Positive electrode active material, method for producing same, positive electrode comprising positive electrode active material, and lithium secondary battery comprising positive electrode active material
The development of a nickel-rich lithium transition metal oxide with controlled manufacturing processes addresses the thermal stability and particle breakage issues in lithium secondary batteries, resulting in improved capacity and lifespan through enhanced particle strength and reduced side reactions.
Patent Information
- Application Number
- PCT/KR2024/007592
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-06-03
- Publication Date
- 2024-12-05
AI Technical Summary
Lithium transition metal oxides used in lithium secondary batteries, particularly those with high nickel content, suffer from low thermal stability and particle breakage during rolling, leading to side reactions with the electrolyte and reduced battery performance.
A positive electrode active material with a nickel content of 60 mol% or more, manufactured using a method that includes primary and secondary calcination steps with controlled temperature ranges and temperature increase rates, resulting in a single-particle lithium transition metal oxide with enhanced particle strength and reduced fine powder content, thereby minimizing particle cracking during rolling.
The solution effectively suppresses particle cracking and side reactions, improving the capacity and lifespan characteristics of lithium secondary batteries by maintaining a high degree of single-particle formation and crystallinity, even under high pressure, thus enhancing the energy density and durability of the battery.
Smart Images

Figure KR2024007592_05122024_PF_FP_ABST
Abstract
Description
Positive electrode active material, method for producing the same, and positive electrode and lithium secondary battery including the same
[0001] Cross-citation with related applications
[0002] This application claims the benefit of priority from Korean Patent Application No. 10-2023-0071871, filed June 2, 2023, the entire contents of which are incorporated herein by reference.
[0003] Technology field
[0004] The present invention relates to a positive electrode active material, a method for producing the same, and a positive electrode and a lithium secondary battery including the same.
[0005]
[0006] As technological development and demand for mobile devices increase, the demand for secondary batteries as an energy source is rapidly increasing. Among these secondary batteries, lithium secondary batteries, which boast high energy density and voltage, long cycle life, and low self-discharge rates, are commercialized and widely used.
[0007] Lithium-transition metal composite oxides are used as cathode active materials in lithium secondary batteries. Among these, lithium-cobalt composite metal oxides such as LiCoO2, which exhibit high operating voltage and excellent capacity characteristics, are primarily used. However, LiCoO2 suffers from poor thermal properties due to crystal structure instability following delithiation. Furthermore, its high cost limits its mass use as a power source in fields such as electric vehicles.
[0008] As a material to replace the above LiCoO2, lithium manganese composite metal oxides (such as LiMnO2 or LiMn2O4), lithium iron phosphate compounds (such as LiFePO4), or lithium nickel composite metal oxides (such as LiNiO2) have been developed. Among these, research and development on lithium nickel composite metal oxides, which have a high reversible capacity of about 200 mAh / g and make it easy to implement large-capacity batteries, is being actively studied. However, LiNiO2 has inferior thermal stability compared to LiCoO2, and there was a problem that the positive electrode active material itself decomposed when an internal short circuit occurred due to external pressure in a charged state, causing the battery to rupture and catch fire. Accordingly, as a method to improve the low thermal stability of LiNiO2 while maintaining the excellent reversible capacity, lithium transition metal oxides in which some of the Ni was replaced with Co, Mn, or Al were developed.
[0009] However, in the case of lithium ion batteries using lithium transition metal oxides, especially lithium transition metal oxides containing a high nickel (Ni-rich) content, as positive electrode active materials, although a high capacity can be achieved as the nickel content increases, there is a disadvantage in that the rolling density of the particles is low.
[0010] In order to maximize the volumetric energy density of the battery, a method of rolling the positive electrode active material layer using a roll press is used during electrode manufacturing to reduce the voids between positive electrode active material particles so that a positive electrode active material layer with a denser structure can be manufactured. However, if the particles break during rolling, the contact area with the electrolyte becomes excessively wide, which may cause a side reaction with the electrolyte, and the broken positive electrode active material particles may block the path for the electrolyte to penetrate into the positive electrode active material layer or become a factor that reduces conductivity.
[0011] Therefore, there is a need for the development of a cathode active material that can improve energy volume density and improve life characteristics by suppressing particle breakage during rolling for cathode manufacturing.
[0012]
[0013] [Prior Art Literature]
[0014] [Patent Document]
[0015] (Patent Document 1) KR 2021-0117212 A
[0016] (Patent Document 2) KR 10-2022-0048191 A
[0017] (Patent Document 3) KR 10-2022-0048192 A
[0018]
[0019] The object of the present invention is to provide a positive electrode active material in which particle breakage is reduced during rolling.
[0020] Another object of the present invention is to provide a method for manufacturing a positive electrode active material in which particle breakage is reduced during rolling.
[0021]
[0022] To solve the above problem, the present invention provides a positive electrode active material, a method for producing the same, and a positive electrode and a lithium secondary battery including the same.
[0023] (1) The present invention includes a lithium transition metal oxide in the form of a single particle, wherein the lithium transition metal oxide contains nickel in an amount of 60 mol% or more among the total transition metals, and has a cathode active material having a density of 6,500 kgf / cm 2 When pressure is applied, a positive electrode active material is provided in which the content of fine particles having a particle size of 1 ㎛ or less based on the total volume of the positive electrode active material after the pressure is applied is 10% by volume or less.
[0024] (2) In the present invention, in the above (1), the positive electrode active material has an average particle diameter (D 50 ) provides a positive electrode active material having a diameter of 2 ㎛ or more and 12 ㎛ or less.
[0025] (3) The present invention provides a positive electrode active material having a particle strength of 500 MPa or more and 1,500 MPa or less in the above (1) or (2), and the particle strength (MPa) is a value obtained by collecting a sample of lithium transition metal oxide particles, placing the collected sample on a glass, and applying a pressure of 100 mN to the sample with a tip until the particle breaks and the tip touches the glass on which the sample is placed.
[0026] (4) The present invention provides a single particle type positive electrode active material having a composition represented by the following chemical formula 1, wherein the positive electrode active material is in any one of the above (1) to (3):
[0027] [Chemical Formula 1]
[0028] Li a Ni x Co y M 1 z M 2 1-x-y-z O2
[0029] In the above chemical formula 1, M 1 is at least one selected from the group consisting of Mn and Al, and M 2 is at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf, and 1.0≤a≤1.3, 0.6≤x<1.0, 0 <y<0.4, 0<z<0.4, 0≤1-x-y-z≤0.4이다.
[0030] (5) The present invention provides a positive electrode active material in which the content of fine particles having a particle size of 1 ㎛ or less before rolling is 0% by volume or more and 1% by volume or less based on the total volume of the positive electrode active material in any one of the above (1) to (4).
