Semiconductor nanoparticle composite and ink composition
The semiconductor nanoparticle composite addresses the issue of excessive ligand coordination by optimizing ligand amount and thermal behavior, ensuring high weather resistance and fluorescence efficiency with enhanced blue light absorption.
Patent Information
- Application Number
- PCT/JP2026/016647
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-04-27
- Publication Date
- 2026-11-12
AI Technical Summary
Existing semiconductor nanoparticle composites face issues with decreased fluorescence properties and weather resistance due to excessive ligand coordination, leading to reduced absorption of blue light and external quantum efficiency.
A semiconductor nanoparticle composite with a low ligand coordination amount, characterized by an SP value of 8.5 or higher, a mass ratio of 5.0% to 30.0% by mass, and specific thermal analysis behavior, including a peak in the 150°C to 290°C range, achieves high weather resistance and fluorescence properties.
The composite maintains excellent fluorescence properties and weather resistance while promoting blue light absorption, increasing external quantum efficiency, and allowing for higher nanoparticle content in products.
Smart Images

Figure JP2026016647_12112026_PF_FP_ABST
Abstract
Description
Semiconductor nanoparticle composites and ink compositions
[0001] This invention relates to a semiconductor nanoparticle composite.
[0002] Semiconductor nanoparticles (quantum dots, QDs) small enough to exhibit quantum confinement effects have a band gap that depends on their particle size. Excitons formed within semiconductor nanoparticles by means of photoexcitation or charge injection recombine and emit photons at an energy corresponding to the band gap. Therefore, by appropriately selecting the composition and particle size of the semiconductor nanoparticles, emission at a desired wavelength can be obtained.
[0003] In the early stages of semiconductor nanoparticle research, studies focused primarily on elements containing Cd and Pb. However, because Cd and Pb are regulated substances subject to restrictions such as the restriction of use of specific hazardous substances, research on non-Cd and non-Pb semiconductor nanoparticles has shifted in recent years.
[0004] Semiconductor nanoparticles are being explored for various applications, including displays, biolabeling, and solar cells. In these diverse applications, semiconductor nanoparticles are often used in the form of a dispersion. Since different types of dispersion media are used depending on the application, a well-dispersed dispersion can be obtained by coordinating ligands appropriate for each dispersion medium to the surface of the semiconductor nanoparticles.
[0005] International Publication No. 241874 (2020)
[0006] Ligands provide dispersibility to semiconductor nanoparticles, but if the amount of ligand coordinating to the semiconductor nanoparticles increases, there is a problem in that the amount of semiconductor nanoparticles in the product decreases when the semiconductor nanoparticles are applied to the product. A low amount of semiconductor nanoparticles in the product leads to a decrease in the absorption of blue light, which in turn leads to a decrease in the product's external quantum efficiency.
[0007] However, ligands also have the function of providing weather resistance to semiconductor nanoparticles by coordinating with them. Therefore, simply reducing the amount of ligand coordinating to the semiconductor nanoparticles will decrease the fluorescence properties or weather resistance of the semiconductor nanoparticles themselves, and the aforementioned problem will not be resolved.
[0008] Therefore, in view of these problems, the present invention provides a semiconductor nanoparticle composite with a low ligand coordination amount and high weather resistance.
[0009] In order to solve the above problems, after diligent research, we discovered a semiconductor nanoparticle composite that exhibits excellent fluorescence properties even with a small amount of ligand coordination and also has high weather resistance. Furthermore, the inventors found commonalities in the thermal analysis behavior of the semiconductor nanoparticles that solve the above problems, and thus completed the present invention.
[0010] In other words, the present invention (1) provides a semiconductor nanoparticle composite in which a ligand is coordinated to the surface of semiconductor nanoparticles, wherein the SP value of the ligand is 8.5 or higher, the mass ratio of the ligand to the semiconductor nanoparticle composite is 5.0% by mass or more and 30.0% by mass or less, the weight derivative curve (ΔTG) of the semiconductor nanoparticle composite in thermogravimetric analysis has a peak in the range of 150°C to 290°C, and the ratio (PH / PL) of the peak height (PH) appearing on the side of ΔTG at a temperature higher than 290°C to the peak height (PL) in the range of 150°C to 290°C in ΔTG is 0 to 0.50.
[0011] Furthermore, in the present invention (2), the ligand is of the following general formula (I): X-(CH(R 1 )CH(R 2 )O) n -R 3 (I) (wherein X is a coordinating group, R 1 , R 2 Each of these is independently H or CH 3 And R 3 The present invention provides a semiconductor nanoparticle composite of (1) comprising a ligand represented by ) where is H or an alkyl group, and n is a natural number less than or equal to 10.
[0012] Furthermore, the present invention (3) provides a semiconductor nanoparticle composite of (2) wherein the number-average molecular weight of the ligand represented by the general formula (I) is 350 or less.
[0013] Further, the present invention (4) provides the semiconductor nanoparticle composite according to (2) or (3), wherein the number average molecular weight of the ligand represented by the general formula (I) is 300 or less.
[0014] Further, the present invention (5) provides the semiconductor nanoparticle composite according to (1), wherein the ligand comprises a ligand represented by the following general formula (II): X-R 4 -C(=O)-Y-(CH(R 5 )CH(R 6 )O) n -R 7 (II) (wherein, X is a coordinating group, Y is O or NH, R 4 is an alkylene group, R 5 , R 6 are each independently H or CH 3 , R 7 is H or an alkyl group, and n is a natural number of 11 or less.)
[0015] Further, the present invention (6) provides the semiconductor nanoparticle composite according to (5), wherein the number average molecular weight of the ligand represented by the general formula (II) is 600 or less.
[0016] Further, the present invention (7) provides the semiconductor nanoparticle composite according to (5) or (6), wherein the number average molecular weight of the ligand represented by the general formula (II) is 550 or less.
[0017] Further, the present invention (8) provides the semiconductor nanoparticle composite according to any one of (5) to (7), wherein R 4 in the general formula (II) is an alkylene group having 6 or less carbon atoms.
[0018] Further, the present invention (9) provides the semiconductor nanoparticle composite according to any one of (1) to (8), wherein in a heat and moisture resistance test in which the semiconductor nanoparticle composite is made into a 1 mass% chloroform dispersion, and the dispersion is held at a temperature of 60°C and a relative humidity of 90% for 100 hours, the change rate of the fluorescence quantum efficiency before and after the test is less than 10%.
[0019] Furthermore, the present invention (10) provides a semiconductor nanoparticle composite according to any of (2) to (8), wherein the ligand further comprises an aliphatic ligand in which the organic group is an aliphatic hydrocarbon group.
[0020] Furthermore, the present invention (11) provides a semiconductor nanoparticle composite of (10) wherein the coordinating group of the aliphatic ligand includes at least one of a thiol group, a carboxyl group, and an amino group.
[0021] Furthermore, the present invention (12) provides a semiconductor nanoparticle composite according to any of (1) to (11), wherein the semiconductor nanoparticle is a core-shell type semiconductor nanoparticle comprising a core particle and a shell covering at least a portion of the surface of the core particle, the core particle comprising In and P, and the shell comprising at least one element from at least Zn, Se, and S.
[0022] Furthermore, the present invention (13) provides a semiconductor nanoparticle composite according to any of (1) to (12), wherein the rate of change in optical density when the semiconductor nanoparticle composite is diluted to 1 mg / mL is less than 30% compared to the optical density when the semiconductor nanoparticle is diluted to 1 mg / mL.
[0023] Furthermore, the present invention (14) provides an ink composition containing any of the semiconductor nanoparticle composites described in (1) to (13).
[0024] The semiconductor nanoparticle composite of the present invention can provide a semiconductor nanoparticle composite with a low ligand coordination amount and high weather resistance.
[0025] Figure 1 shows the results of the weight derivative curve obtained by thermogravimetric analysis of a semiconductor nanoparticle composite according to Example 1, which is an embodiment of the present invention. Figure 2 shows the results of the weight derivative curve obtained by thermogravimetric analysis of a semiconductor nanoparticle composite according to Example 4, which is an embodiment of the present invention. Figure 3 shows the results of the weight derivative curve obtained by thermogravimetric analysis of a semiconductor nanoparticle composite according to Example 9, which is an embodiment of the present invention. Figure 4 shows the results of the weight derivative curve obtained by thermogravimetric analysis of a semiconductor nanoparticle composite according to Comparative Example 1. Figure 5 shows the results of the weight derivative curve obtained by thermogravimetric analysis of a semiconductor nanoparticle composite according to Comparative Example 2.
[0026] The semiconductor nanoparticle composite of the present invention is a semiconductor nanoparticle composite in which a ligand is coordinated to the surface of semiconductor nanoparticles, wherein the SP value of the ligand is 8.5 or higher, the mass ratio of the ligand to the semiconductor nanoparticle composite is 5.0% by mass or more and 30.0% by mass or less, the weight derivative curve (ΔTG) of the semiconductor nanoparticle composite in thermogravimetric analysis has a main peak in the range of 150°C to 290°C, and the ratio (PH / PL) of the peak height appearing on the side of ΔTG at a temperature higher than 290°C to the peak height (PL) in the range of 150°C to 290°C in ΔTG is 0 to 0.50.
[0027] The present invention relates to a semiconductor nanoparticle composite in which a ligand is coordinated to the surface of semiconductor nanoparticles. The present invention provides high weather resistance despite the small amount of coordinated ligand.
