Cathode active material, preparation method therefor, and cathode and lithium secondary battery which comprise same

The development of a single-particle lithium composite transition metal oxide with specific structural and compositional features addresses the thermal and cost issues of LiCoO2, enhancing the energy density and lifespan of lithium secondary batteries, making them suitable for high-capacity applications like electric vehicles.

WO2024248563A1PCT designated stage expired Publication Date: 2024-12-05LG CHEM LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/007558
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-06-03
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Lithium secondary batteries face challenges with the thermal stability and cost of LiCoO2 as a positive electrode active material, leading to limitations in their use for high-capacity and long-life applications, particularly in electric vehicles, due to the material's instability and high cost.

Method used

A positive electrode active material composed of a single-particle type lithium composite transition metal oxide with specific structural and compositional characteristics, including disk-shaped primary particles and a composition represented by LiNi_xCo_yM_zO_2, where M can include Mn or Al, is developed, enhancing thermal stability and lifespan while maintaining high energy density.

Benefits of technology

The new active material improves the energy volume density and lifespan characteristics of lithium secondary batteries, reducing the risk of internal short circuits and ignition, and is more cost-effective than traditional materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024007558_05122024_PF_FP_ABST
    Figure KR2024007558_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a cathode active material capable of improving the performance of a lithium secondary battery, and to a cathode active material, a preparation method therefor, and a cathode and a lithium secondary battery which comprise same, the cathode active material comprising: a discrete-particle-type first lithium composite transition metal oxide; and, optionally, a discrete-particle-type second lithium composite transition metal oxide, wherein: the single-particle-type first lithium composite transition metal oxide is composed of 30 or fewer disk-type primary particles; the disk-type primary particles observed in an SEM image of the surface or cross-section of the cathode active material have interior angles on the same side are 150° to 210° and the aspect ratio (major axis / minor axis) is 1.5 or more, when, with respect to two boundary lines of primary particles, that are within an angle of 45° or less in the long diameter direction, an imaginary tangent line with the maximum number of contact points is drawn and one imaginary line crossing the two tangent lines is drawn; and the cathode active material comprises 20-100 vol% of the first lithium composite transition metal oxide on the basis of the total volume of the cathode active material.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode active material, method for producing the same, and positive electrode and lithium secondary battery containing the same

[0001] Cross-citation with related applications

[0002] This application claims the benefit of priority from Korean Patent Application No. 10-2023-0071872, filed June 2, 2023, the entire contents of which are incorporated herein by reference.

[0003] Technology field

[0004] The present invention relates to a positive electrode active material, a method for producing the same, and a positive electrode and a lithium secondary battery including the same.

[0005]

[0006] As technological development and demand for mobile devices increase, the demand for secondary batteries as an energy source is rapidly increasing. Among these secondary batteries, lithium secondary batteries, which boast high energy density and voltage, long cycle life, and low self-discharge rates, are commercialized and widely used.

[0007] Lithium-transition metal composite oxides are used as cathode active materials in lithium secondary batteries. Among these, lithium-cobalt composite metal oxides such as LiCoO2, which exhibit high operating voltage and excellent capacity characteristics, are primarily used. However, LiCoO2 suffers from poor thermal properties due to crystal structure instability following delithiation. Furthermore, its high cost limits its mass use as a power source in fields such as electric vehicles.

[0008] As a material to replace the above LiCoO2, lithium manganese composite metal oxides (such as LiMnO2 or LiMn2O4), lithium iron phosphate compounds (such as LiFePO4), or lithium nickel composite metal oxides (such as LiNiO2) have been developed. Among these, research and development on lithium nickel composite metal oxides, which have a high reversible capacity of about 200 mAh / g and make it easy to implement large-capacity batteries, is being actively studied. However, LiNiO2 has inferior thermal stability compared to LiCoO2, and there was a problem that the positive electrode active material itself decomposed when an internal short circuit occurred due to external pressure in a charged state, causing the battery to rupture and catch fire. Accordingly, as a method to improve the low thermal stability of LiNiO2 while maintaining the excellent reversible capacity, lithium composite transition metal oxides in which some of the Ni was replaced with Co, Mn, or Al were developed.

[0009] In the case of lithium ion batteries that use lithium composite transition metal oxides, especially lithium composite transition metal oxides containing a high nickel (Ni-rich) content, as cathode active materials, the capacity, high output, and whether gas is generated at high temperatures of the battery are affected not only by the chemical properties of the cathode active material, such as the composition of the cathode active material, the content of impurities, and the content of lithium byproducts present on the surface, but also by the physical properties, such as the size, surface area, density, and shape of the cathode active material particles. Therefore, when using a lithium composite transition metal oxide containing a high nickel (Ni-rich) content as a cathode active material, efforts are required to appropriately balance the capacity characteristics, output characteristics, high-temperature characteristics, and life characteristics of the battery.

[0010] Therefore, there is a need for the development of a cathode active material that can exhibit excellent energy volume density and lifespan characteristics.

[0011]

[0012] [Prior Art Literature]

[0013] [Patent Document]

[0014] (Patent Document 1) KR 2021-0117212 A

[0015]

[0016] The object of the present invention is to provide a positive electrode active material capable of exhibiting excellent energy volume density and lifespan characteristics.

[0017] Another object of the present invention is to provide a manufacturing method for manufacturing the positive electrode active material.

[0018] Another object of the present invention is to provide a positive electrode including the positive electrode active material and a lithium secondary battery including the same.

[0019]

[0020] In order to solve the above problem, the present invention provides a positive electrode active material, a method for producing the positive electrode active material, a positive electrode for a lithium secondary battery including the positive electrode active material, and a lithium secondary battery.

[0021]

[0022] (1) The present invention comprises a single particle type first lithium composite transition metal oxide; And optionally, a single-particle type second lithium composite transition metal oxide; A positive electrode active material comprising a first lithium composite transition metal oxide, wherein the single-particle type first lithium composite transition metal oxide is composed of 30 or fewer disk-type primary particles, and the disk-type primary particles are such that, when two imaginary tangent lines having the largest number of contact points are drawn for two boundaries of the primary particles existing within an angle of 45° or less with respect to the major axis direction in a SEM image of the surface or cross-section of the positive electrode active material, and one imaginary line crossing the two tangent lines is drawn, the coaxial angle is 150° or more and 210° or less, and the aspect ratio (major axis / minor axis) is 1.5 or more, and the positive electrode active material comprises the first lithium composite transition metal oxide in an amount of 20% by volume or more and 100% by volume or less based on the total volume of the positive electrode active material.

[0023] (2) The present invention provides a positive electrode active material according to (1), wherein the positive electrode active material comprises the first lithium composite transition metal oxide in an amount of 20% by volume or more and 70% by volume or less relative to the total volume of the positive electrode active material.

[0024] (3) The present invention provides a positive electrode active material in (1) or (2) above, wherein the first lithium composite transition metal oxide has an aspect ratio (long axis / short axis) of 1.5 or more and 10 or less.

[0025] (4) In the present invention, in the above (1) to (3), when the volume value is calculated from the following equation 1 for each of the primary particles observed from the SEM image of the surface or cross-section of the positive electrode active material, the single particle degree (V) corresponding to the volume at the point where the cumulative volume distribution of the primary particles is 50% 50 ) is 1.2 ㎛ 3 Provides a positive electrode active material that is ideal.

[0026] [Formula 1]

[0027]

[0028] In the above equation 1, radius is the radius of the surface or cross-section of the primary particle assuming that the surface or cross-section of the primary particle observed from the SEM image (measurement magnification 3,000 times) is circular.

[0029] (5) In any one of the above (1) to (4), the first lithium composite transition metal oxide is a first lithium composite transition metal oxide having an average radius (R) at a point where the radius of each primary particle observed from a SEM image (measurement magnification 3,000 times) of the surface or cross-section of the positive electrode active material is 50% of the cumulative radius distribution of the particles. 50) is 1 ㎛ or more and 15 ㎛ or less, and the radius is the radius of the surface or cross-section of the primary particle when the surface or cross-section of the primary particle is assumed to be circular.

[0030] (6) The present invention provides a positive electrode active material in any one of the above (1) to (5), wherein the first lithium composite transition metal oxide has a composition represented by the following chemical formula 1.

[0031] [Chemical Formula 1]

[0032] Li a Ni x Co y M 1 z M 2 1-x-y-z O2

[0033] In the above chemical formula 1, M 1 is at least one selected from the group consisting of Mn and Al, and M 2 is at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf, and 0.9≤a≤1.3, 0.6≤x<1.0, 0 <y<0.4, 0<z<0.4, 0≤1-x-y-z<0.4이다.

[0034] (7) The present invention provides a positive electrode comprising a positive electrode active material according to any one of (1) to (6).

[0035] (8) The present invention provides a lithium secondary battery including a positive electrode according to (7) above.

[0036] (9) The present invention provides a method for producing a positive electrode active material, comprising the steps of: (A) mixing a positive electrode active material precursor and a first lithium-containing raw material, the internal density of which is lower than that of the external density, to produce a mixture; and (B) firing the mixture for the first time at a temperature of 800°C or more and 950°C or less to produce a first fired product; wherein the internal area is a region corresponding to 50% or less of a radius from the center of the positive electrode active material precursor to the outermost direction, the positive electrode active material is in the form of a single particle composed of 30 or fewer primary particles, and includes a first lithium composite transition metal oxide in the form of a disk, and the first lithium composite transition metal oxide is included in an amount of 20% by volume or more and 100% by volume or less based on the total volume of the positive electrode active material.

[0037] (10) The present invention provides a method for manufacturing a positive electrode active material, which further includes a step (B1) of crushing the primary sintered product immediately after the step (B) in the above (9).

[0038] (11) The present invention provides a method for manufacturing a positive electrode active material, which further includes, in the above (9) or (10), a step of, after the step (B), (C) mixing a second lithium-containing raw material into the first fired product and then performing a second firing at a temperature of 680°C or higher and 850°C or lower to manufacture a second fired product.

[0039] (12) The present invention provides a method for manufacturing a positive electrode active material, which further includes a step (C1) of crushing the secondary sintered product immediately after the step (C) in the above (11).

[0040] (13) The present invention, in any one of (9) to (12), wherein the positive electrode active material precursor comprises: (S1) a step of introducing a transition metal-containing solution and an ammonium ion-containing solution into a reactor including a stirring device at a constant flow rate, introducing a basic aqueous solution, and stirring while maintaining a stirring speed to prepare a mixed solution for seeds; (S2) a step of introducing the transition metal-containing solution, the ammonium ion-containing solution, and the basic aqueous solution into the mixed solution for seeds, and stirring while gradually reducing the stirring speed to prepare a mixed solution for particle growth; And (S3) a step of preparing a mixed solution for a positive electrode active material precursor by adding the transition metal-containing solution to the mixed solution for particle growth at an increased flow rate compared to step (S2), gradually adding the ammonium ion-containing solution at an increased flow rate, adding the basic aqueous solution, and stirring while maintaining the stirring speed; wherein the basic aqueous solution is added so that the pH of the mixed solution for seeds is kept constant, so that the pH of the mixed solution for particle growth is gradually reduced, and so that the pH of the mixed solution for the positive electrode active material precursor is kept constant. A method for preparing a positive electrode active material is provided.

[0041] (14) The present invention provides a method for producing a positive electrode active material, wherein, in the above (13), the basic aqueous solution is introduced so that the pH of the mixed solution for particle growth is gradually reduced from pH 12 to 13 to pH 11.2 to 12.6.

[0042] (15) The present invention provides a method for producing a positive electrode active material, wherein in the step (13) or (14), the stirring speed is gradually reduced from 700 rpm to 900 rpm to 500 rpm to 650 rpm in the step (S2).

