High-strength wear-resistant lightweight fabric, and preparation method therefor and use thereof
By plasma modification and finishing agent modification of ultra-fine denier ultra-high molecular weight polyethylene yarn, high-strength, wear-resistant, and lightweight fabrics are prepared, solving the problem that lightweight materials cannot simultaneously meet the requirements of high strength, wear resistance, and comfort, thus achieving both lightweighting and performance improvement of the fabric.
Patent Information
- Application Number
- PCT/CN2025/146725
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2025-12-29
- Publication Date
- 2026-11-12
AI Technical Summary
Existing high-strength abrasion-resistant fabrics face technical bottlenecks in terms of performance, lightweighting, and comfort, making it difficult to simultaneously achieve a balance between high strength, abrasion resistance, and comfort.
Plasma modification was used to treat ultrafine denier ultra-high molecular weight polyethylene yarn, which was then mixed with a finishing agent and interwoven with ultrafine denier N66 yarn to prepare a high-strength, wear-resistant, and lightweight fabric.
It achieves lightweight fabric while improving tear resistance and abrasion resistance, meeting the needs of use in extreme environments and demanding scenarios.
Smart Images

Figure PCTCN2025146725-FTAPPB-I100001 
Figure PCTCN2025146725-FTAPPB-I100002 
Figure PCTCN2025146725-FTAPPB-I100003
Abstract
Description
A high-strength, wear-resistant, lightweight fabric, its preparation method, and its application.
[0001] This application claims priority to Chinese Patent Application No. 202510585388.4, filed on May 8, 2025, entitled "A High-Strength Wear-Resistant Lightweight Fabric and Its Preparation Method and Application", the entire contents of which are incorporated herein by reference. Technical Field
[0002] This invention relates to the field of functional fabric technology, and in particular to a high-strength, wear-resistant, lightweight fabric, its preparation method, and its application. Background Technology
[0003] With the rapid development of the textile industry, the market demand for functional fabrics is increasing, especially in outdoor sports, military equipment, and high-end clothing, where higher requirements are placed on the strength, abrasion resistance, and service life of fabrics. However, the high-strength abrasion-resistant fabrics currently on the market still face certain technical bottlenecks in terms of performance, lightweight, and comfort. This is because lightweight materials often cannot simultaneously achieve a balance between high strength, abrasion resistance, and comfort.
[0004] Therefore, providing an innovative method for preparing high-strength and wear-resistant fabrics, which produces fabrics that possess excellent mechanical properties and durability while also being lightweight and multifunctional, thus meeting the usage requirements of various extreme environments and demanding scenarios, remains a problem that urgently needs to be solved in this field. Summary of the Invention
[0005] To address the aforementioned technical problems, this invention provides a high-strength, abrasion-resistant, lightweight fabric, its preparation method, and its applications. The fabric prepared using the method provided by this invention has a relatively low overall weight and exhibits excellent tear resistance and abrasion resistance.
[0006] To achieve this objective, the present invention adopts the following technical solution:
[0007] In a first aspect, the present invention provides a method for preparing a high-strength, wear-resistant, and lightweight fabric, the method comprising the following steps:
[0008] (1) Plasma modification treatment of ultrafine denier ultra-high molecular weight polyethylene yarn under the action of argon gas;
[0009] (2) The plasma-modified ultrafine denier ultra-high molecular weight polyethylene yarn obtained in step (1) is mixed with a finishing agent for modification;
[0010] (3) The mixed modified ultrafine denier ultra-high molecular weight polyethylene yarn obtained in step (2) is interwoven with ultrafine denier N66 yarn to obtain the high-strength wear-resistant lightweight fabric.
[0011] In step (1) of this invention, the ultra-fine denier ultra-high molecular weight polyethylene yarn is first subjected to plasma modification treatment, which can significantly increase the surface roughness of the polyethylene yarn. The molecular chain of the polyethylene yarn is composed of long-chain polyethylene (-CH2-CH2-) repeating units. Argon gas ionization generates high-density argon ions and other high-energy particles. These high-energy particles bombard the surface of the polyethylene yarn at high speed, causing some CH molecular chains to break. The free radicals generated by the breakage combine with the free radicals on the adjacent molecular chains to form new CC bonds, connecting the originally independent molecular chains into a three-dimensional network structure, achieving better overall interaction, which is beneficial to improving the wear resistance and tear resistance of the obtained fabric. At the same time, it is also beneficial to its combination and adsorption with finishing agents, enabling it to adsorb more finishing agents and undergo sufficient modification during the mixing and modification process with finishing agents, further improving the wear resistance and tear resistance of the obtained fabric.
