Porous organic-inorganic composite electrolyte membrane, manufacturing method therefor, and lithium secondary battery comprising same
The porous organic-inorganic composite electrolyte membrane, formed by integrating an oxide-based inorganic electrolyte within a fluorine-based polymer matrix, addresses the limitations of organic and inorganic electrolytes in lithium secondary batteries, enhancing stability and performance by suppressing side reactions and maintaining a stable cubic phase, thus improving ionic conductivity and surface properties.
Patent Information
- Application Number
- PCT/KR2024/007117
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-05-24
- Filing Date
- 2024-05-25
- Publication Date
- 2024-12-05
AI Technical Summary
Current lithium secondary batteries face challenges with organic electrolytes due to flammability, corrosiveness, thermal instability, and high voltage vulnerability, while oxide-based inorganic solid electrolytes like LLZO have high ionic conductivity but are difficult to manufacture and have insufficient surface characteristics.
A porous organic-inorganic composite electrolyte membrane is developed by incorporating an oxide-based inorganic electrolyte within a fluorine-based polymer matrix, using a specific solvent combination to suppress side reactions and maintain a cubic phase crystal structure, enhancing ionic conductivity and surface properties.
The solution provides a lithium secondary battery with improved chemical and mechanical stability, excellent lifespan characteristics, and high-rate battery performance by stabilizing the oxide-based inorganic electrolyte and ensuring effective lithium ion transport.
Smart Images

Figure KR2024007117_05122024_PF_FP_ABST
Abstract
Description
Porous organic-inorganic composite electrolyte membrane, method for manufacturing the same, and lithium secondary battery including the same
[0001] The present disclosure relates to a porous organic-inorganic composite electrolyte membrane, a method for manufacturing the same, and a lithium secondary battery including the same.
[0002] With the recent increase in demand for eco-friendly energy, research on electrochemical devices is being conducted in various fields, including electronic devices such as mobile phones and PCs, as well as electric vehicles. Lithium secondary batteries, a general-purpose electrochemical device, are typically composed of a lithium transition metal oxide anode, a graphite-based anode, and an organic electrolyte. To enhance electrochemical performance, such as high capacity, high output, and long life, as well as external effects, such as high / low temperature characteristics, safety, durability, and performance reliability, various new materials are being developed and applied to develop high-performance, next-generation lithium secondary batteries.
[0003] Specifically, in order to solve the safety problems caused by flammability, corrosiveness, thermal instability, and high voltage vulnerability of organic electrolytes, the application of solid electrolytes is being attempted. Among them, garnet-type LLZO (Li7La3Zr2O 12 ) has high ionic conductivity, excellent thermal and chemical stability, and excellent mechanical strength, and exhibits the effect of suppressing lithium dendrites, but has the problem that the manufacturing process is difficult and the surface characteristics are inadequate.
[0004] To solve this problem, research on organic-inorganic composite electrolytes is being conducted, but there are still shortcomings such as poor ionic conductivity and contact performance with Li due to side reactions on the surface of LLZO, and poor surface properties.
[0005] Therefore, there is an urgent need for research and development of solid electrolytes with excellent surface properties, high ionic conductivity, excellent thermal and chemical stability, and outstanding mechanical strength.
[0006] One object of the present disclosure is to provide a porous organic-inorganic composite electrolyte membrane having excellent ionic conductivity and surface properties by effectively suppressing side reactions on the surface of an oxide-based inorganic electrolyte, and a method for manufacturing the same.
[0007] In addition, another object of the present disclosure is to provide a composite electrolyte including the porous organic-inorganic composite electrolyte membrane and the organic electrolyte.
[0008] In addition, another object of the present disclosure is to provide a lithium secondary battery having excellent life characteristics and high-rate battery performance including the composite electrolyte.
[0009] The present disclosure includes an oxide-based inorganic electrolyte and a fluorine-based polymer matrix, wherein the oxide-based inorganic electrolyte is contained within the fluorine-based polymer matrix, and the result of X-ray photoelectron spectroscopy (XPS) analysis of the surface shows that Zr3d in the Zr3d spectrum 5 / 2 A porous organic-inorganic composite electrolyte membrane is provided, wherein the ratio (SCO3 / SZr) of the area of the peak corresponding to CO3 in the C1s spectrum to the area of the peak corresponding to CO3 (SCO3) is greater than 0 and less than or equal to 5.0.
[0010] According to one embodiment, the oxide-based inorganic electrolyte may exhibit a first peak in the 2θ range of 16.5±1.0 as a result of X-ray diffraction analysis (XRD).
[0011] According to one embodiment, the lattice parameter of the oxide-based inorganic electrolyte unit cell calculated by the Rietveld refinement method based on the X-ray diffraction analysis (XRD) spectrum may be 12.90 Å < a=b=c < 13.05 Å.
[0012] According to one embodiment, the oxide-based inorganic electrolyte has a unit cell volume (V) of 2147.0 to 2216.5 Å. 3 It could be.
[0013] According to one embodiment, the oxide-based inorganic electrolyte may be one or a combination of two or more selected from the group consisting of a garnet-type oxide (LLZO), a NASICON-type oxide, and a perovskite-type oxide.
[0014] According to one embodiment, the fluorinated polymer has a Hansen solubility parameter (δ) of 20 to 30 MPa. 0.5 It could be a person.
[0015] According to one embodiment, the porosity of the porous organic-inorganic composite electrolyte membrane may be 30% or more.
[0016] The present disclosure can provide an organic-inorganic composite electrolyte including the porous organic-inorganic composite electrolyte membrane and the organic electrolyte described above.
[0017] According to one embodiment, the organic-inorganic composite electrolyte has an ionic conductivity of 1 x 10 -4 It can be more than S / cm.
[0018] The present disclosure can provide a lithium secondary battery including the above-described organic-inorganic composite electrolyte.
[0019] The present disclosure comprises the steps of (S1) preparing an organic / inorganic electrolyte slurry comprising a fluorine-based polymer, an oxide-based inorganic electrolyte, a first solvent, and a second solvent; and
[0020] (S2) a step of drying the electrolyte slurry to manufacture a porous organic-inorganic composite electrolyte membrane;
[0021] A method for manufacturing a porous organic-inorganic composite electrolyte membrane is provided, wherein the first solvent and the second solvent do not phase separate from each other, and the second solvent and the fluorine-based polymer phase separate from each other.
[0022] In one embodiment, the first solvent may be a polar organic solvent and the second solvent may be a non-polar organic solvent.
[0023] According to one embodiment, the Hansen solubility factor (δ) of the first solvent s1 ) and the Hansen solubility factor (δ) of the above fluorinated polymer m ) may satisfy the following equation 1.
[0024] [Equation 1] δ m - δ s1 < 10 MPa 0.5
[0025] According to one embodiment, the Hansen solubility factor (δ) of the first solvent s1 ) is 17 to 24 MPa 0.5 It could be.
[0026] According to one embodiment, the Hansen solubility factor (δ) of the second solvent s2 ) and the Hansen solubility factor (δ) of the above fluorinated polymer m ) may satisfy the following equation 2.
