Light absorber, radiation shield, and optical lattice clock
A low-cost light absorber with randomly stacked particles and dendritic microstructures effectively absorbs electromagnetic waves across multiple wavelength bands, addressing the limitations of existing absorbers in quantum devices.
Patent Information
- Application Number
- PCT/JP2026/017521
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-11-13
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-12
AI Technical Summary
Existing light absorbers either have high manufacturing costs or limited wavelength absorption capabilities, failing to effectively absorb electromagnetic waves across multiple bands, particularly in quantum devices affected by stray light and blackbody radiation.
A light absorber comprising a particle group with randomly stacked particles and a black film featuring dendritic microstructures, formed by oxidation or nitriding, which can absorb electromagnetic waves in multiple wavelength bands.
The absorber achieves low-cost manufacturing and efficient absorption of electromagnetic waves from several hundred nanometers to several hundred micrometers, minimizing stray light and blackbody radiation effects.
Smart Images

Figure JP2026017521_12112026_PF_FP_ABST
Abstract
Description
Light absorbers, radiation shields, and optical lattice clocks
[0001] This specification discloses improvements to light absorbers, radiation shields, and optical lattice clocks.
[0002] Conventionally, light absorbers that absorb electromagnetic waves such as light are known. Light absorbers are generally created spontaneously or artificially by combining the optical properties, optical coherence, or surface microstructures that confine electromagnetic waves of the material. Examples of light absorbers include, for example, VANTABLACK®, ACTARU BLACK, SUGOKURO®, materials with nanostructures formed on their surface by vapor deposition, oxidation treatment, or wet etching, and various other materials (Non-Patent Literature 1 and Non-Patent Literature 2).
[0003] Light absorbers are used, for example, in quantum devices utilizing atoms and ions, optical sensors, telescopes, solar energy conversion devices, and other optical instruments in general, primarily to reduce electromagnetic waves such as stray light.
[0004] "Carbon nanotube-based black coatings", J.Lehman, C.Yung, N.Tomlin, D.Conklin, and M.Stephens, Applied Physics Reviews 5, 011103(2018)"Blackening of metals using femtosecond fiber laser", Huan Huang, Lih-Mei Yang, Shuang Bai, and Jian Liu, Applied Optics 54 (2015) 324
[0005] Incidentally, it would be desirable to have an optical absorber that can be manufactured at low cost and that can absorb electromagnetic waves in multiple wavelength bands (frequency bands). Although not limited to this, for example, in a quantum device that may be affected by both stray light with wavelengths of several hundred nm to about 1 μm and blackbody radiation from the surroundings with wavelengths of 10 μm or more, using an optical absorber that can absorb electromagnetic waves in both wavelength bands of stray light and blackbody radiation can reduce the effects of both stray light and blackbody radiation on the quantum device.
[0006] Furthermore, VANTABLACK, as mentioned above, can absorb electromagnetic waves across a wide range of wavelengths from several hundred nanometers to several hundred micrometers. However, VANTABLACK has high manufacturing costs due to the need to grow long carbon nanotubes. On the other hand, the aforementioned light absorbers with nanostructures formed on their surfaces have relatively low manufacturing costs, but the wavelength range of electromagnetic waves they can absorb is relatively narrow.
[0007] The objective of the light absorbers disclosed herein is to be able to be manufactured at low cost and to be able to absorb electromagnetic waves in multiple wavelength bands.
[0008] The light absorber disclosed herein is a particle group comprising a plurality of randomly stacked particles, the particle group having a plurality of gaps formed between the particles and a plurality of wall portions that are part of the surface of each particle facing the gap and are oriented in random directions, and a black film formed by oxidizing or nitriding the surface of each particle, the black film having a plurality of dendritic microstructures oriented in random directions formed by the oxidation or nitriding treatment.
[0009] The particles may have a size on the order of micrometers.
[0010] The black film may have a fractal structure that includes the plurality of dendritic microstructures.
[0011] The particles are preferably made of a non-magnetic material.
[0012] It is preferable that the aforementioned multiple particles are bound together with each other.
[0013] The present invention further comprises a substrate having multiple pits on its surface, wherein the group of particles is preferably randomly stacked on the surface of the substrate.
[0014] It is preferable that the size of the pit is larger than the size of the particle.
[0015] The pit may have a size on the order of millimeters.
[0016] The shape of the pit may be a polygonal pyramidal shape, a conical shape, or a spherical notch shape.
[0017] The present invention further comprises a substrate having multiple protrusions on its surface, wherein the group of particles is preferably randomly stacked on the surface of the substrate.
[0018] It is preferable that the size of the protrusions is larger than the size of the particles.
[0019] The aforementioned protrusions may have a size on the order of millimeters.
[0020] The shape of the projection may be a polygonal pyramidal shape, a conical shape, or a spherical notch shape.
[0021] The radiation shield disclosed herein is characterized by comprising a case member having an internal space and an opening, and a light absorber provided on the inner wall of the case member.
[0022] The light absorber may further include an ultrathin metal film having a thickness on the order of angstroms, which is provided so as to cover the group of particles, each of which has the black film formed on its surface.
[0023] The optical lattice clock disclosed herein is characterized by comprising: an atomic oven that emits atoms to form an atomic beam; an MOT device for capturing the atoms; an optical resonator that forms an optical lattice for confining the captured atoms and moving them into a clock transition space; and a radiation shield disposed inside the optical resonator so as to include the clock transition space.
[0024] The light absorbers disclosed herein can be manufactured at low cost and can absorb electromagnetic waves in multiple wavelength bands.
