Cathode active material and lithium secondary battery including same

The positive electrode active material with a gradient of primary particle circumference addresses the structural and thermal stability issues in lithium secondary batteries by reducing the electrolyte contact area, improving lifespan and gas generation, and maintaining high capacity and conductivity.

WO2024248415A1PCT designated stage expired Publication Date: 2024-12-05POSCO FUTURE M CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/007025
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-05-21
Filing Date
2024-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

High-capacity lithium secondary batteries face issues with structural collapse and low thermal stability due to oxidation number problems in existing layered cathode active materials like LiNiO2, leading to deterioration and gas generation, which affects battery lifespan and reversibility.

Method used

A positive electrode active material composed of secondary particles with a specific gradient of primary particle circumference, where the average perimeter increases from the center to the surface, reducing the contact surface area with the electrolyte and stabilizing the battery, thereby suppressing deterioration and gas generation.

Benefits of technology

The solution enhances the lifespan stability and reduces gas generation in lithium secondary batteries by minimizing the specific surface area in contact with the electrolyte, preventing rock-salt phase formation and maintaining high capacity and conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024007025_05122024_PF_FP_ABST
    Figure KR2024007025_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A cathode active material according to the present invention is in the form of a secondary particle comprising a plurality of primary particles and satisfies relation 1, wherein relation 1 is represented by (the average circumference of the primary particles in the region from the center of the secondary particle to 2 / 3R to 3 / 3R) ≥ 1.5×(the average circumference of the primary particles in the region from the center of the secondary particle to 1 / 3R), and, in relation 1, R is the distance from the center of the secondary particle to the surface of the secondary particle. The cathode active material has suppressed deterioration and an excellent gas generation reduction effect.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode active material and lithium secondary battery containing the same

[0001] The present invention relates to a positive electrode active material, specifically, a positive electrode active material in the form of secondary particles including a plurality of primary particles, and a lithium secondary battery including the same.

[0002] Recently, with the explosive increase in demand for IT mobile devices, small electric power devices (e-bikes, small EVs, etc.), and energy storage systems (ESS; Energy Storage Systems), the development of high-capacity, high-energy-density secondary batteries to power these devices is actively underway worldwide. To manufacture these high-capacity batteries, high-capacity cathode materials must be used.

[0003] Among the existing layered cathode active materials, the material with the highest capacity is LiNiO2 (275 mAh / g), but its commercialization is difficult due to the low thermal stability caused by oxidation number problems that easily cause structural collapse during charge and discharge.

[0004] To solve these problems, the unstable Ni site must be replaced with another stable transition metal (Co, Mn, etc.), and for this purpose, a ternary NCM system with Co and Mn substituted was developed.

[0005] Conventional high-nickel NCM cathode active materials are composed of secondary particles in which primary particles are aggregated, and the circumference and size of the primary particles within the secondary particles are similar. In this case, the size of the primary particles located on the surface of the secondary particles that directly contact the electrolyte is as small as the size of the primary particles within the secondary particles, so the specific surface area of ​​the cathode active material increases. A cathode active material with a large specific surface area has the problem of deterioration of the cathode active material because the area in contact with the electrolyte increases.

[0006] When the positive electrode active material deteriorates, some stability issues may arise at the cell level due to gas generation, and when electrochemical reactions are repeated as charge / discharge progresses, some problems arise in which the reversibility of the positive electrode active material capacity is reduced as a rock-salt phase material is generated on the surface of the positive electrode active material.

[0007] Therefore, there is a need for the development of a cathode active material that can increase the life stability of a battery and reduce gas generation by reducing the specific surface area in contact with the electrolyte.

[0008] The present invention aims to provide a cathode active material that suppresses deterioration and has an excellent gas generation reduction effect.

[0009] In addition, the present invention seeks to provide a lithium secondary battery having excellent life stability and suppressing gas generation.

[0010] The present invention provides a positive electrode active material in the form of a secondary particle including a plurality of primary particles and satisfying the following equation 1.

[0011] [Formula 1]

[0012] (Average circumference of primary particles existing within a 2 / 3 to 3 / 3R region from the center of the secondary particles) ≥ 1.5 × (Average circumference of primary particles existing within a 1 / 3R region from the center of the secondary particles)

[0013] In the above equation 1,

[0014] R is the distance from the center of the secondary particle to the surface of the secondary particle.

[0015] In addition, the present invention provides a lithium secondary battery including a positive electrode including the positive electrode active material described above; a negative electrode; and a non-aqueous electrolyte.

[0016] The positive electrode active material according to the present invention has the advantage of suppressing deterioration and having an excellent gas generation reduction effect.

[0017] In addition, the lithium secondary battery according to the present invention has the advantages of excellent life stability and suppression of gas generation.

[0018] Figures 1 to 12 are images illustrating measurements of the perimeter of primary particles within each region of secondary particles of positive electrode active materials according to examples and comparative examples.

[0019] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples and are not intended to limit the present invention. The present invention is defined solely by the scope of the claims set forth below.

[0020] In the present invention, when it is said that a member is located “on” another member, this includes not only cases where a member is in direct contact with another member, but also cases where another member is interposed between the two members.

