Stainless steel material for cutter and method for producing same
A stainless steel composition with controlled chromium nitride distribution and heat treatment improves cold workability, hardness, and corrosion resistance, addressing the limitations of existing martensitic stainless steels for cutlery.
Patent Information
- Application Number
- PCT/JP2026/016883
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-04-28
- Publication Date
- 2026-11-12
AI Technical Summary
Existing martensitic stainless steels used for cutlery applications face challenges in achieving high hardness, corrosion resistance, and cold workability, with issues in chromium carbide and nitride distribution and high Ni content leading to inefficiencies in manufacturing processes.
A stainless steel composition with precise C and N content, combined with controlled chromium nitride distribution, is used to enhance cold workability, hardness after quenching and tempering, and corrosion resistance, achieved through a specific heat treatment process.
The solution results in a stainless steel material with excellent cold workability, high hardness, and high corrosion resistance, minimizing cracks during cold rolling and ensuring high-quality cutlery production.
Smart Images

Figure JP2026016883_12112026_PF_FP_ABST
Abstract
Description
Stainless steel material for cutlery and method for producing the same
[0001] The present invention relates to a stainless steel material for cutlery and a method for producing the same.
[0002] Martensitic stainless steel is known as a stainless steel used for cutlery applications such as razors and kitchen knives. This martensitic stainless steel not only achieves high hardness through quenching and tempering, but also contains 12 to 13% Cr, so it is resistant to rust and widely used for cutlery applications.
[0003] In order to maintain both high hardness and high corrosion resistance, martensitic stainless steel needs to contain not only a high Cr content but also a high C content, and there is a problem in hot and cold workability during production compared to high carbon steel. For example, in Patent Document 1, in mass %, C: 0.14 to 0.21%, N: 0.05 to 0.11%, Si: 0.1 to 0.6%, Mn: 0.4 to 1.2%, Cr: 14.0 to 17.0%, C + N: 0.2 to 0.32%, the balance consists of Fe and unavoidable impurities, and 25 particles / 100 μm in the microstructure 2 or more of chromium carbides and / or chromium nitrides are distributed, the precipitation temperature of the chromium carbides is 950°C or lower, the PREN value (pitting resistance index) of formula (1): Cr + 3.3Mo + 16N is 16 or more, and the value of formula (2): 674 + 569C - 4.17Si + 0.46Mn + 10.3Cr + 193N is 950 or lower, a highly corrosion-resistant martensitic stainless hot-rolled annealed steel sheet is disclosed. According to the description of Patent Document 1, it is stated that workability can be improved by controlling the fine chromium carbides in the microstructure to be uniformly distributed.
[0004] Furthermore, Patent Document 2 proposes a high-hardness martensitic stainless steel with excellent corrosion resistance and cold workability, characterized by a composition in mass%, comprising: C: 0.10 to 0.40%, Si: less than 2.0%, Mn: less than 2%, S: less than 0.010%, Cu: 0.01 to 3.0%, Ni: greater than 1.0% to 3.0%, Cr: 11.0 to 15.0%, one or two of Mo and W (Mo + 1 / 2W): 0.01 to 1.0%, N: 0.13 to 0.18%, Al: less than 0.02%, O: less than 0.010%, with the remainder being substantially Fe.
[0005] Japanese Patent Publication No. 2023-517590, Japanese Patent Publication No. 2000-239805
[0006] The highly corrosion-resistant martensitic stainless steel hot-rolled annealed sheet described in Patent Document 1 is a useful invention with high corrosion resistance, but the hardness is low with the aforementioned C+N content, and there is room for improvement, especially for blade applications where sharp cutting edge and wear resistance are important. Furthermore, since chromium carbides and chromium nitrides are not clearly distinguished, there is room for further improvement in the cold workability of the stainless steel material, which is the heat-treated material (annealed material) before quenching and tempering. Similarly, although the high-hardness martensitic stainless steel described in Patent Document 2 is a useful invention with high corrosion resistance, the hardness is low with the C+N content disclosed, similar to Patent Document 1, and there is room for improvement, especially for blade applications where sharp cutting edge and wear resistance are important. In addition, the Ni content is very high, from more than 1.0% to 3.0%, and in order to improve cold workability, a two-stage annealing process is required, which involves heating at 750°C and then cooling, followed by heating at 650°C and then cooling, so there is room for improvement from the standpoint of manufacturing rationality. Therefore, the object of the present invention is to provide a stainless steel material for cutlery and a method for manufacturing the same, which has excellent cold workability and, when the cold-rolled steel strip is hardened and tempered to produce a stainless steel strip for cutlery, the said stainless steel strip for cutlery can have both high hardness and high corrosion resistance.
