Cathode active material for lithium secondary battery, preparation method therefor, lithium secondary battery comprising same
The use of Zr and Y in nickel-containing lithium transition metal oxides for lithium secondary batteries addresses the limitations of conventional cathode materials by forming single particles with improved strength and energy density, enhancing electrochemical properties and stability.
Patent Information
- Application Number
- PCT/KR2024/007028
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional lithium secondary battery cathode active materials, such as NCM-based lithium composite transition metal oxides, have issues with low particle strength, stability, and electrode energy density due to secondary particle formation, high sintering temperatures causing electrochemical property deterioration, and excessive lithium by-products.
A nickel-containing lithium transition metal oxide with Zr and Y as grain growth promoting elements, formulated to have a specific composition and sintered at a lower temperature, resulting in single particle form with improved crystal grain size, particle strength, and energy density.
The solution enhances electrochemical properties, particle strength, and lifespan characteristics while maintaining thermal stability and reducing manufacturing costs by maximizing grain size and adjusting the content of Zr and Y within the lithium transition metal oxide.
Smart Images

Figure KR2024007028_05122024_PF_FP_ABST
Abstract
Description
Positive electrode active material for lithium secondary batteries, method for producing the same, and lithium secondary batteries comprising the same
[0001] The present invention relates to a positive electrode active material for a lithium secondary battery, a method for producing the same, and a lithium secondary battery comprising the same, and more specifically, to a positive electrode active material for a single-particle lithium secondary battery, a method for producing the same, and a lithium secondary battery comprising the same.
[0002]
[0003] Lithium secondary batteries produce electrical energy through oxidation and reduction reactions when lithium ions are inserted / deintercalated from the positive and negative electrodes, while an organic electrolyte or polymer electrolyte is charged between the positive and negative electrodes, which are made of active materials capable of intercalating and deintercalating lithium ions.
[0004] Lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2 or LiMn2O4, etc.), and lithium iron phosphate compound (LiFePO4) have been used as cathode active materials for lithium secondary batteries. Among these, lithium cobalt oxide (LiCoO2) is widely used due to its high operating voltage and excellent capacity characteristics, and is applied as a cathode active material for high voltage. However, due to the rising price of cobalt (Co) and unstable supply, it is difficult to use it in large quantities as a power source in fields such as electric vehicles, and the need for the development of a cathode active material that can replace it has arisen.
[0005] Accordingly, nickel-cobalt-manganese lithium composite transition metal oxides (hereinafter simply referred to as 'NCM-based lithium composite transition metal oxides') in which some of the cobalt (Co) is replaced with nickel (Ni) and manganese (Mn) have been developed. However, the NCM-based lithium composite transition metal oxides developed previously are generally in the form of secondary particles in which primary particles are aggregated, and have a large specific surface area, low particle strength, and a high content of lithium byproducts, which causes problems such as large gas generation during cell operation and low stability.
[0006] Accordingly, development is underway for single-particle cathode active materials, rather than the conventional secondary particle form. However, producing single-particle cathodes requires firing at higher temperatures than secondary particle production. This often leads to over-firing, resulting in layered crystal structure defects and deterioration of electrochemical characteristics such as capacity and output.
[0007] And, when the sintering temperature is lowered to solve this problem, the grain size within the single particle does not grow sufficiently, which deteriorates the particle strength and life characteristics, and the particle diameter of the single particle does not grow sufficiently, which lowers the rolling density and deteriorates the electrode energy density.
[0008]
[0009] Accordingly, one object of the present invention is to provide a cathode active material for a lithium secondary battery, which is a single particle, has excellent electrochemical properties due to a small number of layered structure crystal defects, has excellent particle strength and lifespan properties due to a maximized crystal grain size, and has an increased average particle diameter to improve electrode energy density, a method for producing the same, and a lithium secondary battery including the same.
[0010]
[0011] One embodiment of the present invention provides a cathode active material for a lithium secondary battery, which is a nickel-containing lithium transition metal oxide in the form of a single particle, wherein the nickel content is 50 to 70 mol% based on the total mole number of transition metals, the lithium transition metal oxide includes Zr and Y as grain growth promoting elements, and the total content of Zr and Y is 2500 to 5200 ppm based on the weight of the lithium transition metal oxide.
[0012] The content of the above Zr may be 1300 to 2800 ppm based on the weight of the above lithium transition metal oxide.
[0013] The content of the above Y may be 1400 to 2400 ppm based on the weight of the lithium transition metal oxide.
[0014] The content of cobalt in the above lithium transition metal oxide may be 5 to 20 mol% based on the total mole number of transition metals.
[0015] The content of manganese in the above lithium transition metal oxide may be 10 mol% or more based on the total mole number of transition metals.
[0016] The above-mentioned cathode active material for a lithium secondary battery may have a crystallite size of 200 nm or more.
[0017] The cation mixing ratio of nickel cations in the lithium layer in the above lithium transition metal oxide may be 3.8% or less.
