Multiphase gradient dispersion-chemical coupling method for preparing aerogel slurry
By employing a multiphase gradient dispersion-chemical coupling method, combined with shear dispersion and ultrasonic dispersion techniques, the dispersibility and stability issues of aerogel powder in aqueous systems were resolved, enabling the preparation of efficient and environmentally friendly aerogel slurries and improving their dispersibility and stability in aqueous systems.
Patent Information
- Application Number
- PCT/CN2025/113484
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2025-08-08
- Publication Date
- 2026-11-12
AI Technical Summary
Existing aerogel powders are difficult to disperse in aqueous systems, leading to structural damage and stratification, which affects their physicochemical properties and ease of use.
A multiphase gradient dispersion-chemical coupling method was adopted, using materials such as dispersants, coupling agents, carboxymethyl cellulose nanofiber whiskers, ammonium polyphosphate, polyethylene glycol, and carbon nanotubes, combined with shear dispersion and ultrasonic dispersion techniques, to form a stable three-dimensional network structure, thereby improving the dispersibility and stability of aerogels in aqueous systems.
It achieves good dispersion of aerogel in aqueous systems, avoids structural damage and stratification, improves the solid content and stability of aerogel slurry, simplifies the operation process, and meets green and environmental protection requirements.
Smart Images

Figure CN2025113484_12112026_PF_FP_ABST
Abstract
Description
A multiphase gradient dispersion-chemical coupling method for preparing aerogel slurry Technical Field
[0001] This invention relates to the technical field of aerogel slurry preparation, and more specifically, to a multiphase gradient dispersion-chemical coupling method for preparing aerogel slurries. Background Technology
[0002] Aerogels are novel solid materials with nanoporous structures, possessing excellent physicochemical properties such as high porosity, large specific surface area, low density, low thermal conductivity, and low dielectric constant, and are widely used in fields such as thermal insulation, adsorption, and catalysis. However, existing aerogel powders are difficult to disperse in aqueous systems due to their strong hydrophobicity, requiring high-speed stirring or prolonged dispersion, which can easily lead to structural damage and reduce their physicochemical properties. Furthermore, aerogel slurries have low solid content and tend to separate into layers after prolonged standing, requiring re-dispersion and stirring before use, which is inconvenient.
[0003] Chinese patent CN115676839A discloses a process for preparing aerogel slurry. This involves mixing water and a nano-stabilizer to form a solution, then adding aerogel powder and a nano-modifier to the solution and stirring to obtain the aerogel slurry. This patent solves the problem of hydrophobic aerogel powder being difficult to disperse in aqueous systems during use. Chinese patent CN117430372A discloses dispersible aerogel particles and its preparation method, including dissolving a dispersant and a wetting agent in water to form a dispersion, then adding aerogel powder, a silane coupling agent, and ammonium polyphosphate to react, and finally granulating and drying to obtain dispersible aerogel particles. The aerogel particles prepared by this patent have a hydrophobic inner layer and a hydrophilic outer layer, exhibiting good dispersibility in aqueous systems. It can be observed that while existing technologies optimize the dispersibility of aerogel powder in aqueous systems to some extent, the impact of various additives on the stability and compatibility of the aerogel slurry needs further improvement. Furthermore, the related preparation process steps and conditions limit the preparation efficiency and product quality of aerogel particles. To address the aforementioned issues, there is an urgent need to develop a highly efficient and high-quality method for preparing aerogel slurries, enabling aerogels to disperse well in aqueous systems, improving the solid content and stability of the aerogel slurries, avoiding stratification and water separation, thereby enhancing the ease of application of aerogel slurries. Summary of the Invention
[0004] To address the aforementioned technical problems in related technologies, this invention provides a multiphase gradient dispersion-chemical coupling method for preparing aerogel slurries, which can solve the above problems.
[0005] To achieve the above-mentioned technical objectives, the technical solution of the present invention is implemented as follows:
[0006] A multiphase gradient dispersion-chemical coupling method for preparing aerogel slurry includes the following steps:
[0007] S1. Weigh out the aerogel precursor, carboxymethyl cellulose nanofiber whiskers, ammonium polyphosphate, polyethylene glycol, carbon nanotubes, dispersant, and coupling agent according to the mass ratio of aerogel precursor: carboxymethyl cellulose nanofiber whiskers: ammonium polyphosphate: polyethylene glycol: carbon nanotubes: dispersant: coupling agent = 100: 2~5: 1~3: 0.8~1.5: 0.3~0.7: 0.5~1: 0.3~0.5 respectively, and measure out the solvent according to the mass-volume ratio of aerogel precursor: solvent = 1g: 20~30ml.