[0007] To solve the above problems, the inventors investigated methods to simultaneously improve cold workability, hardness after quenching and tempering, and corrosion resistance. As a result, they discovered that by precisely adjusting the C and N content in the stainless steel components and dispersing an appropriate amount of chromium nitride in the microstructure of the stainless steel material, it is possible to simultaneously improve the cold workability, hardness after quenching and tempering, and corrosion resistance of the stainless steel material, leading to the present invention. That is, one aspect of the present invention is a stainless steel material for cutting tools having a composition in mass%, of C: 0.38 to 0.58%, Si: 0.10 to 0.40%, Mn: 0.10 to 1.50%, Cr: 10.5 to 13.0%, Mo and W alone or in combination (Mo + W / 2): 0 to 2.10%, Cu + Ni: 0 to 0.5%, N: 0.050 to 0.120%, with the remainder being Fe and unavoidable impurities, characterized in that the area ratio of chromium nitride is 0.8 to 5.0%, the average equivalent circle diameter of chromium nitride is 0.15 to 0.45 μm, and the maximum equivalent circle diameter is 1.00 μm or less.
[0008] Another aspect of the present invention is a method for producing stainless steel material for cutting tools, comprising at least the following steps: a heating and holding step to obtain a heat-treated material by heating and holding a stainless steel material having a composition in mass%, of C: 0.38 to 0.58%, Si: 0.10 to 0.40%, Mn: 0.10 to 1.50%, Cr: 10.5 to 13.0%, Mo and W individually or in combination (Mo + W / 2): 0 to 2.10%, Cu + Ni: 0 to 0.5%, N: 0.05 to 0.12%, with the remainder being Fe and unavoidable impurities, at a temperature of 780 to 870°C for 0.5 hours or more; and a cooling step to cool the heat-treated material to 690°C at a cooling rate of 5 to 50°C / h.
[0009] The stainless steel material for cutlery of the present invention has excellent cold workability and can achieve both high hardness and high corrosion resistance after quenching and tempering. Therefore, when this stainless steel material for cutlery is used and cold-rolled to produce stainless steel strip for cutlery, the occurrence of cracks during cold rolling can be suppressed. Furthermore, by quenching and tempering the stainless steel strip for cutlery, a hardened stainless steel strip suitable for cutlery applications can be obtained that possesses both high hardness and high corrosion resistance.
[0010] This is a photograph of the appearance of the stainless steel material for cutting tools according to the present invention after cold rolling. This is a photograph of the appearance of the stainless steel material for cutting tools according to the comparative example after cold rolling. This is an image showing the distribution of nitrides in the cross-sectional microstructure of the stainless steel material for cutting tools according to the present invention.
[0011] One embodiment of the present invention will be described below. However, the present invention is not limited to the embodiment described herein, and can be appropriately combined and improved without departing from the technical idea of the invention. The "stainless steel material for cutlery (hereinafter also simply referred to as stainless steel material)" of the present invention can be any form as long as it is subjected to a cold rolling process later, for example, a steel billet (slab) before hot rolling, a hot-rolled material, or a cold-rolled material, and is a steel material to which the heat treatment of the present invention described later has been applied. Note that the stainless steel material for cutlery in the present invention is in the state of a material for quenching before quenching to obtain the hardness required for cutlery. The metal structure at this time is a steel mainly composed of the ferrite phase, or in other words, it can also be described as a ferritic stainless steel material. By performing quenching and tempering on this stainless steel material for cutlery having a metal structure mainly composed of the ferrite phase, a quenched stainless steel strip for cutlery mainly composed of the martensite phase can be obtained. Here, "mainly composed of the ferrite phase" means that when the microstructure of the stainless steel material is observed at room temperature, the proportion of the ferrite phase in the matrix excluding carbides is 90% or more in area. Furthermore, the material before it becomes a stainless steel material mainly composed of the ferrite phase is called "stainless steel material," the steel strip obtained by cold rolling the stainless steel material is called "stainless steel strip for cutlery (stainless steel strip)," and the stainless steel strip for cutlery that has been hardened or hardened and tempered to become mainly composed of the martensite phase is called "hardened stainless steel strip for cutlery (hardened stainless steel strip)."
