxide (carbonated water, carbonated nanobubble water, etc.) to a hardened cement body (see Non-Patent Document 1). However, dissolving a large amount of carbon dioxide in water lowers the pH and reduces the carbonate ion concentration, so the efficiency of carbon dioxide immobilization is not very high.
[0006] Japanese Patent Application Laid-Open No. 2023-022383
[0007] Shogo Katamura, Yosaku Ikeo, Yukiko Nishioka, and Hayato Takeuchi, "Improvement of Recycled Fine Aggregate by CO2 Fixation and Its Effect on Mortar Basic Properties," Published by the Japan Concrete Institute, Proceedings of the Japan Concrete Institute Annual Meeting, Vol. 44, No. 1, June 15, 2022, pp. 1186-1191
[0008] An object of the present invention is to provide a method for immobilizing carbon dioxide, which can efficiently immobilize carbon dioxide in a hardened cement body, a carbon dioxide-immobilized hardened cement body in which carbon dioxide has been immobilized by the immobilization method, and a method for producing the same.
[0009] The above object is achieved by the following example of the present invention. That is, this example of the present invention is as follows. <1> A method for immobilizing carbon dioxide in a hardened cement body, comprising a carbonate supplying step of supplying the hardened cement body with an aqueous solution of at least one carbonate selected from the group consisting of sodium carbonate, sodium bicarbonate, potassium carbonate, and potassium bicarbonate. <2> The method for immobilizing carbon dioxide according to <1>, in which the aqueous solution contains potassium carbonate, and the potassium carbonate concentration in the aqueous solution is 15 mass% or more. <3> The method for immobilizing carbon dioxide according to <1>, in which the method for supplying the aqueous solution to the hardened cement body is a method of immersing the hardened cement body in the aqueous solution. <4> The method for immobilizing carbon dioxide according to <1>, in which the method for supplying the aqueous solution to the hardened cement body is a method of spraying the aqueous solution on the hardened cement body. <5> The method for immobilizing carbon dioxide according to <1>, in which the carbon dioxide equivalent amount 6 immobilized per ton at the site where carbon dioxide is immobilized is 30 kg or more. <6> The method for immobilizing carbon dioxide according to <1>, comprising a carbon dioxide gas absorption step of causing an aqueous solution containing potassium ions to absorb carbon dioxide gas to obtain an aqueous solution of potassium carbonate, wherein the carbon dioxide gas absorption step is carried out prior to the carbonate supply step. <7> A carbon dioxide-immobilized hardened cement body, in which carbon dioxide has been immobilized in whole or in part by the method for immobilizing carbon dioxide according to any one of <1> to <6>. <8> A method for producing a carbon dioxide-immobilized hardened cement body, comprising a step of immobilizing carbon dioxide in whole or in part of the hardened cement body by the method for immobilizing carbon dioxide according to any one of <1> to <6>.
[0010] The present invention can provide a carbon dioxide fixation method that can efficiently fix carbon dioxide in a hardened cement body, a carbon dioxide-fixed hardened cement body in which carbon dioxide has been fixed by the fixation method, and a method for producing the same.
[0011] 1 is a graph showing the results of Example 1 and Comparative Example 1. FIG. 2 is a graph showing the results of Example 2. FIG. 3 is a graph showing the results of Example 3.
[0012] The carbon dioxide immobilization method according to this embodiment includes a carbonate supplying step of supplying an aqueous solution of at least one carbonate selected from the group consisting of sodium carbonate, sodium bicarbonate, potassium carbonate, and potassium bicarbonate (hereinafter referred to as a "supply liquid") to a hardened cement body. The carbon dioxide immobilization method according to this embodiment, a method for producing a carbon dioxide immobilized hardened cement body, includes a step of immobilizing carbon dioxide in all or part of the hardened cement body by the carbon dioxide immobilization method according to this embodiment, will be described below together.
[0013] [Carbonate Supplying Step] (Hardened Cement Product) The hardened cement product used in this embodiment is an object for immobilizing carbon dioxide, and any object made of hardened cement can be used without any particular limitation. Specific examples of the hardened cement product used in this embodiment include hardened cement paste or mortar, concrete, recycled aggregate, concrete sludge, etc.
[0014] In this embodiment, the hardened cement product may have any shape, such as powder, particles, blocks, rods, plates, blocks, walls, decorative shapes, regular shapes, or irregular shapes. The hardened cement product may also be a part of some kind of object or structure, or may be movable property or immovable property.
