Solid electrolyte layers, preparation method thereof, and all-solid-state rechargeable batteries
A solid electrolyte layer with controlled porosity and hardness addresses lithium dendrite growth issues in all-solid-state secondary batteries, enhancing charge/discharge performance and lifespan through optimized manufacturing processes.
Patent Information
- Application Number
- PCT/KR2025/018930
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2025-11-17
- Publication Date
- 2026-11-12
AI Technical Summary
Conventional all-solid-state secondary batteries face issues with lithium dendrite growth during charging and discharging, leading to short circuits and reduced lifespan due to suboptimal porosity and hardness of the solid electrolyte layer.
A solid electrolyte layer with controlled porosity of 4% to 8% and hardness of HK 63 to HK 79, composed of sulfide-based solid electrolyte particles, is manufactured by mixing with a binder and solvent, then dried at 100°C to 140°C, and optionally pressurized to enhance structural stability.
The solution effectively suppresses lithium dendrite growth, improving charge/discharge performance and lifespan characteristics by preventing cracks and internal short circuits.
Smart Images

Figure KR2025018930_12112026_PF_FP_ABST
Abstract
Description
Solid electrolyte layer and method of manufacturing the same, and all-solid-state secondary battery
[0001] This invention relates to a solid electrolyte layer, a method for manufacturing the same, and an all-solid-state secondary battery.
[0002] Lithium-ion batteries, which offer high energy density and portability, are primarily used as the power source for mobile information terminals such as mobile phones, laptops, and smartphones. Recently, active research is being conducted to utilize high-energy-density lithium-ion batteries as power sources for driving or energy storage in hybrid and electric vehicles.
[0003] Since commercially available lithium secondary batteries use electrolytes containing flammable organic solvents, there are safety issues where the battery may explode or catch fire in the event of collisions or penetrations.
[0004] Accordingly, all-solid-state secondary batteries utilizing solid electrolytes instead of liquid electrolytes are being proposed. All-solid-state secondary batteries are composed entirely of solid materials; they offer the advantages of safety by eliminating risks such as explosions caused by electrolyte leakage, and facilitate the fabrication of thin batteries. Furthermore, the reduction in negative electrode thickness enables improved high-speed charging and discharging performance, as well as the realization of high-voltage operation and high energy density.
[0005] One embodiment aims to provide a solid electrolyte layer capable of improving charge / discharge performance and lifespan characteristics by suppressing the growth of lithium dendrites, a method for manufacturing the same, and an all-solid-state secondary battery.
[0006] One embodiment provides a solid electrolyte layer comprising sulfide-based solid electrolyte particles, having an area-based porosity of 4% to 8% and a hardness of HK 63 to HK 79.
[0007] One embodiment provides a method for manufacturing a solid electrolyte layer comprising preparing a slurry for forming a solid electrolyte layer by mixing sulfide-based solid electrolyte particles, a binder, and a solvent, applying the slurry for forming a solid electrolyte layer onto a substrate, and drying at a temperature of 100°C to 140°C to obtain a solid electrolyte layer, wherein the slurry for forming a solid electrolyte layer comprises 1.0% to 2.4% by weight of the binder based on 100% by weight of the total of the sulfide-based solid electrolyte particles and the binder.
[0008] One embodiment provides an all-solid-state secondary battery comprising a positive electrode, a negative electrode, and the aforementioned solid electrolyte layer located between the positive electrode and the negative electrode.
[0009] According to one embodiment, a solid electrolyte layer capable of improving charge / discharge performance and lifespan characteristics by suppressing the growth of lithium dendrites, a method for manufacturing the same, and an all-solid-state secondary battery can be provided.
[0010] FIG. 1 is a schematic cross-sectional view of an all-solid-state secondary battery according to one embodiment.
[0011] FIG. 2 is a schematic cross-sectional view of an all-solid-state secondary battery including a precipitation type negative electrode according to one embodiment.
[0012] FIG. 3 is a schematic cross-sectional view of an all-solid-state secondary battery having two unit cells stacked according to one embodiment.
[0013] Figure 4 is a scanning electron microscope (SEM) image of a cross-section of the solid electrolyte layer taken by disassembling the all-solid-state secondary battery prepared in Example 1.
[0014] Figure 5 is a scanning electron microscope (SEM) image of a cross-section of the solid electrolyte layer taken by disassembling the all-solid-state secondary battery prepared in Example 2.
[0015] Figure 6 is a scanning electron microscope (SEM) image of a cross-section of the solid electrolyte layer taken by disassembling the all-solid-state secondary battery prepared in Example 3.
[0016] Figure 7 is a scanning electron microscope (SEM) image of a cross-section of the solid electrolyte layer after disassembling the all-solid-state secondary battery prepared in Comparative Example 1.
[0017] Figure 8 is a scanning electron microscope (SEM) image of a cross-section of the solid electrolyte layer after disassembling the all-solid-state secondary battery prepared in Comparative Example 2.
[0018] Figure 9 is a scanning electron microscope (SEM) image of a cross-section of the solid electrolyte layer after disassembling the all-solid-state secondary battery prepared in Comparative Example 3.
[0019] Figure 10 is a scanning electron microscope (SEM) image of a cross-section of the solid electrolyte layer after disassembling the all-solid-state secondary battery prepared in Comparative Example 4.
[0020] FIG. 11 shows the results of the change in discharge capacity as the cycle progresses for all-solid-state secondary batteries prepared in Examples 1 and 2 and Comparative Examples 1 to 4.
[0021] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples and are not intended to limit the present invention, and the present invention is defined only by the scope of the claims set forth below.
[0022] Unless otherwise specifically stated in this specification, when a part such as a layer, film, region, plate, etc. is described as being "on" another part, this includes not only cases where it is "immediately on" another part, but also cases where there is another part in between.
[0023] Unless otherwise specified in this specification, a singular form may also include a plural form. Additionally, unless otherwise specified, "A or B" may mean "including A, including B, or including A and B."
[0024] In this specification, "combination of these" may mean a mixture of components, a laminate, a composite, a copolymer, an alloy, a blend, and a reaction product, etc.
[0025] Unless otherwise defined in this specification, particle size may be the average particle size. Additionally, particle size refers to the average particle size (D) which means the diameter of the particle whose cumulative volume in the particle size distribution is 50 volume%. 50 It means ). Average particle size (D 50 The measurement can be performed using methods widely known to those skilled in the art, for example, by using a particle size analyzer, or by using transmission electron microscope (TEM) or scanning electron microscope (SEM) images. Alternatively, the measurement may be performed using a measuring device utilizing dynamic light scattering, and after analyzing the data to count the number of particles for each particle size range, the average particle size (D) is calculated from this. 50 ) values can be obtained. Alternatively, it can be measured using the laser diffraction method. When measuring by the laser diffraction method, more specifically, after dispersing the particles to be measured in a dispersion medium, they are introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000), and ultrasound at approximately 28 kHz is irradiated at an output of 60 W. Then, the average particle size (D) at the 50% reference of the particle size distribution in the measuring device 50 ) can be produced.
[0026] The terms "include," "equip," or "have" used herein are intended to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and should be understood as not excluding in advance the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0027] In addition, the term “layer” here includes not only the shape formed on the entire surface when viewed in a plan view, but also the shape formed on some surfaces.
[0028] The term “metal” is interpreted as a concept that includes common metals, transition metals, and metalloids (semimetals).
[0029] "Thickness" may be measured, for example, through photographs taken with an electron microscope such as a scanning electron microscope or an optical microscope.
[0030] solid electrolyte layer
[0031] One embodiment provides a solid electrolyte layer comprising sulfide-based solid electrolyte particles, having an area-based porosity of 4% to 8% and a hardness of HK 63 to HK 79.
[0032] In all-solid-state secondary batteries, as the charging and discharging process progresses, lithium dendrites grow at the negative electrode, causing a short circuit, which limits the lifespan of the battery.
[0033] The solid electrolyte layer of conventional all-solid-state secondary batteries exhibited an area-based porosity of 9%, exceeding 8%, and a hardness of 60 HK. Using a solid electrolyte layer with such porosity and hardness, it was difficult to suppress the growth of lithium dendrites during the charging and discharging process of the all-solid-state secondary battery, resulting in a relatively short lifespan and limiting the improvement of the lifespan of the all-solid-state secondary battery.
[0034] Accordingly, in one embodiment, the growth of lithium dendrites is effectively suppressed by controlling and optimizing the porosity and hardness of the solid electrolyte layer, and the charge / discharge performance and lifespan characteristics of the all-solid-state secondary battery are also improved.