[0012] First, the reason for the limitation on the component composition of the stainless steel material for cutlery according to the present invention will be explained. In the explanation of the component composition, "%", which is the unit of content of the component composition, means "mass%". C: 0.38 to 0.58% C is an important element that solid-solves from carbides into the matrix at the austenitization temperature during quenching and determines the hardness of the martensite phase produced during quenching. Here, the C in the stainless steel material is divided into those that solid-solve in the matrix and those that precipitate as carbides, and the ratio of these is determined by the interaction of Cr and Mo and / or W. Therefore, it is important that Cr and Mo and / or W, along with C, are kept within the composition range described later. The lower limit of C for obtaining the stainless steel material for cutlery according to the present invention, which has improved cold workability, hardness after quenching and tempering, and corrosion resistance compared to conventional materials, is set at 0.38%. The preferred lower limit is 0.40%, and the more preferred lower limit is 0.43%. On the other hand, if there is too much carbon (C), there will be an excessive amount of carbides, and the carbides will also become coarser (i.e., the average and maximum diameters of the equivalent circle will increase). For example, when cold rolling (cold working) is performed using stainless steel material, the cold workability will decrease, cracks may form at the ends of the cold-rolled material, and the yield may decrease. Therefore, the upper limit for carbon (C) is set at 0.58%. A preferred upper limit is 0.55%, a more preferred upper limit is 0.52%, and an even more preferred upper limit is 0.50%.
[0013] Si: 0.10–0.40% Si is used as a deoxidizing agent during refining and also dissolves in stainless steel material, suppressing softening during low-temperature tempering. Therefore, the lower limit is set at 0.10%. On the other hand, excessive content drastically reduces the hot and cold workability of stainless steel material for cutlery. For this reason, the upper limit for Si is set at 0.40%. A preferred upper limit is 0.37%, a more preferred upper limit is 0.35%, and a preferred upper limit is 0.33%.
[0014] Mn: 0.10–1.50% Like Si, Mn acts as a deoxidizing agent during refining and dissolves in the stainless steel material and, consequently, in the stainless steel matrix, enhancing its hardenability. If the amount of Mn is too low, the hardenability of the stainless steel material will decrease, and there is a possibility that the hardening will not be sufficient in the center of the thickness of the stainless steel material. Therefore, the lower limit of Mn is set at 0.10%. On the other hand, excessive Mn content may reduce hot workability and lead to a decrease in yield due to surface defects. Therefore, the upper limit of Mn is set at 1.50%. A preferred upper limit is 1.20%, and a more preferred upper limit is 1.00%.
[0015] Cr: 10.5–13.0% Cr is an element necessary to form a strong non-conductive film on stainless steel strips and, consequently, on cutting tools, which are made by quenching and tempering stainless steel materials, thereby obtaining excellent corrosion resistance. Cr mainly forms carbides with C and nitrides mainly with N. If Cr is excessively high, the carbides become coarser (i.e., the average and maximum diameters of the equivalent circle increase), and the amount of Cr dissolved in the stainless steel material increases relatively, reducing the cold workability of the stainless steel material. For example, when cold-rolling stainless steel, cracks may form at the ends of the cold-rolled material, potentially reducing the yield. Therefore, to improve cold workability, the upper limit of Cr should be 13.0%. A preferred upper limit of Cr is 12.8%, a more preferred upper limit of Cr is 12.6%, an even more preferred upper limit of Cr is 12.4%, and an even more preferred upper limit of Cr is 12.2%. Furthermore, if Cr is low, the corrosion resistance after quenching and tempering decreases drastically, so the lower limit of Cr should be 10.5%. The preferred lower limit of Cr is 11.0%, the more preferred lower limit of Cr is 11.3%, and the even more preferred lower limits of Cr are 11.6% and 11.7%.
[0016] Mo and W, individually or in combination, in the ratio (Mo + W / 2): 0-2.10%. Mo and W have similar effects and are defined as (Mo + W / 2) based on their atomic weight relationship. Mo and W can be included individually or in combination. Mo and W have a high effect in stabilizing the passivation of stainless steel strips and, consequently, cutting tools, and are effective elements in improving corrosion resistance by increasing the pitting potential in chloride solutions. It is preferable that the lower limit for obtaining this effect be 0.01%. On the other hand, excessive addition of Mo and W can drastically reduce the workability of stainless steel materials during hot working, leading to an increase in surface scratches and a decrease in yield. Therefore, the upper limit for the (Mo + W / 2) amount is 2.10%. The preferred upper limit for the (Mo + W / 2) amount is 2.00%. If the effect of stabilizing passivation can be compensated for by other additive elements, it is acceptable to have no Mo and W added (0%). Furthermore, if you intend to include 0.5% or more of the above-mentioned substance, it is advisable to choose Mo. Of course, even if you actively add 0.5% or more of Mo, it is also acceptable to add a small amount of W (0.01% or more) in combination.