[0015] (Supply Liquid) In this embodiment, the supply liquid supplied to the hardened cement body is an aqueous solution of sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, or a mixture of two or more of these carbonates. These alkali metal (sodium, potassium) ions can absorb large amounts of carbon dioxide gas (carbon dioxide), and therefore can contribute to the efficient fixation of carbon dioxide.
[0016] Among these, potassium can take in a larger amount of carbon dioxide gas, so that the feed liquid is preferably an aqueous solution containing potassium carbonate or potassium bicarbonate, more preferably an aqueous solution containing potassium carbonate, and even more preferably an aqueous solution of potassium carbonate. Furthermore, even at low concentrations, an aqueous solution of potassium carbonate exhibits a high alkalinity of pH 11 or higher, so that in this respect it is also preferred as a feed liquid where a high alkalinity is to be maintained, as will be described later.
[0017] To increase the efficiency of carbon dioxide fixation, it is preferable that the concentration of alkali metal carbonate (including alkali metal hydrogencarbonate; hereinafter the same applies to "alkali metal carbonate") in the supply liquid is high, specifically, preferably 1 mass % or more, more preferably 5 mass % or more, and even more preferably 10 mass % or more. Note that if the hardened cement body to be supplied (contacted with the liquid) is wet or contains moisture, the concentration of alkali metal carbonate in the supply liquid can be adjusted taking into account the moisture content.
[0018] Furthermore, potassium carbonate has a higher solubility in water than sodium carbonate and can therefore be used at a higher concentration, and the concentration of potassium carbonate in the supply liquid is preferably 15% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more.
[0019] In this embodiment, the preparation of the feed liquid is not particularly limited, and the feed liquid may be obtained as an industrial product or by-product, or may be supplied from an external source such as another company or other entity. Alternatively, potassium carbonate contained in plant ash, biomass ash, or the like may be dissolved in water to obtain a feed liquid containing a predetermined amount of carbonate ions and potassium ions. Alternatively, the feed liquid may be obtained by the operation of the carbon dioxide gas absorption step described below.
[0020] (Supply of supply liquid to hardened cement body) In the carbonate supplying step, the method of supplying the supply liquid to the hardened cement body is not particularly limited as long as it can bring the supply liquid into contact with the hardened cement body. Specific examples include a method of immersing the hardened cement body in the supply liquid, a method of spraying the supply liquid onto the hardened cement body, and a method of allowing the supply liquid to permeate the hardened cement body.
[0021] When the size of the hardened cement body is small, the method of immersing the hardened cement body in the supply liquid is preferred because carbon dioxide can be efficiently immobilized by impregnating the entire surface of the hardened cement body. On the other hand, when the size of the hardened cement body is large, or when it is part of an object or structure, or real estate, the method of sprinkling the supply liquid onto the hardened cement body is preferred. There are no particular limitations on the method of sprinkling the supply liquid onto the hardened cement body, and examples include a method of pouring the supply liquid using a hose or the like, and a method of spraying the supply liquid in shower or mist form using a spray or atomizer.
[0022] When supplying the liquid to the hardened cement body, the impregnation may be promoted by applying pressure or pressure to the hardened cement body so that the liquid can be efficiently impregnated into the hardened cement body.
[0023] The pH of the supply liquid supplied in this embodiment is preferably 9 or higher, and more preferably 11 to 14. Since the supply liquid supplied in this embodiment has a high pH, amorphous calcium carbonate is first generated, and then crystalline basic calcium carbonate and calcium carbonate are generated. Furthermore, the high pH of the supply liquid allows carbon dioxide after immobilization to exist in the form of carbonate ions, and acidic deterioration and the like are less likely to occur.
[0024] By supplying (contacting) the supply liquid to the hardened cement body, amorphous calcium carbonate and basic calcium carbonate are efficiently produced, and carbon dioxide is efficiently immobilized. Amorphous calcium carbonate and basic calcium carbonate are produced by the reaction of calcium ions originally contained in the hardened cement body with carbonate ions contained in the supply liquid, so the carbonate ions in the supply liquid are consumed, making it possible to stably immobilize carbon dioxide in the hardened cement body.
