Aqueous coating composition, curable coating layer, articles having the same, and manufacturing process thereof

An aqueous coating composition using acrylate, polyurethane, and amino-functional silicone emulsions addresses the balance of anti-soiling, easy cleaning, and soft touch in vehicle interior coatings.

WO2026232314A1PCT designated stage Publication Date: 2026-11-12DOW GLOBAL TECHNOLOGIES LLC +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/093117
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-07
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing coatings for synthetic and artificial leathers in vehicle interiors struggle to achieve a balance between anti-soiling, easy cleaning, low gloss appearance, and soft touch (slippage).

Method used

An aqueous coating composition comprising non-silicone type film-forming emulsions, such as acrylate and polyurethane emulsions, combined with silicone-elastomer-forming and amino-functional silicone emulsions, which form a coating film that provides anti-soiling, easy cleaning, and a soft feel.

Benefits of technology

The composition achieves a good performance balance of anti-soiling, easy cleaning, low gloss, and slippage (soft feeling) on synthetic and artificial leathers, particularly for car seat applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2025093117-FTAPPB-I100001
    Figure PCTCN2025093117-FTAPPB-I100001
  • Figure PCTCN2025093117-FTAPPB-I100002
    Figure PCTCN2025093117-FTAPPB-I100002
  • Figure PCTCN2025093117-FTAPPB-I100003
    Figure PCTCN2025093117-FTAPPB-I100003
Patent Text Reader

Abstract

The present disclosure relates to aqueous coating composition, curable coating layer, articles having the same, and manufacturing process thereof. The aqueous coating composition comprises: (A) at least one non-silicone type film-forming emulsion selected from (A1) acrylate emulsion, (A2) polyurethane emulsion or both; (B) a silicone-elastomer-forming emulsion; and (C) an amino-functional silicone emulsion. The aqueous coating composition can be applied and cured on the surface of substrates, especially synthetic and / or artificial leather for vehicle interior materials, to form an anti-soiling coating layer with balanced performance including anti-soiling, easy cleaning, low gloss appearance and slippage (soft feeling).
Need to check novelty before this filing date? Find Prior Art

Description

AQUEOUS COATING COMPOSITION, CURABLE COATING LAYER, ARTICLES HAVING THE SAME, AND MANUFACTURING PROCESS THEREOFCROSS REFERENCE TO RELATED APPLICATIONS

[0001] None.TECHNICAL FIELD

[0002] The present disclosure relates to aqueous coating composition, curable coating layer, articles having the same, and manufacturing process thereof. The aqueous coating composition can be used to form a coating layer on substrates, especially on synthetic and / or artificial leather for vehicle interior applications. The coating layer exhibits excellent anti-soiling, easy-cleaning properties, low gloss appearance and a soft feeling (slippage) .BACKGROUND

[0003] In the field of vehicle interior materials, synthetic and artificial leathers are widely used. However, it is a challenge to achieve a balance among anti-soiling, easy cleaning, low gloss appearance and a soft touch (slippage) for the coating layers on these leathers.

[0004] Patent Document 1 describes a synthetic leather characterized by a cellulosic substrate with a surface layer containing polyurethane resin and silicone rubber (mass ratio 95: 5-25: 75, preferably 80: 20-50: 50) . The polyurethane resin may include carbonate / ether bonds, with silicone from emulsion forming elastic films. It may have nubuck / silver finishes, an anchor coat layer, and is made by coating, bonding, and peeling.

[0005] Patent Document 2 and Patent Document 3 describe a silicone-based coating composition for substrates, which contains specific silicone polymers and additives. The composition can form a protective, anti-soiling and water-repellent layer on surfaces like leather.

[0006] Currently, it is difficult to take performance balance including anti-soiling, easy cleaning, appearance like low gloss, and slippage (soft feeling) . RELATED ART DOCUMENTS Patent Documents

[0007] [Patent Document 1] JP2020059965 [Patent Document 2] WO2020 / 255895A1 [Patent Document 3] WO2012 / 002571A1SUMMARYPROBLEMS TO BE SOLVED

[0008] The present invention has been created in order to solve the abovementioned problems, and an objective thereof is to provide an anti-soiling coating, which is useful for top coating of car seat leather. The coating contains amino silicone emulsion, silicone elastomer emulsion, and acrylate emulsion and / or polyurethane emulsion. The silicone elastomer emulsion can be used in the anti-soiling coating. Also, colloidal silica can be used, with or without increased content of colloidal silica, in silicone elastomer emulsion for enhancing anti-soiling performance. MEANS FOR SOLVING THE PROBLEM

[0009] As a result of conducting diligent research on the problems described above, the present inventors arrived at the present invention. That is, one object of the present invention is achieved by an aqueous coating composition comprising: (A) at least one non-silicone type film-forming emulsion selected from (A1) acrylate emulsion, (A2) polyurethane emulsion or both; (B) a silicone-elastomer-forming emulsion; and (C) an amino-functional silicone emulsion.

[0010] In an embodiment of this disclosure, it provides an anti-soiling coating film obtained by curing the aqueous coating composition of this disclosure.

[0011] In an embodiment of this disclosure, it provides a substrate having an anti-soiling coating film on a substrate surface, which is obtained by removing water content from the aqueous coating composition.

[0012] In an embodiment of this disclosure, it provides a vehicle interior material having an anti-soiling coating film on a substrate surface, which is obtained by removing water content from the aqueous coating composition.

[0013] In an embodiment of this disclosure, it provides a process for manufacturing a substrate having an anti-soiling coating film on a surface of the substrate, comprising: (I) applying the aqueous coating composition onto the surface of the substrate; and (II) forming an anti-soiling coating film by removing water content from the aqueous coating composition. EFFECTS OF THIS INVENTION

[0014] Through this invention, good performance balance including anti-soiling, easy cleaning, appearance like low gloss, and slippage (soft feeling) can be achieved. The anti-soiling coating of this disclosure can be used for synthetic leather and artificial leather, particularly those for car seat leather.DETAILED DESCRIPTION

[0015] [Component (A) , Non-silicone type film-forming emulsion] In the field of synthetic and / or artificial leather coatings, non-silicone type film-forming emulsions generally serve  as a foundational matrix for coating compositions, providing essential mechanical properties, adhesion, and base film-forming capability. Typically, the non-silicone type film-forming emulsions comprise acrylate emulsions (A1) , polyurethane emulsions (A2) or both. In some embodiments, component (A) is in the range of 40-70 mass%, 45-65 mass%, 50-60 mass%, or 55-60 mass%, based on the total solid content of (A) , (B) and (C) .

[0016] Acrylate emulsions are water-based dispersions of polymers derived from acrylic monomers, such as methyl methacrylate, butyl acrylate, and ethyl acrylate. These polymers form a crosslinkable or non-crosslinkable matrix with hydrophobic backbones for water resistance and functional groups (e.g., hydroxyl, carboxyl) for compatibility with crosslinkers (e.g., isocyanates, carbodiimides) . For example, the acrylate emulsions can be selected from HYDRHOLACTM series emulsions available from DOW, e.g., HYDRHOLAC CL-1 Emulsion (37%solids acrylate polymer emulsion with high film-forming efficiency, providing hardness and initial adhesion to leather substrates) , HYDRHOLAC AD-1 Emulsion (asilica / acrylate composite emulsion (24%solids) , where colloidal silica enhances abrasion resistance and matting effects without compromising flexibility) and etc.

