Environment-friendly thermoplastic elastomer composition and article produced therefrom
The thermoplastic elastomer composition, combining thermoplastic elastomer, polyolefin resin, vegetable oil, and inorganic filler, addresses the limitations of conventional compositions by enhancing eco-friendliness, thermal stability, and reducing odors, resulting in improved performance and applicability.
Patent Information
- Application Number
- PCT/KR2024/006665
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-16
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional thermoplastic elastomer compositions using petroleum-derived mineral oils face issues with environmental friendliness, thermal decomposition stability, moldability, slip properties, and unpleasant odors, which limit their eco-friendliness and performance.
A thermoplastic elastomer composition comprising 100 parts of thermoplastic elastomer, 3 to 25 parts of polyolefin resin, 50 to 200 parts of vegetable oil with a pyrolysis start temperature of 325 to 365°C, and 5 to 30 parts of inorganic filler, which improves eco-friendliness, thermal decomposition stability, moldability, and reduces unpleasant odors while maintaining mechanical properties.
The composition achieves excellent environmental friendliness, thermal decomposition stability, moldability, slip properties, and low hardness characteristics, effectively reducing unpleasant odors and maintaining mechanical properties, making it suitable for various applications such as gaskets and automobile parts.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Eco-friendly thermoplastic elastomer composition and molded article formed therefrom
[0001] The present invention relates to an environmentally friendly thermoplastic elastomer composition and a molded article formed therefrom. More specifically, the present invention relates to a thermoplastic elastomer composition that exhibits excellent environmental friendliness, thermal decomposition stability, moldability, slip properties, and low hardness, and that can reduce unpleasant odors, and a molded article formed therefrom.
[0002]
[0003] Unlike solid rubbers that are chemically cross-linked, thermoplastic elastomers (TPEs) are physically cross-linked. This allows them to exhibit the elasticity of solid rubbers at room temperature and allow for free extrusion and injection molding. Thermoplastic elastomers are normally composed of long molecules coiled randomly. When tensile force is applied to a thermoplastic elastomer, the molecules elongate in the direction of the force. When the force is removed, the molecules quickly return to their original, disordered arrangement. Due to the advantages of thermoplastic elastomers, such as easy processability and elastic resilience, demand has rapidly increased as a replacement for non-recyclable rubber, leading to the development of various products. For example, thermoplastic elastomers can be applied to a wide range of applications, including construction gaskets, automotive parts, handles, hoses, cushioning materials, and wire insulators.
[0004] When petroleum-derived mineral oils, such as paraffin oil, are applied to thermoplastic elastomer compositions, hardness, moldability, and compression set (C.Set) can be controlled. However, these mineral oils can cause environmental degradation, unpleasant odors, and poor appearance.
[0005] Therefore, there is a need to develop a thermoplastic elastomer composition that has excellent environmental friendliness, thermal decomposition stability, formability, slipperiness, low hardness, and other properties, and can reduce unpleasant odors.
[0006] The background technology of the present invention is disclosed in Korean Patent Publication No. 10-2016-0114994, etc.
[0007]
[0008] The purpose of the present invention is to provide a thermoplastic elastomer composition having excellent environmental friendliness, thermal decomposition stability, formability, slipperiness, low hardness, etc., and capable of reducing unpleasant odor.
[0009] Another object of the present invention is to provide a molded article formed from the thermoplastic elastomer composition.
[0010] The above and other objects of the present invention can all be achieved by the present invention described below.
[0011]
[0012] 1. One aspect of the present invention relates to a thermoplastic elastomer composition. The thermoplastic elastomer composition comprises: about 100 parts by weight of a thermoplastic elastomer; about 3 to about 25 parts by weight of a polyolefin resin; about 50 to about 200 parts by weight of a vegetable oil having a thermal decomposition initiation temperature of about 325 to about 365°C; and about 5 to about 30 parts by weight of an inorganic filler.
[0013] 2. In the above 1 specific example, the thermoplastic elastomer may have a weight average molecular weight of about 100,000 to about 450,000 g / mol.