[0008] S2. Mix the dispersant, coupling agent and solvent, and adjust the pH value to 3-4 with 0.1mol / L hydrochloric acid to obtain mixture A. Then, pre-disperse mixture A for 10-20 minutes under a shear rate of 100-500rpm. Then add the aerogel precursor to mixture A to obtain the primary sol.
[0009] S3. Carboxymethyl cellulose nanofibers, ammonium polyphosphate, polyethylene glycol and carbon nanotubes are added to the primary sol obtained in S2, and the pH value is adjusted to 7-8 using a 0.1 mol / L sodium hydroxide solution to obtain mixture B. Then, the mixture B is dispersed by ultrasonication at a shear rate of 1000-2000 rpm to obtain the secondary sol.
[0010] S4. Adjust the pH of the secondary sol obtained in S3 to 10-11 using a 0.1 mol / L sodium hydroxide solution to obtain a precursor sol. Place the precursor sol in a vacuum environment with a vacuum degree of 0.03-0.05 MPa, and then introduce a high-purity gas stream into the precursor sol under a shear rate of 1000-1500 rpm to obtain an aerogel slurry with excellent dispersibility.
[0011] Furthermore, in S2, after the aerogel precursor is added to the mixture A, it needs to be dispersed for 10 to 20 minutes at a shear rate of 500 to 800 rpm to obtain the primary sol.
[0012] Furthermore, in S3, the ultrasonic frequency is 50kHz, the ultrasonic power is 800W, and the secondary sol can be obtained by ultrasonic dispersion for 20-30 minutes.
[0013] Furthermore, the flow rate of the high-purity gas stream in S3 is 0.3 to 0.5 L / min, and the introduction time of the high-purity gas stream lasts for 10 to 20 min.
[0014] Furthermore, the dispersant is any one of sodium oleate, sodium polyacrylate, and polyethylene glycol-polyacrylate copolymer.
[0015] Furthermore, the coupling agent is any one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570.
[0016] Furthermore, the solvent is water and ethanol.
[0017] Furthermore, the volume ratio of water to ethanol in the solvent is 1:3 to 5.
[0018] Furthermore, the aerogel precursor is any one or two of methyl orthosilicate (TMOS), tetraethyl orthosilicate (TEOS), polysiloxane (PEDS), methyltrimethoxysilane (MTMS), methyltriethoxysilane (MTES), and dimethyldiethoxysilane (DDS).
[0019] Furthermore, the high-purity gas stream is any one of high-purity carbon dioxide, high-purity nitrogen, or high-purity argon.
[0020] The beneficial effects of this invention are as follows: This invention chemically modifies the surface of hydrophobic aerogel powder to make it hydrophilic, and simultaneously combines shear dispersion and ultrasonic dispersion to improve the dispersibility of aerogel in aqueous systems, avoiding the structural damage caused by high-speed stirring or long-term dispersion, thus maintaining the excellent physicochemical properties of aerogel. This invention combines gradient dispersion and chemical coupling to form a stable three-dimensional network structure between aerogel particles and water molecules, effectively preventing stratification and water separation after prolonged standing, improving the solid content and stability of the aerogel slurry, and making it more convenient and faster to use. This invention utilizes dispersants, coupling agents, and carboxymethyl nanofibers... The presence of cellulose whiskers, ammonium polyphosphate, polyethylene glycol, and carbon nanotubes enables the aerogel precursor to react with hydroxyl groups on its surface during gradient dispersion. Simultaneously, polymer segments form physical entanglements with carboxymethyl cellulose nanofiber whiskers and ammonium polyphosphate, achieving a synergistic effect of multiphase interfacial chemical bonding and physical crosslinking. This significantly enhances the stability and compatibility of the aerogel slurry. The invention features a simple, mild, and low-cost preparation process, enabling the efficient and high-quality preparation of well-dispersed aerogel slurries. The preparation process generates no waste, meeting the requirements of green and environmentally friendly sustainable development. It can be promoted for industrial production, offering significant economic benefits. Attached Figure Description
[0021] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0022] The present invention will now be described in further detail with reference to the accompanying drawings.
[0023] Figure 1 is a flowchart of a multiphase gradient dispersion-chemical coupling method for preparing aerogel slurry according to an embodiment of the present invention. Detailed Implementation
[0024] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention are within the scope of protection of the present invention.