[0018] The above-mentioned positive electrode active material for a lithium secondary battery may have an average particle diameter (D50) of 3 μm or more.
[0019] The above lithium transition metal oxide can be represented by the following chemical formula 1.
[0020] [Chemical Formula 1]
[0021] Li a [Ni x Co y Mn z M1 w1 M2w2 ]O2
[0022] In the above chemical formula 1, 0.8≤a≤1.2, 0.5≤x≤0.7, 0.05≤y≤0.2, 0.1≤z≤0.4, 0 <w1≤0.05, 0≤w2≤0.1이고, x+y+z+w1+w2=1이고, M1은 Zr 및 Y이고, M2는 B, Al, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr 또는 이들의 조합이다.
[0023]
[0024] Another embodiment of the present invention provides a method for producing a positive electrode active material for a lithium secondary battery, comprising the steps of: preparing a transition metal precursor containing 50 to 70 mol% of nickel based on the total mole number of transition metals; and forming a mixture including the transition metal precursor, a lithium raw material, a Zr raw material, and a Y raw material, and then firing the mixture at a temperature of 890 to 950°C to form a lithium transition metal oxide in the form of a single particle.
[0025] The total content of Zr and Y in the lithium transition metal oxide formed above may be 2500 to 5200 ppm based on the weight of the lithium transition metal oxide.
[0026] The content of Zr in the lithium transition metal oxide formed above may be 1300 to 2800 ppm based on the weight of the lithium transition metal oxide.
[0027] The content of Y in the lithium transition metal oxide formed above may be 1400 to 2400 ppm based on the weight of the lithium transition metal oxide.
[0028] The above lithium raw material may be Li2CO3.
[0029]
[0030] Another embodiment of the present invention provides a positive electrode for a lithium secondary battery comprising the positive electrode active material described above.
[0031] Another embodiment of the present invention provides a lithium secondary battery including the positive electrode for a lithium secondary battery as described above.
[0032]
[0033] According to one embodiment of the present invention, a cathode active material for a lithium secondary battery includes Zr and Y as grain growth-promoting elements. By appropriately controlling the content of these elements, layered structure crystal defects can be reduced, thereby improving electrochemical characteristics. In addition, the crystal grain size of the cathode active material can be maximized, thereby improving particle strength and lifespan characteristics. In addition, the average particle diameter of the cathode active material can be increased, thereby improving electrode energy density.
[0034]
[0035] Figure 1 is a SEM image of a positive electrode active material manufactured according to Example 2.
[0036] Figure 2 is an SEM image of a positive electrode active material manufactured according to Comparative Example 1.
[0037] Figure 3 is an SEM image of a positive electrode active material manufactured according to Comparative Example 2.
[0038] Figure 4 is an SEM image of a positive electrode active material manufactured according to Comparative Example 3.
[0039] The terms first, second, and third, etc., are used to describe, but are not limited to, various parts, components, regions, layers, and / or sections. These terms are used only to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, a first part, component, region, layer, or section described below may be referred to as a second part, component, region, layer, or section without departing from the scope of the present invention.
[0040] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the present invention. As used herein, the singular forms "singular" and "comprising" include plural forms as well, unless the context clearly dictates otherwise. The word "comprising" as used herein specifies a particular feature, region, integer, step, operation, element, and / or component, but does not exclude the presence or addition of other features, regions, integers, steps, operations, elements, and / or components.
[0041] When a part is referred to as being "on" or "over" another part, it can be directly on or over the other part, or there may be other parts intervening. Conversely, when a part is referred to as being "directly on" another part, there are no other parts intervening.
[0042] Although not defined otherwise, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by those of ordinary skill in the technical field to which the present invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with the relevant technical literature and the present disclosure, and are not to be construed as ideal or overly formal unless otherwise defined.
[0043] Also, unless otherwise stated, % means weight%, and 1 ppm is 0.0001 weight%.
[0044] In this specification, the term "combination(s) thereof" described in the expression in the Makushi format means one or more mixtures or combinations selected from the group consisting of the components described in the expression in the Makushi format, and means including any one or more selected from the group consisting of said components.
[0045] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.
[0046]
[0047] 1. Positive active material
[0048] One embodiment of the present invention provides a cathode active material for a lithium secondary battery, which is a nickel-containing lithium transition metal oxide in the form of a single particle, wherein the nickel content is 50 to 70 mol% based on the total mole number of transition metals, the lithium transition metal oxide includes Zr and Y as grain growth promoting elements, and the total content of Zr and Y is 2500 to 5200 ppm based on the weight of the lithium transition metal oxide.
