Preparation method for cellulose-based photochromic and stretching-induced mechanochromic film

By preparing cellulose-based photochromic and stretch-chromic films, a synergistic response of photochromism and stretch-chromism is achieved using dynamic chemical bonds and multiple hydrogen bonds. This solves the problem that existing materials cannot achieve a synergistic response to dual stimuli, and enables the effect of distinguishing stimuli by color differences, thus expanding its application in the fields of sensors and intelligent anti-counterfeiting.

WO2026232893A1PCT designated stage Publication Date: 2026-11-12CHINA NAT PULP & PAPER RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/076768
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2026-02-03
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing stimulus-response materials are unable to achieve synergistic responses to dual stimuli, cannot flexibly switch states, and have difficulty distinguishing stimulus sources, which limits their application in fields such as intelligent anti-counterfeiting, biomedicine, and sensors.

Method used

A method for preparing cellulose-based photochromic and stretch-chromic films was adopted. Through the dynamic chemical bonds and multiple hydrogen bonds between block copolymers, cellulose-based derivatives and isocyanate groups, a synergistic response of photochromism and stretch-chromism was achieved, and the stimulation source was distinguished by color difference.

Benefits of technology

Cellulose-based photochromic and stretch-chromic films possess excellent stretchability and reversible shape memory behavior, enabling them to display different colors under different lighting conditions. This achieves a cascaded dual stimulus response, breaking through the bottleneck of single stimulus response and promoting their application in sensors, flexible electronics, and intelligent anti-counterfeiting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2026076768_12112026_PF_FP_ABST
    Figure CN2026076768_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of cellulose-based films, and provides a preparation method for a cellulose-based photochromic and stretching-induced mechanochromic film. During the preparation of the cellulose-based photochromic and stretching-induced mechanochromic film provided by the present application, a cellulose-based derivative, 4-hydroxyazobenzene, a block copolymer, isophorone diisocyanate and 1,4-butanediol are comprised. The film of the present application exhibits synergistic photochromic and stretching-induced mechanochromic responses, and can achieve tandem photochromism and stretching-induced mechanochromism under visible light and ultraviolet light. Under visible light, the cellulose-based photochromic and stretching-induced mechanochromic film in a stretched state changes from yellow to white; and under ultraviolet light, the cellulose-based photochromic and stretching-induced mechanochromic film changes from dark blue to white during stretching. Moreover, the photochromic and stretching-induced mechanochromic responses have the characteristics of fast response, high stability, good reversibility, etc., and therefore the film can be applied to the fields of packaging anti-counterfeiting, stress sensing, damage warning, etc.
Need to check novelty before this filing date? Find Prior Art

Description

A method for preparing cellulose-based photochromic and stretch-induced color-changing films Technical Field

[0001] This application belongs to the field of cellulose-based thin film technology, and relates to a method for preparing cellulose-based photochromic and stretch-chromic thin films. Background Technology

[0002] In nature, plants and animals respond to various external stimuli. When faced with environmental stimuli, an organism's stimulus-responsiveness can alter its appearance or behavior. Complex and ingenious mechanisms of perception, mimicry, and camouflage defense strategies enable plants and animals to avoid detection by predators. Specifically, the wings of the dead leaf butterfly perfectly mimic dead leaves, camouflaging itself to avoid predator attacks; the body color of the scorpionfish varies greatly depending on the environment, like a chameleon, using camouflage to deceive enemies; and the mimosa plant folds its leaves when touched, subjected to environmental vibrations, or physical stimuli. Inspired by the stimulus-responsive behaviors of plants and animals in nature, scientists are actively engaged in the research and development of novel stimulus-responsive materials. Drawing inspiration from the perception and camouflage behaviors of plants and animals, and cleverly transforming them into material design concepts, has powerfully promoted the vigorous development of stimulus-responsive materials in fields such as intelligent anti-counterfeiting, biomedicine, and sensors. However, most stimulus-responsive materials can only achieve a single stimulus response. When faced with complex environments or receiving multiple instructions, these materials cannot flexibly switch states or accurately distinguish stimulus sources, which greatly restricts the application expansion of stimulus-responsive materials in real-world scenarios and fails to fully meet the rich and varied application needs of various fields. Therefore, developing cellulose-based color-changing materials capable of synergistic responses to multiple stimuli still faces significant challenges.

