The laminated edge ring design with controlled Si:C or B:C ratios in semiconductor manufacturing addresses He gas leakage and adhesion issues, enhancing process stability and plasma resistance, thereby improving the reliability and cost-effectiveness of semiconductor manufacturing.

WO2024248375A1PCT designated stage expired Publication Date: 2024-12-05TOKAI CARBON KOREA CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/006700
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-05-17
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

CVD SiC edge rings in semiconductor manufacturing face issues with He gas leakage due to poor adhesion to other components and high hardness, leading to increased costs and process instability, especially at high temperatures.

Method used

A laminated edge ring design with a high-hardness upper layer (SiC or B4C) and a lower layer (C/SiC or C/B4) having lower hardness, where the lower layer is in contact with internal components, and the raw material ratio of Si:C or B:C is controlled to enhance adhesion and plasma resistance, using methods like CVD deposition and bonding.

Benefits of technology

The solution effectively prevents He gas leakage and improves adhesion to ceramic components, ensuring process stability and plasma resistance in harsh semiconductor manufacturing environments, reducing the risk of damage and costs associated with particle generation and bonding agent issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024006700_05122024_PF_FP_ABST
    Figure KR2024006700_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are an edge ring for a semiconductor manufacturing apparatus and a manufacturing method therefor. The edge ring for a semiconductor manufacturing apparatus comprises: an upper layer having high hardness; and a lower layer positioned below the upper layer and having lower hardness than the upper layer, wherein the lower layer may be positioned to be in contact with an internal component of a plasma etching apparatus.
Need to check novelty before this filing date? Find Prior Art

Description

Edge ring for semiconductor manufacturing equipment and manufacturing method thereof

[0001] The present invention relates to an edge ring for a semiconductor manufacturing device and a manufacturing method thereof.

[0002] In order to ensure the uniformity of plasma irradiated onto the wafer for the manufacture of wafer edge chips, temperature uniformity of the wafer and edge ring (or focus ring) must be ensured, and therefore, a smooth supply of He gas for cooling the edge ring and wafer is required.

[0003] CVD SiC material, which has high corrosion resistance for fine line width and multi-stage etching, has excellent plasma resistance characteristics, but has high hardness compared to silicon, which results in poor adhesion to other parts, and in cases where He leakage for cooling occurs, making product application impossible.

[0004] There is a hybrid method that attaches silicon to CVD SiC, making the lower part where other parts come into contact with silicon and bonding it to the upper part which is CVD SiC. However, there is a high possibility of particle generation during the process due to the use of adhesives, etc., and the manufacturing process is complicated, which can result in high costs due to increased manufacturing costs. In addition, the adhesive strength of the adhesive decreases at high temperatures, causing the CVD SiC part and silicon part to be pulled together, which can cause the upper CVD SiC part to warp or separate during the process.

[0005]

[0006] The present invention, in order to solve the above-mentioned problems, provides a component for semiconductor manufacturing equipment that not only improves adhesion with other components but also enhances plasma resistance by applying high-hardness and low-hardness materials. For example, the present invention can improve the He leakage phenomenon that occurs when using conventional CVD SiC edge rings, and provide an edge ring that not only improves adhesion with other components when installed in a semiconductor manufacturing equipment but also enhances plasma resistance.

[0007] The present invention provides a method for manufacturing a component for a semiconductor manufacturing device, which can manufacture a component for a semiconductor manufacturing device by a simple method such as a continuous deposition (e.g., CVD) process or bonding using a method for controlling the ratio of Si and C in raw materials supplied during a manufacturing process.

[0008] However, the problems to be solved by the present invention are not limited to those mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the description below.

[0009] An edge ring according to one embodiment includes an upper layer having a high hardness; and a lower layer positioned below the upper layer and having a lower hardness than the upper layer, wherein the lower layer may be positioned to contact an internal component of a plasma etching device.

[0010] In one embodiment, the upper layer may be formed of SiC or B4C.

[0011] In one embodiment, the thickness of the upper layer may be greater than or equal to 1 mm.

[0012] In one embodiment, the lower layer may be made of C / SiC or C / B4C.

[0013]

[0014] According to one embodiment, the lower layer may be a C / SiC material, and the atomic ratio of Si:C may be 1:1.4 to 1:1.6.

[0015] According to one embodiment, the lower layer may be a C / B4C material and the atomic ratio of B:C may be greater than 0:1 to less than 4:1.