[0021] When a part of the present invention is said to "include" a certain component, this does not mean that other components are excluded, but rather that other components may be included, unless otherwise specifically stated.

[0022]

[0023] <Cathode active material>

[0024] One aspect of the present invention relates to a positive electrode active material in the form of secondary particles including a plurality of primary particles and satisfying the following equation 1.

[0025] [Formula 1]

[0026] (Average circumference of primary particles existing within a 2 / 3 to 3 / 3R region from the center of the secondary particles) ≥ 1.5 × (Average circumference of primary particles existing within a 1 / 3R region from the center of the secondary particles)

[0027] In the above equation 1,

[0028] R is the distance from the center of the secondary particle to the surface of the secondary particle.

[0029] The cathode active material according to the present invention has an average circumference of the primary particles that increases from the inside to the outside of the secondary particles. Therefore, the contact surface with the electrolyte can be reduced, thereby suppressing the phenomenon of deterioration in the lifespan and providing excellent gas generation reduction effects.

[0030]

[0031] In the present invention, "primary particle" means the smallest particle unit that can be distinguished as a single lump when observing a cross-section of a positive electrode active material through a scanning electron microscope (SEM), and may be composed of a single crystal grain or multiple crystal grains. Here, "crystal grain" means a distinct region in the form of a lattice structure in a certain direction formed by atoms within a primary particle.

[0032] Additionally, "secondary particle" means an aggregate formed by tens to hundreds of primary particles cohesively bonded together by physical or chemical bonding without any intentional cohesion or assembly process for the primary particles.

[0033]

[0034] In the present invention, the “average circumference” can be obtained from an image of a primary particle confirmed from a cross-sectional image obtained based on the center of the secondary particle.

[0035] Specifically, the average circumference of the primary particles may be measured using the Image J Program for the primary particles identified from the cross-sectional SEM image of the secondary particles.

[0036] More specifically, the average circumference of the primary particles may be the average of the circumferences of 10 to 50 primary particles measured in a cross-sectional SEM image of the secondary particles. Specifically, it may be 15 to 50, and even more specifically, 20 to 35.

[0037]

[0038] The positive electrode active material according to the present invention has a gradient satisfying the above equation 1 from the center of the secondary particle to the surface.

[0039] In the present invention, the “center of the secondary particle” may refer to the center of the longest diameter of the secondary particle.

[0040] By having a gradient satisfying the above formula 1 from the center of the secondary particle to the surface, the positive electrode active material according to the present invention has a relatively small specific surface area compared to a similar positive electrode active material in which the sizes of the primary particles contained within the secondary particle are the same, and thus, when applied to a lithium secondary battery, there is an advantage in that the phenomenon of life deterioration can be suppressed as the contact surface with the electrolyte becomes smaller.

[0041]

[0042] In one embodiment of the present invention, the positive electrode active material can satisfy the following equation 2.

[0043] [Formula 2]

[0044] (Average circumference of primary particles existing within a 2 / 3 to 3 / 3R region from the center of the secondary particles) ≥ 1.7 × (Average circumference of primary particles existing within a 1 / 3R region from the center of the secondary particles)

[0045]

[0046] In another embodiment of the present invention, the positive electrode active material can satisfy the following equation 3.

[0047] [Formula 3]

[0048] 3.0 × (average circumference of primary particles existing within a 1 / 3R region from the center of the secondary particles) ≥ (average circumference of primary particles existing within a 2 / 3 to 3 / 3R region from the center of the secondary particles) ≥ 1.8 × (average circumference of primary particles existing within a 1 / 3R region from the center of the secondary particles)

[0049] Specifically, the average circumference of the primary particles existing within a 2 / 3 to 3 / 3R region from the center of the secondary particles may be 1.8 × (average circumference of the primary particles existing within a 1 / 3R region from the center of the secondary particles) or more, and 2.5 × (average circumference of the primary particles existing within a 1 / 3R region from the center of the secondary particles) or less.

[0050]

[0051] When the average circumference of the primary particles existing within the 2 / 3 to 3 / 3R region from the center of the secondary particles of the above-mentioned positive electrode active material satisfies the above formula, there is an advantage in that the effect of suppressing the lifespan deterioration phenomenon is maximized, which is preferable.

[0052]

[0053] In another embodiment of the present invention, the positive electrode active material can satisfy the following equation 4.

[0054] [Formula 4]

[0055] (Average circumference of primary particles existing within a 1 / 3 to 2 / 3R region from the center of the secondary particles) ≥ 1.1 × (Average circumference of primary particles existing within a 1 / 3R region from the center of the secondary particles)

[0056]

[0057] In another embodiment of the present invention, the positive electrode active material can satisfy the following equation 5.

