High-fluidity under-sea non-dispersible high-performance solidified sludge soil and preparation method therefor

By using a synergistic system formed by components such as chitosan quaternary ammonium salt in marine engineering, the problems of fluidity and non-dispersibility of silt have been solved, realizing the resource utilization of silt and improving its environmentally friendly construction performance.

WO2026233473A1PCT designated stage Publication Date: 2026-11-12NANJING HYDRAULIC RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/105841
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2026-06-24
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing technologies struggle to address the high fluidity and non-dispersibility of silt in marine engineering, leading to difficulties in resource utilization and potential environmental pollution.

Method used

Chitosan quaternary ammonium salt was used as a flocculant, combined with cement, fly ash, acrylate emulsion and silica fume, to form a synergistic system through chemical bond interaction and microstructure interpenetration, thereby regulating the fluidity and non-dispersibility of silt and preparing high-fluidity, non-dispersible, high-performance solidified silt for underwater use.

Benefits of technology

This enables the near-situ resource utilization of silt, improves the mechanical properties and underwater non-dispersibility of silt soil, reduces environmental pollution, and meets the needs of marine engineering construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2026105841_12112026_PF_FP_ABST
    Figure CN2026105841_12112026_PF_FP_ABST
Patent Text Reader

Abstract

A high-fluidity under-sea non-dispersible high-performance solidified sludge soil, comprising the following components: sludge, cement, fly ash, an acrylate emulsion, silica fume, a chitosan quaternary ammonium salt, and a water reducer in powder form. The physicochemical properties of the sludge are determined by one or both of T-O clay minerals or T-O-T clay minerals; and the ratio by parts of cement to silica fume and the ratio by parts of cement to fly ash are determined on the basis of the physicochemical properties of the sludge. Further disclosed is a preparation method for the high-fluidity under-sea non-dispersible high-performance solidified sludge soil.
Need to check novelty before this filing date? Find Prior Art

Description

A high-flowability, non-dispersible, high-performance solidified silt soil for underwater use and its preparation method Technical Field

[0001] This invention belongs to the technical field of seabed leveling, repair and erosion prevention in marine engineering, and in particular relates to a high-flowability, non-dispersible, high-performance solidified silt soil for underwater use and its preparation method. Background Technology

[0002] The large amount of silt generated during my country's marine engineering construction has become a pressing problem. This silt not only has low structural strength but also exhibits high spatial and temporal heterogeneity in its material properties and is enriched with various heavy metals, posing challenges to the environment and resource utilization. The traditional method of disposal involves dumping the silt, after approval from relevant authorities, in land or near-shore areas that are unlikely to be developed in the short term. This practice not only wastes land resources but may also induce geological disasters and incur huge transportation costs. Therefore, achieving near-site resource utilization of silt is particularly important.

[0003] Currently, an important approach to the resource utilization of silt is solidification treatment using cement-based materials. By controlling the ratio of cement content to initial moisture content (i.e., the binder-to-water ratio), the mechanical properties of the solidified silt can be regulated. However, if solidified silt is applied to seabed leveling, restoration, and erosion control, its fluidity and non-dispersibility underwater must also be considered. Existing research rarely addresses this area, and the few related studies lack universality, mainly because the high heterogeneity of silt properties leads to significant fluctuations in the performance of solidified silt. Marine engineering silt is mainly composed of clay minerals (such as kaolinite, montmorillonite, illite, etc.) and associated minerals (such as quartz, mica, feldspar, etc.), as well as small amounts of carbonates, trace amounts of sulfates, phosphates, and organic matter. Its basic physicochemical properties are primarily determined by clay minerals. Therefore, this invention, based on the qualitative and quantitative characterization results of clay minerals in silt, determines the preparation ratio of solidified silt to mitigate the negative impact of the high heterogeneity of silt properties. Furthermore, existing flocculants for underwater non-dispersible materials mostly use water-soluble synthetic organic polymers, such as polyacrylamide, which may pollute the marine environment. This invention uses a biopolymer flocculant solution—chitosan quaternary ammonium salt solution—as the flocculant to achieve significant ecological benefits.

