Metal lithium surface treatment agent and use thereof

By treating the surface of metallic lithium with a solution of tetramethylurea and a specific lithium salt, the problem of easy oxidation of metallic lithium in humid air was solved, enabling stable production of lithium batteries and solid-state batteries, and reducing production costs and difficulties.

WO2026233389A1PCT designated stage Publication Date: 2026-11-12ZHANGJIAGANG GUOTAI HUARONG NEW CHEM MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/095335
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-05-08
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Lithium metal is highly susceptible to oxidation in humid air, which means that the production of lithium batteries or solid-state batteries must be carried out in a dry room with an extremely low dew point or in an argon atmosphere, increasing the difficulty and cost of production.

Method used

The surface of metallic lithium is treated with tetramethylurea (TMU) or a TMU solution containing lithium salts, such as LiBOB, LiDFOB, LiDFP, Li-SS, or Li-AK, to improve its stability in humid air.

Benefits of technology

It significantly reduces the oxidation rate of lithium metal electrodes in humid air, maintains the charge and discharge performance of lithium batteries, and reduces production difficulty and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2026095335_12112026_PF_FP_ABST
    Figure CN2026095335_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure relates to a metal lithium surface treatment agent and the use thereof. To address the issue that due to a metal lithium electrode sheet being very prone to oxidation in a normal air environment, a lithium battery or a solid-state battery using a metal lithium negative electrode must be produced under stringent dry and low-oxygen conditions, the present disclosure provides a metal lithium surface treatment agent, which is tetramethylurea (TMU) or a tetramethylurea solution containing a special lithium salt (LiBOB, LiDFOB, LiDFP, Li-SS and Li-AK). Soaking the surface of a metal lithium electrode in the metal lithium surface treatment agent of the present disclosure and then drying same can improve the stability of the metal lithium electrode in humid air and remarkably reduce the oxidation reaction rate, and barely affect the charge-discharge performance of a lithium battery using the treated metal lithium negative electrode. The present disclosure can be used in a production process for a lithium battery or a solid-state battery using a metal lithium negative electrode and is expected to reduce the production difficulty and production cost.
Need to check novelty before this filing date? Find Prior Art

Description

A lithium metal surface treatment agent and its application Technical Field

[0001] This disclosure relates to the field of lithium battery technology, specifically to a metallic lithium surface treatment agent and its application. Background Technology

[0002] Lithium-ion batteries are currently the primary electrochemical energy storage method in applications such as large-scale energy storage, electric vehicles, and consumer electronics. Currently, lithium-ion batteries mainly use graphite materials or graphite-doped silicon anodes. The humidity requirements for the production environment of lithium-ion battery anode sheets are currently far less stringent than those for cathode sheets. However, to achieve higher energy density, researchers have been experimenting with using lithium metal as the anode for lithium-ion or solid-state batteries. Due to the high reactivity of lithium metal, especially under humid conditions, it reacts immediately, turning black and rendering it unusable. Therefore, research on lithium metal batteries or solid-state batteries is generally limited to extremely low dew-point dry rooms or argon-atmosphere glove boxes. This presents significant challenges and high costs for the future development of solid-state battery processes using lithium metal as the anode. Summary of the Invention

[0003] The purpose of this disclosure is to provide a lithium metal surface treatment agent that can improve the stability of lithium metal anodes in humid air without affecting the charge and discharge performance of lithium batteries using the treated lithium metal anodes.

[0004] Another object of this disclosure is to provide a lithium metal electrode treated with the above-mentioned lithium metal surface treatment agent and a lithium battery using the treated lithium metal electrode.

[0005] To achieve the above objectives, the technical solution adopted in this disclosure is as follows:

[0006] The first aspect of this disclosure provides a lithium metal surface treatment agent, which is tetramethylurea (TMU) or a tetramethylurea solution containing a lithium salt, wherein the lithium salt includes one or more of lithium dioxolane borate (LiBOB), lithium difluorooxolane borate (LiDFOB), lithium difluorophosphate (LiDFP), lithium o-benzoylsulfonylimide (Li-SS), and lithium acesulfame potassium (Li-AK).

