Aqueous polyurethane-urea dispersion and applications thereof
The aqueous polyurethane-urea dispersion addresses nozzle clogging and color fastness issues in inkjet printing on synthetic polyurethane leather by using a specific formulation with polyisocyanate and polyester diol, ensuring excellent dry and wet color fastness.
Patent Information
- Application Number
- PCT/EP2026/063374
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2026-04-08
- Filing Date
- 2026-05-08
- Publication Date
- 2026-11-12
AI Technical Summary
Existing inkjet printing technologies face challenges with pigments detaching from synthetic polyurethane leather due to low surface energy and limited absorbency, leading to poor dry and wet color fastness, and nozzle clogging from non-jettable binders.
An aqueous polyurethane-urea dispersion is developed with specific components and properties, including polyisocyanate, polyester diol, and non-ionic hydrophilic agents, ensuring jettable and filterable ink compositions that provide excellent dry and wet color fastness on artificial leather.
The dispersion achieves jettable and filterable ink compositions with excellent dry and very good wet color fastness on synthetic polyurethane leather, reducing nozzle clogging and enhancing print durability.
Smart Images

Figure IMGF000005_0001 
Figure IMGF000005_0002 
Figure IMGF000006_0001
Abstract
Description
[0001] 2025PF30011- Foreign Countries
[0002] AQUEOUS POLYURETHANE-UREA DISPERSION AND APPLICATIONS THEREOF
[0003] TECHNICAL FIELD
[0004] The invention belongs to the technical field of polyurethanes. In particular, the invention relates to an aqueous polyurethane-urea dispersion and applications thereof.
[0005] BACKGROUND ART
[0006] Traditional methods for printing images, such as text, pictures, or designs, onto fabrics -including woven and non-woven substrates- include screen printing, roller printing, and similar techniques. In recent years, inkjet textile printing has gained significant attention. This approach relies on digital image processing and enables direct printing without the need for plates or screens. As a result, plate-making is eliminated, only the required amount of ink is used, waste liquid generation is reduced, and the method is more environmentally favorable and better suited for flexible and small-scale production.
[0007] Inkjet textile printing employs inks containing either pigments or dyes. Dye-based inks are limited to specific textile materials, whereas pigment-based inks are applicable to a broader range of substrates. Additional advantages of pigment-based systems include high lightfastness and the absence of post-print removal steps for colorants. However, pigments do not inherently bind to fibers and are therefore prone to detachment after printing. Textile materials used in garments and related products are subject to repeated washing and mechanical friction during use, which imposes stringent requirements on properties such as dry and wet color fastness.
[0008] To secure pigments to the fibers, a binder component is incorporated into the ink, and this binder largely governs the resulting color fastness. However, the fine nozzles of inkj et print heads, typically only a few micrometers in diameter, are susceptible to clogging Accordingly, the binder must exhibit appropriate filtration behavior to minimize the risk of nozzle blockage. In addition, inkjet ink compositions must be jettable, a requirement that is influenced by multiple formulation parameters, including the properties of the binder. While binder jettability plays a role in ensuring reliable ink ejection, it is not the only factor governing it. Nevertheless, a non-jettable binder can2025PF30011- Foreign Countries
[0009] adversely affect ink flow and may result in nozzle clogging, which is highly undesirable in inkjet printing applications.
[0010] Synthetic polyurethane (PU) leather, a principal class of artificial leather, is a widely used engineered material. However, its low surface energy and limited absorbency complicate printing, often resulting in poor dry color fastness, characterized by abrasion-induced pigment loss, and poor wet color fastness, associated with water-induced swelling, migration, or softening.
[0011] Aqueous polyurethane or polyurethane-urea dispersions are considered one of the suitable binder materials for textile inkjet inks due to their strong cohesion and effective adsorption of pigment molecules. For example, EP 2641943 Al, US 2010 / 0214352 Al, and JP 2015163678 A all disclose the applications of aqueous polyurethane dispersions in inkjet inks. EP 2028205 Al disclosed polyurethane dispersions based on polycarbonate polyols suitable for use in personal care products. The purpose of EP 2028205 Al was to provide a polymer composition which would improve adhesion to hair and also demonstrate excellent curl and style retention, natural feel and look.
[0012] Therefore, there remains a need in the art for an aqueous polyurethane-urea dispersion which is (i) jettable, has (ii) excellent filterability, and (iii) prints of ink compositions containing said aqueous polyurethane-urea dispersion, on artificial leather, have excellent dry color fastness and at least very good, preferably excellent wet color fastness.
[0013] SUMMARY OF THE INVENTION
[0014] One objective of the invention is to provide an aqueous polyurethane-urea dispersion which is (i) jettable, has (ii) excellent filterability, and (iii) prints of ink compositions containing said aqueous polyurethane-urea dispersion, on artificial leather, have excellent dry color fastness and at least very good, preferably excellent wet color fastness.
[0015] According to a first aspect of the invention, there is provided an aqueous polyurethane-urea dispersion as disclosed in the specification. It has been surprisingly found that the aqueous polyurethane-urea dispersion of the invention, is (i) jettable, has (ii) excellent filterability, and (iii) prints of ink compositions containing said aqueous polyurethane-urea dispersion, on artificial leather, have excellent dry color fastness and at least very good, preferably excellent wet color fastness.2025PF30011- Foreign Countries
[0016] According to a second aspect of the invention, there is provided a coating, an adhesive, a sealant or an ink prepared using the aqueous polyurethane-urea dispersion of the invention.
[0017] According to a third aspect of the invention, there is provided an article comprising a substrate coated, bonded, sealed or printed with the coating, adhesive, sealant or ink of the invention.
[0018] According to a fourth aspect of the invention, there is provided a use of the aqueous polyurethane-urea dispersion of the invention as discloses in the specification, for the preparation of coated products, bonded products, sealed products, or printed products.
[0019] DETAILED DESCRIPTION OF THE INVENTION
[0020] The invention is as defined in the claims and as disclosed in the specification. Within the scope of the claims, certain preferments, embodiments and aspects of the invention are described for the purpose of illustration rather than limitation.
[0021] The description for various features in the specification may be combined where there is no contradiction, all of which fall within the scope of the claims.
[0022] The term ‘polyurethane-urea’ as used herein refers to a polymer comprising urethane linkages (-NH-C(=O)-O-) connecting repeating structural units to one another and urea linkages (-NH-C(=O)-NH-) connecting repeating structural units to one another. The polyurethane-urea may optionally further comprise thiourethane linkages (-NH-C(=O)-S-) connecting repeating structural units to one another. Said urethane linkages, said urea linkages and, where present, said thiourethane linkages may independently connect the same or different repeating structural units to one another.
[0023] The term ‘aqueous polyurethane-urea dispersion’ as used in the specification means an aqueous dispersion in which the dispersed polymer is a polyurethane-urea as the latter is defined herein.
[0024] As used herein, the expressions ‘jettable’, ‘having jetting ability’ and ‘having jettability’ are used interchangeably. An aqueous polyurethane-urea dispersion that is classified as jettable is considered as potentially suitable for inkjet printing. An aqueous polyurethane-urea dispersion that forms and ejects droplets from an inkjet nozzle without clogging the nozzle is2025PF30011- Foreign Countries
[0025] classified as jettable. An aqueous polyurethane-urea dispersion that does not form and eject droplets from the inkjet nozzle and / or clogs the inkjet nozzle is classified as not jettable. The term ‘artificial leather’ as used herein means synthetic polyurethane (PU) leather. All percentages in the specification are weight percentages, unless otherwise specified. The analysis and measurements as described in the specification are all performed at 23 ± 2°C (herein ambient temperature), unless otherwise specified.
[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by a person of ordinary skill in the field the invention belongs to. When the definition of a term in the present description conflicts with the meaning as commonly understood by a person of ordinary skill in the field the invention belongs to, the definition described herein shall prevail.
[0027] Unless expressly stated otherwise, all parameters, properties, and values referred to herein are determined in accordance with the methods and conditions described in the present specification; in the absence of an explicit description, such parameters, properties, and values are determined using methods customary in the art.