[0004] In summary, based on practical engineering needs, there is an urgent need to invent a high-flowability, non-dispersible, high-performance solidified silt soil and its preparation method that is based on the physicochemical properties of silt, so as to realize the near-situ resource utilization of marine engineering silt, while reducing environmental pollution and improving economic benefits. Technical issues

[0005] To address the problems in related technologies, this invention proposes a high-flowability, non-dispersible, high-performance solidified silt soil for underwater use and its preparation method, thereby overcoming the aforementioned technical problems existing in the existing related technologies. Technical solutions

[0006] The present invention adopts the following technical solution: a high-flowability, non-dispersible, high-performance solidified silt soil for underwater use, comprising the following components: silt, cement, fly ash, acrylate emulsion, silica fume, chitosan quaternary ammonium salt, and powdered water-reducing agent;

[0007] The physicochemical properties of the silt are determined by one or both of TO-type clay minerals or TOT-type clay minerals; the ratio of cement to silica fume and the ratio of cement to fly ash are determined based on the physicochemical properties of the silt.

[0008] In a further embodiment, when the physicochemical properties of the silt are determined by TO-type clay minerals, the ratio of the cement to the silica fume is 1:(0.4~0.6).

[0009] The ratio of cement to fly ash is 1:(0.01~0.2).

[0010] In a further embodiment, when the physicochemical properties of the silt are determined by TOT-type clay minerals, the ratio of the cement to the silica fume is 1:(0.01~0.2).

[0011] The ratio of cement to fly ash is 1:(0.4~0.5).

[0012] In a further embodiment, when the physicochemical properties of the silt are jointly determined by TO-type clay minerals and TOT-type clay minerals, the ratio of the cement to the silica fume is 1:(0.2~0.4).

[0013] The ratio of cement to fly ash is 1:(0.2~0.4).

[0014] In a further embodiment, the components are included in the following proportions:

[0015] 250-500 parts silt, 100-200 parts cement, 1-50 parts fly ash, 30-100 parts acrylic emulsion, 1-60 parts silica fume, 1-2 parts chitosan quaternary ammonium salt, and 1-2 parts powdered water-reducing agent.

[0016] The preparation method for the high-flowability, non-dispersible, high-performance solidified silt soil for underwater use as described above includes the following steps:

[0017] Step 1: Determine the physicochemical properties of the silt;

[0018] Step 2: Add deionized water to chitosan quaternary ammonium salt to obtain chitosan quaternary ammonium salt solution;

[0019] Step 3: Determine the part ratio of silt, cement, silica fume and fly ash based on the physicochemical properties of Step 1, weigh them, mix and stir until uniform to obtain dry material;

[0020] Step 4: Mix the dry material obtained in Step 3 with the acrylic emulsion, and slowly add the powdered water-reducing agent and chitosan quaternary ammonium salt solution. Stir thoroughly until the cement is free of lumps and meets the expected fluidity.

[0021] In a further embodiment, the physicochemical properties of step one are determined by one or both of TO-type clay minerals or TOT-type clay minerals.

[0022] The following methods were used for characterization and determination: 29 One of the following: Si-nuclear magnetic resonance, X-ray full-spectrum fitting, or thermogravimetric analysis.

[0023] In a further embodiment, the preparation process of the chitosan quaternary ammonium salt solution in step two includes:

[0024] Weigh out samples with a degree of substitution greater than 90% and a molecular weight higher than 4.8 × 10⁻⁶. 4 Chitosan quaternary ammonium salt was added to a reaction vessel, and deionized water was added; the mass ratio of the chitosan quaternary ammonium salt to deionized water was less than 1:3.

[0025] Stir at 120-180 rpm at 75-90°C until completely dissolved.

[0026] In a further embodiment, the solid content of the acrylate emulsion is 30-50%.

