Laminate constructions with polyether sulfone layers

A PESU-based laminate layer with a polyether polyol blend addresses the challenge of heat lamination to PESU foam by maintaining structural integrity and recyclability, achieving strong bonds and reduced weight in composite constructions.

WO2026234536A1PCT designated stage Publication Date: 2026-11-123M INNOVATIVE PROPERTIES CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2026/054359
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-05
Filing Date
2026-05-01
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

The challenge in recycling thermoplastic composites lies in the difficulty of heat lamination of laminate layers to a polyether sulfone (PESU) foam due to similar glass transition temperatures (Tg), which can alter or destroy the foam, and traditional adhesive or mechanical attachments compromise recyclability.

Method used

A PESU-based laminate layer comprising a blend of PESU and polyether polyol with a lower Tg than PESU, allowing heat bonding without damaging the foam, and optionally including glass bubbles to reduce weight, is used.

Benefits of technology

The solution enables strong adhesive bonds to PESU materials without additional adhesives, facilitating recyclability by vaporizing the low molecular weight polyether polyol during melting, resulting in lighter and thinner composite constructions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IB2026054359_12112026_PF_FP_ABST
    Figure IB2026054359_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Adhesive laminate layers are formed from polymeric blends and a fiber reinforcing fabric. The polymeric blends include at least one thermoplastic polyether sulfone material and at least one polyether polyol material. The polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) that is less than the Tg of the at least one thermoplastic polyether sulfone material. The adhesive laminate is capable of heat bonding to a substrate comprising thermoplastic polyether sulfone material. The adhesive laminate layers can be used in multi-layer articles.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] PA103149W002

[0002] LAMINATE CONSTRUCTIONS WITH POLYETHER SULFONE LAYERS

[0003] Summary

[0004] Disclosed herein are adhesive laminate layers prepared from polyether sulfones and multi5 layer articles prepared with these adhesive laminate layers. In some embodiments, the adhesive laminate layer comprises a polymeric blend and at least one fiber-reinforcing fabric. The polymeric blend comprises at least one thermoplastic polyether sulfone material and at least one polyether polyol material. The polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) that is less than the Tg of the at least one thermoplastic polyether sulfone material. The 0 adhesive laminate layer is capable of heat bonding to a substrate comprising thermoplastic polyether sulfone material.

[0005] Also disclosed are multi-layer articles. In some embodiments, the multi-layer article comprises a core layer comprising at least one thermoplastic polyether sulfone material and a laminate layer. The laminate layer comprises a thermoplastic polyether sulfone-based composition comprising a polymeric blend and at least one fiber-reinforcing fabric. The polymeric blend comprises at least one thermoplastic polyether sulfone material and at least one polyether polyol material. The polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) that is less than the Tg of the at least one thermoplastic polyether sulfone material. In some embodiments, the multi-layer article may comprise a second laminate layer on the surface of the core layer opposite the laminate layer.

[0006] Brief Description of the Drawings

[0007] The present application may be more completely understood in consideration of the following detailed description of various embodiments of the disclosure in connection with the 5 accompanying drawings.

[0008] Figure 1 is a cross-sectional view of a laminate article of this disclosure.

[0009] Figure 2 is a cross-sectional view of an article of this disclosure.

[0010] Figure 3 is a DSC thermogram of a polyethersulfone Foam Core Material used in this disclosure.

[0011] Figure 4 is a DSC thermogram of a polyethersulfone material used in this disclosure.

[0012] Figure 5 is a DSC thermogram of the Adhesive Laminate Composition of Example 1.

[0013] Figure 6 is a DSC thermogram of the Adhesive Laminate Composition of Example 2.

[0014] In the following description of the illustrated embodiments, reference is made to the accompanying drawings, in which is shown by way of illustration, various embodiments in which the 5 disclosure may be practiced.Detailed Description

[0015] Composite structures are used in a wide range of applications. A composite is a material which is produced from two or more constituent materials. These constituent materials have notably dissimilar chemical or physical properties and are merged to create a material with properties unlike the individual elements. Within the finished structure, the individual elements remain separate and distinct. Typical engineered composite materials include, for example, reinforced concrete, and composite sandwich structures containing fiber-reinforced polymer or fiberglass. Uses for composite sandwich structures include their use in aircraft manufacturing. While small parts can be manufactured via welding using hot Air Welders, Wedge Welders and Ultrasonic Welders, but for large surfaces, assembly typically involves the use of a heat press, a heat maintained vacuum bag or an autoclave.