[0017] In this disclosure, the acrylate emulsions generally form a continuous, transparent film on leather surfaces, serving as a base layer for subsequent silicone or additive incorporation, provide strong interfacial bonding with synthetic / artificial leather substrates (e.g., PVC, PU) due to polar group interactions, and be compatible with pigments, fillers, and rheology modifiers to tailor gloss (e.g., low gloss for automotive interiors) and texture.

[0018] In this disclosure, the acrylate emulsions typically comprise a solid content of 20-50%in view of a balance between viscosity and film thickness. In some embodiments of this disclosure, the acrylate emulsions comprise a solid content of 24-37%. Further, by monomer selection the acrylate emulsions can have a Glass Transition Temperature (Tg) ranging from -50℃ to 50℃, preferably from -40℃ to 15℃, so as to control coating flexibility / stiffness. In this disclosure, the acrylate emulsions can work synergistically with silicone elastomer emulsions (Component B) and amino-functional silicones (Component C) to enhance anti-soiling and soft touch.

[0019] Polyurethane (PU) emulsions are water-dispersed polyurethane polymers, often derived from polyols (e.g., polyether, polyester, polycarbonate) and diisocyanates (e.g., MDI, TDI) . The polyurethane emulsions used is not particularly limited, and examples thereof include polycarbonate-based polyurethane resins, polyether-based polyurethane resins, and polyester-based polyurethane resins. These may be used alone or in combination of two or more. Among these, it is preferable to use a polycarbonate-based polyurethane resin from the viewpoint of abrasion resistance, and it is preferable to use a polyether-based polyurethane resin from the viewpoint of touch and texture. The polyurethane resin may be commercially available, and from the viewpoint of environmental load, a one-liquid emulsion type (polyurethane emulsion) is preferred. In one embodiment, the polyurethane emulsions can be tailored hard-soft segment ratios for balanced elasticity and durability. Polyether-based PU emulsions are characterized in high flexibility and hydrolysis resistance (e.g., for automotive seat leathers exposed to moisture) . Polycarbonate-based PU emulsions are characterized in superior abrasion and heat resistance (e.g., for dashboard trims) . For example, the PU emulsions can be selected from OPTI-MATT UD-4 DULLER (A25%solids polyurethane matting agent emulsion, providing low gloss and soft texture (UD-4 contains silica itself) ) , PrimalTM Series available from DOW (Polyurethane emulsions with adjustable hardness (JIS A 50-80) and elongation (100-500%) ) , and etc.

[0020] In this disclosure, the PU emulsions generally serve as elastic matrix and form a flexible film that mimics natural leather's stretch and recovery, essential for curved automotive interior surfaces. Also, it can provide crosslinking sites, e.g., hydroxyl or amine groups, for reacting with crosslinkers (e.g., isocyanates in Component D) to improve chemical resistance and durability. Furthermore, the PU emulsions can adjust surface friction (COF 0.3-0.4) when combined with silicone components, enabling the “soft feeling” required for premium interiors.

[0021] In this disclosure, the PU emulsions typically comprise a solid content of 20-60% (e.g., 25%for matting agents, 50%for high-strength coatings) . In this disclosure, PU emulsions can provide a coating with good mechanical strength (e.g., Tensile strength of 5-20 MPa, elongation at break of 200-600%, depending on polyol type (polyether > polyester in flexibility) . Further, PU emulsions can provide weather resistance with UV-stabilized formulations (e.g., with hindered amine light stabilizers) for prolonged outdoor use in automotive applications.

[0022] In some embodiments of this disclosure, the non-silicone type film-forming emulsions can be synergistic formulation, that is, combined use of acrylate and polyurethane emulsions to balance properties. For acrylate-rich formulations (e.g., 60-80%of acrylate) , anti-soiling and cost efficiency can be achieved. For polyurethane-rich formulations (e.g., 50-70%of PU) , good elasticity, lower COF data and tactile quality can be achieved, suitable for topcoats. Based on the total dry mass thereof, acrylate emulsion is 50-80%or 55-75%for film integrity and adhesion, and polyurethane emulsion is 20-50%or 25-45%for softness without compromising hardness.

[0023] In some embodiments, the polyurethane emulsion constituting the surface layer preferably contains a carbonate bond (-O- (C=O) -O-) from the viewpoint of abrasion resistance, and preferably contains an ether bond (-O-) from the viewpoint of tactile feel, and may contain both an ether bond and a carbonate bond from the viewpoint of achieving both tactile feel and abrasion resistance. The ratio of ether bonds to carbonate bonds, in terms of molar ratio, is preferably ether bonds : carbonate bonds=90: 10 to 10: 90, more preferably 80: 20 to 20: 80, and further preferably 50: 50 to 20: 80. By ensuring that the ratio of carbonate bonds is 10%or more, it is possible to prevent deterioration in abrasion resistance, heat resistance, moist heat resistance, and light resistance. Furthermore, by ensuring that the ratio of ether bonds is 10%or more, the effect of improving the feel can be enhanced

[0024] In another embodiment of this disclosure, the content of the polyurethane resin is not particularly limited, but is preferably 20 to 88 mass %, more preferably 45 to 74 mass %, and further preferably 50 to 69 mass %. When the content of the polyurethane resin in the surface layer is 20%by mass or more, the film-forming properties are good and the abrasion resistance can be improved. In addition, by making the content 88%by mass or less, it is possible to suppress the coating feel from becoming too strong, and the texture is less likely to become rough and hard, thereby improving the tactile feel.

[0025] In this disclosure, the non-silicone type film-forming emulsions can comprise other resin components within the range that does not impair the effects of the present invention. Examples of the other resin components include acrylic resin, epoxy resin, and silicone resin.

[0026] [Component (B) , Silicone-elastomer-forming emulsion] In this disclosure, the silicone-elastomer-forming emulsion plays a role in achieving the desired properties of the  final coating, such as elasticity, durability, and anti-soiling performance. In general, the silicone-elastomer-forming emulsion is not particularly limited, which can be a polyorganosiloxane having at least two groups selected from a group consisting of hydroxyl groups, alkoxy groups, and alkoxyalkoxy groups bonded to a silicon atom in one molecule, having a viscosity at 25 ℃. within a range of 100,000 to 20,000,000 mPa-s. A molecular structure of the polyorganosiloxane may be a straight chain, cyclic, branched, dendritic, or reticulated, but is preferably a straight chain or partially branched straight chain. The group selected from a group consisting of hydroxyl groups, alkoxy groups, and alkoxyalkoxy groups may be present at an end of the molecular chain, may be present on a side chain of the molecular chain, or may be present on both. The alkoxy group is preferably a methoxy group, ethoxy group, n-propoxy group, isopropoxy group, n-butoxy group, t-butoxy group, hexyloxy group, cyclohexyloxy group, octyloxy group, decyloxy group, or other alkoxy group having 1 to 10 carbon atoms, and the alkoxyalkoxy group is preferably a methoxymethoxy group, a methoxyethoxy group, an ethoxymethoxy group, a methoxypropoxy group, or other alkoxyalkoxy group having 2 to 10 carbon atoms.