[0058] [Formula 5]

[0059] 2.0 × (average circumference of primary particles existing within a 1 / 3R region from the center of the secondary particles) ≥ (average circumference of primary particles existing within a 1 / 3 to 2 / 3R region from the center of the secondary particles) ≥ 1.2 × (average circumference of primary particles existing within a 1 / 3R region from the center of the secondary particles)

[0060] Specifically, the average circumference of the primary particles existing within a 1 / 3 to 2 / 3R region from the center of the secondary particles may be 1.2 × (average circumference of the primary particles existing within a 1 / 3R region from the center of the secondary particles) or more, and 1.5 × (average circumference of the primary particles existing within a 1 / 3R region from the center of the secondary particles) or less.

[0061] When the average circumference of the primary particles existing within the 1 / 3 to 2 / 3R region from the center of the secondary position of the above-mentioned positive electrode active material satisfies the above formula, it is preferable because it has the advantage of an excellent gas generation reduction effect due to a small specific surface area.

[0062]

[0063] In another embodiment of the present invention, the positive electrode active material can satisfy the following equation 6.

[0064] [Formula 6]

[0065] (Average circumference of primary particles existing within a region 2 / 3 to 3 / 3R from the center of the secondary particles) ≥ 1.1 × (Average circumference of primary particles existing within a region 1 / 3 to 2 / 3R from the center of the secondary particles)

[0066]

[0067] In another embodiment of the present invention, the positive electrode active material can satisfy the following equation 7.

[0068] [Formula 7]

[0069] 2.0 × (average circumference of primary particles existing within a region 1 / 3 to 2 / 3R from the center of the secondary particles) ≥ (average circumference of primary particles existing within a region 2 / 3 to 3 / 3R from the center of the secondary particles) ≥ 1.2 × (average circumference of primary particles existing within a region 1 / 3 to 2 / 3R from the center of the secondary particles)

[0070] Specifically, the average circumference of the primary particles existing within a region 2 / 3 to 3 / 3R from the center of the secondary particles may be 1.2 × (average circumference of the primary particles existing within a region 1 / 3 to 2 / 3R from the center of the secondary particles) or more, and 1.4 × (average circumference of the primary particles existing within a region 1 / 3 to 2 / 3R from the center of the secondary particles) or less.

[0071]

[0072] When the average circumference of the primary particles existing within the 2 / 3 to 3 / 3R region from the center of the secondary position of the positive electrode active material satisfies the above formula, there is an advantage in that the surface area of ​​the surface of the positive electrode active material in contact with the electrolyte can be reduced.

[0073]

[0074] In another embodiment of the present invention, the average circumference of the primary particles existing within a 2 / 3 to 3 / 3R region from the center of the secondary particles may be 3.2 μm or less, preferably 2.00 to 3.15 μm, and more preferably 2.10 to 3.10 μm.

[0075] When the average circumference of the primary particles existing within the 2 / 3 to 3 / 3R region from the center of the secondary particles satisfies the above range, it is preferable that the phenomenon of a rock salt-like substance being generated when the positive electrode active material is applied to a lithium secondary battery can be suppressed.

[0076]

[0077] In another embodiment of the present invention, the average circumference of the primary particles existing within a 1 / 3 to 2 / 3R region from the center of the secondary particles may be 2.5 μm or less, preferably 1.8 to 2.5 μm, and more preferably 1.85 to 2.45 μm.

[0078] When the average circumference of the primary particles existing within the 1 / 3 to 2 / 3R region from the center of the secondary particles satisfies the above range, the phenomenon of deterioration in the life of the positive electrode active material can be suppressed, and when applied to a lithium secondary battery, the phenomenon of stability problems occurring at the cell end due to gas generation can be suppressed, which is preferable.

[0079]

[0080] In another embodiment of the present invention, the average circumference of the primary particles existing within a 1 / 3R region from the center of the secondary particles may be 1.8 μm or less, preferably 1.0 to 1.8 μm, and more preferably 1.1 to 1.7 μm.

[0081] When the average circumference of the primary particles existing within the 1 / 3R region from the center of the secondary particles satisfies the above range, it is preferable to suppress the phenomenon of cracks occurring due to volume expansion when applying the positive electrode active material to a lithium secondary battery.

[0082]

[0083] In another embodiment of the present invention, the secondary particles may have an average particle diameter (D50) of 20 μm or less, preferably 7 to 18 μm, and more preferably 8 to 15 μm.

[0084] In the present invention, the “average particle diameter (D50)” may be measured using a particle size analyzer, or may be obtained from a cross-sectional image, such as the “average circumference.”

[0085] When the average particle diameter of the secondary particles satisfies the above range, it is preferable that the capacity of the positive electrode active material be improved.

[0086]

[0087] In another embodiment of the present invention, the average circumference of the primary particles present in the secondary particles may be 2.0 to 2.5 μm, preferably 2.05 to 2.45 μm. Specifically, the average circumference of the primary particles present in the secondary particles may refer to the average circumference of the primary particles present within 3 / 3R from the center of the secondary particles.

[0088] When the average circumference of the primary particles present in the secondary particles is within the above range, it is preferable that high capacity be realized when applied to a lithium secondary battery, and sufficient capacity can be expressed even with a low conductive material content.

[0089]

[0090] In another embodiment of the present invention, the positive electrode active material may include one or more transition metals selected from the group consisting of nickel, cobalt, and manganese.