[0043] (16) The present invention provides a method for manufacturing a cathode active material, wherein in any one of (13) to (15), the step (S3) introduces the transition metal-containing solution at a flow rate of 1.2 to 1.4 times that of the step (S2), and the step (S3) introduces the ammonium ion-containing solution at a flow rate that is gradually increased to be 20 to 45% that of the transition metal-containing solution.

[0044]

[0045] The cathode active material according to the present invention is a cathode active material comprising a single-particle first lithium composite transition metal oxide; and optionally a single-particle second lithium composite transition metal oxide;

[0046] The above single particle type first lithium composite transition metal oxide is composed of 30 or fewer disk type primary particles, and the disk type primary particles are such that, when two imaginary tangent lines having the greatest number of contact points are drawn for each of the primary particles existing within an angle of 45° or less with respect to the major axis direction in the SEM image of the surface or cross section of the positive electrode active material, and one imaginary line crossing the two tangent lines is drawn, the coaxial internal angle is 150° or more and 210° or less, and the aspect ratio (major axis / minor axis) is 1.5 or more, and the positive electrode active material contains the first lithium composite transition metal oxide in an amount of 20% by volume or more and 100% by volume or less based on the total volume of the positive electrode active material, and thus the positive electrode and lithium secondary battery including the positive electrode active material of the present invention can exhibit excellent energy volume density and lifespan characteristics.

[0047]

[0048] Fig. 1(A) is an SEM image of a cross-section of a positive electrode active material precursor manufactured in Manufacturing Example 1, Fig. 1(B) is an SEM image of a cross-section of a positive electrode active material precursor manufactured in Manufacturing Example 2, Fig. 1(C) is an SEM image of a cross-section of a positive electrode active material precursor manufactured in Manufacturing Example 3, Fig. 1(D) is an SEM image of a cross-section of a positive electrode active material precursor manufactured in Manufacturing Example 4, Fig. 1(E) is an SEM image of a cross-section of a positive electrode active material precursor manufactured in Comparative Manufacturing Example 1, and Fig. 1(F) is an SEM image of a cross-section of a positive electrode active material precursor manufactured in Comparative Manufacturing Example 2.

[0049] Figure 2 is a segmentation image of the positive electrode active material manufactured in Example 1.

[0050] Figure 3 is a segmentation image of the positive electrode active material manufactured in Example 2.

[0051] Figure 4 is a segmentation image of the positive electrode active material manufactured in Example 3.

[0052] Figure 5 is a segmentation image of the positive electrode active material manufactured in Example 5.

[0053] Figure 6 is a segmentation image of the positive electrode active material manufactured in Comparative Example 1.

[0054] Figure 7 is a segmentation image of the positive electrode active material manufactured in Comparative Example 2.

[0055]

[0056] Hereinafter, the present invention will be described in more detail.

[0057] Terms or words used in this specification and claims should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical idea of ​​the present invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best way.

[0058]

[0059] In the present invention, the term "primary particle" refers to the smallest particle unit that can be distinguished as a single lump when observing the cross-section of a positive electrode active material through a scanning electron microscope (SEM), and may be composed of one crystal grain or multiple crystal grains. The "crystal grain" or "grain region" refers to a region in which atoms within a sample are continuously and periodically arranged in one direction. The crystal grain can be analyzed using an electron backscatter diffraction (ESBD) analyzer.

[0060]

[0061] In the present invention, the term "secondary particle" refers to a secondary structure formed by the aggregation of multiple primary particles. The average particle diameter of the secondary particles can be measured using a particle size analyzer.

[0062]

[0063] In the present invention, the term 'single particle form' may be used instead of the term 'single particle type', and means a form that is in contrast to a form of secondary particles formed by agglomeration of hundreds of primary particles manufactured by a conventional method. In addition, the term 'single particle type positive electrode active material' or 'single particle type lithium composite transition metal oxide' in the present invention is a concept that is in contrast to a form of secondary particles formed by agglomeration of hundreds of primary particles manufactured by a conventional method, and may be a single particle composed of one primary particle, or may be a form of secondary particles in which 2 or more, or 5 or more, and 10 or less, 15 or less, 20 or less, 25 or less, or 30 or less primary particles are aggregated.

[0064]

[0065] In the present invention, the term 'volume ratio (volume %)' is a value obtained by calculating the volume value from the following Equation 1 for each of the primary particles observed from the SEM image (measurement magnification 3,000 times) of the surface or cross-section of the positive electrode active material, obtaining the total volume value of the positive electrode active material and the total volume value of the first lithium composite transition metal oxide, then dividing the total volume value of the first lithium composite transition metal oxide by the total volume value of the positive electrode active material, and multiplying by 100.

[0066] [Formula 1]

[0067]

[0068] In the above equation 1,

[0069] The radius is the radius of the surface or cross-section of the primary particle assuming that the surface or cross-section of the primary particle observed from the above SEM image (measurement magnification 3,000 times) is circular.

[0070]

[0071] In the present invention, the term 'average particle diameter (D 50 )' means the particle size at the 50% point of the volume cumulative distribution according to particle size. The above average particle size is calculated by dispersing the powder to be measured in a dispersion medium, introducing it into a commercially available laser diffraction particle size measuring device (e.g. QUANTA FEG 250, FEI) and measuring the difference in diffraction pattern according to particle size when the particles pass through the laser beam, thereby calculating the particle size distribution, and calculating the particle diameter at the point where it becomes 50% of the volume cumulative distribution according to particle size in the measuring device, thereby obtaining D 50 can be measured.

[0072]

[0073] In the present invention, the term 'segmentation image' refers to an image segmented into individual positive electrode active material particles, and can be obtained by a method including a first step of analyzing positive electrode active material powder with a scanning electron microscope to obtain an SEM image, and a second step of removing edges of individual positive electrode active material particles from the SEM image using deep learning or computer image processing techniques, then detecting contours of individual positive electrode active material particles, and using the same to obtain an image segmented into individual positive electrode active material particles. Specifically, the segmentation image can be obtained through the methods described in KR 10-2022-0048191 A and KR 10-2022-0048192 A.

[0074]

[0075] In the present invention, the term 'longitudinal length' refers to the length of the longest line segment when a line is drawn passing through two points of the primary particle boundary in a primary particle observed from an SEM image of the surface or cross-section of a positive electrode active material.

[0076]

[0077] In the present invention, the term 'aspect ratio' refers to a method of first selecting the shape of one primary particle to be measured from an SEM image of the particle, and then measuring the aspect ratio, i.e., the ratio of the major axis to the minor axis, using an eigenvector.

[0078]

[0079] In the present invention, the term 'major axis' means an axis that passes through the center of gravity of a primary particle and at which axial dispersion is maximum, and 'minor axis' means an axis that passes through the center of gravity of a primary particle and at which axial dispersion is minimum.

[0080]

[0081] positive electrode active material

[0082] Hereinafter, the positive electrode active material according to the present invention will be described.

[0083]

[0084] The present inventors have developed a single particle type first lithium composite transition metal oxide; And optionally, a single-particle type second lithium composite transition metal oxide; a cathode active material comprising a single-particle type first lithium composite transition metal oxide, wherein the single-particle type first lithium composite transition metal oxide is composed of 30 or fewer disk-type primary particles, and the disk-type primary particles are such that, in the primary particles observed from an SEM image of the surface or cross-section of the cathode active material, when two imaginary tangent lines having the largest number of contact points are drawn for each of the two boundaries of the primary particles existing within an angle of 45° or less with respect to the major axis direction, and when one imaginary line crossing the two tangent lines is drawn, the same side internal angle is 150° or more and 210° or less, and the aspect ratio (major axis / minor axis) is 1.5 or more, and when the cathode active material contains the first lithium composite transition metal oxide in an amount of 20% by volume or more and 100% by volume or less relative to the total volume of the cathode active material, the cathode active material does not react well with the electrolyte, so that the cathode The present invention was completed by finding that the lifespan characteristics can be improved while maintaining the energy density of a battery containing an active material.

[0085]

[0086] The first lithium composite transition metal oxide is in the form of a single particle composed of 30 or fewer primary particles. That is, the first lithium composite transition metal oxide is in the form of a single particle or a single particle in which 2 or more but 30 or fewer primary particles are aggregated. The single particle form is distinguished from a secondary particle in which more than 30 primary particles are aggregated. When the first lithium composite transition metal oxide has a single particle form, the stability is excellent, so that even when a positive electrode active material including the same is rolled, the positive electrode active material does not break or crack, and thus a side reaction between the positive electrode active material and the electrolyte can be reduced. As a result, the durability against volume changes during charge and discharge of the battery is improved, and the life characteristics can be improved. When the first lithium composite transition metal oxide is in the form of a secondary particle, the positive electrode active material including the same is broken or cracked, and there is a problem of poor life characteristics due to a side reaction between the positive electrode active material and the electrolyte.

[0087]

[0088] Meanwhile, the single-particle first lithium composite transition metal oxide is composed of 30 or fewer disk-shaped primary particles, and the disk-shaped primary particles are such that, in the primary particles observed from an SEM image of the surface or cross-section of the positive electrode active material, when two virtual tangent lines having the greatest number of contact points are drawn for each of the two boundaries of the primary particles existing within an angle of 45° or less with respect to the major axis direction, and one virtual line crossing the two tangent lines is drawn, the coplanar internal angle is 150° or more and 210° or less, and the aspect ratio (major axis / minor axis) is 1.5 or more.

[0089] And, the above disk-shaped primary particle may have a crystal size of the (003) plane of 380 nm or more and 480 nm or less in X-ray diffraction spectrum analysis, specifically 400 nm or more and 450 nm or less, and more specifically 400 nm or more and 440 nm or less.

[0090] Disc-shaped primary particles have the advantage of low reactivity with the electrolyte, so that the positive electrode active material does not experience rapid irreversible damage even after repeated charge and discharge cycles. On the other hand, if the single-particle first lithium composite transition metal oxide is not a disc-shaped primary particle, the irreversible damage to the positive electrode active material increases rapidly with repeated charge and discharge cycles, resulting in poor cycle life characteristics.

[0091]

[0092] The positive electrode active material according to the present invention comprises the first lithium composite transition metal oxide in an amount of 20% by volume or more and 100% by volume or less relative to the total volume of the positive electrode active material. Specifically, the positive electrode active material may comprise the first lithium composite transition metal oxide in an amount of 20% by volume or more, or 25% by volume or more, and 70% by volume or less, 75% by volume or less, 80% by volume or less, 85% by volume or less, 90% by volume or less, 95% by volume or less, or 100% by volume or less relative to the total volume of the positive electrode active material. When the content of the first lithium composite transition metal oxide satisfies the above range, the positive electrode active material may exhibit excellent performance in terms of initial discharge capacity and excellent life characteristics.

[0093]

[0094] According to one embodiment of the present invention, the first lithium composite transition metal oxide may have an aspect ratio (major axis / minor axis) of 1.5 or more and 10 or less. Specifically, it may be 1.5 or more, 1.51 or more, 1.52 or more, 1.53 or more, 1.54 or more, 1.55 or more, 1.56 or more, 1.57 or more, 1.58 or more, 1.59 or more, 1.6 or more, 1.7 or more, 1.8 or more, 1.9 or more, 2.0 or more, 2.5 or more, 3.0 or more, or 4.0 or more, and may be 5.0 or less, 6.0 or less, 7.0 or less, 8.0 or less, 9.0 or less, or 10.0 or less. When the aspect ratio of the first lithium composite transition metal oxide is within the above range, a positive electrode active material including disk-shaped particles can be manufactured, thereby having the effect of improving life characteristics.

[0095]

[0096] According to one embodiment of the present invention, when the volume value is calculated from the following equation 1 for each of the primary particles observed from the SEM image of the surface or cross-section of the positive electrode active material, the single particle degree (V) corresponding to the volume at the point where the cumulative volume distribution of the primary particles is 50% 50 ) is 1.2 ㎛ 3 It could be something like this.