[0027] In a further embodiment, the stirring time in step four is 20 to 30 minutes. Beneficial effects

[0028] The beneficial technical effects of this invention are as follows: Based on the qualitative and quantitative characterization results of clay minerals in the silt, the preparation ratio of the solidified silt is determined, avoiding the problem of significant performance fluctuations in solidified silt caused by the high heterogeneity of silt properties, thus enabling the near-site resource utilization of silt. Simultaneously, the solidified silt and its preparation method, through the addition of solidifying agents, coupling agents, and flocculants, significantly improve the underwater non-dispersibility of the solidified silt in marine environments, while retaining its flowability to meet construction needs. Furthermore, the various mechanical properties of the solidified silt are effectively improved, exhibiting good compressive strength and adhesion, providing guidance in the fields of seabed leveling, repair, and erosion control in marine engineering.

[0029] The curing agent (cement, fly ash) and flocculant (silica fume, chitosan quaternary ammonium salt) form a ternary synergistic network through a coupling agent (acrylate emulsion). The Ca generated during cement hydration... 2+ The initial CSH gel framework is formed by ionic bonding between the hydroxyl groups on the surface of silica powder and the Si-O groups on the surface of CSH. The carboxyl groups in the acrylate emulsion form covalent bonds with the Si-O groups on the surface of CSH through esterification, which improves the toughness of the framework. The Al2O3 on the surface of fly ash dissociates into Al-O groups in an alkaline environment, which combine with the quaternary ammonium cations of chitosan quaternary ammonium salt through electrostatic interaction. At the same time, the spherical particles of fly ash are embedded in the topological network formed by the long chains of chitosan, which improves the underwater anti-dispersion property. The powdered water-reducing agent (polycarboxylic acid system) disperses cement particles through steric hindrance, while the acrylate emulsion reduces the friction coefficient between flocs through the "ball effect". The two work together to regulate the fluidity.

[0030] The quaternary ammonium groups of chitosan quaternary ammonium salt neutralize the negative charge on the surface of clay minerals, forming a dense adsorption layer. Simultaneously, the active SiO2 of silica powder and the hydroxyl groups of chitosan form Si-OC bonds through dehydration condensation, enhancing interfacial chelation under dynamic pH regulation. Silica powder and fly ash, through complementary reactivity and particle size distribution, respectively dominate early strength formation and later pore filling, forming a dense "nano-micro" nested structure. Acrylic ester and water-reducing agent construct hydrogen-bonded stress transmission chains under an adsorption competition mechanism, achieving a dynamic balance of rheological properties. Through chemical bond interactions, microstructural interpenetration, and macroscopic performance coupling, the components form an inseparable synergistic system, fundamentally overcoming the performance limitations of single-functional materials. Attached Figure Description

[0031] Figure 1 shows the crystal structure and scanning electron microscope image of natural kaolinite and montmorillonite.

[0032] Figure 2 is a quantitative analysis diagram of the mineral composition of the sludge raw material using the XRD-Rietveld method in Example 2.

[0033] Figure 3 shows the non-dispersion test results of Example 2.

[0034] Figure 4 is a quantitative analysis diagram of the mineral composition of the sludge raw material using the XRD-Rietveld method in Example 3.

[0035] Figure 5 shows the non-dispersion test results of Example 3.

[0036] Figure 6 is a quantitative analysis diagram of the mineral composition of the sludge raw material using the XRD-Rietveld method in Example 4.

[0037] Figure 7 shows the non-dispersion test results of Example 4. Embodiments of the present invention

[0038] To further illustrate the various embodiments, the present invention provides accompanying drawings, which are part of the disclosure of the present invention. These drawings are mainly used to illustrate the embodiments and can be used in conjunction with the relevant descriptions in the specification to explain the operating principles of the embodiments. With reference to these drawings, those skilled in the art should be able to understand other possible implementation methods and the advantages of the present invention. Example 1

[0039] This embodiment provides a high-flowability, non-dispersible, high-performance solidified silt soil for underwater use, comprising the following components: silt, cement, fly ash, acrylate emulsion, silica fume, chitosan quaternary ammonium salt, and powdered water-reducing agent.

