Residential heating element, thermal tile, and method for manufacturing these
A laminated heating element with a conductive thin film and fiber or mesh layer addresses the inefficiencies of existing heating elements by achieving low power consumption and high energy efficiency, with enhanced safety and design capabilities.
Patent Information
- Application Number
- PCT/JP2026/013927
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-04-02
- Publication Date
- 2026-11-12
AI Technical Summary
Existing layered heating elements for residential use require high power consumption, have low energy efficiency, and are difficult to manufacture, while also lacking sufficient heat generation and safety features.
A laminated heating element structure comprising a conductive thin film layer, such as a copper thin film or single-walled carbon nanotube-SiO2 layer, combined with a fiber or mesh layer, and optionally plastic sol or hot melt adhesive layers, formed without high-temperature processing, enabling efficient heat generation and easy manufacturing.
The laminated structure generates sufficient heat with low power consumption, has high energy efficiency, and can be easily manufactured, providing safety and design flexibility for residential applications.
Smart Images

Figure JP2026013927_12112026_PF_FP_ABST
Abstract
Description
Heating element for residential use, heating tile, and methods for producing the same
[0001] The present invention relates to a novel residential heating element having a specific laminated structure, a novel article such as a residential heating tile including the same, and methods for producing the residential heating element and the residential heating tile including the same.
[0002] Conventionally, in fields such as floor heating sheets, floor panels, and sauna members, various layered heating elements used at relatively low temperatures of, for example, 200°C or lower, having a structure in which various exothermic and heat-radiating substance layers are coated with electrically insulating layers, are known. Examples of such layered heating elements include heating elements obtained by impregnating a fiber cloth with a conductive resin, and those obtained by applying a conductive resin to a base material such as a polyester sheet, a polyimide sheet, or mica, and retaining the same by printing. As a more specific example, a heating tile having design properties has been developed, in which such a layered heating element is sandwiched between layers of a backer material and further combined with a decorative sheet.
[0003] However, most layered heating elements have the disadvantage of high operating costs, as they require a large amount of electric power to obtain sufficient heat generation and have low energy efficiency of heat generation. Accordingly, there is a demand for the development of layered heating elements that can generate sufficient heat even with relatively low power, have high energy efficiency, and can be easily manufactured, as well as products such as heating tiles using such heating elements. In addition, products including heating elements are required to combine sufficient heat generation performance, high safety that can reliably prevent risks caused by scorching or combustion during use, and (if desired) excellent design properties.
[0004] Metal films or metal oxide films, when thinned, possess light transmittance and good thermal conductivity, and are known to function as heat-generating materials (heat-dissipating components) when used in lighting equipment, for example. An example of such a metal film is a copper thin film with high electrical conductivity and antibacterial properties. Metal films or metal oxide films, especially metal thin films with thicknesses on the order of microns or nanometers, are generally formed by vapor phase methods. However, since vapor phase methods such as sputtering require large-scale equipment for film formation, various wet methods for manufacturing metal films are being investigated.
[0005] For example, electroless plating allows for the deposition of a metal film on an inorganic substrate. However, the type of catalyst and other components in the electroless plating solution can affect the physical properties of the formed metal film. In contrast, a method of forming a metal film by applying a metal film-forming composition to a substrate offers greater freedom in selecting the composition of the metal film and the substrate compared to wet methods such as plating. However, such metal film formation methods require heating or sintering at relatively high temperatures, such as 100°C or higher, making it difficult to form metal films for wiring on substrates with poor heat resistance, and also increasing the electricity costs associated with high-temperature processing.
[0006] As a technique capable of solving the disadvantages of such a metal film forming method, a metal film-forming composition that can easily form a dense metal film on a base material without requiring a heat treatment at 100°C or higher, and a method for forming such a metal film have been reported (see Patent Document 1). The so-called molecular precursor method, which is the metal film forming method disclosed in this document, does not require heat treatment at a high temperature, nor does it require irradiation with active energy rays or the like, and is a method for forming a thin film of metal or the like. According to this method, a uniform thin film can be formed by preparing a metal precursor liquid (molecular precursor liquid) having a specific composition as a coating liquid, and applying the coating liquid to a base material. Patent Document 1 describes that the metal film produced by the method is suitably used for, for example, large-scale integrated circuits (LSIs), solar cell wiring, trench embedded wiring, electromagnetic wave shields, infrared blocking glass, heat reflective glass, and the like.
[0007] Japanese Patent No. 7506404
[0008] In consideration of the above-mentioned demands of the prior art, a first object of the present invention is to provide a novel heating element for residential use that generates sufficient heat even with relatively low power and has high energy efficiency, and a novel article such as a warm thermal tile for residential use including the same. A second object of the present invention is to provide a novel heating element for residential use that can generate sufficient heat even with relatively low power, has high energy efficiency, can form an article of a laminated structure having excellent design properties, and can be easily manufactured, and a novel article such as a warm thermal tile for residential use including the same.
[0009] The present inventor conducted intensive studies to solve the above problems, and as a result, found that by combining a conductive thin film layer with a fiber layer or a mesh-like layer, a residential heating element that generates sufficient heat even with relatively low power and has high energy efficiency can be successfully obtained. The present inventor also found that, in a preferred embodiment, a residential heating element that provides sufficient heat generation performance by a simple method can be obtained, and completed the present invention.
[0010] Accordingly, various aspects or embodiments of the present invention for solving the above problems are as follows: [1] A heating element for housing comprising (a) a conductive thin film layer and (c) a fiber layer or mesh-like layer laminated thereon, wherein the conductive thin film layer (a) is a copper thin film or a single-walled carbon nanotube-SiO 2A heating element for residential use, comprising a thin film layer, wherein the (c) fiber layer or mesh layer is a fiber layer or mesh layer formed from a material containing at least one selected from glass fibers and ceramic mesh. [2]. The heating element for residential use according to item [1] above, wherein (a) a conductive thin film layer, (b) a plastic sol layer or hot melt adhesive layer, (c) a fiber layer or mesh layer, and (d) a plastic sol layer or hot melt adhesive layer are laminated in this order. [3]. The heating element for residential use according to item [2] above, wherein the (b) plastic sol layer or hot melt adhesive layer and / or the (d) plastic sol layer or hot melt adhesive layer are integrated with the (c) fiber layer or mesh layer, thereby covering the surface of at least a portion of the fiber or mesh material constituting layer (c) with the plastic sol or hot melt adhesive constituting layers (b) and / or (d). [4]. A residential heating element according to any one of items [1] to [3] above, wherein the conductive thin film layer (a) is a thin film layer having a thickness of 10 nm to 100 μm, which is produced by the molecular precursor method. [5]. An article comprising a residential heating element according to any one of items [1] to [4] above. [6]. An article according to item [5] above, which has at least one use selected from heating, heat retention, snow melting, condensation prevention, and anti-fogging. [7]. A residential thermal tile in which (1) a decorative sheet, (2) a middle backer, (3) a residential heating element according to any one of items [1] to [4] above, (4) a middle backer, and (5) a bottom backer are laminated in this order. [8]. A method for manufacturing a heating element for residential use, comprising the steps of: (c) forming a conductive thin film layer (a) on a substrate including a fibrous layer or a mesh-like layer by a molecular precursor method to obtain a heating element for residential use which is a laminate including the conductive thin film layer (a) and the fibrous layer or mesh-like layer, wherein the conductive thin film layer (a) is a copper thin film or a single-walled carbon nanotube-SiO 2A method for manufacturing a heating element for residential use, wherein the (c) fiber layer or mesh layer is a thin film layer, and the (c) fiber layer or mesh layer is a fiber layer or mesh layer formed from a material containing at least one selected from glass fibers and ceramic mesh. [9]. The method according to item [8] above, wherein the substrate containing the (c) fiber layer or mesh layer is a laminated substrate containing (b) a plastic sol layer or hot melt adhesive layer, the (c) fiber layer or mesh layer, and (d) a plastic sol layer or hot melt adhesive layer in this order.
[10] . A method for manufacturing a thermal tile for residential use, comprising using the heating element for residential use manufactured by the method according to item [8] or [9] above, and laminating (1) a decorative sheet, (2) a middle backer, (3) the heating element for residential use, (4) a middle backer, and (5) a bottom backer in this order to obtain a thermal tile for residential use.
[0011] According to the present invention, it is possible to provide a novel residential heating element that generates sufficient heat even with relatively low power consumption and has high energy efficiency, as well as novel residential thermal tiles and other articles containing the same. Furthermore, the fibrous layer or mesh-like layer has the advantage of contributing to dimensional stability. In addition, according to a preferred embodiment of the present invention, it is possible to provide a novel residential heating element that generates sufficient heat even with relatively low power consumption, has high energy efficiency, can form a laminated structure article with excellent design, and can be easily manufactured, as well as novel residential thermal tiles and other articles containing the same.
[0012] Figure 1 is a schematic diagram of a residential heating element according to one embodiment of the present invention. Figure 2 is a schematic diagram of a residential thermal tile according to one embodiment of the present invention.
[0013] A heating element for residential use according to the first embodiment of the present invention comprises a structure in which (a) a conductive thin film layer and (c) a fiber layer or mesh-like layer are laminated. Here, (a) the conductive thin film layer is a copper thin film or a single-walled carbon nanotube-SiO 2(c) is a thin film layer, and the fiber layer or mesh layer is a fiber layer or mesh layer formed from a material containing at least one selected from glass fibers and ceramic mesh. The heating element for housing according to the second embodiment of the present invention is one aspect of the heating element according to the first embodiment, and comprises a structure in which (a) a conductive thin film layer, (b) a plastic sol layer or hot melt adhesive layer, (c) a fiber layer or mesh layer, and (d) a plastic sol layer or hot melt adhesive layer are laminated in this order. In the heating elements for housing according to the first and second embodiments, these layers may be directly joined together, or any other layer may be interposed between them. Furthermore, in the heating elements for housing according to the first and second embodiments, it is not prevented that other additional layers (for example, a further conductive thin film layer) may be provided on at least one of the end faces of the laminated structure of the above layers. Furthermore, in the residential heating elements according to the first and second embodiments, (a) the conductive thin film layer is usually placed on one side of the heating element that is primarily expected to perform the heat transfer function to the heat-transferring material when the article containing the heating element is used on site. Hereafter, this one side of the residential heating element may be referred to as the "surface side".
[0014] 1. Heating element for residential use (a) Conductive thin film layer (a) The copper thin film layer as a conductive thin film layer can function as a heating layer (core of the heating element) with excellent thermal conductivity. The copper thin film layer is not particularly limited as long as it contains copper as the main component (usually about 50 atomic mol% or more), and may contain one or more other metals, such as lithium, nickel, manganese, zinc, and cobalt. The proportion of copper in the copper thin film layer is preferably 60 atomic mol% or more, 70 atomic mol% or more, 80 atomic mol% or more, 90 atomic mol% or more, or 95 atomic mol% or more, more preferably substantially 100 atomic mol% (the proportion of other elements is below the detection limit). The copper content in the copper thin film layer can be measured, for example, by X-ray diffraction (XRD). By containing copper in the above proportions in the copper thin film layer as a conductive thin film layer, the required high thermal conductivity can be obtained.
[0015] The thickness of the copper thin film layer may usually be 10 nm or more and 100 μm or less, preferably 20 nm or more and 50 μm or less, 50 nm or more and 30 μm or less, 100 nm or more and 20 μm or less, or 200 nm or more and 10 μm or less, from the viewpoint of balancing imparting heat generation property, flexibility in laminate design, production cost and the like.