[0097] [Formula 1]

[0098]

[0099] In the above equation 1,

[0100] The radius is the radius of the surface or cross-section of the primary particle assuming that the surface or cross-section of the primary particle observed from the above SEM image (measurement magnification 3,000 times) is circular.

[0101] Specifically, the single particle magnetization (V 50 ) is 1.2 ㎛ 3 Above, 1.3 ㎛ 3Above, 1.4 ㎛ 3 Above, 1.5 ㎛ 3 Above, 1.6 ㎛ 3 Above, 1.7 ㎛ 3 Above, 1.8 ㎛ 3 Above, 1.9 ㎛ 3 Above, 2.0 ㎛ 3 or 2.1 ㎛ 3 It may be more than 3.6 ㎛ 3 Below, 4.0 ㎛ 3 or less, or 5.0 ㎛ 3 It may be as follows. The above single particle magnetization (V 50 ) is within the above range, there is an effect of improving energy density and life characteristics.

[0102]

[0103] According to one embodiment of the present invention, when the radius of each primary particle observed from the SEM image (measurement magnification 3,000 times) of the surface or cross-section of the positive electrode active material is calculated, the average radius (R) at the point where the cumulative radius distribution of the particles is 50% 50 ) is 1 ㎛ or more and 15 ㎛ or less, and the radius may be the radius of the surface or cross-section of the primary particle when the surface or cross-section of the primary particle is assumed to be circular. Specifically, the average radius (R 50 ) may be 1 ㎛ or more, or 2 ㎛ or more, or may be 10 ㎛ or less, 12 ㎛ or less, or 15 ㎛ or less.

[0104]

[0105] According to one embodiment of the present invention, the positive electrode active material may optionally further include a single-particle second lithium composite transition metal oxide.

[0106] The second lithium composite transition metal oxide is in the form of a single particle composed of 30 or fewer primary particles. That is, the second lithium composite transition metal oxide is in the form of a single particle or a single particle in which 2 to 30 primary particles are aggregated. The single particle form is distinguished from a secondary particle in which more than 30 primary particles are aggregated. When the second lithium composite transition metal oxide has a single particle form, the stability is excellent, so that even when a positive electrode active material including the same is rolled, the positive electrode active material does not break or crack, and thus side reactions between the positive electrode active material and the electrolyte can be reduced. As a result, durability against volume changes during charge and discharge of the battery is improved, and thus life characteristics can be improved. When the second lithium composite transition metal oxide is in the form of a secondary particle, the positive electrode active material including the same is broken or cracked, and there is a problem of poor life characteristics due to a side reaction between the positive electrode active material and the electrolyte.

[0107] In addition, the second lithium composite transition metal oxide does not include a primary particle in the shape of a disk. For example, it may be a polyhedron, sphere, ellipse, cylinder, particle shape, or a similar shape, but does not satisfy the definition of a disk shape.

[0108] The second lithium composite transition metal oxide may have superior reactivity compared to the first lithium composite transition metal oxide, and by including the second lithium composite transition metal oxide, the cathode active material of the present invention may exhibit superior performance in terms of initial discharge capacity.

[0109] In addition, the second lithium composite transition metal oxide has an average particle diameter (D 50 ) may be 1 ㎛ or more, 2 ㎛ or more, 3 ㎛ or more, or 4 ㎛ or more, and may be 5 ㎛ or less, 10 ㎛ or less, or 15 ㎛ or less.

[0110]

[0111] According to one embodiment of the present invention, the first lithium composite transition metal oxide may have a composition represented by the following chemical formula 1.

[0112] [Chemical Formula 1]

[0113] Li a Ni x Co y M 1 z M 2 1-x-y-z O2

[0114] In the above chemical formula 1,

[0115] M 1 is at least one selected from the group consisting of Mn and Al,

[0116] M 2 is at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf,

[0117] 0.9≤a≤1.3, 0.6≤x<1.0, 0 <y<0.4, 0<z<0.4, 0≤1-x-y-z<0.4이다.

[0118] Above M 1 is at least one selected from the group consisting of Mn and Al, and the M 2 is a doping element, specifically, M 2 It may be at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf. The above M 2 Although not necessarily included, if included in an appropriate amount, the particle shape of the positive electrode active material can be improved and the stability of the crystal structure can be enhanced.

[0119] Meanwhile, the above a may be 0.9 or more, 0.95 or more, or 1 or more, and may be 1.1 or less, 1.2 or less, or 1.3 or less. When a satisfies the above range, high capacity characteristics and high energy density per unit volume can be realized.

[0120] The above x is the molar fraction of nickel (Ni) among the total metals excluding lithium in the first lithium composite transition metal oxide, and may be 0.6 or more, 0.65 or more, 0.7 or more, 0.75 or more, or 0.8 or more, and may be 0.9 or less, or less than 1. When x is within the above range, the capacity characteristics of the positive electrode active material can be improved.

[0121] The above y is the mole fraction of cobalt (Co) among the total metals excluding lithium in the first lithium composite transition metal oxide, and may be greater than 0, 0.01 or more, 0.02 or more, or 0.03 or more, and may be 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, 0.1 or less, 0.2 or less, 0.3 or less, or less than 0.4. When y satisfies the above range, structural stability may increase, and decomposition reaction of the electrolyte may be relatively reduced.

[0122] The above z is M of all metals except lithium in the first lithium composite transition metal oxide. 1 The molar fraction of z may be greater than 0, greater than 0.01, greater than 0.02, greater than 0.03, greater than 0.05, greater than 0.06, greater than 0.07, or greater than 0.08, and may be less than or equal to 0.09, less than or equal to 0.1, less than or equal to 0.2, less than or equal to 0.3, or less than 0.4. When z satisfies the above range, the structural stability increases, and the decomposition reaction of the electrolyte may be relatively reduced.

[0123]

[0124] According to one embodiment of the present invention, the second lithium composite transition metal oxide may have a composition represented by the following chemical formula 2.

[0125] [Chemical Formula 2]

[0126] Li a1 Ni x1 Co y1 M 1' z1 M 2' 1-x1-y1-z1O2

[0127] In the above chemical formula 2,

[0128] M 1' is at least one selected from the group consisting of Mn and Al,

[0129] M 2' is at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf,

[0130] 0.9≤a1≤1.3, 0.6≤x1<1.0, 0 <y1<0.4, 0<z1<0.4, 0≤1-x1-y1-z1<0.4이다.

[0131] Above M 1' is at least one selected from the group consisting of Mn and Al, and the M 2' is a doping element, specifically, M 2' It may be at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf. The above M 2' Although not necessarily included, if included in an appropriate amount, the particle shape of the positive electrode active material can be improved and the stability of the crystal structure can be enhanced.

[0132] Meanwhile, the above a1 may be 0.9 or more, 0.95 or more, or 1 or more, and 1.1 or less, 1.2 or less, or 1.3 or less. When a1 satisfies the above range, high capacity characteristics and high energy density per unit volume can be realized.

[0133] The above x1 is the molar fraction of nickel (Ni) among the total metals excluding lithium in the second lithium composite transition metal oxide, and may be 0.6 or more, 0.65 or more, 0.7 or more, 0.75 or more, or 0.8 or more, and may be 0.9 or less, or less than 1. When x1 is within the above range, the capacity characteristics of the positive electrode active material can be improved.

[0134] The above y1 is the mole fraction of cobalt (Co) among the total metals excluding lithium in the second lithium composite transition metal oxide, and may be greater than 0, 0.01 or more, 0.02 or more, or 0.03 or more, and may be 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, 0.1 or less, 0.2 or less, 0.3 or less, or less than 0.4. When y1 satisfies the above range, structural stability may increase, and the decomposition reaction of the electrolyte may be relatively reduced.

[0135] The above z1 is M of all metals except lithium in the second lithium composite transition metal oxide. 1' The molar fraction of z1 may be greater than 0, greater than 0.01, greater than 0.02, greater than 0.03, greater than 0.05, greater than 0.06, greater than 0.07, or greater than 0.08, and may be less than or equal to 0.09, less than or equal to 0.1, less than or equal to 0.2, less than or equal to 0.3, or less than 0.4. When z1 satisfies the above range, structural stability increases, and the decomposition reaction of the electrolyte may be relatively reduced.

[0136]

[0137] The first lithium composite transition metal oxide and the second lithium composite transition metal oxide may have the same or different compositions. For example, the first lithium composite transition metal oxide may have a nickel molar ratio of 70 mol% or more among all metals excluding lithium, and the second lithium composite transition metal oxide may have a nickel molar ratio of 80 mol% to 95 mol% among all metals excluding lithium.

[0138]

[0139] Meanwhile, the first lithium composite transition metal oxide and the second lithium composite transition metal oxide may further include a coating portion on the surface, if necessary, including one or more elements (hereinafter referred to as “coating elements”) selected from the group consisting of Co, Al, B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La, and Hf. When the coating portion as described above is included, contact between the lithium composite transition metal oxide and the electrolyte is blocked, thereby effectively suppressing gas generation and transition metal elution due to side reactions with the electrolyte.

[0140] The above coating portion can be formed by mixing a raw material including a first lithium composite transition metal oxide or a second lithium composite transition metal oxide and the coating element, and then performing a heat treatment at a temperature of 200°C to 800°C.

[0141]

[0142] Method for manufacturing positive electrode active material

[0143] Hereinafter, a method for manufacturing a positive electrode active material according to the present invention will be described. The method for manufacturing a positive electrode active material according to the present invention is a method for manufacturing the positive electrode active material according to the present invention.

[0144]

[0145] The present invention relates to a method for producing a positive electrode active material, comprising: (A) mixing a positive electrode active material precursor and a first lithium-containing raw material, the internal density of which is lower than that of the external density, to produce a mixture; and (B) firing the mixture for the first time at a temperature of 800°C or more and 950°C or less to produce a first fired product; wherein the internal area is a region corresponding to 50% or less of a radius from the center of the positive electrode active material precursor to the outermost direction, and the positive electrode active material is in the form of a single particle composed of 30 or fewer primary particles and includes a first lithium composite transition metal oxide in the form of a disk, and the first lithium composite transition metal oxide is included in an amount of 20% or more by volume and 100% or less by volume based on the total volume of the positive electrode active material.

[0146]

[0147] According to the present invention described above, the type of raw material, the mixing ratio of raw materials, the firing time, etc. can be appropriately adjusted to manufacture the product.

[0148]

[0149] Hereinafter, each step of the present invention will be described in detail.

[0150]

[0151] (A) Step

[0152] The step (A) includes preparing a mixture by mixing a positive electrode active material precursor and a first lithium-containing raw material, the internal density of which is lower than the external density.

[0153]

[0154] The positive electrode active material precursor has an internal density lower than an external density. Here, the internal area is a region corresponding to 50% or less of the radius from the center of the positive electrode active material precursor to the outermost direction. When the internal density of the precursor is lower than the external density, when mixed with a lithium-containing raw material and then fired, a positive electrode active material including a specific content of disk-shaped primary particles can be manufactured. When the internal density of the positive electrode active material precursor is the same as the external density or the internal density is higher than the external density, there is a problem in that disk-shaped primary particles are not formed to a sufficient degree.

[0155]

[0156] According to one embodiment of the present invention, the positive electrode active material precursor comprises: (S1) a step of introducing a transition metal-containing solution and an ammonium ion-containing solution into a reactor including a stirring device at a constant flow rate, introducing a basic aqueous solution, and stirring while maintaining a stirring speed to prepare a mixed solution for seeds; (S2) a step of introducing the transition metal-containing solution, the ammonium ion-containing solution, and the basic aqueous solution into the mixed solution for seeds, and stirring while gradually reducing the stirring speed to prepare a mixed solution for particle growth; And (S3) a step of introducing the transition metal-containing solution into the particle growth mixture at an increased flow rate compared to step (S2), gradually introducing the ammonium ion-containing solution at an increased flow rate, introducing the basic aqueous solution, and stirring while maintaining the stirring speed to prepare a mixed solution for a positive electrode active material precursor; wherein the basic aqueous solution may be introduced so that the pH of the seed mixture solution is maintained constant, so that the pH of the particle growth mixture solution is gradually reduced, and so that the pH of the positive electrode active material precursor mixture solution is maintained constant. In this case, a precursor of a positive electrode active material having a lower internal density than an external density can be effectively manufactured.

