Wound iron core and method for manufacturing same

The wound core design with strategically introduced tensile stress in laminated steel plates addresses the challenge of controlling magnetic domains and iron loss, achieving efficient magnetic flux transfer and reduced iron loss by managing stress states near joints.

WO2024248153A1PCT designated stage expired Publication Date: 2024-12-05NIPPON STEEL CORPORATION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/020114
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-31
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing wound core technologies face challenges in controlling the size of magnetic domains and addressing the stress state near joints, leading to inconsistent iron loss reduction.

Method used

A wound core design with laminated bent steel plates, featuring tensile stress introduction in specific regions to control local stress states near joints, and a manufacturing method that includes bending, cutting, and assembling the steel plates with strategically placed tensile stress areas to reduce iron loss.

Benefits of technology

The solution effectively reduces iron loss by improving the magnetic flux transfer across joints, maintaining stress within elastic limits, and optimizing the stress distribution to enhance magnetic permeability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024020114_05122024_PF_FP_ABST
    Figure JP2024020114_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A wound iron core 10 having a wound shape formed by layering folded steel plates, said wound iron core 10: having four flat parts 4 and four corner parts 3 adjacent to the flat parts 4 when seen in a side view in which the wound shape is viewed from a direction along a steel plate surface, and as a result, forming a rectangular shape which has a hollow section 15 in the center thereof; having one or more joining sections 6 where the end sections of the steel plates abut one another in the winding direction in each layer thereof; having a gap between end sections of the steel plates which face one another at the steel plate joining sections 6 in each layer; and having a tensile force of 10MPa or higher introduced in the plate thickness direction of the steel plates at one or more locations in a prescribed region which is defined according to the positional relationship of a gap of an arbitrary steel plate and a gap of a steel plate layered so as to be adjacent to said arbitrary steel plate in a cross-section extending along the winding direction and perpendicular to the steel plate surface.
Need to check novelty before this filing date? Find Prior Art

Description

Wound core and its manufacturing method

[0001] The present invention relates to a wound core and a method for manufacturing the same.

[0002] It is known that in a wound core produced by bending steel sheet without annealing, iron loss can be reduced by introducing closure domains at the joints (see, for example, Patent Document 1).

[0003] Also, a low-core-loss grain-oriented electrical steel sheet is known in which the local stress state inside the steel sheet is controlled to an appropriate condition (Patent Document 2).

[0004] JP 2022-78444 A JP 2008-127632 A

[0005] However, with the technology described in Patent Document 1, it is difficult to control the size of the extremely fine closure domains, and variations in the size of the closure domains occur, so the effect is not complete. Furthermore, the technology described in Patent Document 2 also does not take into account the influence of the joints between the steel sheets in the wound core, so there is room for improvement.

[0006] In view of the above problems, an object of the present disclosure is to provide a wound core and a manufacturing method thereof that can appropriately control the local stress state inside the steel sheets formed in the vicinity of the joint and reduce iron loss.

[0007] The gist of the present disclosure is as follows.

[0008] (1) A wound core having a wound shape formed by stacking bent steel plates, wherein the wound core has, in a side view of the wound shape seen from a direction along the surfaces of the steel plates, four flat portions and four corner portions adjacent to the flat portions, thereby forming a rectangular shape with a hollow portion in the center, wherein each layer of the steel plates has at least one joint where ends in the winding direction are butted together, and a gap exists between the opposing ends of the steel plates at the joint of each layer of the steel plates, and a tensile stress of 10 MPa or more is introduced in the thickness direction of the steel plates at one or more locations in a predetermined region defined in accordance with the positional relationship between the gap in any steel plate and the gap in a steel plate stacked adjacent to the any steel plate in a cross section perpendicular to the surfaces of the steel plates and along the winding direction.

[0009] (2) A wound core according to (1) above, in which the joints of the steel plates of each layer are arranged on the flat surface portion, and the joints of the steel plates of each layer are arranged with a periodic shift in the direction in which the flat surface portion extends.

[0010] (3) A wound core according to (1) or (2) above, in which, in a wound core in which steel plates are stacked, SM / Stot is 1% or more, where SM is the number of steel plates into which tensile stress in the plate thickness direction is introduced within the specified region and Stot is the total number of stacked steel plates.

[0011] (4) A wound core according to any one of (1) to (3) above, in which, in a wound core in which steel plates are stacked, PM / Ptot is 0.1% or more, where PM is the area of ​​the region in which the tensile stress in the plate thickness direction is introduced within the specified region, and Ptot is the total area of ​​the specified region.

[0012] (5) A wound core according to any one of (1) to (4) above, wherein the maximum value of the tensile stress is equal to or less than the yield stress of the steel plate.

[0013] (6) A wound core according to any one of (1) to (5) above, characterized in that in the cross section perpendicular to the surface of the steel plate and along the winding direction, the region into which the tensile stress is introduced has a width in the winding direction of one such region of 1.4 mm or less.

[0014] (7) A wound core according to any one of (1) to (6) above, characterized in that in the cross section perpendicular to the surface of the steel plate and along the winding direction, the region into which the tensile stress is introduced has a length in the plate thickness direction of one of the regions that is 0.2 to 1 times the plate thickness.

[0015] (8) A wound core according to any one of (1) to (7) above, wherein, in the cross section perpendicular to the surface of the steel plate and along the winding direction, the distance between adjacent regions in the winding direction into which the tensile stress has been introduced is 2 mm or more and 10 mm or less.

[0016] (9) A wound core according to any one of (1) to (8) above, characterized in that in the region into which the tensile stress is introduced, the point at which the tensile stress is at its maximum is located more than 10 μm deep from the surface of the raw steel sheet.

[0017] (10) A wound core according to any one of (1) to (9) above, wherein the region into which the tensile stress is introduced extends continuously or at predetermined intervals in a direction intersecting the winding direction of the steel plate and is provided so as to cross the winding direction.

[0018] (11) A wound core according to any one of (1) to (10) above, wherein the winding direction coincides with the {110}<001> direction of the steel sheet.

[0019] (12) A wound core according to any one of (1) to (11) above, wherein the winding direction coincides with the rolling direction of the steel sheet.

