Separator for alkaline water electrolysis, alkaline water electrolysis cell, and alkaline water electrolysis device
The alkaline water electrolysis separator addresses the challenge of distinguishing between anode and cathode sides by incorporating a visual reflectance difference and multilayer polymer structure, enhancing discriminability and gas barrier properties for improved cell performance.
Patent Information
- Application Number
- PCT/JP2026/015633
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-04-17
- Publication Date
- 2026-11-12
AI Technical Summary
Existing alkaline water electrolysis separators face challenges in distinguishing between the anode and cathode sides during assembly, affecting proper adhesion and gas barrier properties.
The separator features a visual reflectance difference of 0.1% or more between its surfaces, achieved through differences in visual reflectance and transmittance, along with distinct pore diameters and a multilayer polymer structure, ensuring clear differentiation between the sides.
This design enhances the discriminability and workability of the separator, allowing for proper adhesion to electrodes and maintaining effective gas barrier properties, thereby improving the performance of alkaline water electrolysis cells.
Smart Images

Figure JP2026015633_12112026_PF_FP_ABST
Abstract
Description
Separator for alkaline water electrolysis, alkaline water electrolysis cell, and alkaline water electrolysis apparatus
[0001] This disclosure relates to a separator for alkaline water electrolysis, an alkaline water electrolysis cell, and an alkaline water electrolysis apparatus.
[0002] Hydrogen is a clean energy source that does not emit carbon dioxide and is used, for example, as fuel for fuel cell vehicles and household fuel cells. Alkaline water electrolysis, which uses a highly concentrated alkaline aqueous solution as an electrolyte, is a known method for producing hydrogen. By using a renewable energy power generation system as the power source for alkaline water electrolysis, hydrogen can be produced without emitting carbon dioxide, and therefore hydrogen is attracting increasing attention as a fundamental energy source for a sustainable society.
[0003] In alkaline water electrolysis, the bubble-like hydrogen (2H) generated at the cathode is produced. 2 O + 2e - →H 2 +2OH - This prevents the oxygen (4OH) from moving to the anode, and also prevents the bubble-like oxygen (4OH) generated at the anode from moving to the anode. - →O 2 +2H 2 O+4e - To prevent the gas from moving towards the cathode, a gas barrier separator is placed between the cathode and the anode.
[0004] Patent Document 1 describes an alkali hydrolysis-reinforced separator comprising a porous support, a first porous polymer layer adjacent to one side of the support, and a second porous polymer layer adjacent to the opposite side of the support, characterized in that the maximum pore diameter of the outer surface of the first porous polymer layer (PDmax(1)) and the maximum pore diameter of the outer surface of the second porous polymer layer (PDmax(2)) are different from each other, and the ratio of PDmax(2) / PDmax(1) is 1.25 to 10.
[0005] Patent Document 1: Japanese Patent Publication No. 2020-527193
[0006] When assembling alkaline water electrolysis separators by placing them on electrodes, it was sometimes difficult to distinguish between the side of the separator that adheres to the anode electrode and the side that adheres to the cathode electrode. Depending on the alkaline water electrolysis separator, proper adhesion to the anode and cathode electrodes can ensure adequate gas barrier properties. Therefore, there were cases where it was necessary to distinguish between the two sides of the alkaline water electrolysis separator.
[0007] The object of one embodiment of this disclosure is to provide an alkaline water electrolysis separator with excellent double-sided identification. The object of another embodiment of this disclosure is to provide an alkaline water electrolysis cell and an alkaline water electrolysis apparatus using the above-mentioned alkaline water electrolysis separator.
[0008] This disclosure includes the following embodiments: <1> An alkaline water electrolysis separator wherein the difference in visual reflectance measured by a color densitometer between one surface and the other surface is 0.1% or more. <2> The alkaline water electrolysis separator according to <1>, wherein the difference in visual reflectance is 10% or less. <3> The alkaline water electrolysis separator according to <1> or <2>, wherein the visual transmittance measured by a color densitometer is 15% or more. <4> The alkaline water electrolysis separator according to any one of <1> to <3>, wherein one surface and the other surface each have pores, and the average pore diameter of the pores on one surface and the pores on the other surface are different. <5> The alkaline water electrolysis separator according to any one of <1> to <4>, comprising a support base material which is a woven fabric or nonwoven fabric, and a porous polymer layer which embeds at least a part of the support base material. <6> The alkaline water electrolysis separator according to <5>, wherein the distance between the thickness position where the alkaline water electrolysis separator has a thickness of 50% and the thickness position where the support substrate has a thickness of 50% is within the range of 3% to 25% of the thickness of the alkaline water electrolysis separator. <7> The alkaline water electrolysis separator according to <5>, wherein the porous polymer layer contains a coloring agent, and in the thickness direction of the alkaline water electrolysis separator, the content of the coloring agent contained in a first region from one surface of the alkaline water electrolysis separator to the thickness position where the alkaline water electrolysis separator has a thickness of 50% is different from the content of the coloring agent contained in a second region other than the first region of the alkaline water electrolysis separator. <8> The alkaline water electrolysis separator according to any one of <5> to <7>, wherein the porous polymer layer comprises a first porous polymer layer disposed on one side of the support substrate and a second porous polymer layer disposed on the other side of the support substrate. <9> A separator for alkaline water electrolysis according to any one of <1> to <8>, having a thickness of 250 μm or less. <10> An alkaline water electrolysis cell comprising the separator for alkaline water electrolysis according to any one of <1> to <9>. <11> An alkaline water electrolysis apparatus comprising the alkaline water electrolysis cell according to <10>.
[0009] According to one embodiment of the present disclosure, an alkaline water electrolysis separator with excellent double-sided discriminability is provided. According to another embodiment of the present disclosure, an alkaline water electrolysis cell and an alkaline water electrolysis apparatus using the above-mentioned alkaline water electrolysis separator are provided.
[0010] Figure 1 is a schematic diagram illustrating a preferred embodiment of the alkaline water electrolysis system of the present disclosure.