[0025] This is a perspective view of the light absorber according to this embodiment. This is a magnified side view of the light absorber according to this embodiment. This is a photograph showing multiple particles bonded together. This is a photograph showing the dendritic microstructure of the oxide film. This is a conceptual diagram showing how blackbody radiation is absorbed in a group of particles. This is a graph showing the relationship between the angle of incidence of blackbody radiation in a group of particles, the number of times the blackbody radiation is reflected by the particle walls before it exits the light absorber, and the frequency of these reflections. This is a graph showing the relationship between the angle of incidence of blackbody radiation in a group of particles and the average number of times the blackbody radiation is reflected by the particle walls before it exits the light absorber. This is a perspective view of a modified substrate. This is a magnified view of pits provided on the substrate surface. This is a modified light absorber using a substrate with multiple pits. This is a graph showing the intensity of reflected light for each combination of width and depth of multiple pyramidal pits provided without gaps on the substrate surface. This is a photograph showing the surface of a group of particles formed by an electron beam type metal 3D printer. This is a magnified photograph of the surface of a group of particles before the oxide film is formed. This is a photograph showing the surface of a group of particles with an oxide film. This is an external perspective view of the radiation shield. This is an end view of a radiation shield. This is a conceptual diagram showing how an ultrathin metal film is formed on the inner wall of the case member of the radiation shield. This is a simplified diagram of an optical lattice clock equipped with a radiation shield having a light absorber provided according to this embodiment. This is a diagram of a magneto-optical trap (MOT) device. This is a diagram showing a copper oxide jig, with a modified light absorber provided on its inner wall, attached to the MOT device. This is the first diagram for explaining the manufacturing method of the copper oxide jig. This is the second diagram for explaining the manufacturing method of the copper oxide jig. This is the third diagram for explaining the manufacturing method of the copper oxide jig.
[0026] <Structure of the light absorber according to this embodiment> Figure 1 is a perspective view of the light absorber 10 according to this embodiment, and Figure 2 is an enlarged side view of the light absorber 10. The light absorber 10 is capable of suitably absorbing electromagnetic waves of multiple wavelength bands. In this embodiment, the light absorber 10 capable of suitably absorbing light with wavelengths of several hundred nm to about 1 μm (stray light, which is particularly unwanted light) and blackbody radiation from the surroundings with wavelengths of 10 μm or more will be described as an example.
[0027] The light absorber 10 has a structure that includes a flat substrate 12, a particle group 16 consisting of multiple particles 14 randomly stacked on the substrate 12, and an oxide film 18 as a black film formed by oxidizing the surface of each particle 14. "Randomly stacked" means that the multiple particles 14 are stacked without being aligned.
[0028] First, let's explain the particle group 16. In this embodiment, each particle 14 constituting the particle group 16 is spherical in shape. Multiple such particles 14 are stacked on top of each other, forming multiple gaps 20 between the particles 14. Since the multiple particles 14 are stacked randomly, the positions and sizes of the multiple gaps 20 are also random.
[0029] A portion of the surface of each particle 14 faces each gap 20. In this specification, the portion of the surface of a particle 14 facing each gap 20 is referred to as a wall portion 14a. Multiple wall portions 14a of several particles 14 face each gap 20. The multiple wall portions 14a facing each gap 20 are oriented in random directions. Specifically, by randomly stacking multiple particles 14 that constitute the particle group 16, the positions and sizes of the multiple gaps 20 become random, as described above, and the orientation of the multiple wall portions 14a facing each gap 20 also becomes random.
[0030] In this embodiment, the shape of each particle 14 is spherical, but the shape of each particle 14 is not limited to this. Specifically, the shape of each particle 14 is not limited to spherical, as long as multiple gaps 20 are formed in the particle group 16 by stacking multiple particles 14, and the orientation of the multiple wall portions 14a facing each gap 20 is random. For example, the shape of each particle 14 may be an ellipsoid, a polyhedron (e.g., a tetrapod® shape), or a shape such that protrusions are provided on the surface of a polyhedron. In particular, it is preferable that the shape of each particle 14 is such that even if a close-packed structure (e.g., a face-centered cubic structure or a hexagonal close-packed structure) is formed by stacking, gaps 20 are formed, and the orientation of the multiple wall portions 14a facing each gap 20 is random.
[0031] As will be described later, the particle group 16 primarily functions to absorb blackbody radiation from the surroundings having wavelengths of 10 μm or longer. Therefore, the size of each particle 14 constituting the particle group 16 is equal to or slightly larger than the wavelength of the blackbody radiation to be absorbed. In other words, the size of each particle 14 should be determined according to the wavelength of the electromagnetic wave to be absorbed by the particle group 16. To suitably absorb blackbody radiation with wavelengths of about 10 μm to several tens of μm, the particles 14 should have a size on the order of micrometers. In particular, in this embodiment, the diameter of each particle 14 is set to 75 μm. The sizes of the multiple particles 14 may be uniform, but they may also vary somewhat. In this embodiment, the standard deviation of the diameters of the multiple particles 14 was set to 10 μm.
[0032] The material of particle 14 is preferably a non-magnetic material. In this embodiment, particle 14 is made of pure copper. Pure copper is paramagnetic and can be said to be a non-magnetic material. However, the material of particle 14 is not limited to copper. For example, particle 14 may be titanium, aluminum, manganese, chromium, or molybdenum. These are also non-magnetic materials like copper. Alternatively, particle 14 may be made of a magnetic material. For example, particle 14 may be iron, cobalt, or nickel.
[0033] It is preferable that the multiple particles 14 are bonded to each other. Furthermore, it is preferable that the multiple particles 14 that are bonded to each other are bonded to the substrate 12. In this embodiment, the multiple particles 14 are sintered to each other by heating each particle 14 to the extent that the surface of each particle 14 is slightly melted. The multiple particles 14 that are sintered to each other are also sintered to the substrate 12. As a result, the multiple particles 14 are fixed and will not fall off even if the orientation of the light absorber 10 is changed.
[0034] Figure 3 is a photograph showing multiple particles 14 bonded together. Figure 3 shows how spherical particles 14 are bonded to adjacent particles 14 while maintaining their shape. Figure 3 also shows how gaps 20 are formed between the particles 14.
[0035] Next, the oxide film 18 serving as a black film will be described. As described above, the oxide film 18 is formed by subjecting the surface of each particle 14 to an oxidation treatment. The oxide film 18 is also formed on the wall portion 14a which is a part of the surface of each particle 14.
[0036] Further, the oxide film 18 is also preferably a non-magnetic material. In the present embodiment, since the particles 14 are made of pure copper, the oxide film 18 is copper oxide (particularly black copper oxide (copper(II) oxide)). Copper(II) oxide is known to have a Néel temperature of 230 K, exhibiting antiferromagnetism in the low-temperature phase and paramagnetism in the high-temperature phase. Even in the low-temperature phase, the net magnetization becomes zero in units of the crystal lattice, and it is known that no magnetic field is applied to the outside, similarly to the high-temperature phase.
[0037] When the particles 14 are formed of titanium, the oxide film 18 becomes titanium oxide; when the particles 14 are formed of aluminum, the oxide film 18 becomes aluminum oxide; and when the particles 14 are formed of molybdenum, the oxide film 18 becomes molybdenum oxide. Titanium oxide, aluminum oxide, and molybdenum oxide are non-magnetic materials, similarly to copper(II) oxide.