[0027] Examples of an organic group bonded to a silicon atom other than group selected from a group consisting of hydroxyl groups, alkoxy groups and alkoxyalkoxy groups include unsubstituted monovalent hydrocarbon groups and substituted monovalent hydrocarbon groups. The non-substituted monovalent hydrocarbon groups preferably have 1 to 10 carbon atoms from the perspective of an emulsification assisting function, and is preferably an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an alkenyl group having 2 to 10 carbon atoms, and particularly preferably a methyl group or phenyl group.

[0028] Examples of the substituted monovalent hydrocarbon groups include groups where a portion or all hydrogen atoms in the aforementioned unsubstituted monovalent hydrocarbon groups, and particularly alkyl groups or phenyl groups having 1 to 10 carbon atoms, is substituted by a substitution group such as: fluorine, chloride, or other halogen atom; an epoxy function group; a methacrylic functional group; an acrylic functional group; an amino functional group; a sulfur-containing functional group; an alkoxy group; a hydroxycarbonyl group; an alkoxycarbonyl group; or the like.

[0029] From the perspective of the strength and close fitting properties to a substrate of a coating obtained by removing water content of the coating composition of the present invention, reduction of surface pressure-sensitive adhesion (tack) , and reduction of friction, the viscosity of silicone-elastomer-forming emulsion at 25 ℃. is within a range of 100,000 to 20,000,000 mPa-s, more preferably within a range of 300,000 mPa-sto 10,000,000 mPa-s, even more preferably within a range of 500,000 mPa-sto 5,000,000 mPa-s, and most preferably within a range of 750,000 mPa-sto 3, 500,000 mPa-s. If the viscosity of silicone-elastomer-forming emulsion is less than the lower limit described above, the strength of the coating obtained by removing water content from the coating composition and close fitting properties thereof to a substrate may be insufficient. Furthermore, surface tackiness of the coating may occur, and thus a smooth surface may not be achieved. On the other hand, if the viscosity of silicone-elastomer-forming emulsion exceeds the upper limit described above, there are problems where synthesizing by emulsion polymerization is difficult and a stable emulsion is difficult to obtain by an ordinary method.

[0030] Such a silicone-elastomer-forming emulsion is preferably a diorganopolysiloxane having both ends of a molecular chain blocked by hydroxyl groups. An example of such a diorganopolysiloxane with both ends of a molecular chain blocked by hydroxyl groups includes a polyorganosiloxane expressed by the general formula: HO (R12SiO) m. Note that in the formula above, R1 is the same as an unsubstituted or substituted monovalent hydrocarbon group bonded to a silicon atom other than the aforementioned hydroxyl group or hydrolyzable group, and is preferably an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an alkenyl group having 2 to 10 carbon atoms, and particularly preferably a methyl group or phenyl group. m is an integer of 2 or more, and the viscosity at 25 ℃. is in the viscosity range described above and is preferably a number between 100,000 mPa-sand 20,000,000 mPa-s.

[0031] The polyorganosiloxane with the structure described above can be used as a silicone-elastomer-forming emulsion, and a manufacturing method thereof is not particularly limited. A polyorganopolysiloxane obtained by a known manufacturing method such as equilibrium polymerization or the like may be emulsified in water with an emulsifier or the like. However, from the perspective of handling workability during manufacturing and particle size and stability during emulsification and dispersion, an organopolysiloxane obtained by emulsion polymerization using an organopolysiloxane with a lower degree of polymerization, which is a precursor of silicone-elastomer-forming emulsion, can be preferably used.

[0032] It is particularly preferably (a) a polyorganosiloxane having at least two hydroxyl groups or hydrolyzable groups bonded to a silicon atom serving as a precursor of component (B) and (b) a polyorganosiloxane obtained by emulsion polymerizing an organic silicon compound containing an aminoxy group having an average of two aminoxy groups bonded to a silicon atom in one molecule, in the presence of emulsifiers.

[0033] The polyorganosiloxane (a) having at least two hydroxyl or hydrolyzable groups bonded to silicon atoms in one molecule serving as a precursor of component (B) is a raw material component containing component (B) described above, and is preferably a chain polyorganosiloxane with a lower viscosity than component (B) having hydroxyl groups or hydrolyzable groups bonded to a silicon atom at both ends of a molecular chain. More specifically, component (a) is an organopolysiloxane blocked with hydroxyl groups at both ends of a molecular chain, having a viscosity at 25 ℃. that is lower than component (B) , and particularly, 100,000 mPa-sor less, and preferably within a range of 50 to 50,000 mPa-s, and is most preferably a polyorganosiloxane as expressed by HO (R12SiO) nH, where n represents a number in which the viscosity of component (a) at 25 ℃. is within the aforementioned viscosity range, and is preferably within a range of 50 to 50,000 mPa-s. Note that in the formula, R1 is the same as an unsubstituted or substituted monovalent hydrocarbon group bonded to a silicon atom other than the hydroxyl group or hydrolyzable group described above, and is particularly preferably a methyl group or phenyl group.

[0034] The aminoxy group-containing organic silicon compound (b) having an average of two aminoxy groups bonded to a silicon atom in one molecule is a component for promoting the formation of a cured film having favorable surface hardness and rubber-like elasticity without tackiness feel by reacting and cross-linking with component (a) . Component (b) contains an aminoxy group bonded to an average of two silicon atoms in one molecule, and two aminoxy groups may be present on average only on a side chain of a molecular chain, may be present only at both ends of the molecular chain, or one each may be present on average in both an end of the molecular chain and a side chain of the molecular chain. If the average number of aminoxy groups in component (b) is three or more in one molecule, gelation of the mixture may occur inside an emulsifying device or in a pre-mixing process before emulsification. Furthermore, elongation of the resulting cured film may be inferior. Such aminoxy group-containing organic silicon compounds include polydiorganosiloxanes blocked with aminoxy groups at both ends of a molecular chain, diorganosiloxane / organoaminoxysiloxane copolymers blocked with an aminoxy group at one end of a molecular chain, diorganosiloxane / organoaminoxysiloxane copolymers blocked with triorganosilyl groups at both ends of a molecular chain, cyclic diorganosiloxane / organoaminoxysiloxane copolymers, and diaminoxydiorganosilanes. Of these, polydiorganosiloxanes blocked with aminooxy groups at both ends of a molecular chain are preferred. The blending amount of component (b) is 0.1 to 100 parts by mass, preferably 0.5 to 50 parts by mass, and more preferably 1 to 20 parts by mass with regard to 100 parts by mass of component (a) . Component (b) is preferably expressed by general formula: R2R12SiO (R1R3SiO) n (R12 (SiO) pSiR12R2.

