Positive electrode active material, and positive electrode and lithium secondary battery comprising same

A single particle lithium transition metal oxide positive electrode active material, produced through a two-step firing process, addresses structural collapse and energy density issues in high-nickel batteries by maintaining crystallinity and layered structure, enhancing lifespan and energy density.

WO2024248544A1PCT designated stage expired Publication Date: 2024-12-05LG CHEM LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/007495
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-05-31
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

High-nickel positive electrode active materials in lithium secondary batteries face issues with structural collapse and decreased energy density due to microcracks during charging and discharging, and single-crystal nickel-based materials require high firing temperatures, leading to phase changes and increased resistance.

Method used

A single particle lithium transition metal oxide positive electrode active material with specific internal and external boundary ratios, manufactured through a two-step firing process, maintains crystallinity and layered structure, enhancing lifespan and energy density.

Benefits of technology

The solution provides a positive electrode active material with improved lifespan and energy density by maintaining crystallinity and preventing structural collapse, while avoiding the high temperature issues of single-crystal materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024007495_05122024_PF_FP_ABST
    Figure KR2024007495_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a single particle-type positive electrode active material comprising a lithium transition metal oxide in the form of a single particle, and a positive electrode and a lithium secondary battery comprising the positive electrode active material. The lithium transition metal oxide in the form of a single particle comprises an outer boundary surface forming the outer periphery of the particle and an inner boundary surface formed within the particle, and satisfies 0 < length of inner boundary surface / length of outer boundary surface < 0.4.
Need to check novelty before this filing date? Find Prior Art

Description

Cathode active material, and cathode and lithium secondary battery containing the same

[0001] Cross-citation with related applications

[0002] This application claims the benefit of priority from Korean Patent Application No. 10-2023-0071877, filed June 2, 2023, the entire contents of which are incorporated herein by reference.

[0003] Technology field

[0004] The present invention relates to a positive electrode active material for a lithium secondary battery, and a positive electrode and a lithium secondary battery including the same.

[0005]

[0006] Recently, with the advancement of technology such as electric vehicles, the demand for high-capacity secondary batteries is increasing, and accordingly, research on cathodes using high-nickel (High Ni) cathode active materials with excellent capacity characteristics is being actively conducted.

[0007] Since the high-nickel cathode active material uses a co-precipitation method to manufacture it, the manufactured high-nickel cathode active material has the form of secondary particles in which primary particles are aggregated. However, the active material in the form of secondary particles has the disadvantage that microcracks occur in the secondary particles during long-term charge / discharge processes, causing side reactions. In addition, when the electrode density is increased to improve energy density, the secondary particles cause structural collapse, which reduces the active material and electrolyte, resulting in a decrease in energy density and a decrease in life characteristics.

[0008] To address the problems associated with high-nickel cathode active materials in the form of secondary particles, single-crystal nickel-based cathode active materials have recently been developed. Single-crystal nickel-based cathode active materials have the advantage of resisting particle collapse even when increasing electrode density to achieve high energy density. However, because a relatively high firing temperature is required to manufacture single-crystal nickel-based cathode active materials, the R-3m layered structure is not properly maintained, and lithium escapes from the crystal structure, resulting in a phase transition to a Fm-3m rock-salt structure, such as NiO. This deteriorates the crystallinity of the cathode active material, increasing the proportion of NiO on the surface of the manufactured single-crystal particles. This increase in NiO leads to increased resistance, a decrease in energy density, and a decrease in output. Furthermore, when the firing temperature is low, the secondary particles are over-fired, which means that the lifespan and gas generation improvements do not reach the levels expected from single particles.

[0009] Therefore, there is still a need for the development of a cathode active material that has high electrode density and exhibits excellent life and output characteristics.

[0010]

[0011] [Prior Art Literature]

[0012] [Patent Document]

[0013] (Patent Document 1) KR 2019-0094529 A1

[0014]

[0015] The problem to be solved by the present invention is to provide a positive electrode active material having excellent life characteristics.

[0016]

[0017] To solve the above problem, the present invention provides a positive electrode active material, a positive electrode, and a lithium secondary battery.

[0018]

[0019] (1) The present invention is a positive electrode active material comprising a lithium transition metal oxide in the form of a single particle, wherein the lithium transition metal oxide in the form of a single particle includes an external boundary forming the outer surface of the particle and an internal boundary formed within the particle, and satisfies the following equation 1:

[0020] [Formula 1]

[0021] 0 < length of inner boundary / length of outer boundary < 0.4

[0022] The length of the inner boundary is the length obtained by subtracting the length of the boundary measured from the EBSD band contrast map from the length of the boundary measured from the electron backscatter diffraction (EBSD)-IPF map for the lithium transition metal oxide particle, and the length of the outer boundary is the length of the outer boundary of the transition metal oxide particle measured through SEM image segmentation, thereby providing a single particle type positive electrode active material.

[0023] (2) In the present invention, in the above (1), the lithium transition metal oxide in the form of a single particle further provides a single particle type positive electrode active material that satisfies the following formula 2.

[0024] [Formula 2] Length of boundary measured from EBSD IPF map / Length of boundary measured from EBSD band contrast map ≤ 1.4

[0025] The length of the above outer boundary surface is the length of the outer boundary surface of the transition metal oxide particle measured through SEM image segmentation.

[0026] (3) The present invention provides a single particle type positive electrode active material in (1) or (2) above, wherein the single particle type lithium transition metal oxide further satisfies the following formula 3.

[0027] [Formula 3] 0 ≤ (length of inner boundary / length of outer boundary) - (length of boundary measured by length of inner boundary / EBSD band contrast)) ≤ 1

[0028] (4) The present invention provides a positive electrode active material in which the length of the boundary measured from the electron backscatter diffraction (EBSD)-IPF map in any one of the above (1) to (3) includes the length of a weak boundary in which only the atomic arrangement is different and crystallinity is not collapsed and the length of a strong boundary formed by collapse of the layered structure contained in the lithium transition metal oxide particle in the form of a single particle.

[0029] (5) The present invention provides a cathode active material in which the length of the boundary surface measured by the EBSD band contrast map in any one of the above (1) to (4) includes the length of a strong boundary surface formed by the collapse of a layered structure included in the lithium transition metal oxide particle in the form of a single particle.

[0030] (6) The present invention provides a single particle type positive electrode active material in any one of the above (1) to (5), wherein the single particle type lithium transition metal oxide includes 2 to 50 particles.

[0031] (7) The present invention provides a positive electrode active material in any one of the above (1) to (6), wherein the lithium transition metal oxide is a lithium composite transition metal oxide containing nickel, cobalt, and manganese.