[0007] In some embodiments of this disclosure, the concentration of the tetramethylurea solution containing lithium salt is 0.1 wt% to 10 wt%.

[0008] In some more specific embodiments, the lithium metal surface treatment agent is composed of tetramethylurea and a lithium salt, wherein the lithium salt accounts for 0.1% to 10% of the mass of the lithium metal surface treatment agent.

[0009] Furthermore, the concentration of the tetramethylurea solution containing lithium salt is 0.5 wt% to 10 wt%, further to 0.8 wt% to 8 wt%, and even further to 1 wt% to 8 wt%.

[0010] According to some more specific embodiments of this disclosure, the concentration of the tetramethylurea solution of the lithium salt is 1wt% to 5wt%, for example 1wt%, 2wt%, 3wt%, 4wt%, 5wt%.

[0011] A second aspect of this disclosure provides a lithium metal electrode comprising lithium metal and a lithium salt and tetramethylurea formed on the surface of the lithium metal, wherein the lithium salt comprises one or more of lithium dioxolane borate, lithium difluorooxolane borate, lithium difluorophosphate, lithium o-benzoylsulfonylimide, and lithium acesulfame potassium.

[0012] The third aspect of this disclosure provides a lithium metal electrode, which is a lithium metal electrode that has been soaked in and dried by the aforementioned lithium metal surface treatment agent.

[0013] Furthermore, the soaking time is 10-30 minutes.

[0014] The fourth aspect of this disclosure provides a method for processing a lithium metal electrode, comprising immersing a lithium metal electrode sheet in a lithium metal surface treatment agent as described in any of the preceding claims, removing the sheet, and drying it to obtain the lithium metal electrode.

[0015] In some embodiments, the soaking time is 10-30 minutes.

[0016] In some embodiments, the lithium metal electrode sheet is processed in a drying chamber.

[0017] The fifth aspect of this disclosure provides a lithium battery comprising a positive electrode, a lithium metal negative electrode, and an electrolyte, wherein the lithium metal negative electrode is a lithium metal electrode that has been immersed in and dried by the aforementioned lithium metal surface treatment agent.

[0018] In the embodiments disclosed herein, the cathode material is a cathode material commonly used in lithium batteries in the art, including lithium cobalt oxide, lithium iron phosphate, lithium nickel manganese oxide, other ternary cathode materials or other lithium-rich cathode materials.

[0019] In embodiments of this disclosure, the electrolyte comprises a lithium salt and an organic solvent, wherein the organic solvent comprises ethylene glycol dimethyl ether, ethylene carbonate, and ethyl methyl carbonate.

[0020] In the embodiments of this disclosure, the lithium salt includes, but is not limited to, LiPF6, and the lithium salt concentration is 0.5-2 mol / L.

[0021] The sixth aspect of this disclosure provides a lithium battery comprising a positive electrode, a lithium metal negative electrode, and a solid electrolyte, wherein the lithium metal negative electrode is a lithium metal electrode that has been immersed in and dried by the aforementioned lithium metal surface treatment agent.

[0022] In the embodiments of this disclosure, the cathode material is a cathode material commonly used in lithium batteries in the art, including lithium iron phosphate, lithium cobalt oxide, lithium nickel manganese oxide, other ternary cathode materials or other lithium-rich cathode materials.

[0023] In embodiments of this disclosure, the solid electrolyte includes a PVDF / LiTFSI composite solid electrolyte, a PEO / LiTFSI composite solid electrolyte, a PVDF-HFP / LiTFSI composite solid electrolyte, a PVDF / LIFSI composite solid electrolyte, a PEO / LiFSI, or a PVDF-HFP / LiFSI composite solid electrolyte.

