Method and device for spatially resolved measurement of at least one homogeneity parameter, optical element, and lithography system

Raman spectroscopy is used to measure and correct thermal expansion inhomogeneities in quartz glass substrates, addressing precision and destructiveness issues in existing methods, improving EUV projection exposure systems.

WO2026233827A1PCT designated stage Publication Date: 2026-11-12CARL ZEISS SMT GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/062460
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-05
Filing Date
2026-04-30
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing methods for quantifying the spatially resolved distribution of thermal expansion homogeneity in titanium-doped quartz glass substrates are either destructive or lack precision, particularly in the context of EUV projection exposure systems, where precise knowledge of the zero-crossing temperature is crucial for optical element performance.

Method used

A method utilizing Raman spectroscopy to measure the spatial distribution of titanium and OH content in quartz glass substrates, enabling precise determination of thermal expansion coefficients and zero-crossing temperatures through non-destructive, high-resolution mapping, allowing for deterministic correction of inhomogeneities.

Benefits of technology

Enables precise, non-destructive measurement of thermal expansion homogeneity in quartz glass substrates, facilitating improved manufacturing of optical elements by predicting and correcting inhomogeneities, thereby enhancing the performance and reliability of EUV projection exposure systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026062460_12112026_PF_FP_ABST
    Figure EP2026062460_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a method for spatially resolved measurement of at least one homogeneity parameter in a volume of a substrate body (2), in particular a substrate body (2) of an optical element (116, 118, 119, 120, 121, 122, Mi, 207) of a projection exposure apparatus (100, 200), comprising at least the following steps: a) capturing relevant measurement information in at least one volume element (4) of the substrate body (2) by means of a measuring device (3); b) determining a value of the at least one homogeneity parameter from the respective measurement information by means of a computing device (5); c) determining a spatial position of the at least one volume element (4) by means of a position determining device (6); d) determining a spatial distribution (7) of the at least one homogeneity parameter from the spatial position of the at least one volume element (4) and the relevant associated homogeneity parameter by means of the computing device (5).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Method and apparatus for spatially resolved measurement of at least one homogeneity parameter, optical element and lithography system

[0002] The present application claims priority from German patent application No. 102025 117 125.4, the contents of which are incorporated herein in full by reference.

[0003] The invention relates to a method for spatially resolved measurement of at least one homogeneity parameter in a volume of a substrate body.

[0004] The invention further relates to a device for spatially resolved measurement of at least one homogeneity parameter in a volume of a substrate body.

[0005] The invention also relates to an optical element, in particular a mirror of an EUV projection exposure system, with at least one substrate body.

[0006] The invention also relates to a lithography system, in particular a projection exposure system for semiconductor lithography, with an illumination system comprising a radiation source and optics comprising at least one optical element.

[0007] Optical elements for guiding and shaping wavefronts, especially for use in lithography systems, are known from the prior art.

[0008] It is also known from the prior art that optical elements have a substrate body which serves as a support for optically relevant surfaces. Such surfaces are designed in particular to form wavefronts, especially by their shape or profile and / or their coating.

[0009] It is also known from the prior art to form substrate bodies for optical elements from synthetic quartz glass doped with approximately 7.5 wt% titanium dioxide.

[0010] Such titanium dioxide-doped quartz glasses exhibit a temperature-dependent coefficient of thermal expansion (CTE).

[0011] A special characteristic of these quartz glasses is that their coefficient of thermal expansion increases at least approximately monotonically between 0° and 60°C, crossing a zero line in the process. Therefore, for these quartz glasses, there exists a temperature at which the coefficient of thermal expansion equals zero. This temperature is called the zero-crossing temperature (TZC) and can be adjusted, in particular, by selecting a suitable composition of the materials used. The actual thermal expansion is calculated by integrating the temperature-dependent behavior of the coefficient of thermal expansion along the temperature axis.

[0012] This results in a parabolic curve for the actual observed thermal expansion.

[0013] In the vicinity of the zero-crossing temperature, thermal expansion is almost negligible. The further the temperature is from the zero-crossing temperature, the greater the effect of temperature fluctuations on linear expansion.

[0014] Precise knowledge of the zero-crossing temperature is therefore of utmost importance in the design of an optical element. The operating temperature of the optical element should preferably be precisely matched to the zero-crossing temperature.

[0015] A disadvantage of the quartz glasses known from the prior art for forming substrate bodies of optical elements is a potentially insufficient homogeneity of the spatial distribution of the zero crossing temperature in the volume of the quartz glass.

[0016] However, the homogeneity of the coefficient of thermal expansion or the zero-crossing temperature of titanium-doped quartz glass is, alongside the mean zero-crossing temperature, a key property of substrates, especially substrates for mirrors in EUV projection exposure systems.

[0017] The spatially resolved distribution of the coefficient of thermal expansion is significantly influenced by the titanium dioxide content. In quartz glasses known from the prior art, this content is approximately 7.5% to achieve a zero-transit temperature close to room temperature.

[0018] Furthermore, the spatially resolved distribution of the coefficient of thermal expansion also depends on tempering, i.e., the entire thermal history of the substrate. In addition, the hydroxide content, i.e., the OH content, also influences a homogeneous spatially resolved distribution of the coefficient of thermal expansion.

[0019] With substrate bodies known from the prior art, it is possible, with expert process control, for a blank for the substrate body to have the same tempering and an OH content that is constant to within a few percent, at least in an entire optically used area.

[0020] In previously known substrate blanks, thermal homogeneity is primarily determined by homogeneity of the titanium content. It follows that thermal inhomogeneity, which should be avoided, is also dominated by fluctuations in the titanium content. It is known that titanium dioxide is predominantly present as titanium dioxide. 4+ exists in tetrahedral coordination.

[0021] A disadvantage of prior art methods for quantifying the spatially resolved distribution of the Ti content is that they either require at least partial destruction of the blank and / or have poor spatial resolution.

[0022] The present invention is based on the objective of creating a method for spatially resolved measurement of at least one homogeneity parameter, which avoids the disadvantages of the prior art, in particular enabling the most precise possible measurement of the substrate body.

[0023] According to the invention, this problem is solved by a method having the features mentioned in claim 1.

[0024] The present invention further aims to create a device for spatially resolved measurement of at least one homogeneity parameter, which avoids the disadvantages of the prior art, in particular enabling the most precise possible measurement of the substrate body.

[0025] According to the invention, this problem is solved by a device having the features mentioned in claim 12.

[0026] The present invention also aims to create an optical element that avoids the disadvantages of the prior art, in particular by having a precisely measured substrate body.

[0027] According to the invention, this problem is solved by an optical element having the features mentioned in claim 19.

[0028] The present invention further aims to create a lithography system which avoids the disadvantages of the prior art, in particular having highly precisely shaped wavefronts for the exposure of wafers.

[0029] According to the invention, this problem is solved by a lithography system with the features mentioned in claim 20.

[0030] The inventive method for spatially resolved measurement of at least one homogeneity parameter in a volume of a substrate body, in particular a substrate body of an optical element of a projection exposure system, comprises at least the following steps:

[0031] a) Acquisition of a respective measurement information in at least one volume element of the substrate body by means of a measuring device, b) Determination of a value of the at least one homogeneity parameter from the respective measurement information by means of a computing device,

[0032] c) Determination of the spatial position of at least one volume element using a position determination device,

[0033] d) Determination of a spatial distribution of the at least one homogeneity parameter from the spatial position of the at least one volume element and the respective associated homogeneity parameter using the computing device.

[0034] It may be possible to derive a final three-dimensional map of the coefficient of thermal expansion and / or the zero-crossing temperature from determined spatial distributions of titanium and / or OH content. Thus, the titanium and / or OH content serves as measurement information from which the zero-crossing temperature and / or the coefficient of thermal expansion are determined as homogeneity parameters.

[0035] Alternatively or additionally, a known tempering or thermal history of the substrate body can also be used as measurement information, whereby the homogeneity parameter is again given by the zero-crossing temperature and / or the coefficient of thermal expansion and can be determined by means of a materials science model.

[0036] To obtain additional information, it may be necessary to perform destructive absolute measurements, such as the fabrication of a resonator from sample material for measurement on the Fabry-Perot interferometer (FPI), on witness samples and / or on the blank after a tempering process.

[0037] In an advantageous further development of the method according to the invention, it can be provided that in step a) a Raman spectrum is acquired as measurement information in the at least one volume element of the substrate body by means of a Raman device.

[0038] As explained later, it may be possible to measure a titanium-doped quartz glass as the substrate.

[0039] Preferably, a measuring radiation is generated by the Raman device for this purpose.

[0040] The method according to the invention can thus, in particular, comprise a measurement of the CTE homogeneity, especially the relative homogeneity, of a blank and / or a mirror made of titanium-doped quartz glass by mapping a local Ti content, wherein the local Ti content is preferably determined by Raman spectroscopy and by determining a ratio of titanium dioxide to silicon dioxide. The method according to the invention thus offers the possibility of determining a CTE homogeneity distribution and / or an average coefficient of thermal expansion in titanium-doped quartz glass by means of Raman spectroscopy.

[0041] The process may involve scanning a side surface of the substrate and / or scanning a top or bottom surface. Subsequently, a three-dimensional measurement of the homogeneity is performed.

[0042] It may be possible to plan a deterministic correction of layer schlieren or striae, which will be explained later, by using a confocal Raman microscope with a shallow measurement depth and penetration depth as a Raman device when fabricating the optical element from the substrate. This is particularly advantageous when a curved mirror surface is already almost completely polished. In this case, it may be possible to correct only local defects in the fit.

[0043] In particular, it can be provided that a measurement volume or volume element is formed that extends from the surface to a depth of approximately 5 pm within the substrate body. This allows for improved characterization of the lateral and / or surface-tangential extent of the striae. This is particularly advantageous because the material removed during a deterministic correction in the fabrication process of an optical element is typically significantly less than 5 pm.

[0044] A slightly deeper mapping, particularly from 5 pm to 200 pm, preferably 5 to 500 pm, can be provided. This allows prediction of the appearance of the pass after the aforementioned local correction and / or after a global ablation step to remove material from the substrate body. The aforementioned depths are particularly advantageous because striae can have a typical period of approximately 200 pm. Furthermore, global ablation steps can be performed to a similar depth.

[0045] It is particularly advantageous if the method is used iteratively with deterministic correction steps. Specifically, it can be planned that after one or more polishing and / or correction steps, the substrate body is remeasured using the method and a new correction is planned. This can replace or avoid an extremely complex interferometric measurement of the pass in many cases.

[0046] A processing procedure for this will be disclosed later.

[0047] It may be possible to polarize the exciting light or the measurement radiation and optionally analyze the scattered light using a polarizing filter. Particularly in the case of linear polarization of the measurement radiation, four combinations can be implemented: The incident light can be horizontally or vertically polarized; and / or the detected light can be horizontally and / or vertically and / or circularly polarized.

[0048] The underlying layers of the striae are mechanically strained against each other due to their different coefficients of thermal expansion.

[0049] Perpendicular to the striae, only minor stresses occur because there is no opposing force or constraint. However, when an electric field is applied parallel to a plane of the striae (and thus in an xy-plane relative to the substrate), stresses can cause shifts in the bands of the Raman spectrum, resulting in modulation in the z-direction.

[0050] In order to advantageously suppress a signal caused by the striae, the measuring radiation can preferably be emitted in such a way that its E-field is predominantly perpendicular to the striae.

[0051] To determine the location and / or extent of individual striae, parallel polarization is preferably used.

[0052] In an advantageous further development of the method according to the invention, it can be provided that an immersion fluid is applied to a surface of the substrate body.

[0053] Further improvement of the band sensitivity in Raman spectra acquired using the Raman instrument can be achieved by using an immersion oil and / or a refractive index oil. This results in both higher temperature stability and a better z-focus of the measurement radiation in Raman spectroscopy.

[0054] In an advantageous further development of the method according to the invention, it can be provided that the substrate body is rotationally symmetric and / or is produced rotationally symmetrically by means of a Boule process.

[0055] The inventive method is particularly suitable for examining substrate bodies produced on the basis of a Boule process.

[0056] Mirror blanks produced using a Boule process often show a distinct curvature of bands at inhomogeneities.

[0057] Such phenomena are primarily due to a rotational symmetry of the deposition in the Boule process. In particular, if a Boule center lies significantly away from a section used to form the substrate body, stripe-like inhomogeneities, distinguishable from striae, appear on the mirror blank.

[0058] It may be possible to optimize the integration time on a detector of the Raman instrument and / or the number of measurement repetitions. This allows for the measurement of a significantly lower inhomogeneity of the mirror body.

[0059] In the Boule process, a target is typically rotated, which can result in striae with an amplitude of around 0.15% titanium dioxide, in particular up to 1% maximum-minimum difference or peak valley (PV).

[0060] In particular, the process may involve a material deposited in a Boule process and at least one side surface of the substrate body being mapped in the axial z-direction and / or in the radial direction using a surface-sensitive method.

[0061] The surface-sensitive method may in particular be a microprobe method and / or X-ray fluorescence.

[0062] Alternatively or additionally, it may be provided that a method measuring near the surface, in particular confocal Raman microscopy using the Raman device, is used to determine the spatial distribution.

[0063] Within the scope of the invention, a measurement near the surface is understood to mean a measurement within a depth of 2 mm, preferably less than 50 pm, from the surface.

[0064] In an advantageous further development of the method according to the invention, it can be provided that in step a) several volume elements are measured which are arranged along a reference surface.

[0065] The application of this method is particularly advantageous when the substrate body is disc-shaped.

[0066] The process may involve the substrate being a material deposited in a Boule process, and a highly accurate spatial distribution, in particular a highly accurate mapping of at least one side surface of the substrate, being carried out using a surface-sensitive and / or near-surface measuring method.

[0067] Additionally, a conversion to radial coordinates of the boules underlying the substrate body may be performed. Furthermore, the spatial distribution, particularly in the form of a high-resolution homogeneity map of the substrate body and / or the mirror, may be generated from the preceding conversion.

[0068] The Raman spectroscopy described above is particularly suitable for the structural characterization of glasses, especially titanium-doped quartz glasses from Boule processes.

[0069] The wavenumber of Raman-active modes in glasses typically depends on the structure of the components that make up the glass. In titanium-doped quartz glasses, these components can be ring structures of SiO4 tetrahedra and TiOx polyhedra.

[0070] The structure can influence the wavenumber, particularly through its effective mass and / or chemical bonding. The mode intensities depend not only on the intensity of the incident measurement radiation, the measurement time, and the detector's sensitivity, but also on factors such as polarizability, the population density of the vibrational state, and / or the concentration of the vibrating components in the entire sample.

[0071] Furthermore, as explained later, fluorescence and / or surface roughness also influence the intensity of the bands in the Raman spectrum.

[0072] Furthermore, absorption by the sample or substrate influences the intensity. For excitations near an electronic transition, totally symmetric modes can, under certain circumstances, be disproportionately amplified by a resonance Raman effect.

[0073] In an advantageous further development of the method according to the invention, it can be provided that in step d) the spatial distribution of the homogeneity parameter in the entire substrate body is reconstructed from the measurement information of the volume elements along a reference surface.

[0074] It may be provided that in the process an approximately planar top and bottom surface of the substrate body is mapped, preferably using a method such as confocal Raman spectroscopy.

[0075] Furthermore, it may be provided that a tilting of the substrate body relative to the boule underlying the substrate body and / or a local deviation of the inhomogeneities and / or striae to be measured from a rotational symmetry is determined.

