Method for manufacturing positive electrode slurry composition and method for manufacturing positive electrode
The method of cooling and maintaining the positive electrode slurry composition at specific temperatures effectively stabilizes viscosity, addressing gelation issues and improving manufacturing efficiency for lithium secondary batteries with high solid content.
Patent Information
- Application Number
- PCT/KR2024/007490
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-31
- Publication Date
- 2024-12-05
AI Technical Summary
The challenge is to develop a method for producing a positive electrode slurry composition with a high solid content that suppresses viscosity increase over time, preventing gelation and ensuring stable manufacturing of lithium secondary batteries, particularly with lithium nickel composite metal oxides which have poor thermal stability and leave impurities leading to gelation issues.
A method involving mixing a positive electrode active material, conductive material, and binder in a non-aqueous solvent to create a slurry with a solid content over 60%, followed by cooling to -30°C or more and 15°C or less to prepare a slurry precursor, and maintaining this temperature to control viscosity increase, using specific lithium complex transition metal compounds and adjusting the composition to limit viscosity growth.
This approach effectively stabilizes the viscosity of the positive electrode slurry, allowing for improved manufacturing efficiency and quality by preventing gelation, even with high solid content, and extending the storage time of the slurry without significant viscosity increase, thus enhancing the production process.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Method for producing anode slurry composition and method for producing anode
[0001] Cross-citation with related applications
[0002] This application claims the benefit of priority from Korean Patent Application No. 10-2023-0070276, filed May 31, 2023, the entire contents of which are incorporated herein by reference.
[0003] Technology field
[0004] The present invention relates to a method for producing a positive electrode slurry composition and a method for producing a positive electrode.
[0005]
[0006] As technological development and demand for mobile devices increase, the demand for secondary batteries as an energy source is rapidly increasing. Among these secondary batteries, lithium secondary batteries, which boast high energy density and voltage, long cycle life, and low self-discharge rates, are commercialized and widely used.
[0007] Lithium-transition metal composite oxides are used as cathode active materials in lithium secondary batteries. Among these, lithium-cobalt composite metal oxides such as LiCoO2, which exhibit high operating voltage and excellent capacity characteristics, are primarily used. However, LiCoO2 suffers from poor thermal properties due to crystal structure instability following delithiation. Furthermore, its high cost limits its mass use as a power source in fields such as electric vehicles.
[0008] As a material to replace the above LiCoO2, lithium manganese composite metal oxides (such as LiMnO2 or LiMn2O4), lithium iron phosphate compounds (such as LiFePO4), or lithium nickel composite metal oxides (such as LiNiO2) have been developed. Among these, research and development on lithium nickel composite metal oxides, which have a high reversible capacity of about 200 mAh / g and make it easy to implement large-capacity batteries, is being actively studied. However, LiNiO2 has inferior thermal stability compared to LiCoO2, and there was a problem that the positive electrode active material itself decomposed when an internal short circuit occurred due to external pressure in a charged state, causing the battery to rupture and catch fire. Accordingly, as a method to improve the low thermal stability of LiNiO2 while maintaining the excellent reversible capacity, lithium transition metal oxides in which some of the Ni was replaced with Co, Mn, or Al were developed.
[0009] Lithium nickel composite metal oxides and lithium transition metal oxides containing a large amount of nickel leave a relatively large amount of lithium oxide as an impurity during the manufacturing process, and the impurities can be converted to LiOH and Li2CO3, which can cause a gelation phenomenon during the manufacturing process of the positive electrode slurry and the process of manufacturing the positive electrode using the manufactured positive electrode slurry. If the positive electrode slurry gelates, the viscosity increases, which can cause problems in the positive electrode manufacturing process, and thus, a lot of cost and effort are required for process management.
[0010] In addition, increasing the solid content of the positive electrode slurry has effects such as increased productivity, electrode drying efficiency, and improved binder migration, but as the solid content increases, specifically, when the solid content exceeds 60%, the viscosity increases, and the viscosity of the manufactured positive electrode slurry increases rapidly over time. In this way, if the increase in viscosity of the positive electrode slurry becomes severe, problems may occur in the quality of the positive electrode manufactured using it, and the positive electrode slurry itself may become difficult to use in the manufacture of positive electrodes.
[0011] Therefore, there is a need to develop a method that can suppress the increase in viscosity over time after manufacturing a high solids content cathode slurry.
[0012]
[0013] [Prior Art Literature]
[0014] [Patent Document]
[0015] Japanese Patent Publication No. 2007-141649
[0016]
[0017] The object of the present invention is to provide a method for producing a positive electrode slurry composition capable of suppressing an increase in viscosity of a positive electrode slurry composition having a solid content exceeding 60%.
[0018] Another object of the present invention is to provide a method for manufacturing a positive electrode using a positive electrode slurry composition with controlled increase in viscosity.
[0019]
[0020] To solve the above problem, the present invention provides a method for producing a positive electrode slurry composition and a method for producing a positive electrode.
[0021] (1) The present invention comprises the steps of (S1) preparing a mixture having a solid content of more than 60 wt% by mixing a positive electrode active material, a conductive material, and a binder in a non-aqueous solvent; (S2) preparing a positive electrode slurry composition precursor by cooling the mixture to a temperature of -30°C or higher and 15°C or lower; and (S3) maintaining the temperature of the positive electrode slurry composition precursor to V 72 A step of preparing a positive electrode slurry composition having 0% or more and 50% or less of V; comprising: n The present invention provides a method for manufacturing a positive electrode slurry composition, wherein the viscosity increase rate is expressed by the following mathematical formula 1 when the temperature of the positive electrode slurry composition precursor is maintained for n hours.
[0022] [Mathematical Formula 1]
[0023] Viscosity increase rate (Vn[%]) = (VS2[cP] - VS1[cP] X 100 / VS1[cP])
[0024] In the above mathematical expression 1, VS1 is the viscosity [cP] of the mixture, and VS2 is the viscosity [cP] of the positive electrode slurry composition.
[0025] (2) The present invention provides a method for producing a positive electrode slurry composition, wherein, in the above (1), the positive electrode active material comprises at least one selected from among lithium composite transition metal compounds having a composition represented by the following chemical formulas 1 to 4.
[0026] [Chemical Formula 1]
[0027] Li a [Ni b Co c Mn d M 1 1-(b+c+d) ]O2
[0028] In the above chemical formula 1,
[0029] M 1is at least one selected from the group consisting of Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi,
[0030] 0.9≤a≤1.1, 0 <b<1, 0<c<1, 0<d<1, 0<b+c+d≤1이고,
[0031] [Chemical Formula 2]
[0032] Li e Ni 1-f M 2 f O2
[0033] In the above chemical formula 2,
[0034] M 2 is at least one selected from the group consisting of Mn, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi,
[0035] 0.9≤e≤1.1, 0≤f<1,
[0036] [Chemical Formula 3]
[0037] Li g Ni h Mn i M 3 j O2
[0038] In the above chemical formula 3,
[0039] M 3 is at least one selected from the group consisting of Co, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S, B and Bi,
[0040] 1.0≤g≤1.5, 0≤h≤0.5, 0.4≤i≤0.9, 0≤j≤0.1,
[0041] [Chemical Formula 4]
[0042] LiFe 1-k M 4 k PO4
[0043] In the above chemical formula 4,
[0044] M 4 is at least one selected from the group consisting of Mn, Co, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Te, Ir, Gd, Sm, Sb, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi,
[0045] 0≤k<1.
[0046] (3) The present invention provides a method for producing a positive electrode slurry composition, wherein, in the above (1) or (2), the positive electrode active material includes two or more kinds selected from lithium composite transition metal compounds having a composition represented by the following chemical formulas 1 to 4.
[0047] [Chemical Formula 1]
[0048] Li a [Ni b Co c Mn d M 1 1-(b+c+d) ]O2
[0049] In the above chemical formula 1,
[0050] M 1 is at least one selected from the group consisting of Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi,
[0051] 0.9≤a≤1.1, 0 <b<1, 0<c<1, 0<d<1, 0<b+c+d≤1이고,
[0052] [Chemical Formula 2]
[0053] Li e Ni 1-f M 2 f O2
[0054] In the above chemical formula 2,
[0055] M 2 is at least one selected from the group consisting of Mn, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi,
[0056] 0.9≤e≤1.1, 0≤f<1,
[0057] [Chemical Formula 3]
[0058] Li g Ni h Mn i M 3 j O2
[0059] In the above chemical formula 3,
[0060] M 3 is at least one selected from the group consisting of Co, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S, B and Bi,
[0061] 1.0≤g≤1.5, 0≤h≤0.5, 0.4≤i≤0.9, 0≤j≤0.1,
[0062] [Chemical Formula 4]
[0063] LiFe 1-k M 4 k PO4
[0064] In the above chemical formula 4,
[0065] M 4 is at least one selected from the group consisting of Mn, Co, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Te, Ir, Gd, Sm, Sb, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi,
[0066] 0≤k<1.
[0067] (4) The present invention provides a method for producing a positive electrode slurry composition, wherein the positive electrode active material comprises a lithium composite transition metal compound having a composition represented by the following chemical formula 5, in any one of the above (1) to (3).
[0068] [Chemical Formula 5]
[0069] Li a [Ni b' Co c' Mn d' M 5 1-(b'+c'+d')]O2
[0070] M 5 is at least one selected from the group consisting of Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi,
[0071] 0.9≤a'≤1.1, 0.6≤b'<1, 0 <c'<0.4, 0<d'<0.4, 0<b'+c'+d'≤1이다.
[0072] (5) The present invention provides a method for producing a positive electrode slurry composition, wherein, in any one of the above (1) to (4), the mixing is performed so that the positive electrode active material is 85 parts by weight or more and 99 parts by weight or less, the conductive material is 0.5 parts by weight or more and 10 parts by weight or less, and the binder is 0.5 parts by weight or more and 10 parts by weight or less, based on 100 parts by weight of solid content.
