Closure for a product-retaining container

A synthetic wine bottle closure with a thermoplastic core and styrene block copolymer layer addresses leakage, sealing, and appearance issues, offering improved security, recyclability, and reduced oxygen permeability, enhancing the wine preservation and aesthetic appeal.

WO2026233567A1PCT designated stage Publication Date: 2026-11-12VINVENTIONS SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2025/062784
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing synthetic wine bottle closures face challenges such as leakage, difficulty in achieving a secure seal, excessive extraction force, high oxygen permeability, and inadequate appearance similarity to natural cork, while also posing food safety concerns due to potential dye migration and material incompatibilities.

Method used

A synthetic closure comprising a core member made of thermoplastic polymer and a peripheral layer of styrene block copolymer with controlled density and thickness, ensuring a tight seal, low oxygen permeability, and improved adhesion, while minimizing material usage and maintaining appearance similarity to natural cork.

Benefits of technology

The closure provides enhanced leakage resistance, secure sealing, and ease of removal, with reduced oxygen transmission and improved recyclability, while maintaining aesthetic and tactile similarities to natural cork, addressing the limitations of prior art closures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2025062784_12112026_PF_FP_ABST
    Figure EP2025062784_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The disclosure relates to closure for a product-retaining container constructed for being inserted and securely retained in a portal forming neck of said container, said closure comprising at least a) a core member comprising at least one thermoplastic polymer, and b) at least one peripheral layer at least partially surrounding and intimately bonded to at least one surface of the core member, said peripheral layer comprising at least one styrene block copolymer, wherein the core member has a density in the range of from about 100 kg / m3 to 350 kg / m3 and the peripheral layer has a density in the range of from greater than 350 kg / m3 to about 1,500 kg / m3 and a thickness in the range of from 0.15 mm to less than 0.75 mm, characterized in that the at least one styrene block copolymer comprises a bound styrene content, determined according to ASTM D5775-95, of 1 wt.% to 30 wt.%, based on the overall weight of the at least one styrene block copolymer, and / or that the at least one peripheral layer has an overall styrene content of 0.1 wt.% to 10 wt.%, based on the overall weight of the at least one peripheral layer.
Need to check novelty before this filing date? Find Prior Art

Description

May 9, 2025CLOSURE FOR A PRODUCT-RETAINING CONTAINERTECHNICAL FIELD

[0001] The present disclosure relates to a closure for a product retaining container, to a method of preparing a closure for a product retaining container, to a closure that is obtainable by a method of the present disclosure, and to a use of the disclosed closure for sealingly closing a product-retaining container.BACKGROUND

[0002] In view of the wide variety of products that are sold for being dispensed from containers, particularly containers with round necks which define the dispensing portal, numerous constructions have evolved for container stoppers or closure means for the portals, including for example screw caps, stoppers, corks and crown caps, to name a few. Generally, products such as vinegar, vegetable oils, laboratory liquids, detergents, honey, condiments, spices, alcoholic beverages, and the like, have similar needs regarding the type and construction of the closure means used for containers for these products. However, wine sold in bottles represents the most demanding product in terms of bottle closure technology. In an attempt to best meet these demands, most wine bottle closures or stoppers have been produced from a natural material known as "cork."

[0003] While natural cork still remains a dominant material for wine closures, wine closures from alternative materials such as polymers have become increasingly popular over the last years, largely due to the shortage in high quality natural cork material and the awareness of wine spoilage as a result of “cork taint,” a phenomenon that is associated with natural cork materials. In addition, these closures from alternative materials such as polymers have the advantage that by means of closure technology, their material content and physical characteristics can be designed, controlled and fine-tuned to satisfy the varying demands that the wide range of different wine types produced throughout the world impose on closures.

[0004] One of the principal difficulties to which any bottle closure is subjected in the wine industry is the manner in which the closure is inserted into the bottle. Typically, the closure is placed in a jaw clamping member positioned above the bottle portal. The clamping member incorporates a plurality of separate and independent jaw members which peripherally surround the closure member and are movable relative to each other to compress the closure member to a diameter substantially less than its original diameter. Once the closure member has been fully compressed, a plunger moves the closure means from the jaws directly into the neck of the bottle, where the closure member is capable of expanding into engagement with the interior diameter of the bottle neck and portal, thereby sealing the bottle and the contents thereof.

[0005] In view of the fact that the jaw members are generally independent of each other and separately movable in order to enable the closure member to be compressed to the substantially reduced diameter, each jaw member comprises a sharp edge which is brought into direct engagement with the closure member when the closure member is fully compressed. Score lines are frequently formed on the outer surface of the closure member, which prevents a complete, leak-free seal from being created when the closure member expands into engagement with the bottle neck. This can occur, for example, if the jaw members of the bottling equipment are imperfectly adjusted or worn. Leakage of the product, particularly of liquid product, from the container can thus occur.

[0006] Thus, it is generally desirable that any bottle closure be able to withstand this conventional bottling and sealing method. Furthermore, many cork sealing members also incur damage during the bottling process, resulting in leakage or tainted wine.

[0007] A further issue in the wine industry is the general desirability that secure, sealed engagement of the stopper with the neck of the bottle be achieved quickly, if not virtually immediately after the stopper is inserted into the neck of the bottle. During normal wine processing, the stopper is compressed, as detailed above, and inserted into the neck of the bottle to enable the stopper to expand in place and seal the bottle. However, such expansion desirably occurs immediately upon insertion into the bottle since many processors tip the bottle onto its side or neck down after the stopper is inserted into the bottle neck, allowingBU / dp 240580WO 09 May 2025the bottle to remain stored in this position for extended periods of time. If the stopper is unable to rapidly expand into secure, intimate, frictional contact and engagement with the walls of the neck of the bottle, wine leakage can occur.

[0008] It is further desirable that the closure be removable from the bottle using a reasonable extraction force. Although actual extraction forces extend over a wide range, the generally accepted, conventional extraction force is typically below 100 pounds (445 Newtons).

[0009] In achieving a commercially viable stopper or closure, a careful balance must be made between secure sealing and providing a reasonable extraction force for removal of the closure from the bottle. Since these two characteristics are believed to be in direct opposition to each other, a careful balance must be achieved so that the stopper or closure is capable of securely sealing the product, in particular the wine in the bottle, preventing or at least reducing both leakage and gas transmission, while also being removable from the bottle without requiring an excessive extraction force.

[0010] Furthermore, it is generally desirable to effectively prevent or reduce oxygen from entering the bottle. Too much oxygen can cause the premature spoilage of wine. In fact, oxidation may occur over a period of time to render the beverage undrinkable. Thus, it is desirable that the closure has a low oxygen permeability in order to extend and preserve the freshness and shelf life of the product. Apart from reducing the oxygen permeability of the closure, additives that act as oxygen scavengers can be incorporated into the closure. Oxygen migrating through the closure is then quenched by the additive. A combination of a low oxygen permeability and oxygen scavengers inside the closure is particularly effective at reducing oxygen-mediated spoilage of wine. Any commercially viable wine stopper or closure should therefore generally have a low oxygen transfer rate (OTR).

[0011] Additionally, it is often desirable for synthetic closures to resemble natural cork closures as closely as possible in appearance. Both the longitudinal surface and the flat ends of cylindrical cork closures generally have an irregular appearance, for example showing naturally occurring irregularities in color, structure and profile. Methods have been developed for providing synthetic closures with a physical appearance similar to natural cork,BU / dp 240580WO 09 May 2025for example by blending colors to produce a streaking effect in the outer portion of the closure, along the cylindrical axis, or to provide the flat terminating ends of a synthetic closure with a physical appearance similar to natural cork.

[0012] It is, furthermore, often desirable to provide decorative indicia such as letters and ornaments on the surface of wine stoppers (e.g. the crest or emblem of a winery). Natural corks are generally marked by a method commonly referred to as “fire branding”, i.e. by the application of a hot branding tool. Alternatively, natural corks may also be branded by application of colors or dyes. Due to food safety concerns, marking of natural corks with colors or dyes is generally only effected on the curved cylindrical surface of the cork that is not in direct contact with the wine. On the other hand, marking on the flat terminating surfaces of natural corks is generally effected by means of fire branding only since this method does not impose any food safety concerns.

[0013] It is also known to brand synthetic closures. Synthetic closures are commonly branded by means of inkjet or offset printing using special dyes or colors approved for indirect food contact. Since such colors and dyes are normally not approved for direct food contact, marking of synthetic closures with colors or dyes is generally only effected on the curved cylindrical surface of the cork that is not in direct contact with the wine. Such marking can be on the outermost surface, or on an inner surface which is subsequently covered with an outer, preferably substantially transparent, layer. Marking on the flat terminating surfaces of synthetic closures is generally only known for injection molded closures, where marking is effected during the molding process of the closure by providing raised portions on the flat terminating surfaces.

[0014] Methods are available for marking the flat terminating surface of synthetic closures that have been manufactured by means of extrusion, in particular by co-extrusion. Laser marking may, in theory, be a feasible method since it allows the avoidance of direct food contact. This method is, however, inherently slow and expensive since it requires the use of special laser dye additives. Also, there have been concerns that laser marking of the flat terminating surfaces of synthetic closures may adversely change the foam structure of theBU / dp 240580WO 09 May 2025core element, which may, in consequence, adversely affect the sensitive gas permeation properties of such closures.

[0015] A further method involves the application of a decorative layer, in particular of a decorative plastic layer, by means of heat and / or pressure transfer. This method allows for permanent branding of synthetic closures without giving rise to concerns relating to food safety and without negatively impacting the gas permeation and / or mechanical properties of synthetic closures, in particular of co-extruded synthetic closures.

[0016] In addition to the above, it is also desirable, for economic and environmental reasons, to reduce the total amount of material in a synthetic closure. Since the size of the closure is determined by the size of the bottle neck, reducing the amount of material can principally be achieved by reducing the density of the closure, in particular of the core member, which is generally in the form of a foamed material comprising air- or gas-filled cells. However, reducing the density of the core member generally increases the deformability of the core member and thus of the synthetic closure, which in turn results in a worsened sealing capability and thus in increased leakage. In order to avoid this, a thicker and / or denser outer layer or skin is conceivable, as is the incorporation of a stiffer and / or denser central element within the core member. However, either of these approaches increases the total amount of material, thereby diminishing or even eliminating any advantages achieved by reducing the core density. WO 2013 / 182540 Al suggests reducing the amount of material by application of a core member comprising at least one thermoplastic polymer and at least one peripheral layer (outer layer or skin layer) at least partially surrounding and intimately bonded to the at least one surface of the core member, wherein the peripheral layer comprises at least one styrene block copolymer. Typical styrene block copolymer compounds as disclosed by their tradenames in WO 2013 / 182540 Al contain a high bound styrene content resulting in a high styrene content in the peripheral layer. In order to enhance the processing efficiency and flexibility of those styrene containing polymers, the polymers are often blended with oil (oil extended styrene block copolymers). Drawbacks are, however, that the oil might migrate to the surface of the peripheral layer, which may have a detrimental effect on print quality and / or cause the ink to adhere less efficiently to the surface. Additionally, the application of those styrene block copolymer compounds in closures being in contact with high alcoholBU / dp 240580WO 09 May 2025containing beverages might not be compatible with food safety considerations, since the colors might migrate into the beverages when in contact with the closure. Moreover, the high styrene content in the peripheral layer diminishes the recyclability of the closure.

[0017] Furthermore, it is also desirable that the peripheral layer (skin layer) has a good adhesion to the core layer, even though the skin layer has a low thickness. A good adhesion of the core layer to the peripheral layer reduces or even prevents so-called “lipping” during bottling, where, for example, if the closure is not perfectly centered, the edge of the closure can catch on the edge of the bottle rim and the peripheral layer is dragged and folded to form a “lip”. Notably, there is a correlation between leakage of the closure and thickness of the peripheral layer. Typically, lower leakage values should be achieved with increased peripheral layer thickness. However, increased peripheral layer thickness requires use of greater amounts of peripheral material increasing material consumption and hence cost and weight of the closure. It is thus desirable to provide a closure which shows a high leakage resistance and a good adhesion of the peripheral layer to the core layer, while maintaining the thickness of a peripheral layer to a minimum.

[0018] Therefore, there exists a need for a synthetic closure or stopper which particularly comprises at least one of the characteristic features described above, said synthetic closure or stopper having a physical appearance and / or tactile characteristics similar in at least one aspect to a natural cork closure, particularly with only minimal impairment, particularly with no impairment or even with improvement of the other properties of the closure such as, inter alia, OTR, leakage, ease of insertion and removal, compressibility and compression recovery, compatibility with food products.

[0019] Other and more specific needs will in part be apparent and will in part appear hereinafter.BU / dp 240580WO 09 May 2025SUMMARY

[0020] As will become evident from the following detailed disclosure, the synthetic closure of the present disclosure may be employed as a bottle closure or stopper for any desired product. However, for the reasons detailed above, wine products impose the most burdensome standards on a bottle closure. Consequently, in order to clearly demonstrate the universal applicability of the synthetic closure of the present disclosure, the following disclosure focuses on the applicability and usability of the synthetic closure of the present disclosure as a closure or stopper for wine containing bottles. However, this discussion is for exemplary purposes only and is not intended as a limitation of the present disclosure.

[0021] As discussed above, a bottle closure or stopper for wine must be capable of performing numerous separate and distinct functions. One principal function is the ability to withstand the pressure build up due to temperature variations during storage, as well as prevent any seepage or leakage of the wine from the bottle. Furthermore, a tight seal must also be established to prevent unwanted gas exchange between ambient conditions and the bottle interior, so as to prevent any unwanted oxidation or permeation of gases from the wine to the atmosphere. In addition, the unique corking procedures employed in the wine industry also impart substantial restrictions on the bottle closure, requiring a bottle closure which is highly compressible, has high immediate compression recovery capabilities and can resist any deleterious effects caused by the clamping jaws of the bottle closure equipment. Moreover, the closure should show an excellent printability and be suitable for use as a bottle closure or stopper for high alcohol containing beverages. In addition, the adhesion of the peripheral layer to the core of the synthetic cork should be high while maintaining the thickness of the peripheral layer to a minimum. Most importantly, the contained product, in this case wine, should not be spoiled by the closure. Hence, the closure should show an improved leakage resistance compared to the closures disclosed in the prior art.