[0012] This invention employs a process of first subjecting ultra-fine denier ultra-high molecular weight polyethylene yarn to plasma modification and then to finishing agent modification, followed by interweaving it with N66 yarn to obtain a fabric. This not only ensures the lightweight nature of the material but also effectively improves the tear resistance and abrasion resistance of the resulting fabric. This effectively solves the problem that current lightweight materials struggle to simultaneously achieve a balance between high strength, abrasion resistance, and comfort, thus meeting the usage requirements of various extreme environments and demanding scenarios.
[0013] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. The purpose and beneficial effects of the present invention can be better achieved and realized through the following preferred technical solutions.
[0014] As a preferred embodiment of the present invention, in the mixing modification described in step (2), the bath ratio of the plasma-modified ultrafine denier ultra-high molecular weight polyethylene yarn obtained in step (1) to the finishing agent is 1:(35-45), where (35-45) can be, for example, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44 or 45, and specific values between the above values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range. The bath ratio is generally the ratio of weight (g) to volume (L).
[0015] In step (2) of the present invention, preferably, by adjusting the bath ratio of the plasma-modified ultrafine denier ultra-high molecular weight polyethylene yarn obtained in step (1) to the finishing agent to 1:(35-45), the ultrafine denier ultra-high molecular weight polyethylene yarn can be more fully mixed and modified, thereby the resulting fabric has better abrasion resistance and tear resistance. However, when the bath ratio is too high or too low, the finishing agent on the yarn surface may be unevenly distributed, resulting in inconsistent yarn performance or failure to achieve ideal performance, which in turn reduces the abrasion resistance and tear resistance of the resulting fabric.
[0016] As a preferred technical solution of the present invention, the ultra-fine denier ultra-high molecular weight polyethylene yarn in step (1) is 15-20D (for example, it can be 15D, 16D, 17D, 18D, 19D or 20D, etc.) ultra-fine denier ultra-high molecular weight polyethylene yarn.
[0017] Preferably, the weight-average molecular weight of the ultrafine denier ultra-high molecular weight polyethylene yarn is ≥1×10⁻⁶. 6 g / mol.
[0018] Preferably, the ultrafine denier N66 yarn in step (3) is 15-20D (e.g., 15D, 16D, 17D, 18D, 19D, or 20D, etc.) ultrafine denier N66 yarn. N66 yarn usually refers to Nylon 66 yarn, which is a common commercial model name for polyamide 66 fiber.
[0019] The preparation method provided by the present invention is more preferably applicable to 20D ultrafine denier ultra-high molecular weight polyethylene yarn and 15-20D ultrafine denier N66 yarn materials, which are lighter in weight and stronger.
[0020] As a preferred technical solution of the present invention, in step (1), the pressure of the plasma modification treatment is 60-80 Pa, for example, it can be 60 Pa, 62 Pa, 64 Pa, 66 Pa, 68 Pa, 70 Pa, 72 Pa, 74 Pa, 76 Pa, 78 Pa or 80 Pa, as well as specific point values between the above point values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific point values included in the range.
[0021] Preferably, the power of the plasma modification treatment is 200-220W, for example, it can be 200W, 202W, 204W, 206W, 208W, 210W, 212W, 214W, 216W, 218W or 220W, as well as specific values between the above values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0022] Preferably, the plasma modification treatment time is 2-15 min, for example, it can be 2 min, 5 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min or 15 min, as well as specific point values between the above points. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific point values included in the range, but preferably it is 8-10 min.
[0023] In this embodiment of the invention, the plasma treatment process parameters for the yarn (15-20D ultra-fine denier ultra-high molecular weight polyethylene yarn) are precisely controlled. Within the parameter range described in this invention, the effective action of plasma on the yarn surface can be guaranteed, while avoiding poor treatment effect or damage to the yarn structure caused by parameters that are too high or too low. This results in better achieving the effect of lightweight fabric with excellent tear resistance and abrasion resistance.