[0049] According to one embodiment of the present invention, a cathode active material for a lithium secondary battery is a single-particle type cathode active material. In this specification, “single particle” is a term used to distinguish it from the cathode active material particles in the form of secondary particles formed by the agglomeration of tens to hundreds of primary particles that have been commonly used in the past, and is a concept that includes a single particle composed of one primary particle and an aggregate particle of 30 or fewer primary particles. The “secondary particle” refers to an aggregate, i.e., a secondary structure, formed by the physical or chemical bonding between tens to hundreds of primary particles without an intentional agglomeration or assembly process for the primary particles. The single-particle type active material has a smaller specific surface area than conventional general secondary particles, which reduces the amount of gas generated by side reactions with the electrolyte, and has a larger particle strength, which can suppress particle breakage during rolling, and can reduce the occurrence of cracks due to repeated charging and discharging. Accordingly, it has the advantage of superior lifespan and safety compared to secondary particles, and can realize high energy density of the electrode.
[0050] According to one embodiment of the present invention, a positive electrode active material for a lithium secondary battery has a single particle form. As used herein, the term "single particle" refers to a single particle composed of only one primary particle, and is a concept distinct from particles composed of multiple primary particles among single particles. From the perspective of improving the lifespan and safety of the battery, the above characteristics can be more preferably realized when the positive electrode active material is in the form of a single particle composed of only one primary particle.
[0051] In addition, in the lithium transition metal oxide according to the present invention, the nickel content is 50 to 70 mol% based on the total mole number of transition metals. Recently, high-nickel active materials having a nickel molar content of 80 mol% or more have been widely used to increase the capacity of batteries. However, if the nickel content is too high, there may be a thermal propagation issue, i.e., a thermal safety problem, and the cost may increase. Therefore, the lithium transition metal oxide according to the present invention has a nickel content of 70 mol% or less, so that the thermal safety is excellent and the manufacturing cost can be reduced. However, if the nickel content is too low, the capacity may be too low.
[0052] However, when manufacturing a single particle type positive electrode active material, firing is generally performed at a higher temperature than when manufacturing a conventional secondary particle positive electrode active material. At this time, over-firing often occurs, resulting in layered structure crystal defects, which causes deterioration of electrochemical characteristics such as capacity and output.
[0053]
[0054] Accordingly, the lithium transition metal oxide according to the present invention includes Zr and Y as grain growth promoting elements. Accordingly, by lowering the sintering temperature for single particle formation, crystal defects such as an increase in the cation mixing ratio due to high-temperature sintering can be prevented, and the grain size within the single particle and the average grain diameter of the single particle can be efficiently increased during the sintering process. In the present specification, “crystal grain” means a distinct region in which atoms within a primary particle form a lattice structure with a certain direction.
[0055] At this time, the total content of Zr and Y may be 2500 to 5200 ppm based on the weight of the lithium transition metal oxide, and more specifically, 3000 to 4100 ppm or 3200 to 3700 ppm. If the content of the grain growth promoting element is too low, the grain size growth may be minimal, and if the content of the grain growth promoting element is too high, an excessive amount of the grain growth promoting element may be distributed at the precursor interface during the sintering process, which may rather inhibit the grain size growth. Therefore, when the total content of Zr and Y satisfies the above range, the grain size can be maximized.
[0056] More specifically, the content of Zr may be 1300 to 2800 ppm, 1300 to 2200 ppm, or 1300 to 1600 ppm based on the weight of the lithium transition metal oxide.
[0057] More specifically, the content of Y may be 1400 to 2400 ppm, 1600 to 2300 ppm or 1800 to 2300 ppm based on the weight of the lithium transition metal oxide.
[0058] The cobalt content in the lithium transition metal oxide may be 5 to 20 mol% based on the total moles of the transition metal. If the cobalt content is too low, grain size growth may be inhibited, and if the cobalt content is too high, there may be a high price problem.
[0059] The manganese content in the lithium transition metal oxide may be 10 mol% or more, and more specifically, 15 mol%, 20 mol%, or 25 mol% or more, based on the total mole number of transition metals. Manganese is generally disadvantageous for forming a layered structure, and may inhibit grain growth due to its high oxidation number. Therefore, the manganese content within the above range may be disadvantageous from the perspective of maximizing grain size growth of a single particle. However, the lithium transition metal oxide according to the present invention includes Zr and Y as grain growth-promoting elements, and the content thereof is appropriately controlled. Accordingly, even if manganese is contained within the above range, the grain size can sufficiently grow, and the advantage of containing manganese, that is, the effect of improving life characteristics due to improved structural stability of the active material, can be realized.
[0060]
[0061] As the content of grain growth promoting elements, etc. is controlled as described above, the cathode active material for a lithium secondary battery according to the present invention can have a crystallite size of 200 nm or more, and more specifically, can be maximized to 230, 250, 270, or 280 nm or more. As the crystallite size of the cathode active material satisfies the above range, the particle strength is improved, so that particle breakage due to rolling, etc. can be suppressed, and the life characteristics and stability can be improved. In this specification, the “crystallite size” can be estimated using peak broadening of XRD data, and can be quantitatively calculated through the Scherr equation.