[0035] To this end, the solid electrolyte layer according to one embodiment may have a porosity of 4% to 8% based on area. If the porosity is too low, cracks may easily occur in the electrolyte layer, and the effect of inhibiting the growth of lithium dendrites due to the occurrence of cracks may be insufficient; if the porosity is too high, the growth of lithium dendrites cannot be sufficiently inhibited, and cell performance may deteriorate. Accordingly, by controlling the porosity to the aforementioned optimal range, the growth of lithium dendrites can be inhibited while simultaneously preventing the occurrence of cracks, thereby improving charge / discharge characteristics and lifespan characteristics.
[0036] The porosity of the above-mentioned solid electrolyte layer can be calculated by performing image processing on a Scanning Electron Microscope (SEM) image of the pressurized solid electrolyte layer (e.g., using the Image J program). For example, by performing image processing on the SEM image to distinguish solid electrolyte particles within the solid electrolyte layer, the porosity can be measured by considering the area occupied by the pores as the area remaining after excluding the portion occupied by the solid electrolyte particles from the total area.
[0037] A solid electrolyte layer according to one embodiment has a hardness of HK 63 to HK 79, and may be, for example, HK 63.5 to HK 78.9, HK 63.55 to HK 78.75, or HK 63.59 to HK 78.74. When the above hardness range is satisfied, the solid electrolyte layer secures sufficient strength, which not only prevents the growth of lithium dendrites but also prevents the occurrence of cracks and internal short circuits, thereby improving the charge / discharge characteristics and lifespan characteristics of the battery. As an example, the hardness may be measured using a Knoop-type microhardness tester to determine the Knoop hardness.
[0038] A solid electrolyte layer according to one embodiment includes sulfide-based solid electrolyte particles to ensure excellent ionic conductivity. That is, the solid electrolyte layer comprises a sulfide-based solid electrolyte as a solid electrolyte, and the sulfide-based solid electrolyte is, for example, Li2S-P2S5, Li2S-P2S5-LiX (where X is a halogen element, for example, I or Cl), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (m and n are integers, and Z is Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (p and q are integers, and M is P, Si, Ge, B, Al, Ga, or In), Li3PS4, Li7P3S 11 It may include Li7PS6, or a combination thereof.
[0039] For example, such a sulfide-based solid electrolyte can be obtained by mixing Li2S and P2S5 in a molar ratio of 50:50 to 90:10 or 50:50 to 80:20 and optionally heat-treating. Within the above mixing ratio range, a sulfide-based solid electrolyte having excellent ionic conductivity can be manufactured. Additionally, SiS2, GeS2, B2S3, etc., as other components may be further included to further improve ionic conductivity.
[0040] For example, mechanical milling or the solution method can be applied as a mixing method for sulfur-containing raw materials to manufacture sulfide-based solid electrolytes. Mechanical milling is a method in which starting materials are placed in a ball mill reactor and vigorously stirred to finely atomize and mix the starting materials. When using the solution method, starting materials are mixed in a solvent to obtain a solid electrolyte as a precipitate. In addition, if heat treatment is performed after mixing, the crystals of the solid electrolyte can become more robust and the ionic conductivity can be improved. For example, a sulfide-based solid electrolyte can be manufactured by mixing sulfur-containing raw materials and heat-treating them two or more times; in this case, a robust sulfide-based solid electrolyte with high ionic conductivity can be produced.
[0041] For example, a sulfide-based solid electrolyte can be manufactured through a first heat treatment in which sulfur-containing raw materials are mixed and calcined at 120°C to 350°C, and a second heat treatment in which the results of the first heat treatment are mixed and calcined at 350°C to 800°C. The first heat treatment and the second heat treatment can each be carried out in an inert gas or nitrogen atmosphere. The first heat treatment can be performed for 1 to 10 hours, and the second heat treatment can be performed for 5 to 20 hours. Through the first heat treatment, the effect of milling small raw materials can be obtained, and through the second heat treatment, the final solid electrolyte can be synthesized. Through two or more such heat treatments, a high-performance sulfide-based solid electrolyte with high ion conductivity and robustness can be obtained, and such a solid electrolyte can be considered suitable for mass production. The temperature of the first heat treatment may be, for example, 150°C to 330°C or 200°C to 300°C, and the temperature of the second heat treatment may be, for example, 380°C to 700°C or 400°C to 600°C.
[0042] For example, the sulfide-based solid electrolyte particles may include argyrodite-type sulfides. Such argyrodite-type sulfides have an ionic conductivity of 10 at room temperature, which is the ionic conductivity of a typical liquid electrolyte. -4 to 10 -2 It has high ionic conductivity close to the S / cm range. Furthermore, it can form a tight bond between the positive active material and the solid electrolyte without causing a decrease in ionic conductivity, and can form a tight interface between the electrode and the solid electrolyte layer. An all-solid-state secondary battery containing this can improve battery performance such as rate characteristics, Coulomb efficiency, and lifespan characteristics.
[0043] For example, the above azirodite-type sulfide can be represented by the following chemical formula 1.
[0044] [Chemical Formula 1]
[0045] (Li a M1 b M 2 c )(P d M 3 e )(S f M 4 g )X h
[0046] In the above chemical formula 1, 4≤a≤8, and M 1 is Mg, Cu, Ag, or a combination thereof, 0≤b<0.5, and M 2 is Na, K, or a combination thereof, 0≤c<0.5, and M 3 is Sn, Zn, Si, Sb, Ge, or a combination thereof, and 0 <d<4, 0≤e<1 이고, M 4 is O, SO n , or a combination thereof, 1.5≤n≤5, 3≤f≤12, 0≤g<2, and X is F, Cl, Br, I, or a combination thereof, and 0 <h≤2이다.
[0047] For example, M in Chemical Formula 1 1 An element may be required, in which case 0 <b<0.5로 표시될 수 있다. 화학식 1에서 M 3 can be understood as the element substituted at the P position, and 0 <e<1일 수 있다. 화학식 1에서 M 4 is substituted into the S position, for example, 0 <g<2일 수 있으며, S의 비율인 f는 예를 들어 3≤f≤7일 수 있다. M 4 ga SO n In the case of SO n It can be, for example, S4O6, S3O6, S2O3, S2O4, S2O5, S2O6, S2O7, S2O8, SO4, or SO5, and as an example, it can be SO4.
[0048] For example, in Chemical Formula 1, a+b+c+h=7, d+e=1, and f+g+h=6.
[0049] As a specific example, the above azirodite-type sulfide is Li6PS5Cl, Li6PS5Br, Li 5.8 PS 4.8 Cl 1.2 , Li 6.2 PS 5.2 Br 0.8 , Li 5.75 PS 4.75 Cl 1.25 , (Li 5.69 Cu 0.06 )PS 4.75 Cl 1.25 , (Li 5.72 Cu 0.03 )PS 4.75 Cl 1.25 , (Li 5.69 Cu 0.06 )P(S 4.70 (SO4) 0.05 )Cl 1.25 , (Li 5.69 Cu 0.06 )P(S 4.60 (SO4) 0.15 )Cl 1.25 , (Li 5.72 Cu 0.03 )P(S 4.725 (SO4) 0.025 )Cl 1.25 , (Li 5.72 Na 0.03 )P(S 4.725 (SO4) 0.025 )Cl 1.25 , Li 5.75 P(S 4.725 (SO4) 0.025 )Cl 1.25 , or a combination thereof may be included, but is not limited thereto.
[0050] For example, an azirodite-type sulfide can be prepared by mixing, for example, lithium sulfide and phosphorus sulfide, and optionally lithium halide. After mixing these, heat treatment may be performed. The heat treatment may include, for example, two or more heat treatment steps.
[0051] For example, manufacturing an azirodite-type sulfide may include a first heat treatment in which raw materials are mixed and calcined at 120°C to 350°C, and a second heat treatment in which the product of the first heat treatment is mixed again and calcined at 350°C to 800°C.
[0052] For example, the average particle size (D) of the above sulfide-based solid electrolyte particles 50 ) may, for example, be 0.1 μm to 5.0 μm or 0.1 μm to 3.0 μm, be fine particles of 0.1 μm to 1.9 μm, or be coarse particles of 2.0 μm to 5.0 μm. The sulfide-based solid electrolyte particles may be a mixture of fine particles with an average particle size of 0.1 μm to 1.9 μm and coarse particles with an average particle size of 2.0 μm to 5.0 μm. The average particle size of the sulfide-based solid electrolyte particles may be measured using electron microscope images, for example, by measuring the size (diameter or length of the major axis) of about 20 particles from scanning electron microscope images to obtain a particle size distribution, where D 50 It could be that it was calculated.