[0022] Although prior art products have been produced in an attempt to satisfy the need for alternate bottle closures employable in the wine industry, such prior art systems have often been found lacking in one or more of the generally desirable aspects of a bottle closure for wine products. However, by employing the present disclosure, many of the prior artBU / dp 240580WO 09 May 2025disadvantages have been reduced or even obviated and an effective, easily employed, mass-produced closure has been realized.

[0023] In the present disclosure, many of the prior art disadvantages can be reduced or even overcome by achieving a synthetic closure for a product retaining container constructed for being inserted and securely retained in a portal forming neck of said container and a method for producing such a synthetic closure.

[0024] In one aspect the present disclosure provides for a closure for a product-retaining container constructed for being inserted and securely retained in a portal forming the neck of said closure comprising at leasta) a core member comprising at least one thermoplastic polymer, andb) at least one peripheral layer at least partially surrounding and intimately bonded to at least one surface of the core member, said peripheral layer comprising at least one styrene block copolymer,whereinthe core member has a density in the range of from about 100 kg / m3to 350 kg / m3, particularly in the range of from about 150 kg / m3to about 320 kg / m3, particularly in the range of from about 200 kg / m3to about 310 kg / m3, particularly in the range of from about 210 kg / m3to about 300 kg / m3, more particularly in the range of from about 220 kg / m3to about 290 kg / m3, more particularly in the range of from about 225 kg / m3to about280 kg / m3, and the peripheral layer has a density in the range of from greater than350 kg / m3to about 1,500 kg / m3, particularly in the range of from about 450 kg / m3to about 1,300 kg / m3, particularly in the range of from about 550 kg / m3to about 1,250 kg / m3, particularly in the range of from about 650 kg / m3to about 1,200 kg / m3, particularly in the range of from about 700 kg / m3to about 1,150 kg / m3, particularly in the range of from about 750 kg / m3to about 1,100 kg / m3and a thickness in the range of from 0.15 mm to less than 0.75 mm, particularly in the range of from about 0.20 mm to about 0.60 mm, particularly in the range of from about 0.25 mm to about 0.55 mm, more particularly in the range of from about 0.25 mm to about 0.50 mm, more particularly in the range of from about 0.30 mm to about 0.45 mm, more particularly in the range of from about 0.35 mm to about 0.45 mm, whereby exemplary thicknesses are about 0.15 mm, about 0.16 mm, about 0.17 mm, aboutBU / dp 240580WO 09 May 20250.18 mm, about 0.19 mm, about 0.20 mm, about 0.21 mm, about 0.22 mm, about 0.23 mm, about 0.24 mm, about 0.25 mm, about 0.26 mm, about 0.27 mm, about 0.28 mm, about 0.29 mm, about 0.30 mm, about 0.31 mm, about 0.32 mm, about 0.33 mm, about 0.34 mm, about 0.35 mm, about 0.36 mm, about 0.37 mm, about 0.38 mm, about 0.39 mm, about 0.40 mm, about 0.41 mm, about 0.42 mm, about 0.43 mm, about 0.44 mm, about 0.45 mm, about 0.46 mm, about 0.47 mm, about 0.48 mm, or about 0.49 mm, wherein the at least one styrene block copolymer comprises a bound styrene content of 1 wt.% to 30 wt.%, based on the overall weight of the at least one styrene block copolymer, and / or that the at least one peripheral layer has an overall styrene content of 0.1 wt.% to 10 wt.%, based on the overall weight of the at least one peripheral layer. The bound styrene content can be determined according to ASTM D5775-95, in particular according to ASTM D5775-95 (Reapproved 2023). Advantageous embodiments of the product-retaining container described hereinabove are described in the dependent claims 2 to 34.

[0025] The closure of the present disclosure comprises at least one peripheral layer at least partially surrounding and intimately bonded to at least one surface of the core member. The at least one peripheral layer is generally desirable in attaining a synthetic bottle closure which is suitable as a closure or stopper for the wine industry.

[0026] Due to the operation of the cooperating jaws which are employed to compress the stopper for insertion into the bottle, sharp edges of the jaw members are forced into intimate contact with the outer surface of the stopper. Prior art closures have been known to be incapable of resisting these cutting forces. As a result, longitudinal cuts, score lines or slits can be formed in the outer surface of the stopper, enabling liquid to seep from the interior to the exterior of the bottle. This disadvantage, existing with prior art cork and synthetic closures, can be reduced or even eliminated by incorporating at least one peripheral layer according to the present disclosure. In addition, by forming at least one peripheral layer as disclosed herein, the present disclosure provides a synthetic bottle closure which contributes to reducing or even overcoming the prior art disadvantages.BU / dp 240580WO 09 May 2025

[0027] It has surprisingly been found that a peripheral layer comprising a styrene block copolymer that comprises a bound styrene content, determined according to ASTM D5775-95, in particular ASTM D5775-95 (Reapproved 2023), of 1 wt.% to 30 wt.%, based on the overall weight of the at least one styrene block copolymer, and / or that the at least one peripheral layer has an overall styrene content of 0.1 wt.% to 10 wt.%, based on the overall weight of the at least one peripheral layer leads to superior properties of the closure in view of prior art synthetic closures. The low styrene content leads to good processability of the at least one styrene block copolymer even if the styrene block copolymer compound shows a low oil content, is essentially free of oil or processed without the addition of oil. Hence, the printability of the peripheral layer of the closure can be improved. Additionally, such a closure is suitable as a bottle closure for high alcohol containing beverages as the risk of fading of the colors printed on the peripheral layer of the closure decreases with decreasing amount of oil in the peripheral layer. Surprisingly it has further been found that a closure containing a peripheral layer comprising a styrene block copolymer that comprises a such a bound styrene content and / or that the at least one peripheral layer has an overall styrene content as described herein can lead to reduced leakage while there is no impairment or even improvement of the other properties of the closure such as, inter alia, OTR, ease of insertion and removal, compressibility and recovery force as well as skin adhesion. Thus, with the closure according to the invention an improved leakage resistance and a high adhesion of the peripheral layer to the core layer can be obtained, while maintaining the thickness of the peripheral layer to a minimum. In addition, the low bound styrene content and / or the low total styrene content in the peripheral layer may improve the recyclability of the peripheral layer. Particularly if the core member of the closure consists largely or entirely of polyethylene, the closure can be recycled as polyethylene material as long as the total styrene content in the closure (peripheral layer) is kept low. A higher styrene content may on the other hand interfere with the proper recycling of polyethylene.

[0028] According to an exemplary aspect of the present disclosure, a synthetic bottle closure is realized by a peripheral layer peripherally surrounding the core member in intimate, bonded, interengagement therewith. In an exemplary aspect of the present disclosure, the closure comprises a single peripheral layer comprising at least one styrene block copolymer. In further exemplary aspects of the present disclosure, the closure comprises two, three orBU / dp 240580WO 09 May 2025four peripheral layers, each or which peripherally surrounds the core member or a further peripheral layer in intimate bonded interengagement therewith. If two, three or four peripheral layers are comprised, at least one of these, optionally two, three or all of these, but in particular at least the outermost peripheral layer, comprises at least one styrene block copolymer. If two, three or four peripheral layers are comprised, at least one of these, optionally two, three or all of these, but in particular at least the outermost peripheral layer, comprises at least the density and thickness disclosed herein for the at least one peripheral layer.

[0029] The present disclosure particularly provides a closure having at least one peripheral layer, particularly an outermost peripheral layer, with a tough, score and mar resistant surface. In this respect, it is advantageous according to this aspect of the present disclosure that said at least one peripheral layer comprises a density in the disclosed ranges.

[0030] The thicknesses and densities disclosed for the at least one peripheral layer are capable of imparting desired physical characteristics, such as resistance to bottling conditions, to the closure of the present disclosure. The at least one peripheral layer, particularly the outer peripheral layer is, in particular, formed with a greater density than the inner core and with a selected thickness. The disclosed ranges have been found to be effective for a closure which is completely functional and achieves all of the desired goals. In particular, it has been found that by providing a closure with the disclosed features it is possible to reduce the density of the core member and also to reduce the thickness of the at least one peripheral layer compared to known synthetic closures, without impairment, and even with improvement, of desirable properties.

[0031] According to a particular aspect of the present disclosure, the at least one thermoplastic polymer of the core member is different to the at least one styrene block copolymer of the at least one peripheral layer. In particular, according to an exemplary aspect of the present disclosure the composition of the core member is different to the composition of the at least one peripheral layer. According to a particular aspect of the present disclosure, the core member does not comprise a styrene block copolymer or at least does not comprise the same styrene block copolymer as the at least one peripheral layer.BU / dp 240580WO 09 May 2025

[0032] The at least one styrene block copolymer of the peripheral layer comprises at least one block comprising, particularly based on, polymerized styrene monomer units. The at least one styrene block copolymer of the peripheral layer advantageously comprises at least two blocks, particularly at least three blocks, or at least four blocks, at least two of which, or at least three of which, optionally each of which are different from at least one, or at least two, or each of the other blocks comprised. It is possible that one type of block is repeated in the smallest repeating sequence of the block copolymer. Thus, for example, conceivable styrene block copolymers according to the present disclosure can have smallest repeating sequences such as AB, ABC, ABA, ABCD, ABCA, where A, B, C and D respectively represent blocks comprising, preferably based on, a polymer sequence having at least one respective same polymerized monomer unit. If one type of block is repeated in the smallest repeating sequence of the block copolymer, such as represented by block A in the above sequences ABA and ABCA, this repeating block is particularly a block comprising, particularly based on, polymerized styrene monomer units, in particular a block consisting of polymerized styrene monomer units. The respective monomer units are also referred to as repeating units or monomer repeating units. The respective blocks of the exemplary block copolymers can have any length, size or molecular weight, in particular can be based on any number of respective monomer repeating units, in particular can consist of any number of respectively the same monomer repeating units, to provide a block copolymer having properties suitable for imparting desired physical characteristics, such as, for example, resistance to bottling conditions, ease of extraction, and the like, to the closure of the present disclosure. The at least one styrene block copolymer can further be crosslinked, in particular by means of at least one of the monomer units of at least one of the respective blocks, or by a crosslinking agent which is different to the monomer units of the respective blocks, or by both.

[0033] The at least one styrene block copolymer of the peripheral layer can further be distinguished by its properties, such as, for example, hardness, softening point, melting point, molecular weight, purity, viscosity, particularly apparent viscosity, poly dispersity index, block length ratio, volume ratio, degree of crosslinking and the like.BU / dp 240580WO 09 May 2025

[0034] The at least one styrene block copolymer can have a tensile strength as determined by ASTM D412-16 of greater 5 MPa, in particular of greater 6 MPa or of greater 7 MPa, preferably of greater 8 MPa, more preferably of greater 9 MPa or of 10 MPa or greater. The application of a styrene block copolymer with the described tensile strength can lead to increased resilience of the synthetic cork. Since the closure is subjected to stress when inserted into the bottle or opened, a higher tensile strength might reduce the likelihood of cracking of breaking of the closure during these processes. Furthermore, a higher tensile strength could improve the adaptability of the closure to the container, in particular to the bottleneck. This can result in a higher leakage resistance and lower OTR. A lower tensile strength might on the other hand lead to lower leakage resistance and higher OTR.

[0035] The at least one styrene block copolymer has an elongation at break, also referred to as ultimate elongation as determined by ASTM D412-16 of greater 400 %, in particular of greater 500 % or of greater 600 %, preferably of greater 700 % or of greater 800 %, more preferably of greater 850 %. A higher elongation at break can result in a closure that can withstand more flexing and deformation without breaking. This can give the closure a greater ductility, i.e. better ability to conform to the shape of the container or bottle neck. This can be particularly important when inserting and removing the closure, making it easier to handle the filling process and for the costumer.

[0036] The at least one styrene block copolymer can have a hardness (Type A scale) as determined by ASTM D2240-15 of 20 to 85 shore A, in particular of 30 to 80 shore A, preferably of 40 to 75 shore A, more preferably 50 to 75 shore A or of 60 to 75 shore A. The application of a styrene block copolymer with the described hardness can lead to excellent behavior during insertion of the closure into the bottle neck of a wine bottle. A closure containing a styrene block copolymer with such a hardness in the peripheral layer shows good deformation behavior at impact and can thus be compressed prior to insertion into the bottle neck without being damaged by the compression jaws. A styrene block copolymer with a higher hardness might in contrast result in a less flexible closure which is less able to adapt to the bottleneck.BU / dp 240580WO 09 May 2025

[0037] According to a particular aspect of the present disclosure, the at least one styrene block copolymer is a radial styrene block copolymer. A radial styrene block copolymer can lead to improved processability of the styrene block copolymer facilitating the industrial production of the closure. Additionally, a radial styrene block copolymer can lead to improved color stability when being compared to a linear styrene block copolymer. The higher color stability can help to ensure that the appearance of the synthetic closure resembles that of a natural cork as closely as possible.

[0038] According to particular aspect of the present disclosure, the at least one peripheral layer contains an overall styrene content in the range of from 0, 1 wt.% to 9,8 wt.%, in particular from 0,2 wt.% to 9,5 wt.%, preferably from 0,5 wt.% to 9,2 wt.% or from 1 wt.% to 9 wt.%, more preferably from 1,5 wt.% to 8,5 wt.%, from 2 wt.% to8 wt.% or from 4 to 8 wt.%, based on the total weight of the at least one peripheral layer. The low styrene content can improve the softness of the peripheral layer leading to a high leakage resistance. On the other hand, a higher styrene content can lead to an increased stiffness of the peripheral layer. This can cause the cork to adapt less well to the bottle opening resulting in increased leakage and / or a higher OTR. In addition, a higher styrene content can lower the recyclability of the closure.

[0039] According to a particular aspect of the present disclosure, the at least one styrene block copolymer is a non-oil-extended (NOE) styrene block copolymer and / or the at least one styrene block copolymer is essentially oil free. Oil extended means that the styrene block copolymer is blended with oil. This is often the case to enhance the processing efficiency, especially if the styrene block copolymer shows no, or a low melt flow. Typical oils are mineral oils e.g. paraffin and naphthenic oils (white oils). The application of a non-oil extended styrene block copolymer can lead to enhanced printability of the peripheral layer. The absence of oil can increase the adhesion of the color on the outer surface of the peripheral layer. At the same time, color bleeding, especially in contact with beverages that have a high alcohol content, can be reduced or even prevented.