[0014] 3. In the above 1 or 2 specific examples, the polyolefin resin may include at least one of polypropylene; a random copolymer in which two or more monomers of propylene, ethylene, butylene, and octene are polymerized; a block copolymer in which ethylene-propylene rubber is blended with polypropylene; polyethylene; an ethylene-vinylacetate copolymer; and a copolymer of α-olefin.
[0015] 4. In the above specific examples 1 to 3, the polyolefin resin may have a weight average molecular weight of about 100,000 to about 550,000 g / mol.
[0016] 5. In the above specific examples 1 to 4, the polyolefin resin may have a melt flow index (MI) of about 0.5 to about 40 g / 10 min, measured under conditions of 190°C and 2.16 kg load, according to ASTM D1238.
[0017] 6. In the above 1 to 5 specific examples, the vegetable oil may include at least one of olive oil, canola oil, and grape seed oil.
[0018] 7. In the above 1 to 6 specific examples, the inorganic filler may include at least one of talc, calcium carbonate, clay, wollastonite, mica, whiskers, and glass fibers.
[0019] 8. In the above 1 to 7 specific examples, the thermoplastic elastomer composition may have a thermal decomposition onset temperature of about 387 to about 413°C, measured using a thermogravimetric analysis (TGA) method at a heating rate of 20°C / min, a temperature range of 30 to 850°C, and a nitrogen (N2) atmosphere.
[0020] 9. In the above 1 to 8 specific examples, the thermoplastic elastomer composition may have a melt-flow index (MI) of about 15 to about 50 g / 10 min, measured under conditions of 230°C and 5 kgf load, according to ISO 1133.
[0021] 10. In the above 1 to 9 specific examples, the thermoplastic elastomer composition may have an adhesiveness of about 0.05 to about 0.30 as measured using a scratch resistance tester.
[0022] 11. In the above 1 to 10 specific examples, the thermoplastic elastomer composition may have a Shore A hardness of about 30 to about 70, measured using a Shore A durometer after overlapping three 2 mm thick specimens according to ISO 868.
[0023] 12. In the above 1 to 11 specific examples, the thermoplastic elastomer composition may have an odor generation level of 7 to 8 as measured according to the odor evaluation method of GEELY automobiles.
[0024] 13. Another aspect of the present invention relates to a molded article. The molded article is characterized in that it is formed from a thermoplastic elastomer composition according to any one of 1 to 12.
[0025]
[0026] The present invention has the effect of providing a thermoplastic elastomer composition having excellent environmental friendliness, thermal decomposition stability, formability, slipperiness, low hardness, etc., and capable of reducing unpleasant odor, and a molded article formed therefrom.
[0027]
[0028] Hereinafter, the present invention will be described in detail as follows.
[0029] A thermoplastic elastomer composition according to the present invention comprises (A) a thermoplastic elastomer; (B) a polyolefin resin; (C) a vegetable oil; and (D) an inorganic filler.
[0030] In this specification, “a to b” indicating a numerical range is defined as “≥a and ≤b”.
[0031]
[0032] (A) Thermoplastic elastomer
[0033] According to one specific example of the present invention, a thermoplastic elastomer can be applied together with a polyolefin resin, a specific vegetable oil, an inorganic filler, etc., to improve environmental friendliness, thermal decomposition stability, moldability, slipperiness, low hardness characteristics, etc., without deteriorating the mechanical properties of the thermoplastic elastomer composition, and can reduce unpleasant odors. As such, a styrenic thermoplastic elastomer, an amide thermoplastic elastomer, a urethane thermoplastic elastomer, an ester thermoplastic elastomer, etc., which are used in a typical thermoplastic elastomer composition, can be used. Preferably, a styrenic thermoplastic elastomer such as a styrene-ethylene / butylene-styrene (SEBS) copolymer can be used.
