Polyether sulfone hot melt adhesive blend

A PESU-based hot melt adhesive blend with a lower Tg than PESU addresses the recycling challenge by forming strong bonds in PESU composites, ensuring recyclability through vaporization of polyether polyol during recycling.

WO2026234535A1PCT designated stage Publication Date: 2026-11-123M INNOVATIVE PROPERTIES CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2026/054358
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-05
Filing Date
2026-05-01
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Thermoplastic composites, particularly those made from polyether sulfone (PESU), face challenges in recycling due to similar glass transition temperatures (Tg) of their components, leading to difficulties in heat lamination and adhesive bonding that can degrade the foam, reducing recyclability.

Method used

A PESU-based hot melt adhesive blend with polyether polyol, having a lower Tg than PESU, is developed to bond PESU layers without adverse effects, allowing for recyclable composite assemblies.

Benefits of technology

The adhesive blend forms strong bonds between PESU layers, enabling recyclable composite structures by vaporizing the low-molecular-weight polyether polyol during recycling, preserving the quality of recycled PESU materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IB2026054358_12112026_PF_FP_ABST
    Figure IB2026054358_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The hot melt adhesives are a polymeric blend of at least one thermoplastic sulfone polyether and at least one polyether polyol material. The polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) that is less than the Tg of the at least one thermoplastic polyether sulfone material. The polymeric blend is capable of hot melt bonding two substrates comprising thermoplastic polyether sulfone materials to form multi-layer articles.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] PA102920W002

[0002] POLYETHER SULFONE HOT MELT ADHESIVE BLEND

[0003] Summary

[0004] Disclosed herein are hot melt adhesives and multi-layer articles prepared with the hot melt adhesives. In some embodiments, the hot melt adhesive comprises a polymeric blend, where the blend 5 comprises at least one thermoplastic polyether sulfone material and at least one polyether polyol material.

[0005] The polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) that is less than the Tg of the at least one thermoplastic polyether sulfone material. The polymeric blend is capable of hot melt bonding two substrates comprising thermoplastic polyether sulfone materials.

[0006] Also disclosed are multi-layer articles prepared with the hot melt adhesives described above. In 10 some embodiments, the multi-layer article comprises a core layer comprising at least one thermoplastic polyether sulfone material, an adhesive layer comprising a thermoplastic polyether sulfone-based hot melt adhesive, and a skin layer comprising at least one thermoplastic polyether sulfone material, and at least one reinforcing fabric. The hot melt adhesives are described above and comprise a polymeric blend, where the blend comprises at least one thermoplastic polyether sulfone material and at least one polyether polyol material. The polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) that is less than the Tg of the at least one thermoplastic polyether sulfone material.

[0007] Brief Description of the Drawings

[0008] The present application may be more completely understood in consideration of the following detailed description of various embodiments of the disclosure in connection with the accompanying drawings.

[0009] Figure 1 is a cross sectional view of an article of this disclosure.

[0010] Figure 2 is a DSC thermogram of a polyethersulfone material used in this disclosure.

[0011] Figure 3 is a DSC thermogram of a polyethersulfone Foam Core Material used in this disclosure. Figure 4 is a DSC thermogram of a polyethersulfone Skin Layer Material used in this disclosure.

[0012] 25 Figure 5 is a DSC thermogram of the Hot Melt Adhesive of Example 1.

[0013] In the following description of the illustrated embodiments, reference is made to the accompanying drawings, in which is shown by way of illustration, various embodiments in which the disclosure may be practiced.

[0014] Detailed Description

[0015] Composite structures are used in a wide range of applications. A composite is a material which is produced from two or more constituent materials. These constituent materials have notably dissimilar chemical or physical properties and are merged to create a material with properties unlike the individual elements. Within the finished structure, the individual elements remain separate and distinct. Typical engineered composite materials include, for example, reinforced concrete, and composite sandwich 35 structures containing fiber-reinforced polymer or fiberglass. Uses for composite sandwich structuresinclude their use in aircraft manufacturing, such as for airplane cabin interiors. While small parts can be manufactured via welding using hot Air Welders, Wedge Welders and Ultrasonic Welders, but for large surfaces, assembly typically involves the use of a heat press, a heat maintained vacuum bag or an autoclave.