[0031] (6) A method for producing a single-particle type positive electrode active material, comprising: 1) a step of mixing a positive electrode active material precursor containing nickel of 60 mol% or more among the total transition metals and a lithium-containing raw material, heating to a first firing temperature and performing a first firing to produce a sintered product; 2) a step of cooling the sintered product to room temperature; and 3) a step of mixing the sintered product and the lithium-containing raw material, heating to a second firing temperature and performing a second firing to produce a lithium transition metal oxide in the form of a single particle; The present invention provides a method for producing a positive electrode active material, wherein the first firing temperature is 850°C or more and 950°C or less, the second firing temperature is 800°C or more and 850°C or less, and the second firing temperature is lower than the first firing temperature.
[0032] (7) The present invention provides a method for manufacturing a positive electrode active material in the above (6), wherein the temperature increase rate of step 1) and the temperature increase rate of step 3) are each 4°C / min or more and 7°C / min or less.
[0033] (8) The present invention provides a method for manufacturing a positive electrode active material, which further includes a step of 2-1) crushing the plastic product before secondary firing in step 3) in the above (6) or (7).
[0034] (9) The present invention provides a method for manufacturing a positive electrode active material, further comprising the step of pulverizing the secondary sintered product in any one of the above (6) to (8) 3-1).
[0035] (10) The present invention provides a positive electrode comprising any one of the positive electrode active materials (1) to (5).
[0036] (11) The present invention provides a lithium secondary battery comprising the positive electrode of (10); a negative electrode; a separator interposed between the positive electrode and the negative electrode; and an electrolyte.
[0037]
[0038] The cathode active material according to the present invention is a cathode active material including a lithium transition metal oxide in the form of single particles in which the nickel content is 60 mol% or more among the total molar number of transition metals of the lithium transition metal oxide, and the cathode active material is 6,500 kgf / cm 2 When pressure is applied, the content of fine particles having a particle size of 1 ㎛ or less based on the total volume of the positive electrode active material after the pressure is applied is 10% by volume or less, so that the phenomenon of breaking of lithium transition metal oxide particles during rolling for positive electrode manufacturing can be effectively suppressed. Accordingly, when the positive electrode active material according to the present invention is used, the occurrence of side reactions with the electrolyte caused by breaking of lithium transition metal oxide particles can be minimized, and excellent capacity characteristics and life characteristics can be realized.
[0039]
[0040] Figure 1 is a SEM image of the positive electrode active material manufactured in Example 1.
[0041] Figure 2 is an SEM image of the positive electrode active material manufactured in Comparative Example 1.
[0042] Figure 3 is a graph of particle distribution before and after rolling for the positive electrode active material manufactured in Example 1.
[0043] Figure 4 is a graph of the particle distribution before and after rolling for the positive electrode active material manufactured in Example 2.
[0044] Figure 5 is a graph of the particle distribution before and after rolling for the positive electrode active material manufactured in Example 3.
[0045] Figure 6 is a graph of the particle distribution before and after rolling for the positive electrode active material manufactured in Example 4.
[0046] Figure 7 is a graph of particle distribution before and after rolling for the positive electrode active material manufactured in Comparative Example 1.
[0047] Figure 8 is a graph of particle distribution before and after rolling for the positive electrode active material manufactured in Comparative Example 2.
[0048] Figure 9 is a graph of particle distribution before and after rolling for the positive electrode active material manufactured in Comparative Example 3.
[0049] Figure 10 is a graph of particle distribution before and after rolling for the positive electrode active material manufactured in Comparative Example 4.
[0050] Figure 11 is a graph of capacity (mAh / g) according to cycle of secondary batteries including positive electrode active materials manufactured in examples and comparative examples.
[0051]
[0052] Hereinafter, the present invention will be described in more detail.
[0053] Terms or words used in this specification and claims should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical idea of the present invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best way.
[0054]
[0055] In the present invention, the term 'primary particle' means the smallest particle unit that can be distinguished as a single lump when observing the cross-section of a positive electrode active material through a scanning electron microscope (SEM), and may be composed of one crystal grain or multiple crystal grains.
[0056] In the present invention, the term "secondary particle" refers to a secondary structure formed by the aggregation of multiple primary particles. The average particle diameter of the secondary particles can be measured using a particle size analyzer.
[0057] In this specification, the term 'single particle form' is a concept that is contrasted with the spherical secondary particle form formed by agglomeration of tens to hundreds of primary particles manufactured by a conventional method, and means a form formed of 50 or fewer primary particles. Specifically, in the present invention, the single particle form may be a single particle formed of one primary particle, or may be a secondary particle form formed by agglomeration of 2 or more, 3 or more, 4 or more, 5 or more, 10 or more, and 30 or less, 35 or less, 40 or less, 45 or less, or 50 or less primary particles.
[0058] In the present invention, the term 'average particle diameter (D 50 )' means the particle size at the 50% point of the volume cumulative distribution according to particle size. The above average particle size is calculated by dispersing the powder to be measured in a dispersion medium, introducing it into a commercially available laser diffraction particle size measuring device (e.g., S3500 from Microtrac), and measuring the difference in diffraction pattern according to particle size when the particles pass through the laser beam to calculate the particle size distribution, and calculating the particle diameter at the point where it becomes 50% of the volume cumulative distribution according to particle size in the measuring device, thereby obtaining D 50 can be measured.
[0059]
[0060] positive electrode active material
[0061] The present invention comprises a lithium transition metal oxide in the form of a positive electrode single particle, wherein the lithium transition metal oxide contains nickel in an amount of 60 mol% or more among the total transition metals, and the positive electrode active material has a concentration of 6,500 kgf / cm 2 When pressure is applied, the content of fine particles having a particle size of 1 ㎛ or less based on the total volume of the positive electrode active material after pressure is 10% by volume or less.
[0062]
[0063] The lithium transition metal oxide is in the form of a single particle composed of 50 or fewer primary particles. That is, the lithium transition metal oxide is in the form of a single particle or a single particle composed of 2 or more but less than 50 particles. Specifically, the lithium transition metal oxide may be in the form of 2 or more but less than 40, 2 or more but less than 30, 2 or more but less than 20, or 2 or more but less than 10 primary particles, and preferably 2 or more but less than 10. The single particle form is distinguished from secondary particles composed of more than 50 primary particles aggregated together.
[0064] When the lithium transition metal oxide is in the form of a single particle, it has excellent stability, so that even when pressure is applied to the positive electrode active material containing it, the positive electrode active material is less likely to break or crack, thereby reducing side reactions between the positive electrode active material and the electrolyte. This improves durability against volume changes during charge and discharge of the battery, thereby improving life characteristics. On the other hand, the secondary particle lithium transition metal oxide is prone to particle breakage during the electrode rolling process, which increases the surface area of the positive electrode active material, thereby worsening the storage and life performance at high temperatures. In particular, in the case of a lithium transition metal oxide containing a high nickel content, the problem of particle breakage occurring during rolling for the manufacture of the positive electrode occurs more, and in this case, side reactions between the lithium transition metal oxide and the electrolyte may increase, and the physical properties of the battery may deteriorate.