[0016] A trend in the area of engineered composites is recyclability. As thermoplastics have become more important in the assembly of composites, it has become increasingly desirable for waste thermoplastic polymers to be recycled or reprocessed by a mechanical process using melt extrusion, injection, blowing, vacuum, and inflation molding. This method uses 100% utilization and conversion of waste plastic to produce the same or other valuable products. Thermoplastic materials are a type of polymer that becomes soft and moldable when heated (T > Tg), allowing them to be shaped into various forms. These polymers can be melted, molded, and reshaped multiple times without significant chemical changes, making them very versatile and cost-effective in recycling and reusability. The difficulty with thermoplastic composites is that the composites contain other materials and therefore are difficult to recycle and repurpose because the quality of the recycled materials is highly influenced by polymer cross-contamination, additives, non-polymer impurities and degradation.

[0017] One solution being explored being explored to overcome the recycling issues with thermoplastic composites is to prepare composite assemblies comprising different arts / 1 avers made out of the same thermoplastic material in order to allow a successful recycling process. One thermoplastic material being used in this regard is polyether sulfone (PESU). PESU has a desirable combination of properties, being lightweight, stiff and strong, highly temperature resistant and intrinsically flame retardant. These properties may them suitable for complex-shaped components in cars, airplanes and trains. In particular, PESU foams are suitable core materials for structural composites as they are stiff and strong and have excellent dimensional stability at high temperatures. Therefore, structural composites prepared with a PESU foam core and a laminate layer or layers also prepared with PESU would have the combination of desirable performance properties as well as recyclability.However, there is considerable difficulty in preparing such all-PESU composite constructions. Since the materials have the same Tg, heat lamination of the PESU laminate layers to the foam is difficult. Because the materials have the same Tg, heating the laminate layers to a temperature above the Tg of the PESU material in order to laminate it to the PESU foam can alter or destroy the foam. Other methods of adhering the PESU laminate layers to the PESU foam are utilized such as adhesive bonding or mechanical attachment (with for example screws), render the composite not all PESU and therefore diminish the recyclability.

[0018] Another goal of composite constructions is to minimize the weight of the laminate constructions. This is particularly important in the transportation industry, where minimizing the weight can aid in fuel economy, speed, and efficiency in the vehicle. In a related disclosure filed on the same day as the current disclosure with Attorney Docket No. PA102920US01 titled “POLYETHER SULFONE HOT MELT ADHESIVE BLEND” a hot melt adhesive is disclosed that is PESU-based and blended with polyether polyol material.

[0019] In this disclosure, a laminate layer is described that is PESU-based and comprises a blend of a PESU material and a polyether polyol. The blend has a Tg that is significantly lower than the Tg of the PESU material by itself and thus the laminate layer can be applied to PESU foams or laminate layers without causing adverse effects in the PESU materials of those foams or layers. The PESU-based laminate layer forms strong adhesive bonds to the other PESU materials without the need for an additional adhesive layer. The PESU-based laminate layer also comprises a reinforcing fabric and, in some embodiments, further comprises glass bubbles to reduce the weight of the layer.

[0020] Additionally disclosed herein are composite constructions prepared with the PESU-based laminate layers. The composites comprise PESU layers (such as foam layers and / or laminate layers) bonded by the PESU-based laminate layers. While not wishing to be bound by theory, because the polyether polyol materials added to the PESU-based polymeric blends of the laminate layers are of a relatively low molecular weight, when the composite is to be recycled by heating to a temperature to melt the composite, the relatively low molecular weight polyether polyol material will vaporize and be removed from the composite. In this way, the recycled PESU is suitable for repurposing.

[0021] The term “adhesive” as used herein refers to polymeric compositions useful to adhere together two adherends. Examples of adhesives are hot melt adhesives.

[0022] Hot melt adhesives are thermoplastic materials that are solid and non-tacky at room temperature but upon heating melt and flow. The hot melt adhesive is applied in the molten state and forms a bond upon cooling to a solid state.

[0023] As used herein the term “adhesive laminate layer” and “laminate layer” are used interchangeably and refer to a laminate layer that is capable of heat bonding to a substrate.The terms "room temperature" and "ambient temperature" are used interchangeably to mean temperatures in the range of 20°C to 25°C.

[0024] The terms “Tg” and “glass transition temperature” are used interchangeably. If measured, Tg values are determined by Differential Scanning Calorimetry (DSC) as described in the Examples section.