[0040] According to an exemplary aspect of the present disclosure, the peripheral layer is essentially oil free. When the term “essentially oil free” is used here or in any other context,BU / dp 240580WO 09 May 2025it refers to an oil content of less than 1 wt.%, preferably of less than 0,5 wt.%, based on the overall weight of the peripheral layer. Avoidance of oil can further increase the printability of the peripheral layer.

[0041] The at least one styrene block copolymer comprises blocks of polystyrene and blocks of one or more further polymer(s). It is possible to adjust the properties of the copolymer, like the softness / stiffness, melt flow rate, hardness, viscosity etc. by adjusting the bound styrene content and / or the styrene to rubber ratio. In an exemplary aspect of the present disclosure, the styrene block copolymer comprises a bound styrene content, determined according to ASTM D5775-95, of 2 % to 25 %, in particular of 3 % to 21 %, preferably of 5 % to 20 %, more preferably of 6 % to 18 % or of 8 % to 15 % and / or a styrene to rubber ratio, determined according to ASTM D5775, in particular according to ASTM D5775-95, of 1 / 99 to 30 / 70 or of 2 / 98 to 25 / 75, in particular of 3 / 97 to 21 / 79, preferably of 5 / 95 to 18 / 82, more preferably of 8 / 92 to 15 / 85. The number “95” in ASTM D5775-95 indicates the year of original adoption or, in the case of revision, the year of last revision. This standard was reapproved 2023. Hence, the standard can also be described as ASTM D5775-95 (Reapproved 2023). By way of example, if the styrene block copolymer is styrene ethylene butadiene styrene, the rubber ratio refers to the ratio of polystyrene to polyethylenbutadiene (PS : PEB). The bound styrene content and / or styrene to rubber ratio according to the invention results in a copolymer that shows a high softness, a good compatibility when being mixed with other polyolefins, allows the avoidance of process oil (or is non-oil extended) and can, however, be processed by extrusion. Thus, the styrene copolymer shows good processability and allows the production of a peripheral layer that shows good printability. A closure containing such a styrene copolymer in the peripheral layer can show a high leakage resistance due to the high softness of the styrene copolymer. Styrene block copolymers having a bound styrene content of more than 25% or a styrene to rubber ratio of more than 30 / 70 wt.%, as determined according to ASTM D5775, result in more stiff and less elastic materials compared to the styrene block copolymers having a bound styrene content in the exemplary range. In fact, processing oil or the application of oil-extended polystyrene copolymers might be necessary to enhance the softness of the polystyrene copolymer. Yet, this might lead to decreased printability and / or a lower leakage resistance.BU / dp 240580WO 09 May 2025

[0042] According to an exemplary aspect of the present disclosure, the at least one styrene block copolymer has a melt flow rate (MFR) as determined by ASTM DI 238-23 a (230 °C, 5 kg) of greater than 1 g / 10 min or of greater than 2 g / 10 min, in particular of greater than 5 g / 10 min, preferably of greater than 8 g / 10 min, more preferably of greater than lO g / lO min or of greater than 12 g / 10 min. In another exemplary aspect of the present invention, the melt flow rate (MFR) as determined by ASTM D1238-23a (230 °C, 5 kg) is lower than 50 g / 10 min, preferably between 1 g / 10 min to 50 g / 10 min, more preferably between 2 g / 10 min to 50 g / 10 min or between 5 g / 10 min to 50 g / 10 min and more preferably between 8 g / 10 min to 50 g / 10 min, 10 g / 10 min to 50 g / 10 min or 12 g / 10 min to 50 g / 10 min. A styrene block copolymer with the exemplary melt flow rate shows good processing behavior and can facilitate large scale production of the inventive closure. In contrast, a styrene block copolymer with a lower melt flow rate may not be processable by extrusion or may require the addition of additives such as oil to be extruded.

[0043] According to an exemplary aspect of the present disclosure, the at least one styrene block copolymer comprises at least one block comprising, particularly based on polymerized monomer units selected from the group consisting of monomer units which are copolymerizable to form a block copolymer with styrene or with a styrene-based polymer, in particular ethylenically unsaturated monomers, particularly selected from the group consisting of monoethylenically unsaturated monomers and diethylenically unsaturated monomers. The at least one styrene block copolymer can comprise, for example, in addition to at least one styrene block, at least one block based on polymerised ethylenically unsaturated monomer groups, for example at least one block based on polymerised monoethylenically unsaturated monomer groups, or at least one block based on polymerised diethylenically unsaturated monomer groups, or at least one block based on polymerised monoethylenically unsaturated monomer groups and at least one block based on polymerised diethylenically unsaturated monomer groups. Examples of preferred further blocks, in addition to at least one styrene block, are blocks comprising, preferably based on polymerized monomer units selected from the group consisting of olefins, acrylates or methacrylates, in particular olefins, in particular olefins selected from the group consisting of C2-, C3-, C4-, C5-and / or Ce-olefins, in particular selected from the group consisting of C2-, C3-, C4-, C5- and Ce-olefins which are monoethylenically unsaturated and C2-, C3-, C4-, C5- and Ce-olefinsBU / dp 240580WO 09 May 2025which are diethylenically unsaturated. Exemplary monomer units are ethylene, propylene, 1-butylene, cis-2-butene, trans-2-butene, isobutylene, 1,3 -butadiene, 1-pentylene, cis-2-pentene, trans-2-pentene, 2-methylbut-l-ene, 3-methylbut-l-ene (isopentene), 2-methylbut-2-ene (isoamylene), 1,3 -pentadiene (piperylene), 1,4-pentadiene, 2-methyl- 1,3 -butadiene (isoprene), 1-hexene, 2-hexene, 3-hexene, 2-methyl- 1 -pentene, 2-methyl-2-pentene, 3-m ethyl- 1 -pentene, 3-methyl-2-pentene, 4-methyl-l -pentene, 4-methyl-2-pentene, 2-ethyl-l-butene, 2,3-dimethyl-l-butene, 2,3-dimethyl-2-butene, 3,3-dimethyl-l-butene, 1,3-hexadiene, 1,4-hexadiene, 1,5-hexadiene, 2-methylpenta-l,3-diene, 2-methylpenta-l,4-diene, 3-methylpenta-l,3-diene, 3 -m ethylpenta- 1,4-diene, 2-ethyl- 1,3 -butadiene, 2,3-dimethyl- 1,3 -butadiene, as well as isomers thereof, in particular cis-isomers and transisomers.

[0044] If the monomer units should also act as crosslinkers these monomer units can comprise further groups and / or substituents which are capable of providing a crosslinking functionality, for example further groups which are copolymerizable with at least one repeating unit of at least one block, or which can form associations by means of weaker forces such as hydrogen bonding or Van der Waals forces, for example ethylenically unsaturated groups, carbonyl groups, hydroxyl groups, cationic groups, such as quaternary ammonium groups, anionic groups such as C(O)O' and the like. The at least one styrene block copolymer may be hydrogenated.

[0045] According to an exemplary aspect of the present disclosure, the at least one styrene block copolymer is selected from the group consisting of styrene ethylene butadiene styrene block copolymers, styrene ethylene butylene styrene block copolymers, styrene ethylene butylene block copolymers, styrene butadiene styrene block copolymers, styrene butadiene block copolymers, styrene isoprene styrene block copolymers, styrene isobutylene block copolymers, styrene isoprene block copolymers, styrene ethylene propylene styrene block copolymers, styrene ethylene propylene block copolymers and combinations of two or more thereof, preferably of styrene ethylene butylene styrene block copolymers or styrene ethylene butadiene styrene block copolymers. Examples of commercially available styrene block copolymers according to the present disclosure areBU / dp 240580WO 09 May 2025SBS, SIS, SEBS, SIBS, SEPS, SEEPS or MBS. Preferably, the at least one block copolymer is a styrene ethylene butylene styrene block copolymer (SEBS).

[0046] According to one aspect of the present disclosure, the at least one styrene block copolymer is essentially free of antioxidants.

[0047] It is possible for the at least one peripheral layer to consist of at least one styrene block copolymer, in particular to consist of one of the styrene block copolymers mentioned herein. In a particular aspect of the closure according to the present disclosure, the at least one styrene block copolymer is present in an amount in the range of from 0,1 wt.% to 100 wt.%, in particular from 5 wt.% to 95 wt.%, preferably from 10 wt.% to 90 wt.%, more preferably from 25 wt.% to 85 wt.% or from 35 wt.% to 75 wt.%, based on the total weight of the peripheral layer.

[0048] It is also possible for the at least one peripheral layer to consist of a combination of two or more of the styrene block copolymers mentioned herein. It can further be advantageous, for example in terms of cost, weight, processability, or properties of the at least one peripheral layer, to combine the at least one styrene block copolymer with at least one further polymer, in particular with at least one further olefinic polymer.

[0049] According to a particular aspect of the closure according to the present disclosure, therefore, the peripheral layer further comprises at least one further polymer or copolymer which is different to the at least one styrene block copolymer.

[0050] According to a further aspect of the present disclosure, the at least one further polymer or copolymer is a thermoplastic elastomer.

[0051] According to an exemplary aspect of the closure of the present disclosure, therefore, the at least one further polymer or copolymer is particularly selected from the group consisting of polyolefins, polyurethanes, polyamides, copolyesters, vulcanizates, in particular thermoplastic polyolefins, thermoplastic polyurethanes, thermoplastic polyamides, thermoplastic copolyesters and thermoplastic vulcanizates, preferably thermoplasticBU / dp 240580WO 09 May 2025polyolfins. In particular, the at least one peripheral layer can comprise one or more materials selected from foamable thermoplastic polyurethanes, non-foamable thermoplastic polyurethanes, thermoplastic olefins, thermoplastic vulcanizates, EPDM rubber, polyolefins, olefin block copolymers, particularly flexible polyolefins, particularly polyethylenes and polypropylenes, particularly metallocene polyethylenes and polypropylenes, fluoroelastomers, fluoropolymers, fluorinated polyolefins, particularly partially fluorinated or perfluorinated polyethylenes, particularly polytetrafluoroethylenes, olefin block copolymers, polyether-type polyurethanes and mixtures or blends thereof. Particular examples of the at least one further polymer or copolymer for the at least one peripheral layer are polyethylene, particularly metallocene polyethylene, polypropylene, particularly metallocene polypropylene, EPDM rubber, styrene butadiene block copolymers, and mixtures or blends thereof. The terms “metallocene polyethylene” and “metallocene polypropylene” respectively are intended to mean polyethylene and polypropylene obtained by metallocene-catalyzed polymerization. If desired, the material of the at least one peripheral layer is substantially transparent. Furthermore, the at least one further polymer selected for the at least one peripheral layer may be different from the material of the core member.

[0052] In order to form synthetic bottle closures with all of the desirable inherent physical and chemical properties detailed above, it hast been found advantageous to comprise at least one thermoplastic polyolefin, particularly selected from the group consisting of thermoplastic polyolefins, olefin block copolymers and polyolefin plastomers. In particular, the at least one thermoplastic polyolefin can be selected from the group consisting of polyethylene and copolymers of ethylene with one or more further olefins, for example with propylene, butylene, pentylene, hexane, hexene, heptane, octene, nonene, decene, undecylene or dodecylene. As detailed herein, the at least one peripheral layer may comprise at least one further polymer or copolymer, particularly at least one thermoplastic polyolefin as described herein as at least one further polymer or, if desired, the thermoplastic polyolefin may be combined with one or more thermoplastic elastomers, particularly with one or more thermoplastic elastomers as detailed above, as at least one further polymer. In this regard, it has been found advantageous that the at least one peripheral layer particularly comprises one a medium density polyethylene, a medium low-density polyethylene, a low-densityBU / dp 240580WO 09 May 2025polyethylene or an ethylene copolymer, preferably a low-density polyethylene or an ethylene butylene copolymer. If the at least one peripheral layer comprises at least one thermoplastic polyolefin, this is preferably comprised in an amount in the range of from range of 1 wt.% to about 99 wt.%, particularly in an amount in the range of from about 5 wt.% to about 95 wt.%, particularly in an amount in the range of from about 10 wt.% to about 90 wt.%, particularly in an amount in the range of from about 12 wt.% to about 85 wt.%, particularly in an amount in the range of from about 15 wt.% to about 80 wt.%, particularly in an amount in the range of from about 20 wt.% to about 65 wt.%, particularly in an amount in the range of from about 20 wt.% to about 60 wt.%, particularly in an amount in the range of from about 25 wt.% to about 55 wt.%, particularly in an amount in the range of from about 28 wt.% to about 52 wt.%, based on the total weight of the peripheral layer. The weight percent ratio of styrene block copolymer to thermoplastic polyolefin can be in the range of from 100 : 0 to 99,9 : 0,1, in particular in the range of from 1 : 99 to 99 : 1, or in the range of from 5 : 95 to 95 : 5, or in the range of from 10 : 90 to 90 : 10, or in the range from 40: 60 to 80 : 20, or in the range of from 45 : 55 to 75 : 25, or in the range from 48 : 52 to 72 : 28. Exemplary weight percent rations of styrene block copolymer to thermoplastic polyolefin are 99 : 1, 98 : 2, 98 : 2, 97 : 3, 96 : 4, 95 : 5, 94 : 6, 93 : 7, 92 : 8, 91 : 9, 90 : 10, 89 : 11, 88 : 12, 87 : 13, 86 : 14, 85 : 15, 84 : 16, 83 : 17, 82 : 18, 81 : 19, 80 : 20, 75 : 25, 70 : 30, 65 : 35, 60 : 40, 55 : 45, 50 : 50, 45 : 55, 60 : 40. It has been found that combining at the least one styrene block copolymer with at least one polyolefin, for example a polyethylene or a polyethylene copolymer, can improve the adhesion of the at least one peripheral layer to the core and improve the diameter recovery, i.e. the speed and extent of expansion of the cork diameter after release from compression, for example compression during bottling. Additionally, it has been found that combining at the least one styrene block copolymer with at least one polyolefin can improve the leakage resistance of the closure.