[0065] The positive electrode active material of the present invention exhibits a high degree of single particle magnetization and thus can exhibit high particle strength, and when a positive electrode is manufactured using the positive electrode, particle breakage is suppressed even during rolling, resulting in a strength of 6,500 kgf / cm. 2Even under high pressure, the content of fine particles with a particle size of 1 μm or less may be small. In this case, the phenomenon of breaking of lithium transition metal oxide particles during rolling for positive electrode manufacturing can be effectively suppressed. Accordingly, the occurrence of side reactions with the electrolyte due to the breaking of lithium transition metal oxide particles can be minimized, and excellent capacity characteristics and life characteristics can be realized.
[0066] Specifically, 6,500 kgf / cm for the positive electrode active material 2 When pressure is applied, the content of fine particles having a particle size of 1 ㎛ or less based on the total volume of the positive electrode active material after pressure is 10% by volume or less, 9% by volume or less, 8% by volume or less, 7% by volume or less, 6% by volume or less, 5% by volume or less, 4% by volume or less, or 3% by volume or less.
[0067]
[0068] 6,500 kgf / cm above 2 The pressure of the cathode active materials, which are typically suppressed from breaking up particles, is 650 kgf / cm 2 This is a very high level of pressure compared to judging whether particle breakage is suppressed based on the rolling pressure.
[0069] In this way, since the positive electrode active material of the present invention has a high degree of crystallinity and single particle size, it can exhibit an excellent effect of alleviating and suppressing particle breakage during rolling.
[0070]
[0071] According to one embodiment of the present invention, the positive electrode active material has an average particle diameter (D 50 ) may be 2 ㎛ or more, 3 ㎛ or more, 4 ㎛ or more, 5 ㎛ or more, or 6 ㎛ or more, and may be 7 ㎛ or less, 8 ㎛ or less, 9 ㎛ or less, 10 ㎛ or less, 11 ㎛ or less, or 12 ㎛ or less. When the average particle diameter is within the above range, the electrode density can be controlled and the energy density can be controlled.
[0072]
[0073] According to one embodiment of the present invention, the particle strength of the positive electrode active material may be 500 MPa or more and 1,500 MPa or less, specifically, 500 MPa or more, 600 MPa or more, 700 MPa or more, 800 MPa or more, or 900 MPa or more, and may be 1,000 MPa or less, 1,100 MPa or less, 1,200 MPa or less, 1,300 MPa or less, 1,400 MPa or less, or 1,500 MPa or less. The positive electrode material of the present invention can effectively mitigate particle breakage, and thus, can exhibit excellent long-life characteristics when applied to a battery. In this specification, particle strength (MPa) is a value obtained by collecting a sample of lithium transition metal oxide particles, placing the collected sample on a glass, and applying a constant pressure (100 mN) to the sample with a tip, and measuring the force until the particle breaks and the tip touches the glass on which the sample is placed.
[0074]
[0075] Meanwhile, the positive electrode active material includes a lithium transition metal oxide having a molar ratio of nickel among transition metals of 60% or more, and since the high nickel-containing lithium transition metal oxide has a large capacity per unit volume, when applied to a battery, excellent capacity characteristics can be realized.
[0076] Specifically, the positive electrode active material may have a composition represented by the following chemical formula 1.
[0077] [Chemical Formula 1]
[0078] Li a Ni x Co y M 1 z M 2 1-x-y-z O2
[0079] In the above chemical formula 1,
[0080] M 1is at least one selected from the group consisting of Mn and Al,
[0081] M 2 is at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf,
[0082] 1.0≤a≤1.3, 0.6≤x<1.0, 0 <y<0.4, 0<z<0.4, 0≤1-x-y-z≤0.4이다.
[0083] The above a represents the molar ratio of lithium in the lithium transition metal oxide, and may be 1.0≤a≤1.3, specifically 1.0≤a≤1.25, and more specifically 1.0≤a≤1.20.
[0084] The above x represents the molar ratio of nickel among the entire transition metal, and may be 0.6≤x<1.0, specifically 0.6≤x≤0.99 or 0.70≤x≤0.99, and more specifically 0.8≤x≤0.95. When the nickel content satisfies the above range, excellent capacity characteristics can be realized.
[0085] The above y represents the molar ratio of cobalt among the total transition metals, 0 <y<0.40, 구체적으로 0≤y≤0.35, 더욱 구체적으로 0.01≤y≤0.30일 수 있다.
[0086] The above z is the element M among all transition metals 1 It represents the molar ratio of 0 <z<0.40, 구체적으로 0≤z<0.35, 더욱 구체적으로 0.01≤z≤0.30일 수 있다.
[0087] The above 1-xyz is M among all transition metals 2 It represents the molar ratio, and may be 0≤1-xyz≤0.4, specifically 0≤1-xyz≤0.35, and more specifically 0≤1-xyz≤0.30.
[0088]
[0089] Meanwhile, the positive electrode active material may further include, if necessary, a coating layer including one or more elements (hereinafter referred to as “coating elements”) selected from the group consisting of Co, Al, B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La, and Hf on the surface of the lithium transition metal oxide. When the coating layer as described above is included, contact between the lithium transition metal oxide and the electrolyte is blocked, thereby effectively suppressing gas generation and transition metal elution due to side reactions with the electrolyte.
[0090] The above coating layer can be formed by mixing a lithium transition metal oxide and a raw material containing the coating element, and then heat-treating the mixture at a temperature of 200°C or higher and 800°C or lower.
[0091]
[0092] Method for manufacturing positive electrode active material
[0093] The method for manufacturing a positive electrode active material of the present invention comprises the steps of: 1) mixing a positive electrode active material precursor containing nickel of 60 mol% or more among the total transition metals and a lithium-containing raw material, heating to a first firing temperature and performing a first firing to manufacture a sintered product; 2) cooling the sintered product to room temperature; and 3) mixing the sintered product and the lithium-containing raw material, heating to a second firing temperature and performing a second firing to manufacture a lithium transition metal oxide in the form of single particles; wherein the first firing temperature is 850°C or more and 950°C or less, the second firing temperature is 800°C or more and 850°C or less, and the second firing temperature is lower than the first firing temperature.
[0094] The positive electrode active material manufactured by the positive electrode active material manufacturing method of the present invention has the characteristics of high crystallinity and single particle size, and accordingly, the positive electrode active material has a density of 6,500 kgf / cm 2When pressure is applied, the content of fine particles having a particle size of 1 ㎛ or less of the positive electrode active material is 10% by volume or less, that is, the content of fine particles having a particle size of 1 ㎛ or less based on the total volume of the positive electrode active material after pressure is applied is 10% by volume or less, which has high rolling strength and low fine particle generation rate.
