Cathode active material for lithium secondary battery, manufacturing method therefor, and lithium secondary battery comprising same

A single-particle cathode active material with a nickel-containing lithium transition metal oxide and Al/W coating layer addresses the limitations of conventional materials by enhancing capacity and high-temperature performance, achieving improved stability and energy density in lithium secondary batteries.

WO2024248419A1PCT designated stage expired Publication Date: 2024-12-05POSCO FUTURE M CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/007029
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional lithium secondary battery cathode active materials, such as NCM-based lithium composite transition metal oxides, have issues with low particle strength, high specific surface area, and high lithium by-product content, leading to poor lifespan and stability, while single-particle materials face capacity deterioration due to larger crystal grain size and particle diameter.

Method used

A single-particle cathode active material composed of nickel-containing lithium transition metal oxide with a surface coating layer containing Al and W, optimized in composition and heat treatment to achieve improved capacity and high-temperature lifespan characteristics, with specific content ratios and heat treatment conditions.

Benefits of technology

The solution enhances the battery's capacity, energy density, and high-temperature lifespan by controlling the Al and W content, cation mixing ratio, and residual lithium, resulting in improved electrochemical properties and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

The present invention relates to a discrete-particle-form cathode active material for a lithium secondary battery, comprising: a nickel-containing lithium transition metal oxide; and an Al- and W-containing coating layer disposed on the surface of the lithium transition metal oxide, wherein the total amount of Al and W is 2000-6000 ppm on the basis of the total weight of the cathode active material.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode active material for lithium secondary batteries, method for producing the same, and lithium secondary batteries comprising the same

[0001] The present invention relates to a positive electrode active material for a lithium secondary battery, a method for producing the same, and a lithium secondary battery comprising the same, and more specifically, to a positive electrode active material for a lithium secondary battery in the form of a single particle, a method for producing the same, and a lithium secondary battery comprising the same.

[0002]

[0003] Lithium secondary batteries produce electrical energy through oxidation and reduction reactions when lithium ions are inserted / deintercalated from the positive and negative electrodes, while an organic electrolyte or polymer electrolyte is charged between the positive and negative electrodes, which are made of active materials capable of intercalating and deintercalating lithium ions.

[0004] Lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2 or LiMn2O4, etc.), and lithium iron phosphate compound (LiFePO4) have been used as cathode active materials for lithium secondary batteries. Among these, lithium cobalt oxide (LiCoO2) is widely used due to its high operating voltage and excellent capacity characteristics, and is applied as a cathode active material for high voltage. However, due to the rising price of cobalt (Co) and unstable supply, it is difficult to use it in large quantities as a power source in fields such as electric vehicles, and the need for the development of a cathode active material that can replace it has arisen.

[0005] Accordingly, nickel-cobalt-manganese lithium composite transition metal oxides (hereinafter simply referred to as 'NCM-based lithium composite transition metal oxides') in which some of the cobalt (Co) is replaced with nickel (Ni) and manganese (Mn) have been developed. However, the NCM-based lithium composite transition metal oxides developed previously are generally in the form of secondary particles in which primary particles are aggregated, and have a large specific surface area, low particle strength, and a high content of lithium byproducts, which causes a lot of gas generation during cell operation and has problems with low lifespan and stability.

[0006] Accordingly, development is underway for single-particle cathode active materials, rather than conventional secondary particle forms. These single-particle cathode active materials offer the advantages of a small surface area and superior particle strength, leading to improved cycle life and stability. However, single-particle cathode active materials have larger crystal grain sizes and average primary particle diameters than conventional secondary particles, resulting in deteriorated capacity characteristics.

[0007]

[0008] Accordingly, one object of the present invention is to provide a single particle type positive electrode active material having excellent capacity and high-temperature life characteristics, a method for producing the same, and a lithium secondary battery including the same.

[0009]

[0010] One embodiment of the present invention provides a cathode active material for a lithium secondary battery in the form of a single particle, comprising a nickel-containing lithium transition metal oxide and a coating layer containing Al and W disposed on the surface of the lithium transition metal oxide, wherein the total content of Al and W is 2000 to 6000 ppm based on the total weight of the cathode active material.