[0024] As a preferred embodiment of the present invention, the finishing agent in step (2) comprises the following components by mass percentage:
[0025] Polyurethane 8-15%;
[0026] Crosslinking agent 5-10%;
[0027] Surfactant 6-12%;
[0028] Dispersant 5-15%;
[0029] Adhesive 5-10%;
[0030] The remainder is water (deionized water can be used).
[0031] In this invention, the mass percentage of polyurethane can be 8%, 9%, 10%, 11%, 12%, 13%, 14%, or 15%, etc.
[0032] The mass percentage of the crosslinking agent can be 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, or 10%, etc.
[0033] The mass percentage of surfactant can be 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 11%, or 12%, etc.
[0034] The mass percentage of the dispersant can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, or 15%, etc.
[0035] The mass percentage of the adhesive can be 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, or 10%, etc.
[0036] Preferably, the weight-average molecular weight of the polyurethane is 50,000-70,000, for example, it can be 50,000, 52,000, 54,000, 56,000, 58,000, 60,000, 62,000, 64,000, 66,000, 68,000 or 70,000, as well as specific values between the above values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0037] In this invention, the polyurethane may be, for example, any one or a combination of at least two of polyester polyurethane, polyether polyurethane, polycarbonate polyurethane, or waterborne polyurethane dispersion.
[0038] Preferably, the crosslinking agent comprises polysiloxane.
[0039] Preferably, the surfactant comprises secondary alkyl sulfonate and / or sodium sulfonated fatty acid methyl ester.
[0040] Preferably, the dispersant comprises any one or a combination of at least two of fatty alcohol polyoxyethylene ethers, fatty acid polyoxyethylene esters, naphthalene sulfonic acid dispersants, or polycarboxylic acid dispersants.
[0041] It should be noted that there are no special restrictions on the types of fatty alcohol polyoxyethylene ethers, fatty acid polyoxyethylene esters, naphthalene sulfonic acid dispersants, and polycarboxylic acid dispersants in this invention. Commonly used fatty alcohol polyoxyethylene ethers, fatty acid polyoxyethylene esters, naphthalene sulfonic acid dispersants, and polycarboxylic acid dispersants in the art are all applicable.
[0042] For example, the fatty alcohol polyoxyethylene ether includes, but is not limited to: AEO-7, dispersant AT-80, dispersant IW, etc.; the fatty acid polyoxyethylene ester includes, but is not limited to: fatty acid polyoxyethylene ester OEO series, LAE series, SG series, SE series, A-105 / A-110, etc.; the naphthalene sulfonic acid dispersant includes, but is not limited to: methylnaphthalene sulfonate dispersant, naphthalene sulfonate dispersant, naphthalene sulfonic acid formaldehyde condensate dispersant (NNO), etc.; the polycarboxylic acid dispersant includes, but is not limited to: polyacrylic acid (PAA), sodium polyacrylate (PAAS), hydrolyzed polymaleic anhydride (HPMA), maleic acid-acrylic acid copolymer (MA / AA), acrylic acid-2-acrylamide-2-methylpropanesulfonic acid multi-component copolymer (AA / AMPS), polycarboxylic acid ammonium dispersant 5027, modified polycarboxylate (TH-2000), carboxylate-sulfonate-nonionic terpolymer (TH-3100), etc.
[0043] Preferably, the adhesive comprises any one or a combination of at least two of polyurethane adhesives, polyvinyl acetate adhesives, polyacrylate adhesives, or butadiene adhesives.
[0044] It should be noted that there are no special restrictions on the types of polyurethane adhesives, polyvinyl acetate adhesives, polyacrylate adhesives and butadiene adhesives in this invention. Commonly used polyurethane adhesives, polyvinyl acetate adhesives, polyacrylate adhesives and butadiene adhesives in the art are all applicable.
[0045] As a preferred embodiment of the present invention, the mass ratio of the polyurethane to the adhesive is (1.25-2.5):1, wherein (1.25-2.5) can be, for example, 1.25, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4 or 2.5, and specific values between the above values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0046] In the finishing agent of this invention, the mass ratio of polyurethane to adhesive can be (1.25-2.5):1, which can significantly improve the tear strength and abrasion resistance of the resulting fabric. When the mass ratio is too low, the polyurethane molecular chain contains a large number of hydrogen bonds and cross-linking structures, which can improve the overall performance of the material. When its content is too low, the abrasion resistance and mechanical properties of the material will decrease. When the mass ratio is too high, that is, the adhesive concentration is too low, it is impossible to form a complete covering layer. Some areas of the substrate surface are not effectively wrapped by the adhesive, which makes it easy for the polyurethane to peel off from the substrate interface under external force, thereby reducing its abrasion resistance.
