Patterning using metal oxide mandrels

Metal oxide mandrels address the limitations of amorphous silicon or carbon mandrels by providing improved etch selectivity and mechanical strength, ensuring precise and reliable semiconductor device patterning with smaller features and pitches.

WO2026236038A1PCT designated stage Publication Date: 2026-11-12LAM RES CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/026109
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-04-30
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Current double patterning technologies face challenges such as spacer leaning, line bending, patterned spacer collapse, and poor etch selectivity due to the use of amorphous silicon or amorphous carbon mandrels, which result in line critical dimension loss and mechanical weakness, especially for small features and tight pitches.

Method used

Employing metal oxide mandrels, specifically organo-metal oxide resist materials, which are resistant to oxidation and provide improved etch selectivity and mechanical strength, eliminating the need for additional photolithography steps and reducing line wiggling by using high modulus and tensile stress spacer materials.

Benefits of technology

Enhances the precision and reliability of semiconductor device patterning by maintaining feature integrity and reducing defects, enabling smaller critical dimensions and pitches without the limitations of conventional mandrels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026026109_12112026_PF_FP_ABST
    Figure US2026026109_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Organo-metal oxide resist is deposited and developed to be used as mandrels in semiconductor device manufacturing. The organo-metal oxide resist may be optionally treated with reactive gas treatment to harden the mandrels and / or treated with an ion beam to reduce roughness in the mandrels. A conformal layer of spacer material is formed on horizontal surfaces and sidewalls of the mandrels. The spacer material is partially removed to expose the organo-metal oxide resist mandrels and retain the spacer material on the sidewalls of the mandrels. The mandrels are selectively removed while leaving the spacer material to form a plurality of spacers that can be used for patterning underlying layers.
Need to check novelty before this filing date? Find Prior Art

Description

PATTERNING USING METAL OXIDE MANDRELSINCORPORATION BY REFERENCE

[0001] A PCT Request Form is filed concurrently with this specification as part of the present application. Each application that the present application claims benefit of or priority to as identified in the concurrently filed PCT Request Form is incorporated by reference herein in their entireties and for all purposesFIELD

[0002] The present disclosure relates to semiconductor device manufacturing, and more particularly to metal oxide resist films in semiconductor device patterning.BACKGROUND

[0003] In integrated circuit (IC) fabrication, deposition and etching techniques are used for forming patterns of materials, such as for forming metal lines embedded in dielectric layers. Some patterning schemes involve the use of spacers that enable precise patterning and formation of small-scale features. Spacers are formed on a substrate, such that they are separated by defined distances (typically determined by previous patterning), and are used as masks for patterning of underlying layers. The materials of spacers and of surrounding layers are selected to have appropriate etch selectivity that would enable both formation of spacers, and patterning of underlying layers. After the patterning is completed, the spacers are removed by etching, and are not part of the final fabricated semiconductor device.

[0004] Spacers are used for patterning in a variety of applications, including formation of dynamic random-access memory (DRAM), patterning fins in fin field effect transistors (finFETs), and in back end of line (BEOL) processing.

[0005] Spacers can be formed on semiconductor substrates using patterning processes that involve mandrels - larger protruding features that serve as a scaffold for the spacers and that are subsequently selectively removed by etching methods that leave the spacers on the substrate.

[0006] The background description provided herein is for the purpose of generally presenting the context of the present technology. Work of the presently named inventors, to the extent it is described in this background section, as well as aspects of the description that may not otherwise qualify as prior art at the time of filing, are neither expressly nor impliedly admitted as prior art against the present technology.SUMMARY

[0007] A method of processing a semiconductor substrate is disclosed herein. The method includes providing a semiconductor substrate having a photopatterned organo-metal oxide resist layer over an etch stop layer, developing the photopattemed organo-metal oxide resist layer to form a resist mask of metal oxide mandrels, depositing a layer of a spacer material on horizontal surfaces and sidewalls of the metal oxide mandrels, removing a portion of the spacer material from at least the horizontal surfaces of the metal oxide mandrels, and removing the metal oxide mandrels to form a plurality of spacers used as a mask to etch at least the etch stop layer.

[0008] In some implementations, the method further includes depositing an organo-metal oxide EUV-sensitive resist material on the semiconductor substrate, where the organo-metal oxide EUV-sensitive resist material is configured to be exposed to EUV radiation to form the photopattemed organo-metal oxide resist layer. In some implementations, depositing the organo-metal oxide EUV-sensitive resist material includes vapor depositing the organo-metal oxide EUV-sensitive resist material. In some implementations, depositing the organo-metal oxide EUV-sensitive resist material includes vapor depositing two or more layers of organo-metal oxide EUV-sensitive resist layers, where each of the two or more layers comprises varying amounts of cross -linking. In some implementations, the photopattemed organo-metal oxide resist layer has a thickness equal to or greater than about 30 nm. In some implementations, the layer of spacer material is selected from a group consisting of tungsten, tungsten nitride, tungsten oxide, molybdenum, molybdenum oxide, molybdenum nitride, aluminum oxide, zirconium oxide, and hafnium oxide. In some implementations, the layer of spacer material is selected from a group consisting of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, silicon oxycarbonitride, silicon carbonitride, and titanium oxide. In some implementations, the etch stop layer comprises a silicon-containing material. In some implementations, developing the photopatterned organo-metal oxide resist layer comprises dry developing the photopattemed organo-metal oxide resist layer. In some implementations, the method further includes exposing the metal oxide mandrels to one or more halogen gases to harden the metal oxide mandrels. In some implementations, the method further includes exposing the metal oxide mandrels to a reactive ion beam including at least one reactive gas to reduce sidewall roughness in the metal oxide mandrels. In some implementations, the reactive ion beam is an angled reactive ion beam that includes hydrogen, a halogen-containing gas, a hydrocarbon gas, a nitrogen-containing gas, an oxygen-containing gas, or a combinationthereof. In some implementations, the method further includes etching the etch stop layer using the plurality of spacers as the mask. In some implementations, removing the portion of the spacer material includes etching the portion of the spacer material using a halogenbased chemistry. In some implementations, removing the metal oxide mandrels includes etching the metal oxide mandrels using a hydrogen-based chemistry.