[0011] The ratio of the content of Al to the total content of Al and W (Al / Al+W) may be 0.28 to 0.7.

[0012] The above-mentioned positive electrode active material for a lithium secondary battery may have a nickel content of 50 to 70 mol% based on the total mole number of transition metals.

[0013] The above-mentioned positive electrode active material for a lithium secondary battery may have a cobalt content of 5 to 20 mol% based on the total mole number of transition metals.

[0014] The above-mentioned positive electrode active material for a lithium secondary battery may have a manganese content of 10 to 40 mol% based on the total mole number.

[0015] The cation mixing ratio of nickel cations in the lithium layer in the above lithium transition metal oxide may be 2.8% or less.

[0016] The positive electrode active material for the above lithium secondary battery may have a residual lithium content of 3000 ppm or less.

[0017] The above-mentioned positive electrode active material for a lithium secondary battery may have a compressed density of 2.2 g / cc or more.

[0018] The above lithium transition metal oxide can be represented by the following chemical formula 1.

[0019] [Chemical Formula 1]

[0020] Li a [Ni x Co y Mn z M1 w1 ]O2

[0021] In the above chemical formula 1, 0.8≤a≤1.2, 0.5≤x≤0.7, 0.05≤y≤0.2, 0.1≤z≤0.4, 0 <w1≤0.1이고, x+y+z+w1=1이고, M1은 Zr, Y, B, Al, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr 또는 이들의 조합이다.

[0022]

[0023] Another embodiment of the present invention provides a method for manufacturing a cathode active material for a lithium secondary battery, comprising the steps of: preparing a nickel-containing transition metal precursor; mixing the transition metal precursor and a lithium raw material, and then calcining and pulverizing the mixture at a temperature of 900 to 960°C to form a lithium transition metal oxide in the form of single particles; and mixing the lithium transition metal oxide, an Al raw material, and a W raw material, and then heat-treating the mixture at a temperature of 400 to 500°C to form a coating layer.

[0024] The above Al raw material may be Al2O3, Al(OH)3, Al2(SO3)3 or a combination thereof.

[0025] The above W raw material is WO2, - It can be WO3, WS2, WS3 or a combination thereof.

[0026] The above Al raw material and W raw material may be oxides.

[0027] The above heat treatment can be performed for 5 to 8 hours.

[0028] The above heat treatment can be performed in an air atmosphere.

[0029]

[0030] Another embodiment of the present invention provides a positive electrode for a lithium secondary battery comprising the positive electrode active material described above.

[0031] Another embodiment of the present invention provides a lithium secondary battery including the positive electrode for the lithium secondary battery.

[0032]

[0033] A cathode active material for a lithium secondary battery according to one embodiment of the present invention is a single particle, but can simultaneously implement excellent capacity and high-temperature life characteristics by appropriately controlling the coating layer components and composition.

[0034]

[0035] The terms first, second, and third, etc., are used to describe, but are not limited to, various parts, components, regions, layers, and / or sections. These terms are used only to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, a first part, component, region, layer, or section described below may be referred to as a second part, component, region, layer, or section without departing from the scope of the present invention.

[0036] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the present invention. As used herein, the singular forms "singular" and "comprising" include plural forms as well, unless the context clearly dictates otherwise. The word "comprising" as used herein specifies a particular feature, region, integer, step, operation, element, and / or component, but does not exclude the presence or addition of other features, regions, integers, steps, operations, elements, and / or components.

[0037] When a part is referred to as being "on" or "over" another part, it can be directly on or over the other part, or there may be other parts intervening. Conversely, when a part is referred to as being "directly on" another part, there are no other parts intervening.

[0038] Although not defined otherwise, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by those of ordinary skill in the technical field to which the present invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with the relevant technical literature and the present disclosure, and are not to be construed as ideal or overly formal unless otherwise defined.

[0039] Also, unless otherwise stated, % means weight%, and 1 ppm is 0.0001 weight%.

[0040] In this specification, the term "combination(s) thereof" described in the expression in the Makushi format means one or more mixtures or combinations selected from the group consisting of the components described in the expression in the Makushi format, and means including any one or more selected from the group consisting of said components.