[0011] The contents of this disclosure will be described in detail below. The descriptions of constituent elements described below may be based on representative embodiments of this disclosure, but this disclosure is not limited to such embodiments. In this specification, the "~" indicating a numerical range is used to mean that the numbers described before and after it are the lower and upper limits. In numerical ranges described in stages in this disclosure, the upper or lower limit described in one numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Also, in numerical ranges described in this disclosure, the upper or lower limit of that numerical range may be replaced with the values shown in the examples. Furthermore, the term "process" in this specification is included not only in the case of an independent process, but also in the case of a process that is not clearly distinguishable from other processes, as long as the intended purpose of that process is achieved. Furthermore, in this disclosure, a combination of two or more preferred embodiments is a more preferred embodiment.
[0012] [Separator for Alkaline Water Electrolysis] The separator for alkaline water electrolysis of this disclosure (hereinafter also referred to as "separator") is a separator used in alkaline water electrolysis. Alkaline water electrolysis refers to the electrolysis of water using an alkaline aqueous solution as an electrolyte to produce hydrogen and oxygen.
[0013] The separator of this disclosure has a visual reflectance difference of 0.1% or more as measured by a color densitometer.
[0014] In alkaline water electrolysis devices, alkaline water electrolysis cells are sometimes used in which electrodes and separators are bonded together. However, conventionally, it has been difficult to distinguish between the surface bonded to the anode electrode and the surface bonded to the cathode electrode when bonding the electrodes and separators. The separator of this disclosure has excellent distinguishability between both surfaces because the difference in visual reflectance measured by a color densitometer between one surface and the other surface is 0.1% or more. It also offers excellent workability when bonding the electrodes and separators, and when providing a catalyst layer on top of the separator.
[0015] Patent Document 1 does not contain any description that focuses on the difference in visual reflectance between the two sides of the separator.
[0016] <Visual Reflectance> The separator of this disclosure has a difference of 0.1% or more in visual reflectance between one surface and the other surface, as measured with a color densitometer. The separator is usually in the form of a film and has two surfaces. "Surface" means the surface with a relatively larger area among the constituent surfaces of the film.
[0017] A difference of 0.1% or more in visual reflectance allows for distinction between one of the pair of surfaces, resulting in excellent discriminability.
[0018] The difference in visual reflectance is 0.1% or more, preferably 0.5% or more, and more preferably 1.5% or more.
[0019] From the viewpoint of making defects such as pinholes easier to see, the difference in visual reflectance is preferably 25% or less, more preferably 15% or less, and even more preferably 10% or less. That is, the difference in visual reflectance is preferably 0.1% to 25%, more preferably 0.5% to 25%, and even more preferably 1.5% to 15%. Furthermore, the difference in visual reflectance is preferably 0.1% to 15%, more preferably 0.5% to 15%, even more preferably 1.5% to 15%, and most preferably 1.5% to 10%.
[0020] On both sides of the separator, the relatively higher visual reflectance is preferably 40% to 95%, more preferably 50% to 90%. On both sides of the separator, the relatively lower visual reflectance is preferably 20% to 90%, more preferably 30% to 80%.
[0021] The visual reflectance is measured using a color densitometer that indicates optical density based on the ratio of the amount of reflected light detected by a sensor to the amount of irradiated light. As the color densitometer, for example, "X-rite 310TR" manufactured by X-rite Inc. is used. Specifically, black paper is laid under the separator, and the reflection visual density is measured using a color densitometer. The visual reflectance is calculated using the following formula. Visual reflectance (%) = 100 / 10 A A is the reflection visual density. The difference in visual reflectance is calculated from the visual reflectance of both sides.
[0022] The difference in visual reflectance can be adjusted by adding a colorant such as carbon black to one side, or by changing the center position of the colored support substrate in the separator.
[0023] <Visual Transmittance> The separator of the present disclosure preferably has a visual transmittance of 15% or more as measured by a color densitometer.
[0024] When the visual transmittance is 15% or more, defects such as pinholes on the surface of the separator are easily visible.
[0025] The visual transmittance is preferably 15% or more, more preferably 20% or more. From the viewpoint of ensuring sufficient gradation, the visual transmittance is preferably 50% or less, more preferably 30% or less. That is, the visual transmittance is preferably 15% to 50%, more preferably 20% to 50. Further, the visual transmittance is preferably 15% to 30%, more preferably 20% to 30%.
[0026] The visual transmittance is measured using a color densitometer that indicates optical density based on the ratio of the amount of transmitted light detected by a sensor to the amount of irradiated light. As the color densitometer, for example, "X-rite 310TR" manufactured by X-rite Inc. is used. Specifically, the separator is set in the color densitometer, and the transmitted visual density is measured. The visual transmittance is calculated using the following formula. Visual transmittance (%) = 100 / 10 B B is the transmitted visual density.
[0027] The configuration of the separator of the present disclosure is not particularly limited as long as the difference in visual reflectance measured by a color densitometer between one surface and the other surface is 0.1% or more.
[0028] The visual transmittance can be adjusted by adding a colorant such as carbon black, changing the aperture ratio of the support substrate, or changing the coloring degree of the support substrate.
[0029] The separator of the present disclosure preferably includes a support substrate which is a woven fabric or a nonwoven fabric, and a porous polymer layer embedding at least a part of the support substrate.
[0030] Since the support substrate has voids, the porous polymer layer may be formed inside the support substrate. The porous polymer layer may cover at least a part of the outer surface of the support substrate. In the separator, at least a part of the support substrate may be exposed on the surface. Alternatively, the support substrate may not be exposed and may be embedded in the separator. Above all, from the viewpoint of the durability of the separator, the support substrate is preferably embedded in the separator.
[0031] The porous polymer layer embedding the support substrate may be a single layer, or may have a multilayer structure including a first porous polymer layer disposed on one side of the support substrate and a second porous polymer layer disposed on the other side of the support substrate. The first porous polymer layer and the second porous polymer layer refer to different layers, and may be layers different from each other in the type or content of contained components.
[0032] (Supporting material) The supporting material is a woven or nonwoven fabric. The opening ratio of the supporting material is preferably 30% to 80%, more preferably 40% to 70%. The opening ratio is the ratio of the area of voids to the area of a unit area when the supporting material is viewed from above.
