Binder for cellulose-containing materials and composite products comprising the same
A hydrophobizing agent with phenolic biopolymers and alkali silicates enhances water resistance and stability in cellulose-containing materials, addressing hydrophobicity and emission challenges, suitable for use in wood-based composites and meeting environmental standards.
Patent Information
- Application Number
- PCT/EP2026/063362
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-05-08
- Publication Date
- 2026-11-12
AI Technical Summary
Current binders for cellulose-containing materials, such as wood-based composites, face challenges in achieving sufficient hydrophobicity and water resistance, especially in humid environments, while also complying with VOC and VVOC emission standards, and often require hazardous chemicals like formaldehyde and isocyanates, posing safety and health risks.
A hydrophobizing agent comprising phenolic biopolymers, organic acid, alkali silicates, alkali hydroxide, and water is used to enhance the water resistance and boil-proofness of cellulose-containing materials, suitable for use with conventional binders, including protein-based ones, without adding formaldehyde or isocyanates.
The hydrophobizing agent improves water resistance and mechanical stability, meeting EN 322 and EN 1087-1 standards, reduces VOC and VVOC emissions, and is compatible with existing production processes, making the materials suitable for damp areas and reducing the need for hazardous chemicals.
Smart Images

Figure IMGF000018_0001_TABLE 
Figure IMGF000018_0002_TABLE 
Figure IMGF000019_0001_TABLE
Abstract
Description
[0001] Binders for cellulose-containing materials and composite products containing them
[0002] In a first aspect, the present invention relates to water-repellent agents for cellulose-containing materials, which contain at least phenolic biopolymers, organic acid, alkali silicates, alkali hydroxide, and water. In a further aspect, binder compositions for cellulose-containing materials are provided, wherein these binder compositions contain or consist of water-repellent agents according to the invention. Finally, composite material products made from cellulose-containing starting material with binders according to the invention are provided.
[0003] State of the art
[0004] Binders play a crucial role in the production of wood-based composites and wood-based materials in general, as well as materials made from or containing cellulose-containing materials. The use of binders is restricted by the VOC Directive to limit the emission of VOCs (volatile organic compounds) or VVOCs (very volatile organic compounds). Depending on the type and condition of the cellulose-containing materials used, such as lignocellulose, the wood species, the gluing time, and the gluing conditions of the wood or other cellulose-containing materials, VOCs or VVOCs are present in varying chemical compositions and quantities.
[0005] Furthermore, these VOCs and VVOCs, especially formaldehyde, are released when binders based on aminoplasts are used. Since formaldehyde is a major representative of VVOCs, the binder industry is focusing on reducing its emissions. Accordingly, conventional binders, in this case formaldehyde-based resins such as UF (urea-formaldehyde) or MUF (melamine-urea-formaldehyde resins), are being further developed.
[0006] As an alternative to formaldehyde-based binders or resins, isocyanate-based binders, such as PMDI, have been developed. However, these binders pose a problem due to their high cost and the resulting need for protective measures, as isocyanates are classified as hazardous substances and can, for example, produce hydrogen cyanide in the event of a fire. Therefore, stringent safety precautions are necessary when processing isocyanate-based binders. Other binders, such as protein-based binders, have also been developed. Protein-based binders of both animal and plant origin are known. These do not require the addition of formaldehyde for processing, but are not universally applicable.
[0007] The hydrophobization of cellulose-containing materials and products thereof plays a crucial role. Materials containing cellulose are classified, for example, into P1 to P7 for particleboard. While materials and products classified as P1, P2, P4, or P6 are suitable for use in dry areas, classifications P3, P5, or P7 indicate suitability for humid environments. Appropriate hydrophobization is essential, particularly for providing suitable composite materials for humid environments. A challenge for these materials when used in humid environments is their tendency to swell, as well as the need for water resistance. For years, the wood-based industry has used wax dispersions as additives for hydrophobization, typically at concentrations of 0.5 to 2.5% of the dry wood. However, such wood-based products do not achieve the classifications required for humid environments.P3 for particleboard, MDF-H for fiberboard, and also not OSB 3. Rather, such hydrophobization with wax dispersions only reduces the thickness swelling of wood-based materials at high humidity.
[0008] Various other approaches have been taken to achieve sufficient hydrophobization of materials for humid environments, i.e., to improve the water resistance of wood-based materials. For example, in urea-formaldehyde resins (UF resin), the most widely used binder for cellulose-based materials worldwide, melamine is added in high proportions to achieve the necessary water resistance. Formaldehyde-resin-bonded wood-based materials, such as particleboard, fiberboard, plywood, etc., exhibit continuous formaldehyde off-gassing, which, despite compliance with the relevant standard EN 120, is considered problematic from a consumer protection perspective. Indeed, numerous studies have shown that carcinoma formation and damage to the nervous system have been observed at corresponding formaldehyde concentrations. Accordingly, the limit values for formaldehyde were lowered in 2023 from E1 = 0.1 ppm to E0.5 = 0.06 ppm.
[0009] In addition to the aforementioned UF resins, phenol-formaldehyde resins (PUF) are used as an alternative, which are designed for increased water resistance of the resulting wood-based material. This binder is mainly used in the plywood industry.
[0010] As an alternative, the aforementioned isocyanate-based binders, such as PMDI, are used; these exhibit high water resistance. While isocyanates offer advantages over MUF / PUF resins because they chemically bond with cellulose-containing materials like lignin and cellulose, their use is associated with significant drawbacks. Strict protective measures are necessary during the production of these composite products. The entire production line becomes contaminated with wood particles, and workers must wear full protective clothing. Isocyanate is highly toxic and can irritate the respiratory system.
[0011] The aforementioned isocyanate binders also differ in their bonding properties from the corresponding UF resins. UF resins are filler adhesives that, for example, fill the voids between the fibers of wood chips and encapsulate the wood particles as completely as possible. To produce suitable wood-based materials with MUF resins that meet the swelling values according to EN 322 and also pass a boiling test, an increased amount of binder (up to 30%) is required. In contrast, isocyanate-based binders allow for contact bonding. However, here, fine atomization of the isocyanates is necessary to achieve the appropriate cross-linking with cellulose or lignin.
[0012] As previously mentioned, melamine is used as a water-repellent agent in UF resins. Melamine is insoluble in water but readily soluble in formaldehyde. The amount of melamine used, based on the weight of the adhesive, typically ranges from 4 to 24% by weight. However, due to the known side effects of melamine, a ban on its use as an additive in wood-based materials is expected in the medium term. Furthermore, melamine production requires significant energy, so currently, primarily East Asian melamine is used for cost reasons.
[0013] The market therefore demands so-called NAF binders (non-added formaldehyde binders). Efforts are being made to produce these from raw materials that are as close to nature as possible. Accordingly, protein-based binders, both animal and plant-based, are being developed. However, these protein binders (plant-based protein binders) lack the necessary hydrophobicity, meaning the required water resistance is not achieved. Currently, such wood-based materials are only used indoors, for example, as P1 and P2 particleboard.
[0014] Furthermore, it is important that water-repellent agents are suitable for the manufacturing processes. The production of wood-based materials requires heat treatment at high pressing temperatures. This heat treatment is typically in the range above 180°C, especially 220°C and higher. Economic requirements also necessitate that the pressing factor, for example, for MDF / HDF, be 5.5 s / mm of board thickness, while for particleboard, pressing factors are below 4 s / mm. Such speeds can only be achieved with high pressing temperatures, usually in the range of 220°C to 240°C. However, such high temperatures lead to increased emissions of VOCs and VVOCs in the wood and binders. To overcome this problem, corresponding alternative bio-binders have been developed, for example, those based on protein hydroxide aldehyde resin, but also those with proteins and chemical cross-links.based on proteinogenic amino acids and chemical components, with protein as a filler.
[0015] EP 1742542 describes a process for producing an adhesive based on denatured proteins with melamine-formaldehyde. WQ2022 / 0197902 describes a process for producing an aqueous binder from plant proteins, glycerin, peroxide, urea, water glass, and modified lignin. However, the wood-based materials produced according to these regulations showed that the corresponding P3 standards for particleboard and MDF-H were not met for fiberboard. Likewise, the boiling test according to EN 312-1 was not passed.