[0041] In this specification, the term “single particle” is used to distinguish it from the secondary particle type positive electrode active material particle formed by the agglomeration of tens to hundreds of primary particles, which has been commonly used in the past, and is a concept that includes a single particle composed of one primary particle and an aggregate particle of 30 or fewer primary particles. The “secondary particle” refers to an aggregate, i.e., a secondary structure, formed by the physical or chemical bonding between tens to hundreds of primary particles without an intentional agglomeration or assembly process for the primary particles.

[0042] In this specification, “primary particle” means the smallest particle unit that can be distinguished as a single lump when observing the cross-section of a positive electrode active material through a scanning electron microscope (SEM), and may be composed of a single crystal grain or multiple crystal grains.

[0043] In this specification, “crystal grain” means a distinct region in which atoms within a primary particle form a lattice structure with a certain direction.

[0044] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.

[0045]

[0046] 1. Positive active material

[0047] A cathode active material for a lithium secondary battery according to one embodiment of the present invention comprises a nickel-containing lithium transition metal oxide and a coating layer containing Al and W disposed on the surface of the lithium transition metal oxide, and has a single particle form.

[0048] A cathode active material for a lithium secondary battery according to one embodiment of the present invention is a single particle, but includes a coating layer containing Al and W, thereby simultaneously improving the capacity and life characteristics of the battery.

[0049] In particular, the total content of Al and W may be 2000 to 6000 ppm based on the total weight of the positive electrode active material, and more specifically, 2100 to 5900 ppm. By satisfying the above range, the positive electrode active material may have a high compression density, a low cation mixing ratio, and a low residual lithium content. Accordingly, the energy density of the electrode may be increased, and the capacity and life characteristics of the battery may be improved simultaneously.

[0050] In addition, the ratio of the content of Al to the total content of Al and W (Al / Al+W) may be 0.28 to 0.7, and more specifically, 0.29 to 0.7. By satisfying the above range in the ratio of the content of Al to the total content of Al and W, the above-mentioned battery performance improvement effect may be more preferably implemented.

[0051] The cation mixing ratio of nickel cations in the lithium layer of the above lithium transition metal oxide may be 2.8% or less. By satisfying the cation mixing ratio within the above range, the layered structure of the positive electrode active material can be stabilized, thereby improving the life characteristics of the battery.

[0052] The above-mentioned positive electrode active material for a lithium secondary battery may have a residual lithium content of 3000 ppm or less. By satisfying the above range of residual lithium content, gas generation due to side reactions between lithium byproducts and the electrolyte can be reduced, thereby improving the safety and life characteristics of the battery.

[0053] The above-mentioned positive electrode active material for a lithium secondary battery may have a compressed density of 2.2 g / cc or more. In the present specification, the “compressed density” may be calculated by placing 10 g of the positive electrode active material into a cylinder with a diameter of 19.1 mm, applying a force of 108 N, and then measuring the height of the cylinder.

[0054] The above-mentioned positive electrode active material for a lithium secondary battery may have a nickel content of 50 to 70 mol% based on the total mole number of transition metals.

[0055] The above-mentioned positive electrode active material for a lithium secondary battery may have a cobalt content of 5 to 20 mol% based on the total mole number of transition metals.

[0056] The above-mentioned positive electrode active material for a lithium secondary battery may have a manganese content of 10 to 40 mol% based on the total mole number.

[0057] The coating contents of Al and W mentioned above may be more appropriate from the viewpoint of improving the electrochemical properties of the battery mentioned above when the composition of nickel, cobalt and manganese in the lithium transition metal oxide satisfies the above range.

[0058]

[0059] The lithium transition metal oxide can be more specifically represented by the following chemical formula 1.

[0060] [Chemical Formula 1]

[0061] Li a [Ni x Co y Mn z M1 w1 ]O2

[0062] In the above chemical formula 1, 0.8≤a≤1.2, 0.5≤x≤0.7, 0.05≤y≤0.2, 0.1≤z≤0.4, 0 <w1≤0.1이고, x+y+z+w1=1이고, M1은 Zr, Y, B, Al, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr 또는 이들의 조합이다.