[0073] (6) The present invention provides a method for producing a positive electrode slurry composition, wherein the solid content is 70 wt% or more and 85 wt% or less in any one of the above (1) to (5).
[0074] (7) The present invention is one of (1) to (6), V 24 Provided is a method for manufacturing a cathode slurry composition having a content of -5% or more and 30% or less.
[0075] (8) The present invention is one of (1) to (7), V 168 Provided is a method for manufacturing a cathode slurry composition having a content of 0% or more and 80% or less.
[0076] (9) The present invention is one of the above (1) to (8), wherein the V 336 Provided is a method for manufacturing a cathode slurry composition having a content of 1% or more and 120% or less.
[0077] (10) The present invention provides a method for producing a positive electrode slurry composition, wherein the mixture, the positive electrode slurry composition precursor, and the positive electrode slurry composition, in any one of the above (1) to (9), each independently have a viscosity of 20,000 cP or less.
[0078] (11) In any one of the above (1) to (10), the mixing is performed at a temperature of 0°C or more and 15°C or less, and the V 72 Provided is a method for manufacturing a cathode slurry composition having a content of 8% or more and 35% or less.
[0079] (12) In any one of the above (1) to (11), the cooling is performed at a temperature of -30°C or higher and less than 0°C, and the V 72 Provided is a method for producing a cathode slurry composition having a content of 0% or more and 20% or less.
[0080] (13) The present invention provides a method for manufacturing a positive electrode, comprising the steps of: manufacturing a positive electrode slurry composition according to any one of (1) to (12); and (B) applying and drying the positive electrode slurry composition on a current collector to form a positive electrode active material layer.
[0081] (14) The present invention provides a method for manufacturing a positive electrode, which further includes, in the above (13), a step (A1) of transferring the positive electrode slurry composition to a means for applying a positive electrode active material composition immediately before the step (B); and the transfer is performed at a temperature of -30°C or higher and 15°C or lower.
[0082]
[0083] The method for manufacturing a positive electrode slurry composition according to the present invention includes the steps of mixing a positive electrode active material, a conductive material, and a binder in a non-aqueous solvent to manufacture a mixture having a solid content exceeding 60 wt%; and the step of cooling the mixture to a temperature of -30°C or higher and 15°C or lower to manufacture a positive electrode slurry composition precursor; thereby, the viscosity of a positive electrode slurry composition having a high solid content is improved, and accordingly, problems in the positive electrode manufacturing process are improved.
[0084]
[0085] Hereinafter, the present invention will be described in more detail to help understand the present invention.
[0086] Terms or words used in this specification and claims should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical idea of the present invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best way.
[0087]
[0088] In this specification, it should be understood that terms such as “include,” “have,” or “have” are intended to specify the presence of a feature, number, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0089]
[0090] In this specification, the content of each element in the lithium complex transition metal compound may be measured through ICP (Inductive Coupled Plasma) analysis using an inductively coupled plasma optical emission spectrometer (ICP-OES; PerkinElmer, Optima 8000DV).
[0091]
[0092] Method for producing a cathode slurry composition
[0093]
[0094] Hereinafter, a method for manufacturing a positive electrode slurry composition according to the present invention will be described.
[0095]
[0096] The method for manufacturing the positive electrode slurry composition of the present invention comprises the step of preparing the positive electrode slurry composition and then storing it at a certain temperature range to suppress the occurrence of gelation of the positive electrode slurry composition.
[0097] Specifically, the method for manufacturing a positive electrode slurry composition according to the present invention comprises the steps of (S1) mixing a positive electrode active material, a conductive material, and a binder in a non-aqueous solvent to manufacture a mixture having a solid content of more than 60 wt%; (S2) cooling the mixture to a temperature of -30°C or higher and 15°C or lower to manufacture a positive electrode slurry composition precursor; and (S3) maintaining the temperature of the positive electrode slurry composition precursor to V 72 A step of preparing a positive electrode slurry composition having 0% or more and 50% or less of V; comprising: n is the viscosity increase rate when the temperature of the positive electrode slurry composition precursor is maintained for n hours, and the viscosity increase rate is expressed by the following mathematical formula 1.
[0098] [Mathematical Formula 1]
[0099] Viscosity increase rate (Vn[%]) = (VS2[cP] - VS1[cP] X 100 / VS1[cP])
[0100] In the above mathematical expression 1, VS1 is the viscosity [cP] of the mixture, and VS2 is the viscosity [cP] of the positive electrode slurry composition.
[0101]
[0102] When the solid content of the positive electrode slurry composition is 60 wt% or less, there is a problem of low energy density of the manufactured positive electrode.
[0103] Meanwhile, a positive electrode slurry composition prepared by mixing a positive electrode active material, a conductive agent, and a binder in a non-aqueous solvent may undergo gelation due to the -OH groups of the components included in the positive electrode slurry composition and the moisture that may be included therein, thereby increasing the viscosity of the positive electrode slurry. When the solid content of the positive electrode slurry exceeds about 60 wt%, the viscosity of the positive electrode slurry increases, and the viscosity of the positive electrode slurry increases rapidly over time after manufacture. When the viscosity of the positive electrode slurry increases and exceeds a certain viscosity, there is a problem in forming a uniform positive electrode layer when applying the positive electrode slurry to a substrate. In order to form a uniform positive electrode layer, it is preferable to use the positive electrode slurry immediately after manufacture. However, in a commercial positive electrode manufacturing process, the positive electrode slurry may need to be stored for a certain period of time after manufacture, and therefore, there is a need to suppress the increase in viscosity while storing the positive electrode slurry.
[0104] The present inventors have repeatedly studied and found that when the process of preparing a positive electrode slurry composition includes a step of preparing a positive electrode slurry composition precursor by cooling the composition to a temperature of -30°C or higher and 15°C or lower; and a step of maintaining the temperature of the positive electrode slurry composition precursor, the increase in viscosity of the positive electrode slurry composition over time can be suppressed. In addition, the present inventors have found that even when the solid content of the positive electrode slurry composition is high, the increase in viscosity of the positive electrode slurry composition over time can be suppressed, and thus the effect of further increasing the solid content in the positive electrode slurry composition can be exhibited, thereby completing the present invention.
[0105]
[0106] The positive electrode slurry composition according to the present invention described above can be manufactured by appropriately controlling the type of positive electrode active material, the type of conductive material, the type of binder, the type of non-aqueous solvent, and the mixing ratio of the above solutions.
[0107]
[0108] Hereinafter, each step of the present invention will be described in detail.
[0109]
[0110] (S1) Step
[0111] A method for producing a positive electrode slurry composition includes a step (S1) of mixing a positive electrode active material, a conductive agent, and a binder in a non-aqueous solvent to produce a mixture having a solid content of more than 60 wt%. Specifically, the solid content may be more than 60 wt%, 65 wt% or more, or 70 wt% or more, and may be 75 wt% or less, 80 wt% or less, 85 wt% or less, 90 wt% or less, 95 wt% or less, or less than 100 wt%. When the solid content is 60 wt% or less, the viscosity of the positive electrode slurry composition does not increase over time during the production of the positive electrode slurry composition, but there is a problem that the energy density of the produced positive electrode is low. The energy density of a positive electrode manufactured by controlling the solid content to exceed 60 wt% can be improved, and in particular, when the solid content is 70 wt% or more and 85 wt% or less, a positive electrode active material having excellent energy density and improved porosity can be manufactured by controlling the viscosity increase rate.
[0112]
[0113] According to one embodiment of the present invention, the positive electrode active material may include at least one selected from lithium composite transition metal compounds having a composition represented by the following chemical formulas 1 to 4.
[0114] [Chemical Formula 1]
[0115] Li a [Ni b Co c Mn d M 1 1-(b+c+d) ]O2
[0116] In the above chemical formula 1,
[0117] M 1is at least one selected from the group consisting of Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi,
[0118] 0.9≤a≤1.1, 0 <b<1, 0<c<1, 0<d<1, 0<b+c+d≤1이고,
[0119] [Chemical Formula 2]
[0120] Li e Ni 1-f M 2 f O2
[0121] In the above chemical formula 2,
[0122] M 2 is at least one selected from the group consisting of Mn, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi,
[0123] 0.9≤e≤1.1, 0≤f<1,
[0124] [Chemical Formula 3]
[0125] Li g Ni h Mn i M 3 j O2
[0126] In the above chemical formula 3,
[0127] M 3 is at least one selected from the group consisting of Co, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S, B and Bi,
[0128] 1.0≤g≤1.5, 0≤h≤0.5, 0.4≤i≤0.9, 0≤j≤0.1,
[0129] [Chemical Formula 4]
[0130] LiFe 1-k M 4 k PO4
[0131] In the above chemical formula 4,
[0132] M 4 is at least one selected from the group consisting of Mn, Co, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Te, Ir, Gd, Sm, Sb, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi,
[0133] 0≤k<1.
[0134] In the above chemical formula 1,
[0135] Above M 1 is a doping element, specifically, the above M 1 is at least one selected from the group consisting of Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi. The above M 1 Although not essential, it can improve capacity characteristics and life characteristics.
[0136] The above a may be 0.9 or greater, or 1.0 or greater, and 1.1 or less. When a satisfies the above range, high safety and high energy density per unit volume can be achieved.
[0137] The above b is the molar ratio of nickel (Ni) among all metals excluding lithium in the lithium complex transition metal compound, and may be greater than 0, 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or more, 0.8 or more, or 0.9 or more, and may be 0.97 or less, 0.98 or less, 0.99 or less, or less than 1. When b satisfies the above range, high-energy characteristics can be implemented.
