Methods of making high performance aluminum-zirconium antiperspirant active powders containing calcium and glycine with low zirconium content
The method of heating a basic aluminum chloride hydroxide solution with calcium and glycine, then mixing with zirconium hydroxychloride, addresses the economic and stability issues of high zirconium content antiperspirant salts by producing aluminum-zirconium antiperspirant powders with high HPLC peak 4 content and low zirconium and glycine amounts, achieving enhanced efficacy and stability.
Patent Information
- Application Number
- PCT/US2023/086190
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2023-12-28
- Publication Date
- 2024-12-05
AI Technical Summary
Current commercial antiperspirant salts with high zirconium content are economically unfavorable due to high costs and instability, and there is a need for activated aluminum-zirconium antiperspirant powders with high HPLC peak 4 content and low zirconium and glycine contents.
A method involving heating a basic aluminum chloride hydroxide solution with a calcium salt and an amino acid to form an activated solution, then mixing it with a zirconium hydroxychloride solution and drying to produce an aluminum-zirconium antiperspirant active powder with high HPLC peak 4 content, optimizing the sequence of adding glycine to enhance performance and stability.
The method results in aluminum-zirconium antiperspirant powders with high HPLC peak 4 content and low zirconium and glycine amounts, offering enhanced efficacy and stability, suitable for commercial use with improved flowability and performance.
Smart Images

Figure US2023086190_05122024_PF_FP_ABST
Abstract
Description
GULBRA 3.4-007 METHOD OF MAKING HIGH PERFORMANCE ALUMINUM-ZIRCONIUM ANTIPERSPIRANT ACTIVE POWDERS CONTAINING CALCIUM AND GLYCINE WITH LOW ZIRCONIUM CONTENT CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] The present application claims the benefit of the filing date of United States Provisional Patent Application No.63 / 504,529, filed on May 26, 2023, the disclosure of which is hereby incorporated herein by reference. BACKGROUND OF THE INVENTION
[0002] Activated antiperspirant actives having high HPLC peak 4 are in high demand commercially due to their high performance, i.e., strong capability to reduce sweat production. There are several methods to manufacture such actives. One commonly used method involves diluting a basic aluminum chloride hydroxide (BAC) solution from a concentration of 50% to 10-20%, heating the diluted solution for several hours, and then quickly drying the diluted and heated solution to a powder, due to instability of the solution. The resultant powder is called activated aluminum chlorohydrate (ACH), i.e., AACH, or activated aluminum sesquichlorohydrate (AASCH), which has high HPLC peak 4 content of at least 20% or the HPLC peak 4 to peak 3 area ratio of at least 0.5. Zirconium can also be introduced during the process to prepare activated aluminum-zirconium salts.
[0003] Lately, it has been found when calcium and glycine are present in the ACH and AASCH solutions, and the solutions are heated to higher temperature at relatively high concentration, such as 25% to 35%, higher HPLC peak 4 aluminum species are formed. The species are also stable in the solutions, meaning that the species do not convert back to low peak 4 aluminum species quickly. Zirconium can be introduced during the process to further increase efficacy of the salts. However, due to the high hygroscopicity of the active salts, there are currently no activated Al-Zr powder actives containing calcium and glycine available commercially.
[0004] It is well understood that the introduction of zirconium species to the aluminum salt depolymerizes the higher molecular weight aluminum species into lower molecular weight aluminum species, along with causing formation of aluminum dimer and monomer species. Such changes in aluminum structures and the faster hydrolysis rates of the zirconium complexes result in an increased efficacy. It is generally accepted that the presence of higher amounts of zirconium complexes further increases the efficacy of the aluminum-zirconium antiperspirant salts. Further, the known commercial antiperspirant salts claiming to have strong antiperspirancy and or deodorancy are those with high zirconium content, such as aluminum-zirconium-tetra- or-trichlorohydrex glycine actives with Al / Zr mole ratio of less than 6.0 and mostly less than 4. Because zirconium species hydrolyze and precipitate at relatively lower pH than aluminum salts, an amino acid such as glycine is added in order to form a stable zirconium solution at higher pH. Higher glycine is thus required for the aluminum-zirconium salts containing higher zirconium. About 40% to 50% of glycine is considered sufficient in an aluminum- zirconium glycine solution (see AH Rosenberg; JJ Fitzgerald, Chemistry of Aluminum-Zirconium-GlycineGULBRA 3.4-007 (AZG) Complexes, Antiperspirants and Deodorants 5:137-166, 1999). The effect of high glycine (including both free and bounded) on the efficacy of the corresponding aluminum and aluminum-zirconium antiperspirant salts is uncertain. Further, since zirconium and glycine cost more than aluminum, it is economically beneficial to have antiperspirant actives having low zirconium and glycine contents. Therefore, a need exists for activated Al-Zr powders with high peak 4 content and low zirconium and glycine contents. BRIEF SUMMARY OF THE INVENTION
[0005] An aspect of the present disclosure includes a method of making an aluminum-zirconium antiperspirant active powder, may include heating a solution comprising a basic aluminum chloride hydroxide, an amino acid, and a calcium salt at a temperature of from 80 °C to 100 °C to form an activated solution having an HPLC peak 4 content of at least 55%; cooling the activated solution to a temperature of 50 °C or below to form a cooled solution; mixing the cooled solution with a zirconium hydroxychloride solution having the following empirical formula: ZrO(OH)bCl2-b, wherein 0<b<1 to form an aluminum- zirconium solution, and drying the aluminum-zirconium solution to form the aluminum-zirconium antiperspirant active powder. In some embodiments, the HPLC peak 4 content of the activated solution is from 55 % to 80%. In some embodiments, the aluminum-zirconium antiperspirant active powder has HPLC peak 4 content of from 60% to 80%.
[0006] In some embodiments, the heating may be performed for 30 minutes to 8 hours. In some embodiments, the heating is performed for 2 hours to 4 hours.
[0007] In some embodiments, the aluminum-zirconium antiperspirant active powder may be activated aluminum zirconium pentachlorohydrate glycine powder with calcium.
[0008] In some embodiments, the activated solution does not contain a zirconium compound.
[0009] In some embodiments, the basic aluminum chloride hydroxide may be aluminum sesquichlorohydrate. In some other embodiments, the basic aluminum chloride hydroxide may be aluminum chlorohydrate.
[0010] In some embodiments, the activated solution may include a complex having an empirical formula of Al2(OH)6-xClx(AA)y, wherein AA is the amino acid, 1.05<x<1.6, 0.15<y<1.0, wherein the activated solution may have an aluminum to calcium mole ratio of greater than 0.1:1 and to less than 0.8:1. In some embodiments, when x=5, metal to chloride ratio may be from 1.2 to 2.1 and aluminum to zirconium ratio may be from 6 to 10. In some embodiments, metal to chloride ratio may be from 1.51 to 2.1 and aluminum to zirconium ratio may be from 6 to 10.