[0016] A trend in the area of engineered composites is recyclability. As thermoplastics have become more important in the assembly of composites, it has become increasingly desirable for waste thermoplastic polymers to be recycled or reprocessed by a mechanical process using melt extrusion, injection, blowing, vacuum, and inflation molding. This methods use 100% utilization and conversion of waste plastic to produce the same or other valuable products. Thermoplastic materials are a type of polymer that becomes soft and moldable when heated to a temperature T (T > Tg), allowing them to be shaped into various forms. These polymers can be melted, molded, and reshaped multiple times without significant chemical changes, making them very versatile and cost-effective in recycling and reusability. The difficulty with thermoplastic composites is that the composites contain other materials and therefore are difficult to recycle and repurpose because the quality of the recycled materials is highly influenced by polymer cross-contamination, additives, non-polymer impurities and degradation.

[0017] One solution being explored to overcome the recycling issues with thermoplastic composites is to prepare composite assemblies comprising different parts / layers made out of the same thermoplastic material in order to allow a successful recycling process. One thermoplastic material being used in this regard is polyether sulfone (PESU). PESU has a desirable combination of properties, being lightweight, stiff and strong, highly temperature resistant and intrinsically flame retardant. These properties make them suitable for complex-shaped components in cars, airplanes and trains. In particular, PESU foams are suitable core materials for structural composites as they are stiff and strong and have excellent dimensional stability at high temperatures. Therefore, structural composites prepared with a PESU foam core and a laminate layer or layers also prepared with PESU would have the combination of desirable performance properties as well as recyclability.

[0018] However, there is considerable difficulty in preparing such all-PESU composite constructions. Since the materials have the same Tg, heat lamination of the PESU laminate layers to the foam is difficult. Because the materials have almost the same Tg, heating the laminate layers to a temperature above the Tg of the PESU material in order to laminate it to the PESU foam can alter or destroy the foam. Other methods of adhering the PESU laminate layers to the PESU foam are utilized such as adhesive bonding or mechanical attachment (with for example screws), render the composite not all PESU and therefore diminish the recyclability.

[0019] In this disclosure, a hot melt adhesive has been developed that is PESU -based and blended with a polyether polyol material. The blend has a Tg that is significantly lower than the Tg of the PESU material by itself and thus the hot melt adhesive can be applied to PESU foams or laminate layers without causing adverse effects in the PESU foams or laminate layers. The PESU-based hot melt adhesive forms strong adhesive bonds to the other PESU materials.Additionally disclosed herein are composites prepared with the PESU-based hot melt adhesives. The composites comprise PESU layers (such as foam layers and / or laminate layers) bonded by the PESU-based hot melt adhesives. While not wishing to be bound by theory, because the polyether polyol materials added to the PESU-based hot melt adhesives are of a relatively low molecular weight, when the composite is to be recycled by heating to a temperature to melt the composite, the relatively low molecular weight polyether polyol material will vaporize and be removed from the composite. In this way, the recycled PESU is suitable for repurposing.

[0020] The term “adhesive” as used herein refers to polymeric compositions useful to adhere together two adherends. Examples of adhesives are hot melt adhesives.

[0021] Hot melt adhesives are thermoplastic materials that are solid and non-tacky at room temperature but upon heating melt and flow. The hot melt adhesive is applied in the molten state and forms a bond upon cooling to a solid state.

[0022] The terms "room temperature" and "ambient temperature" are used interchangeably to mean temperatures in the range of 20°C to 25°C.

[0023] The terms “Tg” and “glass transition temperature” are used interchangeably. If measured, Tg values are determined by Differential Scanning Calorimetry (DSC) as described in the Examples section.

[0024] The term “adjacent” as used herein when referring to two layers means that the two layers are in proximity with one another with no intervening open space between them. They may be in direct contact with one another (e.g. laminated together) or there may be intervening layers.

[0025] The terms “polymer” and “macromolecule” are used herein consistent with their common usage in chemistry. Polymers and macromolecules are composed of many repeated subunits. As used herein, the term “macromolecule” is used to describe a group attached to a monomer that has multiple repeating units. The term “polymer” is used to describe the resultant material formed from a polymerization reaction.