[0053] For example, in the solid electrolyte layer, the sulfide-based solid electrolyte particles may be included in an amount of 97.6% to 99%, 97.7% to 98.9%, or 98.0% to 98.7% based on 100% by weight of the solid electrolyte layer. Within this range, excellent ion conductivity can be secured while also ensuring the durability of the battery.
[0054] In one embodiment, the solid electrolyte layer may include sulfide-based solid electrolyte particles and a binder. The above binder is, for example, nitrile-butadiene rubber, hydrogenated nitrile-butadiene rubber, styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, natural rubber, polydimethylsiloxane, polyethylene oxide, polyvinylpyrrolidone, polyvinylpyridine, chlorosulfonated polyethylene, polyvinyl alcohol, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-propylene-diene copolymer, polyamideimide, polyimide, poly(meth)acrylate, polyacrylonitrile, polystyrene, polyurethane, and their It may include copolymers, or combinations thereof.
[0055] For example, in the solid electrolyte layer, the binder may be included in an amount of 1.0 to 2.4 wt%, 1.1 to 2.3 wt%, or 1.3 to 2.0 wt% based on 100 wt% of the solid electrolyte layer. When the binder is included within the above range, the components within the solid electrolyte layer can be well bonded without lowering the ionic conductivity of the solid electrolyte, thereby improving the durability and reliability of the battery. In addition, it contributes to controlling the hardness of the solid electrolyte layer, which can prevent the growth of lithium dendrites. Through this, the occurrence of cracks can be prevented and internal short circuits can be prevented. This can effectively contribute to improving the charge / discharge characteristics and lifespan characteristics of the battery.
[0056] For example, the solid electrolyte layer may further include a dispersant, and the dispersant may include, for example, hydrogenated butadiene-based rubber. For example, the dispersant may include rubber prepared by hydrogenating a copolymer of a diene-based monomer and a (meth)acrylonitrile-based monomer. Here, the (meth)acrylonitrile-based monomer may include a methacrylonitrile-based monomer and an acrylonitrile-based monomer. If this is satisfied, it may be advantageous to secure optimal porosity and hardness of the solid electrolyte layer. Through this, the growth of lithium dendrites and the occurrence of cracks can be effectively prevented, and it may contribute to the improvement of the charge / discharge characteristics and lifespan characteristics of the battery.
[0057] The above dispersant may include, for example, hydrogenated nitrile butadiene rubber (HNBR). If this is satisfied, it may be advantageous to secure optimal porosity and hardness of the solid electrolyte layer. Through this, the growth of lithium dendrites and the occurrence of cracks can be effectively prevented, and it can contribute to the improvement of the charge / discharge characteristics and lifespan characteristics of the battery.
[0058] For example, when the solid electrolyte layer comprises the dispersant, the solid electrolyte layer may comprise the sulfide-based solid electrolyte particles in an amount of 96.6 wt% to 98.99 wt%, 97.1 wt% to 98.85 wt%, or 97.6 wt% to 98.6 wt%, and / or the binder may comprise 1.0 wt% to 2.4 wt%, 1.1 wt% to 2.3 wt%, or 1.3 wt% to 2.0 wt% based on 100 wt% of the solid electrolyte layer, and the dispersant may comprise 0.01 wt% to 1.0 wt%, 0.05 wt% to 0.6 wt%, or 0.1 wt% to 0.4 wt% based on 100 wt% of the solid electrolyte layer. When a dispersant is included within the above range, it can effectively contribute to securing optimal porosity and hardness of the solid electrolyte layer. Through this, the growth of lithium dendrites and the occurrence of cracks can be effectively prevented, and it can contribute to improving the charge / discharge characteristics and lifespan characteristics of the battery.
[0059] For example, the thickness of the solid electrolyte layer may be 10 µm to 1000 µm, 20 µm to 900 µm, 30 µm to 500 µm, 40 µm to 300 µm, 45 µm to 200 µm, or 50 µm to 150 µm.
[0060] In one embodiment, the solid electrolyte layer may further include other components such as an alkali metal salt, and / or an ionic liquid, and / or a conductive polymer.
[0061] The above alkali metal salt may be, for example, a lithium salt. The content of the lithium salt in the above solid electrolyte layer may be 1 M or more, for example, 1 M to 4 M. In this case, the lithium salt can improve ion conductivity by improving the lithium ion mobility of the solid electrolyte layer.
[0062] Lithium salts may be applied without limitation of type and may include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiSCN, LiN(CN)2, lithium bis(oxalate)borate (LiBOB), lithium difluoro(oxalate)borate (LiDFOB), lithium difluorobis(oxalate)phosphate (LiDFBOP), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(pentafluoroethanesulfonyl)imide (LiBETI), lithium trifluoromethanesulfonate, lithium tetrafluoroethanesulfonate, or combinations thereof.
[0063] For example, the above lithium salt may be an imide-based lithium salt such as LiTFSI, LiFSI, LiBETI, or a combination thereof. The imide-based lithium salt can maintain or improve ionic conductivity by appropriately maintaining chemical reactivity with the ionic liquid.
[0064] Ionic liquids are salts or room temperature molten salts that have a melting point below room temperature, are in a liquid state at room temperature, and consist only of ions.
[0065] The ionic liquid comprises a) one or more cations selected from ammonium, pyrrolidinium, pyridinium, pyrimidinium, imidazolium, piperidinium, pyrazolium, oxazolium, pyridazinium, phosphonium, sulfonium, triazolium, and mixtures thereof, and b) BF4 - , PF6 - , AsF6 - , SbF6 - , AlCl4 - , HSO4 - , ClO4 - , CH3SO3 - , CF3CO2 - , Cl - , Br - , I - , BF4 -, SO4 - , CF3SO3 - , (FSO2)2N - , (C2F5SO2)2N - , (C2F5SO2)(CF3SO2)N - , and (CF3SO2)2N - It may be a compound containing one or more anions selected from among.
[0066] The above ionic liquid may include, for example, N-methyl-N-propylpyrrolidinium bis(trifluoromethanesulfonyl)imide, N-butyl-N-methylpyrrolidinium bis(3-trifluoromethylsulfonyl)imide, 1-butyl-3-methylimidazolinium bis(trifluoromethylsulfonyl)amide, 1-ethyl-3-methylimidazolinium bis(trifluoromethylsulfonyl)amide, or a combination thereof.
[0067] The weight ratio of the solid electrolyte to the ionic liquid in the above solid electrolyte layer may be 0.1:99.9 to 90:10, and for example, 10:90 to 90:10, 20:80 to 90:10, 30:70 to 90:10, 40:60 to 90:10, or 50:50 to 90:10. A solid electrolyte layer satisfying the above range can maintain or improve ionic conductivity by increasing the electrochemical contact area with the electrode. Accordingly, the energy density, discharge capacity, rate characteristics, etc. of the all-solid-state secondary battery can be improved.
[0068] Method for manufacturing a solid electrolyte layer
[0069] One embodiment provides a method for manufacturing a solid electrolyte layer comprising preparing a slurry for forming a solid electrolyte layer by mixing sulfide-based solid electrolyte particles, a binder, and a solvent, applying the slurry for forming a solid electrolyte layer onto a substrate, and drying at a temperature of 100°C to 140°C to obtain a solid electrolyte layer, wherein the slurry for forming a solid electrolyte layer comprises 0.5% to 2.5% by weight of the binder based on 100% by weight of the total of the sulfide-based solid electrolyte particles and the binder.
[0070] The foregoing description pertains to a method for manufacturing a solid electrolyte layer in one embodiment. Below, descriptions that overlap with the foregoing description of the solid electrolyte layer will be omitted, and the processes for manufacturing the solid electrolyte layer in one embodiment will be described.
[0071] First, a slurry for forming a solid electrolyte layer is prepared by mixing sulfide-based solid electrolyte particles, a binder, and a solvent. At this time, the description above regarding the solid electrolyte layer can be applied in the same way to the sulfide-based solid electrolyte particles and the binder.
[0072] For example, the solvent may be applied without limitation as long as it is a solvent capable of dispersing the sulfide-based solid electrolyte particles and the binder, and conventional solvents known in the art may be used. For example, the solvent may include octyl acetate, isobutyl isobutylate, xylene, toluene, benzene, hexane, or a combination thereof.
[0073] For example, in the slurry for forming the solid electrolyte layer, the sulfide-based solid electrolyte particles may be included in an amount of 97.6% to 99% by weight, 97.7% to 98.9% by weight, or 98.0% to 98.7% by weight, based on 100% by weight of the total of the sulfide-based solid electrolyte particles and the binder. Within this range, excellent ion conductivity can be secured while also ensuring the durability of the battery.