[0011] In some embodiments, the method may further include dissolving a zirconium oxychloride compound into water and thermally treating to form a solution; and admixing the solution with a zirconium basic carbonate compound and aging to form the zirconium solution comprising the zirconium hydroxychloride.GULBRA 3.4-007
[0012] In some embodiments, the method may further include mixing at least one or more of HCl or AlCl3, aluminum chlorohydrate, water, the calcium salt, and the amino acid to prepare a concentrated solution comprising the basic aluminum chloride hydroxide in an amount of 25 to 45 wt%; and diluting the concentrated solution to provide a solution comprising the basic aluminum chloride hydroxide in an amount of 10 to 30 wt%, wherein the basic aluminum chloride hydroxide comprises aluminum chlorohydrate, aluminum sesquichlorohydrate, or a combination thereof. In some embodiments, the aluminum-zirconium antiperspirant active powder may have a molar ratio of total metals M to chlorine Cl (M:Cl) of greater than 1.5:1. In some embodiments, the solution may be a sesquichlorohydrate solution having a mole ratio of aluminum Al to chloride Cl (Al:Cl) of from 1.5-1.8:1. In some embodiments, the aluminum-zirconium antiperspirant active powder may have a molar ratio of aluminum Al to zirconium Zr (Al:Zr) of from 6 to10:1.
[0013] In some embodiments, the amino acid may include glycine, betaine, or a mixture thereof. In some embodiments, the aluminum-zirconium antiperspirant active powder may have the amino acid in an amount ranging from 5 and 10 wt%.
[0014] In some embodiments, the calcium salt may be at least one of calcium chloride, calcium bromide, calcium nitrate, calcium citrate, calcium acetate, calcium gluconate, calcium ascorbate, calcium lactate, calcium glycinate, calcium carbonate, calcium sulfate, calcium hydroxide, or a mixture thereof. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] FIG. 1 is a process diagram showing an in-line mixing setup of step III of Example 1, wherein the feed solution to the spray dryer is prepared by mixing a solution of AASCH glycine with calcium chloride and a ZHC solution.
[0016] FIG. 2 is a process diagram showing an in-line mixing setup of step III of Comparative Example 1, wherein the feed solution to the spray dryer is prepared by mixing AASCH, calcium chloride solution, and zirconium hydroxychloride solution.
[0017] FIG. 3 is a graph showing a comparison of HPLC-ICP results of Example 1 and Comparative Examples 1 to 7. DETAILED DESCRIPTION
[0018] Hereinafter, the present disclosure will be described in detail to aid in understanding of the present disclosure. As used herein, it will be understood that words or terms used in the specification and claims of the present disclosure shall not be construed as being limited to having the meaning defined in commonly used dictionaries. It will be further understood that the words or terms should be interpreted as having meanings that are consistent with their meanings in the context of the relevant art and the technical idea of the invention, based on the principle that an inventor may properly define the meaning of the words or terms to best explain the invention.GULBRA 3.4-007
[0019] Some embodiments of the disclosure are directed to a method of making an aluminum- zirconium antiperspirant active powder, which includes heating a pre-activated solution comprising a basic aluminum chloride hydroxide, an amino acid, and a calcium salt at a temperature of 80 °C to 100 °C, or 85-95 °C, or 80-90 °C, for 4-8 hours, or 2.5-4.5 hours, or 2-3 hours, to form an activated solution having an HPLC peak 4 content of at least 55%, cooling the activated solution to a temperature below 60 °C, or below 55 °C or below 50 °C, mixing the cooled solution with a zirconium solution to form an aluminum- zirconium solution, and drying the aluminum-zirconium solution to form the aluminum-zirconium antiperspirant active powder. In some embodiments, the mixing maybe performed via co-mixing or in- line mixing. In some embodiments, heating of the solution having a basic aluminum chloride hydroxide, an amino acid, and a calcium salt is performed at a temperature of from 80 °C to 100 °C to form an activated solution having an HPLC peak 4 content of from 55% to 80%. In some embodiments, heating of the solution having a basic aluminum chloride hydroxide, an amino acid, and a calcium salt is performed at a temperature of from 80 °C to 100 °C to form an activated solution having an HPLC peak 4 content of from 55% to 75%, 55% to 70% or 55% to 65%.
[0020] The present inventors found that Al-Zr salts containing calcium and glycine can be prepared with good flowability and performance by the novel method described herein. Further, the present inventors found that controlling the sequence of the addition of glycine, which is generally considered as a buffer, to the aluminum stream or the zirconium stream has a great impact on the performance of the resultant Al-Zr-Ca-Glycine salts. According to one or more embodiments, in a preferred method, glycine can be added to the Al stream, i.e., glycine is added to the BAC and CaCl2 solution and forms an Al-Ca- glycine solution, which is heat treated to form an Al-Ca-glycine solution having high peak 4 content of at least 55%, which is then mixed with a Zr stream to form an Al-Zr-Ca-Glycine salt, and the solution can be dried. The resultant Al-Zr-Ca-Glycine salts prepared by addition of glycine to the Al stream have optimum Al chemistry. According to one or more embodiments, in an alternative method, glycine can be added to the Zr stream to form Zr-glycine compounds to prevent Zr from further polymerization upon mixing with Al stream. The resultant Al-Zr-Ca-Glycine salts prepared by addition of glycine to the Zr stream have optimum Zr chemistry. The present inventors found that the Al-Zr-Ca-Glycine salt with optimum Al chemistry prepared according to the present disclosure has better performance compared to the salt with optimum Zr chemistry, especially at low Zr content. In the present disclosure, the Al-Zr-Ca-Glycine salts may have high HPLC peak 4 contents of at least 60%. In some embodiments, Al-Zr-Ca-Glycine salts have high HPLC peak 4 contents from 60% to 80 %. In some embodiments, Al-Zr-Ca-Glycine salts have high HPLC peak 4 contents from 60% to 75 %, 60% to 70 % or 60% to 65 %.
[0021] The powders can be easily manufactured by spray drying the Al-Zr-Ca-Glycine salts. The powders can be formulated into an antiperspirant stick for topical application to a human body. In some embodiments, after spray drying, the powders are micronized to provide particles having a particle sizeGULBRA 3.4-007 distribution wherein at least 70%, or at least 80%, or at least 90% of the particles are less than 10 microns and at least 90%, or at least 95%, or at least 99% of the particles are less than 45 microns. In some embodiments, the method further includes micronizing the active powder, emulsifying the micronized powder, and cooling the emulsion to form the antiperspirant stick. Such emulsifying may include admixing one or more of an emulsifier, an emollient, an oil, and a thickener to prepare an emulsion composition, disposing the micronized aluminum-zirconium antiperspirant active powder in a dispersant to form a dispersion having an anhydrous solids content of about 20 wt%, and admixing the emulsion composition with the dispersion to form the antiperspirant emulsion. Such cooling may include cooling the antiperspirant emulsion at a first cooling temperature of 75-80°C, pouring the cooled antiperspirant emulsion into a mold, and cooling the mold at a second cooling temperature below 50°C to form the antiperspirant stick.
[0022] The present application discloses enhanced efficacy aluminum-zirconium antiperspirant salt compositions comprising relatively low amino acid and zirconium amounts, which are activated at metal to chloride (M / Cl) mole ratios of greater than 1.1, or greater than 1.3, or greater than 1.5, or less than 2.0, or less than 1.8, or less than 1.6. The compositions are prepared by the reaction of a BAC solution, calcium chloride, amino acid or buffer, and zirconium compounds. According to some embodiments, the activated solution comprises a complex having the following empirical formula: Al2(OH)6-xClx(Glycine)y, wherein, 1.05<x<1.6, and 0.15<y<1.0. The BAC solution contains calcium salt having aluminum to calcium mole ratio of greater than 0.1:1 and less than 0.8:1. According to some embodiments, any one or more of the aluminum-zirconium solution, the aluminum-zirconium salt, or the aluminum-zirconium powder includes an Al-Zr-Glycine-Ca, wherein aluminum to zirconium molar ratio is from 6 to 10, with metal (Al+Zr) to chloride molar ratio is from 1.2 to 1.6. In some further embodiments, the salt may be a “penta” salt, that is, a salt of M / Cl ratio of 1.51 and above. In some embodiments, the salt may be an “octa” salt, that is a salt of M / Cl ratio of 1.2 to 2.1.