[0016] In one embodiment, the Vickers hardness of the lower layer is 1000 kg f / mm 2 Up to 2000 kg f / mm 2It could be.

[0017] In one embodiment, the thickness of the lower layer may be 0.2 mm or greater.

[0018] According to one embodiment, the lower layer may be formed by deposition on the upper layer.

[0019] According to one embodiment, the edge ring may be deposited by a CVD method, and if the lower layer is C / SiC, the deposition may be performed while continuously changing the raw material ratio of Si and C, and if the lower layer is C / B4C, the deposition may be performed while continuously changing the raw material ratio of B and C.

[0020] According to one embodiment, the method for manufacturing an edge ring of the present invention may include forming a high-hardness upper layer, forming a lower layer having a lower hardness compared to the upper layer, and processing the upper layer into a part shape.

[0021] In one embodiment, when forming the upper layer, the upper layer may be formed by CVD, reaction sintering, or sintering.

[0022] In one embodiment, when forming the lower layer, the lower layer may be deposited on the upper layer.

[0023] According to one embodiment, when forming the lower layer, the lower layer may be deposited while continuously changing the raw material ratio of B:C or Si:C.

[0024] In one embodiment, when forming the lower layer, the upper layer and the lower layer may be bonded.

[0025] In one embodiment, bonding the upper layer and the lower layer may be accomplished by bonding using at least one or more of an adhesive, heat, and pressure, or a combination thereof.

[0026] A method for regenerating a composite material component for a semiconductor manufacturing device according to one embodiment is a method for regenerating an edge ring, comprising: a step of forming a lower layer on a lower surface of an upper layer of a focus ring; and a step of processing a shape of the focus ring to include the lower layer.

[0027] In one embodiment, the upper layer may comprise SiC or B4C, and the lower layer may comprise C / SiC or C / B4C.

[0028] According to one embodiment, the step of forming the lower layer may include forming the lower layer on at least one of the lower surface, upper surface, and side surface of the focus ring, wherein the upper surface may be a plasma exposed surface.

[0029] According to one embodiment, the step of processing the shape of the focus ring may be processing the shape so that the C / SiC coating layer becomes the lower surface of the focus ring.

[0030] According to one embodiment, the step of processing the shape of the focus ring may be processing the shape into a focus ring having an area designed for wafer mounting, the focus ring including an upper surface which is a plasma exposure surface, and a lower surface.

[0031] According to one embodiment, the step of forming a lower surface on at least one surface of the focus ring may include a step of attaching a coating jig to at least one surface of the focus ring; the step of attaching the coating jig may include a step of attaching the coating jig to an upper surface of the focus ring, and a step of depositing the lower surface on at least one surface of the focus ring to which the jig is attached; and the step of depositing the lower layer may include a step of depositing the lower layer on at least one surface excluding the surface on which the coating jig is formed, and a step of removing the coating jig after the step of depositing the lower layer.

[0032] According to one embodiment, the step may include shaping the lower surface and / or the upper surface of the focus ring.

[0033] According to one embodiment of the present invention, the present invention can provide a component (e.g., an edge ring) for a semiconductor manufacturing device and a method for manufacturing the same, which can prevent damage with excellent resistance in harsh environments (e.g., chemical environments such as plasma, high temperature, high pressure, gas, and etching) in a semiconductor manufacturing process, and can implement process stability by having excellent adhesion to other components (e.g., ceramic components) and a semiconductor substrate (e.g., a wafer substrate) within the semiconductor manufacturing device. According to one embodiment of the present invention, the semiconductor manufacturing device is an edge ring, and, for example, a part where He gas is injected for cooling in a semiconductor plasma treatment process and moves is made of a material (e.g., a C-rich material) having a hardness similar to or lower than silicon (e.g., C / SiC or C / B4C) to increase adhesion to other ceramic components, and a part exposed to plasma is made of a high-hardness material (e.g., SiC or B4C) to solve plasma resistance and He gas leakage problems.

[0034] FIG. 1a illustrates a configuration of an edge ring in which an upper layer (e.g., a SiC layer or B4C) and a lower layer (e.g., C / SiC or C / B4C) according to the present invention are laminated, according to one embodiment of the present invention.

[0035] FIG. 1b illustrates a configuration of an edge ring in which an upper layer (e.g., SiC layer or B4C), an adhesive layer, and a lower layer (e.g., C / SiC or C / B4C) according to the present invention are laminated, according to one embodiment of the present invention.