[0040] Specifically, in this embodiment, cement and fly ash are used as curing agents. The cement used is P·O42.5 ordinary Portland cement, and the fly ash is Grade I fly ash. Cement can significantly enhance the mechanical properties of the solidified silt. The silicate gel generated by fly ash can fill cracks and pores in the matrix. Furthermore, fly ash can improve the thixotropy and fluidity of the freshly mixed grout, optimizing construction performance and ensuring the later-stage strength development of the solidified silt.

[0041] Furthermore, silica powder and chitosan quaternary ammonium salt are used as flocculants. Silica powder has high reactivity and a large specific surface area. Its high reactivity enables it to generate CSH gel with gelling properties, and its large specific surface area allows it to more effectively adsorb surrounding ions and molecules, forming flocs and thus improving the strength and stability of solidified silt in water. Chitosan quaternary ammonium salt, due to its long-chain structure and its tendency to become a positively charged electrolyte, plays multiple roles in neutralizing, binding, bridging, and chelating the negatively charged colloidal system in the solidified silt system, thereby improving the non-dispersibility of the solidified silt in water.

[0042] Correspondingly, powdered water-reducing agents can effectively improve the fluidity of cement mortar, greatly enhancing the construction performance of modified cement mortar and giving it excellent underwater construction and workability.

[0043] The coupling agent is an acrylic emulsion with a solid content of 45%. The acrylic emulsion can form a continuous film between the flocculant-agglomerated particles, which can reduce the friction between the particles and thus significantly improve the fluidity of the solidified silt. At the same time, there are chemical bridging bonds between these films, which can enhance the structural stability of the solidified silt and improve its later strength.

[0044] In a further embodiment, the sludge, cement, fly ash, acrylate emulsion, silica fume, chitosan quaternary ammonium salt, and powdered water-reducing agent are in the following proportions: 250-500 parts sludge, 100-200 parts cement, 1-50 parts fly ash, 30-100 parts acrylate emulsion, 1-60 parts silica fume, 1-2 parts chitosan quaternary ammonium salt, and 1-2 parts powdered water-reducing agent.

[0045] In a further embodiment, to avoid the problem of significant fluctuations in the performance of solidified silt soil due to the high heterogeneity of silt properties, near-site resource utilization of silt can be achieved. This embodiment further analyzes the physicochemical properties of silt and provides corresponding adjustments to the component ratios, as follows:

[0046] The physicochemical properties of the sludge are determined by one or both of TO-type and TOT-type clay minerals. The ratio of cement to silica fume and the ratio of cement to fly ash are determined based on these physicochemical properties. The crystal structure (TO-type or TOT-type) of the clay minerals in the sludge directly affects its physicochemical properties. TO-type clay minerals (such as kaolinite) have a 1:1 layered structure with weak interlayer forces, good thixotropy and fluidity, but insufficient water retention. TOT-type clay minerals (such as montmorillonite) have a 2:1 layered structure, can adsorb a large number of water molecules between layers, have a high specific surface area and strong flocculation ability, but poor thixotropy. If the curing agent ratio is not optimized for the mineral structure, the following problems will occur:

[0047] When TO type is the main component: the slurry is prone to segregation due to insufficient water retention capacity. It is necessary to add more silica powder with high specific surface area to adsorb free water and enhance water retention by generating CSH gel, while inhibiting fluidity loss;

[0048] When TOT type is dominant: Due to excessive flocculation capacity, the viscosity of the slurry increases. It is necessary to add more fly ash to utilize the "ball effect" of its spherical particles to improve thixotropy, and to regulate the hydration process through pozzolanic reaction;

[0049] In the case of a hybrid type: the ratio of silica fume to fly ash needs to be controlled in a coordinated manner to balance water retention and thixotropy, and to avoid performance degradation caused by excessive amount of a single component.