[0016] DE102005051350 A1 shows a lignin adhesive consisting of lignosulfonate. This melamine-based adhesive also does not meet the requirements of EN322; its ingredients are highly hydrophilic.
[0017] Binders for cellulose-containing materials containing animal protein products and phenolic oligomers are known from WO2019057853.
[0018] US patent 2687556A discloses methods for the production of compressed lignocellulose materials with soluble silicates. CN 106118764A describes additives for concrete, which include, among other things, added formaldehyde.
[0019] There are currently no suitable bio-based binders that exhibit strong hydrophobic properties and meet the requirements of EN 322, including a boiling test according to EN1087-1, that comply with VOC values, can be considered sustainable and achieve technical values according to EN312 under production conditions that correspond to those with conventional binders, especially production speeds on existing board production facilities.
[0020] The object of the present invention is therefore to provide suitable hydrophobing agents for cellulose-containing materials, as well as compositions containing or consisting of such hydrophobing agents, with suitable materials made from cellulose-containing materials and binders that meet the requirements for water resistance and boil resistance. Description of the invention
[0021] In a first aspect, the present invention relates to a hydrophobizing agent for cellulose-containing materials comprising
[0022] a. Phenolic polymers;
[0023] b. Organic acid;
[0024] c. Alkali silicates;
[0025] d. Alkali hydroxide;
[0026] e. Water.
[0027] The hydrophobizing agent according to the invention, used alone as a binder or as an additive to known binders, enables the improvement of the water resistance of composite material products, in particular panels and profiles, to make them suitable for damp areas.
[0028] In particular, it has been shown that this agent is suitable for use at high production speeds with minimal compression ratios, while maintaining the desired mechanical stability of the resulting composite products and high water resistance, thus meeting relevant standards for damp environments. A particular advantage is that the hydrophobic agent consists largely of renewable components, thereby meeting relevant environmental requirements and minimizing the use of fossil-based ingredients. These hydrophobic agents are NAF products, meaning formaldehyde-free hydrophobic agents that contribute only minimally to the emission of WC and VVOCs.In particular, it was surprisingly found that the hydrophobizing agent according to the invention is also suitable as an additive for protein-based binders, both animal and especially plant proteins, particularly for the bio-binders currently on the market, which are usually based on protein resins such as protein hydroxyaldehyde resin. These binders can be modified by the hydrophobizing agent according to the invention in such a way that the products manufactured with them meet the requirements for water resistance and boil-proofness according to the relevant guidelines. The hydrophobizing agent can be used in combination with other corresponding additives in the binder or as a replacement for corresponding hydrophobizing agents in known binders. The hydrophobizing agent according to the invention can be easily mixed with conventional binders without significantly altering their consistency. Accordingly, its use is, for example,This is possible when applying glue with conventional equipment and pumps. Preferably, the solids content of the glue is less than 65% and the viscosity does not exceed 600 mPas.
[0029] The hydrophobizing agent allows binders based on plant proteins to achieve the necessary water resistance standards, DEN622 and DEN312, without the need for the addition of other chemical components such as furan, aldehydes, amino-epichlorohydrin or other toxic substances.
[0030] As mentioned, the hydrophobizing agent according to the invention can, for the first time, when using binders based on plant proteins, provide water resistance that meets standards for correspondingly manufactured composite products based on cellulose-containing materials.
[0031] However, it was also shown that, for example, when using the hydrophobizing agent according to the invention in known MUF resins, the use of melamine is reduced by replacing the melamine with the hydrophobizing agent, and thus the hydrophobizing agent according to the invention can be used partially or completely as a melamine replacement in MUF resins.
[0032] It also showed that when using the hydrophobizing agent according to the invention with isocyanate-based binders, the amount of isocyanate can be reduced and substituted by the hydrophobizing agent according to the invention.
[0033] When using the hydrophobizing agent according to the invention with plant protein binders, the desired water resistance could be achieved for the first time, thus the composite material products obtained in this way can be used not only indoors but also in damp areas.
[0034] For the purposes of this document, "cellulose-containing material" refers to materials containing cellulose, hemicellulose, holocellulose, or lignocellulose. Cellulose-containing materials include wood, pulp, straw, and so on. The corresponding raw materials for the production of wood-based materials and engineered wood panels are therefore cellulose-containing materials, such as those made from wood chips, sawdust, wood fibers, and wood veneers. Cellulose-containing materials can also be derived from annual plants such as straw, flax, hemp, coconut, and so forth.
[0035] The cellulose-containing materials in question can be derived from virgin wood or recycled materials. Unless otherwise stated, the term "binder" here refers to suitable binders for use in the wood-based materials industry or as binders for materials based on cellulose-containing materials. Well-known examples include the aforementioned formaldehyde binders, such as UF, MUF, or PMUF resins. Other common binders include isocyanate-based binders, including those based on isocyanates, such as PMDI, polyurethane-based adhesives, or tannin-formaldehyde adhesives. Further adhesives include the aforementioned protein-containing binders, particularly those of plant origin.
[0036] Phenolic biopolymers are natural macromolecules structurally composed of phenolic units—aromatic compounds with at least one hydroxyl group. They are structural components of biomass and are characterized by their aromatic structure, which confers exceptional stability. They are produced by organisms, primarily plants.
[0037] Phenolic biopolymers, also known as phenolic oligomers, are primarily components derived from lignin. Preferably, these phenolic biopolymers have a weight-average molar mass in the range of 1000 to 5000 g / mol, and particularly in the range of 2000 to 4000 g / mol, such as 2500 to 3000 g / mol.
[0038] Suitable components containing phenolic biopolymers are, in particular, lignocelluloses, which are available according to the organosolv process (also known as the soda process), the Minox process, the Formacell process, the Organocell process, and preferably the sulfate process (also known as the Kraft process). A particularly suitable phenolic biopolymer is Kraft lignin. The component containing phenolic biopolymers, preferably Kraft lignin, can be used, in particular, in the form of a spray-dried powder. It is further preferred that the component containing phenolic biopolymers, in particular Kraft lignin, is used in an amount of 5 to 50 wt.% based on the total weight of the hydrophobing agent, as well as in an amount of 7 wt.% to 25 wt.%.
[0039] Suitable organic acids are known to those skilled in the art. These organic acids include, in particular, acids which, when added to the hydrophobic agent according to the invention, exhibit a pH value < 3. The pH value can be determined by standard methods, usually at room temperature using appropriately suitable pH meters. Examples of suitable organic acids are carboxylic acids in general, including citric acid, lactic acid, picric acid, acetic acid, and ascorbic acid, or mixtures thereof. The amounts of added organic acids, which preferably exhibit the aforementioned value when added, are, for example, in the range of 1.0 to 4.0 wt.%, such as 1.5 to 3 wt.% based on the total weight of the hydrophobic agent according to the invention.
[0040] The hydrophobizing agent according to the invention comprises alkali silicates as a further component. The corresponding alkali silicates are known to those skilled in the art. Suitable representatives of such alkali silicates are, in particular, water glass, such as potassium silicate or sodium silicate, or mixtures thereof. The alkali silicates can be used in an amount of 2 to 6 wt.%, such as 2.5 to 5 wt.%, for example, in the case of 2 to 4 wt.%, based on the total weight of the hydrophobizing agent according to the invention.
[0041] The alkali silicates according to the invention are accordingly water-soluble, and the hydrophobizing agent according to the invention is water-based.
[0042] Furthermore, the hydrophobizing agent according to the invention contains an alkali hydroxide. Suitable hydroxides are, in particular, sodium hydroxide and potassium hydroxide. The corresponding alkali hydroxide is preferably present in an amount of 0.5 to 5.0 wt.%, e.g., in an amount of 1.5 to 3 wt.% based on the total amount of the hydrophobizing agent.