[0035] In the formula above, R1 is the same as described above, but is preferably an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an alkenyl group having 2 to 10 carbon atoms, and particularly preferably a methyl group or phenyl group. R3 is an aminoxy group. When n is zero, R2 is an aminoxy group; when n is 1, one R2 is an aminoxy group, and remaining Res are a group selected from a group consisting of unsubstituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, halogen-substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, hydroxyl groups, alkoxy groups having 1 to 10 carbon atoms and alkoxyalkoxy groups having 2 to 10 carbon atoms; and when n is 2, R2 is a group selected from a group consisting of unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms, halogen-substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, hydroxyl groups, 1 to 10 alkoxy groups having 1 to 10 carbon atoms, and alkoxyalkoxy groups having 2 to 10 carbon atoms.

[0036] Examples of the unsubstituted monovalent hydrocarbon group includes the same groups as described above, but is preferably an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an alkenyl group having 2 to 10 carbon atoms, and particularly preferably a methyl group or phenyl group. The halogen-substituted monovalent hydrocarbon group is a group in which a portion or all hydrogen atoms of the aforementioned unsubstituted monovalent hydrocarbon group are substituted with halogen atoms, and is preferably a chloromethyl group, a 3, 3, 3-trifluoropropyl group, a 3, 3, 4, 4, 5, 5, 5-heptafluoropentyl, a difluoromonochloropropyl group, or other halogen-substituted alkyl group. Examples of the alkoxy group and the alkoxyalkoxy group include the same groups as described above.

[0037] Examples of the aminoxy group include groups selected from -ON (R4) 2 and a group expressed by the following formula.

[0038] In the formula, R4 is a straight chain or branched alkyl group having 1 to 5 carbon atoms. In the formula, R<5 >is a divalent hydrocarbon group having 2 to 15 carbon atoms or a divalent organic group having a molecular main chain containing 3 to 17 carbon atoms and 1 to 3 nitrogen atoms or 1 to 2 oxygen atoms, and examples include - (CH2) 2-, - (CH2) 5-, - (CH2) 6-, - (CH2) 7-, - (CH2) 2-O- (CH2) 2-, - (CH-CH) - (CH-CH) -, - (CH-N) - (CH-CH) -, - (C6H4) - (CH2) 2-. Of these, - (CH2) 6-, - (CH2) 2-O- (CH2) 2-are preferred. Of these, a dialkyl aminoxy group in which an alkyl group with 1 to 5 carbon atoms is bonded to a nitrogen atom is preferred. Preferred examples of aminoxy groups include dimethyl aminoxy groups, diethyl aminoxy groups, dipropyl aminoxy groups, dibutyl aminoxy groups, diheptyl aminoxy groups, ethyl methyl aminoxy groups, propyl methyl aminoxy groups, propyl ethyl aminoxy groups, butyl methyl aminoxy groups, butyl ethyl aminoxy groups, butyl propyl aminoxy groups, heptyl methyl aminoxy groups, heptyl ethyl aminoxy groups, heptyl propyl aminoxy groups, and heptyl butyl aminoxy groups. A diethyl aminoxy group is preferred.

[0039] Furthermore, in the formula above, n is 0, 1 or 2, preferably 0 or 2, and more preferably 0. When n is 0, R2 in the formula above is an aminoxy group, and when n is 1, at least one R2 in the formula above is an aminoxy group. Of these, n in the formula above is preferably 0, and R2 is preferably an aminoxy group from the perspective of ease of availability.

[0040] In the formula, p is an integer of 0 or more. Although the upper limit of p is not particularly limited, from the perspective of ease of emulsification, p is preferably an integer within a range of 0 to 1000 more preferably within a range of 2 to 200, and most preferably within a range of 4 to 140.

[0041] Examples of such aminoxy group-containing organic silicon compounds include aminoxy group-containing organic silicon compounds as expressed by the following formulae. Note that in the formulae, Me indicates a methyl group, and Et indicates an ethyl group. (Et2NO) Me2SiOSiMe2 (ONEt2) (Et2NO) Me2SiO (Me2SiO) 12SiMe2 (ONEt2) (Et2NO) Me2SiO (Me2SiO) 40SiMe2 (ONEt2) (Et2NO) Me2SiO (Me2SiO) 80SiMe2 (ONEt2) Me2Si (ONEt2) 2 Me3SiO (MeSi (ONEt2) O) 2SiMe3 Me3SiO (Me2SiO) 4 (MeSi (ON Et2) O) 2SiMe3 Me3SiO (Me2SiO) 15 (MeSi (ON Et2) O) 2SiMe3 Me3SiO (Me2SiO) 3 (MeSi (ONEt2) O) 7SiMe3

[0042] Furthermore, if component (b) remains in the aqueous coating composition, the component contributes to reaction / cross-linking between component (A) and component (B) , and can form a coating with favorable surface hardness and rubber-like elasticity without a tacky feel.

[0043] In particular, examples of component (B) include polydimethylsiloxane emulsions, fluorosilicone emulsions, functionalized silicone emulsions and etc. Polydimethylsiloxane (PDMS) is one of the most commonly used silicone polymers in silicone-elastomer-forming emulsions. PDMS emulsions are popular due to their excellent flexibility, low surface tension, and good weather resistance. The PDMS chains in these emulsions can be linear or branched. Linear PDMS emulsions offer a high degree of flexibility and smoothness to the coating. They can form a continuous and uniform film on the substrate surface, which is beneficial for the anti-soiling property as it reduces the adhesion of dirt and stains. For example, a linear PDMS emulsion with a relatively low molecular weight may have better fluidity during the coating process, allowing it to spread evenly on the synthetic or artificial leather surface used in car interiors. Branched PDMS emulsions, on the other hand, can provide enhanced mechanical strength to the silicone elastomer. The branching structure increases the cross-linking density within the elastomer network, resulting in a coating with better resistance to abrasion and deformation. For instance, in applications where the coated surface is subject to frequent rubbing or scratching, such as car seats, a branched PDMS-based emulsion can be a better choice.

[0044] Fluorosilicone emulsions can combine the properties of fluoropolymers and silicones, which have extremely low surface energy, and gives the coating excellent water and oil repellency, in view of anti-soiling applications. The fluorine atoms in the fluorosilicone structure create a hydrophobic and oleophobic surface. When dirt, water, or oil comes into contact with the coating, it tends to bead up and roll off rather than adhere to the surface. For example, in a car interior environment where spills from beverages or greasy substances are common, a coating containing a fluorosilicone emulsion as Component B can effectively prevent stains from setting in.

[0045] Functionalized silicone emulsions have reactive groups attached to the silicone backbone. These reactive groups can participate in cross-linking reactions during the curing process of the coating, either with other components in the coating composition or with themselves. For example, amino-functionalized silicone emulsions can react with isocyanate-based cross-linkers or other components containing reactive groups. This cross-linking reaction can improve the adhesion of the coating to the substrate and enhance the mechanical properties of the final coating. In addition, epoxy-functionalized silicone emulsions can also be used to increase the hardness and chemical resistance of the coating. The choice of functionalized silicone emulsion depends on the specific requirements of the coating. If better adhesion and mechanical strength are needed, amino-functionalized emulsions may be preferred. If chemical resistance is the main concern, epoxy-functionalized emulsions can be considered.