[0033] Examples of polymers constituting the supporting substrate include polypropylene, polyethylene, polysulfone, polyphenylene sulfide, polyamide, polyethersulfone, polyphenylsulfone, polyethylene terephthalate, polyetheretherketone, sulfonated polyetheretherketone, monochlorotrifluoroethylene, copolymer of ethylene and tetrafluoroethylene or chlorotrifluoroethylene, polyimide, polyetherimide, and m-aramid.
[0034] In particular, the polymer constituting the support substrate preferably includes at least one selected from the group consisting of polypropylene, polyphenylene sulfide, and polyether ether ketone, and more preferably includes at least one selected from the group consisting of polyphenylene sulfide and polyether ether ketone.
[0035] The thickness of the support substrate is preferably 30 μm to 150 μm, more preferably 30 μm to 100 μm, and even more preferably 30 μm to 75 μm.
[0036] The thickness of the support substrate is measured using a constant-pressure thickness measuring instrument compliant with JIS (Japanese Industrial Standards) K6250 (2019). For the support substrate within the separator, the support substrate is removed from the separator using a solvent that dissolves components other than the support substrate, and the thickness of the removed support substrate is measured.
[0037] (Porous polymer layer) The porous polymer layer has the function of blocking the permeation of hydrogen gas and oxygen gas, while allowing hydroxyl ions to permeate.
[0038] The porous polymer layer contains a polymer. Various polymers applicable to the wet phase separation described later can be used as the polymer contained in the porous polymer layer.
[0039] Examples of polymers include fluororesins, olefin resins, polyester resins, aromatic hydrocarbon resins, polysulfones, polyethersulfones, polyphenylene sulfide, polyphenylsulfone, polyacrylates, polyetherimides, polyimides, and polyamideimides. The fluororesin is preferably at least one selected from the group consisting of polyvinylidene fluoride and polytetrafluoroethylene. The olefin resin is preferably polypropylene. The polyester resin is preferably at least one selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, and polybutylene naphthalate. The aromatic hydrocarbon resin is preferably polystyrene.
[0040] The polymer may be used individually or in combination of two or more types.
[0041] In particular, the polymer preferably contains at least one selected from the group consisting of polyvinylidene fluoride, polysulfone, polyethersulfone, and polyphenylsulfone, and more preferably contains at least one selected from the group consisting of polysulfone, polyethersulfone, and polyphenylsulfone.
[0042] The weight-average molecular weight (Mw) of the polymer is not particularly limited. However, from the viewpoint of the handling properties of the doping solution described later and the mechanical strength of the separator, the weight-average molecular weight (Mw) of the polymer is preferably 10,000 to 500,000, and more preferably 20,000 to 300,000.
[0043] In this disclosure, the weight-average molecular weight is measured under the following conditions. Instrument: HLC-8220GPC (Tosoh Corporation) Detector: Differential refractometer (RI (Refractive Index) detector) Pre-column: TSKGUARD COLUMN HXL-L 6mm x 40mm (Tosoh Corporation) Sample-side column: The following three columns are directly connected in order (all Tosoh Corporation): ・TSK-GEL GMHXL 7.8mm x 300mm ・TSK-GEL G4000HXL 7.8mm x 300mm ・TSK-GEL G2000HXL 7.8mm x 300mm Reference-side column: TSK-GEL G1000HXL 7.8mm x 300mm Oven temperature: 40℃ Mobile phase: THF (Tetrahydrofuran) Sample-side mobile phase flow rate: 1.0 mL / min Reference-side mobile phase flow rate: 1.0 mL / min Sample concentration: 0.1% by mass Sample injection volume: 100 μL Data acquisition time: 5 to 45 minutes after sample injection Sampling pitch: 300 milliseconds
[0044] The polymer content is preferably 5% to 50% by mass, more preferably 5% to 40% by mass, even more preferably 7% to 30% by mass, and particularly preferably 9% to 25% by mass, relative to the total amount of the porous polymer layer.
[0045] Furthermore, the polymer content is preferably 15% to 65% by volume, more preferably 25% to 60% by volume, even more preferably 35% to 55% by volume, and particularly preferably 35% to 50% by volume, relative to the total volume of the porous polymer layer.
[0046] The porous polymer layer preferably contains at least one inorganic particle in addition to the polymer.
[0047] From the viewpoint of alkali resistance, the inorganic particles are preferably at least one type of particle selected from the group consisting of metal oxides and metal hydroxides.
[0048] Examples of metal oxides include zirconium oxide, titanium oxide, bismuth oxide, cerium oxide, and magnesium oxide.
[0049] Examples of metal hydroxides include zirconium hydroxide, titanium hydroxide, bismuth hydroxide, cerium hydroxide, and magnesium hydroxide.
[0050] The inorganic particles may also be barium sulfate particles.
[0051] The median diameter (D50) of the inorganic particles is preferably 0.05 μm to 2.00 μm, more preferably 0.1 μm to 1.50 μm, even more preferably 0.15 μm to 1.00 μm, and particularly preferably 0.20 μm to 1.00 μm. The median diameter (D50) refers to the particle size at which the total volume of the particles is 100% and the cumulative volume is 50%. In this disclosure, the median diameter (D50) is measured using a dynamic image analysis device.
[0052] If the porous polymer layer contains inorganic particles, the inorganic particle content is preferably 50% to 95% by mass, more preferably 60% to 95% by mass, even more preferably 70% to 93% by mass, and particularly preferably 75% to 91% by mass, based on the total amount of the porous polymer layer.
[0053] When the porous polymer layer contains inorganic particles, the inorganic particle content is usually 35% by volume or more, preferably 40% by volume or more, more preferably 45% by volume or more, and even more preferably 50% by volume or more, relative to the total volume of the porous polymer layer. The inorganic particle content is preferably 85% by volume or less, more preferably 75% by volume or less, and even more preferably 65% by volume or less, relative to the total volume of the porous polymer layer. In other words, the inorganic particle content is preferably 35% to 85% by volume, more preferably 40% to 75% by volume, even more preferably 45% to 65% by volume, and particularly preferably 50% to 65% by volume, relative to the total volume of the porous polymer layer.
[0054] The inorganic particle content in the porous polymer layer is measured by the following method: The porous polymer layer is scraped from the separator, and the mass of organic matter and inorganic matter (inorganic particles) is quantified by thermal analysis. The inorganic particle content can be calculated using the densities of organic and inorganic matter described in publicly available data.