[0017] Cu + Ni: 0-0.5% Cu and Ni are effective elements for improving corrosion resistance to non-oxidizing acids such as sulfuric acid, and can be included individually or in combination; therefore, in this invention, they are defined as Cu + Ni. However, because they increase the hardness of the stainless steel material before quenching and tempering and decrease its ductility, they drastically reduce the ductility during hot and cold working. For this reason, even when included, the upper limit of (Cu + Ni) is set at 0.5%. The preferred upper limit of (Cu + Ni) is 0.4%, and the more preferred upper limit of (Cu + Ni) is 0.3%. Furthermore, when included, the preferred lower limit of (Cu + Ni) can be set at 0.1%.
[0018] N: 0.050–0.120% Like C, N is an important element that determines the hardness of the martensite phase formed during quenching. It dissolves in the martensite structure, improving the hardness and corrosion resistance of the quenched stainless steel strip and, consequently, the cutting tool after quenching and tempering. It also forms chromium nitrides, mainly with Cr, and is an important element that affects the cold workability of stainless steel. If N is low, the amount of chromium nitride in the stainless steel decreases (i.e., the area ratio of chromium nitrides is small, and the average equivalent circle diameter is small), resulting in a relatively larger amount of Cr dissolved in the stainless steel, thus worsening the cold workability of the stainless steel before quenching and tempering. Therefore, it is necessary for the stainless steel to contain at least 0.050% N. The preferred lower limit for N is 0.060%. On the other hand, too much N can cause bubbles to form during casting, significantly worsening manufacturability. Therefore, the upper limit for N is 0.120%. The preferred upper limit for N is 0.110%, and the more preferred upper limit for N is 0.100%.
[0019] The stainless steel material for cutting tools of this embodiment may contain the following elements in addition to the elements mentioned above: V + Nb: 0.5% or less. V and Nb have similar effects and can be contained individually or in combination, so they are defined as V + Nb. Of these, Nb has a high affinity for C and forms thermally very stable MC carbides. These thermally very stable MC carbides do not dissolve into the high-temperature austenite phase but remain, and the pinning of the carbides suppresses the coarsening of the austenite phase. Similarly, V finely disperses thermally very stable carbides, suppressing the coarsening of the austenite phase and improving hardness which contributes to wear resistance. However, although V and Nb can form fine MC carbides during the heat treatment process of the present invention described later and increase the hardness after quenching and tempering, they lead to a decrease in the cold workability of the stainless steel material and increase the possibility of cracks occurring during cold working. For this reason, even when V and Nb are contained in this embodiment, the upper limit of (V + Nb) is limited to 0.5%. The upper limit for a preferred (V + Nb) is 0.4%, and the upper limit for a more preferred (V + Nb) is 0.3%. When actively adding V and Nb to obtain their advantageous effects, it is preferable to set the lower limit to, for example, more than 0.1%. On the other hand, if the effects of V and Nb can be compensated for by other additive elements, it is preferable to limit the unavoidable impurity level to 0.1% or less in order to further suppress the decrease in cold workability. Generally, Nb is more expensive than V, so if one of them is to be included, it is better to choose V.
[0020] Co: 0.5% or less. Co is an element that dissolves in the martensite phase and increases the resistance to tempering and softening. On the other hand, for applications that may come into contact with the human body, such as razor blades, it may be included in the stainless steel material of this embodiment in a range of 0.5% or less, as it may cause metal allergies.
[0021] In this embodiment, components other than those mentioned above are Fe and unavoidable impurities. Examples of unavoidable impurity elements include P, S, Al, Ti, and O, but they may be included as long as they do not hinder the effects of the present invention, within the ranges shown below: P ≤ 0.04%, S ≤ 0.03%, Al ≤ 0.1%, Ti ≤ 0.1%, and O ≤ 0.05%.