[0050] It should be noted that natural clay minerals are widely distributed in nature. Their crystal structures consist of silicon-oxygen tetrahedral layers and aluminum-oxygen octahedral layers arranged according to certain rules, and are divided into two main categories based on their arrangement characteristics: 1:1 type and 2:1 type. The representative minerals are kaolinite and montmorillonite, respectively. The 1:1 type is also known as the TO type, and the 2:1 type is also known as the TOT type. The crystal structures and scanning electron microscope images of natural kaolinite and montmorillonite are shown in Figure 1.

[0051] Based on the analysis of the above components, when the physicochemical properties of the silt are determined by TO-type clay minerals, the part ratio of the cement to the silica fume is 1:(0.4~0.6); the part ratio of the cement to the fly ash is 1:(0.01~0.2).

[0052] When the physicochemical properties of the silt are determined by TOT-type clay minerals, the ratio of the cement to the silica fume is 1:(0.01~0.2); the ratio of the cement to the fly ash is 1:(0.4~0.5).

[0053] When the physicochemical properties of the silt are determined by both TO-type clay minerals and TOT-type clay minerals, the part ratio of the cement to the silica fume is 1:(0.2~0.4); the part ratio of the cement to the fly ash is 1:(0.2~0.4). Example 2

[0054] This embodiment uses 250 parts of silt, 100 parts of cement, 10 parts of fly ash, 30 parts of acrylate emulsion, 50 parts of silica fume, 1.5 parts of chitosan quaternary ammonium salt, and 1 part of powdered water-reducing agent as an example to disclose a method for preparing high-flowability, non-dispersible, high-performance solidified silt soil for underwater use, including the following steps:

[0055] Step 1, adopt 9 One of the following methods—Si-NMR, X-ray full-spectrum fitting, or thermogravimetric analysis—is used to determine whether the physicochemical properties of the sludge are controlled by clay minerals arranged in a 1:1 ratio of silicon-oxygen tetrahedral layers and aluminum-oxygen octahedral layers (TO type) or by clay minerals arranged in a 2:1 ratio (TOT type). Based on its physicochemical properties, the particulate ratio between cement and silica fume, and the particulate ratio between cement and fly ash, are further selected with reference to the description in Example 1.

[0056] Step 2: Add deionized water to the chitosan quaternary ammonium salt to obtain a chitosan quaternary ammonium salt solution.

[0057] Step 3: Determine the part ratio of silt, cement, silica fume and fly ash based on the physicochemical properties of Step 1, weigh them, mix and stir until uniform to obtain dry material;

[0058] Step 4: Mix the dry material obtained in Step 3 with the acrylic emulsion, and slowly add the powdered water-reducing agent and chitosan quaternary ammonium salt solution. Stir thoroughly until the cement is free of lumps and meets the expected fluidity. Stirring time should be 20-30 minutes. The solid content of the acrylic emulsion should be 30-50%. The prepared solidified silt should be used within 5 hours. Use should be stopped once large particles of clumps appear inside the solidified silt.

[0059] Furthermore, the preparation process of the chitosan quaternary ammonium salt solution in step two includes:

[0060] Weigh out samples with a degree of substitution greater than 90% and a molecular weight higher than 4.8 × 10⁻⁶. 4 Chitosan quaternary ammonium salt was added to a reaction vessel, and deionized water was added; the mass ratio of the chitosan quaternary ammonium salt to deionized water was less than 1:3.

[0061] Stir at 120-180 rpm at 75-90°C until completely dissolved. Furthermore, the amount of chitosan quaternary ammonium salt solution used should be such that the concentration of chitosan quaternary ammonium salt in the liquid is not less than 2.1 g / L.

[0062] As shown in Figure 2, the silt is composed of 73% quartz, 22% kaolinite, 4% muscovite, and 1% dolomite, and its physicochemical properties are mainly determined by TO-type clay minerals. Therefore, the ratio of cement to silica fume in the solidified silt should be between 1:0.4 and 0.6, and the ratio of cement to fly ash should be between 1:0.01 and 0.2.