[0055] When the porous polymer layer contains inorganic particles, the ratio of inorganic particles to polymer content (inorganic particles / polymer) is preferably 10 / 1 to 1 / 1 by mass, more preferably 9 / 1 to 2 / 1, even more preferably 8 / 1 to 3 / 1, particularly preferably 7 / 1 to 4 / 1, and most preferably 6.5 / 1 to 4 / 1.
[0056] When the separator of this disclosure is manufactured using the doping solution described later, a certain amount of good solvent contained in the doping solution inevitably remains in the porous polymer layer. The total content of good solvent in the porous polymer layer is usually 0.01% by mass to 5.00% by mass.
[0057] The separator of this disclosure preferably has a thickness of 600 μm or less, more preferably 300 μm or less, and even more preferably 250 μm or less. The thickness can usually be 30 μm or more, preferably 50 μm or more, and more preferably 100 μm or more. That is, the thickness is preferably 30 μm to 600 μm, more preferably 50 μm to 300 μm, and even more preferably 100 μm to 250 μm.
[0058] The thickness of the separator is measured by the following method.
[0059] Samples are taken at five arbitrary points, and cross-sections are cut out with a razor. A cross-sectional SEM (scanning electron microscope) image is acquired at a magnification (e.g., 400x) that allows the separator cross-section to fit in a single field of view. In the obtained cross-sectional SEM image, assuming that no pores exist (for example, assuming that the pores are filled with polymer), the thickness is measured at 20 equally spaced points at each sampling point, and the arithmetic mean of the total of 100 measurements is adopted.
[0060] In the separator of this disclosure, the thickness position A, which is 50% of the thickness of the separator, and the thickness position B, which is 50% of the thickness of the support base material, may coincide. In this case, the support base material is positioned in the center in the thickness direction of the separator. Alternatively, in the separator of this disclosure, the above positions A and B may not coincide but be offset. In this case, it is preferable that the distance between position A and position B (hereinafter also referred to as "distance M") is 3% to 25% of the thickness of the separator.
[0061] "The thickness position where the separator thickness is 50%" refers to the center position in the thickness direction of the separator (hereinafter also referred to as "the center position of the separator thickness"). Similarly, "the thickness position where the support substrate thickness is 50%" refers to the center position in the thickness direction of the support substrate (hereinafter also referred to as "the center position of the support substrate thickness").
[0062] Furthermore, as described above, the support substrate is preferably embedded inside the separator, and according to the separator manufacturing method I described later, it is preferable that the support substrate is embedded substantially parallel to the surface of the separator. Here, substantially parallel means that the angle between the surface of the separator and the support substrate is within ±3°.
[0063] A distance M of 0 means that the center of the thickness of the support substrate coincides with the center of the thickness of the separator. A longer distance M means that the center of the thickness of the support substrate is further away from the center of the thickness of the separator. Also, if the distance M is approximately 50% of the separator's thickness, it means that the support substrate is located near the surface of the separator. The distance M is measured by the following method.
[0064] Cut the separator in the thickness direction. On the cut surface of the separator, draw a center line at the center of the separator's thickness (i.e., the point where 50% of the thickness is reached when moving from one surface of the separator to the other). Next, draw line A at the center of the support substrate's thickness (i.e., the point where 50% of the thickness is reached when moving from one surface of the support substrate to the other). Measure the length of the perpendicular lines drawn from line A to the center line at five equally spaced points, and use the average of the measured values as distance M.
[0065] The distance M is preferably 0% to 25%, more preferably 3% to 25%, and even more preferably 5% to 20%. When the distance M is 3% or more, the difference in visual reflectance is 0.1% or more, resulting in superior discriminability between the two sides. When the distance M is 25% or less, the flatness of the separator is superior.
[0066] In the separator of this disclosure, the porous polymer layer contains a colorant, and it is preferable that the content of the colorant in a first region from one surface of the separator to a thickness position of 50% of the separator's thickness in the thickness direction of the separator is different from the content of the colorant in a second region of the separator that is other than the first region.
[0067] The first and second regions are two regions that are virtually divided at the center of the separator's thickness. If the amount of colorant in the first region differs from the amount of colorant in the second region, the difference in visual reflectance becomes 0.1% or more, resulting in superior discriminability between the two sides.
[0068] For example, the coloring agent may be contained in both the first and second regions, but with different amounts of the coloring agent, or the coloring agent may be contained in only one of the first or second regions.
[0069] As the coloring agent, commonly known coloring agents are used. The hue of the coloring agent may be chromatic or black. Examples of coloring agents include carbon black, inorganic pigments, and metal catalysts.
[0070] From the viewpoint of gas barrier properties required for porous separators for alkaline water electrolysis, the separator of this disclosure preferably has a bubble point greater than 1 bar, and more preferably greater than 2 bar. The pore diameter and porosity of the pores in the separator of this disclosure should be adjusted to a range that satisfies the above-mentioned bubble point. The bubble point is determined by measuring using a palm porometer based on the bubble point test method described in ASTM (American Society for Testing and Materials) F316-86, and the pressure at which the first bubble is generated in the resulting wet curve is defined as the bubble point.
[0071] The pore diameter of the separator in this disclosure is preferably 10 nm to 1000 nm, more preferably 20 nm to 700 nm, and even more preferably 30 nm to 500 nm, from the viewpoint of exhibiting excellent ion permeability and excellent gas barrier properties. The pore diameter is determined by obtaining the pore diameter distribution from the insertion curve by the mercury intrusion method and taking the average value thereof. Note that the pore diameter referred to here means the pore diameter of the pores included in the entire separator and is distinct from the pore diameter of the pores on the separator surface described later.
[0072] The separator of this disclosure preferably has pores on one surface and on the other surface, and the average pore diameter of the pores on one surface is different from that of the other surface. By individually controlling the average pore diameter of both surfaces, ion permeability and gas barrier properties can be improved. Furthermore, since the separator of this disclosure has excellent distinguishability between its two surfaces, it is possible to distinguish between the surfaces of the separator with different average pore diameters.
[0073] The average pore diameter of the pores on the separator surface is determined by observing SEM images of 10 μm square fields of view on the separator surface in five different fields, determining the maximum Ferret diameter obtained by binary analysis for the pores present in each 10 μm square area, and taking the average value of these values.