[0028] In the present invention, a semiconductor nanoparticle composite is a composite of semiconductor nanoparticles having luminescence properties and a ligand coordinated to the surface of the semiconductor nanoparticles. The semiconductor nanoparticle composite of the present invention is a particle that absorbs light in the 340 nm to 480 nm range and emits light with an emission peak wavelength of 400 nm to 750 nm.
[0029] (Semiconductor Nanoparticles) The semiconductor nanoparticles constituting the semiconductor nanoparticle composite of the present invention are not particularly limited as long as they satisfy the required performance or application characteristics of fluorescence quantum efficiency and full width at half maximum. The semiconductor nanoparticles may be particles made of one type of semiconductor, or particles made of two or more different types of semiconductors. If the semiconductor nanoparticles are particles made of two or more different types of semiconductors, they may constitute a core-shell structure.
[0030] When the semiconductor nanoparticles constitute a core-shell structure made up of two or more types of semiconductors, examples of the composition forming the core include InP, ZnSe, ZnS, CdSe, CdS, CdSeZn, ZnTe, ZnTeSe, ZnTeS, ZnSeS, AgGaS, AgInGaS, etc. From the viewpoint of luminescence characteristics and environmental impact, a composition containing In and P is preferred.
[0031] Examples of compositions that form the shell include group II-VI element semiconductors, specifically ZnSe, ZnS, ZnSeS, ZnSeTe, ZnSTe, and ZnTe. The effects of the present invention can be more strongly obtained when the shell has a structure containing Zn.
[0032] From the viewpoint of having high optical properties, the semiconductor nanoparticles are preferably core-shell type semiconductor nanoparticles comprising a core particle and a shell covering at least a portion of the surface of the core particle, wherein the core particle contains In and P, and the shell contains at least one element from at least Zn, Se, and S.
[0033] As long as the effects of the present invention are not impaired, the composition for forming semiconductor nanoparticles does not necessarily have to be a stoichiometric composition and may contain trace elements as appropriate. Examples of trace elements include Si, Ge, B, Al, Tl, N, P, As, Sb, Bi, Te, and Po.
[0034] In the present invention, the method for producing semiconductor nanoparticles is not particularly limited, and any method may be used, such as conventional methods including hot injection molding, homogeneous solvent methods, reverse micelle methods, and CVD methods.
[0035] The semiconductor nanoparticle composite of the present invention has ligands coordinated to the surface of the semiconductor nanoparticles. Here, coordination refers to the ligand being chemically bonded to the surface of the semiconductor nanoparticles.
[0036] The ligand for the semiconductor nanoparticle composite of the present invention is preferably an organic ligand. The organic ligand has an organic group consisting of a coordinating group that coordinates to the semiconductor nanoparticle and an organic chain.
[0037] The SP value of the ligand in the semiconductor nanoparticle composite of the present invention is 8.5 or higher, preferably 8.6 or higher, and more preferably 9.0 or higher. The SP value of the ligand is calculated using a method called the Y-MB method, which calculates the SP value from the structural formula of the ligand. Having the SP value of the ligand within the above range increases the options for the dispersion medium that can be used when applying the semiconductor nanoparticle composite as a dispersion. Furthermore, there is no particular upper limit to the SP value of the ligand, but it is preferably 10.5 or lower, and more preferably 10.3 or lower.
[0038] The number-average molecular weight of the ligand in the semiconductor nanoparticle composite of the present invention is preferably 600 or less, more preferably 500 or less, and even more preferably 400 or less. By setting the number-average molecular weight of the ligand within the above range, the volume of the semiconductor nanoparticle composite can be reduced, allowing for a greater amount of semiconductor nanoparticles to be included when dispersed in a dispersion medium or product, and further suppressing the discrepancy between the optical density of a dispersion containing semiconductor nanoparticles and a dispersion containing the semiconductor nanoparticle composite. The lower limit of the ligand's molecular weight is not particularly limited, but is preferably 70 or more, more preferably 90 or more.
[0039] In the semiconductor nanoparticle composite of the present invention, the mass ratio of ligand to semiconductor nanoparticle composite is 5.0% by mass or more and 30.0% by mass or less, preferably 5.0% by mass or more and 28.0% by mass or less, and more preferably 5.0% by mass or more and 26.0% by mass or less. By having the above range for the mass ratio of ligand to semiconductor nanoparticle composite, the absorption of blue light by the semiconductor nanoparticles is promoted, the external quantum efficiency can be increased, and the content of semiconductor nanoparticles in products such as ink compositions and films can be increased.
[0040] Preferred ligands for the semiconductor nanoparticle composite of the present invention are described below. Preferred ligands for the semiconductor nanoparticle composite of the present invention include ligand (A) or ligand (B), as described later.
[0041] A preferred ligand (A) in the semiconductor nanoparticle composite of the present invention has a coordinating group and an organic group, and has a structure represented by the following general formula (I): X-(CH(R 1 )CH(R 2 )O) n -R 3 (I) Here, X is a coordinating group, and R 1 , R 2 Each of these is independently H or CH 3 And R 3 is H or an alkyl group, and n is a natural number less than or equal to 10.
[0042] R 3 Preferably, it is a linear or branched saturated alkyl group having 1 to 10 carbon atoms, and more preferably a linear or branched saturated alkyl group having 1 to 6 carbon atoms.
[0043] The coordinating group X of ligand (A) contributes to binding to semiconductor nanoparticles. Preferably, the coordinating group X of ligand (A) contains at least one of an SH group or a COOH group. Having an SH group or a COOH group as the coordinating group of ligand (A) ensures appropriate coordination strength of the ligand to the semiconductor nanoparticles, thereby improving weather resistance. When the ligand binds to semiconductor nanoparticles, the SH group takes the form of -S- and the COOH group takes the form of -COO-, both binding to the semiconductor nanoparticles.
[0044] The organic group of ligand (A) is the group shown in formula (I') below: -(CH(R 1 )CH(R 2 )O) n -R 3 (I') R 1 , R 2 Each of these is independently H or CH 3 And R 3is H or an alkyl group, and n is a natural number less than or equal to 10. The organic group of ligand (A) having the structure shown in formula (I') enhances dispersibility in polar dispersion media for resist inks currently in general use (e.g., PGME (propylene glycol monomethyl ether), PEGMEA (propylene glycol monomethyl ether acetate), etc.) or monomers for inkjet inks (e.g., HDDA (hexamethylene diacrylate)).
[0045] R 3 Preferably, it is a linear or branched saturated alkyl group having 1 to 10 carbon atoms, and more preferably a linear or branched saturated alkyl group having 1 to 6 carbon atoms.
[0046] The number-average molecular weight of ligand (A) is preferably 350 or less, and more preferably 300 or less. Having the number-average molecular weight of ligand (A) within this range allows for a reduced volume of the semiconductor nanoparticle composite, enabling a higher concentration of semiconductor nanoparticles when dispersed in a dispersion medium or product. Therefore, even though the mass ratio of ligand to semiconductor nanoparticles is 5% by mass or more and 30% by mass or less, preferably 5% by mass or more and 28% by mass or less, and more preferably 5% by mass or more and 26% by mass or less, the semiconductor nanoparticle composite of the present invention maintains dispersibility in the dispersion medium while exhibiting high weather resistance. Here, the number-average molecular weight of ligand (A) is calculated by chromatography. The lower limit of the number-average molecular weight of ligand (A) is not particularly limited, but is preferably 70 or more.
[0047] The preferred ligand (B) in the semiconductor nanoparticle composite of the present invention has a coordinating group and an organic group, and has a structure represented by the following general formula (II). X-R 4 -C(=O)-Y-(CH(R 5 )CH(R 6 )O) n -R 7 (II) Here, X is a coordinating group, and Y is O or NH, R 4 R is an alkylene group, 5, R 6 Each of these is independently H or CH 3 And R 7 is H or an alkyl group, and n is a natural number less than or equal to 11.
[0048] R 4 R is preferably a linear or branched saturated alkylene group having 1 to 6 carbon atoms. 4 However, by using a linear or branched saturated alkylene group with 1 to 6 carbon atoms, it is possible to suppress the discrepancy between the optical density of a dispersion containing semiconductor nanoparticles and the optical density of a dispersion containing semiconductor nanoparticle composites.
[0049] R 7 Preferably, it is a linear or branched saturated alkyl group having 1 to 10 carbon atoms, and more preferably a linear or branched saturated alkyl group having 1 to 6 carbon atoms.
[0050] The coordinating group X of ligand (B) contributes to binding to semiconductor nanoparticles. Preferably, the coordinating group X of ligand (B) contains at least one of an SH group or a COOH group. The fact that the coordinating group of ligand (B) is an SH group or a COOH group ensures appropriate coordination strength of the ligand to the semiconductor nanoparticles, thereby improving weather resistance. When the ligand binds to semiconductor nanoparticles, the SH group takes the form of -S- and the COOH group takes the form of -COO-, and they are bound to the semiconductor nanoparticles.
[0051] The organic group of ligand (B) is the group represented by the following general formula (II'): -R 4 -C(=O)-Y-(CH(R 5 )CH(R 6 )O) n -R 7 (II') Here, Y is O or NH, and R 4 R is an alkylene group, 5 , R 6 Each of these is independently H or CH 3 And R 7is H or an alkyl group, and n is a natural number less than or equal to 11. The organic group of ligand (B) having the structure shown in the general formula (II') can improve dispersibility in polar dispersion media for resist inks currently in general use (e.g., PGME (propylene glycol monomethyl ether), PEGMEA (propylene glycol monomethyl ether acetate), etc.) or monomers for inkjet inks (e.g., HDDA (hexamethylene diacrylate)).