[0046] In this disclosure, component (B) is in the range of 5-40 mass%, 7.5-35 mass%, 15-35 mass%, 18-28 mass%, or 21-26 mass%, based on the total solid content of (A) , (B) and (C) . When the amount of Component B is around 7.8-15.7 mass %based on the total solid content of (A) , (B) and (C) , it can provide a certain degree of elasticity and anti-soiling improvement to the coating. When the amount of Component B is increased to 23.5-39.2 mass %based on the total solid content of (A) , (B) and (C) , the coating will exhibit excellent elasticity, anti-soiling, and weather resistance, in particular. When the amount of Component B is relatively low, the elasticity and anti-soiling performance of the coating may be insufficient. The coating may be more brittle and prone to cracking under stress, and it may not be able to effectively repel dirt and stains. On the other hand, if the amount of Component B is too high, it may lead to some negative effects. For example, the coating may become higher gloss which can not meet needs of lower gloss. In addition, an excessive amount of silicone-elastomer-forming emulsion may also cause compatibility issues with other components in the coating composition, resulting in a non-uniform coating or poor adhesion to the substrate.

[0047] In this disclosure, component B interacts closely with component A, the non-silicone type film-forming emulsion. As above said, component A provides the basic film-forming ability and adhesion to the substrate, while component B enhances the elasticity and anti-soiling performance of the coating.

[0048] The silicone-elastomer-forming emulsion in Component B can disperse within the matrix formed by Component A. During the curing process, the two components can form an interpenetrating network structure. This structure not only improves the mechanical properties of the coating but also enhances the anti-soiling performance. For example, the silicone phase in Component B can migrate to the surface of the coating, forming a low-surface-energy layer that repels dirt and stains.

[0049] In this disclosure, component B can also interact with Component C, the amino-functional silicone emulsion. The amino groups in Component C can react with some reactive groups in Component B, such as epoxy groups in functionalized silicone emulsions. This cross-linking reaction can further strengthen the coating structure and improve its performance. In addition, the combination of Component B and Component C can have a synergistic effect on the anti-soiling performance. The silicone-elastomer-forming emulsion in Component B provides a flexible and smooth surface, while the amino-functional silicone emulsion in Component C can improve and lower the surface polarity and hydrophobic to a certain extent, which helps to clean the stains more easily.

[0050] The silicone-elastomer-forming emulsion in Component B is stable in the manufacturing process of the coating composition. During the mixing process with other components, the emulsion should remain stable to ensure a uniform distribution of all components in the final coating. Factors such as pH, temperature, and the presence of other additives can affect the stability of the emulsion. For example, some emulsifiers used in the emulsion may be sensitive to pH changes. If the pH of the coating composition is not properly controlled, the emulsion may break, resulting in phase separation and a non-uniform coating.

[0051] In the manufacturing process, the curing conditions can be adjusted according to the properties of Component B. If the curing temperature is too low or the curing time is too short, the coating may not fully cure, resulting in poor mechanical properties and anti-soiling performance. On the other hand, if the curing temperature is too high or the curing time is too long, it may cause degradation of the coating components and affect the overall performance of the coating.

[0052] In some embodiments, component (B) is in the range of 5-40 mass%, 7.5-35 mass%, 18-28 mass%, or 21-26 mass%, based on the total solid content of (A) , (B) and (C) .

[0053] [Component C, Amino-functional silicone emulsion] In this disclosure, amino-functional silicone emulsions are essential components in coatings for synthetic and  artificial leather, delivering anti-soiling properties, soft tactile feedback, and crosslinking capabilities. The amino-functional silicone emulsions combine low surface energy of silicones with the reactive functionality of amino groups, enabling synergistic performance in leather finishing.

[0054] Amino-functional silicone emulsions are water-based dispersions of amino-modified polysiloxanes, typically comprising amino-modified polysiloxane backbone. Primary structure thereof is linear or branched polydimethylsiloxane (PDMS) chains with terminal or pendant amino groups (e.g., aminoethylaminopropyl, γ-aminopropyl) covalently bonded to silicon atoms. The amino groups provide polarity for substrate interaction and reactivity with crosslinkers (e.g., isocyanates, carbodiimides) .

[0055] In some embodiments, the amino-functional silicone can be described as a siloxane structure having siloxane bonds (-Si-O-Si-) with amine functionality attached through either Si-O-C bonds to Si units on the siloxane structure or Si-C bonds to Si units on the siloxane structure, and comprises in polymerized form, structural units of: (i) (R3SiO1 / 2) a; (ii) (R2Si (OR') xO (2-x)  / 2) b; (iii) (RSi (OR') yO (3-y)  / 2) c; and  (iv) (Si (OR') zO (4-z)  / 2) d; wherein each R' is independently hydrogen, an alkyl group, a functionalized alkyl group, an aryl group or a  functionalized aryl group;wherein each R is independently hydrogen, an alkyl group, or a functionalized alkyl group; wherein at least 10 mole percent of the combination of R and R' groups are amine containing groups of the formula:  -Ra-NHRb where Ra is an alkyl group or an aryl-containing group derived from an amino alcohol and Rb is hydrogen or an alkyl group; wherein a+b+c+d=1.00 (100 mole percent) ; x is either 0 or 1; y is either 0, 1 or 2; and z is either 0, 1, 2, or 3; and the  -NH-equivalent mass of the amino-functional silicone resin is from 50 to 1000, preferably 50 to 750, more preferred 80 to 900, even more preferred 100 to 800, and most preferred 100-700.

[0056] R and / or R' groups can be amine containing groups of the formula: -Ra-NHRb. The amount of all R and R' groups which are amine containing groups of the formula: -Ra-NHRb can be as low as 10 mole percent or 20 mole percent and can independently be as high as 90 mole percent, 50 mole percent or 30 mole percent, with preferred ranges of 10 to 42 mole percent and 20 to 30 mole percent; provided that the -NH-equivalent mass of the amino-functional silicone resin is within the identified ranges. Ra is derived from an amino alcohol represented by the formula HO-Ra-NHRb, wherein Ra is an alkyl group or an aryl-containing group. Preferably Ra is derived from an amino alcohol which is selected from the group of amino alcohols which (a) have steric hindrance around the COH moiety; (b) are secondary or tertiary alcohols; or (c) are mixtures thereof.

[0057] In some embodiments, the amount of all R' groups which are aryl groups or functionalized aryl groups can be as low as 10 mole percent or 20 mole percent and can independently be as high as 100 mole percent, 50 mole percent or 30 mole percent, with preferred ranges of 10 to 60 mole percent and 20 to 50 mole percent.

[0058] In describing silicone resins, R3SiO1 / 2 is also referred to as M, R2SiO2 / 2 is also referred to as D, RSiO3 / 2 is also referred to as T, and SiO4 / 2 is also referred to as Q. In the event a superscript is used next to the M, D, T or Q designations, it refers to the type of R group (s) present. For example, DPh mean that one of the two R groups is a phenyl group. Any R group (s) not described by superscripts is to be understood by those skilled in the art as being methyl groups, unless the specific description of the polymer indicates otherwise. The -NH-equivalent mass of the amino-functional silicone resin is determined by obtaining a 13C-NMR spectrum of a known amount of solution of, or neat sample of, the amino-functional silicone resin and quantifying the peaks associated with the amino-functional Si units of the amino-functional silicone resin relative to those associated with a known amount of an internal standard (typically 1, 4-dioxane) , then adjusting for solvent content present in the sample, if any, as determined by gas chromatography. The amino-functional silicone resin is in the form of a neat liquid, solution, or meltable solid. Each subscript a, b, c or d is an average value across the distribution of units making up the material and is determined for any given material by using calculations based on NMR spectroscopic data (typically 29Si-NMR and 13C-NMR, alternatively 29Si-NMR and 1H-NMR) .