[0138] The above c is the molar ratio of cobalt (Co) among all metals excluding lithium in the lithium complex transition metal compound, and may be greater than 0, 0.01 or more, or 0.02 or more, and may be 0.03 or less, 0.04 or less, 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, 0.1 or less, 0.11 or less, 0.12 or less, 0.13 or less, 0.14 or less, 0.15 or less, 0.16 or less, 0.17 or less, 0.18 or less, 0.19 or less, 0.2 or less, 0.21 or less, 0.22 or less, 0.23 or less, 0.24 or less, 0.25 or less, 0.26 or less, 0.27 or less, 0.28 or less, 0.29 or less, 0.3 or less, It may be 0.31 or less, 0.32 or less, 0.33 or less, 0.34 or less, 0.35 or less, 0.36 or less, 0.37 or less, 0.38 or less, 0.39 or less, 0.4 or less, 0.41 or less, 0.42 or less, 0.43 or less, 0.44 or less, 0.45 or less, 0.46 or less, 0.47 or less, 0.48 or less, 0.49 or less, 0.5 or less, 0.6 or less, 0.7 or less, 0.8 or less, 0.9 or less, or less than 1. When c satisfies the above range, stability can be improved during the charge and discharge process, and rate characteristics can be enhanced.
[0139] The above d is the molar ratio of manganese (Mn) among all metals excluding lithium in the lithium complex transition metal compound, and may be greater than 0, 0.01 or more, or 0.02 or more, and may be 0.03 or less, 0.04 or less, 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, 0.1 or less, 0.11 or less, 0.12 or less, 0.13 or less, 0.14 or less, 0.15 or less, 0.16 or less, 0.17 or less, 0.18 or less, 0.19 or less, 0.2 or less, 0.21 or less, 0.22 or less, 0.23 or less, 0.24 or less, 0.25 or less, 0.26 or less, 0.27 or less, 0.28 or less, 0.29 or less, 0.3 or less, 0.31 or less, 0.32 or less, 0.33 or less, 0.34 or less, 0.35 or less, 0.36 or less, 0.37 or less, 0.38 or less, 0.39 or less, 0.4 or less, 0.41 or less, 0.42 or less, 0.43 or less, 0.44 or less, 0.45 or less, 0.46 or less, 0.47 or less, 0.48 or less, 0.49 or less, 0.5 or less, 0.6 or less, 0.7 or less, 0.8 or less, 0.9 or less, or less than 1. When d satisfies the above range, high temperature stability can be increased, and side reactions with the electrolyte can be relatively reduced.
[0140] The above 1-b+c+d is M among all metals except lithium in the lithium complex transition metal compound. 1 is the molar ratio. The above b+c+d may be greater than 0, 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or more, 0.8 or more, or 0.9 or more, and may be 0.97 or less, 0.98 or less, 0.99 or less, or 1 or less. When the above b+c+d satisfies the above range, the stability of the crystal structure of the positive electrode active material may be improved and the particle shape may be improved.
[0141] In the above chemical formula 2,
[0142] Above M 2is a doping element, specifically the above M 2 is at least one selected from the group consisting of Mn, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi. The M 2 Although not necessarily included, it can improve capacity characteristics and life characteristics.
[0143] The above e may be 0.9 or greater, or 1.0 or greater, and 1.1 or less. When e satisfies the above range, high safety and high energy density per unit volume can be achieved.
[0144] The above 1-f is the molar ratio of nickel (Ni) among all metals excluding lithium in the lithium composite transition metal compound. The above f is the molar ratio of M among all metals excluding lithium in the lithium composite transition metal compound. 2 The molar ratio of f may be 0 or more, or 0.01 or more, and may be 0.1 or less, 0.2 or less, 0.3 or less, 0.4 or less, 0.5 or less, 0.6 or less, 0.7 or less, 0.8 or less, 0.9 or less, or less than 1. When f satisfies the above range, the stability of the crystal structure of the positive electrode active material may be improved and the particle shape may be improved.
[0145] In the above chemical formula 3,
[0146] Above M 3 is a doping element, specifically the above M 3 is at least one selected from the group consisting of Mn, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi. The M 3Although not essential, it can improve capacity characteristics and life characteristics.
[0147] The above g may be 1.0 or more, 1.1 or more, or 1.2 or more, and may be 1.3 or less, 1.4 or less, or 1.5 or less. When g satisfies the above range, high safety and high energy density per unit volume can be achieved.
[0148] The above h is the molar ratio of nickel (Ni) among all metals excluding lithium in the lithium complex transition metal compound, and may be 0 or more, 0.1 or more, or 0.2 or more, and may be 0.3 or less, 0.4 or less, or 0.5 or less. When h satisfies the above range, high-energy characteristics can be realized.
[0149] The above i is the molar ratio of manganese (Mn) among all metals excluding lithium in the lithium complex transition metal compound, and may be 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or less, 0.8 or less, or 0.9 or less. When i satisfies the above range, high-temperature stability may increase, and side reactions with the electrolyte may be relatively reduced.
[0150] The above j is M among all metals except lithium in the lithium complex transition metal compound. 3 The molar ratio of j may be 0 or more, or 0.01 or more, and may be 0.1 or less, 0.2 or less, 0.3 or less, 0.4 or less, 0.5 or less, 0.6 or less, 0.7 or less, 0.8 or less, 0.9 or less, or less than 1. When j satisfies the above range, the stability of the crystal structure of the positive electrode active material may be improved and the particle shape may be improved.
[0151] The above g, h, i, j may be g+h+i+j=2.
[0152] In the above chemical formula 4,
[0153] Above M 4 is a doping element, specifically the above M 4is at least one selected from the group consisting of Mn, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi. The M 4 Although not necessarily included, it can improve capacity characteristics and life characteristics.
[0154] The above 1-k is the molar ratio of Fe among all metals excluding lithium in the lithium iron phosphate compound. The above k is the molar ratio of M among all metals excluding lithium in the lithium iron phosphate compound. 4 The molar ratio of k may be 0 or more, 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, or 0.5 or more, and may be 0.6 or less, 0.7 or less, 0.8 or less, 0.9 or less, or less than 1. When k is within the above range, the particle shape of the positive electrode active material may be improved, the stability of the crystal structure may be improved, and the electrical conductivity may be improved, thereby improving the capacity characteristics.
[0155]
[0156] According to one embodiment of the present invention, the lithium composite transition metal compound having a composition represented by the chemical formula 3 may be a lithium composite transition metal compound having a composition represented by the following chemical formula 3-1.
[0157] [Chemical Formula 3-1]
[0158] m(Li n Ni o Mn p M 3 q O2)·(1-m)(Li2MnO3)
[0159] In the above chemical formula 3-1,
[0160] M 3is at least one selected from the group consisting of Co, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Mg, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Nb, Cu, In, S, B and Bi,
[0161] 0 <m<1, 0.9≤n≤1.1, 0≤o<1, 0<p≤1, 0≤q≤0.1이다.
[0162] The compound represented by the above chemical formula 3-1 may be a compound that simultaneously includes a phase having a crystal structure of the R3-m space group (rhombohedra) and a phase having a crystal structure of the C2 / m space group (monoclinic).
[0163] Above M 3 is a doping element, specifically the above M 3 is at least one selected from the group consisting of Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi. The above M 3 Although not essential, it can improve capacity characteristics and life characteristics.
[0164] The above m refers to the molar ratio of a phase having a crystal structure of the R3-m space group (rhombohedra) in a lithium complex transition metal compound, and may be greater than 0, 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, or 0.7 or more, and may be 0.8 or less, 0.9 or less, or less than 1. When m satisfies the above range, high-capacity characteristics and high energy density per unit volume can be realized. The above 1-m may refer to the molar ratio of a phase having a crystal structure of the C2 / m space group (monoclinic).
[0165] The above n is a molar ratio of lithium (Li) in a phase having a crystal structure of the R3-m space group (rhombohedra), and may be 0.9 or more, 0.95 or more, or 1.0 or more, and may be 1.03 or less, 1.05 or less, 1.07 or less, or 1.1 or less.
[0166] The above o is a molar ratio of nickel (Ni) in a phase having a crystal structure of the R3-m space group (rhombohedra), and may be 0 or more, 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, or 0.5 or more, and may be 0.6 or less, 0.7 or less, 0.8 or less, 0.9 or less, or less than 1. When o satisfies the above range, a high energy density is exhibited, and a high capacity characteristic can be realized.
[0167] The above p is a molar ratio of manganese (Mn) in a phase having a crystal structure of the R3-m space group (rhombohedra), and may be greater than 0, 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, or 0.5 or more, and may be 0.6 or less, 0.7 or less, 0.8 or less, 0.9 or less, or 1 or less. When p satisfies the above range, a high energy density is exhibited, and a high capacity characteristic can be realized.
[0168] The above q is a phase having a crystal structure of the R3-m space group (rhombohedra). 3 The molar ratio of q may be 0 or more, 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, or 0.05 or more, and may be 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, or 0.1 or less. When q satisfies the above range, the stability of the crystal structure of the positive electrode active material may be improved and the particle shape may be improved.
[0169]
[0170] According to one embodiment of the present invention, the positive electrode active material may include two or more selected from lithium composite transition metal compounds having a composition represented by Chemical Formulas 1 to 4. In this case, capacity characteristics, life characteristics, rate characteristics, etc. can be improved compared to a case where only one lithium composite transition metal compound is included.
[0171]
[0172] According to one embodiment of the present invention, the positive electrode active material may include a lithium composite transition metal compound having a composition represented by the following chemical formula 5.