[0043] Finally, the hydrophobizing agent according to the invention comprises water as a suitable solvent. It is present in an amount up to 100 wt.% of the hydrophobizing agent. Hereinafter, the expressions "up to 100 wt.%" and "Ad 100 wt.%" are used synonymously. That is, the water is added to the agent in an amount sufficient to reach a total of 100 wt.%. For example, if the amount of components a. to g. is 36 wt.%, water is added in an amount of 64 wt.% to reach a total of 100 wt.%. The term "ad" is familiar to those skilled in the art in this context.
[0044] In one embodiment, the hydrophobizing agent according to the invention further contains metal salts, such as copper salts, iron salts, or manganese salts, or mixtures of these salts. Copper salts, in particular, have proven to be especially suitable. These metal salts, such as copper salts, are present in the hydrophobizing agent, especially when it is a component of binders for protein binders, particularly those of plant origin.
[0045] A particularly suitable copper salt is copper(II) chloride dihydrate. Other suitable partial salts, especially copper salts, are: copper(II) acetate, copper(II) nitrate hemipentahydrate. In a further embodiment, the hydrophobizing agent according to the invention can also contain an organosilane. Suitable organosilanes are known to those skilled in the art and are commercially available from various companies. A typical example is the product DYNASILAN from Evonik Industries AG. This organosilane consists of bifunctional compounds that have a reactive organic group, e.g., organic epoxides, and hydrolyzable methoxysilyl groups.
[0046] The organosilanes are preferably used in an amount of 1 wt.% to 8 wt.%, 2 to 5 wt.% in the hydrophobizing agent according to the invention.
[0047] In a further embodiment of the hydrophobizing agent according to the invention, a surfactant may also be present. This surfactant may, for example, be added in an amount of 2.5 to 8% by weight based on the total amount of hydrophobizing agent.
[0048] In another embodiment, a hydrophobizing agent according to the invention is a non-ionic surfactant; when using a mixture of surfactants, at least one of the surfactants is an ionic surfactant.
[0049] In one embodiment, the non-ionic surfactant is selected from octylphenol ethoxylates, nonylphenol ethoxylates, alkyl polyglycosides, and / or alkyl glycosides, particularly polysorbate. It has been shown, in particular, that polysorbate improves the properties of water-repellent agents used in binders based on plant proteins. Polysorbates such as the Tween products are especially suitable. The polysorbates can therefore be corresponding polysorbates 20, 21, 40, 60, 61, 65, 80, 81, or 120.
[0050] Unless otherwise stated, the individual components of the hydrophobizing agent according to the invention mentioned herein include both single and multiple such compounds falling under the corresponding groups, such as 2, 3, 4 or more compounds.
[0051] The hydrophobizing agent is produced according to known methods; suitable methods are known to those skilled in the art.
[0052] In one embodiment, the hydrophobizing agent according to the invention for cellulose-containing materials comprises:
[0053] a. Phenolic biopolymers in an amount of 5 to 50 wt.%;
[0054] b. Organic acid in an amount of 1.5 to 4.0 wt.%; c. Alkali silicates in an amount of 2.0 to 6.0 wt.%;
[0055] d. Alkali hydroxide in an amount of 0.5 to 5.0 wt.%;
[0056] e. Possibly metal salt in an amount of 0.3 to 3% by weight;
[0057] f. If necessary, organosilane in an amount of 1.0 to 8.0 wt.%;
[0058] g. If necessary, surfactant in an amount of 2.5 to 8.0 wt.%;
[0059] h. Water up to 100 wt.%.
[0060] In another aspect, the present application relates to binder compositions for cellulose-containing materials, wherein these binders incorporate hydrophobizing agents according to the invention. In one embodiment, a conventional binder can contain the hydrophobizing agent according to the invention as an additive; in another embodiment, the binder can consist essentially of the hydrophobizing agent according to the invention. It has been shown that the binder according to the invention improves the water resistance and boil-proofness of the products. In particular, the binders according to the invention are suitable for imparting corresponding properties to plant-protein-based binders as well.
[0061] In one embodiment, the binder is a binder based on UF / MlIF, PMIIF, protein binder, or isocyanate, in particular a plant-based protein binder, wherein the hydrophobizing agent according to the invention is added to the binder as an additive. The proportion can be in the range of 2-50 wt.%, preferably 5-30 wt.%, particularly preferably 7-15 wt.% based on the total amount of the total binder.
[0062] In one embodiment, the binder according to the invention further comprises conventional components, if necessary. These include: at least one component from the group consisting of hydrowax, fungicides, flame retardants, fragrances, colorants, fillers and mixtures thereof.
[0063] It was found that the hydrophobizing agents and binders according to the invention can be used in conventional production processes. In melamine-containing binders, the melamine can be partially replaced while maintaining the hydrophobic properties. With UF resins, no reduction in pot life was observed after the addition of hardener, and the storage time in the holding tank is not affected.
[0064] In isocyanate binders, the hydrophobizing agent according to the invention can be used as a replacement for the isocyanate. Up to 30% of isocyanate can be saved in OSB boards. Finally, for the first time, hydrophobizing agents for protein binders and corresponding binders can be provided that are sufficiently water-resistant. The basic basis of various protein binders is vegetable protein from soy, rapeseed, pea, corn, etc., and glycerin. The hydrophobizing agent harmonizes very well with these base substances because it is adjusted to a pH range of 8-10 and the proteins cannot denature prematurely.
[0065] Finally, composite products are provided by binding a cellulose-containing starting material with a binder according to the invention and accordingly shaping the desired product.
[0066] Suitable cellulose-containing starting materials include wood or annual plants, such as wood fibers, wood shavings, wood dust or wood flour, wood chips, strands, veneers or material processed using the scrimber method or recycled material.
[0067] In one embodiment, the composite products are panels or molded parts including particleboard, MDF, HDF, OSB, plywood, laminated timber, or insulation panels.
[0068] Finally, processes are provided whereby the composite materials are manufactured using the hydrophobizing agents and binders according to the invention. These processes are conventional manufacturing methods for the corresponding composite products. The heat treatment and pressing of the materials to produce the composites takes place, for example, at a temperature in the range of 100°C to 250°C. The pressure is, for example, in the range of 1 to 250 bar, such as 10 to 80 bar.
[0069] Suitable water repellents include, for example:
[0070] a) For UF resins as binders:
[0071] phenolic macromolecule (biopolymer),
[0072] NaOH,
[0073] water-soluble alkali silicates,
[0074] Copper(II) chloride dihydrate,
[0075] an organosilane
[0076] Citric acid,
[0077] b) For isocyanate-based binders:
[0078] a phenolic macromolecule (biopolymer),
[0079] NaOH,
[0080] water-soluble alkali silicates, copper(II) chloride dihydrate,
[0081] an organosilane
[0082] Citric acid,
[0083] c) For binders based on plant proteins, here undenatured plant proteins, e.g. rapeseed, soy, pea, corn, wheat, broad bean, etc.,
[0084] a plant-based sugar alcohol, propane-1,2,3-triol,
[0085] an oxidizing agent
[0086] a polysorbate
[0087] a phenolic macromolecule (biopolymer),
[0088] NaOH,
[0089] water-soluble alkali silicates,
[0090] Copper(II) chloride dihydrate,
[0091] an organosilane
[0092] Citric acid.
[0093] These fully met the requirements.
[0094] In a preferred embodiment of protein binders, undenatured vegetable proteins in the form of dried rapeseed or soybean meal are used. After cold pressing, these proteins are primarily used as animal feed, in biodiesel, or in biogas production. The protein content is approximately 32% for rapeseed and 55% for soybeans. Protein concentrates with a protein content of 65% or isolates with a protein content greater than 90% can also be used. Concentrates and isolates are currently not preferred from an economic perspective because the binder is less competitive.
[0095] The addition of polysorbate unfolds the protein molecule, thus enabling a more pronounced reaction during the actual denaturation process under heat. The formation of glyceraldehyde from propane-1,2,3-triol (glycerol) occurs using a suitable mild oxidizing agent, preferably hydrogen peroxide. The pressing process during wood-based panel production, at temperatures above 100°C, acts as a catalyst. These compounds can interconvert via an enediol rearrangement (Lobry-de Bryn-van Ekenstein rearrangement). Therefore, it is not necessary to add a pure aldehyde to the binder.