[0016] Single-walled carbon nanotube-SiO as the conductive thin film layer 2 The thin film layer can function as a heat generating layer (core part of the heating element) having excellent thermal conductivity comparable to that of the copper thin film layer. Single-walled carbon nanotube-SiO 2 The thin film layer is not particularly limited as long as it contains a single-walled carbon nanotube and SiO as main components (usually about 50% by mass or more) 2 and may contain any other substance (for example, multi-walled carbon nanotubes with two or more layers, etc.). Single-walled carbon nanotube-SiO 2 The proportion of the composite of single-walled carbon nanotubes and SiO in the thin film layer 2 may preferably be 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, or 95% by mass or more, more preferably substantially 100% by mass (the proportion of other elements is below the detection limit). Single-walled carbon nanotube-SiO 2 The content of the composite of single-walled carbon nanotubes and SiO in the thin film layer 2 can be measured, for example, by X-ray diffraction (XRD). (a) Single-walled carbon nanotube-SiO as the conductive thin film layer 2 When the thin film layer contains the composite of single-walled carbon nanotubes and SiO in the above proportion 2 , the required high thermal conductivity can be obtained.
[0017] Single-walled carbon nanotubes may have a diameter of, for example, 0.5 nm to 500 nm, preferably 3 nm to 100 nm or 5 nm to 50 nm. Single-walled carbon nanotubes may have a length of, for example, 500 μm or less, preferably 100 μm or less. Single-walled carbon nanotubes may be obtained by any conventional manufacturing method, such as catalyst-assisted vapor deposition, arc discharge, laser evaporation, or HiPco (High-pressure carbon monooxide process). Also, single-walled carbon nanotubes and SiO 2 The composite consists of single-walled carbon nanotubes and SiO 2 This may include any composite used in the industry, such as those reported in numerous publications, including, for example, International Publication No. 2004 / 096725, Japanese Patent Publication No. 2007-254189, Japanese Patent Publication No. 2015-171965, and International Publication No. 2016 / 126969.
[0018] Single-walled carbon nanotube - SiO 2 Single-walled carbon nanotubes and SiO in thin film layers 2 The mass ratio of the content is not particularly limited, but may be, for example, 5:95 or more and 95:5 or less, or 10:90 or more and 90:10 or less, 20:80 or more and 80:20 or less, 30:70 or more and 70:30 or less, or 40:60 or more and 60:40 or less.
[0019] Single-walled carbon nanotube - SiO 2 The thickness of the thin film layer, similar to that of the copper thin film layer, is usually 10 nm to 100 μm, preferably 50 nm to 30 μm, 100 nm to 10 μm, 200 nm to 5 μm, or 300 nm to 3 μm, from the viewpoint of balancing the imparting of heat generation, the flexibility of the laminate design, and the manufacturing cost.
[0020] (a) The conductive thin film layer may have one or more holes. The presence of holes in the conductive thin film layer allows the molten plastic sol or hot melt adhesive to penetrate the holes when the (b) plastic sol layer or hot melt adhesive layer, described later, provided on the heating element for housing according to the second embodiment, softens and melts due to heating. This facilitates joining and bonding the heating element to the layered material (for example, the middle backer described later) placed above it. When one or more holes are formed in the conductive thin film layer, the ratio of the area occupied by the holes on the surface of the conductive thin film layer (opening ratio due to holes) is not particularly limited, but from the viewpoint of balancing improved penetration efficiency of the molten material and maintenance of the strength of the conductive thin film layer, it may be, for example, 0.1% to 50%, or 1% to 30%, 2% to 20%, or 3% to 10%.
[0021] (c) Fiber layer or mesh layer In the first embodiment, the fiber layer or mesh layer provides the function of supporting the conductive thin film layer described above (a) on the layer. Alternatively, in the second embodiment, the fiber layer or mesh layer provides the function of supporting the plastic sol layer or hot melt adhesive layer described below on the surface of the fiber or mesh material, and / or supporting the plastic sol layer or hot melt adhesive layer. Furthermore, the fact that this layer is made of fibers or mesh can suppress unevenness in heat transfer, improve in-plane uniformity of heat transfer, and contribute to dimensional stability. The fiber layer or mesh layer is not particularly limited as long as it is formed by including at least one selected from glass fibers and ceramic mesh. The fiber layer or mesh layer may be only one of these layers, or a combination of these layers. The fiber layer or mesh layer may be a single layer, or a laminate of multiple layers.
[0022] The glass fibers used in the fibrous layer or mesh-like layer are not particularly limited, but may be, for example, glass fibers formed from one or more types of glass, such as alkali-free glass with high insulating properties (E glass), alkali-containing glass with excellent acid resistance (C glass), glass with high strength and elastic modulus (S glass, T glass, etc.), glass with excellent alkali resistance (AR glass), NE glass, etc. Both woven and nonwoven fabrics can be used as glass fibers. The glass fibers are not particularly limited, but may be, for example, glass fibers with a fiber diameter of 5 μm to 150 μm, preferably glass fibers with a fiber diameter of 10 μm to 100 μm. The glass fibers may be woven or nonwoven fabrics using fiber bundles composed of multiple fibers. Furthermore, the glass fibers are not particularly limited, but may be, for example, glass fibers with a fiber length of 100 μm to 5 mm, preferably glass fibers with a fiber length of 200 μm to 2 mm. It is preferable that the surface of the glass fibers be surface-treated with a silane coupling agent such as an acrylic silane-based silane coupling agent, urethane resin, polyester resin, epoxy resin, polylactic acid-based resin, etc.
[0023] When glass fibers are used as a fibrous layer or mesh-like layer, the specific surface area is not particularly limited, but from the viewpoint of balancing thermal conductivity and shape retention, for example, it is usually 10 m². 2 / g or more, preferably 50m 2 / g or more, 100m 2 / g or more, 200m 2 / g or more, or 300m 2 It may be 1 / g or more. The upper limit of the specific surface area of the glass fiber is not particularly limited, but for example, 2000 m 2 It may be less than or equal to / g.
[0024] (c) The glass fibers used in the fiber layer or mesh layer may be a woven fabric in which multiple fiber bundles are woven warp and weft. In the glass fibers, the number of fibers constituting the warp fiber bundles and the weft fiber bundles may be the same or different. In a form in which the glass fiber woven fabric is integrated with (b) a plastic sol layer or hot melt adhesive layer and (d) a plastic sol layer or hot melt adhesive layer to form a coating in at least a part of it, as described below, the coated glass fiber woven fabric may have voids in the areas where there is no coating.
[0025] The material of the mesh-like substance used in the fibrous layer or mesh-like layer is not particularly limited as long as it is formed from ceramics. The mesh-like layer is not particularly limited, but for example, it may be a mesh-like layer with an opening size of about 10 μm to 500 μm, and preferably a mesh-like layer with an opening size of about 20 μm to 200 μm. By having the opening size of the mesh-like layer within the above range, sufficient insulation and safety can be obtained, the uniformity of heat transfer in the plane is improved, and the applicability to the backer material is further enhanced.
[0026] The insulating ceramics used in the mesh layer are not particularly limited, but may be, for example, one of aluminum nitride, aluminum oxide, silicon nitride, silicon carbide, zirconium oxide, cordierite, and mullite, or a composite material of several of these.
[0027] The material used to form the fibrous layer or mesh-like layer may include at least one selected from glass fibers and ceramic mesh, in addition to one or more other optional substances. Examples of other optional substances, though not limited to them, include flame retardants, heat storage materials, polymer materials such as thermoplastic resins (binders and coatings), and other insulating substances. The amount of such other optional substances used may be, for example, about 10% by mass or less of the total mass of the material used to form the fibrous layer or mesh-like layer (with the amount of glass fibers and ceramic mesh being 90% by mass or more).
[0028] The fibrous layer or mesh-like layer may be a single layer, but may also be formed from multiple layers. The thickness of the fibrous layer or mesh-like layer (total thickness if it is formed from multiple layers) is usually 10 μm to 3000 μm, preferably 10 μm to 1000 μm, 20 μm to 500 μm, or 30 μm to 200 μm, from the viewpoint of stably supporting the conductive thin film layer (a) or the plastic sol layer or hot melt adhesive layer described later, and from the viewpoint of balancing manufacturing costs, etc.
[0029] In a second embodiment, when a plastic sol layer or hot melt adhesive layer (b) and a plastic sol layer or hot melt adhesive layer (d) are provided, layer (b) has the function of promoting and facilitating the bonding between the conductive thin film layer (a) and the fiber layer or mesh-like layer via it. Alternatively, as described above, in an embodiment in which one or more holes are formed in the conductive thin film layer (a), the molten plastic sol or hot melt adhesive penetrates the holes, thereby facilitating the bonding and adhesion between other members constituting the article (for example, the middle backer in a thermal tile as an article) and the conductive thin film layer (a) and the fiber layer or mesh-like layer (c). Furthermore, in the second embodiment, when (b) a plastic sol layer or hot melt adhesive layer and (d) a plastic sol layer or hot melt adhesive layer are provided, layer (d) has the function of facilitating joining and bonding between (c) a fiber layer or mesh-like layer and other members constituting the article (for example, the middle backer in a thermal tile as an article).
[0030] In this embodiment, when (b) a plastic sol layer or hot melt adhesive layer and (d) a plastic sol layer or hot melt adhesive layer are provided, layers (b) and (d) and the fiber layer or mesh-like layer (c) may form three layers that are in contact with each other and can be separated, or at least in part, layers (b) and / or (d) may be integrated with the fiber layer or mesh-like layer (c), so that the multilayer material of (b) / (c) or (c) / (d) or (b) / (c) / (d) has the appearance of a single aggregate layer. In this integrated form, at least a portion of the surface of the fiber or mesh-like material constituting layer (c) is covered (coated) with the plastic sol or hot melt adhesive constituting layers (b) and / or (d). The thickness of such coating is not particularly limited, but may be, for example, 5 μm or more and 100 μm or less. It is preferable from the viewpoint of homogenizing the performance of the heating element that at least half or substantially the entire surface of at least one of the fibrous or mesh-like material constituting layer (c) is coated with the plastic sol or hot melt adhesive constituting layers (b) and / or (d). Furthermore, it is even more preferable from the viewpoint of homogenizing the performance of the heating element that each of the majority or substantially the entire surfaces of the fibrous or mesh-like material constituting layer (c) is coated with a thin layer of the plastic sol or hot melt adhesive constituting both layers (b) and (d). For example, such a coating can be formed by immersing the fibrous or mesh-like material constituting layer (c) in a liquid containing a plastic sol or hot melt adhesive and curing it. Alternatively, for example, after forming a coating on the raw linear material of each fibrous or mesh-like material, a woven fabric or mesh may be formed using the coated fibrous or linear material.
[0031] When layer (b) or (d) is a plastic sol layer, the plastic sol is not particularly limited as long as it is a sol containing a plastic that performs the above functions. For example, the plastic used in the plastic sol may be polyvinyl chloride resin (PVC resin), polyacrylic resin, polyurethane resin, etc. A polyvinyl chloride resin sol may be obtained by mixing and kneading a polyvinyl chloride resin and any additives such as plasticizers, fillers, weather stabilizers and heat stabilizers, and resins for sol blends other than polyvinyl chloride resin using methods known in the industry to form a sol, and then drying it. Other additives include any lubricant, antioxidant, processing aid, reinforcing agent, nucleating agent, mold release agent, antistatic agent, urea-formaldehyde wax, surfactant, etc., known in the industry. These additives may be used individually or in mixtures of multiple types. The method for forming a polyvinyl chloride resin sol is not particularly limited, but for example, a mixture of the polyvinyl chloride resin and an optional additive can be homogenized in an aqueous medium by adding an emulsifier, and optionally a dispersing aid such as a higher alcohol or higher fatty acid, and an oil-soluble polymerization initiator, and then by fine suspension polymerization, or by emulsion polymerization or seed emulsion polymerization by adding a water-soluble initiator.