[0052] R 4 R is preferably a linear or branched saturated alkylene group having 1 to 6 carbon atoms. 4 However, by using a linear or branched saturated alkylene group with 1 to 6 carbon atoms, it is possible to suppress the discrepancy between the optical density of a dispersion containing semiconductor nanoparticles and the optical density of a dispersion containing semiconductor nanoparticle composites.
[0053] R 7 Preferably, it is a linear or branched saturated alkyl group having 1 to 10 carbon atoms, and more preferably a linear or branched saturated alkyl group having 1 to 6 carbon atoms.
[0054] The number-average molecular weight of ligand (B) is preferably 600 or less, and more preferably 550 or less. Having the number-average molecular weight of ligand (B) within this range allows for a reduced volume of the semiconductor nanoparticle composite, enabling a higher concentration of semiconductor nanoparticles when dispersed in a dispersion medium or product. Therefore, even though the mass ratio of ligand to semiconductor nanoparticles is 5% by mass or more and 30% by mass or less, preferably 5% by mass or more and 28% by mass or less, and more preferably 5% by mass or more and 26% by mass or less, the semiconductor nanoparticles of the present invention exhibit high weather resistance. Here, the number-average molecular weight of ligand (B) is calculated by chromatography.
[0055] The ligand in the semiconductor nanoparticle composite of the present invention may further include ligand (C), which is a ligand different from the preferred ligand (A) or ligand (B) described above.
[0056] The ligand (C) in the semiconductor nanoparticle composite of the present invention preferably has an organic group and a coordinating group. The coordinating group of ligand (C) contributes to binding to the semiconductor nanoparticles. The coordinating group of ligand (C) preferably contains at least one of a thiol group, a carboxyl group, an amino group, a phosphine group, a phosphone group, and a phosphine oxide group. By having at least one of a thiol group, a carboxyl group, an amino group, a phosphine group, a phosphone group, and a phosphine oxide group as the coordinating group of ligand (C), ligand (C) can coordinate to the semiconductor nanoparticles, thereby suppressing the deterioration of the optical properties of the semiconductor nanoparticles.
[0057] The organic group of ligand (C) includes a hydrocarbon group. The organic group of ligand (C) is not particularly limited as long as it is a hydrocarbon group, and may be a saturated hydrocarbon group or an unsaturated hydrocarbon group. Furthermore, the hydrocarbon group related to the organic group of ligand (C) may be linear or branched. The number of carbon atoms in the hydrocarbon group related to the organic group of ligand (C) is not particularly limited, but is preferably 1 to 30. The inclusion of a hydrocarbon group in the organic group of ligand (C) improves the dispersibility of the semiconductor nanoparticle composite, or broadens the range of choices for the type of dispersion medium used to disperse the semiconductor nanoparticle composite.
[0058] Ligand (C) is preferably an aliphatic ligand. An aliphatic ligand has an aliphatic hydrocarbon group as its organic group. The coordinating group of the aliphatic ligand preferably contains at least one of a thiol group, a carboxyl group, or an amino group. The coordinating group of the aliphatic ligand contains at least one of a thiol group, a carboxyl group, or an amino group, which makes the coordination strength of the aliphatic ligand to the semiconductor nanoparticles appropriate, and thus contributes to improving the weather resistance of the semiconductor nanoparticle composite. Aliphatic ligands whose organic group is a saturated aliphatic hydrocarbon group are not particularly limited, but examples include dodecanethiol, octanthiol, acetic acid, propionic acid, myristic acid, stearic acid, octylamine, dioctylamine, and trioctylamine. Aliphatic ligands whose organic group is an unsaturated aliphatic hydrocarbon group are not particularly limited, but examples include oleic acid and oleylamine.
[0059] In the case of the semiconductor nanoparticle composite of the present invention, in which multiple types of ligands are coordinated to semiconductor nanoparticles, the ratio of ligand (A) and / or ligand (B) to the total amount of ligands coordinated to the semiconductor nanoparticles is preferably 70% or more, and more preferably 75% or more, in molar ratio. When the ratio of ligand (A) and / or ligand (B) to the total amount of ligands is 70% or more within the above range, the semiconductor nanoparticle composite exhibits high weather resistance.
[0060] Furthermore, the type and amount of ligands coordinating to semiconductor nanoparticles can be identified by qualitative and quantitative analysis of functional groups using nuclear magnetic resonance spectroscopy (NMR), infrared spectroscopy (IR), and various types of chromatography.
[0061] The semiconductor nanoparticle composite of the present invention is characterized by a low amount of ligand coordination. Therefore, the semiconductor nanoparticle composite of the present invention can suppress the decrease in absorbance caused by an excessive amount of ligand coordination. In this invention, the amount of ligand coordination is expressed using the mass ratio (percentage) of ligand to the semiconductor nanoparticle composite.
[0062] In the semiconductor nanoparticle composite of the present invention, the mass ratio of ligand to the semiconductor nanoparticle composite is 5.0% by mass or more and 30.0% by mass or less, preferably 5.0% by mass or more and 28.0% by mass or less, and more preferably 5% by mass or more and 26.0% by mass or less. Having the above mass ratio of ligand to the semiconductor nanoparticle composite within this range promotes greater absorption of blue light by the semiconductor nanoparticles, thereby increasing the external quantum efficiency. Furthermore, having the above mass ratio of ligand to the semiconductor nanoparticle composite within this range allows for an increase in the semiconductor nanoparticle content in products such as inks and films when the semiconductor nanoparticles are applied to such products. Note that if the semiconductor nanoparticle composite of the present invention is coordinated with multiple types of ligands, the total mass ratio of ligands to the semiconductor nanoparticle composite should be within the above range.
[0063] Furthermore, the semiconductor nanoparticle composite of the present invention can suppress the discrepancy between the optical density of a dispersion containing the same semiconductor nanoparticles as those constituting the semiconductor nanoparticle composite of the present invention and the optical density of a dispersion containing the semiconductor nanoparticle composite of the present invention. The semiconductor nanoparticle composite of the present invention can suppress the rate of change in the optical density (OD value) (x2) when the semiconductor nanoparticle composite is diluted to 1 mg / mL to less than 30% of the optical density (OD value) (x1) when the same semiconductor nanoparticles as those constituting the semiconductor nanoparticle composite of the present invention are diluted to 1 mg / mL. The rate of change in optical density is calculated using the following formula: Rate of change in optical density (%) = ((x1 - x2) / x1) × 100
[0064] In the semiconductor nanoparticle composite of the present invention, the mass ratio of ligand to semiconductor nanoparticle composite is measured by thermogravimetric analysis (TG). When performing thermogravimetric analysis, dry powder of the semiconductor nanoparticle composite is used. Dry powder of the semiconductor nanoparticle composite is prepared and heated in a nitrogen atmosphere from room temperature to 10°C / min, and thermogravimetric analysis (DTA-TG) is performed. Then, from the thermogravimetric analysis results obtained by the thermogravimetric analysis, the mass ratio of ligand to semiconductor nanoparticle composite is determined by the following formula from the mass of the semiconductor nanoparticle composite at a heating temperature of 100°C (y1) and the mass of the semiconductor nanoparticle composite when the mass loss rate per 10°C becomes less than 0.1% (y2). Mass ratio of ligand to semiconductor nanoparticle composite (%) = ((y1 - y2) / y1) × 100 In the present invention, the mass ratio of ligand to semiconductor nanoparticle composite obtained using thermogravimetric analysis (DTA-TG) is used as an indicator of the ligand coordination amount.
[0065] When measuring the mass ratio of ligands to semiconductor nanoparticle composites, the semiconductor nanoparticle composites are first added to a poor solvent to precipitate, then centrifuged, redispersed in the solvent, dried, and measured from the dry powder state. This pretreatment removes excess ligands that are not coordinated to the semiconductor nanoparticles, allowing for accurate measurement of the mass ratio of ligands to the semiconductor nanoparticle composites. In this invention, all ligands were desorbed from the semiconductor nanoparticle composites upon heating up to 600°C, so the measurement temperature range was set from room temperature (25°C) to 600°C. However, it is preferable to adjust the maximum measurement temperature depending on the type of ligand coordinated to the semiconductor nanoparticle composites.
[0066] The semiconductor nanoparticle composite of the present invention exhibits a peak in the range of 150°C to 290°C in the gravimetric differential curve (ΔTG) of the semiconductor nanoparticle composite in thermogravimetric analysis, and the ratio of the peak height (PH) appearing at a temperature higher than 290°C in ΔTG to the peak height (PL) in the range of 150°C to 290°C in ΔTG (PH / PL) is 0 to 0.50, preferably 0 to 0.30. As a result, the semiconductor nanoparticle composite of the present invention has a low ligand coordination amount, excellent fluorescence properties, and high weather resistance. When performing thermogravimetric analysis, the dry powder of the semiconductor nanoparticle composite is used. The dry powder of the semiconductor nanoparticle composite is prepared and heated in a nitrogen atmosphere from room temperature to 10°C / min, and thermogravimetric analysis (DTA-TG) is performed. Then, in the gravimetric differential curve (ΔTG) obtained by thermogravimetric analysis, the peak height (PL) of the peak in the range of 150°C to 290°C and the peak height (PH) of the peak appearing on the side of 290°C or higher are measured, and the value of PH / PL is determined. Here, the peak of ΔTG in thermogravimetric analysis refers to the peak of the gravimetric differential curve in thermogravimetric analysis. In this invention, the peak height of ΔTG means the height from the baseline of ΔTG to the top of the peak, and if multiple peaks are observed in the temperature range of 150°C to 290°C or in the temperature range of 290°C or higher, PL and PH are used as the sum of the peak heights observed in each range, respectively. Furthermore, if no peak is observed on the side of 290°C or higher, for convenience, the height of ΔTG from the baseline at 350°C is calculated as PH.