[0096] The presence of a phenolic macromolecule, i.e., a phenolic biopolymer, such as Kraft lignin with a molar mass of 3000, results in a high hydrophobic property. It is known to those skilled in the art that Kraft lignin, produced by the sulfonate or organosolv process, is insoluble in water. Therefore, an alkali hydroxide, such as NaOH, is added. The incorporation of this lignin (lignin incrustation) leads to a lignification of the cell wall and thus to improved mechanical stability.
[0097] Surprisingly, it was discovered that Kraft lignin can be neutralized by an organic acid, thereby revealing the binder's high hydrophobicity. Additionally, the binder binds with the lignin within the cell structure, ensuring that the required technical properties are achieved even after several hours of boiling.
[0098] The following are some considerations regarding gluing:
[0099] To obtain the “absolute dry wood mass” (atro ), the cellulose- or lignocellulose-containing material is dried at 103°C until a constant weight is achieved (see EN 322 and DIN 53183)
[0100] To overcome the difficulty of producing a hydrophobic, natural additive, aspects of adhesive theory and the properties of the wood material must be taken into account.
[0101] In the production of particleboard (up to 750 kg / m²) 3Wood chips (primarily from pine, spruce / fir, and an increasing proportion of hardwoods) are shredded into various fractions using ring chippers and hammer mills. This material has a wood moisture content of 25–35% in the fiber saturation range for fresh wood. Recycled wood is increasingly being used because the harvest of fresh wood has been significantly reduced by pest infestation. In 2021, the proportion of recycled wood in particleboard was already 50% (17 million m³) and is rising. (European Panel Federation) Recycled wood consists of a mixture of softwood, hardwood, particleboard bonded with UF / MUF resin, OSB bonded with isocyanates, and MDF / HDF bonded with UF / MUF. Only Class A2 wood may be used. Class A2: Glued, coated, and varnished reclaimed wood without halogenated organic compounds in the coating and without PVC content. This material has a moisture content between 8 and 16%.
[0102] The difference in the fiber saturation point of wood is caused by the content of wood extractives and an increased lignin content in the cell walls. If the fiber saturation point is undershot, the swelling water is drawn out of the cell walls. The cell wall dries and shrinks. If drying is driven below 5%, it always results in chemical changes (keratinization) of the wood surface of the chip fraction. Bound water is continuously removed. Below the fiber saturation point, the wood is hygroscopic. It reabsorbs water at increased ambient humidity and swells. In industry, the chip fraction is dried down to 0.8–2.4%.
[0103] In particleboard production, the aqueous bio-based binder with a solids content of 50-65% is mixed with the dried wood chips in a blender. The chips are hygroscopic, and the wood moisture content after gluing is approximately 9% (glue application rate: surface layer 9%, core layer 7%).
[0104] The high hygroscopicity is due to hemicellulose, which in coniferous trees primarily contains hexosans, i.e., monosaccharides. Furthermore, different trees exhibit varying numbers of wood constituents, some of which are highly hygroscopic. These include pine, spruce / fir, larch, linden, aspen, and birch, containing substances such as alkaloids, terpenes, sugars, salts, acids, and also hydrophobic substances like resins, fats, oils, and waxes.
[0105] Furthermore, it should be noted that approximately 10% of the chipped wood is sapwood, which includes the phloem, cambium, and fresh earlywood. This wood is more porous than the heartwood and, due to its larger surface area, more susceptible to swelling after drying. Through its extensive capillary structure, the sapwood draws water from the soil and distributes it to the crown. Sapwood is significantly lighter after drying, with a density of approximately 280 kg / m³ in pine, compared to approximately 500 kg / m³ for heartwood.
[0106] In the production of medium-density fiberboard (MDF, up to 780 kg / m³), the wood is processed into wood chips, just as with particleboard. The wood chips are then treated using the Asplund process with steam at approximately 180°C and a pressure of 8-12 bar. After this plasticization, the material is conveyed to the actual refiner, where it is further broken down into fibers and then transported onward. This entire process is referred to as a refiner system. The refiner system includes components such as a pre-steam hopper, a screw conveyor, a digester, a refiner, and a discharge valve.
[0107] During the cooking process, lignins and hemicellulose are released from the outer walls of the wood chips, and the saturated chips are then fed into the fiberization process in the refiner. The fiberization process takes place under pressure using grinding discs. This process produces lye, which must be disposed of properly. The wood moisture content during this process exceeds 100% based on the dry wood content. (For example, freshly cut logs have a moisture content of 120-180%, depending on the tree species.) Immediately after exiting the refiner's discharge valve, the wet fibers flow at high speed through a blow line and are coated with a binder via nozzles. Only then are the wet, coated fibers fed into a dryer and dried to a moisture content of approximately 9-11%.
[0108] The saturated hemicellulose is exposed to binder at the boundary layers of the wet fibers, and the binder penetrates the fiber structure due to the hygroscopicity of the monosaccharides.
[0109] Functionality of the hydrophobizing agent according to the invention in natural binders
[0110] A valuable property of proteins is their ability to bind formaldehyde. Formaldehyde has a non-rotating amino group on its peptide chain with which the protein can react. This is important because all wood releases formaldehyde at higher temperatures, which can be captured by the adhesive protein (capture function). For this purpose, undenatured proteins are preferred, as they are also responsible for high reactivity and allow for short pressing times. The plant proteins denature within seconds of reaching 100°C during the pressing process, and a lattice structure is formed by the crosslinking agent. Glyceraldehyde acts as the crosslinking agent, which is cleaved in situ from glycerol at temperatures above 95-100°C.
[0111] Furthermore, the water-glycerin mixture contained in the adhesive causes the partial separation of lignin and cellulose in the wood. Although highly efficient extraction of lignin from the wood fibers at high temperature requires a considerable amount of time and even the use of a catalyst, the partial removal of lignin occurs throughout the entire processing time of high-temperature MDF, i.e., boiling, fiberization in the refiner, bonding of the wood fibers via blow-line, drying, and subsequent forming and pressing into fiberboard.
[0112] The densification resulting from the increase in the solid phase in the adhesive during the pressing process under heat causes the mixture to disperse until it hardens. The delignification that occurs during this process leads to an increase in the solids content of the adhesive and exposes the bundles of crystalline cellulose fibers from wood, which, due to hydrogen bonds, are susceptible to interactions with adhesive components in the interface. Delignification is generally accompanied by a change in the natural structure of lignins. This results in a rearrangement reaction in which CO and CC bonds are cleaved and new CC bonds are formed. Such a rearrangement reaction also occurs during the production of wood-based materials with the addition of the hydrophobizing agent according to the invention, hereinafter also referred to as additive LCC.The following interactions can occur in protein binders: hydrogen bonds, dipole-permanent-permanent dipole, and van der Waals dispersion (induced dipole-induced dipole). Hydrogen bonds appear to play the most significant role among these interactions. All basic components of the binder and the additive LCC according to the invention can interact via hydrogen bonds under competitive conditions.
[0113] Protein aggregation or entanglement of protein chain fragments plays a role. Aggregation or entanglement of protein chains (or fragments thereof) can occur during high-temperature pressing under increased pressure of the plate (large vibrations of the free chain fragments are possible).
[0114] The addition of polysorbate proves advantageous in protein-based binders, as it causes the proteins to unfold. The surface area of the proteins becomes larger and more reactive.
[0115] Intermolecular interactions play a crucial role in the production of the adhesive, its durability, and the bonding of chips and fibers. They also influence the properties of the wood-based panel, which must not be compromised by additives. The strength of a boil-proof wood-glue bond is achieved by transitioning the glue from a liquid to a solid state. During this process, the glue gels and forms a symbiotic relationship with the extractives or hemicellulose components of the wood, resulting in strong cohesive and adhesive forces between the glue and the wood. This process is further enhanced by oligomeric phenols (biopolymers) of kraft lignin, which bind to the natural lignin in the wood.