[0062] In addition, the cation mixing ratio of nickel cations in the lithium layer in the lithium transition metal oxide may be 3.8% or less, and more specifically, 3.6% or 3.3% or less. Since the cation mixing ratio of the positive electrode active material is sufficiently low as described above, the problem of deterioration of battery life characteristics due to collapse of the lithium layer during charge and discharge can be prevented. In the present specification, the cation mixing ratio can be measured by dividing the intensity of the (003) peak of the XRD (X-ray Diffraction) data of the positive electrode active material by the intensity of the (104) peak.
[0063] In addition, the positive electrode active material for the lithium secondary battery may have an average particle diameter (D50) of 3 μm, 3.5 μm, or 4.0 μm or more. More specifically, since the lithium transition metal oxide according to the present invention contains grain growth promoting elements of Zr and Y, the particle diameter of a single particle can efficiently increase during the sintering process. Since the average particle diameter of the positive electrode active material satisfies the above range, the rolling density can be improved, thereby improving the electrode energy density. In the present specification, the average particle diameter (D50) can be defined as a particle diameter corresponding to 50% of the volume accumulation amount in the particle diameter distribution curve of the particles. The average particle diameter (D50) can be measured using, for example, a laser diffraction method.
[0064]
[0065] The lithium transition metal oxide according to the present invention can be more specifically represented by the following chemical formula 1.
[0066] [Chemical Formula 1]
[0067] Li a [Ni x Co y Mn z M1 w1 M2 w2 ]O2
[0068] In the above chemical formula 1, 0.8≤a≤1.2, 0.5≤x≤0.7, 0.05≤y≤0.2, 0.1≤z≤0.4, 0 <w1≤0.05, 0≤w2≤0.1이고, x+y+z+w1+w2=1이고, M1은 Zr 및 Y이고, M2는 B, Al, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr 또는 이들의 조합이다.
[0069] In the lithium transition metal oxide of the above chemical formula 1, lithium may be included in a content corresponding to a, that is, 0.8≤a≤1.2. If a is too small, the capacity may be reduced, and if a is too large, the strength of the sintered positive electrode active material may be increased, making pulverization difficult, and the amount of gas generated may increase due to an increase in lithium byproducts. Considering the effect of improving the capacity characteristics of the positive electrode active material according to the control of the lithium content and the sinterability balance during the production of the active material, the lithium may be included in a content of 0.9≤a≤1.1 more preferably.
[0070] In the lithium transition metal oxide of the above chemical formula 1, nickel may be included in an amount corresponding to x, i.e., 0.5≤x≤0.7. If the nickel content is too low, it may be difficult to achieve high capacity of the battery, and if the nickel content is too high, the battery life and thermal safety may be reduced due to a decrease in the structural stability of the active material, and the manufacturing cost may increase.
[0071] In the lithium transition metal oxide of the above chemical formula 1, cobalt may be included in an amount corresponding to y, i.e., 0.05≤y≤0.2. If the cobalt content is too low, grain size growth may be inhibited and output characteristics may deteriorate. If the cobalt content is too high, manufacturing costs may increase and reversible capacity may decrease.
[0072] In the lithium transition metal oxide of the above chemical formula 1, manganese may be included in a content corresponding to z, i.e., 0.1≤z≤0.4. If the manganese content is too low, the production cost may increase and the stability of the active material may decrease. If the manganese content is too high, the capacity and output characteristics of the battery may decrease.
[0073] In the lithium transition metal oxide of the above chemical formula 1, M1 is the content corresponding to w1, i.e., 0 <w1≤0.05로 포함될 수 있다. 이때, M1은 입성장 촉진 원소인 Zr 및 Y이다.
[0074] In the lithium transition metal oxide of the above chemical formula 1, M2 may be included in a content corresponding to w2, that is, 0≤w2≤0.1. At this time, M2 is a doping element other than a grain growth promoting element, and may be appropriately added within a range that does not deteriorate battery performance, and may be B, Al, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr, or a combination thereof.
[0075] Meanwhile, the optimal content of Zr and Y for implementing the effects of the present invention mentioned above may be more appropriate when the composition of the lithium transition metal oxide satisfies the above range, and may be inappropriate when the composition of the lithium transition metal oxide is outside the above range.
[0076]
[0077] 2. Method for manufacturing positive electrode active material
[0078] Another embodiment of the present invention provides a method for producing a positive electrode active material for a lithium secondary battery, comprising the steps of: preparing a transition metal precursor containing 50 to 70 mol% of nickel based on the total mole number of transition metals; and forming a mixture including the transition metal precursor, a lithium raw material, a Zr raw material, and a Y raw material, and then firing the mixture at a temperature of 890 to 950°C to form a lithium transition metal oxide in the form of a single particle.
[0079] Hereinafter, a method for manufacturing a positive electrode active material for a lithium secondary battery according to one embodiment of the present invention will be described step by step.