[0157] The above step (S1) may be a seed formation step, the above step (S2) may be a particle internal growth step, and the above step (S3) may be a particle external growth step. If the stirring speed is not gradually reduced in the above step (S2), there is a problem that it is difficult to manufacture a positive electrode active material having a lower internal density than the external density, and if the above transition metal-containing solution is not added to the particle growth mixed solution at an increased flow rate compared to the above step (S2) in the above step (S3), or the above ammonium ion-containing solution is not added at a gradually increased flow rate, there is a problem that it is difficult to increase the external density compared to the internal density.

[0158]

[0159] First, according to one embodiment of the present invention, the basic aqueous solution may be introduced so that the pH of the particle growth mixture solution gradually decreases from pH 12 to 13 to pH 11.2 to 12.6. Specifically, the basic aqueous solution may be introduced so that the pH of the particle growth mixture solution gradually decreases from pH 12 to 12.5 to pH 11.2 to 11.5. The basic aqueous solution may be introduced so that the pH of the particle growth mixture solution gradually decreases by 0.05 to 0.2 per hour. The basic aqueous solution may be introduced so that the pH of the particle growth mixture solution is maintained constant once the pH reaches the target pH.

[0160]

[0161] According to one embodiment of the present invention, the steps (S1) and (S3) may be stirred at a constant stirring speed. In this case, the particles have the effect of growing to a uniform density.

[0162]

[0163] According to one embodiment of the present invention, the step (S2) may be performed by gradually reducing the stirring speed from 700 rpm to 900 rpm to 500 rpm to 650 rpm. Specifically, the step (S2) may be performed by gradually reducing the stirring speed from 700 rpm to 900 rpm to 500 rpm to 650 rpm, or from 750 rpm to 850 rpm to 500 rpm to 600 rpm. The stirring speed may be the stirring speed from the time when the transition metal-containing solution, the ammonium ion-containing solution, and the basic aqueous solution are added to the seed mixture solution until immediately before performing the step (S3). When the stirring speed in the step (S2) is gradually reduced within the above range and stirred, there is an effect of particles growing at a low density.

[0164]

[0165] According to one embodiment of the present invention, the step (S3) may be to introduce the transition metal-containing solution at a flow rate that is 1.2 times or more and 1.4 times or less compared to the step (S2), and to introduce the ammonium ion-containing solution at a flow rate that is gradually increased to have a flow rate that is 20% or more and 45% or less of the transition metal-containing solution. Specifically, the step (S3) may be to introduce the transition metal-containing solution at a flow rate that is 1.2 times or more, or 1.3 times or more, and 1.4 times or less compared to the step (S2), and to introduce the ion-containing solution at a flow rate that is gradually increased to have a flow rate that is 20% or more, or 25% or more, and 35% or less, 40% or less, or 45% or less compared to the transition metal-containing solution. When the flow rates of the transition metal-containing solution and the ammonium ion-containing solution are adjusted within the above ranges, a positive electrode active material precursor having an increased external density can be manufactured.

[0166]

[0167] (B) Step

[0168] Thereafter, the step (B) includes first firing the mixture at a temperature of 800°C or higher and 950°C or lower to manufacture a first fired product.

[0169]

[0170] Specifically, the mixture is first fired at a temperature of 800°C or higher, or 850°C or higher, 900°C or lower, or 950°C or lower to manufacture a first fired product. When the first fired temperature is within the above range, the primary particles of the positive electrode active material precursor can aggregate to manufacture a structurally stable single-particle fired product. When the first fired temperature is lower than 800°C, it may be difficult to manufacture a single-particle fired product, and when it exceeds 950°C, there is a problem in that a structurally unstable fired product with low crystallinity is manufactured.

[0171]

[0172] The above first calcination may be performed under an oxygen atmosphere in order to prevent the lithium composite transition metal oxide from degenerating into a rock salt structure.

[0173] The above primary firing may be performed for 3 hours or more and 12 hours or less. Specifically, the primary firing may be performed for 3 hours or more, 4 hours or more, or 5 hours or more, and 6 hours or less, 9 hours or less, 10 hours or less, 11 hours or less, or 12 hours or less. In this case, the primary particles may be agglomerated and the crystallinity of the primary fired product may be improved.

[0174] The temperature rise rate during the first firing may be 4°C / min to 7°C / min, and specifically 5°C / min to 7°C / min. When the temperature rise rate during the first firing satisfies the above range, the primary particles of the positive electrode active material precursor may aggregate, thereby forming a structurally more stable single-particle first fired product, and the amount of fine particles having a particle size of 1 μm or less in the final positive electrode active material may be minimized.

[0175]

[0176] According to one embodiment of the present invention, immediately after step (B), a step (B1) of crushing the primary sintered product may be further included. In order to prevent the initial resistance from increasing, the primary sintered product may be crushed to have an average particle diameter (D 50 ) may be pulverized to be 3.50㎛ or more and 10.00㎛ or less. The pulverization may be performed using a pin mill, an ACM, a jet mill, etc. Meanwhile, the pin mill may be performed under conditions of 18,000 rpm, the ACM may be performed under conditions of 6,000 rpm for classification and 12,000 rpm for pulverization using a device from Hosokawa, and the jet mill may be performed under conditions of 6 bar for pulverization pressure and 3,500 rpm for grading using a device from ZM solution. In this case, the desired average particle diameter (D 50 ) can be easily obtained.

[0177]

[0178] According to one embodiment of the present invention, after step (B), the method may further include a step (C) of mixing a second lithium-containing raw material into the first fired product and then firing the second product at a temperature of 680°C or higher and 850°C or lower to manufacture a second fired product. Specifically, the method may include mixing a second lithium-containing raw material into the first fired product and then firing the second product at a temperature of 680°C or higher, 700°C or higher, 720°C or higher, 740°C or higher, 760°C or higher, or 780°C or higher, and 800°C or lower, 820°C or lower, or 850°C or lower to manufacture a second fired product.

[0179] At this time, the first fired product may be cooled to room temperature before the second firing. If the second firing temperature is within the above range, lithium is inserted into the rock salt structure that may form on the surface of the first fired product due to the high temperature during the first firing, restoring it to a layered structure, and there is the advantage of reducing lithium byproducts.

[0180] The above secondary calcination may be performed under an oxygen atmosphere in order to prevent the lithium composite transition metal oxide from degenerating into a rock salt structure.

[0181] The above secondary firing may be performed for 3 hours or more and 12 hours or less. Specifically, the above primary firing may be performed for 3 hours or more, 4 hours or more, 5 hours or more, 6 hours or more, 7 hours or more, or 8 hours or more, and 9 hours or less, 10 hours or less, 11 hours or less, or 12 hours or less. In this case, there is an effect of increasing the crystallinity of the internal crystal structure of the positive electrode active material.

[0182] The heating rate during the secondary firing may be 4°C / min to 7°C / min, and specifically 5°C / min to 7°C / min. When the heating rate during the secondary firing satisfies the above range, lithium can be more effectively inserted into the rock salt structure that may be formed on the surface of the primary fired product, thereby restoring the layered structure, further reducing lithium byproducts, and minimizing the content of fine particles with a particle size of 1 μm or less in the positive electrode active material after rolling.

[0183]

[0184] According to one embodiment of the present invention, immediately after step (C), a step (C1) of crushing the secondary sintered product may be further included. In order to prevent the initial resistance from increasing, the secondary sintered product may be crushed to have an average particle diameter (D 50 ) may be pulverized to be 3.50㎛ or more and 10.00㎛ or less. The pulverization may be performed using a pin mill, an ACM, a jet mill, etc. Meanwhile, the pin mill may be performed under conditions of 18,000 rpm, the ACM may be performed under conditions of 6,000 rpm for classification and 12,000 rpm for pulverization using a device from Hosokawa, and the jet mill may be performed under conditions of 6 bar for pulverization pressure and 3,500 rpm for grading using a device from ZM solution. In this case, the desired average particle diameter (D 50 ) can be easily obtained.

[0185]

[0186] According to one embodiment of the present invention, a cathode active material can be manufactured by a process of introducing a lithium-containing raw material in two stages. That is, the lithium-containing raw material is introduced separately before the first firing and before the second firing. In this case, there is an advantage of facilitating recovery into a layered structure as lithium is inserted into a rock salt structure that may be formed on the surface. On the other hand, if the lithium-containing raw material is introduced all at once before the first firing, there is a problem of deterioration in electrochemical performance due to an increase in lithium byproducts. In addition, if the lithium-containing raw material is not introduced in the second firing step, there is a problem of requiring high temperatures and a long time due to a slow reaction rate.

[0187]

[0188] In the case where the lithium-containing raw material is input in two portions, in the step (A), the first lithium-containing raw material may be mixed so that the ratio (M:Li) of the total mole number (M) of the transition metal included in the positive electrode active material precursor and the mole number (Li) of lithium included in the first lithium-containing raw material is 1:0.98 or more, 0.99 or more, or 1.00 or more, and 1.01 or less, 1.02 or less, 1.03 or less, 1.04 or less, or 1.05 or less, and in the step (C), the second lithium-containing raw material may be mixed so that the ratio (M:Li) of the total mole number (M) of the transition metal included in the first sintered product and the mole number (Li) of lithium included in the first sintered product is 1:1.00 or more, 1.01 or more, 1.02 or more, or 1.03 or more, and 1.05 or less, 1.06 or less, 1.07 or less, or 1.08 It can be mixed to be less than, 1.09 or less, or 1.10 or less.

[0189]

[0190] According to one embodiment of the present invention, (D) a step of mixing the secondary sintered product and the cobalt-containing raw material and then performing a heat treatment may be further included. In this case, a coating portion including Co is formed on the secondary sintered product.

[0191]

[0192] According to one embodiment of the present invention, when mixing the secondary sintered product and the cobalt-containing raw material in step (D), an aluminum-containing raw material, a zirconium-containing raw material, or a combination thereof may be further mixed. In this case, the coating portion may further include Al, Zr, or a combination thereof in addition to Co.

[0193]

[0194] According to one embodiment of the present invention, the cobalt-containing coating raw material may be mixed in an amount such that the ratio (B / A) of the number of moles of cobalt (B) contained in the cobalt-containing raw material to the total number of moles (A) of metals excluding lithium contained in the secondary fired product is 0.01 to 0.03. In this case, there is an advantage in that lithium byproducts can be controlled in a cathode active material manufacturing process that does not include a washing process.

[0195] According to one embodiment of the present invention, the cobalt-containing raw material may be at least one selected from Co(OH)2, Co3O4, CoO, (CH3CO2)2Co, CoCl2, and CoSO4·xH2O, and specifically, may be Co(OH)2.

[0196] According to one embodiment of the present invention, the aluminum-containing raw material may be mixed in an amount of 0.03 to 0.10 parts by weight per 100 parts by weight of the secondary fired product. In this case, structural stability can be secured, thereby improving service life, resistance, and gas generation.

[0197] According to one embodiment of the present invention, the aluminum-containing raw material may be at least one selected from Al(OH)3, Al2(SO4)3·xH2O, Al2O3, Al(NO3)3·9H2O, AlCl3, and C2H5O4Al, and specifically, may be Al(OH)3.