[0025] The term “adjacent” as used herein when referring to two layers means that the two layers are in proximity with one another with no intervening open space between them. They may be in direct contact with one another (e.g. laminated together) or there may be intervening layers.

[0026] The terms “polymer” and “macromolecule” are used herein consistent with their common usage in chemistry. Polymers and macromolecules are composed of many repeated subunits. As used herein, the term “macromolecule” is used to describe a group attached to a monomer that has multiple repeating units. The term “polymer” is used to describe the resultant material formed from a polymerization reaction.

[0027] The term “polyether” refers to a divalent heteroalkylene group that includes at least an alkylene group connected to an oxy group. The heteroalkylene can be linear, branched, cyclic, substituted with alkyl groups, or combinations thereof. Polyethers are also often described as poloxyyalkylenes where the heteroatom is oxygen such as for example,

[0028] -(OCH2CH2)n-. Polyether polyols are polyether groups terminated by alcohol (-OH) groups such as H-(OCH2CH2)n-OH.

[0029] Disclosed herein are laminate layers that are polymeric blends and reinforcing fabrics. In some embodiments, the polymeric blend comprises at least one thermoplastic polyether sulfone material and at least one polyether polyol material. The polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) that is less than the Tg of the at least one thermoplastic polyether sulfone material. The polymeric blend is capable of heat bonding two substrates comprising thermoplastic polyether sulfone materials. The reinforcing fabric of the laminate layers can be a glass fiber web or a CFRP (Carbon Fiber Reinforced Polymer) web.

[0030] In some embodiments, the at least one thermoplastic polyether sulfone material has a Tg as measured by DSC (Differential Scanning Calorimetry) of at least 200°C. In some embodiments, the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is below 150°C. In other embodiments, the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is in the range of 120-150°C. In yet other embodiments, the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is below 120°C.

[0031] The currently disclosed polymeric blends comprise at least one thermoplastic polyether sulfone material. A wide range of polyether sulfone (PESU) materials are suitable for use in the polymeric blends of this disclosure. Known for its exceptional mechanical properties, thermalstability, and chemical resistance, PESU has become indispensable in industries ranging from aerospace and automotive to medical and electronics. PESU is amorphous, meaning it lacks a crystalline structure, which contributes to its transparency and high dimensional stability. They are composed of para-linked aromatics, sulfonyl groups and ether groups. PESU materials typically have the general repeating unit structure:

[0032]

[0033] PESU materials are commercially available from a wide range of suppliers. Examples of suitable materials are those available from BASF AMERICA Houston, TX under the trade name ULTRASON. Examples include ULTRASON E 1010, ULTRASON E 2010, and ULTRASON E 2020. ULTRASON E 1010 NAT is particularly suitable.

[0034] Besides the PESU materials described above other sulfone materials may also be suitable. Examples include PAS (polyarylenesulfone), PSF (polyphenylsulfone), PES (polyethersulfone), PPSU (polyphenylenesulfone), and PSU (poly sulfone).

[0035] The currently disclosed polymeric blends comprise at least one polyether polyol material. A wide range of polyether polyols are suitable. In some embodiments, the at least one polyether polyol material comprises a polyether polyol of general Formula 1 :

[0036] H-(0-(-CH2-)m)n-0H

[0037] Formula 1

[0038] where m is an integer of 2 or greater; and n is an integer of 1 or greater.

[0039] In some embodiments, the polyether polyol material comprises a polyethylene glycol of general Formula 2:

[0040] H-(O-CH2CH2-)n-OH

[0041] Formula 2

[0042] wherein n is an integer of 1 or greater.

[0043] A wide range of polyethylene glycols are commercially available. Examples include those available from Dow Chemical Midland, MI under the trade name CARBOWAX, such as CARBOWAX 300, CARBOWAX 400, CARBOWAX 600, CARBOWAX 1000; and those available under the trade name POLYGLYKOL such as POLYGLYKOL 200, POLYGLYKOL 200 LVC, POLYGLYKOL 300, and POLYGLYKOL 400 from Clariant Louisville, KY. Particularly suitable is POLYGLYKOL 200 LVC.A wide range of compositions of the polymeric blends are suitable. The PESU is present as the major component, meaning that it is present in an amount of greater than 50% by weight based on 100 weight % of the blend. More typically, the polymeric blend comprises:

[0044] 70-95 weight % of at least one thermoplastic polyether sulfone material; and

[0045] 5-30 weight % of at least polyether polyol material, where weight % is based upon 100 weight % of the blend.