[0080]
[0081] First, a transition metal precursor containing 50 to 70 mol% of nickel based on the total mole number of transition metals is prepared.
[0082] The nickel-containing transition metal precursor is not particularly limited, but may be, for example, a transition metal hydroxide.
[0083] The above transition metal hydroxide may be manufactured by, for example, adding a complexing agent-containing solution and a pH adjusting agent-containing solution to a transition metal-containing solution including a nickel raw material and optionally a cobalt raw material or a manganese raw material, and performing a co-precipitation reaction.
[0084] The above nickel raw material is not particularly limited as long as it is used in the art for manufacturing a positive electrode active material precursor. For example, the nickel raw material may be a nickel-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide or oxyhydroxide, and specifically, may be NiSO4, NiSO4·6H2O, Ni(OH)2, NiO, NiOOH, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, fatty acid nickel salt, nickel halide or a combination thereof, but is not limited thereto.
[0085] The above cobalt raw material is not particularly limited as long as it is used in the art for manufacturing a positive electrode active material precursor. For example, the cobalt raw material may be a cobalt-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically, CoSO 4,It may be, but is not limited to, CoSO4ㆍ7H2O, Co(OH)2, CoOOH, Co(OCOCH3)2ㆍ4H2O, Co(NO3)2ㆍ6H2O or a combination thereof.
[0086] The manganese raw material is not particularly limited as long as it is used in the art for manufacturing a precursor of a cathode active material. For example, the manganese raw material may be a manganese-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, oxyhydroxide, or a combination thereof, and specifically, may be a manganese salt such as MnSO4, MnCO3, Mn(NO3)2, manganese acetate, manganese dicarboxylic acid salt, manganese citrate, and manganese fatty acid salt, manganese oxide such as Mn2O3, MnO2, and Mn3O4, oxyhydroxide, manganese chloride, or a combination thereof, but is not limited thereto.
[0087] The above transition metal-containing solution may be prepared by adding a nickel raw material and optionally a cobalt raw material or a manganese raw material to a solvent, specifically, water, or a mixture of water and an organic solvent (e.g., alcohol, etc.) that can be uniformly mixed with water.
[0088] The above complexing agent-containing solution performs the function of forming a complex, and may include, but is not limited to, NH3, NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, NH4CO3 or a combination thereof as the complexing agent. Meanwhile, the complexing agent-containing solution may be used in the form of an aqueous solution, and at this time, water or a mixture of water and an organic solvent (e.g., alcohol, etc.) that can be uniformly mixed with water may be used as the solvent.
[0089] At this time, the molar ratio of nickel, cobalt, and manganese in the precursor can be controlled by controlling the concentration of nickel raw material, cobalt raw material, and manganese raw material.
[0090] Accordingly, the content of nickel in the transition metal precursor may be 50 to 70 mol% based on the total mole number of transition metals.
[0091] Additionally, the content of cobalt in the transition metal precursor may be 5 to 20 mol% based on the total mole number of transition metals.
[0092] Additionally, the content of manganese in the transition metal precursor may be 10 mol% or more based on the total mole number of transition metals, and more specifically, 15 mol%, 20 mol%, or 25 mol% or more.
[0093] The technical significance of controlling the nickel, cobalt, and manganese content in the transition metal precursor is omitted as described above.
[0094]
[0095] Next, a mixture including the transition metal precursor, lithium raw material, Zr raw material, and Y raw material is formed and then calcined at a temperature of 890 to 950°C to form a lithium transition metal oxide in the form of a single particle.
[0096] The above lithium raw material is not particularly limited as long as it is commonly used in the art, but more specifically, it may be, for example, Li2CO3. By using Li2CO3, which is inexpensive, instead of LiOH, which is commonly used as a lithium raw material, a cost reduction effect may be achieved.
[0097] The above Zr raw material may be Zr(SO4)2, ZrS2, ZrO2, Zr(NO3)4 or a combination thereof, but is not necessarily limited thereto.
[0098] The above Y raw material may be Y(SO4)2, Y2(SO4)3, Y2O3, Y(NO3)3 or a combination thereof, but is not necessarily limited thereto.
[0099] At this time, the firing is performed at a temperature of 890 to 950°C. If the firing temperature is too low, the growth of the crystal grain size within the single particle and the average particle size of the single particle may be inhibited, and if the firing temperature is too high, crystal defects may occur, such as an increase in the cation mixing ratio due to over-firing.
[0100] Additionally, the above firing can be performed for 5 to 20 hours, and more specifically, for 7 to 15 hours.
[0101] Additionally, the above-described firing may be performed under an oxygen or air atmosphere. When firing under the above-described atmosphere, the local oxygen partial pressure may increase, thereby improving the crystallinity of the positive electrode active material.
[0102] The total content of Zr and Y in the formed lithium transition metal oxide may be 2500 to 5200 ppm based on the weight of the lithium transition metal oxide, and more specifically, may be 3000 to 4100 ppm or 3200 to 3700 ppm.