[0023] According to some embodiments, the BAC solution for the present disclosure includes an aluminum chlorohydrate, an aluminum sesquichlorohydrate, or a combination thereof. The aluminum chlorohydrate and the aluminum sesquichlorohydrate each independently have an empirical formula of: Al2(OH)6-xClx, wherein 0.95<x<1.6, or 0.95<x<1.05, or 1.05<x<1.6. In some embodiments, the aluminum chlorohydrate has x = 1. In some embodiments, the aluminum sesquichlorohydrate has x = 1.2 The ASCH can be prepared by both direct and indirect processes at 25% to 45%, or 30% to 40% by weight solution concentrations. The direct process relates to the direct reaction between AlCl3 or HCl aqueous solution with Al metal including Al powder and pellet and the indirect process corresponds to the reaction of ACH or ASCH solution with AlCl3 or HCl. The BAC solution may be formed at high concentration and can be diluted to 10-35 wt%, or 10-30 wt% before activation.
[0024] The zirconium compound has the formula: ZrO(OH)bCl2-b, wherein 0<b<1. Zirconium Hydroxy Chloride (ZHC) can by prepared by mixing basic zirconium carbonate with HCl or zirconyl chloride aqueous solution at elevated temperatures, such as 60-90 °C or 70-80 °C for about 30 minutes, about 45 minutes, or about 60 minutes. The molar ratios of Al / Cl of the ASCH solutions and the Zr / Cl ofGULBRA 3.4-007 the ZHC solutions can be varied depending on the M / Cl ratios of the final Al-Zr solutions and powders. The ASCH solutions have Al / Cl molar ratios of 1.25 to 1.9, or 1.3 to 1.9, preferably 1.5 to 1.8, and the ZHC solutions with Zr / Cl ratios of 0.3 to 1.2, preferably 0.5 to 1.0, most preferably 0.7 to 0.8. The Al / Zr molar ratio can be varied from about 3 to about 10, preferably from about 5 to about 10 and most preferably from about 8 to about 10. The aluminum-zirconium salts thus prepared have a M / Cl molar ratio of more than 1.2, or more than 1.3, preferably more than 1.5, or less than 2.0, or less than 1.8, or less than 1.6.
[0025] In some embodiments, the amino acid is glycine, betaine, or a mixture thereof. In some embodiments, the aluminum-zirconium antiperspirant active powder comprises the amino acid in an amount between 5 and 10 wt%, or between 6 and 9 wt%, or between 7 and 8 wt%. In some embodiments, the calcium salt is selected from the group consisting of calcium chloride, calcium bromide, calcium nitrate, calcium citrate, calcium acetate, calcium gluconate, calcium ascorbate, calcium lactate, calcium glycinate, calcium carbonate, calcium sulfate, calcium hydroxide, and a mixture thereof. In some embodiments, the aluminum-zirconium antiperspirant active powder comprises the calcium in an amount between 0.2% and 5 wt%, or between 0.5 and 4 wt%, or between 1 and 3 wt%. In some embodiments, the method further comprises the topical application to the human body of an antiperspirant composition, which may be in a stick form.
[0026] The characterization of aluminum and zirconium species in aluminum-zirconium antiperspirant salts are determined by the following methods.
[0027] HPLC (Size Exclusion Column)
[0028] The degree of the polymerization of aluminum complexes is determined by Size Exclusion Chromatography (SEC) operated via a High Performance Liquid Chromatograph (HPLC) instrument. In this technique, the highest molecular weight Al species are eluted first and are designated as peaks 1 & 2 or otherwise called Band I. Peak 3 (or Band II) and peak 4 (or Band III) are due to intermediate molecular weight Al complexes. Peak 5 or Band IV is due to the lowest molecular weight Al complexes, including monomers and dimmers. The relative area of one or more peaks is determined in order to characterize the distribution of polymeric species in aluminum complexes formed. The aluminum and aluminum-zirconium antiperspirant salts of the present disclosure have SEC-HPLC peak 4 or Band III peak area of at least 55%, or at least 60%.
[0029] Inductively Coupled Plasma Spectroscopy (ICP) SEC-HPLC
[0030] The present disclosure employs ICP-SEC-HPLC analysis to study the polymerization of zirconium species and the distribution of the aluminum polymers. The size exclusion column operated by HPLC has been used to separate the aluminum and zirconium polymers by size. The separated species are sent to the ICP instead of a refractive index (RI) detector as in regular HPLC. The invention will be further illustrated by the following examples. In the examples, parts are by weight unless otherwise specified.
[0031] EXAMPLES
[0032] Example 1GULBRA 3.4-007 Preparation of Activated Aluminum Zirconium Pentachlorohydrex Glycine powder with Calcium by using Aluminum Sesquichlorohydrex Glycine solution with CaCl2 and Zirconium Hydroxychloride solution
[0033] Step-I: Preparation of Activated Aluminum Sesquichlorohydrate Glycine solution with CaCl2
[0034] Table 1 provides a list of the materials and the amounts thereof used to prepare the activated aluminum sesquichlorohydrate Glycine solution with CaCl2: Table 1 No Material name Quantity 1 ACH solution (BACS) 45.5 gm 2 Hydrochloric Acid 1.5 gm 3 Water 46.3 gm 4 Calcium Chloride dihydrate 3.7 gm 5 Glycine 3.0 gm 6 Total 100.0 gm
[0035] Aluminum-Ca-Glycine solution (Aluminum Activation by Calcium, glycine and water) was prepared by adding Hydrochloric acid into aluminum chlorohydrate (ACH) followed by water, CaCl2and Glycine to make Aluminum Sesquichlorohydrex (ASCH) Glycine solution with Calcium Chloride. The resultant solution had approximately 20% anhydrous solids which was thermally treated for about 2 hours at 85 to 1000C. The hot solution was cooled down to below 500C and used as an Aluminum stream. Table 2 provides the Al / Cl mole ratios and HPLC peak contents of AASCH Glycine solution with Calcium Chloride. Table 2 Sp. Al% Cl% Ca% *Al / Cl mole %HPLC %HPLC %HPLC Gravity ratio Peak 3 Peak 4 Peak 5 1.1994 5.98 6.06 0.82 1.70:1 36.27 57.36 4.51 *Al / Cl mole ratio is calculated excluding the chloride from CaCl2.
[0036] Step-II Preparation of Zirconium Hydroxychloride solution
[0037] Table 3 provides a list of the materials and the amounts thereof used to prepare the zirconium hydroxychloride solution: Table 3 No. Material name Quantity 1 Water 36.7 gm 2 Zirconium Oxychloride 41.8 gm 3 Zirconium Basic Carbonate 21.5 gm Total 100 gmGULBRA 3.4-007
[0038] Zirconium Hydroxychloride solution was prepared by dissolving Zirconium Oxychloride (ZOC) into the hot water followed by thermal treatment to 70-800C. To this hot ZOC solution, Zirconium Basic Carbonate (ZBC) was added, and the resulting solution was aged at 70-800C for a minimum of 45 minutes. Quality of the Zirconium Hydroxychloride solution is as below. The hot solution was cooled down to below 500C and used as a Zirconium Hydroxychloride solution stream.