[0032] (8) The present invention provides a positive electrode active material in any one of the above (1) to (7), wherein the lithium transition metal oxide is a lithium composite transition metal oxide represented by the following chemical formula 1:

[0033] [Chemical Formula 1]

[0034] Li a Ni b Co c Mn d M 1 e O2

[0035] In the above chemical formula 1, M 1is at least one selected from the group consisting of Al, Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, Sn, Y, Zn, F, P and S, and 0.9≤a≤1.1, 0.6≤b<1, 0 <c<0.4, 0<d<0.4, 0≤e<0.1, b+c+d+e=1이다.

[0036] (9) The present invention provides a positive electrode active material in any one of the above (1) to (8), wherein the lithium transition metal oxide is a lithium composite transition metal oxide represented by the following chemical formula 2:

[0037] [Chemical Formula 2]

[0038] Li a Ni b Co c Mn d O2

[0039] In the above chemical formula 2, 0.9≤a≤1.1, 0.6≤b<1, 0 <c<0.4, 0<d<0.4, b+c+d=1이다.

[0040] (10) The present invention is characterized in that the average particle diameter (D) is greater than that of the lithium transition metal oxide in the form of a single particle in any one of the above (1) to (9). 50 ) further includes a second lithium transition metal oxide in the form of small single particles and provides a positive electrode active material having a bimodal particle size distribution.

[0041] (11) The present invention provides a positive electrode active material in the above (10), wherein the second lithium transition metal oxide is a lithium composite transition metal oxide represented by the following chemical formula 3.

[0042] [Chemical Formula 3]

[0043] Li a3 Ni b3 Co c3 Mn d3 M 3 e3 O2

[0044] In the above chemical formula 3, M 3is at least one selected from the group consisting of Al, Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, Sn, Y, Zn, F, P and S, and 0.9≤a3≤1.1, 0.6≤b3<1, 0 <c3<0.4, 0<d3<0.4, 0≤e3<0.1, b3+c3+d3+e3=1이다.

[0045] (12) The present invention provides a positive electrode active material in (10) or (11) above, wherein the weight ratio of the lithium transition metal oxide and the second lithium transition metal oxide is 1 to 9:1.

[0046] (13) The present invention is characterized in that the press density is 3.50 g / cm in any one of the above (10) to (12). 2 3.90g / cm 2 It provides a positive electrode active material.

[0047] (14) The present invention provides a positive electrode comprising a positive electrode active material according to any one of (1) to (13).

[0048] (15) The present invention provides a lithium secondary battery including a positive electrode according to (14) above.

[0049]

[0050] The cathode active material of the present invention is a single-particle cathode active material including a lithium transition metal oxide in the form of a single particle, and since the lithium transition metal oxide in the form of a single particle includes a certain amount of internal boundary surface, it can exhibit excellent life characteristics.

[0051]

[0052] Figure 1 shows an SEM photograph, an EBSD band contrast map, an EBSD-IPF map, and an IPF interface for the positive electrode active material of Example 1.

[0053] Figure 2 shows an SEM photograph, an EBSD band contrast map, an EBSD-IPF map, and an IPF interface for the positive electrode active material of Comparative Example 4.

[0054]

[0055] Hereinafter, the present invention will be described in more detail to help understand the present invention.

[0056] The terms or words used in the description and claims of the present invention should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical idea of ​​the present invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best way.

[0057] In the present invention, the term 'primary particle' means the smallest particle unit that can be distinguished as a single lump when observing the cross-section of a positive electrode active material through a scanning electron microscope (SEM), and may be composed of multiple crystal grains.

[0058] In the present invention, the term "secondary particle" refers to a secondary structure formed by the aggregation of multiple primary particles. The average particle diameter of the secondary particles can be measured using a particle size analyzer.

[0059] In the present invention, the term 'single-particle form' may be used instead of the term 'single-crystal' or 'single-particle type', and means a form that is in contrast to a secondary particle form formed by agglomeration of hundreds of primary particles manufactured by a conventional method. In addition, the term 'single-particle type positive electrode active material' or 'single-particle type lithium transition metal oxide' in the present invention means a positive electrode active material or lithium transition metal active material composed of 50 single-crystal particles or less, in contrast to a positive electrode active material in the form of secondary particles formed by agglomeration of hundreds of primary particles manufactured by a conventional method.

[0060] Typically, a single crystal particle refers to a particle in which the entire sample consists of only one grain or grain region. In the present invention, the single-particle type positive electrode active material or the single-particle type lithium transition metal oxide may be a single-particle type positive electrode active material or a single-particle type lithium transition metal oxide in which 1 to 50 particles, specifically 1 to 30 particles, are aggregated, and may exhibit characteristics similar to a single crystal particle by including a small number of single crystal particles. The 'single crystal particle' refers to the smallest particle unit recognized when observing the positive electrode active material through a scanning electron microscope, and the 'grain' or 'grain region' refers to a region in which atoms within the sample are continuously and periodically arranged in one direction. The grain can be analyzed by obtaining an EBSD inverse pole figure (IPF) map using an electron backscatter diffraction (ESBD) analyzer.

[0061] In the present invention, the term 'average particle diameter (D 50 )' means the particle size at the 50% point of the volume cumulative distribution according to particle size. The above average particle size is calculated by dispersing the powder to be measured in a dispersion medium, introducing it into a commercially available laser diffraction particle size measuring device (e.g., S3500 from Microtrac), and measuring the difference in diffraction pattern according to particle size when the particles pass through the laser beam to calculate the particle size distribution, and calculating the particle diameter at the point where it becomes 50% of the volume cumulative distribution according to particle size in the measuring device, thereby obtaining D 50 can be measured.

[0062]

[0063] The cathode active material of the present invention is a cathode active material including a lithium transition metal oxide in the form of a single particle, wherein the lithium transition metal oxide in the form of a single particle includes an external boundary forming the outer surface of the particle and an internal boundary formed within the particle, and satisfies the following equation 1.

[0064] [Formula 1]

[0065] 0 < length of inner boundary / length of outer boundary < 0.4

[0066] The length of the inner boundary is the length of the boundary measured from the electron backscatter diffraction (EBSD)-IPF map for the lithium transition metal oxide particle minus the length of the boundary measured from the EBSD band contrast (BC) map, and the length of the outer boundary is the length of the outer boundary of the transition metal oxide particle measured through SEM image segmentation, providing a positive electrode active material.

[0067] In the present invention, the internal boundary surface may refer to a boundary surface formed when grains included in the lithium transition metal oxide particles in the form of single particles come into contact with each other. Since lithium ions can easily move at the internal boundary surface, which refers to a boundary surface formed when the grains come into contact with each other, degradation occurs preferentially as the charge / discharge cycle progresses, and the more movement paths there are for the lithium ions to easily move, the lower the life characteristics may be. The content of the internal boundary surface can be quantitatively determined through the length of the internal boundary surface included in the lithium transition metal oxide particles in the form of single particles.