[0036] FIG. 2 shows the change in Vicker's hardness of a C / SiC material according to the Si:C raw material ratio according to one embodiment of the present invention.

[0037] FIG. 3a shows the crystal characteristics (XRD) of a SiC material layer (Si:C raw material ratio = 1:1 to 1.1) manufactured in an embodiment of the present invention, according to one embodiment of the present invention.

[0038] FIG. 3b shows the crystal characteristics (XRD) of a C / SiC material (Si: C raw material ratio = 1: 1.2 to 1.4) manufactured in an example according to one embodiment of the present invention.

[0039] Figure 3c shows the crystal characteristics (XRD) of a C / SiC material (Si:C raw material ratio = 1:1.5 to 1.6) manufactured in an example according to one embodiment of the present invention.

[0040] FIG. 4a shows an SEM image of the surface of a C / SiC material according to a Si:C raw material ratio (Si:C raw material ratio = 1:1.1) according to one embodiment of the present invention.

[0041] FIG. 4b shows an SEM image of the surface of a C / SiC material according to a Si:C raw material ratio (Si:C raw material ratio = 1:1.2) according to one embodiment of the present invention.

[0042] FIG. 4c shows an SEM image of the surface of a C / SiC material according to a Si:C raw material ratio (Si:C raw material ratio = 1:1.3) according to one embodiment of the present invention.

[0043] FIG. 4d shows an SEM image of the surface of a C / SiC material according to a Si:C raw material ratio (Si:C raw material ratio = 1:1.4) according to one embodiment of the present invention.

[0044] FIG. 4e shows an SEM image of the surface of a C / SiC material according to a Si:C raw material ratio (Si:C raw material ratio = 1:1.5) according to one embodiment of the present invention.

[0045] Figure 4f shows an SEM image of a C / SiC material layer according to the Si:C raw material ratio (Si:C raw material ratio = 1:1.6) of the composite material manufactured in Example 1.

[0046] FIG. 5a shows the crystal characteristics (XRD) of a B4C (B / C=4) material manufactured in an example according to one embodiment of the present invention.

[0047] FIG. 5b shows the crystal characteristics (XRD) of a C / B4C (B / C=1.2) material manufactured in an example according to one embodiment of the present invention.

[0048] FIG. 5c shows the crystal characteristics (XRD) of a C / B4C (B / C=0.6) composite material manufactured in an example according to one embodiment of the present invention.

[0049] Figure 6 shows the change in Vickers hardness of a C / B4C composite material according to the B / C ratio, according to one embodiment of the present invention.

[0050] FIG. 7 is an exemplary diagram illustrating a process of a method for regenerating a composite material component for a semiconductor manufacturing device according to the present invention (e.g., a method for regenerating a focus ring), according to one embodiment of the present invention.

[0051] FIG. 8 is an exemplary diagram illustrating a process of a method for regenerating a composite material component for a semiconductor manufacturing device according to the present invention (e.g., a method for regenerating a focus ring), according to another embodiment of the present invention.

[0052] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. In describing the present invention, detailed descriptions of related known functions or configurations will be omitted if it is determined that such detailed descriptions may unnecessarily obscure the gist of the present invention. In addition, the terms used in this specification are terms used to appropriately express preferred embodiments of the present invention, and may vary depending on the intention of the user or operator, or the customs of the field to which the present invention belongs. Therefore, the definitions of these terms should be determined based on the contents throughout this specification. The same reference numerals presented in each drawing represent the same elements.

[0053] Throughout the specification, when we say that an element is "on" another element, this includes not only cases where the element is in contact with the other element, but also cases where another element exists between the two elements.

[0054] Throughout the specification, when a part is said to "include" a component, this does not mean that it excludes other components, but rather that it may include other components.

[0055] Hereinafter, the edge ring for a semiconductor manufacturing device of the present invention and its manufacturing method will be described in detail with reference to examples and drawings. However, the present invention is not limited to these examples and drawings.

[0056] According to one embodiment of the present invention, the edge ring may include an upper layer (110) having a high hardness; and a lower layer (120) located below the upper layer and having a lower hardness than the upper layer (110).