[0091] In another embodiment of the present invention, the positive electrode active material may be represented by the following chemical formula 1.

[0092] [Chemical Formula 1]

[0093] Li a Ni x Co y Mn z M1 k O2

[0094] In the above chemical formula 1,

[0095] 0.9 ≤ a ≤ 1.1, 0.3 ≤ x ≤ 1.0, 0 ≤ y ≤ 0.4, 0 ≤ z ≤ 0.4, 0 ≤ k ≤ 0.04, x + y + z + k = 1,

[0096] M1 is one or more elements selected from the group consisting of Al, Zr, Nb, Mo, W, Ti, Ce, Mg, B, P, V, Sr, and B.

[0097] Specifically, the positive electrode active material according to the present invention may have a nickel content of 30 mol% to 95 mol% among the metals in the secondary particles. Specifically, the positive electrode active material according to the present invention may have a nickel content of 60 mol% or more among the metals in the secondary particles. More specifically, the positive electrode active material according to the present invention may have a nickel content of 70 mol% or more among the metals in the secondary particles. Most specifically, the positive electrode active material according to the present invention may have a nickel content of 80 mol% or more among the metals in the secondary particles.

[0098] In short, the positive electrode active material according to the present invention may be a high-nickel positive electrode active material.

[0099]

[0100] The cathode active material according to the present invention has a specific surface area of ​​0.78 m as measured by the BET nitrogen adsorption method. 2 / g or less, preferably 0.40 to 0.71 m 2 / g, more preferably 0.42 to 0.56 m 2 / g may be.

[0101] When the specific surface area of ​​the positive electrode active material according to the present invention is within the above range, it is preferable to provide excellent life stability and a gas generation reduction effect when applied to a lithium secondary battery.

[0102]

[0103] The cathode active material according to the present invention can reduce the contact area with the electrolyte when applied to a lithium secondary battery by increasing the perimeter of the primary particle from the center of the secondary particle to the surface to a range satisfying Equation 1. Therefore, it is possible to suppress the occurrence of stability problems at the cell stage due to deterioration in the lifespan of the cathode active material and gas generation. In addition, when charge / discharge is performed and electrochemical reactions are repeated, the phenomenon of formation of a rock salt phase material, which is a material that reduces the reversibility of the capacity of the cathode active material, on the surface of the cathode active material is suppressed, thereby exhibiting the advantage of excellent lifespan stability and a reduction in gas generation.

[0104]

[0105] The present invention does not limit the method for producing a positive electrode active material satisfying the above formula 1. For example, the positive electrode active material may be obtained by producing a precursor using a co-precipitation method commonly performed in the art, mixing the precursor with a lithium source, and then calcining the precursor, but is not limited thereto.

[0106] The above-mentioned calcination may be performed at a temperature exceeding 730°C and below 940°C, preferably at a temperature of 740 to 900°C, and more preferably at a temperature of 750 to 800°C, but is not limited thereto. However, when the above-mentioned calcination is performed within the above-mentioned range, the desired positive electrode active material can be easily obtained, which is preferable.

[0107]

[0108] Lithium secondary battery

[0109] Another aspect of the present invention relates to a lithium secondary battery comprising a positive electrode including the positive electrode active material described above; a negative electrode; and a non-aqueous electrolyte.

[0110] Specifically, the positive electrode is in the form of a secondary particle including a plurality of primary particles, and may include a positive electrode active material layer containing a positive electrode active material satisfying the above formula 1.

[0111] The lithium secondary battery according to the present invention has a secondary particle form including the plurality of primary particles and is manufactured using a positive electrode active material satisfying the above formula 1, and thus has the advantage of excellent life stability, suppression of gas generation, and excellent electrochemical properties.

[0112]

[0113] The positive electrode active material layer for the above lithium secondary battery may include a binder and a conductive material.

[0114] The above binder can serve to attach the positive electrode active material particles for the lithium secondary battery well to each other and also to attach the positive electrode active material for the lithium secondary battery well to the current collector.

[0115] The above conductive material is used to provide conductivity to the electrode, and any material that does not cause chemical changes and is electronically conductive can be used in the battery being constructed.

[0116]

[0117] The above negative electrode includes a current collector and a negative electrode active material layer formed on the current collector, and the negative electrode active material layer may include a negative electrode active material.

[0118] The above negative active material may include a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide.

[0119] The material capable of reversibly intercalating / deintercalating the lithium ions may be, for example, a carbon material, and any carbon-based negative electrode active material generally used in the lithium secondary battery may be used. For example, crystalline carbon, amorphous carbon, or a combination thereof may be used.

[0120] As the above lithium metal alloy, an alloy of lithium and a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn can be used.

[0121] Materials capable of doping and dedoping the lithium include, for example, Si, SiO. x (0 < x < 2), Si-Y alloy (wherein Y is an element selected from the group consisting of alkali metals, alkaline earth metals, group 13 elements, group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Sn, SnO2, Sn-Y (wherein Y is an element selected from the group consisting of alkali metals, alkaline earth metals, group 13 elements, group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), etc.