[0116] Modern binders in the wood-based materials industry should consist largely of sustainable, non-toxic materials. Plant-based protein binders with integrated water repellents largely meet the following requirements:
[0117] 1. Sustainability
[0118] Definition: Sustainability refers to the use of renewable resources (forests, energy crops) that takes into account their respective regenerative capacity. The goal is long-term thinking, especially long-term economic action, that utilizes nature today in such a way that the foundations of life for future generations are permanently preserved (intergenerational responsibility).
[0119] Source: Schubert: The Political Lexicon 7, updated 2020. The present water-repellent agent has a high sustainability value. 2. - “Cradle to grave”, Carbon Footprint (LCA = life cycle analysis)
[0120] Definition: Carbon Footprint (LCA) is a measure of the total amount of carbon dioxide emissions caused directly and indirectly by activities or generated during the life cycle of a product. This includes transportation and product depreciation. The unit of measurement is kg CO2 generated per kg of product. For example, the value for a binder according to the invention is 1.287 kg CO2 eq / kg binder.
[0121] 3. -Formaldehyde-free — NAF product
[0122] The hydrophobizing agent (H2O blocker) LCC does not introduce any additional formaldehyde into the binder mixture. LCC is a NAF product (non-added formaldehyde).
[0123] 4. Water resistance according to EN 322
[0124] Wood-based panel manufacturers are not satisfied with simply achieving the 24-hour water immersion test and the resulting swelling values. They also conduct a boiling test over 2 or 6 hours, followed by transverse tensile testing. Transverse tensile strength is determined according to the boiling test EN 1087-1. The target values were achieved. (See table below)
[0125] 5. High storage stability and processing using standard equipment
[0126] at the same production speed as with conventional binders.
[0127] 6. Compliance with the prescribed VOC values for particleboard and fiberboard
[0128] (Tested with fresh wood) according to DIN ISO 16000-6, DIN EN ISO 16000-9:2008-04 and DIN EN ISO 16000-11:2006-06; chamber test according to DIN EN 16516; VOC according to DIN 16516, GC / MS; formaldehyde / aldehyde / acetone according to DIN EN 16516, HPLC; evaluation according to AgBB 2018 NIK values (lowest concentration of interest)
[0129] Summary of measurements of all emissions from 16 mm thick single-layer particleboard with 10% glue content on oven-dried wood, 62% solids content. Reference: Urea-formaldehyde resin from BASF Kaurit glue 333. Table 1
[0130] All values in ppm UF MDF MDF LCC 160 g / m2
[0131] +Bio-binder, +Bio-binder,
[0132] +20% Protein, +20% Protein,
[0133] +30% Glycerin +30% Glycerin
[0134] +15% LCC
[0135] Total VVOC ( <C6) 250 109 422 10
[0136] Total VOC (C6-C16) 780 95 119 56
[0137] Total SVOC (C16- <5 <1 <1 <1
[0138] C22)
[0139] TVOC (C6-C16) 780 95 119 56 Formaldehyde 0.051 0.017 0.011 0.000
[0140]
[0141] Limit value 0.06 ppm
[0142] 7. No unpleasant odors during production or in the finished wood-based product.
[0143] 8. All coatings can be carried out without any problems, i.e. paper coating, painting, powder coating, HPL and CPL coating, veneering, metal coating.
[0144] 9. The final product is easily recyclable and compostable due to its natural ingredients.
[0145] Bonding systems for wood-based materials based on natural or near-natural materials do not guarantee compliance with standards for every application, particularly when water resistance is required (swelling values according to EN 322 and transverse tensile strength according to boiling test EN 1087-1).
[0146] The present invention will be further explained by means of examples, without being limited thereto.
[0147] Examples:
[0148] Binder ingredients in the following application examples in wt.% Application example _ _ 1 2 3 4 5 6 Item Ingredient MDF Chipboard OSB Chipboard OSB HDF 1 UF (Silekol No S-120) 78.5
[0149] 2 hardener (ammonium sulfate) 1.5
[0150] 3 PMDI 70
[0151] 4 Soy flour 20 15 19 18 5 Glycerin 80% 30 30 30 30 6 Peroxide 30% 4 2
[0152] 7 NaOH 1 1 1 1 2 2 8 Lignin 40% 9 14 14 12 19 19 9 Polysorbate 0.5 1 1 0 0 1 10 Citric acid 2.5 3 2.5 3 4 4 11 Copper sulfate 2 1 1.5 2 3 3 12 Sodium water glass 2 2 2 2 2 2 13 Dynasilan 3 1 4 0 0 3
[0153]
[0154] 14 H2O 30 18 23 0 0 21
[0155] 100 100 100 100 100 100The following summarizes the components of the hydrophobizing agent according to the invention as LCC (components 7 to 13).
[0156] APPLICATION EXAMPLE 1
[0157] MDF (Bio-binder + LCC)
[0158] On a ContiRoll press from the company Siempelkamp (Krefeld), 16 mm MDF boards were produced using a bio-based binder according to this invention. Press length = 28 meters.
[0159] The board weighed 720 kg / m³. Adhesive was applied using a blow line. The fibers were made from fresh pine wood. The adhesive application rate was 9% of the oven-dried wood.
[0160] The fiber moisture content after drying the glued fibers was 11%.
[0161] The single-component binder mixture used had a solids content of 55%, of which 15% was the additive LCC. (64.8 kg solids, 117.8 kg wet glue).
[0162] LCC including polysorbate with 59.3% solids content. (17.6 kg wet additive LCC).
[0163] The solids content of the binder includes all organic and inorganic components of the binder, including glycerin.
[0164] Pressure factor = 5.5 see / mm
[0165] Pressing temperature = 220 °C
[0166] EN 320 flexural strength
[0167] Position Length Width Thickness Weight Specific Force Duration Bending Elasticity mm mm mm g Weight N s Strength Modulus kg / m3 N / mm 2 N / mm 2 Standard EN 312 24 2200 1 370 51 16.53 219.77 728 455 45.1 26.5 2612.12 2 370 50.6 16.28 220.67 731 406 43.5 28.4 2379.55 3 370 51 .4 16.66 216.15 716 419 40.9 24.7 2511 .34 4 370 51 .1 16.59 220.98 732 443 49.2 29.3 2728.11
[0168]
[0169] Average 51.02 16.49 219.39 727 430 44.7 27.22 2557.76 EN 317 Water Absorption and Dieken Swelling (Bio-Binder + LCC)
[0170] Position Length Width Thickness Specific Thickness Weight Swelling Absorption mm mm mm weight Ge2h 24h 2h 24h 2h 24h 2h 24h g weight mm mm gg % % % % kg / m 3
[0171] Standard MDF H 8
[0172] 1 51 ,1 51 ,2 16.53 28.08 728 17.58 17.76 53.29 57.44 6.39 7.47 83.25 97.52 2 51 ,1 51 ,1 16.28 29.48 731 17.25 17.53 53.19 57.04 5.99 7.72 81 .04 94.15 3 51 ,2 51 ,1 16.66 28.74 716 17.90 18.04 53.39 56.27 7.45 8.34 85.78 98.55 4 51 51.2 16.59 28.07 732 17.55 17.88 52.63 56.83 5.83 7.78 84.86 99.61 5 50.8 50.8 16.62 28.49 726 19.05 50.75 50.75 56.09 6.17 8.12 80.67 99.68 Through3.18 7.88 83.12 99.68
[0173]
[0174] cut 51 51.1 16.5 28.67 727 17.58 18.05 52.5 56.73 EN 317 Water Absorption and Dieken Swelling (Bio-binder without LCC) Through 73.4 93.3 127 154.62
[0175]
[0176] average 51 50.6 16.4 28.41 732 28.44 31.70 64.5 72.34
[0177] EN 319 Tensile strength
[0178] Position Length Width Thickness Weight Specific Force Durability Tensile Strength mm mm mm g Weight N s N / mm 2 kg / m 3
[0179] Standard MDF.H 0.75
[0180] 1 51 51 ,3 16.59 29.08 728 1870 9.1 0.79 2 51 ,2 51 ,1 16.52 29.38 731 1841 12.5 0.83 3 51 51 ,3 16.38 28.34 716 1789 10.3 0.73 4 51 ,4 51 16.48 28.47 732 1852 14.1 0.97 5 51 50.3 16.51 28.09 726 1849 13.6 0.82
[0181] Through
[0182]
[0183] cut 51.1 51.2 16.47 28.67 727 1840 11.9 0.83 APPLICATION EXAMPLE 2
[0184] Chipboard (Bio-binder + LCC)
[0185] On a ContiRoll press from Siempelkamp (Krefeld), 16 mm thick, three-layer particleboards were produced using a bio-based binder plus the additive LCC according to this invention. The press length was 28 meters. The board weight was 640 kg / m³. Adhesive was applied using a blender for the surface layers and the core layer.