[0103] The content of Zr in the formed lithium transition metal oxide may be 1300 to 2800 ppm based on the weight of the lithium transition metal oxide, and more specifically, may be 1300 to 2200 ppm or 1300 to 1600 ppm.
[0104] The content of Y in the formed lithium transition metal oxide may be 1400 to 2400 ppm based on the weight of the lithium transition metal oxide, and more specifically, may be 1600 to 2300 ppm or 1800 to 2300 ppm.
[0105] The technical significance of controlling the Zr and Y content in lithium transition metal oxides is as described above and is therefore omitted.
[0106] Meanwhile, when doping with other doping elements other than the growth promoting element, other doping raw materials may be added during the formation of the mixture and then sintered to further dope the lithium transition metal oxide with other doping elements.
[0107]
[0108] Next, optionally, the lithium transition metal oxide can be decomposed as needed.
[0109] This allows for easier formation of lithium transition metal oxides in the form of single particles. Crushing can be performed using methods commonly used in the art. For example, crushing can be performed using a jet mill, but is not necessarily limited thereto.
[0110]
[0111] 3. Lithium secondary battery
[0112] Another embodiment of the present invention provides a positive electrode for a lithium secondary battery comprising the positive electrode active material described above.
[0113] More specifically, the positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, and including the positive electrode active material described above.
[0114] The positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 μm, and fine unevenness may be formed on the surface of the positive electrode current collector to increase the adhesion of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.
[0115] The above-described positive electrode active material layer may include a binder and / or a conductive material together with the above-described positive electrode active material.
[0116] At this time, the binder plays a role of improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one kind alone or a mixture of two or more kinds thereof may be used, but is not limited thereto. The binder may be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.
[0117] And, the conductive material is used to provide conductivity to the electrode, and in the battery to be constructed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One type alone or a mixture of two or more types among these may be used, but the present invention is not limited thereto. The conductive material may typically be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.
[0118] The above positive electrode can be manufactured according to a conventional positive electrode manufacturing method, except that the above positive electrode active material is used.
[0119] Specifically, the positive electrode can be manufactured by applying a composition for forming a positive electrode active material layer, including the positive electrode active material described above and optionally a binder, a conductive agent, or a solvent, on a positive electrode current collector, followed by drying and rolling. At this time, the types and contents of the positive electrode active material, binder, and conductive agent are as described above.
[0120] The solvent may be a solvent generally used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water. One of these may be used alone or a mixture of two or more thereof may be used. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, taking into account the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the positive electrode.
[0121] Alternatively, the positive electrode may be manufactured by casting the composition for forming the positive electrode active material layer on a separate support, and then laminating the resulting film on a positive electrode current collector by peeling it off from the support.
[0122]
[0123] Another embodiment of the present invention provides a lithium secondary battery including the positive electrode for a lithium secondary battery as described above.
[0124] The above lithium secondary battery may more specifically include a positive electrode; a negative electrode; a separator; and an electrolyte.
[0125] The above lithium secondary battery may optionally further include a battery container that houses the electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.
[0126] The above negative electrode may include a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.
[0127] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.
[0128] The negative electrode active material layer may optionally include a binder and a conductive material together with the negative electrode active material. As an example, the negative electrode active material layer may be manufactured by applying a composition for forming a negative electrode active material layer comprising the negative electrode active material and optionally a binder and a conductive material onto a negative electrode current collector and drying the composition, or by casting the negative electrode forming composition onto a separate support and then laminating the resulting film onto a negative electrode current collector by peeling the film off from the support.
[0129] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples thereof include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, and Al alloy; metallic oxides capable of doping and dedoping lithium, such as SiOβ (0 < β < 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include natural graphite or artificial graphite in the form of amorphous, plate-like, flaky, spherical, or fiber-like forms, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes.
[0130] The above binder and conductive material may be the same as those described above for the positive electrode.
[0131]
[0132] The above separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used as a separator in lithium secondary batteries can be used without any particular restrictions. In particular, a separator having low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength may be used, and may optionally be used in a single-layer or multi-layer structure.
[0133]
[0134] The above electrolyte may include, but is not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.
[0135] Specifically, the organic liquid electrolyte may include an organic solvent and a lithium salt.
[0136] The organic solvent may be used without any particular limitation as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; Carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (wherein R is a C2 to C20 linear, branched, or cyclic hydrocarbon group, and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, a carbonate solvent is preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery and a linear carbonate compound having low viscosity (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate, etc.) is more preferable.In this case, the performance of the electrolyte may be improved when the cyclic carbonate and the chain carbonate are mixed and used in a volume ratio of about 1:1 to about 1:9.
[0137] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2. LiCl, LiI, or LiB(C2O4)2. It is preferable that the concentration of the lithium salt be used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.
