Down-proof textile fabric, and preparation method therefor and use thereof

By coating the base fabric with a specific ratio of anti-downing finishing agent and an interwoven structure of ultra-fine denier yarns, the balance between lightweight and anti-downing performance of textile fabrics is solved, resulting in high-strength, low-weight anti-downing textile fabrics suitable for high-performance applications in extreme environments.

WO2026232840A1PCT designated stage Publication Date: 2026-11-12BOSIDENG DOWN WEAR LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/146728
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2025-12-29
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing textile fabrics struggle to balance lightweight and down-proof properties, especially in extreme environments where they cannot meet the multiple demands for safety, durability, and comfort. Traditional fabrics also fall short in terms of down-proof performance and strength.

Method used

A down-proof finishing agent is prepared by compounding polyurethane resin, crosslinking agent, surfactant, dispersant and adhesive with water in a specific ratio. This agent is then coated onto the surface of the base fabric to form a coating. Combined with the interlaced structure of ultra-fine denier yarns, this results in a down-proof textile fabric with good flexibility and strength.

Benefits of technology

It achieves excellent down-proof performance and high tear strength while maintaining a low weight, making it suitable for high-performance fabric applications in extreme environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025146728_12112026_PF_FP_ABST
    Figure CN2025146728_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of textile materials, and provides a down-proof textile fabric, and a preparation method therefor and the use thereof. The down-proof textile fabric comprises a base fabric and a coating provided on the base fabric, wherein raw materials for preparing the coating comprise a down-proof finishing agent. The down-proof finishing agent comprises the following components in percentages by mass: 12-20% of a polyurethane resin, 3-8% of a cross-linking agent, 10-12% of a surfactant, 10-15% of a dispersant, 4-10% of a binder, and 35-65% of water. The weight-average molecular weight of the polyurethane resin is 50,000-70,000 g / mol. The down-proof textile fabric provided in the present invention has better mechanical properties, a lower gram weight, and a down-proof effect.
Need to check novelty before this filing date? Find Prior Art

Description

A down-proof textile fabric, its preparation method and application

[0001] This application claims priority to Chinese Patent Application No. 202510585391.6, filed on May 8, 2025, entitled "A Downproof Textile Fabric and Its Preparation Method and Application", the entire contents of which are incorporated herein by reference. Technical Field

[0002] This invention belongs to the field of textile materials technology, specifically relating to a down-proof textile fabric, its preparation method, and its application. Background Technology

[0003] With continuous technological advancements and increasing consumer demands for functionality, the textile industry faces significant challenges in material innovation. Especially in outdoor sports, military equipment, and high-end fashion, ultralight and high-strength textile fabrics have become crucial for improving product performance and user experience. Traditional textile fabrics often present a trade-off between weight and strength: lightweight fabrics typically lack sufficient strength, while high-strength fabrics are often bulky, impacting comfort and athletic performance. Currently, some lightweight, high-performance fabrics exist, but they still have shortcomings in strength, durability, and down-proof properties, particularly in extreme environments, failing to meet consumers' diverse needs for safety, durability, and comfort.

[0004] Down jackets are increasingly trending towards lightweight designs, and the use of lining fabrics to prevent down from seeping in is no longer sufficient to meet people's demand for lightweight and soft down jackets. When traditional textile fabrics are used in the manufacture of down jackets, down tends to leak out through the pores of the fabric, resulting in poor down-proof performance.

[0005] CN114575016A discloses a method for preparing a down-proof lightweight fabric. The preparation method includes the following steps: (1) Fabric weaving: both warp and weft yarns are made of ultra-fine denier polyester filament fibers with specifications of 33D / 120F to 50D / 216F, and are interwoven in a 1:1 plain weave structure with high density; (2) Pre-dyeing and finishing treatment: the fabric woven in step (1) is subjected to descaling, scalding and bleaching treatment, and loose processing is adopted; (3) Dyeing: the fabric treated in step (2) is dyed by a dyeing machine, and then dried and set; (4) Calendering treatment; (5) Air softening treatment; (6) Finished product inspection. Although the down-proof lightweight fabric prepared by this technical solution can achieve softness and good down-proof effect, the weight is 58-62 g / m². 2 It is still not light and thin enough.