[0074] The porosity of the separator in this disclosure is preferably 30% to 70%, more preferably 40% to 60%, from the viewpoint of exhibiting excellent ion permeability and excellent gas barrier properties. The porosity is a value calculated from the insertion curve by the mercury intrusion method.
[0075] The separator of this disclosure has an ionic resistance of 0.01 Ω·cm from the viewpoint of hydroxyl ion permeability. 2 ~0.30 Ω·cm 2 Preferably, 0.01 Ω·cm 2 ~0.15Ω·cm 2 This is more preferable. Ion resistance is a value measured by AC impedance method at 90°C with a circularly punched separator set in a cell.
[0076] The separator of this disclosure has a water permeability of 100 mL / (h·m) from the viewpoint of mass balance between the cathode and anode sides of the electrolyte. 2 ・bar)~2000mL / (h・m 2 A water permeability of 100 mL / (h·m) is preferred. Furthermore, from the viewpoint of not requiring operational modifications to the alkaline water electrolysis cell, such as changing the permeability of the electrolyte on the anode and cathode sides, a water permeability of 100 mL / (h·m) is preferred. 2 ・bar)~1000mL / (h・m 2 A pressure of 1 bar is more preferable. The permeability is calculated by setting a circularly punched separator in a filter holder and measuring the volume of liquid (mL) when a 30% potassium hydroxide aqueous solution is passed through the circular separator for 30 seconds under conditions of 90°C and a gauge pressure of 1 bar.
[0077] The separator of this disclosure can be preferably used as a separator in a pressurized alkaline water electrolysis system (separator for pressurized alkaline water electrolysis). The separator of this disclosure can also be used as a separator in an alkaline water electrolysis system used under normal pressure (separator for alkaline water electrolysis). The separator of this disclosure may be in the form of a long sheet wound into a roll, or it may be pre-cut into a predetermined shape according to the intended use, equipment, etc. Furthermore, the separator of this disclosure may be stored immersed in a preservation solution such as pure water. Alternatively, the separator of this disclosure may be stored as a dry film without being immersed in a preservation solution.
[0078] The method for manufacturing the separator of this disclosure is not particularly limited. The separator of this disclosure can be manufactured, for example, by forming a porous polymer layer by wet phase separation. For example, one method (hereinafter referred to as "manufacturing method I") includes forming the porous polymer layer by wet phase separation while the support substrate is placed in a coating film formed with a dope solution obtained by dissolving the polymer. This step yields a separator comprising a support substrate and a porous polymer layer that embeds at least a portion of the support substrate. Another method (hereinafter referred to as "manufacturing method II") includes forming the porous polymer layer by wet phase separation, which includes performing liquid induction phase separation on a coating film formed by casting a film-forming solution obtained by dissolving the polymer onto a release film, while the release film is peeled off. This step yields a separator composed of a porous polymer layer and not containing a support substrate.
[0079] (Doping solution) The doping solution may contain, for example, the polymer contained in the porous polymer layer and a solvent, and may also contain inorganic particles. Details of the polymer contained in the porous polymer layer are as described above. Details of the inorganic particles that may be contained in the doping solution are as described above.
[0080] The solvent contained in the doping solution in the wet phase separation can be any solvent that can dissolve the above polymer (a good solvent), and is preferably miscible with water. The solvent is preferably selected from N-methylpyrrolidone (NMP), N-ethylpyrrolidone (NEP), N-butylpyrrolidone (NBP), N,N-dimethylformamide (DMF), formamide, dimethyl sulfoxide (DMSO), N,N-dimethylacetamide (DMAC), acetonitrile, and mixtures thereof, with at least one of NMP and NBP being more preferred.
[0081] If the doped solution contains inorganic particles, the solvent content in the doped solution is preferably 10% to 85% by mass, more preferably 15% to 80% by mass, even more preferably 25% to 70% by mass, even more preferably 30% to 65% by mass, even more preferably 32% to 60% by mass, and even more preferably 35% to 50% by mass. If the doped solution does not contain inorganic particles, the solvent content in the doped solution is preferably 20% to 95% by mass, more preferably 25% to 90% by mass, even more preferably 30% to 80% by mass, even more preferably 40% to 80% by mass, even more preferably 45% to 75% by mass, and even more preferably 50% to 75% by mass.
[0082] If the doping solution contains inorganic particles, the polymer content in the doping solution is preferably 2% to 30% by mass, more preferably 4% to 20% by mass, even more preferably 5% to 15% by mass, and still more preferably 6% to 15% by mass. If the doping solution does not contain inorganic particles, the polymer content in the doping solution is preferably 2% to 30% by mass, more preferably 4% to 30% by mass, even more preferably 6% to 25% by mass, and still more preferably 8% to 20% by mass.
[0083] In this disclosure, inorganic particles are particles that exist dispersed in the dope solution without dissolving, and this dispersion state is also referred to as the dope solution. That is, the "solution" in dope solution refers to the state in which the polymer is dissolved in the solvent. When the dope solution contains inorganic particles, the content of inorganic particles in the dope solution is preferably 10% to 85% by mass, more preferably 15% to 80% by mass, even more preferably 20% to 70% by mass, and particularly preferably 25% to 60% by mass.
[0084] The doping solution may contain components other than the solvent, polymer, and inorganic particles. For example, in wet phase separation, to control the formation of pores in the porous polymer layer, the doping solution may contain polyhydric alcohols such as polyethylene glycol, polypropylene glycol, ethylene glycol, tripropylene glycol, and glycerol; dibutyl phthalate, diethyl phthalate, diundecyl phthalate, isononanoic acid or neodecanoic acid, polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl acetate, polyethyleneimine, polyacrylic acid, methylcellulose, dextran, calcium chloride, magnesium chloride, lithium chloride, etc.
[0085] If the doping solution contains other components and inorganic particles, the total content of the other components in the doping solution is preferably 0.1% to 15% by mass, more preferably 0.2% to 10% by mass, and even more preferably 0.5% to 5% by mass. If the doping solution contains other components but does not contain inorganic particles, the total content of the other components in the doping solution is preferably 1% to 25% by mass, more preferably 5% to 25% by mass, and even more preferably 7% to 20% by mass.