[0173] [Chemical Formula 5]
[0174] Li a [Ni b' Co c' Mn d' M 5 1-(b'+c'+d')]O2
[0175] M 5 is at least one selected from the group consisting of Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi,
[0176] 0.9≤a'≤1.1, 0.6≤b'<1, 0 <c'<0.4, 0<d'<0.4, 0<b'+c'+d'≤1이다.
[0177] In the above chemical formula 5,
[0178] Above M 5 is a doping element, specifically, the above M 5 is at least one selected from the group consisting of Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi. The above M 5 Although not necessarily included, it can improve capacity characteristics and life characteristics.
[0179] The above a' may be 0.9 or greater, or 1.0 or greater, and 1.1 or less. When a' satisfies the above range, high safety and high energy density per unit volume can be achieved.
[0180] The above b' is the molar ratio of nickel (Ni) among all metals excluding lithium in the lithium complex transition metal compound, and may be 0.6 or more, 0.7 or more, 0.8 or more, or 0.9 or more, and may be 0.97 or less, 0.98 or less, 0.99 or less, or less than 1. When b' satisfies the above range, high-energy characteristics can be implemented.
[0181] The above c' is the molar ratio of cobalt (Co) among all metals excluding lithium in the lithium complex transition metal compound, and may be greater than 0, 0.01 or more, or 0.02 or more, and may be 0.03 or less, 0.04 or less, 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, 0.1 or less, 0.11 or less, 0.12 or less, 0.13 or less, 0.14 or less, 0.15 or less, 0.16 or less, 0.17 or less, 0.18 or less, 0.19 or less, 0.2 or less, 0.21 or less, 0.22 or less, 0.23 or less, 0.24 or less, 0.25 or less, 0.26 or less, 0.27 or less, 0.28 or less, 0.29 or less, 0.3 c' may be less than, 0.31 or less, 0.32 or less, 0.33 or less, 0.34 or less, 0.35 or less, 0.36 or less, 0.37 or less, 0.38 or less, 0.39 or less, or less than 0.4. When c' satisfies the above range, stability can be improved and rate characteristics can be enhanced during the charge and discharge process.
[0182] The above d' is the molar ratio of manganese (Mn) among all metals excluding lithium in the lithium complex transition metal compound, and may be greater than 0, 0.01 or more, or 0.02 or more, and may be 0.03 or less, 0.04 or less, 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, 0.1 or less, 0.11 or less, 0.12 or less, 0.13 or less, 0.14 or less, 0.15 or less, 0.16 or less, 0.17 or less, 0.18 or less, 0.19 or less, 0.2 or less, 0.21 or less, 0.22 or less, 0.23 or less, 0.24 or less, 0.25 or less, 0.26 or less, 0.27 or less, 0.28 or less, 0.29 or less, 0.3 or less, 0.31 or less, 0.32 or less, 0.33 or less, 0.34 or less, 0.35 or less, 0.36 or less, 0.37 or less, 0.38 or less, 0.39 or less, or less than 0.4. When d' satisfies the above range, high temperature stability can be increased, and side reactions with the electrolyte can be relatively reduced.
[0183] The above 1-b'+c'+d' is M among all metals except lithium in the lithium complex transition metal compound. 5 is the molar ratio. The above b'+c'+d' may be greater than 0, 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or more, 0.8 or more, or 0.9 or more, and may be 0.97 or less, 0.98 or less, 0.99 or less, or 1 or less. When the above b'+c'+d' satisfies the above range, the stability of the crystal structure of the positive electrode active material may be improved and the particle shape may be improved.
[0184] Among the positive electrode active materials, lithium composite transition metal oxides (hereinafter referred to as nickel-rich lithium composite transition metal oxides) in which the nickel content is 60 mol% or more out of the total metals excluding lithium, have a relatively large amount of lithium byproducts remaining on the surface of the lithium composite transition metal oxide during the manufacturing process. Since the impurities are converted to LiOH and Li2CO3, viscosity increase and gelation phenomena may occur more prominently in the positive electrode slurry composition using the nickel-rich lithium composite transition metal oxide as the positive electrode active material. Therefore, in the case of the positive electrode slurry composition using the nickel-rich lithium composite transition metal oxide, if stored at ambient temperature without separate measures, there is a problem that the viscosity increases rapidly over time, and the viscosity increases even more rapidly as the temperature increases. Therefore, the present invention can be more effectively applied to the manufacture of a positive electrode slurry composition including a nickel-rich lithium composite transition metal oxide, which has a high risk of viscosity increase and gelation in the positive electrode slurry.
[0185]
[0186] Meanwhile, the positive electrode active material may optionally further include a coating layer comprising one or more elements (hereinafter referred to as “coating elements”) selected from the group consisting of Al, Ti, W, B, F, P, Mg, Ni, Co, Fe, Cr, V, Cu, Ca, Zn, Zr, Nb, Mo, Sr, Sb, Bi, Si, Y, and S, as needed, on the surface of the positive electrode active material. When such a coating layer is included, contact between the positive electrode active material and the electrolyte is blocked, so that gas generation and transition metal elution due to side reactions with the electrolyte can be effectively suppressed.
[0187] The above coating layer can be formed by mixing a positive electrode active material and a raw material including the coating element, and then heat-treating the mixture at a temperature of 200°C to 800°C.
[0188]
[0189] The above conductive material is used to provide conductivity to the electrode, and in the battery to be formed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One of these may be used alone or a mixture of two or more may be used.
[0190]
[0191] The above binder serves to improve adhesion between positive electrode active material particles and adhesion between the positive electrode active material and the current collector. Specific examples thereof include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluoroelastomer, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof.
[0192]
[0193] The above non-aqueous solvent may be a non-aqueous solvent commonly used in the relevant technical field, and may be at least one selected from the group consisting of dimethyl sulfoxide (DMSO), dimethyl formamide (DMF), isopropyl alcohol, dimethylacetamide, N-methylpyrrolidone (NMP), and acetone.
[0194] The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, taking into account the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied for subsequent positive electrode manufacturing.
[0195] The above mixture may optionally contain additives as needed.
[0196]
[0197] According to one embodiment of the present invention, the mixing may be performed so that the positive electrode active material is 85 parts by weight or more and 99 parts by weight or less, the conductive material is 0.5 parts by weight or more and 10 parts by weight or less, and the binder is 0.5 parts by weight or more and 10 parts by weight or less, based on 100 parts by weight of solid content. Specifically, the mixing may be, based on 100 parts by weight of solid content, the positive electrode active material may be 85 parts by weight or more, 86 parts by weight or more, 87 parts by weight or more, 88 parts by weight or more, 89 parts by weight or more, or 90 parts by weight or more, 91 parts by weight or less, 92 parts by weight or less, 93 parts by weight or less, 94 parts by weight or less, 95 parts by weight or less, 96 parts by weight or less, 97 parts by weight or less, 98 parts by weight or less, or 99 parts by weight or less, and the conductive material may be 0.5 parts by weight or more, 0.6 parts by weight or more, 0.7 parts by weight or more, 0.8 parts by weight or more, 0.9 parts by weight or more, 1 part by weight or more, 2 parts by weight or more, or 3 parts by weight or more, 4 parts by weight or less, 5 parts by weight or less, 6 parts by weight or less, 7 parts by weight or less, 8 parts by weight or less, 9 parts by weight or less, or 10 parts by weight or less. And, the binder may be 0.5 parts by weight or more, 0.6 parts by weight or more, 0.7 parts by weight or more, 0.8 parts by weight or more, 0.9 parts by weight or more, 1 part by weight or more, 2 parts by weight or more, or 3 parts by weight or more, 4 parts by weight or less, 5 parts by weight or less, 6 parts by weight or less, 7 parts by weight or less, 8 parts by weight or less, 9 parts by weight or less, or 10 parts by weight or less. In this case, a positive electrode slurry composition having a high solid content can be effectively manufactured.
[0198]
[0199] The step of preparing the above mixture can be typically performed by a method of mixing a positive electrode active material, a conductive material, and a binder in a non-aqueous solvent. At this time, the mixing can be performed at a temperature of -30°C or higher and 75°C or lower, and specifically, -30°C or higher, -20°C or higher, or -10°C or higher, and 55°C or lower, 60°C or lower, 65°C or lower, 70°C or lower, or 75°C or lower. When the mixing is performed within the above temperature range, the effect of minimizing gelation of the mixture during mixing can be expected. In particular, when the mixing is performed at a temperature of 0°C or higher and 15°C or lower, the mixture prepared by the mixing can be more effective in maintaining low viscosity. The temperature during mixing and the temperature of the mixture can be the same.
[0200]
[0201] (S2) Step
[0202]
[0203] After step (S1), step (S2) is included to manufacture a positive electrode slurry composition precursor by cooling the mixture to a temperature of -30°C or higher and 15°C or lower.
[0204] Specifically, the mixture is cooled to -30°C or higher, and -23°C or lower, -20°C or lower, -10°C or lower, 0°C or lower, 10°C or lower, or 15°C or lower to prepare a positive electrode slurry composition precursor. When the mixture is cooled within the above temperature range, gelation or viscosity increase of the positive electrode slurry composition can be suppressed. Accordingly, even after the positive electrode slurry composition is prepared, the positive electrode slurry composition can maintain an appropriate viscosity for forming a positive electrode layer even after a period of time. In particular, when the cooling is performed at a temperature of -30°C or higher and lower than 0°C, the viscosity can be maintained low even if the solid content is high, thereby forming a uniform positive electrode layer. When the above mixture is cooled to below -30°C, there is a problem of poor manufacturing efficiency due to excessive energy required for cooling, and when the mixture is cooled to above 15°C or no cooling is performed, gelation or viscosity increase of the positive electrode slurry composition is not suppressed, so there is a problem of viscosity increasing exponentially over time.