[0032] (b) or (d) The polyvinyl chloride resin constituting the sol layer of the polyvinyl chloride resin is, for example, polyvinyl chloride (polyvinyl chloride homopolymer); vinyl chloride / vinyl acetate copolymer, vinyl chloride / (meth)acrylic acid copolymer, vinyl chloride / methyl (meth)acrylate copolymer, vinyl chloride / (meth)acrylate copolymer, vinyl chloride / ethyl (meth)acrylate copolymer, vinyl chloride / maleic acid copolymer, vinyl chloride / ethylene copolymer, vinyl chloride / propylene copolymer, vinyl chloride / styrene copolymer, vinyl chloride / isobutylene copolymer, vinyl chloride / vinylidene chloride copolymer, vinyl chloride Examples include vinyl chloride copolymers of vinyl chloride and other monomers copolymerizable with vinyl chloride, such as styrene-maleic anhydride terpolymer, vinyl chloride-styrene-acrylonitrile terpolymer, vinyl chloride-butadiene copolymer, vinyl chloride-isoprene copolymer, vinyl chloride-chlorinated propylene copolymer, vinyl chloride-vinylidene chloride-vinyl acetate terpolymer, vinyl chloride-acrylonitrile copolymer, and vinyl chloride-various vinyl ether copolymers; and modified (chlorinated, etc.) polyvinyl chloride and vinyl chloride copolymers, such as post-chlorinated vinyl copolymers. Furthermore, chlorinated polyolefins, such as chlorinated polyethylene, which have a chemical structure similar to polyvinyl chloride, may also be used. Such chlorinated polyolefins with a chemical structure similar to polyvinyl chloride are also included in the category of "polyvinyl chloride resins" as used herein. One or more of these can be used as polyvinyl chloride resins.
[0033] Examples of plasticizers used in polyvinyl chloride resin sols include polyester plasticizers, phthalate ester plasticizers, trimellitic acid ester plasticizers, pyromellitic acid ester plasticizers, adipic acid ester plasticizers, itaconic acid ester plasticizers, citrate ester plasticizers, cyclohexane dicarboxylate plasticizers, and epoxy plasticizers. One or more of these plasticizers or mixtures thereof can be used. The amount of plasticizer is not particularly limited, but is usually greater than 0 parts by mass and less than or equal to 80 parts by mass, preferably 5 parts by mass or more and less than or equal to 50 parts by mass, 10 parts by mass or more and less than or equal to 40 parts by mass, or 15 parts by mass or more and less than or equal to 30 parts by mass, relative to 100 parts by mass of polyvinyl chloride resin. Furthermore, the amount of additives other than plasticizers in the sol constituting the sol layer of the polyvinyl chloride resin of (b) or (d) is not particularly limited (if used), but for example, it may be more than 0 parts by mass, and 20 parts by mass or less, 10 parts by mass or less, or 5 parts by mass or less, per 100 parts by mass of the polyvinyl chloride resin.
[0034] Examples of polyacrylic resins that constitute the sol layer of the polyacrylic resin in (b) or (d) include polymethyl methacrylate, polyethyl methacrylate, polybutyl methacrylate, polyacrylonitrile, and other polyacrylic resins, or copolymers having acrylate units and styrene units or urethane structures. One or more of these can be used as the polyacrylic resin.
[0035] The polyacrylic resin sol may be obtained by mixing and kneading the above-mentioned resin components with any additives such as plasticizers, fillers, weather stabilizers and heat stabilizers, and resins for sol blends other than polyacrylic resins, using methods known in the industry, to form a sol, and then drying it. In addition, silane coupling agents and the like may be used as tackifiers to improve adhesion with adjacent layers in the laminate. Other additives include any lubricants, antioxidants, processing aids, reinforcing agents, nucleating agents, mold release agents, antistatic agents, urea-formaldehyde wax, surfactants, and other additives known in the industry. These additives may be used individually or in mixtures of multiple types. The amount of additives in the sol constituting the polyacrylic resin sol layer of (b) or (d) (if used) is not particularly limited, but for example, it may be more than 0 parts by mass, and 20 parts by mass or less, 10 parts by mass or less, or 5 parts by mass or less, per 100 parts by mass of the above-mentioned polyacrylic resin.
[0036] Examples of polyurethane resins that constitute the sol layer of the polyurethane resin in (b) or (d) include polyester-based polyurethane resins, polylactone-based polyurethane resins, polyether-based polyurethane resins, polyurethane resins crosslinked with epoxy resins, or ionomer-type polyurethane resins. One or more of these can be used as the polyurethane resin.
[0037] The polyurethane resin sol may be obtained by mixing and kneading the above-mentioned resin components with any additives such as plasticizers, fillers, weather stabilizers and heat stabilizers, and resins for sol blends other than polyurethane resins, using methods known in the industry, to form a sol, and then drying it. In addition, silane coupling agents and the like may be used as tackifiers to improve adhesion with adjacent layers in the laminate. Other additives include any lubricants, antioxidants, processing aids, reinforcing agents, nucleating agents, mold release agents, antistatic agents, urea-formaldehyde wax, surfactants, and other additives known in the industry. These additives may be used individually or in mixtures of multiple types. The amount of additives in the sol constituting the polyurethane resin sol layer of (b) or (d) (if used) is not particularly limited, but for example, it may be more than 0 parts by mass, and 20 parts by mass or less, 10 parts by mass or less, or 5 parts by mass or less per 100 parts by mass of the polyurethane resin.
[0038] When layer (b) or (d) is a hot melt adhesive layer, the hot melt adhesive is not particularly limited as long as it contains a resin that performs the above functions and has hot melt adhesive properties. Examples of resins that make up hot melt adhesives include one or more of the following: ABS, polyvinyl chloride, polyamide, polyester, polyurethane, polycarbonate, polystyrene, polyethylene, polypropylene, poly-1-butene, polyisobutylene, polymethylpentene, ethylene-α-olefin copolymers such as ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-hexene copolymer, and ethylene-octene copolymer; ethylene-unsaturated ester copolymers such as ethylene-vinyl acetate copolymer (EVA) and ethylene-ethyl acrylate copolymer (EEA); cyclic olefin-containing copolymers such as copolymers of cyclopentadiene and ethylene and / or propylene; ethylene-glycidyl methacrylate copolymer, ethylene-propylene-diene copolymer, ethylene-vinyl acetate-maleic anhydride terpolymer, ethylene-ethyl acrylate-maleic anhydride terpolymer; ethylene-unsaturated carboxylic acid copolymers such as ethylene-vinyl acetate-glycidyl methacrylate terpolymer and ethylene-ethyl acrylate-glycidyl methacrylate terpolymer.
[0039] The hot melt adhesive constituting the hot melt adhesive layer of (b) or (d) may optionally contain, in addition to the resin, additives such as tackifiers to improve adhesion. The tackifier is not particularly limited, but examples include one or a mixture of several types of silane coupling agents, phenol resins, modified phenol resins, terpene phenol resins, xylene phenol resins, cyclopentadiene-phenol resins, xylene resins, aliphatic, alicyclic or aromatic petroleum resins, hydrogenated aliphatic, alicyclic or aromatic petroleum resins, phenol-modified petroleum resins, rosin ester resins, hydrogenated rosin ester resins, low molecular weight polystyrene resins, terpene resins, and hydrogenated terpene resins.
[0040] Other additives that may be used in hot melt adhesives include, but are not limited to, waxes for reducing viscosity, such as carnauba wax, candelilla wax, montan wax, paraffin wax, microwax, Fischer-Tropsch wax, polyethylene wax, polypropylene wax, oxides of these waxes, ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, etc., one or more of these, and mixtures thereof. Other additives that may be used in hot melt adhesives include any antioxidant, filler, flame retardant, plasticizer, antistatic agent, light stabilizer, UV absorber, heavy metal deactivator, etc., known in the art. These additives may be used individually or in mixtures thereof. The amount of these additives in the hot melt adhesive constituting the hot melt adhesive layer of (b) or (d) (if used) is not particularly limited, but for example, it may be more than 0 parts by mass per 100 parts by mass of the resin, and 20 parts by mass or less, 10 parts by mass or less, or 5 parts by mass or less.
[0041] The plastic sol layer or hot melt adhesive layer of (b) or (d) may be a single layer, but may also be formed from multiple layers. When the layer of (b) or (d) is a single layer, that layer, or when the layer of (b) or (d) is formed from multiple layers, one of those layers may be integrated with the (c) fiber layer or mesh-like layer as described above to form the appearance of a single aggregate layer. The thickness of the plastic sol layer or hot melt adhesive layer of (b) or (d) (total thickness if formed from multiple layers), or the thickness including the coating of the plastic sol or hot melt adhesive when integrated with the (c) fiber layer or mesh-like layer, may usually be 10 μm or more and 1000 μm or less after the formation of the laminated structure (after melting and curing), preferably 20 μm or more and 500 μm or less, 30 μm or more and 300 μm or less, or 40 μm or more and 100 μm or less, from the viewpoint of providing sufficient bonding and adhesion functions as described above and from the viewpoint of balancing manufacturing costs, etc. In the second embodiment, when (b) a plastic sol layer or hot melt adhesive layer and (d) a plastic sol layer or hot melt adhesive layer are formed, the composition and / or thickness of layer (b) and the composition and / or thickness of layer (d) may be the same or different.
[0042] Figure 1 shows a schematic diagram of an example of a residential heating element according to a second embodiment of the present invention. In the figure, reference numeral 1 denotes (a) a conductive thin film layer, reference numeral 2 denotes (b) a plastic sol layer or hot melt adhesive layer, reference numeral 3 denotes (c) a fiber layer or mesh-like layer, reference numeral 4 denotes (d) a plastic sol layer or hot melt adhesive layer, and reference numeral 100 denotes the entire residential heating element. Furthermore, as described above, layer 2(b) and / or layer 4(d) may be integrated with layer 3(c) a fiber layer or mesh-like layer, so that the multilayer material of (b) / (c) or (c) / (d) or (b) / (c) / (d) has the appearance of a single layer. In the figure, the conductive thin film layer 1 is located on one side of the residential heating element 100, which is mainly expected to perform a heat transfer function to the heat-transferring material when the article containing the residential heating element 100 is used on site.
[0043] As an additional embodiment, from the viewpoint of increasing heat transfer, the heating element for residential use according to the first embodiment may be configured to include a further conductive thin film layer similar to the conductive thin film layer on the side of the (c) fiber layer or mesh-like layer opposite to the (a) conductive thin film layer. Alternatively, as another additional embodiment, from the viewpoint of increasing heat transfer, the heating element for residential use according to the second embodiment may be configured to include a further conductive thin film layer similar to the conductive thin film layer on the side of the (d) plastic sol layer or hot melt adhesive layer opposite to the (a) conductive thin film layer.
[0044] A residential heating element according to any embodiment of the present invention can provide sufficient heat even with relatively low power, has high energy efficiency, and can form a laminated structure article with excellent design, making it suitable for use in various articles such as thermal tiles. Furthermore, according to the preferred manufacturing method described later, (a) the conductive thin film layer can be easily manufactured without requiring heat treatment of 100°C or higher, so the entire residential heating element according to any embodiment of the present invention, including this layer, can also be easily manufactured.