[0026] The term “alkyl” refers to a monovalent group that is a radical of an alkane, which is a saturated hydrocarbon. The alkyl can be linear, branched, cyclic, or combinations thereof and typically has 1 to 20 carbon atoms. In some embodiments, the alkyl group contains 1 to 18, 1 to 12, 1 to 10, 1 to 8, 1 to 6, or 1 to 4 carbon atoms. Examples of alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, n-hexyl, cyclohexyl, n-heptyl, n-octyl, and ethylhexyl.

[0027] The term “aryl” refers to a monovalent group that is aromatic and carbocyclic. The aryl can have one to five rings that are connected to or fused to the aromatic ring. The other ring structures can be aromatic, non-aromatic, or combinations thereof. Examples of aryl groups include, but are not limited to, phenyl, biphenyl, terphenyl, anthryl, naphthyl, acenaphthyl, anthraquinonyl, phenanthryl, anthracenyl, pyrenyl, perylenyl, and fluorenyl.

[0028] The term “alkylene” refers to a divalent group that is a radical of an alkane. The alkylene can be straight-chained, branched, cyclic, or combinations thereof. The alkylene often has 1 to 20 carbon atoms. In some embodiments, the alkylene contains 1 to 18, 1 to 12, 1 to 10, 1 to 8, 1 to 6, or 1 to 4 carbonatoms. The radical centers of the alkylene can be on the same carbon atom (i.e., an alkylidene) or on different carbon atoms.

[0029] The term “arylene” refers to a divalent group that is carbocyclic and aromatic. The group has one to five rings that are connected, fused, or combinations thereof. The other rings can be aromatic, nonaromatic, or combinations thereof. In some embodiments, the arylene group has up to 5 rings, up to 4 rings, up to 3 rings, up to 2 rings, or one aromatic ring. For example, the arylene group can be phenylene.

[0030] The term “polyether” refers to a divalent heteroalkylene group that includes at least an alkylene group connected to an oxy group. The heteroalkylene can be linear, branched, cyclic, substituted with alkyl groups, or combinations thereof. Polyethers are also often described as poloxyyalkylenes where the heteroatom is oxygen such as for example the group: -(OCH2CH2)n-. Polyether polyols are polyether groups terminated by alcohol (-OH) groups such as H-(OCH2CH2)n-OH.

[0031] Disclosed herein are hot melt adhesives that are polymeric blends. In some embodiments, the polymeric blend comprises at least one thermoplastic polyether sulfone material and at least one polyether polyol material. The polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) that is less than the Tg of the at least one thermoplastic polyether sulfone material. The polymeric blend is capable of hot melt bonding two substrates comprising thermoplastic polyether sulfone materials.

[0032] In some embodiments, the at least one thermoplastic polyether sulfone material has a Tg as measured by DSC (Differential Scanning Calorimetry) of at least 200°C. In some embodiments, the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is below 150°C. In other embodiments, the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is in the range of 120-150°C. In yet other embodiments, the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is below 120°C.

[0033] The currently disclosed hot melt adhesives comprise at least one thermoplastic polyether sulfone material. I wide range of polyether sulfone (PESU) materials are suitable for use in the polymeric blends of the hot melt adhesives of this disclosure. Known for its exceptional mechanical properties, thermal stability, and chemical resistance, PESU has become indispensable in industries ranging from aerospace and automotive to medical and electronics. PESU is amorphous, meaning it lacks a crystalline structure, which contributes to its transparency and high dimensional stability. They are composed of para-linked aromatics, sulfonyl groups and ether groups. PESU materials typically have the general repeating unit structure:

[0034]

[0035] PESU materials are commercially available from a wide range of suppliers. Examples of suitable materials are those available from BASF AMERICA Houston, TX under the trade name ULTRASON. Examples include ULTRASON E 1010, ULTRASON E 2010, ULTRASON E 1010 NAT, and ULTRASON E 2020. ULTRASON E 1010 NAT is particularly suitable.

[0036] Besides the PESU materials described above other sulfone materials may also be suitable. Examples include PAS (polyarylenesulfone), PSF (polyphenylsulfone), PES (polyethersulfone), PPSU (polyphenylenesulfone), and PSU (polysulfone).