[0034] In a specific example, the thermoplastic elastomer may have a weight average molecular weight measured by gel permeation chromatography (GPC) of about 100,000 to about 450,000 g / mol, for example, about 150,000 to about 400,000 g / mol. Within this range, the thermoplastic elastomer composition may have excellent mechanical properties, elastic recovery properties, etc.
[0035]
[0036] (B) Polyolefin resin
[0037] A polyolefin resin according to one specific example of the present invention can be applied together with a thermoplastic elastomer, a specific vegetable oil, an inorganic filler, etc., to improve environmental friendliness, thermal decomposition stability, processability, moldability, slipperiness, low hardness characteristics, etc., without deteriorating the mechanical properties of the thermoplastic elastomer composition, and can reduce unpleasant odors. A polyolefin resin used in a typical thermoplastic resin composition can be used.
[0038] In specific examples, the polyolefin resin may include polypropylene; a random copolymer in which two or more monomers of propylene, ethylene, butylene, and octene are polymerized; a block copolymer in which ethylene-propylene rubber is blended with polypropylene; polyethylene; an ethylene-vinylacetate copolymer; a copolymer of α-olefins; a combination thereof, and the like.
[0039] In a specific example, the polyolefin resin may have a weight average molecular weight measured by GPC of about 100,000 to about 550,000 g / mol, for example, about 150,000 to about 500,000 g / mol. Within this range, the mechanical properties, elastic recovery properties, etc. of the thermoplastic elastomer composition may be excellent.
[0040] In a specific example, the polyolefin resin may have a melt flow index of about 0.5 to about 40 g / 10 min, for example, about 0.8 to about 40 g / 10 min, measured under conditions of 190°C and a load of 2.16 kg according to ASTM D1238. Within this range, the moldability of the thermoplastic elastomer composition may be excellent.
[0041] In a specific example, the polyolefin resin may be included in an amount of about 3 to about 25 parts by weight, for example, about 5 to about 20 parts by weight, based on about 100 parts by weight of the thermoplastic elastomer. If the content of the polyolefin resin is less than about 3 parts by weight based on about 100 parts by weight of the thermoplastic elastomer, there is a concern that the moldability, slipperiness, etc. may deteriorate and an unpleasant odor may not be reduced, and if it exceeds about 25 parts by weight, the thermal decomposition stability, slipperiness, etc. of the thermoplastic elastomer composition may deteriorate and the melt flow index may excessively increase, which may deteriorate workability (control of molding conditions).
[0042]
[0043] (C) Vegetable oil
[0044] According to one specific example of the present invention, a vegetable oil is an eco-friendly material, and when applied together with a thermoplastic elastomer, a polyolefin resin, an inorganic filler, etc., it can improve the eco-friendliness, thermal decomposition stability, moldability, slipperiness, low hardness characteristics, etc. without deteriorating the mechanical properties of the thermoplastic elastomer composition, and can reduce unpleasant odors. As the vegetable oil, a vegetable oil derived from a plant and having a thermal decomposition temperature of about 325 to about 365°C can be used.
[0045] In a specific example, the vegetable oil may have a thermal decomposition temperature of about 325 to about 365°C, for example, about 325 to about 360°C, as measured using a thermal gravimetric analysis (TGA) method under conditions of a heating rate of 20°C / min, a temperature range of 30 to 850°C, and a nitrogen (N2) atmosphere. When the thermal decomposition temperature of the vegetable oil is less than about 325°C, the thermal decomposition stability, moldability, and / or slipperiness of the thermoplastic elastomer composition may deteriorate, and an unpleasant odor may not be reduced. When the thermal decomposition temperature exceeds about 365°C, the miscibility, moldability, and the like of the thermoplastic elastomer composition may deteriorate.
[0046] In specific examples, the vegetable oil may include olive oil, canola oil, grapeseed oil, combinations thereof, and the like.
[0047] In a specific example, the vegetable oil may have a kinematic viscosity measured at 40°C of about 90 to about 180 cSt, for example, about 100 to about 160 cSt, according to ASTM D445. Within this range, the thermoplastic elastomer composition may have excellent processability, flexibility, etc.