[0025] Fixation of carbon dioxide by supplying (contacting) a supply liquid to a hardened cement paste is efficient and the reaction is rapid, so the time required for fixation (curing time, number of curing days) can be shortened. Although it depends on the supply method (contacting method) of the supply liquid, the fixation reaction can proceed even with a curing time of about 24 hours. Therefore, the curing time can be set to a shorter time than 24 hours, such as 18 hours, 12 hours, 8 hours, or 4 hours. In fixation using carbon dioxide, it takes several days or more for the fixation reaction to proceed to a certain extent. Therefore, according to this embodiment (fixation by supplying a supply liquid), the curing time (number of curing days) can be significantly shortened.
[0026] There are no particular limitations on the temperature of the liquid to be supplied to the hardened cement body, and it may be room temperature (for example, 20°C to 30°C). Lower temperatures are also acceptable, but temperatures that are too low reduce reactivity, so a temperature of 5°C or higher is preferred, and 10°C or higher is more preferred. Furthermore, for example, if a high concentration of alkali metal carbonate is contained in a high-temperature state, the liquid may be supplied (contacted with the liquid) while maintaining a temperature that maintains that concentration, and then the temperature may be maintained, or the liquid may be left to develop as it goes.
[0027] Furthermore, there are no particular limitations on the ambient temperature when supplying the liquid to the hardened cement body, and it may be room temperature (for example, 20°C to 30°C). In the case of a method in which the hardened cement body is immersed in the liquid to be supplied, the ambient temperature is less likely to affect the temperature, but in the case of a method in which the liquid to be supplied is sprayed onto the hardened cement body, the temperature of the liquid to be supplied is affected by the ambient temperature after spraying. Therefore, if it is desired to maintain the temperature of the liquid to be supplied, it is preferable to keep the temperature of the liquid to be the same as or close to the ambient temperature (for example, within ±10°C, preferably within ±5°C).
[0028] [Carbon dioxide gas absorption step] The carbon dioxide fixation method according to this embodiment may include a carbon dioxide gas absorption step of absorbing carbon dioxide gas into an aqueous solution containing potassium ions to obtain an aqueous solution of potassium carbonate.
[0029] The carbon dioxide gas absorption step is carried out prior to the carbonate supply step, and the aqueous potassium carbonate solution obtained in the carbon dioxide gas absorption step is used as a supply liquid in the subsequent carbonate supply step.
[0030] Examples of aqueous solutions containing potassium ions include aqueous potassium hydroxide solutions, aqueous potassium carbonate solutions, and aqueous potassium hydrogen carbonate solutions.
[0031] The operation of the carbon dioxide absorption step is a carbon dioxide separation and recovery technique known as a "chemical absorption method," in which carbon dioxide contained in exhaust gas with a high carbon dioxide concentration is absorbed in an alkaline solution to separate and recover carbon dioxide from other components. This method can be applied to the present embodiment as the operation of the carbon dioxide absorption step.
[0032] In particular, a hot potassium carbonate absorption method in which carbon dioxide is absorbed into an aqueous potassium carbonate solution can be suitably applied as the operation of the carbon dioxide absorption step. Examples of hot potassium carbonate absorption methods include the Benfield method and the Catacarb (registered trademark) method. The operation and conditions of the carbon dioxide absorption step have been conventionally known, and such known steps and conditions may also be applied to this embodiment.
[0033] The carbon dioxide absorption step can be easily performed in a closed space. The subsequent carbonate supply step can also be performed in a closed space. Even if the carbonate supply step is performed in an open space, the carbon dioxide is contained in the supply liquid, so there is little risk of it being released as carbon dioxide gas. Therefore, according to the carbon dioxide fixation method of this embodiment, there is little risk of carbon dioxide gas being released throughout all steps, including the carbon dioxide absorption step. In contrast, fixation of carbon dioxide using carbon dioxide gas is not easy to perform in a closed space.
[0034] [Carbon dioxide immobilized hardened cement body] A carbon dioxide immobilized hardened cement body can be efficiently produced by a process of immobilizing carbon dioxide in whole or in part using the carbon dioxide immobilization method according to the above embodiment. The carbon dioxide immobilized hardened cement body produced in this manner can be used as a construction member. By using an object or structure in which carbon dioxide is immobilized as a construction member, carbon dioxide can be immobilized semi-permanently. In this embodiment, the term "construction member" refers to a part or all of an architectural structure or civil engineering structure, or construction materials (architectural materials and civil engineering materials) used in an architectural structure or civil engineering structure.