[0067] The fact that the ΔTG peak of the semiconductor nanoparticle composite of the present invention is below 290°C means that ligand desorption occurs below 290°C in the semiconductor nanoparticle composite of the present invention. Furthermore, a semiconductor nanoparticle composite in which the ratio of the peak height (PH) appearing on the side of ΔTG above 290°C to the peak height (PL) of ΔTG between 150°C and 290°C (PH / PL) is 0 to 0.50 means that a large amount of ligand desorption occurs below 290°C. On the other hand, for semiconductor nanoparticle composites in which the ΔTG peak exceeds 290°C, it means that the temperature at which ligand desorption occurs exceeds 290°C. The inventors have found the following: In conventional semiconductor nanoparticle composites in which the ΔTG peak exceeds 290°C, it tends to be difficult to obtain a stable high fluorescence quantum efficiency because the binding strength of the ligand to the semiconductor nanoparticle is too strong. In contrast, in the semiconductor nanoparticle composite of the present invention, where the ΔTG peak is between 150°C and 290°C, the binding strength of the ligand to the semiconductor nanoparticle is appropriate. Therefore, in the semiconductor nanoparticle composite of the present invention, by using a ligand such that the ΔTG peak of the semiconductor nanoparticle composite appears between 150°C and 290°C, it is possible to have stable and high fluorescence quantum efficiency and improved weather resistance. Furthermore, by setting the (PH / PL) ratio to 0 to 0.50, preferably 0 to 0.30, a good balance between fluorescence quantum efficiency and weather resistance is achieved, and it is possible to provide a semiconductor nanoparticle composite with a small amount of ligand coordination, excellent fluorescence characteristics, and high weather resistance.
[0068] Conventionally, attempts have been made to improve the weather resistance of semiconductor nanoparticle composites by coordinating large molecular weight organic substances to the ligands of the semiconductor nanoparticle composites or by relatively increasing the amount of ligands. However, when semiconductor nanoparticles are applied to products, this leads to problems such as a decrease in the absolute amount of semiconductor nanoparticles in the product and a decrease in external quantum efficiency. In the semiconductor nanoparticle composite of the present invention, a minimum amount of ligands with relatively small molecular weights are coordinated, thus resolving the problems of a decrease in the absolute amount of semiconductor nanoparticles in the product and a decrease in external quantum efficiency that have been problems with conventional semiconductor nanoparticle composites when semiconductor nanoparticles are applied to products. Furthermore, a feature of the semiconductor nanoparticle composite of the present invention is that it has high weather resistance even when a minimum amount of ligands with relatively small molecular weights are coordinated.
[0069] Furthermore, if a large amount of ligand is detached from the ligand coordinated to the semiconductor nanoparticle composite at temperatures below 290°C, the semiconductor nanoparticle composite becomes more reactive with other substances at temperatures below 290°C. This is effective, for example, when further ligand exchange is required for the semiconductor nanoparticle composite, or when other additives are applied to the semiconductor nanoparticles when introducing the semiconductor nanoparticle composite into an ink or film. Therefore, since the ligand is detached from the semiconductor nanoparticles at temperatures below 290°C in the semiconductor nanoparticle composite of the present invention, ligand exchange and the application of additives can be performed at relatively low temperatures, which offers advantages in the use of the semiconductor nanoparticle composite.
[0070] Conventionally, semiconductor nanoparticle composites were designed in which ligands detached at high temperatures. Therefore, if further processing of the semiconductor nanoparticles was required, a desorption process was necessary to detach the firmly coordinated ligands. However, since this desorption process was performed at high temperatures, it damaged the semiconductor nanoparticles themselves, leading to a decrease in their optical properties. In contrast, the semiconductor nanoparticle composite of the present invention has ligands that detach at temperatures below 290°C. Therefore, the ligands can be detached at temperatures below 290°C, allowing processing to be performed at relatively low temperatures with minimal damage to the semiconductor nanoparticles themselves.
[0071] As described above, the semiconductor nanoparticle composite of the present invention is a semiconductor nanoparticle composite in which the ligand desorbs at relatively low temperatures (below 290°C), while at the same time possessing high weather resistance. The semiconductor nanoparticles of the present invention have a ΔTG peak between 150°C and 290°C, and furthermore, despite the ratio of the peak height (PH) appearing on the side of ΔTG above 290°C to the peak height (PL) of ΔTG between 150°C and 290°C (PH / PL) being 0 to 0.50, it has been confirmed that the semiconductor nanoparticle composite exhibits high weather resistance. Conventionally, it was thought that strong ligand coordination enhances the weather resistance of a semiconductor nanoparticle composite, and semiconductor nanoparticle composites were designed in which ligand desorbs even at higher temperatures. However, it has been confirmed that the semiconductor nanoparticles of the present invention possess high weather resistance even though they are semiconductor nanoparticles coordinated with ligands that desorb below 290°C.
[0072] In this application, the retention rate of fluorescence quantum efficiency in heat and humidity resistance tests is used as an indicator of the weather resistance of the semiconductor nanoparticle composite. The higher the retention rate of fluorescence quantum efficiency in the heat and humidity resistance tests, the better the weather resistance. Specifically, the semiconductor nanoparticle composite is dispersed in chloroform at a weight percent concentration to form a chloroform dispersion, and the resulting dispersion is kept in a constant temperature and humidity chamber at 60°C and 90% relative humidity for a certain period of time (100 hours in this application). The retention rate of fluorescence quantum efficiency before and after the heat and humidity resistance test is evaluated by the retention rate of fluorescence quantum efficiency before and after the heat and humidity resistance test. The retention rate of fluorescence quantum efficiency before and after the heat and humidity resistance test is calculated using the fluorescence quantum efficiency before the heat and humidity resistance test (QYa) and the fluorescence quantum efficiency after the heat and humidity resistance test (QYb) using the following formula (1): Retention rate of fluorescence quantum efficiency (%) = (QYb / QYa) × 100 (1)
[0073] The fluorescence quantum efficiency of the semiconductor nanoparticle composite of the present invention in heat resistance and humidity resistance tests is 80% or higher, preferably 90% or higher, and more preferably 92% or higher.
[0074] The full width at half maximum (FWHM) of the emission spectrum of the semiconductor nanoparticle composite of the present invention is preferably 40 nm or less, and more preferably 35 nm or less. Having the FWHM of the emission spectrum within this range allows the semiconductor nanoparticle composite to emit light with high color purity when applied to displays or the like.
[0075] The fluorescence quantum efficiency (QY) of the semiconductor nanoparticle composite of the present invention is preferably 80% or higher, and more preferably 85% or higher. A fluorescence quantum efficiency of 80% or higher in the semiconductor nanoparticle composite enables efficient color conversion in relation to the amount of absorbed light.
[0076] In this invention, the full width at half maximum (FWHM) and fluorescence quantum efficiency of the semiconductor nanoparticle composite can be measured using a quantum efficiency measurement system. An emission spectrum is obtained by irradiating a dispersion of semiconductor nanoparticles in a dispersion medium with excitation light. From the emission spectrum obtained here, the peak wavelength (λmax), fluorescence quantum efficiency (QY), and FWHM are calculated from the re-excitation corrected emission spectrum, which excludes the re-excitation fluorescence emission spectrum of the nanoparticles that have been re-excited and emitted fluorescence. Examples of dispersion mediums include n-hexane, octadecene, toluene, acetone, and PGMEA (propylene glycol monomethyl ether acetate). The excitation light used for measurement is a single light of 450 nm, and the dispersion is prepared by adjusting the concentration of semiconductor nanoparticles so that the absorption rate is 20-30%.
[0077] The semiconductor nanoparticle composite of the present invention can be applied to a wide range of uses. Depending on the application, it can be used in the form of a dispersion liquid dispersed in a dispersion medium, an ink composition mixed with monomers or prepolymers, or an optical film dispersed within a film.
[0078] The semiconductor nanoparticle composite of the present invention is obtained, for example, by reacting a mixture of semiconductor nanoparticles, a ligand, and zinc organic acid to coordinate the ligand to the semiconductor nanoparticles. The mixture is preferably stirred after preparation, and more preferably stirred while heating. The heating temperature of the mixture is preferably 50 to 200°C, and more preferably 80 to 150°C.
[0079] In the manufacturing of the semiconductor nanoparticle composite of the present invention, the synthesized semiconductor nanoparticles may be used as is, or purified semiconductor nanoparticles may be used. If the synthesized semiconductor nanoparticles are used as is, there is no need to go through a purification process, so the equipment for obtaining the semiconductor nanoparticle composite can be simplified. On the other hand, if purified semiconductor nanoparticles are used, excess additives added during synthesis can be removed, so they are not incorporated as impurities when obtaining the semiconductor nanoparticle composite, and the properties of the resulting semiconductor nanoparticle composite are stable.
[0080] The ligand to be mixed with the semiconductor nanoparticles is preferably the ligand described above, and more preferably ligand (A) and / or ligand (B) described above. Furthermore, ligand (C) described above may be used in combination with ligand (A) and / or ligand (B).