[0122] Examples of the above transition metal oxide include vanadium oxide, lithium vanadium oxide, etc. The negative electrode active material layer also includes a binder and may optionally further include a conductive material.

[0123] The above binder can serve to attach the negative electrode active material particles well to each other and also to attach the negative electrode active material well to the current collector.

[0124] The above conductive material is used to provide conductivity to the electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed.

[0125]

[0126] The above-mentioned current collector may be selected from the group consisting of, for example, aluminum foil, nickel foil, stainless steel foil, titanium foil, nickel foam, aluminum foam, a polymer substrate coated with a conductive metal, and combinations thereof.

[0127] The above negative and positive electrodes can be manufactured by mixing an active material, a conductive material, and a binder in a solvent to manufacture an active material composition, and applying this composition to a current collector. The present invention does not limit the method for manufacturing the electrodes.

[0128] The above solvent may include, but is not limited to, N-methylpyrrolidone.

[0129]

[0130] The above electrolyte may be a non-aqueous electrolyte or a solid electrolyte, and one in which a lithium salt is dissolved is used.

[0131] The non-aqueous electrolyte may include an organic solvent, and the non-aqueous organic solvent may serve as a medium through which ions involved in the electrochemical reaction of the battery can move.

[0132] Examples of the organic solvent include cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and vinylene carbonate; chain carbonates such as dimethyl carbonate, methylethyl carbonate, and diethyl carbonate; esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; ethers such as 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydrofuran, 1,2-dioxane, and 2-methyltetrahydrofuran; nitriles such as acetonitrile; and amides such as dimethylformamide. These may be used singly or in combination. In particular, a mixed solvent of a cyclic carbonate and a chain carbonate can be preferably used.

[0133] Additionally, as an electrolyte, a gel polymer electrolyte impregnated with an electrolyte solution in a polymer electrolyte such as polyethylene oxide or polyacrylonitrile, or an inorganic solid electrolyte such as LiI or Li3N may be used.

[0134] The above lithium salt is a substance that is dissolved in an organic solvent and acts as a source of lithium ions within the battery, enabling the operation of a basic lithium secondary battery and promoting the movement of lithium ions between the positive and negative electrodes.

[0135] The lithium salt may be any one commonly used in the art without limitation as long as it does not impede the purpose of the present invention. For example, the lithium salt may be one selected from the group consisting of LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiSbF6, LiAlO4, LiAlCl4, LiCl, and LiI.

[0136]

[0137] Depending on the type of the lithium secondary battery, a separator may be present between the positive and negative electrodes. Such separators may include polyethylene, polypropylene, polyvinylidene fluoride, or multilayer films of two or more layers thereof. Of course, mixed multilayer films such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, or a polypropylene / polyethylene / polypropylene three-layer separator may also be used.

[0138] Lithium secondary batteries can be classified into lithium ion batteries, lithium ion polymer batteries, and lithium polymer batteries depending on the type of separator and electrolyte used, and can be classified into cylindrical, square, coin, and pouch types depending on the shape, and can be divided into bulk type and thin film type depending on the size.

[0139] The structure and manufacturing method of the battery are not limited in the present invention.

[0140]

[0141] Hereinafter, preferred embodiments and comparative examples of the present invention are described. However, the following examples are only preferred embodiments of the present invention, and the present invention is not limited to the following examples.

[0142]

[0143] Examples and Comparative Examples

[0144] Preparation of precursors

[0145] Precursors were prepared using a general coprecipitation method. Specifically, NiSO4·6H2O was used as the nickel raw material, CoSO4·7H2O as the cobalt raw material, and MnSO4·H2O as the manganese raw material. These raw materials were dissolved in distilled water to prepare an aqueous metal salt solution.

[0146] After preparing the co-precipitation reactor, N2 was purged to prevent oxidation of metal ions during the co-precipitation reaction, and the reactor temperature was maintained at 50°C.

[0147] NH4(OH) was added as a chelating agent to the co-precipitation reactor, and NaOH was used to adjust the pH. The precipitate obtained through the co-precipitation process was filtered, washed with distilled water, and dried in a 100°C oven for 24 hours to prepare a positive electrode active material precursor.

[0148]

[0149] Manufacturing of positive electrode active materials

[0150] LiOH·H2O, a lithium source, was uniformly mixed in the manufactured precursor according to the stoichiometric ratio, but the molar ratio of lithium (Li) to the total metal (Me) (Li / Me) was slightly over 1.

[0151] The mixture was fired in a box-shaped furnace with oxygen flowing in at a rate of 25,000 mL / min for the firing temperature and firing time according to Table 1 below, thereby producing a cathode active material (LiNi) in the form of secondary particles in which primary particles according to the examples and comparative examples were aggregated. 0.9 Co 0.03 Mn 0.07O2, average particle size (D50): 12㎛) was obtained.

[0152]

[0153] Firing temperature (℃) Firing time (h) Example 175012 Example 275010 Comparative example 174012 Comparative example 274010

[0154]

[0155] Experimental example

[0156] (1) Cross-sectional analysis of positive electrode active material

[0157] The cathode active materials manufactured according to the examples and comparative examples were cut into cross sections using FIB (Focused ion beam) equipment under vacuum conditions, and cross-sectional images of the cathode active materials were obtained using SEM (Scanning Electron Microscopy) analysis equipment, and these are shown in Figures 1 to 12 (see Table 2 below).