[0046] In some embodiments, the at least one PESU is present in an amount of 75-90 weight %, or 85-90 weight %,. In some embodiments, the polyether polyol is present in an amount of at least 71, 72, 73, 74, 75, 76, 77, 78, 79, 80 81, 82, 83, 84, 85, 86, 87,88, 89, 90, 91, 92, 93 or 94 weight % and no more than 94, 93, 92, 91, 90, 89, 88, 87, 86, 85, 84, 83, 82, 81, 80, 79, 78, 77, 76, 75, 74, 73, 72, or 71 weight %.

[0047] In some embodiments, the at least one polyether polyol is present in an amount of 8-25 weight %, or 10-15 weight %,. In some embodiments, the polyether polyol is present in an amount of at least 6, 7, 8, 9, 10, 11, 12,13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, or 29 weight % and no more than 29, 28, 27, 26, 25, 24, 23, 22, 21, 20, 19, 18, 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, or 6 weight %.

[0048] In some embodiments, the polymeric blend further comprises glass bubbles. Glass bubbles are hollow glass spheres. The addition of glass bubbles to the polymeric blend can decrease the weight of the polymeric blend by decreasing the density of the adhesive blend. In some embodiments, the adhesive blend has a density of less than or equal to 1.0 g / cm3. A wide range of glass bubbles are suitable. In some embodiments, the glass bubbles comprise hollow borosilicate glass bubbles with a true density of from 0.1-0.8 g / cm3. Examples of suitable glass bubbles include XLD3000 glass bubbles, S32HS glass bubbles, and S28HS glass bubbles from 3M Company, St. Paul, MN. The S32HS glass bubbles are particularly suitable and have a density of 0.32 g / cm3. In some embodiments, the polymeric blend 0-50 parts by weight of the glass bubbles per 100 parts by weight of the other blend components. Often the term phr (parts per hundred resin) is used to describe this, where the amount of the additive (in this case glass bubbles) is described in terms of parts by weight per 100 parts by weight of other components in the mixture (in this case the PESU and the polyether polyol). For example, 20 phr of glass bubbles would describe a composition with 20 parts per weight of glass beads added to a composition with 80 parts by weight of PESU and 20 parts by weight of polyether polyol. The amount of glass bubbles can also be calculated as weight %, where the weight % of glass bubbles is based upon 100 weight % of the total polymeric blend (i.e. the sum of PESU, polyether polyol, and glass bubbles). In some embodiments, the glass bubbles comprise 5-20 weight % based upon 100 weight % of the total polymeric blend.The laminating layer further comprises a reinforcing fabric. A wide range of reinforcing fabrics are suitable. In some embodiments, the reinforcing fabric comprises a glass fiber reinforcing web or a CFRP (Carbon Fiber Reinforced Polymer) web. Particularly suitable is the glass fiber fabric HEXFORCE 7781 from Hexcel Corporation, Stamford, CT.

[0049] A variety of methods can be used to prepare the laminate layers of this disclosure. Generally, the polymeric blend is prepared as described below and layers of the polymeric blend are formed. The reinforcing fabric is disposed between layers of the polymeric blend to form a construction, and the laminate layer is formed by heat pressing the construction to form a composite layer. The fabric layer embeds within the polymeric blend layers.

[0050] Typically, the polymeric blends are prepared by melt blending of the PESU and the polyether polyol. Hot melt blending is often carried out in an extruder. Typically, the PESU is hot melt bended in an extruder and the polyether polyol is fed into the extruder to prepare the blend. If used, glass bubbles can be added to the hot melt mixer. The blend prepared in the hot melt mixing apparatus is an intimately mixed blend. In some embodiments, the polyether polyol is a liquid, in other embodiments the polyether polyol is a solid at room temperature.

[0051] The adhesive laminate layer thus formed can have a wide range of thicknesses. The laminate thickness can be selected for suitability for use in preparing multi-layer articles as described below. In some embodiments, the adhesive laminate layer has a thickness of from 50-500 micrometers.

[0052] Also disclosed herein are multi-layer articles. In some embodiments, the multi-layer article comprises a core layer comprising at least one thermoplastic polyether sulfone material, and a laminate layer comprising a polymeric blend and at least one reinforcing fabric. The polymeric blend comprises at least one thermoplastic polyether sulfone material and at least one polyether polyol material and may optionally include glass bubbles. The polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) that is less than the Tg of the at least one thermoplastic polyether sulfone material. Suitable polymeric blends, reinforcing fabrics, and glass bubbles are described in detail above.