[0003] Stimulus-responsive color-changing materials are a class of smart materials capable of sensing changes in the external environment (such as temperature, pH, light, electric fields, magnetic fields, pressure, etc.) and causing reversible or irreversible color changes through alterations in their own structure or chemical composition. Among many external stimuli, light, as a clean energy source, is highly favored by researchers due to its controllability and adjustability. However, integrating dual stimulus-responsive properties into a single material often requires extremely complex structural designs. Currently, achieving dual-response functionality and clearly distinguishing different stimulus types through color changes remains a critical challenge in the preparation of stimulus-responsive materials. Summary of the Invention

[0004] The technical problem to be solved by this application is to provide a method for preparing a cellulose-based photochromic and stretch-chromic film, which not only responds synergistically to external stimuli but also easily distinguishes the stimulus source based on the visual color difference. Moreover, the cellulose-based photochromic and stretch-chromic film has excellent stretchability (elongation at break of 800%) and reversible shape memory behavior.

[0005] To solve the above-mentioned technical problems, this application provides the following technical solution:

[0006] This application provides a cellulose-based photochromic and stretch-chromic film, which mainly comprises 10-40 parts by weight of cellulose-based derivative (CD), 1-10 parts by weight of 4-hydroxyazobenzene (AZO), 10-40 parts by weight of block copolymer (BC), 30-40 parts by weight of isophorone diisocyanate (IPDI), 1-5 parts by weight of catalyst (CA), and 1-10 parts by weight of 1,4-butanediol (BDO).

[0007] The aforementioned cellulose-based derivatives are any one of hydroxyethyl cellulose, hydroxypropyl cellulose, and ethyl cellulose.

[0008] The block copolymers mentioned above are any one of poloxamer 124, poloxamer 188, and poloxamer 407.

[0009] The catalyst mentioned above is any one of dimethyl stannate, dibutyltin dilaurate, and stannous octoate.

[0010] This application provides a method for preparing a cellulose-based photochromic and stretch-chromic thin film as described above, comprising the following steps:

[0011] a1. The block copolymer is mixed with isophorone diisocyanate and stirred at low temperature to dissolve, thus obtaining mixed solution A;

[0012] a2. Add a catalyst and 4-hydroxyazobenzene to the mixed solution A, mix them evenly, raise the temperature to carry out the reaction, and obtain the prepolymer solution B;

[0013] a3. Add the cellulose-based derivative to the prepolymer solution B, and slowly add isophorone diisocyanate and 1,4-butanediol dropwise at a certain water bath temperature. After stirring evenly for a certain period of time, a PE solution is obtained.

[0014] a4. Add anhydrous ethanol to the PE solution to obtain a mixed solution PE-EA. Pour the mixed solution PE-EA into a silicone mold and dry it in a vacuum drying oven at 60°C for 24 hours to obtain a cellulose-based photochromic and stretch-chromic film.

[0015] The temperature mentioned in step a2 above is 60-90℃, and the reaction time is 1-3h.

[0016] The water bath temperature mentioned in step a3 above is 60-90℃, and the stirring time is 2-4 hours.

[0017] The main benefits of this application are as follows:

[0018] 1. The block copolymers, cellulose derivatives and isocyanate groups in cellulose-based photochromic and stretch-chromic films possess excellent stretchability and stretch-chromic properties. By synergistically combining photochromism and stretch-chromism, a series of dual color-changing responses is achieved, exhibiting different colors under different lighting conditions, and the stimulus source can be easily distinguished based on the color.

[0019] 2. This application utilizes the dynamic urethane bond formed by the hydroxyl groups of cellulose-based derivatives and isocyanate groups to endow cellulose-based photochromic and stretch-sensitive films with excellent stretchability, thus overcoming the rigidity limitation of cellulose;

[0020] 3. This application achieves a synergistic response of photochromism and stretch-induced color change, which not only enables a series response to dual stimuli, but also ensures that the responses to the dual stimuli do not interfere with each other. This breaks through the bottlenecks of single-stimuli-responsive materials in terms of synergy, stability and functional complexity, and promotes the application of this cellulose-based film in sensors, flexible electronics, smart anti-counterfeiting and other fields.