[0158]

[0159] Drawings Embodiment 1 Figures 1 to 3 Embodiment 2 Figures 4 to 6 Comparative Example 1 Figures 7 to 9 Comparative Example 2 Figures 10 to 12

[0160]

[0161] In the cross-sectional SEM images according to Examples 1 and 2 and Comparative Examples 1 and 2, 1 / 3R, 2 / 3R, and 3 / 3R regions were set from the center of the secondary particles, and then the perimeter of the primary particles identified therefrom was measured using the Image J Program, and the average perimeter and the total perimeter were calculated, and these are shown in Tables 3 to 6, respectively. At this time, referring to FIGS. 1 to 3, the 1 / 3R region existing within the 1 / 4 quadrant based on the center of the secondary particles was arbitrarily divided into region A, the 1 / 3R to 2 / 3R regions were arbitrarily divided into region B, and the 2 / 3R to 3 / 3R regions were arbitrarily divided into region C, and the number of primary particles was measured.

[0162]

[0163] Perimeter of primary particle in region A (㎛)Perimeter of primary particle in region B (㎛)Perimeter of primary particle in region C (㎛)1.681.582.080.874.363.751.292.101.612.032.962.931.511.261.692.620.941.831.251.841.812.053.552.200.510.442.522.710.723.191.662.671.894.382.791.731.901.452.862.183.304.341.432.282.422.071. 771.882.422.612.192.272.262.342.75-2.461.693.84-1.33-1.591.004.16-0.37-1.910.772.43-1.30-0.583.272.56-0.82-3.163.043.37-1.84-3.421.763.46-1.69-1.822.134.34-1.29-3.202.715.31-1.35-3.64-3.76-average Circumference (㎛): 1.58 Average Circumference (㎛): 2.24 Average Circumference (㎛): 2.96 Total Circumference (㎛): 42.60 Total Circumference (㎛): 78.38 Total Circumference (㎛): 80.05 Average Circumference (㎛) of Primary Particles in Area A+B+C: 2.26 Total Circumference (㎛) of Primary Particles in Area A+B+C: 201.03 Total Circumference (㎛) of Primary Particles Contained in the Cross-Section of Positive Electrode Active Material: 804.14

[0164]

[0165] Circumference (㎛) of primary particles in area A Circumference (㎛) of primary particles in area B Circumference (㎛) of primary particles in area C Circumference (㎛) 1.141.413.323.221.942.072.192.032.333.051.502.621.573.262.681.031.841.142.502.061.232.262.372.973.062.042.982.102.633.061.013.192.452.683.081.302.402.112.721.731.651.491.242.462.831.243.072.802.812.281.592.361.243.473.061.891. 612.592.152.640.702.43-3.153.721.101.79-2.284.011.322.92-1.872.711.482.03-3.943.021.472.26-2.743.612.071.89-2.763.021.873.81-2.433.892.011.45-2.133.982.032.64-2.953.281.583.06-2.812.501.402.07-2.820.971.372.68-3.111.49-2.48-2.88-average Circumference (㎛): 1.50Average Circumference (㎛): 2.27Average Circumference (㎛): 2.80Total Circumference (㎛): 36.12Total Circumference (㎛): 83.90Total Circumference (㎛): 136.74Average Circumference (㎛) of Primary Particles in Area A+B+C: 2.33Total Circumference (㎛) of Primary Particles in Area A+B+C: 256.76Total Circumference (㎛) of Primary Particles Contained in the Cross-Section of Positive Electrode Active Material: 1,027.02

[0166]

[0167] Perimeter of primary particle in region A (㎛)Perimeter of primary particle in region B (㎛)Perimeter of primary particle in region C (㎛)0.931.830.951.411.571.271.551.111.321.152.301.352.293.321.391.621.550.902.401.992.471.451.342.012.261.462.172.471.481.122.121.392.213.212.561.911.141.861.882 .022.101.741.401.331.001.881.572.431.721.391.621.671.652.012.312.401.571.702.091.301.601.521.531.811.741.802.351.552.092.511.601.091.202.291.302.051.532.061.631.31 1.782.112.011.240.991.491.461.401.792.201.621.851.151.19-2.441.361.571.491.292.31-1.912.651.820.941.811.94-1.281.591.251.461.081.87-2.041.201.261.571.131.49-1.571 .621.231.331.551.15-1.932.151.66-2.151.55-2.181.292.48-1.162.95-1.691.911.81-1.220.89-1.653.911.91-1.661.77-2.672.311.71-1.611.37-1.613.002.17-1.650.91-1.371.70-average Circumference (㎛): 1.46 Average Circumference (㎛): 1.57 Average Circumference (㎛): 1.93 Total Circumference (㎛): 27.73 Total Circumference (㎛): 98.77 Total Circumference (㎛): 143.10 Average Circumference (㎛) of Primary Particles in Area A+B+C: 1.73 Total Circumference (㎛) of Primary Particles in Area A+B+C: 269.60 Total Circumference (㎛) of Primary Particles Contained in the Cross-Section of Positive Electrode Active Material: 1,078.40