[0047] Preferably, the hybrid modification in step (2) includes a heating stage, a heat preservation stage, and a cooling stage.
[0048] Preferably, the heating stage includes heating to 175-185℃, for example, 175℃, 176℃, 177℃, 178℃, 179℃, 180℃, 181℃, 182℃, 183℃, 184℃ or 185℃, as well as specific values between the above points. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0049] Preferably, the heating rate during the heating stage is 2-8℃ / min, for example, it can be 2℃ / min, 3℃ / min, 4℃ / min, 5℃ / min, 6℃ / min, 7℃ / min or 8℃ / min, as well as specific values between the above values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0050] Preferably, the heat preservation stage lasts for 25-35 minutes, for example, 25 minutes, 26 minutes, 27 minutes, 28 minutes, 29 minutes, 30 minutes, 31 minutes, 32 minutes, 33 minutes, 34 minutes, or 35 minutes, as well as specific values between the above values. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific values included in the range.
[0051] Preferably, the cooling stage includes cooling to 55-65℃, for example, 55℃, 56℃, 57℃, 58℃, 59℃, 60℃, 61℃, 62℃, 63℃, 64℃ or 65℃, as well as specific values between the above points. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0052] Preferably, the cooling rate during the cooling stage is 2-8℃ / min, for example, it can be 2℃ / min, 3℃ / min, 4℃ / min, 5℃ / min, 6℃ / min, 7℃ / min or 8℃ / min, as well as specific values between the above values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0053] Preferably, the mixing modification is carried out under stirring.
[0054] Preferably, the stirring speed is 800-1200 r / min, for example, it can be 800 r / min, 850 r / min, 900 r / min, 950 r / min, 1000 r / min, 1050 r / min, 1100 r / min, 1150 r / min or 1200 r / min, and specific values between the above values. Due to space limitations and for the sake of brevity, the present invention will not exhaustively list the specific values included in the range.
[0055] As a preferred embodiment of the present invention, the method for preparing the high-strength, wear-resistant, and lightweight fabric specifically includes the following steps:
[0056] (1) Plasma modification treatment is performed on 15-20D ultrafine denier ultra-high molecular weight polyethylene yarn. The pressure of the plasma modification treatment is 60-80Pa, the power is 200-220W, and the time is 2-15min.
[0057] (2) The plasma-modified ultrafine denier ultra-high molecular weight polyethylene yarn obtained in step (1) and the finishing agent are mixed and modified at a bath ratio of 1:(35-45).
[0058] (3) The mixed modified ultrafine denier ultra-high molecular weight polyethylene yarn obtained in step (2) is interwoven with 15-20D ultrafine denier N66 yarn, and optionally dyed and set to obtain a high-strength, wear-resistant, and lightweight fabric.
[0059] The interweaving generally refers to a woven or woven form involving warp and weft yarns. This invention does not impose special limitations on the dyeing and setting of interwoven fabrics; procedures well-known to those skilled in the art can be employed.
[0060] Secondly, the present invention provides a high-strength, wear-resistant, and lightweight fabric, which is prepared according to the preparation method described in the first aspect.
[0061] Preferably, the abrasion resistance of the high-strength, abrasion-resistant, and lightweight fabric is 210,000-320,000 revolutions (e.g., 210,000, 230,000, 250,000, 280,000, 300,000, or 320,000 revolutions, referencing GB / T 21196.2-2007 "Textiles - Martindale Method for Determination of Abrasion Resistance of Fabrics - Part 2: Determination of Specimen Breakage"); referencing GB / T Standard 3917.2-2009, "Textiles - Tear Properties of Fabrics - Part 2: Determination of Tear Strength of Trousers Specimens (Single Seam)," specifies that the warp strength is 24-32 N (e.g., 24 N, 25 N, 26 N, 27 N, 28 N, 29 N, 30 N, 31 N, or 32 N), the weft strength is 24-38 N (e.g., 24 N, 26 N, 28 N, 30 N, 32 N, 34 N, 36 N, or 38 N), and the basis weight is 30-35 GSM (e.g., 30 GSM, 31 GSM, 32 GSM, 33 GSM, 34 GSM, or 35 GSM).