[0076] Alternatively or additionally, the process may involve providing the substrate body, in particular a mirror body, with an already nearly completely formed and / or preferably already polished mirror surface, and measuring it with a confocal and / or quasi-confocal Raman device. Preferably, a measuring head of the Raman device is configured by means of a positioning device to scan a mirror surface while maintaining a surface-normal measuring direction.

[0077] In an advantageous further development of the method according to the invention, it can be provided that the spatial distribution is determined by locating a previously known mapping of the at least one homogeneity parameter in the substrate body.

[0078] This enables efficient reconstruction of the complete mapping from the previously known mapping and a fragment of the spatial distribution based on the measurement information.

[0079] Therefore, a map alignment using a pre-known measurement can be provided.

[0080] It may be possible to reconstruct the position of the substrate body relative to a mapping of the homogeneity parameter previously determined on the boule and / or by utilizing symmetries in and / or on a part of the boule, and / or any tilting and / or rotation relative to a coordinate system of the boule underlying the substrate body. For this purpose, a spoke can be extracted from which, due to rotational symmetry, the map of the entire boule can be determined.

[0081] The previously known mapping may be based in particular on an ultrasound measurement, especially a transit time measurement, and / or an interferometric measurement of the wavefront at the point of passage.

[0082] The determination of the measurement information can provide a relative distribution of the CTE of the substrate body, which can be compared with a CTE distribution of the same substrate body determined beforehand in absolute values.

[0083] This makes it possible to locate individual areas within the substrate body again.

[0084] In an advantageous further development of the method according to the invention, it can be provided that the known mapping is located in the substrate body by identifying at least one pattern of at least a part of the known mapping based on the measurement information of the volume elements.

[0085] The at least one pattern can in particular be relative values ​​of the at least one measurement information and / or the at least one homogeneity parameter.

[0086] Using the preferably employed Raman spectroscopy, relative values ​​of the measurement information can be determined with high efficiency. This allows for the efficient creation of a relative-value-correct mapping within a limited volume segment, i.e., a relative partial mapping.

[0087] The relative partial mapping shows the same patterns as the previously known mapping, even if the absolute values ​​differ. Furthermore, the advantage of using Raman spectroscopy over, for example, ultrasound and interferometry measurements is that Raman spectroscopy is point-selective in three-dimensional space, while the other methods are performed by integrating over a measurement path and therefore usually require plane-parallel surfaces.

[0088] If at least one pattern of the relative sub-mapping can be recognized in the previously known mapping, for example by means of a pattern recognition algorithm and / or by means of artificial intelligence and / or correlation analyses in Fourier space, then in particular the previously known mapping can be superimposed on the relative sub-mapping.

[0089] In order to align the previously known mapping with the relative sub-mapping, a coordinate system of the previously known mapping can preferably be compressed, stretched, rotated and / or translated.

[0090] The embodiments of the method described above are particularly advantageous when a coordinate system for the previously known mapping relative to the substrate body is not known.

[0091] In an advantageous further development of the method according to the invention, it can be provided that the reference surface is used.

[0092] a virtual radial cross-section of the substrate body, and / or

[0093] at least a section of a lateral surface of the substrate body, and / or

[0094] an actual radial cross-sectional area of ​​a spoke of the substrate body, and / or an actual radial cross-sectional area of ​​a sister substrate body of the substrate body, is measured.

[0095] The radial direction here is in particular a radial direction of the rotationally symmetric boules underlying the substrate body.

[0096] The method may include the creation of a spatial distribution, in particular a 3D map, over a total thickness of at least 5 cm using a Raman device in a 90° configuration and / or a quasi-confocal Raman device.

[0097] In particular, the procedure described above can be applied to a, preferably entire, boule and / or a large substrate body. Specifically, it can be provided that the method is used to optimize a combination of a mirror type and a cutout location of the substrate body in the boule. Furthermore, it can be provided that, in the inventive method extended by cutout optimization, an efficiency or yield of at least 90% is achieved when measuring the cutout substrate body, in particular a mirror body.

[0098] In an advantageous further development of the method according to the invention, it can be provided that several volume elements are measured along a line perpendicular to the striae of the substrate body (line scan), and / or that X-ray fluorescence is recorded as measurement information.

[0099] A measurement error in recording the Raman spectrum and / or in determining at least one homogeneity parameter may depend in particular on the parameters chosen.

[0100] The selected parameters can include, in particular, laser intensity, focus spot size, integration time, and / or the number of repetitions. It is especially advantageous if the required resolution is predefined based on the aforementioned parameters.

[0101] For the purpose of predetermining and / or selecting the aforementioned parameters, the previously described, lower-resolution line scan can be performed perpendicular to the striae. This means that several volume elements are measured along a line perpendicular to the striae of the substrate body.

[0102] It may be provided that a maximum-minimum distance or peak-valley distance of the Ti / Si ratio is converted to an advantageously achievable or desirable resolution with respect to the zero-crossing temperature, in particular in units of Kelvin.

[0103] In particular, a previously known, minimal TiO2 fluctuation within the period of the striae can be used for this purpose.

[0104] It may be planned that a calibration curve is determined.

[0105] In an advantageous further development of the method according to the invention, it can be provided that a titanium-doped quartz glass is measured as the substrate body and / or that X-ray fluorescence is recorded as measurement information.

[0106] The inventors have recognized that the relative intensities of titanium-containing glasses can deviate significantly from a linear relationship with the Ti concentration. Furthermore, the inventors have recognized that, in the case of titanium-doped quartz glass, this non-linear behavior of the intensities with concentration can lead to an underestimation of the fluctuations in the titanium content of the striae and inhomogeneities.

[0107] Therefore, it is particularly advantageous to determine a calibration function or calibration curve.

[0108] In particular, it may be provided that the calibration curve is determined by measurements of TiO2-SiO2 glasses with known Ti content.

[0109] For this purpose, in particular, back-calculated mappings of a zero-crossing temperature and / or X-ray fluorescence measurements can be used.

[0110] It is advantageous if the value of at least one measurement piece of information is corrected by the calibration function.

[0111] Furthermore, it is advantageous if the measurement error determined from the striae is corrected by the calibration function.

[0112] It may be necessary to first demonstrate the linearity and / or nonlinearity of Ti-doped quartz glasses. Furthermore, it may be necessary to determine the measurement error of the measurement information and / or the homogeneity parameter based on the calibration curve.

[0113] In this context, quantitative analysis using, for example, X-ray fluorescence (XRF) or glow-discharge optical emission spectroscopy (GD-OES) is particularly advantageous.

[0114] For this purpose, either a spatially resolved measurement, in particular using XRF, can be carried out perpendicular to the striae, whereby a large gradient over an amplitude of the striae enables coverage of a large variation in the titanium content.

[0115] Alternatively or additionally, a measurement, particularly by XRF, can be performed using a sample of titanium-doped quartz glass as a substrate, the substrate preferably exhibiting a known Ti inhomogeneity. Calibration using different samples can also be advantageous, provided they originate from the same blank and / or have undergone the same annealing process. This is particularly beneficial because the relative intensity of Ti and Si can also be influenced by the thermal history of the sample.

[0116] Furthermore, the calibration curve can also be generated from the spatially resolved measurement of the zero-crossing temperature. For this purpose, it may be possible to calculate the titanium concentration using the zero-crossing temperature. It may also be possible to predetermine a maximum tolerable measurement error.

[0117] The maximum tolerable measurement error can be determined, in particular, using the striae from a sample of titanium-doped quartz glass. The measurement error of the intensity ratio can be estimated, for example, from confidence intervals derived from the Poisson distribution of the intensities. Furthermore, the measurement error can be determined from a moving average and a moving standard deviation, with the measurement error of the average decreasing with the square root of n. Here, n represents the number of data points included in the moving average.

[0118] Using the aforementioned embodiments of the method according to the invention, at least one homogeneity parameter can be determined with high reproducibility.

[0119] Striae within titanium-doped quartz glass exhibit a higher Ti variation within a striae period than variations in the relevant inhomogeneity, which determines the zero-crossing temperature. The measurement of striae-independent Ti inhomogeneities benefits from the high sensitivity of the Raman intensity achieved in the inventive method. High reproducibility of the Ti / Si ratio is particularly advantageous in this regard.

[0120] The roughness of ground and / or etched side surfaces and / or back surfaces of the substrate body, especially mirrors or blanks, places particular demands on the Raman resolution of the titanium inhomogeneity, for which the aforementioned embodiments of the method are particularly suitable. This is primarily due to the fact that the Raman resolution is strongly influenced by light scattering.

[0121] The inventors have realized that the measurement error decreases with increasing measurement time.

[0122] Regarding the optimal Raman laser wavelength for investigating Ti-doped or titanium-doped quartz glasses, the inventors have determined that a 532 nm laser has the best signal-to-noise ratio.

[0123] Striae in titanium-doped quartz glass can appear on both polished and rough surfaces. It is particularly advantageous to normalize the Raman spectroscopic data obtained from these observations, allowing for their absolute evaluation.

[0124] It may be possible to determine the relative band intensity of Ti-O to Si-O for quantifying the TiO2 content. For Ti-O, a band at 937 1 / cm is preferably used. For SiO2, a band at 400 1 / cm, 485 1 / cm, 600 1 / cm, or 800 1 / cm may be used.

[0125] The invention further relates to a device with the features mentioned in claim 12. The device according to the invention for spatially resolved measurement of at least one homogeneity parameter in a volume of a substrate body, in particular a substrate body of an optical element of a projection exposure system, comprises at least:

[0126] a measuring device for recording a respective measurement information in at least one volume element of the substrate body,

[0127] a computing device for determining a value of at least one homogeneity parameter from the respective measurement information,

[0128] a position determination device for determining the spatial location of at least one volume element.

[0129] The computing device is configured to determine a spatial distribution of the at least one homogeneity parameter from the spatial position of the at least one volume element and the respective value of the associated homogeneity parameter.

[0130] The device according to the invention has the advantage that the spatial distribution of the at least one homogeneity parameter can be digitally reconstructed by means of the appropriately configured computing device.

[0131] In an advantageous further development of the device according to the invention, it can be provided that the measuring device has a Raman device for detecting a Raman spectrum as measurement information in the at least one volume element of the substrate body.

[0132] It is particularly advantageous to use Raman spectroscopy for the detection of Ti content, especially in titanium-doped quartz glass.

[0133] Titanium-doped quartz glass often has a layered structure due to its production in a so-called Boule process, caused by the deposition process.

[0134] The period of the resulting striae can be 100 pm to 400 pm, in particular 200 pm.

[0135] The layer streaks can be oriented approximately parallel to a top surface of the blank.

[0136] In other words, it can be provided that the substrate body is manufactured in such a way that the streaks are arranged at least approximately parallel to a top surface of the substrate body. This can be achieved in particular by cutting the substrate body blank horizontally from a boule and not by reshaping it.

[0137] However, it can happen that the layered streaks exhibit a slight curvature and a more pronounced upward slope towards the original edge of the boule. The layered streaks regularly differ from their surroundings in that they have altered titanium dioxide contents.

[0138] Amplitudes of approximately 0.15 wt% titanium dioxide can occur. However, such a variation in titanium dioxide content also means a variation in the zero-crossing temperature of approximately 9 K peak-to-valley (PV) and spatial gradients of typically 45 K per cm.

[0139] In extreme cases, fluctuations in titanium content of up to 1% can occur, and / or periods of 100 pm can occur, resulting in larger gradients of 50 K per cm to 150 K per cm, and in particular more than 1 K per cm, due to the smaller spacing of the layer streaks. Such variations may be unacceptable under certain circumstances.

[0140] Typically, inhomogeneities that are relevant when selecting blanks for the substrate body or when correcting the fit during processing of the substrate body for a later operating temperature only occur at gradients of a maximum of 1 Kelvin per cm.

[0141] This applies particularly to an area of ​​the blank which is located near the reflective surface of the optical element at a later stage of the manufacturing process.

[0142] In the context of the invention, a passe can be understood in particular as a specifically produced shape of the substrate body designed as a mirror body prior to the application of any coatings.

[0143] It may be provided that in the aforementioned further development of the device according to the invention, a top surface of the blank is measured using a surface-sensitive method, such as confocal Raman spectroscopy with a short focal length or an X-ray fluorescence method.

[0144] In this case, the striae are only measured or cut at a shallow angle, which makes their spatial frequency in an area of ​​the surface appear erroneously to be part of the set of tolerable inhomogeneities.

[0145] The problem here is that the amplitude, measured around the vibration center and not just at the peaks, is approximately five times larger than the values ​​determined by confocal Raman spectroscopy and / or X-ray fluorescence. This prevents a meaningful separation of those macroscopic inhomogeneities that are relevant for assessing the suitability of the blank for optical element production. This is especially true when using a surface-sensitive method such as X-ray fluorescence, microprobe analysis, X-ray photoelectron spectroscopy, and / or electron paramagnetic resonance spectroscopy, and / or a method with limited penetration, such as many implementations of confocal Raman microscopy in commonly used standard settings.

[0146] The diameter of a measurement spot in the Raman instrument, and thus the volume element, can preferably be configured to range from a few micrometers to a few millimeters, depending on the objective. Larger diameters offer the advantage of allowing more light into the detector of the Raman instrument, thereby reducing noise, shortening measurement time, and decreasing the amount of data.

[0147] With larger beam diameters or diameters of the measurement spot, which can exceed 10 pm, especially several hundred pm, the striae that usually occur are no longer resolved, which may be advantageous under certain circumstances.

[0148] It may be provided that the length of a beam waist or the extent of an active measuring volume of the Raman device within the blank or the substrate body or its volume is designed at least approximately below the side surface in such a way that the extent of the active measuring volume does not significantly influence the acquisition of the measurement information.

[0149] This can be achieved in particular due to a rotational symmetry of the boules, which results in only slight changes occurring in a direction perpendicular to the side surface, which is designed as a cylindrical shell.

[0150] It can be advantageous if the active measurement volume is focused so far into the substrate that detection only begins 50 pm to 200 pm, preferably 100 pm, below the surface. This means that such a measurement is not dependent on a rough, disturbed, and / or contaminated surface in the area of ​​the side face.

[0151] It is particularly advantageous if the beam waist is dimensioned in such a way that efficient and / or low-noise measurement can be carried out.

[0152] The features and explanations described above are particularly important in connection with confocal Raman microscopy and thus in connection with a Raman device designed as a confocal Raman microscope.

[0153] Alternatively or additionally, a pseudo-confocal setup can be used. In this setup, one or more laser beams can be directed past an objective lens of the Raman device into a focal area of ​​the lens. The Raman device can be configured to include a radiation source. Preferably, the radiation source is designed to generate a measurement beam, particularly in the form of a laser beam.

[0154] It may be provided that the measurement radiation has a wavelength spectrum within a visible range, in particular a line spectrum at 532 nm.

[0155] Furthermore, it may be provided that the radiation source is set up to generate parallel and / or collimated measurement radiation.

[0156] Alternatively or additionally, it can be provided that the measurement radiation is focused by optics of the Raman device.

[0157] It is particularly advantageous if the beam waist of the laser beam and the point spreading function of the lens overlap as closely as possible.

[0158] Alternatively or additionally, it may be provided that the radiation source is set up to generate several laser beams of the same and / or different wavelengths simultaneously and / or at different times.

[0159] The use of multiple laser beams, which preferably overlap only within the active measurement or detection volume, advantageously reduces the stress on the surface of the substrate body or blank. The surface can be more sensitive than the solid material within the blank or substrate body due to processing damage and / or contamination.

[0160] Alternatively or additionally, the radiation source can be configured to generate pulsed beams. In particular, the pulsed beam can be designed such that the measurement radiation can excite Raman scattering at least approximately exclusively within the overlap volume through two-photon absorption.