[0057] According to one embodiment, the upper layer (110) may include SiC or B4C, and the lower layer (120) may include a C-rich material, for example, C / SiC or C / B4C. That is, since the C-rich material (e.g., C / SiC or C / B4C) has high processability and lower hardness than the upper layer (110), the He leak phenomenon due to the high hardness characteristic of the upper layer (110) can be solved. According to one embodiment of the present invention, the edge ring is formed of a C / SiC or C / B4C material in which amorphous carbon is uniformly distributed within SiC (e.g., CVD SiC) or B4C (e.g., CVD B4C) in the lower layer (120) that comes into contact with other components, and CVD SiC or CVD B4C having plasma resistance is formed in the plasma exposed area, thereby improving adhesion with other components and the He leak phenomenon. That is, CVD SiC or CVD B4C tends to have poor adhesion to other ceramic parts due to its high hardness, but adhesion to other parts can be improved by using C / SiC or C / B4C materials containing amorphous carbon with a hardness similar to silicon.

[0058] In one embodiment, the upper layer (110) has a plasma exposed surface, and the thickness of the upper layer (110) may be at least 1 mm or more; 1.5 mm or more; 1 mm to 10 mm; or 1 mm to 5 mm. The maximum or minimum thickness value may be selected from the mentioned values. If it is within the above thickness range, it may have plasma resistance and maintain adhesion when fixed to other ceramic components. In one embodiment, the upper layer (110) includes a portion (A) on which a semiconductor wafer substrate is mounted, and for example, the thickness (a) of the portion (A) may be at least 1 mm or more; 1.5 mm or more; or 1 mm to 5 mm.

[0059] According to one embodiment, the lower layer (120) may be positioned to contact an internal component (e.g., quartz) of a plasma etching device and may include a fastening portion (B) that is fixed and adhered to the internal component. The thickness of the lower layer (120) may be at least 0.2 mm or more; 0.3 mm or more; 0.5 mm or more; 0.2 mm to 10 mm; or 0.2 mm to 2 mm. It may correspond to a maximum or minimum thickness value among the mentioned values. When it is included within the above thickness range, it can have plasma resistance and maintain adhesion when fixed to other ceramic components.

[0060] According to one embodiment, the lower layer (120) is a lower surface having a contact surface with another component (e.g., quartz) and includes a fastening portion (B) that is fixed and adhered to the other component, and for example, the thickness (b) of the portion may be at least 0.2 mm or more; 0.3 mm or more; or 0.2 mm to 2 mm.

[0061] According to one embodiment, the lower layer (120) includes a C / SiC material, and the physical properties can be controlled by the ratio of raw materials during C / SiC deposition. For example, the raw material ratio of Si:C during deposition of the C / SiC composite layer (110) can be 1:1.4 to 1:1.6; 1:1.4 to 1:1.6 (less than); 1:1.41 to 1:1.59, 1:1.44 to 1:1.57; 1:1.49 to 1:1.57; or 1:1.5 to 1:1.55. By controlling the raw material ratio, damage to semiconductor components due to collision or impact in a semiconductor process such as a plasma environment can be prevented, and an appropriate Vickers hardness can be secured so that the edge ring has adhesion to other components.

[0062] According to one embodiment, the lower layer (120) includes a C / B4C material, and the physical properties can be controlled by the ratio of raw materials during C / B4C deposition, and the atomic ratio of B:C in the C / B4C material can be more than 0: less than 1 to 4: 1; 0.1: 1 to less than 4: 1; 0.2: 1 to 3: 1; 0.3: 1 to 2: 1; or 0.5: 1 to 1.5: 1, and by controlling the atomic ratio, damage to semiconductor components due to collision or impact in a semiconductor process such as a plasma environment can be prevented, and an appropriate Vickers hardness can be secured so that the edge ring has adhesion to other components.

[0063] In one embodiment, the Vickers hardness of the lower layer (120) (C / SiC or C / B4C) is 1000 kg f / mm 2 Up to 2000 kg f / mm 2 , and preferably may have a Vickers hardness similar to or lower than that of silicon.

[0064] The Vickers hardness of the above lower layer is 1000 kg f / mm 2 If it is less than 2000 kg, handling may be difficult due to impact or chipping from impact due to low hardness, and if the hardness of the lower layer is less than 2000 kg f / mm 2 If it exceeds, the high hardness may cause low adhesion to other parts, which may lead to a problem of He gas leakage.