[0063] Correspondingly, solidified silt was prepared based on the above proportions and preparation method, and its non-dispersibility was tested, as shown in Figure 3. It can be seen that the solidified silt can be directly poured into a beaker, exhibiting good fluidity. After the solidified silt was poured into water, the water in the beaker did not immediately become turbid. The solidified silt settled in the beaker, and the settling process was relatively slow and concentrated. The water became slightly turbid after the solidified silt settled, but the overall turbidity was low, showing good non-dispersibility.

[0064] In this embodiment, the unconfined compressive strength, fluidity, and setting time of the solidified silt mixture with this mix proportion were tested using CJ / T526-2018 "Softening and Curing Agent", GB / T1346-2011 "Standard Consistency Water Requirement, Setting Time and Soundness Test Methods for Cement", and GB / T 50123-2019 "Standard for Geotechnical Test Methods". The test results are shown in Table 1. All measured parameters meet the design requirements.

[0065] Table 1

[0066]

[0067] Furthermore, this embodiment also provides a corresponding comparative example. If a TOT-type mix design (cement: silica fume: fly ash = 1:0.1:0.4) is directly adopted without mineral analysis, it leads to slurry segregation, with a 28-day compressive strength of only 480 kPa and a fluidity of 390 mm. During the settling process of the solidified soil, the surrounding water immediately becomes turbid, and the dispersion of cement and soil particles in the water is poor, with poor underwater non-dispersibility. Example 3

[0068] High-flowability, non-dispersible, high-performance solidified silt soil for underwater use comprises the following raw materials in parts: silt, solidifying agent, coupling agent, flocculant, and water-reducing agent.

[0069] Specifically, the curing agent is P•O42.5 ordinary Portland cement and Grade I fly ash. Cement can significantly enhance the mechanical properties of the solidified silt. The silicate gel formed by fly ash can fill the cracks and pores in the matrix. In addition, fly ash can improve the thixotropy and fluidity of the freshly mixed grout, optimize construction performance, and ensure the later strength development of the solidified silt.

[0070] Specifically, the coupling agent is an acrylic emulsion with a solid content of 45%. The acrylic emulsion can form a continuous film between the flocculant-agglomerated particles, which can reduce the friction between the particles and thus significantly improve the fluidity of the solidified silt. At the same time, there are chemical bridging bonds between these films, which can enhance the structural stability of the solidified silt and improve its later strength.

[0071] Specifically, the flocculants are silica powder and chitosan quaternary ammonium salt. Silica powder has high reactivity and a large specific surface area. Its high reactivity enables it to form CSH gel with gelling properties, and its large specific surface area allows it to more effectively adsorb surrounding ions and molecules, forming flocs and thus improving the strength and stability of the solidified silt in water. Chitosan quaternary ammonium salt, due to its long-chain structure and its tendency to become a positively charged electrolyte, plays multiple roles in neutralizing, binding, bridging, and chelating the negatively charged colloidal system in the solidified silt system, thereby improving the non-dispersibility of the solidified silt in water.

[0072] Specifically, powdered water-reducing agents can effectively improve the fluidity of cement mortar, significantly enhancing the construction performance of modified cement mortar and giving it excellent underwater construction and workability.

[0073] In this embodiment, the curing agent is P•O42.5 ordinary silicate cement and Grade I fly ash, the coupling agent is acrylate emulsion with a solid content of 45%, and the flocculant is silica powder and chitosan quaternary ammonium salt.

[0074] This embodiment discloses a method for preparing high-flowability, non-dispersible, high-performance solidified silt soil for underwater applications, using 250 parts of silt, 100 parts of cement, 40 parts of fly ash, 50 parts of acrylate emulsion, 3 parts of silica powder, 2 parts of chitosan quaternary ammonium salt, and 1 part of powdered water-reducing agent. The preparation method can refer to the steps in Example 2. The difference is that the physicochemical properties of the silt are mainly determined by TOT-type clay minerals.