[0038] The oxide film 18 in the present embodiment has a plurality of dendritic microstructures with wall portions oriented in random directions, which are formed by oxidation treatment. The size of the dendritic microstructures included in the oxide film 18 is considerably smaller than the wall portions 14a included in the particle group 16. In particular, the size of the dendritic microstructures is on the nanometer order. Thereby, as will be described later, the oxide film 18 having a fine dendritic structure that can be regarded as a fractal exerts a function of absorbing light (stray light) having a wavelength of mainly about several hundred nm to 1 μm by causing the light to be reflected and scattered in a complicated manner.
[0039] FIG. 4 is a photograph showing the dendritic microstructure of the oxide film 18. FIG. 4 is at a scale of 1 / 100 that of FIG. 3. That is, FIG. 4 shows that the size of the dendritic microstructure is considerably smaller than the size of the particles 14. The surface of each branch included in the dendritic microstructure constitutes a wall portion oriented in a random direction.
[0040] In addition, the black film may be a nitride film formed by subjecting the surface of each particle 14 to nitriding treatment. For example, by subjecting the surface of the particles 14 formed of titanium, zirconium, or aluminum to nitriding treatment, a black nitride film may be formed on the surface of those particles 14.
[0041] <Effects of the light absorber according to the present embodiment> First, the principle by which blackbody radiation is absorbed by the particle group 16 will be described. Figure 5 is a conceptual diagram showing how blackbody radiation is absorbed in the particle group 16. When blackbody radiation is incident on the particle group 16, some of the blackbody radiation is reflected on the outer surface of the particle group 16 and output to the outside of the light absorber 10, as shown by optical path A in Figure 5. However, when the blackbody radiation enters the gaps 20 and is reflected on the wall portions 14a (on the surfaces of which the oxide film 18 is formed), since the wall portions 14a face in random directions, the traveling direction of the reflected light becomes random. As a result, the blackbody radiation is reflected a plurality of times on the wall portions 14a or the base body 12, as in optical path B or C. Note that after multiple reflections on the wall portions 14a or the base body 12, some of the light is output to the outside of the light absorber 10 (optical path B), and after multiple reflections, some of the light is absorbed into the interior of the light absorber 10 (particle group 16) via reflection (optical path C).
[0042] For example, assuming that the reflectance of blackbody radiation on the wall portions 14a is ρ (%), the intensity of the blackbody radiation that is reflected N times on the wall portions 14a and output to the outside of the light absorber 10 is (ρ / 100) of the intensity of the incident light N times. For example, when the reflectance of blackbody radiation on the wall portions 14a is 20%, even if the blackbody radiation is reflected 5 times on the wall portions 14a and output to the outside of the light absorber 10, the intensity of the blackbody radiation is (20 / 100) of the intensity of the incident light 5 times, that is, 1 / 3125 (0.032%). In other words, due to multiple reflections (at least 4 to 5 reflections) on the wall portions 14a, the reflectance of blackbody radiation as the light absorber 10 can be approximately 0%, and it can be said that the effectively incident blackbody radiation is trapped by the light absorber 10.
[0043] Figure 6 is a graph showing the relationship between the angle of incidence of blackbody radiation in the particle group 16, the number of times the blackbody radiation is reflected by the wall portion 14a of the particle 14 before it exits the light absorber 10, and the frequency of these reflections. Figure 7 is a graph showing the relationship between the angle of incidence of blackbody radiation in the particle group 16 and the average number of times the blackbody radiation is reflected by the wall portion 14a of the particle 14 before it exits the light absorber 10. Figure 6 shows that the number of reflections of blackbody radiation at the wall portion 14a does not depend on the angle of incidence of the blackbody radiation. Figure 7 shows that, regardless of the angle of incidence of the blackbody radiation, on average the blackbody radiation is reflected at least four times or more at the wall portion 14a. In other words, in the light absorber 10 according to this embodiment, the reflectivity of blackbody radiation as a light absorber 10 is approximately 0%, regardless of the angle of incidence of the blackbody radiation.
[0044] By making the size of each particle 14 equal to or slightly larger than the wavelength of blackbody radiation, the blackbody radiation is made more easily reflected by the wall portion 14a, and the blackbody radiation is made more easily reflected multiple times by the wall portion 14a, as in optical path B or C. If the size of each particle 14 is considerably smaller than the wavelength of blackbody radiation, the blackbody radiation will have difficulty entering the gap 20, and if the size of each particle 14 is considerably larger than the wavelength of blackbody radiation, the blackbody radiation reflected by the particle 14 or substrate 12 will easily pass through the particle group 16 and be output to the outside.
[0045] Since an oxide film 18 having a dendritic microstructure (see Figure 4) is formed on the surface of the wall portion 14a, absorption of blackbody radiation can also be expected from the oxide film 18. However, because the size of the dendritic microstructure formed on the oxide film 18 is considerably smaller than the wavelength of blackbody radiation, the absorption performance of blackbody radiation by the oxide film 18 alone may not be sufficient. With the light absorber 10, the structure of the particle group 16 (especially the multiple wall portions 14a oriented in random directions) improves the absorption performance of blackbody radiation at least compared to the oxide film 18 alone.
[0046] The principle by which stray light is absorbed in the oxide film 18 is basically the same as the principle by which blackbody radiation is absorbed in the particle group 16 described above. In the oxide film 18, there are multiple dendritic fine structures oriented in random directions, so the direction of propagation of stray light reflected by the dendritic fine structures is also random. As a result, stray light is absorbed by being reflected multiple times by the multiple dendritic fine structures.
[0047] Because dendritic microstructures have a size on the order of nanometers, they readily reflect stray light with wavelengths of several hundred nanometers to about 1 μm, and the stray light is easily reflected multiple times within the dendritic microstructure.
[0048] Strontium 1 S 0 - 1 P 1 The reflectivity of the light absorber 10 was experimentally investigated for laser light with a wavelength of 461 nm, which corresponds to the excitation light between energy levels. Here, only specular reflectivity is considered, and diffuse reflectivity is not considered. When the incident angle was 45 degrees, the reflectivity of the light absorber 10 for the laser light was found to be less than 1%.