[0081] The zinc organic acid mixed with the semiconductor nanoparticles is preferably zinc carboxylate. Zinc carboxylate is not particularly limited, but examples include zinc acetate, zinc propionate, zinc butyrate, zinc hexanoate, zinc octanoate, zinc laurate, zinc tridecylate, zinc myristate, zinc palmitate, zinc stearate, zinc neodecanoate, and zinc 2-ethylhexanoate. The amount of zinc organic acid mixed with the semiconductor nanoparticles is preferably 0.01 or more in molar ratio to the ligand mixed with the semiconductor nanoparticles.
[0082] The preparation and reaction of the mixture may be carried out multiple times. When the preparation and reaction of the mixture are carried out multiple times, a step of purification may be included after the previous reaction but before preparing the mixture. For example, after preparing and reacting the mixture (adding stirring or heating as necessary), the mixture is purified to obtain a reaction product. The reaction product is then mixed again with the ligand, zinc organic acid, and a dispersion medium as necessary, and the mixture is prepared again. By carrying out the preparation and reaction of the mixture multiple times, the desired ligand can be coordinated more effectively, and the resulting semiconductor nanoparticle composite has high weather resistance. The purification method is not particularly limited, and known purification methods such as centrifugation or purification methods using filters may be used as appropriate.
[0083] Furthermore, the configurations, methods, procedures, and processes described herein are illustrative and do not limit the present invention; numerous variations are applicable within the scope of the present invention.
[0084] The present invention will be described below based on specific experimental examples, but the present invention is not limited to these.
[0085] [Method for producing semiconductor nanoparticles] <Production of core particles (green)> Indium acetate (0.28 mmol) and zinc oleate (0.56 mmol) were added to a mixture of oleic acid (0.8 mmol), 1-dodecanethiol (0.1 mmol), and octadecene (10 mL), and the mixture was heated from room temperature to 120°C at a heating rate of 10°C per minute under vacuum (<20 Pa) and reacted for 1 hour. The mixture reacted under vacuum (<20 Pa) was then heated to 25°C under a nitrogen atmosphere, and tris(trimethylsilyl)phosphine (0.23 mmol) was added, followed by heating to 280°C at a heating rate of 5°C per minute and reacting for 10 minutes. Furthermore, the reaction mixture was cooled to 25°C, octanoic acid chloride (0.50 mmol) was injected, and the mixture was heated to 240°C at a rate of 10°C per minute. After reacting for 2 minutes, it was cooled to 25°C to obtain a dispersion solution of core particles (green) that emit light in the green wavelength region.
[0086] <Production of core particles (red)> Indium acetate (0.3 mmol) and zinc oleate (0.05 mmol) were added to a mixture of oleic acid (0.9 mmol), 1-dodecanethiol (0.1 mmol), and octadecene (10 mL). The mixture was heated under vacuum (<20 Pa) at a rate of 10°C per minute from room temperature to 120°C and reacted for 1 hour. The mixture reacted under vacuum (<20 Pa) was then heated to 25°C under a nitrogen atmosphere, and tris(trimethylsilyl)phosphine (0.15 mmol) was added. The mixture was then heated at a rate of 10°C per minute to 300°C and reacted for 10 minutes. Furthermore, the reaction mixture was cooled to 25°C, octanoic acid chloride (0.60 mmol) was injected, and the mixture was heated to 250°C at a rate of 10°C per minute. After reacting for 30 minutes, it was cooled to 25°C to obtain a dispersion solution of core particles (red) that emit light in the red wavelength region.
[0087] <Precursors for shell formation> 40 mmol of zinc oleate and 75 mL of octadecene were mixed and heated under vacuum at 110°C for 1 hour to prepare a Zn precursor solution with [Zn] = 0.4 M. 22 mmol of selenium powder and 10 mL of trioctylphosphine were mixed in nitrogen and stirred until completely dissolved to obtain selenized trioctylphosphine with [Se] = 2.2 M. 22 mmol of sulfur powder and 10 mL of trioctylphosphine were mixed in nitrogen and stirred until completely dissolved to obtain sulfurized trioctylphosphine with [S] = 2.2 M.
[0088] One of the following shells (1 to 3) was formed on the obtained core particles using the method described below. The resulting semiconductor nanoparticles were numbered according to the type of core particle and the type of shell formation process, as shown in Table 1.
[0089]
[0090] <Formation of Shell 1> The core particle dispersion solution was heated to 250°C. At 250°C, 4.3 mL of Zn precursor solution and 1.5 mL of selenide trioctylphosphine were added and reacted for 30 minutes to form a ZnSe shell on the surface of the InP-based semiconductor nanoparticles. Furthermore, 3.8 mL of Zn precursor solution and 0.5 mL of sulfide trioctylphosphine were added, the temperature was raised to 280°C, and the reaction was allowed to proceed for 1 hour to form a ZnS shell.
[0091] <Formation of Shell 2> The core particle dispersion solution was heated to 250°C. At 250°C, 5.6 mL of Zn precursor solution and 2.0 mL of selenide trioctylphosphine were added and reacted for 30 minutes to form a ZnSe shell on the surface of the InP-based semiconductor nanoparticles. Furthermore, 4.9 mL of Zn precursor solution and 0.7 mL of sulfide trioctylphosphine were added, the temperature was raised to 280°C, and the reaction was carried out for 1 hour to form a ZnS shell.
[0092] <Formation of Shell 3> The core particle dispersion solution was heated to 250°C. At 250°C, 6.0 mL of Zn precursor solution and 2.0 mL of selenide trioctylphosphine were added and reacted for 30 minutes to form a ZnSe shell on the surface of the InP-based semiconductor nanoparticles. Furthermore, 4.0 mL of Zn precursor solution and 1.8 mL of sulfide trioctylphosphine were added, the temperature was raised to 280°C, and the reaction was allowed to proceed for 1 hour to form a ZnS shell.
[0093] <Purification of Semiconductor Nanoparticles> The reaction solution of the obtained semiconductor nanoparticles was added to acetone and mixed well, then centrifuged. The centrifugal acceleration was set to 4000 G. The precipitate was collected, and n-hexane was added to the precipitate to prepare a dispersion. This operation was repeated several times to obtain purified semiconductor nanoparticles.
[0094] Furthermore, the obtained semiconductor nanoparticles were dispersed in toluene at a concentration of 1 mg / mL to prepare a toluene dispersion. This toluene dispersion was placed in an optical cell with a path length of 1 cm, and the absorbance at 450 nm was measured using a visible-ultraviolet spectrophotometer to determine the OD value (QD) of the semiconductor nanoparticles.
[0095] [Preparation of Ligands] Ligand 1: Preparation of Triethylene Glycol Monomethyl Ether Thiol 86 g of triethylene glycol monomethyl ether and 93 g of triethylamine were placed in a flask and dissolved in 420 mL of THF (tetrahydrofuran). The solution was cooled to 0°C, and 51 g of methanesulfonic acid chloride was gradually added dropwise under a nitrogen atmosphere, taking care not to let the reaction solution temperature exceed 5°C due to the heat of reaction. The reaction solution was then raised to room temperature and stirred for 2 hours. This solution was extracted with a chloroform-aqueous system, and the organic phase was recovered. The obtained solution was dried over magnesium sulfate, and after removing the magnesium sulfate by filtration, the filtrate was concentrated by evaporation to obtain an oily intermediate. This was transferred to another flask, and 400 mL of 1.3 M aqueous thiourea solution was added under a nitrogen atmosphere. The solution was refluxed for 2 hours, then 21 g of NaOH was added, and refluxed for a further 1.5 hours. The reaction solution was cooled to room temperature, and neutralized by adding 1 M HCl aqueous solution until the pH reached 7. The resulting solution was extracted using a chloroform-aqueous system to obtain the target ligand (triethylene glycol monomethyl ether thiol).
[0096] Ligand 2: Preparation of PEG 3-mercaptopropionate (number average molecular weight 490) 4.2 g of 3-mercaptopropionic acid (40 mmol), 19.2 g of methoxyPEG-OH (number average molecular weight 400, 48 mmol), and 0.2 g of concentrated sulfuric acid were mixed in a flask under a nitrogen atmosphere. The solution was stirred at 60°C and reacted for 24 hours under reduced pressure to below 30 mmHg. After cooling the reaction solution to room temperature, it was dissolved in toluene and washed sequentially with saturated sodium bicarbonate solution, water, and saturated saline solution. The resulting organic phase was dried using magnesium sulfate, and then filtered and concentrated by evaporation to obtain the target ligand (PEG 3-mercaptopropionate, number average molecular weight 490).
[0097] Ligand 3: Preparation of 2-(2-methoxyethoxy)ethyl-3-mercaptopropionate 4.2 g of 3-mercaptopropionic acid (40 mmol), 5.8 g of diethylene glycol monomethyl ether (48 mmol), and 0.2 g of concentrated sulfuric acid were mixed in a flask under a nitrogen atmosphere. The solution was stirred at 60°C and reacted under reduced pressure to below 30 mmHg for 24 hours. After cooling the reaction solution to room temperature, it was dissolved in toluene and washed sequentially with saturated sodium bicarbonate solution, water, and saturated saline solution. The resulting organic phase was dried over magnesium sulfate, filtered, and concentrated by evaporation to obtain the target ligand (2-(2-methoxyethoxy)ethyl-3-mercaptopropionate).