[0053] The adhesion of the peripheral layer to the core can be determined by measuring the force necessary to peel off a strip of the peripheral layer which is attached to the core. A larger peeling force indicates a better adhesion. In an exemplary aspect of the present disclosure the closure has an adhesion of the at least one peripheral layer to the core member (skin-core adhesion) according to the herein described test method of at least 9,5 N, particularly of at least 10,0 N or of at least 10,8 N, preferably of at least 11,0 N or of at leastBU / dp 240580WO 09 May 202511,5 N, more preferably of at least 11,8 N or of at least 12 N. In an exemplary aspect, the adhesion (skin-core adhesion) measured in this way according to the herein described test method lies in the range of from about 9,5 N to about 16,0 N or from about 10,0 N to about 15,9 N, particularly in the range of from about 10,8 N to about 15,8 N or from about 11,0 N to about 15,7 N, preferably in the in the range of from about 11,5 N to about 15,6 N or from about 11,8 N to about 15,5 N, more preferably in the range of 12,0 to about 15,5 N. A better adhesion of the peripheral layer to the core reduces or even prevents so-called “lipping” during bottling, where, for example, if the closure is not perfectly centered, the edge of the closure can catch on the edge of the bottle rim and the peripheral layer is dragged and folded to form a “lip”. Hence, a lower skin-core adhesion bears a higher risk of “lipping”.

[0054] The recovery force can be measured by compressing the closure to a diameter of 15.7 mm in bottling jaws mounted on a compression / traction bench. In a first step, the force to be applied by the apparatus on the jaws to compress the closure is measured. The jaws are then opened to a diameter of 18.5 mm and the force to compensate for the compression of the rebounding closure (= recovery force) is measured. In an exemplary aspect of the present disclosure, the closure has a recovery force determined on hour after bottling according to the herein described test method of about 200 N to about 400 N, particularly of about 220 N to about 380 N, preferably of about 250 N to about 360 N, more preferably of about 260 to about 350 N. The recovery force can be linked to the elasticity and of the stiffness of the closure. While the elasticity of the closure is mostly influenced by the core member (e.g. its density and cell size), the peripheral layer has bigger influence on the stiffness of the closure. A closure with a recovery force as described above shows an excellent balance between elasticity and stiffness. Hence, a closure can be produced that allows for good processability in terms of insertion into the neck of a wine bottle and has a high leakage resistance and low OTR.

[0055] Another formulation which has been found to be highly effective in providing a peripheral layer comprises at least one thermoplastic polyolefin elastomer as at least one further polymer.BU / dp 240580WO 09 May 2025

[0056] Another formulation which has been found to be highly effective in providing a peripheral layer which provides at least one, particularly more than one, particularly almost all or even all physical and chemical attributes to attain a commercially viable closure comprises at least one of at least one polyethylene and at least one olefin block copolymer or a blend of at least two thereof as at least one further polymer or copolymer.

[0057] In the exemplary construction of this embodiment, the particular polyethylene which can be employed as at least one further polymer for forming the at least one peripheral layer comprises a low-density polyethylene (LLDPE), preferably LLDPE 6118 NSF, manufactured by SABIC®. This compound has been found to produce an outer layer in combination with at least one styrene block copolymer which provides at least one, particularly more than one, particularly almost all or even all of the physical and chemical characteristics suitable for attaining a highly effective closure for the wine industry.

[0058] In another exemplary construction of this embodiment, the particular thermoplastic polyolefin elastomer (POE) which can be employed as at least one further polymer for forming the at least one peripheral layer comprises an ethylene- 1 -butene copolymer, preferably LUCENE™ LC575, manufactured by LG Chem. This compound has been found to produce an outer layer in combination with at least one styrene block copolymer which provides at least one, particularly more than one, particularly almost all or even all of the physical and chemical characteristics suitable for attaining a highly effective closure for the wine industry.

[0059] Still further additional compounds which have been found to provide highly effective peripheral layers for forming closures, as further polymer or further copolymer in accordance with the present disclosure, comprise teflon, fluoroelastomeric compounds and fluoropolymers. These compounds, whether employed individually or in combination with each other or with the other compounds detailed above have been found to be highly effective as further polymer or further copolymer in producing a peripheral layer which is capable of providing at least one, particularly more than one, particularly almost all or even all of the properties making it suitable for synthetic bottle closures.BU / dp 240580WO 09 May 2025

[0060] In principle, any of the compounds detailed herein as at least one further polymer and at least one further copolymer for providing the at least one peripheral layer can be comprised singly or in combination with each other, in combination or not in combination with at least one styrene block copolymer, particularly in the weight ratios indicated herein, to produce a peripheral layer which is securely and integrally bonded to the core member and / or to a different peripheral layer, as a foamed outer layer or a non-foamed outer layer, or as an intermediate layer. Independent of the selection of the material for the at least one further polymer and / or at least one further copolymer, the properties of the closure such as diameter recovery and adhesion of the peripheral layer to the core as described herein are considered as exemplary aspects of the closures according to the present disclosure.

[0061] In an exemplary aspect of the closure according to the present disclosure, the at least one styrene block copolymer is present in an amount in the range of from about 0.1 wt.% to about 100 wt.%, particularly in an amount in the range of from about 1 wt.% to about 99 wt.%, particularly in an amount in the range of from about 5 wt.% to about 95 wt.%, particularly in an amount in the range of from about 10 wt.% to about 90 wt.%, particularly in an amount in the range of from about 15 wt.% to about 88 wt.%, particularly in an amount in the range of from about 20 wt.% to about 85 wt.%, particularly in an amount in the range of from about 25 wt.% to about 85 wt.%, particularly in an amount in the range of from about 30 wt.% to about 85 wt.%, particularly in an amount in the range of from about 35 wt.% to about 80 wt.%, particularly in an amount in the range of from about 35 wt.% to about 75 wt.%, particularly in an amount in the range of from about 40 wt.% to about 75 wt.% or from about 48 wt.% to about 72 wt.% and the at least one further polymer and / or at least one further copolymer is or are present in an amount in the range of from 0 wt.% to about 99.9 wt.%, particularly in an amount in the range of from 1 wt.% to about 99 wt.%, particularly in an amount in the range of from about 5 wt.% to about 95 wt.%, particularly in an amount in the range of from about 10 wt.% to about 90 wt.%, particularly in an amount in the range of from about 12 wt.% to about 85 wt.%, particularly in an amount in the range of from about 15 wt.% to about 80 wt.%, particularly in an amount in the range of from about 20 wt.% to about 65 wt.%, particularly in an amount in the range of from about 20 wt.% to about 60 wt.%, particularly in an amount in the range of from about 25 wt.% to about 55 wt.%, particularly in an amount in the range of from about 28 wt.% to about 52 wt.%, inBU / dp 240580WO 09 May 2025each case based on the total weight of the at least one styrene block copolymer and the at least one further polymer and / or the at least one further copolymer. The amounts and ranges can be selected depending on criteria such as the desired properties of the peripheral layer, the desired properties of the closure, whether the at least one peripheral layer is the outermost peripheral layer or an inner peripheral layer, or whether it is intended to print on the peripheral layer. According to an aspect of the present disclosure, it can be advantageous if the at least one styrene block copolymer is present in an amount in the range of from about 25 wt.% to about 80 wt.%, or in an amount in the range of from about 30 wt.% to about 80 wt.%, particularly in an amount in the range of from about 35 wt.% to about 80 wt.%, particularly in an amount in the range of from about 40 wt.% to about 80 wt.%, particularly in an amount in the range of from about 45 wt.% to about 74 wt.%, particularly in an amount in the range of from about 50 wt.% to about 70 wt.%, and the at least one further polymer and / or at least one further copolymer is or are present in an amount in the range of from about 10 wt.% to about 80 wt.%, in an amount in the range of from about 15 wt.% to about 75 wt.%, particularly in an amount in the range of from about 20 wt.% to about 70 wt.%, particularly in an amount in the range of from about 25 wt.% to about 65 wt.%, particularly in an amount in the range of from about 25 wt.% to about 60 wt.%, particularly in an amount in the range of from about 25 wt.% to about 55 wt.%, in each case based on the total weight of the at least one styrene block copolymer and the at least one further polymer and / or the at least one further copolymer. These ranges have been found to be advantageous for reasons of cost, or, for example, if it is intended to print on the peripheral layer, for example by means of in-line printing. In these ranges an advantageous print quality can be achieved substantially without loss of other advantageous properties such as resistance to bottling conditions and ease of extraction. Additionally, these ranges allow a high skin adhesion (skin-core adhesion) and a high leakage resistance. Hence, by using these ranges a closure can be achieved with improved resistance to bottling conditions, without disadvantageously affecting other advantageous properties of the closure, such as ink adhesion, appearance and efficiency of printing or OTR. Exemplary wt.% ratios of the at least one styrene block copolymer to the at least one further polymer and / or the at least one further copolymer are 95 : 5, 90 : 10, 85 : 15, 80 : 20, 75 : 25, 70 : 30, 65 : 35, 60 : 40, 55 : 45, 50 : 50, based on the total weight of theBU / dp 240580WO 09 May 2025at least one styrene block copolymer and the at least one further polymer and / or the at least one further copolymer.

[0062] A composition that has been found to be highly effective in providing at least one, particularly more than one, particularly almost all or even all of the desirable attributes for at least one peripheral layer is a composition comprising as components at least one thermoplastic olefin and at least one styrene butadiene block copolymer. In the exemplary aspect, the blend of at least one thermoplastic olefin and at least one styrene butadiene block copolymer comprises the thermoplastic olefin in an amount in the disclosed ranges, based upon the weight of the at least one thermoplastic olefin and at least one styrene butadiene block copolymer in the composition. The construction of a closure using a peripheral layer formed from this blend provides a closure which is highly suitable for use as a wine bottle closure. In a particular exemplary aspect of the present disclosure, the at least one thermoplastic olefin is thermoplastic polyolefin elastomer, in particular an ethylene- 1 -butene copolymer or a polyethylene, in particular a linear low-density polyethylene. In an exemplary aspect of the disclosure, the at least one peripheral layer comprises as styrene butadiene block copolymer SEBS or SEPS and as at least one further thermoplastic polyolefin elastomer. The composition can be used in the form of a mixture which is formed by simple mixing of the components of the composition prior to forming the peripheral layer, or in the form of a blend which is formed by combining and heating the components substantially at the point of forming the peripheral layer.

[0063] By employing the materials disclosed herein as at least one further polymer or copolymer in combination with at least one styrene block copolymer and forming the combined material in peripheral, surrounding, bonded engagement with any desired foamed core member, a highly effective, multi-layer closure is attained which is able to provide at least one, particularly more than one, particularly almost all or even all properties suitable for a wine bottle closure.

[0064] The at least one peripheral layer, particularly the outer peripheral layer particularly comprises a thickness and a density which are capable of imparting desired physical characteristics, such as resistance to bottling conditions, to the closure produced by theBU / dp 240580WO 09 May 2025method of the present disclosure. The at least one peripheral layer, particularly the outer peripheral layer is, in particular, formed with a greater density than the inner core, particularly with a substantially greater density than the inner core, and with a selected thickness as disclosed. The exemplary thickness of the at least one peripheral layer can be selected according to criteria such as, for example, the composition, physical properties and / or density of the material of the at least one peripheral layer, the composition, physical properties and / or density of the material of the at least one peripheral layer, and the desired properties of the at least one peripheral layer. It has surprisingly been found that by using the present disclosure it is possible to provide a closure with the same or even improved properties compared to known closures, but with reduced amounts of material. It has been found, for example, that the same or even better properties are achieved, even with a lower density of the core member, and / or with a thinner peripheral layer, compared to known closures.

[0065] The present disclosure particularly provides a closure having a peripheral layer with a tough, score and mar resistant surface. This particularly improves the resistance to bottling conditions.

[0066] Depending upon the sealing process to be employed for inserting the synthetic closure produced by the method of the present disclosure in a desired bottle, additives, such as slip additives, lubricating agents, and sealing compounds may be comprised in at least one peripheral layer of the synthetic closure produced by the method of the present disclosure, for example to provide lubrication of the synthetic closure during the insertion process. In addition, other additives typically employed in the bottling industry may also be incorporated into the synthetic closure produced by the method of the present disclosure for improving the sealing engagement of the synthetic closure with the bottle as well as reducing the extraction forces necessary to remove the synthetic closure from the bottle for opening the bottle.

[0067] Advantageously, the closure according to the present disclosure has an extraction force determined one hour after bottling according to the herein described test method of not more than about 450 N, particularly of not more than about 400 N, particularly of not more than about 350 N, particularly of not more than about 300 N, particularly of not more than about 280 N, particularly of not more than about 250 N, particularly of not more than aboutBU / dp 240580WO 09 May 2025240 N, particularly of not more than about 230 N, particularly of not more than about 220 N, more particularly of not more than about 210 N, more particularly of not more than about 200 N, whereby the extraction force is in the range of from about 100 N to about 450 N, particularly in the range of from about 110N to about 400 N, particularly in the range of from about 130 N to about 300 N, particularly in the range of from about MON to about 200 N, particularly in the range of from about 150 N to about 190 N are advantageously achieved. The extraction force describes the force needed to remove a closure from a container, in particular from a bottle, under standardized conditions. A lower extraction force relates to a greater ease of extraction of the closure. An extraction force in the range of from about 100 N to about 450 N is generally considered acceptable for a wine bottle closure. It is surprising that the present disclosure achieves improved properties such as reduced leakage, while maintaining extraction force within the range considered acceptable for wine bottle closures.