[0059] The amino-functional silicone resin of the present invention can be produced by reacting (1) a silicone resin having hydroxy or alkoxy functionality with (2) an amino alcohol and aryl alcohol. The silicone resin having hydroxy or alkoxy functionality can be derived from polysiloxanes, alkoxysilanes, or chlorosilanes. The hydroxy or alkoxy functionality of the silicone resin (1) composition is sometimes referred to as the “OZ” content and is stated in terms of mole percent. Non-limiting examples of suitable silicone resins include DOWSILTM 2403, DOWSILTM 3074 and DOWSILTM 3037, available from The Dow Chemical Company; Shin-Etsu Silicone KR-213 and KR-510, available from Shin-Etsu Chemical Co., Ltd.; and  IC232 and  SY231, available from Wacker Chemie AG.

[0060] The amino alcohol can be represented by the formula HO-Ra-NHRb, as previously described. Non-limiting examples of suitable amino alcohols include 2-amino-1-ethanol, 1-amino-2-propanol, 1-amino-2-methylpropan-2-ol, 2-amino-1-propanol, 3-amino-1-propanol, 2-amino-1-butanol, 3-amino-1-butanol, neopentanolamine (3-amino-2, 2-dimethyl-1-propanol) , 2-amino-1-methyl-1-propanol, 2-amino-2-methyl-1-propanol, 2-amino-2-ethylpropane-1, 3-diol, 2-amino-2-methylpropane-1, 3-diol, 5-amino-1-pentanol, 1, 2-dimethylethanolamine, 3-alloxy-2-hydroxy-propylamine, 1-amino-2-methyl-pentanol, N-methylethanolamine, N-hydroxyethylpropanediamine, N-cyclohexylethanolamine, p- (beta-hydroxyethyl) -aniline, N- (beta-hydroxypropyl) -N′- (beta-aminoethyl) piperazine, 2-hydroxy-3- (m-ethylphenoxy) propylamine, 2-hydroxy-2-phenylethyl amine, tris (hydroxymethyl) aminomethane, 2-aminobenzyl alcohol, 3-aminobenzyl alcohol, 3-amino-o-cresol, 4-amino-o-cresol, 5-amino-o-cresol, 2-amino-p-cresol, 4-amino-m-cresol, 6-amino-m-cresol, 1-amino-1-cyclopentane methanol, 2- (2-aminoethoxy) ethanol, 2- (2-aminoethylamino) ethanol, 6-amino-1-hexanol, 3- (1-hydroxyethyl) aniline, 2-amino-1-phenylethanol, 1-aminomethyl-1-cyclohexanol, 8-amino-2-naphthol, 2-amino-phenethyl alcohol, 4-aminophenethyl alcohol, 3- (alpha-hydroxyethyl) aniline, Mannich bases, the reaction product of an aminoalcohol with cis-2-pentenenitrile followed by an hydrogenation step, aminophenols such as p-aminophenol, tyrosine, tyramine and the like, epoxy-amine adducts and mixtures thereof. Preferred amino alcohols include without limitation, 1-amino-2-propanol and 1-amino-2-methylpropan-2-ol.

[0061] In some embodiments, component (C) is in the range of 5-55 mass%, 8-45mass%, 8-35mass%, or 15-31 mass%, based on the total solid content of (A) , (B) and (C) .

[0062] [Component (D) , a crosslinking agent] In this disclosure, the aqueous coating composition can optionally further comprise (D) a crosslinking agent for the  non-silicone type film-forming emulsion (A) . The type of the crosslinking agent as used are not particularly limited, and examples thereof including poly-carbodiimides, polyfunctional aziridines, blocked isocyanates, polyisocyanates, such as those commonly used in preparing polyacrylate resin and / or polyurethane, preferably their oligomeric forms. The concentration of the crosslinking agent may be, based on the total weight of the coating composition, from 0 to 15%by weight, from 1%to 10%by weight, or from 2%to 8%by weight. In this disclosure, the crosslinking agent can be selected from XR-5580 available from STAHL, ARCHROMA PHOBOL XAN available from ARCHROMA, or MEIKANATE CX available from Meisei Chemical Industry Co., Ltd.

[0063] [Component (E) , a colloidal silica] In this disclosure, the aqueous coating composition can optionally further comprise (E) colloidal silica. The colloidal  silica herein refers to a dispersion of silica particles, which are typically dispersed in water, suitably in the presence of stabilizing cations such as metal ions, NH4+, organic cations; primary, secondary, tertiary, and quaternary amines; or mixtures thereof. Preferably, the colloidal silica particles are negatively charged. Colloidal silica may be derived from, for example, precipitated silica, fumed silica, pyrogenic silica or silica gels, and mixtures thereof. Silica content of the colloidal silica may be present, based on the weight of colloidal silica, from 20%to 80%by weight, from 25%to 70%by weight, or from 30%to 60%by weight. The higher the silica content, the more concentrated the resulting colloidal silica dispersion will become. The pH value of the colloidal silica may be from 1 to 13, from 6 to 12, or from 7.5 to 11.

[0064] The colloidal silica useful in the present invention may have an average particle size less than 150 nanometers (nm) , 100 nm or less, or ranging from 2 nm to 70 nm, or from 5 nm to 50 nm. The average particle size of the colloidal silica may be determined according to the HG / T 2521-2008 method. The colloidal silica may be present in the coating composition, by solids weight based on the total solids weight of the aqueous coating composition, in an amount of 5%or more or 7%or more, and at the same time, 30%or less, 20%or less, or even 15%or less.

[0065] [Component (F) , a rheology modifier or a thickener] In this disclosure, the aqueous coating composition can optionally further comprise (F) a rheology modifier or a  thickener, from the perspective of improving workability such as the application properties thereof, improving the storage stability of the composition, and especially the dispersion stability of component (B) . In particular, using a thickener including a water-soluble organic polymer such as a water-soluble acrylic resin or the like has an advantage where the viscosity of the water can be increased, and thus the aqueous coating composition of the present invention can have enhanced workability and application properties to a substrate, without substantially impairing the technical effects of the present invention and the heat resistance of a cured film. The added amount of the thickener is arbitrary, but when a thickener is used, the amount is preferably selected such that the total composition is within the viscosity range described below (1000 mPa s or higher at 25℃. ) .