[0022] <Chromium Nitride> In this embodiment, the stainless steel material for cutting tools has a chromium nitride area ratio of 0.8 to 5.0% in the cross-sectional structure, an average equivalent circle diameter of 0.15 to 0.45 μm, and a maximum equivalent circle diameter of 1.00 μm or less. This chromium nitride (hereinafter also simply referred to as nitride) mainly consists of Cr and N and is distributed spherically in the microstructure of the stainless steel material. Compared to carbides, this nitride has a higher elemental ratio of Cr and can efficiently reduce solid-solution Cr (Cr dissolved in the ferrite structure of the stainless steel material) which is detrimental to cold workability. Therefore, by keeping the nitride area ratio and the average and maximum equivalent circle diameters within the above ranges, the cold workability of the stainless steel material can be further improved. A more preferable upper limit for the nitride area ratio is 4.0%, an even more preferable upper limit for the nitride area ratio is 3.8%, and an even more preferable upper limit for the nitride area ratio is 3.5%. Furthermore, the lower limit for a more preferable nitride area ratio is 1.0%, and the lower limit for an even more preferable nitride area ratio is 1.2%. Also, the upper limit for the average equivalent circle diameter of preferred chromium nitrides is 0.40 μm, and the upper limit for the average equivalent circle diameter of more preferable chromium nitrides is 0.38 μm. Furthermore, the lower limit for the average equivalent circle diameter of preferred chromium nitrides is 0.18 μm, and the lower limit for the average equivalent circle diameter of more preferable chromium nitrides is 0.20 μm. Furthermore, the maximum upper limit for the equivalent circle diameter of preferred chromium nitrides is 0.95 μm, the maximum upper limit for the more preferable equivalent circle diameter is 0.90 μm, and the maximum upper limit for the even more preferable equivalent circle diameter is 0.80 μm. Note that the average and maximum nitride area ratios and equivalent circle diameters in this embodiment are based on elemental mapping of N (magnification 10,000x) using FE-EPMA (field emission electron beam microanalyzer) in a cross-sectional structure perpendicular to the processing direction (stretching direction of rolling) of the stainless steel material for cutting tools, with a field of view of 100 μm. 2 This can be calculated by observing nitrides with an equivalent circle diameter (area equivalent circle diameter) of 0.10 μm or more in the above field of view and performing image analysis. Furthermore, nitrides can be confirmed by quantitative analysis using EDS analysis with a scanning electron microscope. The reason for selecting chromium nitrides with an equivalent circle diameter of 0.10 μm or more is that chromium nitrides with an equivalent circle diameter of less than 0.10 μm were judged to have little effect in efficiently reducing solid solution Cr, which is detrimental to cold workability.
[0023] <Carbides> The stainless steel material for blades in this embodiment contains carbides, and it is preferable that the carbide area ratio in the cross-sectional structure be 8.0 to 20.0%. By keeping the carbide area ratio within the above range, it tends to be possible to further improve the cold workability before quenching and tempering, and the corrosion resistance after quenching and tempering. The upper limit of the more preferable carbide area ratio is 19.0%, and even more preferably 18.5%. The lower limit of the more preferable carbide area ratio is 9.0%, and even more preferably 10.0%. Furthermore, it is preferable that the average equivalent circle diameter (area equivalent circle diameter) of the carbides in the cross-sectional structure be 0.20 to 0.60 μm. The upper limit of the more preferable average equivalent circle diameter is 0.50 μm, and even more preferably 0.48 μm. Furthermore, the lower limit of the preferred average equivalent circle diameter is 0.25 μm, and even more preferably 0.30 μm. Furthermore, it is preferable that the maximum equivalent circle diameter (area equivalent circle diameter) of carbides in the cross-sectional structure is less than 1.50 μm. A more preferable maximum upper limit for the equivalent circle diameter is 1.20 μm, and an even more preferable maximum upper limit for the equivalent circle diameter is 1.15 μm. In this embodiment, the average and maximum area ratio and equivalent circle diameter of carbides are based on a cross-sectional structure perpendicular to the processing direction of the stainless steel material (stretching direction of rolling), with a field of view of 100 μm captured by a scanning electron microscope (magnification 10,000x). 2 The carbides can be observed within the above field of view and calculated by image analysis. Note that carbides with an equivalent circle diameter of less than 0.10 μm can be excluded from the measurement, as they do not significantly improve processability. Furthermore, carbides can be confirmed by elemental mapping using EPMA (electron beam microanalyzer).