[0068] When an EBSD IPF map is obtained using the EBSD IPF measurement method for the lithium transition metal oxide particles in the single particle form, the grains contained in the lithium transition metal oxide particles in the single particle form can be distinguished. Accordingly, from the EBSD IPF map, the boundary formed when one grain contained in the lithium transition metal oxide particles in the single particle form comes into contact with another grain can be identified.

[0069] However, among the boundaries identified by the EBSD IPF map, not only the boundaries between grains (weak boundaries) where the arrangement direction of atoms simply changes with respect to the boundary, but also boundaries (strong boundaries) where there is a change in the arrangement direction of atoms and a collapse of the layered structure of the transition metal oxide layer, particularly a collapse of the layered structure of the NiO layer, are included. Therefore, in order to obtain only the boundaries between grains, it is necessary to exclude boundaries where there is a collapse of the layered structure of the transition metal oxide layer.

[0070] When a BC map is obtained by EBSD for the lithium transition metal oxide particles in the single particle form, a weak boundary where only the atomic arrangement is different and crystallinity is not collapsed cannot be distinguished within the lithium transition metal oxide particles in the single particle form, but a strong boundary where the layered structure of the transition metal oxide is collapsed can be distinguished. The boundary where the layered structure of the transition metal oxide is collapsed may be a boundary formed between one single crystal particle of the lithium transition metal oxide particles in the single particle form and another single crystal particle.

[0071] The length of the boundary surface measured from the EBSD IPF map may include the length of the boundary surface between grains included in the lithium transition metal oxide particle in the single particle form, the boundary surface formed by the collapse of the layered structure, and the length of the outer boundary surface of the particle.

[0072] Additionally, the length of the boundary surface measured from the EBSD BC map may include the length of the boundary surface formed by the collapse of the layered structure included in the lithium transition metal oxide particle in the single particle form and the length of the outer boundary surface.

[0073] Therefore, the length of the inner boundary is the length of the boundary measured from the EBSD IPF map for the lithium transition metal oxide particle excluding the length of the boundary measured from the EBSD BC map, and since the length of the outer perimeter (outer boundary) of the single-particle transition metal oxide particle is measured in the same way in the EBSD IPF map and the EBSD BC map, if this is excluded, it can be expressed as follows.

[0074]

[0075] Length of inner boundary

[0076] = [Boundary length measured from EBSD IPF map] - [Boundary length measured from EBSD BC map]

[0077] = [Length of strong boundary + length of weak boundary] - [Length of strong boundary]

[0078] = length of weak boundary

[0079]

[0080] In addition, the length of the external boundary surface of the single particle-shaped transition metal oxide particle can be obtained by obtaining an SEM image of the single particle-shaped lithium transition metal oxide particle and segmenting the SEM image to obtain the length of the external boundary surface forming the external surface of the transition metal oxide particle.

[0081]

[0082] The above equation 1 is a numerical value that quantifies the degree of inclusion of the internal boundary surface of the single-particle type transition metal oxide particle by dividing the length of the internal boundary surface by the length of the external boundary surface.

[0083] The decrease in the value of the length of a line formed inside an object of a circular, circular or similar shape calculated using a two-dimensional image obtained using EBSD and SEM divided by the length of the outer edge of the object may reflect a decrease in the length of a weak boundary inside the single-particle-shaped transition metal oxide particle, and the single-particle-shaped positive electrode active material of the present invention has a ratio of the length of the inner boundary / the length of the outer boundary of Equation 1 of less than 0.4, and by satisfying the above value, the single-particle-shaped positive electrode active material of the present invention can exhibit excellent life characteristics by reducing the phenomenon in which degradation occurs preferentially in a movement path through which lithium ions easily move.

[0084] The value of the length of the inner boundary surface / the length of the outer boundary surface in the above formula 1 can specifically satisfy a value greater than 0 and less than or equal to 0.3, and more specifically greater than 0.01 and less than or equal to 0.2. If the value of the above formula 1 is excessive, the effect of improving the life characteristics of the single-particle type positive electrode active material may be reduced. In addition, if the value of the above formula 1 is 0, the effect of improving the capacity characteristics and life characteristics of the single-particle type positive electrode active material may be reduced.

[0085] Therefore, when the lithium transition metal oxide in the form of a single particle of the present invention satisfies the value of Equation 1, it can exhibit a more excellent life characteristic improvement effect.

[0086] The single crystallinity of the single-particle-shaped transition metal oxide particle can be determined through the value of the above formula 1. For example, if the single-particle-shaped transition metal oxide particle is a single crystal, the value of the above formula 1 becomes 0, and if the single-particle-shaped transition metal oxide particle contains a large amount of crystals and has a low single crystallinity, the value of the above formula 1 increases.

[0087]

[0088] In addition, the lithium transition metal oxide in the form of a single particle may additionally satisfy the following equation 2.

[0089] [Formula 2]

[0090] Length of boundary measured from EBSD IPF map / Length of boundary measured from EBSD band contrast map ≤ 1.4

[0091] The above equation 2 is the value obtained by dividing the sum of the lengths of the strong boundary and the weak boundary measured from the EBSD IPF map by the length of the strong boundary measured by the EBSD BC map.

[0092] The value of the above equation 2 becomes smaller as the ratio of the length of the weak boundary, which is simply a different atomic arrangement and has not collapsed crystallinity, among the boundaries of single-particle transition metal oxides decreases or the ratio of the strong boundary formed by collapse of the layered structure compared to the weak boundary increases.

[0093] The positive electrode active material of the present invention can satisfy a ratio of the length of the boundary surface measured from the EBSD IPF map of the above formula 2 / the length of the boundary surface measured from the EBSD band contrast map of specifically 1 to 1.4, more specifically 1 to 1.3.

[0094] When the value of the above formula 2 satisfies the above range, excellent life characteristics can be properly exhibited, and when the value of the above formula 2 is excessive, the life characteristics of the positive electrode active material may deteriorate.

[0095] Therefore, when the lithium transition metal oxide in the form of a single particle of the present invention satisfies the value of Equation 1 and the value of Equation 2 satisfies the above range, it can exhibit even better life characteristics.

[0096] The length of the above outer boundary surface is the length of the outer boundary surface of the transition metal oxide particle measured through SEM image segmentation.

[0097] The length of the external boundary surface of the above single particle-shaped transition metal oxide particle can be obtained by obtaining an SEM image of the above single particle-shaped lithium transition metal oxide particle and segmenting the SEM image to obtain the length of the external boundary surface forming the external surface of the above transition metal oxide particle.

[0098]

[0099] In addition, the positive electrode active material of the present invention can satisfy the following equation 3, which is the difference between the value of equation 2 and the value of equation 1.