[0009] Also provided herein is a method of processing a semiconductor substrate. The method includes dry depositing a first organo-metal oxide EUV-sensitive resist material over an etch stop layer on the semiconductor substrate, where the first organo-metal oxide EUV-sensitive resist material is configured to be exposed to EUV radiation to form a first photopattemed organo-metal oxide resist layer. The method further includes dry developing the first photopatterned organo-metal oxide resist layer to form first a resist mask of first metal oxide mandrels arranged in a first direction, conformally depositing a layer of first spacer material on horizontal surfaces and sidewalls of the first metal oxide mandrels, removing a portion of the first spacer material from at least the horizontal surfaces of the first metal oxide mandrels, removing the first metal oxide mandrels to form a plurality of first spacers, and etching the etch stop layer using the plurality of first spacers as the mask to form patterned etch stop features.

[0010] In some implementations, the method further includes removing the plurality of first spacers, depositing gapfill material in gaps between the patterned etch stop features, dry depositing a second organo-metal oxide EUV-sensitive resist material over the gapfill material and patterned etch stop features, where the second organo-metal oxide EUV-sensitive resist material is configured to be exposed to EUV radiation to form a second photopatterned organo-metal oxide resist layer, dry developing the second photopatterned organo-metal oxide resist layer to form a second resist mask of second metal oxide mandrels arranged in a second direction different from the first direction, conformally depositing a layer of second spacer material on horizontal surfaces and sidewalls of the second metal oxide mandrels, removing a portion of the second spacer material from at least the horizontal surfaces of the second metal oxide mandrels, and removing the second metal oxide mandrels to form a plurality of second spacers used as a mask to etch an underlying layer. In some implementations, each of the first organo-metal oxide EUV-sensitive resist material and the second organo-metal oxide EUV-sensitive resist material has a thickness equal to or greater than about 30 nm. In some implementations, the method further includes exposing the first metal oxide mandrels to one or more halogen gases to harden the first metal oxide mandrels. In some implementations, the method further includes exposing the first metal oxidemandrels to a reactive ion beam comprising at least one reactive gas to reduce sidewall roughness in the first metal oxide mandrels. In some implementations, dry depositing a first organo-metal oxide EUV-sensitive resist material includes vapor depositing two or more layers of first organo-metal oxide EUV-sensitive resist layers, where each of the two or more layers comprises varying amounts of cross -linking.BRIEF DESCRIPTION OF DRAWINGS

[0011] Figures 1A-1I show cross-sectional schematic illustrations of various stages of an example multiple patterning scheme (e.g., self-aligned double patterning) using conventional techniques.

[0012] Figure 2 shows a cross-sectional schematic illustration of an example conventional mandrel that is affected by CD loss and sidewall oxidation.

[0013] Figure 3 presents a flow diagram of an example method of processing a semiconductor substrate according to some implementations.

[0014] Figures 4A-4P show cross-sectional schematic illustrations of various stages of an example multiple patterning scheme according to some implementations, using metal oxide mandrels in a patterning process.

[0015] Figures 5A-5C show schematic isometric views of a semiconductor substrate undergoing a multiple patterning process using conventional techniques.

[0016] Figure 6 depicts a schematic illustration of an example plasma apparatus for implementing certain implementations and operations such as dry development and / or etch.

[0017] Figure 7 depicts a schematic illustration of an example apparatus for implementing certain implementations and operations such as bake.

[0018] Figure 8 depicts a schematic illustration of an example apparatus for implementing certain implementations and operations such as thermal dry development, thermal etch, and / or thermal treatment.

[0019] Figure 9 depicts a schematic illustration of an example plasma apparatus for implementing certain implementations and operations such as deposition, etch, dry development, and / or clean.

[0020] Figure 10 depicts a schematic illustration of an example apparatus for implementing certain implementations and operations such as dry deposition.

[0021] Figure 11 depicts a schematic illustration of an example multi- station processing tool suitable for implementation of various operations in accordance with some implementations.

[0022] Figure 12 depicts a schematic illustration of an example processing system including multiple substrate processing tools and storage buffer systems in accordance with some implementations.DETAILED DESCRIPTION

[0023] In the present disclosure, the terms “semiconductor wafer,” “wafer,” “substrate,” “wafer substrate,” and “partially fabricated integrated circuit” are used interchangeably. One of ordinary skill in the art would understand that the term “partially fabricated integrated circuit” can refer to a silicon wafer during any of many stages of integrated circuit fabrication. A wafer or substrate used in the semiconductor device industry typically has a diameter of 200 mm, or 300 mm, or 450 mm. The following detailed description assumes the present disclosure is implemented on a wafer. However, the present disclosure is not so limited. The work piece may be of various shapes, sizes, and materials. In addition to semiconductor wafers, other work pieces that may take advantage of the present disclosure include various articles such as printed circuit boards and the like.

[0024] As used herein, the term “about” means + / -10% of any recited value, unless otherwise specified. As used herein, this term modifies any recited value, range of values, or endpoints of one or more ranges.

[0025] As used herein, “etchant” is meant any compound used to remove a material such as a layer, byproduct or contaminant from a surface.

[0026] In some embodiments, selective etch chemistries are used to remove certain materials or features on a substrate without removing other materials or features. As used herein, the etch chemistry “removes” a material or feature when at least 90% (such as 100%) of the material or feature is removed (referring to thickness in vertical direction). The term “without removing”, as used herein means that at least 50% of material or feature (such as at least 80%) remains after the etch, where % refers to thickness in a vertical direction.

[0027] In some embodiments provided methods are used to remove materials from horizontal surfaces without removing materials residing at sidewalls of protruding features. It is understood that horizontal surfaces, as used herein, include surfaces with local deviations from horizontal plane, such as convex caps on top of protruding features.

[0028] As used herein, “photop attemed organo-metal oxide resist” is meant a thin film which may have an organo-metal oxide layer disposed on a substrate layer to be etched. The photopattemed organo-metal oxide resist may be provided after exposure in a scanner, such as extreme ultraviolet (EUV) exposure in an EUV scanner. In some implementations, the photopattemed organo-metal oxide resist may be provided after exposure in a scannerand after a post-exposure bake (PEB) treatment. The photopatterned organo-metal oxide resist includes non-exposed regions and exposed regions, such as non-EUV exposed regions and EUV-exposed regions. In some implementations, the non-exposed regions may be removed in a dry development process by exposure to a dry development chemistry. In some implementations, the photopatterned organo-metal oxide resist may be an organo-metal oxide EUV- sensitive resist.