[0065] According to one embodiment, the lower layer (120) and the upper layer (110) are formed by deposition, and a bonding layer-free (non-adhesive layer) (FIG. 1a) may be formed between the lower layer (120) and the upper layer (110). This can be achieved by increasing the carbon source from a certain thickness or more during the formation of the upper layer (110) (e.g., CVD SiC or CVD B4C) and forming a dense C / SiC composite layer or C / B4C with improved adhesion to other ceramic components through a continuous CVD deposition method.

[0066] According to one embodiment, the edge ring may be deposited by a CVD method, and if the lower layer (120) is C / SiC, the deposition may be performed while continuously changing the raw material ratio of Si and C, and if the lower layer (120) is C / B4C, the deposition may be performed while continuously changing the raw material ratio of B and C.

[0067] In one embodiment, when forming the upper layer (110), the upper layer (110) may be formed by CVD, reaction sintering, or sintering. In one embodiment, when forming the lower layer (120), the lower layer (120) may be deposited on the upper layer (110).

[0068] According to one embodiment, an upper layer (110) is formed on a substrate, and the substrate may be graphite or the like, but is not limited thereto. According to one embodiment, the upper layer (110) may be formed by CVD, reaction sintering, or sintering, for example, 1100 Inland 1700 ; or 1200 to control growth rate and raw material cost 1450 inland can be formed at a temperature of . The conditions mentioned may be process conditions applied to CVD, reaction sintering, or sintering. For example, 1100 Inland 1700 ; or 1200 to control growth rate and raw material cost 1450 inland and a pressure of 700 torr to 760 torr. The mentioned conditions may be process conditions applied to CVD, reaction sintering, or sintering. According to one embodiment, the raw material ratio of Si: C or the raw material ratio of B: C applied during deposition of each layer according to the temperature, the pressure, or both may be selected within the range of the raw material ratio of Si: C or the raw material ratio of B: C mentioned above in order to secure the properties of the edge ring, which is a component for a semiconductor manufacturing device of the present invention. According to one embodiment, when forming the lower layer (120), the lower layer (120) may be deposited while continuously changing the raw material ratio of B: C or Si: C.

[0069] According to one embodiment, the lower layer (120) and the upper layer (110) may be bonded to each other. For example, the bonding may be performed using at least one of heat, pressure, and an adhesive. According to one embodiment, when forming the lower layer (120), the upper layer (110) and the lower layer (120) may be bonded. According to one embodiment, bonding the upper layer (110) and the lower layer (120) may be performed using at least one of an adhesive, heat, and pressure, or a combination thereof. According to one embodiment, as shown in FIG. 1B, an edge ring including an adhesive layer (130) may be formed between the upper layer (110) and the lower layer (120). For example, the upper layer (110) and the lower layer (120) may be formed on a substrate, respectively, and an adhesive may be applied to the upper layer (110), the lower layer (120), or their surfaces, and then bonded. Heat, pressure, or both may be applied during bonding. Any adhesive that is applicable to ceramic bonding may be used without limitation.

[0070] According to one embodiment, the upper layer (110) and the lower layer (120) may be formed on a substrate, respectively, and the upper layer (110) and the lower layer (120) may be placed in contact with each other, and then bonded by applying heat, pressure, or both.

[0071] According to one embodiment, after forming the upper layer (110) and forming the lower layer (120), they can be processed into a component shape (edge ​​ring). For example, the edge ring can be processed so that the lower layer (120) (C / B4C layer or C / SiC layer), which is a part that comes into contact with other parts, is positioned, and the upper layer (110) (SiC layer or B4C layer) that is exposed to plasma and on which the semiconductor wafer is seated and in contact is positioned. The specific shape of the edge ring can utilize a shape and processing method known in the technical field of the present invention, and can be appropriately selected as long as it does not deviate from the purpose and scope of the present invention, and is not specifically mentioned in this specification.

[0072] Example 1

[0073] C / SiC materials were fabricated using the CVD method according to the Si / C ratios shown in Table 2. The XRD and Vickers hardness characteristics of the C / SiC materials were measured. The results are shown in Table 1 and Fig. 2.

[0074] The Vickers hardness of the C / SiC material according to the Si:C raw material ratio and process temperature of the composite material manufactured in Example 1 was measured and shown in Table 1 and Fig. 2.

[0075]

[0076] The XRD of the CSiC material according to the raw material ratio of Si:C and process temperature of the composite material manufactured in Example 1 was measured and shown in Figs. 3a to 3c, and the XRD peak values ​​are shown in Tables 2 and 3.