[0086] -Manufacturing Method I- In Manufacturing Method I, a separator can be manufactured that includes a support substrate and a porous polymer layer that embeds at least a portion of the support substrate by wet phase separation while a support substrate is placed in a coating film formed with a doped solution obtained by dissolving a polymer. In wet phase separation, the support substrate is placed on a coating film formed by casting the doped solution onto a substrate, and the support substrate is immersed in the coating film to impregnate the support substrate with the doped solution. Next, the support substrate, which has been impregnated with the doped solution, is immersed in a solvent (poor solvent, coagulation bath) that does not dissolve the polymer and is miscible with the good solvent. When the proportion of the good solvent in the coating film of the doped solution decreases due to this immersion, the polymer and the solvent undergo phase separation (liquid-induced phase separation), the polymer gels (coagulates), and a porous polymer layer is formed. A separator is then obtained that includes a support substrate and a porous polymer layer that embeds at least a portion of the support substrate.
[0087] -Manufacturing Method II- In Manufacturing Method II, a porous polymer layer can be produced by forming a porous polymer layer and not containing a support substrate by wet phase separation, which includes liquid-induced phase separation of the coating film formed by casting a film-forming solution obtained by dissolving a polymer onto a release film, with the release film removed. In the wet phase separation, the film-forming solution is cast onto the release film, and the surface is dried as appropriate to form a coating film. Next, the laminate with the coating film of the film-forming solution formed on the release film is immersed in a solvent (poor solvent, coagulation bath) that does not dissolve the polymer and is miscible (miscible) with the good solvent, and the release film is removed during the immersion. As the proportion of the good solvent in the coating film of the film-forming solution decreases due to this immersion, the polymer and solvent undergo phase separation (liquid-induced phase separation), the polymer gels (coagulates), and a porous polymer layer is formed. A separator composed of a porous polymer layer and not containing a support substrate is then obtained.
[0088] As a poor solvent, for example, water, or a mixed solvent of water and a hydrophilic organic solvent (an organic solvent miscible with water) or a water-soluble polymer can be used. Examples of hydrophilic organic solvents include aprotic solvents such as N-methylpyrrolidone (NMP), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and dimethylacetamide (DMAC), and alcohols such as ethanol, propanol, or isopropanol. Examples of water-soluble polymers include water-soluble polymers such as polyvinylpyrrolidone (PVP) or polyvinyl alcohol (PVA). Among these, water is preferred as the poor solvent.
[0089] The temperature of the coagulation bath is preferably 20°C to 90°C, more preferably 40°C to 70°C.
[0090] It is also preferable to expose the coating film to the vapor of the poor solvent before immersing it in the poor solvent to induce vapor-induced phase separation (vapor-induced phase separation). By performing vapor-induced phase separation, it is possible to suppress the formation of a dense skin layer on the surface. Therefore, in the above wet phase separation, vapor-induced phase separation and liquid-induced phase separation can also be performed in combination. Furthermore, it is preferable to perform a washing step with pure water or the like after wet phase separation, preferably after liquid-induced phase separation.
[0091] In vapor induction phase separation, the support substrate coated with the dope solution is exposed to a non-solvent vapor, preferably humid air. As a method for performing vapor induction phase separation, for example, the description of Figure 2 and its explanation in Japanese Patent Publication No. 2023-531792 can be appropriately referred to and applied in accordance with this disclosure. The poor solvent vapor used in vapor induction phase separation is preferably humid air. The space for performing vapor induction phase separation can be, for example, provided between the step of coating the support substrate with the dope solution and the step of performing liquid induction phase separation, continuous with the apparatus for each step, and further shielded from the external environment using insulating metal plates. The degree and speed of water movement in the vapor induction phase separation step can be adjusted by adjusting the air velocity, relative humidity and temperature of the air, and exposure time. The relative humidity within the vapor induction phase separation region can be adjusted by the temperature of the solidification bath and shielding the vapor induction phase separation region from the environment. Vapor-induced phase separation performed on a support substrate coated with a doping solution may be carried out under the same conditions on both sides or under different conditions. The relative humidity and temperature in the region where vapor-induced phase separation is performed can be adjusted using an insulating metal plate, for example, when using the apparatus described in Figure 2 of Japanese Patent Publication No. 2023-531792. If the metal plate completely shields the region from the external environment, the relative humidity and temperature are determined by the temperature of the solidification bath used in the subsequent liquid-induced phase separation. The higher the relative humidity in the region where vapor-induced phase separation is performed, and the higher the air velocity, the larger the maximum pores in the resulting porous material. The relative humidity in the region where vapor-induced phase separation is performed can be, for example, in the range of 50% to 99%, preferably 60% to 98%, and more preferably 70% to 98%.
[0092] In addition, in the above manufacturing method II, after immersing the coating film in the poor solvent to form a porous polymer layer, it may be immersed in glycols such as ethylene glycol and diethylene glycol, water, etc. This step can remove any remaining solvent in the coating film.
[0093] In the separator obtained by the above manufacturing method, a certain amount of good solvent from the doping solution used in the manufacturing inevitably remains. The amount of residual solvent can be determined by gas chromatography or by pre-drying the separator at 40°C for 12 hours. 1 The amount can be quantified using H-NMR as a mass percentage in 100% by mass of the above-mentioned dried porous separator for alkaline water electrolysis.
[0094] The separator of this disclosure can be used as a separator in a method for producing hydrogen by electrolyzing an alkaline aqueous solution using an electrolytic cell. In particular, it can be suitably used as an alkaline water electrolysis separator in the alkaline water electrolysis system described below.
[0095] Furthermore, the separator of this disclosure may be provided with a catalyst layer on at least one surface to serve as an alkaline water electrolysis member. Since the separator of this disclosure has excellent discriminability on both sides, the catalyst layer can be appropriately provided.
[0096] [Alkaline Water Electrolysis Cell] The alkaline water electrolysis cell of the present disclosure includes the separator of the present disclosure. Specifically, the alkaline water electrolysis cell of the present disclosure preferably includes the separator of the present disclosure and at least one of an anode electrode and a cathode electrode, and more preferably includes the separator of the present disclosure and an anode electrode and a cathode electrode.
[0097] Figure 1 is a schematic diagram illustrating a preferred embodiment of the alkaline water electrolysis system of the present disclosure.