[0049] As described above, the light absorber 10 according to this embodiment can suitably absorb electromagnetic waves of multiple wavelength bands through the combination of the particle group 16 and the oxide film 18.
[0050] In particular, to manufacture the light absorber 10 according to this embodiment, it is sufficient to randomly stack a plurality of particles 14 to form a particle group 16 and oxidize the surface of each particle 14 to form an oxide film 18, thus enabling low-cost manufacturing.
[0051] Furthermore, since each particle 14 is made of a non-magnetic material, the residual magnetic field remaining in the light absorber 10 can be suppressed. In other words, because each particle 14 is made of a non-magnetic material, the light absorber 10 can be used in equipment that is susceptible to the effects of residual magnetic fields (details will be described later).
[0052] <Modified Substrate> Figure 8 is a perspective view of the modified substrate 12'. Figure 9 is an enlarged view of the pit 50 provided on the modified substrate 12'. The substrate 12 in the basic embodiment described above was flat, but the modified substrate 12' is provided with a plurality of pits 50 (recesses).
[0053] The shape of the pit 50 is not limited to these, but it may be a polygonal pyramidal shape, a cone shape, or a spherical notch shape. Alternatively, the shapes of the multiple pits 50 do not all have to be the same, and various shapes may be mixed. In order to provide multiple pits 50 on the surface of the base body 12' with as little gap as possible, the shape of the opening of the pit 50 in plan view may be a triangle, a square, or a hexagon. The surface of the base body 12' shown in Figures 8 and 9 is provided with multiple pyramidal (square pyramidal) pits 50.
[0054] The size of the pit 50 (width and depth of the opening) is considerably larger than the size of the particle 14. For example, the size of the pit 50 is 10 times or more the size of the particle 14. In this embodiment, the particle 14 is on the order of micrometers (75 μm in this embodiment), while the size of the pit 50 is on the order of millimeters (for example, the width of the opening is 1 mm to 3 mm, and the depth is 1 mm to 3 mm).
[0055] Figure 10 is a partially enlarged view of a modified light absorber 10' using a substrate 12' provided with a plurality of pits 50. The modified light absorber 10' has a similar structure to the light absorber 10 according to the basic embodiment, except that a plurality of pits 50 are provided on the surface of the substrate 12'. That is, a plurality of particles 14 are randomly stacked on the surface of the substrate 12' provided with a plurality of pits 50, thereby forming a particle group 16 on the surface of the substrate 12'. Then, the plurality of particles 14 are bonded to each other, and an oxide film 18 is formed on the surface of each particle 14. Because a plurality of pits 50 are provided on the surface of the substrate 12', the plurality of particles 14 are also randomly stacked on the inner walls 52 of the pits 50 (see Figure 9).
[0056] The modified light absorber 10' is capable of absorbing electromagnetic waves more effectively than the light absorber 10 according to the basic embodiment. Consider the case where electromagnetic waves (for example, blackbody radiation) incident on the light absorber 10 according to the basic embodiment pass through the particle group 16 and reach the substrate 12. In the light absorber 10 according to the basic embodiment, since the substrate 12 is flat, the electromagnetic waves that reach the substrate 12 are reflected by the substrate 12 and propagate away from the substrate 12 (i.e., in the direction away from the light absorber 10). If the electromagnetic waves reflected by the substrate 12 pass through the particle group 16 further, such electromagnetic waves will leave the light absorber 10, that is, they will not be absorbed by the light absorber 10.
[0057] On the other hand, if an electromagnetic wave incident on the modified light absorber 10' passes through the particle group 16 (particularly the particle group 16 stacked on the inner wall 52 of the pit 50) and reaches the substrate 12', the electromagnetic wave is reflected by the inner wall 52 of the pit 50. Since the orientation of the inner wall 52 is not parallel to the extension direction of the substrate 12', when an electromagnetic wave is reflected by the inner wall 52 of the pit 50, the electromagnetic wave does not necessarily travel away from the substrate 12'. For example, an electromagnetic wave reflected by the inner wall of the pit 50 (here referred to as inner wall 52a as shown in Figure 9) may travel towards another inner wall 52b opposite to inner wall 52a. In that case, even if the electromagnetic wave reflected by inner wall 52a passes through the particle group 16 stacked on inner wall 52a again, it will be incident on the particle group 16 stacked on inner wall 52b. Furthermore, it is expected that the electromagnetic waves will be reflected (i.e., their intensity will be attenuated) by the wall portion 14a within the particle group 16 stacked on the inner wall 52b.
[0058] In this way, by providing a plurality of pits 50 on the surface of the substrate 12', the modified light absorber 10' can reflect electromagnetic waves within the light absorber 10' more times than the light absorber 10 according to the basic embodiment. Therefore, the modified light absorber 10' is capable of absorbing electromagnetic waves more effectively than the light absorber 10 according to the basic embodiment.
[0059] Figure 11 is a graph showing the intensity of reflected light for each combination of width and depth of multiple pyramidal pits 50 (see Figure 8) that are provided without gaps on the surface of the substrate 12'.
[0060] The horizontal axis of the graph in Figure 11 represents the type of sample. Specifically, Case 0 shows a light absorber 10 according to the basic embodiment, that is, a light absorber 10 including a substrate 12 without pits 50; Case 1 shows a light absorber 10' including a substrate 12' with a plurality of pits 1 mm wide and 1 mm deep; Case 2 shows a light absorber 10' including a substrate 12' with a plurality of pits 2 mm wide and 1 mm deep; Case 3 shows a light absorber 10' including a substrate 12' with a plurality of pits 2 mm wide and 2 mm deep; Case 4 shows a light absorber 10' including a substrate 12' with a plurality of pits 3 mm wide and 2 mm deep; and Case 5 shows a light absorber 10' including a substrate 12' with a plurality of pits 3 mm wide and 3 mm deep. Note that Case-1 refers to an aluminum mirror, not the light absorbers 10,10'.
[0061] The vertical axis of the graph in Figure 11 represents the light intensity of the reflected light when a blue laser beam with a wavelength of 461 nm is irradiated onto the sample surface. The squares, circles, upper triangles, and lower triangles in the graph in Figure 11 indicate the light intensity of the reflected light when the incident angle of the laser beam irradiating the sample is 80 degrees, 60 degrees, 45 degrees, and 30 degrees, respectively.