[0062] Thirdly, the present invention provides an application of the high-strength, abrasion-resistant, and lightweight fabric as described in the second aspect in outdoor sports equipment, military equipment, clothing, packaging materials, or household goods.
[0063] Compared with the prior art, the present invention has at least the following beneficial effects:
[0064] (1) The present invention adopts a method of preparing fabric by sequentially performing plasma modification treatment and finishing agent modification on ultra-fine denier ultra-high molecular weight polyethylene yarn and then interweaving it with N66 yarn. This method can effectively improve the tear resistance and wear resistance of the obtained fabric, thereby effectively solving the problem that lightweight materials are difficult to balance with high strength, wear resistance and comfort at the same time. This method can meet the usage requirements of various extreme environments and high-requirement scenarios.
[0065] (2) The preparation method provided by the present invention has prepared a high-strength wear-resistant lightweight fabric with a wear resistance of 210,000-320,000 revolutions, a warp strength of 24-32N, a weft strength of 24-38N, and a weight of 30-35GSM. Detailed Implementation
[0066] To facilitate understanding of the present invention, the following embodiments are provided. Those skilled in the art should understand that these embodiments are merely illustrative and should not be construed as limiting the scope of the invention.
[0067] Unless otherwise specified, all raw materials and reagents used in the following examples are commercially available products. Some raw material information is as follows:
[0068] Polyethylene yarn: LX254 from Dongguan Lanxin New Material Weaving Technology Co., Ltd.
[0069] Nylon yarn: N66, purchased from Shenzhen Shunlong Thread Industry Co., Ltd.;
[0070] Polyurethane: for Wanhua Chemical 7865;
[0071] Crosslinking agent: polysiloxane, purchased from Hubei Xinghengye Company, model number 110-18-9;
[0072] Surfactant: Sodium sulfonated fatty acid methyl ester, purchased from Hubei Shineng Chemical Technology Co., Ltd., model number 93348-22-2;
[0073] Dispersant: Fatty acid polyoxyethylene ester, purchased from Wuhan Jixin Yibang Co., Ltd., model number 106-08-1;
[0074] Adhesive: Polyurethane acrylate, purchased from Hunan Jinhai Technology Co., Ltd., model JS311.
[0075] Preparation Examples 1-7
[0076] Preparation Examples 1-7 each provide a finishing agent. The components and amounts contained therein, based on a total mass of 100%, are shown in Table 1. In Table 1, the amount of each component is expressed in "%".
[0077] Table 1. Dosage of finishing agent components in preparation examples 1-7
[0078] Example 1
[0079] This embodiment provides a high-strength, wear-resistant, and lightweight fabric, the preparation method of which includes the following steps:
[0080] (1) Plasma modification treatment was carried out on 20D ultrafine denier ultra-high molecular weight polyethylene yarn. The treatment gas was argon, the pressure was 70Pa, the power was 210W, and the treatment time was 3min.
[0081] (2) The ultrafine denier ultra-high molecular weight polyethylene yarn treated by plasma in step (1) was mixed with the finishing agent (Preparation Example 1) at a bath ratio of 1:40 for modification. The temperature was set at 180°C, the heating rate was 3°C / min, the rotation speed was 1000 r / min, and the temperature was kept stable for 30 min before cooling down at a rate of 5°C / min until it dropped to 60°C, thus obtaining the modified ultrafine denier ultra-high molecular weight polyethylene yarn.
[0082] (3) The modified ultrafine denier ultra-high molecular weight polyethylene yarn described in step (2) is interwoven with 20D ultrafine denier N66 yarn, dyed and set to obtain the high-strength wear-resistant lightweight fabric.
[0083] Example 2
[0084] This embodiment provides a high-strength, wear-resistant, and lightweight fabric, the preparation method of which includes the following steps:
[0085] (1) Plasma modification treatment was carried out on 20D ultrafine denier ultra-high molecular weight polyethylene yarn. The treatment gas was argon, the pressure was 60Pa, the power was 200W, and the treatment time was 8min.
[0086] (2) The ultrafine denier ultra-high molecular weight polyethylene yarn after plasma treatment in step (1) was modified with finishing agent (preparation example 2) at a bath ratio of 1:35. The temperature was set at 175°C, the heating rate was 2°C / min, the rotation speed was 800 r / min, and the temperature was kept stable for 35 min before cooling down at a rate of 8°C / min until it dropped to 55°C, thus obtaining the modified ultrafine denier ultra-high molecular weight polyethylene yarn.