[0020] (13) A wound core according to any one of (1) to (12) above, in which the tensile stress is introduced only in the predetermined region in the cross section perpendicular to the surface of the steel plate and along the winding direction.

[0021] (14) A method for manufacturing a wound core according to any one of (1) to (13) above, comprising the steps of: bending steel sheets; cutting the steel sheets; stacking the bent and cut steel sheets in layers and assembling them into a wound shape by butting together end portions in the winding direction; and introducing tensile stress in the sheet thickness direction near the end portions or near positions that would become the end portions before cutting.

[0022] According to the present disclosure, a wound core and a manufacturing method thereof are provided that are capable of appropriately controlling the local stress state inside the steel sheets formed in the vicinity of the joint and reducing iron loss.

[0023] 7A is a perspective view schematically showing an embodiment of a wound core. FIG. 7B is a side view of the wound core shown in the embodiment of FIG. 1. FIG. 7C is a side view schematically showing another embodiment of the wound core. FIG. 7D is a view schematically showing an example of a bent portion (curved portion) of a grain-oriented electromagnetic steel sheet. FIG. 7E is a view schematically showing an example of a grain-oriented electromagnetic steel sheet for one layer in a wound core body. FIG. 7F is a view schematically showing an example of a grain-oriented electromagnetic steel sheet for one layer in a wound core body. FIG. 7G is a schematic view showing the detailed shape and arrangement of the joints in region A1 or region A2 of FIG. 2 or FIG. 3, and a region where a region where tensile stress is introduced in the sheet thickness direction is provided for a specific joint. FIG. 7H is a schematic view for explaining region M where a region where tensile stress is introduced in the sheet thickness direction is provided for all joints in FIG. 7A. FIG. 7H is a schematic view showing a cross section of a steel sheet, and a view schematically showing how regions where tensile stress is introduced in the sheet thickness direction are periodically provided in the X-axis direction (winding direction). FIG. 1 is a perspective view of a steel sheet, and is a diagram schematically showing a state in which a region where tensile stress is introduced in the sheet thickness direction is provided in a direction intersecting the winding direction (Y-axis direction perpendicular to the winding direction). FIG. 2 is a diagram for explaining the effect of providing a region where tensile stress is introduced in the sheet thickness direction. FIG. 3 is a diagram for explaining the effect of providing a region where tensile stress is introduced in the sheet thickness direction. FIG. 4 is a diagram schematically showing a manufacturing apparatus for a wound core in the form of a unicore. FIG. 5 is a diagram for explaining the detailed dimensions of the wound core.

[0024] Hereinafter, several embodiments of the present invention will be described with reference to the drawings. However, these descriptions are intended to merely exemplify preferred embodiments of the present invention and are not intended to limit the present invention to such specific embodiments. In the following description, similar components will be designated by the same reference numerals.

[0025] A wound core according to one embodiment of the present invention will be described in detail below. However, the present invention is not limited to the configuration disclosed in this embodiment, and various modifications are possible without departing from the spirit of the present invention. Note that the numerical ranges listed below include the lower and upper limits. Numerical values ​​indicated as "greater than" or "less than" do not include the numerical range. Furthermore, "%" in relation to chemical composition means "mass %" unless otherwise specified.

[0026] Furthermore, terms used in this specification that specify shapes, geometric conditions, and their degrees, such as "parallel," "vertical," "same," and "right angle," as well as values ​​of lengths and angles, are not to be construed as being bound by strict meanings, but rather as including a range within which similar functions can be expected.

[0027] Furthermore, in this specification, a "grain-oriented electrical steel sheet" may be simply referred to as a "steel sheet" or an "electrical steel sheet," and a "wound core" may be simply referred to as a "wound core body" or an "iron core."

[0028] A wound core according to one embodiment of the present invention is a wound core formed by stacking folded steel sheets. When viewed from the side of the wound core from a direction along the surface of the steel sheets, the wound core has a rectangular structure with a central hollow, including four flat portions and four corner portions adjacent to the flat portions. Here, the flat portions refer to straight portions other than the bent portions. The radius of curvature r on the inner surface side of the bent portion in side view is, for example, 1.0 mm or more and 5.0 mm or less. The grain-oriented electrical steel sheet, for example, has a chemical composition containing, by mass, 2.0 to 7.0% Si, with the remainder consisting of Fe and impurities, and has a texture oriented in the Goss orientation. For example, a grain-oriented electrical steel strip as defined in JIS C 2553:2019 can be used as the grain-oriented electrical steel sheet.

[0029] Next, the shapes of the wound core and grain-oriented electrical steel sheet according to one embodiment of the present invention will be specifically described. The shapes of the wound core and grain-oriented electrical steel sheet described here are not particularly new, but merely conform to the shapes of known wound cores and grain-oriented electrical steel sheets.

[0030] Fig. 1 is a perspective view schematically showing one embodiment of a wound core. Fig. 2 is a side view of the wound core shown in the embodiment of Fig. 1, showing a side view of the wound core. Fig. 3 is a side view schematically showing another embodiment of the wound core.

[0031] The side view refers to the winding shape of the wound core viewed from a direction along the surface of the steel sheet, and more specifically, refers to the winding shape of the wound core viewed from the axial direction of the windings of the wound core (perpendicular to the plane of the paper in FIG. 2 ). In other words, the side view refers to the view in the width direction (the Y-axis direction in FIG. 1 ) of the long grain-oriented electrical steel sheets that make up the wound core. The side view is a diagram that shows the shape as seen from the side (a diagram in the Y-axis direction in FIG. 1 ).

[0032] A wound core 10 according to one embodiment of the present invention comprises a wound core body that is substantially polygonal in side view. The wound core body 10 has a laminated structure in which grain-oriented electromagnetic steel sheets 1 are stacked in the thickness direction, resulting in a substantially rectangular shape in side view. The wound core body 10 may be used as a wound core as is, or may be equipped with known fasteners such as cable ties to integrally fasten the stacked grain-oriented electromagnetic steel sheets, as needed.