[0161] Such a method based on two-photon absorption is particularly advantageous when the absorption of the material under investigation, the blank and / or the substrate body, along beam paths of the measurement radiation is too high at a desired short excitation wavelength and / or the material would be damaged at too high a power density of the measurement radiation at shorter wavelengths.

[0162] Typical titanium-doped quartz glasses have only a small amount of Ti. 3+This results in such quartz glasses exhibiting only weak and broadband absorption of less than 1% per cm. Therefore, a sufficiently high Raman scattering can be generated using a measuring radiation, which is designed as the light of a continuous-wave laser and preferably has a wavelength of 532 nm.

[0163] In particular, the use of two-photon absorption offers a potential advantage due to a potentially higher spatial resolution, since the two-photon condition is maintained only in a smaller volume.

[0164] Especially in the case of titanium-doped quartz glass from a so-called SOOT process, i.e., a manufacturing process from particles, with a lower OH content and a higher Ti content 3+ The use of two-photon excitation may be advantageous in some cases.

[0165] Alternatively or additionally, excitation using time-shifted pulses and / or excitation with multiple wavelengths can be provided. This allows further bands of the Raman spectrum and / or further species to be detected via nonlinear and / or stimulated Raman scattering.

[0166] It will be explained later that pulsed radiation can also be used to bleach the volume element.

[0167] However, as the inventors have recognized, this is advantageous for the sufficiently sensitive determination of the ratio of TiÜ2 to SiÜ2, which is explained below, but is not absolutely necessary.

[0168] In an advantageous further development of the device according to the invention, it can be provided that a ratio of TiÜ2 to SiÜ2 can be determined as measurement information and a coefficient of thermal expansion can be determined as a homogeneity parameter in the volume element.

[0169] If the ratio of titanium dioxide to silicon dioxide is used as measurement information, the inventors believe that a particularly reliable prediction of the spatial distribution of the coefficient of thermal expansion can be determined.

[0170] Striae pose a particular machining problem because the material removal rate during machining of the substrate depends on, or fluctuates with, the titanium content. Furthermore, it may be necessary to perform a high-resolution measurement of the shape of a future mirror surface or a fit measurement so that high-frequency errors in the future mirror surface or fit errors can be corrected deterministically, particularly by a robot and / or an ion beam.

[0171] A high-resolution measurement using the device according to the invention, particularly on a side surface of the substrate body, allows a prediction as to whether the investigated substrate body or blank is suitable for a specific type of mirror. Furthermore, it enables a prediction of where the striae will penetrate or terminate on the future mirror surface. In particular, in conjunction with a scanning measurement of a mirror surface of the substrate body that has already been polished within predetermined specifications and which may exhibit local fitting errors with, for example, a lateral extent of several centimeters, data for deterministic processing of the mirror surface can be obtained using the device according to the invention, especially with the Raman device, without the need for an interferometric measurement of the mirror surface.

[0172] Interferometric measurement requires corrective optics or a test cascade and can only be reliably performed when the mirror surface is already approximately in a target shape or a target fit.

[0173] The knowledge of the striae obtained by the device according to the invention allows for earlier deterministic correction and saves expensive setup and measurement time in the test cascade.

[0174] For the thermal behavior of the substrate body or the optical element, in particular mirror heating or pass at operating temperature, the striae may be of minor importance due to their small thickness.

[0175] If the goal is merely to obtain a precise homogeneity map or to recover the registration of a previously known mapping already determined on the boule underlying the substrate body, the inventors have recognized that dissolving the striae offers no advantage and may even be detrimental.

[0176] It may therefore be possible to design a laterally large volume element or large measurement spot of the Raman device for this purpose and / or to obtain the homogeneity data from the acquired high-frequency data by means of computational low-pass filtering.

[0177] In an advantageous further development of the device according to the invention, it can be provided that a positioning device is available which positions the measuring device to the substrate body in such a way that the measurement information can be detected in the at least one volume element.

[0178] The positioning device can, in particular, enable scanning of a side surface of the blank.

[0179] It may be provided that a side surface is scanned using a Raman method, in particular Raman spectroscopy and / or Raman microscopy using the Raman device.

[0180] It may be provided that water and / or an index-matched immersion fluid is used as the immersion medium, thus enabling the measurement of rough surfaces of the blank or substrate body. In the case of curved and / or complexly shaped side surfaces, it may be provided that a negative mold or matrix, preferably as a mounting plate, is used, which is preferably made of quartz glass and / or titanium-doped quartz glass.

[0181] In this case, it is particularly advantageous if the tracking of a position of a focus of the Raman device is programmed based on the known shape of the matrix.

[0182] The positioning device can preferably be configured to tilt an excitation and a detection beam of the Raman device relative to a plane of the striae by 1° to 10°, preferably 2° to 5°, particularly preferably 4°.

[0183] This reduces diffraction effects. It is particularly advantageous if the detection volume or volume element is significantly longer than the average distance between the striae. Alternatively or additionally, such a tilt is also advantageous if the detection volume is located far from the surface within the blank.

[0184] Particularly when dealing with complexly shaped surfaces of the blank or substrate body, it is advantageous to mount and use a confocal Raman microscope as a Raman device on a robot arm as a positioning device. Preferably, the positioning device is configured to swivel in at least two planes.

[0185] Knowledge of the radial coordinates of the volume elements to be measured is advantageous. Preferably, the positioning device is also configured to rotate the blank or substrate body. This makes it possible to convert the measured data to the entire blank in three dimensions, assuming rotational symmetry in the boule, and thus to determine the spatial distribution of at least one homogeneity parameter.

[0186] In an advantageous further development of the device according to the invention, it can be provided that the measuring device has a Fourier-transform infrared spectrometer for detecting an infrared spectrum of the at least one volume element.

[0187] The inventors recognized that the use of a Fourier-transform infrared (FTIR) spectrometer is particularly advantageous for acquiring an infrared spectrum. The infrared spectrum can provide further and supplementary information. Accurate and high-resolution mapping of at least one homogeneity parameter is especially possible through a combination of FTIR and Raman spectroscopy or Raman microscopy.

[0188] FTIR has advantageously low noise, but FTIR and normal IR transmission measurements often require plane-parallel surfaces and the measurement is performed integrating along the beam path. OH determination using Raman may exhibit higher noise, but has the advantage of being applicable in three dimensions and can advantageously be performed together with Ti determination.

[0189] For this purpose, it may be possible, in particular, to map the blank in at least one measurement direction in two dimensions and, in addition, to measure spatially distributed measurement points or volume elements using the Raman device. The data thus acquired can preferably then be combined to form a three-dimensional map, i.e., a spatial distribution of the at least one homogeneity parameter.

[0190] Infrared spectroscopy is particularly advantageous for determining OH content.

[0191] The OH content can be reliably determined, particularly by transmission measurements in the water bands. Transmission measurements at a wavelength of 2.75 pm are especially advantageous.

[0192] Transmission measurements are typically performed by integrating along a given measurement path. For conventional spectrometers, FTIR spectrometers are particularly suitable for the infrared range being measured.

[0193] However, the aforementioned FTIR spectroscopy often only allows for an incomplete three-dimensional mapping in a non-destructive manner, since the integrating measurement principle, via an integration path along the measurement path with increasing measurement depth, prevents the extraction of information about where along the measurement path the inhomogeneity to be detected is located.

[0194] A combination with a measurement of the substrate body using the Raman device is therefore particularly advantageous.

[0195] The device may be configured for tomographic reconstruction. In this case, a particularly high signal-to-noise ratio is desirable.

[0196] Using the FTIR spectroscopy described above, an advantageously high three-dimensional resolution can be achieved if thin edge slices, i.e., thin partial segments of the cylindrical shell of the blank, are cut off and mapped over their entire surface. While this allows for high-resolution measurement of their area, statements about the inner volume of the blank can only be made by means of a potentially error-prone extrapolation. In an advantageous embodiment of the device according to the invention, the Raman unit can be configured to perform confocal Raman spectroscopy.

[0197] The device can be configured to measure the OH content as measurement information using the Raman device. In particular, a combination with the previously described FTIR spectroscopy can be especially advantageous.

[0198] The Raman device for measuring the OH content may be configured with a 90° setup, a double 45° setup, and / or a quasi-confocal setup. This allows for the use of high laser powers for the measurement radiation, which in turn can lead to improved sensitivity.

[0199] It may be possible to use the Raman array in a 90° configuration, a 2x 45° configuration, and / or a quasi-confocal configuration. For this purpose, the foci of the excitation beam and the detection beam path may coincide.

[0200] In an advantageous embodiment of the device according to the invention, it can be provided that an irradiation device is available and configured to bleach the at least one volume element by means of bleaching radiation, and / or

[0201] A temperature control device is available and set up to at least partially temperature-control the substrate body, and / or

[0202] A temperature measuring device is present and set up to record the temperature of the substrate body.

[0203] The presence of the irradiation device is particularly advantageous in combination with the Raman device, and especially in the measurement of titanium-doped quartz glass.

[0204] In titanium-doped quartz glass or TiO2-SiO2-glass systems, charge-transfer transitions or CT transitions may occur, in which an electron from the oxygen atoms is transferred to an empty d-orbital of the Ti atom. 4+ is transferred, which is subsequently referred to as Ti 3+ This is present. As a result, the intensities of Raman-active modes may change, since a proportion of Ti 4+ Ü4 decreases.

[0205] Depending on the wavelength of the measurement radiation or the incident laser, a resonance Raman effect and / or fluorescence can occur. The resonance Raman effect is stronger the smaller the energy difference between O and Ti. 4+ The transition to the excitation wavelength occurs. The aforementioned CT transition further alters the absorption and thus the penetration depth of the laser or the measurement radiation, which can particularly increase positional inaccuracies.

[0206] Furthermore, errors in Raman band intensity can be negatively affected by fluorescence phenomena. Such fluorescence phenomena can originate from a surface area, for example, from surface deposits of organic substances. In addition, such fluorescence phenomena can also originate from bulk material within the substrate under investigation.

[0207] Fluorescence phenomena often shift a background signal in the Raman spectrum being acquired. If background subtraction is performed without considering the fluorescence, an error may occur due to the subtraction process.

[0208] Interfering Raman modes, which originate from impurities, can also negatively affect the analysis. This is because these interfering Raman modes are measured together with so-called glass modes originating from the titanium-doped quartz glass being analyzed. This can lead to inaccurate determination of the glass modes. In other words, the bands overlap, and the sum of the bands is measured.

[0209] This prevents another band from being superimposed on the desired glass mode, which would cause an apparent tilting of the mode. This, in turn, prevents the center of gravity and / or amplitude from being incorrectly determined.

[0210] Temporal gating of the detector relative to the exciting laser pulse can be implemented. In particular, to avoid the aforementioned problem, a short and tunable detector gate can be provided in the Raman setup.

[0211] Preferably, the temperature measuring device is configured to measure the temperature in the at least one volume element, in particular at the point of measurement.

[0212] Using a different Raman laser wavelength for the measurement radiation can potentially have a positive effect on luminescence, as luminescence may be wavelength-dependent. However, using a different Raman laser wavelength can be detrimental for homogeneity testing or the investigation of the homogeneity parameter in a system of Ti-doped quartz glasses due to a poorer signal-to-noise ratio.

[0213] Fluorescence phenomena in a bulk material of the substrate body can be induced, for example, by titanium accumulations, especially in the form of nanocrystals, in the titanium-doped quartz glass to be measured.

[0214] Because the irradiation device is present and set up to bleach at least one volume element using bleaching radiation, the fluorescence phenomena can be effectively suppressed.

[0215] To increase measurement accuracy, particularly the stability of the Ti / Si band ratio, during Raman measurements of Ti-doped quartz glasses, laser bleaching can be used. In this process, laser light is preferably generated or used as the bleaching radiation. The bleaching radiation preferably has a laser wavelength of 532 nm. This can particularly involve bleaching at the location of the subsequent Raman measurement, i.e., in-situ bleaching.

[0216] Bleaching or photobleaching can also be used alternatively or additionally for organic materials, such as pigments.

[0217] A reduction in measurement error regarding the determination of the Ti / Si band ratio of the striae can be achieved for Ti-doped quartz glasses by bleaching. Here, bleaching is preferably carried out by laser irradiation of the respective volume element of the Raman measurement before the Raman measurement is started on the volume element. When using a laser with a power of 80 mW, irradiation with the bleaching radiation or bleaching for at least 2 minutes, preferably more than 4 minutes, is particularly advantageous for measuring titanium inhomogeneity in Ti-doped quartz glasses.

[0218] Fluorescence phenomena can exhibit a temporal dependence. Such a temporal dependence is particularly possible for organic or organic-chemical materials. For crystalline materials, Ti 3+ At low concentrations, they may also be potentially luminescent.

[0219] Another possibility for a time-dependent Raman sensitivity lies in a single-photon absorption that is influenced by scattered light.

[0220] The time dependence of the Ti / Si Raman intensity on Ti-doped quartz glass can be demonstrated, in particular, by repeat measurements with identical measurement parameters at a constant measurement position. The time dependence of the Ti / Si ratio can be determined by pre-irradiation.

[0221] The inventors have recognized that a reduction in error regularly occurs with the measurement time, particularly at a measurement radiation wavelength of 532 nm. This reverse reaction can exhibit a time constant of more than 30 minutes.

[0222] It may be provided that the irradiation facility is equipped to carry out pre-irradiation of the substrate body with bleaching radiation (pre-bleaching).

[0223] To reduce the measurement time with the Raman device for determining the at least one homogeneity parameter and / or for performing the inhomogeneity measurement, pre-irradiation can be carried out. Pre-bleaching is preferably performed by irradiating the at least one volume element with laser radiation as bleaching radiation. The laser radiation preferably has a wavelength of 532 nm and a power of more than 50 mW.

[0224] Alternatively or additionally, pre-irradiation can be achieved by using at least one green LED to generate the bleaching radiation. The inventors have recognized that pre-bleaching using broadband green LED light is possible in an efficient manner.

[0225] It may be provided that the pre-irradiation is carried out until saturation and / or a stable state is reached. In particular, it may be provided that the pre-irradiation takes place over a period of at least 30 minutes. According to the inventors' findings, a reverse reaction of the bleaching process takes more than 30 minutes. However, since the reverse reaction increases the measurement error again, it is advantageous to start the Raman measurement directly after pre-bleaching or pre-irradiation.

[0226] For a large number of measurement points, intermediate irradiation or bleaching may be necessary. It is particularly advantageous to combine the aforementioned in-situ bleaching, performed during the Raman measurement, with pre-irradiation or pre-bleaching.

[0227] The irradiation device may include a pulsed laser for the preferred formation of bleaching radiation with a wavelength of 532 nm.

[0228] A pulse duration of picoseconds to nanoseconds can be specified.

[0229] Since luminescence is based on a slower process than Raman scattering, a pulsed 532 nm laser can be used.

[0230] For this purpose, the use of a gated detector system as part of the Raman setup is particularly advantageous. The implementation of detection time windows enables time-resolved photon detection. This allows luminescence to be excluded from the measurement.

[0231] Another advantage is the presence of the temperature control device for monitoring or adjusting the temperature of the volume elements of the substrate body to be measured.

[0232] The temperature control device can be configured for temperature monitoring with an error tolerance of less than ±0.1 °C. This allows for advantageously high accuracy in determining the TZC, in particular an accuracy of 1 K. Alternatively, the temperature control device can be configured for temperature monitoring with an error tolerance of less than ±0.1 mK. This allows for advantageously high accuracy in determining the TZC, in particular an accuracy of 0.1 K.