[0077] Looking at Table 1 and Figures 2 and 3a to 3c, it can be confirmed that when the Si:C raw material ratio is 1:1.5 or higher, crystalline SiC and crystalline carbon are formed and have low hardness. The Si:C raw material ratio is in the range of 1:1.44 to 1.49, which is similar to the Vickers hardness of silicon and quartz, and can provide excellent adhesion with silicon and quartz materials. That is, it can be confirmed that the hardness of the C / SiC material changes according to the Si:C ratio, as shown in Table 1 and Figure 2, and the Vickers hardness of silicon is 2080 kg f / mm 2 And Si: C raw material ratio is 1300 at process temperature ~ 1400 In 1:1.44 ~ 1.48, 1200 1300 inland In , the Si:C raw material ratio of 1:1.49 to 1.57, preferably 1:1.5 to 1.55, may be advantageous in securing adhesion with other parts. This may correspond to a C / SiC material that can implement hardness applicable to edge rings.

[0078] Table 2 shows the SiC (111) peak intensity values ​​measured by XRD of the CSiC material according to the raw material ratio of Si:C and process temperature of the composite material manufactured in Example 1.

[0079]

[0080] Table 3 shows the peak intensity value of carbon by measuring XRD of CSiC material according to the raw material ratio of Si:C and process temperature of the composite material manufactured in Example 1.

[0081]

[0082] Tables 2 and 3 show the SiC (111) diffraction intensity of C / SiC material and the diffraction intensity of carbon peak of CSiC material under each process condition. Si:C raw material ratio is 1:1.5 or more, and process temperature is 1300 From the above, it can be confirmed that the diffraction intensity of SiC (111) decreases and the diffraction intensity of carbon increases due to the increase in crystalline carbon.

[0083] Figure 3a shows Si:C raw material ratio = 1:1 to 1.1 (deposition temperature: 1300 ) is an XRD pattern of CSiC material, and Fig. 3b shows that the Si: C raw material ratio = 1: 1.2 ~ 1.4 (deposition temperature: 1300 ) is an XRD pattern of CSiC material, and Fig. 3c shows that the Si: C raw material ratio = 1: 1.5 ~ 1.6 (deposition temperature: 1300 ) is an XRD pattern of CSiC material. In Fig. 3c, it can be confirmed that the peak of crystalline carbon grows as the carbon raw material ratio increases.

[0084] FIGS. 4a, 4b, 4c, 4d, 4e, and 4f are SEM images of the C / SiC material layer according to the Si:C raw material ratio of the composite material manufactured in Example 1. FIG. 4a shows a Si:C raw material ratio of 1:1.1, FIG. 4b shows a Si:C raw material ratio of 1:1.2, FIG. 4c shows a Si:C raw material ratio of 1:1.3, FIG. 4d shows a Si:C raw material ratio of 1:1.4, FIG. 4e shows a Si:C raw material ratio of 1:1.5, and FIG. 4f shows a Si:C raw material ratio of 1:1.6. As can be seen from FIGS. 4a, 4b, 4c, 4d, 4e, and 4f, the microstructure of the surface of the C / SiC material changes and pores are formed as the Si:C raw material ratio increases.

[0085] Example 2

[0086] B4C and SiC materials were fabricated using the CVD method. The plasma etching rates for each material were evaluated and are shown in Table 4.

[0087]

[0088] * The etching improvement rate in Table 4 is the value related to CVD-B4C.

[0089] As shown in Table 4, it can be confirmed that the CVD B4C material has plasma corrosion resistance that is about 35% better than that of CVD SiC, and the present invention can provide an edge ring using a CVD B4C material having excellent plasma corrosion resistance.

[0090] Example 3

[0091] C / B4C materials were produced using the CVD method according to the B / C ratios shown in Table 2. XRD and Vickers hardness characteristics of the C / B4C materials were measured. The results are shown in Table 5 and Fig. 5.

[0092]

[0093] As shown in Figures 5a to 5c, the CVD B4C material shows carbon and B4C peaks in the XRD pattern. It can be confirmed that the intensity of the carbon peak increases as the B / C ratio decreases.

[0094] The hardness of the CVD B4C material tends to decrease with decreasing B / C ratio, as shown in Fig. 6 and Table 5. Here, the Vickers hardness of silicon is approximately 2080 kg. f / mm 2 And based on this standard, if the B / C ratio is 1.2 or less, it has a hardness lower than silicone and can secure adhesion with other parts.