[0039] Table 4 provides the Zr / Cl mole ratios and specific gravity of the prepared zirconium hydroxychloride solution (“ZHC solution”). Table 4 Sp. Gravity Zirconium Chloride **Zr / Cl mole ratio 1.39 18.10% 9.14% 0.75:1 **Zr / Cl ratio is calculated excluding the chloride from Calcium Chloride
[0040] Step-III Feed solution Preparation, Spray drying and Micronization
[0041] As illustrated in the process diagram of FIG.1, a solution feed of AASCH Glycine solution with Calcium Chloride and a ZHC solution were in-line mixed, and the resultant was pumped to the spray dryer.
[0042] Table 5 provides a list of the materials and the amounts thereof used to prepare the feed solution including AASCH Glycine solution with Calcium Chloride and a ZHC solution. Table 5 No. Material name Quantity 1 AASCH Glycine solution with CaCl2 88.3 gm 2 Zirconium Hydroxychloride solution 11.7 gm 3 Total 100 gm
[0043] Table 6 provides the properties of the resulting Activated Aluminum Zirconium Pentachlorohydrex Glycine powder with CaCl2. Table 6 No. Parameter Results 1. Appearance Off white 2. pH (15% w / w in water) 3.40 3. LOD (105°C / 2hrs) 5.08 4. Aluminum (%) 17.45 5. Zirconium (%) 7.41 6. Chloride (%) 20.84 7. Calcium (%) 2.26GULBRA 3.4-007 8. Glycine (%) 8.57 9. Al / Zr mole ratio 8.11:1 10. Metals / Cl Active mole ratio 1.53:1 11. Fe in ppm 43 ppm 12. % Anhydrous 72.05 13. HPLC Peak 1+2 1.32% 14. HPLC Peak 3 30.15% 15. HPLC Peak 4 61.57% 16. HPLC Peak 5 6.97% 17. Particle Size %< 10 um 86.09 18. Particle Size %< 45 um 100
[0044] Comparative Example 1 Preparation of Activated Aluminum Zirconium Pentachlorohydrex Glycine powder with CaCl2using starting material ASCH solution, ZHC-Glycine solution and CaCl2aqueous solution as the feed compositions.
[0045] Step-I (Preparation of Activated-Aluminum Sesquichlorohydrate solution)
[0046] ASCH solution was prepared by treating the Hydrochloric acid with ACH in presence of water at elevated temperature. The ASCH was diluted with water and heat treated to form the AASCH. The AASCH solution was mixed with ZHC-Glycine solution and CaCl2aqueous solution simultaneously to make the feed-stock.
[0047] Table 7 provides the Al / Cl mole ratios and specific gravity of the prepared zirconium hydroxychloride solution (“ZHC solution”) Sp. Gravity Aluminum Chloride Al / Cl mole ratio % HPLC Peak 4 1.0944 4.02% 2.98% 1.77:1 49.54
[0048] Step-II Preparation of Zirconium Hydroxychloride Glycine solution
[0049] Table 8 provides a list of the materials and the amounts thereof used to prepare the zirconium hydroxychloride glycine solution. Table 8 No. Material name Quantity 1 Water 16.1 gm 2 Zirconium Oxychloride (ZOC) 32.1 gm 3 Zirconium Basic Carbonate (ZBC) 16.1 gmGULBRA 3.4-007 4 Glycine 13.5 gm 6 Total 100 gm
[0050] Zirconium Hydroxychloride Glycine solution was prepared by dissolving ZOC into hot water followed by thermal treatment to 70-800C reaction temperature. To this hot ZOC solution, ZBC powder was charged, and the resulting solution was aged at 70-800C for a minimum of 45 minutes. Glycine was charged at 65-800C temperature into the batch and temperature was maintained to 70-800C for a minimum of 1.5 hours. Below was the quality of the ZHC-Glycine solution. Table 9 provides the Zr / Cl mole ratios and specific gravity of the prepared zirconium hydroxychloride solution. Table 9 Sp. Gravity Zirconium Chloride Zr / Cl mole ratio 1.456 17.29% 9.32% 0.71:1
[0051] Step-III Preparation of CaCl2 solution from CaCl2*2H2O crystals
[0052] Table 10 provides a list of the materials and the amounts thereof used to prepare the calcium solution. Table 10 No. Material name Quantity 1 CaCl2*2H2O 50.0 gm 2 Water 50.0 gm 3 Total 100 gm
[0053] CaCl2*2H2O was put into the beaker, water was added at 1:1 weight ratio. The mixture was agitated until a clear solution was obtained.
[0054] Table 11 provides the specific gravity the amounts of chloride and calcium and turbidity of the calcium solution. Table 11 Sp. Gravity Chloride Calcium Turbidity 1.3702 24.63% 13.12% 84 ntu
[0055] Step IV: Feed solution preparation, Spray drying and Micronization
[0056] As illustrated in the process diagram of FIG.2, an AASCH solution, a CaCl2solution, and a ZHC-Glycine solution were in-line mixed, and the resultant was pumped to the spray dryer.
[0057] Table 12 provides a list of the materials and the amounts thereof used to prepare the feed solution for spray drying including AASCH solution, a CaCl2solution, and a ZHC-Glycine solution.GULBRA 3.4-007 Table 12 No. Material name Quantity 1 AASCH solution 87.2 gm 2 ZHC solution 8.4 gm 3 CaCl2aqueous solution 4.4 gm 4 Total 100.0 gm
[0058] Table 13 provides the properties of the resulting Activated Aluminum Zirconium Pentachlorohydrex powder with CaCl2.Table 13 No. Parameter Results 1. Appearance Off white 2. pH (15% w / w in water) 3.58 3. LOD (105° / 2hrs) 4.60 4. Aluminum (%) 17.03 5. Zirconium (%) 7.01 6. Chloride (%) 20.84 7. Calcium (%) 2.49 8. Glycine (%) 7.04 9. Al / Zr mole ratio 8.37:1 10. Metals / Cl Active mole ratio 1.52:1 11. Fe in ppm 77 12. % Anhydrous 69.93 13. HPLC Peak 1+2 1.44% 14. HPLC Peak 3 49.52% 15. HPLC Peak 4 43.11% 16. HPLC Peak 5 5.93% 17. Particle Size % < 10 um 85.51 18. Particle Size % < 45 um 100
[0059] Comparative Example 2 Making of Aluminum Zirconium Pentachlorohydrex Glycine powder with CaCl2 using starting material ASCH solution, ZHC solution and CaCl2 solution
[0060] Step-I Preparation of activated Aluminum Sesquichlorohydrate solution
[0061] Aluminum Sesquichlorohydrate solution was prepared by direct process, i.e., reacting Hydrochloric acid with Aluminum ingot in the presence of water at elevated temperature. The batch wasGULBRA 3.4-007 pulled when the desired Al / Cl mole ratio (i.e., between 1.70:1 and 1.80:1). The solution was filtered to achieve desired clarity subsequently, the solution was diluted with water and heat treated to form the AASCH solution.