[0233] The Raman intensities that can be determined in a Raman spectrum of the respective volume elements are generally dependent on the temperature prevailing in that volume element. It may be the case that for compounds where disorder increases with temperature, the Raman intensities of some modes are also strongly temperature-dependent. This can be caused, in particular, by a Bose-Einstein occupancy factor.

[0234] To minimize the dependence of Raman intensities on temperature fluctuations of glasses in general, and of titanium-doped quartz glasses or SiO2-TiO2 glasses in particular, it may be possible to acquire the measurement data at temperatures that deviate from room temperature. Specifically, it may be possible to set a temperature below room temperature using the temperature control device.

[0235] This allows for high sensitivity for Ti / Si homogeneity measurement.

[0236] The temperature control system may include a heating plate and / or a cooling plate. Alternatively or additionally, the temperature control system may include a temperature-controlled sample chamber with a thermostat.

[0237] Furthermore, the temperature control unit can be configured to operate in a protective gas atmosphere. This helps to avoid additional scattering effects.

[0238] Preferably, the temperature control device is configured to reduce the temperature during measurement by the Raman device. By reducing the temperature during measurement, the dependence on disorder in the system can be reduced, thus increasing band sensitivity.

[0239] Furthermore, a transition probability for electronic transitions, especially of Ti, can also be calculated.4+ to the 3+ , will be reduced.

[0240] This can reduce the previously described required bleaching time. This, in turn, can reduce the measurement time.

[0241] The temperature control unit allows for efficient dissipation of heat input from the laser energy through active cooling. Alternatively or additionally, passive temperature measurement can be performed using the temperature measuring device, followed by correction, particularly using a Bose-Einstein equation.

[0242] For this purpose, it is particularly advantageous if the temperature measuring device is designed to measure the temperature over the largest possible sample range with the sensitivity specified above.

[0243] The invention further relates to an optical element having the features mentioned in claim 19.

[0244] The optical element according to the invention, in particular a mirror of an EUV projection exposure system, comprises at least one substrate body. According to the invention, the substrate body is at least partially manufactured using the aforementioned method and / or the aforementioned device according to the invention.

[0245] The optical element according to the invention benefits in particular from the application of the device and / or method according to the invention in its manufacture.

[0246] In particular, compared to the state of the art, the optical element exhibits superior microscopic properties with regard to the homogeneity of the coefficient of thermal expansion and a highly precisely machined surface, since striae and inhomogeneities with regard to a titanium dioxide content, especially in titanium-doped quartz glass, can be taken into account.

[0247] The optical element can, in particular, be a mirror for EUV lithography made of titanium-doped quartz glass from a Boule process. The mirror is preferably measured using the method according to the invention, wherein the data obtained by means of the method according to the invention were used to ensure that the mirror surface or shape corresponds to a target shape to a greater extent at an operating temperature of the mirror than at room temperature.

[0248] In particular, the optical element may be a mirror for EUV lithography with a diameter of more than 1 m. Furthermore, the mirror may be monolithic, at least in the lateral direction. Finally, the homogeneity may be measured using the method according to the invention.

[0249] The optical element can be a mirror for EUV lithography, since it was manufactured in such a way that a fit allowance is formed based on the measured values ​​determined with the method according to the invention, so that, due to the fit allowance, the shape of the mirror corresponds to a target shape at an operating temperature.

[0250] It may be provided that the optical element according to the invention is a mirror for EUV lithography, which is mapped in at least one volume region near a mirror surface laterally and / or axially to the substrate body, and / or tangentially or normally to the mirror surface, in a finer grid than in the mirror volume and / or further out on the substrate body.

[0251] The optical element can be a cooled mirror for EUV lithography, in which the material of the substrate body above at least one cooling channel and / or the walls of the at least one cooling channel has a grid or volume elements of less than 1 mm. 3 preferably smaller than 0.5 mm 3 , especially preferably smaller than 0.1 mm 3 is measured.

[0252] The optical element according to the invention can be a mirror in which a mapping is measured after the introduction of the cooling channels, preferably mechanically, by means of bonding and / or laser ablation, using the method according to the invention.

[0253] It may be provided that a surface correction for use at a later operating temperature has been or is being carried out based on the mapping or the determined spatial distribution. It may also be provided that the pass achieves an accuracy of less than 0.1 nm.

[0254] The optical element can be a reticle or mask for a projection exposure system, which extends in its full thickness and / or laterally at least within an optically used volume with a resolution or a volume element size of no more than 2 mm. 3 is mapped. Furthermore, the mask can be designed such that its pass is corrected based on the spatial distribution or map created by means of the inventive method for an expected operating temperature, in particular an expected spatial operating temperature profile.

[0255] The optical element can be designed so that the thermal expansion coefficient of the substrate increases strictly monotonically between at least -150 and +120°C. Whether the thermal expansion coefficient exhibits a zero crossing can be defined or predetermined by the titanium content. The titanium content is preferably chosen such that a zero crossing occurs.

[0256] Depending on the application, the zero crossing can be selected at a temperature between 0°C and 60°C.

[0257] This section discloses a processing method for an optical element.

[0258] In the disclosed processing method, a deterministic fit correction is provided based on a spatial distribution of the homogeneity parameter determined by means of the inventive method and / or the inventive device.

[0259] In particular, deterministic fit correction can be performed based on a high-resolution Raman measurement of a side surface and / or a subsequent mirror surface of the substrate body. It may be possible to apply the measurement and the deterministic fit correction iteratively.

[0260] Furthermore, the disclosed processing method may include a provision for a correction for variations in the titanium dioxide content of a titanium-doped quartz glass in the form of striae, already for a later operating temperature.

[0261] Furthermore, the inventive method and / or device can be used to determine the local location of inhomogeneities and / or striae. Additionally, post-processing of the substrate and / or selection of a tilt of a mirror surface can be provided to optimize the location and / or spatial frequency of sectioned striae with regard to their correctability and effect.

[0262] Furthermore, it may be provided that a measurement at a depth of several millimeters is carried out to detect the inhomogeneities, preferably independently of any, in particular local, course of the striae.

[0263] It is particularly advantageous to reconstruct the spatial distribution of the homogeneity parameter or the homogeneity map using data from measurements of a side surface of the substrate. Preferably, measurement data from the top and / or bottom surface are used, either alternatively or additionally. Thus, reconstructing the homogeneity map from data from the top and bottom surfaces alone, from data from the side surfaces alone, and / or from a combination of data from the top, bottom, and side surfaces is advantageous, especially using surface-sensitive methods or methods that measure near the surface.

[0264] The disclosed processing method may include the possibility of correcting the striae for a later operating temperature.

[0265] Furthermore, a substrate body, in particular a mirror body for an EUV projection exposure system, is disclosed at this point.

[0266] The disclosed substrate body, in particular a mirror body, is preferably produced by a forming process or has been subjected to a forming process. In the disclosed substrate body, a map transformation is corrected after forming by near-surface measurement using the device and / or method according to the invention.

[0267] Alternatively or additionally, a new spatial distribution in near-surface regions of the disclosed substrate body is determined using the inventive method and / or the inventive device. Preferably, the spatial distribution is used to calculate a pass allowance, so that the pass allowance is designed based on the calculation.

[0268] The substrate body according to the invention, in particular the mirror body, can consist of several axially stacked and bonded blanks or sub-substrate bodies. Preferably, a rotation and / or displacement of the sub-substrate bodies relative to their respective origin is optimized from the spatial distribution or 3D maps determined by means of the device and / or the method according to the invention.

[0269] The substrate body according to the invention can be a substrate body made of a soot material.

[0270] It may be possible to determine and / or map the CTE homogeneity of the Soot blank by mapping the Ti content using Raman spectroscopy and / or the OH content using transmission spectroscopy. Furthermore, the Ti content and / or OH content data may be combined.

[0271] Alternatively or additionally, it may be provided that Raman spectroscopy is used for three-dimensional resolved mapping of the OH content instead of transmission spectroscopy.

[0272] Alternatively or additionally, it may be possible to supplement an integrating transmission measurement using transmission spectroscopy with three-dimensional support points from Raman spectroscopy.

[0273] The invention further relates to a lithography system having the features mentioned in claim 20.

[0274] The lithography system according to the invention, in particular a projection exposure system for semiconductor lithography, comprises an illumination system with a radiation source and optics comprising at least one optical element. According to the invention, it is provided that at least one of the optical elements

[0275] a substrate body which is at least partially measured using the device according to the invention, and / or

[0276] a substrate body which is at least partially measured using a method according to the invention and / or

[0277] at least partially an optical element according to the invention.

[0278] It may be provided that at least one of the optical elements

[0279] a substrate body which is at least partially produced using the device according to the invention and / or

[0280] comprising a substrate body which is produced at least partially using a method according to the invention and / or a disclosed processing method.

[0281] The lithography system according to the invention comprises optical elements, in the case of an EUV projection exposure system mirrors, which are processed particularly reliably due to the measurement according to the invention and the manufacture or processing based on the measurement according to the invention.

[0282] The microscopic properties of the optical elements used in the lithography system according to the invention are therefore superior to the prior art, particularly with regard to the correction of striae and / or inhomogeneities of a titanium content.

[0283] The device and / or method according to the invention, or their further developments, can in particular avoid or solve the problems described below.

[0284] Firstly, substrate bodies, especially EUV blanks, are often inaccurately cut out relative to a pre-existing three-dimensional homogeneity map.

[0285] Using the device and / or method according to the invention, the coordinate system of a previously known homogeneity mapping can be recovered or reconstructed.

[0286] Secondly, substrate bodies, especially EUV blanks for mirrors in a high-NA EUV projection system, are often so large that destructive measurement of the spatial distribution of the homogeneity parameter is not possible. For this purpose, similar substrate bodies or blanks can be destructively measured, and a similarity can be established based on production date, machine condition, and rough axial measurements of the ultrasonic velocity. Using the device and / or method according to the invention, the complete spatial distribution or a full 3D map, at least of the topmost boule from a stack of boules, can be provided.

[0287] Thirdly, with methods known from the prior art, a resolution of 5 mm x 5 mm for the spatial distribution or homogeneity map in the radial r-direction and the axial z-direction of the rotationally symmetric substrate body or boules is often insufficient. In the r-direction, an interferometer can typically achieve a resolution of 1 mm. However, in this case, the data are disturbed by high-frequency artifacts.

[0288] To avoid excessive phase differences when using the interferometer to irradiate the substrate parallel to the striae, the sample can be tilted so that the irradiation does not occur along individual striae. However, this limits the z-resolution to approximately 3 mm for a sample approximately 2-3 cm thick, regardless of the interferometer resolution. This is due to the spatial smearing caused by tilting the substrate. Using the device and / or method according to the invention, a spatial distribution with a resolution of 1 mm x 1 mm or better can be achieved.

[0289] At this point, another possible and advantageous embodiment of the method according to the invention is described below, which can also be advantageously carried out using the device according to the invention.

[0290] In the embodiment described above, the execution of steps a) to d) of the method according to the invention involves measuring quartz glass as the substrate body, wherein the quartz glass is preferably characterized as a homogeneity parameter based on a spatial distribution of the hydroxyl concentration and / or the spatial distribution of the OH content and / or a spatial distribution of a hydrogen concentration or an H2 concentration.

[0291] In particular, synthetic quartz glass as a substrate can be measured with respect to its specific spatially distributed OH content and / or H2 content using a Raman setup and / or Raman spectroscopy. Alternatively or additionally, a Fourier-transform infrared (FTIR) spectrometer can be used.

[0292] The production of a large number of lens blanks with varying geometries and homogeneity requirements may be planned. Therefore, it may be necessary to optimize the utilization of the lens blank using a computer based on many possible delivery blanks. This allows for a prediction as to whether, and if so, with what probability, the blank cut from the lens blank will meet the requirements placed on the substrate body and / or the optical element.

[0293] It may be stipulated that the cut blank be subjected to a z-integrating homogeneity measurement. Furthermore, it may be stipulated that inhomogeneities running diagonally, due to a burner signature, and / or horizontally, due to events during deposition, are integrated. This may result in a loss of information. At the same time, errors from the measurement and, in particular, from the polished surface are added.

[0294] In the described embodiment, a combination of the above-described measurement of synthetic quartz glass as a substrate body with regard to the specific spatially distributed OH content and / or the specific spatially distributed H2 content can be carried out with a reconstruction of a property distribution, in particular the determination of the spatial distribution of the at least one homogeneity parameter according to step d), utilizing the rotational symmetry of the substrate body. For this purpose, a measurement of a sample can be carried out. The sample is preferably taken from the substrate body, in particular the boule, or from a part of the surface of the substrate body, in particular the boule.

[0295] It may be provided that the accuracy of the determined spatial distribution of the at least one homogeneity parameter and / or the mapping and / or a rotational symmetry is 0.1 cm to 5 cm, preferably 1 cm.

[0296] Alternatively or additionally, it may be provided that the accuracy of the determined spatial distribution of the at least one homogeneity parameter and / or the mapping and / or a rotational symmetry is given by a defined fraction, in particular one per mille, of a sub-aperture diameter of the optical element to be manufactured of the projection exposure system and / or of a signed sub-aperture ratio of the optical element to be manufactured of the projection exposure system.

[0297] In the embodiment of the method according to the invention described above, it can be provided that the measurement in step a) is carried out on at least one strip or cut-out strip.

[0298] The data collected in this way can be used, in particular, for selecting the material and / or the section of the substrate to be used. Specifically, a corresponding three-dimensional map can be created and provided.

[0299] It may also be provided that the location of the previously known mapping or map positioning described above is carried out and, in particular, improved by at least one measurement on the previously described reference surface, the blank, and / or the cut-out strip, in particular a small witness strip, close to the blank.

[0300] A check of the lateral cutting accuracy of the spoke and / or the reference surface can preferably be carried out by measuring a blank in a passage geometry.

[0301] It may be provided that, in carrying out the method according to the invention, the blank of the substrate body or the optical element has an excess. Alternatively or additionally, the measurement of the blank, which has already been formed into a cylindrical shape, and a comparison with the mapping may be provided.

[0302] Due to z-integration during an integrating measurement, a reconstruction with a resolution of approximately 5 mm can be achieved. If the blank still has a rectangular excess, a transverse measurement can also be performed to determine the z-coordinate when locating the previously known mapping. Since the glass of the substrate body may exhibit so-called event-related striae in the transverse direction, in addition to the previously described striae, which can, for example, have a period of approximately 2 mm, a reconstruction of the z-coordinate with an accuracy of less than 1 mm can be achieved by comparing it with the previously described measurement on the cut-out strip.

[0303] Particularly in the case of excess material, the reference surface can be provided by obtaining one or more thin slices that are partially or at least approximately completely cut parallel to an r-coordinate of the substrate body's boules. Alternatively or additionally, a penetration measurement integrating in a circumferential direction can be enabled, particularly by grinding windows on a surface of the substrate body or the boules.

[0304] Alternatively or additionally, a core sample can be taken from the boule. Since the glass may exhibit a strong striae structure, an interferometric transverse measurement of the cut strip and / or the witness samples can be performed under a tilt of several degrees.

[0305] The inventors have recognized that optical inhomogeneity of the substrate, and in particular of synthetic quartz glass, can be caused by and / or closely correlated with spatial variations in the OH and / or Fh content. Specifically, the inventors have recognized that the Fh content can be "smeared" after annealing due to a faster diffusion rate compared to OH species.

[0306] Alternatively or additionally to the homogeneity measurements described above, measurements in a transverse direction can be performed to determine stress birefringence, particularly using optical shadowing methods, transmission spectroscopy, especially in the water band region at wavelengths of 1.4 pm, 2.3 pm, and / or 2.7 pm, and / or transmission spectroscopy at ultraviolet and / or infrared edges. Furthermore, measurements in the transverse direction can be carried out using the Raman device or Raman spectroscopy and / or ultrasound. The use of the Raman device, in particular, advantageously eliminates the need for transmission measurements with two finely ground and / or polished opposing and essentially parallel surfaces. Furthermore, the Raman device can be used to determine and / or map the H₂ content with spatial resolution, in addition to the OH content.