[0024] <Method for Manufacturing Stainless Steel Material> Next, the method for manufacturing stainless steel material for cutlery according to the present invention will be described. The method for manufacturing stainless steel material for cutlery according to the present invention involves at least two steps: a heating and holding step in which a stainless steel material having the aforementioned component composition is heated and held at a temperature of 780 to 870°C for 0.5 hours or more to obtain a heat-treated material, and a cooling step in which the heat-treated material is cooled to 690°C at a cooling rate of 5 to 50°C / h to obtain the stainless steel material for cutlery according to the present invention. In other words, this heating and holding step and cooling step can be described as annealing performed before cold rolling.
[0025] <Heating and Holding Process> The heating and holding process of the manufacturing method in this embodiment primarily aims to uniformly precipitate chromium nitride in the microstructure of the stainless steel material, and as a secondary effect, uniform carbide can also be precipitated. In particular, nitride has a lower solid solution temperature in stainless steel material compared to carbide, and the distribution state can be changed by changing the heating and holding temperature and the subsequent cooling conditions, thereby changing the cold workability of the stainless steel material. In the heating and holding process, nitride, which affects the cold workability in the subsequent cooling process, is uniformly precipitated in the stainless steel material to make a heat-treated material. In this embodiment, the heating and holding temperature is set to 780 to 870°C. If the heating temperature is below 780°C, nitride hardly precipitates, making it difficult to obtain an excellent cold workability improvement effect. Also, if the heating temperature exceeds 870°C, carbide precipitates preferentially, and nitride, which can efficiently consume Cr, does not precipitate, and the cold workability of the stainless steel material tends to deteriorate. The preferred lower limit of the heating temperature is 790°C, and the more preferred lower limit is 800°C. Furthermore, the preferred upper limit of the heating temperature is 860°C, and the more preferred upper limit is 850°C.
[0026] The lower limit of the holding time in the aforementioned heating and holding process is set to 0.5 hours in order to uniformly precipitate Cr-based nitrides on the stainless steel material. The preferred lower limit of the holding time is 3 hours, the more preferred lower limit is 5 hours, and the still preferred lower limit is 6 hours. There is no particular limit to the upper limit of the holding time, but since prolonged holding impairs manufacturing efficiency and the uniform precipitation effect of the nitrides mentioned above tends to saturate, it is practical to set the upper limit to 15 hours. The preferred upper limit of the holding time is 13 hours, and the more preferred upper limit of the holding time is 12 hours.
[0027] <Cooling Process> In the cooling process of the heat-treated material following the heating and holding process, the material is cooled from the aforementioned heating and holding temperature (780-870°C) to 690°C at a cooling rate of 5-50°C / h. If the cooling rate is low, more nitrides or carbides can precipitate on the heat-treated stainless steel material, which is desirable for improving cold workability. However, this increases the overall processing time of the heat treatment process, impairing manufacturing efficiency. Therefore, the lower limit of the cooling rate is set at 5°C / h. A preferred lower limit is 6°C / h, a more preferred lower limit is 7°C / h, and an even more preferred lower limit is 8°C / h. On the other hand, if the cooling rate is high, the matrix that transformed into the austenite phase during heating and holding transforms into the martensite phase during cooling, increasing the hardness of the heat-treated stainless steel material and drastically worsening its cold workability. Therefore, the upper limit of the cooling rate is set at 50°C / h. A preferred upper limit is 30°C / h, a more preferred upper limit is 20°C / h, and a particularly preferred upper limit is 15°C / h. Furthermore, in the cooling process, if the above cooling rate is maintained, an isothermal holding process may be carried out for a period of one-third or less of the cooling time to promote the precipitation of nitrides in the stainless steel material.
[0028] <Processes after cold rolling> Next, the stainless steel strip for cutlery and the hardened stainless steel strip for cutlery according to the present invention will be described. In this embodiment, a stainless steel strip for cutlery can be obtained by performing at least cold rolling on the stainless steel material for cutlery of the present invention. As described above, the stainless steel material for cutlery of the present invention has excellent cold workability, which tends to suppress the occurrence of cracks during cold rolling and yield a high-quality stainless steel strip for cutlery. In the case of a cold-rolled stainless steel strip, the preferred thickness is 0.50 mm or less, the more preferred thickness is 0.20 mm or less, and the even more preferred thickness is 0.10 mm or less.