[0100] [Formula 3]

[0101] 0 ≤ (length of inner boundary / length of outer boundary) - (length of inner boundary / length of boundary measured from EBSD band contrast map) ≤ 1

[0102] The cathode active material of the present invention can specifically satisfy the above formula 3 of 0 to 0.8, 0 to 0.7, or 0 to 0.5, and more specifically 0 to 0.3. When the above formula 3 satisfies the above range, it can exhibit an appropriate capacity expression effect while exhibiting excellent life characteristics.

[0103]

[0104] In the positive electrode active material according to an example of the present invention, the particles included in the positive electrode active material have an average particle diameter (D 50 ) may be 0.1 ㎛ to 10 ㎛. When the average particle diameter of the particles included in the positive electrode active material satisfies the above range, when they aggregate to form a single-particle type positive electrode active material or a single-particle type lithium transition metal oxide, it may have advantages in terms of rolling rate, electrode pores, etc., and when the average particle diameter is less or greater than the above range, performance may be degraded in terms of electrode capacity, life characteristics, resistance, etc.

[0105]

[0106] In the positive electrode active material according to an example of the present invention, the lithium transition metal oxide in the form of a single particle may be a lithium composite transition metal oxide containing nickel (Ni), cobalt (Co), and manganese (Mn).

[0107] Specifically, the lithium transition metal oxide in the form of a single particle may be a lithium composite transition metal oxide represented by the following chemical formula 1.

[0108]

[0109] [Chemical Formula 1]

[0110] Li a Ni b Co c Mn d M 1 e O2

[0111] In the above chemical formula 1, M 1 is at least one selected from the group consisting of Al, B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf, and 0.9≤a≤1.1, 0.6≤b<1, 0 <c<0.4, 0<d<0.4, 0≤e<0.1, b+c+d+e=1이다.

[0112]

[0113] In addition, specifically, the lithium transition metal oxide may be a positive electrode active material that is a lithium composite transition metal oxide represented by the following chemical formula 2.

[0114] [Chemical Formula 2]

[0115] Li a Ni b Co c Mn d O2

[0116] In the above chemical formula 2, 0.9≤a≤1.1, 0.6≤b<1, 0 <c<0.4, 0<d<0.4, b+c+d=1이다.

[0117]

[0118] The above positive electrode active material has an average particle diameter (D) of 1 to 50 ㎛, taking into account the specific surface area and positive electrode composite density. 50 ) and specifically, an average particle diameter (D) of 2 to 20 ㎛ 50 ) may have. When the average particle diameter of the positive electrode active material satisfies the above range, it may have advantages in rolling rate, electrode pores, etc., and when the average particle diameter is less or greater than the above range, performance may be degraded in electrode capacity, life characteristics, resistance, etc.

[0119] In one embodiment of the present invention, the positive electrode active material may be composed of 2 to 50 particles or less, 2 to 40 particles or less, 2 to 30 particles or less, 2 to 20 particles or less, 2 to 15 particles or less, 2 to 10 particles or less, or 2 to 5 particles or less.

[0120]

[0121] In one example of the present invention, the lithium transition metal oxide particle in the form of a single particle may be manufactured by mixing a transition metal oxide precursor and a lithium raw material, performing a first firing, and then crushing and then performing a second firing of the plastic product manufactured by the first firing.

[0122] Specifically, the lithium transition metal oxide particles in the form of single particles can be manufactured by a method including: (A) a step of mixing a positive electrode active material precursor including Ni, Co, and Mn, and a first lithium-containing raw material to prepare a mixture; (B) a step of first firing the mixture at a temperature of 800°C to 950°C to prepare a first fired product; and (C) a step of second firing the mixture at a temperature of 680°C to 850°C after mixing a second lithium-containing raw material into the first fired product to prepare a second fired product.

[0123] When the mixture is first fired at a temperature of 800°C to 950°C, the primary particles of the positive electrode active material precursor aggregate to produce a primary fired product in the form of single particles. Specifically, the primary firing temperature may be 800°C, 810°C, 820°C, 830°C, 840°C, 850°C or higher, and 900°C, 910°C, 920°C, 930°C, 940°C, or 950°C or lower. When the primary firing temperature is within the above range, the primary particles of the positive electrode active material precursor aggregate to form a structurally stable primary fired product in the form of single particles. When the primary firing temperature is less than 800°C, there is a problem that the primary particles do not sufficiently aggregate, and when it is more than 950°C, there is a problem that a structurally unstable fired product with low crystallinity is produced.

[0124] The above first calcination may be performed under an oxygen atmosphere in order to prevent the lithium transition metal oxide from degenerating into a rock salt structure.

[0125] The above first firing may be performed for 3 to 12 hours, specifically 3 hours, 4 hours, 5 hours, 6 hours or more and 9 hours, 10 hours, 11 hours, or 12 hours or less, in order to agglomerate the primary particles and improve the crystallinity of the first fired product.

[0126]

[0127] When the above-mentioned first fired product is subjected to a second firing at a temperature of 680°C to 850°C, lithium is inserted into the first fired product, thereby producing a second fired product. At this time, the second fired product is a lithium composite transition metal oxide in the form of single particles. Specifically, the second firing temperature may be 680°C, 700°C, 720°C, 740°C, 760°C, 780°C, 800°C or higher, 840°C, or 850°C or lower. When the second firing temperature is within the above range, lithium is inserted into the rock salt structure that may be formed on the surface of the first fired product due to the high temperature during the first firing, thereby restoring it to a layered structure, and there is an advantage of reducing lithium byproducts. Meanwhile, when the secondary firing temperature is lower than 680℃, there is a problem that the lithium insertion speed is slow due to the low temperature, and when it is higher than 850℃, there is a problem that the surface of the primary firing product degenerates into a rock salt structure due to the high temperature, and lithium byproducts remain.

[0128] The above secondary calcination may be performed under an oxygen atmosphere in order to prevent the lithium transition metal oxide from degenerating into a rock salt structure.

[0129] The above secondary firing may be performed for 3 to 12 hours, specifically 3 hours, 4 hours, 5 hours, 6 hours, 9 hours or more, and 9 hours, 10 hours, 11 hours, or 12 hours or less, in order to increase the crystallinity of the internal crystal structure of the positive electrode active material.

[0130] In addition, the method for manufacturing a cathode active material according to the present invention may further include, before step (C), a step (B') of crushing the first sintered product. In step (B'), the first sintered product is crushed to have an average particle diameter (D) in order to prevent the initial resistance from increasing. 50 ) may be ground to a size of 3 ㎛ to 20 ㎛.

[0131] In addition, the method for manufacturing a cathode active material according to the present invention may further include a step (C') of crushing the secondary sintered product. In addition, in the step (C'), the secondary sintered product may be crushed to have an average particle diameter (D) in order to prevent the initial resistance from increasing. 50 ) may be ground to a size of 3 ㎛ to 20 ㎛.