[0063]

[0064] 2. Method for manufacturing positive electrode active material

[0065] Another embodiment of the present invention provides a method for manufacturing a cathode active material for a lithium secondary battery, comprising the steps of: preparing a nickel-containing transition metal precursor; mixing the transition metal precursor and a lithium raw material, and then calcining and pulverizing the mixture at a temperature of 900 to 960°C to form a lithium transition metal oxide in the form of single particles; and mixing the lithium transition metal oxide, an Al raw material, and a W raw material, and then heat-treating the mixture at a temperature of 400 to 500°C to form a coating layer.

[0066] The above Al raw material may be Al2O3, Al(OH)3, Al2(SO3)3 or a combination thereof.

[0067] The above W raw material is WO2, It can be WO3, WS2, WS3 or a combination thereof.

[0068] The mixing amount of the above Al raw material and W raw material can be appropriately controlled so that the content of Al and W in the coating layer of the finally obtained positive electrode active material satisfies the above-mentioned range.

[0069] The above Al raw material and W raw material may be oxides. Since the Al raw material and W raw material are oxides, the aforementioned battery performance improvement effect can be more preferably implemented.

[0070] The above heat treatment can be performed for 5 to 8 hours.

[0071] The above heat treatment can be performed in an air atmosphere.

[0072]

[0073] 3. Cathode ray and lithium secondary battery

[0074] Another embodiment of the present invention provides a positive electrode for a lithium secondary battery comprising the positive electrode active material described above.

[0075] More specifically, the positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, and including the positive electrode active material described above.

[0076] The positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 μm, and fine unevenness may be formed on the surface of the positive electrode current collector to increase the adhesion of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.

[0077] The above-described positive electrode active material layer may include a binder and / or a conductive material together with the above-described positive electrode active material.

[0078] At this time, the binder plays a role of improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one kind alone or a mixture of two or more kinds thereof may be used, but is not limited thereto. The binder may be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.

[0079] And, the conductive material is used to provide conductivity to the electrode, and in the battery to be constructed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One type alone or a mixture of two or more types among these may be used, but the present invention is not limited thereto. The conductive material may typically be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.

[0080] The above positive electrode can be manufactured according to a conventional positive electrode manufacturing method, except that the above positive electrode active material is used.

[0081] Specifically, the positive electrode can be manufactured by applying a composition for forming a positive electrode active material layer, including the positive electrode active material described above and optionally a binder, a conductive agent, or a solvent, on a positive electrode current collector, followed by drying and rolling. At this time, the types and contents of the positive electrode active material, binder, and conductive agent are as described above.

[0082] The solvent may be a solvent generally used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water. One of these may be used alone or a mixture of two or more thereof may be used. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, taking into account the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the positive electrode.

[0083] Alternatively, the positive electrode may be manufactured by casting the composition for forming the positive electrode active material layer on a separate support, and then laminating the resulting film on a positive electrode current collector by peeling it off from the support.

[0084]

[0085] Another embodiment of the present invention provides a lithium secondary battery including the positive electrode for a lithium secondary battery as described above.

[0086] The above lithium secondary battery may more specifically include a positive electrode; a negative electrode; a separator; and an electrolyte.

[0087] The above lithium secondary battery may optionally further include a battery container that houses the electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0088] The above negative electrode may include a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.

[0089] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.

[0090] The negative electrode active material layer may optionally include a binder and a conductive material together with the negative electrode active material. As an example, the negative electrode active material layer may be manufactured by applying a composition for forming a negative electrode active material layer comprising the negative electrode active material and optionally a binder and a conductive material onto a negative electrode current collector and drying the composition, or by casting the negative electrode forming composition onto a separate support and then laminating the resulting film onto a negative electrode current collector by peeling the film off from the support.

[0091] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples thereof include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, and Al alloy; metallic oxides capable of doping and dedoping lithium, such as SiOβ (0 < β < 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include natural graphite or artificial graphite in the form of amorphous, plate-like, flaky, spherical, or fiber-like forms, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes.

[0092] The above binder and conductive material may be the same as those described above for the positive electrode.