[0029] By quenching and tempering the stainless steel strip for cutlery according to the present invention, a quenched stainless steel strip for cutlery possessing both high hardness and high corrosion resistance can be obtained. In this case, the quenching temperature can be set to 1050 to 1200°C. In the case of the component composition specified in the present invention, if the quenching temperature is less than 1050°C, the carbides will not sufficiently dissolve in the austenite phase, which may reduce the strength. Also, if the quenching temperature exceeds 1200°C, the ductility will be significantly reduced due to the excessive solid-solution of C and N. The preferred lower limit of the quenching temperature is 1070°C, and the more preferred lower limit is 1090°C. The preferred upper limit of the quenching temperature is 1150°C, and the more preferred upper limit is 1120°C.
[0030] When obtaining the stainless steel hardened strip for cutlery according to the present invention, a sub-zero treatment may be performed after the hardening process described above. The temperature during the sub-zero treatment can be set to -50°C or lower. By adjusting to this temperature, it is possible to further improve the strength of the stainless steel hardened strip. No lower limit is specifically set, but assuming treatment with liquid nitrogen, for example, the lower limit may be set to -196°C. In the sub-zero treatment of this embodiment, a mixture of dry ice and alcohol at -75°C is used, but liquefied carbon dioxide or liquid nitrogen may also be used. Electric refrigeration equipment may also be used, or gases such as carbon dioxide may be used.
[0031] When obtaining the stainless steel hardened strip for cutlery according to the present invention, the tempering temperature performed after the quenching (or sub-zero treatment) process can be set to 100 to 400°C. If the tempering temperature is less than 100°C, the ductility tends to be excessively low. On the other hand, if the tempering temperature exceeds 400°C, a large amount of carbides precipitate from the martensite structure, leading to a decrease in strength. The preferred upper limit of the tempering temperature is 370°C, and the preferred lower limit of the tempering temperature is 120°C.
[0032] Ten kg of molten metal, melted in a high-frequency induction melting furnace, was cast to produce ingots for stainless steel material for cutlery, having the component composition shown in Table 1. Next, these ingots were hot forged with a forging ratio (cross-sectional area before forging / cross-sectional area after forging) of approximately 10, cooled, and then annealed in a batch-type annealing furnace at a holding temperature of 780°C for 4 hours to obtain annealed material for stainless steel. Subsequently, the annealed material was held at a holding temperature of 1150°C for 30 minutes, then hot-rolled with a rolling ratio (cross-sectional area before rolling / cross-sectional area after rolling) of approximately 5, and cooled to room temperature to obtain stainless steel material. Note that element V is not shown in Table 1, and in this component system, its content was at an unavoidable impurity level of less than 0.1%.
[0033]
[0034] The obtained stainless steel material was subjected to a heating and holding process using a batch-type annealing furnace, where it was held at a heating and holding temperature of 800 to 840°C for 7 to 11 hours. This was followed by a cooling process where it was cooled to 690°C at a rate of 8.3 to 11.1°C / h to obtain stainless steel material for cutting tools with a thickness of 2 mm. Table 2 shows the conditions for the heating and holding process and the cooling process.
[0035]
[0036] The cold workability of the stainless steel materials for cutting tools obtained in the present invention and comparative examples was evaluated. Cold workability was evaluated by cutting a 40 × 50 × 2.0 mm test piece from the above-mentioned stainless steel material for cutting tools (annealed material) and rolling it at room temperature to a reduction ratio of 95%, and then determining whether or not cracks occurred in the cold-rolled material. The evaluation criteria were as follows: if no cracks were visually observed at the end after cold rolling to a reduction ratio of 95%, or if very minor cracks of less than 0.5 mm occurred, it was classified as "A (Excellent)"; if cracks of 0.5 mm or more occurred at the end, it was classified as "B (Poor)".
[0037] To observe the nitrides in stainless steel material for cutting tools, the microstructure at the center of the thickness direction in a cross-section perpendicular to the stretching direction of the rolling process of the stainless steel material for cutting tools was observed using elemental mapping of nitrogen (10,000x magnification) with FE-EPMA (Field Emission Micro-X-ray Spectrometer). The elemental mapping was performed using a JEOL JXA-8530F, with an acceleration voltage of 15.0 kV, irradiation current of 0.05 μA, and analysis time of 20 ms per point. The characteristic X-ray intensity of nitrogen was measured using a spectroscopic crystal LDE1H. Figure 3 shows the elemental mapping of nitrogen in the stainless steel material of Invention Example 3, binarized with characteristic X-ray intensities above 7 as black and those below 7 as white, and further image processed with a median filter. In Figure 3, the distributed material visible as a granular black contrast phase is chromium nitride. The field of view area is approximately 100 μm². 2 By performing image analysis, the area ratio of nitrides with an equivalent circle diameter of 0.10 μm or more was measured. The image processing software "ImageJ" was used for the above image analysis.