[0027] [Formula 2] 7 MPa 0.5 ≤δ m - δ s2
[0028] According to one embodiment, the Hansen solubility factor (δ) of the second solvent s2 ) is 17 MPa 0.5 It could be as follows:
[0029] According to one embodiment, the first solvent to the second solvent can satisfy a weight ratio of 5 to 50:1.
[0030] According to one embodiment, the step (S2) may include: (a) applying the electrolyte slurry; (b) drying a first solvent of the electrolyte slurry at a first drying temperature; and (b) drying a second solvent of the electrolyte slurry at a second drying temperature.
[0031] In one embodiment, the second drying temperature may be higher than the first drying temperature.
[0032] The present disclosure can provide a method for manufacturing an organic-inorganic composite electrolyte, including the steps of manufacturing the porous organic-inorganic composite electrolyte membrane described above; and the step of impregnating the porous organic-inorganic composite electrolyte membrane with an organic electrolyte.
[0033] A porous organic-inorganic composite electrolyte membrane according to one embodiment of the present disclosure can exhibit excellent surface properties while possessing high ionic conductivity, superior thermal and chemical stability, and outstanding mechanical strength. Furthermore, a lithium secondary battery including the porous organic-inorganic composite electrolyte membrane can exhibit a significantly improved chemical and mechanical stability compared to a case where an organic electrolyte is used alone, and can exhibit excellent battery performance with excellent cycle life characteristics and high rate characteristics.
[0034] Figure 1 is an image showing changes observed after the organic-inorganic composite electrolyte slurry of Example 1 and Comparative Example 1 was prepared and left at room temperature for 1 hour.
[0035] Fig. 2 is an SEM analysis image of the surface of a porous organic-inorganic composite electrolyte membrane according to Example 1. Specifically, Fig. 2 (a) is an SEM image measured at low magnification, and (b) is an SEM image measured at high magnification.
[0036] Figure 3 shows (a) a SEM analysis image of a cross-section of a porous organic-inorganic composite electrolyte membrane according to Example 1, (b) a porosity analysis result using the Image J program and EDX mapping (c) La element and (d) F element images, and (e) a SEM analysis image of a cross-section of a porous organic-inorganic composite electrolyte membrane according to Example 2, (f) a porosity analysis result using the Image J program and EDX mapping (g) La element and (h) F element images.
[0037] Figure 4 is an X-ray photoelectron spectroscopy (XPS) spectrum of the surface of a porous organic-inorganic composite electrolyte membrane according to Example 1. Specifically, (a) is a C1s spectrum and (b) is a Zr3d spectrum.
[0038] Figure 5 is an X-ray photoelectron spectroscopy (XPS) spectrum of the surface of the electrolyte membrane according to Comparative Example 1. Specifically, (a) is a C1s spectrum and (b) is a Zr3d spectrum.
[0039] Figure 6 is an X-ray photoelectron spectroscopy (XPS) spectrum of the surface of the electrolyte membrane according to Comparative Example 2. Specifically, (a) is a C1s spectrum and (b) is a Zr3d spectrum.
[0040] Figure 7 is an X-ray diffraction analysis (XRD) spectrum of a porous organic-inorganic composite electrolyte membrane according to Example 1.
[0041] Figure 8 is an image of a porous organic-inorganic composite electrolyte membrane according to Example 1, through which the membrane shape and flexibility derived from the excellent surface properties of the porous organic-inorganic composite electrolyte membrane were confirmed.
[0042] Figure 9 is a graph evaluating the high-rate characteristics and life characteristics of the organic-inorganic composite electrolytes of Examples 1 to 3, Comparative Examples 3 and 4.
[0043] The present disclosure is further described in detail through the following implementation examples or examples. However, the following implementation examples or examples are merely references for describing the present disclosure in detail and are not intended to limit the present disclosure, and the present disclosure may be implemented in various forms.
[0044] Additionally, unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure pertains. The terminology used in the description of this disclosure is merely for the purpose of describing particular embodiments and is not intended to be limiting.
[0045] Additionally, the singular forms used in the specification and the appended claims are intended to include the plural forms as well, unless the context clearly dictates otherwise.
[0046] Additionally, when a part is said to "include" a component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.
[0047] In addition, units used in this specification without special mention are based on weight, and for example, units of % or ratio mean weight% or weight ratio, and weight% means the weight% that any one component of the entire composition occupies in the composition unless otherwise defined.
[0048] Additionally, the numerical ranges used herein include lower and upper limits and all values within that range, increments logically derived from the shape and width of the defined range, all doubly defined values, and all possible combinations of upper and lower limits of numerical ranges defined in different shapes. Unless otherwise specifically defined in the specification of the present invention, values outside the numerical range that may arise due to experimental error or rounding of values are also included in the defined numerical range.
[0049] In addition, the term 'Hansen solubility factor' in this specification means the Hansen solubility parameter (proposed by Dr. C. Hansen in 1967) calculated by considering three factors of the degree of bonding within a substance: nonpolar dispersion bonding, polar bonding due to permanent dipoles, and hydrogen bonding.
[0050] Conventionally, when manufacturing organic-inorganic composite solid electrolytes using oxide-based inorganic electrolytes, excessive side reactions with the solvent occur, increasing the viscosity of the slurry and making film formation difficult. Furthermore, the crystal structure of the inorganic electrolyte changes to a tetragonal phase, resulting in significantly degraded surface properties and various other problems, such as reduced ionic conductivity and contact with Li.
[0051] A porous organic-inorganic composite electrolyte membrane according to one embodiment of the present disclosure includes an oxide-based inorganic electrolyte and a fluorine-based polymer matrix, and the oxide-based inorganic electrolyte can be contained within the fluorine-based polymer matrix.
[0052] The porous organic-inorganic composite electrolyte membrane above was analyzed by X-ray photoelectron spectroscopy (XPS) on the surface of the porous organic-inorganic composite electrolyte membrane, and Zr3d was detected in the Zr3d spectrum. 5 / 2 The ratio (SCO3 / SZr) of the area of the peak corresponding to CO3 in the C1s spectrum to the area of the peak corresponding to CO3 (SCO3) in the C1s spectrum may be greater than 0 and less than or equal to 5.0. Accordingly, an oxide-based inorganic electrolyte having a cubic phase crystal structure can be stably formed, thereby suppressing side reactions and ensuring excellent ionic conductivity.
[0053] Hereinafter, each configuration of a porous organic-inorganic composite electrolyte membrane according to an embodiment of the present disclosure will be described.
[0054] The present disclosure provides an organic-inorganic composite electrolyte membrane comprising an oxide-based inorganic electrolyte and a fluorine-based polymer matrix, wherein the oxide-based inorganic electrolyte is contained within the fluorine-based polymer matrix, and as a result of X-ray photoelectron spectroscopy (XPS) analysis of the surface of the electrolyte membrane, Zr3d in the Zr3d spectrum 5 / 2 The area of the peak corresponding to (S Zr ) for the area of the peak corresponding to CO3 in the C1s spectrum (S CO3 ) of the ratio (S) CO3 / S Zr ) provides a porous organic-inorganic composite electrolyte membrane (hereinafter, electrolyte membrane) having a porosity greater than 0 and less than or equal to 5.0.