[0087] (3) The modified ultrafine denier ultra-high molecular weight polyethylene yarn described in step (2) is interwoven with 20D ultrafine denier N66 yarn, dyed and set to obtain the high-strength wear-resistant lightweight fabric.
[0088] Example 3
[0089] This embodiment provides a high-strength, wear-resistant, and lightweight fabric, the preparation method of which includes the following steps:
[0090] (1) Plasma modification treatment was carried out on 20D ultrafine denier ultra-high molecular weight polyethylene yarn. The treatment gas was argon, the pressure was 80Pa, the power was 220W, and the treatment time was 15min.
[0091] (2) The polyethylene yarn treated by plasma in step (1) was modified with finishing agent (preparation example 3) at a bath ratio of 1:45. The temperature was set at 185°C, the heating rate was 8°C / min, the rotation speed was 1000 r / min, the temperature was kept stable for 25 min and then the temperature was lowered at a rate of 8°C / min until it dropped to 6°C, thus obtaining modified ultrafine denier ultra-high molecular weight polyethylene yarn.
[0092] (3) The modified ultrafine denier ultra-high molecular weight polyethylene yarn described in step (2) is interwoven with 20D ultrafine denier N66 yarn, dyed and set to obtain the high-strength wear-resistant lightweight fabric.
[0093] Example 4
[0094] This embodiment provides a high-strength, wear-resistant, and lightweight fabric. The only difference between this embodiment and Embodiment 1 is that the liquor ratio in step (2) is adjusted from 1:40 to 1:30. All other steps and parameter settings are the same as in Embodiment 1.
[0095] Example 5
[0096] This embodiment provides a high-strength, wear-resistant, and lightweight fabric. The only difference between this embodiment and Embodiment 1 is that the bath ratio in step (2) is adjusted from 1:40 to 1:50. All other steps and parameter settings are the same as in Embodiment 1.
[0097] Example 6
[0098] This embodiment provides a high-strength, wear-resistant, and lightweight fabric. The only difference between this embodiment and Embodiment 1 is that the air pressure in step (1) is adjusted from 70Pa to 50Pa. All other steps and parameter settings are the same as in Embodiment 1.
[0099] Example 7
[0100] This embodiment provides a high-strength, wear-resistant, and lightweight fabric. The only difference between this embodiment and Embodiment 1 is that the air pressure in step (1) is adjusted from 70Pa to 90Pa. All other steps and parameter settings are the same as in Embodiment 1.
[0101] Example 8
[0102] This embodiment provides a high-strength, wear-resistant, and lightweight fabric. The only difference between this embodiment and Embodiment 1 is that the power in step (1) is adjusted from 210W to 190W. All other steps and parameter settings are the same as in Embodiment 1.
[0103] Example 9
[0104] This embodiment provides a high-strength, wear-resistant, and lightweight fabric. The only difference between this embodiment and Embodiment 1 is that the power in step (1) is adjusted from 210W to 230W. All other steps and parameter settings are the same as in Embodiment 1.
[0105] Example 10
[0106] This embodiment provides a high-strength, wear-resistant, and lightweight fabric. The only difference between this embodiment and Embodiment 1 is that the finishing agent (Preparation Example 1) in step (2) is replaced with a finishing agent (Preparation Example 4). All other steps and parameter settings are the same as in Embodiment 1.
[0107] Example 11
[0108] This embodiment provides a high-strength, wear-resistant, and lightweight fabric. The only difference between this embodiment and Embodiment 1 is that the finishing agent (Preparation Example 1) in step (2) is replaced with the finishing agent (Preparation Example 5). All other steps and parameter settings are the same as in Embodiment 1.
[0109] Example 12
[0110] This embodiment provides a high-strength, wear-resistant, and lightweight fabric. The only difference between this embodiment and Embodiment 1 is that the finishing agent (Preparation Example 1) in step (2) is replaced with a finishing agent (Preparation Example 6). All other steps and parameter settings are the same as in Embodiment 1.
[0111] Example 13
[0112] This embodiment provides a high-strength, wear-resistant, and lightweight fabric. The only difference between this embodiment and Embodiment 1 is that the finishing agent (Preparation Example 1) in step (2) is replaced with a finishing agent (Preparation Example 7). All other steps and parameter settings are the same as in Embodiment 1.