[0062] Figure 11 shows that, compared to the basic embodiment (Case 0) having a flat plate-shaped base 12, the modified examples (Cases 1-5) having a base 12' with multiple pits 50 have lower reflected light intensity (i.e., absorb more light) at all angles of incidence. In particular, at an angle of incidence of 45 degrees (upper triangle), it can be seen that the modified examples absorb significantly more light than the basic embodiment.
[0063] Furthermore, comparing Case 2 and Case 3, or Case 4 and Case 5, which have the same width, it can be seen that the deeper the pit, the more light is absorbed. In the case of an ideal pyramidal pit 50, the surface roughness (root mean square roughness) R of the substrate 12' q If the depth of pit 50 is d, It is represented by R. Generally, q A larger size means that it can absorb more reflected light.
[0064] The modified base 12' shown in Figures 8 to 10 was provided with a plurality of pits 50, but as another modified base 12', a base 12' provided with a plurality of protrusions on its surface may be used.
[0065] The shape of such protrusions is not limited to these, but may be a polygonal pyramidal, conical, or spherical notch. Alternatively, the shapes of multiple protrusions do not all need to be the same, and various shapes may be mixed. In order to provide multiple protrusions on the surface of the base 12' with as few gaps as possible, the shape of the protrusions in plan view may be a triangle, a square, or a hexagon.
[0066] The size (width and height) of the protrusions may be considerably larger than the size of the particle 14. For example, the size of the protrusions may be 10 times or more the size of the particle 14. For example, if the particle 14 is on the order of micrometers (75 μm in this embodiment), the size of the protrusions may be on the order of millimeters.
[0067] A modified light absorber 10' having a substrate 12' provided with multiple protrusions has a similar structure to the light absorber 10 according to the basic embodiment, except that multiple protrusions are provided on the surface of the substrate 12'. That is, multiple particles 14 are randomly stacked on the surface of the substrate 12' provided with multiple protrusions, thereby forming a group of particles 16 on the surface of the substrate 12'. Then, the multiple particles 14 are bonded to each other, and an oxide film 18 is formed on the surface of each particle 14. Because multiple protrusions are provided on the surface of the substrate 12', the multiple particles 14 are also randomly stacked on the protrusions.
[0068] In the modified embodiment having a base 12' provided with multiple protrusions, electromagnetic waves can be absorbed more effectively than in the basic embodiment, similar to the modified embodiment having a base 12' provided with multiple pits 50. The principle is the same as in the modified embodiment having a base 12' provided with multiple pits 50. That is, when an electromagnetic wave passes through the group of particles 16 stacked on the protrusions and reaches the base 12', the electromagnetic wave is reflected by the surface of the protrusion. Since the orientation of the surface of the protrusion is not parallel to the extension direction of the base 12', when an electromagnetic wave is reflected by the surface of a protrusion, the electromagnetic wave does not necessarily travel away from the base 12'. For example, an electromagnetic wave reflected by the surface of a certain protrusion may travel towards another protrusion in the vicinity of that protrusion. In that case, even if the electromagnetic wave reflected by the surface of the protrusion passes through the group of particles 16 stacked on that protrusion again, it will be incident on the group of particles 16 stacked on another protrusion in the vicinity of that protrusion. Furthermore, it is expected that the electromagnetic waves will be reflected (i.e., their intensity will be attenuated) by the wall portion 14a within the particle group 16 stacked on the other protrusions.
[0069] As described above, by providing multiple protrusions on the substrate 12', the modified light absorber 10' can reflect electromagnetic waves within the light absorber 10' more times than the light absorber 10 according to the basic embodiment. Therefore, the modified light absorber 10' is capable of absorbing electromagnetic waves more effectively than the light absorber 10 according to the basic embodiment.
[0070] <Method for manufacturing a light absorber according to this embodiment> The outline of the method for manufacturing the light absorber 10 is as follows. First, a plurality of particles 14 are dropped onto the substrate 12 from random positions. Each particle 14 scatters randomly on the substrate 12 and eventually piles up. With the plurality of particles 14 piled up, the particles 14 are bonded to each other, and to the substrate 12. Here, the plurality of particles 14 are heated to their melting point, and the particles 14 are sintered to each other, and to the substrate 12. After sintering, heating is stopped and the mixture is cooled to room temperature. This first forms a group of particles 16. Next, an oxide film 18 is formed on the surface of each particle 14 by heating the surface of each particle 14 or by a chemical method.
[0071] Hereinafter, several specific examples of the method for manufacturing the light absorber 10 will be described. Note that the method for manufacturing the light absorber 10 is not limited to the following examples.
[0072] The particle group 16 can be formed using an electron beam type metal 3D printer. As a modeling method, a powder bed fusion bonding method can be used. As described above, pure copper with an average diameter of 75 μm (standard deviation 10 μm) is used as the powder for the particles 14. FIG. 12 is a photograph showing the surface of the particle group 16 formed by an electron beam type metal 3D printer. FIG. 13 is an enlarged photograph of the surface of the particle group 16 before the oxide film 18 is formed. FIG. 13 shows that the state of the unmelted residual particles 14 that were not powder-melted and bonded near the surface of the particle group 16 is very similar to the three-dimensionally and randomly stacked state of the particles 14 shown in FIG. 1 and the like.
[0073] As another method, the particle group 16 may be formed using a laser beam type metal 3D printer that uses copper powder.
[0074] Considering cases such as when the light absorber 10 is used in an ultra-high vacuum environment, it is not preferable that the gaps 20 are formed at positions sufficiently deep from the surface layer that may cause virtual leaks. In addition, it is not preferable that the gaps 20 containing impurity gases are formed. Therefore, the particle group 16 is preferably formed under vacuum or in an inert gas atmosphere, and each particle 14 is sufficiently melted to form a laminate with a high filling rate. For example, during layered printing by a metal 3D printer, cuprous oxide (I) (Cu 2 O) that may be formed at a low oxygen partial pressure, or when some undesired chemical modification has proceeded, it is preferable to perform cleaning before the formation process of the oxide film 18, for example, with dilute nitric acid or a reducing agent, so that the surface of each particle 14 is restored to pure copper.
[0075] Furthermore, the particle group 16 can also be formed without using a metal 3D printer. For example, the particle group 16 may be formed using copper foil as the substrate 12, fine copper powder as the particles 14, and a vacuum furnace. Here, the fine copper powder is spherical, and its statistically average diameter is equal to or greater than the upper limit wavelength of the electromagnetic wave to be absorbed.