[0205]
[0206] (S3) Step
[0207] (S2) After step, the temperature of the positive electrode slurry composition precursor is maintained at V 72 It includes a step (S3) of preparing a positive electrode slurry composition having a content of 0% or more and 50% or less.
[0208]
[0209] In the present invention, the viscosity increase rate (V n [%]) was evaluated and expressed as a parameter represented by the following mathematical formula 1. The viscosity increase rate referred to in the present invention is a value that is controlled according to the viscosity of the positive electrode slurry composition (VS2[cP]) and the viscosity of the mixture (VS1[cP]), and the closer the viscosity of the positive electrode slurry composition is to the viscosity of the mixture, the lower the viscosity increase rate appears.
[0210] [Mathematical Formula 1]
[0211] Viscosity increase rate (Vn[%]) = (VS2[cP] - VS1[cP] X 100 / VS1[cP])
[0212] In the above mathematical expression 1, VS1 is the viscosity [cP] of the mixture, and VS2 is the viscosity [cP] of the positive electrode slurry composition.
[0213] For example, if the viscosity of the positive electrode slurry composition and the viscosity of the mixture are the same, the viscosity increase rate is 0, and when the positive electrode active material, conductive material, and binder are mixed in a non-aqueous solvent to prepare a mixture, the viscosity of the mixture is measured, and then the viscosity of the positive electrode slurry composition prepared therefrom is measured, the viscosity does not increase.
[0214]
[0215] According to the present invention, by maintaining the temperature of the positive electrode slurry composition precursor, specifically, V 72 A cathode slurry composition is prepared in which the V may be 0% or more, 1% or more, 2% or more, 3% or more, 4% or more, 5% or more, 6% or more, 7% or more, or 8% or more, and 20% or less, 25% or less, 30% or less, 35% or less, 40% or less, 45% or less, or 50% or less. 72 When the above range is within the above range, the viscosity increase of the positive electrode slurry composition over time is suppressed, so that the positive electrode slurry composition can be used to form a positive electrode layer without having to use it immediately after manufacturing, and thus the manufactured positive electrode slurry composition can be stored for a certain period of time. Therefore, since there is no need to use the positive electrode slurry composition for manufacturing the positive electrode immediately after manufacturing, flexibility can be provided in the design of the positive electrode manufacturing process. On the other hand, the above V 72 When the content exceeds 50%, there is a problem in that it is difficult to manufacture a cathode with the cathode slurry composition stored for a certain period of time or longer due to the increase in viscosity of the cathode slurry composition over time.
[0216]
[0217] According to one embodiment of the present invention, the mixing in step (S1) is performed at a temperature of 0°C or more and 15°C or less, and the V 72 may be 8% or more and 35% or less, and the cooling of step (S2) is performed at a temperature of -30℃ or more and less than 0℃, and the V 72 It can be between 0% and 20%.
[0218]
[0219] According to one embodiment of the present invention, V 24 may be -5% or more and 30% or less. Specifically, the V 24 may be -5% or more, -4% or more, -3% or more, -2% or more, or -1% or more, and may be 20% or less, 25% or less, or 30% or less. The above V 24 When the viscosity is within the above range, the increase in viscosity of the positive electrode slurry composition over time is suppressed, so that the positive electrode slurry composition can exhibit an appropriate viscosity for use in forming a positive electrode layer even without being used immediately after production, and thus the produced positive electrode slurry composition can be stored for a certain period of time.
[0220]
[0221] According to one embodiment of the present invention, V 168 may be 0% or more and 80% or less. Specifically, the V 168 The V may be 0% or more, 1% or more, 2% or more, or 3% or more, and may be 55% or less, 60% or less, 65% or less, 70% or less, 75% or less, or 80% or less. 168 Within this range, the increase in viscosity of the positive electrode slurry composition over time is suppressed, so that the positive electrode slurry composition can exhibit an appropriate viscosity for use in forming a positive electrode layer even without being used immediately after production, and thus the effect of being able to store the produced positive electrode slurry composition for a certain period of time can be exhibited.
[0222]
[0223] According to one embodiment of the present invention, V 336 It may be 1% or more and 120% or less. Specifically, the above V 336 The V may be 1% or more, 2% or more, or 3% or more, and may be 75% or less, 80% or less, 85% or less, 90% or less, 95% or less, 100% or less, 105% or less, 110% or less, 115% or less, or 120% or less. 336 Within this range, the increase in viscosity of the positive electrode slurry composition over time is suppressed, so that the positive electrode slurry composition can exhibit an appropriate viscosity for use in forming a positive electrode layer even without being used immediately after production, and thus the effect of being able to store the produced positive electrode slurry composition for a certain period of time can be exhibited.
[0224]
[0225] According to one embodiment of the present invention, the mixture, the positive electrode slurry composition precursor, and the positive electrode slurry composition may each independently have a viscosity of 20,000 cP or less. Specifically, the mixture, the positive electrode slurry composition precursor, and the positive electrode slurry composition may each independently have a viscosity of 0 cP or more, or 3,000 cP or more, and may be 9,000 cP or less, 10,000 cP or less, 11,000 cP or less, 12,000 cP or less, 13,000 cP or less, 14,000 cP or less, 15,000 cP or less, 16,000 cP or less, 17,000 cP or less, 18,000 cP or less, 19,000 cP or less, or 20,000 cP or less. When the viscosity is within the above range, the viscosity can be maintained low when preparing the positive electrode slurry composition, and the positive electrode slurry composition can have a viscosity suitable for use in forming a positive electrode layer.
[0226]
[0227] Method for manufacturing anode
[0228] In addition, the present invention provides a method for manufacturing a positive electrode.
[0229]
[0230] The method for manufacturing the positive electrode of the present invention may include a step of manufacturing the positive electrode using the positive electrode slurry composition manufactured by the method for manufacturing the positive electrode slurry composition described above.
[0231] Specifically, the method for manufacturing the positive electrode of the present invention may include (A) a step of manufacturing a positive electrode slurry composition according to the method for manufacturing the positive electrode slurry composition; and (B) a step of applying and drying the positive electrode slurry composition on a current collector to form a positive electrode layer.
[0232]
[0233] Accordingly, the method for manufacturing the positive electrode according to the present invention may include a method for manufacturing the positive electrode slurry composition, and accordingly, processes such as steps (S1) and (S2) described in the method for manufacturing the positive electrode slurry composition described above may be performed.
[0234]
[0235] Hereinafter, each step of the present invention will be described in detail.
[0236]
[0237] (A) Step
[0238] It includes a step (A) of manufacturing a positive electrode slurry composition according to the above method for manufacturing a positive electrode slurry composition.
[0239] The step of preparing the positive electrode slurry composition includes a process of preparing the positive electrode slurry composition according to the above-described method for preparing the positive electrode slurry composition, and specifically, (S1) a step of mixing a positive electrode active material, a conductive material, and a binder in a non-aqueous solvent to prepare a mixture having a solid content of more than 60 wt%; (S2) a step of cooling the mixture to a temperature of -30°C or higher and 15°C or lower to prepare a positive electrode slurry composition precursor; and (S3) a step of maintaining the temperature of the positive electrode slurry composition precursor to V 72 A step of preparing a positive electrode slurry composition having 0% or more and 50% or less of V; comprising: n is the viscosity increase rate when the temperature of the positive electrode slurry composition precursor is maintained for n hours, and the viscosity increase rate may be expressed by the mathematical formula 1 described in the present specification.
[0240]
[0241] (B) Step
[0242] Thereafter, a step (B) of applying and drying the positive electrode slurry composition on a current collector to form a positive electrode layer may be included.
[0243] In the above step (B), the manufactured positive electrode slurry composition is applied and dried on a current collector to form a positive electrode layer.
[0244] The above step (B) can be performed according to a conventional method for manufacturing a cathode, except that the cathode slurry composition of the above step (A) is used.
[0245] For example, a positive electrode slurry composition manufactured according to a method for manufacturing a positive electrode slurry composition according to one embodiment of the present invention may be applied to one side of a positive electrode current collector or on a positive electrode, and then dried and rolled to form a positive electrode layer on the positive electrode current collector. The positive electrode layer may be formed to have a porosity of 10% to 30% by volume, specifically 15% to 30% by volume, and more specifically 18% to 27% by volume.
[0246] A method for manufacturing a positive electrode according to one embodiment of the present invention further includes a step (A1) of transferring the positive electrode slurry composition to a means for applying a positive electrode active material composition immediately before the step (B) for applying the positive electrode slurry composition in the step (B); wherein the transfer may be performed at a temperature of -30°C or higher and 15°C or lower. When the transfer is performed within the temperature range, an increase in the viscosity of the positive electrode slurry composition can be suppressed as much as possible, thereby forming a more uniform positive electrode layer.
[0247]
[0248] The positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 ㎛, and fine unevenness may be formed on the surface of the positive electrode current collector to increase the adhesive strength of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.
[0249]
[0250] Alternatively, the cathode slurry composition may be produced by, for example, casting the cathode slurry composition onto a separate support, peeling the resulting film from the support, and laminating the resulting film onto a cathode current collector.
[0251] In addition, an electrochemical device including the positive electrode can be manufactured using the positive electrode manufactured by the above-mentioned method for manufacturing the positive electrode. The electrochemical device can be specifically a battery, a capacitor, etc., and more specifically, a lithium secondary battery.
[0252] The method for manufacturing the positive electrode of the present invention may be a method for manufacturing a positive electrode for a lithium secondary battery, and the positive electrode manufactured through the manufacturing method may be used as a positive electrode for a lithium secondary battery.
[0253]
[0254] The lithium secondary battery specifically includes a positive electrode, a negative electrode positioned opposite the positive electrode, and a separator and an electrolyte interposed between the positive electrode and the negative electrode, and the positive electrode may be a positive electrode manufactured by the above-described positive electrode manufacturing method.