[0198] According to one embodiment of the present invention, the zirconium-containing raw material is Zr(OH)4, ZrO2, Zr(NO3)4, ZrCl4, ZrS2, Zr(SO4)2 and C8H 12 It can be one or more types selected from O8Zr.

[0199]

[0200] According to one embodiment of the present invention, the heat treatment may be performed under an oxygen atmosphere to prevent the lithium composite transition metal oxide from degenerating into a rock salt structure.

[0201]

[0202] According to the present invention, the heat treatment may be performed at a temperature of 600°C or higher, 610°C or higher, 620°C or higher, 630°C or higher, 640°C or higher, or 650°C or higher, and 720°C or lower, 740°C or lower, 760°C or lower, 780°C or lower, or 800°C or lower, and then lowering the temperature to 450°C or higher and 550°C or lower, and then heat treating at a temperature of 450°C or higher, 460°C or higher, 470°C or higher, 480°C or higher, and 520°C or lower, 530°C or lower, 540°C or lower, or 550°C or lower. That is, after the first heat treatment is performed at a temperature of 600℃ or higher and 800℃ or lower in one firing profile, the second heat treatment may be performed at a temperature of 450℃ or higher and 550℃ or lower.

[0203]

[0204] According to one embodiment of the present invention, the heat treatment may be performed for a time of 1 hour or more, 2 hours or more, 3 hours or more, and 8 hours or less, 9 hours or less, or 10 hours or less in order to increase the crystallinity of the coating portion.

[0205]

[0206] The above transition metal-containing solution may include at least one selected from the group consisting of Ni, Co, and Mn, and specifically may include Ni, Co, and Mn.

[0207] Additionally, the transition metal-containing solution may include additional metal-containing raw materials, such as Al, Ti, W, B, F, P, Mg, Fe, Cr, V, Cu, Ca, Zn, Zr, Nb. It may be an oxide, hydroxide, oxyhydroxide, carbonate, sulfate, halide, sulfide, acetate, nitrate, carboxylate or a combination thereof containing one or more elements selected from the group consisting of Mo, Sr, Sb, Bi, Si, Cr, Hf, Ta, La, Ba, Ce, Sn, Y and S, and specifically, ZnO, Al2O3, Al(OH)3, AlSO4, AlCl3, Al-isopropoxide, AlNO3, TiO2, WO3, AlF, H2BO3, HBO2, H3BO3, H2B4O7, B2O3, C6H5B(OH)2, (C6H5O)3B, [(CH3(CH2)3O)3B, C3H9B3O6, (C3H7O3)B, Li3WO4, (NH4) 10 W 12 O 41 ㆍExamples include, but are not limited to, 5H2O, NH4H2PO4, etc.

[0208]

[0209] anode

[0210] In addition, the present invention provides a positive electrode for a lithium secondary battery, comprising a positive electrode active material layer including the positive electrode active material. Specifically, the positive electrode comprises a positive electrode current collector, and a positive electrode active material layer positioned on at least one surface of the positive electrode current collector, the positive electrode active material layer including the positive electrode active material. The positive electrode active material layer may have a porosity of 10% to 30% by volume, specifically 15% to 30% by volume, and more specifically 18% to 27% by volume.

[0211] The positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 μm, and fine unevenness may be formed on the surface of the positive electrode current collector to increase the adhesive strength of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.

[0212]

[0213] The above-described positive electrode active material layer may include a conductive material and a binder together with the positive electrode active material according to the present invention described above.

[0214] The above positive electrode active material may be included in an amount of 80 to 99 wt%, more specifically 85 to 98 wt%, based on the total weight of the positive electrode active material layer. When included in the above content range, excellent capacity characteristics may be exhibited.

[0215] The conductive material is used to provide conductivity to the electrode, and in the battery to be formed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One of these may be used alone or a mixture of two or more may be used. The conductive material may be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.

[0216] The above binder serves to improve the adhesion between positive electrode active material particles and the adhesive strength between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluoroelastomer, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof. The binder may be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.

[0217]

[0218] The above positive electrode can be manufactured according to a conventional positive electrode manufacturing method, except that the positive electrode active material according to the present invention is used. Specifically, the positive electrode active material layer forming composition, which is manufactured by dissolving or dispersing the above positive electrode active material and optionally a binder, a conductive agent, and additives as needed in a solvent, is applied onto a positive electrode current collector, followed by drying and rolling. At this time, the types and contents of the positive electrode active material, binder, and conductive agent are as described above.

[0219]

[0220] The solvent may be a solvent generally used in the relevant technical field, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water. One of these may be used alone or a mixture of two or more thereof may be used. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, taking into account the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the positive electrode.

[0221]

[0222] Additionally, in another method, the positive electrode may be manufactured by casting the composition for forming the positive electrode active material layer on a separate support, and then laminating the resulting film on a positive electrode current collector by peeling it off from the support.

[0223]

[0224] lithium secondary battery

[0225] In addition, the present invention can manufacture an electrochemical device including the positive electrode. The electrochemical device may be a battery, a capacitor, or the like, and more specifically, a lithium secondary battery.

[0226] The lithium secondary battery specifically includes a positive electrode, a negative electrode positioned opposite the positive electrode, and a separator and electrolyte interposed between the positive electrode and the negative electrode. Since the positive electrode is the same as described above, a detailed description thereof will be omitted, and only the remaining components will be described in detail below.

[0227] In addition, the lithium secondary battery may optionally further include a battery container that houses the electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0228]

[0229] In the above lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.

[0230] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 ㎛ to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.

[0231]

[0232] The above negative electrode active material layer optionally includes a binder and a conductive material together with the negative electrode active material.

[0233] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; SiO β (0<β<2), SnO2, vanadium oxide, lithium vanadium oxide, and other metal oxides capable of doping and dedoping lithium; or composites containing the above metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include natural graphite or artificial graphite in the form of amorphous, plate-like, flaky, spherical, or fiber-like forms, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes.

[0234] The above negative electrode active material may be included in an amount of 80 to 99 parts by weight based on 100 parts by weight of the total weight of the negative electrode active material layer.

[0235]

[0236] The above binder is a component that assists in bonding between the conductive material, the active material, and the current collector, and is typically added in an amount of 0.1 to 10 parts by weight based on 100 parts by weight of the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.

[0237] The conductive agent is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10 parts by weight or less, preferably 5 parts by weight or less, based on 100 parts by weight of the total weight of the negative electrode active material layer. The conductive agent is not particularly limited as long as it has conductivity and does not cause a chemical change in the battery, and examples thereof include graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber or metal fiber; metal powders such as fluorocarbon, aluminum, and nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0238]

[0239] For example, the negative electrode active material layer can be manufactured by applying and drying a negative electrode composite prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material in a solvent, on a negative electrode current collector, or by casting the negative electrode composite on a separate support and then laminating the resulting film on a negative electrode current collector by peeling it off from the support.

[0240]

[0241] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used in lithium secondary batteries can be used without special restrictions, and in particular, one having low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. can also be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength can be used, and can optionally be used in a single-layer or multi-layer structure.

[0242]

[0243] In addition, examples of the electrolyte used in the present invention include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.

[0244] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0245] As the organic solvent, any solvent that can serve as a medium through which ions involved in the electrochemical reaction of the battery can move may be used without particular limitation. Specifically, the organic solvent includes ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); Alcohol solvents such as ethyl alcohol, isopropyl alcohol, etc.; nitriles such as R-CN (R is a linear, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes, etc. can be used. Among these, carbonate solvents are preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferable.In this case, the performance of the electrolyte may be improved when the cyclic carbonate and the chain carbonate are mixed and used in a volume ratio of about 1:1 to about 1:9.

[0246]

[0247] The above lithium salt can be used without any special limitation as long as it is a compound that can provide lithium ions used in a lithium secondary battery. Specifically, the above lithium salt is LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2) 2. LiCl, LiI, or LiB(C2O4)2 can be used. It is recommended that the concentration of the lithium salt be within the range of 0.1 to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.

[0248]

[0249] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 to 5 parts by weight based on 100 parts by weight of the total weight of the electrolyte.

[0250]

[0251] As described above, a lithium secondary battery including a cathode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and lifespan characteristics, and is therefore useful in portable devices such as mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0252] Accordingly, according to another embodiment of the present invention, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same are provided.

[0253] The above battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0254] There is no particular limitation on the external shape of the lithium secondary battery of the present invention, but it may be a cylindrical shape using a can, a square shape, a pouch shape, or a coin shape.

[0255] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but can also be preferably used as a unit battery in a medium- to large-sized battery module including a plurality of battery cells.

[0256]

[0257] Hereinafter, the present invention will be described in detail with reference to examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention should not be construed as being limited to the examples described below. The examples of the present invention are provided to more fully explain the present invention to those of ordinary skill in the art.

[0258]

[0259] Manufacturing example

[0260] Manufacturing Example 1

[0261] NiSO4, CoSO4, and MnSO4 were mixed in water in amounts such that the molar ratio of nickel:cobalt:manganese was 88.5:3.5:8 to prepare a 2.4 M transition metal-containing solution, and a 25 wt% NaOH aqueous solution and a 9 wt% NH4OH aqueous solution were prepared.

[0262] 5 L of deionized water was placed in a 30 L reactor including a stirring device, and nitrogen gas was purged into the reactor at a rate of 10 L / min to remove dissolved oxygen in the water and create a non-oxidizing atmosphere inside the reactor. Then, NaOH aqueous solution and NH4OH aqueous solution were added to adjust the solution inside the reactor to pH 12.0, and the initial conditions were set such that the temperature of the reactor was 54°C and the stirring speed was 750 rpm.

[0263] A mixture solution for seeds was prepared by adding a transition metal-containing solution at a flow rate of 25 mL / min and an NH4OH aqueous solution at a flow rate of 8 mL / min to the reactor, adding an NaOH aqueous solution, and stirring for 1 hour while maintaining the stirring speed at 750 rpm. At this time, the NaOH aqueous solution was added so that the pH of the mixture solution for seeds was maintained at a constant pH of 12.

[0264] After that, while adding a transition metal-containing solution at a flow rate of 25 mL / min and an NH4OH aqueous solution at a flow rate of 8 mL / min to the seed mixture solution, an NaOH aqueous solution was added, and the stirring speed was gradually reduced by 50 rpm per hour from 750 rpm to 600 rpm, and stirred for 3 hours, and then the stirring speed was maintained at 600 rpm for 17 hours, thereby producing a particle growth mixture solution having a particle size of 2.5 μm. At this time, the NaOH aqueous solution was added so that the pH of the particle growth mixture solution gradually decreased by 0.2 per hour from pH 12 to pH 11.4, and then added so that the pH of the particle growth mixture solution was constantly maintained at pH 11.4.

[0265] Then, a transition metal-containing solution was injected into the above-mentioned particle growth mixture solution at a flow rate of 32.5 ml / min, and a NaOH aqueous solution was injected at a flow rate that was gradually increased from 8 mL / min to 11.375 ml / min, and the stirring speed was maintained at 600 rpm and stirred for 72 hours to obtain the average particle diameter (D) of the positive electrode active material precursor in the solution. 50 ) was prepared as a mixed solution for a positive electrode active material precursor having a particle size of 4.0 μm. At this time, the transition metal-containing solution was introduced at a flow rate 1.3 times greater than the flow rate introduced when preparing the mixed solution for particle growth, the NH4OH aqueous solution was introduced at a flow rate gradually increased to 35% of the flow rate of the transition metal-containing solution, and the NaOH aqueous solution was introduced so that the pH of the mixed solution for the positive electrode active material precursor was constantly maintained at pH 11.4.

[0266] The above mixed solution for the positive electrode active material precursor was filtered and dried to produce a positive electrode active material precursor having a lower internal density than the external density.