[0035] When hardened cement paste, mortar, or concrete is used as the hardened cement product, it can be used as a construction material consisting of or containing these, and is environmentally friendly because carbon dioxide can be fixed in the construction material. Also, when recycled aggregate is used as the hardened cement product, it can be used as a recycled aggregate (construction material) with excellent resource conservation properties, and because carbon dioxide can be fixed in the aggregate, it is environmentally friendly because it also saves resources.
[0036] Furthermore, when concrete sludge is used as the hardened cement body, it can be reused as concrete materials such as fine aggregate and coarse aggregate, or as recycled roadbed material (all of these are construction materials), and carbon dioxide can be fixed in the concrete materials and recycled roadbed material, making it environmentally friendly.
[0037] According to the carbon dioxide fixation method of this embodiment, carbon dioxide can be efficiently fixed in the hardened cement body, and when this is used as a building component, a large amount of carbon dioxide can be fixed in the building component. For example, it is possible to provide a building component in which the carbon dioxide equivalent of 30 kg or more per ton has been fixed in the part where carbon dioxide has been fixed, which has not been easy to fix until now.
[0038] The "carbon dioxide equivalent" is CaCO 3 Of the total amount of carbon dioxide fixed as CO 2 It is generally referred to as "CO 2 This is referred to as a "fixed amount." 2 The amount of immobilization can be measured, for example, by the method carried out in the Examples described below.
[0039] The above-described embodiments merely show typical forms of the present invention, and the present invention is not limited to these embodiments. That is, a person skilled in the art can implement the present invention by making various modifications in accordance with conventionally known knowledge without departing from the gist of the present invention. As long as such modifications still comprise the carbon dioxide fixation method of the present invention and the construction member in which carbon dioxide is fixed by said method, they are of course included in the scope of the present invention.
[0040] The present invention will be described below with reference to examples, but is not limited to the following examples. The operations of Example 1 in [Test 1] and Example 2 in [Test 2] were carried out in parallel.
[0041] [Test 1] <Example 1> (1) Preparation of Sample A (Hardened Cement Body) Recycled fine aggregate L (compliant with JIS A 5023 Appendix A), which is a recycled material to which a hardened cement body to be used for immobilizing carbon dioxide is attached, was prepared.
[0042] Prior to the test, measurements were taken in accordance with "JIS A 1109: Test method for density and water absorption of fine aggregates." The surface dry density was 2.23 g / cm 3 , bone dry density is 1.99 g / cm 3 The water absorption rate was 12.50% (JIS A 5023 recycled fine aggregate L standard value: 13.0% or less), the fine particle content was 3.4% (JIS A 5023 recycled fine aggregate L standard value: 10.0% or less), and the particle size was 5 mm or less.
[0043] The prepared recycled fine aggregate L sample A was left in an air-dried state, and a portion of the sample was taken and analyzed using CO 2 The content (before the test) was measured. The remaining sample A was divided into smaller portions, and 10 equal portions of 100 g or more (amount required per test) were collected (5 levels of curing time, n=2).
[0044] (2) Preparation of Feed Liquid A (Potassium Carbonate Aqueous Solution) 30 g of potassium carbonate was added to 100 ml of water and thoroughly stirred to dissolve the potassium carbonate, thereby preparing a 23 mass % aqueous solution of potassium carbonate as feed liquid A.
[0045] (3) Supply of supply liquid A to sample A (carbonate supply step) Approximately 100 g of sample A was immersed in 400 g or more of supply liquid A (20°C) in an environment of 20°C and 60% RH and allowed to stand. The curing (standing) time was set to five levels: 3 hours, 9 hours, 15 hours, 24 hours (1 day), and 72 hours (3 days), and tests were performed with n=2 for each level. After the curing time had elapsed, supply liquid A was removed with a dropper or the like, and sample A was taken out.
[0046] (4) Drying of Sample A The collected sample A was immersed in acetone and left to stand for 6 hours or more to remove free water. Subsequently, it was evacuated in a vacuum drying oven for 6 hours or more to dry it completely.
[0047] (5) Post-treatment of Sample A Sample A in an absolutely dried state was crushed to a size of about 100 μm in a ball mill while appropriately reducing the size, and then vacuum dried to prepare a sample for analytical testing. Sample A was stored in a desiccator until the analytical testing was performed.