[0055] According to one embodiment, the results of X-ray photoelectron spectroscopy (XPS) analysis of the surface of the electrolyte membrane show that Zr3d in the Zr3d spectrum 5 / 2 The area of the peak corresponding to (S Zr ) for the area of the peak corresponding to CO3 in the C1s spectrum (S CO3) of the ratio (S) CO3 / S Zr ) may be greater than 0 and less than 5.0, or greater than 0 and less than 4, or greater than 0 and less than 3, or greater than 0 and less than 2.5, or greater than 0 and less than 2, or greater than 0 and less than 1.7, or greater than 0 and less than 1.5, or greater than 0 and less than 1, or greater than 0 and less than 0.5. Or may be 0.1 to 5, 0.1 to 4.6, 0.1 to 4, 0.1 to 3, 0.1 to 2.5, 0.1 to 2, 0.1 to 1.7, 0.1 to 1.5, or 0.1 to 1, 0.1 to 0.5, or 0.5 to 5, 0.5 to 4.0, 0.5 to 3, 0.5 to 2.5, 1.0 to 2.5, 1.0 to 2. According to one embodiment, the electrolyte membrane is CO3 / S Zr ) satisfies the above range, side reactions are effectively suppressed, and an electrolyte membrane having excellent surface characteristics and ionic conductivity can be realized. Although not intended to be bound by a specific theory, the peak corresponding to CO3 may be related to the amount of Li2CO3 produced on the surface of the oxide-based inorganic electrolyte of the electrolyte membrane according to one embodiment.
[0056] According to one embodiment, the fluorinated polymer matrix may be a porous matrix including a fluorinated polymer. A specific description of the fluorinated polymer and the oxide-based inorganic electrolyte will be provided below.
[0057] According to one embodiment, the oxide-based inorganic electrolyte may exhibit a first peak in a 2θ range of 16.5±1.0 as a result of X-ray diffraction analysis (XRD). In addition, the oxide-based inorganic electrolyte may exhibit a second peak in a 2θ range of 30.5±1.0 as a result of XRD, and may exhibit a third peak in a 2θ range of 33.5±1.0.
[0058] According to one embodiment, the oxide-based inorganic electrolyte may have a lattice parameter of a unit cell of 12.90 Å < a=b=c < 13.05 Å, or 12.95 Å < a=b=c < 13.05 Å, or 12.97 Å < a=b=c < 13.04 Å, calculated by the Rietveld refinement method based on an X-ray diffraction (XRD) spectrum.
[0059] According to one embodiment, the volume (V) of the oxide-based inorganic electrolyte unit cell is 2146.69 to 2217.34 Å. 3 may be 2147.0 to 2216.5 Å 3 may be 2165.0 to 2216.5 Å 3 may be 2180.0 to 2190.0 Å 3 It could be.
[0060] According to an embodiment of the present invention, the oxide-based inorganic electrolyte of the porous organic-inorganic composite electrolyte membrane effectively suppresses side reactions with a solvent, thereby stably forming a cubic phase crystal structure having superior ionic conductivity to that of a tetragonal phase.
[0061] According to one embodiment, the thickness of the porous organic-inorganic composite electrolyte membrane may be, but is not limited to, 5 μm to 100 μm, or 10 μm to 80 μm, or 15 μm to 50 μm.
[0062] According to one embodiment, the average pore size of the porous organic-inorganic composite electrolyte membrane may be, but is not limited to, 10 nm to 100 μm, or 20 nm to 50 μm.
[0063] According to one embodiment, the porosity of the porous organic-inorganic composite electrolyte membrane may be 10 to 90%, or 20 to 80%, or 30% or more, or 35% or more, or 40% or more, or 40 to 60%, or 60% or less, or 40 to 50%.
[0064] According to one embodiment, the porous organic-inorganic composite electrolyte membrane can have superior surface properties compared to conventional technologies. Here, the surface properties can be confirmed through the appearance of the electrolyte membrane or the high-rate characteristics of a battery manufactured using the porous organic-inorganic composite electrolyte membrane. If excessive side reactions occur on the surface of the oxide-based inorganic electrolyte, not only is it not flexible, it cannot be manufactured in the form of a membrane, and the movement of lithium ions is restricted, resulting in unstable and poor charge-discharge characteristics during high-rate operation of the battery. However, as shown in FIG. 8, the porous organic-inorganic composite electrolyte membrane according to one embodiment can have a flexible appearance because the side reactions on the surface are effectively suppressed. In addition, as shown in FIG. 9, the lithium secondary battery manufactured using the porous organic-inorganic composite electrolyte membrane according to one embodiment can realize excellent high-rate characteristics because the movement of lithium ions is possible through the surface of the oxide-based inorganic electrolyte.
[0065] The present disclosure can provide an organic-inorganic composite electrolyte comprising the porous organic-inorganic composite electrolyte membrane described above and an organic electrolyte. The organic-inorganic composite electrolyte may be a porous organic-inorganic composite electrolyte membrane impregnated with an organic electrolyte, and may be provided primarily in the form of an organic-inorganic composite electrolyte to a lithium secondary battery described below.
[0066] According to one embodiment, the organic electrolyte may be one or more selected from the group consisting of a liquid electrolyte, a gel polymer electrolyte, a solid polymer electrolyte, etc., and any commonly used or known organic electrolyte may be used without significant limitation as long as it does not impair the physical properties aimed at by the present disclosure. However, the organic electrolyte may not include a fluorine-based organic electrolyte.
[0067] According to one embodiment, the organic electrolyte may include a carbonate-based, ester-based, ether-based, ketone-based, alcohol-based, or aprotic solvent, and the solvents may be used alone or in combination of two or more, and when two or more are used in combination, the mixing ratio may be appropriately adjusted depending on the desired battery performance. For example, two or more may be selected and used from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), and butylene carbonate (BC). In addition, a known solvent in the relevant technical field may be used, but is not limited thereto.
[0068] According to one embodiment, the organic electrolyte may include a lithium salt. The lithium salt may serve as a source of lithium ions in the battery to enable the basic operation of a lithium secondary battery and promote the movement of lithium ions between the positive and negative electrodes. Non-limiting examples of the lithium salt include LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO3C2F5)2, LiN(CF3SO2)2, LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1SO2)(x and y are natural numbers), LiCl, LiI, LiB(C2O4)2 or a combination thereof, but is not limited thereto. The concentration of the lithium salt may be used within the range of 0.1 M to 5.0 M or 0.1 M to 2.0 M.
[0069] According to one embodiment, the organic electrolyte may further include pyridine, triethyl phosphate, triethanolamine, cyclic ether, ethylene diamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxy ethanol, aluminum trichloride, etc. to improve charge-discharge characteristics, flame retardancy characteristics, etc., as needed. In some cases, the organic electrolyte may further include halogen-containing solvents such as carbon tetrachloride and trifluoroethylene to impart incombustibility, and may further include FEC (fluoro-ethylene carbonate), PRS (propene sultone), FPC (fluoro-propylene carbonate), etc. to improve high-temperature storage characteristics.
[0070] According to one embodiment, the thickness of the organic-inorganic composite electrolyte may be, but is not limited to, 5 μm to 500 μm, or 10 μm to 300 μm, or 15 μm to 200 μm.