[0095]
[0096] When a mixture of a positive electrode active material precursor containing nickel at 60 mol% or more of the above-mentioned total transition metal and a lithium-containing raw material is first fired at a temperature of 850°C or higher and 950°C or lower, the primary particles of the positive electrode active material precursor are aggregated to produce a plastic product in the form of single particles.
[0097] The cathode active material precursor containing nickel at 60 mol% or more among the above-mentioned total transition metals may be a cathode active material precursor containing nickel at 60 mol% or more among the total transition metals, specifically including Ni, Co, and Mn.
[0098] The above first firing temperature is specifically performed at a temperature of 850°C or higher, 860°C or higher, 870°C or higher, 880°C or higher, 900°C or higher, or 910°C or higher, and 930°C or lower, 940°C or lower, or 950°C or lower. When the first firing temperature is within the above range, the primary particles of the positive electrode active material precursor may aggregate, thereby forming a structurally stable single-particle sintered product. When the first firing temperature is lower than 850°C, the primary particles may not sufficiently aggregate, and when it exceeds 950°C, there is a problem in that a structurally unstable sintered product with low crystallinity is manufactured.
[0099] The above first calcination may be performed under an oxygen atmosphere in order to prevent the lithium transition metal oxide from degenerating into a rock salt structure.
[0100] The above primary calcination may be performed for 3 hours or more, 4 hours or more, 5 hours or more, or 6 hours or more, and 10 hours or less, 11 hours or less, or 12 hours or less, in order to agglomerate primary particles and improve the crystallinity of the calcined product.
[0101]
[0102] According to one embodiment of the present invention, the temperature rising rate of step 1) may be 4°C / min or more and 7°C / min or less, specifically, 4°C / min or more, or 5°C / min or more, and 7°C / min or less. When the temperature rising rate during the first firing satisfies the above range, the primary particles of the positive electrode active material precursor may aggregate, thereby forming a structurally more stable single-particle plastic product, and the content of fine particles having a particle size of 1 μm or less in the final positive electrode active material may be minimized. When the temperature rising rate during the first firing exceeds 7°C / min, the primary particles may not sufficiently aggregate, thereby increasing the content of fine particles having a particle size of 1 μm or less in the final positive electrode active material, and when the temperature rising rate during the first firing is less than 4°C / min, the entire first firing time may become longer than necessary.
[0103] When the above-mentioned plastic product is obtained, the plastic product is cooled to room temperature, and then the plastic product and the lithium-containing raw material are mixed, and the temperature is raised to the secondary firing temperature to perform the secondary firing, thereby producing a lithium transition metal oxide in the form of single particles.
[0104] When the above-mentioned sintered product is subjected to a second firing at a temperature of 800°C or higher and 850°C or lower, lithium is inserted into the sintered product, thereby producing a second sintered product. At this time, the second sintered product is a lithium transition metal oxide in the form of single particles. Specifically, the second sintering temperature is performed at a temperature of 800°C or higher, 810°C or higher, 820°C or higher, or 830°C or higher, and 840°C or lower, or 850°C or lower. When the second sintering temperature is within the above range, lithium is inserted into the rock salt structure that may be formed on the surface of the sintered product due to the high temperature during the first sintering, thereby restoring it to a layered structure, and there is an advantage of reducing lithium byproducts. Meanwhile, if the secondary firing temperature is less than 800℃, the lithium insertion speed may be slow due to the low temperature, and if it exceeds 850℃, the temperature may be high, causing the surface of the sintered product to degenerate into a rock salt structure and lithium byproducts to remain.
[0105] The above secondary calcination may be performed under an oxygen atmosphere in order to prevent the lithium transition metal oxide from degenerating into a rock salt structure.
[0106] The above secondary firing may be performed for 3 hours or more, 4 hours or more, 5 hours or more, or 6 hours or more, and 10 hours or less, 11 hours or less, or 12 hours or less, in order to increase the crystallinity of the internal crystal structure of the positive electrode active material.
[0107]
[0108] In addition, the temperature rise rate during the second firing of step 3) may be 4°C / min or more and 7°C / min or less, and specifically, 4°C / min or more, or 5°C / min or more, and 7°C / min or less. When the temperature rise rate during the second firing satisfies the above range, lithium can be more effectively inserted into the rock salt structure that may be formed on the surface of the plasticizer, so that the layered structure can be restored, and lithium byproducts can be further reduced. In addition, when the temperature rise rate during the second firing is too fast, it is difficult to obtain the same effect as when the appropriate temperature rise rate is satisfied, and the increase in crystallinity of the final manufactured positive electrode active material is insufficient, so that the content of fine powder having a particle size of 1 μm or less in the positive electrode active material after rolling may increase. In addition, when the temperature rise rate during the first firing is slow compared to the above range, the entire second firing time may become longer than necessary.
[0109]
[0110] According to one embodiment of the present invention, before the plastic product cooled to room temperature in step 2) is subjected to secondary firing in step 3), the step 2-1) may further include the step of crushing the plastic product. In order to prevent the initial resistance from increasing, the step 2-1) may further include crushing the plastic product to an average particle diameter (D 50 ) may be ground to a size of 3.50㎛ to 6.00㎛.
[0111]
[0112] According to one embodiment of the present invention, the step 3-1) may further include a step of crushing the secondary sintered product. In addition, in order to prevent the initial resistance from increasing, the step 3-1) may further include crushing the secondary sintered product to an average particle diameter (D 50 ) may be ground to a size of 3.50㎛ to 6.00㎛.
[0113] The grinding in steps 2-1) and 3-1) above can be performed using a pin mill, ACM, jet mill, etc. Meanwhile, the pin mill can be performed under conditions of 18,000 rpm, the ACM can be performed under conditions of 6,000 rpm for classification and 12,000 rpm for main processing using a device from Hosokawa, and the jet mill can be performed under conditions of 6 bar for grinding pressure and 3,500 rpm for classification using a device from ZM solution. In this case, the desired average particle size (D 50 ) can be easily obtained.
[0114]
[0115] The cathode active material according to the present invention can be manufactured by a process of introducing lithium-containing raw materials in two stages. That is, the lithium-containing raw materials can be introduced separately before the first firing and before the second firing. In this case, there is an advantage in that lithium is inserted into the rock salt structure that can be formed on the surface, thereby facilitating recovery into a layered structure. On the other hand, if the lithium-containing raw materials are introduced all at once before the first firing, there is a problem of deterioration in electrochemical performance due to an increase in lithium byproducts. In addition, if the lithium-containing raw materials are not introduced in the second firing stage, there is a problem of requiring high temperatures and a long time due to a slow reaction rate.