[0132] The grinding of the above steps (B') and (C') can be performed using a pin mill, an ACM, a jet mill, etc. Meanwhile, the pin mill can be performed under conditions of 18,000 rpm, the ACM can be performed under conditions of 6,000 rpm for classification and 12,000 rpm for main milling using a device from Hosokawa, and the jet mill can be performed under conditions of 6 bar for grinding pressure and 3,500 rpm for classification using a device from ZM solution. In this case, the desired average particle size (D 50 ) can be easily obtained.

[0133] The cathode active material according to the present invention is manufactured by a process in which lithium-containing raw materials are introduced in two stages. That is, the lithium-containing raw materials are introduced separately before the first firing and before the second firing. In this case, there is an advantage in that lithium is inserted into the rock salt structure that may be formed on the surface, thereby facilitating recovery into a layered structure. On the other hand, if the lithium-containing raw materials are introduced all at once before the first firing, there is a problem of deterioration in electrochemical performance due to an increase in lithium byproducts. In addition, if the lithium-containing raw materials are not introduced in the second firing stage, problems arise in that a slow reaction rate, high temperature, and long time are required.

[0134] In the case where the lithium-containing raw material is input in two portions, in the step (A), the first lithium-containing raw material may be mixed so that the ratio (M:Li) of the total mole number (M) of the transition metal included in the positive electrode active material precursor and the mole number (Li) of lithium included in the first lithium-containing raw material is 1:0.98, 1:0.99, 1:1.00, 1:1.01, 1:1.02 or more, 1:1.04, 1:1.05 or less, and in the step (C), the second lithium-containing raw material may be mixed so that the ratio (M:Li) of the total mole number (M) of the transition metal included in the positive electrode active material precursor of the step (A) and the mole number (Li) of lithium included in the second lithium-containing raw material is 1:0.01 or more, 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09, It can be mixed to a ratio of 1:0.10 or less.

[0135]

[0136] In addition, the present invention provides a lithium transition metal oxide in the form of a single particle (hereinafter, the first lithium transition metal oxide) having an average particle diameter (D 50 ) further includes a second lithium transition metal oxide in the form of small single particles and provides a positive electrode active material having a bimodal particle size distribution.

[0137] A cathode active material having a bimodal particle size distribution comprises two types of lithium transition metal oxides of different sizes, and the second lithium transition metal oxide is filled between the first lithium transition metal oxides, so that the rolling density is high, and thus a desired electrode thickness can be achieved without applying high pressure. In addition, when rolling for electrode manufacture, the stress applied to the first lithium transition metal oxide is dispersed, so that particle breakage can be prevented.

[0138] When the positive electrode active material according to the present invention has a bimodal particle size distribution, the first lithium transition metal oxide has an average particle diameter (D 50) may be 5㎛ to 9㎛. Specifically, the average particle diameter (D of the first lithium transition metal oxide 50 ) may be 5㎛, 5.5㎛, 6㎛, 6.5㎛ or more, 7.5㎛, 8㎛, 8.5㎛, or 9㎛ or less. And, the second lithium transition metal oxide may have an average particle diameter (D 50 ) may be 1 μm to 4 μm. Specifically, the average particle diameter (D of the second lithium transition metal oxide 50 ) can be 1㎛, 1.5㎛, 2㎛, 2.5㎛ or more, 2.5㎛, 3㎛, ​​3.5㎛, or 4㎛ or less.

[0139] The average particle diameter (D) of the first lithium transition metal oxide and the second lithium transition metal oxide 50 ) is within the above range, the second lithium transition metal oxide may be appropriately distributed between the first lithium transition metal oxide, so that the filling rate may be excellent.

[0140] The ratio of the average particle size of the first lithium transition metal oxide to the average particle size of the second lithium transition metal oxide may be 2 to 5:1. When the ratio of the average particle size of the first lithium transition metal oxide to the average particle size of the second lithium transition metal oxide is within the above range, not only is the filling ratio excellent, but there is also the advantage of improved rolling density.

[0141] According to the present invention, the second lithium transition metal oxide may be a lithium composite transition metal oxide represented by the following chemical formula 3.

[0142] [Chemical Formula 3]

[0143] Li a3 Ni b3 Co c3 Mn d3 M 3 e3 O2

[0144] In the above chemical formula 3, M 3is at least one selected from the group consisting of Al, Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, Sn, Y, Zn, F, P and S, and 0.9≤a3≤1.1, 0.6≤b3<1, 0 <c3<0.4, 0<d3<0.4, 0≤e3<0.1, b3+c3+d3+e3=1이다.

[0145] According to the present invention, the weight ratio of the first lithium transition metal oxide and the second lithium transition metal oxide may be 1 to 9:1. When the weight ratio of the first lithium transition metal oxide and the second lithium transition metal oxide is within the above range, the packing density of the particles can be increased, and consequently, the capacity of the battery can be increased when applied to the battery.

[0146] When the positive electrode active material according to the present invention has a bimodal particle size distribution, the positive electrode active material has a press density of 3.50 g / cm 2 3.90g / cm 2 It can be. Specifically, the rolling density of the positive electrode active material is 3.50 g / cm 2 , 3.55g / cm 2 , 3.60g / cm 2 Above, 3.80g / cm 2 , 3.85g / cm 2 , 3.90g / cm 2 It may be as follows. When the rolling density of the positive electrode active material is within the above range, the energy density per volume may increase.

[0147]

[0148] anode

[0149] According to another embodiment of the present invention, a positive electrode comprising the above-described positive electrode active material is provided.

[0150] Specifically, the positive electrode includes a positive electrode current collector, and a positive electrode active material layer formed on the positive electrode current collector and including the positive electrode active material described above.

[0151] The positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 μm, and fine unevenness may be formed on the surface of the positive electrode current collector to increase the adhesive strength of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.

[0152] The above positive electrode active material layer may include a conductive material and a binder together with the positive electrode active material described above.

[0153] At this time, the conductive material is used to provide conductivity to the electrode, and in the battery to be formed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskey such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like, and one type alone or a mixture of two or more types thereof may be used. The conductive material may typically be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.

[0154] The above binder serves to improve the adhesion between positive electrode active material particles and the adhesive strength between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluoroelastomer, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof. The binder may be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.

[0155] The above-mentioned positive electrode can be manufactured according to a conventional positive electrode manufacturing method, except that the above-mentioned positive electrode active material is used. Specifically, the positive electrode active material layer forming composition, which is manufactured by mixing or dispersing the above-mentioned positive electrode active material and optionally a binder and a conductive agent in a solvent, is applied onto a positive electrode current collector, followed by drying and rolling. At this time, the types and contents of the positive electrode active material, binder, and conductive agent are as described above.

[0156] The solvent may be a solvent generally used in the relevant technical field, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water. One of these may be used alone or a mixture of two or more thereof may be used. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, taking into account the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the positive electrode.

[0157] Additionally, in another method, the positive electrode may be manufactured by casting the composition for forming the positive electrode active material layer on a separate support, and then laminating the resulting film on a positive electrode current collector by peeling it off from the support.