[0168]

[0169] Circumference of primary particles in region A (㎛) Circumference of primary particles in region B (㎛) Circumference of primary particles in region C (㎛) 2.05 2.13 2.10 1.84 1.21 1.11 2.12 1.58 1.67 1.30 3.54 1.93 1.31 1.22 2.22 1.75 1.35 2.49 1.14 1.62 1.80 2.12 1.52 1.49 1.64 1.41 2.36 1.04 1.43 1.82 1.86 1.38 1.610 67 0.94 2.74 0.92 1.42 0.81 1.47 1.29 2 .851.101.532.621.441.242.570.651.241.441.231.711.452.090.763.040.901.911.270.912.112.010.741.581.921.662.061.831.811.631.612.611.181.221.721.891.981.121.461.241.890.841.78 0.920.921.871.731.473.411.251.001.651.762.161.831.590.752.051.851.730.641.370.961.921.951.932.120.881.152.021.782.221.08-1.263.812.362.571.58-1.332.861.382.591.87-2.051.4 31.121.491.85-3.001.031.171.551.18-0.931.980.902.321.40-1.921.651.532.441.60-1.761.041.651.171.60-1.481.361.943.312.78-2.381.772.871.352.36---0.931.512.15---1.171.052.35Average Circumference (㎛): 1.43 Average Circumference (㎛): 1.69 Average Circumference (㎛): 1.73 Total Circumference (㎛): 27.19 Total Circumference (㎛): 94.40 Total Circumference (㎛): 155.68 Average Circumference (㎛) of Primary Particles in Area A+B+C: 1.68 Total Circumference (㎛) of Primary Particles in Area A+B+C: 277.27 Total Circumference (㎛) of Primary Particles Contained in the Cross-Section of Positive Electrode Active Material: 1,198.08

[0170]

[0171] Additionally, the calculated values ​​related to Equation 1 are shown in Table 7 below.

[0172]

[0173] abcBET (m 2 / g)Discharge capacity (mAh / g)0.1 / 0.1C 3-4.3VHigh temperature lifespan (%)0.5 / 1C @45℃, same operating voltageExample 11.421.321.880.55220.393.1Example 21.511.231.850.71220.993.0Comparative example 11.071.231.320.79219.392.2Comparative example 21.181.031.210.95218.692.8a: Average circumference of area B ÷ Average circumference of area Ab: Average circumference of area C ÷ Average circumference of area Bc: Average circumference of area C ÷ Average circumference of area A

[0174]

[0175] (2) BET surface area measurement

[0176] After 4 g of the positive electrode active material precursor manufactured according to the examples and comparative examples were vacuum-dried at 300°C, nitrogen gas was adsorbed / desorbed on the surface of the positive electrode active material precursor and the adsorption amount was measured according to partial pressure to measure the specific surface area of ​​the material, and the results are shown in Table 7 above.

[0177]

[0178] (3) Discharge capacity evaluation and high temperature life evaluation

[0179] In order to evaluate the physical properties and electrochemical properties of the positive electrode active material according to the example, a coin-type half-cell was manufactured as follows.

[0180] Specifically, a positive electrode active material, a polyvinylidene fluoride binder (trade name: KF9700), and a carbon black conductive material were mixed in a weight ratio of 96.5:1.5:2, and the mixture was added to an N-methyl-2-pyrrolidone solvent so that the solid content was about 60 wt% to prepare a positive electrode active material slurry.

[0181] The above slurry was coated on an aluminum foil (Al foil, thickness: 20 μm) as a positive electrode current collector using a doctor blade, dried, and rolled to manufacture a positive electrode. The loading amount of the positive electrode was about 16 mg / cm2, and the rolling density was about 3.5 g / cm 3 It was.

[0182] A 2032 coin-type half-cell was manufactured using the above positive electrode, lithium metal negative electrode (200 μm thick, Welcos), electrolyte and polyethylene separator by a conventional method. The electrolyte was a mixed solution prepared by dissolving 1 M LiPF6 in a mixed solvent of 2% VC (vinylene carbonate) ethylene carbonate (EC), dimethyl carbonate (DMC) and diethyl carbonate (DEC) (mixing ratio EC:DMC:DEC = 1:2:1 volume %).

[0183]

[0184] For the manufactured coin-type half-cell, first, formation was performed by charging and discharging for one cycle at a current density of 0.1 C in a voltage range of 3 to 4.3 V, and then charging and discharging were performed by applying a current density of 0.1 C in the same voltage range, thereby evaluating the discharge capacity, and the results are shown in Table 7 above.

[0185] In addition, the manufactured coin-type half-cell was subjected to 50 cycles of charge and discharge at 0.5C and 1C discharge (reference capacity 200 mAh / g) under an operating voltage of 3 to 4.3 V at 45°C, and the capacity retention rate at the 50th cycle compared to the first cycle was measured, and the results are shown in Table 7 above.