[0068] The closure according to the present disclosure advantageously has an oxygen transfer rate (OTR) in axial direction of from about 0.0001 to about 0.1000 cc / day / closure, in particular from about 0.0005 to about 0.050 cc / day / closure. Methods to precisely measure the oxygen transfer rate (OTR) are known to the person skilled in the art. Detailed description of oxygen measurement technologies and protocols can be found, for example, in Dieval J-B., Vidal S. and Aagaard O., Packag. Technol. Sci. 2011; DOI: 10.1002 / pts.945. Preferably, the oxygen transfer rate (OTR) is measured by Mocon measurement, e.g. by the Mocon Ox-tran® method (Mocon Inc., Minneapolis, USA). This method is widely applied and recommended in different standards. More preferably, the oxygen transfer rate (OTR) is measured by Mocon measurement according to ASTM F-1307 using 100% oxygen, in particular according to ASTM F-1307-02 (2007). Another suitable method to measure the oxygen transfer rate is by a non-destructive technique known as Nomasense® technology. This method allows measurement of OTR through the closure by luminescence-based technology using separate sensors supplied by PreSens® (Precision Sensing GmbH, Regensburg, Germany). A detailed description of this method can be found in Dieval J-B., Vidal S. and Aagaard O., Packag. Technol. Sci. 2011; DOI: 10.1002 / pts.945.BU / dp 240580WO 09 May 2025

[0069] In an advantageous aspect of the closure according to the present disclosure, the closure has a leakage value measured according to the herein described test method of not more than 500 mm2, particularly of not more than 200 mm2or less, preferably of not more than 100 mm2, more preferably of not more than 80 mm2. The leakage value mm2, in particular of not more than 450 mm2, in particular of not more than 350 mm2, in particular of not more than 300 mm2, in particular of not more than 200 mm2, in particular of not more than 150 mm2, particularly of not more than 100 mm2, in particularly of not more than 80 mm2, in particularly of not more than 50 mm2, provides a measure of the amount of liquid which leaks from a bottle immediately after insertion of the closure using standard bottling equipment which has been adjusted to mimic wear observed on industrial bottling machines after many hours of working, in particular many hours of working without proper maintenance. The leakage value is therefore related to the resistance of the closure to bottling conditions. A lower leakage value indicates a better resistance of the closure to bottling conditions. A leakage value of 0 mm2represents the lowest possible leakage value which can be obtained and indicates that no leakage occurs under the test conditions. Alternative lower limits for the leakage value are, for example, 1 mm2, 2 mm2, 3 mm2, 4 mm2, 5 mm2, 6 mm2, 7 mm2, 8 mm2, 9 mm2, 10 mm2, 15 mm2, 20 mm2, 25 mm2, 30 mm2, 35 mm2, 40 mm2, 45 mm2, 50 mm2, 55 mm2, 60 mm2, 65 mm2, 70 mm2, 75 mm2, 80 mm2, 85 mm2, 90 mm2, 95 mm2, 100 mm2, 110 mm2, 120 mm2, 130 mm2, 140 mm2, 150 mm2, 160 mm2, 170 mm2, 180 mm2or 190 mm2. The particular lower limits can be combined with any of the particular upper limits to form a range of advantageous leakage values. It is expected that better resistance to bottling conditions, for example lower leakage values, should be achieved with increased peripheral layer thickness. However, increased peripheral layer thickness requires use of greater amounts of peripheral layer material, increasing both cost and weight of a closure. Surprisingly, with the closures disclosed herein it is possible to achieve improved resistance to bottling conditions, in particular as measured by low leakage values, with peripheral layers which have the same thickness or are even thinner than peripheral layers in known closures. More surprisingly, it is even possible to achieve good or even improved resistance to bottling conditions, in particular as measured by low leakage values, with a combination of a low core density and a thin peripheral layer or layers compared to known closures.BU / dp 240580WO 09 May 2025

[0070] It is expected that better resistance to bottling conditions, for example lower leakage values, should be achieved with increased density of a closure, in particular with increased density of the core member. For example, increased density of the closure, in particular increased density of the core member, generally results in a stiffer or firmer closure which better resists deformation during bottling and better recovers from the compression which occurs during bottling. It has, however, been found that closures according to the present disclosure have improved or at least not worsened resistance to bottling conditions even with lower densities of the closure, in particular lower densities of the core member, compared to known closures with higher densities, in particular higher densities of the core member.

[0071] The closure according to the present disclosure can thus advantageously be defined in that the core member has a density in the range of from about 100 kg / m3to less than 235 kg / m3, in particular a density in the range of from about 150 kg / m3to less than 235 kg / m3, in particular a density in the range of from about 200 kg / m3to less than 235 kg / m3, in particular a density in the range of from about 210 kg / m3to less than 235 kg / m3, in particular a density in the range of from about 220 kg / m3to less than 235 kg / m3, in particular a density in the range of from about 225 kg / m3to less than 235 kg / m3, and the closure has a leakage value measured according to the herein described test method of not more than 500 mm2, in particular of not more than 400 mm2, in particular of not more than 350 mm2, in particular of not more than 300 mm2, in particular of not more than 250 mm2, in particular of not more than 200 mm2, in particular of not more than 150 mm2, in particular of not more than 100 mm2, in particular of not more than 80 mm2, in particular of not more than 50 mm2, in particular in a range of from about 0 mm2to about 400 mm2, in particular in a range of from about 0 mm2to about 300 mm2, in particular in a range of from about 0 mm2to about 250 mm2, in particular in a range of from about 0 mm2to about 200 mm2; in particular in a range of from about 0 mm2to about 150 mm2; in particular in a range of from about 0 mm2to about 100 mm2, in particular in a range of from about 0 mm2to about 80 mm2, in particular in a range of from about 0 mm2to about 50 mm2; or in that the core member has a density in the range of from 235 kg / m3to 280 kg / m3, in particular a density in the range of from about 236 kg / m3to 280 kg / m3, and the closure has a leakage value measured according to the herein described test method of not more than 200 mm2, in particular of not more than 180 mm2, in particular of not more than 150 mm2, inBU / dp 240580WO 09 May 2025particular of not more than 100 mm2, in particular of not more than 80 mm2, in particular of not more than 50 mm2, in particular in a range of from about 0 mm2to 200 mm2, in particular in a range of from about 0 mm2to about 150 mm2, in particular in a range of from about 0 mm2to about 100 mm2, in particular in a range of from about 0 mm2to about 80 mm2, in particular in a range of from about 0 mm2to about 50 mm2; or in that the core member has a density in the range of from greater than 260 kg / m3to 350 kg / m3, in particular a density in the range of from about 261 kg / m3to 330 kg / m3, in particular a density in the range of from about 261 kg / m3to 320 kg / m3, in particular a density in the range of from about 261 kg / m3to 310 kg / m3, and the closure has a leakage value measured according to the herein described test method of not more than 100 mm2, in particular of not more than 80 mm2, in particular of 70 mm2or less, in particular of not more than 60 mm2, in particular of not more than 50 mm2, in particular of 40 mm2or less, in particular of 30 mm2or less, in particular of 20 mm2or less, in particular of 10 mm2or less, in particular in a range of from 0 mm2to 100 mm2, in particular in a range of from about 0 mm2to about 80 mm2, in particular in a range of from about 0 mm2to about 70 mm2, in particular in a range of from about 0 mm2to about 60 mm2, in particular in a range of from about 0 mm2to about 50 mm2, in particular in a range of from about 0 mm2to about 40 mm2, in particular in a range of from about 0 mm2to about 30 mm2, in particular in a range of from about 0 mm2to about 20 mm2, in particular in a range of from about 0 mm2to about 10 mm2.

[0072] In an advantageous aspect of the closure according to the present disclosure, the core member comprises a plurality of cells. Such a plurality of cells is generally achieved in a foamed material, also referred to as a foam or as a foamed plastic. The closure according to the present disclosure particularly comprises at least one foamed material. In a particular aspect of the method, the core material comprises a foamed material. The peripheral layer can also comprise an at least partially foamed material. However, the at least one peripheral layer is formed with a substantially greater density than the core material, in order to impart desired physical characteristics to the synthetic bottle closure of the present disclosure. According to an exemplary aspect of the method according to the present disclosure, the core member is foamed and the at least one peripheral layer is substantially not foamed, particularly not foamed.BU / dp 240580WO 09 May 2025

[0073] Where the closure according to the present disclosure comprises a plurality of cells, as in a foamed material, in particular if the core member comprises a plurality of cells, it is advantageous that the cell size and / or cell distribution in the foam, particularly in the core member, are substantially uniform throughout the entire length and / or diameter of the foamed material, particularly are substantially uniform throughout the entire length and / or diameter of the core member. In this way closures with substantially uniform properties, such as, for example OTR, compressibility and compression recovery, can be provided.

[0074] The plurality of cells of the disclosed closure is further advantageously defined as being a plurality of substantially closed cells, or that the foam is a substantially closed cell foam. In particular, the core member is exemplarily defined as comprising substantially closed cells. Closed cell foams are generally defined as comprising cells, also referred to as pores, which are substantially not interconnected with each other. Closed cell foams have higher dimensional stability, lower moisture absorption coefficients, and higher strength compared to open-cell-structured foams.

[0075] In order to assure that the core member of the closure possesses inherent consistency, stability, functionality and capability of providing long-term performance, the cell size of the foamed core material is particularly substantially homogeneous throughout its entire length and diameter. The foam thus particularly comprises a cell size characterized by a range of from about 0.025 mm minimum to about 0.5 mm maximum, in particular from about 0.05 mm minimum to about 0.35 mm maximum. The cell size is measured according to standard test methods known to the skilled person.

[0076] In another exemplary aspect of the present disclosure, the core member comprises closed cells having at least one of an average cell size in the range of from about 0.02 millimeters to about 0.50 millimeters, and a cell density in the range of from about 8,000 cells / cm3to about 25,000,000 cells / cm3. Although this cell configuration has been found to produce a highly effective product, it has been found that even more advantageous products comprise an average cell size in the range of from about 0.05 mm to about 0.35 mm, and / or a cell density in the range of from about 10,000 cells / cm3to about 8,000,000 cells / cm3.BU / dp 240580WO 09 May 2025

[0077] In order to control the cell size in the core member of the closure, and attain the desired cell size detailed above, a nucleating agent can be employed. In a particular embodiment, it has been found that by employing a nucleating agent selected from the group consisting of calcium silicate, talc, clay, titanium oxide, silica, barium sulfate, diatomaceous earth, and mixtures of citric acid and sodium bicarbonate, the desired cell density and cell size is achieved.

[0078] As is well known in the industry, a blowing agent can be employed in forming extruded foam plastic material such as is advantageous for the core member. In the present disclosure, a variety of blowing agents can be employed during the extruded foaming process whereby the core member is produced. Typically, either physical blowing agents or chemical blowing agents are employed. Suitable blowing agents that have been found to be efficacious in producing the core member of the present disclosure comprise one or more selected from the group consisting of: aliphatic hydrocarbons having 1-9 carbon atoms, halogenated aliphatic hydrocarbons having 1-9 carbon atoms and aliphatic alcohols having 1-3 carbon atoms. Aliphatic hydrocarbons include methane, ethane, propane, n-butane, isobutane, n-pentane, isopentane, neopentane, and the like. Among halogenated hydrocarbons and fluorinated hydrocarbons they include, for example, methylfluoride, perfluoromethane, ethyl fluoride, 1,1-difluoroethane (HFC-152a), 1,1,1-trifluoroethane (HFC-430a), 1,1, 1,2 -tetrafluoroethane (HFC-134a), pentafluoroethane, perfluoroethane, 2,2-difluoropropane, 1,1,1-trifluoropropane, perfluoropropane, perfluorobutane, perfluorocyclobutane. Partially hydrogenated chlorocarbon and chlorofluorocarbons for use in this disclosure include methyl chloride, methylene chloride, ethyl chloride, 1,1,1-trichlorethane, 1,1-dichlorol-fluoroethane (HCFC-141b), l-chlorol,l-difluoroethane (HCFC-142b), l,l-dichloro-2,2,2-trifluoroethane (HCFC-123) and 1-chloro-l,2,2,2-tetrafluoroethane (HCFC-124). Fully halogenated chlorofluorocarbons include trichloromonofluoromenthane (CFC11), dichlorodifluoromenthane (CFC-12), trichlorotrifluoroethane (CFC-113), dichlorotetrafluoroethane (CFC-114), chloroheptafluoropropane, and dichlorohexafluoropropane. Fully halogenated chlorofluorocarbons are not preferred due to their ozone depiction potential. AliphaticBU / dp 240580WO 09 May 2025alcohols include methanol, ethanol, n-propanol and isopropanol. Chemical blowing agents include azodicarbonamic, azodiisobutyro-nitride, benzenesulfonhydrazide, 4,4-oxybenzene sulfonylsemicarbazide, p-toluene sulfonylsemicarbazide, barium azodicarboxlyate, N,N'-Dimethyl-N,N'-dinitrosoterephthalamide, trihydrazinotriazine, and hydrocerol. An example of a suitable chemical blowing agent is sold by Clariant International Ltd, BU Masterbatches (Rothausstr. 61, 4132 Muttenz, Switzerland) under the trade name Hydrocerol®.

[0079] In a particular aspect, inorganic (or physical) blowing agents are used in making the foamed material according to the method according to the present disclosure. Examples of inorganic blowing agents include carbon dioxide, water, air, helium, nitrogen and argon. Carbon dioxide is a particularly useful blowing agent.

[0080] According to another exemplary embodiment of the method according to the present disclosure, in order to produce the desired product, the blowing agent may be incorporated into the plastic melt in a quantity ranging from about 0.005% to about 10% by weight of the weight of the plastic material.

[0081] In an exemplary aspect according to the method according to the present disclosure the synthetic bottle closure of the present disclosure comprises, as its principal component, a core member which is formed from extruded, foamed, thermoplastic polymers, copolymers, or homopolymers, or blends thereof. Although any known foamable thermoplastic polymeric material can be employed in the bottle closure of the present disclosure, the thermoplastic plastic material must be selected for producing physical properties similar to natural cork, so as to be capable of providing a synthetic closure for replacing natural cork as a closure for wine bottles. By way of example, the thermoplastic plastic material for the core member can be a closed cell plastic material.

[0082] According to an exemplary aspect of the method according to the present disclosure, said closure particularly comprises one or more thermoplastic polymers. Particularly at least one, particularly both of the core material and the material of the at least one peripheral layer comprise one or more thermoplastic polymers. In an exemplary aspect, the at least oneBU / dp 240580WO 09 May 2025peripheral layer comprises a thermoplastic polymer identical or similar to the thermoplastic polymer comprised in the core member. However, as detailed herein, the physical characteristics imparted to the peripheral layer particularly differ substantially from the physical characteristics of the core member.