[0158]

[0159] lithium secondary battery

[0160] According to another example of the present invention, an electrochemical device including the positive electrode is provided. The electrochemical device may be, specifically, a battery, a capacitor, or the like, and more specifically, a lithium secondary battery.

[0161] The lithium secondary battery specifically includes a positive electrode, a negative electrode positioned opposite the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, wherein the positive electrode is as described above. In addition, the lithium secondary battery may optionally further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0162] In the above lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.

[0163] The above negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.

[0164] The above negative electrode active material layer optionally includes a binder and a conductive material together with the negative electrode active material.

[0165] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; SiO x(0 < x < 2), SnO2, vanadium oxide, lithium vanadium oxide, and other metal oxides capable of doping and dedoping lithium; or composites containing the above metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include natural graphite or artificial graphite in the form of amorphous, plate-like, flaky, spherical, or fiber-like forms, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes.

[0166] Additionally, the binder and the conductive material may be the same as those described above for the positive electrode.

[0167] The above-described negative electrode active material layer may be manufactured by, for example, applying a negative electrode forming composition prepared by dispersing a negative electrode active material, and optionally a binder and a conductive material in a solvent, onto a negative electrode current collector and drying the coating, or by casting the negative electrode forming composition onto a separate support and then laminating the resulting film onto a negative electrode current collector by peeling it off from the support.

[0168] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used as a separator in lithium secondary batteries can be used without special restrictions, and in particular, one having low resistance to ion movement of the electrolyte and excellent electrolyte moisture retention capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. can also be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength can be used, and can optionally be used in a single-layer or multi-layer structure.

[0169] In addition, examples of the electrolyte used in the present invention include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.

[0170] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0171] As the organic solvent, any solvent that can serve as a medium through which ions involved in the electrochemical reaction of the battery can move may be used without particular limitation. Specifically, the organic solvent includes ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); Alcohol solvents such as ethyl alcohol, isopropyl alcohol, etc.; nitriles such as R-CN (wherein R is a C2 to C20 linear, branched, or cyclic hydrocarbon group, which may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, carbonate solvents are preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferable.In this case, the performance of the electrolyte may be improved when the cyclic carbonate and the chain carbonate are mixed and used in a volume ratio of about 1:1 to about 1:9.

[0172] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2. LiCl, LiI, or LiB(C2O4)2. It is preferable that the concentration of the lithium salt be used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.

[0173] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 to 5 wt% based on the total weight of the electrolyte.

[0174] As described above, a lithium secondary battery including a cathode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention, and is therefore useful in portable devices such as mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0175] Accordingly, according to another embodiment of the present invention, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same are provided.

[0176] The above battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0177] There is no particular limitation on the external shape of the lithium secondary battery of the present invention, but it may be a cylindrical shape using a can, a square shape, a pouch shape, or a coin shape.

[0178] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but can also be preferably used as a unit battery in a medium- to large-sized battery module including a plurality of battery cells.

[0179]

[0180] Example

[0181] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.

[0182]

[0183] Example 1

[0184] Positive electrode active material precursor [Composition: Ni 0.95 Co 0.03 Mn 0.02 (OH)2, average particle size (D) 50 ) 10.0 ㎛] and LiOH as a lithium raw material were mixed in a molar ratio of 1:1.05, and a plastic product was manufactured by first firing at a temperature of 850°C for 6 hours under an oxygen atmosphere, and the plastic product was then manufactured with an average particle diameter (D 50 ) was pulverized to 5.0 ㎛, and then fired a second time at 750°C for 9 hours in an oxygen atmosphere to produce a fired product. Thereafter, 2 mol% of Co(OH)2 was mixed into the fired product, and heat-treated at 700°C for 6 hours to produce a lithium transition metal oxide in the form of single particles.

[0185]

[0186] Example 2

[0187] Positive electrode active material precursor [Composition: Ni 0.86 Co 0.05 Mn 0.09 (OH)2, average particle size (D) 50 ) 10.0 ㎛] and LiOH as a lithium raw material were mixed in a molar ratio of 1:1.05, and a plastic product was manufactured by first firing at a temperature of 870℃ for 6 hours under an oxygen atmosphere, and the plastic product was then manufactured with an average particle diameter (D 50 ) was pulverized to 4.0 ㎛, and then fired a second time at 780°C for 9 hours in an oxygen atmosphere to produce a fired product. Thereafter, 2 mol% of Co(OH)2 was mixed into the fired product, and heat-treated at 700°C for 6 hours to produce a lithium transition metal oxide in the form of single particles.

[0188]

[0189] Example 3

[0190] Positive electrode active material precursor [Composition: Ni 0.83 Co 0.05 Mn 0.12 (OH)2, average particle size (D) 50) 10.0 ㎛] and LiOH as a lithium raw material were mixed in a molar ratio of 1:1.05, and a plastic product was manufactured by first firing at a temperature of 890℃ for 6 hours under an oxygen atmosphere, and the plastic product was then manufactured with an average particle diameter (D 50 ) After grinding to 4.0 ㎛, the product was manufactured by secondary firing at 800℃ for 9 hours in an oxygen atmosphere. Afterwards, 2 mol% of Co(OH)2 was mixed into the product and heat-treated at 700℃ for 6 hours to manufacture a lithium transition metal oxide in the form of single particles.

[0191]

[0192] Example 4

[0193] Positive electrode active material precursor [Composition: Ni 0.6 Co 0.1 Mn 0.3 (OH)2, average particle size (D) 50 ) 4 ㎛] and LiOH as a lithium raw material were mixed in a molar ratio of 1:1.05, and the first firing was performed at a temperature of 970°C for 9 hours in an oxygen atmosphere to manufacture a plastic product, and the plastic product was then subjected to an average particle diameter (D 50 ) was pulverized to 4 ㎛, and then fired a second time at 900°C for 9 hours in an oxygen atmosphere to produce a fired product. Thereafter, 3 mol% of Co(OH)2 was mixed into the fired product, and heat-treated at 790°C for 6 hours to produce a lithium transition metal oxide in the form of single particles.

[0194]

[0195] Comparative Example 1

[0196] Positive electrode active material precursor [Composition: Ni 0.95 Co 0.03 Mn 0.02 (OH)2, average particle size (D) 50 ) 5.0 ㎛] and LiOH as a lithium raw material were mixed in a molar ratio of 1:1.07, and a plastic product was manufactured by first firing at a temperature of 850°C for 6 hours under an oxygen atmosphere, and the plastic product was then manufactured with an average particle diameter (D 50) was pulverized to 5.0 ㎛, and then fired a second time at 750°C for 9 hours in an oxygen atmosphere to produce a fired product. Thereafter, 2 mol% of Co(OH)2 was mixed into the fired product, and heat-treated at 700°C for 6 hours to produce a lithium transition metal oxide in the form of single particles.