[0033] In this embodiment, there is no particular limit to the core length of the wound core body 10. As long as the number of bends 5 is the same, even if the core length of the wound core 10 changes, the volume of the bends 5 remains constant, and therefore the iron loss generated at the bends 5 remains constant. A longer core length reduces the volume ratio of the bends 5 to the wound core body 10, and therefore reduces the impact on iron loss degradation. Therefore, a longer core length is preferable for the wound core body 10. The core length of the wound core body 10 is preferably 1.5 m or more, and more preferably 1.7 m or more. In the present invention, the core length of the wound core body 10 refers to the circumferential length at the center point of the wound core body 10 in the lamination direction when viewed from the side. Such a wound core can be suitably used for any conventionally known application.

[0034] The iron core according to this embodiment is characterized by its substantially polygonal shape in side view. In the following explanation using figures, for simplicity of illustration and explanation, a generally-shaped substantially rectangular (quadrilateral) iron core will be described. However, iron cores of various shapes can be manufactured by changing the angle and number of bent portions 5 and the length of the flat portions 4. For example, if all bent portions 5 have an angle of 45° and the flat portions 4 are the same length, the iron core will be octagonal in side view. On the other hand, if there are six bent portions 5 with an angle of 60° and the flat portions 4 are the same length, the iron core will be hexagonal in side view.

[0035] As shown in FIGS. 1 and 2 , the wound core body 10 includes grain-oriented electrical steel sheets 1, each having alternating flat portions 4, 4 a and bent portions 5 in the longitudinal direction, stacked in the sheet thickness direction. The laminated structure 2 has a generally rectangular shape in side view, with a hollow portion 15. Each corner portion 3, including the bent portions 5, has two or more bent portions 5 that are curved in side view, and the sum of the bending angles of the bent portions 5 in one corner portion 3 is, for example, 90°. The corner portion 3 has a flat portion 4 a between adjacent bent portions 5, 5, which is shorter than the flat portion 4. Therefore, the corner portion 3 has two or more bent portions 5 and one or more flat portion 4 a. In the embodiment of FIG. 2 , one bent portion 5 is 45°. In the embodiment of FIG. 3 , one bent portion 5 is 30°.

[0036] As shown in these examples, the wound core of this embodiment can be configured with bent portions having various angles. However, from the viewpoint of suppressing distortion due to deformation during processing and thereby suppressing iron loss, the bending angle φ (φ1, φ2, φ3) of the bent portion 5 is preferably 60° or less, and more preferably 45° or less. The bending angle φ of the bent portions of one iron core can be configured arbitrarily. For example, φ1 = 60° and φ2 = 30°. From the viewpoint of production efficiency, it is preferable that the bending angles (bending angles) are equal. However, if the iron loss of the iron core can be reduced by reducing the number of deformation points above a certain level, a combination of different angles may be used. The design can be selected arbitrarily based on the points that are important in iron core processing.

[0037] The bent portion 5 will be described in more detail with reference to FIG. 4 . FIG. 4 is a diagram schematically illustrating an example of a bent portion (curved portion) 5 of a grain-oriented electrical steel sheet 1. The bending angle of the bent portion 5 refers to the angular difference between the straight portion on the rear side and the straight portion on the front side in the bending direction at the bent portion of the grain-oriented electrical steel sheet, and is expressed as the angle φ, which is the supplementary angle formed by two imaginary lines Lb-elongation1 and Lb-elongation2 obtained by extending the straight portions that are the surfaces of the flat portions 4, 4a on both sides of the bent portion 5 on the outer surface of the grain-oriented electrical steel sheet 1. In this case, the points where the extended lines depart from the steel sheet surface are the boundaries between the flat portions 4 and the bent portion 5 on the outer surface of the steel sheet, and in FIG. 4 , these are points F and G.

[0038] Furthermore, lines perpendicular to the outer surface of the steel plate are extended from each of points F and G, and the intersections with the inner surface of the steel plate are respectively points E and D. These points E and D are the boundaries between the flat portion 4 and the bent portion 5 on the inner surface of the steel plate.

[0039] In the present invention, the bent portion 5 is a portion of the grain-oriented electrical steel sheet 1 that is surrounded by the points D, E, F, and G in a side view of the grain-oriented electrical steel sheet 1. In Fig. 4, the steel sheet surface between points D and E, i.e., the inner surface of the bent portion 5, is shown as La, and the steel sheet surface between points F and G, i.e., the outer surface of the bent portion 5, is shown as Lb.

[0040] This figure also shows the inner surface curvature radius r of the bent portion 5 in a side view. The curvature radius r of the bent portion 5 is obtained by approximating the above La with an arc passing through points E and D. The smaller the curvature radius r, the sharper the curve of the curved portion of the bent portion 5, and the larger the curvature radius r, the gentler the curve of the curved portion of the bent portion 5.

[0041] In the wound core of the present invention, the radius of curvature r of each bent portion 5 of each grain-oriented electrical steel sheet 1 stacked in the sheet thickness direction may vary to some extent. This variation may be due to forming accuracy, or it may be due to unintended variation caused by handling during stacking. Such unintended errors can be suppressed to approximately 0.2 mm or less in current, standard industrial manufacturing. If such variation is significant, a representative value can be obtained by measuring and averaging the radius of curvature for a sufficiently large number of steel sheets. It is also possible to intentionally vary the radius of curvature for some reason, but this is not excluded by the present invention. The radius of curvature r of the bent portion 5 (the inner radius of curvature of the bent portion 5 in a side view) is preferably 1 mm or more and 5 mm or less. By setting the radius of curvature r to 1 mm or more and 5 mm or less, the building factor (BF) can be further suppressed.

[0042] There are no particular limitations on the method for measuring the radius of curvature r of the bent portion 5, and it can be measured, for example, by observing at 200x magnification using a commercially available microscope (Nikon ECLIPSE LV150). Specifically, the center of curvature A is determined from the observation results. For example, if the intersection point A is defined as the point of intersection between line segments EF and DG extended inward on the opposite side from point B, then the magnitude of the radius of curvature r corresponds to the length of line segment AC. Here, when points A and B are connected by a straight line, the intersection point C on the arc DE on the inside of the bent portion of the steel plate is defined as the point of intersection.

[0043] 5 and 6 are diagrams schematically showing an example of one layer of grain-oriented electrical steel sheet 1 in a wound core body. The grain-oriented electrical steel sheet 1 used in the examples of Fig. 5 and Fig. 6 is bent to realize a wound core in a unicore form, and has two or more bent portions 5 and a flat portion 4, and forms a substantially polygonal ring in side view via joint portions 6 (gaps) that are the end faces in the longitudinal direction of one or more grain-oriented electrical steel sheets 1.