[0024] Due to the application of the above technical solution, this disclosure has the following advantages compared with the prior art:

[0025] This disclosure uses TMU or a TMU solution of a special lithium salt as a lithium metal surface treatment agent to immerse and dry the surface of a lithium metal electrode, which improves the stability of the lithium metal electrode in humid air, significantly reduces the oxidation reaction rate, and has virtually no impact on the charge and discharge performance of lithium batteries using the treated lithium metal anode. It can be used in the production process of lithium batteries or solid-state batteries using lithium metal anodes, and is expected to reduce production difficulty and production costs. Attached Figure Description

[0026] Figure 1 shows the oxidation of lithium metal electrode sheets treated with the treatment agents of Examples 1-6 and Comparative Examples 1-7 (immersion for 10 min) and the untreated control after exposure to a normal indoor environment for 1 minute.

[0027] Figure 2 shows the oxidation of lithium metal electrode sheets treated with the treatment agents of Examples 1-6 and Comparative Examples 1-7 (immersion for 10 min) and the untreated control after exposure to a normal indoor environment for 10 minutes.

[0028] Figure 3 shows the oxidation of lithium metal electrode sheets treated with the treatment agents of Examples 1-6 and Comparative Examples 1-7 (immersion for 10 min) and the untreated control after exposure to a normal indoor environment for 20 minutes. Detailed Implementation

[0029] To address the problem that lithium metal electrodes are highly susceptible to oxidation in normal air environments, necessitating the production of lithium-ion batteries or solid-state batteries using lithium metal anodes under stringent dry and low-oxygen conditions, this disclosure involves extensive research and experimental verification. It was discovered that soaking lithium metal sheets in tetramethylurea (TMU) can improve their stability in humid air to some extent. Furthermore, the inventors of this disclosure experimented with introducing different types and concentrations of lithium salts, finding that only certain specific lithium salts could further improve the stability of lithium metal sheets in humid air, while the addition of some lithium salts offered no improvement in stability, and even accelerated the oxidation rate of lithium metal sheets in humid air. Based on this, the technical solution of this disclosure is: using tetramethylurea (TMU) or a tetramethylurea solution containing specific lithium salts (LiBOB, LiDFOB, LiDFP, Li-SS, Li-AK) as a surface treatment agent for lithium metal.

[0030] The present disclosure will be further described below with reference to embodiments. However, the present disclosure is not limited to the following embodiments. The implementation conditions used in the embodiments can be further adjusted according to different requirements of specific use, and the implementation conditions not specified are conventional conditions in the industry. The technical features involved in the various embodiments of the present disclosure can be combined with each other as long as they do not conflict with each other.

[0031] Unless otherwise specified, all raw materials used in the following examples and comparative examples are commercially available products. Concentration in this document refers to the percentage of the mass of the lithium salt relative to the total mass of the lithium salt and TMU.

[0032] The lithium metal surface treatment agents of Examples 1 to 11 and Comparative Examples 1 to 14 are shown in Table 1.

[0033] Table 1

[0034]

[0035] In Table 1: TMU: Tetramethylurea; LiPF6: Lithium hexafluorophosphate; LiBF4: Lithium tetrafluoroborate; LiClO4: Lithium perchlorate; LiBOB: Lithium dioxolane-borate; LiTFSI: Lithium bis(trifluoromethanesulfonyl)imide; LiDFOB: Lithium difluorooxolane-borate; LiNO3: Lithium nitrate; LiFSI: Lithium difluorosulfonylimide; LiDFP: Lithium difluorophosphate; LiDFOP: Lithium difluorobis(oxolane-)phosphate; Li-SS: Lithium o-benzoylsulfonylimide; Li-AK: Lithium acesulfame potassium. Processing of lithium metal electrode sheets:

[0036] In a drying room (dew point temperature: -40℃), open the vacuum-packed lithium metal electrode sheet, soak it in the above-mentioned treatment agent for 10 minutes or 30 minutes, then remove it, wipe it dry and set it aside for use.