[0113] Comparative Example 1
[0114] This comparative example provides a high-strength, wear-resistant, and lightweight fabric, the preparation method of which includes the following steps:
[0115] (1) Interweave 15-20D ultrafine denier ultra-high molecular weight polyethylene yarn with 15-20D ultrafine denier N66 yarn, dye and fix to obtain the base fabric.
[0116] (2) The base fabric obtained in step (1) is subjected to plasma modification treatment. The treatment gas is argon, the pressure is 70Pa, the power is 210W, and the treatment time is 3min.
[0117] (3) The base fabric treated by plasma in step (1) is mixed with finishing agent (preparation example 1) at a liquor ratio of 1:40 for modification. The temperature is set at 180°C, the heating rate is 3°C / min, the rotation speed is 1000r / min, the temperature is kept stable for 30min and then the temperature is lowered at a rate of 5°C / min until it drops to 60°C. The fabric is then dyed and set to obtain the high-strength wear-resistant lightweight fabric.
[0118] Comparative Example 2
[0119] This comparative example provides a high-strength, wear-resistant, and lightweight fabric, the preparation method of which includes the following steps:
[0120] (1) 15-20D ultrafine denier ultra-high molecular weight polyethylene yarn was mixed with a finishing agent (Preparation Example 1) at a bath ratio of 1:40 for modification. The temperature was set at 180℃, the heating rate was 3℃ / min, the rotation speed was 1000r / min, and the temperature was kept stable for 30min before cooling down at a rate of 5℃ / min until it dropped to 60℃, thus obtaining modified ultrafine denier ultra-high molecular weight polyethylene yarn.
[0121] (2) The modified ultrafine denier ultra-high molecular weight polyethylene yarn described in step (1) is interwoven with 15-20D ultrafine denier N66 yarn, and after dyeing and setting, the high-strength wear-resistant lightweight fabric is obtained.
[0122] Performance tests were conducted on Examples 1-13 and Comparative Examples 1-2, and the test methods / standards are as follows:
[0123] Abrasion resistance test: Refer to GB / T 21196.2-2007 "Textiles - Martindale Method - Determination of Abrasion Resistance of Fabrics - Part 2: Determination of Specimen Breakage";
[0124] Strength test: Refer to GB / T 3917.2-2009 "Textiles - Tear properties of fabrics - Part 2: Determination of tear strength of trousers specimens (single seam)";
[0125] Weight test method: Weigh using an electronic balance.
[0126] The test results are shown in Table 2.
[0127] Table 2 Comparison of Performance Test Results of Examples
[0128] The test results show that:
[0129] (1) As can be seen from Examples 1 to 13, the present invention adopts a specific preparation method of first performing plasma modification treatment on ultra-fine denier ultra-high molecular weight polyethylene yarn and then mixing it with finishing agent to modify it. This method enables the fabric to have excellent abrasion resistance and tear resistance while ensuring a relatively light weight (30-35 GSM). Its abrasion resistance is 210,000-320,000 revolutions, warp strength is 24-32 N, and weft strength is 24-38 N.
[0130] (2) By comparing Example 1 with Examples 4 and 5, it can be seen that by further limiting the bath ratio of ultrafine denier ultra-high molecular weight polyethylene yarn after plasma treatment during the finishing agent modification process, the present invention can make the fabric with better abrasion resistance and tear resistance.
[0131] (3) By comparing Example 1 with Examples 6-9, it can be seen that the present invention further limits the gas pressure and power in the plasma modification process, thereby ensuring the effective action of plasma on the yarn surface and avoiding poor treatment effect or damage to the yarn structure due to excessively high or low parameters. In this way, the overall fabric weight is light, and the tear resistance and abrasion resistance are excellent.
[0132] (4) By comparing Example 1 with Examples 10-13, it can be seen that the mass ratio of polyurethane to adhesive in Example 12 is lower than 1.25:1, and the mass ratio of polyurethane to adhesive in Example 13 is higher than 2.5:1. The abrasion resistance and tear strength of the fabrics obtained by both examples are lower than those of Examples 10 and 11. This shows that by further limiting the mass ratio of polyurethane to adhesive in the finishing agent to (1.25-2.5):1, the present invention can significantly improve the tear strength and abrasion resistance of the obtained fabrics.