[0095] Vickers hardness is 500 kg f / mm 2If it is less than 1000 kg, it may be difficult to handle due to the material being prone to chipping from impact or collision. f / mm 2 This is required and can be achieved with a B / C ratio of CB4C of 1 to 1.2.

[0096] The present invention bonds B4C (B / C ratio) of 4 and silicon or C-rich boron carbide (CBC) material having a B / C ratio of 1 to 1.2 through a physical or chemical bonding method, and such bonding material can be utilized as a material for an edge ring. That is, in the edge ring, the silicon or C-rich boron carbide part can be configured as a part that comes into contact with other ceramic parts, and the B4C can be configured as a part that is exposed to plasma. An edge ring having such a configuration can have improved plasma durability and adhesion to other parts.

[0097] The present invention can provide an edge ring formed with a C / B4C or C / SiC material having a high C content and a hardness similar to silicon in a part requiring adhesion with other ceramic parts, thereby securing the flame resistance of CVD SiC while resolving the low adhesion and He gas leakage due to the high hardness of the existing CVD SiC.

[0098] A method for regenerating a composite material component for a semiconductor manufacturing device according to one embodiment is a method for regenerating an edge ring, comprising: a step of forming a lower layer on a lower surface of an upper layer of a focus ring; and a step of processing a shape of the focus ring to include the lower layer.

[0099] FIG. 7 is an exemplary diagram illustrating a process of a method for regenerating a composite material component for a semiconductor manufacturing device according to the present invention (e.g., a method for regenerating a focus ring), according to one embodiment of the present invention.

[0100] FIG. 8 is an exemplary diagram illustrating a process of a method for regenerating a composite material component for a semiconductor manufacturing device according to the present invention (e.g., a method for regenerating a focus ring), according to another embodiment of the present invention.

[0101] Referring to FIGS. 7 and 8, FIGS. 7 and 8 illustrate a process of a reproduction method according to the shape of the focus ring (100) used, and may include a step (S110) of attaching a coating jig (200) on the upper surface in FIG. 7, a step (S120) of depositing a C / SiC coating layer (300) to surround the lower surface and the side surface; a step (S130) of removing the jig (200); and a step (S210) of processing the C / SiC coating layer (300); and a step (S220) of processing the upper surface. The C / SiC coating layer (300) may be processed in the step (S130) of removing the jig (200).

[0102] In Fig. 8, it may include a step of attaching a coating jig (200) on the upper surface (S110), a step of depositing a C / SiC coating layer (300) to surround the lower surface and the side surface (S120); a step of removing the jig (200) (S130); and a step of processing the upper surface (S220).

[0103] The step of processing the upper surface (S220) can remove a silicon or SiC layer damaged by etching, etc., from the used focus ring.

[0104] In one embodiment, the upper layer may comprise SiC or B4C, and the lower layer may comprise C / SiC or C / B4C.

[0105] According to one embodiment, the step of forming the lower layer may include forming the lower layer on at least one of the lower surface, upper surface, and side surface of the focus ring, wherein the upper surface may be a plasma exposed surface.

[0106] According to one embodiment, the step of processing the shape of the focus ring may be processing the shape so that the C / SiC coating layer becomes the lower surface of the focus ring.

[0107] According to one embodiment, the step of processing the shape of the focus ring may be processing the shape into a focus ring having an area designed for wafer mounting, the focus ring including an upper surface which is a plasma exposure surface, and a lower surface.

[0108] According to one embodiment, the step of forming a lower surface on at least one surface of the focus ring may include a step of attaching a coating jig to at least one surface of the focus ring; the step of attaching the coating jig may include a step of attaching the coating jig to an upper surface of the focus ring, and a step of depositing the lower surface on at least one surface of the focus ring to which the jig is attached; and the step of depositing the lower layer may include a step of depositing the lower layer on at least one surface excluding the surface on which the coating jig is formed, and a step of removing the coating jig after the step of depositing the lower layer.

[0109] According to one embodiment, the step may include shaping the lower surface and / or the upper surface of the focus ring.

[0110] Although the embodiments described above have been described with limited examples and drawings, those skilled in the art will recognize that various modifications and variations are possible based on the above teachings. For example, appropriate results can be achieved even if the described techniques are performed in a different order than described, and / or the described components are combined or combined in a different manner than described, or are replaced or substituted with other components or equivalents. Therefore, other implementations, other embodiments, and equivalents of the claims also fall within the scope of the claims described below.