[0037] The currently disclosed hot melt adhesive blends comprise at least one polyether polyol material. A wide range of polyether polyols are suitable. In some embodiments, the at least one polyether polyol material comprises a polyether polyol of general Formula 1 :

[0038] H-(O-(-CH2-)m)„-OH

[0039] Formula 1

[0040] where m is an integer of 2 or greater; and n is an integer of 1 or greater.

[0041] In some embodiments, the polyether polyol material comprises a polyethylene glycol of general Formula 2:

[0042] H-(O-CH2CH2-)n-OH

[0043] Formula 2

[0044] wherein n is an integer of 1 or greater.

[0045] A wide range of polyethylene glycols are commercially available. Examples include those available from Dow Chemical Midland, MI under the trade name CARBOWAX, such as CARBOWAX 300, CARBOWAX 400, CARBOWAX 600, CARBOWAX 1000; and those available under the trade name POLYGLYKOL such as POLYGLYKOL 200, POLYGLYKOL 200 LVC, POLYGLYKOL 300, and POLYGLYKOL 400 from Clariant Louisville, KY. Particularly suitable is POLYGLYKOL 200 LVC.

[0046] A wide range of compositions of the polymeric blends are suitable. The PESU is present as the major component, meaning that it is present in an amount of greater than 50% by weight based on 100 weight % of the blend. More typically, the polymeric blend comprises:

[0047] 80-95 weight % of at least one thermoplastic polyether sulfone material; and

[0048] 5-20 weight % of at least poly ether polyol material, where weight % is based upon 100 weight % of the blend.

[0049] In some embodiments, the at least one PESU is present in an amount of 83-93 weight %, or 85-90 weight %. In some embodiments, the poly ether polyol is present in an amount of at least 81, 82, 83, 84, 85, 86, 87,88, 89, 90, 91, 92, 93 or 94 weight % and no more than 94, 93, 92, 91, 90, 89, 88, 87, 86, 85, 84, 83, 82, or 81 weight %.

[0050] In some embodiments, the at least one polyether polyol is present in an amount of 8-17 weight %, or 10-15 weight %. In some embodiments, the polyether polyol is present in an amount of at least 6, 7, 8, 9, 10, 11, 12,13, or 14 weight % and no more than 14, 13, 12, 11, 10, 9, 8, 7, or 6 weight %.A variety of methods can be used to prepare the hot melt adhesives of this disclosure. Typically, the hot melt adhesives are prepared by melt blending of the PESU and the polyether polyol. Hot melt blending is often carried out in an extmder. Typically, the PESU is hot melt bended in an extruder and the polyether polyol is fed into the extruder to prepare the blend. The blend prepared in the hot melt mixing apparatus is an intimately mixed blend. In some embodiments, the polyether polyol is a liquid, in other embodiments the poly ether polyol is a solid at room temperature.

[0051] Also disclosed herein are multi-layer articles. In some embodiments, the multi-layer article comprises a core layer comprising at least one thermoplastic polyether sulfone material, an adhesive layer comprising a thermoplastic polyether sulfone-based hot melt adhesive, and a skin layer comprising at least one thermoplastic polyether sulfone material, and at least one reinforcing fabric. The hot melt adhesive comprises a polymeric blend comprising at least one thermoplastic polyether sulfone material and at least one polyether polyol material. The polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) that is less than the Tg of the at least one thermoplastic polyether sulfone material. Suitable hot melt adhesive blends are described in detail above.

[0052] The multi-layer articles have a core layer. The core layer comprises at least one thermoplastic polyether sulfone (PESU) material. In some embodiments, the core layer comprises a single PESU material, in other embodiments the core layer comprises a mixture of PESU materials. PESU materials are described in detail above.

[0053] In some embodiments, the core layer comprises a foam layer or a honeycomb layer. Particularly suitable for the PESU core layers are the foam core layers commercially available from Diab Group Helsingborg, Sweden under the trade name DIVINYLCELL F, including DIVINYLCELL F40, DIVINYLCELL F50, DIVINYLCELL F90, DIVINYLCELL F130. Particularly suitable is the PESU foam core DIVINYLCELL F40.