[0037] Surface stability comparison:

[0038] The lithium metal electrode sheets treated in the drying chamber (dew point temperature: -40℃) still retained their metallic luster. They were then transferred from the drying chamber atmosphere to a normal indoor environment (relative humidity: 46%, room temperature: 18.8℃). Timing was started from the moment the normal indoor environment was connected. Figure 1 shows photographs of the lithium metal electrode sheets treated with the treatment agents of Examples 1-6 and Comparative Examples 1-7 (immersion for 10 min) and the untreated control after 1 minute. Figure 2 shows photographs of the lithium metal electrode sheets treated with the treatment agents of Examples 1-6 and Comparative Examples 1-7 (immersion for 10 min) and the untreated control after 10 minutes. Figure 3 shows photographs of the lithium metal electrode sheets treated with the treatment agents of Examples 1-6 and Comparative Examples 1-7 (immersion for 10 min) and the untreated control after 20 minutes. The degree of oxidation on the surface of the lithium metal electrode sheets was graded, and the statistical results are shown in Table 2.

[0039] Table 2

[0040]

[0041] "0": No reaction; "1": Almost no change; "2": Slight reaction; "3": Partial reaction; "4": Mostly reaction; "5": Complete reaction.

[0042] The results show that, compared to untreated lithium metal electrode sheets, the lithium metal electrode sheets treated with the surface treatment agents described in the examples exhibit improved stability in humid air and a significantly slower oxidation reaction rate. However, treatment with certain comparative surface treatment agents did not significantly improve the oxidation reaction; some comparative surface treatment agents (including LiPF6, LiBF4, and LIFSI) even exacerbated the reaction between the lithium metal surface and humid air. TMU solutions of specific lithium salts can further improve the stability of lithium metal electrode sheets. Specifically, TMU solutions of LiBOB, LiDFOB, LiDFP, Li-SS, and Li-AK all reduce the rate of reaction between lithium metal and humid air, with the slowing effect being: LiDFP TMU solution > Li-SS TMU solution > LiBOB TMU solution > Li-AK TMU solution > LiDFOB TMU solution.

[0043] The results also show that the treatment agent with a higher lithium salt concentration (5wt%) has a better treatment effect than the treatment agent with a lower lithium salt concentration (1wt%), and the treatment agent with a higher lithium salt concentration (5wt%) can shorten the surface treatment time.

[0044] The effect of treatment agents on the performance of lithium metal electrode sheets:

[0045] In an argon-filled glove box (H2O < 10 ppm), lithium metal electrode sheets treated for 10 min by any of the treatment agents in Examples 1-6 and Comparative Examples 1-7 were assembled into LCO||Li liquid coin-type lithium-ion batteries (4.2 V, ~1.5 mAh). The electrolyte consisted of lithium salt and organic solvent. The lithium salt was 1M LiPF6, and the organic solvent was a mixed solvent of DME / EC / EMC = 1 / 1 / 1 (volume ratio). The separator was Celgard 2320. The capacity retention rate of the LCO||Li liquid coin-type lithium-ion batteries after 100 cycles of charge-discharge at 0.5C at room temperature (18.8 °C) was tested (Table 3). LCO||Li liquid coin-type lithium-ion batteries assembled with freshly opened (untreated) lithium metal sheets were used as a control to evaluate the effect of the treatment agent on the performance of the lithium metal electrode sheets.

[0046] Table 3

[0047]

[0048] Table 3 shows that the capacity retention of LCO||Li liquid coin lithium-ion batteries with metal lithium electrode sheets treated with the above-mentioned different treatment agents is not significantly different from that of LCO||Li liquid coin lithium-ion batteries with untreated metal lithium electrode sheets after 100 cycles at room temperature.

[0049] In an argon-filled glove box (H2O < 10 ppm), lithium metal electrode sheets treated with any of the treatment agents in Examples 1-6 and Comparative Examples 1-7 for 10 min were assembled into LFP||Li solid-state coin cell lithium-ion batteries (3.65 V, ~1.5 mAh). A composite solid electrolyte with PVDF / LiTFSI = 1 / 1 (mass ratio) was used. The capacity retention rate of the LFP||Li coin cell lithium-ion batteries after 50 cycles of charge-discharge at 0.2C at 60°C was tested (Table 4). LFP||Li solid-state coin cell lithium-ion batteries assembled with freshly opened (untreated) lithium metal sheets were used as a control to evaluate the effect of the treatment agent on the performance of the lithium metal electrode sheets.