[0066] The thickener used in the present invention is not particularly limited, and examples include one or more types selected from thickeners containing a water-soluble organic polymer. Examples of the thickener containing a water-soluble organic polymer include water-soluble organic polymers such as a polymer polysaccharide or a water-soluble acrylic resin, and these may be used individually, or in the form of combinations thereof. In particular, the use of a water-soluble organic polymer containing a carboxylate group or acrylate group is preferred, and preferred examples include polyacrylates, which are carboxyl-containing attached polymers, such as sodium polyacrylates, sodium polymethacrylates, and the like, for example, acrylate / methacrylate copolymer lotion. In some embodiments, the thickeners used in the aqueous coating composition of the present invention may include polyvinyl alcohol (PVA) , acid derivatives, acid copolymers, urethane associate thickeners (UAT) , polyether urea polyurethanes (PEUPU) , polyether polyurethanes (PEPU) , or mixtures thereof. Examples of suitable thickeners include alkali swellable emulsions (ASE) such as sodium or ammonium neutralized acrylic acid polymers; hydrophobically modified alkali swellable emulsions (HASE) such as hydrophobically modified acrylic acid copolymers; associative thickeners such as hydrophobically modified ethoxylated urethanes (HEUR) , e.g., ACRYSOL RM-819W available from DOW; and cellulosic thickeners such as methyl cellulose ethers, hydroxymethyl cellulose (HMC) , hydroxyethyl cellulose (HEC) , hydrophobically-modified hydroxy ethyl cellulose (HMHEC) , sodium carboxymethyl cellulose (SCMC) , sodium carboxymethyl 2-hydroxyethyl cellulose, 2-hydroxypropyl methyl cellulose, 2-hydroxyethyl methyl cellulose, 2-hydroxybutyl methyl cellulose, 2-hydroxyethyl ethyl cellulose, and 2-hydoxypropyl cellulose.

[0067] The concentration of the thickener may be, based on the total weight of the aqueous coating composition, from 0 to 5%by weight, from 0.01%to 3%by weight, or from 0.1%to 1%by weight.

[0068] [Optional additives] In addition to the components described above, the aqueous coating composition of the present invention may  further comprise any one or combination of the following additives: wetting agents, leveling agents, pigments and / or extenders, dispersants, humectants, surfactants, ultra -violet (UV) stabilizers, antioxidants, solvents, defoamers, toughening agents, mildewcides, biocides, anti-skinning agents, adhesion promoters, and grind vehicles. These additives may be present in a combined amount of from 0 to 10%by weight, or from 0.01%to 2%by weight, based on the total weight of the coating composition.

[0069] In some embodiments, the aqueous coating composition may include one or more wetting agents to improve wetting of the leather substrate and stability of the dispersion during processing. The types of wetting agents are not particularly limited, and Examples thereof include a nonionic silicone polyether (such as XiameterTM OFX-5211 or DOWSILTM OFX-5211) , an anionic sulfonate-based surfactant and etc.

[0070] The aqueous coating composition of the present invention may further comprise one or more coalescents. Examples of suitable coalescents include 2-n-butoxyethanol, dipropylene glycol n-butyl ether, propylene glycol n-butyl ether, dipropylene glycol methyl ether, propylene glycol methyl ether, propylene glycol n-propyl ether, diethylene glycol monobutyl ether, ethylene glycol monobutyl ether, ethylene glycol monohexyl ether, triethylene glycol monobutyl ether, dipropylene glycol n-propyl ether, n-butyl ether, or mixtures thereof. The concentration of the coalescents may be, based on the total weight of the coating composition, from 0 to 15%by weight, from 0.01%to 10%by weight, or from 0.1%to 5%by weight.

[0071] The aqueous coating composition of the present invention may further comprise pigments and / or extenders. However, from the technical viewpoint of anti-soiling performance on the coating film, the pigments and / or extenders is not preferred to comprise this composition. Some solid fillers may impact negatively for anti-soiling performance on the coating film, and such solid fillers may be excluded from this coating composition in some embodiments. “Pigments” herein refer to materials that can provide whiteness and color including inorganic pigments and organic pigments. “Extenders” herein refer to white transparent or semi-transparent components, whose purpose is to reduce the cost of the coating by increasing the area covered by a given weight of pigment.

[0072] [Method for producing the aqueous coating composition] The aqueous coating composition of the present invention can be produced by a method known in the field of  producing a coating. Examples thereof include: Step (I) : a step of emulsifying and dispersing component (A) , component (B) , and optionally, if necessary, components (C) and (E) , using an emulsifier such as a homomixer, homogenizer, colloid mill, combomixer, in-line continuous emulsifier, vacuum emulsifier, ultrasonic emulsifier, continuous mixing device, or the like; and Step (II) : a step of adding and dispersing optional components (D) and (F) in the emulsion obtained in the aforementioned step.

[0073] Herein, component (A) , component (B) , component (C) , component (E) , and other optional additives may be added in either of the aforementioned steps, or may be divided and added to both steps.

[0074] [Applications of Aqueous coating compositions] The aforementioned aqueous coating composition is applied to the surface of a substrate using techniques known in  the art, such as by spraying, brushing, scraping, overcoating or roll -coating. When the water content is removed by evaporation / heating, or the like, to form a cured film having rubber-like elasticity, a tack-free surface, and friction-reducing properties, and therefore the composition can be used as a surface treatment agent for the purpose of modifying the surface of a substrate.

[0075] In other words, the aqueous coating composition of the present invention performs a surface treatment on a substrate surface, and at least a portion of the substrate surface can be covered by the cured film described above, and thus the surface condition can be modified. The substrates to which the aqueous coating composition of the present invention can be applied are not particularly limited, but examples include metal, ceramic, concrete, cement, mortar, paper, textile natural fiber fabric, synthetic fiber fabric, non-woven fabric, plastic, glass, rubber, wood, stone, and other composite materials as described above. In particular, the aqueous coating composition of the present invention is capable of forming a cured film having rubbery and elastic properties, a tack-free surface, and friction-reducing properties when water is removed, and thus can be used to improve the functionality of functional fabrics such as airbags, emergency chutes for aircraft and hot air balloons, and building materials such as concrete. Furthermore, if necessary, water repellency, weatherability, chemical resistance, soft texture, and the like can be provided to the surface of various substrates by the silicone elastic body, and furthermore, improvements in heat resistance and flame retardancy can be expected due to the silicone elastic body.

[0076] The method of applying the aqueous coating composition includes the steps of (I) coating the substrate surface with the aqueous coating composition, and (II) removing water in the aqueous coating composition on the substrate surface to form a cured film.

[0077] Specific means of step (I) can be a coating method or application method that is used with paints or coating materials, without any particular limitation, and examples include brush application, spray application, dipping (dipping) , flow coating, dispenser application, roller application using a gravure roller, knife coating, spin coating, and the like. In addition, the surface of the material to be coated or be applied upon may be pre-cleaned, dried and primed, prior to coating. In addition, the amount of coating / application is not particularly limited, and the coating may be thinly applied on a functional fabric such as an airbag or on a synthetic and / or artificial leather coating surface to reduce weight, or can be applied thickly to form a cured film having an excellent durability on the surface of the substrate. The coating layer exhibits excellent anti-soiling, easy-cleaning properties, low gloss appearance and a soft feeling (slippage) on said substrate, through combinational effect of said components (A) to (C) .