[0307] It is preferably possible to perform a near-surface measurement using a Raman device, in particular a Raman microscope. Alternatively or additionally, it is possible to perform a measurement at an angle by overlapping an excitation beam and a detection beam. Advantageously, one or two adjacent coarsely ground surfaces can be provided. The measurement can alternatively or additionally be performed on a cylindrical circumference and / or on a polished lens surface of the optical element, which is already at least partially completed.It may be provided that a basic rotational symmetry of the deposition process for the production of the boule underlying the substrate body or a specific blank obtained from the boule is achieved by producing and measuring several strips and / or by comparing the prediction based on the measurement of the strips with several of the previously described verification measurements on blanks and / or witness samples.

[0308] At this point, a blank made of synthetic quartz glass is disclosed, which is obtained from a Boule-Direct deposition process and which, according to the disclosure, is selected according to a three-dimensional map.

[0309] This document discloses a method for creating and / or reconstructing and / or improving a previously known mapping or map using FTIR, Raman spectroscopy, shadow techniques and / or polarized light.

[0310] At this point, a method for assembling the lens blanks and their relative orientation based on the three-dimensional map is revealed.

[0311] Features described in connection with one of the subject matter of the invention, in particular those provided by the inventive method, the inventive device, the inventive optical element, the disclosed processing method, the disclosed substrate body, or the inventive lithography system, can also be advantageously implemented for the other subject matter of the invention. Likewise, advantages mentioned in connection with one of the subject matter of the invention can also be understood to relate to the other subject matter of the invention.

[0312] It should also be noted that terms such as "comprehensive," "exhibiting," or "with" do not exclude other characteristics or steps. Furthermore, terms such as "a" or "the," which indicate a singular number of steps or characteristics, do not exclude a plurality of characteristics or steps—and vice versa.

[0313] In a purist embodiment of the invention, however, it may also be provided that the features introduced in the invention with the terms "comprising," "comprising," or "with" are exhaustively listed. Accordingly, one or more lists of features within the scope of the invention may be considered complete, for example, for each claim. The invention may, for instance, consist exclusively of the features mentioned in claim 1.

[0314] It should be noted that designations such as "first" or "second", etc., are used primarily for the purpose of distinguishing the respective device or process features and are not necessarily intended to indicate that the features are mutually dependent or related to one another. Exemplary embodiments of the invention are described in more detail below with reference to the drawing.

[0315] The figures each show preferred embodiments in which individual features of the present invention are combined with one another. Features of an embodiment can also be implemented independently of the other features of the same embodiment and can therefore be readily combined by a person skilled in the art to form further meaningful combinations and subcombinations with features of other embodiments.

[0316] In the figures, functionally identical elements are provided with the same reference symbols.

[0317] They show:

[0318] Figure 1 shows an EUV projection exposure system in meridional section;

[0319] Figure 2 shows a DUV projection exposure system;

[0320] Figure 3 shows a schematic representation of a possible embodiment of a device according to the invention;

[0321] Figure 4 shows a schematic representation of a possible shape of a substrate body to be measured;

[0322] Figure 5 shows another schematic representation of a possible shape of the substrate body to be measured;

[0323] Figure 6 shows another schematic representation of a possible shape of the substrate body to be measured;

[0324] Figure 7 shows a top view of the substrate body according to Figure 6 during measurement;

[0325] Figure 8 shows a top view of the substrate body in a boule;

[0326] Figure 9 shows a top view of the substrate body according to Figure 6 in another possible way of measuring;

[0327] Figure 10 shows a top view of the substrate body according to Figure 6 in another possibility of the

[0328] Surveying; Figure 11 shows a possible position of a mirror in the substrate body before the mirror is machined out;

[0329] Figure 12 shows a side view of a substrate body using another measurement method;

[0330] Figure 13 shows a schematic representation of another possible shape of the substrate body to be measured;

[0331] Figure 14 shows a schematic representation of another possible shape of the substrate body to be measured;

[0332] Figure 15 shows a block diagram representation of a possible embodiment of a method according to the invention;

[0333] Figure 16 shows a side view of the substrate body using another measurement method;

[0334] Figure 17 shows a side view of the substrate body using another measurement method;

[0335] Figure 18 shows a side view of the substrate body using another measurement method;

[0336] Figure 19 shows a side view of the substrate body using another measurement method;

[0337] Figure 20 is a schematic representation of a possible shape of a boules;

[0338] Figure 21 shows a schematic representation of a Raman spectrum;

[0339] Figure 22 shows a schematic representation of an infrared spectrum;

[0340] Figure 23 shows a schematic representation of the ratio of TiÜ2 to SiO2;

[0341] Figure 24 shows a schematic representation of the effect of bleaching radiation;

[0342] Figure 25 is a schematic representation of the effect of pre-irradiation; and

[0343] Figure 26 shows a schematic representation of a temperature correction of a spectrum.

[0344] The following section describes, with reference to Figure 1, the essential components of an EUV projection exposure system 100 for microlithography as an example of a lithography system. The description of the basic structure of the EUV projection exposure system 100 and its components is not intended to be restrictive. An illumination system 101 of the EUV projection exposure system 100 comprises, in addition to a radiation source 102, an illumination optic 103 for illuminating an object field 104 in an object plane 105. A reticle 106 arranged in the object field 104 is exposed. The reticle 106 is held by a reticle holder 107. The reticle holder 107 can be moved, particularly in a scanning direction, via a reticle displacement drive 108.

[0345] Figure 1 shows a Cartesian xyz coordinate system for illustrative purposes. The x-direction runs perpendicular to the plane of the drawing. The y-direction runs horizontally, and the z-direction runs vertically. In Figure 1, the scan direction runs along the y-direction. The z-direction runs perpendicular to the object plane 105.

[0346] The EUV projection exposure system 100 comprises a projection optic 109. The projection optic 109 serves to image the object field 104 onto an image field 110 in an image plane 111. The image plane 111 is parallel to the object plane 105. Alternatively, an angle other than 0° between the object plane 105 and the image plane 111 is also possible.

[0347] A structure on the reticulum 106 is imaged onto a photosensitive layer of a wafer 112 located in the image plane 111 within the image field 110. The wafer 112 is held by a wafer holder 113. The wafer holder 113 can be displaced, particularly along the y-direction, via a wafer transfer drive 114. The displacement of the reticulum 106 via the reticulum transfer drive 108 and of the wafer 112 via the wafer transfer drive 114 can be synchronized.

[0348] Radiation source 102 is an EUV radiation source. Specifically, radiation source 102 emits EUV radiation 115, which is also referred to as useful radiation or illumination radiation. The useful radiation 115 has a wavelength in the range between 5 nm and 30 nm. Radiation source 102 can be a plasma source, for example, an LPP source (laser-produced plasma) or a DPP source (gas-discharged produced plasma). It can also be a synchrotron-based radiation source. Radiation source 102 can be a free-electron laser (FEL).

[0349] The illumination radiation 115, emanating from the radiation source 102, is focused by a collector 116. The collector 116 can be a collector with one or more ellipsoidal and / or hyperboloid reflective surfaces. The at least one reflective surface of the collector 116 can be illuminated with the illumination radiation 115 at grazing incidence (Gl), i.e., with angles of incidence greater than 45°, or at normal incidence (NI), i.e., with angles of incidence less than 45°. The collector 116 can be structured and / or coated, on the one hand, to optimize its reflectivity for the useful radiation 115 and, on the other hand, to suppress stray light.

[0350] After the collector 116, the illumination radiation 115 propagates through an intermediate focus in an intermediate focal plane 117. The intermediate focal plane 117 can represent a separation between a radiation source module, comprising the radiation source 102 and the collector 116, and the illumination optics 103.

[0351] The illumination optics 103 comprise a deflecting mirror 118 and, downstream in the beam path, a first faceted mirror 119. The deflecting mirror 118 can be a planar deflecting mirror or, alternatively, a mirror with an effect that influences the beam beyond the mere deflection effect. Alternatively or additionally, the deflecting mirror 118 can be designed as a spectral filter that separates a useful wavelength of the illumination radiation 115 from stray light of a different wavelength. If the first faceted mirror 119 is arranged in a plane of the illumination optics 103 that is optically conjugate to the object plane 105 as a field plane, it is also referred to as a field faceted mirror. The first faceted mirror 119 comprises a plurality of individual first facets 120, which are hereinafter also referred to as field facets. Only a few of these facets 120 are shown in Figure 1 as examples.

[0352] The first facets 120 can be designed as macroscopic facets, in particular as rectangular facets or as facets with an arcuate or semicircular border contour. The first facets 120 can be designed as planar facets or alternatively as convexly or concavely curved facets.

[0353] As is known, for example, from DE 10 2008 009 600 A1, the first facets 120 themselves can each be composed of a plurality of individual mirrors, in particular a plurality of micromirrors. The first facet mirror 119 can in particular be designed as a microelectromechanical system (MEMS system). For details, reference is made to DE 10 2008 009 600 A1.

[0354] Between the collector 116 and the deflecting mirror 118, the illumination radiation 115 runs horizontally, i.e. along the y-direction.

[0355] In the beam path of the illumination optics 103, a second faceted mirror 121 is arranged downstream of the first faceted mirror 119. If the second faceted mirror 121 is arranged in a pupil plane of the illumination optics 103, it is also referred to as a pupil faceted mirror. The second faceted mirror 121 can also be arranged at a distance from a pupil plane of the illumination optics 103. In this case, the combination of the first faceted mirror 119 and the second faceted mirror 121 is also referred to as a specular reflector. Specular reflectors are known from US 2006 / 0132747 A1, EP 1 614008 B1 and US 6,573,978. The second faceted mirror 121 comprises a plurality of second facets 122. The second facets 122 are also referred to as pupil facets in the case of a pupil faceted mirror.

[0356] The second facets 122 can also be macroscopic facets, which may, for example, have round, rectangular, or hexagonal edges, or alternatively, facets composed of micromirrors. Reference is also made to DE 102008 009600 A1 in this regard.

[0357] The second facets 122 can have planar or alternatively convex or concave curved reflective surfaces.

[0358] The illumination optics 103 thus form a double-faceted system. This basic principle is also known as a fly's eye integrator.

[0359] It may be advantageous not to arrange the second faceted mirror 121 exactly in a plane which is optically conjugate to a pupil plane of the projection optics 109.

[0360] With the aid of the second faceted mirror 121, the individual first facets 120 are imaged into the object field 104. The second faceted mirror 121 is the last beam-shaping, or indeed the last, mirror for the illumination radiation 115 in the beam path before the object field 104.

[0361] In another embodiment of the illumination optics 103, not shown, a transmission optic can be arranged in the beam path between the second facet mirror 121 and the object field 104, which contributes in particular to imaging the first facets 120 into the object field 104. The transmission optic can have exactly one mirror, or alternatively two or more mirrors, which are arranged one behind the other in the beam path of the illumination optics 103. The transmission optic can in particular comprise one or two mirrors for normal incidence (Nl mirrors, "normal incidence" mirrors) and / or one or two mirrors for grazing incidence (Gl mirrors, "grazing incidence" mirrors).

[0362] In the embodiment shown in Figure 1, the lighting optics 103 has exactly three mirrors after the collector 116, namely the deflecting mirror 118, the field facet mirror 119 and the pupil facet mirror 121.

[0363] In a further embodiment of the lighting optics 103, the deflecting mirror 118 can also be omitted, so that the lighting optics 103 can then have exactly two mirrors after the collector 116, namely the first faceted mirror 119 and the second faceted mirror 121.

[0364] The imaging of the first facets 120 by means of the second facets 122, or with the second facets 122 and a transmission optic into the object plane 105, is regularly only an approximate imaging. The projection optic 109 comprises a plurality of mirrors Mi, which are numbered according to their arrangement in the beam path of the EUV projection exposure system 100.

[0365] In the example shown in Figure 1, the projection optics 109 comprises six mirrors M1 to M6. Alternatives with four, eight, ten, twelve, or any other number of mirrors Mi are also possible. The penultimate mirror M5 and the last mirror M6 each have an aperture for the illumination radiation 115. The projection optics 109 is a double-obscured optic. The projection optics 109 has an image-side numerical aperture greater than 0.5, and which can also be greater than 0.6, for example, 0.7 or 0.75.

[0366] The reflective surfaces of the mirrors Mi can be designed as freeform surfaces without an axis of rotational symmetry. Alternatively, the reflective surfaces of the mirrors Mi can be designed as aspherical surfaces with exactly one axis of rotational symmetry of the reflective surface shape. The mirrors Mi, like the mirrors of the illumination optics 103, can have highly reflective coatings for the illumination radiation 115. These coatings can be designed as multilayer coatings, in particular with alternating layers of molybdenum and silicon.

[0367] The projection optics 109 has a large object-image offset in the y-direction between a y-coordinate of the center of the object field 104 and a y-coordinate of the center of the image field 110. This object-image offset in the y-direction can be approximately as large as a z-distance between the object plane 105 and the image plane 111.

[0368] The number of intermediate image planes in the x- and y-directions in the beam path between the object field 104 and the image field 110 can be the same or, depending on the design of the projection optics 109, can differ. Examples of projection optics with different numbers of such intermediate images in the x- and y-directions are known from US 2018 / 0074303 A1.

[0369] Each of the pupil facets 122 is assigned to exactly one of the field facets 120 to form an illumination channel for illuminating the object field 104. This can result, in particular, in illumination according to Köhler's principle. The far field is divided into a multitude of object fields 104 by means of the field facets 120. The field facets 120 generate a plurality of images of the intermediate focus on the pupil facets 122 assigned to each of them.

[0370] The field facets 120 are each superimposed on the reticulum 106 by an associated pupil facet 122 to illuminate the object field 104. The illumination of the object field 104 is particularly homogeneous and preferably exhibits a uniformity error of less than 2%. Field uniformity can be achieved by superimposing different illumination channels. The illumination of the entrance pupil of the projection optics 109 can be geometrically defined by arranging the pupil facets. By selecting the illumination channels, especially the subset of pupil facets that guide light, the intensity distribution in the entrance pupil of the projection optics 109 can be adjusted. This intensity distribution is also referred to as the illumination setting.

[0371] Another preferred pupil uniformity in the area of ​​defined illuminated sections of an illumination pupil of the illumination optics 103 can be achieved by a redistribution of the illumination channels.

[0372] Further aspects and details of the illumination of the object field 104 and, in particular, the entrance pupil of the projection optics 109 are described below.

[0373] The projection optic 109 can, in particular, have a homocentric entrance pupil. This may be accessible. It may also be inaccessible.

[0374] The entrance pupil of the projection optics 109 cannot be precisely illuminated by the pupil facet mirror 121. When the projection optics 109 image the center of the pupil facet mirror 121 telecentrically onto the wafer 112, the aperture rays often do not intersect at a single point. However, a surface can be found where the pairwise determined separation of the aperture rays is minimized. This surface represents the entrance pupil or a surface conjugate to it in real space. In particular, this surface exhibits a finite curvature.

[0375] The projection optics 109 may have different entrance pupil positions for the tangential and sagittal beam paths. In this case, an imaging element, in particular an optical component of the transmission optics, should be provided between the second faceted mirror 121 and the reticle 106. This optical component will allow the different positions of the tangential and sagittal entrance pupils to be taken into account.