[0045] 2. Articles Including Heating Elements for Residential Use The heating elements of any embodiment of the present invention can be used as articles for various purposes, including the heating element. The uses of articles including heating elements for residential use are not particularly limited, as long as they are for applications where heat supply is preferred or required, and are intended for houses or structures related to houses. Examples of such uses for articles include heating mats such as tiles, carpets, and hot carpets in apartments and general houses, floor heating equipment, wall heating equipment, roof snow melting heaters, sheet heaters used inside houses, anti-fog heaters and anti-fog glass for removing water droplets and ice-induced fogging from windows and mirrors in houses, and condensation prevention heaters.
[0046] Preferred uses for the article include, for example, at least one use selected from heating, heat retention, snow melting, condensation prevention, and anti-fogging. A particularly preferred example of a preferred use for the article is a residential thermal tile that can be used in the floors and walls of residential buildings for heating, heat retention, condensation prevention, etc.
[0047] 3. Thermal Tiles for Residential Use In one embodiment, the thermal tiles for residential use according to the present invention have a structure in which (1) a decorative sheet, (2) a middle backer, (3) a heating element for residential use according to any embodiment of the present invention (typically a heating element for residential use according to the second embodiment described above), (4) a middle backer, and (5) a bottom backer are laminated in this order. Here, (1) the decorative sheet and (2) the middle backer are usually arranged on one side of the heating element for residential use (3), which is mainly expected to perform a heat transfer function to the heat transfer material when the thermal tiles for residential use are used on site. The thermal tiles for residential use may further include any one or more layers other than (1) to (5) described above (for example, layers such as heat-resistant adhesive applied between each layer), as long as the desired thermal function is not hindered.
[0048] The decorative sheet that constitutes the residential thermal tiles is not particularly limited, as long as it provides the desired design and aesthetic appeal. For example, any colored or uncolored resin sheet can be used as the decorative sheet.
[0049] Examples of resins used in colored or uncolored resin sheets that can be used as decorative sheets include, but are not limited to, polyester resins such as aromatic polyesters and aliphatic polyesters; acrylic resins; polycarbonate resins; poly(meth)acrylimide resins; polyolefin resins such as polyethylene, polypropylene, and polymethylpentene; cellulosic resins such as cellophane, triacetylcellulose, diacetylcellulose, and acetylcellulose butyrate; styrene resins such as polystyrene, acrylonitrile-butadiene-styrene copolymer (ABS resin), styrene-ethylene-propylene-styrene copolymer, styrene-ethylene-ethylene-propylene-styrene copolymer, and styrene-ethylene-butadiene-styrene copolymer; polyvinyl chloride resins; polyvinylidene chloride resins; fluorine-containing resins such as polyvinylidene fluoride; and others such as polyvinyl alcohol, ethylene vinyl alcohol, polyetheretherketone, nylon, polyamide, polyimide, polyurethane, polyetherimide, polysulfone, and polyethersulfone. These resin sheets include unoriented sheets, uniaxially oriented sheets, and biaxially oriented sheets. Laminated sheets, which consist of two or more layers of one or more of the above-mentioned resin sheets, may also be used.
[0050] The decorative sheet may optionally include a printed layer on its surface to enhance its aesthetic appeal. The printed layer is provided to give it a high level of design appeal and can be formed by printing any pattern using any ink and any printing press.
[0051] The printing layer can be applied directly or via an anchor coat to the resin sheet, either entirely or partially. Examples of patterns include metallic patterns such as hairline finishes, wood grain patterns, stone patterns mimicking the surface of rocks such as marble, fabric patterns mimicking cloth or cloth-like textures, tile patterns, brick patterns, parquet patterns, and patchwork. As the printing ink, a binder can be used that contains pigments, solvents, stabilizers, plasticizers, catalysts, and curing agents in appropriate proportions. Examples of binders that can be used include polyurethane resins, vinyl chloride / vinyl acetate copolymer resins, vinyl chloride / vinyl acetate / acrylic copolymer resins, chlorinated polypropylene resins, acrylic resins, polyester resins, polyamide resins, butyral resins, polystyrene resins, nitrocellulose resins, and cellulose acetate resins, as well as compositions of these resins. Furthermore, in order to create a metallic appearance, aluminum, tin, titanium, indium, and their oxides may be deposited onto the resin sheet, either directly or via an anchor coat, either entirely or partially, by known methods.
[0052] In one modified form, the decorative sheet is composed of a printed layer, and the printed layer may be formed on the surface of the middle backer (2) as a resin substrate. In this modified form, the middle backer (2) can function as a substitute for the above-mentioned colored or uncolored resin sheet.
[0053] The thickness of the decorative sheet (including the printed layer if one is formed) is not particularly limited, but is usually 50 μm or more, preferably 100 μm or more, and more preferably 200 μm or more. Also, from the viewpoint of meeting the demand for thinner articles, the thickness of the decorative sheet is usually 3000 μm or less, preferably 2000 μm or less, and more preferably 1000 μm or less.
[0054] The surface side of the decorative sheet may optionally be further provided with a transparent film layer and / or transparent coating layer (hereinafter, these layers may be collectively referred to as the "clear layer") containing an acrylic resin, fluororesin, or polyvinyl chloride resin, which has the function of providing high weather resistance, scratch resistance, and impact resistance to the laminate of residential thermal tiles. The clear layer may form the outermost surface of the residential thermal tile. Such a clear layer may also be called a protective layer in terms of its function. In this specification, "acrylic resin" refers to either acrylic resin or methacrylic resin. "Transparent" of the transparent film layer and transparent coating layer means a state in which light in substantially the entire wavelength range of visible light, or light in a part of the wavelength range of visible light, passes through the clear layer, and one side of the clear layer is visible from the other side. "Transparent" for the transparent film layer and transparent coating layer includes not only colorless transparency, but also colored transparency and translucency. The clear layer, which may contain acrylic resin, fluororesin, or vinyl chloride resin, may be a single layer or a laminate of multiple layers with identical or different compositions. The transparent film layer may be an unoriented film, a uniaxially oriented film, or a biaxially oriented film. If the transparent film layer is a laminate of multiple layers, it may be formed from a combination of two or more of the unoriented film, uniaxially oriented film, and biaxially oriented film. The transparent coating layer may be formed by methods such as spin coating, spray coating, bar coating, knife coating, roll coating, blade coating, die coating, or gravure coating. The transparent coating layer may have a multilayer structure. The transparent coating layer may also be laminated on top of the transparent film layer.
[0055] Examples of acrylic resins used as the main component of the clear coat include, but are not limited to, (meth)acrylic acid ester (co)polymers, copolymers mainly containing (usually 50 mol% or more) structural units derived from (meth)acrylic acid esters, and modified versions thereof. (Meth)acrylic means acrylic or methacrylic. (Co)polymer means polymer or copolymer. As the acrylic resin used as the main component of the clear coat, one of these resins can be used alone or in the form of any mixture of two or more. Examples of (meth)acrylic acid ester (co)polymers include poly(meth)acrylic acid methyl, poly(meth)acrylic acid ethyl, poly(meth)acrylic acid propyl, poly(meth)acrylic acid butyl, (meth)acrylic acid methyl / (meth)acrylic acid butyl copolymer, and (meth)acrylic acid ethyl / (meth)acrylic acid butyl copolymer. These resins can be used alone or in the form of any mixture of two or more.
[0056] Examples of fluororesins used as the main component of the clear coat include, but are not limited to, polyvinyl fluoride (PVF), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene (PCTFE), polyethylene tetrafluoroethylene (ETFE), polytetrafluoroethylene (PTFE), tetrafluoroethylene perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), chlorotrifluoroethylene-ethylene copolymer (ECTFE), fluoroolefin-vinyl ether copolymer, or modified versions of these fluororesins. These resins can be used individually or in any mixture of two or more.
[0057] Examples of vinyl chloride resins used as the main component of the clear layer include, but are not limited to, homopolymers of vinyl chloride or copolymers of vinyl chloride with other monomers. Examples of these other monomers include, but are not limited to, olefins such as ethylene, propylene, and isobutene or their chlorinated derivatives; dienes such as isoprene and butadiene; vinyl compounds such as acrylonitrile, methacrylonitrile, and vinyl acetate; maleic acid or its esters or acid anhydrides; acrylic acid or its esters; methacrylic acid or its esters; and vinylidene chloride. Furthermore, the vinyl chloride resin may be a resin in which the homopolymer or copolymer is partially crosslinked. These resins can be used individually or in any mixture of two or more.
[0058] The clear layer may optionally contain other components besides the resin constituting the main component, to the extent that it does not contradict the objectives of the present invention. Examples of such optional components include resins such as core-shell rubber and ethylene-vinyl acetate copolymer, ultraviolet absorbers, light stabilizers, flame retardants, photopolymerization initiators, antistatic agents, surfactants, leveling agents, thixotropic agents, antifouling agents, printability improvers, antioxidants, weather-resistant stabilizers, heat stabilizers, pigments, and fillers. The amount of the optional components (if used) is not particularly limited, but is usually about 0.01 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the main component resin forming the clear layer.
[0059] The thickness of the clear layer (or the total thickness if it consists of multiple layers) is not particularly limited, but from the viewpoint of balancing the provision of high weather resistance and impact resistance with manufacturing costs and ease of handling, it may be, for example, 1 μm or more and 1000 μm or less. This thickness may preferably be 80 μm or more, 100 μm or more, 150 μm or more, 200 μm or more, or 300 μm or more, and / or 800 μm or less, 700 μm or less, 600 μm or less, 500 μm or less, or 400 μm or less.
[0060] The middle backers (2) and (4) and the bottom backer (5) that constitute the residential thermal tile are layers of backup material formed from synthetic resin. The middle backers (2) and (4) and the bottom backer (5) are all provided for the purpose of imparting hardness and strength to the residential thermal tile article, mitigating unevenness on the surface of the adherend, and providing impact resistance.
[0061] (2) and (4) as the middle backer and (5) as the bottom backer, a resin sheet made of thermoplastic resin can usually be used. Examples of such thermoplastic resins include polyolefins such as polypropylene and polyethylene, polyacrylics, polymethylenes, polymethylpentenes, polyethylene terephthalates, polybutylene terephthalates, polycarbonates, polyarylates, polyimides, polystyrenes, polyamides, polyvinyl chlorides, polyurethanes, ethylene-vinyl alcohol copolymers, polyethylene naphthalate-isophthalate copolymers, and ABS resins. These resins can be used individually or in combination of two or more.
[0062] The thickness of the middle backer in (2) and (4) and the bottom backer in (5) can be appropriately selected according to the requirements of each product, but from the viewpoint of balancing the provision of hardness, strength, impact resistance, etc., the specifications of the resulting product, aesthetics, and manufacturing costs, it is usually 0.5 mm to 20 mm, preferably 1 mm to 15 mm, 3 mm to 12 mm, or 5 mm to 10 mm.
[0063] Figure 2 shows a schematic diagram of an example of a residential thermal tile including a residential heating element according to one embodiment of the present invention. In the figure, reference numeral 10 denotes a decorative sheet, reference numeral 20 denotes a middle backer, reference numeral 100a denotes a residential heating element according to one embodiment of the present invention, reference numeral 30 denotes a middle backer, reference numeral 40 denotes a bottom backer, and reference numeral 200 denotes the entire residential thermal tile. In the figure, the decorative sheet 10 and the middle backer 20 are arranged on one side of the residential heating element 100a, which is mainly expected to perform a heat transfer function to the heat-transferring material when the residential thermal tile 200 including the residential heating element 100a is used on site.
[0064] A residential thermal tile containing a residential heating element according to any embodiment of the present invention can be designed to provide sufficient heat even with relatively low power consumption, have high energy efficiency, and offer excellent design. Furthermore, as described below, since the conductive thin film layer (a) included in the residential heating element (3) can be easily manufactured without requiring heat treatment of 100°C or higher, the entire residential thermal tile containing the residential heating element according to any embodiment of the present invention can also be easily manufactured.