[0071] According to one embodiment, the ionic conductivity of the organic-inorganic composite electrolyte is 1 x 10 -6 S / cm or more, or 1 x 10 -4 S / cm or more, or 3 x 10 -4 S / cm or more, or 5 x 10 -4 S / cm or more, or 7.5 x 10 -4 S / cm or more, or 1 x 10 -2 S / cm or less, or 5 x 10 -4 1 x 10 -2It can be S / cm, but is not limited to this.
[0072] The present disclosure can provide a lithium secondary battery comprising the above-described organic-inorganic composite electrolyte. The type of the lithium secondary battery is not particularly limited, but a non-limiting example may include a lithium ion battery. Since the lithium ion battery is well known and its configuration is also known, a detailed description thereof will not be provided in the present disclosure.
[0073] A lithium secondary battery according to one embodiment may include a separator between a positive electrode and a negative electrode and the above-described organic-inorganic composite electrolyte. In this case, the positive electrode and negative electrode may be used without limitation as long as they are commonly used in lithium secondary batteries.
[0074] A lithium secondary battery according to an embodiment may have excellent life characteristics, and may have a capacity retention rate after 200 cycles of 80% or more, or 85% or more, or 90% or more, 94% or more, or 99.9% or less according to the evaluation method described below, but is not limited thereto.
[0075] A lithium secondary battery according to an embodiment may have excellent high-rate characteristics, and may have a discharge capacity at 2C according to an evaluation method described below of 50 mAh / g or more, or 60 mAh / g or more, or 90 mAh / g or more, or 100 mAh / g or more, or 110 mAh / g or more, or 200 mAh / g or less, but is not limited thereto.
[0076] Hereinafter, a method for manufacturing a porous organic-inorganic composite electrolyte membrane according to an embodiment will be described in more detail.
[0077] The present disclosure provides a method for manufacturing a porous organic-inorganic composite electrolyte membrane, comprising the steps of (S1) manufacturing an organic-inorganic electrolyte slurry including a fluorinated polymer, an oxide-based inorganic electrolyte, a first solvent, and a second solvent; and (S2) drying the electrolyte slurry to manufacture a porous organic-inorganic composite electrolyte membrane, wherein the first solvent and the second solvent do not phase-separate from each other, and the second solvent and the fluorinated polymer phase-separate from each other. Accordingly, side reactions between the solvent and the oxide-based inorganic electrolyte can be effectively suppressed, thereby improving the storage stability and manufacturing processability of the electrolyte slurry, and stably forming an oxide-based inorganic electrolyte having a cubic phase crystal structure, thereby exhibiting excellent ionic conductivity. Furthermore, a lithium secondary battery having excellent processability, excellent electrochemical performance, and excellent chemical and physical stability can be manufactured using the porous organic-inorganic composite electrolyte membrane.
[0078] According to one embodiment, the fluorinated polymer may be used without significant limitations as long as it is a polymer comprising a repeating unit containing one or more fluorine atoms. When the fluorinated polymer is used, it can exhibit improved thermal stability, high-voltage stability, and mechanical properties.
[0079] Non-limiting examples of the above fluorinated polymers include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinylidene fluoride-co-hexafluoropropylene copolymer (PVdF-co-HFP), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-chlorotrifluoroethylene copolymer (TFE / CTFE), polychlorotrifluoroethylene (PCTFE), and ethylene-chlorotrifluoroethylene copolymer (ECTFE).
[0080] According to one embodiment, the fluorinated polymer may be a polyvinylidene fluoride-co-hexafluoropropylene copolymer (PVdF-co-HFP), or a polyvinylidene fluoride-co-hexafluoropropylene copolymer (PVdF-co-HFP) containing 1 to 50 wt%, or 5 to 30 wt%, or 10 to 20 wt% of HFP.
[0081] According to one embodiment, the fluorinated polymer may have a weight average molecular weight (Mw) of, but not limited to, 100,000 to 5,000,000 g / mol, or 200,000 to 3,000,000 g / mol, or 200,000 to 2,000,000 g / mol, or 300,000 to 1,000,000 g / mol. In addition, the fluorinated polymer may have a number average molecular weight (Mn) of, but not limited to, 50,000 to 3,000,000 g / mol, or 50,000 to 1,000,000 g / mol.
[0082] According to one embodiment, the fluorinated polymer has a Hansen solubility parameter (δ) of 10 to 50 MPa. 0.5 , or 15 to 40 MPa 0.5 , or 20 to 30 MPa 0.5 It could be.
[0083] According to one embodiment, the oxide-based inorganic electrolyte may be any commonly used or known oxide-based inorganic solid electrolyte without significant limitation, or may be any one or a combination of two or more selected from the group consisting of a garnet-type oxide (LLZO), a NASICON-type oxide, and a perovskite-type oxide. The garnet-type oxide may be Li A M1 B La C M2D Zr E M3 F M4 G O H X I (M1 is a monovalent cation, a divalent cation, a trivalent cation, or a combination thereof, M2 is a monovalent cation, a divalent cation, a trivalent cation, or a combination thereof, M3 is a divalent cation, a trivalent cation, a tetravalent cation, a pentavalent cation, a hexavalent cation, or a combination thereof, M4 is Ir, Ru, Mn, Sn, or a combination thereof, X is a monovalent anion, a divalent anion, a trivalent anion, or a combination thereof, 6≤A≤8, 0≤B<2, 2.8≤C≤3, 0≤D≤0.2, 0 <E<2.0, 0<F<2.0, 0<G≤0.2, 9≤H≤12, 및 0≤I≤2)일 수 있고, 상기 나시콘 형 산화물은 Na + x Zr2Si2P 3- x O 12 (0≤x≤3) and the perovskite type oxide is Li a La b TiO c (0 <a≤1, 0<b≤1, 1≤c≤5)일 수 있다.
[0084] According to one embodiment, the fluorine-based polymer to oxide-based inorganic electrolyte can satisfy a weight ratio of 10 to 100:10, or 10 to 50:10, or 15 to 50:10, or 15 to 30:10.
[0085] According to one embodiment, the oxide-based inorganic electrolyte may be included in an amount of 10 to 99.9 wt%, or 20 to 90 wt%, or 30 to 85 wt%, or 50 to 80 wt% based on the total weight of the porous organic-inorganic composite electrolyte membrane.
[0086] According to one embodiment, the Hansen solubility factor (δ) of the first solvent s1 ) and the Hansen solubility factor (δ) of the second solvent s2 ) is δ s2 < δs1 , or δ s2 ≤ δ m -9 MPa 0.5 < δ s1 , or δ s2 ≤ δ m -10 MPa 0.5 < δ s1 can be satisfied. Here, δ m is the Hansen solubility factor of the above fluorinated polymer.