[0048] <Comparative Example 1> (1) Preparation of Sample B (Hardened Cement Body) Sample B for Comparative Example 1 was prepared in the same manner as in "(1) Preparation of Sample A (Hardened Cement Body)" in Example 1 (water content and CO 2 (Including measurement of content.) However, the number of samples taken was 6 (3 levels of curing time, n=2).
[0049] (2) Supply of carbon dioxide gas to sample B (carbonation curing) Sample B was evenly spread in a suitable sized tray and placed in a carbonation curing tank to begin carbonation curing. The curing environment in the carbonation curing tank was a carbon dioxide concentration of 17%, 20°C, and 60% RH. The curing (standing) time was set to three levels: 24 hours (1 day), 48 hours (2 days), and 72 hours (3 days), and each test was performed with n=2. After the curing time had elapsed, sample B was removed from the carbonation curing tank and appropriately reduced in size. At this time, a portion of the sample was taken to measure the moisture content after curing.
[0050] (3) Treatment after Curing Sample B was dried and post-treated in the same manner as in "(4) Drying of Sample A" and "(5) Post-treatment of Sample A" in Example 1, and then stored in a desiccator.
[0051] <CO 2 Measurement of the amount of fixation> For Sample A and Sample B obtained in Example 1 and Comparative Example 1 after each test, 2 The CO content (after the test) was measured. 2 Including the content (before testing), CO 2The content was determined by the "wet analysis method." In the wet analysis method, the sample is decomposed with hydrochloric acid, and the carbon dioxide produced is introduced into and absorbed in a barium chloride and sodium hydroxide solution, and then titrated with a standard hydrochloric acid solution to determine the CO 2 This is a method for measuring the content.
[0052] The obtained CO 2 Content (before test) and CO 2 From the measurement results of the content (after the test), CO 2 The fixed amount was calculated.
[0053]
[0054] The terms in the above formula (1) are as follows: CO 2Fix :CO 2 Fixed amount [kg / t] CO 2 ':CO 2 Content (before test) [%] CO 2 :CO 2 Content (after test) [%]
[0055] Since the test was conducted with n=2 for each curing period in Example 1 and Comparative Example 1, the average of the two measured values was used as the CO 2 The obtained CO 2 The results of the immobilization amounts are shown in Table 1 below and in the graph of FIG.
[0056] *The figures in the table are CO 2 It is a fixed amount (kg / t).
[0057] <Consideration of the results of Example 1 and Comparative Example 1> As can be seen from Table 1 above and the graph in Figure 1, the results of Comparative Example 1 (CO 2 CO gas (concentration 17%) 2 The fixed amount was 16.3 kg / t after 24 hours of curing and 27.3 kg / t after 72 hours of curing, whereas in Example 1 (immersion in potassium carbonate aqueous solution (concentration 23%)), it was 34.5 kg / t after 24 hours of curing and 38.2 kg / t after 72 hours of curing. 2 It can be seen that the immobilization efficiency is very high.
[0058] In Example 1, even with a curing time of only 3 hours, CO 2 The fixed amount was 20.7 kg / t, which is larger than the 24-hour curing time in Comparative Example 1. 2 It can be seen that the reaction proceeds gradually when immobilized using gas, whereas the reaction proceeds immediately in a short period of time when using potassium carbonate aqueous solution.
[0059] In Example 1, the results of X-ray diffraction showed that the CO 2 It was confirmed that CO2 was fixed and existed as calcium carbonate, which is a stable phase. In Comparative Example 1, the generation of calcium carbonate was also confirmed as a result of X-ray diffraction. In both Example 1 and Comparative Example 1, CO2 was generated in the hardened cement body due to the generation of calcium carbonate, similar to the conventional carbonation / carbonation reaction. 2 It was confirmed that the fixation of the
[0060] [Test 2] <Example 2> (1) Preparation of Sample C (Hardened Cement Body) Sample C for Example 2 was prepared in the same manner as in "(1) Preparation of Sample A (Hardened Cement Body)" in Example 1 (water content and CO 2 (Including measurement of content.) However, the number of samples taken was 6 (3 levels of potassium carbonate concentration, n=2).
[0061] (2) Preparation of Feed Liquids B to D (Potassium Carbonate Aqueous Solutions) Three aqueous solutions of potassium carbonate were prepared as Feed Liquid B (30% by mass), Feed Liquid C (40% by mass), and Feed Liquid D (53% by mass) by adding potassium carbonate in varying amounts relative to water and dissolving the potassium carbonate under thorough stirring so that the potassium carbonate concentrations were 30%, 40%, and 53% by mass. Note that the 53% by mass potassium carbonate concentration is the concentration of a saturated aqueous potassium carbonate solution.