[0029] Reference is made herein in detail to specific embodiments of the disclosure. Examples of the specific embodiments are illustrated in the accompanying drawings. While the disclosure will be described in conjunction with these specific embodiments, it will be understood that it is not intended to limit the disclosure to such specific embodiments. On the contrary, it is intended to cover alternatives, modifications, and equivalents as may be included within the spirit and scope of the disclosure. In the following description, numerous specific details are set forth in order to provide a thorough understanding of the present disclosure. The present disclosure may be practiced without some or all of these specific details. In other instances, well known process operations have not been described in detail so as to not unnecessarily obscure the present disclosure.Introduction

[0030] Advancements in technology have increased the demand for shrinking device features and smaller pitches in semiconductor devices. Various patterning techniques and methods have been employed to achieve smaller device features and smaller pitches but often reach certain limits. For example, high-resolution photolithography may be used to print small features to obtain small critical dimensions (CDs), but high-resolution photolithography may not be able to print features beyond a certain limit (e.g., 40 nm or less) and so the pitch may not be more than the limit.

[0031] Generally speaking, the resolution achieved using photolithography is dependent on wavelength. Photoresist masks have optical properties dependent on wavelength, with longer wavelength photoresist masks exposed to longer wavelength light having larger theoretical CDs and shorter wavelength masks exposed to shorter wavelength light having smaller theoretical CDs. However, the use of shorter wavelength photoresist masks may present additional challenges over longer wavelength photoresist masks. For example, shorter wavelength photoresist masks may not have a selectivity as high as longer wavelength photoresist masks and may more easily deform under plasma etch conditions.Even if photolithography is optionally combined with a trimming step that produces small features, what is produced may not necessarily have small pitch.

[0032] Multiple patterning has been used to extend lithographic technology beyond its optical limits. Double patterning and quad patterning are example technologies used to extend lithographic technology beyond its optical limits and double patterning is now widely used in the industry for pitches less than about 80 nm. For example, if a pitch of about 100 nm from one or more lines is produced, double patterning may shrink the one or more lines, deposit spacers, and etch back the spacers so as to increase the number of lines and double the pitch to about 50 nm. This can be referred to as “pitch doubling,” where the increased number of lines can be used as a subsequent mask or hard mask.

[0033] Current double patterning technologies often use sidewall spacers with two masking steps to pattern trenches. Methods of double patterning, particularly line patterning, in both positive and negative double patterning processes, have involved the use of spacers and masks. Spacers can be deposited by atomic layer deposition (ALD) or plasma enhanced atomic layer deposition (PEALD) on a patterned core and may be used to create a smaller pitch pattern. As devices shrink and pitch decreases, issues such as spacer leaning, line bending, and patterned spacer collapse arise, which can degrade device performance and even lead to device failure.

[0034] Figures 1A-1I are schematic illustrations of substrates in an example multiple patterning scheme using conventional techniques. Figure 1A shows a substrate having a lithographically defined or patterned core 101 on a first layer 103, a second layer 105 underlying the first layer 103, and a third layer 107 underlying the second layer 105. In some implementations, the first layer 103 may also be referred to as a second core 103, and the second layer 105 may also be referred to as a target layer 105. One of ordinary skill in the art will appreciate that a multi-layer stack suitable for semiconductor processing as described herein may also include other layers, such as etch stop layers, cap layers, and other underlayers.

[0035] As shown in Figure 1A, the patterned core 101 may include an amorphous carbon or amorphous silicon material. The patterned core 101 may be deposited over the first layer 103 by any suitable deposition technique, such as plasma enhanced chemical vapor deposition (PECVD), and the deposition technique may involve generating a plasma in the deposition chamber from deposition gases such as a hydrocarbon precursor. For example,a hydrocarbon precursor may be defined by the formula CxHy, where x is an integer between 2 and 10, and y is an integer between 2 and 24.

[0036] The patterned core 101 may also be referred to as a “mandrel.” As discussed above, a mandrel is a patterned structure used as a template or scaffold for depositing spacers in a patterning process, where the mandrel is subsequently removed so that the spacers are left on the substrate. Mandrels are generally larger protruding features on a substrate.

[0037] Typically, mandrels in the patterned core 101 are made of materials such as amorphous carbon or amorphous silicon. In order to form the patterned core 101, a mandrel layer is blanket deposited over the substrate. To pattern the mandrel layer, a photoresist layer such as a polymer-based chemically amplified resist (CAR), is deposited on the mandrel layer using vapor-based techniques or liquid-based spin-on techniques. The photoresist layer is photopatterned by exposure to patterning radiation such as EUV radiation to form unexposed regions and exposed regions in the photoresist layer. The photopattemed photoresist layer may be developed using any suitable wet development or dry development technique that selectively removes the exposed regions (positive-tone) relative to the unexposed regions, or that selectively removes the unexposed regions (negative-tone) relative to the exposed regions, to form a resist mask. Using suitable etch chemistry, pattern transfer occurs to pattern the mandrel layer to form the patterned core 101, where the patterned core 101 has protruding features that serve as mandrels. The resist mask may be removed by a photoresist strip process.

[0038] The first layer 103, the second layer 105, or the third layer 107 may be the target layer ultimately to be patterned in the multiple patterning process. The target layer may be a semiconductor, dielectric, or other layer and may be made of silicon (Si), silicon oxide (SiCh), silicon nitride (SisN4), or titanium nitride (TiN), for example. In some embodiments, the target layer is referred to as a hardmask layer and includes a metal nitride, such as titanium nitride. The target layer may be deposited by ALD, PEALD, chemical vapor deposition (CVD), or other suitable deposition technique. In some implementations, the first layer 103 is an etch stop layer. The etch stop layer 103 may be a silicon-based material, such as SiCh, SiN, or any of SiC, SiOC, SiNO, SiCNO, and SiCN. In some implementations, the second layer 105 is a target layer or hardmask layer, which may be made of Si, SiCh, SiN, or TiN. In some implementations, the third layer 107 is a back-end-of-line (BEOL) layer that includes a plurality of metal lines embedded in a layer of dielectric material.