[0048] In a specific example, the vegetable oil may be included in an amount of about 50 to about 200 parts by weight, for example, 100 to 150 parts by weight, relative to about 100 parts by weight of the thermoplastic elastomer. If the content of the vegetable oil is less than about 50 parts by weight relative to about 100 parts by weight of the thermoplastic elastomer, the environmental friendliness, thermal decomposition stability, moldability, slipperiness, etc. of the thermoplastic elastomer composition may be reduced, and an unpleasant odor may not be reduced. If the content of the vegetable oil exceeds about 200 parts by weight, the slipperiness, workability (control of molding conditions), etc. of the thermoplastic elastomer composition may be reduced.
[0049] In a specific example, the weight ratio of the polyolefin resin and the vegetable oil may be from about 1:4 to about 1:50, for example from about 1:5 to about 1:20. In this range, the slip properties, low hardness properties, etc. of the thermoplastic elastomer composition may be better.
[0050]
[0051] (D) Weapon filler
[0052] An inorganic filler according to one specific example of the present invention can be applied together with a thermoplastic elastomer, a polyolefin resin, a specific vegetable oil, etc., to improve environmental friendliness, thermal decomposition stability, moldability, slipperiness, low hardness characteristics, etc., without deteriorating the mechanical properties of the thermoplastic elastomer composition, and can reduce unpleasant odors. Inorganic fillers used in conventional thermoplastic elastomer compositions can be used.
[0053] In specific examples, the inorganic filler may include talc, calcium carbonate, clay, wollastonite, mica, whiskers, glass fibers, combinations thereof, and the like. For example, the inorganic filler may include, but is not limited to, talc, calcium carbonate, combinations thereof, and the like.
[0054] In a specific example, the inorganic filler may have an average particle size (D50) of about 1.5 to about 3.5 μm, for example, about 1.65 to about 3.5 μm, as measured by a particle size analyzer (Malvern mastersizer 3000), a moisture content of about 0.3% or less, and a specific surface area of about 11,500 to about 13,500 cm 3 / g. In the above range, the thermoplastic elastomer composition may have excellent slip properties, low hardness properties, etc.
[0055] In a specific example, the inorganic filler may be included in an amount of about 5 to about 30 parts by weight, for example, about 10 to about 25 parts by weight, based on about 100 parts by weight of the thermoplastic elastomer. If the content of the inorganic filler is less than about 5 parts by weight based on about 100 parts by weight of the thermoplastic elastomer, there is a concern that the slipperiness, workability (control of molding conditions), etc. of the thermoplastic elastomer composition may be reduced, and if it exceeds about 30 parts by weight, there is a concern that the moldability, slipperiness, low-hardness characteristics, etc. of the thermoplastic elastomer composition may be reduced.
[0056] In a specific example, the weight ratio of the polyolefin resin and the inorganic filler may be from about 1:0.4 to about 1:5, for example from about 1:0.6 to about 1:3. In this range, the moldability, low hardness properties, etc. of the thermoplastic elastomer composition may be better.
[0057] In a specific example, the weight ratio of the vegetable oil and the inorganic filler may be from about 1:0.05 to about 1:0.5, for example from about 1:0.1 to about 1:0.25. Within this range, the thermoplastic elastomer composition may exhibit better slip properties, low hardness properties, and the like.
[0058]
[0059] A thermoplastic elastomer composition according to one embodiment of the present invention may further include additives included in conventional thermoplastic elastomer compositions. Examples of the additives include, but are not limited to, antioxidants, flame retardants, anti-drip agents, heat stabilizers, slip agents, and mixtures thereof. When the additives are used, the content thereof may be about 0.001 to about 40 parts by weight, for example, about 0.1 to about 10 parts by weight, based on about 100 parts by weight of the thermoplastic elastomer.