[0065] 4. Method for Manufacturing a Heating Element for Residential Use The method for manufacturing a heating element for residential use according to any embodiment of the present invention described above is not particularly limited, as long as the above-described configuration can be obtained. The heating element for residential use according to the first embodiment described above can be manufactured, for example, by individually creating (a) a conductive thin film layer and (c) a fibrous layer or mesh-like layer (and any other arbitrary layer as needed) and laminating them by known means, or by applying the raw material or precursor of the conductive thin film layer (a) onto the (c) fibrous layer or mesh-like layer (or a laminate of the same and any other arbitrary layer) and subjecting it to a treatment such as drying under predetermined conditions as needed. The heating element for residential use according to the second embodiment described above can be manufactured, for example, by individually creating (a) a conductive thin film layer, (b) a plastic sol layer or hot melt adhesive layer, (c) a fiber layer or mesh-like layer, and (d) a plastic sol layer or hot melt adhesive layer, as well as any other arbitrary layer as needed, and laminating them by known means, or by applying the raw material or precursor of the conductive thin film layer (a) onto a laminate of (b) a plastic sol layer or hot melt adhesive layer, (c) a fiber layer or mesh-like layer, and (d) a plastic sol layer or hot melt adhesive layer (or a laminate including any other arbitrary layer as needed), and subjecting it to a treatment such as drying under predetermined conditions as needed. Here, in a laminate of layer (b), layer (c), and layer (d) (or a laminate including any other layer as needed), layers (b) and / or (d) may be integrated with layer (c) so that at least a portion of the surface of the fibrous or mesh-like material constituting layer (c) is covered with the plastic sol or hot melt adhesive constituting layers (b) and / or (d).
[0066] The so-called molecular precursor method can be used as a method in which (a) raw materials or precursors for the conductive thin film layer are applied onto (c) a fibrous layer or mesh-like layer or (d) a plastic sol layer or hot melt adhesive layer (or any other layer applied on top of any of these layers), and if necessary, drying or other treatments are performed under predetermined conditions. This method is described below.
[0067] Formation of a conductive thin film layer (a) of a heating element according to any embodiment of the present invention: (a) copper thin film or single-walled carbon nanotube-SiO 2 The thin film layer can be manufactured by any method known in the art, but preferably by the so-called molecular precursor method. The molecular precursor method does not require high-temperature heating or irradiation with active energy rays, thus allowing for the simple formation of a conductive thin film layer on substrates with poor heat resistance. Furthermore, the molecular precursor method allows for the generation of sufficient heat even with relatively low power (e.g., using only dry cell batteries), resulting in a highly energy-efficient conductive thin film layer. The copper thin film or single-walled carbon nanotube-SiO obtained by the molecular precursor method... 2 The thin film layer has a dense structure and high purity, resulting in excellent electrical and thermal conductivity. Subsequently, copper thin films or single-walled carbon nanotubes-SiO2 are produced by the molecular precursor method. 2 A method for manufacturing thin film layers will be described. Note that the molecular precursor method for manufacturing these layers described below includes embodiments in which a portion of the copper constituting the copper thin film is replaced with one or more other arbitrary metals, such as lithium, nickel, manganese, zinc, and cobalt, as well as a single-walled carbon nanotube-SiO2 2 Thin film composed of single-walled carbon nanotubes - SiO 2 The same can be applied to embodiments in which a portion of the composite is replaced with any other material (e.g., multilayered carbon nanotubes with two or more layers).
[0068] A method for producing a copper thin film by molecular precursor typically includes: (Step I) reacting at least one copper complex and / or copper salt with at least one selected from ammonia and amine in a mixed solution containing at least one copper complex and / or copper salt, at least one selected from ammonia and amine, and a solvent to obtain a copper precursor solution; (Step II) preparing a copper thin film forming composition containing the obtained copper precursor solution and an organic reducing agent; and (Step III) applying the obtained copper thin film forming composition to a substrate.
[0069] (Step I) The copper salt used in Step I is preferably a copper salt soluble in water at 25°C. Soluble in water at 25°C means that the solubility in water at 25°C is 0.1% by mass or more, and preferably 1% by mass or more. Because the copper salt is soluble in water, it dissociates in a water-containing solvent to become copper ions, and these copper ions react with amines contained in the solvent to obtain a copper complex. The copper salt is not particularly limited, but examples include copper formate, copper acetate, and copper chloride. Furthermore, if the solvent optionally contains a compound for complex formation described later, the copper ions may react with the compound for complex formation to form a copper complex.
[0070] The copper complex that the mixture may contain is NH that can form a copper complex. 3 Ligand, RNH 2 The copper complex is preferably a reaction product of copper ions with one or more compounds for copper complex formation selected from compounds having a ligand (R represents an alkylene group), a diamine-derived ligand such as ethylenediamine or hexamethylenediamine as a substructure. As the copper complex, a copper complex previously produced by the above reaction can be used. Examples of copper complexes are not particularly limited, but ethylenediaminetetraacetate copper, tetraamminecopper, etc. are preferred. In addition to amines, OH is also a preferred compound for copper complex formation. 2 This may include compounds that have ligands as substructures.
[0071] More specifically, compounds for copper complex formation include ammonia, ammonium formate, and ethylenediaminetetraacetic acid (H 4At least one selected from EDTA is an example. These compounds are preferably included in the mixture as an aqueous solution. In particular, the mixture contains H as a compound for copper complex formation. 4 It is more preferable to include an aqueous solution of EDTA.
[0072] The amines used in the mixture include primary amines, secondary amines, and tertiary amines. Examples of amines include alkylamines. The mixture may contain ammonia in place of or in addition to amines. Hereafter, at least one selected from ammonia and amines will be referred to as amines. Amines may be included in the mixture as salt compounds. The mixture may contain only one type of amine, or two or more types. Amines are basic and react with copper complexes and / or copper salts in the mixture to obtain a copper precursor solution.
[0073] The solvent used in the mixture may be water, or a mixture of one or more aqueous solvents such as a mixture of water and an alcohol. The water may be purified water, deionized water, or pure water. Examples of alcohols include monohydric alcohols having 1 to 10 carbon atoms such as methanol, ethanol, isopropanol, n-propanol, isobutanol, and n-butanol, and polyhydric alcohols such as ethylene glycol, propylene glycol, diethylene glycol, polyethylene glycol, and glycerin. As the aqueous solvent, water or a mixture of water and a monohydric alcohol having 1 to 5 carbon atoms is preferred, water or a mixture of water and an alcohol selected from methanol, ethanol, and propanol is more preferred, and water is even more preferred. When a mixture of water and an alcohol is used as the solvent, for example, the alcohol content relative to the total amount of the water-alcohol mixture is preferably 1% by mass or more and 60% by mass or less. According to this manufacturing method, even when water is used as the solvent, a uniform copper precursor solution can be obtained, and by using the obtained copper precursor solution, a dense copper thin film can be formed through the process described later.
[0074] A copper precursor solution can be prepared by thoroughly stirring and mixing a copper complex and / or copper salt with amines in a solvent. Mixing may be carried out at room temperature, or the solvent may be heated to 40°C to 60°C to promote dissolution. Known stirring methods can be applied. Stirring methods include placing the solution containing the copper complex and / or copper salt with amines in a container and stirring with a rotor such as a magnetic stirrer, stirring with a stirring device equipped with a rotating stirring blade such as a paddle, placing the solution in a sealable container and stirring by shaking the container, and irradiating with ultrasonic waves. A simple method is to use a stirring device equipped with a stirring blade. The rotation speed of the rotor can be 300 rpm (revolutions / min: the same applies below) to 800 rpm, with 400 rpm to 600 rpm being preferred. Stirring is preferably carried out until the reaction between the copper complex and / or copper salt and the amines proceeds sufficiently. When stirring with a stirring device equipped with a rotor at room temperature as described above, stirring is preferably carried out for about 30 to 90 minutes, and more preferably for about 50 to 80 minutes. For example, when preparing a copper precursor solution containing a copper complex, a sufficiently stirred copper precursor solution will exhibit a blue color due to copper ions.
[0075] Step I is preferably made to include the following Step I-2 from the viewpoint of obtaining a copper precursor of higher purity. Step I-2 is a reaction apparatus equipped with a pair of electrolyte tanks connected via a channel with a filter that does not allow copper ions to pass through but allows hydrogen ions to pass through, wherein an electrolyte containing an amine is stored in each of the pair of electrolyte tanks, and copper electrodes are placed in a position where at least a portion of them are in contact with the electrolyte, and the pair of electrodes are connected via a DC power supply, and a voltage is applied between the pair of electrodes by the DC power supply to react copper ions derived from the copper electrodes with the electrolyte in the electrolyte tank in which the electrode that will become the anode is immersed, in order to obtain a copper precursor solution.
[0076] A filter that does not allow copper ions to pass through but allows hydrogen ions to pass through is a filter that has the function of controlling permeability or non-permeability depending on the size of the ions, and is not particularly limited as long as it functions as a semipermeable membrane that does not allow copper ions to pass through but allows hydrogen ions to pass through. Examples of such filters include cellulose-based filters such as regenerated cellulose membranes (cellophane), acetylcellulose membranes, collodion membranes, and cellulose tubes for dialysis; ceramic filters such as unglazed plates and porous ceramics; porous membranes such as polyacrylonitrile, polysulfone, and polyester polymer alloys; and semipermeable membranes selected from membrane filters containing fluororesin, cellulose acetate, etc. Among these, cellulose-based filters selected from ceramic filters, cellulose tubes for dialysis, etc. are preferred from the viewpoint of having good durability even when in constant contact with the electrolyte. Examples of commercially available products include Visking tubes from Nippon Medical Science Co., Ltd., which are commercially available as cellulose-based filters used in hemodialysis.
[0077] As the electrolyte, an electrolyte capable of reacting with the generated copper ions to form a copper complex is used. The electrolyte contains amines capable of forming a copper complex. The amines are the same as those used in step I, and NH 3 Ligand, RNH 2 It is preferable that the copper complex-forming compound is one or more compounds selected from compounds having a ligand (R represents an alkylene group), ethylenediamine, hexamethylenediamine, or other diamine-derived ligand as a substructure. It is preferable that the amines are included in the electrolyte as an aqueous solution. In addition, as a copper complex-forming compound, in addition to amines, OH 2 This may include compounds having ligands as substructures. More specifically, copper complex-forming compounds include ammonia, ammonium formate, and ethylenediaminetetraacetic acid (H), which are included in the amine group. 4 Preferably, it is an aqueous solution containing at least one amine selected from EDTA, H 4 It is more preferable to include an aqueous solution of EDTA. Amines may be included in the electrolyte as salt compounds.
[0078] The electrolyte may contain only one copper complex-forming compound, such as amines, or two or more. In particular, the electrolyte may contain NH 3 Ammonia containing a ligand, or RNH 2 At least one ammonium derivative such as ammonium formate having a ligand, and H having a ligand derived from a diamine 4 It is preferable to include at least one type of EDTA. The content of amines for copper complex formation in the electrolyte is preferably in the range of 0.1% to 20% by mass, more preferably 0.5% to 10% by mass, and even more preferably 1% to 8% by mass.
[0079] The solvent for the electrolyte may be the same as that used in the mixture in step I as described above. The electrolyte can be prepared by mixing water, which is the solvent, with a compound containing amines for copper complex formation and stirring. The electrolyte may be prepared at room temperature (25°C), or the solvent may be heated to 30°C to 60°C to promote dissolution. It is preferable to continue stirring until the compound for copper complex formation is dissolved and the electrolyte becomes a visually uniform solution. When preparing the electrolyte at room temperature, it is preferable to stir for about 30 to 90 minutes, and more preferably for about 50 to 80 minutes. Stirring can be carried out using known stirring devices. Known stirring devices include stirrers, paddle mixers, impeller mixers, etc., but the stirring device is not limited to the above devices.