[0006] CN101629346A discloses an ultralightweight casual sportswear fabric and its production method. The warp and weft yarns of the ultralightweight casual sportswear fabric are entirely composed of 10-20D synthetic fiber yarns, and the finished fabric has a weight of 20-80 g / m². 2 The down-proof performance is level 4 or higher. While the ultra-lightweight casual sportswear fabric provided by this technical solution achieves lower weight and better down-proof performance, its tear strength is relatively low.

[0007] Therefore, there is a need to develop a high-performance fabric that simultaneously possesses good mechanical properties, low weight, and down-proof performance. Summary of the Invention

[0008] To address the shortcomings of existing technologies, the present invention aims to provide a down-proof textile fabric, its preparation method, and its applications. The down-proof textile fabric simultaneously possesses good mechanical properties, low weight, and down-proof performance.

[0009] To achieve this objective, the present invention employs the following technical solution:

[0010] In a first aspect, the present invention provides a down-proof textile fabric, the down-proof textile fabric comprising a base fabric and a coating disposed on the base fabric; the coating is prepared by means of a down-proof finishing agent, the down-proof finishing agent comprising the following components by mass percentage: 12%–20% polyurethane resin (e.g., 13%, 14%, 15%, 16%, 17%, 18%, or 19%, etc.), 3%–8% crosslinking agent (e.g., 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, or 7.5%, etc.), 10%–12% surfactant (e.g., 10.2%, 10.4%, 10.6%, 10.8%, 11%, 11.2%, 11.4%, 11.6%, or 11.8%, etc.), and 10%–15% dispersant (e.g., 10.5%, 11%, 11%). The polyurethane resin comprises 0.5%, 12%, 12.5%, 13%, 13.5%, 14%, or 14.5%, etc.), 4% to 10% (e.g., 5%, 6%, 7%, 8%, or 9%) of adhesive and 35% to 65% (e.g., 38%, 41%, 44%, 47%, 50%, 53%, 56%, 59%, or 62%) of water; the weight-average molecular weight of the polyurethane resin is 50,000 to 70,000 g / mol (e.g., 52,000 g / mol, 54,000 g / mol, 56,000 g / mol, 58,000 g / mol, 60,000 g / mol, 62,000 g / mol, 64,000 g / mol, 66,000 g / mol, or 68,000 g / mol), more preferably 50,000 to 60,000 g / mol.

[0011] In this invention, the weight-average molecular weight of the polyurethane resin is 50,000–70,000 g / mol. If the weight-average molecular weight of the polyurethane resin is too low, the molecular chains of the polyurethane resin are shorter, and the intermolecular forces are weaker, which will lead to lower mechanical properties of the coating and the formed down-proof textile fabric. The coating is prone to cracking and wear when subjected to external forces, resulting in poor down-proof effect. If the weight-average molecular weight of the polyurethane resin is too high, the viscosity of the polyurethane resin and the down-proof finishing agent will increase, making the formed down-proof textile fabric brittle and reducing the tear strength of the down-proof textile fabric.

[0012] In this invention, the mass percentage of polyurethane resin in the anti-downing finishing agent is 12% to 20%. If the mass percentage of polyurethane resin is too low, the anti-downing finishing agent cannot achieve good encapsulation and bonding effects, making it difficult to form a complete and robust coating on the base fabric surface. This leads to a decrease in coating strength, a reduction in the tear strength of the anti-downing textile fabric, and a decrease in the anti-downing effect. If the mass percentage of polyurethane resin is too high, excessive polyurethane resin will reduce the flexibility of the coating and increase its hardness. Excessive hardness will make the coating prone to cracking under dynamic stress or bending, reducing its abrasion resistance. The preferred mass percentage of polyurethane resin in the anti-downing finishing agent is 15% to 20%, and when the weight-average molecular weight of the polyurethane resin is controlled to be 50,000 to 60,000 g / mol, a uniform, dense coating with good flexibility and strength can be formed on the surface of the base fabric. Within this mass percentage and weight-average molecular weight range, the interaction between polyurethane molecules reaches a good balance, ensuring that the coating has sufficient cohesive force and adhesion, as well as a certain degree of elasticity, which can effectively resist external wear and tear, improve the abrasion resistance and strength of the anti-downing textile fabric, and significantly enhance the anti-down leakage effect, resulting in better performance.