[0025] As shown in Figure 1, the present invention discloses a multiphase gradient dispersion-chemical coupling method for preparing aerogel slurry, comprising the following steps:
[0026] S1. Weigh out the aerogel precursor, carboxymethyl cellulose nanofiber whiskers, ammonium polyphosphate, polyethylene glycol, carbon nanotubes, dispersant, and coupling agent according to the mass ratio of aerogel precursor: carboxymethyl cellulose nanofiber whiskers: ammonium polyphosphate: polyethylene glycol: carbon nanotubes: dispersant: coupling agent = 100: 2~5: 1~3: 0.8~1.5: 0.3~0.7: 0.5~1: 0.3~0.5 respectively, and measure out the solvent according to the mass-volume ratio of aerogel precursor: solvent = 1g: 20~30ml.
[0027] S2. Mix the dispersant, coupling agent and solvent, and adjust the pH value to 3-4 with 0.1mol / L hydrochloric acid to obtain mixture A. Then, pre-disperse mixture A for 10-20 minutes under a shear rate of 100-500rpm. Then add the aerogel precursor to mixture A to obtain the primary sol.
[0028] S3. Carboxymethyl cellulose nanofibers, ammonium polyphosphate, polyethylene glycol and carbon nanotubes are added to the primary sol obtained in S2, and the pH value is adjusted to 7-8 using a 0.1 mol / L sodium hydroxide solution to obtain mixture B. Then, the mixture B is dispersed by ultrasonication at a shear rate of 1000-2000 rpm to obtain the secondary sol.
[0029] S4. Adjust the pH of the secondary sol obtained in S3 to 10-11 using a 0.1 mol / L sodium hydroxide solution to obtain a precursor sol. Place the precursor sol in a vacuum environment with a vacuum degree of 0.03-0.05 MPa, and then introduce a high-purity gas stream into the precursor sol under a shear rate of 1000-1500 rpm to obtain an aerogel slurry with excellent dispersibility. Example 1:
[0030] 0.48 g of sodium polyacrylate, 0.27 g of silane coupling agent KH560, and 1.8 L of water / ethanol solvent (water to ethanol volume ratio 1:3) were mixed, and the pH was adjusted to 3.8 using 0.1 mol / L hydrochloric acid to obtain mixture A. Mixture A was then pre-dispersed for 14 min at a shear rate of 180 rpm. Then, 70 g of tetraethyl orthosilicate was added to mixture A, and dispersion was continued for 13 min at a shear rate of 550 rpm to obtain a primary sol. 2.16 g of carboxymethyl cellulose nanofibers, 1.38 g of ammonium polyphosphate, 0.72 g of polyethylene glycol, and 0.34 g of carbon nanotubes were added to the primary sol, and the pH was adjusted to 7.6 using 0.1 mol / L sodium hydroxide solution to obtain mixture B. Subsequently, under a shear rate of 1500 rpm, ultrasonic dispersion mixture B was simultaneously used at a frequency of 50 kHz and a power of 800 W for 26 min to obtain a secondary sol. The pH of the secondary sol was adjusted to 10.3 using a 0.1 mol / L sodium hydroxide solution to obtain the precursor sol. The precursor sol was placed in a vacuum environment with a vacuum degree of 0.04 MPa, and then a high-purity carbon dioxide gas flow was introduced into the precursor sol at a shear rate of 1400 rpm at a flow rate of 0.35 L / min for 12 min, resulting in an aerogel slurry with excellent dispersibility. Example 2:
[0031] 0.82 g of polyethylene glycol-polyacrylate copolymer, 0.47 g of silane coupling agent KH570, and 3.2 L of water / ethanol solvent (water to ethanol volume ratio 1:4) were mixed, and the pH was adjusted to 3.4 using 0.1 mol / L hydrochloric acid to obtain mixture A. Mixture A was then pre-dispersed for 17 min at a shear rate of 350 rpm. Then, a mixture of 120 g of tetraethyl orthosilicate and polysiloxane (tetraethyl orthosilicate to polysiloxane mass ratio 2:3) was added to mixture A, and dispersion was continued for 18 min at a shear rate of 750 rpm to obtain a primary sol. 4.35 g of carboxymethyl cellulose nanofibers, 3.22 g of ammonium polyphosphate, 1.28 g of polyethylene glycol, and 0.63 g of carbon nanotubes were added to the primary sol, and the pH was adjusted to 7.3 using 0.1 mol / L sodium hydroxide solution to obtain mixture B. Subsequently, under a shear rate of 1400 rpm, ultrasonic dispersion mixture B was simultaneously used at a frequency of 50 kHz and a power of 800 W for 22 min to obtain a secondary sol. The pH of the secondary sol was adjusted to 10.5 using a 0.1 mol / L sodium hydroxide solution to obtain the precursor sol. The precursor sol was placed in a vacuum environment with a vacuum degree of 0.05 MPa, and then a high-purity nitrogen gas flow was introduced into the precursor sol at a shear rate of 1200 rpm at a flow rate of 0.42 L / min for 16 min, resulting in an aerogel slurry with excellent dispersibility. Example 3:
[0032] 0.76 g of sodium oleate, 0.35 g of silane coupling agent KH550, and 2.4 L of water / ethanol solvent (water to ethanol volume ratio 1:3) were mixed, and the pH was adjusted to 3.2 using 0.1 mol / L hydrochloric acid to obtain mixture A. Mixture A was then pre-dispersed for 12 min at a shear rate of 200 rpm. Then, 90 g of methyl orthosilicate was added to mixture A, and dispersion was continued for 16 min at a shear rate of 600 rpm to obtain a primary sol. 3.75 g of carboxymethyl cellulose nanofibers, 2.46 g of ammonium polyphosphate, 1.16 g of polyethylene glycol, and 0.57 g of carbon nanotubes were added to the primary sol, and the pH was adjusted to 7.2 using 0.1 mol / L sodium hydroxide solution to obtain mixture B. Subsequently, under a shear rate of 1700 rpm, ultrasonic dispersion mixture B was simultaneously used at a frequency of 50 kHz and a power of 800 W for 25 min to obtain a secondary sol. The pH of the secondary sol was adjusted to 10.7 using a 0.1 mol / L sodium hydroxide solution to obtain the precursor sol. The precursor sol was placed in a vacuum environment with a vacuum degree of 0.04 MPa, and then a high-purity argon gas flow was introduced into the precursor sol at a shear rate of 1000 rpm at a flow rate of 0.47 L / min for 18 min, resulting in an aerogel slurry with excellent dispersibility. Example 4:
[0033] 1.58 g of sodium polyacrylate, 0.96 g of silane coupling agent KH570, and 5.7 L of water / ethanol solvent (water to ethanol volume ratio 1:5) were mixed, and the pH was adjusted to 3.7 using 0.1 mol / L hydrochloric acid to obtain mixture A. Mixture A was then pre-dispersed for 16 min at a shear rate of 400 rpm. Then, a mixture of 210 g of methyl orthosilicate and methyltriethoxysilane (methyl orthosilicate to methyltriethoxysilane mass ratio 4:1) was added to mixture A, and dispersion was continued for 12 min at a shear rate of 650 rpm to obtain a primary sol. 7.64 g of carboxymethyl cellulose nanofibers, 4.82 g of ammonium polyphosphate, 2.13 g of polyethylene glycol, and 1.16 g of carbon nanotubes were added to the primary sol, and the pH was adjusted to 7.5 using 0.1 mol / L sodium hydroxide solution to obtain mixture B. Subsequently, under a shear rate of 1600 rpm, ultrasonic dispersion mixture B was simultaneously used at a frequency of 50 kHz and a power of 800 W for 23 min to obtain a secondary sol. The pH of the secondary sol was adjusted to 10.6 using a 0.1 mol / L sodium hydroxide solution to obtain the precursor sol. The precursor sol was placed in a vacuum environment with a vacuum degree of 0.05 MPa, and then a high-purity carbon dioxide gas flow was introduced into the precursor sol at a shear rate of 1300 rpm at a flow rate of 0.38 L / min for 14 min, resulting in an aerogel slurry with excellent dispersibility. Example 5:
[0034] 2.65 g of sodium oleate, 1.36 g of silane coupling agent KH550, and 7.8 L of water / ethanol solvent (water to ethanol volume ratio 1:4) were mixed, and the pH was adjusted to 3.5 using 0.1 mol / L hydrochloric acid to obtain mixture A. Mixture A was then pre-dispersed for 20 min at a shear rate of 450 rpm. Then, a mixture of 300 g of methyltrimethoxysilane and dimethyldiethoxysilane (mass ratio 3:7) was added to mixture A, and dispersion was continued for 14 min at a shear rate of 700 rpm to obtain a primary sol. 13.26 g of carboxymethyl cellulose nanofibers, 5.83 g of ammonium polyphosphate, 3.92 g of polyethylene glycol, and 1.47 g of carbon nanotubes were added to the primary sol, and the pH was adjusted to 7.8 using 0.1 mol / L sodium hydroxide solution to obtain mixture B. Subsequently, under a shear rate of 1300 rpm, ultrasonic dispersion mixture B was simultaneously used at a frequency of 50 kHz and a power of 800 W for 28 min to obtain a secondary sol. The pH of the secondary sol was adjusted to 10.2 using a 0.1 mol / L sodium hydroxide solution to obtain the precursor sol. The precursor sol was placed in a vacuum environment with a vacuum degree of 0.03 MPa, and then a high-purity nitrogen gas flow was introduced into the precursor sol at a shear rate of 1500 rpm at a flow rate of 0.46 L / min for 15 min, resulting in an aerogel slurry with excellent dispersibility.