[0076] The specific method for manufacturing the particle group 16 is as follows. First, fine powder is placed on a copper foil and spread evenly. That is, the fine powder particles 14 are randomly layered. The surface thickness of the fine powder is made to be thicker than the upper limit wavelength of the electromagnetic waves to be absorbed. Next, the copper foil with the fine powder is set in a vacuum furnace and vacuum is applied to prevent oxidation during the sintering process. After that, it is heated to around the melting point of copper, and after waiting for an appropriate amount of time, the heating is stopped. As a result, multiple fine powders are sintered with each other, and multiple fine powders and copper foil are also sintered. Regarding the waiting time during the sintering process, it is advisable to determine in advance, through heating experiments and observations using a microscope, the time required for the fine powders to sinter while maintaining their shape.
[0077] The oxide film 18 is formed by heating the surface of each particle 14. Specifically, the formed particle group 16 (each particle 14) is washed with acetone ultrasonic cleaning or ethanol ultrasonic cleaning, and then heated in air at 400°C for about 24 hours. As a result, the surface of each particle 14 is oxidized, and copper(II) oxide (CuO) is formed. Figure 14 is a photograph showing the surface of the particle group 16 on which the oxide film 18 is formed.
[0078] As reported in "CuO Nanowires Can Be Synthesized by Heating Copper Substrates in Air", Xuchuan Jiang, Thurston Herricks, and Younan Xia, Nano Letters, 2(2002) 1333, when copper is thermally oxidized in air, a black copper(II) oxide film with a nano-sized needle-like fractal structure is formed. Thus, the oxide film 18 has a fractal structure containing multiple dendritic microstructures oriented in random directions.
[0079] Alternatively, the oxide film 18 may be formed by a method that chemically promotes an oxidation reaction of copper. "In-vacuum scattered light reduction with black cupric oxide surfaces for sensitive fluorescence detection", EB Norrgard, N. Sitaraman, JF Barry, DJ McCarron, MH Steinecker, D. DeMille, REVIEW OF SCIENTIFIC INSTRUMENTS 87, 053119 (2016) mentions NaOH and NaClO 2 The copper piece is immersed in the solvent, and the copper surface is treated with Cu(OH) 2 A method has been described in which CuO is obtained by heating to about 100°C and dehydrating the material. It has been reported that a black body with a nano-sized dendritic fractal structure was obtained using this chemical method. Therefore, the oxide film 18 may be formed by such a chemical method.
[0080] When a chemical oxidation reaction is used to form the oxide film 18, the solvent is preferably a gaseous or low-viscosity solution that can penetrate the gaps 20 between the particle group 16. If a highly viscous solution is used, it is preferable to dilute it with a low-viscosity solvent such as acetone or toluene.
[0081] <Examples of Use of the Light Absorber According to This Embodiment> <<Radiation Shield>> Examples of use of the light absorber 10 will be described below. Examples of use of the light absorber 10 are not limited to these, but here we will describe an example in which the light absorber 10 is used on the inner wall of a hollow radiation shield having an internal space. An example of a hollow radiation shield 30 having an internal space is the radiation shield proposed in Japanese Patent No. 7189588.
[0082] Figure 15 is an external perspective view of the radiation shield 30. Figure 16 is an end view of the radiation shield 30. The radiation shield 30 is constructed including a case member 32 that forms an internal space on the inside. In the examples of Figures 15 and 16, the outer shape of the case member 32 is spherical and hollow.
[0083] The case member 32 has an aperture 32a, which is an opening. In the example shown in Figures 15 and 16, two apertures 32a are provided in positions that are directly opposite each other. As will be described later, the radiation shield 30 according to this embodiment is used in an optical lattice clock, and a clock transition space is formed inside the radiation shield 30, with the two apertures 32a serving as paths for the atomic ensemble, the optical lattice light beam, and the laser light for the clock transition. Note that the use of the radiation shield 30 is not limited to optical lattice clocks.
[0084] A light absorber 10 is provided on the inner wall of the case member 32. As a result, electromagnetic waves of multiple wavelength bands (in this embodiment, blackbody radiation and stray light from the surroundings) are absorbed inside the case member 32.
[0085] Conventionally, it has been difficult to form a light absorber 10 on the inner wall of a closed space, such as the inner wall of a case member 32. However, the light absorber 10 according to this embodiment has the advantage that it can be easily formed on the inner wall of such a closed space.
[0086] Specifically, the case member 32 is formed using a metal 3D printer as described above, with powder such as pure copper. This allows the case member 32 itself to become a group of particles 16. Then, by thermally or chemically oxidizing the case member 32, an oxide film 18 can be formed on the surface of each particle 14 forming the case member 32. If it is desired to remove the oxide film 18 from the outer wall of the case member 32, for example, to reduce the emissivity of the outer wall of the case member 32, the aperture 32a can be masked with a Teflon® resin resistant to acidic solutions, and then the outer wall can be immersed in an acid such as dilute hydrochloric acid to remove the oxide film 18.
[0087] Figure 17 is a conceptual diagram showing how an ultrathin metal film 34 is formed on the inner wall of the case member 32 of the radiation shield 30. When a light absorber 10 is provided on the inner wall of the case member 32, an ultrathin metal film 34 made of metal may be provided so as to cover the inner wall, in other words, so as to cover the group of particles 16 consisting of individual particles 14 on which an oxide film 18 is formed on the surface. In order to minimize the influence on the electromagnetic wave absorption performance of the light absorber 10, the thickness of the ultrathin metal film 34 should be as thin as possible. For example, the ultrathin metal film 34 may have a thickness on the order of angstroms (for example, 2 to 5 angstroms).
[0088] If the oxide film 18 is an insulator, it may become charged. Depending on the intended use of the radiation shield 30, it may be undesirable for the oxide film 18 to become charged. For example, if the radiation shield 30 is used in an optical lattice clock, the charge on the oxide film 18 may disrupt the quantum state of the atom being measured via the Stark effect. In such cases, the charging of the light absorber 10 can be suppressed by providing an ultrathin metal film 34.
[0089] While not limited to this, an ultrathin metal film 34 can be formed by depositing a metal such as gold. For example, a chemically stable and heat-resistant heating wire 36, such as a tungsten wire, is passed through the aperture 32a, and a metal 38 with a low boiling point, such as gold or aluminum, is attached to the heating wire 36 in the internal space of the case member 32. When an electric current is passed through the heating wire 36 in this state, the metal 38 generates heat and evaporates radially, allowing the metal 38 to be deposited so as to cover the oxide film 18. This forms an ultrathin metal film 34. The thickness of the ultrathin metal film 34 can be controlled by the time the electric current is passed through the heating wire 36, etc.