[0044] In this embodiment, it is sufficient that the wound core body 10 has a laminated structure that is generally polygonal in side view as a whole. As shown in the example of Fig. 5, one grain-oriented electromagnetic steel sheet may constitute one layer of the wound core body via one joint 6 (one grain-oriented electromagnetic steel sheet is connected via one joint 6 per turn), or as shown in the example of Fig. 6, one grain-oriented electromagnetic steel sheet 1 may constitute approximately half the circumference of the wound core, and two grain-oriented electromagnetic steel sheets 1 may constitute one layer of the wound core body via two joints 6 (two grain-oriented electromagnetic steel sheets 1 are connected to each other via two joints 6 per turn).

[0045] The thickness of the grain-oriented electrical steel sheet 1 used in this embodiment is not particularly limited and may be selected appropriately depending on the application, etc., but is usually in the range of 0.15 mm to 0.35 mm, and preferably in the range of 0.18 mm to 0.27 mm.

[0046] In the example of Fig. 5, one joint 6 of one grain-oriented electrical steel sheet that constitutes one layer of the wound core body is located in region A1 shown in Fig. 2 and Fig. 3. In the example of Fig. 6, two joints 6 of two grain-oriented electrical steel sheets that constitute one layer of the wound core body are located in regions A1 and A2 shown in Fig. 2 and Fig. 3. Note that detailed shapes and arrangements of joints 6 in region A1 or region A2 are omitted from Fig. 2 and Fig. 3.

[0047] FIG. 7A is a schematic diagram illustrating the detailed shape and arrangement of the joints 6 in region A1 or region A2 in FIG. 2 or FIG. 3 , and the region where a region 12 where tensile stress is introduced in the sheet thickness direction is provided for a specific joint. FIG. 7A schematically illustrates a cross section perpendicular to the surface of the steel sheet and along the winding direction. As shown in FIG. 7A , the positions of the joints 6 (gaps in the joints 6 are indicated as 6(n-1), 6(n), ..., etc.) of the grain-oriented electrical steel sheets 1 constituting each layer are offset in the X-axis direction along which the planar portion 4 extends. This reduces the magnetic resistance of the wound core and iron loss compared to when the joints 6 of each layer are positioned at the same position in the X-axis direction. FIG. 7A particularly illustrates a state in which the joints 6 are periodically offset in the X-axis direction.

[0048] Furthermore, the wound core body 10 having the joints 6 is excellent in productivity and ease of shape design. On the other hand, the presence of the joints 6 means that the steel sheets are cut at the joints 6, which can be a factor in increasing iron loss and noise.

[0049] The inventors have thoroughly investigated the effect of the internal stress state of the steel sheet on core characteristics and found that controlling the tensile stress in the steel sheet thickness direction is particularly effective in reducing iron loss in wound cores having joints 6. Based on this finding, in this embodiment, the internal stress state (strain distribution) of the steel sheet is controlled near the joints 6 of the wound core. While the mechanism behind this is not entirely clear at this point, the inventors' extensive investigations suggest that the tensile stress in the thickness direction makes it easier for magnetic flux passing through the steel sheet to bend in the thickness direction. Because the steel sheet is interrupted at the joints 6 of the wound core 10, magnetic flux must pass through the gap at the joints 6. In this case, if tensile stress in the thickness direction is present near the joints, the magnetic permeability increases in the direction along the tensile stress, making it easier for magnetic flux to deviate from the in-plane direction (direction along the steel sheet surface) and leak outside the steel sheet surface. Therefore, magnetic flux that is prevented from traveling in the in-plane direction by the gaps at the joints 6 can be smoothly transferred to adjacent steel sheets that are stacked and in contact with each other. In other words, it is believed that the transfer of magnetic flux to adjacent steel sheets occurs smoothly. Such smooth transfer is believed to reduce losses compared to passing through the gaps at the joints 6. In the following explanation, the mechanism of action of tensile stress in the thickness direction near the joints in this invention will be explained based on the above phenomenon (smooth transfer of magnetic flux). However, it should be noted that this is merely a hypothesis at this time to theoretically support the empirical law discovered by the inventors as a result of extensive research. It is hoped that the academically correct mechanism will be elucidated in the future.

[0050] In this embodiment, as shown in FIG. 7A , a grain-oriented electrical steel sheet 1 has a continuous region 12 (hereinafter also referred to as stress region 12) in which a tensile stress of 10 MPa or more is introduced in the thickness direction. The stress values ​​within the thickness direction were determined by measuring the strain of the crystal lattice in three directions using an X-ray diffraction method, and using material properties such as elastic modulus to determine the stress values ​​in the rolling direction, thickness direction, and width direction. The crystal strain in these three directions can be determined by irradiating the steel sheet with X-rays and detecting and evaluating the reflected and transmitted X-rays. Specifically, the steel sheet (test piece) is scanned while moving, and the shift in the diffraction angle (2θ) of the reflected X-ray diffraction peak is evaluated using a reflection method, thereby determining the strain in the thickness direction. Furthermore, the strain in the rolling direction and width direction is determined by evaluating the shift in the diffraction angle of the transmitted X-ray diffraction peak using a transmission method. The strain can be converted into stress values ​​using the relationship between stress and strain in three directions according to the material properties (Young's modulus, Poisson's ratio). These methods are well known, but for example, by using the method described in the strain scanning method using high-energy synchrotron radiation to measure residual stress distribution (literature: Transactions of the Japan Society of Mechanical Engineers (Part A), Vol. 71, No. 711, 2005, pp. 1530), it is possible to obtain stress values ​​within the plate thickness as described above.

[0051] The stress regions 12 are basically provided near the joints 6 of the steel plates, and when focusing on any one void 6, it is preferable to determine the region where the stress region 12 should be located, including multiple steel plates adjacent in the stacking direction. The region where the stress region 12 should be located (hereinafter also referred to as the stress location region) will be described in detail below.