[0186]

[0187] Referring to Tables 1 to 7, it can be seen that the positive electrode active material according to the example has a small specific surface area, and that the lithium secondary battery using the positive electrode active material has an excellent high-temperature lifespan.

[0188]

[0189] The present invention is not limited to the above-described embodiments, but can be manufactured in a variety of different forms. Those skilled in the art will appreciate that the present invention can be implemented in other specific forms without altering the technical spirit or essential characteristics of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive.

Claims

1. It is a secondary particle form containing multiple primary particles, A positive electrode active material satisfying the following equation 1: [Formula 1] (Average circumference of primary particles existing within a 2 / 3 to 3 / 3R region from the center of the secondary particles) ≥ 1.5 × (Average circumference of primary particles existing within a 1 / 3R region from the center of the secondary particles) In the above equation 1, R is the distance from the center of the secondary particle to the surface of the secondary particle.

2. In paragraph 1, A positive electrode active material satisfying the following equation 2. [Formula 2] (Average circumference of primary particles existing within a 2 / 3 to 3 / 3R region from the center of the secondary particles) ≥ 1.7 × (Average circumference of primary particles existing within a 1 / 3R region from the center of the secondary particles) 3. In paragraph 2, A positive electrode active material satisfying the following equation 3. [Formula 3] 3.0 × (average circumference of primary particles existing within a 1 / 3R region from the center of the secondary particles) ≥ (average circumference of primary particles existing within a 2 / 3 to 3 / 3R region from the center of the secondary particles) ≥ 1.8 × (average circumference of primary particles existing within a 1 / 3R region from the center of the secondary particles) 4. In paragraph 1, A positive electrode active material satisfying the following equation 4. [Formula 4] (Average circumference of primary particles existing within a 1 / 3 to 2 / 3R region from the center of the secondary particles) ≥ 1.1 × (Average circumference of primary particles existing within a 1 / 3R region from the center of the secondary particles) 5. In paragraph 4, A positive electrode active material satisfying the following equation 5. [Formula 5] 2.0 × (average circumference of primary particles existing within a 1 / 3R region from the center of the secondary particles) ≥ (average circumference of primary particles existing within a 1 / 3 to 2 / 3R region from the center of the secondary particles) ≥ 1.2 × (average circumference of primary particles existing within a 1 / 3R region from the center of the secondary particles) 6. In paragraph 1, A positive electrode active material satisfying the following equation 6. [Formula 6] (Average circumference of primary particles existing within a region 2 / 3 to 3 / 3R from the center of the secondary particles) ≥ 1.1 × (Average circumference of primary particles existing within a region 1 / 3 to 2 / 3R from the center of the secondary particles) 7. In paragraph 6, A positive electrode active material satisfying the following equation 7. [Formula 7] 2.0 × (average circumference of primary particles existing within a region 1 / 3 to 2 / 3R from the center of the secondary particles) ≥ (average circumference of primary particles existing within a region 2 / 3 to 3 / 3R from the center of the secondary particles) ≥ 1.2 × (average circumference of primary particles existing within a region 1 / 3 to 2 / 3R from the center of the secondary particles) 8. In paragraph 1, A positive electrode active material, wherein the average circumference of the primary particles existing within a 2 / 3 to 3 / 3R region from the center of the secondary particles is 3.2㎛ or less.

9. In paragraph 1, A positive electrode active material, wherein the average circumference of the primary particles existing within a 1 / 3 to 2 / 3R region from the center of the secondary particles is 2.5㎛ or less.

10. In paragraph 1, A positive electrode active material in which the average circumference of the primary particles existing within a 1 / 3R region from the center of the secondary particles is 1.8㎛ or less.

11. In paragraph 1, The above secondary particles are a positive electrode active material having an average particle diameter (D50) of 20㎛ or less.

12. In paragraph 1, A positive electrode active material represented by the following chemical formula 1: [Chemical Formula 1] Li a Ni x Co y Mr z M1 k O2 In the above chemical formula 1, 0.9 ≤ a ≤ 1.1, 0.3 ≤ x ≤ 1.0, 0 ≤ y ≤ 0.4, 0 ≤ z ≤ 0.4, 0 ≤ k ≤ 0.04, x + y + z + k = 1, M1 is one or more elements selected from the group consisting of Al, Zr, Nb, Mo, W, Ti, Ce, Mg, B, P, V, Sr, and B.

13. A positive electrode comprising a positive electrode active material according to any one of claims 1 to 12; cathode; and A lithium secondary battery containing a non-aqueous electrolyte.

Citation Information

Patent Citations

  • Positive electrode active material precursor and preparation method thereof, and positive electrode active material

    CN111370679A

  • Cathode material, preparing method thereof and lithiumsecondary battery

    KR1020040106207A

  • Fixing structure of Ball joint having upper cap screw combining type and Fixing method thereof

    KR1020240075109A

  • Nickel-based active material for lithium secondary battery, positive electrode and lithium secondary battery comprising thereof

    KR102357941B1

  • Nickel-based lithium metal composite oxide, preparing method thereof, and lithium secondary battery including a positive electrode including the same

    KR102392379B1