[0186] The fibers were made from 80% recycled wood and 20% fresh pine wood. The fresh pine wood was used exclusively in the top layer.
[0187] The amount of glue applied was 9% of the dry wood for the top layers and 7% for the middle layer.
[0188] The top layers 2 x 17.5%; middle layer 65%.
[0189] The moisture content of the chips after drying and before gluing was 4.0%. The fiber moisture content after gluing was 9%.
[0190] The one-component binder mixture used had a solids content of 60%, of which 20% was additive LCC.
[0191] Per m 3 The following quantities of glue are used in chipboard:
[0192] Top layers: 9% absolute at 35% content = 20.16 kg solid and 33.6 kg wet glue. Middle layer: 7% absolute at 65% content = 29.12 kg solid and 48.5 kg wet glue. Total binder = 82.1 kg wet glue.
[0193] LCC including polysorbate with 59.3% solids content (16.42 kg wet additive LCC)
[0194] The solid content of the binder includes all organic and inorganic components of the glue, including glycerin.
[0195] Pressure factor = 6.0 see / mm
[0196] Pressing temperature = 230 °C EN 320 Bending strength
[0197] Position Length Width Thickness Weight Specific Force Duration Bending Elasticity mm mm mm g Weight N s Strength Modulus kg / m 3 N / mm 2 N / mm 2 Norm P3 14 1950 1 370 51 16.59 202.91 645 416 45.1 15.14 2702.38 2 370 50.8 16.38 197.72 642 361 43.5 16.7 2499.43 3 370 51 16.48 200.79 646 386 40.9 16.39 2510.35 4 370 51 .2 16.51 204.77 655 441 49.2 17.6 2628.86
[0198]
[0199] Average 51.1 16.49 201.55 647 401 44.7 16.45 2585.25 EN 317 Water Absorption and Dieken Swelling
[0200] Position Length Width Thickness Specific Thickness Weight Swelling Absorption mm mm mm weight Ge2h 24h 2h 24h 2h 24h 2h 24h g weight mm mm gg % % % % kg / m 3
[0201] Standard 14
[0202] 1 51 ,1 51 ,2 16.56 28.08 641 17.05 18.05 47.47 51.62 3.46 9.03 63.25 77.52 2 51 ,1 51 ,1 16.38 29.98 642 16.95 17.99 46.67 50.84 3.59 9.88 61 .04 75.44 3 51 ,2 51 ,1 16.48 28.34 646 17.16 18.02 45.69 49.75 4.12 9.36 61 .22 75.55 4 51 51.2 16.51 28.47 655 17.15 18.12 45.43 48.28 3.89 9.78 59.58 69.61 5 50.8 50.8 16.52 28.09 659 17.12 18.02 44.57 47.66 3.65 9.12 58.67 69.68 Through3.74 9.43 60.75 73.56
[0203]
[0204] cut 51 51.1 16.53 28.67 648 17.07 18.04 45.96 49.63
[0205] EN 317 Water absorption and Dieken swelling (Bio-binder without LCC)
[0206] Through
[0207]
[0208] cut 51 50.9 16.87 29.21 656 46.05 52.3 82.5 114.73 173 210 283 392 EN 319 tensile strength
[0209] Position Length Width Thickness Weight Specific Force Durability Tensile Strength mm mm mm g Weight N s N / mm 2 kg / m3
[0210] Norm P3 0.45
[0211] 1 51 51 ,3 16.56 29.09 662 1770 8.8 0.68 2 51 ,2 51 ,1 16.38 29.98 670 1777 27.1 0.68 3 51 51 ,2 16.48 28.34 646 1604 8.4 0.61 4 51 ,4 51 16.51 28.47 665 1734 19.1 0.66 5 51 50.3 16.52 27.71 666 1879 14.6 0.72
[0212] Through
[0213]
[0214] average 51.1 51.2 16.47 28.52 662 1753 15.6 0.67
[0215] APPLICATION EXAMPLE 3
[0216] OSB (Biobinder + LCC)
[0217] On a laboratory press, 18 mm single-layer OSB boards were produced using a bio-based binder plus the additive LCC according to this invention. The board weight was 640 kg / m³. The adhesive was applied using a blender. The flakes were made from fresh pine wood and provided to the laboratory. The adhesive application rate was 10% of the dry wood. The wood moisture content after drying before gluing was 3.5%. The moisture content of the flakes after gluing was 10%.
[0218] The one-component binder mixture used had a solids content of 60%, of which 20% was additive LCC.
[0219] Glue quantity: 10%, 64 kg solid and 106.6 kg wet glue
[0220] LCC including polysorbate with 59.3% solids content. (21.32 kg wet additive LCC)
[0221] The solid content of the binder includes all organic and inorganic components of the glue, including glycerin.
[0222] Pressure factor = 8.0 see / mm
[0223] Pressing temperature = 230 °C
[0224] EN 320 flexural strength
[0225] Position Length Width Thickness Weight Specific Force Duration Bending Elasticity mm mm mm g Weight N s Strength Modulus kg / m 3 N / mm 2 N / mm 2 Standard OSB 3 20 3500 1 370 51 .1 18.26 223.2 645 476 42.1 24.1 3708.44 2 370 50.8 18.12 217.49 667 401 39.5 26.89 3911 .24 3 370 51 18.42 220.86 632 398 42.9 20.49 3510.15 4 370 51 .2 18.31 225.24 659 452 46.7 25.5 3622.36
[0226]
[0227] Average 51.02 18.27 221.69 651 416 42.8 24.24 3688.04 EN 317 Water Absorption and Dieken Swelling
[0228] Position Length Width Thickness Specific Thickness Weight Swelling Absorption mm mm mm weight Ge2h 24h 2h 24h 2h 24h 2h 24h g weight mm mm gg % % % % kg / m 3
[0229] Standard 14
[0230] 1 51 ,1 51 ,2 18.26 29.08 671 22.42 22.6 53.29 57.44 35.39 36.47 83.25 97.52 2 51 ,1 51 ,1 18.12 29.38 679 21.93 22.17 53.19 57.04 32.27 33.72 81 .04 94.15 3 51 ,2 51 ,1 18.42 28.34 655 21.61 21.94 52.65 56.27 30.65 32.65 85.78 98.55 4 51 51.2 18.31 28.47 662 21.65 22.02 52.63 56.83 31 .53 33.78 84.86 99.61 5 50.8 50.8 18.64 28.09 659 20.81 21.33 50.75 56.09 25.97 29.12 80.67 99.68 Through31.16 33.15 83.12 99.68
[0231]
[0232] cut 51 51.1 18.34 28.67 665 21.68 22.01 52.5 56.73
[0233] EN 317 Water absorption and Dieken swelling (Biobinder without LCC)
[0234] Through
[0235]
[0236] cut 50.6 51.3 18.42 29.04 653 30.94 39.05 66.7 79.3 168 212 129 173 EN 319 tensile strength
[0237] Position Length Width Thickness Weight Specific Force Durability Tensile Strength mm mm mm g Weight N s N / mm 2 kg / m 3
[0238] Standard 0.32
[0239] 1 50 51 ,1 18.26 29.08 671 2105 21 ,3 0.58 2 51 ,3 50.1 18.12 29.38 679 2167 22.1 0.63 3 51 51 ,2 18.42 28.34 655 1964 18.4 0.51 4 50.4 51 18.31 28.47 662 2016 19.4 0.61 5 51 ,3 50.7 18.64 28.09 659 2007 18.6 0.69
[0240] Through
[0241]
[0242] cut 50.8 50.8 18.34 28.67 665 2051 19.96 0.60 APPLICATION EXAMPLE 4
[0243] Chipboard with UF+LCC
[0244] 12 mm single-layer particleboards were produced on a laboratory press using a UF resin plus the additive LCC according to this invention. The weight of the board was 720 kg / m³.