[0062] Table 14 provides the properties of the activated Aluminum Sesquichlorohydrate solution after water dilution and thermal treatment. Table 14 Parameter Aluminum Chloride Al / Cl ratio HPLC Peak 4 Results 4.0% 3.0% 1.77:1 55.3%
[0063] Step-II Preparation of Zirconium Hydroxychloride Glycine solution
[0064] Table 15 provides a list of the materials and the amounts thereof used to prepare the zirconium hydroxy glycine solution. Table 15 No. Material name Quantity 1 Water 22.3 gm 2 Zirconium Oxychloride (ZOC) 40.4 gm 3 Zirconium Basic Carbonate (ZBC) 20.3 gm 4 Glycine 17.0 gm 6 Total 100 gm
[0065] Zirconium Hydroxychloride Glycine solution was prepared by dissolving Zirconium Oxychloride (ZOC) into hot water followed by thermal treatment at 70-800C. To this hot solution, Zirconium Basic Carbonate (ZBC) was charged, and the resulting Zirconium Hydroxychloride solution was aged at 70-800C for a minimum of 45 minutes. Glycine was then charged in hot solution and the material was further aged at 70-800C for a minimum 1.5 hours. A clear yellow solution was obtained.
[0066] Table 15 provides the properties of the Zirconium Hydroxychloride Glycine solution. Table 15 Parameter Results Sp. Gravity 1.4562 Turbidity 6 ntu Zirconium 17.29% Chloride 9.32% Zr / Cl mole ratio 0.71:1
[0067] Step-III Preparation of Calcium Chloride solutionGULBRA 3.4-007
[0068] Calcium Chloride dihydrate was dissolved in the water at ambient temperature (1:1) and thus a clear CaCl2 solution was obtained. Table 16 provides the properties of the calcium chloride solution. Table 16 Parameter Results Sp. Gravity 1.3702 Turbidity 84 ntu Chloride 24.63% Calcium 13.12%
[0069] Step-IV Feed solution preparation, Spray drying and Micronization
[0070] Table 17 provides a list of the materials and the amounts thereof used to prepare the feed solution for spraying drying. Table 17 No. Material name Quantity 1 Activated-Aluminum Sesquichlorohydrate solution 87.3 gm 2 Zirconium Hydroxychloride Glycine solution 8.2 gm 3 Calcium Chloride-Aqueous solution 4.5 gm 4 Total 100 gm
[0071] The spray dried powder was micronized into the mill to achieve desired particle size required to make a stick formulation.
[0072] Table 18 provides the properties of the resulting Activated Aluminum Zirconium Pentachlorohydrex Glycine powder with CaCl2. Table 18 Sr. No. Parameter Results 1. Appearance Off white 2. pH (15% w / w in water) 3.65 3. LOD (105°C / 2hrs) 5.30% 4. Aluminum (%) 16.92 5. Zirconium (%) 7.02 6. Chloride (%) 20.27 7. Calcium (%) 2.37 8. Glycine (%) 7.34 9. Al / Zr mole ratio 8.31:1GULBRA 3.4-007 10. Metals / Cl Active mole ratio 1.55:1 11. Fe in ppm 78 12. % Anhydrous 69.44 13. HPLC Peak 1+2 0.78% 14. HPLC Peak 3 48.79% 15. HPLC Peak 4 45.54% 16. HPLC Peak 5 4.89% 17. Particle Size % < 10 um 85.36 18. Particle Size % < 45 um 100
[0073] Comparative Example 3 Preparation of Activated Aluminum Zirconium Pentachlorohydrex Glycine powder with Calcium using the feed solution comprising AASCH solution, ZHC Glycine solution and CaCl2
[0074] Step-I Preparation of AASCH solution
[0075] To the ACH solution, HCl was added to achieve desired Al / Cl ratio followed by water dilution and thermal treatment for aluminum activation. The resulting AASCH solution was mixed with ZHC-Glycine solution with CaCl2to make the feed-stock.
[0076] Table 19 provides the properties of the AASCH solution. Table 19 Sp. Gravity Aluminum Chloride Al / Cl mole ratio HPLC Peak 4 (by area%) 1.0953 4.05% 3.0% 1.77:1 49.88
[0077] Step-II Preparation of Zirconium Hydroxychloride Glycine solution with CaCl2
[0078] Table 20 provides a list of the materials and the amounts thereof used to prepare the zirconium hydroxychloride glycine solution with CaCl2: Table 20 No. Material name Quantity 1 Water 21 gm 2 Zirconium Oxychloride 31 gm 3 Zirconium Basic Carbonate 17 gm 4 Glycine 13 gm 5 Calcium Chloride di-hydrate 18 gm 6 Total 100 gmGULBRA 3.4-007
[0079] ZHC solution with CaCl2 was prepared by dissolving ZOC into hot water followed by thermal treatment to attend 70-800C reaction temperature. To this hot ZOC solution, ZBC powder was charged, and the resultant solution was aged at 70-800C for a minimum of 45 minutes. Glycine was charged at 65-800C temperature into the batch and temperature was maintained to 70-800C for a minimum of 1.5 hours. The resulting solution was cooled down to below 500C and CaCl2*2H2O flake was charged and agitated till complete dissolution. Below is the quality of the ZHC-Glycine solution with Calcium Chloride.
[0080] Table 21 provides the properties of the ZHC-Glycine solution with Calcium Chloride. Table 21 Sp. Gravity Zirconium Chloride Calcium Zr / Cl ratio 1.5408 13.49% 17.04% 5.6% 0.73:1
[0081] Step-III Feed solution preparation, Spray drying and Micronization
[0082] Table 22 provides a list of the materials and the amounts thereof used to prepare the feed solution for spray drying: Table 22 Sr. No. Material name Quantity 1 AASCH solution 89 gm 2 ZHC-Glycine-CaCl2 solution 11 gm 3 Total 100 gm
[0083] Table 23 provides the properties of the resulting Activated Aluminum Zirconium Pentachlorohydrex Glycine powder. Table 23 Sr. No. Parameter Results 1. Appearance Off white 2. pH (15% w / w in water) 3.61 3. LOD (105° / 2hrs) 4.73% 4. Aluminum (%) 17.07 5. Zirconium (%) 7.06 6. Chloride (%) 20.60 7. Calcium (%) 2.58 8. Glycine (%) 6.95 9. Al / Zr mole ratio 8.33:1 10. Metals / Cl Active mole ratio 1.57:1GULBRA 3.4-007 11. Fe in ppm 84 12. % Anhydrous 70.0% 13. HPLC Peak 1+2 0.983% 14. HPLC Peak 3 49.20% 15. HPLC Peak 4 44.61% 16. HPLC Peak 5 5.21% 17. Particle Size % < 10 um 88.55 18. Particle Size % < 45 um 100
[0084] Comparative Example 4 Making Aluminum Zirconium Pentachlorohydrex glycine powder containing calcium using Aluminum Sesquichlorohydrate solution and Zirconium Hydroxychloride Glycine solution with CaCl2. Here, Aluminum Sesquichlorohydrate solution was directly prepared from Aluminum Metal, water and Hydrochloric acid.