[0052] First, the stress distribution region is defined as a region extending inward from the in-plane end of the steel plate member constituting the wound core by at least two times the thickness of the steel plate. The in-plane end of a steel plate member is generally formed by shearing and therefore undergoes significant plastic deformation, potentially resulting in an undesirable stress state for the stress region 12 intended in this application. For this reason, the stress distribution region excludes such end regions. One end region, in the wound core shown in FIG. 1 , is the region extending from the surface in the Y-axis direction, i.e., the surface when viewed from the side of the wound core, to twice the thickness of the steel plate toward the interior of the steel plate (Y-axis direction). The other end region is the region extending from the end of the steel plate facing each other across a gap at the joint 6 of the wound member to twice the thickness of the steel plate toward the interior of the steel material (X-axis direction in FIG. 6 ). Direct observation of the stress distribution region requires the removal of the end regions. Examples of such a method include removing the end regions by methods that are less likely to introduce distortion, such as electrical discharge machining or pickling edging.

[0053] The stress distribution region provided near the joint 6 will now be described. Figure 7A is a schematic diagram of a cross section of the joint 6 of the wound core 10, taken along the XZ plane, at a distance of at least twice the plate thickness from the end of the wound core 10 in the Y-axis direction toward the interior of the steel material. The phrase "a cross section at a distance of at least twice the plate thickness toward the interior of the steel material" is intended to avoid the end region. As shown in Figure 7A , in the nth steel plate (here, the third steel plate from the inside in the figure) counting from the innermost side in the direction from the inside to the outside of the wound core body 10 (the lamination direction of the steel plates, or the Z-axis direction), the gap between the opposing ends of the steel plates at the joint 6 formed by cutting the steel plate is designated as 6(n). Position An is the position that is twice the plate thickness in the positive direction of the X axis from the end of gap 6(n) on the positive side of the X axis, and position Bn is the position that is twice the plate thickness in the negative direction of the X axis from the end of gap 6(n) on the negative side of the X axis.

[0054] For this void 6(n), stress distribution regions M(n) are defined on both sides of the X-axis and Z-axis. The range in the Z-axis direction of stress distribution region M(n) based on void 6(n) is a range equivalent to three steel plates, including the (n-1)th steel plate, the nth steel plate, and the (n+1)th steel plate from the inside. However, in the n=1 steel plate, the n-1th steel plate does not exist, and in the n=Nmax steel plate, where the total number of stacked plates is Nmax, the n+1th steel plate does not exist. Since stress distribution region M(n) is meaningless in regions where no steel plates exist, the range in the Z-axis direction of stress distribution region M based on the void 6 between the two plates where n=1 and n=Nmax is equivalent to two steel plates.

[0055] The range of the stress allocation region on the positive side of the X axis relative to void 6(n) is the range from position An to either position B(n-1) or position B(n+1), whichever is closer to position An and located on the positive side of the X axis. Similarly, the range of the stress allocation region on the negative side of the X axis relative to void 6(n) is the range from position Bn to either position A(n-1) or position A(n+1), whichever is closer to position Bn and located on the negative side of the X axis. Here, if neither position B(n-1) nor position B(n+1) is located on the positive side of the X axis relative to position An, the range of the stress allocation region on the positive side of the X axis is the same distance from position An as the range of the stress allocation region on the negative side of the X axis. Furthermore, if neither position A(n-1) nor position A(n+1) exists on the negative side of position Bn along the X axis, the range of the stress allocation region on the negative side of the X axis is set to the same distance from position Bn as the range of the stress allocation region on the positive side of the X axis. Furthermore, if neither position B(n-1) nor position B(n+1) exists on the positive side of the X axis from position An, and neither position A(n-1) nor position A(n+1) exists on the negative side of the X axis from position Bn, it is assumed that no stress allocation region based on void 6(n) exists. Note that if the positions of void 6(n) and void 6(n-1) or void 6(n+1) in the X-axis direction are close to each other, and there is no region between A(n) and either B(n-1) or B(n+1) (B(n-1) or B(n+1) is located on the negative side of the X-axis relative to A(n)), then it is assumed that no stress distribution region exists on the positive side of the X-axis relative to void 6(n) for the three plates in question. Similarly, if there is no region between B(n) and either A(n-1) or A(n+1), it is assumed that no stress distribution region exists on the negative side of the X-axis relative to void 6(n) for the three plates in question. In Figure 7A, the stress distribution regions M(n), M(n+3), and M(n+7) relative to voids 6(n), 6(n+3), and 6(n+7), as determined according to the above definition, are indicated by hatching. The region at the joint 6 from the opposing steel plate ends that form a gap to twice the plate thickness in the X-axis direction is the end region described above, and is excluded from the stress distribution region, so is not hatched.

[0056] When stress distribution regions M are set for each individual void 6 as described above, a situation may arise in which the stress distribution regions M partially overlap. FIG. 7B is a schematic diagram illustrating the regions M in which regions in which tensile stress is introduced in the plate thickness direction are provided for all joints 6 in FIG. 7A . For example, when the voids 6 are periodically arranged in the X-axis direction as shown in FIG. 7B , a stress distribution region M(n) based on a specific void 6 (e.g., void 6(n)) will have a portion with the same range in the X-axis direction as a stress distribution region M(n+1) based on the void 6 of the steel plate adjacent in the Z-axis direction (void 6(n+1) in FIG. 7B ). In FIG. 7B , the region where the stress distribution regions M partially overlap is indicated by cross-hatching.

[0057] 8A is a schematic diagram showing a cross section of a steel sheet, and is a diagram showing a state in which a plurality of stress regions 12 are provided in the X-axis direction (winding direction). The stress regions 12 may be provided at predetermined intervals in the X-axis direction in the cross section of the steel sheet; in other words, the stress regions 12 may be provided periodically. Therefore, the stress regions 12 are provided in the stress distribution region M, but may also be provided throughout the entire steel sheet other than the stress distribution region M.

[0058] In FIG. 8A, the width D in the X-axis direction (width in the winding direction) of the stress region 12 is preferably 1.4 mm or less. The width D is preferably 0.3 to 1.1 mm, and more preferably 0.7 to 1.1 mm. The length L in the Z-axis direction (width in the plate thickness direction) is preferably 0.2*t≦L<t, where t is the plate thickness of the steel plate. The length L is more preferably 0.4*t≦L≦0.8*t. If the width D is 1.4 mm or more, the position of the magnetic flux transfer will vary widely in the X-axis direction, resulting in increased iron loss. Furthermore, if the length L in the Z-axis direction is too short, the effect of the magnetic flux transfer will not be achieved. Therefore, it is preferable that the width D and length L be within the above ranges.