[0028] The invention provides an aqueous polyurethane-urea dispersion comprising
[0029] (i) a polyurethane-urea, wherein the polyurethane-urea is obtained by reacting at least the following components a) to f), preferably obtained by reacting only the following components a) to f):
[0030] a) at least one polyisocyanate, preferably wherein the amount of component a) is 15-30 wt.% of the polyurethane-urea,
[0031] b) at least one polyester diol, preferably wherein the at least one polyester diol has a numberaverage molecular weight, determined as described in the specification, of 800-4000 g / mol, more preferably 1000-3000 g / mol, preferably wherein the at least one polyester diol is an aromatic polyester diol, wherein the amount of component b) is 60-80 wt.%, preferably 63-80 wt.%, more preferably 63 -75 wt.% of the polyurethane-urea,
[0032] c) 2,2-bis(hydroxymethyl) butyric acid in an amount of 1.6-4.8 wt.%, preferably 1.6-4.7 wt.% of the polyurethane-urea,2025PF30011- Foreign Countries
[0033] d) at least one non-ionic hydrophilic agent selected from compounds represented by Formula I, Formula II, Formula III, Formula IV, Formula V, and combinations thereof
[0034]
[0035] Formula I
[0036] wherein
[0037] g is an integer from 0 to 70, preferably from 0 to 35, more preferably from 0 to 10,
[0038] x is an integer from 10 to 70, preferably from 10 to 55, more preferably from 15 to 50, with the proviso that x is not less than g when g is greater than 10,
[0039] Ri is a Ci-Cis, preferably C1-C14, more preferably C1-C12, even more preferably C1-C10, most preferably Ci-Cs, especially Ci-Ce hydrocarbon group, or a group consisting of 2 to 18 carbon atoms, preferably 2 to 14 carbon atoms, more preferably 2 to 12 carbon atoms, even more preferably 2 to 10 carbon atoms, most preferably 2 to 8 carbon atoms, especially 2 to 6 carbon atoms, hydrogen atoms, and 1 to 8 oxygen atoms, preferably 1 to 6 oxygen atoms, more preferably 1 to 5 oxygen atoms, even more preferably 1 to 4 oxygen atoms, most preferably 1 to 3 oxygen atoms, especially 1 to 2 oxygen atoms, more especially 1 oxygen atom, wherein each oxygen atom present forms part only of ether linkages other than oxirane groups, and wherein Ri is covalently bonded to the oxygen atom of Formula I via a carbon atom of Ri via a carbon-oxygen single bond,
[0040] HO
[0041]
[0042] wherein
[0043] n is an integer from 0 to 70, preferably from 0 to 35, more preferably from 0 to 10,
[0044] m is an integer from 10 to 70, preferably from 10 to 55, more preferably from 15 to 50, with the proviso that m is not less than n when n is greater than 10,2025PF30011- Foreign Countries
[0045] R2 is a C1-C18, preferably C1-C14, more preferably C1-C12, even more preferably C1-C10, most preferably Ci-Cs, especially Ci-Ce hydrocarbon group, or a group consisting of 2 to 18 carbon atoms, preferably 2 to 14 carbon atoms, more preferably 2 to 12 carbon atoms, even more preferably 2 to 10 carbon atoms, most preferably 2 to 8 carbon atoms, especially 2 to 6 carbon atoms, hydrogen atoms, and 1 to 8 heteroatoms, preferably 1 to 6 heteroatoms, more preferably 1 to 5 heteroatoms, even more preferably 1 to 4 heteroatoms, most preferably 1 to 3 heteroatoms, especially 1 to 2 heteroatoms selected from oxygen and nitrogen, wherein the number of nitrogen atoms is 1 and wherein each oxygen atom forms part only of ether linkages other than oxirane groups and the nitrogen atom either forms part of a -C=N-C- linkage or it is directly covalently bonded only to carbon atoms via carbon-nitrogen single bonds, and wherein R2 is covalently bonded to the nitrogen atom of Formula II via a carbon atom of R2 via a carbon-nitrogen single bond,
[0046] R3 is a C1-C18, preferably C1-C14, more preferably C1-C12, even more preferably C1-C10, most preferably Ci-Cs, especially Ci-Ce hydrocarbon group, or a group consisting of 2 to 18 carbon atoms, preferably 2 to 14 carbon atoms, more preferably 2 to 12 carbon atoms, even more preferably 2 to 10 carbon atoms, most preferably 2 to 8 carbon atoms, especially 2 to 6 carbon atoms, hydrogen atoms, and 1 to 8 heteroatoms, preferably 1 to 6 heteroatoms, more preferably 1 to 5 heteroatoms, even more preferably 1 to 4 heteroatoms, most preferably 1 to 3 heteroatoms, especially 1 to 2 heteroatoms selected from oxygen and nitrogen, wherein the number of nitrogen atoms is 1, and wherein each oxygen atom forms part only of ether linkages other than oxirane groups and the nitrogen atom either forms part of a -C=N-C- linkage or it is directly covalently bonded only to carbon atoms via carbon-nitrogen single bonds, and wherein R3 is covalently bonded to the nitrogen atom of Formula II via a carbon atom of R3 via a carbon-nitrogen single bond,
[0047]
[0048] Formula III2025PF30011- Foreign Countries
[0049] wherein
[0050] n’ is an integer from 0 to 70, preferably from 0 to 35, more preferably from 0 to 10,
[0051] m’ is an integer from 10 to 70, preferably from 10 to 55, more preferably from 15 to 50, with the proviso that m’ is not less than n’ when n’ is greater than 10,
[0052] R4 is a C3-C10, preferably C3-C8, more preferably C3-C6, even more preferably C3-C5, most preferably C4-C5 hydrocarbon group, or a group consisting of 3 to 10 carbon atoms, preferably 3 to 8 carbon atoms, more preferably 3 to 6 carbon atoms, even more preferably 3 to 5 carbon atoms, most preferably 4 to 5 carbon atoms, hydrogen atoms, and 1 or 2 heteroatoms selected from oxygen and nitrogen, and wherein each oxygen atom forms part only of ether linkages other than oxirane groups and each nitrogen atom forms part either of a -C=N-C- linkage, or it is directly covalently bonded only to carbon atoms via carbon-nitrogen single bonds, and wherein R4 is covalently bonded to the nitrogen atom of Formula III via two distinct carbon atoms of R4, each via a carbon-nitrogen single bond,
[0053] HO
[0054] HO
[0055]
[0056] Formula IV
[0057] wherein
[0058] y is an integer from 0 to 70, preferably from 0 to 35, more preferably from 0 to 10,
[0059] z is an integer from 10 to 70, preferably from 10 to 55, more preferably from 10 to 50, with the proviso that z is not less than y when y is greater than 10,
[0060] Rs is a C1-C18, preferably C1-C14, more preferably C1-C12, even more preferably C1-C10, most preferably Ci-Cs, especially Ci-Ce, more especially C1-C4, even more especially C1-C3, most especially C1-C2 hydrocarbon group particularly a methyl group, or a group consisting of 2 to 18 carbon atoms, preferably 2 to 14 carbon atoms, more preferably 2 to 12 carbon atoms, even more preferably 2 to 10 carbon atoms, most preferably 2 to 8 carbon atoms, especially 2 to 6 carbon atoms, hydrogen atoms, and 1 to 8 oxygen atoms, preferably 1 to 6 oxygen atoms, more preferably 1 to 5 oxygen atoms, even more preferably 1 to 4 oxygen atoms, most preferably 1 to 3 oxygen atoms, especially 1 to 2 oxygen atoms, more especially 1 oxygen atom, wherein each oxygen2025PF30011- Foreign Countries
[0061] atom forms part only of ether linkages other than oxirane groups, and wherein R5 is covalently bonded to the oxygen atom of Formula IV via a carbon atom of R5, via a carbon-oxygen single bond,
[0062]
[0063] Formula V
[0064] wherein
[0065] p is an integer from 0 to 70, preferably from 0 to 35, more preferably from 0 to 10,
[0066] q is an integer from 10 to 70, preferably from 10 to 55, more preferably from 10 to 50, with the proviso that q is not less than p when p is greater than 10,
[0067] and wherein the amount of component d) is 1-5 wt.% of the polyurethane-urea,
[0068] e) at least one chain extender selected from hydrazine, primary amines having a molar mass of 32-500 g / mol optionally containing at most 2 hydroxyl groups, preferably at most 1 hydroxyl groups, more preferably containing no hydroxyl groups, and secondary amines having a molar mass of 32-500 g / mol optionally containing at most 2 hydroxyl groups, preferably at most 1 hydroxyl groups, more preferably containing no hydroxyl groups, and combinations thereof, preferably the primary amines and / or the secondary amines are aliphatic, preferably wherein the amount of component e) is 0.1-3.0 wt.%, more preferably 0.1-2.5 wt.% of the polyurethane-urea, f) at least one neutralizing agent selected from alkali metal hydroxides, ammonia, tertiary amines optionally containing at most three hydroxyl groups, and combinations thereof, preferably the neutralizing agent is selected from alkali metal hydroxides, ammonia, tertiary amines having a molar mass of at most 400 g / mol, preferably at most 200 g / mol, optionally containing at most three hydroxyl groups, and combinations thereof, more preferably the neutralizing agent is selected from alkali metal hydroxides, ammonia, tertiary amines having a molar mass of at most 400 g / mol, preferably at most 200 g / mol, containing no hydroxyl groups, and combinations thereof, even more preferably the neutralizing agent is selected from tertiary amines having a molar mass of at most 400 g / mol, preferably at most 200 g / mol, containing no hydroxyl groups, and combinations thereof, preferably wherein the amount of component f) is 0.10-10.0 wt.%,2025PF30011- Foreign Countries
[0069] more preferably 0.15-9.0 wt.%, even more preferably 0.15-8.0 wt.%, most preferably 0.15-7.0 wt.% of the polyurethane-urea,
[0070] and
[0071] (ii) optionally an organic solvent.
[0072] Preferably, the aqueous polyurethane-urea dispersion of the invention is as disclosed herein, wherein the aqueous polyurethane-urea dispersion has a solid content, determined as described in the specification, of 30-65 wt.%, preferably 30-50 wt.%, more preferably 30-40 wt.%, and most preferably 30-36 wt.%.
[0073] Preferably, the aqueous polyurethane-urea dispersion of the invention is as disclosed herein, wherein the aqueous polyurethane-urea dispersion has a viscosity, determined as described in the specification, of 1-1000 mPa.s, preferably 1-500 mPa.s, more preferably 1-300 mPa.s.
[0074] Preferably, the aqueous polyurethane-urea dispersion of the invention is as disclosed herein, wherein the aqueous polyurethane-urea dispersion has z-average diameter, determined as described in the specification, of 30-100 nm, more preferably 30-70 nm.
[0075] Preferably, the aqueous polyurethane-urea dispersion of the invention is as disclosed herein, wherein the aqueous polyurethane-urea dispersion has a pH, determined as described in the specification, of 4-10.
[0076] Preferably, the aqueous polyurethane-urea dispersion of the invention is as disclosed herein, wherein the aqueous polyurethane-urea dispersion has a solid content of 30-36 wt.%, a z-average diameter of 30-100 nm and a viscosity of 1-300 mPa- s.
[0077] Preferably, the aqueous polyurethane-urea dispersion of the invention is as disclosed herein, wherein the aqueous polyurethane-urea dispersion has at least one of the following characteristics:
[0078] a viscosity of 1-1000 mPa- s;
[0079] a solid content of 30-65 wt.%;
[0080] a z-average diameter of 30- 100 nm;
[0081] pH value of 4-10.
[0082] Preferably, the aqueous polyurethane-urea dispersion of the invention is as disclosed herein, wherein the at least one polyisocyanate is selected from diisocyanates of formula Y(NCO)2, wherein Y is a divalent aliphatic hydrocarbon group containing 4-12 carbon atoms, a divalent cycloaliphatic hydrocarbon group containing 6-15 carbon atoms, a divalent aromatic hydrocarbon group containing 6-15 carbon atoms, or a divalent araliphatic hydrocarbon group2025PF30011- Foreign Countries
[0083] containing 7-15 carbon atoms, preferably Y is a divalent aliphatic hydrocarbon group containing 4-12 carbon atoms or a divalent cycloaliphatic hydrocarbon group containing 6-15 carbon atoms. More preferably the at least one polyisocyanate is selected from tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, dodecamethylene diisocyanate, 1,4-cyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, dicyclohexylpropane diisocyanate, and l,3-bis(isocyanatomethyl)cyclohexane, 1,4-bis(isocyanatomethyl)cyclohexane, and combinations thereof, more preferably isophorone diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, and combinations thereof, even more preferably isophorone diisocyanate, dicyclohexylmethane diisocyanate, and combinations thereof.