[0083] According to an exemplary aspect of the method of the present disclosure, therefore, the core member comprises at least one thermoplastic polymer selected from the group consisting of polyethylenes, metallocene catalyst polyethylenes, polybutanes, polybutylenes, polyurethanes, silicones, vinyl-based resins, thermoplastic elastomers, polyesters, ethylenic acrylic copolymers, ethylene-vinyl-acetate copolymers, ethylene-methyl-acrylate copolymers, thermoplastic polyurethanes, thermoplastic olefins, thermoplastic vulcanizates, flexible polyolefins, fluorelastomers, fluoropolymers, polyethylenes, polytetrafluoroethylenes, and blends thereof, ethylene-butyl-acrylate copolymers, ethylenepropyl ene-rubb er, styrene butadiene rubber, styrene butadiene block copolymers, styrene block copolymers, ethylene-ethyl-acrylic copolymers, ionomers, polypropylenes, and copolymers of polypropylene and copolymerizable ethylenically unsaturated comonomers, olefin block copolymers and mixtures thereof. If a polyethylene is employed, in an exemplary aspect of the method disclosed herein the polyethylene comprises one or more polyethylenes selected from the group consisting of high density, medium density, low density, linear low density, ultra high density, and medium low density polyethylenes. Particularly useful plastic materials for the core element can be polyethylene, in particular LDPE, and / or ethylene-vinyl-acetate copolymer (EVA). These materials can be used alone or in combination with one or more other thermoplastic polymers disclosed herein, in particular with metallocene PE or metallocene PP, particularly with metallocene PE.

[0084] According to an aspect of the present disclosure the core member does not comprise a fatty acid or a fatty acid derivative.

[0085] According to another aspect of the present disclosure, the core member further comprises at least one of at least one fatty acid and at least one fatty acid derivative. In order to achieve this, one or more fatty acid derivatives can be added to the at least one thermoplastic polymer which is used to prepare the core member. Exemplary fatty acidBU / dp 240580WO 09 May 2025derivatives according to the present disclosure are fatty acid esters or fatty acid amides such as stearamides. The addition of at least one fatty acid derivative to the polymer composition of the synthetic closure imparts superior properties to the synthetic closure. In particular, it has been found that the oxygen transfer rate of the closure can be reduced substantially, thus further reducing unwanted oxidation of wine. In addition, it has been found that the use of a fatty acid derivative as additive does not have a negative impact on the performance characteristics of synthetic corks such as extraction force, ovality control, diameter control and length control. In order to impart the desired OTR-reducing effect to the closure, the fatty acid derivative, if present, is used according to an exemplary aspect of the present disclosure in a concentration from about 0.01 wt.% to about 10 wt.%, in particular from about 0.1 wt.% to about 5 wt.%, more particularly from about 1 wt.% to about 3 wt.%, based on the total weight of thermoplastic polymer.

[0086] If the core member comprises a fatty acid or a fatty acid derivative as disclosed herein, the closure can advantageously have a leakage value measured according to the herein described test method of not more than 100 mm2, particularly of not more than 80 mm2, particularly of not more than 50 mm2, particularly of not more than 30 mm2, particularly of not more than 20 mm2, particularly of not more than 10 mm2.

[0087] The closure according to any of the preceding claims particularly has a substantially cylindrical shape comprising substantially flat terminating surfaces forming the opposed ends of said closure and the substantially flat terminating surfaces of the core member are substantially devoid of the peripheral layer. The closure has a substantially cylindrical form comprising a substantially cylindrical peripheral surface and two substantially flat terminating faces at the opposing ends of the cylindrical form. In addition to a core member which possesses a construction with physical characteristics similar to natural cork, and has a substantially cylindrical form with a substantially cylindrical peripheral surface, the closure of the present disclosure comprises at least one peripheral layer at least partially surrounding and intimately bonded to at least one surface, particularly the substantially cylindrical surface, of the core member. The ends of the closure can be beveled or chamfered, as is known from the prior art. Although any desired bevel or chamfered configuration can be employed, such as a radius, curve, or flat surface, it has been found that merely cutting theBU / dp 240580WO 09 May 2025terminating ends at the intersection with the longitudinal cylindrical surface of the elongated length of material, with or without at least one peripheral layer as described herein, at an angle in the range of from about 30 ° to about 75 °, for example in the range of from about 35 ° to about 70 °, particularly in the range of from about 40 ° to about 65 °, allows formation of a closure which is easier to insert into the neck of a container. Angles of about 45 °, 46 °, 47 °, 48 °, 49 °, 50 °, 51 °, 52 °, 53 °, 54 °, 55 °, 56 °, 57 °, 58 °, 59 ° or 60 ° have been found particularly to contribute to the present disclosure. The bevel or chamfer angle is measured relative to the longitudinal axis of the cylindrical closure.

[0088] The closure of the present disclosure advantageously has an overall density of from about 100 kg / m3to about 800 kg / m3, in particular from about 200 kg / m3to about 500 kg / m3, in particular from about 220 kg / m3to about 400 kg / m3, in particular from about 250 kg / m3to about 375 kg / m3.

[0089] The closure of the present disclosure particularly comprises the at least one peripheral layer intimately bonded to substantially the entire substantially cylindrical surface of the core member. If any large unbonded areas exist, flow paths for gas and liquid could result. Consequently, secure, intimate, bonded interengagement of the at least one peripheral layer with the core member is advantageous for attaining a bottle closure for the wine industry.

[0090] In order to achieve integral bonded interconnection between the at least one peripheral layer and the core member, the at least one peripheral layer is formed about the core member in a manner which assures intimate bonded engagement. The closure according to the present disclosure is particularly formed by extrusion.

[0091] Particularly, the desired secure, intimate, bonded, interengagement is attained by simultaneous co-extrusion of the at least one peripheral layer and the core member or by applying the at least one peripheral layer to the continuous, elongated length of material after the continuous, elongated length of material has been formed. By employing either process, intimate bonded interengagement of the at least one peripheral layer to the continuous, elongated length of material is attained.BU / dp 240580WO 09 May 2025

[0092] In one aspect where the closure is formed by extrusion, said core member and said at least one peripheral layer are therefore extruded substantially simultaneously.

[0093] In another aspect where the closure is formed by extrusion, therefore, said core member is extruded separately and subsequent thereto said at least one peripheral layer is formed in extrusion equipment peripherally surrounding and enveloping the pre-formed core member.

[0094] In further aspects of the disclosed closure, comprising two or more peripheral layers, it is possible that a first peripheral layer which is in secure, intimate, bonded, interengagement with the outer cylindrical surface of the core member is formed by either substantially simultaneous extrusion with the core member, or by subsequent extrusion, as described herein. A second and subsequent peripheral layers can then be formed likewise by either substantially simultaneous extrusion with the core member and the first or further peripheral layers, or by subsequent extrusion, as described herein for the first peripheral layer. With multiple peripheral layers it is also possible that two or more peripheral layers are extruded subsequently, as described herein, but substantially simultaneously with each other.

[0095] It has also been found that further additional additives may be incorporated into either the core member and / or the at least one peripheral layer of the synthetic closure according to the present disclosure in order to provide further enhancements and desirable performance characteristics. These additional additives incorporate antimicrobial agents, antibacterial compounds, and or oxygen scavenging materials. Suitable additives are known to the person skilled in the art. The antimicrobial and antibacterial additives can be incorporated into the closure to impart an additional degree of confidence that in the presence of a liquid the potential for microbial or bacterial growth is extremely remote. These additives have a longterm time release ability and further increase the shelflife without further treatments by those involved with the bottling of wine. Furthermore, it is possible for the cells of the closure to be substantially filled with a non-oxidizing gas, in order to further reduce oxygen ingress into the container. Ways of achieving this are known in the prior art.BU / dp 240580WO 09 May 2025

[0096] As discussed above, intimate bonded inter engagement of the at least one peripheral layer to the core member is advantageous for providing a synthetic bottle closure capable of being used in the wine industry. In this regard, although it has been found that the methods detailed above provide secure intimate bonded interengagement of the at least one peripheral layer to the continuous, elongated, substantially cylindrically shaped length of a material, alternative layers or bonding chemicals can be employed, depending upon the particular materials used for forming the continuous, elongated, substantially cylindrically shaped length of a material and the at least one peripheral layer.

[0097] If desired, bonding agents or tie layers known to the skilled person can be employed on the outer surface of the continuous, elongated, substantially cylindrically shaped length of a material in order to provide secure intimate bonded interengagement of the at least one peripheral layer therewith. If a tie layer is employed, the tie layer would effectively be interposed between the continuous, elongated, substantially cylindrically shaped length of a material and the at least one peripheral layer to provide intimate bonded interengagement by effectively bonding the peripheral layer and the continuous, elongated, substantially cylindrically shaped length of a material to the intermediately positioned tie layer. However, regardless of which process or bonding procedure is employed, all of these alternate embodiments are within the scope of the present disclosure. If more than one peripheral layer is present, such bonding agents or tie layers can similarly be employed between respective peripheral layers.

[0100] In addition, the closures obtained by the method of the present disclosure may also comprise decorative indicia such as letters, symbols, colors, graphics, and wood tones printed on at least one peripheral layer and / or one of the substantially flat terminating surfaces forming the opposed ends of said closure or stopper. Printing of these indicia can be performed in-line, during production of the closure or in a separate step after the closure has been manufactured. Accordingly, the closure of the present disclosure may comprise a decorative effect on at least one of the peripheral layer and the substantially flat terminating surfaces forming the opposed ends of said closure or stopper.BU / dp 240580WO 09 May 2025

[0101] The closure according to the present disclosure can further comprise a silicone layer on at least one of its surfaces, in particular on its peripheral surface. Such a layer can help for example with insertion of the closure into a container. If a silicone layer is present, this is particularly formed by extrusion and / or by tumbling.

[0102] The present disclosure further relates to a method for producing a closure as described herein, said method comprising at least the steps of:A. providing a first composition comprising at least one thermoplastic polymer;B. optionally providing at least one blowing agent to the composition comprising at least one thermoplastic polymer to obtain a composition comprising at least one thermoplastic polymer and at least one blowing agent;C. at least one of before, during and after method step B., heating the composition provided in method step A. or the composition obtained in method step B. to obtain a heated composition;D. extruding a continuous, elongated, substantially cylindrically shaped length of the heated composition obtained in method step C. to obtain, as core member, a continuous elongated length of thermoplastic polymer having a cylindrical surface;E. providing a second composition comprising at least one styrene block copolymer, wherein the at least one styrene block copolymer comprises a bound styrene content, determined according to ASTM D5775-95, of 1 wt.% to 30 wt.%, based on the overall weight of the at least one styrene block copolymer,and / orwherein the at least one peripheral layer has an overall styrene content of 0.1 wt.% to 10 wt.%, based on the overall weight of the at least one peripheral layer;F. extruding a separate and independent peripheral layer of the composition provided in method step E. separately to, co-axially to and in intimate bonded engagement with the continuous, elongated length of thermoplastic polymer obtained in method step D., said separate and independent peripheral layer peripherally surrounding and substantially enveloping the cylindrical surface of the continuous, elongated length of thermoplastic polymer to obtain a multi-component elongated structure having a cylindrical surface;BU / dp 240580WO 09 May 2025G. cutting the multi-component elongated structure obtained in method step F. in a plane substantially perpendicular to the central axis of said multi-component elongated structure to obtain a closure;H. optionally printing, coating, or post-treating at least one of the continuous elongated length of thermoplastic polymer obtained in method step D., the multi-component structure obtained in method step F. and the closure obtained in method step G.

[0103] The details regarding the composition provided in method step A. are the same as the details for the thermoplastic polymers described herein for the core member of the closure of the present disclosure. If a combination of thermoplastic polymers is used, the composition provided in method step A. comprises this combination.

[0104] The details regarding the blowing agent provided in method step B. are the same as the details for the blowing agent described herein with respect to the closure of the present disclosure. Further additives can also be provided in method step B., such as, for example, at least one nucleating agent. Details regarding such additives are the same as the details regarding additives described herein with respect to the closure of the present disclosure.

[0105] If a fatty acid or a fatty acid derivative should be present in the closure according to the disclosure, this is advantageously provided in method step A. or in method step B. Details regarding suitable fatty acids and fatty acid derivatives are the same as the details regarding suitable fatty acids and fatty acid derivatives described herein with respect to the closure of the present disclosure.

[0106] The heating in method step C. preferably occurs to a temperature at which the composition provided in method step A., or the composition obtained in method step B. are soft enough to enable foaming to the desired density and / or extrusion of the respective composition. If a blowing agent is used which requires heat to provide the blowing effect, the heating in method step C. preferably occurs to a temperature at which this blowing effect can occur. Suitable temperatures depend principally on the thermoplastic polymer and blowing agent selected and can be easily determined by the skilled person based on theBU / dp 240580WO 09 May 2025known properties of the thermoplastic polymer and blowing agent and / or based on simple trials.

[0107] Method step D. can occur in any way known to the skilled person and appearing suitable, in particular using known extrusion equipment.

[0108] The details regarding the composition provided in method step E. are the same as the details regarding suitable materials, compounds and compositions described herein with respect to the at least one peripheral layer of the closure of the present disclosure.

[0109] According to an aspect of the method according to the present disclosure, method step F. occurs substantially simultaneously with method step D.

[0110] According to a further aspect of the method according to the present disclosure, method step F. can be repeated one or more times in order to obtain one or more further peripheral layers, whereby the one or more further peripheral layers are separately extruded in intimate bonded engagement with the cylindrical outer surface of the multi-component elongated structure to form a multilayer elongated length of material.[OHl] After the extrusion in method step D. and / or in method step F., the continuous elongated length of thermoplastic polymer or the multi-component elongated structure can be cooled by methods known to the skilled person.

[0112] The cutting in method step G. and the optional printing, coating, or post-treating of method step H. can be carried out in any way known and appearing suitable to the skilled person. Post-treating can comprise, for example, surface treatments such as plasma treatment, corona treatment, or providing a lubricant to the surface of the closure.

[0113] All details disclosed herein for the closures according to the present disclosure are also relevant for the method according to the present disclosure and therefore also form part of the disclosure of the method disclosed herein.BU / dp 240580WO 09 May 2025

[0114] The present disclosure also relates to a closure produced according to a method as described herein.