[0053] The multi-layer articles have a core layer. The core layer comprises at least one thermoplastic polyether sulfone (PESU) material. In some embodiments, the core layer comprises a single PESU material, in other embodiments the core layer comprises a mixture of PESU materials. PESU materials and described in detail above.

[0054] In some embodiments, the core layer comprises a foam layer or a honeycomb layer. Particularly suitable for the PESU core layers are the foam core layers commercially available from Diab Group Helsingborg, Sweden under the trade name DIVINYLCELL F, including DIVINYLCELL F40, DIVINYLCELL F50, DIVINYLCELL F90, DIVINYLCELL F130. Particularly suitable is the PESU foam core DIVINYLCELL F40.The multi-layer articles also comprise a PESU-based laminate layer that comprise a polymeric blend of PESU and polyether polyol and optionally include glass bubbles, and a reinforcing fabric. In some embodiments, the at least one thermoplastic polyether sulfone material of the polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) of at least 200°C. In some embodiments, the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is below 150°C. In other embodiments, the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is in the range of 120-150°C. In yet other embodiments, the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is below 120°C.

[0055] The PESU-based polymeric blends have been described in detail above. A wide range of polyether sulfone (PESU) materials are suitable for use in the polymeric blends of this disclosure. Examples of suitable materials are those available from BASF AMERICA Houston, TX under the trade name ULTRASON. Examples include ULTRASON E 1010, ULTRASON E 2010, and ULTRASON E 2020. ULTRASON E 1010 NAT is particularly suitable.

[0056] The polymeric blends comprise at least one polyether polyol material. A wide range of polyether polyols are suitable. In some embodiments, the polyether polyol material comprises a polyethylene glycol of general Formula 2:

[0057] H-(O-CH2CH2-)n-OH

[0058] Formula 2

[0059] wherein n is an integer of 1 or greater.

[0060] Examples of suitable polyether polyols include those available from Dow Chemical Midland, MI under the trade name CARBOWAX, such as CARBOWAX 300, CARBOWAX 400, CARBOWAX 600, CARBOWAX 1000; and those available under the trade name POLYGLYKOL such as POLYGLYKOL 200, POLYGLYKOL 300, and POLYGLYKOL 400 from Clariant Louisville, KY. Particularly suitable is POLYGLYKOL 400.

[0061] A wide range of compositions of the polymeric blends are suitable. In some embodiments, the polymeric blend comprises 80-95 weight % of at least one thermoplastic polyether sulfone material, and 5-20 weight % of at least polyether polyol material, where weight % is based upon 100 weight % of the blend.

[0062] As mentioned above, the polymeric blend may also comprise glass bubbles. Glass bubbles are advantageous in the polymeric blends to decrease the density of the polymeric blend and therefore to decrease the overall weight of the laminate layer. Suitable glass bubbles are described above and are added in the polymeric blend in an amount of 0-50 phr, or as described above, 0-50 parts by weight of glass bubbles per 100 parts by weight of the polymeric blendThe laminate layer articles also comprise a reinforcing fabric. A wide variety of reinforcing fabrics are suitable. In some embodiments, the reinforcing fabric comprises a glass fiber reinforcing web or a CFRP (Carbon Fiber Reinforced Polymer) web. Glass fiber reinforcing webs are particularly suitable.

[0063] The layers of the multi-layer articles of this disclosure can have a variety of thicknesses. In some embodiments the article comprises:

[0064] a core layer with a thickness of 100-6000 micrometers; and

[0065] a laminate layer with a thickness of 35-600 micrometers.

[0066] As mentioned above, an advantage of the current laminate layers and articles formed from them is that the laminate layers are heat-bondable, meaning that upon the application of heat and optionally pressure, the laminate layer adheres to the core layer at a temperature that does not adversely affect the core layer. Also, because there is no need for a separate adhesive layer to adhere the core layer to the laminate layer, the formed articles can be thinner and lighter than if such am adhesive layer was necessary. Additionally, the inclusion of glass bubbles decreases the density of the laminate layer and thus can further decrease the weight of the multi-layer articles.