[0116] In the case where the lithium-containing raw material is input in two portions, in the step 1), the first lithium-containing raw material may be mixed so that the ratio (M:Li) of the total mole number (M) of the transition metal included in the positive electrode active material precursor and the mole number (Li) of the lithium included in the first lithium-containing raw material is 1:0.98 or more, 0.99 or more, 1.00 or more, 1.01 or more, or 1.02 or more, and 1:1.04 or less, 1.05 or less, and in the step 3), the second lithium-containing raw material may be mixed so that the ratio (M':Li) of the total mole number (M') of the transition metal included in the plasticizer of the step 1) and the mole number (Li) of the lithium included in the total mole number (Li) is 1:1.01 or more, or 1.05 or more, and 1.06 or less, 1.07 or less, 1.08 or less, 1.09 or less, or 1.10 or less. there is.
[0117] The method for manufacturing a cathode active material according to the present invention may further include the step of 4) mixing the lithium transition metal oxide and the cobalt-containing raw material, and then performing a heat treatment. In this case, a coating portion containing Co is formed on the lithium transition metal oxide in the form of a single particle.
[0118] According to the present invention, when mixing the lithium transition metal oxide and the cobalt-containing raw material in step 4), an aluminum-containing raw material, a zirconium-containing raw material, or a combination thereof may be further mixed. In this case, the coating portion may further include Al, Zr, or a combination thereof in addition to Co.
[0119] According to the present invention, the cobalt-containing raw material may be mixed in an amount such that the ratio (B / A) of the number of moles of cobalt (B) contained in the cobalt-containing raw material to the total number of moles (A) of metals excluding lithium contained in the lithium transition metal oxide is 0.01 to 0.03. In this case, there is an advantage in that lithium byproducts can be controlled in a cathode active material manufacturing process that does not include a washing process.
[0120] The above cobalt-containing raw material may be at least one selected from Co(OH)2, Co3O4, CoO, (CH3CO2)2Co, CoCl2, and CoSO4·xH2O, and specifically may be Co(OH)2.
[0121] According to the present invention, the aluminum-containing raw material may be mixed in an amount of 0.03 to 0.10 parts by weight per 100 parts by weight of the lithium transition metal oxide. In this case, the lifespan, resistance, and gas generation amount can be improved by ensuring structural stability.
[0122] The above aluminum-containing raw material may be at least one selected from Al(OH)3, Al2(SO4)3·xH2O, Al2O3, Al(NO3)3·9H2O, AlCl3, and C2H5O4Al, and specifically, may be Al(OH)3.
[0123] The above zirconium-containing raw materials are Zr(OH)4, ZrO2, Zr(NO3)4, ZrCl4, ZrS2, Zr(SO4)2 and C8H 12 It can be one or more types selected from O8Zr.
[0124]
[0125] According to the present invention, the heat treatment may be performed under an oxygen atmosphere to prevent the lithium transition metal oxide from degenerating into a rock salt structure.
[0126]
[0127] According to the present invention, the heat treatment may be performed by first performing heat treatment at a temperature of 600°C or higher, 610°C or higher, 620°C or higher, 630°C or higher, 640°C or higher, or 650°C or higher, and 720°C or lower, 740°C or lower, 760°C or lower, 780°C or lower, or 800°C or lower, and then performing second heat treatment at a temperature of 450°C or higher, 460°C or higher, 470°C or higher, or 480°C or higher, and 520°C or lower, 530°C or lower, 540°C or lower, or 550°C or lower, in order to form a coating portion with an appropriate thickness. That is, after performing heat treatment at 600°C to 800°C in one firing profile, heat treatment may be performed at 450°C to 550°C.
[0128]
[0129] According to the present invention, the heat treatment may be performed for 1 hour or more, 2 hours or more, 3 hours or more, and 9 hours or less, 10 hours or less, 11 hours or less, or 12 hours or less in order to increase the crystallinity of the coating portion.
[0130]
[0131] anode
[0132] In addition, the present invention provides a positive electrode for a lithium secondary battery, comprising a positive electrode active material layer including the positive electrode active material. Specifically, the positive electrode comprises a positive electrode current collector, and a positive electrode active material layer positioned on at least one surface of the positive electrode current collector and including the positive electrode material. The positive electrode active material layer may have a porosity of 10% to 30% by volume, specifically 15% to 30% by volume, and more specifically 18% to 27% by volume.
[0133] When the positive electrode active material layer has the above porosity, the positive electrode may include particles having a particle size of less than 1 μm at 50% or less based on the total number of particles in the positive electrode active material layer when measuring PSD (Particle Size Distribution).
[0134] The positive electrode may specifically include particles having a diameter of less than 1 μm in an amount of 0.01% to 50%, 0.05% to 30%, 0.1% to 28%, 0.05% to 27.5%, 0.1% to 27.5%, 0.05% to 15%, or 0.1% to 15% based on the total number of positive electrode active material particles.
[0135] The above positive electrode can contain only a small amount of fine powder having a particle size of less than 1 ㎛ within the above range, even when the positive electrode active material layer is rolled to have a porosity within the above range during the manufacture of the positive electrode due to the alleviation of particle breakage of the positive electrode material.
[0136] The number of particles having a particle diameter of less than 1 ㎛ may be measured by measuring the number of particles located in the positive electrode active material layer when, after forming a positive electrode active material layer including the positive electrode active material, the positive electrode active material is rolled to 10% to 30% by volume, specifically 15% to 30% by volume, and more specifically 18% to 24% by volume, and then heat-treated in an air atmosphere at a temperature of 500°C for 2 hours.
[0137] The number of particles having a diameter of less than 1 ㎛ above may be a ratio of the number when the total number of positive electrode active material particles included in the positive electrode active material layer is set to 100%, and specifically, after measuring PSD using 'MICROTRAC S3500' of MICROTRAC, 'CILAS920, France' of CILAS, and 'Mastersizer2000, USA' of MALVERN, the area of particles having a diameter of less than 1 ㎛ in the PSD graph may be obtained by dividing the area by the total area.
[0138]
[0139] The positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 μm, and fine unevenness may be formed on the surface of the positive electrode current collector to increase the adhesive strength of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.
[0140]
[0141] The above-described positive electrode active material layer may include a conductive material and a binder together with the positive electrode active material according to the present invention described above.
[0142] The above positive electrode active material may be included in an amount of 80 to 99 wt%, more specifically 85 to 98 wt%, based on the total weight of the positive electrode active material layer. When included in the above content range, excellent capacity characteristics may be exhibited.
[0143] The conductive material is used to provide conductivity to the electrode, and in the battery to be formed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One of these may be used alone or a mixture of two or more may be used. The conductive material may be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.
[0144] The above binder serves to improve the adhesion between positive electrode active material particles and the adhesive strength between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluoroelastomer, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof. The binder may be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.
[0145]
[0146] The above-described positive electrode can be manufactured according to a conventional positive electrode manufacturing method, except that the positive electrode active material according to the present invention is used. Specifically, the positive electrode active material layer forming composition, prepared by dissolving or dispersing the above-described positive electrode material and optionally a binder, a conductive agent, and additives as needed in a solvent, is applied onto a positive electrode current collector, followed by drying and rolling. At this time, the types and contents of the positive electrode material, binder, and conductive agent are as described above.