[0255] In addition, the lithium secondary battery may optionally further include a battery container that houses the electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.
[0256]
[0257] In the above lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.
[0258] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 ㎛ to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.
[0259]
[0260] The above negative electrode active material layer optionally includes a binder and a conductive material together with the negative electrode active material.
[0261] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; SiO β (0<β<2), SnO2, vanadium oxide, lithium vanadium oxide, and other metal oxides capable of doping and dedoping lithium; or composites containing the above metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include natural graphite or artificial graphite in the form of amorphous, plate-like, flaky, spherical, or fiber-like forms, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes.
[0262] The above negative electrode active material may be included in an amount of 80 to 99 parts by weight based on 100 parts by weight of the total weight of the negative electrode active material layer.
[0263]
[0264] The above binder is a component that assists in bonding between the conductive material, the active material, and the current collector, and is typically added in an amount of 0.1 to 10 parts by weight based on 100 parts by weight of the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.
[0265] The conductive agent is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10 parts by weight or less, preferably 5 parts by weight or less, based on 100 parts by weight of the total weight of the negative electrode active material layer. The conductive agent is not particularly limited as long as it has conductivity and does not cause a chemical change in the battery, and examples thereof include graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber or metal fiber; metal powders such as fluorocarbon, aluminum, and nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0266]
[0267] For example, the negative electrode active material layer can be manufactured by applying and drying a negative electrode composite prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material in a solvent, on a negative electrode current collector, or by casting the negative electrode composite on a separate support and then laminating the resulting film on a negative electrode current collector by peeling it off from the support.
[0268]
[0269] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used in lithium secondary batteries can be used without special restrictions, and in particular, one having low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength may be used, and may optionally be used in a single-layer or multi-layer structure.
[0270]
[0271] In addition, examples of the electrolyte used in the present invention include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.
[0272] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0273] As the organic solvent, any solvent that can serve as a medium through which ions involved in the electrochemical reaction of the battery can move may be used without particular limitation. Specifically, the organic solvent includes ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); Alcohol solvents such as ethyl alcohol, isopropyl alcohol, etc.; nitriles such as R-CN (R is a linear, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes, etc. can be used. Among these, carbonate solvents are preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferable.In this case, the performance of the electrolyte may be improved when the cyclic carbonate and the chain carbonate are mixed and used in a volume ratio of about 1:1 to about 1:9.
[0274]
[0275] The above lithium salt can be used without any special limitation as long as it is a compound that can provide lithium ions used in a lithium secondary battery. Specifically, the above lithium salt is LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2) 2. LiCl, LiI, or LiB(C2O4)2 can be used. It is recommended that the concentration of the lithium salt be within the range of 0.1 to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.
[0276]
[0277] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 to 5 parts by weight based on 100 parts by weight of the total weight of the electrolyte.
[0278]
[0279] As described above, a lithium secondary battery including a cathode material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and lifespan characteristics, and is therefore useful in portable devices such as mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0280] Accordingly, according to another embodiment of the present invention, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same are provided.
[0281] The above battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.
[0282] There is no particular limitation on the external shape of the lithium secondary battery of the present invention, but it may be a cylindrical shape using a can, a square shape, a pouch shape, or a coin shape.
[0283] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but can also be preferably used as a unit battery in a medium- to large-sized battery module including a plurality of battery cells.
[0284]
[0285] Hereinafter, the present invention will be described in detail with reference to examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention should not be construed as being limited to the examples described below. The examples of the present invention are provided to more fully explain the present invention to those of ordinary skill in the art.
[0286]
[0287] Manufacturing example
[0288] Manufacturing Example 1
[0289] A 2M transition metal solution was prepared by dissolving NiSO4, CoSO4, and MnSO4 in water in an amount such that the molar ratio of nickel:cobalt:manganese was 96:2:2.
[0290] A container containing the above transition metal-containing solution and, additionally, a 25 wt% NaOH solution and a 15 wt% NH4OH aqueous solution were each connected to a 200 L batch reactor set at 55°C.
[0291] Next, deionized water was added to the batch reactor, and nitrogen gas was purged to remove dissolved oxygen in the water, creating a non-oxidizing atmosphere within the reactor. Afterwards, NaOH was added, and stirring was performed at a stirring speed of 250 rpm, maintaining the pH within the co-precipitation reactor at 11.7.
[0292] Afterwards, the transition metal-containing solution was injected into the co-precipitation reactor at a rate of 250 mL / hr, NH4OH aqueous solution was injected at a rate of 40 m L / hr, and NaOH aqueous solution was injected at a rate such that the pH of the reaction solution could be maintained at 11.7. After 6 hours of reaction, stirring was stopped and the supernatant was removed to concentrate. This process was repeated 4 to 5 times to obtain the average particle diameter (D 50 ) were grown until the particles reached approximately 14 μm.
[0293] The transition metal oxide precursor particles thus manufactured were filtered through a filter press and dried at 130°C for 24 hours to obtain Ni. 0.96 Co 0.02 Mn 0.02A positive electrode active material precursor having a composition represented by (OH)2 was obtained. Subsequently, the positive electrode active material precursor and LiOH·H2O were mixed so that the molar ratio of (Ni+Co+Mn):Li was 1:1.06, and calcined at 775°C for 13.5 hours in an oxygen atmosphere, thereby obtaining LiNi 0.96 Co 0.02 Mn 0.02 With a composition represented by O2, the average particle size (D 50 ) was 14 ㎛, and a positive electrode active material (lithium transition metal oxide) in the form of secondary particles was manufactured.
[0294]
[0295] Manufacturing Example 2
[0296] Positive electrode active material precursor [Composition: Ni 0.96 Co 0.02 Mn 0.02 (OH)2, average particle size (D) 50 ) 4.5 ㎛] and LiOH were mixed so that the molar ratio of (Ni+Co+Mn):Li was 1:1.05, and the plastic product was manufactured by first firing at 850℃ for 9 hours under an oxygen atmosphere.
[0297] After disintegrating the above-mentioned plastic product, it was fired a second time at 750℃ for 9 hours under an oxygen atmosphere to obtain LiNi. 0.96 Co 0.02 Mn 0.02 With a composition represented by O2, the average particle size (D 50 ) was 14 ㎛, and a single particle type positive electrode active material (lithium transition metal oxide) was manufactured.
[0298]
[0299] Example 1
[0300] The positive electrode active material, carbon black (Denka, DenkaBlack), PVdF (Kureha, KF9709), and non-aqueous solvent (Daejung Chemicals, N-methylpyrrolidone (NMP)) manufactured in the above Manufacturing Example 1 were left in a chamber at 20°C for 6 hours so that each temperature became 20°C.
[0301] At room temperature, 200 g of the positive electrode active material, 3.43 g of carbon black as a conductive material, and 4.36 g of PVdF as a binder were dispersed and mixed in 80.8 g of a non-aqueous solvent (NMP) using a homo disper mixer (Homo Disper 2.5, PRIMIX) to prepare a mixture having a solid content of 72.0 wt%. During mixing, the temperature of the mixture increased due to the resistance of the mixer and the mixture, and the mixing temperature was maintained at 45°C.
[0302] The mixture was cooled to 0°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while being stored to prepare a positive electrode slurry composition.
[0303]
[0304] Example 2
[0305] A positive electrode slurry composition was prepared in the same manner as in Example 1, except that the mixture was cooled to 10°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while being stored.
[0306]
[0307] Example 3
[0308] A positive electrode slurry composition was prepared in the same manner as in Example 1, except that the mixture was cooled to -5°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while being stored.
[0309]
[0310] Example 4
[0311] A positive electrode slurry composition was prepared in the same manner as in Example 1, except that the mixture was cooled to -10°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while being stored.
[0312]
[0313] Example 5
[0314] A positive electrode slurry composition was prepared in the same manner as in Example 1, except that the mixture was cooled to -20°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while being stored.
[0315]
[0316] Example 6
[0317] A positive electrode slurry composition was prepared in the same manner as in Example 1, except that the mixture was cooled to -30°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while being stored.
[0318]
[0319] Example 7
[0320] The positive electrode active material, carbon black (Denka, DenkaBlack), PVdF (Kureha, KF9709), and solvent (Daejung Chemicals, N-methylpyrrolidone (NMP)) manufactured in the above Manufacturing Example 1 were left in a chamber at 10°C for 6 hours so that each temperature became 10°C.
[0321] While controlling the internal surface and internal space of the mixing chamber where mixing is performed to be 10℃, 200 g of the positive electrode active material, 3.43 g of carbon black as a conductive material, and 4.36 g of PVdF as a binder were dispersed and mixed in 80.8 g of a non-aqueous solvent (NMP) using a homo disper mixer (homo disper mixer, PRIMIX, Homo Disper 2.5) to prepare a mixture having a solid content of 72.0 wt%. The heat generated by the resistance of the mixer and the mixture during mixing was removed to maintain the mixing temperature at 10℃.
[0322] The mixture was cooled to -10°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while being stored to prepare a positive electrode slurry composition.
[0323]
[0324] Example 8
[0325] The positive electrode active material, carbon black (Denka, DenkaBlack), PVdF (Kureha, KF9709), and solvent (Daejung Chemicals, N-methylpyrrolidone (NMP)) manufactured in the above Manufacturing Example 1 were left in a chamber at -10°C for 6 hours so that each temperature became -10°C.
[0326] While controlling the internal surface and internal space of the mixing chamber where mixing is performed to be -10℃, 200 g of the positive electrode active material, 3.43 g of carbon black as a conductive material, and 4.36 g of PVdF as a binder were dispersed and mixed in 80.8 g of a non-aqueous solvent (NMP) using a homo disper mixer (homo disper mixer, PRIMIX, Homo Disper 2.5) to prepare a mixture having a solid content of 72.0 wt%. The heat generated by the resistance of the mixer and the mixture during mixing was removed to maintain the mixing temperature at -10℃.