[0087] According to one embodiment, the first solvent may be a polar organic solvent, a polar protic organic solvent, a polar aprotic organic solvent, or a mixture thereof. Non-limiting examples of the polar organic solvent include N-methyl-2-pyrrolidone (NMethyl-2-pyrrolidone; NMP), acetone, dimethyl sulfoxide (DMSO), cyclohexyl-pyrrolidinone (CHP), N-dodecyl-pyrrolidone (N 12P), Benzyl Benzoate, N-Octyl-pyrrolidone (N8P), dimethyl-imidazolidinone (DMEU), Cyclohexanone, dimethylacetamide (DMA), N-Methyl Formamide (NMF), Bromobenzene, Chloroform, Chlorobenzene, Benzonitrile, Quinoline, Benzyl Ether, Ethanol, Isopropyl Alcohol, Methanol, Butanol, 2-Ethoxyethanol, 2-Butoxyethanol, 2-Methoxypropanol, Tetrahydrofuran (THF), Ethylene Glycol, Pyridine, Examples include, but are not limited to, N-vinylpyrrolidone, methyl ethyl ketone (butanone), alpha-terpeneol, formic acid, ethyl acetate, diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), and acrylonitrile.
[0088] In one embodiment, the dipole moment of the first solvent may be from 2 to 10D, or from 2 to 8D, or from 3 to 6D.
[0089] According to one embodiment, the first solvent may be an ether organic solvent. The ether organic solvent may be an acyclic ether organic solvent, a cyclic ether organic solvent, or a mixture thereof. Non-limiting examples of the above ether organic solvents include 1,2-dimethoxyethane, 1,2-diethoxyethane, 1,2-dibuthoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol diethyl ether, 1,3-dioxolane, 4,5-dimethyl-dioxolane, 4,5-diethyl-dioxolane, 4-methyl-1,3-dioxolane, 4-ethyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, 2,5-dimethyl tetrahydrofuran, 2,5-dimethoxy tetrahydrofuran, 2-ethoxy tetrahydrofuran, 2-methoxy-1,3-dioxolane, 2-vinyl-1,3-dioxolaneExamples include 2,2-dimethyl-1,3-dioxolane, 2-methoxy-1,3-dioxolane, 2-ethyl-2-methyl-1,3-dioxolane, tetrahydropyran, 1,4-dioxane, 1,2-dimethoxy benzene, 1,3-dimethoxy benzene, 1,4-dimethoxy benzene, isosorbide dimethyl ether, etc.
[0090] According to one embodiment, the Hansen solubility factor (δ) of the first solvent s1 ) and the Hansen solubility factor (δ) of the above fluorinated polymer m ) can satisfy the following equation 1, or equation 1-1, or equation 1-2, or equation 1-3.
[0091] [Equation 1] δ m - δ s1 < 10 MPa 0.5
[0092] [Formula 1-1] 2.0 MPa 0.5 ≤δ m - δ s1 ≤ 9 MPa 0.5
[0093] [Formula 1-2] 3.0 MPa 0.5 ≤δ m - δ s1 ≤ 6.0 MPa 0.5
[0094] [Formula 1-3] 7.0 MPa 0.5 ≤δ m - δ s1 ≤ 8.5 MPa 0.5
[0095] When the above formula 1, or formula 1-1, or formula 1-2, or formula 1-3 is satisfied, the solubility of the fluorine-based polymer is excellent and phase separation occurs with the second solvent, thereby enabling the production of a porous organic-inorganic composite electrolyte membrane having excellent surface properties and high ionic conductivity.
[0096] According to one embodiment, the Hansen solubility factor (δ) of the first solvent s1 ) is 15 to 25 MPa 0.5 , 17 to 24 MPa 0.5 , or 17.5 to 23.5 MPa 0.5 , or 17.5 to 22.5 MPa 0.5 , 17.5 to 19.0 MPa 0.5 , or 21.0 to 22.0 MPa 0.5 It could be.
[0097] In one embodiment, the first solvent may have a boiling point of 100°C or less, or 0 to 80°C, or 20 to 80°C. Alternatively, the first solvent may have a boiling point less than the boiling point of the second solvent, or 150°C or less, or 10 to 120°C, 50 to 115°C, or 90 to 110°C.
[0098] In one embodiment, the first solvent may have a vapor pressure at room temperature that exceeds the vapor pressure at room temperature of the second solvent, or may be 20 mmHg or more, or 25 to 150 mmHg.
[0099] According to one embodiment, the second solvent may be a nonpolar organic solvent that does not undergo phase separation with the first solvent but undergoes phase separation with the fluorinated polymer. Alternatively, the dipole moment of the second solvent may be 0 to 2D, or 0 to 1D, or 0 to 0.5D.
[0100] According to one embodiment, the second solvent may be a hydrocarbon-based organic solvent, or may be one or a combination of two or more selected from the group consisting of aliphatic hydrocarbon-based organic solvents such as hexane, octane, and heptane; alicyclic hydrocarbon-based organic solvents such as cyclohexane, cyclohexene, ethylcyclohexane, methylcyclohexane, and methylcyclohexene; and aromatic hydrocarbon-based organic solvents such as benzene, toluene, xylene, ethylbenzene, diethylbenzene, trimethylbenzene, and triethylbenzene.
[0101] According to one embodiment, the hydrocarbon-based organic solvent is C 3-30 Hydrocarbon organic solvent, or C 5-12 It may be a hydrocarbon-based organic solvent. Alternatively, the second solvent may be one or a combination of two or more selected from the group consisting of pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane, etc.
[0102] According to one embodiment, the Hansen solubility factor (δ) of the second solvent s2 ) and the Hansen solubility factor (δ) of the above fluorinated polymer m ) can satisfy Equation 2, Equation 2-1, or Equation 2-2.
[0103] [Formula 2] 7 MPa 0.5 ≤δ m - δ s2
[0104] [Formula 2-1] 7 MPa 0.5 ≤δ m - δ s2 ≤ 20 MPa 0.5
[0105] [Formula 2-2] 8 MPa 0.5 ≤δ m - δ s2 ≤ 15 MPa 0.5
[0106] When the second solvent satisfies the dipole moment condition and Equation 2, or Equation 2-1, or Equation 2-2, when the second solvent satisfying the above conditions is used, the side reaction between the oxidizing inorganic electrolyte and the solvent is effectively suppressed, thereby improving the storage stability of the slurry, and an oxidizing inorganic electrolyte having a cubic crystal structure can be stably formed, thereby producing a porous organic-inorganic composite electrolyte membrane having excellent surface properties and ionic conductivity.
[0107] According to one embodiment, the Hansen solubility factor (δ) of the second solvent s2 ) is 17 MPa 0.5 or less, or 1 to 17 MPa 0.5 , or 7 to 17 MPa 0.5 , or 10 to 17 MPa 0.5 It could be.
[0108] In one embodiment, the second solvent may have a boiling point greater than the boiling point of the first solvent, or may be 100°C or higher, or 100 to 300°C, or 110 to 230°C.
[0109] In one embodiment, the second solvent may have a vapor pressure at room temperature less than the vapor pressure at room temperature of the first solvent, or may be 15 mmHg or less, or 0.5 to 12 mmHg.
[0110] According to one embodiment, the first solvent to the second solvent may have a weight ratio of 0.1 to 100:1, or 1 to 80:1, or 5 to 50:1, or 10 to 30:1.
[0111] According to one embodiment, the first solvent and the second solvent can achieve the purpose to be implemented in the present disclosure by satisfying the above-described properties within a specific range.