[0267]

[0268] Manufacturing Example 2

[0269] NiSO4, CoSO4, and MnSO4 were mixed in water in amounts such that the molar ratio of nickel:cobalt:manganese was 88.5:3.5:8 to prepare a 2.4 M transition metal-containing solution, and a 25 wt% NaOH aqueous solution and a 9 wt% NH4OH aqueous solution were prepared.

[0270] 5 L of deionized water was placed in a 30 L reactor including a stirring device, and nitrogen gas was purged into the reactor at a rate of 10 L / min to remove dissolved oxygen in the water and create a non-oxidizing atmosphere inside the reactor. Thereafter, NaOH aqueous solution and NH4OH aqueous solution were added to adjust the solution inside the reactor to pH 12.0, and the initial conditions were set such that the temperature of the reactor was 54°C and the stirring speed was 800 rpm.

[0271] A mixture solution for seeds was prepared by adding a transition metal-containing solution at a flow rate of 25 mL / min and an NH4OH aqueous solution at a flow rate of 8 mL / min to the reactor, adding an NaOH aqueous solution, and stirring for 1 hour while maintaining the stirring speed at 800 rpm. At this time, the NaOH aqueous solution was added so that the pH of the mixture solution for seeds was maintained at a constant pH of 12.

[0272] After that, while adding a transition metal-containing solution at a flow rate of 25 mL / min and an NH4OH aqueous solution at a flow rate of 8 mL / min to the seed mixture solution, an NaOH aqueous solution was added, and the stirring speed was gradually reduced by 40 rpm per hour from 800 rpm to 600 rpm, and stirred for 5 hours, and then the stirring speed was maintained at 600 rpm for 25 hours, thereby producing a particle growth mixture solution having a particle size of 2.0 μm. At this time, the NaOH aqueous solution was added so that the pH of the particle growth mixture solution gradually decreased by 0.12 per hour from pH 12 to pH 11.4, and then added so that the pH of the particle growth mixture solution was constantly maintained at pH 11.4.

[0273] Then, a transition metal-containing solution was injected into the above-mentioned particle growth mixture solution at a flow rate of 32.5 ml / min, and a NaOH aqueous solution was injected at a flow rate that was gradually increased from 8 ml / min to 10 ml / min, and the stirring speed was maintained at 600 rpm and stirred for 60 hours to obtain the average particle diameter (D) of the positive electrode active material precursor in the solution. 50 ) was prepared as a mixed solution for a positive electrode active material precursor having a particle size of 4.0 μm. At this time, the transition metal-containing solution was introduced at a flow rate 1.3 times greater than the flow rate introduced when preparing the particle growth mixed solution, the NH4OH aqueous solution was introduced at a flow rate gradually increased to 30% of the flow rate of the transition metal-containing solution, and the NaOH aqueous solution was introduced so that the pH of the mixed solution for the positive electrode active material precursor was constantly maintained at pH 11.4.

[0274] The above mixed solution for the positive electrode active material precursor was filtered and dried to produce a positive electrode active material precursor having a lower internal density than the external density.

[0275]

[0276] Manufacturing Example 3

[0277] NiSO4, CoSO4, and MnSO4 were mixed in water in amounts such that the molar ratio of nickel:cobalt:manganese was 88.5:3.5:8 to prepare a 2.4 M transition metal-containing solution, and a 25 wt% NaOH aqueous solution and a 9 wt% NH4OH aqueous solution were prepared.

[0278] 5 L of deionized water was placed in a 30 L reactor including a stirring device, and nitrogen gas was purged into the reactor at a rate of 10 L / min to remove dissolved oxygen in the water and create a non-oxidizing atmosphere inside the reactor. Then, NaOH aqueous solution and NH4OH aqueous solution were added to adjust the solution inside the reactor to pH 12.0, and the initial conditions were set such that the temperature of the reactor was 54°C and the stirring speed was 850 rpm.

[0279] A mixture solution for seeds was prepared by adding a transition metal-containing solution at a flow rate of 25 mL / min and an NH4OH aqueous solution at a flow rate of 8 mL / min to the reactor, adding an NaOH aqueous solution, and stirring for 1 hour while maintaining the stirring speed at 850 rpm. At this time, the NaOH aqueous solution was added so that the pH of the mixture solution for seeds was maintained at a constant pH of 12.

[0280] After that, while adding a transition metal-containing solution at a flow rate of 25 mL / min and an NH4OH aqueous solution at a flow rate of 8 mL / min to the seed mixture solution, an NaOH aqueous solution was added, and the stirring speed was gradually reduced by 40 rpm per hour from 850 rpm to 600 rpm, and the stirring was performed for about 6.25 hours, and the stirring was performed while maintaining the stirring speed at 600 rpm for 23.75 hours, thereby producing a particle growth mixture solution having a particle size of 1.5 μm in the solution. At this time, the NaOH aqueous solution was added so that the pH of the particle growth mixture solution gradually decreased by 0.1 per hour from pH 12 to pH 11.4, and then the pH of the particle growth mixture solution was added so that the pH was constantly maintained at pH 11.4.

[0281] Then, a transition metal-containing solution was injected into the above-mentioned particle growth mixture solution at a flow rate of 32.5 ml / min, and a NaOH aqueous solution was injected at a flow rate that was gradually increased from 8 mL / min to 8.125 ml / min, and the stirring speed was maintained at 600 rpm and stirred for 50 hours to obtain the average particle diameter (D) of the positive electrode active material precursor in the solution. 50 ) was prepared as a mixed solution for a positive electrode active material precursor having a particle size of 4.0 μm. At this time, the transition metal-containing solution was introduced at a flow rate 1.3 times greater than the flow rate introduced when preparing the mixed solution for particle growth, the NH4OH aqueous solution was introduced at a flow rate gradually increased to 25% of the flow rate of the transition metal-containing solution, and the NaOH aqueous solution was introduced so that the pH of the mixed solution for the positive electrode active material precursor was constantly maintained at pH 11.4.

[0282] The above mixed solution for the positive electrode active material precursor was filtered and dried to produce a positive electrode active material precursor having a lower internal density than the external density.

[0283]

[0284] Manufacturing Example 4

[0285] NiSO4, CoSO4, and MnSO4 were mixed in water in amounts such that the molar ratio of nickel:cobalt:manganese was 88.5:3.5:8 to prepare a 2.4 M transition metal-containing solution, and a 25 wt% NaOH aqueous solution and a 9 wt% NH4OH aqueous solution were prepared.

[0286] 5 L of deionized water was placed in a 30 L reactor including a stirring device, and nitrogen gas was purged into the reactor at a rate of 10 L / min to remove dissolved oxygen in the water and create a non-oxidizing atmosphere inside the reactor. Thereafter, NaOH aqueous solution and NH4OH aqueous solution were added to adjust the pH of the solution inside the reactor to 12.0, and the initial conditions were set such that the temperature of the reactor was 54°C and the stirring speed was 700 rpm.

[0287] A solution containing a transition metal was initially introduced into the reactor at a flow rate of 35 mL / min for 10 seconds, then continuously introduced at a flow rate of 25 mL / min, and while introducing an aqueous NH4OH solution at a flow rate of 8 mL / min, an aqueous NaOH solution was introduced, and the mixture was stirred for 1 hour at a stirring speed of 700 rpm to prepare a mixed solution for seeds. At this time, the aqueous NaOH solution was introduced so that the pH of the mixed solution for seeds was constantly maintained at pH 12.

[0288] After that, while adding a transition metal-containing solution at a flow rate of 25 mL / min and an NH4OH aqueous solution at a flow rate of 8 mL / min to the seed mixture solution, an NaOH aqueous solution was added, and the stirring speed was gradually reduced by 30 rpm per hour from 700 rpm to 600 rpm, and the mixture was stirred for 3.3 hours, and the stirring speed was maintained at 600 rpm for 16.7 hours, thereby producing a particle growth mixture solution having a particle size of 3.0 μm. At this time, the NaOH aqueous solution was added so that the pH of the particle growth mixture solution gradually decreased by 0.2 per hour from pH 12 to pH 11.4, and then the pH of the particle growth mixture solution was added so that the pH was constantly maintained at pH 11.4.

[0289] Then, a transition metal-containing solution was injected into the above-mentioned particle growth mixture solution at a flow rate of 32.5 ml / min, and a NaOH aqueous solution was injected at a flow rate that was gradually increased from 8 ml / min to 13 ml / min, and the stirring speed was maintained at 600 rpm and stirred for 72 hours to obtain the average particle diameter (D) of the positive electrode active material precursor in the solution. 50 ) was prepared as a mixed solution for a positive electrode active material precursor having a particle size of 4.0 μm. At this time, the transition metal-containing solution was introduced at a flow rate 1.3 times greater than the flow rate introduced when preparing the particle growth mixed solution, the NH4OH aqueous solution was introduced at a flow rate gradually increased to 40% of the flow rate of the transition metal-containing solution, and the NaOH aqueous solution was introduced so that the pH of the mixed solution for the positive electrode active material precursor was constantly maintained at pH 11.4.

[0290] The above mixed solution for the positive electrode active material precursor was filtered and dried to produce a positive electrode active material precursor having a lower internal density than the external density.

[0291]

[0292] Comparative Manufacturing Example 1

[0293] NiSO4, CoSO4, and MnSO4 were mixed in water in amounts such that the molar ratio of nickel:cobalt:manganese was 88.5:3.5:8 to prepare a 2.4 M transition metal-containing solution, and a 25 wt% NaOH aqueous solution and a 9 wt% NH4OH aqueous solution were prepared.

[0294] 5 L of deionized water was placed in a 30 L reactor including a stirring device, and nitrogen gas was purged into the reactor at a rate of 10 L / min to remove dissolved oxygen in the water and create a non-oxidizing atmosphere inside the reactor. Then, NaOH aqueous solution and NH4OH aqueous solution were added to adjust the solution inside the reactor to pH 12.0, and the initial conditions were set such that the temperature of the reactor was 54°C and the stirring speed was 750 rpm.

[0295] A solution containing a transition metal was injected into the reactor at a flow rate of 25 mL / min, an aqueous NH4OH solution was injected at a flow rate of 8 mL / min, and an aqueous NaOH solution was injected, and the stirring speed was maintained at 750 rpm and stirred for 100 hours to determine the average particle diameter (D) of the positive electrode active material precursor in the solution. 50 ) was prepared as a mixed solution for a positive electrode active material precursor having a particle size of 4.0 μm. At this time, the NaOH aqueous solution was added so that the pH of the mixed solution for the positive electrode active material precursor was maintained at a constant pH of 12.

[0296] The above mixed solution for the positive electrode active material precursor was filtered and dried to produce a positive electrode active material precursor having the same internal and external density.

[0297]

[0298] Comparative Manufacturing Example 2

[0299] NiSO4, CoSO4, and MnSO4 were mixed in water in amounts such that the molar ratio of nickel:cobalt:manganese was 88.5:3.5:8 to prepare a 2.4 M transition metal-containing solution, and a 25 wt% NaOH aqueous solution and a 9 wt% NH4OH aqueous solution were prepared.

[0300] 5 L of deionized water was placed in a 30 L reactor including a stirring device, and nitrogen gas was purged into the reactor at a rate of 10 L / min to remove dissolved oxygen in the water and create a non-oxidizing atmosphere inside the reactor. Then, NaOH aqueous solution and NH4OH aqueous solution were added to adjust the solution inside the reactor to pH 12.0, and the initial conditions were set such that the temperature of the reactor was 54°C and the stirring speed was 950 rpm.

[0301] A solution containing a transition metal was introduced into the reactor at a flow rate of 25 mL / min, an aqueous NH4OH solution was introduced at a flow rate of 8 mL / min, and an aqueous NaOH solution was introduced. The mixture solution for seeds was prepared by stirring for 1 hour while maintaining the stirring speed at 950 rpm. At this time, the aqueous NaOH solution was introduced so that the pH of the mixed solution for seeds was maintained at a constant pH of 12.2.