[0147]
[0148] The solvent may be a solvent generally used in the relevant technical field, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water. One of these may be used alone or a mixture of two or more thereof may be used. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, taking into account the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the positive electrode.
[0149]
[0150] Additionally, in another method, the positive electrode may be manufactured by casting the composition for forming the positive electrode active material layer on a separate support, and then laminating the resulting film on a positive electrode current collector by peeling it off from the support.
[0151]
[0152] lithium secondary battery
[0153] In addition, the present invention can manufacture an electrochemical device including the positive electrode. The electrochemical device may be a battery, a capacitor, or the like, and more specifically, a lithium secondary battery.
[0154] The lithium secondary battery specifically includes a positive electrode, a negative electrode positioned opposite the positive electrode, and a separator and electrolyte interposed between the positive electrode and the negative electrode. Since the positive electrode is the same as described above, a detailed description thereof will be omitted, and only the remaining components will be described in detail below.
[0155] In addition, the lithium secondary battery may optionally further include a battery container that houses the electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.
[0156]
[0157] In the above lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.
[0158] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 ㎛ to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.
[0159]
[0160] The above negative electrode active material layer optionally includes a binder and a conductive material together with the negative electrode active material.
[0161] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; SiO β(0<β<2), SnO2, vanadium oxide, lithium vanadium oxide, and other metal oxides capable of doping and dedoping lithium; or composites containing the above metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include natural graphite or artificial graphite in the form of amorphous, plate-like, flaky, spherical, or fiber-like forms, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes.
[0162] The above negative electrode active material may be included in an amount of 80 to 99 parts by weight based on 100 parts by weight of the total weight of the negative electrode active material layer.
[0163]
[0164] The above binder is a component that assists in bonding between the conductive material, the active material, and the current collector, and is typically added in an amount of 0.1 to 10 parts by weight based on 100 parts by weight of the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.
[0165] The conductive agent is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10 parts by weight or less, preferably 5 parts by weight or less, based on 100 parts by weight of the total weight of the negative electrode active material layer. The conductive agent is not particularly limited as long as it has conductivity and does not cause a chemical change in the battery, and examples thereof include graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber or metal fiber; metal powders such as fluorocarbon, aluminum, and nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0166]
[0167] For example, the negative electrode active material layer can be manufactured by applying and drying a negative electrode composite prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material in a solvent, on a negative electrode current collector, or by casting the negative electrode composite on a separate support and then laminating the resulting film on a negative electrode current collector by peeling it off from the support.
[0168]
[0169] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used in lithium secondary batteries can be used without special restrictions, and in particular, one having low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. can also be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength can be used, and can optionally be used in a single-layer or multi-layer structure.
[0170]
[0171] In addition, examples of the electrolyte used in the present invention include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.
[0172] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0173] As the organic solvent, any solvent that can serve as a medium through which ions involved in the electrochemical reaction of the battery can move may be used without particular limitation. Specifically, the organic solvent includes ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); Alcohol solvents such as ethyl alcohol, isopropyl alcohol, etc.; nitriles such as R-CN (R is a linear, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes, etc. can be used. Among these, carbonate solvents are preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferable.In this case, the performance of the electrolyte may be improved when the cyclic carbonate and the chain carbonate are mixed and used in a volume ratio of about 1:1 to about 1:9.
[0174]
[0175] The above lithium salt can be used without any special limitation as long as it is a compound that can provide lithium ions used in a lithium secondary battery. Specifically, the above lithium salt is LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2) 2. LiCl, LiI, or LiB(C2O4)2 can be used. It is recommended that the concentration of the lithium salt be within the range of 0.1 to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.
[0176]
[0177] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 to 5 parts by weight based on 100 parts by weight of the total weight of the electrolyte.
[0178]
[0179] As described above, a lithium secondary battery including a cathode material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and lifespan characteristics, and is therefore useful in portable devices such as mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0180] Accordingly, according to another embodiment of the present invention, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same are provided.
[0181] The above battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.
[0182] There is no particular limitation on the external shape of the lithium secondary battery of the present invention, but it may be a cylindrical shape using a can, a square shape, a pouch shape, or a coin shape.
[0183] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but can also be preferably used as a unit battery in a medium- to large-sized battery module including a plurality of battery cells.
[0184]
[0185] Hereinafter, the present invention will be described in detail with reference to examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention should not be construed as being limited to the examples described below. These examples are provided to more fully explain the present invention to those of ordinary skill in the art.
[0186]
[0187] Examples and Comparative Examples
[0188]
[0189] Example 1
[0190] Positive electrode active material precursor [Composition: Ni 0.85 Co 0.05 Mn 0.10 (OH)2, average particle size (D) 50 ) 4.0 ㎛] and LiOH were mixed in a molar ratio of 1:1.04, heated at a heating rate of 5°C / min, and first fired at 910°C for 10 hours in an oxygen atmosphere to manufacture a plastic product, which was then cooled to room temperature.
[0191] After the above-mentioned plastic product was pulverized using an air jet mill, 0.01 mol of LiOH was additionally added, the temperature was increased at a heating rate of 5°C / min, and secondary firing was performed at a temperature of 830°C for 10 hours in an oxygen atmosphere to produce a positive electrode active material (lithium transition metal oxide) in the form of single particles containing 60 mol% or more of nickel.
[0192]
[0193] Example 2
[0194] A positive electrode active material (lithium transition metal oxide) in the form of a single particle containing nickel at 60 mol% or more was manufactured in the same manner as in Example 1, except that the temperature during the first firing was changed to 930°C.
[0195]
[0196] Example 3
[0197] A positive electrode active material (lithium transition metal oxide) in the form of a single particle containing nickel at 60 mol% or more was manufactured in the same manner as Example 1, except that the temperature during the first firing was changed to 930°C and the temperature during the second firing was changed to 850°C.
[0198]
[0199] Example 4
[0200] A cathode active material (lithium transition metal oxide) in the form of a single particle containing nickel at 60 mol% or more was manufactured in the same manner as Example 1, except that the first firing was performed at a firing temperature of 930°C by increasing the temperature at a heating rate of 7°C / min during the first firing, and the second firing was performed at a firing temperature of 830°C by increasing the temperature at a heating rate of 7°C / min during the second firing.
[0201]
[0202]
[0203] Comparative Example 1
[0204] Positive electrode active material precursor [Composition: Ni 0.85 Co 0.05 Mn 0.10 (OH)2, average particle size (D) 50 ) 4.0 ㎛] and LiOH were mixed in a molar ratio of 1:1.05, heated at a heating rate of 5°C / min, and first fired at a temperature of 800°C for 5 hours in an oxygen atmosphere to manufacture a plastic product, which was then cooled to room temperature.