[0098] In the alkaline water electrolysis system 20 shown in Figure 1, the alkaline water electrolysis cell 10 includes a separator 11, a cathode electrode 12 positioned on one surface of the separator 11, and an anode electrode 13 positioned on the other surface of the separator 11. The alkaline water electrolysis cell 10 is immersed in a high-concentration alkaline aqueous solution 14.
[0099] The alkaline aqueous solution 14 is, for example, an aqueous solution of potassium hydroxide or an aqueous solution of sodium hydroxide.
[0100] When an electric current flows between the electrodes, electrons are supplied to the cathode side, causing water to produce bubble-like hydrogen (H₂). 2) occurs (2H 2 O + 2e - →H 2 +2OH - ). Hydroxyl ions (OH) generated along with the generation of hydrogen. - ) moves to the anode side after passing through the separator 11, and electrons are removed at the anode to form bubble-shaped oxygen (O 2 ) occurs (4OH - →O 2 +2H 2 O+4e - ).
[0101] Since the separator 11 is in contact with the cathode electrode 12 and the anode electrode 13, the distance traveled by the hydroxyl ions is short, which is advantageous in terms of ion conduction efficiency.
[0102] In the above-described alkaline water electrolysis system, the components other than the separator, such as the cathode electrode and anode electrode, are not particularly limited, and ordinary components used in alkaline water electrolysis systems can be applied as appropriate.
[0103] [Alkaline Water Electrolysis Apparatus] The alkaline water electrolysis apparatus of this disclosure includes the alkaline water electrolysis cell of this disclosure. The alkaline water electrolysis apparatus of this disclosure can produce hydrogen by supplementing the necessary components, components, etc., depending on the configuration of the alkaline water electrolysis cell of this disclosure.
[0104] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to the following examples unless it exceeds the spirit of the disclosure.
[0105] <Example 1> 119 kg of polysulfone (product name "Udel P-3500 LCD MB7", Mw: approximately 80,000, manufactured by Solvay) is added to 397 kg of N-butylpyrrolidone (manufactured by TCI), and the mixture is stirred at 60°C for 5 hours to completely dissolve it. Next, 10 kg of polyvinylpyrrolidone (product name "PVP K90", manufactured by Merck) is added, and the mixture is stirred at 60°C for 1 hour, after which ZrO 2474 kg of particles (product name "E101", manufactured by Luxfer) are added and stirred for a further 3 hours to obtain coating solution 1A. Then, 0.4 kg of carbon black is added to coating solution 1A and stirred for a further 1 hour to obtain coating solution 1B. The obtained coating solutions 1A and 1B are fed into a double-slot die disclosed in Figure 2 of International Publication No. 2009 / 147084, and cast onto the woven fabric (product name "PPSP150", manufactured by NBC Meshtec), which is the supporting substrate, on both sides of the fabric (side A and side B) so that the thickness of the porous polymer layer after drying is 250 μm for each side. Subsequently, the material is gently immersed in a solidification bath (pure water) cooled to 10°C to form a porous polymer layer. Further washing is performed with water at 50°C for 10 minutes, followed by washing with water at 90°C for 1 hour. This results in a separator in which the woven fabric is embedded at the center of the thickness by two porous polymer layers. The separator has a thickness of 500 μm. Furthermore, of the two sides of the separator, the average pore diameter of the surface formed on side A using coating liquid 1A (one side) is 0.11 μm, while the average pore diameter of the surface formed on side B using coating liquid 1B (the other side) is 2.14 μm. Thus, the average pore diameters of the two sides are different.
[0106] <Example 2> A separator is prepared in the same manner as in Example 1, except that coating solution 1A and coating solution 1B are cast on both sides (side A and side B) of the woven fabric so that the thickness of the porous polymer layer after drying is 125 μm on each side.
[0107] <Example 3> A separator is prepared in the same manner as in Example 1, except that coating solution 1A and coating solution 1B are cast on both sides (side A and side B) of the woven fabric so that the thickness of the porous polymer layer after drying is 100 μm on each side.
[0108] <Example 4> A separator is prepared in the same manner as in Example 1, except that coating solution 1A and coating solution 1B are cast on both sides (side A and side B) of the woven fabric so that the thickness of the porous polymer layer after drying is 75 μm.
[0109] <Example 5> Separators are prepared in the same manner as in Example 1, except that coating solution 1A is cast on both sides of the woven fabric (side A and side B) so that the thickness of the porous polymer layer after drying is 270 μm and 230 μm, respectively.
[0110] <Example 6> Separators are prepared in the same manner as in Example 1, except that coating solution 1A is cast on both sides (side A and side B) of the woven fabric so that the thickness of the porous polymer layer after drying is 145 μm and 105 μm, respectively.
[0111] <Example 7> Separators are prepared in the same manner as in Example 1, except that coating solution 1A is cast on both sides (side A and side B) of the woven fabric so that the thickness of the porous polymer layer after drying is 120 μm and 90 μm, respectively.
[0112] <Example 8> Separators are prepared in the same manner as in Example 1, except that coating solution 1A is cast on both sides (side A and side B) of the woven fabric so that the thickness of the porous polymer layer after drying is 85 μm and 65 μm, respectively.
[0113] <Comparative Example 1> A separator is prepared in the same manner as in Example 1, except that coating solution 1A is cast on both sides (side A and side B) of the woven fabric so that the thickness of the porous polymer layer after drying is 250 μm on each side.
[0114] <Comparative Example 2> Separators are prepared in the same manner as in Example 1, except that coating solution 1A is cast on both sides (side A and side B) of the woven fabric so that the thickness of the porous polymer layer after drying is 110 μm on each side.
[0115] (Separator Thickness) Samples are taken at five arbitrary points, and cross-sections are cut out with a razor. A cross-sectional SEM (scanning electron microscope) image is acquired at a magnification (e.g., 400x) that allows the separator cross-section to fit in a single field of view. In the obtained cross-sectional SEM image, assuming that no pores exist (for example, assuming that the pores are filled with polymer), the thickness is measured at 20 equally spaced points at each sampling point, and the arithmetic mean of the total of 100 measurements is adopted.