[0080] By applying a voltage between a pair of electrodes using a DC power supply, a copper precursor solution containing a reaction product is obtained by reacting the electrolyte with copper ions derived from the anode electrode in an electrolyte tank in which the anode electrode is immersed. The previously prepared electrolyte is stored in a pair of electrolyte tanks, and electrodes (copper plates) are placed in positions where they will be immersed in the electrolyte stored in the electrolyte tanks. A voltage is then applied between the electrode (anode) and the electrode (cathode) using a DC power supply. The applied voltage can be greater than 0V and less than or equal to 100V, preferably in the range of 1V to 80V, and more preferably in the range of 10V to 60V. As the power supply, a known DC power supply can be appropriately selected and used. Examples of known DC power supplies that can be used include a DC stabilized power supply (PMC18-2, trade name, Kikusui Electronics Co., Ltd.).
[0081] The general reaction when a direct current is applied to electrodes is similar to that in processes such as copper electrolytic refining. As shown in the following reaction equation, the copper at the anode is oxidized and dissolves as copper ions, while a reduction reaction occurs at the cathode. Anode: Cu → Cu 2+ +2e - Cathode: H + +2e - →H 2
[0082] Furthermore, the same reaction occurs when the same set of electrodes are placed in one electrolyte bath and a voltage is applied. Subsequently, as the reaction progresses and the copper ion concentration in the electrolyte increases, over time, the above hydrogen (H) is produced at the cathode. 2 Compared to the reaction of producing Cu 2+ +2e - →The reaction with Cu preferentially occurs. This is because the copper ions (Cu) that are produced 2+ ) generates hydrogen ions (H) on the cathode side. + This phenomenon occurs because the ionization tendency is lower than that of ). Therefore, as shown below, when the copper ion concentration in the electrolyte exceeds a certain amount, copper is deposited on the cathode side, and the copper ion concentration in the electrolyte does not increase beyond the certain amount. If the voltage is continued to be applied, the efficiency of metal complex formation tends to decrease over time. Anode: Cu → Cu 2+ +2e -Cathode: Cu 2+ +2e - →Cu
[0083] In step I-2, a preferred embodiment of step I, a filter is provided in the flow path connecting the pair of electrolyte tanks. Therefore, copper ions generated in the electrolyte tank where the anode is located do not move to the electrolyte tank where the cathode is located, but remain in the electrolyte in the electrolyte tank on the anode side, and react with the copper complex-forming compound in the electrolyte to form a copper complex. For example, as the copper complex-forming compound, H 4 When EDTA is used, the following reaction occurs: Cu 2+ +H 4 EDTA→[Cu(H 2 EDTA) 2- +2H + On the other hand, the hydrogen ions produced in this reaction can pass through the filter and move to the electrolyte tank on the cathode side, where the above-mentioned "H + +2e - →H 2 The reaction proceeds as follows, generating hydrogen. The copper ions on the anode side are used to form a copper complex, so on the anode side, the reaction proceeds as follows: Cu → Cu 2+ +2e - The reaction proceeds, and it is thought that a copper complex as a copper precursor is efficiently produced. Therefore, in the manufacturing method of this disclosure, by including step I-2, a copper precursor solution containing a high concentration of copper precursor stably can be efficiently produced without going through intermediates such as copper salt compounds.
[0084] (Step II) Step II is a step of preparing a copper thin film forming composition comprising the copper precursor solution obtained in Step I (preferably including Step I-2) and an organic reducing agent. In Step II, it is preferable to prepare the copper thin film forming composition by mixing the copper precursor solution obtained in Step I with an aqueous solution containing an organic reducing agent. The copper precursor solution used in Step II is a solution obtained in Step I that contains at least a copper complex and / or copper salt and amines. The copper complex contained in the copper precursor solution may be a reaction product of a copper salt, amines, and optionally further contained compounds for copper complex formation as described above, or it may be a pre-prepared copper complex. The copper precursor solution may contain only one type of copper complex and / or copper salt, or it may contain two or more types.
[0085] The organic reducing agent used in the preparation of the copper thin film forming composition preferably contains at least one compound selected from compounds having a carboxyl group. It is preferable to appropriately select and use an organic carboxylic acid compound that has a carboxyl group in its molecule and functions as an organic reducing agent. Examples of such organic reducing agents include at least one selected from ascorbic acid, citric acid, oxalic acid, formic acid, and 3,4,5-trihydroxybenzoic acid. From the viewpoint of better copper thin film formation, the organic reducing agent is preferably at least one selected from ascorbic acid, citric acid, and 3,4,5-trihydroxybenzoic acid, and more preferably at least one selected from ascorbic acid and citric acid. Including ascorbic acid as the organic reducing agent is one preferred embodiment of the copper thin film forming composition.
[0086] The organic reducing agent is preferably used as an aqueous solution. The water used to prepare the aqueous solution should not contain metal ions, or should have the lowest possible metal ion concentration, from the viewpoint of uniformity of the resulting copper thin film. Therefore, it is preferable to use purified water, deionized water, or pure water for preparing the aqueous solution. When dissolving the organic reducing agent in water, the water solvent may be heated to 30°C to 60°C, and preferably to 35°C to 45°C, in order to improve solubility. Dissolution may be carried out with stirring, and the stirring method can be the same as the stirring method described in the section on the preparation of the copper complex solution. The content of the organic reducing agent in the aqueous solution is preferably in the range of 10% to 40% by mass, and more preferably in the range of 10% to 30% by mass. A content of 10% by mass or more of the organic reducing agent relative to the total volume of the aqueous solution ensures that the aqueous solution contains a sufficient amount of organic reducing agent for the reaction, while a content of 40% by mass or less results in better stability of the aqueous solution.
[0087] In step II, there are no particular restrictions on the content of the copper precursor solution and the organic reducing agent in the copper thin film forming composition obtained by mixing the copper precursor solution and the organic reducing agent solution, and these can be appropriately selected according to the target copper thin film. The copper ions (contained in the copper precursor solution) can be 50 to 400 parts by mass per 100 parts by mass of the organic reducing agent contained in the copper thin film forming composition, and in particular, from the viewpoint of obtaining better copper thin film forming properties of the resulting copper thin film forming composition, it is preferable that the copper ions are 100 to 350 parts by mass per 100 parts by mass of the organic reducing agent, and more preferably that the copper ions are 150 to 350 parts by mass per 100 parts by mass of the organic reducing agent.
[0088] By setting the copper ion content in the organic reducing agent to the above-mentioned preferred range, a more efficient and denser copper thin film can be formed on the substrate. The inventors' theory is that when the copper ion content is 50 parts by mass or more per 100 parts by mass of organic reducing agent, the reducing power of the copper ions is further improved, and the deposition of copper by the reduction of copper ions attached to the substrate becomes more rapid, resulting in the formation of a dense copper thin film. Furthermore, when the copper ion content is 400 parts by mass or less per 100 parts by mass of organic reducing agent, the deposition rate of copper due to the reduction of copper ions is maintained within a good range, and the deposition of copper particles that do not adhere to the substrate due to the redissolution of the deposited copper thin film is suppressed.
[0089] The obtained copper thin film forming composition is useful for forming copper thin films. The content of the copper precursor solution in the preparation of the copper thin film forming composition can be controlled by adjusting the type and content of the metal complex when preparing the copper precursor solution in step I, or by adjusting the type of electrolyte, the concentration of the electrolyte, the applied energy of the DC current, and the application time in step I-2. In general, it is difficult to measure the content of the copper complex and / or copper salt relative to the total amount of the copper thin film forming composition. However, the physical properties of the copper thin film formed by the copper thin film forming composition depend on the copper content in the copper thin film forming composition. From the viewpoint of being able to form a dense and uniform copper thin film, the copper content relative to the total amount of the copper thin film forming composition is preferably in the range of 0.5% to 10% by mass, and more preferably in the range of 1% to 8% by mass. When the copper content is within the above range, the structure of the copper thin film formed by the copper thin film forming composition becomes more uniform, and the electrical conductivity and thermal conductivity can be improved.
[0090] The copper content in a copper thin film forming composition can be measured, for example, by the method described in "Fundamentals of Coordination Chemistry: Werner Complexes and Organometallic Complexes" (KS Chemistry Textbook: Kodansha, 1989). On the other hand, the content of organic reducing agents in a copper thin film forming composition can be measured, for example, by the following method. First, the copper thin film forming composition is dried to produce a powder. The content of organic reducing agents can be measured by analyzing the obtained powder using a thermogravimetric differential thermal analyzer (TG-DTA). As a specific example, the content of organic reducing agents in a copper thin film forming composition can be measured using a TG-DTA2000S (product name) manufactured by MacScience, Inc., while passing 100 ml (milliliters) of air through it at a heating rate of 10°C / min.
[0091] The pH of the copper thin film forming composition at room temperature (25°C) is preferably 6 to 8, and more preferably in the neutral range around pH 7.5. The pH of the copper thin film forming composition can be measured using a known pH meter.
[0092] The copper thin film forming composition used in this manufacturing method contains an organic reducing agent as an organic component, and as a metallic component, it contains only copper ions that contribute to the formation of the desired copper thin film. It does not need to contain other metallic components, such as reducing metals used in displacement plating or catalysts used in electroless plating. Therefore, copper thin films formed with such a copper thin film forming composition do not contain catalysts, are highly pure, and can become dense copper thin films.
[0093] (Step III) Step III is the step of applying the copper thin film forming composition obtained in Step II to a substrate. The copper thin film forming composition obtained through Step II described above has copper complexes uniformly present at high concentrations in an aqueous solvent, and the stability of the copper complexes is good due to the function of the coexisting organic reducing agent. The copper complexes contained in the composition have good adsorption properties to the surface of hard substrates, so a copper thin film with a dense structure can be formed on the substrate surface. That is, in Step III, by applying the copper thin film forming composition to a substrate, copper complexes are adsorbed to the substrate surface, and a dense copper thin film is formed. Copper nanoparticles derived from the copper complexes adhere to the substrate to form a copper thin film, and the formed copper thin film can have excellent electrical and thermal conductivity. When the copper complexes contained in the copper thin film forming composition have ligands derived from ammonium groups, ethylenediamine, etc., the copper complexes can have particularly good adhesion to glass fiber substrates. Therefore, copper thin films formed using such copper complexes can be expected to have excellent adhesion to inorganic substrates.
[0094] In the manufacture of the heating element according to the first embodiment of the present invention described above, the substrate to which the copper thin film forming composition is applied is usually (c) a fibrous layer or a mesh-like layer. In this case, the copper thin film forming composition can be applied to the surface of the fibrous layer or mesh-like layer. Furthermore, in the manufacture of the heating element according to the second embodiment of the present invention described above, the substrate to which the copper thin film forming composition is applied may be a laminate in which (b) a polyvinyl chloride sol layer or a hot melt adhesive layer, (c) a fibrous layer or a mesh-like layer, and (d) a polyvinyl chloride sol layer or a hot melt adhesive layer are laminated in this order. In this case, the copper thin film forming composition can usually be applied to the surface of the polyvinyl chloride sol layer or the hot melt adhesive layer.
[0095] In step III, the obtained copper thin film forming composition is applied to a substrate to form a layer of the copper thin film forming composition. Since the copper complex contained in the copper thin film forming composition has good adsorption properties to the substrate, a dense copper thin film is formed on the substrate by removing the solvent from the copper thin film forming composition layer. There are no particular restrictions on the method of applying the copper thin film forming composition to the substrate in step III, and known coating methods can be appropriately selected.