[0067] Typically, the multi-layer articles of this disclosure are prepared by preparing the laminate article as described above and disposing the laminate article on a core layer to form a construction and heat pressing the construction to form the multi-layer article. Typically the laminate articles are disposed on both major surfaces of the core layer. The laminate article can be heat pressed to the core layer at a temperature below the Tg of the core layer because the polymeric blend of the laminate layer has a Tg that is well below that of the core layer, even though both layers are PESU-based. As mentioned above, an advantage of the layers of the multi-layer article being PESU-based is that such articles have increased recyclability.

[0068] a laminate layer with a thickness of 35-600 micrometers;

[0069] a core layer with a thickness of 100-6000 micrometers; and

[0070] a second laminate layer with a thickness of 35-600 micrometers.

[0071] The articles of this disclosure may be more fully understood by the Figures. Figures 3-6 are DSC thermograms that are discussed in the Examples section below. Figure 1 shows a cross-sectional view of laminate article 100 which is a composite layer comprising Reinforcing Fabric Layer 130, and Adhesive Laminate layers 120. Each of these layers is described in detail above. It should be understood that while the layers are shown as separate layers, layer 130 embeds within the layers 120.

[0072] Figure 2 shows the final article 200 comprising Foam Core 210, and Composite Layers 100, where Composite Layers 100 comprise sublayers 130 (Reinforcing Fabric Layer) and 120 (Adhesive Laminate layers) as described in Figure 1.Examples

[0073] These examples are merely for illustrative purposes only and are not meant to be limiting on the scope of the appended claims. All parts, percentages, ratios, etc. in the examples and the rest of the specification are by weight, unless noted otherwise. The following abbreviations are used; m = meters; cm = centimeters; mm = millimeters; g = grams; kg = kilograms; min = minutes; h = hours; K = Kelvin, N = Newtons; and kN = kiloNewtons. The terms “weight %”, “% by weight”, and “wt%” are used interchangeably.

[0074] Table of Abbreviations

[0075] Abbreviation or Description

[0076] Trade

[0077] Designation

[0078] PESU Polyethersulfone with a Tg: ~ 236°C, available as ULTRASON E-1010 NAT from BASF AMERICA, Houston, TX

[0079] PEG Polyethylene glycol, commercially available as POLYGLYKOL 200 LVC from Clariant, Louisville, KY

[0080] PESU Foam Polyethersulfone Foam with a density of 40 / g / L and a Tg of ~ 232°C,

[0081] available as DIVINYLCELL F40 from Diab Group Helsingborg, Sweden Fabric Glass fiber Fabric, 8H Satin, 299 g / m2; 0.22 mm thickness from Hexcel,

[0082] Stamford, CT.

[0083] GB Hollow glass bubbles; 0.32 g / cm3available from 3M Company, St. Paul,

[0084]

[0085] MN as GLASS BUBBLES32HS

[0086] Test Methods

[0087] Climbing Drum Peel

[0088] Climbing Drum Peel was tested according to EN 2243-3. The test panel was designed according to Figure 2 by laminating a Laminate article of Figure 1 (Adhesive Laminate Layer / Fabric / Adhesive Laminate Layer) of 30 x 7.5 x 0.015-0.035 cm to a PESU Foam Core measuring 30 x 7.5 x 1.1 cm. The Final Article has a thickness of approximately 1.2 cm. Excess material at the edges of the specimens, was removed with a knife. Samples were tested and the value was reported. The test was conducted at a rate of 25 mm / minute at ambient temperature. Results are reported in Newtons (N).

[0089] Differential Scanning Calorimetry (DSC)

[0090] A DSC 214 Polyma from Netzsch was used to measure the DSC profile. The resulting thermograms are shown as Figures 3-6. The DSC thermograms show the second heating cycle, thescan that was used throughout to determine the Tg. Figure 3 is the PESU foam, Figure 4 is pure PESU, Figure 5 is Example 1 (described below), and Figure 6 is Example 2 (described below). The DSC was conducted using the heat / cooling cycles shown in Table 1:

[0091] Table 1: DSC parameters

[0092] Nr. °C K / min

[0093] 1 -70

[0094] 2 180 10

[0095] 3 -70 10

[0096] 4 -70

[0097] 5 400 30

[0098] 6 420

[0099] 7 20 50

[0100] 8 20

[0101]

[0102] The DSC results shown in Figures 3-6 can be summarized as follows:

[0103] Figure 3 (Foam Core PESU): Tg is 232°C

[0104] Figure 4 (PESU): Tg is 236°C

[0105] Figure 5 (Example 1): showed a significantly lower Tg of < 125°C

[0106] Figure 6 (Example 2): showed a significantly lower Tg of < 125°C

[0107] Weight / Density Calculation

[0108] Six specimens measuring 5 x 5 cm were cut from random parts of the fdms of Example 1 and 2. The thickness of each specimen was tested at three positions of the respective film by means of a digital thickness gauge (L&W Micrometer) and the mean was calculated. The weight of each specimen was measured using a fine balance and a mean was calculated per group. The Density was calculated using equation (1):

[0109] (1) D — Mean / (A * tMean)

[0110] D = Density in g / cm3

[0111] W = Weight in g

[0112] A = surface in cm2

[0113] t = thickness in cmExamples 1 and 2: Preparation of a Multi-layer article

[0114] Adhesive Laminate Formulations

[0115] Adhesive Laminate Formulations were prepared according to the components of Table 2.

[0116] Table 1: PESU based Adhesive Laminate Formulations.

[0117] Material Example 1 Example 2

[0118] (wt%) (wt%)

[0119] PESU 86.0 75.0

[0120] PEG 14.0 12.0

[0121] GB 0 13.0

[0122]

[0123] SUM 100 100

[0124] Film Preparation

[0125] Film samples of the Formulations of Examples 1 and 2 were produced using a 18 mm twin screw extruder with a L / D of 44. PESU pellets were added into the extruder at barrel 1, followed by injection of liquid PEG into barrel 2. GB were added through a side feeder at barrel 8. The screw design is designed to provide homogeneous melting and mixing of both materials. Extruder barrels were heated to 230°C. A total extrusion rate of 3.8 kg / h and 4.4 kg / h were used. To produce a film (70-150 micrometers) of PESU / PEG and PESU / PEG / GB respectively, the polymer melt was cast onto a casting roll using a conventional extrusion slot die. The casting roll was heated to 90°C.

[0126] Multi-Layer Article Preparation

[0127] A, Preparation of Laminate Article

[0128] A multi-layer laminate article as shown in Figure 1 was produced using a heat-press (190°C, 1 min, 10 kN). The layers were arranged in the order: Adhesive Laminate Layer / Fabric / Adhesive Laminate Layer, where the Adhesive Laminate Layer is one of those prepared above. The thickness of the Laminate Article was between 150-350 micrometers.

[0129] B, Preparation of Final Article

[0130] The multi-layer articles as shown in Figure 2 were prepared using a heat press (190°C, I min). The upper- and bottom plate of the heat-press were adjusted so that minimal pressure was applied to the multi-layer article to avoid collapse of the PESU foam. Adhesive Laminate Layers of two Laminate Articles were added to both sides of a Foam Core to give a final arrangement order: Adhesive Laminate Layer / Fabric / Adhesive Laminate Layer / Foam Core / Adhesive Laminate Layer / Fabric / Adhesive Laminate Layer, where the Adhesive Laminate Layers are one of those prepared above. The thickness of the final articles was about 1.2 cm.Evaluation

[0131] A, Climbing Drum Peel

[0132] To evaluate the bonding capabilities of the Adhesive Laminate Layer of Example 1 and 2, a climbing drum peel specimen of each was manufactured and tested at ambient temperatures. Very good adhesion was found for Examples 1 and 2 resulting in a split in the PESU foam as shown in Table 3 below.

[0133] Table 3: Evaluation of Examples 1 and 2

[0134] Property / Method Example 1 Example 2

[0135] (N) Mean Mean

[0136]

[0137] Climbing Drum Peel at RT 45 37

[0138] B, Density

[0139] The weight density for the films of Examples 1 and 2 were calculated using the Test Method described above. The data for each of the 6 specimens as well as the calculated densities are shown in Table 4. The film according to Example 2 showed a significantly reduced density (0.641 g / cm3) compared to Example 1 (1.352 g / cm3) due to the use of glass bubbles.

[0140] Table 4: Weight Density

[0141] Specimen Example 1 Example 2

[0142] Thickness Weight Thickness Weight (g)

[0143] (micrometers) (g) (micrometers)

[0144] #1 0.270 76.7 0.157 98.7

[0145] #2 0.271 79.2 0.163 100.4

[0146] #3 0.265 80.8 0.159 99.0

[0147] #4 0.268 79.3 0.156 98.5

[0148] #5 0.270 82.6 0.157 97.1

[0149] #6 0.26 80.0 0.159 99.3

[0150] Mean 0.27 79.6 1.58 98.9

[0151]

[0152] Density (g / cm3) 1.352 0.641

Claims

What is claimed is:

1. An adhesive laminate layer comprising:a polymeric blend, wherein the polymeric blend comprises:at least one thermoplastic polyether sulfone material; andat least one polyether polyol material, andat least one fiber-reinforcing fabric, wherein the polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) that is less than the Tg of the at least one thermoplastic polyether sulfone material, and wherein the adhesive laminate is capable of heat bonding to a substrate comprising thermoplastic polyether sulfone material.