[0013] In this invention, by controlling the weight-average molecular weight and content of polyurethane resin in the anti-downing finishing agent within a specific range, it helps to improve the anti-downing effect while maintaining good mechanical properties.

[0014] Preferably, the base fabric has a weaving structure formed by alternating single and double yarns of ultra-fine denier yarn.

[0015] In this invention, the weaving structure formed by the alternating single and double yarns of the ultra-fine denier yarn is shown in Figure 1 (1 is a vertical single yarn group; 2 is a vertical double yarn group; 3 is a horizontal single yarn group; 4 is a horizontal double yarn group). The ultra-fine denier yarn includes vertical yarn groups and horizontal yarn groups. The vertical yarn groups include several vertical single yarn groups 1 and several vertical double yarn groups 2. The horizontal yarn groups include several horizontal single yarn groups 3 and several horizontal double yarn groups 4. The vertical single yarn groups 1 are arranged between two vertical double yarn groups 2, and the horizontal single yarn groups 3 are arranged between two horizontal double yarn groups 4. The horizontal single yarn groups 3 and horizontal double yarn groups 4 pass through the upper or lower sides of the multiple vertical single yarn groups 1 and vertical double yarn groups 2 respectively to achieve the weaving purpose.

[0016] In this invention, the ultra-fine denier yarn can be woven into a base fabric structure through alternating single and double yarns, giving the downproof textile fabric high tear strength. By using polyurethane resin, crosslinking agent, surfactant, dispersant, adhesive and water to prepare a downproof finishing agent, and coating it onto the base fabric to prepare a coating, the downproof effect can be improved while maintaining good mechanical properties and low weight.

[0017] Preferably, the polyurethane resin includes any one or a combination of at least two of polyester-type polyurethane, polycarbonate-type polyurethane, or polyether-type polyurethane.

[0018] Preferably, the crosslinking agent comprises any one or a combination of at least two of polysiloxane, blocked isocyanate, or epoxy silane.

[0019] Preferably, the dispersant comprises any one or a combination of at least two of fatty alcohol polyoxyethylene ethers, fatty acid polyoxyethylene esters, naphthalene sulfonic acid dispersants, or polycarboxylic acid dispersants.

[0020] Preferably, the adhesive comprises any one or a combination of at least two of polyurethane adhesives, polyvinyl acetate adhesives, polyacrylate adhesives, or butadiene adhesives.

[0021] Preferably, the specification of the ultrafine denier yarn is 15-20D, such as 16D, 17D, 18D or 19D.

[0022] Preferably, the material of the ultrafine denier yarn is nylon or polyethylene.

[0023] Preferably, the nylon is nylon 66.

[0024] Preferably, the polyethylene includes ultra-high molecular weight polyethylene.

[0025] Preferably, the number average molecular weight of the ultra-high molecular weight polyethylene is ≥1 million, such as 1.5 million, 2 million, 2.5 million, 3 million, 3.5 million or 4 million.

[0026] Preferably, the weight of the down-proof textile fabric is 30-40 g / m². 2 For example, 31g / m 2 32g / m 2 33g / m 2 34g / m 2 35g / m 2 36g / m 2 37g / m 2 38g / m 2 Or 39g / m 2 wait.

[0027] Preferably, the basis weight of the coating is 3–10 g / m³. 2 For example, 4g / m 2 5g / m 2 6g / m 2 7g / m 2 8g / m 2 or 9g / m 2 wait.

[0028] In this invention, the weight of the coating can be calculated by subtracting the weight of the base fabric from the weight of the downproof textile fabric.

[0029] In a second aspect, the present invention provides a method for preparing a downproof textile fabric as described in the first aspect, the method comprising the following steps: coating a downproof finishing agent onto the surface of a base fabric and pressing it to obtain the downproof textile fabric.

[0030] Preferably, the preparation method includes the following steps:

[0031] (1) The ultra-fine denier yarn is interwoven with single and double threads to prepare the greige fabric (also known as the raw fabric).

[0032] (2) The fabric obtained in step (1) is pretreated, dyed and shaped to prepare the base fabric.

[0033] (3) Apply the anti-downing finishing agent to the surface of the base fabric obtained in step (2) and press it to obtain the anti-downing textile fabric.