[0062] (3) Supply of supply liquids B to D to sample C (carbonate supply step) Approximately 100 g of sample C was immersed in 400 g or more of each of supply liquids B to D (20°C) in an environment of 20°C and 60% RH, and allowed to stand. The curing (standing) time was 24 hours (1 day), and the test was performed with n=2. After the curing time had elapsed, supply liquids B to D were each removed with a dropper or the like, and sample C was taken out. Hereinafter, sample C immersed in supply liquid B will be referred to as sample CB, sample C immersed in supply liquid C will be referred to as sample CC, and sample C immersed in supply liquid D will be referred to as sample CD.
[0063] (4) Treatment after Curing Similar to "(4) Drying of Sample A" and "(5) Post-treatment of Sample A" in Example 1, Samples CB, CC, and CD were each dried, post-treated, and stored in a desiccator.
[0064] <CO 2 Measurement of the amount of immobilization> For the samples CB, CC, and CD obtained in Example 2 after each test, CO 2 The content (after the test) was measured. 2 Content (before test) and CO 2 From the measurement results of the content (after the test), it was found that CO 2 The fixed amount was calculated.
[0065] In Example 2, the test was conducted with n=2 for each potassium carbonate concentration, and the average of the two measured values was used as the CO 2 The obtained CO 2 The results of the immobilization amount are shown in Table 2 below and in the graph of Figure 2. Table 2 and Figure 2 also include the results of Example 1, where the curing time was 24 hours, as data on the potassium carbonate concentration of 23%.
[0066] *The figures in the table are CO 2 It is a fixed amount (kg / t).
[0067] <Consideration of the results of Example 2> As can be seen from Table 2 above and the graph of FIG. 2, the higher the potassium carbonate concentration of the supply liquid, the greater the CO 2 The fixation efficiency is improved, and the highest CO2 fixation efficiency is achieved at a saturated potassium carbonate aqueous solution concentration of 53 mass%.2 The immobilization efficiency.
[0068] In Example 2, the results of X-ray diffraction showed that the CO 2 It was confirmed that the calcium carbonate was immobilized and existed as a stable phase, calcite (calcium carbonate).
[0069] [Test 3] <Example 3> (1) Preparation of Sample D (hardened cement body) A sludge cake of concrete sludge extracted from wastewater from the washings of a mixer truck was prepared. After dehydration pressing, the water content of the prepared sludge cake was 45.1% and the CaO content was 66.5%.
[0070] The sludge cake was crushed to 10 mm or less using a jaw crusher and sieved to adjust the particle size to 1.2 to 5 mm to obtain sandy concrete sludge. The obtained concrete sludge was immersed in acetone and left to stand for 6 hours or more to remove free water. Subsequently, it was evacuated in a vacuum drying furnace for 6 hours or more to dry it out, and concrete sludge sample D was prepared as a hardened cement product for carbon dioxide fixation.
[0071] The prepared sample D was obtained by taking a part of the sample and subjecting it to CO 2 The content (before the test) was measured. The remaining sample D was divided into equal portions of approximately 200 g (amount required per test, depending on the amount of sample that can be collected) x 8 (K 2 CO 3 Samples were taken at two concentration levels, two curing days, and n=2.
[0072] (2) Preparation of Feed Liquids E to G (Potassium Carbonate Aqueous Solutions) Potassium carbonate was added to water in varying amounts so that the potassium carbonate concentrations were 15 mass%, 27 mass%, and 53 mass%, and the mixture was thoroughly stirred to dissolve the potassium carbonate, thereby preparing three aqueous solutions of potassium carbonate: Feed Liquid E (15 mass%), Feed Liquid F (27 mass%), and Feed Liquid G (53 mass%).
[0073] The feed liquid G obtained here was the same as the feed liquid D obtained in Example 2, and had a concentration equivalent to that of a saturated aqueous potassium carbonate solution. The potassium carbonate aqueous solution concentration of feed liquid F, 27% by mass, was set based on an amount corresponding to the amount of calcium in the concrete sludge, and the 15% by mass of feed liquid E was set based on half the amount corresponding to the amount of calcium in the concrete sludge.