Claims

1. An upper layer having high hardness; and A lower layer located below the upper layer and having a lower hardness than the upper layer is included. The lower layer is characterized in that it is positioned to be in contact with the internal components of the plasma etching device. Edge ring.

2. In paragraph 1, The upper layer is formed of SiC or B4C, Edge Ring 3. In paragraph 1, The thickness of the upper layer is 1 mm or more. Edge ring.

4. In paragraph 1, The above lower layer is made of C / SiC or C / B4C. Edge ring.

5. In paragraph 4, The above lower layer is made of C / SiC material. The atomic ratio of Si:C is 1:1.4 to 1:1.

6. Edge ring.

6. In paragraph 4, The above lower layer is made of C / B4C material. B: The atomic ratio of C is greater than 0: 1 to less than 4: 1, Edge ring.

7. In paragraph 1, The Vickers hardness of the above lower layer is 1000 kg f / mm 2 Up to 2000 kg f / mm 2 person, Edge Ring 8. In paragraph 1, The thickness of the above lower layer is 0.2 mm or more, Edge ring.

9. In paragraph 1, The above lower layer is formed by deposition on the upper layer, Edge ring.

10. In paragraph 9, The above edge ring is deposited by CVD method. If the above lower layer is C / SiC, the raw material ratio of Si and C is continuously changed and deposited, If the above lower layer is C / B4C, it is deposited while continuously changing the raw material ratio of B and C. Edge ring.

11. Form a high-hardness upper layer, Forming a lower layer with a lower hardness compared to the upper layer, Processing into the form of parts, Method for manufacturing edge rings.

12. In paragraph 11, When forming the upper layer The upper layer is formed by CVD, reaction sintering, or sintering. Method for manufacturing edge rings.

13. In paragraph 11, When forming the lower layer The lower layer is deposited on the upper layer, Method for manufacturing edge rings.

14. In paragraph 13, When forming the lower layer The lower layer is deposited by continuously changing the raw material ratio of B:C or Si:C. Method for manufacturing edge rings.

15. As a method of regenerating the edge ring of paragraph 1, A step of forming a lower layer on the lower surface of the upper layer of the focus ring; and A step of processing the shape of the focus ring to include a lower layer; including, Method for regenerating composite material parts for semiconductor manufacturing equipment.

16. In paragraph 15, The upper layer comprises SiC or B4C, The above lower layer comprises C / SiC or C / B4C, Method for regenerating composite material parts for semiconductor manufacturing equipment.

17. In paragraph 15, The step of forming the above lower layer is: Forming the lower layer on at least one of the lower surface, upper surface, and side surface of the above focus ring, The upper surface is a plasma exposure surface, Method for regenerating composite material parts for semiconductor manufacturing equipment.

18. In paragraph 15, The step of processing the shape of the above focus ring is: The C / SiC coating layer is shaped to form the lower surface of the focus ring. Method for regenerating SiC composite parts for semiconductor manufacturing equipment.

19. In paragraph 15, The step of processing the shape of the above focus ring is: having an area designed for wafer mounting, the upper surface being the plasma exposure surface; and It is shaped by processing a focus ring including a lower surface, Method for regenerating composite material parts for semiconductor manufacturing equipment.

20. In paragraph 15, The step of forming a lower surface on at least one side of the above focus ring is: Comprising a step of attaching a coating jig to at least one surface of the focus ring, The steps for attaching the coating jig are: Attaching a coating jig to the upper surface of the above focus ring, A step of depositing a lower surface on at least one side of a focus ring to which the above jig is attached; Including, The step of depositing the above lower layer is: The lower layer is deposited on at least one surface except the surface on which the coating jig is formed, A step of removing the coating jig after the step of depositing the lower layer is included. Method for regenerating composite material parts for semiconductor manufacturing equipment.

21. In paragraph 15, A step of processing the shape of the lower surface or / and the upper surface of the focus ring is included. Method for regenerating composite material parts for semiconductor manufacturing equipment.

Citation Information

Patent Citations

  • Part for semiconductor manufactoring, part for semiconductor manufactoring including complex coating layer and method of manufacturning the same

    KR1020180071747A

  • Electronic device

    KR1020220039053A

  • The decentralized user data storage and sharing system based on DID

    KR1020220120062A

  • Smart damper having variable damping force and washing machine

    KR1020230149707A

  • Method for Issuing Token Linked to Industrial Property Right of the Company

    KR1020240135446A