[0038] Next, the average, maximum, and area ratio of the carbide equivalent diameters in the obtained stainless steel material for cutting tools were measured. The area ratio and equivalent diameter of the carbides were measured in the cross-sectional structure perpendicular to the stretching direction of the stainless steel material for cutting tools, using a scanning electron microscope (magnification 10,000x) with a field of view of 100 μm². 2Carbides of 0.10 μm or larger in the above field of view were measured using an image analyzer. The measurement results are shown in Table 3. In both the inventive examples and the comparative examples of the stainless steel material for cutlery, the proportion of the ferrite phase in the matrix excluding carbides is 90% or more in terms of area ratio. Note that the image processing software "ImageJ" provided by the National Institutes of Health (NIH) of the United States was used for the above image analysis. Table 3 shows the results of quantifying nitrides and carbides in the stainless steel material by the above method, as well as the evaluation results of cold workability.
[0039]
[0040] Subsequently, the hardness and corrosion resistance of the quenched stainless steel strip for cutlery were evaluated. The above-mentioned stainless steel material for cutlery (2 mm in thickness) was repeatedly subjected to cold rolling and annealing to produce a 0.1 mm thick stainless steel strip for cutlery, which was then heated to 1100°C in an Ar atmosphere, followed by a quenching treatment for rapid cooling, subsequently a sub-zero treatment at -75°C for 30 minutes, and finally tempering at a temperature of 150°C, to obtain the quenched stainless steel strips for cutlery of the inventive examples and the comparative examples. The hardness was measured in accordance with JIS-Z2244-1:2024, with a load of 300 gf, and the average value was obtained from the measured values at three points. Regarding corrosion resistance, a salt spray test (based on JIS-Z-2371:2015) using 5% neutral saline solution at 35°C was performed using the above quenched stainless steel strip for cutlery, and the state of rust formation after 1 hour was evaluated by the rusting area ratio. In this example, a rust area ratio of less than 1% was judged as "A (excellent)", and 1% or more was judged as "B (poor)". Table 4 shows the results of evaluating the hardness and corrosion resistance of the quenched stainless steel strip for cutlery.
[0041]
[0042] The results in Tables 2, 3, and 4 show that in Examples 1 to 8 of the present invention, not only was the cold workability of the stainless steel material excellent, but the hardness and corrosion resistance of the quenched stainless steel strip after quenching and tempering were also superior. This is thought to be due to a good balance between the composition and the equivalent circle diameter and area ratio of the nitrides. On the other hand, in Comparative Examples 101 to 110, although the quenched stainless steel strip after quenching and tempering showed excellent hardness, the cold workability was worse compared to the examples of the present invention, and inferior corrosion resistance was confirmed. This is thought to be because the N content of the comparative examples was low, and chromium nitrides were hardly observed, or the average diameter of the nitrides was small, resulting in a high solid solution Cr in the stainless steel material before quenching and tempering. In conclusion, it was confirmed that the examples of the present invention possess good cold workability, hardness after quenching and tempering, and corrosion resistance compared to conventional examples.
Claims
1. A stainless steel material for cutting tools having a composition in mass%, of C: 0.38-0.58%, Si: 0.10-0.40%, Mn: 0.10-1.50%, Cr: 10.5-13.0%, Mo and W alone or in combination (Mo+W / 2): 0-2.10%, Cu+Ni: 0-0.5%, N: 0.050-0.120%, with the remainder being Fe and unavoidable impurities, characterized in that the area ratio of chromium nitride is 0.8-5.0%, the average equivalent circle diameter of chromium nitride is 0.15-0.45 μm, and the maximum equivalent circle diameter is 1.00 μm or less.
2. A method for producing stainless steel material for cutting tools, comprising: a heating and holding step of heating and holding a stainless steel material having a composition in mass%, of C: 0.38-0.58%, Si: 0.10-0.40%, Mn: 0.10-1.50%, Cr: 10.5-13.0%, Mo and W individually or in combination (Mo+W / 2): 0-2.10%, Cu+Ni: 0-0.5%, N: 0.05-0.12%, with the remainder being Fe and unavoidable impurities, at a temperature of 780-870°C for 0.5 hours or more to obtain a heat-treated material; and a cooling step of cooling the heat-treated material to 690°C at a cooling rate of 5-50°C / h to obtain a stainless steel material for cutting tools, by performing at least these steps.