[0096] Methods for applying the copper thin film forming composition to a substrate include, for example, spray coating, spin coating, blade coating, bar coating, roll coating, die coating, and flow coating. Alternatively, the copper thin film forming composition may be applied to the substrate by casting. An appropriate coating method should be selected considering the physical properties of the copper thin film forming composition, such as viscosity, and the thickness of the copper thin film to be formed. As a method for applying the copper thin film forming composition locally to the substrate, printing methods such as screen printing and inkjet printing may be applied. By using printing methods, a copper thin film can be formed locally only in a desired area of the substrate. The amount of copper thin film forming composition applied is not particularly limited, but the wet film thickness is usually in the range of 10 nm to 200 μm, and preferably in the range of 20 nm to 100 μm.
[0097] After applying the copper thin film forming composition to the surface of the substrate to form a coating film of the copper thin film forming composition (copper thin film forming composition layer), it is preferable to allow it to stand for a certain period of time, from the viewpoint of forming a denser film. The standing time is preferably 6 hours or more, and more preferably 12 hours or more, at room temperature (25°C). By allowing the copper thin film forming composition layer formed on the substrate to stand, the copper contained in the copper thin film forming composition is adsorbed onto the substrate to form a copper thin film. There is no particular upper limit to the standing time, but considering productivity, it can be 120 hours or less, and 90 hours or less is preferable.
[0098] Furthermore, when applying the copper thin film forming composition to the surface of a substrate to form a layer of the copper thin film forming composition and then allowing it to stand, the reaction rate can be increased by setting the ambient temperature of the standing area and the liquid temperature of the formed copper thin film forming composition layer to above room temperature, for example, 30°C or higher, preferably 40°C or higher. This allows for the formation of a dense copper thin film in a shorter standing time. From the viewpoint of minimizing the impact on the copper thin film forming composition, a temperature of 80°C or lower is preferred. For example, when the ambient temperature is 35°C, a standing time of 4 hours or more is preferred, and 8 hours or more is more preferred. The upper limit of the standing time is the same as in the case of room temperature. After the copper thin film is formed, any remaining copper thin film forming composition may be removed.
[0099] The thickness of the copper thin film layer formed on the substrate is not particularly limited and can be appropriately controlled by the amount of copper thin film forming composition applied to the substrate, the composition of the copper thin film forming composition, the contact time between the copper thin film forming composition and the substrate (standing time of the copper thin film forming composition layer), etc. From the viewpoint of balancing the imparting of heat generation in the heating element, the flexibility of the laminate design, and the manufacturing cost, the thickness of the copper thin film layer is usually 10 nm to 100 μm, preferably 20 nm to 50 μm, 50 nm to 30 μm, 100 nm to 20 μm, or 200 nm to 10 μm.
[0100] (Drying step) The present method for producing copper thin films may further include other steps in addition to steps I, II, and III. Other steps include, for example, a step of drying the copper thin film forming composition applied in step III.
[0101] The solvent contained in the copper thin film forming composition can be removed by drying, allowing a copper thin film to be formed on the substrate. Drying includes natural drying at room temperature. Furthermore, by performing heat drying or other methods on the copper thin film forming composition as described later, a copper thin film that adheres more closely to the substrate can be formed more quickly than with natural drying. Here, drying refers to reducing the amount of solvent contained in the copper thin film forming composition, and does not necessarily mean completely removing the solvent.
[0102] Drying can be carried out by conventional methods. In addition to the aforementioned natural drying, drying methods include heat drying and drying by blowing air. When natural drying is performed, it is sufficient to leave it at room temperature for 60 minutes to 5 hours. When heat drying is performed, known heating methods can be appropriately selected and applied. Examples of heating methods include contacting the substrate with a heating means such as a plate heater or heat roll from the back surface, passing it through a heating zone such as an electric furnace, irradiating it with energy rays such as infrared rays or microwaves, and blowing hot air. There are no particular restrictions on the heating temperature when heat drying. Considering drying efficiency and minimizing the impact on the substrate, the heating temperature can be in the range of 30°C to less than 100°C, and is preferably in the range of 30°C to 60°C. When heat drying, the drying time is preferably in the range of 10 seconds to 20 minutes from the viewpoint of productivity.
[0103] The process of applying the copper thin film forming composition to a substrate and drying the copper thin film forming composition applied to the substrate may be repeated multiple times. By applying the copper thin film forming composition to the substrate and then drying the copper thin film forming composition, a copper thin film is formed on the substrate. Subsequently, when the copper thin film forming composition is applied again to the substrate on which the copper thin film has been formed, the copper precursor contained in the copper thin film forming composition is adsorbed onto the surface of the copper thin film formed on the substrate. By drying it thereafter, a thicker copper thin film is formed.
[0104] When a copper thin film forming composition is applied to a substrate on which a copper thin film has already been formed, the copper thin film forming composition comes into contact with the already formed copper thin film. Copper precursors contained in the copper thin film forming composition adhere between the copper particles contained in the already formed copper thin film, causing copper nanoparticles to grow and accelerating copper deposition. As a result, the copper nanoparticles contained in the copper thin film become more densely packed, which is expected to improve not only the thickness of the copper thin film but also its physical properties, such as electrical conductivity.
[0105] According to this manufacturing method, small amounts of solvent-derived impurities may remain in the copper thin film, but these are mainly carbon atoms derived from the solvent used as a raw material, and there is no concern that they will impair the properties of the formed copper thin film. This is a significant advantage compared to electroless plating films that require catalysts, and copper thin films formed by precursor methods using anionic copper complexes.
[0106] According to this manufacturing method, a copper thin film can be uniformly formed over the entire surface of the substrate. Furthermore, a copper thin film can also be formed in a patterned manner. As described above, a patterned copper thin film can be formed by applying a copper thin film forming composition to the substrate in an arbitrary pattern using a printing method. As a method for forming a patterned copper thin film, another method is to form a uniform copper thin film on the substrate and then pattern it using a known method such as etching to form a patterned copper thin film.
[0107] In this manufacturing method, instead of the copper thin film forming composition, the above-mentioned single-walled carbon nanotubes and SiO 2 By using a solution containing a composite of the two, a single-walled carbon nanotube-SiO2 can be used as a conductive thin film layer. 2 A thin film layer can be formed on a substrate. The conductive thin film layer can be made of single-walled carbon nanotube-SiO2. 2 One non-limiting example of a method for forming a thin film layer on a substrate is single-walled carbon nanotubes and SiO 2 100 μL of the solution containing the complex is pipetteed onto a quartz glass substrate (20 × 20 mm) 2 The material is dropped onto a surface, followed by a two-step spin coating method (first step: 500 rpm for 5 seconds, second step: 2000 rpm for 30 seconds) to form a thin film, and then dried at 70°C for 10 minutes to form single-walled carbon nanotubes-SiO2. 2 Thin films can be formed. These manufacturing conditions can be appropriately adjusted according to the desired thickness of the thin film, etc.
[0108] 5. Method for Manufacturing Residential Thermal Tiles A residential thermal tile can be obtained by using any of the residential heating elements described above and laminating (1) a decorative sheet, (2) a middle backer, (3) a residential heating element, (4) a middle backer, and (5) a bottom backer in this order. Any of the above-described components can also be used for the (1) decorative sheet, (2) and (4) middle backers, and (5) bottom backer that make up the residential thermal tile.
[0109] The method for obtaining a residential thermal tile by laminating (1) a decorative sheet, (2) a middle backer, (3) a residential heating element, (4) a middle backer, and (5) a bottom backer in this order is not particularly limited, and any method known in the industry may be used. For example, a first partial laminate of (1) a decorative sheet and (2) a middle backer (and a clear layer optionally provided on the surface side of (1) the decorative sheet) may be formed in advance by any lamination method known in the industry, and a second partial laminate of (4) a middle backer and (5) a bottom backer may be formed in advance. Then, the (2) middle backer side of the first partial laminate may face one side of the residential heating element, and the (4) middle backer side of the second partial laminate may face the other side of the residential heating element, and then heat laminate (hot press) may be performed. In this case, a heat-resistant adhesive may be optionally interposed between the layers before heat lamination (hot press). The temperature, time, and other conditions for the thermal lamination process can be appropriately selected from suitable conditions known in the industry. The heat-resistant adhesive for thermal lamination is not particularly limited, but examples include one or more mixtures of epoxy resins, polyimide resins, silicone resins, etc.
[0110] In particular, as described above, in the case of the (3) residential heating element according to the second embodiment, if one or more holes are formed in the (a) conductive thin film layer, the plastic sol or hot melt adhesive of the (b) layer, which is softened and melted by heating, can penetrate these holes, thereby joining and bonding the (3) residential heating element to the (2) middle backer positioned above it. In addition, the plastic sol or hot melt adhesive of the (d) layer, which is softened and melted by heating in the (3) residential heating element, can join and bond the (3) residential heating element to the (4) middle backer positioned below it. When obtaining the residential thermal tile, in addition to the clear layer and heat-resistant adhesive layer provided as described above, any other arbitrary layer may be further arranged between any of the layers as needed.
[0111] Furthermore, residential thermal tiles can be formed to cover a predetermined area to be heated by joining together multiple thermal tile pieces, each having a roughly square or rectangular planar shape with a side length in the range of approximately 100 mm to approximately 1500 mm, typically in the range of approximately 150 mm to approximately 900 mm. The size of the planar shape of the thermal tile pieces may be, for example, roughly square or rectangular, such as approximately 300 mm x approximately 300 mm, approximately 450 mm x approximately 450 mm, approximately 900 mm x approximately 900 mm, or approximately 150 mm x approximately 900 mm. The installation of residential thermal tiles according to the present invention is not particularly limited, but can be carried out by methods such as those described below. In addition, a combination of these methods can be used. (I) One or more electrode wires may be inserted from the bottom side (floor side) of each thermal tile piece toward the surface opposite the bottom side, to the bottom backer (5), the middle backer (4), and the conductive thin film layer (a) of the residential heating element (3), and the lower ends of the electrode wires inserted in each thermal tile piece may be connected to each other. This allows electrode wires to be spread throughout the entire thermal tile consisting of multiple pieces. (II-a) A thin copper tape (e.g., about 0.2 mm to about 0.3 mm thick) may be applied continuously to substantially the entire periphery (e.g., about 5 mm to about 10 mm wide) of the surface of the conductive thin film layer (a) of the residential heating element (3) on the (2) side of each thermal tile piece, and to substantially the entire side surface of the conductive thin film layer (a). This allows the thin copper tape to function as an electrode on each thermal tile piece, ensuring reliable electrical connection of the conductive thin film layers of each heating element throughout the thermal tile consisting of multiple pieces. (II-b) On the side of each thermal tile piece opposite to the conductive thin film layer (a) of the heating element for residential use (the bottom side), a further conductive thin film layer may be provided so as to be in contact with the surface of the (c) fiber layer or mesh layer or the (d) plastic sol layer or hot melt adhesive layer.Furthermore, a thin copper tape (e.g., approximately 0.2 mm to approximately 0.3 mm thick) may be applied continuously to substantially the entire peripheral edge (e.g., approximately 5 mm to approximately 10 mm wide) of the middle backer side surface of the former (a) conductive thin film layer, substantially the entire peripheral edge (e.g., approximately 5 mm to approximately 10 mm wide) of the middle backer side surface of the latter's further conductive thin film layer, and substantially the entire side surface of the laminate including the former (a) conductive thin film layer and the latter's further conductive thin film layer. This allows the thin copper tape to function as an electrode on each thermal tile piece, making the electrical connection of the conductive thin film layers of each heating element more reliable throughout the thermal tile consisting of multiple pieces. (III-a) Each thermal tile piece may be laminated such that two sides of the (a) conductive thin film layer (approximately square or rectangular planar shape) of the (3) residential heating element are exposed by a predetermined width (for example, about 5 mm to about 10 mm) to the corresponding two sides of the (2) middle backer and the (c) fiber layer or mesh layer or (b) plastic sol layer or hot melt adhesive layer of the (3) residential heating element. By joining thermal tile pieces with partially exposed conductive thin film layers to each other to form a thermal tile, the electrical connection of the conductive thin film layer of each heating element can be made reliable. (III-b) Each thermal tile piece may be provided on the side opposite to the (a) conductive thin film layer of the (3) residential heating element (bottom side), in contact with the surface of the (c) fiber layer or mesh layer or the (d) plastic sol layer or hot melt adhesive layer. Furthermore, the former (a) conductive thin film layer (approximately square or rectangular planar shape) may be laminated such that two sides are exposed to the corresponding two sides of (2) the middle backer and the corresponding two sides of the (c) fiber layer or mesh layer or (b) plastic sol layer or hot melt adhesive layer of the (3) housing heating element by a predetermined width (for example, about 5 mm to about 10 mm), while the latter further conductive thin film layer (approximately square or rectangular planar shape) may be laminated such that two sides are exposed to the corresponding two sides of (4) the middle backer and the corresponding two sides of the (c) fiber layer or mesh layer or (d) plastic sol layer or hot melt adhesive layer of the (3) housing heating element by a predetermined width (for example, about 5 mm to about 10 mm).In this case, the exposed edges of the former conductive thin film layer and the exposed edges of the latter further conductive thin film layer may be in corresponding directions, or they may be in partially different directions. By joining together these two partially exposed conductive thin film layers to form a thermal tile, the electrical connection of the conductive thin film layers of each heating element can be made even more reliable.