[0021] 4. The reaction conditions of this application are mild and the synthesis process is simple. The cellulose-based photochromic and stretch-chromic films prepared have high stretchability, good recyclability and reusability, showing great application potential and providing a new solution for the development of green and sustainable materials.

[0022] 5. This application provides a method for preparing cellulose-based photochromic and stretch-chromic films. The cellulose-based films prepared by this method can achieve a synergistic response of photochromism and stretch-chromism, exhibiting significant color differences when stretched under visible and ultraviolet light. Moreover, the cellulose-based films possess excellent high tensile strength, with an elongation at break reaching 800%, indicating that these cellulose-based films have broad application prospects. Attached Figure Description

[0023] Figure 1 is a schematic diagram of the preparation process of a cellulose-based photochromic and stretch-induced color-changing film;

[0024] Figure 2 shows the synergistic response behavior of photoinduced and stretch-induced discoloration of cellulose-based films under ultraviolet and visible light. Detailed Implementation

[0025] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.

[0026] Example 1:

[0027] A cellulose-based photochromic and stretch-chromic film is made from the following components and their mass parts: 20 parts hydroxyethyl cellulose, 5 parts 4-hydroxyazobenzene, 20 parts poloxamer, 40 parts isophorone diisocyanate, 5 parts catalyst, and 10 parts 1,4-butanediol, wherein the catalyst is dibutyltin dilaurate.

[0028] The method for preparing cellulose-based photochromic and stretch-induced color-changing films in this embodiment includes the following steps:

[0029] (1) Mix 20 parts of poloxamer and 20 parts of isophorone diisocyanate and mix them evenly at low temperature to obtain mixed solution A;

[0030] (2) Take 5 parts of dibutyltin dilaurate and 5 parts of 4-hydroxyazobenzene and add them to mixed solution A. After mixing evenly, heat to 80℃. After the temperature stabilizes, set the reaction time to 2h to obtain prepolymer solution B.

[0031] (3) Take 20 parts of hydroxyethyl cellulose and add it to the prepolymer solution B. Slowly add 20 parts of isophorone diisocyanate at a water bath temperature of 80°C, add 10 parts of 1,4-butanediol, mix evenly, and stir for 2 hours to obtain PE solution.

[0032] (4) Pour an appropriate amount of anhydrous ethanol into the PE solution to form a mixed PE-EA solution to remove bubbles in the PE-EA solution. Pour the defoamed PE-EA solution into a silicone mold and dry it in a vacuum drying oven at 60°C for 12 hours to obtain a cellulose-based photochromic and stretch-chromic film.

[0033] The tensile properties of cellulose-based photochromic and stretch-chromic films were tested according to GB / T 1040.3-2006. The tests revealed that the tensile strength of the cellulose-based photochromic and stretch-chromic films was higher than 10 MPa, and the elongation at break was higher than 500%.

[0034] Example 2:

[0035] A cellulose-based photochromic and stretch-chromic film is made from the following components and their mass parts: 20 parts hydroxypropyl cellulose, 10 parts 4-hydroxyazobenzene, 30 parts poloxamer, 30 parts isophorone diisocyanate, 5 parts catalyst, and 5 parts 1,4-butanediol, wherein the catalyst is stannous octoate.

[0036] The method for preparing cellulose-based photochromic and stretch-induced color-changing films in this embodiment includes the following steps:

[0037] (1) Mix 30 parts of poloxamer with 15 parts of isophorone diisocyanate and mix them evenly at low temperature to obtain mixed solution A;

[0038] (2) Take 5 parts of stannous octoate and 5 parts of 4-hydroxyazobenzene and add them to mixed solution A. After mixing evenly, heat to 80°C. After the temperature stabilizes, set the reaction time to 2 hours to obtain prepolymer solution B.

[0039] (3) Take 20 parts of hydroxypropyl cellulose and add it to the prepolymer solution B. Slowly add 15 parts of isophorone diisocyanate at a water bath temperature of 80°C, add 5 parts of 1,4-butanediol, mix evenly, and stir for 2 hours to obtain PE solution.