[0327] The mixture was cooled to -10°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while being stored to prepare a positive electrode slurry composition.
[0328]
[0329] Example 9
[0330] A positive electrode slurry composition was prepared in the same manner as in Example 1, except that the positive electrode active material prepared in Manufacturing Example 2 was mixed to prepare a mixture, the mixture was cooled to -10°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while storing the mixture to prepare a positive electrode slurry composition.
[0331]
[0332] Example 10
[0333] The positive electrode active material, carbon black (Denka, DenkaBlack), PVdF (Kureha, KF9709), and non-aqueous solvent (Daejung Chemicals, N-methylpyrrolidone (NMP)) manufactured in the above Manufacturing Example 1 were left in a chamber at 30°C for 6 hours so that each temperature became 30°C.
[0334] At room temperature, 200 g of the positive electrode active material, 3.43 g of carbon black as a conductive material, and 4.36 g of PVdF as a binder were dispersed and mixed in 80.8 g of a solvent (NMP) using a homo disper mixer (Homo Disper 2.5, PRIMIX) to prepare a mixture having a solid content of 72.0 wt%. During mixing, the temperature of the mixture increased due to the resistance of the mixer and the mixture, and the mixing temperature was maintained at 55°C.
[0335] The mixture was cooled to -10°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while being stored to prepare a positive electrode slurry composition.
[0336]
[0337] Example 11
[0338] A positive electrode slurry composition was prepared in the same manner as in Example 1, except that a mixture was prepared by mixing LiNiO2 as a positive electrode active material, the mixture was cooled to -5°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while storing the mixture to prepare a positive electrode slurry composition.
[0339]
[0340] Example 12
[0341] LiNi as positive electrode active material 1 / 3 Co 1 / 3 Mn 1 / 3 A positive electrode slurry composition was prepared in the same manner as in Example 1, except that the mixture was prepared by mixing O2, the mixture was cooled to -5°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while storing the positive electrode slurry composition.
[0342]
[0343] Example 13
[0344] A positive electrode slurry composition was prepared in the same manner as in Example 1, except that a mixture was prepared by mixing a particulate secondary structure including LiFePO4 having an olivine crystal structure as a positive electrode active material, and the mixture was cooled to -5°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while storing the mixture to prepare a positive electrode slurry composition.
[0345]
[0346] Example 14
[0347] Li as a cathode active material 1.2 Ni 0.35 Mn 0.65A positive electrode slurry composition was prepared in the same manner as in Example 1, except that the mixture was prepared by mixing O2, the mixture was cooled to -5°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while storing the positive electrode slurry composition.
[0348]
[0349] Example 15
[0350] A positive electrode slurry composition was prepared in the same manner as in Example 1, except that a mixture was prepared by mixing a positive electrode material prepared in Manufacturing Example 1 as a positive electrode active material and a particulate secondary structure including LiFePO4 having an olivine crystal structure in a weight ratio of 50:50, and the mixture was cooled to -5°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while storing to prepare a positive electrode slurry composition.
[0351]
[0352] Example 16
[0353] The positive electrode active material manufactured in the above manufacturing example 1 and Li 1.2 Ni 0.35 Mn 0.65 A positive electrode slurry composition was prepared in the same manner as in Example 1, except that a mixture was prepared by mixing a positive electrode material mixed with O2 in a weight ratio of 50:50, the mixture was cooled to -5°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while storing the positive electrode slurry composition.
[0354]
[0355] Example 17
[0356] The positive electrode active material, carbon black (Denka, DenkaBlack), PVdF (Kureha, KF9709), and non-aqueous solvent (Daejung Chemicals, N-methylpyrrolidone (NMP)) manufactured in the above Manufacturing Example 1 were left in a chamber at 20°C for 6 hours so that each temperature became 20°C.
[0357] At room temperature, 200 g of the positive electrode active material, 3.43 g of carbon black as a conductive material, and 4.36 g of PVdF as a binder were dispersed and mixed in 80.8 g of a non-aqueous solvent (NMP) using a homo disper mixer (Homo Disper 2.5, PRIMIX) to prepare a mixture having a solid content of 72 wt%. During mixing, the temperature of the mixture increased due to the resistance of the mixer and the mixture, and the mixing temperature was maintained at 45°C.
[0358] The mixture was cooled to -23°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while being stored to prepare a positive electrode slurry composition.
[0359]
[0360] Comparative Example 1
[0361] A positive electrode slurry composition was prepared in the same manner as in Example 1, except that the mixture was cooled to 20°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while storing the positive electrode slurry composition.
[0362]
[0363] Comparative Example 2
[0364] A positive electrode slurry composition was prepared in the same manner as in Example 1, except that the mixture was cooled to 40°C to prepare a positive electrode slurry composition precursor, and then the temperature of the positive electrode slurry composition precursor was maintained while storing the positive electrode slurry composition.
[0365]
[0366] Comparative Example 3
[0367] A positive electrode slurry composition was prepared in the same manner as in Example 1, except that the mixture was transferred to a constant temperature and humidity chamber without a cooling step and stored at 50°C.
[0368]
[0369] Comparative Example 4
[0370] The positive electrode active material, carbon black (Denka, DenkaBlack), PVdF (Kureha, KF9709), and solvent (Daejung Chemicals, N-methylpyrrolidone (NMP)) manufactured in the above Manufacturing Example 2 were left in a chamber at -10°C for 6 hours so that each temperature became -10°C.
[0371] While controlling the internal surface and internal space of the mixing chamber where mixing is performed to be -10℃, 200 g of the positive electrode active material, 3.43 g of carbon black as a conductive material, and 4.36 g of PVdF as a binder were dispersed and mixed in 80.8 g of a non-aqueous solvent (NMP) using a homo disper mixer (homo disper mixer, PRIMIX, Homo Disper 2.5) to prepare a mixture having a solid content of 72.0 wt%. The heat generated by the resistance of the mixer and the mixture during mixing was removed to maintain the mixing temperature at -10℃.
[0372] A positive electrode slurry composition was prepared in the same manner as in Example 8, except that the mixture was transferred to a constant temperature and humidity chamber without a cooling step and stored at 50°C.
[0373]
[0374] Experimental Example: Viscosity Evaluation
[0375] Using a viscometer (TOKI, viscometer TV-22), the viscosity (cP) of each mixture and positive electrode slurry composition prepared in the above examples and comparative examples was measured, and the viscosity increase rate (V n [%]) was calculated and shown in Table 1 below.
[0376] Specifically, for each mixture and positive electrode slurry composition manufactured in the above examples and comparative examples, the viscosity was measured at 25°C and 1 rpm using a viscometer, and the viscosity of the mixture (VS1[cP]), the viscosity of the positive electrode slurry composition (VS2[cP]), and the percentage (V) of the difference in viscosity of the positive electrode slurry composition and the mixture with respect to the viscosity of the mixture (VS1[cP]) ((VS2[cP] - VS1[cP])) n (%)) was calculated and shown in Table 1 below. The viscosity of the positive electrode slurry composition was measured when the temperature of the positive electrode slurry composition precursor was maintained for 24 hours, 72 hours, 168 hours, and 336 hours, respectively.
[0377] For reference, when measuring viscosity at 25°C, only viscosity changes within the margin of error occur. Furthermore, if the viscosity exceeds 15,000 cP, electrode manufacturing becomes impossible.
[0378]
[0379] Type of cathode active material Temperature (℃) VS1 (cP) 24 hours maintenance 72 hours maintenance 168 hours maintenance 336 hours maintenance Mixed cooling VS2 (cP) V 24 (%)VS2(cP)V 72 (%)VS2(cP)V 168 (%)VS2(cP)V 336(%)Example 1 NMC 14 ㎛ (Ni 96%) 4503, 8003, 8501.34, 25011.85, 15035.55, 60047.4Example 2 NMC 14 ㎛ (Ni 96%) 45103, 6004, 10013.94, 50025.05, 45051.46, 13570.4Example 3 NMC 14 ㎛ (Ni 96%) 45-53, 7003, 7501.44, 25014.94, 20013.54, 35017.6Example 4 NMC 14 ㎛ (Ni 96%)45-103,5003,450-1.44,10017.14,30022.94,15018.6Example 5 NMC 14 ㎛ (Ni 96%)45-203,4003,4501.53,6507.44,10020.64,00017.6Example 6 NMC 14 ㎛ (Ni 96%)45-303,7003,8002.73,9506.84,10010.84,0509.5Example 7 NMC 14 ㎛ (Ni 96%)10-104,0004,1002.54,50012.54,55013.84,50012.5Example 8 NMC 14 ㎛ (Ni 96%) -10-103,9003,850-1.34,2007.74,50015.44,50015.4 Example 9 Single particle NMC 3.5 ㎛ (Ni 96%) 45-104,5004,7004.44,8507.85,25016.75,10013.3 Example 10 NMC 14 ㎛ (Ni 96%) 55-108,0508,1501.28,1501.28,3503.78,95011.2 Example 11 LiNiO 245-54,1004,2503.74,4007.34,3506.14,3506.1 Example 12NMC 14 ㎛ (Ni 33.3%) 45-53, 8003, 9002.63, 9503.94, 1509.23, 9503.9 Example 13LFP 45-54, 2004, 4506.04, 70011.94, 95017.95, 15022.6 Example 14NMX 6.4 ㎛ (Mn 65%) 45-53, 7003, 8504.14, 15012.24, 20013.54, 45020.3 Example 15NMC 14 ㎛ (Ni 96%)+ LFP45-54,3004,5004.74,75010.54,90014.05,10018.6Example 16NMC 14 ㎛(Ni 96%)+NMX 6.4 ㎛ (Mn 65%) 45-53, 8504, 1507.84, 35013.04, 50016.94, 55018.2 Example 17 NMC 14 ㎛ (Ni 96%) 45-233, 2503, 3503.13, 5007.73, 65012.33, 80016.9 Comparative Example 1 NMC 14 ㎛ (Ni 96%) 45204, 3005, 75033.79, 500120.912, 000179.130, 000597.8 Comparative Example 2 NMC 14 ㎛ (Ni 96%) 45404, 50015, 550245.630, 000566.7----Comparative Example 3NMC 14 ㎛ (Ni 96%) 45503,70030,000710.8------Comparative example 4NMC 14 ㎛ (Ni 96%) - 10503,70030,000710.8------.