[0084] The at least one polyester diol refers to a polyester polyol having, an average hydroxyl functionality of two. The at least one polyester diol, may be linear or branched. Suitable polyester diols, especially linear polyester diols or slightly branched polyester diols, can be produced in a known manner from aliphatic, cycloaliphatic or aromatic dicarboxylic acids, such as succinic acid, methylsuccinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, terephthalic acid, isophthalic acid, phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, cyclohexanedicarboxylic acid, maleic acid, fumaric acid, malonic acid or anhydrides, such as phthalic anhydride, succinic anhydride or combinations thereof, by reacting with aliphatic, cycloaliphatic or aromatic diols such as ethylene glycol, di ethylene glycol, tri ethylene glycol, 1,2-propanediol, 1,3 -propanediol, 1,4-butanediol, 1,3 -butanediol, 2,3 -butanediol, 1,5 -pentanediol, 3-methyl-l,5-pentanediol, 1,6-hexanediol, 2,2-dimethyl-l,3-propanediol, dihydroxy cyclohexane l,4-bis(hydroxymethyl)cyclohexane, 1,8-octanediol, 1,10-decanediol, 1,12-dodecanediol, or combinations thereof. Hydroxy carboxylic acids are also suitable to be used as co-reactants in the preparation of polyester diols with terminal hydroxyl groups. Examples of hydroxycarboxylic acids include hydroxyhexanoic acid, hydroxybutyric acid, hydroxy decanoic acid, hydroxystearic acid, and the like. Polyester diols can also be homopolymers or copolymers of lactones, most preferably obtained by adding lactones or lactone mixtures (such as butyrolactone, s-caprolactone, methyl-8-caprolactone, or their combinations) to suitable bifunctional and / or trifunctional starting molecules, such as the low-molar-mass diols mentioned above as forming components of polyester diols. The corresponding polyester diols of 8-caprolactone are preferred. Preferably the polyester diol is based on a diol component selected from butanediol, neopentyl glycol, hexanediol, ethylene glycol, and diethylene glycol, and combinations thereof, and a diacid2025PF30011- Foreign Countries
[0085] component selected from adipic acid, phthalic acid, and isophthalic acid, and combinations thereof; more preferably, the polyester diol is based on a diol component selected from butanediol, neopentyl glycol, and hexanediol, and combinations thereof, and a diacid component selected from adipic acid and phthalic acid, and combinations thereof.
[0086] Preferably, the aqueous polyurethane-urea dispersion of the invention is as disclosed herein, wherein the at least one polyester diol is based on a diol component selected from butanediol, neopentyl glycol, hexanediol, ethylene glycol, and diethylene glycol, and combinations thereof, and a diacid component selected from adipic acid, phthalic acid, and isophthalic acid, and combinations thereof; more preferably, the at least one polyester diol is based on a diol component selected from butanediol, neopentyl glycol, and hexanediol, and combinations thereof, and a diacid component selected from adipic acid and phthalic acid, and combinations thereof.
[0087] 2,2-bis (hydroxymethyl) butyric acid is used as a (latent) ionic hydrophilic compound. The compounds of Formulae I, II, III, IV and V can be obtained by alkoxylation of suitable starting molecules in a known manner. Ethylene oxide and propylene oxide can be used in any sequence for alkoxylation reactions or can be used in the form of a mixture.
[0088] Preferably, the aqueous polyurethane-urea dispersion of the invention is as disclosed herein, wherein the at least one non-ionic hydrophilic agent is selected from compounds represented by Formula I, Formula II, Formula III, Formula IV, Formula V, and combinations thereof, more preferably the at least one non-ionic hydrophilic agent is selected from compounds represented by Formula I, Formula II, Formula III, Formula IV, and combinations thereof, even more preferably the at least one non-ionic hydrophilic agent is selected from compounds represented by Formula I, Formula II, Formula IV, and combinations thereof, most preferably the at least one non-ionic hydrophilic agent is selected from compounds represented by Formula I, Formula IV, and combinations thereof, especially the at least one non-ionic hydrophilic agent is selected from compounds represented by Formula I, and combinations thereof,
[0089] Preferably, the aqueous polyurethane-urea dispersion of the invention is as disclosed herein, wherein the at least one non-ionic hydrophilic agent is selected from compounds represented by Formula I, Formula II, Formula III, Formula IV, Formula V, and combinations thereof, wherein, for compounds represented by at least one of the Formulae I, II, III, IV or V, for the respective one of Formulae I, II, III, IV or V by which those compounds are represented, the corresponding ratio2025PF30011- Foreign Countries
[0090] x / (x+g) for compounds of Formula I,
[0091] m / (m+n) for compounds of Formula II,
[0092] m' / (m'+n') for compounds of Formula III,
[0093] z / (z+y) for compounds of Formula IV, and
[0094] q / (q+p) for compounds of Formula V
[0095] is greater than 0.5, preferably greater than 0.6, more preferably greater than 0.7, most preferably greater than 0.8.
[0096] Preferably, the aqueous polyurethane-urea dispersion of the invention is as disclosed herein, wherein the at least one non-ionic hydrophilic agent is selected from compounds represented by Formula I, Formula II, Formula III, Formula IV, Formula V, and combinations thereof, wherein, for each of said compounds, for the respective one of Formulae I, II, III, IV or V by which that compound is represented, each of the corresponding ratios
[0097] x / (x+g) for compounds of Formula I,
[0098] m / (m+n) for compounds of Formula II,
[0099] m' / (m'+n') for compounds of Formula III,
[0100] z / (z+y) for compounds of Formula IV, and
[0101] q / (q+p) for compounds of Formula V
[0102] is greater than 0.5, preferably wherein each of said ratios is greater than 0.6, more preferably wherein each of said ratios is greater than 0.7, most preferably wherein each of said ratios is greater than 0.8.
[0103] Examples, representative of compounds of Formula I, include but are not limited to Polyether LB 25 (available from Covestro) and MPEG 750 (supplied by Dow). Examples, representative of compounds of Formula IV, include but are not limited to Ymer™ N120 and Ymer™ N180 (each one supplied by Perstorp (Shanghai) Chemical Trading Co, Ltd.).
[0104] Preferably, the aqueous polyurethane-urea dispersion of the invention is as disclosed herein, wherein the chain extender is selected from hydrazine, ethylenediamine, isophorone diamine, diethylenetriamine, ethanolamine, N-methylethanolamine, diethanolamine, diisopropanolamine, 1 ,3 -diamino-2 -propanol, N-(2-hydroxyethyl)-ethylenediamine, N,N-bis(2 -hydroxy ethyl)-ethylenediamine, and 2-propanol amine, preferably selected from isophorone diamine and ethylenediamine.2025PF30011- Foreign Countries
[0105] Preferably, the aqueous polyurethane-urea dispersion of the invention is as disclosed herein, wherein the neutralizing agent is selected from triethylamine, triethanolamine, N,N-diisopropylethylamine, and dimethylethanolamine, preferably triethylamine and dimethyl ethanolamine.
[0106] The aqueous polyurethane-urea dispersion of the invention optionally comprises an organic solvent. The organic solvent is preferably an organic solvent that is miscible with water but inert to isocyanate groups, more preferably the organic solvent is selected from acetone, methyl ethyl ketone, propylene glycol dimethyl ether, other ethers without hydroxyl functional group, and esters without hydroxyl functional groups, and combinations thereof, even more preferably the organic solvent is selected from acetone, butanone and combinations thereof. The organic solvents preferably do not contain pyrrolidone compounds. Preferably, the aqueous polyurethane-urea dispersion of the invention is as disclosed herein, wherein the amount of the organic solvent, if present, is less than 1.0 wt.%, preferably less than 0.8 wt.%, more preferably less than 0.6 wt.%, more preferably less than 0.4 wt.%, even more preferably less than 0.2 wt.%, most preferably less than 0.1 wt.% relative to the total weight of the aqueous polyurethane-urea dispersion; especially, the aqueous polyurethane-urea dispersion of the invention is as disclosed herein, wherein the aqueous polyurethane-urea dispersion is free of any organic solvent.
[0107] The aqueous polyurethane-urea dispersion of the invention may also optionally comprise one or more additional ingredients typically added to aqueous polyurethane-urea dispersions, such as preservatives, external emulsifiers, etc. The amounts of these additional components can be adjusted by a person of ordinary skill in the art as needed to ensure that the aqueous polyurethane-urea dispersion of the invention is not adversely affected. Preferably, the total amount of additional ingredients is at most 10 wt.% of the solid content of the aqueous polyurethane-urea dispersion.
[0108] The aqueous polyurethane-urea dispersion of the invention may be suitably used in ink compositions including inkjet ink compositions. For example, the aqueous polyurethane-urea dispersion of the invention may be suitably used in ink compositions for screen printing, and for inkjet printing.
[0109] The aqueous polyurethane-urea dispersion of the invention may be prepared using conventional methods known in the art, such as emulsifier / shear force method, acetone process, prepolymer mixing method, melt emulsification method, ketimine method, and solid2025PF30011- Foreign Countries
[0110] spontaneous dispersion method or their derivatives. The melt emulsification method or acetone process is preferred, with the acetone process being most preferred. These methods are summarized in ‘Methoden der organischen Chemie’ (Houben-Weyl , Erweitenmgs-und zur4. Auflage, Volume E20, H Bartl and J. Falbe, Stuttgart, New York, Thieme 1987, pp.
[0111] 1671-1682). The components used for preparing the aqueous polyurethane-urea dispersion may be reacted in a conventional manner. Component a) and the components containing isocyanatereactive groups, including components b), c), d), and e), may be added in a single charge or in multiple portions, wherein any component added in a subsequent portion may be identical to or different from the corresponding component added previously. Usually, component e) is added after completion of the reaction of components a), b), c), and d). Water for dispersing the polymer may be added either after reaction of component e) or after reaction of components a), b), c), and d). Component f) may be added at any stage, provided that it is added before addition of the dispersion water.