[0376] In the arrangement of the components of the illumination optics 103 shown in Figure 1, the pupil facet mirror 121 is arranged in a plane conjugate to the entrance pupil of the projection optics 109. The first field facet mirror 119 is arranged tilted relative to the object plane 105. The first facet mirror 119 is arranged tilted relative to an arrangement plane defined by the deflecting mirror 118.

[0377] The first faceted mirror 119 is arranged at an angle to an arrangement plane defined by the second faceted mirror 121.

[0378] Figure 2 shows an exemplary DUV projection exposure system 200. The DUV projection exposure system 200 comprises an illumination system 201, a device called a reticule stage 202 for receiving and precisely positioning a reticule 203, by which the subsequent structures on a wafer 204 are determined, a wafer holder 205 for holding, moving and precisely positioning the wafer 204 and an imaging device, namely a projection optic 206, with several optical elements, in particular lenses 207, which are held in a lens housing 209 of the projection optic 206 via mounts 208.

[0379] Alternatively or in addition to the lenses 207 shown, various refractive, diffractive and / or reflective optical elements, including mirrors, prisms, end plates and the like, may be provided.

[0380] The basic operating principle of the DUV projection exposure system 200 provides that the structures introduced into the reticulum 203 are imaged onto the wafer 204.

[0381] The illumination system 201 provides a projection beam 210 in the form of electromagnetic radiation, which is required for imaging the reticulum 203 onto the wafer 204. A laser, a plasma source, or the like can be used as the source of this radiation. In the illumination system 201, the radiation is shaped by optical elements such that the projection beam 210, upon striking the reticulum 203, exhibits the desired properties with regard to diameter, polarization, wavefront shape, and the like.

[0382] Using the projection beam 210, an image of the reticulum 203 is generated and transferred, appropriately reduced in size, to the wafer 204 by the projection optics 206. The reticulum 203 and the wafer 204 can be moved synchronously, so that areas of the reticulum 203 are mapped onto corresponding areas of the wafer 204 practically continuously during a so-called scan process.

[0383] Optionally, the air gap between the last lens 207 and the wafer 204 can be replaced by a liquid medium with a refractive index greater than 1.0. This liquid medium could, for example, be highly purified water. Such a setup is also known as immersion lithography and offers increased photolithographic resolution.

[0384] The use of the invention is not limited to use in projection exposure systems 100, 200, and in particular not limited to systems with the described configuration. The invention is suitable for any lithography or microlithography systems, but especially for projection exposure systems with the described configuration. The invention is also suitable for EUV projection exposure systems that have a lower image-side numerical aperture than that described in connection with Figure 1 and that do not have an obscured mirror M5 and / or M6. In particular, the invention is also suitable for EUV projection exposure systems that have an image-side numerical aperture of 0.25 to 0.5, preferably 0.3 to 0.4, and most preferably 0.33. Furthermore, the invention and the following embodiments are not to be understood as being limited to a specific design.

[0385] The following figures represent the invention only by way of example and in a highly schematic form. Figure 3 shows a schematic representation of a possible embodiment of a device 1 for spatially resolved measurement of at least one homogeneity parameter in a volume of a substrate body 2, in particular a substrate body 2 of an optical element 116, 118, 119, 120, 121, 122, Mi, 207 of a projection exposure system 100, 200.

[0386] The device 1 comprises at least one measuring device 3 for acquiring respective measurement information in at least one volume element 4 of the substrate body 2. Furthermore, the device 1 comprises at least one computing device 5 for determining a value of the at least one homogeneity parameter from the respective measurement information and a position determination device 6 for determining a spatial position of the at least one volume element 4 in the substrate body 2.

[0387] The computing device 5 is designed to determine a spatial distribution 7 of the at least one homogeneity parameter from the spatial position of the at least one volume element 4 and the respective value of the associated homogeneity parameter.

[0388] The spatial distribution 7 is represented in a highly simplified manner as a 2D map.

[0389] Furthermore, a previously known map 7a is shown, which will be explained later.

[0390] Preferably, the measuring device 3 has a Raman device 12 (see also Figure 6) for detecting a Raman spectrum 12a (see Figure 21) as measurement information in the at least one volume element 4 of the substrate body 2.

[0391] In the embodiment of the device 1 shown in Figure 3, an irradiation unit 22 is preferably provided and configured to bleach the at least one volume element 4 by means of bleaching radiation 23. In the embodiment shown in Figure 3, the irradiation unit 22 is preferably integrally formed with the Raman unit 12.

[0392] Furthermore, in the embodiment of the device 1 shown in Figure 3, a temperature control device 24 is preferably provided and configured to at least partially temperature control the substrate body 2.

[0393] Not shown is a temperature measuring device, which is preferably present and configured to detect the temperature of the substrate body 2.

[0394] Figure 4 shows a schematic representation of a possible shape of the substrate body 2 to be measured.

[0395] Titanium-doped quartz glass, from which the substrate body 2 is preferably formed, is frequently produced using a direct deposition process called the Boule process. In this process, material is deposited radially r from a Boule center 8, forming a Boule 9 (see Figure 8). This can result in a layered streak or stria 10, or multiple striae 10 and / or stripe-shaped inhomogeneities 11 (see Figure 5). The Boule process exhibits high rotational symmetry.

[0396] The Boule 9 can be understood as a blank cut away from the Boule 8's center, or the center of the Boule. The radial coordinate r, or r-coordinate, of the Boule 9 originates at the Boule 8's center.

[0397] Furthermore, a certain asymmetry of the striae 10 is shown, which are flatter on the right than on the left.

[0398] Titanium-doped quartz glass produced using the Boule process exhibits a layered structure due to the deposition process. As shown in Figure 4, the material resembles a stack of pancakes. The period of the striae (or layered streaks) is frequently 200 pm, although periods of 100 to 400 pm are also observed.

[0399] The striae 10 lie approximately parallel to an upper surface of the substrate body 2, which is preferably a mirror blank, provided that the substrate body 2 was cut horizontally from a boule 9 and not reshaped. However, as can be seen in Figure 1, the striae 10 exhibit a slight curvature and a more pronounced upward slope towards the original edge of the boule 9.

[0400] When an amplitude of 0.15 wt% TiÜ2 occurs between the striae 10 and their surroundings, a variation in TZC of approximately 9 K PV and gradients of 45 K / cm can be caused. In extreme cases, fluctuations of up to 1% Ti or periods of 100 pm occur, resulting in gradients of around 100 K / cm.

[0401] Figure 5 shows another schematic representation of a possible shape of the substrate body 2.

[0402] The inhomogeneities 11 shown in Figure 5 run through the striae 10, which are relevant for the selection of substrate bodies 2 for optical elements 116, 118, 119, 120, 121, 122, Mi, 207 or blanks, or for their matching correction for the subsequent operating temperature. However, the inhomogeneities 11 are only located at approximately 2 K in the mirror-proximal region of the substrate body 2, with gradients of at most 1 K / cm.

[0403] Therefore, Figure 5 shows a side view of a substrate body 2 or blank, with a z-axis oriented vertically upwards.

[0404] Figure 6 shows another schematic representation of a possible shape of the substrate body 2.

[0405] Figure 6 shows, in particular, a combination of the striae 10 according to Figure 4 and the inhomogeneities 11 according to Figure 5, which can occur simultaneously in the substrate body 2. Figure 6 shows a side surface S of the substrate body 2, which is to be measured using the measuring device 3. Figure 6 thus shows a side view of the substrate body 2 with the side surface S that intersects the striae 10 and inhomogeneities 11.

[0406] The volume element 4 is preferably scanned over an area z' and r' of the side surface S, wherein z' and r' ideally cover the entire area of ​​the side surface S.

[0407] It may be provided that the, preferably flat, side surface S is also tilted relative to the original axes z and r of the boules 9.

[0408] In particular for measuring the substrate body 2, as shown in Figure 6, it is advantageous that the measuring device 3 of the device 1 preferably has the Raman device 12 for detecting the Raman spectrum 12a (see Figure 21) as measurement information in the at least one volume element 4 of the substrate body 2.

[0409] It may be provided that the side surface S is curved. This is particularly advantageous if the Raman device 12 has an autofocus.

[0410] In particular, the volume element 4 in Figure 6 can be interpreted as a Raman measurement spot in this case.

[0411] Preferably, at least one surface of the side surface S is ground, more preferably etched, lapped and / or polished.

[0412] Alternatively or additionally to measurement with the measuring device 3, it can be provided that at least one spoke of the boules 9 underlying the substrate body is destructively removed, and a map in height z and radius r is obtained from this by measuring the ultrasonic velocity or the refractive index. Assuming rotational symmetry, a three-dimensional map in z, r, phi or x, y, z can be obtained from this.

[0413] Particularly in the manufacture of mirrors 116, 118, 119, 120, 121, 122, Mi for projection exposure systems 100, 200, which have a diameter of more than 1 m, it is advantageous if these mirrors 116, 118, 119, 120, 121, 122, Mi, or the substrate bodies 2 underlying the mirrors 116, 118, 119, 120, 121, 122, Mi, encompass the center 8 of the boule 9 and a large part of the diameter of the boule 9. In this case, a spoke removed for measurement would be missing. Therefore, in this case, only a small piece of "spoke" in the outer diameter of the boule 9 can be obtained. Axially averaged measurements of the speed of sound in the material of the substrate body 2 can be provided. Based on the data obtained in this way, data from other Boules 9 obtained as a surrogate through destructive means are checked for similarity and corrected if necessary.

[0414] However, the inventors have realized that two sets of maps obtained in this way can show strong discrepancies between each other.

[0415] Figure 7 shows a top view of the substrate body 2 according to Figure 6. In the situation shown in Figure 7, the substrate body 2 is measured using the device 1.

[0416] Figure 7 shows in particular a top view of the substrate body 2 or blank together with an area 13 optically used in the mirror 116, 118, 119, 120, 121, 122, Mi.

[0417] In the illustrated embodiment, the Raman device 12 or the Raman spectrometer preferably has a lens 14.

[0418] In addition to the lens 14, a mounting plate A is preferably also present and shown as part of the device 1 in Figure 7.

[0419] The mounting plate A can be used in combination with water or an index-matched immersion fluid to measure rough surfaces of the substrate body 2 or blank surfaces.

[0420] In the case of curved or complexly shaped side surfaces S, the mounting plate A is preferably designed as a negative mold or matrix made of glass or titanium-doped quartz glass.

[0421] Preferably, the device 1 includes a positioning device 15 which is configured to position the measuring device 3 relative to the substrate body 2 in such a way that the measurement information can be detected in the at least one volume element 4.

[0422] In particular, the positioning device 15 can include the autofocus.

[0423] In this case, tracking of the focus of the Raman device 12 by means of the positioning device 15 can preferably be programmed based on the known shape of the mounting plate A or die.

[0424] Figure 8 shows a top view of the substrate body 2 in the boule 9.

[0425] Figure 8 thus shows a top view of the position of the substrate body 2 or the blank before its removal from the boule 9. In the case of substrate bodies 2 or blanks that are at least predominantly symmetrically shaped, these are preferably cut out in such a way that their bisector coincides with a radius R1 of the boule 9.

[0426] The intersection point of R1 with the outer contour, pointing towards the center of the boule 8, is preferably marked with an azimuth marker. For a substantially rectangular substrate body 2 or blank, the side surface S is parallel to a local y-axis of the substrate body 2, but at an angle α to its local radius R2 with respect to the boule 9.

[0427] In particular, if the side surface S is tilted by the angle a relative to the radial R2, the y-coordinates on the side surface S can be converted back to the radial coordinates of the boules underlying the substrate body 2 by a simple scaling.

[0428] Furthermore, if information is available that the substrate body 2 was cut out of the boule 9 with a twist, an opposite side surface S' (not shown) can be measured to determine the twist. In particular, the twist can be deduced from the measurements of the side surfaces.

[0429] If the side surface S is tilted in the yz-plane and / or complexly shaped and / or curved, every measured point or volume element 4 can still be calculated back into the radial coordinates of the boules 9 underlying the substrate body 2.

[0430] The diameter of the measurement spot of the Raman device 12, and thus of the volume element 4, can preferably range from a few pm to a few mm, depending on the objective. Larger diameters allow more of the measurement radiation 16 to enter a detector element (not shown) of the Raman device 12, thereby reducing noise, shortening the measurement time, and decreasing the amount of data.

[0431] In particular, with the aim of recovering the registration of a homogeneity map 7 of the manufacturer, which has been lost due to inaccurate cutting or processing steps, it may be possible to measure a relatively small partial area of ​​the side surface S in small sections r' = y' and z' and compare it with the original homogeneity map 7.

[0432] Preferably, a detection spot or volume element 4 that is rather laterally large and has a distance of more than a typical distance between adjacent striae 10 is chosen.

[0433] Advantageously, lower signal-to-noise ratios are also tolerable if a relative position of the coordinate systems can be reconstructed, preferably by means of a two-dimensional autocorrelation.

[0434] To achieve a high-resolution measurement, a correspondingly small beam spot of the measurement radiation 16 or a correspondingly small volume element 4 can preferably be selected. For example, if a resolution of 1 mm is desired, the beam spot should not be significantly larger.

[0435] If the striae 10 are to be resolved, a beam spot of less than 200 pm in diameter should preferably be selected.

[0436] The inventors have recognized that a pattern of striae 10, particularly with regard to distinguished event striae 10, is repeated essentially everywhere in the substrate body 2. This is especially true over distances of approximately 50 cm.

[0437] It can therefore be provided that the side surface S is scanned with a coarse spatial resolution, while a high-resolution survey in the z-direction takes place only at individual locations, preferably less than 100, particularly preferably less than 10.

[0438] It may preferably be provided that the curvature of a course of the striae 10 is recorded, numerically fitted and / or used in an interpolation between the locations measured in the z-direction.

[0439] Figure 9 shows a schematic representation of a possible embodiment of measuring the substrate body 2 using the device 1.

[0440] The Raman device 12, in particular in the embodiment shown in Figure 7, can be a confocal Raman microscope.

[0441] However, a pseudo-confocal setup as shown in Figure 9 can also be used.

[0442] Here, preferably one or more laser beams are directed as measuring radiation 16 past the lens 14 into a focus area of ​​the lens 14.

[0443] This has the particular advantage that laser powers of more than 2 watts, preferably more than 5 watts, can be used without risk of damaging the lens 14.

[0444] Figure 10 shows a top view of the substrate body 2 according to Figure 6 in another possible measurement position.

[0445] Figure 10 shows an embodiment in which the excitation beam and the detected beam of the measuring radiation 16 are at an angle of 90° to each other. However, a measuring radiation source or laser and the lens 14 are each at approximately 45° to the glass surface of the mounting plate A or the substrate body 2, respectively. In an embodiment described later, it may be provided that the laser beam of the measuring radiation 16 is directed through the, preferably polished, top surface of the substrate body 2 or blank, and that the lens 14 is positioned at 90° to the glass surface.

[0446] Figure 11 shows a possible position of a mirror 116, 118, 119, 120, 121, 122, Mi in the substrate body 2 before the mirror 116, 118, 119, 120, 121, 122, Mi is worked out.

[0447] The substrate body 2 as a mirror blank is shown in dashed lines in Figure 11.

[0448] The substrate body 2 in the form of the mirror 116, 118, 119, 120, 121, 122, Mi is shown in solid lines in Figure 11.

[0449] Measuring the top and / or bottom surfaces of the substrate body 2 in the form of a mirror blank and / or mirror body allows deviations of the homogeneity from the basic rotational symmetry in the Boule 9 and / or a twisted and / or tilted cutting to be detected.