[0034] Preferably, the pretreatment in step (2) includes desizing, scouring, bleaching and mercerizing.

[0035] Generally, sizing is applied to the warp yarns to improve their weaveability, and some sizing is present on the ultra-fine denier yarns. In this invention, the sizing on the fabric can be removed by desizing, which weakens the adhesion between the fibers of the ultra-fine denier yarns, facilitating subsequent processing; scouring uses heat and chemical agents to remove natural impurities and oil stains from the fabric, improving its whiteness and absorbency; bleaching further removes pigments and impurities from the fabric to achieve the desired whiteness; mercerizing, using chemical treatment or mechanical stretching, gives the fabric surface a luster and improves its dimensional stability and wrinkle resistance. The desizing, scouring, bleaching, mercerizing, and dyeing processes can employ methods known to those skilled in the art or existing techniques, and their selection will not significantly affect the mechanical properties and down-proof effect of the resulting down-proof textile fabric, and no special limitations are imposed here.

[0036] Preferably, the shaping in step (2) includes shaping by hot pressing.

[0037] Preferably, the hot-pressing temperature is 190–210°C (e.g., 192°C, 194°C, 196°C, 198°C, 200°C, 202°C, 204°C, 206°C, or 208°C), the hot-pressing pressure is 20–30 kPa (e.g., 21 kPa, 22 kPa, 23 kPa, 24 kPa, 25 kPa, 26 kPa, 27 kPa, 28 kPa, or 29 kPa), and the hot-pressing time is 30–60 seconds (e.g., 33 seconds, 36 seconds, 39 seconds, 42 seconds, 45 seconds, 48 ​​seconds, 51 seconds, 54 seconds, or 57 seconds).

[0038] In this invention, the shape and size of the fabric are fixed by hot pressing, preventing deformation during use.

[0039] Preferably, step (3) further includes a drying step after pressing to form a dry down-proof textile fabric.

[0040] Thirdly, the present invention provides a down jacket, the down jacket comprising the down-proof textile fabric as described in the first aspect.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] The down-proof textile fabric of the present invention includes a base fabric and a coating disposed on the base fabric; the raw materials for preparing the coating include a down-proof finishing agent, which is prepared by compounding a specific polyurethane resin, a crosslinking agent, a surfactant, a dispersant, an adhesive and water, and coating it on the surface of the base fabric to prepare a coating, which can improve the down-proof effect while maintaining good mechanical properties and low weight. Attached Figure Description

[0043] Figure 1 is a schematic diagram of a weaving structure formed by alternating single and double yarns of ultrafine denier yarn in some embodiments;

[0044] Among them, 1-vertical single line group; 2-vertical double line group; 3-horizontal single line group; 4-horizontal double line group;

[0045] Figure 2 is a schematic diagram of the structure of the downproof textile fabric in some embodiments;

[0046] 5-coating; 6-base fabric. Detailed Implementation

[0047] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0048] The sources of some components in the following examples and comparative examples are as follows:

[0049] (1) Polyurethane resin:

[0050] Polyurethane resin A, polyester-type polyurethane, with a weight-average molecular weight of 50,000–60,000 g / mol, grade FS1530, manufactured by Anhui Feimiao New Materials Co., Ltd.

[0051] Polyurethane resin B, polyester-type polyurethane, with a weight-average molecular weight of 60,000–70,000 g / mol, grade FS-108C, manufactured by Anhui Feimiao New Materials Co., Ltd.

[0052] Polyurethane resin C, polyester-type polyurethane, with a weight-average molecular weight of 30,000–40,000 g / mol, grade FS1209, manufactured by Anhui Feimiao New Materials Co., Ltd.

[0053] Polyurethane resin D, polyester-type polyurethane, with a weight-average molecular weight of 73,000 g / mol, grade [not specified]. SF-2400 is manufactured by Guangzhou Haoyi New Material Technology Co., Ltd.

[0054] (2) Crosslinking agent:

[0055] Polysiloxane, model number 110-18-9, manufactured by Hubei Xinghengye Company.

[0056] (3) Surfactants:

[0057] Secondary alkyl sulfonate, brand name SAS60, manufactured by Jinan Daorong Chemical Co., Ltd.

[0058] (4) Dispersant:

[0059] Fatty alcohol polyoxyethylene ether, brand name 68439-49-6, is manufactured by Xingtai Lantian Company.