[0138] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexamethylphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 to 5 wt% based on the total weight of the electrolyte.
[0139] As described above, a lithium secondary battery including a cathode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention, and is therefore useful in portable devices such as mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0140] Accordingly, another embodiment of the present invention provides a battery module including the lithium secondary battery as a unit cell and a battery pack including the same.
[0141] The above battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.
[0142]
[0143] Hereinafter, embodiments of the present invention will be described in more detail through examples. However, the following examples are merely preferred embodiments of the present invention, and the present invention is not limited to the following examples.
[0144]
[0145] Example 1
[0146] (1) Manufacturing of positive electrode active material
[0147] (Mixed) Ni 0.6 Co 0.1 Mn 0.3A precursor having a composition of (OH)2 was prepared. Thereafter, Li2CO3 was added to a mixer so that the molar ratio of lithium to transition metal (Li / M) of the precursor was 1.05, ZrO2 was added so that the weight ratio (wt%) of Zr to lithium transition metal oxide was 2700 ppm, and Y2O3 was added so that the weight ratio (wt%) of Y to lithium transition metal oxide was 2100 ppm, and the mixture was formed by mechanically mixing.
[0148] (After calcination), the mixture was calcined at 940°C for 13 hours under an oxygen atmosphere and then naturally cooled. Thereafter, the calcined product was pulverized to produce a single particle of lithium transition metal oxide.
[0149] (2) Lithium secondary battery manufacturing
[0150] The slurry for manufacturing the electrode plate was mixed with the above-mentioned positive electrode active material: conductive material (carbon black, Denka black): binder (PVDF, KF9700) = 95.0:2.0:3.0 wt%, and the viscosity was adjusted so that the solid content was approximately 60% by adding NMP (N-Methyl-2-pyrrolidone). The manufactured slurry was coated on a 20 μm thick Al foil using a doctor blade, and then dried and rolled. The electrode loading was 16.0 mg / cm 2 and the rolling density (25 ℃, 20 kN) was 3.5 g / cm 3 It was.
[0151] The electrolyte was 1M LiPF6in EC:DMC:DEC=1:2:1 (vol%), with 2.0 vol% VC added to the total amount of the electrolyte, and a coin cell was manufactured using a PP separator and a lithium negative electrode (400 μm, NEBA metal).
[0152]
[0153] Comparative examples, other examples and reference examples
[0154]
[0155] A cathode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the input amounts of ZrO2 and Y2O3 were adjusted so that the contents of doped Zr and Y were controlled as shown in Table 1 below.
[0156] Li / M injection non-firing temperature (℃) Firing time (h) Zr doping amount (ppm) Y doping amount (ppm) Example 11.059401327002100 Example 21.059401314002100 Example 31.059401314001800 Example 41.059401327001400 Comparative example 11.059401300 Comparative example 21.059401302800 Comparative example 31.059401354000 Comparative example 41.059401314001000 Comparative example 51.059401314000
[0157]
[0158] Experimental Example 1: Observation of SEM images of positive electrode active material
[0159] The SEM (scanning electron microscope) images of the positive electrode active materials manufactured according to Example 2, Comparative Example 1, Comparative Example 2, and Comparative Example 3 were evaluated, and are shown in FIGS. 1 to 4, respectively.
[0160] Referring to FIGS. 1 to 4, it was confirmed that the positive electrode active materials of the examples and comparative examples were in the form of single particles.
[0161]
[0162] Experimental Example 2: Evaluation of the properties of positive electrode active materials
[0163] The physical properties of the positive electrode active materials manufactured according to the examples, comparative examples, and reference examples were evaluated, and the results are shown in Table 2 below.
[0164] (1) Average particle size (D50) evaluation
[0165] For the positive electrode active materials manufactured according to the examples and comparative examples, the particle size corresponding to 50% of the volume accumulation amount was measured using the laser diffraction method.
[0166] (2) Crystallite size evaluation
[0167] For the positive electrode active materials manufactured according to the examples and comparative examples, the crystal grain size was measured by quantitatively calculating it using the Scherr equation using the peak broadening of XRD data.
[0168] (3) Evaluation of cation mixing ratio
[0169] For the positive electrode active materials manufactured according to the examples and comparative examples, the cation mixing ratio was measured by dividing the intensity of the (003) peak of the positive electrode active material XRD data by the intensity of the (104) peak.
[0170] Average particle diameter (D50, μm) Cation mixing ratio (%) Grain size (nm) Example 14.33.2298 Example 24.32.8307 Example 34.33.3281 Example 44.43.3285 Comparative Example 13.83.4266 Comparative Example 23.83.4268 Comparative Example 33.93.6273 Comparative Example 44.13.4269 Comparative Example 53.83.4277
[0171]
[0172] Referring to Table 2, in the case of Examples 1 to 4 in which Zr and Y were doped and the contents were appropriately controlled, it was confirmed that the average particle diameter was sufficiently large overall, the cation mixing ratio was small, and the crystal grain size was large. On the other hand, in the case of Comparative Example 1 in which Zr and Y were not doped, or Comparative Examples 2, 3, and 5 in which only one of Zr and Y was doped, it was confirmed that the average particle diameter was inferior overall, the cation mixing ratio was large, and the crystal grain size was small.