[0380] Through the above Table 1, the positive electrode slurry compositions manufactured in Examples 1 to 17, i.e., (S1) a step of mixing a positive electrode active material, a conductive material, and a binder in a non-aqueous solvent to manufacture a mixture having a solid content of more than 60 wt%; (S2) a step of cooling the mixture to a temperature of -30°C or higher and 15°C or lower to manufacture a positive electrode slurry composition precursor; and (S3) a step of maintaining the temperature of the positive electrode slurry composition precursor, in the case of the positive electrode slurry composition manufactured by performing the following steps: V 72 It was confirmed that V was 0% or more and 50% or less, and 24 is -5% or more and 30% or less, and V 168 is 0% or more and 80% or less, and V 336 is 1% or more and 120% or less, and the viscosity and V of the mixture 24 , V 72 , V 168 , V 336 It was confirmed that it was less than 20,000cP.
[0381] In particular, in the case of the positive electrode slurry compositions manufactured in Examples 6 and 17, that is, the positive electrode slurry compositions manufactured by performing the step of manufacturing a positive electrode slurry composition precursor by cooling the mixture to a temperature of -30°C or higher and -23°C or lower, the viscosity of the positive electrode slurry composition precursor is 3,800 cP or less when the temperature is maintained for 24 hours, 3,950 cP or less when the viscosity is maintained for 72 hours, 4,100 cP or less when the viscosity is maintained for 168 hours, and 4,050 cP or less when the viscosity is maintained for 336 hours, and V 24 is less than 3.1%, V 72 is less than 7.7%, V 168 Silver 12.3% or less, V 336 It was confirmed that the viscosity of the positive electrode slurry composition was 16.9% or less. This means that when the step of manufacturing the positive electrode slurry composition precursor by cooling the mixture to a temperature of -30°C or higher and -23°C or lower is included, the viscosity of the positive electrode slurry composition is low and the viscosity increase rate is low even over time.
[0382] On the other hand, in the case of the positive electrode slurry compositions manufactured in Comparative Examples 1 to 4, i.e., the step of manufacturing the positive electrode slurry composition precursor without including the step of cooling the mixture or without cooling the mixture to 15° C. or lower, V 72 It was confirmed that V exceeded 50%. 24 is over 30%, and V 168 is over 80%, and V 336 It was confirmed that the viscosity exceeded 120% and reached the limit viscosity of 30,000 cP of the viscometer after a certain period of time, making it difficult to measure further and impossible to manufacture the electrode.
Claims
1. (S1) A step of mixing a positive electrode active material, a conductive agent, and a binder in a non-aqueous solvent to prepare a mixture having a solid content exceeding 60 wt%; (S2) a step of cooling the mixture to a temperature of -30°C or higher and 15°C or lower to prepare a positive electrode slurry composition precursor; and (S3) Maintaining the temperature of the above positive electrode slurry composition precursor V 72 A step of preparing a cathode slurry composition having a content of 0% or more and 50% or less; comprising: Above V n is the viscosity increase rate when the temperature of the positive electrode slurry composition precursor is maintained for n hours, The above viscosity increase rate is expressed by the following mathematical formula 1: A method for manufacturing a positive electrode slurry composition: [Mathematical Formula 1] Viscosity increase rate (Vn[%]) = (VS2[cP] - VS1[cP] X 100 / VS1[cP]) In the above mathematical expression 1, VS1 is the viscosity of the mixture [cP], and VS2 is the viscosity of the positive electrode slurry composition [cP].
2. In paragraph 1, A method for producing a cathode slurry composition, wherein the cathode active material comprises at least one selected from lithium composite transition metal compounds having a composition represented by the following chemical formulas 1 to 4: [Chemical Formula 1] Li a [Ni b Co c Mr d M 1 1-(b+c+d) ]O2 In the above chemical formula 1, M 1 is at least one selected from the group consisting of Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi, 0.9≤a≤1.1, 0 <b<1, 0<c<1, 0<d<1, 0<b+c+d≤1이고, [Chemical formula 2] Li e Ni 1-f M 2 f O2 In the above chemical formula 2, M 2 is at least one selected from the group consisting of Mn, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi, 0.9≤e≤1.1, 0≤f<1, [Chemical Formula 3] Li g Ni h Mr i M 3 j O2 In the above chemical formula 3, M 3 is at least one selected from the group consisting of Co, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S, B and Bi, 1.0≤g≤1.5, 0≤h≤0.5, 0.4≤i≤0.9, 0≤j≤0.1, [Chemical Formula 4] LiFe 1-k M 4 k PO4 In the above chemical formula 4, M 4 is at least one selected from the group consisting of Mn, Co, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Te, Ir, Gd, Sm, Sb, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi, 0≤k<1.
3. In paragraph 1, A method for producing a cathode slurry composition, wherein the cathode active material comprises two or more selected from lithium composite transition metal compounds having a composition represented by the following chemical formulas 1 to 4: [Chemical Formula 1] Li a [Ni b Co c Mr d M 1 1-(b+c+d) ]O2 In the above chemical formula 1, M 1 is at least one selected from the group consisting of Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi, 0.9≤a≤1.1, 0 <b<1, 0<c<1, 0<d<1, 0<b+c+d≤1이고, [Chemical formula 2] Li e Ni 1-f M 2 f O2 In the above chemical formula 2, M 2 is at least one selected from the group consisting of Mn, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi, 0.9≤e≤1.1, 0≤f<1, [Chemical Formula 3] Li g Ni h Mr i M 3 j O2 In the above chemical formula 3, M 3 is at least one selected from the group consisting of Co, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S, B and Bi, 1.0≤g≤1.5, 0≤h≤0.5, 0.4≤i≤0.9, 0≤j≤0.1, [Chemical Formula 4] LiFe 1-k M 4 k PO4 In the above chemical formula 4, M 4 is at least one selected from the group consisting of Mn, Co, Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Te, Ir, Gd, Sm, Sb, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi, 0≤k<1.
4. In paragraph 1, A method for producing a cathode slurry composition, wherein the cathode active material comprises a lithium composite transition metal compound having a composition represented by the following chemical formula 5: [Chemical Formula 5] Li a [Ni b' Co c' Mr d' M 5 1-(b'+c'+d')]O2 M 5 is at least one selected from the group consisting of Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, F, Ta, Mo, Sc, V, Zn, Cu, In, S and Bi, 0.9≤a'≤1.1, 0.6≤b'<1, 0 <c'<0.4, 0<d'<0.4, 0<b'+c'+d'≤1이다.
5. In paragraph 1, A method for producing a positive electrode slurry composition, wherein the mixing is performed so that the positive electrode active material is 85 parts by weight or more and 99 parts by weight or less, the conductive material is 0.5 parts by weight or more and 10 parts by weight or less, and the binder is 0.5 parts by weight or more and 10 parts by weight or less, based on 100 parts by weight of solid content.
6. In paragraph 1, A method for producing a cathode slurry composition having a solid content of 70 wt% or more and 85 wt% or less.
7. In paragraph 1, V 24 A method for producing a cathode slurry composition having a content of -5% or more and 30% or less.
8. In paragraph 1, V 168 A method for producing a cathode slurry composition having a content of 0% or more and 80% or less.
9. In paragraph 1, V 336 A method for producing a cathode slurry composition having a content of 1% or more and 120% or less.
10. In paragraph 1, A method for producing a cathode slurry composition, wherein the mixture, the cathode slurry composition precursor and the cathode slurry composition each independently have a viscosity of 20,000 cP or less.
11. In paragraph 1, The above mixing is performed at a temperature of 0℃ or higher and 15℃ or lower. Above V 72 A method for producing a cathode slurry composition having a content of 8% or more and 35% or less.
12. In paragraph 1, The above cooling is performed at a temperature of -30℃ or higher and less than 0℃. Above V 72 A method for producing a cathode slurry composition having a content of 0% or more and 20% or less. 13.(A) A step of manufacturing a cathode slurry composition according to any one of the manufacturing methods of clauses 1 to 12; and (B) A method for manufacturing a positive electrode, comprising the step of applying and drying the positive electrode slurry composition on a current collector to form a positive electrode active material layer.
14. In paragraph 13, Immediately before the step (B), the step (A1) of transferring the positive electrode slurry composition to a means for applying a positive electrode active material composition is further included; A method for manufacturing an anode, wherein the above transport is performed at a temperature of -30℃ or higher and 15℃ or lower.
Citation Information
Patent Citations
Manufacturing method of positive mix paste for nonaqueous electrolyte secondary battery, and the nonaqueous electrolyte secondary battery using the positive mix paste
JP2007141649A
Method for manufacturing positive electrode plates for non-aqueous secondary batteries
JP5126802B2
Method of preparing cathode for secondary battery
KR1020180091092A
Pharmaceutical composition for preventing or treating metabolic diseases comprising Licochalcone D or analogs thereof
KR102879424B1
KR20200035582A