[0054] The multi-layer articles also comprise a PESU -based hot melt adhesive that comprises a polymeric blend of PESU and polyether polyol. In some embodiments, the at least one thermoplastic poly ether sulfone material of the hot melt adhesive has a Tg as measured by DSC (Differential Scanning Calorimetry) of at least 200°C. In some embodiments, the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is below 150°C. In other embodiments, the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is in the range of 120-150°C. In yet other embodiments, the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is below 120°C.

[0055] The PESU-based hot melt adhesives have been described in detail above. A wide range of polyether sulfone (PESU) materials are suitable for use in the polymeric blends of the hot melt adhesives of this disclosure. Examples of suitable materials are those available from BASF AMERICA Houston, TX under the trade name ULTRASON. Examples include ULTRASON E 1010, ULTRASON E 2010, ULTRASON E 1010 NAT, and ULTRASON E 2020. ULTRASON E 1010 NAT is particularly suitable.The hot melt adhesives comprise at least one polyether polyol material. A wide range of polyether polyols are suitable. In some embodiments, the polyether polyol material comprises a polyethylene glycol of general Formula 2:

[0056] H-(O-CH2CH2-)„-OH

[0057] Formula 2

[0058] wherein n is an integer of 1 or greater.

[0059] Examples of suitable polyether polyols include those available from Dow Chemical Midland, MI under the trade name CARBOWAX, such as CARBOWAX 300, CARBOWAX 400, CARBOWAX 600, CARBOWAX 1000; and those available under the trade name POLYGLYKOL such as POLYGLYKOL 200, POLYGLYKOL 200 LVC, POLYGLYKOL 300, and POLYGLYKOL 400 from Clariant Louisville, KY. Particularly suitable is POLYGLYKOL 200 LVC.

[0060] A wide range of compositions of the polymeric blends are suitable. In some embodiments, the polymeric blend comprises 80-95 weight % of at least one thermoplastic polyether sulfone material, and 5-20 weight % of at least poly ether polyol material, where weight % is based upon 100 weight % of the blend.

[0061] The multi-layer articles also comprise a skin layer. The skin layer comprises a PESU material and a reinforcing fabric. Suitable PESU materials include the materials described above as suitable for the hot melt adhesive polymeric blend. The PESU material may be the same as used in the core layer, the hot melt adhesive layer, or both, or it may be different from the materials used in these layers. A wide variety of reinforcing fabrics are suitable. In some embodiments, the reinforcing fabric comprises a glass fiber reinforcing web or a CFRP (Carbon Fiber Reinforced Polymer) web. Glass fiber reinforcing webs are particularly suitable.

[0062] The layers of the multi-layer articles of this disclosure can have a variety of thicknesses. In some embodiments the article comprises: a core layer with a thickness of 100-6000 micrometers; an adhesive layer with a thickness of 10-200 micrometers; and a skin layer with a thickness of 25-400 micrometers.

[0063] Depending upon the desired use for the multi-layer articles of this disclosure, the articles may contain additional layers. For example, if the multi-layer articles are to be used in airplane cabin interiors, it may be desirable to have articles with skin layers on both exterior surfaces of the composite construction. For example, it may be desirable to prepare a 5-layer construction comprising: skin layer / adhesive layer / foam core / adhesive layer / skin layer.

[0064] A variety of methods can be used to prepare the multi-layer articles of this disclosure. In some embodiments, the article is formed by hot melt coating the adhesive layer onto the core layer and laminating the skin layer to the hot melt coated adhesive layer. In other embodiments, the article is formed by preparing an assembly comprising the core layer and the adhesive layer, heat pressing the assembly, and laminating the skin layer to the adhesive layer.

[0065] The articles of this disclosure may be more fully understood by the Figures. Figures 2-5 are DSC thermograms that are discussed in the Examples section below. Figure 1 shows a cross-sectional view ofarticle 100 which is a multi-layer article comprising Foam Core layer 110, Hot Melt Adhesive layers 120, and Skin Layers 130. Each of these layers is described in detail above.

[0066] Examples

[0067] These examples are merely for illustrative purposes only and are not meant to be limiting on the scope of the appended claims. All parts, percentages, ratios, etc. in the examples and the rest of the specification are by weight, unless noted otherwise. The following abbreviations are used: cm = centimeters; mm = millimeters; kg = kilograms; min = minutes; h = hours; K = Kelvin, and N = Newtons. The terms “weight %”, “%by weight”, and “wt%” are used interchangeably.