[0059] It is desirable that the maximum stress in the stress region 12 exists at a depth of more than 10 μm from the surface of the steel sheet. If it exists in a region shallower than 10 μm, the bending of the magnetic flux when it passes becomes steep, resulting in an increase in thin current loss and a decrease in the iron loss reduction effect. Therefore, the maximum stress in the stress region 12 exists at a depth of more than 10 μm from the surface of the steel sheet, preferably 30 to 80 μm, and more preferably 40 to 70 μm.

[0060] When the stress regions 12 are periodically arranged at predetermined intervals in the X-axis direction, the interval between the stress regions 12 in the X-axis direction affects magnetic domain refinement due to the interaction between adjacent stress regions 12. Therefore, if the interval is too large, the effect of reducing iron loss is reduced. To sufficiently reduce iron loss, the interval between the stress regions 12 is preferably 10.0 mm or less, and more preferably 7.0 mm or less. It is preferable that the interval between the stress regions 12 be approximately 5 mm. However, since the stress regions 12 also act as an obstacle to magnetic flux in the in-plane direction (magnetization direction) of the steel sheet, and if the interval is too small, it can cause an increase in iron loss. Therefore, the interval between the stress regions 12 in the X-axis direction is preferably 2 mm or more.

[0061] FIG. 8B is a perspective view of a steel sheet, schematically illustrating a state in which stress regions 12 are provided in a direction intersecting the winding direction (in FIG. 8B, the Y-axis direction perpendicular to the winding direction). As shown in FIG. 8B, the stress regions 12 may extend in a direction intersecting the winding direction and be provided so as to cross the winding direction. Furthermore, the stress regions 12 may be provided continuously in the direction intersecting the winding direction, or may be provided periodically at predetermined intervals. To ensure smoother transfer of magnetic flux near the joint and further suppress the reduction of iron loss, the stress regions 12 preferably extend in a direction forming an angle of 60 to 120° with respect to the X-axis direction in a view along the Z-axis. More preferably, they extend in a direction forming an angle of 80 to 110°.

[0062] In the present invention, the stress region 12 is defined as a continuous region in which the tensile stress in the plate thickness direction is 10 MPa or more. If the tensile stress in the plate thickness direction is less than 10 MPa, the effect of the magnetic permeability is small compared to the gap in the joint 6, and therefore the effect of providing the region 12 in which the tensile stress is introduced cannot be fully obtained.

[0063] Furthermore, in the stress region 12, the maximum value of the tensile stress in the plate thickness direction is preferably equal to or less than the yield stress of the steel plate, which is the raw material. If the maximum value of the tensile stress becomes large, the plastic region expands, and the decrease in magnetic permeability due to plastic strain becomes significant, resulting in an increase in iron loss. In general, the point at which the stress state changes significantly from the elastic region to the plastic region can be determined by the yield stress of the raw material.

[0064] For the above reasons, in this embodiment, it is preferable that the maximum value of the tensile stress in the plate thickness direction in the stress region 12 is equal to or less than the yield stress value of the material. The maximum value of the tensile stress is more preferably 80 to 200 MPa.

[0065] 9A and 9B are diagrams for explaining the effect of providing the stress region 12. As mentioned above, the explanation of Fig. 9A and Fig. 9B is one possibility regarding the mechanism of action of the present invention. In Fig. 9A, arrows indicate the flow of magnetic flux when the stress region 12 is provided.

[0066] On the other hand, in Figure 9B, the arrows indicate the flow of magnetic flux when no stress region 12 is provided. As shown in Figure 9B, the flow of magnetic flux from one steel sheet to an adjacent steel sheet is called "magnetic flux crossing." When no stress region 12 is provided, it is more difficult for magnetic flux to cross from one steel sheet to an adjacent steel sheet than when the stress region 12 is provided, and iron loss increases. As shown in Figure 9A, the provision of the stress region 12 makes it easier for magnetic flux to cross from one steel sheet to an adjacent steel sheet, and iron loss decreases.

[0067] In the present invention, the stress region 12 and the stress distribution region M are defined as described above. The effects of the present invention are realized when the stress region 12 exists within the stress distribution region M. In this case, it is not necessary for the entire stress region 12 to exist within the stress distribution region M. The effects of the present invention can be realized as long as only a portion of one stress region 12 overlaps the stress distribution region M. Furthermore, the effects of the present invention can be realized even when only a portion of the stacked steel plates overlaps the stress distribution region M. The degree of overlap of the above regions is preferably 0.1% or greater, where Ptot is the total area of ​​the stress distribution region M within the observation region and PM is the total area of ​​the stress regions 12 within the stress distribution region M when observing a region that is 1 / 2 the stack thickness in the Z-axis direction and 1 / 2 the stack thickness in the X-axis direction. PM / Ptot is less than 0.1%, and sufficient effects of the present invention cannot be achieved. The ratio is preferably 2% or greater, and more preferably 5% or greater. On the other hand, the stress regions 12 also act as an obstacle to magnetic flux in the in-plane direction (magnetization direction) of the steel sheet, and therefore, excessive presence of the stress regions 12 in the stress distribution region M can cause deterioration in iron loss. For this reason, it is preferable that PM / Ptot is 40% or less, and more preferably 30% or less.

[0068] In the present invention, the degree of overlap is defined as the ratio of the number of steel plates SM in which a stress region 12 exists within a stress distribution region M to the total number of stacked steel plates Stot. A steel plate in which a stress region 12 exists within a stress distribution region M is a steel plate in which at least one stress region 12 exists within at least one stress distribution region M. In the present invention, SM / Stot is preferably 1% or more, more preferably 2% or more, more preferably 5% or more, and even more preferably 10% or more. Of course, it is preferable that all steel plates have stress regions 12 within their stress distribution regions M, i.e., 100%.

[0069] Since the stress region 12 can be an obstacle to magnetic flux in the in-plane direction of the steel sheet and can cause iron loss deterioration, the stress region 12 is provided only within the stress distribution region M, and the stress region 12 does not have to be provided outside the stress distribution region M. In other words, tensile stress may be introduced only in the stress distribution region M.