[0074] (3) Supply of supply liquids E to G to sample D (carbonate supply step) Approximately 200 g of sample D was immersed in 1,000 g or more of each of supply liquids E to G (20°C) in an environment of 20°C and 60% RH, and allowed to stand. Two curing (standing) days were set: 1 day and 3 days, and tests were performed with n=2 for each. After the curing days had elapsed, supply liquids E to G were each removed with a dropper or the like, and sample D was taken out. Hereinafter, sample D immersed in supply liquid E will be referred to as sample DE, sample D immersed in supply liquid F will be referred to as sample DF, and sample D immersed in supply liquid G will be referred to as sample DG.
[0075] (4) Treatment after Curing In the same manner as in "(4) Drying of Sample A" and "(5) Post-treatment of Sample A" in Example 1, Sample DE, Sample DF, and Sample DG were each dried, post-treated, and stored in a desiccator.
[0076] <CO 2 Measurement of fixed amount> Samples DE, DF, and DG obtained in Example 3 after each test were subjected to CO 2 The content (after the test) was measured. 2 Content (before test) and CO 2 From the measurement results of the content (after the test), it was found that CO 2 The fixed amount was calculated.
[0077] In Example 3, the test was conducted twice for each potassium carbonate concentration and each curing period, and the average of the two measured values was used as the CO 2 The obtained CO 2 The results of the immobilization amounts are shown in Table 3 below and in the graph of FIG.
[0078] *The figures in the table are CO 2It is a fixed amount (kg / t).
[0079] <Discussion of the Results of Example 3> As can be seen from Table 3 above and the graph in Figure 3, at all potassium carbonate concentrations, a large amount of carbon dioxide, approximately 120 g / t, could be immobilized in a short curing time (1 day). This is presumably because concrete sludge as a hardened cement product is porous and has a large specific surface area, and also contains a large amount of calcium components derived from cement hydrates such as calcium hydroxide, allowing carbon dioxide to be immobilized sufficiently efficiently even in a short curing time. When the curing time was further extended to three days, samples with a higher potassium carbonate concentration were able to immobilize even more carbon dioxide, but the immobilization efficiency decreased over the extended curing period compared to the initial curing period.
[0080] In Example 3, the results of X-ray diffraction showed that the CO 2 It was confirmed that the calcium carbonate was immobilized and existed as a stable phase, calcite (calcium carbonate).
Claims
1. A method for fixing carbon dioxide in a hardened cement body, comprising a carbonate supplying step of supplying to the hardened cement body an aqueous solution of at least one carbonate selected from the group consisting of sodium carbonate, sodium hydrogen carbonate, potassium carbonate and potassium hydrogen carbonate.
2. The method for fixing carbon dioxide as described in claim 1, wherein the aqueous solution contains potassium carbonate and the concentration of potassium carbonate in the aqueous solution is 15 mass% or more.
3. The method for fixing carbon dioxide according to claim 1, wherein the method for supplying the aqueous solution to the hardened cement body is a method for immersing the hardened cement body in the aqueous solution.
4. The method for fixing carbon dioxide according to claim 1, wherein the method for supplying the aqueous solution to the hardened cement body comprises spraying the aqueous solution onto the hardened cement body.
5. The method for immobilizing carbon dioxide according to claim 1, wherein the amount of immobilized carbon dioxide per ton at the site where carbon dioxide is immobilized is 30 kg or more.
6. The method for fixation of carbon dioxide according to claim 1, comprising a carbon dioxide gas absorption step of obtaining an aqueous solution of potassium carbonate by absorbing carbon dioxide gas into an aqueous solution containing potassium ions, the operation of said carbon dioxide gas absorption step being carried out prior to said carbonate supply step.
7. A hardened cement product with immobilized carbon dioxide, in which carbon dioxide has been immobilized in whole or in part by the method for immobilizing carbon dioxide according to any one of claims 1 to 6.
8. A method for producing a hardened cement body with immobilized carbon dioxide, comprising a step of immobilizing carbon dioxide in the whole or part of the hardened cement body by the method for immobilizing carbon dioxide according to any one of claims 1 to 6.
Citation Information
Patent Citations
Concrete and method for producing the same
JP2021155311A
Method for recovering cement paste from waste concrete
JP2022126254A
Carbon dioxide gas fixation method and method for manufacturing existing concrete structure including carbon dioxide gas fixation part
JP2023040557A