2. The adhesive laminate layer of claim 1, wherein the layer comprises 3 layers:a first layer comprising the polymeric blend;a second layer comprising a layer of fiber-reinforcing fabric; anda third layer comprising the polymeric blend.

3. The adhesive laminate layer of claim 1, wherein the polymeric blend further comprises 0-50 parts by weight of glass bubbles per 100 parts by weight of the polymeric blend.

4. The adhesive laminate layer of claim 1, wherein the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is below 150°C.

5. The adhesive laminate layer of claim 1, wherein the Tg as measured by DSC (Differential Scanning Calorimetry) of the polymeric blend is below 120°C.

6. The adhesive laminate layer of claim 1, wherein the at least one thermoplastic polyether sulfone material has a Tg as measured by DSC (Differential Scanning Calorimetry) of at least 200°C.

7. The adhesive laminate layer of claim 1, wherein the at least one polyether polyol material comprises a polyether polyol of general Formula 1 :H-(0-(-CH2-)m)n-0HFormula 1wherein m is an integer of 2 or greater; andn is an integer of 1 or greater.

8. The adhesive laminate layer of claim 1, wherein the polyether polyol material comprises a polyethylene glycol of general Formula 2:H-(O-CH2CH2-)n-OHFormula 2wherein n is an integer of 1 or greater.

9. The adhesive laminate layer of claim 1, wherein the polymeric blend comprises:70-95 weight % of at least one thermoplastic polyether sulfone material; and5-30 weight % of at least polyether polyol material, where weight% is based upon 100 weight % of the blend.

10. The adhesive laminate layer of claim 1, wherein the adhesive laminate layer has a thickness of from 50-500 micrometers.

11. The adhesive laminate layer of claim 2, wherein the adhesive blend has a density of less than or equal to 1.0 g / cm3.

12. A multi-layer article comprising:a core layer comprising at least one thermoplastic polyether sulfone material; anda laminate layer comprising:a thermoplastic polyether sulfone-based composition comprising a polymericblend comprising:at least one thermoplastic polyether sulfone material; andat least one polyether polyol material, wherein the polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) that is less than the Tg of the at least one thermoplastic polyether sulfone material; andat least one fiber-reinforcing fabric.

13. The article of claim 12, wherein the laminate layer comprises 3 layers:a first layer comprising the polymeric blend;a second layer comprising a layer of fiber-reinforcing fabric; anda third layer comprising the polymeric blend.

14. The article of claim 12, wherein the core layer comprises a foam layer or a honeycomb layer.

15. The article of claim 12, wherein the fiber-reinforcing fabric comprises a glass fiber reinforcing web or a CFRP (Carbon Fiber Reinforced Polymer) web.

16. The article of claim 12, wherein the laminate layer further comprises glass bubbles in an amount of 0-50 parts by weight per 100 parts by weight of the polymeric blend.

17. The article of claim 12, wherein the polymeric blend has a Tg as measured by DSC (Differential Scanning Calorimetry) of below 150°C.

18. The article of claim 12, wherein the at least one thermoplastic polyether sulfone material has a Tg as measured by DSC (Differential Scanning Calorimetry) of at least 200°C.

19. The article of claim 12, wherein the polyether polyol material comprises a polyethylene glycol of general Formula 2:H-(O-CH2CH2-)n-OHFormula 2wherein n is an integer of 1 or greater.

20. The article of claim 12, wherein the polymeric blend comprises:70-95 weight % of at least one thermoplastic polyether sulfone material; and5-30 weight % of at least polyether polyol material, where weight% is based upon 100 weight % of the blend.

21. The article of claim 12, wherein the article comprises:a core layer with a thickness of 100-6000 micrometers; anda laminate layer with a thickness of 35-600 micrometers.

22. The article of claim 12, wherein the article further comprises a second laminate layer such that the article comprises in sequence:a laminate layer with a thickness of 35-600 micrometers;a core layer with a thickness of 100-6000 micrometers; anda second laminate layer with a thickness of 35-600 micrometers.