[0039] In Figure IB, a first conformal film 109 is deposited over the mandrels of the patterned core 101. The first conformal film 109 may be deposited by ALD or PEALD in some implementations. The first conformal film 109 may be an oxide, such as SiCh or TiCh, or may be a nitride, such as SiN. Other suitable spacer materials that can be used include SiC, SiOC, SiNO, SiCNO, and SiCN. The first conformal film 109 constitutes a layer of spacer material deposited over both the horizontal surfaces and sidewalls of the protruding features of the patterned core 101. As shown in Figure IB, the first conformal film 109 is deposited over the first layer 103 and over the patterned core 101, including the sidewalls of the patterned core 101. It is preferable to deposit the layer of spacer material conformally to form the first conformal film 109, where conformal films as used herein generally follow the contour of the substrate. The thickness of the conformal film is about the same (with a fluctuation of less than 50%) on all horizontal and vertical surfaces. In some implementations, the fluctuation of thickness in the deposited conformal film is less than 15%.

[0040] In Figure 1C, the first conformal film 109 may be directionally etched to form first spacers 119. Spacer material may be removed from the horizontal surfaces, without completely removing the spacer material at sidewalls of the protruding features (i.e., mandrels) of the patterned core 1010. This step may be performed using a spacer etch chemistry. The first conformal film 109 is partially removed so that spacer material is removed from the horizontal surfaces such that the top surfaces of the patterned core 101 and the first layer 103 are exposed, while the first conformal film 109 at the sidewalls of the patterned core 101 are not completely removed, thereby leaving the first spacers 119 intact. The first spacers 119 may be an oxide, such as SiCh or TiCh, or may be a nitride, such as SiN. Other suitable spacer materials that can be used include SiC, SiOC, SiNO, SiCNO, and SiCN. The pattern of the first spacers 119 is used to pattern subsequent layers. It will be understood that the term “spacer” as used herein means a mask material adjacent to a core material.

[0041] When the first spacers 119 are silicon-based, such as SiO2, SiN or any of SiC, SiOC, SiNO, SiCNO, and SiCN, a fluorine-based etch may be used. For example, a plasma fluorocarbon etch chemistry can be used to selectively etch the silicon-containing spacer. When the first spacers 119 include TiO2 it can be selectively etched using a chlorine-based chemistry. Chlorine-based etch chemistry includes exposing the substrate to a reactant containing Cl (typically plasma activated), such as plasma- activated Ch, BCh, etc.

[0042] In Figure ID, the patterned core 101 is selectively etched, leaving free-standing first spacers 119 on the substrate. This process selectively removes the patterned core 101 without fully removing the first spacers 119 that previously resided at sidewalls of the protruding features (i.e., mandrels) of the patterned core 101, thereby forming a plurality of free-standing first spacers 119. Selective removal or selecting etching as used herein is defined as etching one material selective to another. For example, in Figure ID, the patterned core 101 is selectively etched relative to the first spacers 119. It will be understood that in some implementations, if a first material is etched selective to a second material, the etch rate of the first material is faster than the etch rate of the second material such that for a given duration, more of the first material is etched than the second material.

[0043] The pattern of the first spacers 119 may have a desired pitch, where the desired pitch may be equal to or less than about 50 nm. In Figure IE, the first layer 103 is etched using the patterned first spacers 119 as a mask, thereby transferring the pattern to the first layer 103 to form patterned first layer 113. The patterned first layer 113 may be etched using a chemistry suitable for etching the first layer 103 but not the patterned first spacers 119. In some implementations, the patterned first layer 113 may be an amorphous carbon layer, amorphous silicon layer, or a photoresist, such as poly(methyl methacrylate) or poly(methyl glutarimide) (PMGI) or phenol formaldehyde resin.

[0044] In Figure IF, the first spacers 119 are selectively removed to leave patterned first layer 113. In one example, the first spacers 119 may be removed using a fluorocarbon-based plasma. The patterned first layer 113 may provide a mask with a smaller CD for forming features with a smaller CD. However, the patterned first layer 113 may alternatively provide a second core material for subsequent patterning.

[0045] In Figure 1G, a second conformal film 120 may be deposited over the patterned first layer 113 (e.g., second core material). The second conformal film 120 may be a dielectric material deposited by ALD or PEALD. For example, the second conformal film 120 may be silicon oxide. In some implementations, the second conformal film 120 may have the same or similar composition to that of the first conformal film 109.

[0046] In Figure 1H, the second conformal film 120 is directionally etched to form second spacers 121 flanking the patterned first layer 113. Dielectric material of the second conformal film 120 may be removed from the horizontal surfaces, without completely removing the dielectric material at sidewalls of the protruding features of the patterned firstlayer 113. The second conformal film 120 is partially removed so that dielectric material is removed from the horizontal surfaces such that the top surfaces of the patterned first layer 113 and the second layer 105 are exposed, while the second conformal film 120 at the sidewalls of the patterned first layer 113 are not completely removed, thereby leaving the second spacers 121 intact.

[0047] In Figure II, the patterned first layer 113 is selectively removed to leave freestanding second spacers 121. Here, the patterned first layer 113 may be etched using the same or similar chemistry as etching the patterned core 101 in Figure ID. The second spacers 121 may provide a mask with an even smaller CD for forming features with an even smaller pitch.

[0048] The aforementioned process illustrated in Figures 1A-1I shows a multiple patterning process scheme such as self-aligned double patterning (SADP). Conventional multiple patterning processes use materials like amorphous carbon or amorphous silicon as mandrels or patterned cores for subsequent spacer deposition. However, typical mandrels or patterned cores suffer from a variety of drawbacks. First, typical mandrels or patterned cores require using photolithography steps to pattern the mandrels or patterned cores. This involves blanket deposition of a mandrel layer, deposition of a photoresist layer on the mandrel layer, exposure to photo-pattern the photoresist layer, development to form a resist mask over the mandrel layer, and pattern transfer etch to form the mandrels or patterned cores. Such photolithography steps to form the mandrels or patterned cores can be costly, time-consuming, and cumbersome. In addition, such photolithography steps to form the mandrels or patterned cores can result in line roughness due to stochastics of patterning radiation exposure, photoresist development, and pattern transfer etch to the mandrel layer. Second, typical mandrels or patterned cores use amorphous silicon or amorphous carbon material. These materials readily suffer line critical dimension (CD) loss due to sidewall oxidation during downstream processes. These materials also suffer from poor etch selectivity with spacer materials such as TiCF and hardmask materials such as SiCF. Furthermore, line wiggling is often observed for small line CDs, such as line CDs less than about 20 nm, as typical mandrels or patterned cores using amorphous silicon or amorphous carbon exhibit poor mechanical strength. For instance, typical mandrels or patterned cores using materials exhibiting low modulus (e.g., 30-60 GPa) and high compressive stress (e.g., 0.6 GPa or greater).