[0060]
[0061] A thermoplastic elastomer composition according to one specific example of the present invention may be in the form of pellets obtained by mixing the above components and melt-extruding them at about 150 to about 250°C, for example, about 170 to about 230°C, using a conventional twin-screw extruder.
[0062] In a specific example, the thermoplastic elastomer composition is environmentally friendly, with the content of the environmentally friendly material (vegetable oil) being about 50 parts by weight or more, for example, about 100 parts by weight or more, based on about 100 parts by weight of the thermoplastic elastomer.
[0063] In a specific example, the thermoplastic elastomer composition may have a thermal decomposition onset temperature of about 387 to about 413°C, for example, about 390 to about 410°C, measured using a thermogravimetric analysis (TGA) method in a nitrogen (N2) atmosphere at a heating rate of 20°C / min and a temperature range of 30 to 850°C.
[0064] In a specific example, the thermoplastic elastomer composition may have a melt flow index of about 15 to about 50 g / 10 min, for example, about 15 to about 45 g / 10 min, measured under conditions of 230°C and 5 kgf load according to ISO 1133.
[0065] In a specific example, the thermoplastic elastomer composition may have an adhesiveness measured using a scratch resistance tester of about 0.05 to about 0.30, for example, about 0.05 to about 0.25.
[0066] In a specific example, the thermoplastic elastomer composition may have a Shore A hardness of about 30 to about 70, for example, about 30 to about 60, as measured by a Shore A durometer after overlapping three 2 mm thick specimens according to ISO 868. If it is outside the above range, appropriate elasticity may not be obtained, and thus may not be suitable for the use of the present invention.
[0067] In a specific example, the thermoplastic elastomer composition may have an odor generation level of 7 to 8 as measured according to the odor evaluation method of GEELY automobiles.
[0068]
[0069] A molded article according to the present invention is formed from the thermoplastic elastomer composition. The thermoplastic elastomer composition can be manufactured in the form of pellets, and the manufactured pellets can be manufactured into various molded articles (products) through various molding methods such as injection molding, extrusion molding, vacuum molding, and casting molding. Such molding methods are well known to those skilled in the art to which the present invention pertains. The molded article has excellent environmental friendliness, thermal decomposition stability, moldability, slipperiness, and low hardness characteristics, and can reduce unpleasant odors, and is useful as sealing parts, shock absorbing parts, and the like, and is particularly useful as construction gaskets, automobile interior parts, and tool grips.
[0070]
[0071] Hereinafter, the present invention will be described in more detail through examples; however, these examples are for the purpose of explanation only and should not be construed as limiting the present invention.
[0072]
[0073] Example
[0074] Below, the specifications of each component used in the examples and comparative examples are as follows.
[0075] (A) Thermoplastic elastomer
[0076] Styrene-ethylene / butylene-styrene (SEBS) copolymer (manufacturer: Kraton Corp., product name: G1651, weight average molecular weight: approximately 350,000 g / mol) was used.
[0077] (B) Polyolefin resin
[0078] Polypropylene resin (random copolymer, manufacturer: Lotte Chemical, product name: SB-520, weight average molecular weight: approximately 450,000 g / mol, melt flow index (190°C, 2.16 kg load): approximately 1 g / 10 min) was used.
[0079] (C) Oil
[0080] (C1) Canola oil (Manufacturer: Lotte Confectionery, thermal decomposition start temperature: approximately 355℃) was used.
[0081] (C2) Olive oil (Manufacturer: Lotte Confectionery, thermal decomposition start temperature: approximately 333℃) was used.
[0082] (C3) Grape seed oil (Manufacturer: Lotte Confectionery, thermal decomposition start temperature: approximately 329℃) was used.
[0083] (C4) Paraffin oil (Manufacturer: Michang Petrochemical, Product Name: W-1900H, Thermal Decomposition Start Temperature: Approximately 230℃) was used.
[0084] (C5) Castor oil (Manufacturer: GIRNAR Ind., Product name: Castor oil, Thermal decomposition start temperature: approximately 324℃) was used.