[0112] A method for preparing an aqueous polyurethane-urea dispersion according to the invention comprises the following steps:
[0113] (A) reacting components, a), b), c), and d) at a temperature of 60-120 °C to form an NCO-terminated prepolymer, optionally in the presence of an organic solvent or followed by dissolution in an organic solvent;
[0114] (B) reacting the prepolymer with component e) at a temperature of 20-60 °C;
[0115] (C) adding component f);
[0116] (D) adding demineralized water to effect dispersion and emulsification;
[0117] (E) removing, if present, the organic solvent by distillation under reduced pressure to obtain the aqueous polyurethane-urea dispersion.
[0118] In the above-described method for preparing an aqueous polyurethane-urea dispersion according to the invention, component f) may alternatively be added during step (A), after step (A), or after step (D). Component e) may alternatively be added after step (D). Step (A) may also be carried out in the presence of an organic solvent. Step (E) may be conducted simultaneously with step (D).
[0119] Preferably, the aqueous polyurethane-urea dispersion is prepared by a method comprising the following steps:2025PF30011- Foreign Countries
[0120] (A) reacting components, a), b), c), and d) at a temperature of 60-120 °C to form an NCO-terminated prepolymer, followed by dissolution of the prepolymer in an organic solvent;
[0121] (B) adding component f);
[0122] (C) reacting the prepolymer solution with component e) at a temperature of 20-60 °C; (D) adding demineralized water to effect dispersion and emulsification;
[0123] (E) removing the organic solvent by distillation under reduced pressure to obtain the aqueous polyurethane-urea dispersion,
[0124] wherein step (E) may be conducted simultaneously with step (D).
[0125] If isolated, the NCO-terminated prepolymer is a solid or a liquid at ambient temperature. To accelerate the reaction rate of step (A), catalysts commonly used in prepolymer preparation may be employed, including triethylamine, l,4-diazabicyclo[2.2.2]octane, tin dioctate, and dibutyltin dilaurate, as well as other organometallic catalysts such as organic or inorganic salts of titanium, bismuth, zirconium, zinc, or lead. The catalyst may be introduced together with the components of step (A) or added subsequently. The extent of conversion in step (A) may be monitored by determining the NCO content of the reaction mixture. This can be achieved by analytical techniques such as spectroscopic methods (e.g., infrared or near-infrared spectroscopy), refractive index measurements, or chemical analysis (e.g., titration), performed on withdrawn samples. Organic solvents suitable for use in the preparation of the aqueous polyurethane-urea are preferably water-miscible and inert toward isocyanate groups. Preferred solvents include acetone, methyl ethyl ketone, propylene glycol dimethyl ether, other ethers lacking hydroxyl functionality, and esters lacking hydroxyl functionality; more preferably acetone and methyl ethyl ketone. Preferably, the organic solvent does not contain pyrrolidone compounds. When used, the organic solvent may be removed, for example by distillation, during or after preparation of the polyurethane-urea dispersion.
[0126] Coatings, adhesives, or inks
[0127] The invention also provides a coating, an adhesive, a sealant, or an ink prepared using the aqueous polyurethane-urea dispersion of the invention. The coating, adhesive or ink preferably further comprises appropriate additives. The additive is preferably one or more of the following: adhesion promoters, lubricants, emulsifiers, light stabilizers, antioxidants, fillers, anti-settling agents, defoamers, wetting agents, rheology modifiers, anti-static agents, film-forming aids,2025PF30011- Foreign Countries
[0128] reactive diluents, catalysts, thickeners, pigments, dyes, thickeners, and matting agents. In principle, selection and amount of the additives are known and easily measurable by a person of ordinary skill in the art. The aqueous polyurethane-urea dispersion of the invention can also be mixed with other oligomers or polymers containing water or solvents for use, such as polyesters, polyurethanes, polyurethane-polyacrylates, polyacrylates, polyethers, polyesterpolyacrylates, alkyds, addition polymers, polyamides / imides or polyepoxides containing water or solvents. The compatibility of such mixtures must be assessed using simple preliminary experiments in each case. The aqueous polyurethane-urea dispersion of the invention can also be mixed with other compounds containing functional groups such as carboxyl, hydroxyl, and / or blocked isocyanate groups before use. The coating, adhesive or ink of the invention are processed and obtained according to methods known to a person of ordinary skill in the art.
[0129] Articles and uses
[0130] The invention also provides an article comprising a substrate coated, bonded, sealed or printed with the coating, adhesive, sealant or ink of the invention. Preferably, the substrate is selected from wood, metal, glass, fiber, textile, artificial leather, genuine leather, paper, plastic, rubber, foam, ceramic, polymer coating, and combinations thereof. The coating may be conducted by applying the coating, adhesive or ink onto the entire surface of the substrate or only onto one or more parts of the surface of the substrate. The application of a coating may be done by brush coating, dipping, spray coating, roller coating, knife coating, flow coating, pouring or printing. The preferred printing method is inkjet printing.
[0131] The invention also provides the use of the aqueous polyurethane-urea dispersion of the invention for preparing coated products, bonded products, sealed products, or printed products.
[0132] For a person of ordinary skill in the art, the invention may be modified or changed in various manners within the scope of the claimed invention. Any modification, equivalent replacement, improvement and the like made within the scope of the claimed invention shall fall within the scope of the claimed invention.2025PF30011- Foreign Countries
[0133] Examples
[0134] The conception of the invention, the specific structure and the resulting technical effects will be further illustrated hereinafter in conjunction with the Examples, so that a person of ordinary skill in the art can fully understand the objectives, features and effects of the invention. The Examples herein are for the purpose of illustration only.
[0135] Chemicals
[0136] The chemicals used in the following Examples are as follows. Unless otherwise specified, all the chemical reagents used are chemically pure.
[0137] Desmodur® H: 1,6-hexam ethylene diisocyanate, available from Covestro AG.
[0138] Desmodur® I: isophorone diisocyanate, available from Covestro AG.
[0139] Desmodur® W: dicyclohexylmethane diisocyanate, available from Covestro AG.
[0140] Desmophen® P200H is representative of a polyester (polyhexylene phthalate) diol having an average hydroxyl functionality of two (as reported by the supplier) and a number-average molecular weight, determined as described in the specification, of 1528 g / mol, available from Covestro.
[0141] Desmophen® PE170HN is representative of a polyester diol (synthesized from adipic acid, hexylene glycol, and neopentyl glycol), having an average hydroxyl functionality of two (as reported by the supplier) and a number-average molecular weight, determined as described in the specification, of 2006 g / mol, available from Covestro.
[0142] Desmophen® C2202 is representative of a polycarbonate diol having an average hydroxyl functionality of two (as reported by the supplier) and a number-average molecular weight, determined as described in the specification, of 2085 g / mol, available from Covestro.
[0143] Desmophen® C1200 is representative of a polycarbonate-polycaprolactone diol (copolymer wherein the mass ratio of polycarbonate: poly caprolactone is 1.2:1) having an average hydroxyl functionality of two (as reported by the supplier) and a number-average molecular weight, determined as described in the specification, of 2131 g / mol, available from Covestro.
[0144] Desmophen® 2060 BD is representative of a polyether diol (polypropylene oxide diol) having an average hydroxyl functionality of two (as reported by the supplier), and a number-2025PF30011- Foreign Countries
[0145] average molecular weight, determined as described in the specification, of 1936 g / mol, available from Covestro.
[0146] PEG2000 is representative of a polyether diol (polyethylene oxide diol) having an average hydroxyl functionality of two (as reported by the supplier) and a number-average molecular weight, determined as described in the specification, of 2012 g / mol (supplied by Sinopharm Group).
[0147] Polyether LB 25 (available from Covestro) and MPEG 750 (supplied by Dow), each one is representative of compounds of Formula I; Ymer™ N120 and Ymer™ N180 (each supplied by Perstorp (Shanghai) Chemical Trading Co., Ltd.), each one is representative of compounds of Formula IV.
[0148] 2.2-bis(hydroxymethyl)butyric acid (DMBA), supplied by Sinopharm Group.
[0149] Ethylene diamine, supplied by Sinopharm Group.
[0150] Hydrazine hydride, supplied by Sinopharm Group.
[0151] Triethylamine (TEA), supplied by Sinopharm Group.
[0152] Neopentyl glycol, supplied by Sinopharm Group.
[0153] 2.2-bis(hydroxymethyl)propionic acid (DMPA), supplied by Sinopharm Group.
[0154] 3,3’-(Oxybis(2,l-ethanediyloxy)) bis-l-popanamine (CAS No. 4246-51-9), purity > 98% (GC), identical to Ancamine® 1922 A, supplied by Shanghai Aladdin Biochemical Technology Co., LTD.
[0155] SP 9111, a red pigment paste supplied by Shanghai Xude Fine Chemicals Co., Ltd., had a solid content, as reported by the supplier, of 40 wt.%.
[0156] 1.2-propylene glycol, used as a humectant, was supplied by Sinopharm Group.
[0157] TEGO® Foamex 825 (a polyether siloxane-based surfactant, in particular an emulsion of a polyether siloxane copolymer; active matter, as reported by the supplier, 20 wt.%), used as a surfactant, was supplied by Tego Additives.
[0158] BYK-349 (a polyether siloxane-based surfactant, in particular a polyether modified siloxane; active substance, as reported by the supplier, of 100 wt.%), used as a surfactant, was supplied by BYK-Chemie.2025PF30011- Foreign Countries
[0159] Borchi® gel L75N (non-volatile content, as reported by the supplier, of 48-52%), used as a thickener, was supplied by OMG Additives.
[0160] Imprafix® IO 3025, a polyisocyanate available from Covestro AG, was used as a crosslinking agent.
[0161] Analytical and testing methods
[0162] pH
[0163] The pH of an aqueous polyurethane-urea dispersion was determined at 23 °C using a PB-10 pH meter from Sartorius, Germany.
[0164] Isocyanate group (NCO) content
[0165] The isocyanate group (NCO) content (in wt.%) was determined in accordance with DIN-EN ISO 11909:2007.