[0078] The water content removal of step (II) may be performed by allowing to air dry at room temperature, or by leaving at an ambient temperature adjusted to 20 to 200 ℃.INDUSTRIAL APPLICABILITY

[0079] As above said, the aqueous coating composition of this invention can be applied to a surface of the substrate using techniques known in the art. The nominal dry film thickness (DFT) of the coating is greater than or equal to 0.3 mil, preferably greater than or equal to 0.4 mils, more preferably greater than or equal to 0.5 mils, and most preferably greater than or equal to 0.6 mils. One mil is equal to one -thousandth of an inch. Examples of substrates that can be coated include, but are not limited to, plastics, wood, metals such as aluminum, steel or galvanized sheet, tin -plated steel, concrete, glass, composites, polyurethane elastomers, primed (painted) substrates and so on, particularly synthetic and / or artificial leather, especially those (e.g., vehicle interior finishing sheet) for vehicle interior applications. The anti-soiling coating film can be obtained by removing water content from the aqueous coating composition on a substrate surface. Alternatively, the coating can be cured at room temperature or at elevated temperatures in a forced -air oven using other types of heating sources. EXAMPLES

[0080] These examples are intended to illustrate the invention to one skilled in the art and are not to be interpreted as limiting the scope of the invention set forth in the claims.

[0081] The Components in Table 1 were used in these Examples.

[0082] Table 1. Components of the aqueous coating composition

[0083] [Experimental equipment] The following experimental equipment were used in the Examples. 1. RW 20. n Overhead Stirrer, available from IKA -Werke GmbH &Co. KG; 2. #3 K Hand coater, available from RK Print Coat Instruments Ltd: 24um wet thickness; 3. Achilles PVC or PU auto seat leather crust, available from Kunshan Achilles New Material Technology Co., Ltd; 4. BYK Spectro-guide sphere gloss meter, available from BYK -Gardner GmbH; 5. EMPA-128 standard soiling cloth, available from EMPA Materials Science and Technology; 6. Martindale abrasion machine, available from James Heal Ltd; 7. Soft cotton clean gauze, available from Jiangsu WLD Medical Co., Ltd; 8. Neutral clean agent fit with VDA 230-212, available from Henkel AG &Co; 9. MXD-02 coefficient of friction tester, available from Jinan Labthink Electronic Technology Co., Ltd; and 10. Delta E value meter X-Rite brand, available from X -Rite, Incorporated.

[0084] [Preparation of the aqueous coating composition] All the components were added one by one under stirring around 500 rpm using RW 20. n Overhead Stirrer, and  mixed for 15 minutes after the crosslinker and thickener were added, to form a formulated mixture.

[0085] [Experimental operations] 1. The formulated mixture were coated as topcoat on PVC auto seat leather crust by #3 K Hand coater. Then the  leather crust was put into an oven at 120℃-125℃ to forced dry for 3 minutes. The leather sample was moved out of the oven, cooling down to room temperature, leave it for one week for complete cured. 2. COF data was measured using MXD-02 coefficient of friction tester. For soiling testing, on Martindale abrasion  machine with EMPA-128 cloth, delta E value and grade after soiled were measured using X-Rite brand of sphere Spectro photo meter according to DA 230-212. After a half of soiled leather sample was cleaned by a standard clean agent, delta E value and grade after clean were also measured using X-Rite brand of sphere Spectro photo meter according to DA 230-212.

[0086] Inventive Examples 1-13 of this disclosure were listed in Table 2. And Comparative Examples 1-6 were listed in Table 3.

[0087] Table 2 Table 2. Cont. Note: E-excellent; G-good and P-poor.

[0088] Table 3 Note: E-excellent; G-good and P-poor.

[0089] [Standard of Measurement]Anti-Soiling In Examples (Ex) and Comparative Examples (Comp. Ex) , anti-soiling method follow with VDA 230-212 from  Verband der Automobilindustrie-brief VDA (German Automobile Industry Association) . Anti-soiling, cleaning and measurement operation are as follows: 1. Martindale abrasion tester, according to ISO 12947-1 with a loading weight the testing measure of 12 kPa  (according to ISO-1249-7) . A 60x60mm sized Lissajous figure is used, soiled cloth is EMPA-128. 2. Grey scale for assessment of color fastness according to ISO-105-A03. Grade 1-5. Grade 4 is acceptable,  below grade 4 is not acceptable, this is fit for after soiling and after cleaning. 3. Cleaning solution: 0.5%aqueous solution of sodium lauryl ether sulfate (TEXAPON GNSO) CAS -No.  9004-82-4. 4. Cloth for cleaning: Cotton fabric corresponding to ISO 105-F09Gloss at 60° standard Gloss at 60° standard follow with VW 50190, Dark leather 0.8-1.1unit, light leather 1.1-1.5 unit. In this invention, a  light color of flat surface PVC leather which did not have print patterns was used, so the gloss will not reach to 1.1-1.5, but is able to reach to around 2.5. After embossed patterns, the gloss will lower to around to 1.5, this is generally production practice.COF control COF control follow with standard of VDA 230-206 but using a General COF instrument MXD-02 which follow  standard of GB / T 10006 or ISO 8295 to control the statistic friction and dynamic friction around 0.3 but below 0.4.

[0090] For Inventive Examples 1-13, superior gloss, anti-soiling properties and static COF were achieved in the coating film / layer in combination of components (A) to (C) in this invention. On the other hand, as shown in comparative examples 1-6, lacking at least one component of components (A) to (C) resulted in poor performance in the coating layer in comparison with inventive examples.

Claims

1.An aqueous coating composition comprising:(A) at least one non-silicone type film-forming emulsion selected from (A1) acrylate emulsion, (A2) polyurethane emulsion or both;(B) a silicone-elastomer-forming emulsion; and(C) an amino-functional silicone emulsion.2.The aqueous coating composition according to claim 1, further comprising (D) a crosslinking agent for the non-silicone type film-forming emulsion (A) .3.The aqueous coating composition according to claim 1, wherein component (B) further comprises (E) colloidal silica.4.The aqueous coating composition according to claim 1, further comprising (F) a rheology modifier.5.The aqueous coating composition according to any one of claims 1 to 4, wherein component (A) is in the range of 40-70 mass%, component (B) is in the range of 5-40 mass%, and component (C) is in the range of 5-55 mass%, based on the total solid content of (A) , (B) and (C) .6.The aqueous coating composition according to claim 5, wherein component (A) is in the range of 45-65 mass%, component (B) is in the range of 7.5-35 mass%, and component (C) is in the range of 8-35mass%, based on the total solid content of (A) , (B) and (C) .7.An anti-soiling coating film obtained by curing the aqueous coating composition according to any one of claims 1 to 6.8.A substrate having an anti-soiling coating film on a substrate surface, which is obtained by removing water content from the aqueous coating composition according to any one of claims 1 to 6.9.The substrate according to claim 8, wherein the anti-soiling coating film is overcoated on a synthetic and / or artificial leather surface.10.The substrate according to claim 8 or 9, which is applied for vehicle interior material.11.A vehicle interior material having an anti-soiling coating film on a substrate surface, which is obtained by removing water content from the aqueous coating composition according to any one of claims 1 to 6.12.The vehicle interior material according to claim 11, which is a vehicle interior finishing sheet.13.A process for manufacturing a substrate having an anti-soiling coating film on a surface of the substrate, comprising:(I) applying the aqueous coating composition according to any one of claims 1 to 6 onto the surface of the substrate; and(II) forming an anti-soiling coating film by removing water content from the aqueous coating composition.