[0112] The method for manufacturing a porous organic-inorganic composite electrolyte membrane according to an embodiment of the present invention can use any method commonly used or known for manufacturing a porous membrane without significant limitations, as long as it does not impair the physical properties aimed at in the present disclosure, and specifically, a dry phase inversion method can be used.
[0113] According to one embodiment, the step (S2) may include: (a) applying the electrolyte slurry; (b) drying the first solvent of the electrolyte slurry at a first drying temperature (hereinafter, primary drying); and (b) drying the second solvent of the electrolyte slurry at a second drying temperature (hereinafter, secondary drying).
[0114] According to one embodiment, the coating may be applied using a conventional or known coating or application method without significant limitation, and for example, spin coating, dip coating, ink-jet printing, spray coating, screen printing, drop casting, or a doctor blade may be used. In addition, the amount of application may be easily controlled depending on the thickness of the electrolyte membrane to be manufactured.
[0115] According to one embodiment, the second drying temperature may be higher than the first drying temperature. The first drying is a step in which the first solvent is dried, and the first drying temperature may be 0 to 80°C, or 10 to 50°C. The second drying is a step in which the second solvent is dried, and the second drying temperature may be 80 to 300°C, or 90 to 150°C.
[0116] The present disclosure can provide a porous organic-inorganic composite electrolyte membrane manufactured according to the above-described manufacturing method, and can satisfy the above-described physical properties.
[0117] The present disclosure can provide a method for manufacturing an organic-inorganic composite electrolyte, including the steps of manufacturing a porous organic-inorganic composite electrolyte membrane according to the method for manufacturing a porous organic-inorganic composite electrolyte membrane described above; and the step of impregnating the porous organic-inorganic composite electrolyte membrane with an organic electrolyte. The method for impregnating the organic electrolyte can be used without limitation by methods used in the same technical field, and can be easily selected and performed according to known methods. Since specific performance conditions are publicly known, they are not specifically described in the present disclosure.
[0118] According to one embodiment, an organic-inorganic composite electrolyte may be manufactured by injecting an organic electrolyte including a lithium salt and a solvent into the porous organic-inorganic composite electrolyte membrane described above; or by injecting and curing an organic electrolyte including a curable monomer and an initiator. However, the present invention is not limited thereto. The organic electrolyte may be injected or impregnated according to a conventional or known method used in the relevant field, and when the organic-inorganic composite electrolyte according to one embodiment is used, the side reaction of the oxide-based inorganic electrolyte is minimized compared to when a conventional organic electrolyte is used alone, so that the effect of significantly improving ionic conductivity can be realized.
[0119] The present disclosure is described in more detail based on the following examples and comparative examples. However, the following examples and comparative examples are merely illustrative examples for further explaining the present disclosure, and the present disclosure is not limited by the following examples and comparative examples.
[0120] First, the method for measuring and evaluating the properties of the membrane is explained.
[0121] [Physical property evaluation method]
[0122] 1. X-ray photoelectron spectroscopy (XPS)
[0123] The surface of the manufactured electrolyte membrane was analyzed using an XPS (X-ray Photoelectron Spectrometer) (Thermo Scientific ESCALAB 250Xi). The measurement conditions are as follows. For surface analysis, the surface was etched with Ar ions and then measured, and the measured XPS spectra are shown in Figures 4 to 6.
[0124] [XPS measurement conditions]
[0125] -X-ray type: Source - Al Ka(alpha) 1486.68eV, Beam size 900 ㎛
[0126] -Analyzer: CAE Mode
[0127] -Number of scans: 2(survey scan), 20 (Narrow Scan)
[0128] -Pass energy: 150eV (survey Scan), 20eV (Narrow Scan)
[0129] -Ion gun: Ar ion
[0130] Also, in the Zr3d spectrum, Zr3d 5 / 2 The area of the peak corresponding to (S Zr ) and the area of the peak corresponding to CO3 in the C1s spectrum (S CO3 ) was analyzed based on XPS analysis to calculate the area obtained by analyzing each element peak. Specifically, in the C1s spectrum, peaks corresponding to CC (284.8 eV), CO, C=O, CO3, and CF were analyzed, and the area corresponding to each peak was calculated, and the area of C=O was obtained among them. The method for obtaining the area was using a commonly used analysis technique.
[0131] 2. X-ray diffraction analysis (XRD)
[0132] The electrolyte membrane was analyzed using an X-ray diffractometer (PANalytical). The measurement conditions were as follows.
[0133] [XRD measurement conditions]
[0134] -Anode material: Cu
[0135] -K-Alpha1 wavelength:1.540598 Å
[0136] -Generator voltage: 45 kV
[0137] -Tube current: 40 mA
[0138] -Scan Range: 10~80°
[0139] - Incidence Beam: BBHD
[0140] -Divergence slit: 1 / 4°
[0141] -Antiscatter slit: 1°
[0142] The analysis results of the measured XRD spectrum using the Rietveld method are shown in Fig. 7, through which the peaks corresponding to the crystal planes of the (112) plane, (024) plane, and (224) plane were analyzed, and the lattice parameter and lattice volume (V) of the oxide-based inorganic electrolyte unit cell are also shown in Table 2 below.
[0143] 3. Porosity (%)
[0144] Porosity was measured by calculating the pore area of the cross-sectional SEM image of the electrolyte membrane using the automatic contrast function of the Image J program.
[0145] 4. Electrolyte uptake rate (%)
[0146] The electrolyte impregnation rate of the manufactured electrolyte membrane was measured using the following calculation formula 1 and is shown in Table 2 below.
[0147] [Calculation Formula 1]
[0148] Electrolyte impregnation rate (%) =
[0149] In the above calculation formula 1, W0 is the weight of the pure electrolyte membrane, and W is the weight of the electrolyte membrane impregnated with the organic electrolyte (1.0 M LiPF6-EC / EMC (3 / 7, v / v) + FEC 5 wt.%).
[0150] 5. Ionic conductivity [S / cm]
[0151] The manufactured porous organic-inorganic composite electrolyte membrane was sandwiched between stainless steel (1 mm thick), 1 M LiPF6 was dissolved in a mixed solvent containing EC / EMC in a volume ratio of 3:7, and an organic electrolyte containing 5 wt.% of FEC was injected to manufacture a coin cell type battery including an organic-inorganic composite electrolyte.
[0152] The manufactured battery was analyzed by EIS (Electrochemical Impedance Spectroscopy, measurement conditions: Frequency 1.0 MHz to 0.1 Hz, Amplitude potential 10 mV) and the ionic conductivity was measured using the following calculation formula 2, which is shown in Table 2 below.
[0153] [Calculation Formula 2]
[0154]
[0155] (In the above calculation formula 2, σ is ionic conductivity, R is resistance (Z), L is thickness, and A is area.)