[0098] Ligand 4: Preparation of PEG-SH (number average molecular weight 430) 210 g of methoxyPEG-OH (number average molecular weight 400) and 93 g of triethylamine were placed in a flask and dissolved in 420 mL of THF (tetrahydrofuran). The solution was cooled to 0°C, and 51 g of methanesulfonic acid chloride was gradually added dropwise under a nitrogen atmosphere, taking care not to let the reaction solution temperature exceed 5°C due to the heat of reaction. The reaction solution was then raised to room temperature and stirred for 2 hours. This solution was extracted with a chloroform-aqueous system, and the organic phase was recovered. The obtained solution was dried over magnesium sulfate, and after removing the magnesium sulfate by filtration, the filtrate was concentrated by evaporation to obtain an oily intermediate. This was transferred to another flask, and 400 mL of 1.3 M aqueous thiourea solution was added under a nitrogen atmosphere. The solution was refluxed for 2 hours, then 21 g of NaOH was added, and refluxed for a further 1.5 hours. The reaction solution was cooled to room temperature, and neutralized by adding 1 M HCl aqueous solution until the pH reached 7. The resulting solution was extracted using a chloroform-aqueous system to obtain the target ligand (PEG-SH, number-average molecular weight 430).
[0099] Ligand 5: Preparation of Tripropylene Glycol Monomethyl Ether Thiol 108 g of tripropylene glycol monomethyl ether and 93 g of triethylamine were placed in a flask and dissolved in 420 mL of THF (tetrahydrofuran). The solution was cooled to 0°C, and 51 g of methanesulfonic acid chloride was gradually added dropwise under a nitrogen atmosphere, taking care not to let the reaction heat cause the temperature of the reaction solution to exceed 5°C. The reaction solution was then raised to room temperature and stirred for 2 hours. This solution was extracted with a chloroform-aqueous system, and the organic phase was recovered. The obtained solution was dried over magnesium sulfate, and after removing the magnesium sulfate by filtration, the filtrate was concentrated by evaporation to obtain an oily intermediate. This was transferred to another flask, and 400 mL of 1.3 M aqueous thiourea solution was added under a nitrogen atmosphere. The solution was refluxed for 2 hours, then 21 g of NaOH was added, and refluxed for a further 1.5 hours. The reaction solution was cooled to room temperature, and neutralized by adding 1 M HCl aqueous solution until the pH reached 7. The resulting solution was extracted using a chloroform-aqueous system to obtain the target ligand (tripropylene glycol monomethyl ether thiol).
[0100] Ligand 6: Preparation of [2-(2-methoxymethylethoxy)methylethoxy]isopropylthioglycolate 3.7 g of thioglycolic acid (40 mmol), 9.9 g of tripropylene glycol monomethyl ether (48 mmol), and 0.2 g of concentrated sulfuric acid were mixed in a flask under a nitrogen atmosphere. The solution was stirred at 60°C and reacted under reduced pressure to below 30 mmHg for 24 hours. After cooling the reaction solution to room temperature, it was dissolved in toluene and washed sequentially with saturated sodium bicarbonate solution, water, and saturated saline solution. The resulting organic phase was dried over magnesium sulfate, and the organic phase was filtered and concentrated by evaporation to obtain the target ligand [2-(2-methoxymethylethoxy)methylethoxy]isopropylthioglycolate.
[0101] Table 2 lists the compound names of the ligands used in the examples and comparative examples, along with the SP values of each ligand. For ligand 7, dodecanethiol, we used a product manufactured by Sigma-Aldrich.
[0102]
[0103] [Example 1] A QD1-1-octadecene dispersion was prepared by dispersing QD1 in 1-octadecene in a flask at a mass ratio of 10% by mass. 10.0 g of the prepared QD1-1-octadecene dispersion was placed in the flask, and 1.5 g of ligand 1 and 0.15 g of zinc acetate were added to prepare mixture 1. Mixture 1 was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, and then transferred to a centrifuge tube. It was centrifuged at 4000 G for 20 minutes, separating it into a clear 1-octadecene phase and a phase containing semiconductor nanoparticle composites. The 1-octadecene phase was removed, and the phase containing semiconductor nanoparticle composites was recovered. PGMEA (polypropylene glycol monomethyl ether acetate) was added to the remaining semiconductor nanoparticle composite phase, and a QD-PGMEA dispersion was prepared by adjusting the semiconductor nanoparticles to a mass ratio of 10% by mass. The prepared QD-PGMEA dispersion was placed in a flask, and 1.5 g of ligand 1 and 0.15 g of zinc acetate were added to prepare mixture 2. Mixture 2 was stirred at 110°C for 60 minutes under a nitrogen atmosphere and cooled to 25°C. The cooled dispersion was transferred to a centrifuge tube, 50 mL of n-hexane was added to the dispersion, and the mixture was centrifuged at 4000 G for 20 minutes to recover the semiconductor nanoparticle composite phase. 5.0 mL of acetone was added to the recovered semiconductor nanoparticle composite phase to prepare a dispersion. 50 mL of n-hexane was added to the recovered dispersion and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed and the precipitate was recovered. This procedure was repeated several times to obtain a purified semiconductor nanoparticle composite.
[0104] [Example 2] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that the semiconductor nanoparticle used was QD2.
[0105] [Example 3] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that the amounts of ligand 1 and zinc acetate added to mixture 1 were 1.2 g and 0.12 g, respectively, and the amounts of ligand 1 and zinc acetate added to mixture 2 were also 1.2 g and 0.12 g, respectively.
[0106] [Example 4] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that the amounts of ligand 1 and zinc acetate added to mixture 1 were 1 g and 0.1 g, respectively, and the amounts of ligand 1 and zinc acetate added to mixture 2 were 1 g and 0.1 g, respectively.
[0107] [Example 5] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that the amounts of ligand 1 and zinc acetate added to mixture 1 were 1 g and 0.1 g, respectively, and the amounts of ligand 1 and zinc acetate added to mixture 2 were 0.5 g and 0.1 g, respectively.
[0108] [Example 6] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that the semiconductor nanoparticle used was QD2, the ligand used in the preparation of mixture 1 and mixture 2 was ligand 2, the amounts of ligand 2 and zinc acetate added in the preparation of mixture 1 were 1.2 g and 0.12 g, respectively, and the amounts of ligand 2 and zinc acetate added in the preparation of mixture 2 were 1.2 g and 0.12 g, respectively.
[0109] [Example 7] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that the ligand used in the preparation of mixture 1 and mixture 2 was ligand 3, the amounts of ligand 3 and zinc acetate added to mixture 1 were 1.2 g and 0.12 g, respectively, and the amounts of ligand 3 and zinc acetate added to mixture 2 were also 1.2 g and 0.12 g, respectively.
[0110] [Example 8] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that the semiconductor nanoparticle used was QD3, the amount of ligand 1 and zinc acetate added to mixture 1 was 1.2 g and 0.12 g, respectively, and the amount of ligand 1 and zinc acetate added to mixture 2 was also 1.2 g and 0.12 g, respectively.
[0111] [Example 9] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that the semiconductor nanoparticle used was QD3, the amount of ligand 1 and zinc acetate added to mixture 1 was 1.0 g and 0.10 g, respectively, and the amount of ligand 1 and zinc acetate added to mixture 2 was also 1.0 g and 0.10 g, respectively.
[0112] [Example 10] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that the semiconductor nanoparticle used was QD3, the ligand used in the preparation of mixture 1 and mixture 2 was ligand 3, the amounts of ligand 3 and zinc acetate added in the preparation of mixture 1 were 1.0 g and 0.10 g, respectively, and the amounts of ligand 3 and zinc acetate added in the preparation of mixture 2 were also 1.0 g and 0.10 g, respectively.
[0113] [Example 11] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that the ligand used in the preparation of mixture 1 and mixture 2 was ligand 5, the amounts of ligand 5 and zinc acetate added to mixture 1 were 1.2 g and 0.12 g, respectively, and the amounts of ligand 5 and zinc acetate added to mixture 2 were also 1.2 g and 0.12 g, respectively.
[0114] [Example 12] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that the ligand used in the preparation of mixture 1 and mixture 2 was ligand 6, the amounts of ligand 6 and zinc acetate added to mixture 1 were 1.2 g and 0.12 g, respectively, and the amounts of ligand 6 and zinc acetate added to mixture 2 were also 1.2 g and 0.12 g, respectively. [Example 13] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that the amounts of ligand 1 and zinc acetate added to mixture 1 were 1.5 g and 0.15 g, respectively, and the amounts of ligand 1 and zinc acetate added to mixture 2 were 0.5 g and 0.05 g, respectively.
[0115] [Reference Example 1] A QD1-1-octadecene dispersion was prepared by dispersing QD1 in 1-octadecene in a flask at a mass ratio of 10% by mass. 10.0 g of the prepared QD1-1-octadecene dispersion was placed in a flask, and 2.0 g of ligand 1 and 0.20 g of zinc acetate were added to prepare a mixture. The mixture was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, and then transferred to a centrifuge tube. It was centrifuged at 4000 G for 20 minutes, separating it into a clear 1-octadecene phase and a phase containing semiconductor nanoparticle composites. The 1-octadecene phase was removed, and the phase containing semiconductor nanoparticle composites was recovered. PGMEA (dispersion medium) was added to the remaining semiconductor nanoparticle composite phase to prepare a QD-PGMEA dispersion in which semiconductor nanoparticles were adjusted to a mass ratio of 10% by mass. The prepared QD-PGMEA dispersion was placed in a flask, and 2.0 g of ligand 1 and 0.20 g of zinc acetate were added to prepare mixture 2. Mixture 2 was stirred at 110°C for 60 minutes under a nitrogen atmosphere and cooled to 25°C. The cooled dispersion was transferred to a centrifuge tube, 50 mL of n-hexane was added to the dispersion, and the mixture was centrifuged at 4000 G for 20 minutes to recover the semiconductor nanoparticle composite phase. 5.0 mL of acetone was added to the recovered semiconductor nanoparticle composite phase to prepare a dispersion. 50 mL of n-hexane was added to the recovered dispersion and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed and the precipitate was recovered. This procedure was performed only once to obtain a purified semiconductor nanoparticle composite.