[0166] Viscosity
[0167] The viscosity of an aqueous polyurethane-urea dispersion was measured using a Brookfield DV-II+Pro viscometer in accordance with ISO 2555:2018 standard. Specifically, 150 g of polyurethane-urea dispersion were weighed and placed into a glass bottle, and the viscosity was measured at 23 °C using a rotor with the serial number of S62 at a speed of 30 rpm (herein, ‘rpm’ stands for revolutions per minute).
[0168] Number-average molecular weight and weight-average molecular weight
[0169] The number-average molecular weight (Mn) and, the weight-average molecular weight (Mw) were determined by Size Exclusion Chromatography (SEC) calibrated with 12 narrowly dispersed polyethyleneglycol standards with molecular weights ranging from 232 to 44000 g / mol and using as eluent tetrahydrofuran at a flow rate of 0.7 mL / min. More specifically, 80 mg of a sample e.g. polyol (of component b), were dissolved in 10 mL of eluent for 24 hours at ambient temperature. 20 pL of the solution thus prepared were injected into the system for the measurement. The SEC measurements were carried out on an EcoSEC Elite® HLC-8420 GPC system equipped with a dual flow refractive index detector at 40°C and four columns, namely, TSKgel® G4000, TSKgel® G3000, TSKgel® G2500, and TSKgel® G4000HXL supplied by Tosoh Bioscience LLC. The Mnand Mwwere determined by the use of suitable software.2025PF30011- Foreign Countries
[0170] Z-average diameter of an aqueous polyurethane-urea dispersion
[0171] The average hydrodynamic diameter XDLS, as determined by dynamic light scattering (DLS) in accordance with DIN ISO 22412:2018-09, reflects the central value of the underlying particle size distribution. When determined by dynamic light scattering using the cumulants method, this average corresponds to a scattered light intensity-weighted harmonic mean particle diameter, referred to as the z-average diameter, wherein such determination is carried out in accordance with DIN ISO 22412:2018-09, with a Zetasizer Nano ZS particle size analyzer (supplied by Malvern Panalytical) using the technique of DLS, under the measurement conditions specified herein.
[0172] Samples were prepared by diluting 0.05 g of an aqueous polyurethane-urea dispersion in 20 mL of demineralized water and were analyzed at 23.0 ± 0.1 °C; as a reference material parameter setting, a polystyrene latex was used having a RI of 1.590 and absorption of 0.010, in demineralized water with a viscosity of 0.9308 cP and a RI of 1.330. The measurements were performed in disposable cuvettes DTS0012 obtained from Malvern Instruments (Malvern, Worcestershire, United Kingdom) after 60 sec equilibration period, under a 173° back-scatter angle as an average of 10 measurements (each measurement consisting of 10 sub-runs optimized by the machine itself, each run having a duration of 10 sec). The data were analyzed using a general-purpose (normal resolution) data fitting software.
[0173] Solid content of an aqueous polyurethane-urea dispersion.
[0174] The solid content (wt.%) of an aqueous polyurethane-urea dispersion refers to the nonvolatile substances in the aqueous polyurethane-urea dispersion. The solid content was measured using a Mettler Toledo halogen moisture analyzer (Mettler Toledo Halogen Moisture Analyzer Excellence HS 153) in accordance with DIN-EN ISO 3251 :2019. A piece of glass fiber filter paper was placed on a standard aluminum scale pan. 1 g of aqueous polyurethane-urea dispersion was dropped onto the glass fiber filter paper and was dried using standard drying procedures at a drying temperature of 120 °C, with a termination criteria level 5 (1 mg / 140 s). That is, the sample was heated to 120 °C and weighed continuously. If the weight loss of the sample was less than 1 mg within 140 seconds, the measurement was stopped, and the remaining weight percentage was recorded as solid content (wt.%).2025PF30011- Foreign Countries
[0175] Filterability performance
[0176] The polyurethane-urea dispersions of respective inventive examples and respective comparative examples were diluted with water to a solid content of 20 wt.%. 10 mL of the solution was drawn with a syringe and extruded from syringe filters with different pore sizes at a constant pressure of 2 kg, where the filterability performance was scored according to the following criteria:
[0177] 1: 10 mL of sample completely passes through a filter with a pore size of 0.22 microns (1 micron= 1 * 10'6m) within 1 minute.
[0178] 2: 10 mL of sample fails to completely pass through a filter with a pore size of 0.22 microns within 1 minute, with a residual amount less than 5 mL, but it can completely pass through a filter with a pore size of 0.45 microns within 1 minute.
[0179] 3: 10 mL of sample fails to completely pass through a filter with a pore size of 0.22 microns within 1 minute, with a residual amount greater than 5 mL, but it can completely pass through a filter with a pore size of 0.45 microns within 1 minute.
[0180] 4: 10 mL of sample fails to completely pass through a filter with a pore size of 0.45 microns within 1 minute, with a residual amount less than 5 mL, but it can completely pass through a filter with a pore size of 0.80 microns within 1 minute.
[0181] 5: 10 mL of sample fails to completely pass through a filter with a pore size of 0.45 microns within 1 minute, with a residual amount greater than 5 mL, but it can completely pass through a filter with a pore size of 0.80 microns within 1 minute.
[0182] 6: 10 mL of sample fails to completely pass through a filter with a pore size of 0.80 microns within 1 minute.
[0183] A score lower than 3 is considered as excellent filterability.
[0184] A score equal to or higher than 3 is considered as poor filterability.
[0185] Jettability test
[0186] The filtered aqueous polyurethane-urea dispersion was introduced into the ink cartridge of a digital direct-to-textile printing system equipped with EPSON 13200 / 2 industrial printheads. The printing program was configured for high-speed bidirectional operation with 8 passes and an ink load of 150%. The system was used to assess the jettability of the aqueous polyurethane-urea dispersion under these conditions. An aqueous polyurethane-urea dispersion that forms2025PF30011- Foreign Countries
[0187] and ejects droplets from an inkjet nozzle without clogging the nozzle is classified as jettable. An aqueous polyurethane-urea dispersion that does not form and eject droplets from the inkjet nozzle and / or clogs the inkjet nozzle is classified as not jettable.
[0188] Dry and wet color fastness
[0189] Step 1: Red-colored ink compositions, in the form of pastes (hereinafter ‘printing pastes’) were prepared using the following ingredients, formulated as described below (the total, red-colored printing paste composition being 100 wt.%). The amounts of the ingredients are given on an as-is basis, i.e. based on the total weight of each ingredient as provided, without regard to solid content, active matter or volatile constituents.
[0190] Ingredient Amount
[0191] PUD to be evaluated 82 wt.%
[0192] SP 9111 10 wt.%
[0193] 1,2-propanediol 3 wt.%
[0194] TEGO® Foamex 825 0.5 wt.%
[0195] BYK-349 0.5 wt.%
[0196] Borchi® gel L75N 1 wt.%
[0197] Imprafix® IO 3025 3 wt.%
[0198]
[0199] Step 2: Preparation of printed samples
[0200] 1. The printing paste prepared above was printed onto a white artificial leather substrate using a custom-made 120-mesh nylon screen, applied with a doctor blade in six successive passes.
[0201] 2. Placing the printed sample in an environment with a relative humidity of 50 % at 25 °C for 72 hours for natural air drying.
[0202] Step 3 : Assessment of dry and wet color fastness
[0203] The dry and wet color fastness were assessed using a Color Fastness to Rubbing tester (GT-7034-A, Gotech Testing Machines INC.) in accordance with the AATCC-8-2016 standard testing method. The staining, after 20 back-and-forth rubbing cycles, was graded with a grey scale according to the CTA Standard on a 1 to 5 grading scale, wherein the reported values are Grade 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5 or 5.2025PF30011- Foreign Countries
[0204] Dry color fastness with a score of 4 or less is considered insufficient, a score of 4.5 is considered very good, and a score of 5 is considered excellent. Wet color fastness with a score of 4 or less is considered insufficient, a score of 4.5 is considered very good, and a score of 5 is considered excellent.
[0205] Inventive Example 1 (El)
[0206] 270 g of Desmophen® P200H and 9.8 g of Polyether LB25 were dehydrated at 100 °C and 100 mbar (1 mbar= 100 Pa= 100 N / m2) for 1 hour. 13.8 g of DMBA was then added at 65 °C while stirring for 30 minutes. 11.9 g of Desmodur® W and 72.2 g of Desmodur® I were then added, the mixture was reacted at 80 °C until an isocyanate group content of 2.78% was reached and was then dissolved in 672g of acetone and cooled to 40 °C to obtain a reaction solution. 9.9 g of TEA was then added while stirring for 10 minutes. A solution of 4.9 g of ethylenediamine in 35.7 g of water was then added with vigorous stirring for 10 minutes. 690 g of water was then added to disperse the mixture, then acetone was removed by distillation to obtain an aqueous polyurethane-urea dispersion PUD1. PUD 1 had a z-average diameter of 68 nm, a viscosity of 29 mPa-s, a pH value of 7.37, and a solid content of 35.62 wt.%.
[0207] Inventive Example 2 (E2)
[0208] 43.5 g of Desmophen® P200H, 320 g of Desmophen® PE170HN, and 13.5 g of Polyether LB25 were dehydrated at 100 °C and 100 mbar for 1 hour. 18.3 g of DMBA was then added at 65 °C while stirring for 30 minutes. 17.8 g of Desmodur® W and 108.2 g of Desmodur® I were then added, and the mixture was reacted at 80 °C until an isocyanate group content of 3.50% was reached. The mixture was dissolved in 927 g of acetone and cooled to 40 °C to obtain a reaction solution. 12.7 g of TEA was then added while stirring for 10 minutes. A solution of 8.1 g ethylenediamine in 53.5 g of water was then added with vigorous stirring for 10 minutes. 904 g of water was then added to disperse the mixture, then acetone was removed distillation to obtain an aqueous polyurethane-urea dispersion PUD2. PUD 2 had a z-average diameter of 98 nm, a viscosity of 71 mPa-s, a pH value of 7.52, and a solid content of 35.16 wt.%.
[0209] Inventive Example 3 (E3)
[0210] 277.6 g of Desmophen® P200H and 18.6 g of Polyether LB25 were dehydrated at 100 °C and 100 mbar for 1 hour. 6.8 g of DMBA was then added at 65°C while stirring for 30 minutes.