[0049] Figure 2 shows a cross-sectional schematic illustration of an example conventional mandrel that is affected by CD loss and sidewall oxidation. The mandrel may be made of a conventional material such as amorphous silicon or amorphous carbon. Downstream processes may result in oxidation on surfaces of the mandrel, which can result in CD loss. On the left-side of Figure 2, a photoresist mask 200 is provided over a mandrel 210. During photoresist stripping or photoresist ashing, the mandrel 210 may be exposed to plasma. The photoresist stripping / ashing process can result in oxidation (e.g., plasma oxidation) growth on sidewalls of the mandrel 210. Oxides 220 form and grow on the sidewalls of the mandrel 210. In the middle of Figure 2, the mandrel 210 is shown after photoresist stripping / ashing and after spacer deposition. Spacers (not shown) often involve deposition of oxide-based materials such as TiO2 or SiO2, where the deposition of spacer materials can lead to oxidation of the sidewalls and top surfaces of the mandrel 210. The oxides 220 grow even more along the sidewalls and top surfaces of the mandrel 210 after oxidation from spacer deposition to result in the formation of a conformal spacer layer 230. In the right-hand side of Figure 2, the mandrel 210 is shown after selective etching of the conformal spacer layer 230. Selective etching of the conformal spacer layer 230 can utilize etch chemistries that result in oxidation or involve exposure to oxidizing environments that lead to native oxide growth. Oxidation of the mandrel 210 causes line CD loss that can become a significant limitation in fine-pitch self-aligned double patterning processes. As shown in Figure 2, the width of the mandrel 210 at the top surface went from 37 nm to 34 nm, and the width of the mandrel 210 at the bottom surface went from 57 nm to 42 nm.

[0050] In the present disclosure, a metal oxide resist such as an organo-metal oxide resist is employed as a mandrel for patterning. The organo-metal oxide resist may be resistant to oxidation during downstream processes. The organo-metal oxide resist may be deposited and developed over target layer to form a resist mask, where the resist mask includes metal oxide features that serve as mandrels. Because the organo-metal oxide resist serves as the mandrel layer itself, no other photoresist mask is needed to pattern the mandrel layer, thereby simplifying processing. In some implementations, the organo-metal oxide resist includes two or more layers of organo-metal oxide resist materials having varying amounts of cross -linking. For example, the organo-metal oxide resist may be deposited as a bilayer with different compositions, which can increase the modulus and etch selectivity to prevent line wiggling. In some implementations, the organo-metal oxide resist is optionally treated with a reactive chemical treatment that can selectively remove organic groups in the organo-metal oxide resist and harden the organo-metal oxide resist and promote cross-linking. Insome implementations, the organo-metal oxide resist is exposed to an ion beam to reduce roughness in the mandrels. A conformal layer of spacer material is formed on horizontal surfaces and sidewalls of the organo-metal oxide resist mandrels. The spacer material may include materials with a high modulus, tensile stress, and good etch selectivity with respect to the organo-metal oxide resist mandrels. For example, the spacer material may include tungsten (W), tungsten nitride (WN), tungsten oxide (WO3), molybdenum (Mo), molybdenum oxide (M0O3 or M0O2), molybdenum nitride (MoN or M02N), titanium oxide (TiCh), aluminum oxide (AI2O3), zirconium oxide (ZrCh), or hafnium oxide (HfCh). After the conformal layer of spacer material is partially removed to form spacers on sidewalls of the organo-metal oxide resist mandrels, the mandrels are selectively removed to leave freestanding spacers that can be used as a mask for patterning underlying layers.

[0051] Figure 3 presents a flow diagram of an example method of processing a semiconductor substrate according to some implementations. The operations of a process flow 300 may be performed in different orders and / or with different, fewer, or additional operations. In some implementations, the operations of the process flow 300 may be implemented, at least in part, according to software stored in one or more non-transitory computer readable media. Aspects of the process flow 300 may be described in the Figures 4A-4G.

[0052] At block 302 of the process 300, an organo-metal oxide EUV-sensitive resist material may be deposited on a semiconductor substrate. The organo-metal oxide EUV-sensitive resist material is configured to be exposed to EUV radiation to form a photopattemed organo-metal oxide resist layer. Deposition of the metal-containing photoresist may be a dry deposition process such as a vapor deposition process or a wet process such as a spin-on deposition process. EUV lithography makes use of EUV-sensitive photoresists, which may be metal oxide-based resists produced by dry vapor-deposited techniques. In some cases, the EUV-sensitive resist material may be an organo-metal oxide EUV-sensitive resist material, where the EUV-sensitive resist material can include one or more ligands (e.g., EUV labile ligands) that can be removed, cleaved, or cross-linked by radiation (e.g., EUV radiation). Accordingly, the EUV-sensitive resist material itself can be altered by exposure to such radiation. In some implementations, the EUV-sensitive resist material includes an organometallic material or metal-oxide-containing material. The organo-metal oxide EUV-sensitive resist material comprises a metal that can have a high patterning radiation absorption (e.g., an EUV absorption cross-section that is equal to or greater than IxlO7cm2 / mol). In some implementations, the metal is selected from a groupconsisting of tin (Sn), bismuth (Bi), tellurium (Te), cesium (Cs), antimony (Sb), indium (In), molybdenum (Mo), hafnium (Hf), iodine (I), zirconium (Zr), iron (Fe), cobalt (Co), nickel, (Ni), copper (Cu), zinc (Zn), silver (Ag), platinum (Pt), germanium (Ge), and lead (Pb). For example, the metal includes tin. As such, the EUV-sensitive resist material may include organotin oxide in some implementations.