[0074] In the above slurry for forming a solid electrolyte layer, the binder is included in an amount of 1.0% to 2.4% by weight based on 100% by weight of the total of the sulfide-based solid electrolyte particles and the binder. When the binder is included within this range, the components within the solid electrolyte layer can be well bonded without lowering the ionic conductivity of the solid electrolyte, thereby improving the durability and reliability of the battery. In addition, it contributes to controlling the hardness of the solid electrolyte layer, which can prevent the growth of lithium dendrites. Through this, the occurrence of cracks can be prevented and internal short circuits can be prevented. This can effectively contribute to improving the charge / discharge characteristics and lifespan characteristics of the battery.
[0075] For example, in the slurry for forming the solid electrolyte layer, the binder may be included in an amount of 1.1% to 2.3% by weight, or 1.3% to 2.0% by weight, based on 100% by weight of the total of the sulfide-based solid electrolyte particles and the binder.
[0076] For example, the slurry for forming the solid electrolyte layer may further include a dispersant, and the description above regarding the solid electrolyte layer can be applied in the same way.
[0077] For example, when the slurry for forming the solid electrolyte layer comprises the dispersant, the slurry for forming the solid electrolyte layer may comprise the sulfide-based solid electrolyte particles in an amount of 96.6 wt% to 98.99 wt%, 97.1 wt% to 98.85 wt%, or 97.6 wt% to 98.6 wt% based on 100 wt% of the total of the sulfide-based solid electrolyte particles, the binder, and the dispersant, and / or the binder may comprise 1.0 wt% to 2.4 wt%, 1.1 wt% to 2.3 wt%, or 1.3 wt% to 2.0 wt% based on 100 wt% of the solid electrolyte layer, and the dispersant may comprise 0.01 wt% to 1.0 wt%, 0.05 wt% to 0.6 wt%, or 0.1 wt% to It may be included in an amount of 0.4 wt%. When the dispersant is included within the above range, it can effectively contribute to securing optimal porosity and hardness of the solid electrolyte layer. Through this, the growth of lithium dendrites and the occurrence of cracks can be effectively prevented, and it can contribute to improving the charge / discharge characteristics and lifespan characteristics of the battery.
[0078] Next, the slurry for forming the solid electrolyte layer is applied onto a substrate. Any method commonly known in the relevant technical field may be used as the application method without limitation. For example, methods such as bar coating, spin coating, die coating, transfer coating, and spray coating may be used. At this time, any material commonly known in the relevant technical field may be used as the substrate without limitation.
[0079] Subsequently, a slurry for forming a solid electrolyte layer coated on the above substrate is dried at a temperature of 100°C to 140°C to obtain a solid electrolyte layer. In conventional solid electrolyte layer manufacturing, drying was typically performed at a temperature of 80°C or lower. However, in the method for manufacturing a solid electrolyte layer according to one embodiment, by controlling the drying temperature to a temperature range of 100°C to 140°C, which is higher than usual, capillary action and boiling phenomena can be controlled, and thereby the porosity and hardness of the solid electrolyte layer can be secured within an optimal range, thereby improving cell performance.
[0080] For example, the drying can be performed under a vacuum atmosphere. If this is satisfied, it can prevent oxidation and moisture exposure, thereby contributing to the formation of a uniform pore structure and preventing unnecessary side reactions. Furthermore, it can prevent excessive boiling during the drying process, allowing for uniform pore formation.
[0081] For example, the drying may be performed for 30 minutes to 10 hours, 1 hour to 8 hours, or 2 hours to 5 hours. Within this range, excessive capillary action and boiling phenomena during the drying process can be prevented, thereby forming uniform pores and contributing to the improvement of the structural stability of the membrane.
[0082] For example, the drying may include raising the temperature to the drying temperature at a heating rate of 5 ℃ / min to 30 ℃ / min or 10 ℃ / min to 20 ℃ / min, and, for example, maintaining the temperature at the drying temperature for a set drying time. If this is satisfied, capillary action and boiling phenomenon can be controlled, thereby securing the porosity and hardness of the solid electrolyte layer within an optimal range, and improving cell performance.
[0083] For example, after the above drying, the method may further include applying pressure, and the pressure may be hydrostatic pressure applied under hydrostatic pressure conditions. By satisfying this, uniform pressure can be delivered to the entire solid electrolyte layer, thereby forming pores uniformly in the solid electrolyte layer, which can contribute to securing excellent mechanical strength, and thereby may be advantageous for suppressing lithium dendrite formation and improving structural stability.
[0084] For example, the above pressurization may be performed at a pressure of 100 MPa to 1000 MPa, 300 MPa to 900 MPa, 400 MPa to 800 MPa, or 500 MPa to 700 MPa. Within this range, it may be advantageous to secure optimal porosity and hardness for the solid electrolyte layer, and by preventing problems such as microcracks occurring or pores collapsing due to increased internal stress in the solid electrolyte layer caused by excessive pressure, the structural stability of the solid electrolyte layer can be improved and the formation of lithium dendrites can be effectively prevented.
[0085] For example, the pressurization may be performed for 10 minutes to 5 hours, 20 minutes to 4 hours, 30 minutes to 3 hours, or 30 minutes to 2 hours. Within this range, problems such as microcracks in the solid electrolyte layer or increased internal stress that may occur during pressurization can be prevented, thereby improving the structural stability of the solid electrolyte layer and effectively preventing the formation of lithium dendrites.
[0086] For example, the pressurization can be performed at a temperature of 60°C to 100°C, 70°C to 90°C, or 75°C to 85°C. Within this range, problems such as microcracks in the solid electrolyte layer or increased internal stress that may occur during pressurization can be prevented, thereby improving the structural stability of the solid electrolyte layer and effectively preventing the formation of lithium dendrites.
[0087] For example, the above-mentioned pressurization may mean pressurizing the laminate after manufacturing the laminate comprising an anode, a cathode, and a solid electrolyte layer, and the solid electrolyte layer may be obtained after applying hydrostatic pressure to the laminate.
[0088] All-solid-state secondary battery
[0089] One embodiment provides an all-solid-state secondary battery comprising a positive electrode, a negative electrode, and the aforementioned solid electrolyte layer located between the positive electrode and the negative electrode.
[0090] FIG. 1 is a cross-sectional view of an all-solid-state secondary battery according to one embodiment. Referring to FIG. 1, the all-solid-state secondary battery (100) may have a structure in which a laminate comprising a negative electrode (400) including a negative electrode current collector (401) and a negative electrode active material layer (403), a solid electrolyte layer (300), and a positive electrode (200) including a positive electrode active material layer (203) and a positive electrode current collector (201) is housed in a battery case. The all-solid-state secondary battery (100) may further include an elastic sheet (500) on the outer side of at least one of the positive electrode (200) and the negative electrode (400). FIG. 1 illustrates a single unit cell that is a laminate comprising a negative electrode (400), a solid electrolyte layer (300), and a positive electrode (200). However, as illustrated in FIG. 3, a solid-state secondary battery may be manufactured by stacking two unit cells, or a solid-state secondary battery may be manufactured by stacking two or more unit cells, for example, 2 to 100, 3 to 50, 4 to 20, etc. Additionally, the unit cell may include one or more negative electrodes, and likewise may include one or more solid electrolyte layers and one or more positive electrodes. For example, the unit cell may be a monocell with a positive electrode / solid electrolyte layer / negative electrode structure, or a bicell with a negative electrode / solid electrolyte layer / positive electrode / solid electrolyte layer / negative electrode structure.
[0091] anode
[0092] The above-mentioned anode comprises an anode current collector and an anode active material layer formed on the anode current collector. The anode active material layer comprises an anode active material, may further comprise a solid electrolyte, and may further comprise a binder and / or a conductive material.
[0093] The above-mentioned positive electrode active material may be applied without limitation as long as it is commonly used in all-solid-state secondary batteries, for example, a compound capable of reversible intercalation and deintercalation of lithium may be used, may include a lithium transition metal complex oxide, and may include a compound represented by any one of the following chemical formulas. a A 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Mn 2-b X b O 4-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Ni 1-b-c Co b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Mn b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni b Co c L 1 d G e O2(0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, 0≤e≤0.1); Li a NiG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li aCoG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-b G b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn2G b O4(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-g G g PO4(0.90≤a≤1.8, 0≤g≤0.5); Li (3-f) Fe2(PO4)3(0≤f≤2); Li a FePO4(0.90≤a≤1.8).
[0094] The above-mentioned positive electrode active material may include, for example, lithium cobalt oxide (LCO), lithium nickel oxide (LNO), lithium nickel cobalt oxide (NC), lithium nickel cobalt aluminum oxide (NCA), lithium nickel cobalt manganese oxide (NCM), lithium nickel manganese oxide (NM), lithium manganese oxide (LMO), lithium iron phosphate oxide (LFP), or a combination thereof.