[0211] 20.1 g of Desmodur® W and 48.0 g of Desmodur® I were then added, and the mixture was reacted at 80 °C until an isocyanate group content of 2.34% was reached. The mixture was then dissolved2025PF30011- Foreign Countries
[0212] in 660 g of acetone and cooled to 40°C to obtain a reaction solution. 4.5 g of TEA was then added while stirring for 10 minutes. A solution of 5.0 g ethylenediamine in 28.6 g of water was then added with vigorous stirring for 10 minutes. 670 g of water was then added to disperse the mixture, then acetone was removed by distillation to obtain an aqueous polyurethane-urea dispersion PUD3. PUD 3 had a z-average diameter of 68 nm, a viscosity of 145 mPa-s, a pH value of 7.53, and a solid content of 35.16 wt.%.
[0213] Inventive Example 4 (E4)
[0214] 258.5 g of Desmophen® P200H and 6.1 g of Ymer™ N180 were dehydrated at 100 °C and 100 mbar for 1 hour. 18 g of DMBA was then added at 65 °C while stirring for 30 minutes. 27.6 g of Desmodur® W and 65.9 g of Desmodur® I were then added, and the mixture was reacted at 80 °C until an isocyanate group content of 3.14% was reached. The mixture was then dissolved in 669 g of acetone and cooled to 40 °C to obtain a reaction solution. 12.1 g of TEA was then added while stirring for 10 minutes. A solution of 5.4 g ethylenediamine in 39.2 g of water was then added with vigorous stirring for 10 minutes. 705 g of water was then added to disperse the mixture, then acetone was removed by distillation to obtain an aqueous polyurethane-urea dispersion PUD4. PUD 4 had a z-average diameter of 36 nm, a viscosity of 273 mPa-s, a pH value of 7.93, and a solid content of 34.84 wt.%.
[0215] Inventive Example 5 (E5)
[0216] 235 g of Desmophen® P200H and 5.5 g of MPEG 750 were dehydrated at 100 °C and 100 mbar for 1 hour. 16.7 g of DMBA was then added at 65 °C while stirring for 30 minutes. 25.1 g of Desmodur® W and 59.9 g of Desmodur® I were then added, and the mixture was reacted at 80 °C until an isocyanate group content of 3.21% was reached. The mixture was then dissolved in 609 g of acetone and cooled to 40 °C to obtain a reaction solution. 11.2 g of TEA was then added while stirring for 10 minutes. A solution of 4.9 g ethylenediamine in 35.7 g of water was then added with vigorous stirring for 10 minutes. 657 g of water was then added to disperse the mixture, then acetone was removed by distillation to obtain an aqueous polyurethane-urea dispersion PUD5. PUD 5 had a z-average diameter of 38 nm, a viscosity of 224 mPa-s, a pH value of 7.53, and a solid content of 34.67 wt.%.
[0217] Inventive Example 6 (E6)
[0218] 308 g of Desmophen® P200H and 5.9 g of Polyether LB25 were dehydrated at 100 °C and 100 mbar for 1 hour. 14.9 g of DMBA was then added at 65 °C while stirring for 30 minutes.2025PF30011- Foreign Countries
[0219] 27.6 g of Desmodur® W and 65.9 g of Desmodur® I were then added, and the mixture was reacted at 80 °C until an isocyanate group content of 2.89% was reached. The mixture was dissolved in 751 g of acetone and cooled to 40 °C to obtain a reaction solution. 10 g of TEA was then added while stirring for 10 minutes. A solution of 5.4 g of ethylenediamine in 39.2 g of water was then added with vigorous stirring for 10 minutes. 754 g of water was then added to disperse the mixture, then acetone was removed by distillation to obtain an aqueous polyurethane-urea dispersion PUD6. PUD 6 had a z-average diameter of 70 nm, a viscosity of 88 mPa-s, a pH value of 7.75, and a solid content of 35.70 wt.%.
[0220] Inventive Example 7 (E7)
[0221] 243 g of Desmophen® P200H and 8.1 g of Polyether LB25 were dehydrated at 100 °C and 100 mbar for 1 hour. 13.3 g of DMBA was then added at 65 °C while stirring for 30 minutes.
[0222] 73.9 g of Desmodur® H was then added, and the mixture was reacted at 80 °C until an isocyanate group content of 2.97% was reached. The mixture was dissolved in 601 g of acetone and cooled to 40 °C to obtain a reaction solution. 8.9 g of TEA was then added while stirring for 10 minutes. A solution of 4.4 g of ethylenediamine in 32.1 g of water was then added with vigorous stirring for 10 minutes. 696 g of water was then added to disperse the mixture, then acetone was removed by distillation to obtain an aqueous polyurethane-urea dispersion PUD7. PUD 7 had a z-average diameter of 53 nm, a viscosity of 50 mPa-s, a pH value of 7.52, and a solid content of 32.79 wt.%.
[0223] Comparative Example 1 (CE1)
[0224] 190 g of Desmophen® P200H, 70 g of Desmophen® 2060 BD, and 9.0 g of Polyether LB25 were dehydrated at 100 °C and 100 mbar for 1 hour. 15.6 g of DMBA was then added at 65 °C while stirring for 30 minutes. 72.2 g of Desmodur® I and 11.9 g of Desmodur® W were then added, and the mixture was reacted at 80 °C until an isocyanate group content of 3.03% was reached. The mixture was then dissolved in 655 g of acetone and cooled to 40 °C to obtain a reaction solution. 10.4 g of TEA was then added while stirring for 10 minutes. A solution of 4.9 g of ethylenediamine in 35.7 g of water was then added with vigorous stirring for 10 minutes. 786 g of water was then added to disperse the mixture, then acetone was removed by distillation to obtain an aqueous polyurethane-urea dispersion PUD8. PUD 8 had a z-average diameter of 114 nm, a viscosity of 120 mPa-s, a pH value of7.84, and a solid content of 31.75 wt.%.2025PF30011- Foreign Countries
[0225] Comparative Example 2 (CE2)
[0226] 281.2 g of Desmophen® P200H and 9.1 g of Poly ether LB25 were dehydrated at 100 °C and 100 mbar for 1 hour. 5.1 g of DMBA was then added at 65 °C while stirring for 30 minutes. 19.1 g of Desmodur® W and 45.6 g of Desmodur® I were then added, and the mixture was reacted at 80 °C until an isocyanate group content of 2.34% was reached. The mixture was dissolved in 640 g of acetone and cooled to 40 °C to obtain a reaction solution. 3.4 g of TEA was then added while stirring for 10 minutes. A solution of 3.7 g of ethylenediamine in 27.1 g of water was then added with vigorous stirring for 10 minutes. 652 g of water was then added to disperse the mixture, then acetone was removed by distillation; precipitation occurred prior to completion of acetone removal, such that, although the polyurethane-urea was successfully synthesized, no aqueous dispersion was formed. Thus, no further characterization or evaluation of CE2 was pursued.
[0227] Comparative Example 3 (CE3)
[0228] 167.9 g of Desmophen® P200H and 6.3 g of Polyether LB25 were dehydrated at 100 °C and 100 mbar for 1 hour. 13.0 g of DMBA was then added at 65 °C while stirring for 30 minutes.
[0229] 18.3 g of Desmodur® W and 43.8 g of Desmodur® I were then added, and the mixture was reacted at 80 °C until an isocyanate group content of 3.15% was reached. The mixture was then dissolved in 443 g of acetone and cooled to 40 °C to obtain a reaction solution. 8.7 g of TEA was then added while stirring for 10 minutes. A solution of 3.6 g of ethylenediamine in 26 g of water was then added with vigorous stirring for 10 minutes. 461 g of water was then added to disperse the mixture, then acetone was removed by distillation to obtain an aqueous polyurethane-urea dispersion PUD9. PUD 9 had a z-average diameter of 43 nm, a viscosity of 1516 mPa- s, a pH value of 7.86, and a solid content of 34.39 wt.%.
[0230] Comparative Example 4 (CE4)
[0231] 310 g of Desmophen® P200H and 3.9 g of Polyether LB25 were dehydrated at 100 °C and 100 mbar for 1 hour. 14.9 g of DMBA was then added at 65 °C while stirring for 30 minutes.
[0232] 27.6 g of Desmodur® W and 65.9 g of Desmodur® I were then added, and the mixture was reacted at 80 °C until an isocyanate group content of 2.88% was reached. The mixture was then dissolved in 751 g of acetone and cooled to 40 °C to obtain a reaction solution. 10.0 g of TEA was then added while stirring for 10 minutes. A solution of 5.4 g of ethylenediamine in 39.2 g of water was then added with vigorous stirring for 10 minutes. 754 g of water was then added to disperse the mixture, then acetone was removed by distillation to obtain an aqueous polyurethane-urea2025PF30011- Foreign Countries
[0233] dispersion PUD10. PUD 10 had a z-average diameter of 127 nm, a viscosity of 29 mPa-s, a pH value of 7.33, and a solid content of 35.58 wt.%.
[0234] Comparative Example 5 (CE5)
[0235] 240.5 g of Desmophen® P200H was dehydrated at 100 °C and 100 mbar for 1 hour. 16.7 g of DMBA was then added at 65 °C while stirring for 30 minutes. 25.1 g of Desmodur® W and 59.9 g of Desmodur® I were then added, and the mixture was reacted at 80 °C until an isocyanate group content of 3.23% was reached. The mixture was then dissolved in 609 g of acetone and cooled to 40 °C to obtain a reaction solution. 11.2 g of TEA was then added while stirring for 10 minutes. A solution of 4.9 g of ethylenediamine in 35.7 g of water was then added with vigorous stirring for 10 minutes. 597 g of water was then added to disperse the mixture, then acetone was removed by distillation to obtain an aqueous polyurethane-urea dispersion PUD11. PUD 11 had a z-average diameter of 44 nm, a viscosity greater than 3000 mPa-s, a pH value of 7.96, and a solid content of 36.60 wt.%.
[0236] Comparative Example 6 (CE6)
[0237] 247.5 g of Desmophen® P200H and 20 g of Polyether LB25 were dehydrated at 100 °C and 100 mbar for 1 hour. 12.7 g of DMBA was then added at 65 °C while stirring for 30 minutes.