[0085] Step-I Preparation of Activated Aluminum Sesquichlorohydrate solution
[0086] Table 24 provides a list of the materials and the amounts thereof used to prepare the activated aluminum sesquichlorohydrate solution: Table 24 Sr. No. Material name Quantity 1 ASCH solution 33 gm 2 Water 67 gm 3 Total 100 gm
[0087] Aluminum Sesquichlorohydrate solution was prepared by reacting the Hydrochloric acid with Aluminum metal in aqueous solution at elevated temperature. The batch was pulled at desired Al / Cl mole ratio (preferable Al / Cl atomic ratio: 1.70 to 1.80:1). The solution was filtered to achieve desired clarity. To the Aluminum Sesquichlorohydrate solution, water was added, and thermal treatment was applied for Aluminum activation. The resulting AASCH solution was mixed with ZHC-Glycine-CaCl2solution to make the feed-stock for spray drying.
[0088] Table 25 provides the properties of the activated aluminum sesquichlorohydrate solution. Table 25 Sp. Gravity Aluminum Chloride Turbidity Al / Cl atomic ratio % HPLC Peak 4 1.0914 4.04% 2.97% 14 ntu 1.79:1 54.88
[0089] Step-II Preparation of Zirconium Hydroxychloride Glycine solution with CaCl2GULBRA 3.4-007
[0090] Table 26 provides a list of the materials and the amounts thereof used to prepare the zirconium hydroxychloride glycine solution with CaCl2: Table 26 Sr. No. Material name Quantity 1 Water 21 gm 2 Zirconium Oxychloride 31 gm 3 Zirconium Basic Carbonate 17 gm 4 Glycine 13 gm 5 Calcium Chloride di-hydrate 18 gm 6 Total 100 gm
[0091] ZHC solution with CaCl2 was prepared by dissolving ZOC into hot water followed by thermal treatment to attend 70-800C reaction temperature. To this hot ZOC solution, ZBC powder was charged, and the resulting solution was aged at 70-800C for a minimum of 45 minutes. Glycine was charged at 65-800C temperature into the batch and temperature was maintained at 70-800C for a minimum of 1.5 hours. The resulting solution was cooled to below 500C and CaCl2*2H2O flake was charged and agitated until completely dissolved. Table 27 provides the properties of the ZHC-Glycine solution with Calcium Chloride. Table 27 Sp. Gravity Zirconium Chloride Calcium Zr / Cl ratio 1.5384 13.35% 16.96% 5.6% 0.72:1
[0092] Step-III Feed solution preparation, Spray drying and Micronization
[0093] Table 28 provides a list of the materials and the amounts thereof used to prepare the feed solution for spray drying: Table 28 Sr. No. Material name Quantity 1 AASCH solution 89 gm 2 ZHC-Glycine-CaCl2 solution 11 gm 3 Total 100 gm
[0094] Table 29 provides the properties of the resulting Activated Aluminum Zirconium Pentachlorohydrex Glycine powder with CaCl2.Table 29 Sr. No. Parameter Results 1. Appearance Off whiteGULBRA 3.4-007 Sr. No. Parameter Results 2. pH (15% w / w in water) 3.68 3. LOD (105° / 2hrs) 5.37 4. Aluminum (%) 17.34 5. Zirconium (%) 7.41 6. Chloride (%) 20.72 7. Calcium (%) 2.24 8. Glycine (%) 8.28 9. Al / Zr mole ratio 8.06:1 10. Metals / Cl Active mole ratio 1.53:1 11. Fe in ppm 90.73 12. % Anhydrous 71.69 13. HPLC Peak 1+2 1.03% 14. HPLC Peak 3 50.93% 15. HPLC Peak 4 42.96% 16. HPLC Peak 5 5.07% 17. Particle Size % < 10 um 87.04 18. Particle Size % < 45 um 100
[0095] Comparative Example 5 / / Al-Zr tetra ZAG powder Preparing Aluminum Zirconium tetrachlorohydrex Glycine powder using Aluminum Sesquichlorohydrate solution and Zirconium Hydroxychloride Glycine solution. Here, Aluminum Sesquichlorohydrate solution was used to prepared Aluminum Zirconium Tetrachlorohydrex Glycine powder and no heating is involved here.
[0096] Step-I Preparation of Aluminum Sesquichlorohydrate solution
[0097] Aluminum Sesquichlorohydrate solution was prepared by reacting Hydrochloric acid with aluminum metal in aqueous solution at elevated temperature and atmospheric pressure. The batch was pulled at desired Al / Cl mole ratio (Preferable 1.70:1 to 1.80:1). The solution was filtered to achieve desired clarity.
[0098] Table 30 provides the properties of aluminum sesquichlorohydrate solution. Table 30 Sp. Gravity Aluminum Chloride Al / Cl mole ratio Fe content 1.3735 12.70% 9.32% 1.79:1 25 ppm
[0099] Step-II Preparation of Zirconium Hydroxychloride Glycine solution
[0100] Table 31 provides a list of the materials and the amounts thereof used to prepare the zirconium hydroxychloride glycine solution:GULBRA 3.4-007 Table 31 Sr. No. Material name Quantity 1 Water 21.4 gm 2 Zirconium Oxychloride (ZOC) 42.1 gm 3 Zirconium Basic Carbonate (ZBC) 22.0 gm 4 Glycine 14.5 gm 6 Total 100 gm
[0101] Zirconium Hydroxychloride Glycine solution was prepared by dissolving Zirconium Oxychloride (ZOC) into the hot water followed by thermal treatment at 70-800C. To this hot solution, Zirconium Basic Carbonate (ZBC) was charged, and the resultant Zirconium Hydroxychloride solution was aged at 70-800C for a minimum of 45 minutes. Glycine was charged in the hot Zirconium Hydroxychloride solution and the batch was further aged at 70-800C for a minimum of 1.5 hours. Finally, a clear yellow solution was obtained.
[0102] Table 32 provides a list of properties of the zirconium hydroxychloride glycine solution. Table 32 Sp. Gravity Zirconium Chloride Zr / Cl mole ratio 1.4582 18.25% 9.21% 0.76:1
[0103] Step-III Feed solution preparation, Spray drying and Micronization
[0104] Table 33 provides a list of the materials and the amounts thereof used to prepare the feed solution for spray drying: Table 33 Sr. No. Material name Quantity 1 Aluminum Sesquichlorohydrate solution 60.0 gm 2 Zirconium Hydroxychloride Glycine solution 40.0 gm 3 Total 100 gm
[0105] Table 34 provides the properties of the resulting Activated Aluminum Zirconium Tetrachlorohydrex Glycine powders. Table 34 Sr. No. Parameter Results 1. Appearance Off white powder 2. Odor Characteristics 3. pH (15% w / w in water) 3.55GULBRA 3.4-007 Sr. No. Parameter Results 4. LOD (105° / 2hrs) 4.0% 5. Aluminum (%) 14.91 6. Zirconium (%) 14.04 7. Chloride (%) 17.68 8. Glycine (%) 11.02 9. Al / Zr mole ratio 3.66:1 10. Metals / Cl Active mole ratio 1.41:1 11. Fe in ppm 28 ppm 12. % Anhydrous 76.66% 13. HPLC Peak 1+2 13.37% 14. HPLC Peak 3 66.54% 15. HPLC Peak 4 8.18% 16. HPLC Peak 5 11.89% 17. Particle Size %< 10 um 87% 18. Particle Size %< 45 um 100
[0106] Comparative Example 6 Preparation of Aluminum Zirconium Pentachlorohydrex Glycine powder with CaCl2 using Aluminum Sesquichlorohydrate solution and ZHC-Glycine solution with CaCl2 as the feed solution
[0107] Step-I Preparation of Aluminum Sesquichlorohydrate solution
[0108] Aluminum Sesquichlorohydrate solution was directly prepared by reacting hydrochloric acid with aluminum metal in presence of water at elevated temperature and atmospheric pressure. The batch was pulled at desired Al / Cl mole ratio. The solution was filtered to achieve desired clarity and if needed then water was added to achieve the desired %Anhydrous Solids.