[0112] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0113] Measurement of the Surface Temperature of the Heating Element To measure the surface temperature of the heating element (the conductive thin film layer that makes up the surface), the following thermometer was used: Shinwa Measuring Instruments Co., Ltd. infrared thermometer with laser point function; Measurement range: -60 to 500°C; Distance coefficient D:S = 12:1 (D = distance, S = measurement range diameter); Material: ABS resin; Dimensions: 185 mm x 46 mm x 143 mm; Weight: 240 g; Power supply: 2 AAA alkaline batteries; Accuracy: ±2% or ±2 (the higher value is applied); Battery life: 14 hours continuous use; Laser wavelength: 635-660 nm
[0114] Example 1: Example of production of a heating element by forming a copper thin film on glass fiber. 67.4 g of copper sulfate pentahydrate was added to 1161 ml of pure water and stirred at room temperature for 5 minutes. 109.3 ml of aqueous ammonia was then added and stirred at room temperature for 1 hour to obtain an aqueous copper complex solution (copper precursor solution). Furthermore, 161.7 g of L-ascorbic acid was added to this aqueous copper complex solution as an organic reducing agent and stirred at room temperature for 20 minutes to obtain a copper thin film forming composition (Cu 2+ A concentration of 0.18 mmol / g was obtained. (100 x 100 mm) 2A 100 μm thick coupling agent-treated urethane sol coated glass fiber film (raw fabric cloth M95F107 obtained from Unitika Ltd.) was immersed in IPA (isopropyl alcohol), washed by two 15-minute ultrasonic irradiations, and dried in a 70°C dryer for 10 minutes. The washed glass fiber film was immersed in a container (24 mm deep) containing the above-mentioned copper thin film forming composition and left to stand in a 24°C incubator for 24 hours. Next, this coated glass fiber film was immersed in 1 L of pure water and shaken for 1 minute, and this operation was repeated three times. Then, it was dried in a 70°C dryer for 1 hour to obtain a heating element in which a copper thin film layer was formed on the glass fiber film layer.
[0115] When a predetermined voltage was applied to this copper thin film layer and the surface temperature was measured after 10 minutes, the following results were obtained. For voltages of 1.5V, 2.5V, and 3.0V, the temperature reached a substantially constant level after 5 minutes. Furthermore, for a voltage of 3.5V, the temperature exceeded approximately 45°C after 5 minutes, and for a voltage of 4.0V, the temperature exceeded approximately 50°C after 5 minutes. 1.5V - Surface temperature after 10 minutes: 28°C 2.5V - Surface temperature after 10 minutes: 37°C 3.0V - Surface temperature after 10 minutes: 42°C 3.5V - Surface temperature after 10 minutes: 50°C 4.0V - Surface temperature after 10 minutes: 60°C
[0116] Example 2: Single-walled carbon nanotubes-SiO2 onto glass fiber 2 Examples of manufacturing a heating element by thin film formation: By the following operation including spin coating, single-walled carbon nanotubes - SiO 2 A complex was obtained. 10 g of ethanol was mixed with 5.2 g of oxalic acid (anhydrous) and stirred at room temperature for 30 minutes. 4.0 g of tetraethoxysilane was added and refluxed for 1 hour to obtain SiO₂ 2 Thin film forming composition (Si 4+ A concentration of 1.0 mmol / g was obtained. 3.0 g of a single-walled carbon nanotube ethanol dispersion solution (0.2 wt%) was mixed with the SiO obtained above. 2 Add 0.5 g of the thin film forming composition and 1.5 g of ethanol, and stir at room temperature for 1 hour to form single-walled carbon nanotubes - SiO 2A composition for forming a thin film was obtained. 100 x 100 mm 2 A 100 μm thick coupling agent-treated urethane sol coated glass fiber film (raw fabric cloth M95F107 obtained from Unitika Ltd.) was immersed in IPA (isopropyl alcohol), washed with two 15-minute ultrasonic irradiations, and dried in a 70°C dryer for 10 minutes. 2 ml of ethanol was applied to the surface of the washed glass fiber film using a two-stage spin coating method: 500 rpm for 5 seconds, followed by 2000 rpm for 30 seconds. Herein, the single-walled carbon nanotube-SiO2 obtained above was applied. 2 Two ml of the thin-film forming composition was applied by spin coating at 500 rpm for 10 seconds, then dried in a 70°C oven for 10 minutes, and single-walled carbon nanotubes-SiO₂ were placed on the glass fiber film layer. 2 A heating element with a thin film layer was obtained. This single-walled carbon nanotube-SiO 2 When a predetermined voltage was applied to a thin film layer and the surface temperature was measured after 10 minutes, the following results were obtained. For voltages of 10V, 20V, and 30V, the temperature reached a substantially constant level after 5 minutes. Voltage 10V - Surface temperature after 10 minutes: 24°C Voltage 20V - Surface temperature after 10 minutes: 28°C Voltage 30V - Surface temperature after 10 minutes: 37°C
[0117] Comparative Example 1: In Example 1, instead of glass fiber, a stainless steel mesh plate (10 mesh, 0.4 mm thick) purchased from MonotaRO (MonotaRO Co., Ltd., an online sales site for indirect materials for factories for businesses) was cut to 100 mm x 100 mm and used to obtain a heating element. This heating element was heat-laminated and had good adhesion to the backing material, but it had a low resistance and did not generate heat.
[0118] Comparative Example 2: In Example 1, instead of glass fiber, a copper mesh (200 mesh, 0.077 mm opening) purchased from Monotaro was used to obtain a heating element. This heating element was heat-laminated and had good adhesion to the backing material, but it had a low resistance and did not generate heat.
[0119] Comparative Example 3: In Example 1, instead of glass fiber, a transparent film heater without adhesive (double-sided PET) measuring 100 mm x 100 mm (terminal treatment: lug terminals attached to two electrode locations, thickness: 0.14-0.2 mm) purchased from Monotaro was used to obtain a heating element. In this heating element, the transparent film heater deformed during the thermal lamination process, and the adhesion to the backer material was also insufficient.
[0120] Comparative Example 4: In Example 1, instead of glass fiber, an aluminum foil heater (15W capacity, 100 x 100 mm) purchased from Monotaro was used to obtain a heating element. This heating element had insufficient adhesion to the backing material, resulting in unevenness on the surface which impaired the aesthetic appearance of the tile.
[0121] As demonstrated by the embodiments of the present invention described above, a residential heating element that provides sufficient heat with low power and has high energy efficiency can be obtained by a simple method. Such a residential heating element can be suitably used to construct articles such as residential thermal tiles with excellent design by laminating decorative sheets via a middle backer.
[0122] 1: Conductive thin film layer 2: Polyvinyl chloride sol layer or hot melt adhesive layer 3: Fiber layer or mesh layer 4: Polyvinyl chloride sol layer or hot melt adhesive layer 100: Heating element for residential use 10: Decorative sheet 20: Middle backer 100a: Heating element for residential use 30: Middle backer 40: Bottom backer 200: Thermal tile for residential use
Claims
1. A residential heating element comprising (a) a conductive thin film layer and (c) a fiber layer or mesh-like layer, wherein the conductive thin film layer (a) is a copper thin film or a single-walled carbon nanotube-SiO 2 A heating element for residential use, comprising a thin film layer, wherein the (c) fibrous layer or mesh-like layer is formed from a material containing at least one selected from glass fibers and ceramic mesh.
2. The heating element for residential use according to claim 1, wherein (a) a conductive thin film layer, (b) a plastic sol layer or hot melt adhesive layer, (c) a fiber layer or mesh-like layer, and (d) a plastic sol layer or hot melt adhesive layer are laminated in this order.
3. The heating element for residential use according to claim 2, wherein the (b) plastic sol layer or hot melt adhesive layer and / or the (d) plastic sol layer or hot melt adhesive layer are integrated with the (c) fiber layer or mesh-like layer, so that at least a portion of the surface of the fiber or mesh-like material constituting layer (c) is covered with the plastic sol or hot melt adhesive constituting layers (b) and / or (d).
4. The heating element for residential use according to claim 1, wherein the conductive thin film layer (a) is a thin film layer having a thickness of 10 nm to 100 μm, which is produced by a molecular precursor method.
5. An article comprising a heating element for residential use as described in any one of claims 1 to 4.
6. The article according to claim 5, having at least one use selected from heating, heat retention, snow melting, condensation prevention, and anti-fogging.
7. A residential thermal tile comprising (1) a decorative sheet, (2) a middle backer, (3) a residential heating element according to any one of claims 2 to 4, (4) a middle backer, and (5) a bottom backer, laminated in this order.
8. A method for manufacturing a heating element for residential use, comprising the steps of: (c) forming a conductive thin film layer (a) on a substrate including a fibrous layer or a mesh-like layer by a molecular precursor method to obtain a heating element for residential use which is a laminate including the conductive thin film layer (a) and the fibrous layer or mesh-like layer, wherein the conductive thin film layer (a) is a copper thin film or a single-walled carbon nanotube-SiO 2 A method for manufacturing a heating element for residential use, wherein the (c) fibrous layer or mesh-like layer is a thin film layer, and the fibrous layer or mesh-like layer is formed from a material containing at least one selected from glass fibers and ceramic mesh.
9. The method according to claim 8, wherein the substrate containing the (c) fibrous layer or mesh-like layer is a laminated substrate containing (b) a plastic sol layer or hot melt adhesive layer, the (c) fibrous layer or mesh-like layer, and (d) a plastic sol layer or hot melt adhesive layer in this order.
10. A method for manufacturing a residential thermal tile, comprising using a residential heating element manufactured by the method of claim 8 or claim 9, and stacking (1) a decorative sheet, (2) a middle backer, (3) the residential heating element, (4) a middle backer, and (5) a bottom backer in this order to obtain a residential thermal tile.