[0040] (4) Pour an appropriate amount of anhydrous ethanol into the PE solution to form a mixed PE-EA solution to remove bubbles in the PE-EA solution. Pour the defoamed PE-EA solution into a silicone mold and dry it in a vacuum drying oven at 60°C for 12 hours to obtain a cellulose-based photochromic and stretch-chromic film.

[0041] After testing, it was found that the cellulose-based photochromic and stretch-chromic films prepared in this embodiment have good response performance. The stretch-chromic response produces a response behavior from yellow to white when the elongation is 300%, and the photochromic behavior can achieve color switching under visible light and ultraviolet light in only 5 seconds.

[0042] Example 3

[0043] A cellulose-based photochromic and stretch-chromic film is made from the following components and their mass parts: 30 parts ethyl cellulose, 10 parts 4-hydroxyazobenzene, 20 parts poloxamer, 30 parts isophorone diisocyanate, 5 parts catalyst, and 5 parts 1,4-butanediol, wherein the catalyst is dimethyl stannate.

[0044] The method for preparing cellulose-based photochromic and stretch-induced color-changing films in this embodiment includes the following steps:

[0045] (1) Mix 20 parts of poloxamer with 15 parts of isophorone diisocyanate and mix them evenly at low temperature to obtain mixed solution A;

[0046] (2) Take 5 parts of dimethyl stannate and 10 parts of 4-hydroxyazobenzene and add them to mixed solution A. After mixing evenly, heat to 80°C. After the temperature stabilizes, set the reaction time to 2 hours to obtain prepolymer solution B.

[0047] (3) Take 30 parts of ethyl cellulose and add it to the prepolymer solution B. Slowly add 15 parts of isophorone diisocyanate at a water bath temperature of 80℃, add 5 parts of 1,4-butanediol, mix evenly, and stir for 2 hours to obtain PE solution.

[0048] (4) Pour an appropriate amount of anhydrous ethanol into the PE solution to form a mixed PE-EA solution to remove bubbles in the PE-EA solution. Pour the defoamed PE-EA solution into a silicone mold and dry it in a vacuum drying oven at 60°C for 12 hours to obtain a cellulose-based photochromic and stretch-chromic film.

[0049] The tensile properties of cellulose-based photochromic and stretch-chromic films were tested according to GB / T 1040.3-2006. The tests revealed that the tensile strength of the cellulose-based photochromic and stretch-chromic films was higher than 10 MPa, and the elongation at break was higher than 800%. Furthermore, the cellulose-based photochromic and stretch-chromic films exhibited rapid response, reversibility, and recyclability.

[0050] Example 4:

[0051] A cellulose-based photochromic and stretch-chromic film is made from the following components and their mass parts: 20 parts hydroxypropyl cellulose, 10 parts 4-hydroxyazobenzene, 30 parts poloxamer, 30 parts isophorone diisocyanate, 5 parts catalyst, and 5 parts 1,4-butanediol, wherein the catalyst is stannous octoate.

[0052] The method for preparing cellulose-based photochromic and stretch-induced color-changing films in this embodiment includes the following steps:

[0053] (1) Mix 30 parts of poloxamer with 15 parts of isophorone diisocyanate and mix them evenly at low temperature to obtain mixed solution A;

[0054] (2) Take 5 parts of stannous octoate and 10 parts of 4-hydroxyazobenzene and add them to mixed solution A. After mixing evenly, heat to 80°C. After the temperature stabilizes, set the reaction time to 2 hours to obtain prepolymer solution B.

[0055] (3) Take 20 parts of hydroxypropyl cellulose and add it to the prepolymer solution B. Slowly add 15 parts of isophorone diisocyanate at a water bath temperature of 80°C, add 5 parts of 1,4-butanediol, mix evenly, and stir for 2 hours to obtain PE solution.

[0056] (4) Pour an appropriate amount of anhydrous ethanol into the PE solution to form a mixed PE-EA solution to remove bubbles in the PE-EA solution. Pour the defoamed PE-EA solution into a silicone mold and dry it in a vacuum drying oven at 60°C for 12 hours to obtain a cellulose-based photochromic and stretch-chromic film.