[0090] <<Optical Lattice Clock>> Figure 18 is a simplified diagram of an optical lattice clock 40 equipped with a radiation shield 30 on which an optical absorber 10 is provided according to this embodiment. The optical lattice clock 40 is an atomic clock proposed in 2001 by Hidetoshi Katori, one of the inventors of this application. In the optical lattice clock 40, an atomic group is confined within an optical lattice formed by laser light, and the resonant frequency in the visible light region is measured, making it possible to measure with an accuracy of 18 digits, far exceeding the accuracy of a cesium clock.
[0091] Figure 18 is a diagram illustrating the arrangement and configuration of the optical lattice, atoms 42, and radiation shield 30 in an optical lattice clock 40 using a radiation shield 30 having a light absorber 10, with reference to Figure 3 from Japanese Patent No. 7189588. The optical lattice clock 40 is composed of an atomic oven that outputs atoms to form an atomic beam, a MOT device that captures the decelerated atoms, an optical resonator that forms an optical lattice for confining the captured atoms and moving them into the clock transition space, and a radiation shield 30. In the low-temperature operating optical lattice clock 40, clock transition spectroscopy of Sr atoms is performed in an extremely low-temperature environment by surrounding the region around the atoms during spectroscopy with the radiation shield 30. Atoms 42 such as Sr atoms are supplied from the atomic oven and cooled and captured by the light beam of a cooling laser 44 that is three-dimensionally opposed outside the radiation shield 30 (MOT device). After that, they are trapped in the optical lattice created by the optical lattice laser 46. The optical lattice is a standing wave created by opposing light of the same wavelength (e.g., a magic wavelength) arranged, for example in one dimension, so as to penetrate the radiation shield 30. By modulating the wavelength of one of the light beams, trapped atoms can be precisely transported into the radiation shield 30 (moving optical lattice). The atoms 42 are transported into the radiation shield 30 and remain trapped in the optical lattice created by the optical lattice laser 46, while a clock transition is observed at an appropriate position within the radiation shield 30 using optical means such as a clock laser. The operation of these optical lattice clocks 40 is performed in a vacuum chamber with an appropriate range.
[0092] Here, it has been pointed out that stray light, such as leakage from the preceding cooled laser 44, and blackbody radiation from the surroundings can cause perturbations around atoms or disrupt their quantum state (for example, Japanese Patent No. 7189588, or "Long-lived circular Rydberg states of laser-cooled rubidium atoms in a cryostat", T. Cantat-Moltrecht, R. Cortinas, B. Ravon, P. Mehaignerie, S. Haroche, JM Raimond, M. Favier, M. Brune, and C. Sayrin, PHYSICAL REVIEW RESEARCH 2, 022032 (R) (2020)).
[0093] Therefore, in the optical lattice clock 40, blackbody radiation is reduced by keeping the internal space of the radiation shield 30 at a low temperature, and the blackbody radiation is suitably absorbed by the light absorber 10 provided on the inner wall. Thus, it can be said that the light absorber 10 contributes to improving the accuracy of the optical lattice clock 40. Furthermore, since the light absorber 10 can suitably absorb stray light that enters the radiation shield 30 uncontrollably, from this viewpoint as well, it can be said that the light absorber 10 contributes to improving the accuracy of the optical lattice clock 40.
[0094] Furthermore, unwanted magnetic fields near the clock transition space reduce the accuracy of the optical lattice clock 40. However, because the optical absorber 10 (particle group 16 and oxide film 18) is nonmagnetic, the residual magnetic field of the optical absorber 10 is reduced. As a result, the residual magnetic field of the optical absorber 10 does not extend to the clock transition space, and from this viewpoint as well, the optical absorber 10 can contribute to improving the accuracy of the optical lattice clock 40.
[0095] Furthermore, as mentioned above, if the light absorber 10 becomes charged, the charged material may disrupt the quantum state of the atom being measured via the Stark effect. However, by providing the ultrathin metal film 34, the charging of the light absorber 10 can be suppressed. From this viewpoint as well, the light absorber 10 can contribute to improving the accuracy of the optical lattice clock 40.
[0096] <<Magneto-Optical Trap (MOT) Apparatus>> The following describes an example of the use of the modified light absorber 10'. Figure 19 shows the MOT apparatus 60. The MOT apparatus 60 is a device for trapping atoms and can also be used in the optical lattice clock described above.
[0097] The MOT apparatus 60 is a device that achieves atomic cooling and trapping by utilizing the frictional force of laser cooling and the restoring force generated by the Zeeman effect due to the quadrupole magnetic field. In the MOT apparatus, an anti-Helmholtz coil 62 (two coils 62a and 62b through which currents are passed in opposite directions) is used to generate a quadrupole magnetic field at the center of the two coils 62a and 62b. The strength of this quadrupole magnetic field is zero at the center of the anti-Helmholtz coil 62 and increases with distance from the center.
[0098] Furthermore, in each of the three mutually orthogonal directions, pairs of opposing laser beams 64 are irradiated such that the intersection of these laser beams 64 is near the center of the anti-Helmholtz coil 62. The resonance frequency of the atoms is Zeeman-shifted according to their spatial position by the quadrupole magnetic field, and the resonance frequency increases as the distance from the center of the anti-Helmholtz coil 62 increases. At this time, if the polarization of the laser beam 64 is appropriately selected, a restoring force is generated that causes the radiation pressure to move towards the origin. This makes it possible to trap the laser-cooled atoms. The region in which atoms are trapped by this method is called the MOT region 66.
[0099] The atomic beam 68 is irradiated into the MOT region 66. The atomic beam 68 interacts with the opposing decelerating laser beam 70 and magnetic field (not shown in Figure 19), decelerating as it enters the MOT region 66. The atoms that enter the MOT region 66 are trapped in the MOT region 66 using the laser beam 64 and the quadrupole magnetic field generated by the anti-Helmholtz coil 62. The trapped atoms escape from trapping using push laser light, for example, by a method described in the inventor's patent document, International Publication No. 2024 / 004487, and are transported in the direction of arrow A in Figure 19. At the end of the direction of arrow A, a space is prepared for subsequent processes such as a magnetic trap process, a cooling process, and an optical lattice trap process.