[0197]

[0198] Comparative Example 2

[0199] Positive electrode active material precursor [Composition: Ni 0.86 Co 0.05 Mn 0.09 (OH)2, average particle size (D) 50 ) 4.0 ㎛] and LiOH as a lithium raw material were mixed in a molar ratio of 1:1.07, and a plastic product was manufactured by first firing at a temperature of 900°C for 9 hours under an oxygen atmosphere, and the plastic product was then subjected to an average particle diameter (D 50 ) was pulverized to 4.0 ㎛, and then fired a second time at 780°C for 9 hours in an oxygen atmosphere to produce a fired product. Thereafter, 2 mol% of Co(OH)2 was mixed into the fired product, and heat-treated at 700°C for 6 hours to produce a lithium transition metal oxide in the form of single particles.

[0200]

[0201] Comparative Example 3

[0202] Positive electrode active material precursor [Composition: Ni 0.83 Co 0.05 Mn 0.12 (OH)2, average particle size (D) 50 ) 6.0 ㎛] and LiOH as a lithium raw material were mixed in a molar ratio of 1:1.07, and a plastic product was manufactured by first firing at a temperature of 910℃ for 9 hours under an oxygen atmosphere, and the plastic product was then subjected to an average particle diameter (D 50) After grinding to 4.0 ㎛, the product was manufactured by secondary firing at 800℃ for 9 hours in an oxygen atmosphere. Afterwards, 2 mol% of Co(OH)2 was mixed into the product and heat-treated at 700℃ for 6 hours to manufacture a lithium transition metal oxide in the form of single particles.

[0203]

[0204] Comparative Example 4

[0205] Positive electrode active material precursor [Composition: Ni 0.95 Co 0.03 Mn 0.02 (OH)2, average particle size (D) 50 ) 5.0 ㎛] and LiOH as a lithium raw material were mixed in a molar ratio of 1:1.03, and a plastic product was manufactured by first firing at a temperature of 850°C for 6 hours under an oxygen atmosphere, and the plastic product was then manufactured with an average particle diameter (D 50 ) After grinding to 5.0 ㎛, lithium transition metal oxide in the form of single particles was manufactured by secondary calcination at a temperature of 750℃ for 9 hours in an oxygen atmosphere.

[0206]

[0207] Comparative Example 5

[0208] Positive electrode active material precursor [Composition: Ni 0.95 Co 0.03 Mn 0.02 (OH)2, average particle size (D) 50 ) 10.0 ㎛] and LiOH as a lithium raw material were mixed in a molar ratio of 1:1.03, and a plastic product was manufactured by first firing at a temperature of 830°C for 9 hours under an oxygen atmosphere, and the plastic product was then subjected to an average particle diameter (D 50 ) After grinding to 5.0 ㎛, lithium transition metal oxide in the form of single particles was manufactured by secondary calcination at a temperature of 750℃ for 9 hours in an oxygen atmosphere.

[0209]

[0210] Experimental Example 1: Analysis of positive electrode active material

[0211] Each of the powder-type single-particle type positive electrode active materials manufactured in Examples 1 to 4 and Comparative Examples 1 to 5 was subjected to Ar ion milling for 2 hours using an ion milling system (JBOL, IB19520CCP) (acceleration voltage: 6 kV) to prepare cross-sectional samples.

[0212] 1) For each cross-sectional sample of the powder-type single-particle positive electrode active material, an EBSD band contrast map was created using a field emission scanning microscope (SEM, JEOL JSM-7900F with Oxford symmetry EBSD detector) (acceleration voltage: 20 kV). AztecCrystal from OXFORD Instruments was used as the image processing-EBSD quantification analysis software.

[0213] 2) For each cross-section sample of the powder-type single-particle positive electrode active material, the cross-section of the positive electrode was measured and analyzed using a field emission scanning microscope (SEM, JEOL JSM-7900F with Oxford symmetry EBSD detector) (acceleration voltage: 20 kV). EBSD IPF maps were created using AztecCrystal from OXFORD Instruments as the image processing-EBSD quantification analysis software.

[0214] 3) SEM photographs were taken of the cross-sectional surface of a powder-type single-particle cathode active material sample using a scanning electron microscope (SEM, JEOL JSM-7900F).

[0215]

[0216] Experimental Example 2: Measurement of the boundary length

[0217] (1) Calculation of boundary length using EBSD IPF map

[0218] Using the EBSD IPF map, the boundary was detected using the ImageJ program to obtain a boundary image, and the length of the boundary surface measured from the EBSD IPF map was calculated.

[0219] (2) Calculation of boundary length using EBSD band contrast map

[0220] The length of the boundary surface was calculated using the EBSD band contrast map in the same manner as in (1) above.

[0221] (3) Using the SEM image, the inside and outside of the particle were segmented in the same manner as in (1) above to obtain a boundary image, and the length of the SEM outer boundary surface was calculated.

[0222]

[0223] Fig. 1 shows an SEM photograph, an EBSD band contrast map, an EBSD IPF map, and an IPF interface for the positive electrode active material of Example 1, and Fig. 2 shows an SEM photograph, an EBSD band contrast map, an EBSD IPF map, and an IPF interface for the positive electrode active material of Comparative Example 4, respectively.

[0224] Referring to Fig. 1, the positive electrode active material of Example 1 has a boundary formed inside the positive electrode active material particles that is not observed in the positive electrode SEM image of Comparative Example 4, and in addition, a boundary line that was not observed in the EBSD IPF map is additionally observed. In this way, the boundary observed in the EBSD BC map but not in the SEM corresponds to a strong boundary formed by the collapse of the layered structure of the NiO layer, and the boundary observed only in the EBSD IPF map corresponds to a weak boundary in which only the atomic arrangement is different and the crystallinity is not collapsed.

[0225] Referring to Fig. 2, no boundary surface was observed inside the particle of the positive electrode active material of Comparative Example 4 in the SEM photograph, EBSD BC map, and EBSD IPF map, and accordingly, it was confirmed that neither a strong boundary nor a weak boundary was formed inside the particle of the positive electrode active material of Comparative Example 4.

[0226]

[0227] Experimental Example 3: Electrochemical Characteristics Evaluation

[0228] Manufacturing of positive and half-cells

[0229] Using the positive electrode active material manufactured in Example 1, a composition for forming a positive electrode active material layer was manufactured by adding carbon black (Denka, DenkaBlack) as a conductive material and PVdF (Kureha, KF1300) as a binder to a solvent (Daejung Chemicals, N-methylpyrrolidone (NMP)) at a weight ratio of 97.5:1:1.5 (positive electrode active material:conductive material:binder).