[0302] After that, while adding a transition metal-containing solution at a flow rate of 25 mL / min and an NH4OH aqueous solution at a flow rate of 8 mL / min to the seed mixture solution, adding an NaOH aqueous solution, gradually reducing the stirring speed by 70 rpm per hour until the stirring speed becomes 400 rpm from 950 rpm, stirring for 7.9 hours, and maintaining the stirring speed at 400 rpm, stirring for 42.1 hours, the average particle diameter (D) of the seeds in the solution 50) was prepared as a mixed solution for particle growth having a particle size of 1.0 μm. At this time, the NaOH aqueous solution was added so that the pH of the mixed solution for particle growth gradually decreased by 0.1 per hour from pH 12.2 to pH 11.4, and then added so that the pH of the mixed solution for particle growth was constantly maintained at pH 11.4.

[0303] Then, a transition metal-containing solution was added to the above-mentioned particle growth mixture solution at a flow rate of 37.5 ml / min, and a NaOH aqueous solution was added at a flow rate gradually reduced from 8 mL / min to 7.5 ml / min, and the stirring speed was maintained at 400 rpm and stirred for 35 hours to obtain the average particle diameter (D) of the positive electrode active material precursor in the solution. 50 ) was prepared as a mixed solution for a positive electrode active material precursor having a particle size of 4.0 μm. At this time, the transition metal-containing solution was introduced at a flow rate 1.5 times greater than the flow rate introduced when preparing the mixed solution for particle growth, the NH4OH aqueous solution was introduced at a flow rate gradually reduced to 20% of the flow rate of the transition metal-containing solution, and the NaOH aqueous solution was introduced so that the pH of the mixed solution for the positive electrode active material precursor was constantly maintained at pH 11.4.

[0304] The above mixed solution for the positive electrode active material precursor was filtered and dried to produce a positive electrode active material precursor having a higher internal density than the external density.

[0305]

[0306] Example 1

[0307] A mixture was prepared by mixing the positive electrode active material precursor manufactured in Manufacturing Example 1 and LiOH in an alumina crucible so that the molar ratio of Li:(Ni+Co+Mn) was 1:1, and the mixture was first fired for 5.5 hours under an oxygen atmosphere at a temperature of 870°C to prepare a first fired product.

[0308] The average particle diameter (D) of the above primary fired product 50 ) is 4.0 ㎛, and the maximum particle diameter (D max ) was pulverized with a jet mill or pin mill to a particle size of 13.0 ㎛, and the pulverized primary calcined product and LiOH were mixed so that the molar ratio of total Li:(Ni+Co+Mn) was 1.03:1, and then secondary calcined for 8 hours at a temperature of 790°C to manufacture a secondary calcined product. The secondary calcined product was pulverized to an average particle size (D 50 ) is 4.0 ㎛, and the maximum particle diameter (D max ) was ground with a jet mill or pin mill to a particle size of 13.0 μm to manufacture a positive electrode active material.

[0309]

[0310] Example 2

[0311] A secondary sintered product (positive electrode active material) was manufactured in the same manner as in Example 1, except that the positive electrode active material precursor manufactured in Manufacturing Example 2 was used instead of the positive electrode active material precursor manufactured in Manufacturing Example 1.

[0312]

[0313] Example 3

[0314] A secondary fired product (positive electrode active material) was manufactured in the same manner as Example 1, except that the positive electrode active material precursor manufactured in Manufacturing Example 3 was used instead of the positive electrode active material precursor manufactured in Manufacturing Example 1.

[0315]

[0316] Example 4

[0317] A secondary sintered product (positive electrode active material) was manufactured in the same manner as Example 1, except that the positive electrode active material precursor manufactured in Manufacturing Example 4 was used instead of the positive electrode active material precursor manufactured in Manufacturing Example 1.

[0318]

[0319] Comparative Example 1

[0320] A secondary fired product (positive electrode active material) was manufactured in the same manner as Example 1, except that the positive electrode active material precursor manufactured in Comparative Manufacturing Example 1 was used instead of the positive electrode active material precursor manufactured in Manufacturing Example 1.

[0321]

[0322] Comparative Example 2

[0323] A secondary fired product (positive electrode active material) was manufactured in the same manner as Example 1, except that the positive electrode active material precursor manufactured in Comparative Manufacturing Example 2 was used instead of the positive electrode active material precursor manufactured in Manufacturing Example 1.

[0324]

[0325] Experimental Example 1: Analysis of the positive electrode active material precursor

[0326] Each of the positive electrode active material precursors, carbon black (DENKA, FX35) and binder [6:1 weight ratio mixture of PVdF (Kureha, KF9709) and BM730H (zeon)] manufactured in the above manufacturing examples and comparative manufacturing examples were added to a solvent (N-methylpyrrolidone (NMP)) at a weight ratio of 83:10:7, and stirred at 1,500 rpm for 95 minutes using a homogenizer (homogenizing disper model 2.5, primix) to manufacture a positive electrode precursor slurry.

[0327] The above positive electrode precursor slurry was coated on one side of an aluminum foil current collector, dried at 130°C for 3 hours, cut using a cross-section cutter, and then an SEM image of the cross-section of the positive electrode active material precursor was taken using a scanning electron microscope (QUANTA FEG 250, FEI Corporation), and the SEM image is shown in Fig. 1.

[0328]

[0329] FIG. 1 is an SEM image of a cross-section of each of the positive electrode active material precursors manufactured in Manufacturing Example and Comparative Manufacturing Example. Specifically, FIG. 1(A) is an SEM image of a cross-section of the positive electrode active material precursor manufactured in Manufacturing Example 1, FIG. 1(B) is an SEM image of a cross-section of the positive electrode active material precursor manufactured in Manufacturing Example 2, FIG. 1(C) is an SEM image of a cross-section of the positive electrode active material precursor manufactured in Manufacturing Example 3, FIG. 1(D) is an SEM image of a cross-section of the positive electrode active material precursor manufactured in Manufacturing Example 4, FIG. 1(E) is an SEM image of a cross-section of the positive electrode active material precursor manufactured in Comparative Manufacturing Example 1, and FIG. 1(F) is an SEM image of a cross-section of the positive electrode active material precursor manufactured in Comparative Manufacturing Example 2.

[0330]

[0331] Through Fig. 1, it was confirmed that the positive electrode active material precursors manufactured in Manufacturing Examples 1 to 4 had a higher density on the outside than on the inside of the particles.

[0332] On the other hand, it was confirmed that the positive electrode active material precursor manufactured in Comparative Manufacturing Example 1 had a high density on the inside and outside equally, and it was confirmed that the positive electrode active material precursor manufactured in Comparative Manufacturing Example 2 had a lower density on the outside than on the inside.

[0333]

[0334] Experimental Example 2: Analysis of positive electrode active material

[0335] Morphological analysis

[0336] The positive electrode active materials manufactured in the examples and comparative examples were photographed using a scanning electron microscope (JEOL JSM-7900F, JEOL Corporation), and SEM images were obtained.

[0337] From the above SEM images, image analysis was performed based on an artificial intelligence model to segment multiple primary particles to obtain segmentation images, and the segmentation images of each of the positive electrode active materials manufactured in the examples and comparative examples are shown in FIGS. 2 to 7.

[0338]

[0339] Figure 2 is a segmentation image of the positive electrode active material manufactured in Example 1.

[0340] Figure 3 is a segmentation image of the positive electrode active material manufactured in Example 2.

[0341] Figure 4 is a segmentation image of the positive electrode active material manufactured in Example 3.

[0342] Figure 5 is a segmentation image of the positive electrode active material manufactured in Example 5.

[0343] Figure 6 is a segmentation image of the positive electrode active material manufactured in Comparative Example 1.

[0344] Figure 7 is a segmentation image of the positive electrode active material manufactured in Comparative Example 2.

[0345]

[0346] Through Figures 2 to 7, it was confirmed that the positive electrode active materials manufactured in Examples and Comparative Examples were in the form of single particles composed of 30 or fewer primary particles. In addition, it was confirmed that the positive electrode active materials manufactured in Examples 1 and 4 contained a first lithium composite transition metal oxide in the form of a disk at a volume % or more and a volume % or less of 100% or less of the total volume of the positive electrode active materials.

[0347] At this time, the disk shape means a primary particle having an internal angle of 150° or more and 210° or less and an aspect ratio (major axis / minor axis) of 1.5 or more when drawing an imaginary tangent line with the greatest number of contact points between two boundaries of the primary particles existing within an angle of 45° or less based on the major axis direction in the SEM image of the surface of the positive electrode active material, and drawing one imaginary line crossing the two tangent lines.

[0348] For reference, when drawing virtual yellow tangent lines with the most contact points for each of the two boundary lines of the primary particles existing within an angle of 45° or less based on the major axis direction of red in FIGS. 2 to 5, one virtual line (not shown) crossing the two yellow tangent lines satisfies the condition that the same internal angle is 150° or more and 210° or less, and the primary particles corresponding to this case are defined as disk-shaped primary particles.

[0349]

[0350] Aspect ratio analysis

[0351] From the SEM images of the positive electrode active materials obtained from the above morphological analysis, the major and minor axes of the positive electrode active materials manufactured in each example were analyzed and are shown in Figs. 2 to 5 below. For reference, in Figs. 2 to 5, the red arrows represent the minor axes, the blue arrows represent the major axes, and the point of contact between the blue arrows and the red arrows represents the center of gravity of the primary particles. For reference, A shown in Figs. 2 to 5 represents the major axis (blue arrow), and B (red arrow) represents the minor axis.

[0352]

[0353] Through Figures 2 to 5, it was confirmed that the first lithium composite transition metal oxide included in the positive electrode active material manufactured in Examples 1 to 4 was a disk-shaped primary particle with an aspect ratio of 1.5 or more.

[0354]

[0355] Volume fraction, particle size distribution, and average radius analysis

[0356] From the SEM images of the positive electrode active materials obtained from the above morphological analysis, the volume ratio and single particle degree (V) of each example and comparative example 50 ) and average radius (R 50 ) were measured and shown in Table 1 below.

[0357]

[0358] Specifically, the area of ​​each primary particle is measured through the number of pixels corresponding to each of n primary particles observed from an image projected onto a two-dimensional plane by taking an SEM image (measurement magnification: 3,000x) of the surface of the positive electrode active material of the examples and comparative examples. Then, assuming that the surface of the primary particle is circular, that is, using the radius of a circle having the same area as the surface area of ​​each primary particle, the radius of the surface of the primary particle is derived.

[0359] Using the above radius, the volume value is calculated according to the following equation 1, and the total volume value of the positive electrode active material and the total volume value of the first lithium composite transition metal oxide are obtained, and then the total volume value of the first lithium composite transition metal oxide is divided by the total volume value of the positive electrode active material, and the value obtained by multiplying by 100 (the volume ratio (volume %) of the first lithium composite transition metal oxide) is calculated and shown in Table 1 below, and the single particle degree (V) corresponding to the volume at the point where the volume cumulative distribution of the primary particles becomes 50% 50 ) was measured and shown in Table 1 below, and the average radius (R) at the point where 50% of the cumulative distribution of the radii of the particles is 50 ) were measured and shown in Table 1 below.

[0360] [Formula 1]

[0361]

[0362]

[0363] Average particle size analysis

[0364] Using PSA (QUANTA FEG 250, FEI Co.), the average particle diameter (D) of each positive electrode active material manufactured in the examples and comparative examples 50 ) were measured and shown in Table 1 below.