[0095] The above positive active material may include, for example, a lithium nickel-based oxide represented by the following chemical formula 1A, a lithium cobalt-based oxide represented by the following chemical formula 2A, a lithium iron phosphate-based compound represented by the following chemical formula 3A, a cobalt-free lithium nickel-manganese-based oxide represented by the chemical formula 4A, or a combination thereof.
[0096] [Chemical Formula 1A]
[0097] Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 X b1
[0098] In the above chemical formula 1A, 0.9≤a1≤1.8, 0.3≤x1≤1, 0≤y1≤0.7, 0≤z1≤0.7, 0.9≤x1+y1+z1≤1.1, and 0≤b1≤0.1, and M 1 and M2 Each is independently Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Zr, or a combination thereof, and X is F, P, S, or a combination thereof.
[0099] In the above chemical formula 1A, 0.6≤x1≤1, 0≤y1≤0.4, and 0≤z1≤0.4, or 0.8≤x1≤1, 0≤y1≤0.2, and 0≤z1≤0.2.
[0100] [Chemical Formula 2A]
[0101] Li a2 Co x2 M 3 y2 O 2-b2 X b2
[0102] In the above chemical formula 2A, 0.9≤a2≤1.8, 0.7≤x2≤1, 0≤y2≤0.3, 0.9≤x2+y2≤1.1, and 0≤b2≤0.1, and M 3 is Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mn, Mo, Ni, Se, Si, Sn, Sr, Ti, V, W, Y, Zn, Zr, or a combination thereof, and X is F, P, S, or a combination thereof.
[0103] [Chemical Formula 3A]
[0104] Li a3 Fe x3 M 4 y3 PO 4-b3 X b3
[0105] In the above chemical formula 3A, 0.9≤a3≤1.8, 0.6≤x3≤1, 0≤y3≤0.4, and 0≤b3≤0.1, and M 4 is Al, B, Ba, Ca, Ce, Co, Cr, Cu, Mg, Mn, Mo, Ni, Se, Si, Sn, Sr, Ti, V, W, Y, Zn, Zr, or a combination thereof, and X is F, P, S, or a combination thereof.
[0106] [Chemical Formula 4A]
[0107] Li a4 Ni x4 Mn y4 M 5 z4 O 2-b4 X b4
[0108] In the above chemical formula 4A, 0.9≤a4≤1.8, 0.8≤x4<1, 0 <y4≤0.2, 0≤z4≤0.2, 0.9≤x4+y4+z4≤1.1, 및 0≤b4≤0.1이고 M 5 is Al, B, Ba, Ca, Ce, Cr, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ti, V, W, Zr, or a combination thereof, and X is F, P, S, or a combination thereof.
[0109] The above positive active material may be in the form of particles, and the average particle size (D) of the above positive active material 50 ) may be 1 μm to 25 μm, for example, 3 μm to 25 μm, 1 μm to 20 μm, 1 μm to 18 μm, 3 μm to 15 μm, or 5 μm to 15 μm. As an example, the anode active material has an average particle size (D 50 Fine particles with a diameter of 1 μm to 9 μm and an average particle size (D 50 It may include atoms having a particle size range of 10 μm to 25 μm. A positive electrode active material having this particle size range can be harmoniously mixed with other components within the positive electrode active material layer and can achieve high capacity and high energy density. Here, the average particle size is determined by selecting approximately 20 arbitrary particles from a scanning electron microscope image of the positive electrode active material, measuring their particle sizes (diameter, major axis, or length of the major axis), obtaining a particle size distribution, and determining the diameter (D) of the particle whose cumulative volume is 50 volume% in the particle size distribution. 50 It may be that ) was taken as the average particle size.
[0110] The above positive active material may be in the form of secondary particles formed by the aggregation of a plurality of primary particles, or in the form of single particles. In addition, the above positive active material may be spherical or have a shape close to spherical, or may be polyhedral or irregular in shape.
[0111] Meanwhile, the above-mentioned positive electrode active material may include a buffer layer on the particle surface. The buffer layer may be described as a coating layer, a protective layer, etc., and may serve to lower the interfacial resistance between the positive electrode active material and the solid electrolyte particles. As an example, the buffer layer may include a lithium metal oxide, wherein the metal may be, for instance, Al, B, Ca, Ce, Cr, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ta, V, W, Zr, or a combination thereof. The lithium metal oxide is excellent at lowering the interfacial resistance between the positive electrode active material and the solid electrolyte particles while improving the performance of the positive electrode active material by facilitating the movement of lithium ions and electron conduction.
[0112] The above positive active material may be included in an amount of 55% to 99% by weight based on 100% by weight of the above positive active material layer, for example, 65% to 95% by weight, or 75% to 95% by weight.
[0113] The above-mentioned positive electrode active material layer may include a solid electrolyte, for example, a sulfide-based solid electrolyte. In this case, the same description of the solid electrolyte in the aforementioned solid electrolyte layer may be applied to the solid electrolyte included in the above-mentioned positive electrode active material layer.
[0114] Based on 100 weight% of the above positive active material layer, the solid electrolyte may be included in an amount of 0.1 weight% to 35 weight%, for example, 1 weight% to 35 weight%, 5 weight% to 30 weight%, 8 weight% to 25 weight%, or 10 weight% to 20 weight%.
[0115] In addition, based on the total weight of the positive active material and the solid electrolyte in the positive active material layer, 65% to 99% by weight of the positive active material and 1% to 35% by weight of the solid electrolyte may be included, for example, 80% to 90% by weight of the positive active material and 10% to 20% by weight of the solid electrolyte may be included. When the solid electrolyte is included in the positive electrode in such a content, the efficiency and lifespan characteristics of the all-solid-state battery can be improved without reducing the capacity.
[0116] The above binder serves to adhere the positive active material particles well to each other and also to adhere the positive active material well to the current collector. Representative examples include polyvinyl alcohol, carboxymethylcellulose, hydroxypropylcellulose, diacetylcellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto.
[0117] The content of the binder in the above positive active material layer may be 0.1% to 5% by weight based on 100% by weight of the positive active material layer.
[0118] The above positive active material layer may further include a conductive material. The conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanofiber, carbon nanotube, etc.; metal-based materials in the form of metal powder or metal fibers containing copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or conductive materials comprising a mixture thereof.
[0119] The content of the conductive material in the above positive active material layer may be 0% to 3% by weight, 0.01% to 2% by weight, or 0.1% to 1% by weight, based on 100% by weight of the positive active material layer.
[0120] Aluminum foil may be used as the anode current collector, but is not limited thereto.
[0121] cathode
[0122] A negative electrode for an all-solid-state secondary battery according to one embodiment comprises a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector. The negative electrode active material layer comprises a negative electrode active material and may further comprise a binder and / or a conductive material. Alternatively, the negative electrode active material layer may further comprise the aforementioned solid electrolyte.
[0123] The above-mentioned negative electrode active material includes a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide.
[0124] A material capable of reversibly intercalating / deintercalating the lithium ions may include a carbon-based negative electrode active material, for example, crystalline carbon, amorphous carbon, or a combination thereof. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite, and examples of the amorphous carbon include soft carbon or hard carbon, mesophase pitch carbide, calcined coke, etc.
[0125] As the above lithium metal alloy, an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, Sn, or a combination thereof may be used.
[0126] As a material capable of doping and undoping the above lithium, a Si-based negative electrode active material or a Sn-based negative electrode active material may be used, and the Si-based negative electrode active material may include silicon, a silicon-carbon composite, or SiO₂. x(0 <x≤2), Si-Q 합금(상기 Q는 알칼리 금속, 알칼리 토금속, 13족 원소, 14족 원소, 15족 원소, 16족 원소, 전이금속, 희토류 원소 또는 이들의 조합에서 선택되는 원소이며, Si은 아님), 상기 Sn계 음극 활물질로는 Sn, SnO2, Sn-R 합금(상기 R은 알칼리 금속, 알칼리 토금속, 13족 원소, 14족 원소, 15족 원소, 16족 원소, 전이금속, 희토류 원소 또는 이들의 조합에서 선택되는 원소이며, Sn은 아님) 등을 들 수 있고, 또한 이들 중 적어도 하나와 SiO2를 혼합하여 사용할 수도 있다. 상기 원소 Q 및 R로는 Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, 또는 이들의 조합에서 선택되는 것을 사용할 수 있다.