[0116] (Colorant content) The colorant content in the first region up to the center of the separator's thickness and the colorant content in the second region other than the first region are calculated by dissolving the porous polymer layer in a solvent, separating each component by centrifugation, drying the solvent, and measuring the mass of each component.
[0117] (Distance M) The separator is cut in the thickness direction. A center line is drawn at the center of the separator's thickness on the cut surface. Next, line A is drawn at the center of the support base material's thickness. The length of the perpendiculars drawn from line A to the center line is measured at five equally spaced points, and the average of the measured values is adopted as distance M. The center line and line A are drawn on a digital image, and after reading the length of the perpendiculars, distance M is calculated by comparing it with the scaled distance.
[0118] (Difference in visual reflectance) The color densitometer used is the "X-rite 310TR" manufactured by X-rite Corporation. Black paper is placed under the separator, and the reflected visual density is measured using the color densitometer and a visual filter. The visual reflectance is calculated using the following formula: Visual reflectance (%) = 100 / 10 A A is the reflected visual density. The difference in visual reflectance is calculated from the visual reflectance of both sides.
[0119] (Visual Transmittance) The color densitometer used is the "X-rite 310TR" manufactured by X-rite Corporation. The separator is set in the color densitometer, and the transmitted visual density is measured using the visual filter. The visual transmittance is calculated using the following formula: Visual transmittance (%) = 100 / 10 B B is the transmitted visual density.
[0120] (Pore diameter on the separator surface) On each side of the separator, SEM images of a 10 μm square field of view were observed in five different fields of view. For the pores present in each 10 μm square area, the maximum Ferret diameter was determined by binary analysis, and the average value was adopted.
[0121] The following steps involve using separators to evaluate the identifiability of both sides and the visibility of defects.
[0122] (Distinguishing between both sides) In a room with a brightness of 10,000 lux, a 1.5 m square separator is visually inspected and the distinguishing between both sides is evaluated according to the following evaluation criteria. -Evaluation Criteria- A: Both sides can be distinguished within 10 seconds from the start of visual inspection. B: Both sides can be distinguished between 10 seconds and less than 60 seconds from the start of visual inspection. C: It takes 60 seconds or more from the start of visual inspection to distinguish between both sides, or they cannot be distinguished.
[0123] (Defect Visibility) In a room with a brightness of 10,000 lux, a 1.5 m square separator is visually inspected, and the visibility of defects is evaluated according to the following evaluation criteria. In this evaluation, a defect refers to a pinhole with a diameter of 0.1 mm or larger. -Evaluation Criteria- A: The presence or absence of a defect can be confirmed within 3 minutes from the start of visual inspection. B: The presence or absence of a defect can be confirmed between 3 minutes and 10 minutes from the start of visual inspection. C: It takes 10 minutes or more from the start of visual inspection to confirm the presence or absence of a defect, or the presence or absence of a defect cannot be confirmed.
[0124] In Table 1, the "Difference in Coloring" column indicates that "Y" is written when the amount of coloring agent contained in the first region up to the center of the separator's thickness is different from the amount of coloring agent contained in the second region outside the first region, and "N" is written when they are the same. "Distance M / Thickness" means the ratio of distance M to the thickness of the separator. Distance M means the distance between the center of the separator's thickness and the center of the woven fabric's thickness.
[0125]
[0126] As shown in Table 1, in Examples 1 to 8, the difference in visual reflectance measured with a color densitometer between one surface and the other surface was 0.1% or more, indicating excellent discriminability between both surfaces.
[0127] In Comparative Example 1 and Comparative Example 2, the difference in visual reflectance was 0%, meaning that both sides could not be distinguished.
[0128] In Example 2, the visual transmittance is 15% or more, and the defect visibility is superior compared to Example 1. In Example 6, the visual transmittance is 15% or more, and the defect visibility is superior compared to Example 5.
[0129] Furthermore, the disclosure of Japanese Patent Application No. 2025-078883, filed on 9 May 2025, is incorporated herein by reference in its entirety. In addition, all documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually noted to be incorporated by reference.
[0130] 10 Alkaline water electrolysis cell 11 Separator 12 Cathode electrode 13 Anode electrode 14 Alkaline aqueous solution 20 Alkaline water electrolysis system O 2 Bubble-shaped oxygen H 2 Bubble-shaped hydrogen OH - Hydroxy ion e - electronic
Claims
1. A separator for alkaline water electrolysis in which the difference in visual reflectance measured by a color densitometer between one surface and the other surface is 0.1% or more.
2. The alkaline water electrolysis separator according to claim 1, wherein the difference in visual reflectance is 10% or less.
3. The alkaline water electrolysis separator according to claim 1 or claim 2, wherein the visual transmittance measured by a color densitometer is 15% or more.
4. The alkaline water electrolysis separator according to claim 1 or 2, wherein one surface and the other surface each have pores, and the average pore diameter of the pores on the one surface and the pores on the other surface are different.
5. The alkaline water electrolysis separator according to claim 1 or claim 2, comprising a support base material which is a woven or nonwoven fabric, and a porous polymer layer which embeds at least a portion of the support base material.
6. The alkaline water electrolysis separator according to claim 5, wherein the distance between the thickness position which is 50% of the thickness of the alkaline water electrolysis separator and the thickness position which is 50% of the thickness of the support substrate is within the range of 3% to 25% of the thickness of the alkaline water electrolysis separator.
7. The alkaline water electrolysis separator according to claim 5, wherein the porous polymer layer contains a coloring agent, and the content of the coloring agent in a first region from one surface of the alkaline water electrolysis separator to a thickness position that is 50% of the alkaline water electrolysis separator in the thickness direction of the alkaline water electrolysis separator is different from the content of the coloring agent in a second region of the alkaline water electrolysis separator that is other than the first region.
8. The alkaline water electrolysis separator according to claim 5, wherein the porous polymer layer comprises a first porous polymer layer disposed on one side of the support substrate and a second porous polymer layer disposed on the other side of the support substrate.
9. The alkaline water electrolysis separator according to claim 1 or claim 2, wherein the thickness is 250 μm or less.
10. An alkaline water electrolysis cell comprising the alkaline water electrolysis separator described in claim 1 or claim 2.
11. An alkaline water electrolysis apparatus comprising the alkaline water electrolysis cell described in claim 10.