[0060] Fatty acid polyoxyethylene ester, brand name CAS No.4119-82-8, manufacturer is Wuhan Penglei Biotechnology Co., Ltd.

[0061] Naphthalene-based sulfonic acid dispersant, brand name DYWELL DN, manufacturer is Xingtianwai Chemical (Shanghai) Co., Ltd.

[0062] (5) Adhesive:

[0063] Polyurethane adhesives: Waterborne polyurethane resin emulsion, brand name PU7108, manufactured by Shanghai Belt New Material Technology Co., Ltd.

[0064] Example 1

[0065] This embodiment provides a downproof textile fabric and its preparation method. The downproof textile fabric, as shown in Figure 2, includes a base fabric 6 and a coating 5 disposed on the base fabric.

[0066] The preparation method includes the following steps:

[0067] (1) A grey fabric is prepared by interlacing ultra-fine denier yarn (nylon 66 yarn, specification 15D, manufacturer Yongrong Jinjiang, brand DTY) with single and double yarns as shown in Figure 1. The weight of the grey fabric is 30 g / m². 2 ;

[0068] (2) The fabric obtained in step (1) is desized, boiled, bleached, mercerized and dyed in sequence. Then it is hot-pressed for 50 seconds at a temperature of 200℃ and a pressure of 25kPa to fix it and prepare the base fabric.

[0069] The above desizing process includes: treating the fabric with a caustic soda solution (caustic soda concentration of 12 g / L) at 95°C for 30 min to remove the sizing agent, followed by thorough washing with water;

[0070] The above scouring process includes: using a scouring solution prepared with caustic soda solution and surfactant (alcohol ether carboxylate, brand name AEC 240, manufacturer: Guangzhou Xumei Textile Chemical Research Co., Ltd.), treating the grey fabric at 95°C for 60 minutes to remove fiber impurities, and then thoroughly washing with water. The scouring solution contains 0.6% caustic soda by mass and 0.3% surfactant by mass.

[0071] The above bleaching process includes: treating the fabric with an aqueous solution of hydrogen peroxide (hydrogen peroxide concentration of 5 g / L, pH of 10.5) at 92°C for 40 min to improve whiteness, followed by thorough washing with water;

[0072] The mercerizing process includes: treating the greige fabric with a caustic soda solution (caustic soda concentration of 25% by mass) at 25°C for 30 minutes to enhance luster and dimensional stability, followed by thorough washing with water;

[0073] The dyeing process includes: preparing a 5% (w / w) dye solution using disperse dye (brand name E-3RL, manufacturer: Jinan Xucheng Dyestuff Chemical Co., Ltd.) at a liquor ratio of 1:50, dyeing at 60℃ for 60 min, then adding sodium chloride (2% (w / w) to the dye solution, and accelerating the dyeing process at 60℃ for 30 min, then adding soda ash (1% (w / w)) to the dye solution, and fixing the color at 60℃ for 30 min, and finally using a soaping agent aqueous solution to treat at 100℃ for 5 min to remove floating color, wherein the soaping agent (brand name Argacel TCW) in the soaping agent solution has a mass concentration of 3 g / L.

[0074] (3) Apply the anti-fleecing finishing agent to the surface of the base fabric at a coating amount of 10 g / m. 2The fabric is pressed together using a calender to tightly bond it with the greige fabric. The pressing temperature is 200℃, the pressure is 25kPa, and the time is 50 seconds. The fabric is then dried at 100℃ for 20 minutes to obtain the downproof textile fabric.

[0075] The aforementioned anti-fleecing finishing agent comprises the following components by weight percentage: 15% polyurethane resin (polyurethane resin A), 5% crosslinking agent (polysiloxane), 11% surfactant (secondary alkyl sulfonate), 13% dispersant (fatty alcohol polyoxyethylene ether), 6% adhesive (polyurethane adhesive), and 50% water.

[0076] Example 2

[0077] This embodiment provides a down-proof textile fabric and its preparation method. The only difference between this embodiment and Embodiment 1 is that the down-proof finishing agent includes the following components by mass percentage: 16% polyurethane resin (polyurethane resin A), 4% crosslinking agent (polysiloxane), 12% surfactant (secondary alkyl sulfonate), 11% dispersant (fatty acid polyoxyethylene ester), 10% adhesive (polyurethane adhesive), and 47% water. Other conditions are the same as in Embodiment 1.