[0116] [Comparative Example 1] A QD1-1-octadecene dispersion was prepared by dispersing QD1 in 1-octadecene in a flask at a mass ratio of 10% by mass. 10.0 g of the prepared QD1-1-octadecene dispersion was placed in a flask, and 1.0 g of ligand 1 and 0.10 g of zinc acetate were added to prepare a mixture. The mixture 1 was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, and then transferred to a centrifuge tube. It was centrifuged at 4000 G for 20 minutes, separating it into a clear 1-octadecene phase and a phase containing semiconductor nanoparticle composites. The 1-octadecene phase was removed, and the phase containing semiconductor nanoparticle composites was recovered. 5.0 mL of acetone was added to the obtained semiconductor nanoparticle composite phase to prepare a dispersion. 50 mL of n-hexane was added to the obtained dispersion, and it was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed, and the precipitate was recovered. This process was repeated several times to obtain a purified semiconductor nanoparticle composite.
[0117] [Comparative Example 2] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that ligand 1 was replaced with ligand 4 during the preparation of mixture 1.
[0118] [Comparative Example 3] A QD1-1-octadecene dispersion was prepared by dispersing QD1 in 1-octadecene in a flask at a mass ratio of 10% by mass. 10.0 g of the prepared QD1-1-octadecene dispersion was placed in a flask, and 1.0 g of ligand 7 and 0.10 g of zinc acetate were added to prepare mixture 1. Mixture 1 was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, and then transferred to a centrifuge tube. 50 mL of acetone was added, and the mixture was centrifuged at 4000 G for 20 minutes, separating it into a clear supernatant phase and a phase containing semiconductor nanoparticle composites. The supernatant phase was removed, and the phase containing semiconductor nanoparticle composites was recovered. 1-octadecene was added to the remaining semiconductor nanoparticle composite phase, and a QD-octadecene dispersion was prepared by adjusting the semiconductor nanoparticles to a mass ratio of 10% by mass. The prepared QD-octadecene dispersion was placed in a flask, and 1.0 g of ligand 7 and 0.10 g of zinc acetate were added to prepare mixture 2. Mixture 2 was stirred at 110°C for 60 minutes under a nitrogen atmosphere and cooled to 25°C. The cooled dispersion was transferred to a centrifuge tube, 50 mL of acetone was added to the obtained dispersion, and the mixture was centrifuged at 4000 G for 20 minutes to recover the semiconductor nanoparticle composite phase. 5.0 mL of n-hexane was added to the obtained semiconductor nanoparticle composite phase to prepare a dispersion. 50 mL of acetone was added to the obtained dispersion, and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed and the precipitate was recovered. This operation was repeated several times to obtain a purified semiconductor nanoparticle composite.
[0119] [Comparative Example 4] A QD1-1-octadecene dispersion was prepared by dispersing QD1 in 1-octadecene in a flask at a mass ratio of 10% by mass. 10.0 g of the prepared QD1-1-octadecene dispersion was placed in the flask, and 5.0 g of ligand 3 was added to prepare mixture 1. Mixture 1 was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, and then transferred to a centrifuge tube. It was centrifuged at 4000 G for 20 minutes, separating it into a clear 1-octadecene phase and a phase containing semiconductor nanoparticle composites. The 1-octadecene phase was removed, and the phase containing semiconductor nanoparticle composites was recovered. 5.0 mL of acetone was added to the obtained semiconductor nanoparticle composite phase to prepare a dispersion. 50 mL of n-hexane was added to the obtained dispersion, and it was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed, and the precipitate was recovered. This operation was repeated several times to obtain purified semiconductor nanoparticle composites.
[0120] [Comparative Example 5] A QD3-1-octadecene dispersion was prepared by dispersing QD3 in 1-octadecene in a flask at a mass ratio of 10% by mass. 10.0 g of the prepared QD3-1-octadecene dispersion was placed in a flask, and 1.0 g of ligand 1 and 0.10 g of zinc acetate were added to prepare mixture 1. Mixture 1 was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, and then transferred to a centrifuge tube. It was centrifuged at 4000 G for 20 minutes, separating it into a clear 1-octadecene phase and a phase containing semiconductor nanoparticle composites. The 1-octadecene phase was removed, and the phase containing semiconductor nanoparticle composites was recovered. 5.0 mL of acetone was added to the obtained semiconductor nanoparticle composite phase to prepare a dispersion. 50 mL of n-hexane was added to the obtained dispersion, and it was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed, and the precipitate was recovered. This process was repeated several times to obtain a purified semiconductor nanoparticle composite.
[0121] [Comparative Example 6] A QD3-1-octadecene dispersion was prepared by dispersing QD3 in 1-octadecene in a flask at a mass ratio of 10% by mass. 10.0 g of the prepared QD3-1-octadecene dispersion was placed in the flask, and 0.2 g of ligand 7 and 4.0 g of ligand 4 were added to prepare mixture 1. Mixture 1 was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, and then transferred to a centrifuge tube. It was centrifuged at 4000 G for 20 minutes, separating it into a clear 1-octadecene phase and a phase containing semiconductor nanoparticle composites. The 1-octadecene phase was removed, and the phase containing semiconductor nanoparticle composites was recovered. 5.0 mL of acetone was added to the obtained semiconductor nanoparticle composite phase to prepare a dispersion. 50 mL of n-hexane was added to the obtained dispersion, and it was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed, and the precipitate was recovered. This process was repeated several times to obtain a purified semiconductor nanoparticle composite.
[0122] The composition of the obtained semiconductor nanoparticle composite is shown in Table 3.
[0123]
[0124] <Method for Characterization> (Optical Properties) The optical properties of the semiconductor nanoparticle composite were measured using a fluorescence quantum efficiency measurement system (Otsuka Electronics, QE-2100). The semiconductor nanoparticle composite was dispersed in toluene to form a dispersion, and the concentration of the dispersion was adjusted so that the absorption rate of 450 nm light was 20-30%. The obtained dispersion was irradiated with a single 450 nm light (excitation light) to obtain an emission spectrum. From the emission spectrum obtained here, the peak wavelength (λmax), fluorescence quantum efficiency (QY), and full width at half maximum (FWHM) were calculated from the re-excitation corrected emission spectrum, which excludes the re-excitation fluorescence emission spectrum of the portion that was re-excited and emitted fluorescence.
[0125] [Absorbance Measurement] A toluene dispersion was prepared by dispersing the purified semiconductor nanoparticle composite in toluene at a concentration of 1 mg / mL. This toluene dispersion was placed in an optical cell with a path length of 1 cm. The absorbance at 450 nm was measured using a visible-UV spectrophotometer to determine the OD value (optical density) of the semiconductor nanoparticle composite. The rate of change of the OD value of the semiconductor nanoparticle composite (x2) relative to the OD value of the semiconductor nanoparticle (x1) (OD change rate) was calculated using the following formula. The results are shown in Table 5. Rate of change of OD value (%) = ((x1 - x2) / x1) × 100
[0126] (Thermal Properties) For each measurement value obtained by thermal analysis of the semiconductor nanoparticle composite, the values were measured and calculated under the following analytical conditions. 0.1 g of the semiconductor nanoparticle composite used for measurement was redispersed in 1 mL of toluene, 9 mL of a poor solvent (hexane for all but Comparative Example 4, acetone for Comparative Example 4) was added to precipitate, and then the mixture was centrifuged at 4000 G for 20 minutes to redisperse the precipitated semiconductor nanoparticle composite in toluene. The resulting dispersion was dried at 110 °C for 10 minutes to prepare a dry powder. The obtained dry powder was heated from room temperature to 600 °C at a rate of 10 °C / min under a nitrogen atmosphere using a thermogravimetric analyzer (Bruker, product name TG-DTA2000SA) to perform thermogravimetric analysis (DTA-TG) and obtain a gravimetric differential curve (ΔTG). In the ΔTG results for each example of semiconductor nanoparticle composite obtained, the mass ratio of the ligand to the semiconductor nanoparticle composite was determined using the following formula, based on the mass of the semiconductor nanoparticle composite at a heating temperature of 100°C (y1) and the mass of the semiconductor nanoparticle composite when the mass loss rate per 10°C was less than 0.1% (y2). The results are shown in Table 5. Mass ratio of ligand to semiconductor nanoparticle composite (%) = ((y1 - y2) / y1) × 100 In addition, the peak temperature and peak height of the ΔTG confirmed from the ΔTG graph of each example of semiconductor nanoparticle composite are shown in Table 4. If no peak was observed above 290°C, the height of the ΔTG at 350°C was conveniently considered as the pH, and the temperature and peak height are shown in parentheses in Table 4.