[0070] The winding direction of the wound core may be the rolling direction of the steel sheet. The winding direction of the wound core may also be the {110}<001> direction of the steel sheet. Furthermore, in the descriptions of Figures 7A, 7B, 8A, 8B, 9A, and 9B, the X-axis direction may be the rolling direction of the steel sheet or the {110}<001> direction of the steel sheet.

[0071] The method for producing the grain-oriented electrical steel sheet is not particularly limited, and any conventionally known method for producing a grain-oriented electrical steel sheet can be appropriately selected. A preferred specific example of the production method is a method in which a slab having the chemical composition of the grain-oriented electrical steel sheet, except for 0.04 to 0.1 mass %, is heated to 1000°C or higher and hot-rolled, and then annealed as needed, followed by cold-rolling once or twice or more times with intermediate annealing in between to form a cold-rolled steel sheet, which is then heated to 700 to 900°C in a wet hydrogen-inert gas atmosphere to be decarburized and annealed as needed, and further nitriding annealed as needed, and then coated with an annealing separator, followed by finish annealing at about 1000°C, and then forming an insulating coating at about 900°C.

[0072] In addition, in this embodiment, the wound core made up of grain-oriented electromagnetic steel sheets 1 having the above-described configuration is formed by stacking grain-oriented electromagnetic steel sheets 1 that have been individually bent in layers and assembling them into a wound shape, and multiple grain-oriented electromagnetic steel sheets 1 are connected to each other via at least one joint 6 per turn.

[0073] In this embodiment, a method for introducing tensile stress in the thickness direction into the grain-oriented electrical steel sheet is, for example, a method of irradiating with a laser or electron beam, and irradiating in a medium in which the viscosity (mPa·s) of the aqueous solution is 2 to 8 reduces vibration of the steel sheet due to irradiation with the laser or electron beam, making it easier to obtain the desired stress distribution. If the viscosity exceeds 8, it becomes difficult to introduce stress. A method in which the viscosity is controlled by the concentration and temperature of the aqueous solution is desirable because the conditions can be adjusted appropriately. For example, a method using an aqueous ethanol solution with a concentration of 40 to 60% at a temperature of -10°C to 20°C is a preferred example.

[0074] Furthermore, with regard to the timing of introducing tensile stress into the steel sheet, tensile stress may be introduced when the steel sheet is in the coil stage before being cut in the rolling direction, or tensile stress may be introduced when the steel sheet is bent.

[0075] An apparatus that enables the manufacture of a wound core involving the above-described bending of steel sheets is shown schematically in a block diagram in Figure 10. Figure 10 shows a schematic diagram of a manufacturing apparatus 70 for a wound core in the form of a unicore, and this manufacturing apparatus 70 includes a bending unit 71 that individually bends grain-oriented electrical steel sheets 1, and may also include an assembly unit 72 that stacks the folded grain-oriented electrical steel sheets 1 in layers and assembles them into a wound shape, thereby forming a wound core that includes a portion where grain-oriented electrical steel sheets 1, in which flat portions 4 and bent portions 5 are alternately continuous in the longitudinal direction, are stacked in the sheet thickness direction.

[0076] The grain-oriented electromagnetic steel sheet 1 is fed to the bending processing unit 71 by being unwound at a predetermined transport speed from a steel sheet supply unit 75 that holds a hoop material formed by winding the grain-oriented electromagnetic steel sheet 1 in a roll. The grain-oriented electromagnetic steel sheet 1 thus fed is cut to an appropriate size in the bending processing unit 71 and is then subjected to a bending process in which the grain-oriented electromagnetic steel sheet 1 is individually bent in small batches, such as one by one.

[0077] The bending processing portion 71 includes a tensile stress introduction portion 71 a. The tensile stress introduction portion 71 a introduces tensile stress into the grain-oriented electrical steel sheet 1 before cutting the grain-oriented electrical steel sheet 1 or during bending after cutting the grain-oriented electrical steel sheet 1 by the method described above.

[0078] When introducing tensile stress only into the stress distribution region M, the stress distribution region M in each grain-oriented electrical steel sheet 1 is determined in design based on the expected position of each grain-oriented electrical steel sheet 1 when the grain-oriented electrical steel sheets 1, each having alternating succession of flat portions 4 and bent portions 5, are stacked in the sheet thickness direction. For this reason, it is possible to introduce tensile stress only into the stress distribution region M by irradiating each grain-oriented electrical steel sheet 1 with a laser, electron beam, or the like at an expected position that will become the stress distribution region M in the design.

[0079] In the grain-oriented electrical steel sheet 1 obtained in this manner, the radius of curvature of the bent portion 5 generated by the bending process is extremely small, and therefore the bending process imparts extremely small processing strain to the grain-oriented electrical steel sheet 1. While it is assumed that the density of processing strain will increase in this way, if the volume affected by the processing strain can be reduced, the annealing step can be omitted.

[0080] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and any embodiment that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included within the technical scope of the present disclosure.

[0081] The present disclosure will be specifically described below using examples. Note that the conditions in the examples are examples adopted to confirm the feasibility and effects of the present disclosure, and the present disclosure is not limited to the conditions in the examples. Various conditions may be adopted in the present disclosure as long as they do not deviate from the gist of the disclosure and the purpose is achieved.

[0082] In this example, a laser irradiation method is used to introduce tensile stress into a steel sheet. First, a laser was irradiated onto the steel sheet in ethanol at a temperature of about 3°C ​​to 15°C to introduce tensile stress into the steel sheet. Further, a laser was irradiated onto the steel sheet in air, in water at 24°C, and in ethanol at 24°C to introduce tensile stress into the steel sheet.

[0083] At this time, the beam diameter was set to 150 μm under all conditions, and the output was appropriately adjusted, and the laser was irradiated in advance onto the steel plate portion corresponding to the joint 6 .

[0084] The steel plates thus obtained, A, B, C, D, D-2, E, F, G, H, I, J, K, L, M, M-2, M-3, M-4, N, O, P, Q, R, S, T, U, V, W, Z, AA, BB, CC, CC-2, CC-3, CC-4, CC-5, CC-6, DD, EE, FF, and GG, are shown in Table 1 below.