[0127] For example, the negative electrode active material may include silicon-carbon composite particles. The average particle size (D) of the silicon-carbon composite particles 50 ) can be, for example, 0.5 μm to 20 μm. The average particle size (D 50 ) refers to the diameter of a particle whose cumulative volume in the particle size distribution is 50 volume%, as measured by a particle size analyzer. Based on 100 weight% of the silicon-carbon composite particles, silicon may be included in an amount of 10 weight% to 60 weight% and carbon may be included in an amount of 40 weight% to 90 weight%. The silicon-carbon composite particles may include, for example, a core containing silicon particles and a carbon coating layer located on the surface of the core. The average particle diameter (D) of the silicon particles in the core 50) may be 10 nm to 1 µm, or 10 nm to 200 nm. The silicon particles may exist as silicon alone, in the form of a silicon alloy, or in an oxidized form. The oxidized form of silicon is SiO x (0 <x≤2)로 표시될 수 있다. 또한, 상기 탄소 코팅층의 두께는 약 5 ㎚ 내지 100 ㎚일 수 있다.
[0128] For example, the silicon-carbon composite particles may comprise a core containing silicon particles and crystalline carbon, and a carbon coating layer located on the surface of the core containing amorphous carbon. For example, in the silicon-carbon composite particles, the amorphous carbon may not be present in the core but only in the carbon coating layer. The crystalline carbon may be artificial graphite, natural graphite, or a combination thereof, and the amorphous carbon may be formed from coal-based pitch, mesophase pitch, petroleum-based pitch, coal-based oil, petroleum-based heavy oil, or a polymer resin (phenol resin, furan resin, polyimide resin, etc.). In this case, based on 100 weight% of the silicon-carbon composite particles, the content of the crystalline carbon may be 10 weight% to 70 weight%, and the content of the amorphous carbon may be 20 weight% to 40 weight%.
[0129] The core of the silicon-carbon composite particle may include a void in the central portion. The radius of the void may be 30% to 50% of the radius of the silicon-carbon composite particle.
[0130] The aforementioned silicon-carbon composite particles effectively suppress problems such as volume expansion, structural collapse, or particle fragmentation due to charging and discharging, thereby preventing the interruption of conductive paths, enabling high capacity and high efficiency, and making them advantageous for use under high voltage or high-speed charging conditions.
[0131] The above Si-based negative electrode active material or Sn-based negative electrode active material may be used in combination with a carbon-based negative electrode active material. When the Si-based negative electrode active material or Sn-based negative electrode active material and the carbon-based negative electrode active material are mixed and used, the mixing ratio may be 1:99 to 90:10 by weight.
[0132] The content of the negative electrode active material in the above negative electrode active material layer may be 95% to 99% by weight based on the total weight of the negative electrode active material layer.
[0133] In one embodiment, the negative active material layer further comprises a binder and optionally further comprises a conductive material. The content of the binder in the negative active material layer may be 1% to 5% by weight based on the total weight of the negative active material layer. Additionally, when further comprising a conductive material, the negative active material layer may comprise 90% to 98% by weight of the negative active material, 1% to 5% by weight of the binder, and 1% to 5% by weight of the conductive material.
[0134] The above binder serves to effectively bond the negative electrode active material particles to each other and also to effectively bond the negative electrode active material to the current collector. As the binder, a non-aqueous binder, an aqueous binder, a dry binder, or a combination thereof may be used.
[0135] Examples of the above-mentioned non-aqueous binders include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide imide, polyimide, or combinations thereof.
[0136] The above-mentioned water-based binder may be selected from styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic rubber, butyl rubber, fluororubber, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, poly(meth)acrylonitrile, ethylenepropylenediene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and combinations thereof.
[0137] When a water-based binder is used as the above-mentioned cathode binder, a cellulose-based compound capable of imparting viscosity may be further included. As this cellulose-based compound, one or more types such as carboxymethyl cellulose, hydroxypropylmethyl cellulose, methyl cellulose, or alkali metal salts thereof may be mixed and used. Na, K, or Li may be used as the alkali metal.
[0138] The above conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples of the above conductive material include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanofiber, carbon nanotube; metal-based materials in the form of metal powder or metal fibers including copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or conductive materials including mixtures thereof.
[0139] As the above-mentioned cathode current collector, a material selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, or a combination thereof may be used.
[0140] Precipitation type cathode
[0141] As another example, the negative electrode for an all-solid-state secondary battery may be a precipitation type negative electrode. The precipitation type negative electrode may refer to a negative electrode that does not contain a negative electrode active material during battery assembly, but where lithium metal, etc., is precipitated or electrodeposited on the negative electrode during battery charging, and which acts as the negative electrode active material.
[0142] FIG. 2 is a schematic cross-sectional view of an all-solid-state secondary battery including a precipitation type negative electrode. Referring to FIG. 2, the precipitation type negative electrode (400') may include a negative electrode current collector (401) and a negative electrode coating layer (405) located on the negative electrode current collector. An all-solid-state secondary battery having such a precipitation type negative electrode (400') starts initial charging in a state where no negative electrode active material is present. Subsequently, during charging, a high-density lithium metal is precipitated or electrodeposited between the negative electrode current collector (401) and the negative electrode coating layer (405), or on the negative electrode coating layer (405), to form a lithium metal layer (404), which can serve as a negative electrode active material. Accordingly, in a solid-state secondary battery that has undergone one or more charges, the precipitation type negative electrode (400') may include, for example, a negative electrode current collector (401), a lithium metal layer (404) located on the negative electrode current collector, and a negative electrode coating layer (405) located on the lithium metal layer. The lithium metal layer (404) refers to a layer in which lithium metal, etc. is precipitated during the charging process of the battery, and may be referred to as a metal layer, a lithium layer, a lithium electrodeposition layer, or a negative electrode active material layer.
[0143] The above-mentioned cathode coating layer (405) may be a lithium electrodeposition inducing layer or a cathode catalyst layer, and may include a lithium-friendly metal, a carbon material, or a combination thereof.
[0144] The above-mentioned lithium-friendly metal may include, for example, gold, platinum, palladium, silicon, silver, aluminum, bismuth, tin, zinc, or a combination thereof, and may be composed of one of these or may be composed of several types of alloys. When the metal exists in the form of particles, its average particle size (D50 ) can be about 4 μm or less, and for example, 10 nm to 4 μm.
[0145] The carbon material may be, for example, crystalline carbon, amorphous carbon, or a combination thereof. The crystalline carbon may be, for example, natural graphite, artificial graphite, mesophase carbon micro beads, or a combination thereof. The amorphous carbon may be, for example, carbon black, activated carbon, acetylene black, Denka black, Ketjen black, or a combination thereof.
[0146] When the above-mentioned cathode coating layer (405) includes both the metal and the carbon material, the mixing ratio of the metal and the carbon material may be, for example, a weight ratio of 1:10 to 2:1. In this case, the precipitation of lithium metal can be effectively promoted and the characteristics of the all-solid-state secondary battery can be improved. The cathode coating layer (405) may, for example, include a carbon material supported with a catalyst metal, or may include a mixture of metal particles and carbon material particles.
[0147] The above cathode coating layer (405) may, for example, include the lithium-friendly metal and amorphous carbon, in which case the precipitation of lithium metal can be effectively promoted. As a specific example, the cathode coating layer (405) may include a composite in which a lithium-friendly metal is supported on amorphous carbon.
[0148] The above cathode coating layer (405) may further include a binder, and the binder may be, for example, a conductive binder. In addition, the above cathode coating layer (405) may further include general additives such as fillers, dispersants, ion conductive agents, etc.
[0149] The thickness of the above cathode coating layer (405) may be, for example, 100 nm to 20 μm, or 500 nm to 10 μm, or 1 μm to 5 μm.
[0150] The above-mentioned precipitation type cathode (400') may, for example, further include a thin film on the surface of the cathode current collector, that is, between the cathode current collector and the cathode coating layer. The thin film may include an element capable of forming an alloy with lithium. The element capable of forming an alloy with lithium may be, for example, gold, silver, zinc, tin, indium, silicon, aluminum, bismuth, etc., and may be composed of one of these or composed of several types of alloys. The thin film can further flatten the precipitation shape of the lithium metal layer (404) and further improve the characteristics of the all-solid-state secondary battery. The thin film may be formed by, for example, a vacuum deposition method, a sputtering method, a plating method, etc. The thickness of the thin film may be, for example, 1 nm to 500 nm.
[0151] The lithium metal layer (404) may include lithium metal or a lithium alloy. The lithium alloy may be, for example, a Li-Al alloy, a Li-Sn alloy, a Li-In alloy, a Li-Ag alloy, a Li-Au alloy, a Li-Zn alloy, a Li-Ge alloy, or a Li-Si alloy.