[0109] Table 35 provides the properties of aluminum sesquichlorohydrate solution. Table 35 Sp. Gravity Aluminum Chloride Al / Cl mole ratio Fe content 1.3520 12.50% 8.94% 1.84 55 ppm
[0110] Step-II Preparation of Zirconium Hydroxychloride Glycine solution with CaCl2
[0111] Table 36 provides a list of the materials and the amounts thereof used to prepare the zirconium hydroxychloride glycine solution with CaCl2:GULBRA 3.4-007 Table 36 Sr. No. Material name Quantity 1 Water 16.1 gm 2 Zirconium Oxychloride 32.1 gm 3 Zirconium Basic Carbonate 16.1 gm 4 Glycine 13.5 gm 5 Calcium Chloride di-hydrate 22.2 gm 6 Total 100 gm
[0112] Zirconium Hydroxychloride Glycine solution with CaCl2 was prepared by dissolving ZOC into hot water followed by thermal treatment to attend 70-800C reaction temperature. To this hot ZOC solution, ZBC powder was charged, and the resulting solution was aged at 70-800C for a minimum of 45 minutes. Glycine was charged at 65-800C temperature into the batch and temperature is maintained to 70- 800C for a minimum of 1.5 hours. The resulting solution was cooled down to below 500C and CaCl2*2H2O flake was charged and agitated till complete dissolution.
[0113] Table 37 provides the properties of the ZHC-Gly solution with Calcium Chloride. Table 37 Parameter Sp. Gravity Zirconium Chloride Calcium Zr / Cl mole ratio Results 1.5652 13.67% 17.35% 5.75% 0.73:1
[0114] Step-III Feed solution preparation, Spray drying and Micronization
[0115] Table 38 provides the materials and the amounts of the feed solution. Table 38 Sr. No. Material name Quantity 1 Aluminum Sesquichlorohydrate solution 73.5 gm 2 ZHC-Gly solution with CaCl226.5 gm 3 Total 100 gm
[0116] Table 39 provides the properties of the resulting Aluminum Zirconium Pentachlorohydrex Glycine powder with CaCl2.GULBRA 3.4-007 Table 39 Sr. No. Parameter Results 1. Appearance Off white 2. Odor Characteristics 3. pH (15% w / w in water) 4.0 4. Aluminum (%) 18.01 5. Zirconium (%) 7.08 6. Chloride (%) 20.96 7. Calcium (%) 2.31 8. Glycine (%) 8.36 9. Al / Zr mole ratio 8.77:1 10. Metals / Cl Active mole ratio 1.56:1 11. Fe in ppm 114 12. % Anhydrous 73.11 13. HPLC Peak 1+2 12.01% 14. HPLC Peak 3 62.19% 15. HPLC Peak 4 14.75% 16. HPLC Peak 5 11.04% 17. Particle Size % < 10 um 94.39 18. Particle Size % < 45 um 100
[0117] Comparative Example 7 Preparation of Activated-Aluminum Zirconium Octachlorohydrex Glycine powder with CaCl2using AASCH-glycine-CaCl2solution and Zirconium Hydroxychloride solution as feed solutions
[0118] Step-I Preparation of AASCH Glycine solution with CaCl2
[0119] Table 40 provides a list of the materials and the amounts thereof used to prepare the activated aluminum sesquichlorohydrate Gly solution with CaCl2: Table 40 Sr. No. Material name Quantity (gm) 1ACH solution55.922Hydrochloric Acid3.963Water4.394 Calcium Chloride dihydrate3.795Glycine31.94GULBRA 3.4-007 6Total100
[0120] AASCH-Ca-Glycine solution was prepared by adding hydrochloric acid into the ACH solution followed by water addition, CaCl2charging and Glycine addition. The resultant solution had approximated 20% anhydrous solids which was thermally treated for min. 2 hours at 85-1000C. The hot solution was cooled down to below 500C and used as an Al stream.
[0121] Table 41 below is the properties of AASCH Glycine with Calcium Chloride. Table 41 Aluminum Chloride Calcium Al / Cl mole ratio %Peak 3 %Peak 4 %Peak 5 7.46% 8.09% 1.19% 1.64:1 36.28 53.65 9.20
[0122] Step-II Zirconium Hydroxychloride solution preparation
[0123] Table 42 provides a list of the materials and the amounts thereof used to prepare the zirconium hydroxychloride solution: Table 42 Sr. No. Material name Quantity 1 Water 37.0 2 Zirconium Oxychloride 47.4 3 Zirconium Basic Carbonate 15.6 Total 100 gm
[0124] ZHC solution was prepared by dissolving Zirconium Oxychloride (ZOC) into the hot water followed by thermal treatment to 70-800C. To this hot ZOC solution, Zirconium Basic Carbonate (ZBC) was added, and the resulting solution was aged at 70-800C for a minimum of 45 minutes.
[0125] Table 43 provides the properties of the ZHC solution. Table 43 Sp. Gravity Zirconium Chloride Zr / Cl mole ratio 1.3573 17.40% 10.34% 0.64:1
[0126] Step-III Feed solution Preparation, spray drying and micronization
[0127] Table 44 provides a list of the materials and the amounts thereof used to prepare the activated aluminum sesquichlorohydrate Glycine solution with CaCl2. Table 44GULBRA 3.4-007 Sr. No. Material name Quantity 1 AASCH-Glycine solution with CaCl285.7 gm 2 Zirconium Hydroxychloride solution 14.3 gm 3 Total 100 gm
[0128] Table 45 provides the properties of the resulting Activated Aluminum Zirconium Octachlorohydrex Glycine powder with CaCl2Table 45 Sr. No. Item / Parameter Results 1. Appearance Off-white Powder 2. LOD (106°C / 2hrs) 6.4% 3. pH 15% (w / w aq. solution) 3.68 4. Aluminum (%) 16.38 5. Zirconium (%) 6.69 6. Chloride (%) 21.78 7. Calcium (%) 2.65 8. Glycine 8.54 9. Al / Zr mole ratio 8.44:1 10. M / Cl mole ratio (Active ratio) 1.41:1 11. Fe in ppm 60 ppm 12. % Anhydrous 67.84 13. HPLC Peak 1+2 0.89% 14. HPLC Peak 3 36.69% 15. HPLC Peak 4 49.86% 16. HPLC Peak 5 12.56% 17. Particle size: % < 10 um 91 18. Particle size: % < 45 um 100
[0129] As is shown in FIG. 3, Example 1 showed the highest degree of Zirconium polymer distribution, whereas Comparative Example 5 showed the lowest.