[0230] The composition for forming a positive electrode active material layer manufactured as described above was coated on one side of an aluminum foil current collector having a thickness of 12 μm, and dried at 135°C for 3 hours to form a positive electrode active material layer. Subsequently, the positive electrode active material layer was rolled using a roll pressing method, and after rolling, a positive electrode having a porosity of 24% in the positive electrode active material layer was manufactured.

[0231] Instead of the positive electrode active material manufactured in Example 1, positive electrodes were manufactured in the same manner as described above using the positive electrode active materials of Examples 2 to 4 and Comparative Examples 1 to 5, respectively.

[0232] A half-cell was manufactured using lithium metal as an anode together with the above-manufactured anode.

[0233]

[0234] Electrochemical property evaluation

[0235] The coin half-cells manufactured above were charged at 25°C with a constant current (CC) of 0.2 C until the voltage reached 4.25 V, then charged with a constant voltage (CV) until the charge current reached 0.05 C (cut-off current), and the charge capacity was measured. After leaving the cells for 20 minutes, they were discharged with a constant current (CC) of 0.2 C until the voltage reached 2.5 V, and the discharge capacity of the first cycle was measured.

[0236] The cell that completed one cycle was transferred to a 45℃ chamber and charge / discharge was repeated at 0.33 C for 50 cycles. The discharge capacity at the 50th cycle was measured and the capacity retention rate was evaluated by calculating the discharge capacity at the 50th cycle compared to the discharge capacity at the first cycle.

[0237]

[0238] IPF Boundary / BC BoundaryInner Boundary / Outer BoundaryCharge Capacity (mAh / g)Discharge Capacity (mAh / g)50 Cycle Life (%)Example 11.10.2234.4208.495.4Example 21.30.1231.3206.395.2Example 31.30.3228.1203.596.3Example 41.20.3216.4197.296.8Comparative Example 12.31.3235.2209.191.2Comparative Example 22.11232.1207.090.8Comparative Example 31.70.8228.7203.991.6Comparative Example 41.00227.5201.293.2Comparative Example 51.00231.5202.192.5

[0239] Referring to Table 1 above, it can be confirmed that the positive electrode active materials of Examples 1 to 4 exhibit improved life characteristics by showing a higher 50-cycle life compared to the positive electrode active materials of Comparative Examples 1 to 5.

Claims

1. A cathode active material comprising a lithium transition metal oxide in the form of a single particle, The lithium transition metal oxide in the form of a single particle includes an external boundary forming the outer surface of the particle and an internal boundary formed within the particle, and satisfies the following equation 1: [Formula 1] 0 < length of inner boundary / length of outer boundary < 0.4 The length of the inner boundary is the length of the boundary measured from the electron backscatter diffraction (EBSD)-IPF map for the lithium transition metal oxide particle minus the length of the boundary measured from the EBSD band contrast map, and the length of the outer boundary is the length of the outer boundary of the transition metal oxide particle measured through SEM image segmentation, wherein the positive electrode active material.

2. In paragraph 1, The lithium transition metal oxide in the form of a single particle is a cathode active material that additionally satisfies the following formula 2. [Formula 2] Length of boundary measured from EBSD IPF map / Length of boundary measured from EBSD band contrast map ≤ 1.4 3. In paragraph 1, The lithium transition metal oxide in the form of a single particle is a cathode active material that additionally satisfies the following formula 3. [Formula 3] 0 ≤ (length of inner boundary / length of outer boundary) - (length of boundary measured by length of inner boundary / EBSD band contrast) ≤ 1 4. In paragraph 1, The length of the interface measured from the electron backscatter diffraction (EBSD)-IPF map includes the length of a weak interface in which only the atomic arrangement is different and the crystallinity is not collapsed, and the length of a strong interface formed by the collapse of the layered structure, which is included in the lithium transition metal oxide particle in the form of a single particle.

5. In paragraph 1, A cathode active material, wherein the length of the boundary surface measured from the EBSD band contrast map includes the length of the boundary surface formed by the collapse of the layered structure contained in the lithium transition metal oxide particles in the single particle form.

6. In paragraph 1, The lithium transition metal oxide in the form of a single particle is a cathode active material comprising 2 to 50 single crystal particles.

7. In paragraph 1, The above lithium transition metal oxide is a cathode active material that is a lithium composite transition metal oxide containing nickel, cobalt, and manganese.

8. In paragraph 1, The above lithium transition metal oxide is a positive electrode active material which is a lithium composite transition metal oxide represented by the following chemical formula 1: [Chemical Formula 1] Li a Ni b Co c Mr d M 1 e O2 In the above chemical formula 1, M 1 is at least one selected from the group consisting of Al, Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, Sn, Y, Zn, F, P and S, and 0.9≤a≤1.1, 0.6≤b<1, 0 <c<0.4, 0<d<0.4, 0≤e<0.1, b+c+d+e=1이다.

9. In paragraph 1, The above lithium transition metal oxide is a positive electrode active material which is a lithium composite transition metal oxide represented by the following chemical formula 2: [Chemical Formula 2] Li a Ni b Co c Mr d O2 In the above chemical formula 2, 0.9≤a≤1.1, 0.6≤b<1, 0 <c<0.4, 0<d<0.4, b+c+d=1이다.

10. In paragraph 1, The average particle diameter (D) of the lithium transition metal oxide in the form of single particles is 50 ) further comprises a second lithium transition metal oxide in the form of small single particles, A positive electrode active material having a bimodal particle size distribution.

11. In claim 10, The above second lithium transition metal oxide is a positive electrode active material which is a lithium composite transition metal oxide represented by the following chemical formula 3: [Chemical Formula 3] Li a3 Ni b3 Co c3 Mr d3 M 3 e3 O2 In the above chemical formula 3, M 3 is at least one selected from the group consisting of Al, Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, Sn, Y, Zn, F, P and S, and 0.9≤a3≤1.1, 0.6≤b3<1, 0 <c3<0.4, 0<d3<0.4, 0≤e3<0.1, b3+c3+d3+e3=1이다.

12. In claim 10, A cathode active material in which the weight ratio of the above lithium transition metal oxide and the above second lithium transition metal oxide is 1 to 9:

1.

13. In claim 10, Press density is 3.50g / cm 2 3.90g / cm 2 A positive electrode active material.

14. A positive electrode comprising a positive electrode active material according to any one of claims 1 to 13.

15. A lithium secondary battery comprising a positive electrode according to Article 14.

Citation Information

Patent Citations

  • Cathode active material for lithium ion secondary batteries, method for manufacturing the same, and lithium ion secondary batteries including the same

    KR102084689B1

  • Positive electrode sheet for rechargeable battery, rechargeable battery, battery module, battery pack, and device

    EP4071846A1

  • Cathode active materials for lithium batteries, Methodof preparing thereof and lithium secondary batteriescomprising same

    KR1020070097923A

  • Display device and controlling method thereof

    KR1020240157450A

  • Method for hardware resource provisioning optimizating and online service providing method thereof

    KR102844423B1