[0050] Table 4

[0051]

[0052] Table 4 shows that the capacity retention of LFP||Li solid-state coin lithium-ion batteries treated with the above-mentioned different lithium metal electrode sheets is not significantly different from that of LFP||Li solid-state coin lithium-ion batteries using untreated lithium metal electrode sheets after 50 cycles at 60°C.

[0053] As can be seen from Tables 3 and 4, treating the lithium metal electrode sheets with the above-mentioned treatment agents will not significantly affect the charge and discharge performance of the lithium battery.

[0054] In summary, lithium metal itself is highly reactive, especially prone to oxidation under humid air conditions. Treating the surface of lithium metal electrode sheets with TMU solvent and TMU solutions containing certain concentrations of LiBOB, LiDFOB, LiDFP, Li-SS, or Li-AK can significantly improve the electrode sheets' resistance to humid air or moisture without substantially affecting the charge-discharge performance of the assembled lithium battery. This approach is expected to facilitate the development of lithium metal liquid or solid-state batteries. Furthermore, it eliminates the need for the entire battery assembly line to be conducted in an ultra-low dew point drying chamber, greatly reducing the investment and maintenance costs of large-scale dehumidification systems and improving production efficiency.

[0055] The appended independent and dependent claims further define other specific and preferred embodiments of this disclosure. Features of the dependent claims can be freely combined with features of the independent claims, and can be combined with other features not expressly recited in the claims as needed. Each technical solution can be implemented independently or in combination with one or more other technical solutions.

[0056] The disclosure will now be described in conjunction with the various examples and combinations thereof described below.

[0057] 1. Example 1 provides a lithium metal surface treatment agent, which is tetramethylurea or a tetramethylurea solution containing lithium salt, wherein the lithium salt includes one or more of lithium dioxalate borate, lithium difluorooxalate borate, lithium difluorophosphate, lithium o-benzoylsulfonylimide, and lithium acesulfame potassium.

[0058] 2. According to the lithium metal surface treatment agent provided in Example 1, the concentration of the tetramethylurea solution containing lithium salt is 0.1wt%~10wt%.

[0059] 3. In the lithium metal surface treatment agent provided in any of the foregoing examples, the concentration of the tetramethylurea solution containing lithium salt is 1wt% to 5wt%.

[0060] 4. The lithium metal surface treatment agent provided according to any of the foregoing examples, characterized in that the lithium metal surface treatment agent is composed of tetramethylurea and lithium salt.

[0061] 5. Example 5 provides a lithium metal electrode comprising lithium metal and a lithium salt and tetramethylurea formed on the surface of the lithium metal, wherein the lithium salt comprises one or more of lithium dioxalate borate, lithium difluorooxalate borate, lithium difluorophosphate, lithium o-benzoylsulfonylimide, and lithium acesulfame potassium.

[0062] 6. Example 6 provides a lithium metal electrode, which is a lithium metal electrode that has been soaked and dried by any one of the lithium metal surface treatment agents in Examples 1 to 4.

[0063] 7. Example 7 provides a method for processing a lithium metal electrode, wherein a lithium metal electrode sheet is immersed in the lithium metal surface treatment agent described in any one of Examples 1 to 4, and then removed and dried to obtain the lithium metal electrode.

[0064] 8. According to the processing method provided in Example 7, the soaking time is 10-30 minutes.

[0065] 9. The lithium metal electrode sheet is processed in a drying room according to the processing method provided in Example 7 or 8.

[0066] 10. Example 10 provides a lithium battery comprising a lithium metal anode, wherein the lithium metal anode is a lithium metal electrode as described in Example 5 or 6 or a lithium metal electrode obtained by any one of Examples 7 to 9.

[0067] 11. The lithium battery provided in Example 10 also includes a positive electrode and an electrolyte.

[0068] 12. According to the lithium battery provided in Example 11, the electrolyte comprises a lithium salt and an organic solvent, wherein the organic solvent comprises ethylene glycol dimethyl ether, ethylene carbonate and ethyl methyl carbonate.

[0069] 13. The lithium battery provided in Example 10 also includes a positive electrode and a solid electrolyte.