[0068] Table of Abbreviations

[0069] Abbreviation or Description

[0070] Trade

[0071] Designation

[0072] PESU Polyethersulfone with a Tg: ~ 236°C, available as ULTRASON E-1010 NAT from BASF AMERICA, Houston, TX

[0073] PEG Polyethylene glycol, commercially available as POLYGLYKOL 200 LVC from Clariant, Louisville, KY

[0074] PESU Foam Polyethersulfone Foam with a density of 40 g / L and a Tg of ~ 232°C,

[0075] available as DIVINYLCELL F40 from Diab Group Helsingborg, Sweden Skin Layer Polyethersulfone-based glass fiber reinforced fabric, available from Toray,

[0076]

[0077] Tokyo, Japan

[0078] Test Methods

[0079] Climbing Drum Peel

[0080] Climbing Drum Peel was tested according to EN 2243-3. The test panel was designed according to Figure 1 with Skin Layer (130) measuring 30 x 7.5 x 0.016 cm attached to a PESU Foam (110) measuring 30 x 7.5 x 1.1 cm by means of an approximately 100 micrometer thick PESU Hot Melt layer (120) as described herein. Excess hot melt adhesive at the edges of the specimens, was removed with sandpaper. Two samples were tested and the average value, including the standard deviation were reported. The test was conducted at a rate of 25 mm / minute at ambient temperature.

[0081] Differential Scanning Calorimetry (DSC)

[0082] A DSC 214 Polyma from Netzsch was used to measure the DSC profile. The resulting thermograms are shown as Figures 2-5. The DSC thermograms show the second heating cycle, the scan that was used throughout to determine the Tg. Figure 2 is pure PESU, Figure 3 is the PESU foam, Figure 4 is the Skin Layer, and Figure 5 is Example (described below). The DSC was conducted using the heat / cooling cycles shown in Table 1:Table 1: DSC parameters

[0083] Nr. °C K / min

[0084] 1 -70

[0085] 2 180 10

[0086] 3 -70 10

[0087] 4 -70

[0088] 5 400 30

[0089] 6 420

[0090] 7 20 50

[0091] 8 20

[0092]

[0093] The DSC results shown in Figures 2-5 can be summarized as follows:

[0094] Figure 2 (PESU): Tg is 236°C

[0095] Figure 3 (Foam Core): Tg is 232°C

[0096] Figure 4 (Skin Layer): Tg is 206°C

[0097] Figure 5 (Example 1): showed an obvious new appearing glass transition temperature at 115°C.

[0098] Example 1: Preparation of a Multi-layer article

[0099] Hot Melt Adhesive Formulation

[0100] A Hot Melt Adhesive Formulation was prepared according to the components of Table 2.

[0101] Table 2: PESU based Hot Melt Formulation.

[0102] Material Example 1

[0103] (wt%)

[0104] PESU 86.1

[0105] PEG 13.9

[0106]

[0107] SUM 100

[0108] Film Preparation

[0109] Film samples of the Formulation of Example 1 were produced using a 18 mm twin screw extruder with a L / D of 44. PESU pellets were added into the extruder at barrel 1, followed by injection of liquid PEG into barrel 2. The screw design is designed to provide homogeneous melting and mixing of both materials. Extruder barrels were heated to 230°C. A total extrusion rate of 3.8 kg / h was used. To produce a film (~ 100 micrometers) of PESU / PEG the polymer melt was cast onto a cast roll using a conventional extrusion slot die. Cast roll was heated to 90°C.

[0110] Multi-Layer Article Preparation

[0111] A multi-layer article was produced using a heat-press (210°C, 1 min). The upper- and bottom plate of the heat-press were adjusted so that minimal pressure was applied to the multi-layer article toavoid collapse of the PESU foam. The layers were arranged in the order: Skin Layer / Hot Melt Adhesive / Foam Core / Hot Melt Adhesive / Skin Layer.

[0112] Evaluation

[0113] To evaluate the bonding capabilities of the Hot Melt Adhesive of Example 1, two climbing drum peel specimens were manufactured and tested at ambient temperatures. Very good adhesion was found for Example 1 resulting in a split in the PESU foam as shown in Table 3 below.