[0238] 22.6 g of Desmodur® W and 53.9 g of Desmodur® I were then added, and the mixture was reacted at 80 °C until an isocyanate group content of 2.70% was reached. The mixture was then dissolved in 634 g of acetone and cooled to 40 °C to obtain a reaction solution. 8.5 g of TEA was then added while stirring for 10 minutes. A solution of 4.4 g of ethylenediamine in 32.1 g of water was then added with vigorous stirring for 10 minutes. 667 g of water was then added to disperse the mixture, then acetone was removed by distillation to obtain an aqueous polyurethane-urea dispersion PUD12. PUD 12 had a z-average diameter of 67 nm, a viscosity of 1640 mPa-s, a pH value of 7.91, and a solid content of 34.67 wt.%.
[0239] Comparative Example 7 (CE7)
[0240] 249.3 g of Desmophen® P200H and 8.8 g of PEG2000 were dehydrated at 100 °C and 100 mbar for 1 hour. 12.3 g of DMBA was then added at 65 °C while stirring for 30 minutes. 22.6 g of Desmodur® W and 53.9 g of Desmodur® I were then added, and the mixture was reacted at 80 °C until an isocyanate group content of 2.81% was reached. The mixture was then dissolved in 617 g of acetone and cooled to 40 °C to obtain a reaction solution. 8.3 g of TEA was then added while stirring for 10 minutes. A solution of 4.4 g of ethylenediamine in 32.1 g of water was then2025PF30011- Foreign Countries
[0241] added with vigorous stirring for 10 minutes. 659 g of water was added to disperse the mixture, then acetone was removed by distillation to obtain an aqueous polyurethane-urea dispersion PUD13. PUD 13 had, a z-average diameter of 85 nm, a viscosity of 542 mPa-s, a pH value of 7.82, a solid content of 34.64 wt.%.
[0242] Comparative Example 8 (CE8)
[0243] 394.5 g of Desmophen® C2202 and 12.6 g of Polyether LB25 were dehydrated at 100 °C and 100 mbar for 1 hour. 9.8 g of DMPA was then added at 65 °C while stirring for 30 minutes.
[0244] 8.2 g of Desmodur® H and 83.7 g of Desmodur® I were then added, and the mixture was reacted at 80 °C until an isocyanate group content of 2.56% was reached. The mixture was then dissolved in 905 g of acetone and cooled to 40 °C to obtain a reaction solution. 7.3 g of TEA was then added while stirring for 10 minutes. A solution of 5.6 g of ethylenediamine in 39.9 g of water was then added with vigorous stirring for 10 minutes. 896 g of water was then added to disperse the mixture, then acetone was removed by distillation to obtain an aqueous polyurethane-urea dispersion PUD14. PUD 14 had a z-average diameter of 82 nm, a viscosity of 48 mPa-s, a pH value of 7.43, and a solid content of 35.37 wt.%.
[0245] Comparative Example 9 (CE9)
[0246] 342 g of Desmophen® C1200 and 14.5 g of Ymer™ N120 were dehydrated at 100 °C and 100 mbar for 1 hour. 9.3 g of DMBA was then added at 65 °C while stirring for 30 minutes. 14.2 g of Desmodur® W and 86.6 g of Desmodur® I were then added, and the mixture was reacted at 80 °C until an isocyanate group content of 3.21% was reached. The mixture was then dissolved in 894 g of acetone and cooled to 40 °C to obtain a reaction solution. 6.4 g of TEA was then added while stirring for 10 minutes. A solution of 6.5 g of ethylenediamine in 42.8 g of water was then added with vigorous stirring for 10 minutes. 873 g of water was then added to disperse the mixture, then acetone was removed by distillation to obtain an aqueous polyurethane-urea dispersion PUD15. PUD 15 had a z-average diameter of 84 nm, a viscosity of 15 mPa-s, a pH value of 7.10, and a solid content of 35.92 wt.%.
[0247] Comparative Example 10 (CE10)
[0248] 422.7 g of Desmophen® C2202 and 13.7 g of Polyether LB25 were dehydrated at 100 °C and 100 mbar for 1 hour. 11 g of DMBA was then added at 65 °C while stirring for 30 minutes.
[0249] 8.8 g of Desmodur® H and 88.5 g of Desmodur® I were then added, and the mixture was reacted at 80 °C until an isocyanate group content of 2.22% was reached. The mixture was dissolved in2025PF30011- Foreign Countries
[0250] 968 g of acetone and cooled to 40 °C to obtain a reaction solution. 7.4 g of TEA was then added while stirring for 10 minutes. A solution of 6.0 g of ethylenediamine in 42.8 g of water was then added with vigorous stirring for 10 minutes. 966 g of water was then added to disperse the mixture, then acetone was removed by distillation to obtain an aqueous polyurethane-urea dispersion PUD16. PUD 16 had a z-average diameter of 87 nm, a viscosity of 6 mPa-s, a pH value of 7.77, and a solid content of 35.92 wt.%.
[0251] Comparative Example 11 (CE11)
[0252] Comparative Example 11 corresponds to Example El of EP 2028205 Al. Example El of EP 2028205 Al was repeated by following the processes described in EP 2028205 Al, employing the materials, reaction conditions, and sequence of steps as described in EP 2028205 Al and without modification (herein PUD 17). PUD 17 had a z-average diameter of 243 nm, a viscosity of 2579 mPa-s, a pH value of 8.56, and a solid content of 28.00 wt.%.
[0253] Comparative Example 12 (CE12)
[0254] Comparative Example 12 corresponds to Example E2 of EP 2028205 Al. Example E2 of EP 2028205 Al was repeated by following the processes described in EP 2028205 Al, employing the materials, reaction conditions, and sequence of steps as described in EP 2028205 Al and without modification (herein PUD 18). PUD 18 had a z-average diameter of 100 nm, a viscosity of 36 mPa-s, a pH value of 8.38, and a solid content of 32.78 wt.%.
[0255] Comparative Example 13 (CE13)
[0256] Comparative Example 13 corresponds to Example E5 of EP 2028205 Al. Example E5 of EP 2028205 Al was repeated by following the processes described in EP 2028205 Al, employing the materials, reaction conditions, and sequence of steps as described in EP 2028205 Al without modification (herein PUD19). PUD 19 had a z-average diameter of 83 nm, a viscosity of 219 mPa-s, a pH value of 8.07, and a solid content of 39.73 wt.%.2025PF30011- Foreign Countries
[0257] Table 1 presents the jettability of the inventive and comparative aqueous polyurethane-urea dispersion, their filterability performance, and the dry and wet color fastness of prints of ink compositions containing said aqueous polyurethane-urea dispersions, on artificial leather. In Table 1, ‘n.d.’ indicates that the value was not determined.
[0258] Table 1
[0259] Jettability of Filterability of Dry color
[0260] Wet color aqueous aqueous fastness on
[0261] fastness on polyurethane- polyurethane- artificial
[0262] artificial leather urea dispersion urea dispersion leather
[0263] El Jettable 1 (Excellent) 5 (Excellent) 5 (Excellent)
[0264] E2 Jettable 1 (Excellent) 5 (Excellent) 4.5 (Very good) E3 Jettable 1 (Excellent) 5 (Excellent) 5 (Excellent)
[0265] E4 Jettable 1 (Excellent) 5 (Excellent) 5 (Excellent)
[0266] E5 Jettable 1 (Excellent) 5 (Excellent) 5 (Excellent)
[0267] E6 Jettable 2 (Excellent) 5 (Excellent) 5 (Excellent)
[0268] E7 Jettable 2 (Excellent) 5 (Excellent) 5 (Excellent) CE1 Not jettable 3 (Poor) n.d. n.d.
[0269] CE3 Not jettable 4 (Poor) n.d. n.d.
[0270] CE4 Not jettable 5 (Poor) n.d. n.d.
[0271] CE5 Not jettable 2 (Excellent) n.d. n.d.
[0272] CE6 Not jettable 5 (Poor) n.d. n.d.
[0273] CE7 Not jettable 5 (Poor) n.d. n.d.
[0274] CE8 Not jettable 4 (Poor) n.d. n.d.
[0275] CE9 Jettable 1 (Excellent) 5 (Excellent) 4 (Insufficient) CE10 Jettable 2 (Excellent) 5 (Excellent) 3.5 (Insufficient) CE11 Not jettable 6 (poor) 5 (Excellent) 3.5 (Insufficient) CE12 Not jettable 6 (poor) 5 (Excellent) 3 (Insufficient) CEI3 Not jettable 3 (poor) 5 (Excellent) 3.5 (Insufficient)
[0276]
[0277] 2025PF30011- Foreign Countries
[0278] One objective of the invention was to provide an aqueous polyurethane-urea dispersion which is (i) jettable, has (ii) excellent filterability, and (iii) prints of ink compositions containing said aqueous polyurethane-urea dispersion, on artificial leather, have excellent dry color fastness and at least very good, preferably excellent wet color fastness.
[0279] The comparative examples failed to provide an aqueous polyurethane-urea dispersion which is (i) jettable, has (ii) excellent filterability, and (iii) prints of ink compositions containing said aqueous polyurethane-urea dispersion, on artificial leather, have excellent dry color fastness and at least very good, preferably excellent wet color fastness. More particularly, Comparative Example CE11 and CE 12 demonstrate that when component b) was not present in the polyurethane-urea, the resulting aqueous polyurethane-urea dispersions were not jettable, their filterability was poor, and they afforded prints with insufficient wet color fastness. Comparative Example CE9 and CE10 demonstrate that when component b) was not present in the polyurethane-urea, the resulting aqueous dispersion afforded prints with insufficient wet color fastness. Comparative Example CE1 demonstrates that when the amount of component b) is lower than 60 wt.% of the polyurethane-urea, the aqueous polyurethane-urea dispersion was not jettable, and the filterability was poor. Comparative Example CE8 demonstrates that when component c) was not present in the polyurethane-urea, the resulting aqueous polyurethane-urea dispersion was not jettable, and its filterability was poor. Comparative Example CE2 demonstrates that when the amount of component c) was lower than 1.6 wt.% in the polyurethane-urea, no aqueous polyurethane-urea dispersion was formed. Comparative Example CE3 demonstrates that when the amount of component c) was greater than 4.8 wt.% of the polyurethane-urea, the resulting aqueous polyurethane-urea dispersion was not jettable, and its filterability was poor. Comparative Example CE4 demonstrates that when the amount of component d) was less than 1 wt.% of the polyurethane-urea, the resulting aqueous polyurethane-urea dispersion was not jettable, and its filterability was poor. Comparative Examples CE5 and CE7 demonstrate that when component d) was not present in the polyurethane-urea, the resulting aqueous polyurethane-urea dispersion was not jettable and in case of CE7 the filterability was also poor. Comparative Example CE6 demonstrates that when the amount of component d) was greater than 5 wt.% of the polyurethane-urea, the resulting aqueous polyurethane-urea dispersion was not jettable, and its filterability was poor. Comparative Example CE13 demonstrates that when components b) and c) are not present in the polyurethane-2025PF30011- Foreign Countries
[0280] urea, the resulting aqueous polyurethane-urea dispersion was not jettable, its filterability was poor, and it afforded prints with insufficient wet color fastness.