[0093]

[0094] The above separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used as a separator in lithium secondary batteries can be used without any particular restrictions. In particular, a separator having low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength may be used, and may optionally be used in a single-layer or multi-layer structure.

[0095]

[0096] The above electrolyte may include, but is not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.

[0097] Specifically, the organic liquid electrolyte may include an organic solvent and a lithium salt.

[0098] The organic solvent may be used without any particular limitation as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; Carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (wherein R is a C2 to C20 linear, branched, or cyclic hydrocarbon group, and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, a carbonate solvent is preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery and a linear carbonate compound having low viscosity (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate, etc.) is more preferable.In this case, the performance of the electrolyte may be improved when the cyclic carbonate and the chain carbonate are mixed and used in a volume ratio of about 1:1 to about 1:9.

[0099] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2. LiCl, LiI, or LiB(C2O4)2. It is preferable that the concentration of the lithium salt be used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.

[0100] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexamethylphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 to 5 wt% based on the total weight of the electrolyte.

[0101] As described above, a lithium secondary battery including a cathode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention, and is therefore useful in portable devices such as mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0102] Accordingly, another embodiment of the present invention provides a battery module including the lithium secondary battery as a unit cell and a battery pack including the same.

[0103] The above battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0104]

[0105] Hereinafter, embodiments of the present invention will be described in more detail through examples. However, the following examples are merely preferred embodiments of the present invention, and the present invention is not limited to the following examples.

[0106]

[0107] Example 1

[0108] (1) Manufacturing of positive electrode active material

[0109] (lithium transition metal oxide formation) Ni 0.6 Co 0.1 Mn 0.3After preparing a precursor having a composition of (OH)2, LiOH·H2O and the precursor were placed in a mixer and mechanically mixed so that the molar ratio of lithium to transition metal (Li / M) of the precursor was 1.05 to form a mixture. Thereafter, the mixture was calcined at 940°C for 15 hours under an oxygen atmosphere, naturally cooled, and the calcined product was pulverized to produce a lithium transition metal oxide of single particles.

[0110] (Formation of coating layer) Al2O3 and WO3 were added to the lithium transition metal oxide of single particles obtained as described above so that Al and W were 700 ppm and 1400 ppm, respectively, and mechanically mixed in a mixer, and then heat-treated at 460° C. for 6 hours in an air atmosphere, thereby manufacturing a lithium transition metal oxide according to Example 1.

[0111] (2) Lithium secondary battery manufacturing

[0112] The slurry for manufacturing the electrode plate was mixed with the above-mentioned positive electrode active material: conductive material (carbon black, Denka black): binder (PVDF, KF9700) = 96.5:2.0:1.5 wt%, and the viscosity was adjusted so that the solid content was approximately 60% by adding NMP (N-Methyl-2-pyrrolidone). The manufactured slurry was coated on a 20 μm thick Al foil using a doctor blade, and then dried and rolled. The electrode loading was 16.0 mg / cm 2 and the rolling density (25 ℃, 20 kN) was 3.5 g / cm 3 It was.

[0113] The electrolyte was 1M LiPF6in EC:DMC:DEC=1:2:1 (vol%), with 2.0 vol% VC added to the total amount of the electrolyte, and a coin cell was manufactured using a polyethylene separator and a lithium metal negative electrode (400 μm, NEBA metal).

[0114]

[0115] Other Examples and Comparative Examples

[0116] A positive electrode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the amounts of Al and W added were changed when forming the coating layer, as shown in Tables 1 and 2 below.

[0117]

[0118] Experimental Example 1: Evaluation of Active Material Properties According to Changes in Total Al and W Contents

[0119] (1) Compression density evaluation (g / cc)

[0120] The compression density was evaluated by placing 10 g of positive electrode active material in a cylinder with a diameter of 19.1 mm, applying a pressure of 108 N, and measuring the height of the cylinder.

[0121] (2) Evaluation of cation mixing ratio (%)

[0122] For the positive electrode active material, the cation mixing ratio was measured by dividing the intensity of the (003) peak in the XRD data by the intensity of the (104) peak.