[0078] Example 3

[0079] This embodiment provides a down-proof textile fabric and its preparation method. The only difference between this embodiment and Embodiment 1 is that the down-proof finishing agent includes the following components by mass percentage: 14% polyurethane resin (polyurethane resin A), 8% crosslinking agent (polysiloxane), 10% surfactant (secondary alkyl sulfonate), 15% dispersant (naphthalene sulfonic acid dispersant), 4% adhesive (polyurethane adhesive), and 49% water. Other conditions are the same as in Embodiment 1.

[0080] Example 4

[0081] This embodiment provides a downproof textile fabric and its preparation method. The only difference between this embodiment and Embodiment 1 is that the ultrafine denier yarn in step (1) is polyethylene yarn with a specification of 15D, manufactured by Dongguan Lanxin New Material Weaving Technology Co., Ltd., and grade LX254. Other conditions are the same as in Embodiment 1.

[0082] Example 5

[0083] This embodiment provides a downproof textile fabric and its preparation method. The only difference between this embodiment and Embodiment 1 is that the mass percentage of polyurethane resin (polyurethane resin A) in the downproof finishing agent is adjusted to 12%, and the mass percentage of water is adjusted to 53%. Other conditions are the same as in Embodiment 1.

[0084] Example 6

[0085] This embodiment provides a downproof textile fabric and its preparation method. The only difference between this embodiment and Embodiment 1 is that the mass percentage of polyurethane resin (polyurethane resin A) in the downproof finishing agent is adjusted to 20%, and the mass percentage of water is adjusted to 45%. Other conditions are the same as in Embodiment 1.

[0086] Example 7

[0087] This embodiment provides a downproof textile fabric and its preparation method. The only difference between this embodiment and Embodiment 1 is that the polyurethane resin (polyurethane resin A) in the downproof finishing agent is replaced with the same mass of polyurethane resin (polyurethane resin B). All other conditions are the same as in Embodiment 1.

[0088] Comparative Example 1

[0089] This comparative example provides a down-proof textile fabric and its preparation method. The only difference between this example and Example 1 is that the polyurethane resin (polyurethane resin A) in the down-proof finishing agent is replaced with the same mass of polyurethane resin (polyurethane resin C), while the other conditions are the same as in Example 1.

[0090] Comparative Example 2

[0091] This comparative example provides a down-proof textile fabric and its preparation method. The only difference between this example and Example 1 is that the polyurethane resin (polyurethane resin A) in the down-proof finishing agent is replaced with the same mass of polyurethane resin (polyurethane resin D). All other conditions are the same as in Example 1.

[0092] Comparative Example 3

[0093] This comparative example provides a downproof textile fabric and its preparation method. The only difference between this example and Example 1 is that the mass percentage of polyurethane resin (polyurethane resin A) in the downproof finishing agent is adjusted to 10%, and the mass percentage of water is adjusted to 55%. Other conditions are the same as in Example 1.

[0094] Comparative Example 4

[0095] This comparative example provides a textile fabric and its preparation method. The only difference between this example and Example 1 is that the textile fabric is a base fabric, and the preparation method does not include step (3). Other conditions are the same as in Example 1.

[0096] The following tests were conducted on the downproof textile fabrics provided in Examples 1 to 7, Comparative Examples 1 to 3, and Comparative Example 4:

[0097] (1) Tear strength: The tear strength was determined in accordance with GB / T 3917.2-2009 "Textiles - Tear properties of fabrics - Part 2: Determination of tear strength of trousers (single seam)".

[0098] (2) Downproof performance: The test was conducted in accordance with GB / T 12705.1-2009 "Textiles - Test methods for downproofness of fabrics - Part 1: Friction method".

[0099] (3) Weight: The weight was measured using a GS-323 electronic balance.

[0100] The test results are shown in Table 1 below:

[0101] Table 1 Comparison of Textile Fabric Performance Test Results

[0102] As shown in Table 1, the down-proof textile fabrics provided in Examples 1 to 7 have a down-proof number of ≤4 threads, a warp tear strength ≥21N, and a weft tear strength ≥20N, exhibiting excellent down-proof performance while maintaining good mechanical properties and low weight.