[0070] 14. The cathode material of the lithium battery provided in Example 10 or 13 includes lithium iron phosphate, lithium cobalt oxide, lithium nickel manganese oxide, other ternary lithium cathode materials or other lithium-rich cathode materials.

[0071] 15. According to the lithium battery provided in Example 13, the solid electrolyte comprises a PVDF / LiTFSI composite solid electrolyte, a PEO / LiTFSI composite solid electrolyte, a PVDF-HFP / LiTFSI composite solid electrolyte, a PVDF / LIFSI composite solid electrolyte, a PEO / LiFSI composite solid electrolyte, or a PVDF-HFP / LiFSI composite solid electrolyte.

[0072] The above detailed description of this disclosure is intended to enable those skilled in the art to understand and implement its contents, but it should not be construed as limiting the scope of protection of this disclosure. All equivalent changes or modifications made in accordance with the spirit and essence of this disclosure should be included within the scope of protection of this disclosure.

Claims

1. A metal lithium surface treatment agent, characterized by, It is tetramethyl urea or a tetramethyl urea solution containing a lithium salt, wherein the lithium salt includes one or more of lithium bis(oxalato)borate, lithium difluoro(oxalato)borate, lithium difluorophosphate, lithium o-benzoyl benzenesulfonimide, and lithium acetyl sulfonimide.

2. The metal lithium surface treatment agent according to claim 1, characterized by, The concentration of the tetramethyl urea solution containing a lithium salt is 0.1wt%-10wt%.

3. The metal lithium surface treatment agent according to claim 2, characterized by, The concentration of the tetramethyl urea solution containing a lithium salt is 1wt%-5wt%.

4. The metal lithium surface treatment agent according to any one of claims 1 to 3, characterized by, The metal lithium surface treatment agent is composed of tetramethyl urea and a lithium salt.

5. A metal lithium electrode, characterized by, It includes metal lithium and a lithium salt and tetramethyl urea formed on the surface of the metal lithium, wherein the lithium salt includes one or more of lithium bis(oxalato)borate, lithium difluoro(oxalato)borate, lithium difluorophosphate, lithium o-benzoyl benzenesulfonimide, and lithium acetyl sulfonimide.

6. The lithium metal electrode of claim 5, wherein, It is a metal lithium electrode soaked and dried by the metal lithium surface treatment agent according to any one of claims 1-4.

7. A method of processing a metal lithium electrode, characterized by, A metal lithium electrode piece is soaked with the metal lithium surface treatment agent according to any one of claims 1-4, taken out and dried to obtain the metal lithium electrode.

8. The treatment method according to claim 7, characterized in that, The soaking time is 10-30min.

9. The treatment method according to claim 7 or 8, characterized in that, The metal lithium electrode piece is processed in a drying room.

10. A lithium battery, characterized by, It includes a metal lithium negative electrode, which is the metal lithium electrode according to claim 5 or 6 or the metal lithium electrode processed by the processing method according to any one of claims 7-9.

11. The lithium battery of claim 10, wherein, It further includes a positive electrode and an electrolyte.

12. The lithium battery of claim 11, wherein, The electrolyte includes a lithium salt and an organic solvent, and the organic solvent includes ethylene glycol dimethyl ether, vinyl carbonate, and methyl ethyl carbonate.

13. The lithium battery of claim 10, wherein, It further includes a positive electrode and a solid-state electrolyte.

14. The lithium battery according to claim 10 or 13, characterized in that, The positive electrode material includes lithium iron phosphate, lithium cobaltate, lithium nickel manganese oxide, other ternary lithium positive electrode materials, or other lithium-rich positive electrode materials.

15. The lithium battery of claim 13, wherein, The solid-state electrolyte includes a PVDF / LiTFSI composite solid-state electrolyte, a PEO / LiTFSI composite solid-state electrolyte, a PVDF-HFP / LiTFSI composite solid-state electrolyte, a PVDF / LiFSI composite solid-state electrolyte, a PEO / LiFSI composite solid-state electrolyte, or a PVDF-HFP / LiFSI composite solid-state electrolyte.