[0450] The underside of a substrate body 2 designed as a mirror often has large flat areas that can be preferably measured. However, these areas are far removed from a mirror surface 17 that will be used optically in later operation and therefore contribute little to the thermal behavior.

[0451] On the upper surface of a mirror body, in addition to the actual optically used mirror surface 17, there can be 7 flat horizontal areas that are closer to the mirror surface 17. These areas can preferably be measured.

[0452] The information obtained can be used to verify the registration and / or validity of the previously known mapping 7a, as explained in connection with Figure 15.

[0453] Figure 12 shows a side view of the substrate body 2 in another possible measurement scenario;

[0454] To obtain precise knowledge about the CTE homogeneity of the material of the substrate body 2 immediately below the later mirror surface 17, it is particularly advantageous to create an already ground and at least roughly polished mirror surface 17 and to scan it.

[0455] This can be achieved with a confocal or quasi-confocal setup of the Raman device 12. One measurement direction of the Raman device 12 can be fixed parallel to the z-direction, especially if the mirror surface 17 is only slightly curved.

[0456] Preferably, in the embodiment shown in Figure 12, the Raman device 12 is therefore configured to perform confocal Raman spectroscopy. For more strongly curved mirrors 116, 118, 119, 120, 121, 122, Mi, it is advantageous to pivot a measuring head of the Raman device 12, preferably by means of the positioning device 15, so that measurements can always be taken in an approximately normal direction to the mirror surface or mirror area 17.

[0457] It is advantageous if a mapping or the spatial distribution 7 of at least one homogeneity parameter extends a few mm in depth axially with respect to the substrate body 2 or normal to the mirror surface 17.

[0458] The mapping 7 can preferably be used for a fit correction of the substrate body 2 or the mirror surface 17.

[0459] In the fit correction, the substrate body 2 is preferably machined and measured at room temperature. The correction can be calculated such that a desired fit or shape of the mirror surface 17 is achieved at an operating temperature or a temperature profile that develops during operation.

[0460] Figure 13 shows a schematic representation of another possible shape of the substrate body 2 to be measured in the form of a mirror blank.

[0461] Figure 14 shows a schematic representation of another possible shape of the substrate body 2 to be measured in the form of a mirror body.

[0462] Figures 13 and 14 illustrate a difficulty that arises when measuring the upper or lower surfaces of the substrate body 2 or mirror surfaces 17.

[0463] It can be observed that on the upper side of the substrate body 2 according to Figure 14 and / or the mirror top or mirror surface 17 according to Figure 14, a package of striae 10 is cut off during a measurement at a shallow angle.

[0464] This allows the spatial wavelength on the surface, typically 0.2 mm perpendicular to the striae 10, to increase by a factor of 5 to approximately 500. The spatial wavelength of the striae 10 is thus located within the range of the spacing of typical inhomogeneities 11.

[0465] At the same time, the amplitude of the striae 10 is still approximately a factor of 5 higher than that of the sought-after inhomogeneities 11, which makes it difficult to separate the two phenomena.

[0466] It may therefore be possible to use a shallow measurement depth and penetration depth of the Raman device 12, in particular the confocal Raman microscope, for planning a deterministic correction of the striae 10. Regarding the reference numerals in Figures 3 to 14, please refer to the preceding figures.

[0467] Figure 15 shows a block diagram representation of a possible embodiment of a method for spatially resolved measurement of at least one homogeneity parameter in the volume of the substrate body 2.

[0468] In a measurement information block 30, the respective measurement information is recorded in at least one volume element 4 of the substrate body 2 by means of the measuring device 3.

[0469] Within the framework of measurement information block 30, it may be provided that an immersion fluid is applied to a surface of the substrate body 2.

[0470] Within the measurement information block 30, it can preferably be provided that several volume elements 4 are measured along a line perpendicular to the striae 10 of the substrate body 2 and / or that X-ray fluorescence is recorded as measurement information.

[0471] In a parameter block 31, the value of at least one homogeneity parameter is determined from the respective measurement information using the computing device 5.

[0472] In a position determination block 32, a spatial location of at least one volume element 4 is determined by means of the position determination device 6.

[0473] In a mapping block 33, the spatial distribution 7 of the at least one homogeneity parameter is determined from the spatial position of the at least one volume element 4 and the respective associated homogeneity parameter by means of the computing device 5.

[0474] Preferably, within the framework of the measurement information block 30, the Raman spectrum 12a is recorded as measurement information in the at least one volume element 4 of the substrate body 2 by means of the Raman device 12.

[0475] Within a manufacturing block 34, preferably preceding it chronologically, the substrate body 2 is preferably produced rotationally symmetrically using a Boule process. Alternatively or additionally, the substrate body 2 enters blocks 30 to 33 already in a rotationally symmetrical form or microstructure.

[0476] It may be provided that in step a) several volume elements 4 are measured which are arranged along a reference surface 35 (see e.g. Figure 16). Within the framework of the mapping block 33, the spatial distribution 7 of the homogeneity parameter in the entire substrate body 2 is preferably reconstructed from the measurement information of one or more volume elements 4 which are arranged along the reference surface 35, which may in particular be given by the side surface S and / or the mirror surface 17.

[0477] Within the mapping block 33, the spatial distribution 7 is preferably determined by locating a previously known mapping 7a (see Figure 3) of the at least one homogeneity parameter in the substrate body 2.

[0478] In the previously known mapping 7a shown in Figure 3, the orientation is incorrect, but the spatial distribution is correct.

[0479] Within the mapping block 33, the previously known mapping 7a is preferably located in the substrate body 2 by identifying at least one sample of at least a part of the previously known mapping 7a based on the measurement information of the volume elements 4.

[0480] This enables an efficient reconstruction of the complete mapping 7 from the previously known mapping 7a and a fragment of the spatial distribution 7 based on the measurement information.

[0481] Therefore, at least one section on the lateral surface of the substrate body 2 can preferably be used as the reference surface 35 as the side surface S.

[0482] Furthermore, in the exemplary embodiments shown in the figures, it is preferably provided that a titanium-doped quartz glass is measured as the substrate body 2.

[0483] In particular, the volume element 4 or a measurement volume can be positioned such that it extends from the surface of the substrate body 2 by 1 pm to 5 pm in depth. In this way, a good characterization of the lateral and / or surface-tangential extension of the striae 10 is possible.

[0484] This is particularly advantageous because the material removal in any subsequent deterministic correction process is significantly less than 5 pm.

[0485] It may also be provided that a virtual radial cross-sectional surface of the substrate body 2 is used as the reference surface 35.

[0486] It may be intended that the procedure is applied iteratively, i.e., after one or more polishing or correction steps, measurements are taken again and a new correction is planned.

[0487] This allows, for example, the definition of a processing procedure. It can be stipulated that a pass adjustment is planned during the pass correction process without considering the striae 10. In this case, the mirror 116, 118, 119, 120, 121, 122, Mi is brought into a target pass, and the striae 10 and other pass errors are corrected based on an interferometric measurement.

[0488] It may be planned that subsequently from a 5 mm 3 A passport correction is calculated and executed for the resolved mapping 7 of the CTE.

[0489] Mapping 7, for example, could originate from a manufacturer of titanium-doped quartz glass.

[0490] It may be provided that the pass correction described above maintains the effect of the spatial distribution 7 of the at least one homogeneity parameter, in particular the 3D-CTE, on the pass at the generally higher operating temperature.

[0491] Preferably, a final processing of the substrate body 2 by computer-aided polishing (CCP) or ion beam processing (IBF) can be provided. However, this may again expose the striae 10.

[0492] Preferably, the correction process for the pass can be carried out in such a way that it is based on, firstly, a coarsely resolved mapping 7 of the CTE, and secondly, a mapping 7 of the striae 10 near the surface of the substrate body 2, or is calculated and applied on this basis.

[0493] The coarse-resolution mapping 7 can preferably originate from a manufacturing process of the substrate body 2 and / or from measurements on the substrate body 2 using the device 1.

[0494] In addition, it may be advantageous to measure the mirror surface 17 in a final measurement or scan before processing it in fine steps of approximately 5 to 20 pm up to about 400 pm normally into the depth of the substrate body 2.

[0495] This allows the local thickness of the sectioned striae 10 to be preferably determined. Preferably, the determined thickness can be included in the correction calculation.

[0496] For the acquisition of the homogeneity map 7 in near-surface regions of the substrate body 2, the exposed striae 10 may be disadvantageous if they exhibit a larger amplitude than the inhomogeneities 11 being sought or investigated and are hardly distinguishable from the inhomogeneities 11 according to their spatial frequency and curvature around the Boule center 8. To improve differentiation, the optical measurement volume or volume element 4 can therefore be adjusted by appropriately selecting a relatively long focal length and a small numerical aperture of the objective 14 of the Raman device 12 such that the depth of the volume element 4 is greater than the average distance between adjacent striae 10. It can be provided that the numerical aperture of the objective 14 is 0.5 to 0.7, preferably 0.55.

[0497] In particular, it may be provided that the volume element 4 has a depth of 500 pm or more.

[0498] Alternatively or additionally, it is advantageous to numerically average several measurement points or several measurement pieces of information from different volume elements 4 at different depths.

[0499] Preferably, the scan area of ​​the Raman device 12 extends to a depth of 1 cm to 5 cm, preferably 3 cm, of the substrate body 2. Since confocal microscopes and 2x45° setups, as illustrated in Figure 10, reach their limits in this case, a quasi-confocal setup of the Raman device 12 according to Figure 12 is suitable.

[0500] If a substrate body 2 or blank is pre-bent or slumped to achieve a better volume yield or to adapt a curvature of the striae 10 to a mirror curvature of the mirror surface 17, it is advantageous if the homogeneity map 7 determined on the uncurved substrate body 2 or blank is transformed under the assumption of a flow model.

[0501] Here too, scanning a curved surface, especially the mirror surface 17, ideally in conjunction with a depth scan into the depth of the substrate body 2, offers significant advantages.

[0502] Figure 16 shows a side view of a substrate body 2 under another measurement method.

[0503] If a complete three-dimensional homogeneity map 7 is to be obtained, a 90° setup according to Figure 16 is suitable.

[0504] For this purpose, a substrate body 2 is preferably polished or ground on at least two sides and provided with mounting plates A (not shown) and immersion fluid.

[0505] The measuring radiation 16 is preferably designed as a laser beam and is directed through a surface of the substrate body 2. The objective 14 focuses a beam waist of the laser beam onto the Raman device 12, which is preferably designed as a Raman spectrometer.

[0506] Preferably, several laser beams of the measuring radiation 16 can be brought into overlap. Preferably, the positioning device 15 (not shown) is configured to move the substrate body 2, the measuring radiation source, in particular a laser, and / or an optic, in particular the lens 14, in three dimensions.

[0507] If an inhomogeneity 11 is to be detected, it may preferably be provided to use a measuring volume or a volume element 14 which extends at least 1 mm in the z-direction z.

[0508] It may be possible to measure the volume near the side surface S of the substrate body 2. In this case, the beam path of the measuring radiation 16 can be reversed. In particular, excitation can be performed from above and detection from the side.

[0509] As reference surface 35, at least a section of a lateral surface of the substrate body 2 is measured.

[0510] This allows, for example, a fragmentarily known homogeneity map 7a to be reconstructed with particular accuracy (see the explanations in connection with Figure 15).

[0511] Figure 17 shows a side view of a substrate body 2 under another measurement method.

[0512] Alternatively or in addition to the “classic” 90° setup of the Raman device 12 according to Figure 16, a quasi-confocal setup according to Figure 17 can be implemented.

[0513] Figure 18 shows a side view of a substrate body 2 under another measurement method.

[0514] Alternatively or in addition to the “classic” 90° setup of the Raman device 12 according to Figure 16 and / or the quasi-confocal setup according to Figure 17, a 2x 45° setup according to Figure 18 can be implemented.

[0515] The structures according to Figure 17 and Figure 18 have the advantage that only one side surface S of the substrate body 2 needs to be polished.

[0516] Preferably, however, polishing of a side surface is avoided. Instead, measurement is preferably taken from the top and / or bottom.

[0517] If this is the top surface or the future mirror surface 17, a particularly high-resolution measurement can be performed near the top surface, while measurement accuracy and spatial resolution decrease with increasing depth. However, this is acceptable, as the homogeneity parameter no longer has a significant influence on the mirror surface 17 at that depth. For particularly thick substrate bodies 2 or blanks, especially from a thickness of 20 cm, it can be advantageous to measure the substrate body 2 or the blank from the top and / or bottom surface to slightly beyond a mid-plane of the substrate body 2.

[0518] If one of the beams of the measurement radiation 16, usually the excitation beam in the 90° setup according to Figure 12, is coupled into the side surface S, it may be useful to tilt the beam by a few degrees relative to the striae 10 in order to prevent diffraction effects at the striae 10.

[0519] Preferably, a complete spatial distribution 7 of the at least one homogeneity parameter can be determined over an entire volume of the substrate body 2.

[0520] A complete 3D mapping 7 allows the selection of an optimal cutting position of the substrate body 2, in particular a mirror body, and thus a spatial selection which has advantages over conventional mappings 7.

[0521] In conventional mapping 7, there is an uncertainty regarding the quality of the rotational symmetry.

[0522] A particular advantage arises with substrate bodies 2, especially for mirrors 116, 118, 119, 120, 121, 122, Mi, of more than 0.8 m diameter, especially of more than 1 m diameter, which consist of one or more axially stacked and bonded blanks with large lateral dimensions, especially lateral dimensions of 70 cm to 1.20 m, made from Boule deposition.

[0523] For the aforementioned diameters of the substrate body 2, it is advantageous to avoid destructive sampling to determine the distribution 7 of homogeneity along r and z.

[0524] It is advantageous if an actual radial cross-sectional surface of a sister substrate body of the substrate body 2 is measured as the reference surface 35.

[0525] It may be provided that a selection of suitable substrate bodies 2 or blanks is made based on sister parts measured destructively.

[0526] Alternatively or additionally, rudimentary axial integrating measurements and r, z measurements can be provided in an outer area of ​​the Boule 9.

[0527] This allows the 3D mapping 7 to select suitable boules 9. Preferably, the interaction of inhomogeneities 11 of several boules 9 in the bonded stack can be taken into account. If a 3D mapping 7 has been created for each boule, deviations from rotational symmetry can also be corrected by rotating the boules 9 around their longitudinal axis and / or by laterally shifting each individual boule 9 to a respective point of maximum rotational symmetry determined or identified by measurement.

[0528] Furthermore, preferably with knowledge of the 3D mapping 7, the substrate body 2 can be deliberately cut out off-center from the boule 9. The combination of optimized lateral displacement and rotation of the substrate body 2 within the mirror body allows for a minimization of errors due to mirror heating.

[0529] A Boule 9, which requires only slight processing, in particular the removal of axially or radially outer areas that are unevenly shaped and have poor homogeneity, and from which many different types of mirrors can still be obtained geometrically, can preferably be mapped as a whole in this state at least with coarse resolution, in particular in a three-dimensional manner.

[0530] This has the advantage that optimal cutting locations for substrate body 2 can be determined for different mirror types with varying geometries and homogeneity requirements. This is more efficient than selecting supposedly good cutting locations solely based on a bubble map and a spoke measured for homogeneity.

[0531] If a more precise measurement using the Raman device 12, interferometry and / or ultrasound is necessary on the cut-out substrate body 2, a pre-selection increases the chance that the substrate body 2 will pass this further test and not have to be discarded.

[0532] It may preferably be provided that an actual radial cross-sectional surface of a spoke of the substrate body 2 is measured as the reference surface 35.

[0533] The device 1 and the described method can also be applied to substrate bodies 2 that are not fully formed by a Boule process.