[0156] 6. Life characteristics and high-rate characteristics
[0157] Graphite cathode / organic-inorganic composite electrolyte / LiNi 0.8 Mn 0.1 Co 0.1Coin cell type batteries manufactured with O2 cathode configuration were subjected to various charge and discharge conditions at voltages from 2.5 V to 4.2 V, and current densities of 0.1 C, 0.3 C, 0.3 C, 0.5 C, 1.0 C, 2.0 C, and 5.0 C were charged and discharged 5 times each to observe the changes, and the discharge capacity [mAh / g] under 2C discharge conditions is shown in Table 2 below. Then, 200 charge and discharge cycles were performed under 0.5 C charge conditions / 1.0 C discharge conditions to evaluate the life characteristics of the battery. The life characteristics were measured by measuring the capacity retention rate after charge and discharge, which is expressed as the ratio (%) of the discharge capacity after 200 cycles of repeated charge and discharge to the initial discharge capacity, and the results are shown in Table 3 below, and the graph of the results is illustrated in Fig. 9.
[0158] [Example 1]
[0159] P(VdF-co-HFP) (HFP 12 wt%, Hansen solubility factor (δ)) as a fluorinated polymer in the first solvent (THF) m ): 26.4 MPa 0.5 ) was dissolved at a concentration of 10 wt%, and then garnet-type LLZO and the second solvent (octane) were added and stirred / ball milled to prepare an electrolyte slurry. At this time, the Hansen solubility factor (δ) of the first solvent s1 ) and the Hansen solubility factor (δ) of the second solvent s2 ) are shown in Table 1 below. In addition, the first solvent to the second solvent were added in a weight ratio of 17:1, and the fluorinated polymer to the garnet-type LLZO were added in a weight ratio of 3:7. In order to evaluate the storage stability of the manufactured slurry, the changes after leaving it at room temperature for 1 hour were observed and shown in Fig. 1.
[0160] The prepared slurry was cast onto an electrode or a release film using a doctor blade, and dried at room temperature to produce a porous fluorine-based polymer matrix film. Subsequently, the film was dried at 100°C under vacuum to obtain a porous organic-inorganic composite electrolyte membrane according to Example 1.
[0161] [Example 2]
[0162] A porous organic-inorganic composite electrolyte membrane according to Example 2 was manufactured in the same manner as Example 1, except that the weight ratio of the fluorine-based polymer to the garnet-type LLZO in Example 1 was introduced so as to satisfy 2:8.
[0163] [Example 3]
[0164] A porous organic-inorganic composite electrolyte membrane according to Example 3 was manufactured in the same manner as Example 2, except that EMC (ethyl methyl carbonate) was used as the first solvent in Example 2.
[0165] [Comparative Example 1]
[0166] The same procedure as Example 1 was followed, except that DMF was used as the first solvent.
[0167] [Comparative Example 2]
[0168] The same procedure as Example 1 was followed, except that acetone was used as the first solvent.
[0169] [Comparative Example 3]
[0170] The same procedure as Example 1 was followed, except that zirconium oxide (ZrO2) was used instead of garnet-type LLZO in Example 1.
[0171] [Comparative Example 4]
[0172] The same procedure as Example 2 was followed, except that zirconium oxide (ZrO2) was used instead of garnet-type LLZO in Example 2.
[0173] First solvent, second solvent type δ s1 [MPa 0.5 ]Typeδ s2 [MPa 0.5]Example 1THF 21.9 octane 15.5Example 2THF 21.9 octane 15.5Example 3EMC 18.0 octane 15.5Comparative Example 1DMF 24.9 octane 15.5Comparative Example 2Acetone 20.0 octane 15.5Comparative Example 3DMF 24.9 octane 15.5Comparative Example 4Acetone 20.0 octane 15.5
[0174] The physical properties of the porous organic-inorganic composite electrolyte membranes obtained according to Examples 1 to 3 and Comparative Examples 1 to 4, such as XPS, XRD, porosity, electrolyte impregnation amount, surface characteristics, and ionic conductivity, were analyzed / measured and shown in Table 2 below. However, in the case of Comparative Examples 1 and 2, the membrane forming solution gelled, making it impossible to manufacture the membrane, and thus the porosity, electrolyte impregnation amount, and ionic conductivity could not be measured.
[0175] In addition, scanning electron microscope (SEM) images of the surface and cross-section of the porous inorganic composite electrolyte membranes of Examples 1 and 2 are shown in Fig. 2, and EDX mapping images are shown in Fig. 3. From the EDX mapping images, it can be confirmed that the oxide-based inorganic electrolyte and the fluorine-based polymer electrolyte are evenly distributed within the electrolyte membrane.
[0176] S CO3 / S Zr Lattice constant a=b=c[Å]Lattice volume[Å 3 ]Porosity [%]Electrolyte impregnation rate [%]Ionic conductivity [S / cm]Example 11.0712.98842191.1540.435.14.8 x10 -4 Example 20.1712.98372188.7844.337.58.7 x10 -4 Example 31.513.035732215.16542.736.88.3 x10 -4 Comparative Example 15.713.058122226.598---Comparative Example 226.413.062102228.636---Comparative Example 3---41.536.33.4 x10 -4 Comparative Example 4---45.838.77.5 x10 -4
[0177] As shown in Table 2 above, S in the X-ray photoelectron spectroscopy (XPS) spectra of the porous organic-inorganic composite electrolyte membrane surfaces according to Examples 1 to 3 CO3 / S Zr While Comparative Examples 1 and 2 both showed values exceeding 5, the porous organic-inorganic composite electrolyte membrane according to one embodiment confirmed that the side reaction of the oxide-based inorganic electrolyte on the surface was effectively suppressed.
[0178] Specifically, in the case of Examples 1 to 3, since the oxide-based inorganic electrolyte surface was stably maintained, lithium ion transfer through the oxide particles and the oxide surface was activated, resulting in high ionic conductivity. In particular, in the case of Example 2, it was confirmed that higher ionic conductivity was exhibited than in Example 1 as the oxide-based inorganic electrolyte content increased. In addition, through Fig. 8, it was confirmed that the porous organic-inorganic composite electrolyte membrane according to Example 1 had excellent surface characteristics and a flexible appearance.
[0179] Through this, it was confirmed that the porous organic-inorganic composite electrolyte membrane according to one embodiment exhibited superior values in porosity, impregnation rate, and ionic conductivity compared to the comparative example.
[0180]
[0181] In addition, the composite electrolytes manufactured according to Examples 1 to 3 and Comparative Examples 3 and 4 were evaluated for life characteristics and high-rate characteristics according to the evaluation method described above, and the results are shown in Table 3 and Figure 9 below.
[0182] Ionic Conductivity [S / cm] Discharge Capacity (@2C) [mAh / g] Capacity Retention [%] Example 14.8 x10 -4 7592 Example 28.7 x10 -4 11992 Example 38.3 x10 -4 11795 Comparative Example 33.4 x10 -4 1642 Comparative Example 47.5 x10 -4 1743
[0183] As shown in Table 3 above, the battery including the organic-inorganic composite electrolyte according to one embodiment exhibited a very high discharge capacity even at a high rate compared to the comparative example, and the capacity retention rate measured after 200 cycles also showed an excellent value of more than twice.