[0173] In addition, in the case of Comparative Example 4, which was doped with Zr and Y but had too little Y doping content, it was confirmed that the average particle diameter was inferior, the cation mixing ratio was large, and the crystal grain size was small.
[0174]
[0175] Although the preferred embodiments of the present invention have been described above, the present invention is not limited thereto, and various modifications can be made within the scope of the patent claims, the detailed description of the invention, and the attached drawings, and it is obvious that this also falls within the scope of the present invention.
[0176] Accordingly, the actual scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A nickel-containing lithium transition metal oxide in the form of a single particle, The content of the above nickel is 50 to 70 mol% based on the total mole number of transition metals, The above lithium transition metal oxide contains Zr and Y as grain growth promoting elements, A positive electrode active material for a lithium secondary battery, wherein the total content of Zr and Y is 2500 to 5200 ppm based on the weight of the lithium transition metal oxide.
2. In paragraph 1, A positive electrode active material for a lithium secondary battery, wherein the content of Zr is 1300 to 2800 ppm based on the weight of the lithium transition metal oxide.
3. In paragraph 1, A positive electrode active material for a lithium secondary battery, wherein the content of Y is 1400 to 2400 ppm based on the weight of the lithium transition metal oxide.
4. In paragraph 1, A positive electrode active material for a lithium secondary battery, wherein the content of cobalt in the lithium transition metal oxide is 5 to 20 mol% based on the total mole number of transition metals.
5. In paragraph 1, A positive electrode active material for a lithium secondary battery, wherein the content of manganese in the lithium transition metal oxide is 10 mol% or more based on the total mole number of transition metals.
6. In paragraph 1, A cathode active material for a lithium secondary battery having a crystallite size of 200 nm or more.
7. In paragraph 1, A cathode active material for a lithium secondary battery, wherein the cation mixing ratio of nickel cations in the lithium layer of the lithium transition metal oxide is 3.8% or less.
8. In paragraph 1, A cathode active material for a lithium secondary battery having an average particle diameter (D50) of 3 μm or more.
9. In paragraph 1, The above lithium transition metal oxide is a positive electrode active material for a lithium secondary battery represented by the following chemical formula 1: [Chemical Formula 1] Li a [Ni x Co y Mr z M1 w1 M2 w2 ]O2 In the above chemical formula 1, 0.8≤a≤1.2, 0.5≤x≤0.7, 0.05≤y≤0.2, 0.1≤z≤0.4, 0 <w1≤0.05, 0≤w2≤0.1이고, x+y+z+w1+w2=1이고, M1은 Zr 및 Y이고, M2는 B, Al, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr 또는 이들의 조합이다.
10. A step of preparing a transition metal precursor containing 50 to 70 mol% of nickel based on the total mole number of transition metals; and Comprising a step of forming a mixture including the above transition metal precursor, lithium raw material, Zr raw material, and Y raw material, and then calcining at a temperature of 890 to 950°C to form a lithium transition metal oxide in the form of a single particle. A method for manufacturing a cathode active material for a lithium secondary battery.
11. In paragraph 10, A method for producing a positive electrode active material for a lithium secondary battery, wherein the total content of Zr and Y in the formed lithium transition metal oxide is 2500 to 5200 ppm based on the weight of the lithium transition metal oxide.
12. In paragraph 10, A method for producing a positive electrode active material for a lithium secondary battery, wherein the content of Zr in the formed lithium transition metal oxide is 1300 to 2800 ppm based on the weight of the lithium transition metal oxide.
13. In paragraph 10, A method for producing a positive electrode active material for a lithium secondary battery, wherein the content of Y in the formed lithium transition metal oxide is 1400 to 2400 ppm based on the weight of the lithium transition metal oxide.
14. In paragraph 10, The above lithium raw material is a method for manufacturing a positive electrode active material for a lithium secondary battery, wherein the positive electrode active material is Li2CO3.
15. A positive electrode for a lithium secondary battery comprising the positive electrode active material of any one of claims 1 to 9.
16. A lithium secondary battery comprising the positive electrode for a lithium secondary battery of Article 15.
Citation Information
Patent Citations
Positive electrode active material for rechargeable lithium battery, method for menufacturing the same, and rechargeable lithium battery including the same
KR1020170075596A
Preparation method of positive electrode active material for lithium secondary battery and positive electrode active material for lithium secondary battery prepared by using the same
KR1020180004672A
Rod-type battery array module, straight-line rod-type battery pack manufactured by same, and bus bar used therefor
KR1020230114617A
Substrate processing apparatus
KR102728247B1
KR20190117199A