[0281] Only the aqueous polyurethane-urea dispersions according to the invention (see Inventive Examples E1-E7) were (i) jettable, had (ii) excellent filterability, and (iii) prints of ink compositions containing said aqueous polyurethane-urea dispersion, on artificial leather, had excellent dry color fastness and at least very good (some had excellent) wet color fastness.
Claims
2025PF30011- Foreign CountriesClaims1. An aqueous polyurethane-urea dispersion comprising(i) a polyurethane-urea, wherein the polyurethane-urea is obtained by reacting at least the following components a) to f):a) at least one polyisocyanate,b) at least one polyester diol, wherein the amount of component b) is 60-80 wt.% of the polyurethane-urea,c) 2,2-bis(hydroxymethyl) butyric acid in an amount of 1.6-4.8 wt.% of the polyurethane-urea, d) at least one non-ionic hydrophilic agent selected from compounds represented by Formula I, Formula II, Formula III, Formula IV, Formula V, and combinations thereofFormula Iwhereing is an integer from 0 to 70, preferably from 0 to 35, more preferably from 0 to 10,x is an integer from 10 to 70, preferably from 10 to 55, more preferably from 15 to 50, with the proviso that x is not less than g when g is greater than 10,Ri is a Ci-Cis hydrocarbon group, or a group consisting of 2 to 18 carbon atoms, hydrogen atoms, and 1 to 8 oxygen atoms, wherein each oxygen atom present forms part only of ether linkages other than oxirane groups, and wherein Ri is covalently bonded to the oxygen atom of Formula I via a carbon atom of Ri via a carbon-oxy gen single bond,HOwhereinn is an integer from 0 to 70, preferably from 0 to 35, more preferably from 0 to 10,m is an integer from 10 to 70, preferably from 10 to 55, more preferably from 15 to 50,2025PF30011- Foreign Countrieswith the proviso that m is not less than n when n is greater than 10,R2 is a C1-C18 hydrocarbon group, or a group consisting of 2 to 18 carbon atoms, hydrogen atoms, and 1 to 8 heteroatoms selected from oxygen and nitrogen, wherein the number of nitrogen atoms is 1 and wherein each oxygen atom forms part only of ether linkages other than oxirane groups and the nitrogen atom either forms part of a -C=N-C- linkage or it is directly covalently bonded only to carbon atoms via carbon-nitrogen single bonds, and wherein R2 is covalently bonded to the nitrogen atom of Formula II via a carbon atom of R2 via a carbon-nitrogen single bond, R3 is a C1-C18 hydrocarbon group, or a group consisting of 2 to 18 carbon atoms, hydrogen atoms, and 1 to 8 heteroatoms selected from oxygen and nitrogen, wherein the number of nitrogen atoms is 1, and wherein each oxygen atom forms part only of ether linkages other than oxirane groups and the nitrogen atom either forms part of a -C=N-C- linkage or it is directly covalently bonded only to carbon atoms via carbon-nitrogen single bonds, and wherein R3 is covalently bonded to the nitrogen atom of Formula II via a carbon atom of R3 via a carbon-nitrogen single bond,Formula IIIwhereinn’ is an integer from 0 to 70, preferably from 0 to 35, more preferably from 0 to 10,m’ is an integer from 10 to 70, preferably from 10 to 55, more preferably from 15 to 50, with the proviso that m’ is not less than n’ when n’ is greater than 10,R4 is a C3-C10 hydrocarbon group, or a group consisting of 3 to 10 carbon atoms, hydrogen atoms, and 1 or 2 heteroatoms selected from oxygen and nitrogen, and wherein each oxygen atom forms part only of ether linkages other than oxirane groups and each nitrogen atom forms part either of a -C=N-C- linkage, or it is directly covalently bonded only to carbon atoms via carbon-nitrogen single bonds, and wherein ds covalently bonded to the nitrogen atom of Formula III via two distinct carbon atoms of R4, each via a carbon-nitrogen single bond,2025PF30011- Foreign CountriesyFormula IVwhereiny is an integer from 0 to 70, preferably from 0 to 35, more preferably from 0 to 10,z is an integer from 10 to 70, preferably from 10 to 55, more preferably from 10 to 50, with the proviso that z is not less than y when y is greater than 10,Rs is a C1-C18 hydrocarbon group, or a group consisting of 2 to 18 carbon atoms, hydrogen atoms, and 1 to 8 oxygen atoms, wherein each oxygen atom forms part only of ether linkages other than oxirane groups, and wherein R5 is covalently bonded to the oxygen atom of Formula IV via a carbon atom of Rs via a carbon-oxy gen single bond,Formula Vwhereinp is an integer from 0 to 70, preferably from 0 to 35, more preferably from 0 to 10,q is an integer from 10 to 70, preferably from 10 to 55, more preferably from 10 to 50, with the proviso that q is not less than p when p is greater than 10,and wherein the amount of component d) is 1-5 wt.% of the polyurethane-urea,e) at least one chain extender wherein the chain extender is selected from hydrazine, primary amines having a molar mass of 32-500 g / mol, optionally containing at most 2 hydroxyl groups, secondary amines having a molar mass of 32-500 g / mol optionally containing at most 2 hydroxyl groups, and combinations thereof,f) at least one neutralizing agent wherein the neutralizing agent is selected from alkali metal hydroxides, ammonia, tertiary amines optionally containing at most three hydroxyl groups, and combinations thereof, preferably the at least one neutralizing agent is selected from alkali metal2025PF30011- Foreign Countrieshydroxides, ammonia, tertiary amines having a molar mass of at most 400 g / mol, preferably at most 200 g / mol, optionally containing at most three hydroxyl groups, and combinations thereof, and(ii) optionally an organic solvent.
2. The aqueous polyurethane-urea dispersion according to claim 1, wherein the amount of component a) is 15-30 wt.% of the polyurethane-urea, the amount of component e) is 0.1-3.0 wt.% of the polyurethane-urea, and the amount of component f) is 0.10-10.0 wt.% of the polyurethane-urea.
3. The aqueous polyurethane-urea dispersion according to any one of claims 1-2, wherein the at least one polyester diol has a number-average molecular weight, determined as described in the specification, of 800-4000 g / mol, preferably 1000-3000 g / mol.
4. The aqueous polyurethane-urea dispersion according to any one of claims 1-3, wherein the at least one polyester diol is selected from aromatic polyester diols.
5. The aqueous polyurethane-urea dispersion according to any one of claims 1-4, wherein the at least one non-ionic hydrophilic agent is selected from compounds represented by Formula I, Formula II, Formula III, Formula IV, Formula V, and combinations thereof, wherein, for each of said compounds, for the respective one of Formulae I, II, III, IV or V by which that compound is represented, each of the corresponding ratiosx / (x+g) for compounds of Formula I,m / (m+n) for compounds of Formula II,m' / (m'+n') for compounds of Formula III,z / (z+y) for compounds of Formula IV, andq / (q+p) for compounds of Formula Vis greater than 0.5, preferably wherein each of said ratios is greater than 0.6, more preferably wherein each of said ratios is greater than 0.7, most preferably wherein each of said ratios is greater than 0.8.2025PF30011- Foreign Countries6. The aqueous polyurethane-urea dispersion according to any one of claims 1-5, wherein the aqueous polyurethane-urea dispersion has a solid content, determined as described in the specification, of 30-65 wt.%, preferably 30-50 wt.%, more preferably 30-40 wt.%, and most preferably 30-36 wt.%.
7. The aqueous polyurethane-urea dispersion according to any one of claims 1-6, wherein the aqueous polyurethane-urea dispersion has a viscosity, determined as described in the specification, of 1-1000 mPa.s, preferably 1-500 mPa.s, more preferably 1-300 mPa.s.
8. The aqueous polyurethane-urea dispersion according to any one of claims 1-7, wherein the aqueous polyurethane-urea dispersion has a z-average diameter, determined as described in the specification, of 30-100 nm.
9. The aqueous polyurethane-urea dispersion according to any one of claims 1-8, wherein the aqueous polyurethane-urea dispersion has a pH, determined as described in the specification, of 4-10.
10. The aqueous polyurethane-urea dispersion according to any one of claims 1-9, wherein the at least one polyisocyanate is selected from diisocyanates of formula Y(NCO)2, wherein Y is a divalent aliphatic hydrocarbon group containing 4-12 carbon atoms, a divalent cycloaliphatic hydrocarbon group containing 6-15 carbon atoms, a divalent aromatic hydrocarbon group containing 6-15 carbon atoms, or a divalent araliphatic hydrocarbon group containing 7-15 carbon atoms, preferably Y is a divalent aliphatic hydrocarbon group containing 4-12 carbon atoms or a divalent cycloaliphatic hydrocarbon group containing 6-15 carbon atoms.
11. The aqueous polyurethane-urea dispersion according to any of claims 1-10, wherein the amount of the organic solvent, if present, is less than 1.0 wt.%.
12. A coating, an adhesive, a sealant or an ink prepared using the aqueous polyurethane-urea dispersion according to any of claims 1-11.2025PF30011- Foreign Countries13. An article comprising a substrate coated, bonded, sealed or printed using a coating, adhesive, sealant or ink of claim 12.
14. The article according to claim 13, wherein the substrate is selected from wood, metal, glass, fiber, textile, artificial leather, genuine leather, paper, plastic, rubber, foam, ceramic, polymer coating, and combinations thereof.