[0053] In some implementations, the organo-metal oxide EUV-sensitive resist material includes two or more layers of varying composition. In one example, the two or more layers may provide varying percentages of metal atoms bonded to organic ligands at different vertical positions along a thickness of the organo-metal oxide EUV-sensitive resist material. In another example, the two or more layers may provide varying amounts of cross-linking at different vertical positions along a thickness of the organo-metal oxide EUV-sensitive resist material. For instance, the organo-metal oxide EUV-sensitive resist material may include a bilayer, each layer having a desired level of cross -linking. A first layer (bottom layer) may be deposited as a “blended” resist film. The “blended” resist film refers to a resist deposited using a mixture of different precursors. The resist may be deposited as a homogeneously blended film or a vertically heterogeneous film. In some cases, the mixture of different precursors may include a first metal precursor with a first organometal and a second metal precursor with no metal-carbon bonds or a second organometal. With a blended resist film, the composition of the resist may be finely tuned through selection of appropriate precursors and / or adjustment of ratios of the precursors during delivery to a process chamber. By fine-tuning the composition of the resist, the resist may have a desired level of cross-linking and may have increased sensitivity to radiation for photopatterning. In some implementations, the “blended” resist film may have increased sensitivity to EUV radiation. The desired level of cross-linking in the “blended” resist film provides preexisting cross-linking in the resist so that the intensity of the exposure step and / or postexposure bake step can be reduced. This results in a lower shrinkage contrast between exposed and unexposed regions, which reduces stress-induced defects. The “blended” resist film can exhibit not only improved properties such as sensitivity, but also improved properties in resolution and line-edge roughness. In some implementations, the “blended” resist film deposits the resist using a vapor deposition process such as a chemical vapor deposition (CVD) process, where the substrate is exposed to at least one first metal precursor, at least one second metal precursor, and a reactant. The first metal precursor may have at least one metal-carbon bond. The second metal precursor may have no metal-carbon bonds or may have at least one metal-carbon bond that is weaker than the metal-carbon bondof the first metal precursor. Aspects of deposition of a “blended” resist film are described in further detail in International Application No. PCT / US2024 / 052528, filed October 23, 2024, entitled “BLENDED AND VERTICAL COMPOSITION GRADIENT EUV RESISTS,” which is incorporated herein by reference in its entirety and for all purposes. A second layer (top layer) may be deposited over the first layer. The second layer may be deposited with or without blending. The second layer may be deposited using a metal precursor and a reactant. The second layer deposits a resist material using a vapor deposition process such as a CVD process, where the substrate is exposed to a metal precursor and a reactant. For example, the metal precursor is an organo-metallic precursor having a formula of MlaRlbLlc, where: Ml is a metal having a high patterning radiation-absorption crosssection, R1 is an organic group that survives the reaction between the metal precursor and the reactant and is cleavable from Ml under exposure to patterning radiation, LI is a ligand, ion, or other moiety that reacts with the reactant, and a > 1, b > 1, and c > 1. Accordingly, in some implementations, the organo-metal oxide EUV-sensitive resist material may have multiple layers such that the lower layers may have higher amounts of pre-existing crosslinking relative to the upper layers. The organo-metal oxide EUV-sensitive resist material with multiple layers may increase modulus and etch selectivity to prevent line wiggling.

[0054] Though not shown in the process flow 300, an underlayer may be deposited on a substrate prior to deposition of the organo-metal oxide EUV-sensitive material at block 302. In some embodiments, the underlayer may be deposited over a hard mask such as an ashable hard mark (AHM). The underlayer is configured to increase adhesion between the subsequently-formed photoresist and the substrate. The underlayer is also configured to reduce radiation dose for effective patterning exposure of the photoresist. The underlayer may include a vapor-deposited film of an amorphous hydrogenated carbon. In some instances, the amorphous hydrogenated carbon is doped with a non-carbon heteroatom such as oxygen (O), silicon (Si), nitrogen (N), tungsten (W), boron (B), iodine (I), chlorine (Cl), or a combination thereof. The amorphous hydrogenated carbon film may have a density between about 0.7 g / cc and about 2.9 g / cc, such as between about 0.7 g / cc and about 1.4 g / cc. Reactive species may be generated in the underlayer that can diffuse into the organo-metal oxide EUV resist to form metal-oxygen bonds in the organo-metal oxide EUV resist. For example, an underlayer comprising an amorphous hydrogenated carbon film doped with iodine may improve generation of secondary electrons in the photoresist upon exposure to patterning radiation. The underlayer may have a thickness equal to or less than about 25 nm, such as a thickness between about 2 nm and about 20 nm. In some implementations,the underlayer may be deposited using a vapor deposition technique such as PECVD or ALD.

[0055] Though not shown in the process flow 300, an optional post-application bake (PAB) may be performed after deposition of the organo-metal oxide EUV-sensitive resist material prior to EUV exposure. The PAB treatment may involve a combination of thermal treatment, chemical exposure, and moisture to increase the EUV sensitivity of the organo-metal oxide EUV-sensitive resist material, which can reduce the EUV dose to develop a pattern.

[0056] Though not shown in the process flow 300, the organo-metal oxide EUV-sensitive resist material is exposed to EUV radiation. Exposure to EUV radiation forms a photo pattern in the EUV-sensitive resist material. In some embodiments, EUV exposure may occur at doses ranging from about 10 mJ / cm2to about 100 mJ / cm2. Generally speaking, EUV exposure causes a change in the chemical composition and cross-linking in the EUV-sensitive resist material, creating a contrast in etch selectivity that can be exploited for subsequent development. The organo-metal oxide EUV-sensitive resist material may be photo patterned by exposing a region to EUV light, typically under relatively high vacuum. Exposed areas of the EUV-sensitive resist material are created through EUV photo patterning that have altered physical or chemical properties relative to unexposed areas. The difference in properties between exposed and unexposed areas may be exploited in subsequent processing. After exposure, the organo-metal oxide EUV-sensitive resist material is patterned to form a photopatterned organo-metal oxide resist layer on the semiconductor substrate.

[0057] Though not shown in the process flow 300, the photopatterned organo-metal oxide resist layer is exposed to a post-exposure bake (PEB). The PEB treatment may further increase contrast in etch selectivity of the organo-metal oxide resist layer after photo patterning by EUV exposure. During PEB, the photopatterned organo-metal oxide resist layer is thermally treated in the presence of various chemical species to facilitate crosslinking in the EUV-exposed regions of the photopatterned organo-metal oxide resist layer. The PEB treatment temperature may be controlled to further increase etch contrast in the resist layer, where the PEB treatment temperature may be between about 100°C and about 300°C, such as between about 170°C and about 290°C. The bake ambient may be controlled to further increase etch contrast in the resist layer, where the bake ambient may control pressure as well as introduction of reactive gases such as air, H2O, H2O2, CO2, CO, O2, O3, CH4, CH3OH, N2, H2, NH3, N2O, NO, alcohol, acetyl acetone, formic acid, Ar, He, or theirmixtures. The PEB treatment can be designed to drive evaporation of organic fragments that are generated during EUV exposure, oxidize the metal hydride species into metal hydroxide, and facilitate cross-linking between neighboring -OH groups and form a crosslinked metal oxide network.