[0057] This application provides a cellulose-based photochromic and stretch-chromic film that simultaneously achieves a synergistic response of photochromism and stretch-chromism, with the two stimuli not interfering with each other but acting in a synergistic series. Dynamic chemical bonds and multiple hydrogen bonds between cellulose-based derivatives, block copolymers, and isocyanate groups enhance the stretchability and tensile strength of the cellulose-based photochromic and stretch-chromic film. Furthermore, under visible light, the cellulose-based film exhibits a visible transition from yellow to white upon stretching; under ultraviolet light, it exhibits a color switch from dark purple to white upon stretching, achieving synergistic color change.

[0058] The preferred embodiments disclosed above are merely illustrative of this application. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. These embodiments have been selected and specifically described in this specification to better explain the principles and practical applications of this application, thereby enabling those skilled in the art to better understand and utilize this application. This application is limited only by the claims and their full scope and equivalents.

Claims

1. A cellulose-based photochromic and stretch-chromic film, characterized in that, It mainly includes 10-40 parts by weight of cellulose-based derivatives, 1-10 parts by weight of 4-hydroxyazobenzene, 10-40 parts by weight of block copolymers, 30-40 parts by weight of isophorone diisocyanate, 1-5 parts by weight of catalyst, and 1-10 parts by weight of 1,4-butanediol.

2. The cellulose-based photochromic and stretch-induced color-changing film according to claim 1, characterized in that, The cellulose-based derivative is any one of hydroxyethyl cellulose, hydroxypropyl cellulose, and ethyl cellulose.

3. The cellulose-based photochromic and stretch-induced color-changing film according to claim 1, characterized in that, The block copolymer is any one of poloxamer 124, poloxamer 188, and poloxamer 407.

4. The cellulose-based photochromic and stretch-chromic film according to claim 1, characterized in that, The catalyst is any one of dimethyl stannate, dibutyltin dilaurate, and stannous octoate.

5. The cellulose-based photochromic and stretch-induced color-changing film according to claim 1, characterized in that, It is made from the following components in parts by weight: 20 parts hydroxyethyl cellulose, 5 parts 4-hydroxyazobenzene, 20 parts poloxamer, 40 parts isophorone diisocyanate, 5 parts catalyst and 10 parts 1,4-butanediol.

6. The cellulose-based photochromic and stretch-chromic film according to claim 1, characterized in that, It is made from the following components in parts by weight: 30 parts ethyl cellulose, 10 parts 4-hydroxyazobenzene, 20 parts poloxamer, 30 parts isophorone diisocyanate, 5 parts catalyst and 5 parts 1,4-butanediol.

7. The method for preparing the cellulose-based photochromic and stretch-chromic thin film according to claim 1, comprising the following steps: a1. The block copolymer is mixed with isophorone diisocyanate and stirred at low temperature to dissolve, thus obtaining mixed solution A; a2. Add a catalyst and 4-hydroxyazobenzene to the mixed solution A, mix them evenly, raise the temperature to carry out the reaction, and obtain the prepolymer solution B; a3. Add the cellulose-based derivative to the prepolymer solution B, and slowly add isophorone diisocyanate and 1,4-butanediol dropwise at a certain water bath temperature. After stirring evenly for a certain period of time, a PE solution is obtained. a4. Add anhydrous ethanol to the PE solution to obtain a mixed solution PE-EA. Pour the mixed solution PE-EA into a silicone mold and dry it in a vacuum drying oven at 60°C for 24 hours to obtain the cellulose-based photochromic and stretch-chromic film.

8. The preparation method according to claim 7, characterized in that, The temperature mentioned in step a2 is 60-90°C, and the reaction time is 1-3 hours.

9. The preparation method according to claim 7, characterized in that, The water bath temperature in step a3 is 60-90°C, and the stirring time is 2-4 hours.

10. The preparation method according to claim 7, characterized in that, The mass fractions of isophorone diisocyanate mentioned in steps a1 and a3 are 20 parts each.

11. The preparation method according to claim 7, characterized in that, The mass fractions of isophorone diisocyanate mentioned in steps a1 and a3 are 15 parts each.