[0103] Compared to Example 1, if the weight-average molecular weight of the polyurethane resin is too low (Comparative Example 1), the resulting down-proof textile fabric is prone to cracking and wear under external force, resulting in a decrease in down-proof performance. If the weight-average molecular weight of the polyurethane resin is too high (Comparative Example 2), the resulting down-proof textile fabric becomes brittle, leading to a significant decrease in its tear strength. Therefore, it can be concluded that a polyurethane resin with a weight-average molecular weight of 50,000–70,000 g / mol produces a more effective down-proof textile fabric.

[0104] Compared to Example 1, if the mass percentage of polyurethane resin is too low (Comparative Example 3), the anti-downing agent cannot achieve good encapsulation and bonding effects, making it difficult to form a complete and robust coating on the base fabric surface. This results in a decrease in coating strength, a reduction in the tear strength of the anti-downing textile fabric, and a decrease in the anti-downing effect. Compared to Example 1, if the coating is not prepared using an anti-downing agent (Comparative Example 4), the resulting textile fabric has poor anti-downing performance.

[0105] The present invention has been illustrated through the above embodiments, but the present invention is not limited to the above process steps, that is, it does not mean that the present invention must rely on the above process steps to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials used in the present invention, additions of auxiliary components, and selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A down-proof textile fabric, characterized in that, The down-proof textile fabric includes a base fabric and a coating disposed on the base fabric; The coating is prepared using an anti-flocking finishing agent, which comprises the following components by mass percentage: 12%–20% polyurethane resin, 3%–8% crosslinking agent, 10%–12% surfactant, 10%–15% dispersant, 4%–10% binder, and 35%–65% water; the polyurethane resin has a weight-average molecular weight of 50,000–70,000 g / mol.

2. The downproof textile fabric according to claim 1, characterized in that, The base fabric has a weaving structure formed by alternating single and double yarns of ultra-fine denier yarns; The polyurethane resin includes any one or a combination of at least two of polyester polyurethane, polycarbonate polyurethane, or polyether polyurethane. The crosslinking agent includes any one or a combination of at least two of polysiloxane, blocked isocyanate, or epoxy silane.

3. The downproof textile fabric according to claim 1, characterized in that, The dispersant includes any one or a combination of at least two of the following: fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester, naphthalene sulfonic acid dispersant, or polycarboxylic acid dispersant.

4. The downproof textile fabric according to claim 1, characterized in that, The adhesive includes any one or a combination of at least two of the following: polyurethane adhesives, polyvinyl acetate adhesives, polyacrylate adhesives, or butadiene adhesives.

5. The downproof textile fabric according to claim 2, characterized in that, The specifications of the ultrafine denier yarn are 15-20D; The ultra-fine denier yarn is made of nylon or polyethylene. The nylon is nylon 66; The polyethylene includes ultra-high molecular weight polyethylene; The weight of the downproof textile fabric is 30-40 g / m². 2 ; The basis weight of the coating is 3-10 g / m³. 2 .

6. A method for preparing a down-proof textile fabric as described in any one of claims 1 to 5, characterized in that, The preparation method includes the following steps: coating the anti-downy finishing agent onto the surface of the base fabric and pressing it to obtain the anti-downy textile fabric.

7. The preparation method according to claim 6, characterized in that, The preparation method includes the following steps: (1) A grey fabric is prepared by interlacing ultrafine denier yarn with single and double threads at intervals; (2) The greige fabric obtained in step (1) is pretreated, dyed and shaped to prepare the base fabric; (3) Apply the anti-downing finishing agent to the surface of the base fabric obtained in step (2) and press it to obtain the anti-downing textile fabric.

8. The preparation method according to claim 7, characterized in that, The pretreatment in step (2) includes desizing, boiling, bleaching and mercerizing.

9. The preparation method according to claim 7, characterized in that, The shaping process in step (2) includes shaping by hot pressing; The hot pressing temperature is 190–210°C, the hot pressing pressure is 20–30 kPa, and the hot pressing time is 30–60 seconds; Step (3) further includes a drying step after pressing.

10. A down jacket, characterized in that, The down jacket includes the down-proof textile fabric as described in any one of claims 1 to 5.