[0127]
[0128] Figure 1 shows the results of the thermogravimetric analysis of Example 1. From the mass loss graph, it was confirmed that the mass percentage of the ligand / semiconductor nanoparticle composite of Example 1 was 19.3%. Furthermore, from the ΔTG graph of Example 1, it was confirmed that the ΔTG peaks were at 214.3°C and 234.9°C. Since no ΔTG peaks were observed in the temperature range above 290°C, the ΔTG value at 350°C was used as the pH, and the pH / PL was calculated to be 0.05.
[0129] Figure 2 shows the results of the thermogravimetric analysis of Example 4. From the mass loss graph, it was confirmed that the mass percentage of the ligand / semiconductor nanoparticle composite in Example 4 was 15.9 mass%. Furthermore, the ΔTG graph for Example 4 showed relatively large peaks at 209.1°C and 239.0°C, and a relatively small peak at 360.6°C. The pH / PL of Example 4 was calculated to be 0.10.
[0130] Figure 3 shows the results of the thermogravimetric analysis of Example 9. From the mass loss graph, it was confirmed that the mass percentage of the ligand / semiconductor nanoparticle composite in Example 9 was 26.0%. Furthermore, the ΔTG graph for Example 9 showed a relatively large peak at 251.8°C, and relatively small peaks at 349.4°C and 459.3°C. When the heights of the ΔTG peaks at temperatures above 290°C were added together to calculate the PH / PL for Example 9, the value was 0.38.
[0131] Figure 4 shows the results of the thermogravimetric analysis of Comparative Example 1. From the mass loss graph, it was confirmed that the mass percentage of the ligand / semiconductor nanoparticle composite in Comparative Example 1 was 13.7%. Furthermore, the ΔTG graph for Comparative Example 1 was found to have peaks at 229.6°C and 359.6°C. The pH / PL of Comparative Example 2 was calculated to be 0.55.
[0132] Figure 5 shows the results of the thermogravimetric analysis of Comparative Example 2. From the mass loss graph, it was confirmed that the mass percentage of the ligand / semiconductor nanoparticle composite in Comparative Example 2 was 25.0%. In addition, in the ΔTG graph for Comparative Example 2, a ΔTG peak was observed only at 298°C, and no peak was observed below 290°C.
[0133] (Heat and Humidity Resistance Test) The fluorescence quantum efficiency (QYa) of the obtained semiconductor nanoparticle composite was measured. Next, the semiconductor nanoparticle composite was dispersed in chloroform at a concentration of 1 wt percent to form a chloroform dispersion. The resulting dispersion was placed in a constant temperature and humidity chamber (ESPEC Corporation: PHP-2J) set to a temperature of 60°C and a relative humidity of 90%, and kept there for 100 hours. After 24 hours, the fluorescence quantum efficiency (QYb) of the nanoparticle composite was measured again. The rate of change in fluorescence quantum efficiency before and after the heat and humidity resistance test was calculated using the fluorescence quantum efficiency (QYa) before the heat and humidity resistance test and the fluorescence quantum efficiency (QYb) after the heat and humidity resistance test using the following formula (1): Maintenance rate of fluorescence quantum efficiency (%) = (QYb / QYa) × 100 (1) The maintenance rate (weather resistance) of the fluorescence quantum efficiency of the obtained nanoparticle composite is shown in Table 5.
[0134] (Photoconversion efficiency of the film) 84 parts by mass of 1,6-hexanediol diacrylate, 10 parts by mass of trimethylolpropane triacrylate, 5 parts by mass of pentaerythritol tetrakis(3-mercaptopropionate), and 1 part by mass of 2,2-dimethoxy-2-phenylacetophenone were mixed to obtain an ultraviolet-curable resin. The ultraviolet-curable resin was mixed with the above-mentioned semiconductor nanoparticle composite to obtain a semiconductor nanoparticle composite composition. At this time, the amount of semiconductor nanoparticles in the composition was adjusted so that the mass fraction of semiconductor nanoparticles in the semiconductor nanoparticle composite composition was 25% by mass. The above-mentioned semiconductor nanoparticle composite composition was formed on glass by spin coating and heated at 90°C for 3 minutes to evaporate the solvent. After photocuring by irradiation with ultraviolet light in air, it was baked at 200°C for 20 minutes to obtain a semiconductor nanoparticle composite cured film. The spectral radiance Lb(λ) of an Advanced Illumination side-emitting backlight (455 nm) was acquired using a Topcon SR-5 spectroradiometer. A semiconductor nanoparticle composite cured film was placed on the side-emitting backlight, and the spectral radiance Ls(λ) was similarly measured with the SR-5. For the semiconductor nanoparticle composite cured film, the ratio of the amount of energy emitted by the semiconductor nanoparticle composite cured film (target wavelength 495 nm to 780 nm) to the amount of energy absorbed (target wavelength 380 nm to 495 nm) ((emitted energy / absorbed energy) × 100) was calculated as the optical conversion efficiency of the film. The optical conversion efficiencies of films containing each semiconductor nanoparticle composite are shown in Table 5.
[0135]
[0136] In the table, the ligand mass ratio is the mass ratio of the ligand to the semiconductor nanoparticle composite. The fluorescence quantum efficiency maintenance rate is the fluorescence quantum efficiency maintenance rate in the heat and humidity resistance tests. In Comparative Example 3, the compatibility with the UV-curing resin was low, aggregation of semiconductor nanoparticles was observed, and it was not possible to obtain the film itself. Therefore, the photoconversion efficiency in Table 5 is indicated as "-".
[0137] Conventionally, highly weather-resistant semiconductor nanoparticle composites were obtained by preparing semiconductor nanoparticle composites with high molecular weight ligands, or semiconductor nanoparticle composites with a high ligand / semiconductor nanoparticle composite ratio, as shown in Reference Example 1 or Comparative Example 2. However, the semiconductor nanoparticle composite of the present invention exhibits high weather resistance even when the ligand / semiconductor nanoparticle composite ratio is adjusted to be low for relatively low molecular weight ligands.
Claims
1. A semiconductor nanoparticle composite in which a ligand is coordinated to the surface of semiconductor nanoparticles, wherein the SP value of the ligand is 8.5 or higher, the mass ratio of the ligand to the semiconductor nanoparticle composite is 5.0% by mass or higher and 30.0% by mass or lower, the weight derivative curve (ΔTG) of the semiconductor nanoparticle composite in thermogravimetric analysis has a peak in the range of 150°C to 290°C, and the ratio (PH / PL) of the peak height (PH) appearing on the side of ΔTG at a temperature higher than 290°C to the peak height (PL) in the range of 150°C to 290°C in ΔTG is 0 to 0.
50.
2. The ligand is given by the following general formula (I): X-(CH(R 1 )CH(R 2 )O) n -R 3 (I) (wherein X is a coordinating group, R 1 , R 2 Each of these is independently H or CH 3 And R 3 The semiconductor nanoparticle composite according to claim 1, comprising a ligand represented by (where is H or an alkyl group, and n is a natural number less than or equal to 10).
3. The semiconductor nanoparticle composite according to claim 2, wherein the number-average molecular weight of the ligand represented by the general formula (I) is 350 or less.
4. The semiconductor nanoparticle composite according to claim 2 or claim 3, wherein the number-average molecular weight of the ligand represented by the general formula (I) is 300 or less.
5. The aforementioned ligand is represented by the following general formula (II): X-R 4 -C(=O)-Y-(CH(R 5 )CH(R 6 )O) n -R 7 (II) (wherein, X is a coordinating group, Y is O or NH, R 4 is an alkylene group, R 5 , R 6 are each independently H or CH 3 , R 7 is H or an alkyl group, and n is a natural number of 11 or less.) The semiconductor nanoparticle composite according to claim 1, comprising the ligand represented by the formula.
6. The semiconductor nanoparticle composite according to claim 5, wherein the number-average molecular weight of the ligand represented by the general formula (II) is 600 or less.
7. The semiconductor nanoparticle composite according to claim 5, wherein the number-average molecular weight of the ligand represented by the general formula (II) is 550 or less.
8. R represented by the general formula (II) above 4 The semiconductor nanoparticle composite according to claim 5, wherein is an alkylene group having 6 or fewer carbon atoms.
9. The semiconductor nanoparticle composite according to claim 1, wherein in a heat and humidity resistance test in which the semiconductor nanoparticle composite is dispersed in a 1% by mass chloroform dispersion and the dispersion is held at a temperature of 60°C and a relative humidity of 90% for 100 hours, the rate of change in fluorescence quantum efficiency before and after the test is less than 10%.
10. The semiconductor nanoparticle composite according to claim 2 or 5, wherein the ligand further comprises an aliphatic ligand whose organic group is an aliphatic hydrocarbon group.
11. The semiconductor nanoparticle composite according to claim 10, wherein the coordinating group of the aliphatic ligand includes at least one of a thiol group, a carboxyl group, and an amino group.
12. The semiconductor nanoparticle composite according to claim 1, wherein the semiconductor nanoparticle is a core-shell type semiconductor nanoparticle comprising a core particle and a shell covering at least a portion of the surface of the core particle, the core particle comprising In and P, and the shell comprising at least one element from at least Zn, Se, and S.
13. The semiconductor nanoparticle composite according to claim 1, wherein the rate of change in optical density when the semiconductor nanoparticle composite is diluted to 1 mg / mL is less than 30% compared to the optical density when the semiconductor nanoparticles are diluted to 1 mg / mL.
14. An ink composition containing the semiconductor nanoparticle composite described in claims 1 to 13.