[0058] At block 304 of the process flow 300, the semiconductor substrate having the photopattemed organo-metal oxide resist layer over an etch stop layer is provided. The semiconductor substrate may be provided in a process chamber such as a development chamber. The semiconductor substrate may include several layers on which the photopattemed organo-metal oxide resist layer is disposed on, including the etch stop layer. In some implementations, the semiconductor substrate includes an etch stop layer, a target layer underlying the etch stop layer, and a BEOL layer underlying the target layer that can include a plurality of metal lines embedded into a layer of dielectric material. In some implementations, the semiconductor substrate includes an etch stop layer comprising amorphous silicon, a target layer comprising SiCh, and an ashable hardmask layer underlying the target layer. The semiconductor substrate may undergo multiple patterning processes.

[0059] At block 306 of the process flow 300, the photopattemed organo-metal oxide resist layer is developed to form a resist mask of metal oxide mandrels. In some embodiments, the exposed regions are removed (positive tone) relative to the unexposed regions. In some embodiments, the unexposed regions are removed (negative tone) relative to the exposed regions. Development may be performed using wet or dry processes. A wet development process exposes the resist layer to a solvent for selective removal of portions of the resist layer. A dry development process exposes the photopatterned organo-metal oxide resist layer to an etch gas for selective removal of unexposed or EUV-exposed regions of the resist layer. In some embodiments, the dry development can involve a thermal process, a plasma process, or a combination of a thermal process and a plasma process. In some embodiments, the etch gas can include a halogen-containing gas such as a hydrogen halide.

[0060] The metal oxide mandrels may include tin oxide mandrels. Tin oxide can be etched selectively to a wide variety of materials using hydrogen-based etches that convert tin oxide to volatile tin hydride products (e.g., tin tetrahydride). The term “tin hydride” as used herein includes a plurality of tin hydrides (compounds with tin-hydrogen bonding) and is not limited only to tin tetrahydride (SnH4)). Terms like “tin chloride” and “silicon fluoride” similarly may include multiple chlorides and fluorides. Tin tetrahydride, unlike hydrides of many other metals, has a low boiling point, and therefore can be easily removedfrom the process chambers by purging and / or evacuation thereby making hydrogen-based etch a particularly attractive process for selective tin oxide etching.

[0061] Tin oxide, as used herein, refers to materials that include tin (Sn) and oxygen (O), and may optionally include hydrogen. Tin oxide, as used herein, may further include small amounts of other elements, such as carbon, and nitrogen (e.g., SnOxNy), where the total amount of other elements is 10 atomic % or less (where hydrogen is not included in the calculation of the content). For example, tin oxide can contain about 0.5 - 5 atomic % carbon. The stoichiometry of tin oxide generally can vary. In some embodiments the atomic ratio of tin to oxygen is about 1:2 (SnCh). It is understood that small deviations from 1:2 tin to oxygen stoichiometry are possible in SnCb and are within the scope of SnCb structure. For example, O to Sn atomic ratio is between about 2.0 - 2.3 in some examples of SnCh. Tin oxides with O to Sn ratio of between about 1.5 - 2.5 are within the scope of SnCF material, as used herein. Tin oxide materials described herein are distinct from indium tin oxide materials, and other mixed metal oxides.

[0062] Metal oxide mandrels such as tin oxide mandrels may be formed over the etch stop layer after development. A distance between neighboring mandrels may be, for example, between about 10 nm and about 100 nm. The distance between the centers of the closest mandrels, which is also referred to as pitch, is, in some embodiments, between about 30 nm and about 130 nm. The height of a mandrel is typically between about 20 nm and about 200 nm. For example, the metal oxide mandrels may have a height equal to or greater than about 30 nm. The material of the mandrels is selected preferably to allow subsequent selective etching of the metal oxide mandrel material in the presence of exposed spacer material, and selective etching of the etch stop layer material in the presence of exposed spacer material.

[0063] Aspects of tin oxide mandrels are described in further detail in International Application No. PCT / US2019 / 015559, filed January 29, 2019, entitled “TIN OXIDE MANDRELS IN PATTERNING,” which is incorporated herein by reference in its entirety and for all purposes.

[0064] Though not shown in the process flow 300, the resist mask of metal oxide mandrels is exposed to a reactive chemical treatment. The reactive chemical treatment may use one or more halogen gases to selectively remove organic ligands in the metal-containing photoresist and further densifies the photoresist. Selective removal of organic ligands after development can further harden the resist mask. Selective removal of organic ligands after development can densify the metal oxide mandrels and increase cross-linking in the metaloxide mandrels. In some implementations, the one or more halogen gases chlorine (Ch). The reactive chemical treatment may also improve the etch resistance of the resist mask of metal oxide mandrels. In some embodiments, the reactive chemical treatment uses reactive Ch gas at an elevated temperature between about 120°C and about 180°C to harden the resist mask of metal oxide mandrels after development, where the reactive chemical treatment removes residual organic components and completes metal-oxygen-metal networking. The etch rate is reduced after hardening with the reactive chemical treatment.

[0065] Aspects of reactive chemical treatment are described in further detail in U.S. Provisional Patent Application No. 63 / 735,784, filed December 18, 2024, entitled “REACTIVE CHEMICAL TREATMENTS OF METAL-CONTAINING PHOTORESIST,” which is incorporated herein by reference in its entirety and for all purposes.