[0085] (D) Weapon filler
[0086] Calcium carbonate (Manufacturer: KOCH, Product name: CMS-8000) was used.
[0087]
[0088] Examples 1 to 8 and Comparative Examples 1 to 8
[0089] Each of the above components was added in the amounts shown in Tables 2, 3, 4, and 5 below, and then extruded at a barrel temperature of approximately 220°C to produce pellets. The extrusion was performed using a twin-screw extruder with an L / D of 36 and a diameter of 45 mm, and the produced pellets were dried at approximately 100°C for approximately 4 hours or more, and then injection-molded in a 150-ton injection molding machine (cylinder temperature: approximately 200°C, mold temperature: approximately 40°C) to produce specimens. The physical properties of the produced specimens were evaluated using the following methods, and the results are shown in Tables 2, 3, 4, and 5 below.
[0090]
[0091] Method of measuring physical properties
[0092] (1) Thermal decomposition stability (unit: ℃): Using thermal gravimetric analysis (TGA), the thermal decomposition onset temperature was measured using a Q5000 instrument (manufacturer: TA Instrument, Pan Type: aluminum oxide (Al2O3) crucible) at a heating rate of 20℃ / min, in a temperature range of 30 to 850℃, and in a nitrogen (N2) atmosphere. It was determined that the higher the thermal decomposition onset temperature, the better the thermal decomposition stability.
[0093] (2) Formability (unit: g / 10 min): Melt flow index (MI) was measured under conditions of 230℃ and 5 kgf load according to ISO 1133. A higher melt flow index was considered to indicate better formability.
[0094] (3) Slip: Adhesion was calculated according to Equation 1 below.
[0095] [Formula 1]
[0096] Adhesion (μ) = Coefficient of static friction (μs) - Coefficient of dynamic friction (μk)
[0097] In the above equation 1, the static friction coefficient and the dynamic friction coefficient were measured by contacting a flat plate specimen measuring 2 mm × 50 mm × 150 mm with an indenter containing an aluminum tip (R-processed tip) with a load of 0.5 kgf using a Scratch Resistance Tester (manufacturer: Heidon, model number: type 18L) at a speed of 100 mm / sec. The friction coefficient measured from the force applied to the indenter in a stationary state was defined as the static friction coefficient, and the friction coefficient measured from the force applied to the indenter when moving was defined as the dynamic friction coefficient. It was determined that the lower the adhesiveness, the better the slipperiness.
[0098] (4) Hardness: According to ISO 868, three 2 mm thick specimens were overlapped and the Shore A hardness was measured using a Shore A durometer.
[0099] (5) Degree of odor occurrence (unit: grade): For 100 g of a pellet-shaped thermoplastic elastomer composition sample, in accordance with the Q / JLY J7110538C standard, which is the odor evaluation method of GEELY automobiles, five trained evaluators with experience in evaluating the standard's evaluation method more than 10 times evaluated the odor grade according to the criteria in Table 1 below, and the odor grades of each evaluator were averaged including the decimal point, and then the final grade was selected. According to Table 1 below, the lower the odor grade, the more unpleasant the odor.