[0075] As shown in Figure 4, the silt is composed of 26% quartz, 40% illite, 21% montmorillonite, and 13% feldspar, and its physicochemical properties are mainly determined by TOT-type clay minerals. Therefore, the ratio of cement to silica fume in the solidified silt should be between 1:0.01 and 0.2, and the ratio of cement to fly ash should be between 1:0.4 and 0.5.

[0076] In this embodiment, the underwater non-dispersibility test results of the solidified silt mixture are shown in Figure 5. It can be seen that the solidified silt can be directly poured into the beaker, exhibiting good fluidity. After the solidified silt is poured into the water, the water in the beaker does not immediately become turbid. The solidified silt settles in the beaker, and the settling process is relatively slow and concentrated. The water becomes slightly turbid after the solidified silt settles, but the overall turbidity is low, demonstrating good non-dispersibility.

[0077] In this embodiment, the unconfined compressive strength, fluidity, and setting time of the solidified silt mixture with this mix proportion were tested using CJ / T526-2018 "Softening and Curing Agent", GB / T1346-2011 "Standard Consistency Water Requirement, Setting Time and Soundness Test Methods for Cement", and GB / T 50123-2019 "Standard for Geotechnical Test Methods". The test results are shown in Table 2. All measured parameters meet the design requirements.

[0078] Table 2

[0079]

[0080] Furthermore, this embodiment provides a corresponding comparative example. Without analyzing the minerals, a TO-type mix ratio (cement: silica fume: fly ash = 1:0.5:0.1) was directly used. The slurry viscosity increased dramatically, the fluidity was 80 mm, the 28-day strength was 550 kPa, and the underwater non-dispersibility was high. Example 4

[0081] This embodiment uses 250 parts silt, 100 parts cement, 30 parts fly ash, 40 parts acrylate emulsion, 25 parts silica fume, 2 parts chitosan quaternary ammonium salt, and 1 part powdered water-reducing agent as an example to disclose a method for preparing high-flowability, non-dispersible, high-performance solidified silt soil for underwater use. The preparation method can refer to the steps in Example 2, but the difference lies in that the physicochemical properties of the silt are mainly determined by TO-type and TOT-type clay minerals. As shown in Figure 6, the silt is composed of 57% quartz, 16% montmorillonite, 15% kaolinite, and 12% feldspar, and its physicochemical properties are mainly determined by both TO-type and TOT-type clay minerals. Therefore, the ratio of cement to silica fume in the solidified silt soil should be between 1:0.2 and 0.4, and the ratio of cement to fly ash should be between 1:0.2 and 0.4.

[0082] Figure 7 shows the underwater non-dispersibility test results of the solidified silt mixture in this embodiment. It can be seen that the solidified silt can be directly poured into the beaker, exhibiting good fluidity. After the solidified silt is poured into the water, the water in the beaker does not immediately become turbid. The solidified silt settles in the beaker, and the settling process is relatively slow and concentrated. The water becomes slightly turbid after the solidified silt settles, but the overall turbidity is low, demonstrating good non-dispersibility.

[0083] In this embodiment, the unconfined compressive strength, fluidity, and setting time of the solidified silt mixture with this mix proportion were tested using CJ / T526-2018 "Softening and Curing Agent", GB / T1346-2011 "Standard Consistency Water Requirement, Setting Time and Soundness Test Methods for Cement", and GB / T 50123-2019 "Standard for Geotechnical Test Methods". The test results are shown in Table 3. All measured parameters meet the design requirements.

[0084] Table 3

[0085]

[0086] Furthermore, this embodiment provides a corresponding comparative example. To ensure underwater non-dispersibility, existing technologies often blindly increase the silica fume content (cement: silica fume: fly ash = 1:0.6:0.1), which leads to early cracking, a 28-day strength of only 580 kPa, and a fluidity of 140 mm. The comparative example shows that when the curing agent ratio is mismatched with the silt mineral type, the compressive strength of the solidified body can decrease by up to 30%, the fluidity loss exceeds 50%, and the underwater dispersibility is significantly deteriorated. This fully demonstrates the decisive role of ratio control based on mineral analysis in improving overall performance.