[0245] The glue was applied using a blender. The shavings were produced from fresh pine wood and provided to the laboratory. The glue application rate was 8% of the dry wood. The moisture content of the wood after drying before gluing was 2.2%. The moisture content of the shavings after gluing was 8.5%.
[0246] UF binder from the company Silekol No: S-137.
[0247] The UF + LCC binder mixture used had a solids content of 62%, of which 20% was the LCC additive. A hardener (ammonium sulfate) of 1.5% was added to the system. Adhesive quantity: 8%, 57.6 kg solids and 92.9 kg wet adhesive.
[0248] LCC with 59.3% solids content. (18.58 kg wet additive LCC).
[0249] Pressure factor = 8.0 see / mm
[0250] Pressing temperature = 200 °C
[0251] EN 320 flexural strength
[0252] Position Length Width Thickness Weight Specific Force Duration Bending Elasticity mm mm mm g Weight N s Strength Modulus kg / m 3 N / mm 2 N / mm 2 Standard 15 2050 1 370 51 .3 12.2 165.97 788 287 34.3 18.47 2605.11 2 370 50.2 12.7 172.91 740 276 32.5 16.8 2519.48 3 370 50.5 12.1 164.69 750 237 39.1 15.29 2214.85 4 370 50.2 12.4 168.56 761 249 31 .2 16.6 2320.73
[0253]
[0254] Average 50.5 12.35 168.03 760 262 34.27 16.79 2415.05 EN 317 Water Absorption and Dieken Swelling
[0255] Position Length Width Thickness Specific Thickness Weight Swelling Absorption mm mm mm weight Ge2h 24h 2h 24h 2h 24h 2h 24h g weight mm mm gg % % % % kg / m 3
[0256] 1 51 ,1 51 ,3 12.2 23.05 745 22.42 27.6 57.62 66.26 35.39 36.47 49.97 87.52 2 51 ,1 50.2 12.7 24.01 734 21.93 26.17 60.02 69.04 32.27 33.72 49.94 87.54 3 51 ,2 50.5 12.1 22.87 718 21.61 26.94 57.17 65.27 30.65 32.65 49.78 85.39 4 51 50.2 12.4 23.41 728 21.65 26.02 58.52 67.29 31 .53 33.78 49.76 86.44 5 50.8 50.8 12.3 23.69 734 20.81 25.33 59.22 68.09 25.97 29.12 47.67 87.12 Through31.16 33.15 49.42 86.80
[0257]
[0258] average 51 50.6 12.34 23.4 731 21.68 26.41 58.51 67.19
[0259] EN 317 Water absorption and Dieken swelling (UF without LCC)
[0260] Through
[0261]
[0262] cut 50.4 51 12.44 23.7 739 27.26 30.34 58.94 48.66 119 144 81.18 105.32EN 319 tensile strength
[0263] Position Length Width Thickness Weight Specific Force Durability Tensile Strength mm mm mm g Weight N s N / mm 2 kg / m 3
[0264] Standard 0.45
[0265] 1 51 51 ,3 12.2 23.05 745 1920 21 ,3 0.72 2 51 ,2 51 ,1 12.7 24.01 734 1867 20.1 0.68 3 51 51 ,4 12.1 22.87 718 1712 15.6 0.48 4 51 ,4 51 12.4 23.41 728 1831 19.8 0.56 5 51 50.3 12.3 23.69 734 1879 20.4 0.66
[0266] Through
[0267]
[0268] cut 51.1 51.2 16.47 23.4 731 1842 19.4 0.62 APPLICATION EXAMPLE 5
[0269] OSB (PMDI+ 30% LCC; use of LCC to reduce the cost of the approach.)
[0270] On a laboratory press, 18 mm thick, three-layer OSB panels were produced using a bio-based binder plus the additive LCC according to this invention. The panel weight was 640 kg / m³. The adhesive was applied using a blender. The flakes were made from fresh pine wood and provided to the laboratory.
[0271] The PMDI+ LCC order volume was 5% of the dry wood, of which 30% was LCC.
[0272] The wood moisture content after drying and before gluing was 3.5%. The moisture content of the flakes after gluing was 10%.
[0273] Glue quantity: total 5% for top and middle layers, of which 30% is LCC additive = 22.4 kg PMDI and 9.6 kg wet additive LCC.
[0274] LCC with 59.3% solids content.
[0275] Pressure factor = 8.0 see / mm
[0276] Pressing temperature = 230 °C
[0277] EN 320 flexural strength
[0278] Position Length Width Thickness Weight Specific Force Duration Bending Elasticity mm mm mm g Weight N s Strength Modulus kg / m 3 N / mm 2 N / mm 2 Norm 18 3500 1 370 51 .1 18.89 222.91 643 416 37.1 26.17 3901 .38 2 370 50.8 18.2 217.72 639 402 35.5 20.7 3879.37 3 370 51 18.58 220.6 641 411 40.1 25.22 3870.03 4 370 51 .2 18.5 225.54 654 448 42.2 27.1 4128.34
[0279]
[0280] Average 51.1 16.49 211.69 644 419 38.7 24.04 3944.78 EN 317 Water Absorption and Dieken Swelling
[0281] Position Length Width Thickness Specific Thickness Weight Swelling Absorption mm mm mm weight Ge2h 24h 2h 24h 2h 24h 2h 24h g weight mm mm gg % % % % kg / m 3
[0282] Standard 15
[0283] 1 51 ,1 51 ,2 18.89 30.95 643 22.42 22.6 53.29 57.44 18.6 19.64 72.18 85.58 2 51 ,1 51 ,1 18.2 30.23 639 21.93 22.17 53.19 57.04 20.49 21 ,81 75.95 88.68 3 51 ,2 51.1 18.58 30.63 641 21.61 21.94 52.65 56.27 16.30 18.08 71 ,89 83.17 4 51 51.2 18.5 31.32 654 21.65 22.02 52.63 56.83 17.02 19.02 68.03 81.14 5 50.8 50.8 18.45 30.19 648 20.81 21.33 50.75 56.09 12.79 15.6 68.10 85.78 Through 17.04 18.83 71.23 84.87
[0284]
[0285] cut 51 51.1 18.52 30.66 665 21.68 22.01 52.5 56.73EN 317 Water Absorption and Dieken Swelling (PMDI without LCC)
[0286] Through
[0287]
[0288] average 51.3 51 18.45 31.22 661 21.52 22.08 33.7 39.3 16.8 20 14.6 35.3
[0289] EN 319 Tensile strength
[0290] Position Length Width Thickness Weight Specific Force Durability Tensile Strength mm mm mm g Weight N s N / mm 2 kg / m 3
[0291] Standard 0.32
[0292] 1 51 51 ,3 18.89 30.95 643 2070 20.3 0.61 2 51 ,2 51 ,1 18.2 30.23 639 2111 20.7 0.57 3 51 51 ,4 18.58 30.63 641 1988 18.4 0.62 4 51 ,4 51 18.5 30.32 654 2154 22.3 0.68 5 51 50.3 18.45 30.19 648 2105 22.6 0.65
[0293] Through
[0294]
[0295] average 51.1 51.2 18.52 30.66 665 2085 20.8 0.63
[0296] APPLICATION EXAMPLE 6
[0297] Fiberboard HDF (biobinder + LCC)
[0298] _On a laboratory press, 3 mm HDF boards were produced using a bio-binder plus the additive LCC according to this invention. The weight of the board was 820 kg / m³.
[0299] The glue was applied using a blender. The fibers were produced from fresh pine wood and provided to the laboratory.