[0152] The thickness of the lithium metal layer (404) may be 1 μm to 500 μm, 1 μm to 200 μm, 1 μm to 100 μm, or 1 μm to 50 μm. Within the above range, it can sufficiently perform the role of a lithium storage tank and prevent performance degradation due to an increase in battery volume.
[0153] When such a precipitation type cathode is applied, the cathode coating layer (405) can protect the lithium metal layer (404) and suppress the precipitation growth of lithium dendrites. Accordingly, short circuits and capacity degradation of the all-solid-state battery are suppressed, and lifespan characteristics can be improved.
[0154] The shape of the above-described all-solid-state secondary battery is not particularly limited and may be, for example, coin-type, button-type, sheet-type, stacked-type, cylindrical-type, flat-type, etc. Furthermore, the above-described all-solid-state secondary battery can be applied to large batteries used in electric vehicles, etc. For example, the above-described all-solid-state secondary battery can be used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). In addition, it can be used in fields requiring a large amount of power storage, for example, in electric bicycles or power tools. Furthermore, the above-described all-solid-state secondary battery can be used in various fields such as portable electronic devices.
[0155] Examples and comparative examples of the present invention are described below. The following examples are merely illustrative of the present invention, and the present invention is not limited to the following examples.
[0156] Example 1
[0157] 1. Preparation of Solid Electrolyte Layer
[0158] In a binder solution in which an acrylic binder (SX-A334, Zeon) is dissolved in an isobutyl isobutylate (IBIB) solvent, a solid electrolyte Li6PS5Cl (D 50 A slurry for forming a solid electrolyte layer was prepared by adding a dispersant (= 3㎛) and an HNBR dispersant and stirring with a Thinky Mixer.
[0159] At this time, the slurry for forming the solid electrolyte layer was adjusted to contain 98.3 wt% of sulfide-based solid electrolyte particles, 1.3 wt% of binder, and 0.4 wt% of dispersant.
[0160] A solid electrolyte layer was prepared by applying the above-mentioned slurry for forming a solid electrolyte layer onto a release PET film using a bar coater, then heating to 100°C at a heating rate of 10°C / min under a vacuum atmosphere, and maintaining at 100°C for 2 hours for drying.
[0161] 2. Manufacture of the anode
[0162] LiNi 0.8 Co 0.15 Mn 0.05 O2 positive electrode active material 85 wt%, solid electrolyte Li6PS5Cl(D 50 A slurry for forming an anode active material layer was prepared by mixing 13.5 wt% of (= 3㎛), 1.0 wt% of polyvinylidene fluoride binder, and 0.5 wt% of carbon nanotube conductive material. The prepared slurry for forming an anode active material layer was coated onto an aluminum foil using a bar coater, and an anode was manufactured by drying and rolling.
[0163] 3. Preparation of the cathode
[0164] Primary particle size (D 50 Carbon black with a diameter of approximately 30 nm and an average particle size (D 50 An Ag / C composite was prepared by mixing silver (Ag) with a thickness of approximately 60 nm in a weight ratio of 3:1, and 0.25 g of the composite was added to 2 g of an NMP solution containing 7 wt% of a polyvinylidene fluoride binder and mixed to prepare a composition for forming a cathode coating layer. The composition for forming a cathode coating layer was applied to a nickel foil current collector using a bar coater and vacuum dried to prepare a precipitation type cathode with a cathode coating layer formed on the current collector.
[0165] 4. Manufacturing of all-solid-state secondary batteries
[0166] The prepared anode, cathode, and solid electrolyte layer were cut, and a bicell-type cell structure was manufactured by stacking them in the order of cathode / solid electrolyte layer / anode / solid electrolyte layer / cathode. Then, the structure was placed in an aluminum pouch laminate film and subjected to a warm isostatic press (WIP) at 80°C and 500 MPa for 30 minutes to manufacture a final all-solid-state secondary battery. At this time, the thickness of the pressurized anode layer was approximately 80 μm, the thickness of the cathode layer was approximately 7 μm, and the thickness of the solid electrolyte layer was 60 μm.
[0167] Example 2
[0168] A solid electrolyte layer and an all-solid-state secondary battery were manufactured in substantially the same manner as in Example 1, except that drying was performed at 120°C for 2 hours under a vacuum atmosphere when manufacturing the solid electrolyte layer.
[0169] Example 3
[0170] A solid electrolyte layer and an all-solid-state secondary battery were manufactured in substantially the same manner as in Example 1, except that drying was performed at 140°C for 2 hours under a vacuum atmosphere when manufacturing the solid electrolyte layer.
[0171] Comparative Example 1
[0172] A solid electrolyte layer and an all-solid-state secondary battery were manufactured in substantially the same manner as in Example 1, except that drying was performed at 80°C for 2 hours under a vacuum atmosphere when manufacturing the solid electrolyte layer.
[0173] Comparative Example 2
[0174] A solid electrolyte layer and an all-solid-state secondary battery were manufactured in substantially the same manner as in Example 1, except that drying was performed at 160°C for 2 hours under a vacuum atmosphere when manufacturing the solid electrolyte layer.
[0175] Comparative Example 3
[0176] A solid electrolyte layer and an all-solid-state secondary battery were manufactured in substantially the same manner as in Example 1, except that when manufacturing the solid electrolyte layer, the composition of the slurry for forming the solid electrolyte layer was changed to 99.1 wt% solid electrolyte and 0.9 wt% binder, and drying was performed at 120°C for 2 hours under a vacuum atmosphere.
[0177] Comparative Example 4
[0178] A solid electrolyte layer and an all-solid-state secondary battery were manufactured in substantially the same manner as in Example 1, except that when manufacturing the solid electrolyte layer, the composition of the slurry for forming the solid electrolyte layer was changed to 97 wt% solid electrolyte and 2.5 wt% binder, and drying was performed at 120°C for 2 hours under a vacuum atmosphere.
[0179] Evaluation Example 1: Porosity Evaluation
[0180] Cross-sections of the solid electrolyte layer obtained by disassembling the all-solid-state secondary batteries prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were photographed using a scanning electron microscope (SEM). Among these, representative SEM images for Examples 1 to 3 and Comparative Examples 1 to 4 are shown in FIGS. 4 to 10, respectively.
[0181] For each SEM image, after performing image processing using the Image J program, solid electrolyte particles were isolated from the solid electrolyte layer, and the portion remaining after excluding the area occupied by the solid electrolyte particles from the total area was considered as pores, with a value of 2000 µm 2 Based on the cross-section, the area occupied by the voids was measured and is shown as the void ratio (%) based on area in Table 1 below.
[0182] Evaluation Example 2: Hardness Evaluation
[0183] For the solid electrolyte layer obtained by disassembling the all-solid-state secondary batteries prepared in Examples 1 to 3 and Comparative Examples 1 to 4, Knoop hardness was measured using a Knoop-type microhardness tester according to ASTM E384-17 standards, and the results are shown in Table 1 below. At this time, the Knoop hardness was measured under conditions where a test load of 25 gf was applied for 15 seconds.
[0184] Porosity based on area [%] Hardness [HK] Example 1: 478.74 Example 2: 671.44 Example 3: 863.59 Comparative Example 1: 280.10 Comparative Example 2: 1051.09 Comparative Example 3: 679.10 Comparative Example 4: 655.34
[0185] Referring to Table 1 above, it can be seen that in the case of Examples 1 to 3, the area-based porosity is 4% to 8% and the hardness is HK 63 to HK 79.
[0186] On the other hand, in the case of Comparative Examples 1 and 2, it can be seen that the area-based porosity does not meet 4% to 8%, and the hardness also does not meet HK 63 to HK 79.
[0187] In the case of Comparative Examples 3 and 4, the area-based porosity satisfies 4% to 8%, but it can be confirmed that the hardness exceeds HK 63 to HK 79.
[0188] Evaluation Example 3: Evaluation of Initial Charge / Discharge Characteristics
[0189] For the all-solid-state secondary batteries prepared in Examples 1 to 3 and Comparative Examples 1 to 4, an initial charge and discharge process was performed at 45°C with a constant current of 0.33C to an upper limit voltage of 4.25V, and then with a constant voltage of 0.1C, followed by discharging at 0.33C to a cutoff voltage of 2.5V. After measuring the initial charge capacity and discharge capacity, the initial efficiency (%), which is the ratio of the latter to the former, was measured, and the results are shown in Table 2 below.
[0190] Initial Charge Capacity (mAh / g) Initial Discharge Capacity (mAh / g) Initial Efficiency (%) Example 1 235.95 201.7 085.49 Example 2 235.71 200.5 685.09 Example 3 236.63 202.3 085.49 Comparative Example 1 240.93 201.8 483.76 Comparative Example 2 239.71 199.7 283.32 Comparative Example 3 236.85 200.2 684.55 Comparative Example 4 242.86 202.6 783.45
[0191] Referring to Table 2 above, it can be seen that the initial efficiency of Examples 1 to 3 is superior compared to Comparative Examples 1 to 4.