[0100] Odor rating Detailed description Human senses 10 No odor Comfortable 9 Barely perceptible, difficult to identify the type of odor 8 Presence of odor detected, slightly comfortable 7 Non-irritating odor, clearly detected Certain irritating, tolerable 6 Slightly irritating odor, clearly detected 5 Moderately irritating odor, clearly detected Somewhat annoying, intolerable 4 Unpleasant odor, slightly less disgusting 3 Irritating odor, disgusting Irritating, nauseating 2 Irritating odor, very disgusting 1 Feeling short of breath, intolerable
[0101]
[0102] Example 1234 (A) (parts by weight) 100 100 100 100 (B) (parts by weight) 20 20 20 20 (C1) (parts by weight) 100 150--(C2) (parts by weight)--100-(C3) (parts by weight)---100 (C4) (parts by weight)----(C5) (parts by weight)----(D) (parts by weight) 15 15 15 15 Thermal decomposition start temperature 40 5 4 10 4 0 2 3 9 5 Melt flow index 30 35 34 3 4 Tackiness 0.13 0.10 0.23 0.17 Shore A hardness 44 33 49 5 1 Odor rating 78 77
[0103]
[0104] Example 5678 (A) (parts by weight) 100 100 100 100 (B) (parts by weight) 515 1515 (C1) (parts by weight) 100 100 100 100 (C2) (parts by weight) ---- (C3) (parts by weight) ---- (C4) (parts by weight) ---- (C5) (parts by weight) ---- (D) (parts by weight) 15 15 1025 Thermal decomposition start temperature 4 10 39 0 39 0 39 0 Melt flow index 1 5 28 32 15 Tackiness 0.10 0.18 0.20 0.08 Shore A hardness 4 3 5 5 4 5 5 3 Odor rating 7 7 7 7
[0105]
[0106] Comparative Example 1234 (A) (parts by weight) 100 100 100 100 (B) (parts by weight) 130 20 20 (C1) (parts by weight) 100 100 40 210 (C2) (parts by weight) ---- (C3) (parts by weight) ---- (C4) (parts by weight) ---- (C5) (parts by weight) ---- (D) (parts by weight) 15 15 15 15 Thermal decomposition start temperature 4 1 3 3 7 5 3 8 0 4 2 0 Melt flow index 1 2 5 5 1 3 5 5 Tackiness 0.36 0.32 0.47 0.39 Shore A hardness 3 3 6 2 6 4 4 2 Odor rating 6 7 6 8
[0107]
[0108] Comparative Example 5678 (A) (parts by weight) 100 100 100 100 (B) (parts by weight) 20 20 20 20 (C1) (parts by weight) -- 100 100 (C2) (parts by weight) -- (C3) (parts by weight) -- (C4) (parts by weight) 100 --- (C5) (parts by weight) - 100 -- (D) (parts by weight) 15 15 135 Thermal decomposition start temperature 38 33 8 5 40 5 40 5 Melt flow index 28 13 6 0 13 Adhesion 0.3 3 0.5 2 0.4 3 0.49 Shore A hardness 50 57 31 7 1 Odor rating 4477
[0109]
[0110] From the above results, it can be seen that the thermoplastic elastomer composition of the present invention has excellent environmental friendliness, thermal decomposition stability (thermolysis start temperature), moldability (melt flow index), slipperiness (adhesion), low hardness characteristics (Shore A hardness), etc., and can reduce unpleasant odor.
[0111] On the other hand, in the case of Comparative Example 1, where the content of polyolefin resin is less than the range of the present invention, it can be seen that the moldability, slipperiness, etc. are reduced and the unpleasant odor is not reduced, and in the case of Comparative Example 2, where the content of polyolefin resin exceeds the range of the present invention, there is a problem that the thermal decomposition stability, slipperiness, etc. are reduced and the melt flow index is too high, making it difficult to control the molding conditions. In the case of Comparative Example 3, where the content of vegetable oil is below the range of the present invention, it can be seen that the eco-friendliness, thermal decomposition stability, formability, slipperiness, etc. are deteriorated, and the unpleasant odor is not reduced. In the case of Comparative Example 4, where the content of vegetable oil exceeds the range of the present invention, it can be seen that the slipperiness, etc. are deteriorated, and the melt flow index becomes too high. In the case of Comparative Example 5, where paraffin oil (C4) having a thermal decomposition start temperature below the range of the present invention is applied instead of the vegetable oil of the present invention, it can be seen that the thermal decomposition stability, slipperiness, etc. are deteriorated, and the unpleasant odor is not reduced. In the case of Comparative Example 6, where castor oil (C5) having a thermal decomposition start temperature below the range of the present invention is applied, the thermal decomposition stability, formability, slipperiness, etc. are deteriorated, and the unpleasant odor is not reduced. In addition, in the case of Comparative Example 7, where the content of the inorganic filler is below the range of the present invention, it can be seen that the slipperiness, etc. are reduced and the melt flow index is too high, and in the case of Comparative Example 8, where the content of the inorganic filler exceeds the range of the present invention, it can be seen that the moldability, slipperiness, low hardness characteristics, etc. are reduced.