[0133] (5) As can be seen from the comparison between Example 1 and Comparative Example 1, the present invention, through a specific preparation method of first performing plasma modification treatment on ultra-fine denier ultra-high molecular weight polyethylene yarn and then mixing it with a finishing agent for modification, can make the fabric have excellent wear resistance and tear resistance while ensuring its lightweight.
[0134] (6) By comparing Example 1 and Comparative Example 2, it can be seen that in the fabric preparation method of the present invention, plasma modification treatment of ultra-fine denier ultra-high molecular weight polyethylene yarn can significantly improve its wear resistance and tear resistance while ensuring the lightweight of the obtained fabric. Without this step, the excellent effect cannot be obtained.
[0135] The above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A method for preparing a high-strength, wear-resistant, lightweight fabric, characterized in that, The preparation method includes the following steps: (1) Plasma modification treatment of ultrafine denier ultra-high molecular weight polyethylene yarn under the action of argon gas; (2) The plasma-modified ultrafine denier ultra-high molecular weight polyethylene yarn obtained in step (1) is mixed with a finishing agent for modification; (3) The mixed modified ultrafine denier ultra-high molecular weight polyethylene yarn obtained in step (2) is interwoven with ultrafine denier N66 yarn to obtain the high-strength wear-resistant lightweight fabric.
2. The method for preparing high-strength, wear-resistant, and lightweight fabric according to claim 1, characterized in that, In the mixed modification described in step (2), the ratio of the plasma-modified ultrafine denier ultra-high molecular weight polyethylene yarn obtained in step (1) to the finishing agent is 1:(35-45).
3. The method for preparing the high-strength, wear-resistant, lightweight fabric according to claim 1, characterized in that, The ultra-fine denier ultra-high molecular weight polyethylene yarn mentioned in step (1) is 15-20D ultra-fine denier ultra-high molecular weight polyethylene yarn; The ultrafine denier N66 yarn mentioned in step (3) is 15-20D ultrafine denier N66 yarn.
4. The method for preparing the high-strength, wear-resistant, lightweight fabric according to claim 3, characterized in that, In step (1), the pressure of the plasma modification treatment is 60-80 Pa; The power of the plasma modification treatment is 200-220W; The plasma modification treatment time is 2-15 minutes.
5. The method for preparing the high-strength, wear-resistant, lightweight fabric according to claim 1, characterized in that, The finishing agent in step (2) comprises the following components by mass percentage: Polyurethane 8-15%; Crosslinking agent 5-10%; Surfactant 6-12%; Dispersant 5-15%; Adhesive 5-10%; The remainder is water.
6. The method for preparing the high-strength, wear-resistant, lightweight fabric according to claim 5, characterized in that, The mass ratio of the polyurethane to the adhesive is (1.25-2.5):
1.
7. The method for preparing the high-strength, wear-resistant, lightweight fabric according to any one of claims 1-6, characterized in that, The preparation method specifically includes the following steps: (1) Plasma modification treatment is performed on 15-20D ultrafine denier ultra-high molecular weight polyethylene yarn. The pressure of the plasma modification treatment is 60-80Pa, the power is 200-220W, and the time is 2-15min. (2) The plasma-modified ultrafine denier ultra-high molecular weight polyethylene yarn obtained in step (1) and the finishing agent are mixed and modified at a bath ratio of 1:(35-45). (3) The mixed modified ultrafine denier ultra-high molecular weight polyethylene yarn obtained in step (2) is interwoven with 15-20D ultrafine denier N66 yarn, dyed and set to obtain the high-strength wear-resistant lightweight fabric.
8. A high-strength, wear-resistant, lightweight fabric, characterized in that, The high-strength, abrasion-resistant, and lightweight fabric is prepared by the method described in any one of claims 1-7.
9. The high-strength, wear-resistant, lightweight fabric according to claim 8, characterized in that, The abrasion resistance of the high-strength, abrasion-resistant, and lightweight fabric is 210,000-320,000 revolutions; the warp strength of the high-strength, abrasion-resistant, and lightweight fabric is 24-32N, the weft strength is 24-38N, and the weight is 30-35GSM.
10. The application of a high-strength, abrasion-resistant, lightweight fabric as described in claim 8 or 9 in outdoor sports equipment, military equipment, clothing, packaging materials, or household goods.