[0115] The closure produced according to the method described herein particularly has a leakage value measured according to the herein described test method of not more than 400 mm2, in particular of not more than 200 mm2, preferably of not more than 100 mm2or of not more than 80 mm2, more preferably of not more than 50 mm2. If the product is packaged under inert conditions, the closure advantageously has an oxygen ingress rate of less than about 1 mg oxygen per container in the first 100 days after closing the container, whereby the oxygen ingress rate is advantageously selected from the group consisting of less than about 0.5 mg oxygen, less than about 0.25 mg oxygen, less than about 0.2 mg oxygen and less than about 0.1 mg oxygen, per container in the first 100 days after closing the container.

[0116] According to a further aspect of the closure produced according to the method according to the present disclosure, the closure comprises the peripheral layer surrounding and intimately bonded to the cylindrical surface of the core member and the end surfaces of the core member are devoid of said layer.

[0117] The present disclosure also relates to a use of a closure as disclosed herein or produced according to a method described herein for sealing closed a container.

[0118] All details given in the present disclosure relating to the closures disclosed herein, to their properties, as well as relating to their production and their uses, also apply to the closures according to these aspects of the disclosure.

[0119] According to the present disclosure, a closure can be realized which is capable of providing at least one, particularly more than one, particularly almost all or even all of the needs imposed thereupon by the wine industry, as well as any other bottle closure / packaging industry. As a result, a synthetic bottle closure can be attained that can be employed for completely sealing and closing a desired bottle for securely and safely storing the product retained therein, optionally with desired markings and / or indicia printed thereon.BU / dp 240580WO 09 May 2025

[0120] The present disclosure accordingly comprises an article of manufacture possessing the features, properties, and relation of elements which will be exemplified in the article herein described, and the scope of the present disclosure will be indicated in the claims.BRIEF DESCRIPTION OF THE DRAWINGS

[0121] For a fuller understanding of the nature and objects of the present disclosure herein described, reference should be had to the following detailed description taken in connection with the accompanying drawings, in which:

[0122] FIGURE 1 is a perspective view of a synthetic closure according to an aspect of the present disclosure;

[0123] FIGURE 2 is a cross sectional-side elevation of a synthetic closure according to an aspect of the present disclosure;

[0124] FIGURE 3 is a schematic depiction of the jaws of a bottling machine which have been adjusted in order to misalign the jaws, before compression;

[0125] FIGURE 4 is a schematic depiction of the jaws of a bottling machine which have been adjusted in order to misalign the jaws, during compression;

[0126] FIGURE 5 is a schematic depiction of a jaw of a bottling machine showing the assembling screws;

[0127] FIGURE 6 shows schematically particular steps of the skin adhesion test method.

[0128] By referring to the FIGURES, along with the following detailed disclosure, the construction and production method for the synthetic closures of the present disclosure can best be understood. In these Figures, as well as in the detailed disclosure herein, the synthetic closure of the present disclosure, and its method of production, is depicted and discussed as a bottle closure for wine products. However, as detailed herein, the present disclosure is applicable as a synthetic closure for use in sealing and retaining any desired product in any desired closure system. However, due to the stringent and difficult demands placed upon closures for wine products, the detailed disclosure herein focuses upon the applicability of the synthetic bottle closures of the present disclosure as a closure for wineBU / dp 240580WO 09 May 2025bottles. However, it is to be understood that this detailed discussion is provided merely for exemplary purposes and is not intended to limit the present disclosure to this particular application and embodiment.

[0129] In FIGURES 1 and 2, the exemplary construction of a synthetic closure 20 is depicted comprising a generally cylindrical shape formed by core member 22 and peripheral layer 24 which peripherally surrounds and is intimately bonded to core member 22. In the exemplary aspect, core member 22 comprises a substantially cylindrically shaped surface 26, terminating with substantially flat end surfaces 27 and 28. Whenever applicable, the following detailed description of a synthetic closure having a layered structure, i.e. a core member and a peripheral layer, shall also apply to multilayer closures having more than one peripheral layer.

[0130] In an exemplary aspect, peripheral layer 24 is intimately bonded directly to core member 22, peripherally surrounding and enveloping surface 26 of core member 22.Peripheral layer 24 incorporates exposed surface 29, which comprises a substantially cylindrical shape and forms the outer surface of synthetic bottle closure 20 of the present disclosure, along with surfaces 27 and 28 of the substantially flat terminating ends.

[0131] In order to assist in assuring entry of synthetic bottle closure 20 into the portal of the bottle into which closure 20 is inserted, terminating edge 31 of peripheral layer 24 may be beveled or chamfered. Similarly, terminating edge 32 of peripheral layer 24 also may comprise a similar bevel or chamfer. Although any desired bevel or chamfered configuration can be employed, such as a radius, curve, or flat surface, it has been found that by merely cutting ends 31 and 32 with an angle of about 45 ° or about 60 ° the desired reduced diameter area is provided for achieving the desired effect.

[0132] By incorporating chamfered or beveled ends 31 and 32 an synthetic bottle closure 20, automatic self-centering is attained. As a result, when synthetic bottle closure 20 is compressed and ejected from the compression jaws into the open bottle for forming the closure thereof, synthetic bottle closure 20 is automatically guided into the bottle opening, even if the clamping jaws are slightly misaligned with the portal of the bottle. By employingBU / dp 240580WO 09 May 2025this configuration, unwanted difficulties in inserting bottle closure 20 into any desired bottle are obviated. However, in applications which employ alternate stopper insertion techniques, chamfering of ends 31 and 32 may not be needed. Further, in order to facilitate the insertion of the closure into the bottle neck, the outer surface can fully or partly be coated with suitable lubricants, in particular with silicones. Coating with lubricants such as silicones can be effected by a variety of techniques known in the art, including tumbling and / or extrusion coating.

[0133] In order to produce the attributes suitable for use in the wine industry, core 22 is formed from foam plastic material as described herein using a continuous extrusion process. Although other prior art systems have employed molded foamed plastic material, these processes have proven to be more costly and incapable of providing a final product with the attributes of the present disclosure.

[0134] In order to demonstrate the efficacy of the present disclosure, samples of synthetic bottle closures 20, manufactured in accordance with the present disclosure and having a foamed core member and a solid peripheral layer were produced and tested.

[0135] Test Methods

[0136] The Mocon test for oxygen transfer rate (OTR) / oxygen ingress rate was carried out according to ASTM F-1307. A detailed description for the measurement of the OTR is described in Dieval J-B., Vidal S. and Aagaard O., Packag. Technol. Sci. 2011; DOI: 10.1002 / pts.945 (Mocon Ox-tran measurement, p. 378) which is herewith incorporated and forms part of the present disclosure. The tests for extraction force and compression recovery were carried out on a random sample selection according to the methods described in WO 03 / 018304 Al (compression test, p. 45, 1. 9 - p. 48, 1. 12; extraction test, p. 48, 1. 13 - p. 49, 1. 10), which are herewith incorporated and form part of the present disclosure.Instantaneous Diameter

[0137] The instantaneous diameter is determined using an optical micrometer (Keyence 7650 and DATAQ 158-U Analog to Digital converter) positioned at the outlet of the corkingBU / dp 240580WO 09 May 2025machine, which measures the diameter of the closure immediately after the closure has exited the corking machine into the bottle.Recovery Force

[0138] The recovery force is determined using a Tinus Olsen H5KT device. The closure is compressed to a diameter of 15.7 mm in bottling jaws mounted on a compression / traction bench and the force to be applied by the apparatus to the jaws to compress of the closure is measured. The jaws are then opened to a diameter of 18.5 mm and the force to compensate for the compression of the rebounding closure (= recovery force) is measured.Extraction Force

[0139] Three empty, clean “Bordeaux” style wine bottles were stoppered using a semiautomatic corking machine (Model 4040 from GAI S.p.A., Italy). The bottles were stored for one hour. The closures were then extracted at ambient temperature using a Dillon AFG-1000 N force gauge (from Dillon / Quality Plus, Inc., USA) to measure the force required for extraction.Leakage

[0140] A Monobloc Comet 200 Multi bottling machine, manufactured by Costral S.A. (Riquewihr, France) was used in the tests. The line speed was 2025 bottles / hour, the program selected was Liege 4 and the compression diameter was 15 mm. The fill level was set to 63 mm and checked throughout the test. By reference to Figures 3 to 5, the compression jaws 40 (two fixed jaws 41 and two mobile jaws 42) were adjusted by tightening the assembling screws 43 in order to set a gap 44 of 0.2 mm between the mobile 42 and the fixed jaws 41. This gap 44 mimics the wear observed on industrial bottling machines after many hours of working without adjustment. Such wear is a typical source of damage to closures which can cause leakage. In all other respects the bottling machine was operated according to the operating instructions. Bottle racks were prepared with white folded paper towel at the bottom. Clean 750 ml bottles were prepared. The filling hopper was filled with red wine at ambient temperature, about 22 °C. The bottles were filled and corked without vacuum, using closures and comparative closures as described below. Directly after bottling and corking the bottleneck was wiped to remove any wine splash. The bottles were placed upside down inBU / dp 240580WO 09 May 2025the bottle rack for 30 minutes, then removed from the bottle rack. If any red wine spot or spots were visible on the white paper towel, this leakage area was measured as follows: it is assumed that the leakage areas are ellipses. The smallest (di) and the largest (Di) diameters are measured in mm. The total leakage area is calculated according to formula (I):Area = n *£(Di*di) / 4 (I)

[0141] Nine closures were used per sample lot, and the average values determined. In addition, a control lot was systematically tested at the end of each measurement session.Skin Adhesion (peel force)This test provides a measure of the strength of adhesion of the peripheral layer to the core. Reference is made to Fig. 6. A closure 20 to be tested is scored along the length of the closure parallel to the longitudinal axis thereof, with two parallel cuts 50 at a distance of approx. 8 mm from each other, to a depth equating approximately to the thickness of peripheral layer 24. The cuts are made using a tool having two parallel blades in order to maintain the same distance between the two cuts along the length of the closure. A 5-10 mm portion of peripheral layer 24 is then peeled away from core 22 without detaching, as shown in Fig. 6 a). A clamp 51 is attached to an Tinius Olsen force gauge (Model H5KS, from Tinium Olsen, Horsham, PA, USA) or to an Imada force gauge (Model DS2, equipped with a MV 220 motorised test stand and a RS-232 connection kit) and the force gauge zeroed (not depicted in the Figure). The speed is set to 300 mm / minute. The closure 20 is placed in cork holder 52 with the cut lines 50 aligned within the open area 53 of cork holder 52. The peeled portion of peripheral layer 24 is then held firmly in clamp 51, with the clamp wing nut 54 pointing upwards (Fig. 6 b)), and the measurement is started. The measurement is stopped either when the entire strip of peripheral layer 24 has been peeled off or when the force gauge stops moving. The test is repeated two more times at different positions for the same closure. At least two closures are tested, giving in total at least six measurements. Each measurement gives up to 200 or more pieces of data, which are averaged for each reading, to give individual averages for each measurement. An average value is then calculated based on these individual averages. A larger value indicates a better adhesion of peripheral layer 24 to core 22.BU / dp 240580WO 09 May 2025Example 1 (comparative)

[0142] The sample products were produced on conventional co-extrusion equipment. Core member 22 was produced by employing low density polyethylene (LDPE) using an inert gas as physical blowing agent. The degree of foaming was adjusted so as to produce samples having a density of 231 kg / m3. In forming peripheral layer 24, an oil-extended SEBS compound (Monprene RG29058 by Teknor Apex) was employed. In the co-extrusion process, the peripheral layer 24 was formed at a layer thickness of 0,45 mm encapsulating the core member 22, and being intimately bonded thereto. The resulting products were cut to lengths suitable for forming bottle closure 20, followed by a chamfer being formed in edges 31 and 32, and finally printed and surface treated. The resulting closure has an overall diameter of 23,0 mm.Example 2

[0143] The samples were prepared in an identical manner as in Example 1, with the difference that the peripheral layer 24, is a non-oil extended SEBS compound comprising either a non-oil extended SEBS compound (NOE-SEBS like Globalprene 9645D or TC8060 by LCY Chemical Corporation) and / or a polyolefin elastomer (POE; Lucene LC575 by LG Chem), and / or a linear-low density polyethylene (LLDPE; Sabie LLDPE NSF6118). The polymer components of the peripheral layer were either pre-compounded into a polymer blend which is fed directly to the extrusion equipment, or each polymer component of the peripheral layer was supplied to a separate reservoir and then fed from this reservoir to the extrusion equipment where the respective peripheral layer components were blended with each other and extruded. The details of the products and the comparative products are shown in Table 1. The product numbers in Table 2 refer to the product numbers as defined in Table 1.BU / dp 240580WO 09 May 2025

[0144] Table 1

[0145] Samples were tested for the properties of instant recovery, average extraction force after 1 hour of bottling, recovery force, skin adhesion and leakage. The comparative closure was subject to the same tests as the closures according to the present disclosure.

[0146] Table 2BU / dp 240580WO 09 May 2025

[0147] The examples show a comparison between a closure with a peripheral layer containing an oil-extended SEBS compound and the closure according to the invention. Surprisingly, the examples show that the leakage values can be improved with the closures according to the disclosures compared to known closures, even with a thinner peripheral layer (< 0,45 mm), without significant impairment or even with improvement of other performance properties of the closure. Besides improved leak resistance, the adhesion of the skin the center foam (skin adhesion) can be improved by including a proportion of a polyolefin elastomer (POE), such as an ethyl ene-1 -butene copolymer, or a polyolefin plastomer (POP) such as a linear low-density polyethylene. Thus, the skin adhesion can be increased to > 11,4 N.

[0148] It can thus be seen that the samples prepared according to the present disclosure have significantly better resistance to bottling conditions, as measured by the test methods described herein, in particular as measured by the amount of leakage, compared to the comparative sample, without significantly worsening or even with improvement in other performance properties measured. It is thus possible, using the present disclosure, to reduce the overall amount of materials in a closure, by reducing the thickness of the peripheral layer to (< 0,45 mm), while maintaining or even improving the performance properties of the closure, especially with regard to the skin adhesion. With the closure according to the present invention, it is possible to increase the peel force (skin adhesion) to > 11,4 N which provides better control on possible delamination of the skin (peripheral layer) and foam (core member). In addition, the low bound styrene content of the styrene block copolymer and / or the low styrene content in the peripheral layer allows to avoid oil in the peripheral layer without impairment of the processability of the styrene block copolymer compound. Thus, the printing performance on the peripheral layer is improved as there is no migration of oil to the surface which can reduce the printability on the peripheral layer.