[0205] The above-mentioned plastic product was pulverized using an air jet mill, and then heated at a heating rate of 5°C / min, and then secondary calcined at a temperature of 400°C for 5 hours in an oxygen atmosphere to produce a positive electrode active material (lithium transition metal oxide) in the form of single particles containing 60 mol% or more of nickel.
[0206]
[0207] Comparative Example 2
[0208] Positive electrode active material precursor [Composition: Ni 0.85 Co 0.05 Mn 0.10 (OH)2, average particle size (D) 50 ) 11.0 ㎛] and LiOH were mixed in a molar ratio of 1:1.05, heated at a heating rate of 5°C / min, and first fired at a temperature of 830°C for 5 hours in an oxygen atmosphere to manufacture a plastic product, and then cooled to room temperature.
[0209] The above-mentioned plastic product was pulverized using an air jet mill, and then heated at a heating rate of 5°C / min, and then secondary calcined at a temperature of 400°C for 5 hours in an oxygen atmosphere to produce a positive electrode active material (lithium transition metal oxide) in the form of single particles containing 60 mol% or more of nickel.
[0210]
[0211] Comparative Example 3
[0212] Positive electrode active material precursor [Composition: Ni 0.85 Co 0.05 Mn 0.10 (OH)2, average particle size (D) 50 ) 4.0 ㎛] and LiOH were mixed in a molar ratio of 1:1.05, heated at a heating rate of 8°C / min, and calcined at a temperature of 810°C for 15 hours in an oxygen atmosphere to produce a cathode active material (lithium transition metal oxide) in the form of single particles containing nickel at 60 mol% or more.
[0213]
[0214] Comparative Example 4
[0215] Positive electrode active material precursor [Composition: Ni 0.85 Co 0.05 Mn 0.10 (OH)2, average particle size (D) 50 ) 4.0 ㎛] and LiOH are mixed in a molar ratio of 1:1.04, heated at a heating rate of 8°C / min, and first fired at a temperature of 810°C for 10 hours in an oxygen atmosphere to manufacture a plastic product.
[0216] After the above-mentioned plastic product was pulverized using an air jet mill, 0.01 mol of LiOH was additionally added, the temperature was increased at a heating rate of 5°C / min, and secondary firing was performed at a temperature of 600°C for 10 hours in an oxygen atmosphere to produce a positive electrode active material (lithium transition metal oxide) in the form of single particles containing 60 mol% or more of nickel.
[0217]
[0218] 1st firing crushing 2nd firing Heating rate (℃ / min) Firing temperature (℃) Time (h) Heating rate (℃ / min) Firing temperature (℃) Time (h) Example 1591010 Jet mill 583010 Example 2593010 Jet mill 583010 Example 3593010 Jet mill 585010 Example 4793010 Jet mill 783010 Comparative example 1580010 Jet mill 54005 Comparative example 258305 Jet mill 54005 Comparative example 3881015----Comparative example 4881010 Jet mill 560010
[0219] Experimental Example 1
[0220] 1) SEM image
[0221] SEM images of the positive electrode active materials manufactured in the examples and comparative examples were obtained using a scanning electron microscope (SEM, JEOL JSM-7900F), and the SEM images of the positive electrode active materials manufactured in Example 1 and Comparative Example 1 are shown in FIGS. 1 and 2, respectively.
[0222]
[0223] Figure 1 is a SEM image of the positive electrode active material manufactured in Example 1.
[0224] Figure 2 is an SEM image of the positive electrode active material manufactured in Comparative Example 1.
[0225]
[0226] 2) Measurement of particle size distribution
[0227] PSD measurement of positive electrode active material particles before rolling
[0228] The positive electrode active material particles manufactured in the examples and comparative examples were added to 20 mL of deionized water (DI water) containing a 10% aqueous solution (5 mL) of sodium metahexaphosphate as a dispersant and the positive electrode active material particles, and dispersed using ultrasonic waves for 2 minutes. Then, the PSD of the positive electrode active material particles before rolling was measured using 'MICROTRAC S3500' of MICROTRAC, and the number of particles of 1 ㎛ or less based on the total number of positive electrode active materials was calculated as a % value, and the fine powder content of 1 ㎛ or less before rolling (%) was shown in Table 2 below.
[0229] PSD measurement of positive electrode active material particles after rolling
[0230] Each of the positive electrode active materials, conductive agent (FX35), and binder (KF9700 and BM73OH mixed in a weight ratio of 1.35:0.15) manufactured in the examples and comparative examples were mixed in a weight ratio of 97.5:1:1.5 in N-methyl-2-pyrrolidone (NMP) solvent to manufacture a positive electrode slurry. The positive electrode slurry was applied to one surface of an aluminum current collector, dried at 130°C, and then applied at a pressure of 6,500 kgf / cm 2 The positive electrode was manufactured by rolling under pressure.
[0231] After heat-treating the above-mentioned manufactured positive electrode in an air atmosphere at 500℃ for 2 hours, positive electrode active material particles were collected from the positive electrode, and then 20 mL of deionized (DI) water was filled with a 10% aqueous solution (5 mL) of sodium metahexaphosphate as a dispersant and the positive electrode active material particles, followed by ultrasonic dispersion for 2 minutes. After rolling, the PSD of the positive electrode active material particles was measured using 'MICROTRAC S3500' of MICROTRAC, and the volume of particles of 1 ㎛ or less based on the total volume of the positive electrode active material was calculated as a % value, and the fine powder content of 1 ㎛ or less after rolling (%) is shown in Table 2 below.
[0232] In addition, graphs of particle distribution before and after rolling for the positive electrode active materials manufactured in Examples 1 to 4 and Comparative Examples 1 to 4 are shown in FIGS. 3 to 10, respectively.
[0233] Figure 3 is a graph of particle distribution before and after rolling for the positive electrode active material manufactured in Example 1.
[0234] Figure 4 is a graph of the particle distribution before and after rolling for the positive electrode active material manufactured in Example 2.
[0235] Figure 5 is a graph of the particle distribution before and after rolling for the positive electrode active material manufactured in Example 3.
[0236] Figure 6 is a graph of the particle distribution before and after rolling for the positive electrode active material manufactured in Example 4.
[0237] Figure 7 is a graph of particle distribution before and after rolling for the positive electrode active material manufactured in Comparative Example 1.
[0238] Figure 8 is a graph of particle distribution before and after rolling for the positive electrode active material manufactured in Comparative Example 2.
[0239] Figure 9 is a graph of particle distribution before and after rolling for the positive electrode active material manufactured in Comparative Example 3.
[0240] Figure 10 is a graph of particle distribution before and after rolling for the positive electrode active material manufactured in Comparative Example 4.
[0241]
[0242] Experimental Example 2
[0243] Life Characteristics Assessment
[0244] Lithium secondary batteries were manufactured using each positive electrode manufactured in Experimental Example 1, and the life characteristics of each lithium secondary battery were evaluated.