[0085]

[0086] A wound core was then produced from the steel sheets shown in Table 1. Detailed dimensions of the wound core are shown in FIG. 11 and Table 2. Note that the overlap length in Table 2 indicates the distance between two adjacent joints 6 in the X-axis direction (for example, the length from the end of gap 6(n) on the positive side of the X-axis to the end of gap 6(n-1) on the negative side of the X-axis shown in FIG. 7A). The number of steps is the number of steel sheets by which the joints 6 are periodically shifted in the X-axis direction ("6" in FIG. 7A).

[0087]

[0088] The iron loss of the wound core was then evaluated, and the results are shown in Table 3 below.

[0089]

[0090] In the evaluations in Table 3, iron loss at 50 Hz and a magnetic flux density of 1.7 T was measured by the excitation current method. Test Nos. 8 to 55, in which a tensile stress of 10 MPa or more was introduced, had a low iron loss ratio, while Test Nos. 1 to 7, in which a tensile stress of less than 10 MPa was introduced, had a high iron loss ratio. As shown in Tables 1 and 3, the iron loss ratios of steel sheets B, C, D, D-2, E, F, G, H, I, J, K, L, M, M-2, M-3, M-4, N, O, P, Q, R, S, T, U, V, W, Z, AA, BB, CC, CC-2, CC-3, CC-4, CC-5, CC-6, DD, EE, FF, and GG, in which a tensile stress of 10 MPa or more was introduced in the thickness direction, were 1.14 or less. On the other hand, in steel sheet A in which a tensile stress of 10 MPa or more was not introduced in the sheet thickness direction, the iron loss ratio exceeded 1.14.

[0091] Furthermore, as shown in Table 3, the examples of the invention in which SM / Stot was 2% or more had a lower iron loss ratio than the examples of the invention in which SM / Stot was less than 2%, and the iron loss ratio decreased significantly as SM / Stot increased.

[0092] Furthermore, as shown in Table 3, the examples of the invention in which PM / Ptot was 0.1% or more had a lower iron loss ratio than the examples of the invention in which PM / Ptot was less than 0.1%, and the iron loss ratio decreased significantly as PM / Ptot increased.

[0093] DESCRIPTION OF SYMBOLS 1 Grain-oriented electrical steel sheet 2 Laminated structure 3 Corner portion 4, 4a Planar portion 5 Bent portion 6 Joint portion 10 Wound core 12 Region 15 Hollow portion 70 Manufacturing device 71 Processing portion 71a Tensile stress introduction portion 72 Assembly portion 75 Steel sheet supply portion

Claims

1. A wound core having a wound shape formed by stacking folded steel plates, wherein, in a side view of the wound shape seen from a direction along the faces of the steel plates, the wound core has four flat portions and four corner portions adjacent to the flat portions, thereby forming a rectangular shape with a hollow portion in the center, each layer of the steel plates has at least one joint where ends in the winding direction are butted together, and at the joint of the steel plates of each layer, a gap exists between the opposing ends of the steel plates, and a tensile stress of 10 MPa or more is introduced in the thickness direction of the steel plates at one or more locations in a specified region that is defined in accordance with the positional relationship between the gap of a steel plate and the gap of a steel plate stacked adjacent to the given steel plate, in a cross section perpendicular to the faces of the steel plates and along the winding direction.

2. A wound core as set forth in claim 1, wherein the joints of the steel plates of each layer are arranged on the flat surface, and the joints of the steel plates of each layer are arranged with a periodic shift in the extending direction of the flat surface.

3. A wound core as described in claim 1 or 2, in which, in a wound core in which steel plates are laminated, SM is the number of steel plates into which tensile stress in the plate thickness direction is introduced within the specified region, and Stot is the total number of laminated steel plates, and SM / Stot is 1% or more.

4. A wound core as claimed in claim 1 or 2, in which, in a wound core in which steel sheets are laminated, when the area of ​​the region in which the tensile stress in the sheet thickness direction within the specified region is PM and the total area of ​​the specified region is Ptot, PM / Ptot is 0.1% or more.

5. A wound core as claimed in claim 1 or 2, wherein the maximum value of the tensile stress is equal to or less than the yield stress of the steel plate.

6. A wound core as claimed in claim 1 or 2, characterized in that in the cross section perpendicular to the plane of the steel plate and along the winding direction, the region into which the tensile stress is introduced has a width in the winding direction of one of the regions not exceeding 1.4 mm.

7. A wound core as claimed in claim 1 or 2, characterized in that in the cross section perpendicular to the surface of the steel plate and along the winding direction, the length in the plate thickness direction of one of the regions to which the tensile stress has been introduced is between 0.2 and 1 times the plate thickness.

8. A wound core as claimed in claim 1 or 2, wherein in the cross section perpendicular to the surface of the steel plate and along the winding direction, the distance between adjacent regions in the winding direction to which the tensile stress has been introduced is 2 mm or more and 10 mm or less.

9. A wound core according to claim 1 or 2, characterized in that in the region where the tensile stress is introduced, the point at which the tensile stress is maximum is present at a depth of more than 10 μm from the surface of the steel sheet material.

10. A wound core as described in claim 1 or 2, wherein the region into which the tensile stress is introduced extends continuously or at predetermined intervals in a direction intersecting the winding direction of the steel plate and is provided so as to cross the winding direction.

11. A wound core according to claim 1 or 2, wherein the winding direction coincides with the {110}<001> direction of the steel sheets.

12. A wound core according to claim 1 or 2, wherein the winding direction coincides with the rolling direction of the steel sheet.

13. A wound core according to claim 1 or 2, wherein the tensile stress is introduced only to the specified region in the cross section perpendicular to the surface of the steel plate and along the winding direction.

14. A method for manufacturing a wound core as claimed in claim 1 or 2, comprising the steps of: bending a steel sheet; cutting the steel sheet; stacking the folded and cut steel sheets in layers and assembling them into a wound shape by butting ends in the winding direction together; and introducing a tensile stress in the sheet thickness direction near the ends or near positions that would become the ends before cutting.

Citation Information

Patent Citations

  • Low core loss grain-oriented magnetic steel sheet

    JP2008127632A

  • Wound core

    JP2022078444A

  • Winding iron core, method for manufacturing winding iron core, and winding iron core manufacturing apparatus