[0123] (3) Residual lithium assessment

[0124] After adding distilled water to the positive electrode active material, the residual lithium was extracted using a stirrer, and the positive electrode active material powder and the extract were separated using a filtering device. The extract was then measured through neutralization titration using a Metrohm potentiometric titrator to evaluate the residual lithium.

[0125] Al coating content (ppm)W coating content (ppm)Al and W total coating content (ppm)Press density (g / cc)Cation mixing (%)Residual lithium (ppm)Comparative example 170070014002.0812.92600Example 1700140021002.2262.62500Example 21600160032002.2362.62800Example 31400320046002.2402.62800Example 41700420059002.2482.52700Comparative example 22100420063002.1982.53200

[0126] Referring to Table 1, in the case of Examples 1 to 4, where the total contents of Al and W, which are coating elements, were appropriately adjusted to the range according to the present invention, it was confirmed that the compression density was large, which predicted an improvement in electrode energy density, and that the cation mixing ratio was small and the residual lithium content was low. On the other hand, in the case of Comparative Example 1, where the total contents of Al and W were too small, it was confirmed that the cation mixing ratio was too large.

[0127] Additionally, in the case of Comparative Example 2 where the total content of Al and W was too high, it was confirmed that the residual lithium content was too high.

[0128]

[0129] Experimental Example 2: Evaluation of battery electrochemical characteristics according to Al / Al+w coating content ratio

[0130] (1) Evaluation of initial discharge capacity and initial efficiency

[0131] The manufactured coin-type half-cells were aged at room temperature (25°C) for 10 hours and then subjected to charge-discharge tests. Capacity evaluation was conducted using a reference capacity of 200 mAh / g, and charge-discharge conditions were applied at CC / CV 2.5–4.4 V with a 1 / 20 C cutoff. The initial capacity was measured by charging at 0.1 C and discharging at 0.1 C.

[0132] (2) Evaluation of high temperature life characteristics (45℃, 50 cycles, %)

[0133] The manufactured coin-type half-cell was subjected to 50 cycles of charge and discharge at 0.5C and 1C discharge (reference capacity 200 mAh / g) under an operating voltage of 2.5 to 4.4 V at 45°C, and the capacity retention rate at the 50th cycle compared to the first cycle was measured.

[0134] (3) Evaluation of high temperature resistance characteristics (45℃, 50 cycles, %)

[0135] The increase in the resistance at 60 seconds of the 50th cycle discharge compared to the resistance at 60 seconds of the first cycle discharge was measured using the method of equation 1 below.

[0136] [Relationship 1]

[0137] {(50 cycle resistance)-(first resistance)} / (first resistance)x100(%)

[0138] Coating amount (ppm) Content ratio (Al / Al+W) 0.1 / 0.1C Discharge capacity (mAh / g) 0.1 / 0.1C Efficiency (%) 45 ℃ 0.5 / 1C 50cyc High temperature life (%) 45 ℃ 0.5 / 1C 50cyc compared to 1cyc Resistance increase (%) Comparative example 3 Al 0W 28000 195.69 0.69 2.5 13 1.3 Example 3 Al 1400W 32000.31 95.79 0.99 4.87 5.5 Example 4 Al 1700W 42000.29 195.49 1.09 5.76 4.6 Example 2 Al 1600W 16000.5 195.69 1.09 5.86 7.8 Example 5 Al 2100W 14000.6195.591.095.568.7Example 6Al 2100W 9000.7195.290.895.473.0Comparative Example 4Al 1400W 01194.290.395.580.2

[0139] Referring to Table 2, in the case of Examples 2 to 6 where the Al / Al+W content ratio was appropriately adjusted, it was confirmed that the battery capacity, initial efficiency, high-temperature lifespan, and resistance characteristics were generally very excellent. On the other hand, in the case of Comparative Example 3 where the Al / Al+W content ratio was too low, it was confirmed that the high-temperature lifespan characteristics were somewhat deteriorated and the high-temperature resistance characteristics were very deteriorated.

[0140] Additionally, in the case of Comparative Example 4 where the Al / Al+W content ratio was too high, it was confirmed that the capacity and high-temperature resistance characteristics were deteriorated.