[0100] In this MOT apparatus 60, a problem may arise in which fluorescence spontaneously emitted by atoms trapped in the MOT region 66 leaks out as stray light in the direction of arrow A without attenuation.
[0101] Figure 20 shows a modified example of a copper oxide jig 80, in which a light absorber 10' is provided on the inner wall, attached to the MOT apparatus 60. As will be described later, the copper oxide jig 80 is a jig made of copper. As shown in Figure 20, the copper oxide jig 80 is provided so as to surround the MOT region 66 (see Figure 19). The copper oxide jig 80 is hollow inside so as not to obstruct the laser light 64 and atomic beam 68, or to avoid contact with captured atoms.
[0102] A modified light absorber 10' is provided on the inner wall of the copper oxide jig 80. In this example, a plurality of pyramidal pits 50 are periodically provided on the inner wall of the copper oxide jig 80, which serves as the substrate 12' for the light absorber 10'. Multiple particles 14 are randomly stacked on the inner wall (substrate 12') of the copper oxide jig 80 where the multiple pits 50 are provided, and the multiple particles 14 are bonded to each other. Furthermore, an oxide film 18 is formed on the surface of each particle 14. In this way, the light absorber 10' provided on the inner wall of the copper oxide jig 80 absorbs the fluorescence spontaneously emitted by atoms trapped in the MOT region 66. This suppresses the leakage of fluorescence generated by atoms as stray light in the direction of arrow A.
[0103] Furthermore, the copper oxide jig 80 is provided with a waveplate mirror 82. The waveplate mirror 82 reflects the laser light 64, and each opposing pair of laser light 64 consists of the incident light and the reflected light that has been reflected by the waveplate mirror 82. This suppresses the leakage of the laser light 64 in the direction of arrow A.
[0104] The manufacturing method for the copper oxide jig 80 will be described below with reference to Figures 21 to 23. In this example, the copper oxide jig 80 is formed using a powder bed type metal 3D printer. A powder bed type metal 3D printer uses copper powder whose average particle size and its deviation can be controlled, and forms a three-dimensional shape by melting and layering it with an electron beam. Nowadays, in manufacturing using 3D printers, it is common to create objects based on STL (Stereolithography) files, and it is sufficient to prepare numerical data that represents the 3D model as a collection of small triangular meshes.
[0105] The process of creating a set of three-dimensional objects Ω of an arbitrary shape by subtracting pyramidal pits 50 is explained below. The pits 50 are defined locally and modeled as volume removals (set differences) that are pushed in the direction of the normal vector of each point.
[0106] The shape of the base three-dimensional set Ω is an arbitrary three-dimensional set. Let's assume that its surface ∂Ω is a smooth two-dimensional curved surface.
[0107] Regarding pit P, as a local definition, any surface point In this case, the unit normal vector The orthogonal unit vector in that tangent space In the local coordinate system, pit 50 is defined by the following volume: Here, a represents the half-length of the base of pit P, and d represents the depth. Given multiple pits 50, the set P of pits 50 is: This is defined (see Figure 22).
[0108] The new shape Ω' (see Figure 23), obtained by subtracting the pit set P from the base three-dimensional set Ω, is defined as follows: This operation creates pyramidal pits 50 that are pressed in the normal direction at various points on the surface of the base three-dimensional assembly Ω.
[0109] Here, we have described the case where the shape of the pit 50 is pyramidal, but even if the pit 50 has other shapes, it can be formed using the same method by appropriately changing the formula that represents the volume of the pit 50.
[0110] 10,10' Light absorber, 12,12' Substrate, 14 Particles, 14a Wall, 16 Particle group, 18 Oxide film, 20 Gap, 30 Radiation shield, 32 Case member, 32a Aperture, 34 Ultrathin metal film, 36 Heating wire, 38 Metal, 40 Optical lattice clock, 50 Pit, 52 Inner wall, 60 MOT device, 80 Copper oxide jig.
Claims
1. A light absorber comprising: a particle group consisting of a plurality of randomly stacked particles, the particle group having a plurality of gaps formed between the particles and a plurality of wall portions that are part of the surface of each particle facing the gap and are oriented in random directions; and a black film formed by oxidizing or nitriding the surface of each particle, the black film having a plurality of dendritic microstructures oriented in random directions formed by the oxidation or nitriding treatment.
2. The light absorber according to claim 1, characterized in that the particles have a size on the order of micrometers.
3. The light absorber according to claim 1, characterized in that the black film has a fractal structure including the plurality of dendritic microstructures.
4. The light absorber according to claim 1, characterized in that the particles are formed of a non-magnetic material.
5. The light absorber according to claim 1, characterized in that the plurality of particles are bonded to each other.
6. The light absorber according to claim 1, further comprising a substrate having a plurality of pits on its surface, wherein the group of particles is randomly stacked on the surface of the substrate.
7. The light absorber according to claim 6, characterized in that the size of the pit is larger than the size of the particle.
8. The light absorber according to claim 7, characterized in that the pit has a size on the order of millimeters.
9. The light absorber according to any one of claims 6 to 8, characterized in that the shape of the pit is polygonal pyramidal, conical, or spherically pitted.
10. The light absorber according to claim 1, further comprising a substrate having a plurality of protrusions on its surface, wherein the group of particles is randomly stacked on the surface of the substrate.
11. The light absorber according to claim 10, characterized in that the size of the protrusions is larger than the size of the particles.
12. The light absorber according to claim 11, characterized in that the projection has a size on the order of millimeters.
13. The light absorber according to any one of claims 10 to 12, characterized in that the shape of the projection is a polygonal pyramidal, conical, or spherical notch.
14. A radiation shield comprising: a case member having an internal space formed on the inside and an opening; and a light absorber according to claim 1 provided on the inner wall of the case member.
15. The radiation shield according to claim 14, characterized in that the light absorber is provided so as to cover the group of particles, each of which has the black film formed on its surface, and further comprises an ultrathin metal film having a thickness on the order of angstroms.
16. An optical lattice clock comprising: an atomic oven that emits atoms to form an atomic beam; an MOT device for capturing the atoms; an optical resonator that forms an optical lattice for confining the captured atoms and moving them into a clock transition space; and a radiation shield according to claim 14 or claim 15, disposed to include the clock transition space inside the optical lattice clock.