[0112]
[0113] The present invention has been described with reference to exemplary embodiments. Those skilled in the art will appreciate that the present invention can be implemented in modified forms without departing from its essential characteristics. Therefore, the disclosed embodiments should be considered illustrative rather than limiting. The scope of the present invention is set forth in the claims, not the foregoing description, and all differences within the scope equivalent thereto should be construed as being encompassed by the present invention.
Claims
1. About 100 parts by weight of thermoplastic elastomer; About 3 to about 25 parts by weight of polyolefin resin; About 50 to about 200 parts by weight of a vegetable oil having a thermal decomposition start temperature of about 325 to about 365°C; and A thermoplastic elastomer composition comprising about 5 to about 30 parts by weight of an inorganic filler.
2. A thermoplastic elastomer composition according to claim 1, characterized in that the thermoplastic elastomer has a weight average molecular weight of about 100,000 to about 450,000 g / mol.
3. A thermoplastic elastomer composition according to claim 1 or 2, wherein the polyolefin resin comprises at least one of polypropylene; a random copolymer in which two or more monomers selected from propylene, ethylene, butylene, and octene are polymerized; a block copolymer in which ethylene-propylene rubber is blended with polypropylene; polyethylene; an ethylene-vinylacetate copolymer; and a copolymer of α-olefin.
4. A thermoplastic elastomer composition according to any one of claims 1 to 3, wherein the polyolefin resin has a weight average molecular weight of about 100,000 to about 550,000 g / mol.
5. A thermoplastic elastomer composition according to any one of claims 1 to 4, wherein the polyolefin resin has a melt flow index of about 0.5 to about 40 g / 10 min, measured under conditions of 190°C and 2.16 kg load according to ASTM D1238.
6. A thermoplastic elastomer composition according to any one of claims 1 to 5, characterized in that the vegetable oil comprises at least one of olive oil, canola oil, and grape seed oil.
7. A thermoplastic elastomer composition according to any one of claims 1 to 6, wherein the inorganic filler comprises at least one of talc, calcium carbonate, clay, wollastonite, mica, whiskers, and glass fibers.
8. A thermoplastic elastomer composition according to any one of claims 1 to 7, characterized in that the thermoplastic elastomer composition has a thermal decomposition start temperature of about 387 to about 413°C as measured using a thermogravimetric analysis method.
9. A thermoplastic elastomer composition according to any one of claims 1 to 8, characterized in that the thermoplastic elastomer composition has a melt flow index of about 15 to about 50 g / 10 min, measured under conditions of 230°C and 5 kgf load according to ISO 1133.
10. A thermoplastic elastomer composition according to any one of claims 1 to 9, characterized in that the thermoplastic elastomer composition has an adhesiveness of about 0.05 to about 0.30 as measured using a scratch hardness measuring device.
11. A thermoplastic elastomer composition according to any one of claims 1 to 10, characterized in that the thermoplastic elastomer composition has a Shore A hardness of about 30 to about 70, measured using a Shore A durometer after overlapping three 2 mm thick specimens according to ISO 868.
12. A thermoplastic elastomer composition according to any one of claims 1 to 11, characterized in that the thermoplastic elastomer composition has an odor generation level of 7 to 8 as measured according to the odor evaluation method of GEELY automobiles.
13. A molded product characterized by being formed from a thermoplastic elastomer composition according to any one of claims 1 to 12.
Citation Information
Patent Citations
Thermoplastic elastomer
JP2006117767A
Elastomer composition
JP2010275458A
Eco-friendly bio floor prepared
KR1020090050225A
Nature - friendly soft MBS resin composition
KR1020160061300A
Thermoplastic elastomer compositions having biorenewable content
US20160376432A1