[0245] At this time, a lithium metal disk was used as the negative electrode, and an electrode assembly was manufactured by interposing a separator between the positive and negative electrodes, and then this was placed inside a battery case, and an electrolyte was injected into the case to manufacture a lithium secondary battery. At this time, an electrolyte was used in which 1 M LiPF6 was dissolved in an organic solvent mixed with ethylene carbonate: ethyl methyl carbonate: diethyl carbonate in a volume ratio of 3:3:4.
[0246] Next, each manufactured lithium secondary battery was charged in CC / CV mode at a constant current of 0.1C at 25°C to 4.25 V (CV 0.05 C), and then discharged in CC mode until it reached 3.0 V, and the initial charge capacity and discharge capacity were measured for the first time.
[0247] In addition, after performing CC / CV mode charging up to 4.25 V in the range of 3.0 to 4.25 V at 45°C (CV 0.05C), charging and discharging in CC mode until the voltage reached 3.0 V was considered one cycle, and the cycle was repeated 50 times to measure the capacity retention rate (discharge capacity at 50 cycles / initial discharge capacity × 100) of each lithium secondary battery at 50 cycles. The measurement results are shown in Fig. 11 and Table 2 below.
[0248]
[0249] Figure 11 is a graph showing the capacity (mAh / g) according to cycle of secondary batteries including positive electrode active materials manufactured in Examples and Comparative Examples. Specifically, A* represents data for Example 1, B* represents data for Example 2, C* represents data for Example 3, D* represents data for Example 4, E* represents data for Comparative Example 1, F* represents data for Comparative Example 2, G* represents data for Comparative Example 3, and H* represents data for Comparative Example 4.
[0250]
[0251] Fine powder content of 1 ㎛ or less before rolling (%) Fine powder content of 1 ㎛ or less after rolling (%) Initial charge capacity (25℃) (mAh / g) Initial discharge capacity (25℃) (mAh / g) Capacity retention rate (50 cycles) (%) Example 102.05 229.2 202.39 6.1 Example 201.46 230.6 203.196.2 Example 300.76 232.4 206.196.6 Example 40.46 1.93 229.3 202.196.2 Comparative example 1093.79 222.3 200.194.8 Comparative example 2018.16 230.1208.595.1 Comparative example 30.59 11.39 228.9 201.49 3.3 Comparative example 4010.71228.4200.994.1
[0252] As can be confirmed in Table 2 above, in the case of the positive electrode active materials manufactured in Examples 1 to 4, the positive electrode active materials had a pressure of 6,500 kgf / cm 2 When pressure was applied, it was confirmed that the content of fine particles with a particle size of 1 ㎛ or less was 10% by volume or less based on the total volume of the positive electrode active material after pressure was applied. On the other hand, in the case of the positive electrode active materials manufactured in Comparative Examples 1 to 4, the positive electrode active material was subjected to a pressure of 6,500 kgf / cm 2 When pressure was applied, it was confirmed that the content of fine particles having a particle size of 1 ㎛ or less was more than 10% by volume based on the total volume of the positive electrode active material after the pressure was applied. Meanwhile, in the case of secondary batteries including the positive electrode active materials manufactured in Examples 1 to 4, it was confirmed that the capacity retention rate was superior to that of secondary batteries including the positive electrode active materials manufactured in Comparative Examples 1 to 4. In addition, in the case of secondary batteries including the positive electrode active materials manufactured in Examples 1 to 4, it was confirmed that the initial charge capacity was 229.2 mAh / g or more, and the initial discharge capacity was 202.1 mAh / g or more.
Claims
1. Contains lithium transition metal oxide in the form of single particles, The above lithium transition metal oxide contains nickel in an amount of 60 mol% or more among the total transition metals, 6,500 kgf / cm for positive electrode active material 2 A positive electrode active material having a fine particle content of 1 ㎛ or less in particle size of 1 ㎛ or less based on the total volume of the positive electrode active material after applying pressure, wherein the content is 10% by volume or less.
2. In paragraph 1, The above positive electrode active material has an average particle diameter (D 50 ) A positive electrode active material having a diameter of 2 ㎛ or more and 12 ㎛ or less.
3. In paragraph 1, The above positive electrode active material has a particle strength of 500 Mpa or more and 1,500 Mpa or less, The above particle strength (MPa) is a value obtained by collecting a sample of lithium transition metal oxide particles, placing the collected sample on glass, and applying a pressure of 100 mN to the sample with a tip until the particle breaks and the tip touches the glass on which the sample is placed.
4. In paragraph 1, The above positive electrode active material is a positive electrode active material having a composition represented by the following chemical formula 1: [Chemical Formula 1] Li a Ni x Co y M 1 z M 2 1-x-y-z O2 In the above chemical formula 1, M 1 is at least one selected from the group consisting of Mn and Al, M 2 is at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf, 1.0≤a≤1.3, 0.6≤x<1.0, 0 <y<0.4, 0<z<0.4, 0≤1-x-y-z≤0.4이다.
5. In paragraph 1, A positive electrode active material having a fine powder content of 1 ㎛ or less in particle size before rolling of 0% or more and 1% or less based on the total number of the above positive electrode active materials. 6.1) A step of mixing a positive electrode active material precursor containing nickel at 60 mol% or more of the total transition metal and a lithium-containing raw material, heating the mixture to a first firing temperature, and performing a first firing to manufacture a plastic product; 2) A step of cooling the above plastic product to room temperature; and 3) A method for producing a cathode active material, comprising the steps of mixing the above-mentioned plastic product and lithium-containing raw material, heating to a secondary firing temperature, and performing a secondary firing to produce a lithium transition metal oxide in the form of single particles; A method for manufacturing a positive electrode active material, wherein the first firing temperature is 850°C or more and 950°C or less, the second firing temperature is 800°C or more and 850°C or less, and the second firing temperature is lower than the first firing temperature.
7. In paragraph 6, A method for manufacturing a positive electrode active material, wherein the heating rate of step 1) and the heating rate of step 3) are each 4°C / min or more and 7°C / min or less.
8. In paragraph 6, A method for manufacturing a positive electrode active material, further comprising the step of crushing the above-mentioned plastic product before the secondary firing in step 3).
9. In paragraph 6, 3-1) A method for manufacturing a positive electrode active material, further comprising a step of crushing the above secondary sintered product.
10. A positive electrode comprising a positive electrode active material according to any one of claims 1 to 5.
11. The anode according to Article 10; cathode; a separator interposed between the anode and the cathode; and A lithium secondary battery comprising an electrolyte.
Citation Information
Patent Citations
System of manufacturing bi-cell of all-solid-state battery
KR1020230149037A
Machine learning-based perimeter intrusion detection system using radar
KR102377226B1
An air purification and sterilization system using electric precipitation and ozone
KR102454605B1
Data driving device and method for driving the same
KR1020210129327A
Manufacturing method of recycled polyvinyl chloride and manufacturing device of recycled polyvinyl chloride