Claims

1. A high-flowability, non-dispersible, high-performance solidified silt soil for underwater use, characterized in that, It includes the following components: sludge, cement, fly ash, acrylate emulsion, silica fume, chitosan quaternary ammonium salt, and powdered water-reducing agent; The physicochemical properties of the silt are determined by one or both of TO-type clay minerals or TOT-type clay minerals; the ratio of cement to silica fume and the ratio of cement to fly ash are determined based on the physicochemical properties of the silt.

2. The high-flowability, non-dispersible, high-performance solidified silt soil for underwater use according to claim 1, characterized in that, When the physicochemical properties of the silt are determined by TO-type clay minerals, the ratio of the cement to the silica fume is 1:(0.4~0.6). The ratio of cement to fly ash is 1:(0.01~0.2).

3. The high-flowability, non-dispersible, high-performance solidified silt soil for underwater use according to claim 1, characterized in that, When the physicochemical properties of the silt are determined by TOT-type clay minerals, the ratio of the cement to the silica fume is 1:(0.01~0.2). The ratio of cement to fly ash is 1:(0.4~0.5).

4. The high-flowability, non-dispersible, high-performance solidified silt soil for underwater use according to claim 1, characterized in that, When the physicochemical properties of the silt are determined by both TO-type clay minerals and TOT-type clay minerals, the ratio of the cement to the silica fume is 1:(0.2~0.4). The ratio of cement to fly ash is 1:(0.2~0.4).

5. The high-flowability, non-dispersible, high-performance solidified silt soil for underwater use according to claim 1, characterized in that, According to the proportions, it includes the following components: 250-500 parts silt, 100-200 parts cement, 1-50 parts fly ash, 30-100 parts acrylic emulsion, 1-60 parts silica fume, 1-2 parts chitosan quaternary ammonium salt, and 1-2 parts powdered water-reducing agent.

6. A method for preparing high-flowability, non-dispersible, high-performance solidified silt soil for underwater applications as described in any one of claims 1 to 5, characterized in that, Includes the following steps: Step 1: Determine the physicochemical properties of the silt; Step 2: Add deionized water to chitosan quaternary ammonium salt to obtain chitosan quaternary ammonium salt solution; Step 3: Determine the part ratio of silt, cement, silica fume and fly ash based on the physicochemical properties of Step 1, weigh them, mix and stir until uniform to obtain dry material; Step 4: Mix the dry material obtained in Step 3 with the acrylic emulsion, and slowly add the powdered water-reducing agent and chitosan quaternary ammonium salt solution. Stir thoroughly until the cement is free of lumps and meets the expected fluidity.

7. The method for preparing high-flowability, non-dispersible, high-performance solidified silt soil for underwater use according to claim 6, characterized in that, The physicochemical properties of step one are determined by one or both of TO-type clay minerals or TOT-type clay minerals. The following methods were used for characterization and determination: 29 One of the following: Si-nuclear magnetic resonance, X-ray full-spectrum fitting, or thermogravimetric analysis.

8. The method for preparing high-flowability, non-dispersible, high-performance solidified silt soil for underwater applications according to claim 6, characterized in that, The preparation process of the chitosan quaternary ammonium salt solution in step two includes: Weigh out samples with a degree of substitution greater than 90% and a molecular weight higher than 4.8 × 10⁻⁶. 4 Chitosan quaternary ammonium salt was added to a reaction vessel, and deionized water was added; the mass ratio of the chitosan quaternary ammonium salt to deionized water was less than 1:

3. Stir at 120-180 rpm at 75-90°C until completely dissolved.

9. The method for preparing high-flowability, non-dispersible, high-performance solidified silt soil for underwater use according to claim 6, characterized in that, The solid content of the acrylate emulsion is 30-50%.

10. The method for preparing high-flowability, non-dispersible, high-performance solidified silt soil for underwater use according to claim 6, characterized in that, The stirring time in step four is 20-30 minutes.