[0184] Specifically, Examples 1 to 3, especially Examples 2 and 3, maintained the oxide-based inorganic electrolyte surface stably, so that lithium ion transfer through oxide particles and the oxide surface was activated, and thus excellent high-rate characteristics and stable charge-discharge performance were exhibited compared to Comparative Examples 3 and 4. In addition, in the case of Example 2, the high-rate characteristics were improved as the oxide-based inorganic electrolyte content increased compared to Example 1, and in the case of Example 3, it was confirmed that the capacity retention rate was improved compared to Example 2. On the other hand, in the case of Comparative Examples 3 and 4, since an oxide that does not contain lithium ions was used, additional lithium ion transfer was impossible, which was disadvantageous in securing high-rate performance.
[0185] Through this, it was confirmed that when a lithium secondary battery is manufactured including an organic-inorganic composite electrolyte according to one embodiment, significantly improved life characteristics and high-rate characteristics can be realized.
[0186] Therefore, a porous organic-inorganic composite electrolyte membrane according to an embodiment is manufactured using an electrolyte slurry including a first solvent, a second solvent, a fluorinated polymer, and an oxide-based inorganic electrolyte that satisfy the above-described conditions, thereby exhibiting excellent surface properties and minimizing side reactions of the oxide-based inorganic electrolyte, thereby realizing the effect of significantly improving ionic conductivity. In addition, it was confirmed that when a lithium secondary battery is manufactured using an organic-inorganic composite electrolyte including the porous organic-inorganic composite electrolyte membrane, it can have cycle-life characteristics and high-rate characteristics that are superior to those of the prior art.
[0187] Although the present disclosure has been described with specific details and limited examples, these are provided only to help a more general understanding of the present disclosure, and the present disclosure is not limited to the above examples, and those skilled in the art to which the present disclosure pertains can make various modifications and variations based on these descriptions.
[0188] Therefore, the present disclosure should not be limited to the embodiments described above, and all things that are equivalent or equivalent to the claims described below as well as the same are included in the scope of the present disclosure.
Claims
1. Contains an oxide-based inorganic electrolyte and a fluorine-based polymer matrix, The above oxide-based inorganic electrolyte is contained within the fluorine-based polymer matrix, X-ray photoelectron spectroscopy (XPS) analysis of the surface, Zr3d spectrum 5 / 2 The area of the peak corresponding to (S Zr ) for the area of the peak corresponding to CO3 in the C1s spectrum (S CO3 ) of the ratio (S) CO3 / S Zr ) is greater than 0 and less than or equal to 5.
0.
2. In paragraph 1, The above oxide-based inorganic electrolyte is a porous organic-inorganic composite electrolyte membrane, which exhibits a first peak in the 2θ range of 16.5±1.0 as a result of X-ray diffraction analysis (XRD).
3. In paragraph 1, A porous organic-inorganic composite electrolyte membrane having a lattice parameter of the oxide-based inorganic electrolyte unit cell calculated by the Rietveld refinement method based on an X-ray diffraction analysis (XRD) spectrum of 12.90 Å < a=b=c < 13.05 Å.
4. In paragraph 1, The above oxide-based inorganic electrolyte has a unit cell volume (V) of 2147.0 to 2216.5 Å. 3 A porous organic-inorganic composite electrolyte membrane.
5. In paragraph 1, The above oxide-based inorganic electrolyte is a porous organic-inorganic composite electrolyte membrane, which is one or a combination of two or more selected from the group consisting of a garnet-type oxide (LLZO), a NASICON-type oxide, and a perovskite-type oxide.
6. In paragraph 1, The above fluorinated polymer has a Hansen solubility parameter (δ) of 20 to 30 MPa. 0.5 A porous organic-inorganic composite electrolyte membrane.
7. In paragraph 1, A porous organic-inorganic composite electrolyte membrane having a porosity of 30% or more.
8. An organic-inorganic composite electrolyte comprising a porous organic-inorganic composite electrolyte membrane and an organic electrolyte according to any one of claims 1 to 7.
9. In paragraph 8, Ionic conductivity is 1 x 10 -4 Organic / inorganic composite electrolyte with a density of S / cm or more.
10. A lithium secondary battery comprising the organic-inorganic composite electrolyte of Article 8. 11.(S1) A step of preparing an organic / inorganic electrolyte slurry including a fluorine-based polymer, an oxide-based inorganic electrolyte, a first solvent, and a second solvent; and (S2) a step of drying the electrolyte slurry to manufacture a porous organic-inorganic composite electrolyte membrane; The first solvent and the second solvent do not phase separate from each other, A method for manufacturing a porous organic-inorganic composite electrolyte membrane in which the second solvent and the fluorine-based polymer are phase-separated from each other.
12. In paragraph 11, A method for manufacturing a porous organic-inorganic composite electrolyte membrane, wherein the first solvent is a polar organic solvent and the second solvent is a non-polar organic solvent.
13. In paragraph 11, Hansen solubility factor (δ) of the first solvent s1 ) and the Hansen solubility factor (δ) of the above fluorinated polymer m ) is a method for manufacturing a porous organic-inorganic composite electrolyte membrane that satisfies the following equation 1. [식 1] d m - d s1 < 10 MPa 0.5 14. In paragraph 11, Hansen solubility factor (δ) of the first solvent s1 ) is 17 to 24 MPa 0.5 A method for manufacturing a porous organic-inorganic composite electrolyte membrane.
15. In paragraph 11, Hansen solubility factor (δ) of the above second solvent s2 ) and the Hansen solubility factor (δ) of the above fluorinated polymer m ) is a method for manufacturing a porous organic-inorganic composite electrolyte membrane that satisfies the following equation 2. [Formula 2] 7 MPa 0.5 ≤δ m - δ s2 16. In paragraph 11, Hansen solubility factor (δ) of the above second solvent s2 ) is 17 MPa 0.5 A method for manufacturing a porous organic-inorganic composite electrolyte membrane is described below.
17. In paragraph 11, A method for manufacturing a porous organic-inorganic composite electrolyte membrane in which the first solvent and the second solvent satisfy a weight ratio of 5 to 50:
1.
18. In paragraph 11, A method for manufacturing a porous organic-inorganic composite electrolyte membrane, wherein the step (S2) comprises: (a) applying the electrolyte slurry; (b) drying a first solvent of the electrolyte slurry at a first drying temperature; and (b) drying a second solvent of the electrolyte slurry at a second drying temperature.
19. In paragraph 18, A method for manufacturing a porous organic-inorganic composite electrolyte membrane, wherein the second drying temperature is higher than the first drying temperature.
20. A step of manufacturing a porous organic-inorganic composite electrolyte membrane according to any one of claims 11 to 19; and A method for manufacturing an organic-inorganic composite electrolyte, comprising the step of impregnating an organic electrolyte into the porous organic-inorganic composite electrolyte membrane.
Citation Information
Patent Citations
Composite solid electrolyte slurry, film, preparation method and all-solid-state battery
CN112687945A
Composite electrolyte membrane, preparation method thereof and all-solid-state lithium battery
CN115312836A
Organic / inorganic composite electrolyte, electrode-electrolyte assembly and lithium secondary battery containing the same, and manufacturing method of the electrode-electrolyte assembly
KR1020160068464A
Organic-inorganic complex solid polymer electrolytes membrane, manufacturing method thereof and all solid battery including thereof
KR1020160079405A
Volumetric chip and method for detecting analyte using the same