[0192] Evaluation Example 4: Life Characteristics Evaluation
[0193] For the all-solid-state secondary batteries prepared in Examples 1 and 2 and Comparative Examples 1 to 4, charging at 45°C with a constant current of 0.33C to an upper limit voltage of 4.25V, charging with a constant voltage of 0.1C, and then discharging at 0.33C to a cutoff voltage of 2.5V was repeated 100 times.
[0194] Figure 11 shows the change in discharge capacity as the cycle progresses for the all-solid-state secondary batteries prepared in Examples 1 and 2 and Comparative Examples 1 to 4.
[0195] Referring to Fig. 11, it can be seen that in the case of Examples 1 and 2, there is no short circuit during 100 cycles, and the discharge capacity in 100 cycles is also high.
[0196] On the other hand, in the case of Comparative Example 1, it can be seen that the discharge capacity at 100 cycles is low.
[0197] In addition, in the case of Comparative Example 2, it can be confirmed that not only does a micro-short circuit occur repeatedly during 100 cycles, but the discharge capacity at 100 cycles is also very low.
[0198] In addition, in the case of Comparative Examples 3 and 4, it can be confirmed that micro-short circuits occurred repeatedly during 100 cycles.
[0199] Evaluation Example 5: Evaluation of crack presence
[0200] The occurrence of microcracks was observed using a scanning electron microscope (SEM) on the solid electrolyte layer obtained by disassembling the all-solid-state secondary batteries prepared in Examples 1 and 2, which underwent the life evaluation of Evaluation Example 4, and Comparative Examples 1 to 4, and the results are shown in Table 3 below.
[0201] Crack Occurrence Example 1 No crack Example 2 No crack Comparative Example 1 Crack Occurrence Comparative Example 2 Crack Occurrence Comparative Example 3 Crack Occurrence Comparative Example 4 Crack Occurrence
[0202] Referring to Table 3 above, it can be seen that in the case of Examples 1 and 2, no cracks occurred, whereas in the case of Comparative Examples 1 to 4, cracks occurred.
[0203] Evaluation Example 6: Evaluation of lithium dendrite formation
[0204] Regarding the solid electrolyte layer obtained by disassembling the all-solid-state secondary batteries prepared in Examples 1 and 2, in which the life evaluation of Evaluation Example 4 was conducted, and Comparative Examples 1 to 4, the occurrence of lithium dendrites on the surface in contact with the negative electrode was observed using scanning electron microscope (SEM) images. In the images, cases where lithium dendrites occurred were marked with '○', and cases where lithium dendrites did not occur were marked with '×', and the occurrence of lithium dendrites is shown in Table 4 below.
[0205] Occurrence of lithium dendrites Example 1 × Example 2 × Comparative Example 1 ○ Comparative Example 2 ○ Comparative Example 3 ○ Comparative Example 4 ○
[0206] Referring to Table 4 above, in the case of Examples 1 and 2, no lithium dendrites were generated, and it can be confirmed that the effect of suppressing lithium dendrite formation was achieved by optimizing the porosity and hardness of the solid electrolyte layer.
[0207] On the other hand, in the case of Comparative Example 1, lithium dendrites occurred, and it is determined that lithium dendrites occurred because the porosity of the solid electrolyte layer of Comparative Example 1 was too low and the hardness was too high, causing microcracks to form.
[0208] In addition, in the case of Comparative Example 2, the porosity of the solid electrolyte layer is too high and the hardness is too low, so it is determined that lithium dendrites grew easily.
[0209] In addition, in the case of Comparative Example 3, it is determined that lithium dendrites were generated because microcracks were formed due to the hardness being too high, and in the case of Comparative Example 4, it is determined that lithium dendrites grew easily because the hardness was too low.
[0210] Although preferred embodiments have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements by those skilled in the art using the basic concepts defined in the following claims are also included within the scope of the present invention.
[0211] [Explanation of the symbol]
[0212] 100: All-solid-state secondary battery 200: Cathode
[0213] 201: Positive current collector 203: Positive active material layer
[0214] 300: Solid electrolyte layer 400: Cathode
[0215] 401: Cathode current collector 403: Cathode active material layer
[0216] 400': Precipitation type cathode 404: Lithium metal layer
[0217] 405: Cathode coating layer 500: Elastic sheet
Claims
1. Contains sulfide-based solid electrolyte particles, and The porosity based on area is 4% to 8%, and A solid electrolyte layer with a hardness of HK 63 to HK 79.
2. In Paragraph 1, The above sulfide-based solid electrolyte particles are a solid electrolyte layer containing a azirodite-type sulfide.
3. In Paragraph 2, The above azirodite-type sulfide is a solid electrolyte layer represented by the following chemical formula 1: [Chemical Formula 1] (Li a M 1 b M 2 c (P) d M 3 e )(S f M 4 g )X h In the above chemical formula 1, 4≤a≤8, and M 1 is Mg, Cu, Ag, or a combination thereof, 0≤b<0.5, and M 2 is Na, K, or a combination thereof, 0≤c<0.5, and M 3 is Sn, Zn, Si, Sb, Ge, or a combination thereof, and 0 <d<4, 0≤e<1 이고, M 4 is O, SO n , or a combination thereof, 1.5≤n≤5, 3≤f≤12, 0≤g<2, and X is F, Cl, Br, I, or a combination thereof, and 0 <h≤2이다.
4. In Paragraph 1, Average particle size D of the above sulfide-based solid electrolyte particles 50 A solid electrolyte layer having a thickness of 0.1 μm to 5.0 μm.
5. In Paragraph 1, A solid electrolyte layer comprising the above sulfide-based solid electrolyte particles in an amount of 97.6% to 99% by weight based on 100% by weight of the solid electrolyte layer.
6. In Paragraph 1, The above solid electrolyte layer comprises sulfide-based solid electrolyte particles and a binder, and A solid electrolyte layer comprising the above binder in an amount of 1.0% to 2.4% by weight based on 100% by weight of the solid electrolyte layer.
7. In Paragraph 1, The above solid electrolyte layer is a solid electrolyte layer further comprising a dispersant.
8. In Paragraph 7, The above-mentioned dispersant is a solid electrolyte layer comprising hydrogenated butadiene-based rubber.
9. In Paragraph 7, The above-mentioned dispersant is a solid electrolyte layer comprising rubber prepared by hydrogenating a copolymer of a diene monomer and a (meth)acrylonitrile monomer.
10. In Paragraph 7, The above dispersant is a solid electrolyte layer containing hydrogenated nitrile butadiene rubber.
11. In Paragraph 7, A solid electrolyte layer comprising 0.01% to 1.0% by weight of the above dispersant based on 100% by weight of the solid electrolyte layer.
12. In Paragraph 1, A solid electrolyte layer with a thickness of 10 μm to 1000 μm.
13. Prepare a slurry for forming a solid electrolyte layer by mixing sulfide-based solid electrolyte particles, a binder, and a solvent, and The above slurry for forming a solid electrolyte layer is applied onto a substrate, and The method comprises obtaining a solid electrolyte layer by drying at a temperature of 100 ℃ to 140 ℃, and A method for manufacturing a solid electrolyte layer comprising, based on 100 weight% of the total of the sulfide-based solid electrolyte particles and the binder, 1.0 weight% to 2.4 weight% of the binder in the slurry for forming the solid electrolyte layer.
14. In Paragraph 13, A method for manufacturing a solid electrolyte layer in which the above drying is performed under a vacuum atmosphere for 30 minutes to 10 hours.
15. In Paragraph 13, A method for manufacturing a solid electrolyte layer, further comprising applying pressure after the above drying.
16. In Paragraph 15, A method for manufacturing a solid electrolyte layer in which the above pressurization is performed at a pressure of 100 MPa to 1000 MPa.
17. In Paragraph 16, A method for manufacturing a solid electrolyte layer in which the above-mentioned pressurization is performed for 10 minutes to 5 hours.
18. Bipolar, cathode, and An all-solid-state secondary battery comprising a solid electrolyte layer according to any one of claims 1 to 12 located between the anode and the cathode.
19. In Paragraph 18, The above cathode is cathode current collector, and An all-solid-state secondary battery comprising a negative electrode coating layer located on the above-mentioned negative electrode current collector and comprising a lithium-friendly metal, a carbon material, or a combination thereof.
20. In Paragraph 19, An all-solid-state secondary battery further comprising a lithium metal layer formed by charging between the above-mentioned negative electrode current collector and the above-mentioned negative electrode coating layer.