[0130] Antiperspirant stick formulations have been prepared using Comparative Example 5 and Example 1 as the active ingredients. Table 46 lists the other ingredients included in the respective antiperspirant stick formulations. Antiperspirant Stick Formulations Sr. No. Ingredient % By weight Comparative Example Example 1 5GULBRA 3.4-007 1Cyclomethicone31.660 29.7502Alkyl benzoate C12-153.000 3.0003Isopyl myristate6.000 6.0004PPG 15 stearyl ether9.000 9.0005Behenyl alcohol14.000 14.0006Castor wax2.750 2.7507Polyethylene wax4.000 4.0008Silica dimethyl silylate1.500 1.5009Talc2.000 2.00010 Fragrance0.000 0.00011 Active (~ 20% anhydrous)26.090 -12 Active (~ 20% anhydrous) - 28.000
[0131] The ingredients no.1 to 10 were admixed in a stainless steel vessel at a temperature range of 80-85°C to make lump free composition including emulsifiers, thickeners, emollients, and the like. As mixing continued, the batch was subjected to cooling at temperature range of 75-80°C. Ingredient no.11 was added in the composition at a temperature range of 75-80°C and mixed well to ensure uniform distribution of all contents. As mixing continued, the batch was subjected to a cooling to temperature range of 65-70°C. Hot contents were poured into molds. Solid antiperspirant sticks, with a uniform, random orientation of crystals, were obtained upon cooling below approximately 50°C.
[0132] Additional antiperspirant stick formulations have been prepared using Comparative Example 5 and Example 1 as the active ingredients. Table 47 lists the other ingredients included in the respective antiperspirant stick formulations. Antiperspirant Stick Formulations Sr. No. Ingredient % By weight Example IDComparative Example 5 Comparative Example 61 Silica dimethyl silylate 01.500 01.500 2 Cyclomethicone 31.660 29.750 3 Talc 02.000 02.000 4 Alkyl benzoate C12-15 03.000 03.000 5 Behenyl alcohol 14.000 14.000 6 Isopropyl myristate 06.000 06.000 7 Castor wax 02.750 02.750 8 Polyethylene wax 04.000 04.000 9 Ppg 15 stearyl ether 09.000 09.000GULBRA 3.4-007 10 Fragrance 00.000 0.000 11 Active (~ 20 % anhydrous 26.10 00.000 11 Active (~ 20 % anhydrous 00.000 28.000
[0133] The ingredients no.1 to 10 were admixed in a stainless steel vessel at a temperature range of 80-90°C to make lump free composition.As the mixing continued, the batch was subjected to cooling at a temperature range of 75-80C. Ingredient no 11 was added in the composition at a temperature range of 78-80°C and mixed well to ensure well distribution of all contents. As the mixing continued, the batch was subjected to a cooling to temperature range of 70-75°C. Hot contents were poured into molds. Solid antiperspirant sticks were obtained upon cooling below approximately 55°C.
[0134] Hot room study results of antiperspirant sticks
[0135] Example 1 vs. Comparative Example 5
[0136] The assessment of the antiperspirant effect was performed according to the Guidelines for Effectiveness Testing of OTC Antiperspirant Drug Products by the Food and Drug Administration (FDA) and below efficacy results:
[0137] After 48 hours of the last product's application with Example 1, an average decrease in sweat weight of 18% found in comparison to Comparative Example 5. This decrease is statistically significant with a p-value of 0.009.
[0138] After 72 hours of the last product's application with Example 1, an average decrease in sweat weight of 21% found in comparison to Comparative Example 5. This decrease is statistically significant with a p-value 0.001.
Claims
GULBRA 3.4-007 Claims 1. A method of making an aluminum-zirconium antiperspirant active powder, comprising: heating a solution comprising a basic aluminum chloride hydroxide, an amino acid, and a calcium salt at a temperature of from 80 °C to 100 °C to form an activated solution having an HPLC peak 4 content of at least 55%; cooling the activated solution to a temperature of 50 °C or below to form a cooled solution; mixing the cooled solution with a zirconium hydroxychloride solution having the following empirical formula: ZrO(OH)bCl2-b, wherein 0<b<1 to form an aluminum-zirconium solution, and drying the aluminum-zirconium solution to form the aluminum-zirconium antiperspirant active powder.
2. The method of claim 1, wherein the heating is performed for 30 minutes to 8 hours.
3. The method of claim 2, wherein the heating is performed for 2 hours to 4 hours.
4. The method of claim 1, wherein the aluminum-zirconium antiperspirant active powder is activated aluminum zirconium pentachlorohydrate glycine powder with calcium.
5. The method of claim 1, wherein the activated solution does not contain a zirconium compound.
6. The method of claim 1, wherein the basic aluminum chloride hydroxide is aluminum sesquichlorohydrate.
7. The method of claim 1, wherein the basic aluminum chloride hydroxide is aluminum chlorohydrate.
8. The method of claim 1, wherein the activated solution comprises a complex having an empirical formula of Al2(OH)6-xClx(AA)y, wherein AA is the amino acid, 1.05<x<1.6, 0.15<y<1.0, wherein the activated solution has aluminum to calcium mole ratio of greater than 0.1:1 to less than 0.8:
1.
9. The method of claim 1, wherein the aluminum-zirconium antiperspirant active powder has the metals to chloride molar ratio is from 1.2 to 2.1 and aluminum to zirconium ratio is from 6 to 10.
10. The method of claim 1, wherein the aluminum-zirconium antiperspirant active powder has the metals to chloride molar ratio is from 1.51 to 2.1 and aluminum to zirconium ratio is from 6 to 10.
11. The method of claim 1, further comprising:GULBRA 3.4-007 dissolving a zirconium oxychloride compound into water and thermally treating to form a solution; and admixing the solution with a zirconium basic carbonate compound and aging to form the zirconium solution comprising the zirconium hydroxychloride.
12. The method of claim 1, further comprising: mixing at least one or more of HCl or AlCl3, aluminum chlorohydrate, water, the calcium salt, and the amino acid to prepare a concentrated solution comprising the basic aluminum chloride hydroxide in an amount of 25 to 45 wt%; and diluting the concentrated solution to provide a solution comprising the basic aluminum chloride hydroxide in an amount of 10 to 30 wt%, wherein the basic aluminum chloride hydroxide comprises aluminum chlorohydrate, aluminum sesquichlorohydrate, or a combination thereof.
13. The method of claim 1, wherein the aluminum-zirconium antiperspirant active powder has a molar ratio of total metals M to chlorine Cl (M:Cl) of greater than 1.5:
1.
14. The method of claim 1, wherein the solution is a sesquichlorohydrate solution having a mole ratio of aluminum Al to chloride Cl (Al:Cl) of from 1.5-1.8:
1.
15. The method of claim 1, wherein the aluminum-zirconium antiperspirant active powder has a molar ratio of aluminum Al to zirconium Zr (Al:Zr) of from 6 to10:
1.
16. The method of claim 1, wherein the amino acid comprises glycine, betaine, or a mixture thereof.
17. The method of claim 1, wherein the aluminum-zirconium antiperspirant active powder comprises the amino acid in an amount ranging from 5 and 10 wt%.
18. The method of claim 1, wherein the calcium salt is at least one of calcium chloride, calcium bromide, calcium nitrate, calcium citrate, calcium acetate, calcium gluconate, calcium ascorbate, calcium lactate, calcium glycinate, calcium carbonate, calcium sulfate, calcium hydroxide, or a mixture thereof.
19. The method of claim 1, wherein the HPLC peak 4 content of the activated solution is from 55 % to 80%.
20. The method of claim 1, wherein the aluminum-zirconium antiperspirant active powder has HPLC peak 4 content of from 60% to 80%.
Citation Information
Patent Citations
High pH antiperspirant compositions of enhanced efficacy
US20050265939A1
Particulate enhanced efficacy antiperspirant salt with raised ph
WO2007004163A1
Betaine with calcium and / or strontium antiperspirants
WO2008063188A2