[0149] It will thus be seen that the needs set forth above, among those made apparent from the preceding description, are efficiently obtained and, since certain changes may be made in carrying out the above method without departing from the scope of this disclosure, it is intended that all matter contained in the above description or shown in the accompanying drawings shall be interpreted as illustrative and not in a limiting sense. Furthermore, it should be understood that the details of the disclosure described in the foregoing detailedBU / dp 240580WO 09 May 2025description are not limited to the specific embodiments shown in the drawings but are rather meant to apply to the present disclosure in general as outlined in the summary of the present disclosure and in the claims.

[0150] It is also to be understood that the following claims are intended to cover all of the generic and specific features of the present disclosure herein described, and all statements of the scope of the present disclosure which, as a matter of language, might be said to fall there between.BU / dp 240580WO 09 May 2025

Claims

May 9, 2025C l a i m s1. A closure (20) for a product-retaining container constructed for being inserted and securely retained in a portal forming neck of said container, said closure (20) comprising at leasta) a core member (22) comprising at least one thermoplastic polymer, andb) at least one peripheral layer (24) at least partially surrounding and intimately bonded to at least one surface of the core member (22), said peripheral layer (24) comprising at least one styrene block copolymer,whereinthe core member (22) has a density in the range of from about 100 kg / m3to 350 kg / m3and the peripheral layer (24) has a density in the range of from greater than 350 kg / m3to about 1,500 kg / m3and a thickness in the range of from 0.15 mm to less than 0.75 mm, characterized in that the at least one styrene block copolymer comprises a bound styrene content, determined according to ASTM D5775-95, of 1 wt.% to 30 wt.%, based on the overall weight of the at least one styrene block copolymer,and / orthat the at least one peripheral layer (24) has an overall styrene content of 0.1 wt.% to 10 wt.%, based on the overall weight of the at least one peripheral layer.

2. The closure (20) according to claim 1, wherein the at least one thermoplastic polymer of the core member (22) is different to the at least one styrene block copolymer of the at least one peripheral layer (24).

3. The closure (20) according to claim 1 or 2, wherein the at least one styrene block co polymer is a radial styrene block copolymer.

4. The closure (20) according to any one of the preceding claims, wherein the at least oneperipheral layer (24) contains an overall styrene content in the range of from 0,1 wt.% to 9,8 wt.%, in particular from 0,2 wt.% to 9,5 wt.%, preferably from 0,5 wt.% to 9,2 wt.% or from 1 wt.% to 9 wt.%, more preferably from 1,5 wt.% to 8,5 wt.% or from 2 wt.% to 8 wt.%, based on the total weight of the at least one peripheral layer (24).

5. The closure (20) according to any one of the preceding claims, wherein the at least one styrene block copolymer is selected from the group consisting of styrene ethylene butadiene styrene block copolymers, styrene ethylene butylene styrene block copolymers, styrene ethylene butylene block copolymers, styrene butadiene styrene block copolymers, styrene butadiene block copolymers, styrene isoprene styrene block copolymers, styrene isobutylene block copolymers, styrene isoprene block copolymers, styrene ethylene propylene styrene block copolymers, styrene ethylene propylene block copolymers and combinations of two or more thereof, preferably of styrene ethylene butylene styrene block copolymers.

6. The closure (20) according to any one of the preceding claims, wherein the at least one styrene block copolymer is a non-oil-extended (NOE) styrene block copolymer and / or wherein the at least one styrene block copolymer is essentially oil free.

7. The closure (20) according to any of the preceding claims, wherein the peripheral layer (24) is essentially oil free.

8. The closure (20) according to any one of the preceding claims, wherein the at least one styrene block copolymer comprises a bound styrene content, determined according to ASTM D5775-95, of 2 % to 25 %, in particular of 3 % to 21 %, preferably of 5 % to 20 %, more preferably of 6 % to 18 % or of 8 % to 15 % and / or a styrene to rubber ratio, determined according to ASTM D5775, in particular according to ASTM D5775-95, of 1 / 99 to 30 / 70 or of 2 / 98 to 25 / 75, in particular of 3 / 97 to 21 / 79, preferably of 5 / 95 to 18 / 82, more preferably of 8 / 92 to 15 / 85.

9. The closure (20) according to any one of the preceding claims, wherein the at least one styrene block copolymer has a melt flow rate (MFR) as determined by ASTM DI 238-23 a (230 °C, 5 kg) of greater than 1 g / 10 min or of greater than 2 g / 10 min, in particular of greaterBU / dp 240580WO 09 May 2025than 5 g / 10 min, preferably of greater than 8 g / 10 min, more preferably of greater than 10 g / 10 min or of greater than 12 g / 10 min.

10. The closure (20) according to any one of the preceding claims, wherein the at least one styrene block copolymer has a tensile strength as determined by ASTM D412- 16 of greater 5 MPa, in particular of greater 6 MPa, preferably of greater 8 MPa, more preferably of greater 9 MPa.

11. The closure (20) according to any one of the preceding claims, wherein the at least one styrene block copolymer has an elongation at break as determined ASTM D412- 16 of greater 400 %, in particular of greater 500 % or of greater 600 %, preferably of greater 700 % or greater 800 %, more preferably of greater 850 %.

12. The closure (20) according to any one of the preceding claims, wherein the at least one styrene block copolymer has a hardness (Type A scale) as determined by ASTM D2240-15 of 20 to 85 shore A, in particular of 25 to 80 shore A, preferably of 35 to 75 shore A, more preferably 50 to 75 shore A.

13. The closure (20) according to any one of the preceding claims, wherein the at least one styrene block copolymer is essentially free of antioxidants.

14. The closure (20) according to any one of the preceding claims, wherein the at least one styrene block copolymer is present in an amount in the range of from 0,1 wt.% to 100 wt.%, in particular from 5 wt.% to 95 wt.%, preferably from 10 wt.% to 90 wt.%, more preferably from 25 wt.% to 85 wt.% or from 35 wt.% to 75 wt.%, based on the total weight of the peripheral layer (24).

15. The closure (20) according to any one of the preceding claims, wherein the peripheral layer (24) further comprises at least one further polymer or copolymer different to the at least one styrene block copolymer.BU / dp 240580WO 09 May 202516. The closure (20) according to claim 15, wherein the at least one further polymer or copolymer is a thermoplastic elastomer.

17. The closure (20) according to claim 15 or claim 16, wherein the at least one further polymer or copolymer selected from the group consisting of thermoplastic polyolefins, thermoplastic polyurethanes, thermoplastic polyamides, thermoplastic copolyesters and thermoplastic vulcanisates, preferably from thermoplastic polyolefins.

18. The closure (20) according to any one of claims 15 to 17, wherein the at least one further polymer or copolymer is selected from the group consisting of thermoplastic polyolefin elastomers, olefin block copolymers and polyolefin plastomers.

19. The closure (20) according to any one of claims 15 to 18, wherein the at least one further polymer or copolymer is present in an amount in the range of from 0 wt.% to 99.9 wt.%, in particular from 1 wt.% to 99 wt.%, preferably from 5 wt.% to 95 wt.%, more preferably from 10 wt.% to 90 wt.% or from 20 wt.% to 60 wt.% based on the total weight of the peripheral layer.

20. The closure (20) according to any one of the preceding claims, having an extraction force determined one hour after bottling according to the herein described test method of not more than 450 N, in particular of not more than 400 N, preferably of not more than 300 N, more preferably of not more than 250 N.

21. The closure (20) according to any one of the preceding claims, having an oxygen transfer rate (OTR) in axial direction of from about 0.0001 to about 0.1000 cc / day / closure, in particular from about 0.0005 to about 0.050 cc / day / closure.

22. The closure (20) according to any one of the preceding claims, wherein the closure has a leakage value measured according to the herein described test method of not more than 500 mm2, in particular of not more than 200 mm2, preferably of not more than 100 mm2, more preferably of not more than 80 mm2.BU / dp 240580WO 09 May 202523. The closure (20) according to any one of the preceding claims, wherein the core member (22) has a density in the range of from about 100 kg / m3to less than 235 kg / m3and the closure (20) has a leakage value measured according to the herein described test method of not more than 500 mm2, orthe core member (22) has a density in the range of from 235 kg / m3to 280 kg / m3and the closure (20) has a leakage value measured according to the herein described test method of not more than 200 mm2, orthe core member (22) has a density in the range of from greater than 260 kg / m3to 350 kg / m3and the closure (20) has a leakage value measured according to the herein described test method of not more than 100 mm2.

24. The closure (20) according to any one of the preceding claims, wherein the closure (20) has an adhesion of the at least one peripheral layer (24) to the core member (22) (skincore adhesion) according to the herein described test method of at least 11.5 N, preferably of at least 12 N.

25. The closure (20) according to any one of the preceding claims, wherein the core member (22) comprises a plurality of cells.

26. The closure (20) according to claim 25, wherein at least one of the size and the distribution of the plurality of cells in the core member (22) is substantially uniform throughout at least one of the length and the diameter of the core member (22).

27. The closure (20) according to claim 25 or claim 26, wherein the plurality of cells is a plurality of substantially closed cells.

28. The closure (20) according to any one of claims 25 to 27, wherein the plurality of cells comprises a cell size in a range of from about 0.025 mm to about 0.5 mm, in particular from about 0.05 mm to about 0.35 mm.

29. The closure (20) according to any one of the preceding claims, wherein said core member (22) comprises at least one of closed cells having an average cell size ranging fromBU / dp 240580WO 09 May 2025about 0.02 millimeters to about 0.50 millimeters and a cell density ranging from about 8,000 cells / cm3to about 25,000,000 cells / cm3, in particular wherein said core member comprises at least one of an average cell size ranging from about 0.05 mm to about 0.1 mm and a cell density ranging from about 1,000,000 cells / cm3to about 8,000,000 cells / cm3.

30. The closure (20) according to any of the preceding claims, wherein said closure (20) has a substantially cylindrical shape comprising substantially flat terminating surfaces (27, 28) forming the opposed ends of said closure (20) and the substantially flat terminating surfaces (27, 28) of the core member (22) are substantially devoid of the peripheral layer (24).

31. The closure (20) according to any one of the preceding claims, wherein the core member (22) comprises at least one thermoplastic polymer selected from the group consisting of polyethylenes, metallocene catalyst polyethylenes, polybutanes, polybutylenes, polyurethanes, silicones, vinyl-based resins, thermoplastic elastomers, polyesters, ethylenic acrylic copolymers, ethylene-vinyl-acetate copolymers, ethylene-methyl-acrylate copolymers, thermoplastic polyurethanes, thermoplastic olefins, thermoplastic vulcanizates, flexible polyolefins, fluorelastomers, fluoropolymers, polyethylenes, polytetrafluoroethylenes, and blends thereof, ethylene-butyl-acrylate copolymers, ethyl ene-propylene-rubb er, styrene butadiene rubber, styrene butadiene block copolymers, ethylene-ethyl-acrylic copolymers, ionomers, polypropylenes, and copolymers of polypropylene and copolymerizable ethylenically unsaturated comonomers, olefin copolymers, olefin block copolymers and mixtures thereof.

32. The closure (20) according to any one of the preceding claims having an overall density of from about 100 kg / m3to about 800 kg / m3, in particular from about 200 kg / m3to about 500 kg / m3.

33. The closure (20) according to any one of the preceding claims, wherein said closure is formed by extrusion.

34. The closure (20) according to claim 33, wherein said core member (22) and said peripheral layer (24) are extruded substantially simultaneously or said core member (22) isBU / dp 240580WO 09 May 2025extruded separately and subsequent thereto said peripheral layer (24) is formed in extrusion equipment peripherally surrounding and enveloping the pre-formed core member (22).

35. A method for producing a closure (20) according to any one of claims 1 to 34, said method comprising at least the steps of:A. providing a first composition comprising at least one thermoplastic polymer;B. optionally providing at least one blowing agent to the composition comprising at least one thermoplastic polymer to obtain a composition comprising at least one thermoplastic polymer and at least one blowing agent;C. at least one of before, during and after method step B., heating the composition provided in method step A. or the composition obtained in method step B. to obtain a heated composition;D. extruding a continuous, elongated, substantially cylindrically shaped length of the heated composition obtained in method step C. to obtain, as core member (22), a continuous elongated length of thermoplastic polymer having a cylindrical surface;E. providing a second composition comprising at least one styrene block copolymer, wherein the at least one styrene block copolymer comprises a bound styrene content, determined according to ASTM D5775-95, of 1 wt.% to 30 wt.%, based on the overall weight of the at least one styrene block copolymer,and / orwherein the at least one peripheral layer has an overall styrene content of 0.1 wt.% to 10 wt.%, based on the overall weight of the at least one peripheral layer;F. extruding a separate and independent peripheral layer (24) of the composition provided in method step E. separately to, co-axially to and in intimate bonded engagement with the continuous, elongated length of thermoplastic polymer obtained in method step D., said separate and independent peripheral layer (24) peripherally surrounding and substantially enveloping the cylindrical surface of the continuous, elongated length of thermoplastic polymer to obtain a multi-component elongated structure having a cylindrical surface; G. cutting the multi-component elongated structure obtained in method step F. in a plane substantially perpendicular to the central axis of said multi-component elongated structure to obtain a closure (20);BU / dp 240580WO 09 May 2025H. optionally printing, coating, or post-treating at least one of the continuous elongated length of thermoplastic polymer obtained in method step D., the multi-component structure obtained in method step F. and the closure (20) obtained in method step G.

36. A closure (20) produced according to a method according to claim 35.

37. The closure (20) according to claim 36, wherein said closure (20) has a leakage value measured according to the herein described test method of not more than 400 mm2, in particular of not more than 200 mm2, preferably of not more than 100 mm2or of not more than 80 mm2.

38. Use of a closure (20) according to any one of claims 1 to 34, 36 or 37 for sealing closed a container.BU / dp 240580WO 09 May 2025