[0141]

[0142] Although the preferred embodiments of the present invention have been described above, the present invention is not limited thereto, and various modifications can be made within the scope of the patent claims, the detailed description of the invention, and the attached drawings, and it is obvious that this also falls within the scope of the present invention.

[0143] Accordingly, the actual scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A lithium secondary battery cathode active material in the form of a single particle, comprising a nickel-containing lithium transition metal oxide and a coating layer containing Al and W, disposed on the surface of the lithium transition metal oxide, A cathode active material for a lithium secondary battery, wherein the total content of Al and W is 2000 to 6000 ppm based on the total weight of the cathode active material.

2. In paragraph 1, A cathode active material for a lithium secondary battery, wherein the ratio of the content of Al to the total content of Al and W (Al / Al+W) is 0.28 to 0.

7.

3. In paragraph 1, A cathode material for a lithium secondary battery, wherein the content of nickel in the lithium transition metal oxide is 50 to 70 mol% based on the total mole number of transition metals.

4. In paragraph 1, A positive electrode active material for a lithium secondary battery, wherein the content of cobalt in the lithium transition metal oxide is 5 to 20 mol% based on the total mole number of transition metals.

5. In paragraph 1, A cathode active material for a lithium secondary battery, wherein the manganese content in the lithium transition metal oxide is 10 to 40 mol% based on the total mole number of transition metals.

6. In paragraph 1, A cathode active material for a lithium secondary battery, wherein the cation mixing ratio of nickel cations in the lithium layer of the lithium transition metal oxide is 2.8% or less.

7. In paragraph 1, A cathode active material for a lithium secondary battery having a residual lithium content of 3000 ppm or less.

8. In paragraph 1, A cathode active material for a lithium secondary battery having a compression density of 2.2 g / cc or more.

9. In paragraph 1, The above lithium transition metal oxide is a cathode material for a lithium secondary battery represented by the following chemical formula 1: [Chemical Formula 1] Li a [Ni x Co y Mr z M1 w1 ]O2 In the above chemical formula 1, 0.8≤a≤1.2, 0.5≤x≤0.7, 0.05≤y≤0.2, 0.1≤z≤0.4, 0 <w1≤0.1이고, x+y+z+w1=1이고, M1은 Zr, Y, B, Al, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr 또는 이들의 조합이다.

10. Step of preparing a nickel-containing transition metal precursor; A step of mixing the above transition metal precursor and lithium raw material, then calcining and crushing at a temperature of 900 to 960°C to form a lithium transition metal oxide in the form of single particles; and A step of forming a coating layer by mixing the lithium transition metal oxide, Al raw material and W raw material and then heat-treating them at a temperature of 400 to 500°C, A method for manufacturing a cathode active material for a lithium secondary battery.

11. In paragraph 10, A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein the above Al raw material is Al2O3, Al(OH)3, Al2(SO3)3 or a combination thereof.

12. In paragraph 10, The above W raw material is WO2, A method for producing a cathode active material for a lithium secondary battery comprising WO3, WS2, WS3 or a combination thereof.

13. In paragraph 10, The above Al raw material and W raw material are a method for manufacturing a positive electrode active material for a lithium secondary battery, which is an oxide.

14. In paragraph 10, A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein the above heat treatment is performed for 5 to 8 hours.

15. In paragraph 10, A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein the above heat treatment is performed in an air atmosphere.

16. A positive electrode for a lithium secondary battery comprising the positive electrode active material of any one of claims 1 to 9.

17. A lithium secondary battery comprising the positive electrode for a lithium secondary battery of Article 16.

Citation Information

Patent Citations

  • Monocrystal ternary positive electrode material as well as preparation method and application thereof

    CN114243014A

  • Multi-element coated and modified single-crystal lithium nickel cobalt manganate positive electrode material, preparation method thereof and lithium ion battery

    CN115863602A

  • Positive electrode active material for lithium ion secondary battery, and lithium ion secondary battery

    JP2014143032A

  • How to build a homepage with improved loading speed

    KR1020210156368A

  • Mixing tip for impression cartridge

    KR102273859B1