[0365]

[0366] Volume ratio (vol%) of the first lithium composite transition metal oxide and degree of single particle magnetization (V 50 )(㎛ 3 )Average radius (R) 50 )(㎛)Average particle diameter(D) 50 )(㎛)Example 156 Volume % 4.812.164.74Example 240 Volume % 4.752.214.82Example 327 Volume % 4.102.364.78Example 475 Volume % 1.374.24.92Comparative Example 19 Volume % 1.344.134.79Comparative Example 26 Volume % 2.363.214.94

[0367] Through Table 1, it was confirmed that the positive electrode active materials manufactured in Examples 1 to 4, i.e., the positive electrode active materials manufactured using a positive electrode active material precursor having a lower internal density than the external density, contained the first lithium composite transition metal oxide in an amount of 20% by volume or more and 100% by volume or less relative to the total volume of the positive electrode active material, and the single particle size distribution (V 50 ) is 1.2 ㎛ 3 The ideal point and mean radius (R 50 ) was confirmed to be 1 ㎛ or more and 15 ㎛ or less.

[0368] On the other hand, in the case of the positive electrode active materials manufactured in Comparative Examples 1 and 2, i.e., the positive electrode active materials manufactured using a positive electrode active material precursor having an internal density equal to or higher than an external density, it was confirmed that the first lithium composite transition metal oxide was included in an amount of less than 20% by volume relative to the total volume of the positive electrode active material, and the single particle size (V 50 ) is 1.2 ㎛ 3 The ideal point and mean radius (R 50 ) was confirmed to be 1 ㎛ or more and 15 ㎛ or less.

[0369]

[0370] Experimental Example 3: Battery Characteristics Evaluation

[0371] Coin-type half-cell manufacturing

[0372] Each of the positive electrode active material, conductive agent (FX35), and binder (KF9700 and BM73OH mixed at a weight ratio of 2.8:0.2) manufactured in the examples and comparative examples was mixed at a weight ratio of 95:2:3 in an N-methyl-2-pyrrolidone (NMP) solvent to manufacture a positive electrode slurry.

[0373] The above positive electrode slurry was applied to one surface of an aluminum current collector, dried at 130°C, and then rolled to a porosity of 20% to manufacture a positive electrode.

[0374] A lithium metal electrode (Li metal disk) was used as the negative electrode, and an electrode assembly was manufactured by interposing a separator between the positive and negative electrodes, which was then placed inside a battery case, and an electrolyte was injected into the case to manufacture a coin-type half-cell. At this time, the electrolyte used was an electrolyte in which 1 M LiPF6 was dissolved in an organic solvent containing ethylene carbonate: ethyl methyl carbonate: diethyl carbonate in a volume ratio of 3:3:4.

[0375] After manufacturing the coin-type half-cell, the cell was evaluated using the following method.

[0376]

[0377] Capacity and output characteristics evaluation

[0378] For each of the above coin-type half-cells, CC / CV mode charging was performed at 0.1 C constant current at 25°C to 4.25 V (cut-off current 0.05 C), and then CC mode discharging was performed at 0.1 C constant current until the voltage reached 2.5 V. The charge capacity (mAh / g) and discharge capacity (mAh / g) at this time were measured. The measured charge capacity (mAh / g) and discharge capacity (mAh / g) are shown in Table 2 below.

[0379]

[0380] Life Characteristics Assessment

[0381] For each of the above coin-type half-cells, a CC / CV mode charge was performed at 45°C with a 0.2 C constant current to 4.25 V (cut-off current 0.05 C), and then a cycle of discharging in CC mode at a 0.2 C constant current until 2.5 V was reached was counted as 1 cycle, and a total of 30 cycles of charging and discharging were repeated. The discharge capacities in the first and 30th cycles were measured, and the percentage of the discharge capacity in the 30th cycle to the discharge capacity in the first cycle (capacity retention rate (%)) was calculated, and the results are shown in Table 2 below.

[0382]

[0383] 25℃45℃Charge capacity (mAh / g)Discharge capacity (mAh / g)Capacity retention rate (%)Example 1230.1203.398.19Example 2230.2203.897.96Example 3230.5204.197.63Example 4229.8201.298.54Comparative example 1230.8204.296.67Comparative example 2230.7203.896.75

[0384] Through Table 2, it was confirmed that in the case of Examples 1 to 4, that is, batteries manufactured with a cathode active material comprising a single-particle first lithium composite transition metal oxide composed of 30 or fewer disk-shaped primary particles in an amount of 20% to 100% by volume relative to the total volume of the cathode active material, the capacity retention rate at high temperatures was superior to that in Comparative Examples 1 and 2, that is, batteries manufactured with a cathode active material comprising a single-particle first lithium composite transition metal oxide composed of 30 or fewer disk-shaped primary particles in an amount of less than 20% by volume relative to the total volume of the cathode active material.

[0385] Meanwhile, in the case of Examples 1 to 3, i.e., a battery manufactured with a cathode active material comprising a single-particle first lithium composite transition metal oxide in an amount of 20% by volume or more and 70% by volume or less relative to the total volume of the cathode active material, it was confirmed that the discharge capacity was greater than in Example 4, i.e., a battery manufactured with a cathode active material comprising a single-particle first lithium composite transition metal oxide in an amount exceeding 70% by volume relative to the total volume of the cathode active material.

[0386] In conclusion, it was confirmed that a cathode active material containing a single-particle first lithium composite transition metal oxide having 30 or fewer disk-type primary particles in a specific volume range has the effect of simultaneously improving output characteristics and life characteristics.

Claims

1. A cathode active material comprising a single-particle first lithium composite transition metal oxide; and optionally a single-particle second lithium composite transition metal oxide; The above single particle type first lithium composite transition metal oxide is composed of 30 or fewer disk type primary particles, The above disk-type primary particle is, in the case of the primary particle observed from the SEM image of the surface or cross-section of the positive electrode active material, when an imaginary tangent line having the greatest number of contact points is drawn for each of the two boundaries of the primary particle existing within an angle of 45° or less based on the major axis direction, and when one imaginary line crossing the two tangent lines is drawn, the same-side internal angle is 150° or more and 210° or less, and the aspect ratio (major axis / minor axis) is 1.5 or more, The above positive electrode active material is a positive electrode active material comprising the first lithium composite transition metal oxide in an amount of 20% by volume or more and 100% by volume or less relative to the total volume of the positive electrode active material.

2. In paragraph 1, The positive electrode active material is a positive electrode active material comprising the first lithium composite transition metal oxide in an amount of 20% by volume or more and 70% by volume or less relative to the total volume of the positive electrode active material.

3. In paragraph 1, The above first lithium composite transition metal oxide is a positive electrode active material having an aspect ratio (long axis / short axis) of 1.5 or more and 10 or less.

4. In paragraph 1, The above first lithium composite transition metal oxide is a single particle size (V) corresponding to the volume at the point where the cumulative volume distribution of the primary particles reaches 50% when the volume value is calculated from the following equation 1 for each of the primary particles observed from the SEM image of the surface or cross-section of the positive electrode active material. 50 ) is 1.2 ㎛ 3 The positive electrode active material is: [Formula 1] In the above equation 1, The radius is the radius of the surface or cross-section of the primary particle assuming that the surface or cross-section of the primary particle observed from the above SEM image (measurement magnification 3,000 times) is circular.

5. In paragraph 1, The above first lithium composite transition metal oxide is the average radius (R) at the point where 50% of the cumulative radius distribution of the particles is calculated for each primary particle observed from the SEM image (measurement magnification 3,000 times) of the surface or cross-section of the positive electrode active material. 50 ) is 1 ㎛ or more and 15 ㎛ or less, The above radius is the radius of the surface or cross-section of the primary particle assuming that the surface or cross-section of the primary particle is circular.

6. In paragraph 1, The above first lithium composite transition metal oxide is a positive electrode active material having a composition represented by the following chemical formula 1: [Chemical Formula 1] Li a Ni x Co y M 1 z M 2 1-x-y-z O2 In the above chemical formula 1, M 1 is at least one selected from the group consisting of Mn and Al, M 2 is at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf, 0.9≤a≤1.3, 0.6≤x<1.0, 0 <y<0.4, 0<z<0.4, 0≤1-x-y-z<0.4이다.

7. A positive electrode comprising a positive electrode active material according to any one of claims 1 to 6.

8. A lithium secondary battery comprising the positive electrode of Article 7. 9.(A) A step of preparing a mixture by mixing a positive electrode active material precursor and a first lithium-containing raw material, the internal density of which is lower than the external density; and (B) A method for manufacturing a positive electrode active material, comprising the step of manufacturing a first sintered product by first firing the mixture at a temperature of 800°C or higher and 950°C or lower; The above interior is an area corresponding to less than 50% of the radius in the outermost direction from the center of the positive electrode active material precursor, A method for manufacturing a positive electrode active material, wherein the positive electrode active material is in the form of a single particle composed of 30 or fewer primary particles and includes a first lithium composite transition metal oxide in the form of a disk, and the first lithium composite transition metal oxide is included in an amount of 20% by volume or more and 100% by volume or less relative to the total volume of the positive electrode active material.

10. In paragraph 9, A method for manufacturing a positive electrode active material, further comprising a step (B1) of crushing the primary sintered product immediately after the step (B).

11. In paragraph 9, A method for producing a cathode active material, further comprising, after the above step (B), a step (C) of mixing a second lithium-containing raw material into the first fired product and then firing it a second time at a temperature of 680°C or higher and 850°C or lower to produce a second fired product.

12. In paragraph 11, A method for manufacturing a positive electrode active material, further comprising a step (C1) of crushing the secondary sintered product immediately after the step (C).

13. In paragraph 9, The above positive electrode active material precursor is, (S1) A step of preparing a mixed solution for seeds by introducing a transition metal-containing solution and an ammonium ion-containing solution at a constant flow rate into a reactor including a stirring device, introducing a basic aqueous solution, and stirring while maintaining the stirring speed; (S2) A step of adding the transition metal-containing solution, the ammonium ion-containing solution, and the basic aqueous solution to the seed mixture solution, and stirring while gradually reducing the stirring speed to prepare a mixed solution for particle growth; and (S3) a step of preparing a mixed solution for a positive electrode active material precursor by adding the transition metal-containing solution to the particle growth mixed solution at an increased flow rate compared to step (S2), gradually adding the ammonium ion-containing solution at an increased flow rate, adding the basic aqueous solution, and stirring while maintaining the stirring speed; A method for manufacturing a positive electrode active material, wherein the alkaline aqueous solution is added so that the pH of the mixed solution for the seed is maintained constant, the pH of the mixed solution for particle growth is gradually reduced, and the pH of the mixed solution for the positive electrode active material precursor is added so that the pH is maintained constant.

14. In paragraph 13, A method for producing a positive electrode active material, wherein the basic aqueous solution is introduced so that the pH of the mixed solution for particle growth is gradually reduced from pH 12 to 13 to pH 11.2 to 12.

6.

15. In paragraph 13, The above (S2) step is a method for producing a positive electrode active material, wherein the stirring speed is gradually reduced from 700 rpm to 900 rpm to 500 rpm to 650 rpm.

16. In paragraph 13, A method for manufacturing a cathode active material, wherein the step (S3) comprises injecting the transition metal-containing solution at a flow rate of 1.2 to 1.4 times that of the step (S2), and gradually increasing the flow rate of the ammonium ion-containing solution to a flow rate of 20% to 45% that of the transition metal-containing solution.

Citation Information

Patent Citations

  • System of manufacturing bi-cell of all-solid-state battery

    KR1020230149037A

  • Machine learning-based perimeter intrusion detection system using radar

    KR102377226B1

  • Composite hydroxide containing transition metal and process for manufacturing the same and cathode active material for non-aqueous electrolyte secondary battery and process for manufacturing the same

    JP2018095505A

  • Method for searching stuff using bluetooth low energy

    KR1020200139441A

  • Nickel-based active material precursor for lithium secondary battery, preparing method thereof, nickel-based active material for lithium secondary battery formed thereof, and lithium secondary battery comprising positive electrode including the nickel-based active material

    KR102473535B1