[0534] In addition to titanium-doped quartz glass, which is produced by direct deposition in a Boule process, methods using a so-called Soot deposition are also known.

[0535] In this process, a soot body is either deposited using one or more burners, dried, sintered and, if necessary, homogenized.

[0536] Alternatively or additionally, a powder is produced using only one burner, which is then collected, pressed, and / or sintered. Forming processes are preferably carried out. The homogeneity with respect to the titanium content is preferably determined destructively on edge plates of the substrate body 2. Alternatively or additionally, longitudinal and transverse samples are taken in earlier process steps, and assumptions are made about the flow behavior during forming.

[0537] Even though the homogeneity with regard to the titanium content of such soot materials is often better than in the Boule process, a reliable non-destructive mapping of the homogeneity in 3D is not possible.

[0538] Here too, the embodiments of the invention described above can be used, whereby the striae 10 play a subordinate role after homogenization or in soot compression.

[0539] The titanium content in Soot materials is generally much more homogeneous than in a Boule process.

[0540] However, to achieve good temperature stability, an OH content of 10 - 300 ppm is preferably used.

[0541] Is bonding with titanium-doped quartz glass from a Boule process planned and / or is a gradient of < 1.5 ppb / K required? 2 To achieve temperatures at 20°C, it can be provided that the material is doped to a titanium content of up to 800 ppm, preferably 600 ppm to 800 ppm.

[0542] The OH content of the Soot material is preferably adjusted during drying and / or sintering.

[0543] OH can diffuse readily through the partially porous structure of the Soot material. Since the porosity decreases gradually and potentially inhomogeneously during sintering, inhomogeneities in the OH content can arise. Therefore, the contribution of the OH content to the CTE homogeneity in Soot materials is often of the same order of magnitude as, or even greater than, that of Ti.

[0544] Figure 19 shows a side view of the substrate body 2 in another possible measurement scenario.

[0545] In the embodiment of the device 1 shown in Figure 19, the measuring device 3 preferably comprises a Fourier transform infrared spectrometer 18 for detecting an infrared spectrum 19 (see Figure 22) of the at least one volume element 4.

[0546] Figure 19 thus shows a substrate body 2 or blank, which is irradiated with monochromatic light from the measuring radiation 16.

[0547] The intensity of the incident light is measured via a beam splitter 20, another detector measures the transmitted light.

[0548] In addition to classical spectrometers, FTIR spectrometers 18 are particularly suitable in the IR (infrared) range. Figure 20 shows a schematic representation of a possible shape of a Boules 9.

[0549] Here, the striae 10 are visible, which run parallel to the top or bottom surface, but perpendicular to the side surface S.

[0550] Regarding the reference symbols in Figures 15 to 20, please refer to the preceding figures.

[0551] Figure 21 shows a schematic representation of a Raman spectrum 12a.

[0552] The Raman spectrum 12a of a titanium-doped quartz glass is shown as a solid curve.

[0553] For comparison, the Raman spectrum 12a of a simple quartz glass is shown as a dashed line.

[0554] A Raman shift in 1 / cm is shown on a horizontal axis, and an intensity in arbitrary units is shown on a vertical axis.

[0555] Figure 22 shows a schematic representation of an infrared spectrum 19.

[0556] The exemplary infrared spectrum 19 was measured on a quartz glass using the Fourier-transform infrared spectrometer 18.

[0557] A wavenumber in 1 / cm is shown on a horizontal axis, and a transmission in arbitrary units is shown on a vertical axis.

[0558] Figure 23 shows a schematic representation of a ratio of TiÜ2 to SiO2, which was extracted from a Raman spectrum 12a according to Figure 21.

[0559] In the device 1, preferably a ratio of TiÜ2 to SiÜ2 can be determined as measurement information and a coefficient of thermal expansion in the volume element 4 as a homogeneity parameter.

[0560] The image shows the ratio of a TiO band to a SiO band when measuring points several micrometers apart with 10 repetitions over one second each. The band ratio is determined by a band at 937 1 / cm to a band at 485 1 / cm.

[0561] A measurement line or the location of the recording is plotted on a horizontal axis in any units.

[0562] The ratio of the bands is plotted on a vertical axis in arbitrary units. The course of the striae 10 can be deduced from the periodicity of the measurement points.

[0563] Figure 24 shows a schematic representation of an effect of bleaching radiation 23.

[0564] By using bleaching radiation 23 or laser bleaching, a reduction in the measurement error of the Ti / Si band ratio in Ti-doped quartz glasses can be achieved.

[0565] A continuous measurement number, and thus at least approximately the time, is plotted on a horizontal x-axis.

[0566] The ratio of the titanium band to the silicon band is plotted on a vertical axis in arbitrary units.

[0567] The longer the bleaching process is carried out, the lower the measurement error.

[0568] Figure 25 shows a schematic representation of the effect of pre-irradiation with bleaching radiation 23.

[0569] By using an LED as part of the irradiation device 22 to generate the bleaching radiation 23 and by performing pre-irradiation or pre-bleaching, a reduction of the measurement error of the Ti / Si band ratio in Ti-doped quartz glasses can be achieved.

[0570] In the example shown in Figure 25, the substrate body 2 was preferably pre-irradiated with the bleaching radiation 23 for more than 30 min.

[0571] A continuous measurement number, and thus at least an approximate representation of time, is plotted on a horizontal x-axis.

[0572] The ratio of the titanium band to the silicon band is plotted on a vertical axis in arbitrary units.

[0573] Figure 26 shows a schematic representation of a temperature correction of a spectrum.

[0574] Within the framework of measurement information block 30 and / or parameter block 31, it may be provided that a passive temperature measurement with subsequent correction, in particular by means of a Bose-Einstein equation, is carried out.

[0575] Figure 26 shows raw data on the left, in this case several Raman spectra of a titanium-doped quartz glass, which were recorded in a temperature range of 30°C to 60°C. A change in the spectra with temperature is particularly visible at low Raman shifts. This is illustrated in Figure 26 by a broadened intensity range at the aforementioned low Raman shifts.

[0576] On the right are Bose-Einstein temperature-corrected data based on the raw data shown on the left.

[0577] On a horizontal axis, a Raman shift in 1 / cm is shown, and on a vertical axis, an intensity in arbitrary units is shown.

[0578] It may be provided that a temperature measuring device (not shown) is included as part of the device 1.

[0579] Figure 3 thus shows an optical element 21, in particular a mirror 116, 118, 119, 120, 121, 122, Mi of the EUV projection exposure system 100, with at least one substrate body 2, wherein the substrate body 2 is at least partially manufactured using the method and / or device 1 as described in connection with the figures.

[0580] The lithography system shown in Figures 1 and 2 benefits particularly from the method and / or device 1 described above.

[0581] Figures 1 and 2 thus show a lithography system, in particular a projection exposure system 100, 200 for semiconductor lithography with an illumination system 101, 201 with a radiation source 102 and optics 103, 109, 106, which has at least one optical element 116, 118, 119, 120, 121, 122, Mi, 207.

[0582] In the embodiment shown in Figures 1 and 2, at least one of the optical elements 116, 118, 119, 120, 121, 122, Mi, 207 has at least a partial substrate body 2 which is at least partially measured and / or manufactured using the method described in connection with Figure 15 and / or is at least partially measured and / or manufactured using the device 1.

[0583] Alternatively or additionally, in the embodiment shown in Figures 1 and 2, at least one of the optical elements 116, 118, 119, 120, 121, 122, Mi, 207 is at least partially the optical element 21 described above.

[0584] The lithography system shown in Figures 1 and 2 benefits particularly from the surface shape of its optical elements 116, 118, 119, 120, 121, 122, Mi, 207, which is especially reliable under heat during operation. This ensures particularly good exposure quality of wafers. Reference numerals

[0585] 1 Device

[0586] 2 substrate bodies

[0587] 3 Measuring device

[0588] 4 volume element

[0589] 5 Computer equipment

[0590] 6 Position determination device

[0591] 7 Spatial distribution or mapping 7a Prior mapping

[0592] 8 Boule Center

[0593] 9 Boules

[0594] r radial direction

[0595] 10 striae or layered streaks

[0596] 11 Inhomogeneity

[0597] S side surface

[0598] z' z-range of the survey

[0599] r' radial area of ​​measurement

[0600] 12 Raman facility

[0601] 12a Raman spectrum

[0602] 13 optically used area

[0603] 14 Lens

[0604] A mounting plate

[0605] 15 Positioning device

[0606] R1 radius of the boules

[0607] a angle

[0608] R2 local radius

[0609] y local y-axis of the substrate body 16 Measurement radiation

[0610] z local z-axis of the substrate body 17 mirror surface

[0611] 18 Fourier transform infrared spectrometer 19 Infrared spectrum

[0612] 20 beam splitters

[0613] 21 optical element

[0614] 22 Irradiation facility

[0615] 23 Bleach radiation

[0616] 24 Temperature control unit

[0617] 30 Measurement information block 31 Parameter block

[0618] 32 Position determination block

[0619] 33 Mapping block

[0620] 34 Manufacturing block

[0621] 35 Reference area

[0622] 100 EUV projection system

[0623] 101 Lighting system

[0624] 102 Radiation source

[0625] 103 Lighting optics

[0626] 104 object field

[0627] 105 Object level

[0628] 106 reticles

[0629] 107 label holders

[0630] 108 Reticle displacement drive

[0631] 109 Projection optics

[0632] 110 image field

[0633] 111 Image plane

[0634] 112 wafers

[0635] 113 wafer holders

[0636] 114 Wafer transfer drive

[0637] 115 EUV / Useful / Illumination radiation

[0638] 116 Collector

[0639] 117 Intermediate focus plane

[0640] 118 Deflection mirrors

[0641] 119 first faceted mirror / field faceted mirror 120 first facets / field facets

[0642] 121 Second faceted mirror / Pupil faceted mirror 122 Second facets / Pupil facets

[0643] 200 DUV projection exposure system

[0644] 201 Lighting system

[0645] 202 reticulation days

[0646] 203 reticles

[0647] 204 wafers

[0648] 205 wafer holders

[0649] 206 Projection optics

[0650] 207 lens

[0651] Version 208

[0652] 209 lens bodies

[0653] 210 Projection beam Mi mirror

Claims

67 Patent claims:

1. Method for spatially resolved measurement of at least one homogeneity parameter in a volume of a substrate body (2), in particular a substrate body (2) of an optical element (116, 118, 119, 120, 121, 122, Mi, 207) of a projection exposure system (100, 200), comprising at least the following steps: a) Acquisition of a respective measurement information in at least one volume element (4) of the substrate body (2) by means of a measuring device (3), b) Determination of a value of at least one homogeneity parameter from the respective measurement information using a computing device (5), c) Determination of a spatial position of the at least one volume element (4) using a position determination device, (6) d) Determination of a spatial distribution (7) of the at least one homogeneity parameter from the spatial position of the at least one volume element (4) and the respective associated homogeneity parameter using the computing device (5).

2. Method according to claim 1 , characterized by the fact that in step a) a Raman spectrum (12a) is acquired as measurement information in at least one volume element (4) of the substrate body (2) by means of a Raman device (12).

3. Method according to claim 2, characterized by the fact that an immersion fluid is applied to a surface of the substrate body (2).

4. Method according to claim 1, 2 or 3, characterized by the fact that the substrate body (2) is rotationally symmetric and / or is produced rotationally symmetrically using a Boule process.

5. Method according to any one of claims 1 to 4, characterized by the fact that In step a) several volume elements (4) are measured which are arranged along a reference surface (35).

6. Method according to claim 6, characterized by the fact that In step d) the spatial distribution (7) of the homogeneity parameter in the entire substrate body (2) is reconstructed from the measurement information of the volume elements (4) along the reference surface (35).68 7. Method according to any one of claims 1 to 6, characterized by the fact that the spatial distribution (7) is determined by locating a previously known mapping (7a) of the at least one homogeneity parameter in the substrate body (2).

8. Method according to claim 7, characterized by the fact that the previously known mapping (7a) is located in the substrate body (2) by identifying at least one pattern of at least a part of the previously known mapping (7a) based on the measurement information of the volume elements (4).

9. Method according to any one of claims 5 to 8, characterized by the fact that as reference area (35) a virtual radial cross-sectional surface of the substrate body (2), and / or at least a section of a lateral surface of the substrate body (2), and / or an actual radial cross-sectional area of ​​a spoke of the substrate body (2) and / or an actual radial cross-sectional area of ​​a sister substrate body of the substrate body (2), is measured.

10. Method according to any one of claims 1 to 9, characterized by the fact that Several volume elements (4) are measured along a line perpendicular to the striae (10) of the substrate body (2).

11. Method according to any one of claims 1 to 10 characterized by the fact that as substrate body (2) a titanium-doped quartz glass is measured and / or that X-ray fluorescence is recorded as measurement information.

12. Device (1) for spatially resolved measurement of at least one homogeneity parameter in a volume of a substrate body (2), in particular a substrate body (2) of an optical element (116, 118, 119, 120, 121, 122, Mi, 207) of a projection exposure system (100, 200), comprising at least: a measuring device (3) for recording a respective measurement information in at least one volume element (4) of the substrate body (2), a computing device (5) for determining a value of at least one homogeneity parameter from the respective measurement information,69 a position determination device (6) for determining a spatial position of the at least one volume element (4), wherein the computing device (5) is configured to determine a spatial distribution (7) of the at least one homogeneity parameter from the spatial position of the at least one volume element (4) and the respective value of the associated homogeneity parameter.

13. Device (1) according to claim 12, characterized by the fact that the measuring device (3) includes a Raman device (12) for recording a Raman spectrum (12a) as measurement information in the at least one volume element (4) of the substrate body (2).

14. Device (1) according to claim 12 or 13, characterized by the fact that as measurement information a ratio of TiÜ2 to SiÜ2 and as homogeneity parameter a coefficient of thermal expansion in the volume element (4) can be determined.

15. Device (1) according to any one of claims 12 to 14, characterized by the fact that a positioning device (15) is provided which positions the measuring device (3) to the substrate body (2) in such a way that the measurement information can be detected in the at least one volume element (4).

16. Device (1) according to any one of claims 12 to 15, characterized by the fact that the measuring device (3) comprises a Fourier transform infrared spectrometer (18) for recording an infrared spectrum (19) of the at least one volume element (4).

17. Device (1) according to any one of claims 13 to 16, characterized by the fact that the Raman device (12) is set up to perform confocal Raman spectroscopy.

18. Device (1) according to any one of claims 12 to 17, characterized by the fact that an irradiation device (22) is available and equipped to bleach the at least one volume element (4) by means of bleaching radiation (23), and / or a temperature control device (24) is available and configured to at least partially temperature control the substrate body (2), and / or A temperature measuring device is present and set up to measure the temperature of the 70 to detect substrate body (2).

19. Optical element (21), in particular mirrors (116, 118, 119, 120, 121, 122, Mi) of an EUV projection exposure system (100), with at least one substrate body (2), characterized by the fact that the substrate body (2) at least partially using a method according to any one of claims 1 to 11, and / or a device according to any one of claims 12 to 18, is manufactured.

20. Lithography system, in particular projection exposure system (100, 200) for semiconductor lithography, with an illumination system (101, 201) with a radiation source (102) and optics (103, 109, 206) which has at least one optical element (116, 118, 119, 120, 121, 122, Mi, 207), characterized by the fact that at least one of the optical elements (116, 118, 119, 120, 121, 122, Mi, 207) a substrate body (2) which is at least partially measured using a device (1) according to one of claims 12 to 18 and / or comprising a substrate body (2) which is at least partially measured using a method according to one of claims 1 to 11, and / or at least partially an optical element (21) according to claim 19.