[0114] Table 3: Evaluation of Example 1

[0115] Property / Method Example 1

[0116] (N) Mean (SD)

[0117] Climbing Dmm Peel at RT 61.5 (1.5)

[0118]

Claims

What is claimed is:

1. A hot melt adhesive comprising:a polymeric blend, wherein the blend comprises:at least one thermoplastic polyether sulfone material; andat least one polyether polyol material,wherein the polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) that is less than the Tg of the at least one thermoplastic polyether sulfone material, and wherein the polymeric blend is capable of hot melt bonding two substrates comprising thermoplastic poly ether sulfone materials.

2. The hot melt adhesive of claim 1, wherein the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is below 150°C.

3. The hot melt adhesive of claim 1, wherein the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is in the range of 120-150°C.

4. The hot melt adhesive of claim 1, wherein the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is below 120°C.

5. The hot melt adhesive of claim 1, wherein the at least one thermoplastic poly ether sulfone material has a Tg as measured by DSC (Differential Scanning Calorimetry) of at least 200°C.

6. The hot melt adhesive of claim 1, wherein the at least one poly ether polyol material comprises a poly ether polyol of general Formula 1 :H-(O-(-CH2-)m)„-OHFormula 1wherein m is an integer of 2 or greater; andn is an integer of 1 or greater.

7. The hot melt adhesive of claim 1, wherein the poly ether polyol material comprises a polyethylene glycol of general Formula 2:H-(O-CH2CH2-)„-OHFormula 2wherein n is an integer of 1 or greater.

8. The hot melt adhesive of claim 1, wherein the polymeric blend comprises:80-95 weight % of at least one thermoplastic polyether sulfone material; and5-20 weight % of at least poly ether polyol material, where weight % is based upon 100 weight % of the blend.

9. A multi-layer article comprising:a core layer comprising at least one thermoplastic polyether sulfone material;an adhesive layer comprising a thermoplastic polyether sulfone-based hot melt adhesive comprising a polymeric blend comprising:at least one thermoplastic polyether sulfone material; andat least one poly ether polyol material, wherein the polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) that is less than the Tg of the at least one thermoplastic polyether sulfone material; anda skin layer comprising at least one thermoplastic polyether sulfone material, and at least one reinforcing fabric.

10. The article of claim 9, wherein the core layer comprises a foam layer or a honeycomb layer.

11. The article of claim 9, wherein the reinforcing fabric comprises a glass fiber reinforcing web or a CFRP (Carbon Fiber Reinforced Polymer) web.

12. The article of claim 9, wherein hot melt adhesive polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) of below 150°C.

13. The article of claim 9, wherein the at least one thermoplastic polyether sulfone material has a Tg as measured by DSC (Differential Scanning Calorimetry) of at least 200°C.

14. The article of claim 9, wherein the polyether polyol material comprises a polyethylene glycol of general Formula 2:H-(O-CH2CH2-)„-OHFormula 2wherein n is an integer of 1 or greater.

15. The article of claim 9, wherein the polymeric blend comprises:80-95 weight % of at least one thermoplastic polyether sulfone material; and5-20 weight % of at least poly ether polyol material, where weight % is based upon 100 weight % of the blend.

16. The article of claim 9, wherein the article is formed by hot melt coating the adhesive layer onto the core layer and laminating the skin layer to the hot melt coated adhesive layer.

17. The article of claim 9, wherein the article is formed by preparing an assembly comprising the core layer and the adhesive layer, heat pressing the assembly, and laminating the skin layer to the adhesive layer.

18. The article of claim 9, wherein the article comprises:a core layer with a thickness of 100-6000 micrometers;an adhesive layer with a thickness of 10-200 micrometers; anda skin layer with a thickness of 25-400 micrometers.

19. The article of claim 9, further comprising additional layers such that the article comprises:a skin layer with a thickness of 25-400 micrometersan adhesive layer with a thickness of 10-200 micrometers;a core layer with a thickness of 100-6000 micrometers;an adhesive layer with a thickness of 10-200 micrometers; anda skin layer with a thickness of 25-400 micrometers.