[0035] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A multiphase gradient dispersion-chemical coupling method for preparing aerogel slurry, characterized in that, Includes the following steps: S1. Weigh out the aerogel precursor, carboxymethyl cellulose nanofiber whiskers, ammonium polyphosphate, polyethylene glycol, carbon nanotubes, dispersant, and coupling agent according to the mass ratio of aerogel precursor: carboxymethyl cellulose nanofiber whiskers: ammonium polyphosphate: polyethylene glycol: carbon nanotubes: dispersant: coupling agent = 100: 2~5: 1~3: 0.8~1.5: 0.3~0.7: 0.5~1: 0.3~0.5 respectively, and measure out the solvent according to the mass-volume ratio of aerogel precursor: solvent = 1g: 20~30ml. S2. Mix the dispersant, coupling agent and solvent, and adjust the pH value to 3-4 with 0.1mol / L hydrochloric acid to obtain mixture A. Then, pre-disperse mixture A for 10-20 minutes under a shear rate of 100-500rpm. Then add the aerogel precursor to mixture A to obtain the primary sol. S3. Carboxymethyl cellulose nanofibers, ammonium polyphosphate, polyethylene glycol and carbon nanotubes are added to the primary sol obtained in S2, and the pH value is adjusted to 7-8 using a 0.1 mol / L sodium hydroxide solution to obtain mixture B. Then, the mixture B is dispersed by ultrasonication at a shear rate of 1000-2000 rpm to obtain the secondary sol. S4. Adjust the pH of the secondary sol obtained in S3 to 10-11 using a 0.1 mol / L sodium hydroxide solution to obtain a precursor sol. Place the precursor sol in a vacuum environment with a vacuum degree of 0.03-0.05 MPa, and then introduce a high-purity gas stream into the precursor sol under a shear rate of 1000-1500 rpm to obtain an aerogel slurry with excellent dispersibility.
2. The multiphase gradient dispersion-chemical coupling method for preparing aerogel slurry according to claim 1, characterized in that, In step S2, after the aerogel precursor is added to the mixture A, it needs to be dispersed for 10 to 20 minutes at a shear rate of 500 to 800 rpm to obtain the primary sol.
3. The multiphase gradient dispersion-chemical coupling method for preparing aerogel slurry according to claim 2, characterized in that: The ultrasonic frequency described in S3 is 50kHz, the ultrasonic power is 800W, and the secondary sol can be obtained by ultrasonic dispersion for 20-30 minutes.
4. The multiphase gradient dispersion-chemical coupling method for preparing aerogel slurry according to claim 3, characterized in that: The high-purity gas flow rate described in S3 is 0.3 to 0.5 L / min, and the high-purity gas flow is introduced for 10 to 20 min.
5. The multiphase gradient dispersion-chemical coupling method for preparing aerogel slurry according to claim 1, characterized in that: The dispersant is any one of sodium oleate, sodium polyacrylate, and polyethylene glycol-polyacrylate copolymer.
6. The multiphase gradient dispersion-chemical coupling method for preparing aerogel slurry according to claim 1, characterized in that: The coupling agent is any one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570.
7. The multiphase gradient dispersion-chemical coupling method for preparing aerogel slurry according to claim 1, characterized in that: The solvents are water and ethanol.
8. The multiphase gradient dispersion-chemical coupling method for preparing aerogel slurry according to claim 7, characterized in that: The volume ratio of water to ethanol in the solvent is 1:3 to 5.
9. The multiphase gradient dispersion-chemical coupling method for preparing aerogel slurry according to claim 1, characterized in that: The aerogel precursor is any one or two of the following: methyl orthosilicate (TMOS), tetraethyl orthosilicate (TEOS), polysiloxane (PEDS), methyltrimethoxysilane (MTMS), methyltriethoxysilane (MTES), and dimethyldiethoxysilane (DDS).
10. The multiphase gradient dispersion-chemical coupling method for preparing aerogel slurry according to claim 1, characterized in that: The high-purity gas stream is any one of high-purity carbon dioxide, high-purity nitrogen, or high-purity argon.