[0300] The amount of glue applied was 11% of the dried wood.
[0301] The wood moisture content after drying and before gluing was 4.5%. The fiber moisture content after gluing was 11%.
[0302] The one-component binder mixture used had a solids content of 60%, of which 20% was additive LCC.
[0303] Glue quantity: 11%, 94.6 kg solid and 157.6 kg wet glue
[0304] LCC including polysorbate with 59.3% solids content (31.4 kg wet additive LCC).
[0305] The solid content of the binder includes all organic and inorganic components of the glue, including glycerin.
[0306] Pressure factor = 8.0 see / mm
[0307] Pressing temperature = 220 °C
[0308] EN 320 flexural strength
[0309] Position Length Width Thickness Weight Specific Force Duration Bending Elasticity mm mm mm g Weight N s Strength Modulus kg / m 3 N / mm 2 N / mm 2Norm 27 2700 1 150 51 .1 3.08 17.77 795 81 55.1 74.14 4215 2 150 50.2 3.12 17.95 822 76 53.5 72.7 4976 3 150 51 3.24 19.23 816 95 50.3 93.39 5234 4 150 51 .7 3.09 18.31 835 101 59.2 95.6 5322
[0310]
[0311] Average 51.1 3.13 18.31 817 88 54.5 83.95 4936EN 317 Water Absorption and Dieken Swelling
[0312] Position Length Width Thickness Specific Thickness Weight Swelling Absorption mm mm mm weight Ge2h 24h 2h 24h 2h 24h 2h 24h g weight mm mm gg % % % % kg / m 3
[0313] Standard 30
[0314] 1 51 ,1 51 ,2 3.08 6.77 795 3.42 4.02 9.46 10.45 11.02 30.07 39.97 64.78 2 51 ,1 51 ,1 3.12 6.84 822 3.58 3.98 9.23 10.74 14.7 27.56 34.94 57.01 3 51 ,2 51 ,1 3.24 6.97 816 3.81 4.03 10.65 11 ,27 17.76 24.38 52.79 61 ,69 4 51 51.2 3.09 6.82 832 3.5 4.01 9.73 10.84 13.33 29.77 42.66 58.94 5 50.8 50.8 3.1 6.72 806 3.71 3.87 9.84 10.92 19.60 24.83 46.42 62.50 Divided by 1 43.35 60.98
[0315]
[0316] cut 51 51.1 3.12 6.82 814 3.60 3.98 9.78 10.84 5.88 27.32
[0317] EN 317 Water absorption and Dieken swelling (Biobinder without LCC)
[0318] Through
[0319]
[0320] cut 50.6 50.4 3.21 7.02 819 5.58 6.75 11.34 13.21 173 210 161 188 EN 319 tensile strength
[0321] Position Length Width Thickness Weight Specific Force Durability Tensile Strength mm mm mm g Weight N s N / mm 2 kg / m 3
[0322] Norm 0.7 1 51 51 ,3 3.08 6.77 795 2016 6.6 0.78 2 51 ,2 51 ,1 3.12 6.84 822 2235 7.1 1.18 3 51 51 ,4 3.24 6.97 816 1674 5.8 0.86 4 51 ,4 51 3.09 6.82 832 2286 6.7 1.32 5 51 50.3 3.1 6.72 806 2676 8.2 0.92 By
[0323]
[0324] cut 51.1 51.2 3.12 6.82 814 2177 6.88 1.01 Cooking test according to EN 1087-1.
[0325] 16 mm MDF fiberboard with a weight of 720 kg / m³
[0326] Swelling, cooking + cross-draft
[0327] 2 h 24h 2 h 6 h
[0328] Standard MDF H 8% > 0.1 N / mm2
[0329] UF 122 184
[0330] MUF (15% melamine) 2.3 8.66
[0331] UF + LCC 31 36
[0332] Protein binder 173 210
[0333] Protein binder 3.75 9.5 0.18 0.07
[0334] + LLC
[0335] Protein binder +LCC 2.91 8.13 0.21 0.09
[0336] + Aquaveg 50A-1301 from
[0337] EMULCO (Hydrowax)
[0338] Unless otherwise stated, all figures in % refer to weight %
Claims
Patent claims:
1. Hydrophobing agent for cellulose-containing materials containing a. Phenolic polymers; b. Organic acid; c. Alkali silicates; d. Alkali hydroxide; e. Water.
2. A hydrophobizing agent for cellulose-containing materials according to claim 1, wherein this hydrophobizing agent does not contain formaldehyde.
3. Hydrophobizing agent for cellulose-containing materials according to claim 1 or 2, further comprising a metal salt, in particular a copper salt.
4. Hydrophobizing agent for cellulose-containing materials according to one of the preceding claims, further comprising organosilane.
5. Hydrophobizing agent for cellulose-containing materials according to one of the preceding claims further comprising a surfactant, in particular a non-ionic surfactant, such as polysorbate.
6. Hydrophobing agent for cellulose-containing materials according to any of the preceding claims, comprising a. Phenolic biopolymers in an amount of 5 to 50 wt.%; b. Organic acid in an amount of 1.5 to 4.0 wt.%; c. Alkali silicates in an amount of 2.0 to 6.0 wt.%; d. Alkali hydroxide in an amount of 0.5 to 5.0 wt.%; e. Possibly metal salt in an amount of 0.3 to 3% by weight; f. If necessary, organosilane in an amount of 1.0 to 8.0 wt.%; g. If necessary, surfactant in an amount of 2.5 to 8.0 wt.%; h. Water to 100 wt.%.
7. A water-repellent agent for cellulose-containing materials according to any one of the preceding claims, wherein the phenolic biopolymers are selected from the group of lignins, in particular organosolv or Kraft lignins.
8. A water-repellent agent for cellulose-containing materials according to any one of the preceding claims, wherein the organic acid is selected from an organic acid having a pH value < 3 when added to the water-repellent agent, in particular a carboxylic acid including citric acid, lactic acid, picric acid, acetic acid, ascorbic acid and mixtures thereof.
9. Hydrophobizing agent for cellulose-containing materials according to any of the preceding claims, wherein the alkali hydroxides are selected from sodium hydroxide or potassium hydroxide.
10. Hydrophobizing agent for cellulose-containing materials according to one of the preceding claims, wherein the alkali silicates are water glass, in particular potassium or sodium water glass.
11. Binder composition for cellulose-containing materials comprising or consisting of a hydrophobizing agent according to any one of claims 1 to 10.
12. Binder composition for cellulose-containing materials according to claim 11, wherein the base binder is selected from UF(urea-formaldehyde) / MUF(melamine-urea-formaldehyde), PMIIF (phenol-melamine-urea-formaldehyde), protein binder or isocyanate-based binders.
13. Binder composition for cellulose-containing materials according to claim 12, wherein the base binder is a plant-based protein binder.
14. Binder composition for cellulose-containing materials according to one of claims 11 to 13, wherein the binder may comprise further additives, in particular at least one from the group consisting of hydrowax, fungicides, flame retardants, perfumes, colorants, fillers and mixtures thereof.
15. Composite product obtainable by bonding a cellulose-containing starting material with a binder according to any one of claims 11 to 14 and forming it into a product, in particular wherein the product is a sheet or a molded part.
16. Composite product according to claim 15, characterized in that the cellulose-containing starting material is wood or annual plants, such as wood fibers, wood chips, wood dust or wood flour, wood chips, strands, veneers or material processed according to the scrimber process or recycled material.
17. Method for producing a composite material product from cellulose-containing material and a binder according to any one of claims 11 to 14, comprising a heat treatment under pressure.
18. Method for producing a composite product according to claim 17, wherein this is a composite product according to any one of claims 15 to 16.
19. Method for producing a composite material product according to claim 17 or 18, wherein the heat treatment is carried out under pressure at a temperature in the range of 100 to 250 degrees Celsius, in particular at a pressure of 1 to 250 bar, preferably 10 to 80 bar.
20. Use of a hydrophobizing agent according to any one of claims 1 to 10 or a binder composition according to any one of claims 11 to 14 for the production of cellulose-containing composite products.