[0066] Though not shown in the process flow 300, the resist mask of the metal oxide mandrels may be exposed to a reactive ion beam to reduce roughness in the metal oxide mandrels. A reactive ion beam of a reactive gas such as oxygen may be utilized to smooth a resist mask after development. Suitable reactive ion beams include angled reactive ion beams, where the angled reactive ion beam may have an angle of incidence from about 5 degrees to about 90 degrees or from about 10 degrees to about 85 degrees. The ion energy of the ion beam may be from about 20 V to about 2000 V. In some embodiments, the reactive gas may be an oxygen-containing gas such as O2, ozone O3, CO, CO2, CH3OH, H2O vapor, COS, SO2, NO, N2O, NO2, a peroxide, hydrogen peroxide, an alcohol, a dihydroxy alcohol, a polyhydroxy alcohol, a fluorinated dihydroxy alcohol, a fluorinated polyhydroxy alcohol, a fluorinated glycol, formic acid, and other sources of hydroxyl moieties, as well as combinations thereof. In some embodiments, the reactive gas may be a hydrogen-containing gas such as H2, CH4, C2H2, C2H4, C3H6, C4H10, C6H12, CeHe, C?Hs, or a combination thereof. Application of the ion beam enables reduction of scum, nanobridges, contaminants, sidewall roughness, or a combination thereof, and patterned mask material loss is minimized. Application of the ion beam reduces line wiggling, where the line wiggling in the resist mask of the metal oxide mandrels may be less than about 1 nm. The reactive ion beam may trim line CD to a desired target and smoothen the resist mask line roughness by removing any sidewall protrusions, footing, scumming. In some cases, the line width roughness is reduced from about 3 nm to about 1 nm or less. By way of an example, the reactive ion beam is an O2 or H2 reactive ion beam.

[0067] Aspects of ion beam treatment to reduce roughness are described in further detail in U.S. Provisional Patent Application No. 63 / 662,970, filed June 21, 2024, entitled “REACTIVE ION BEAM ETCH TO REDUCE LINE-SPACE PATTERN LINE WIDTH ROUGHNESS AND PHOTORESIST LOSS,” which is incorporated herein by reference in its entirety and for all purposes.

[0068] The resist mask of the metal oxide mandrels may each have two or more layers of varying composition / cross-linking for improved modulus, reduced roughness, improved etch selectivity, and reduced line wiggling. In addition, the metal oxide mandrels may be treated with a reactive chemical treatment and / or reactive ion beam to increase its mechanical properties, increase its etch resistance, and reduce its line roughness. This may offer significant improvements over conventional mandrels made of amorphous silicon or amorphous carbon. The metal oxide mandrels of the present disclosure are resistant to sidewall oxidation during downstream processes and do not have line wiggling issues observed in conventional amorphous silicon or amorphous carbon mandrels. In some implementations, the metal oxide mandrels of the present disclosure have a much higher material modulus, such as a modulus between about 100 GPa and about 300 GPa and may have tensile stress rather than compressive stress. In some implementations, the steps of development, reactive chemical treatment for hardening, and reactive ion beam exposure to reduce roughness can be integrated on the same platform, where the aforementioned processes may be performed without a vacuum break in between chambers.

[0069] Additionally, the resist mask of the metal oxide mandrels of the present disclosure eliminates multiple processing steps of conventional mandrels that rely on a photoresist mask to pattern the conventional mandrels. The resist mask of the metal oxide mandrels are formed by deposition (e.g., dry deposition) and development (e.g., dry development) of an organo-metal oxide resist material, where the organo-metal oxide resist material is deposited and developed over the etch stop layer of the semiconductor substrate. In contrast, conventional mandrels require deposition of a mandrel layer followed by deposition of a photoresist layer, where the photoresist layer undergoes exposure and development to pattern the photoresist, and where the mandrel layer is patterned in a pattern transfer etch step using the photoresist. Thus, the resist mask of the metal oxide mandrels of the present disclosure simplifies processing.

[0070] At block 308 of the process flow 300, a layer of spacer material is deposited on horizontal surfaces and sidewalls of the metal oxide mandrels. The layer of spacer material may be deposited over the etch stop layer and over the metal oxide mandrels, including thesidewalls of the metal oxide mandrels. The layer of spacer material may be conformally deposited using any suitable method such as CVD, ALD, sputtering, etc. In some embodiments, the thickness of the spacer material is deposited conformally to a thickness between about 5 nm and about 30 nm, or between about 10 nm and about 20 nm. In some implementations, the spacer material may include TiCb. In some implementations, the spacer material may include a silicon-containing material such as SiCh, SisN4, SiC, SiOC, SiNO, SiCNO, and SiCN.

[0071] In some implementations, the spacer material may be selected to good etch selectivity relative to the metal oxide mandrels to prevent or minimize line wiggling. In some implementations, the spacer material may include W, WN, WO3, Mo, M0O2, M0O3, MoN, M02N, TiCh, AI2O3, ZrO2, or HfCb. As such, another metal or metal oxide film may be deposited conformally as a spacer layer on the metal oxide mandrels. Such spacer materials may have tensile stress, high material modulus, and high etch selectivity relative to the metal oxide mandrels. The tensile spacer material can reduce line width roughness and minimize self-aligned double patterning pitch walking. The spacer material may be deposited conformally by ALD.

[0072] At block 310 of the process flow 300, a portion of the layer of the spacer material is removed from at least the horizontal surfaces of the metal oxide mandrels. This is done without completely removing the spacer material at the sidewalls of the metal oxide mandrels. This step is performed using a spacer etch chemistry. The spacer material is removed from the horizontal surfaces such that the metal oxide mandrels and the etch stop layer are exposed, while the spacer material at the sidewalls is not completely removed. Preferably after this etch at least 50% , such as at least 80% or at least 90% of the initial height of the metal oxide mandrels at the sidewalls is preserved. The spacer etch chemistry is preferably selective to both the metal oxide mandrels and the etch stop layer material. In some implementations, the spacer etch chemistry is a fluorine-based etch chemistry such as a fluorocarbon etch chemistry. In some implementations, the spacer etch chemistry is a chlorine-based etch chemistry. The etch selectivity between the spacer material and the metal oxide mandrel is tunable by using different etch chemistries. For example, BCI3 / CI2-based chemistry can be used to obtain comparable etch rates on both metal oxide mandrels and spacer materials such as metal oxide spacer materials. Alternatively, a CF^CL / Ar- based chemistry can be used to etch an aluminum oxide spacer material but not the metal oxide mandrel such as a tin oxide mandrel.

[0073] At block 312 of the process flow 300, the metal oxide mandrels are removed to form a plurality of spacers used as a mask to etch at least the etch stop layer. After the spacer material is removed from horizontal surfaces, the metal oxide mandrels are exposed and removed without fully removing the spacer material that has previously resided at the sidewalls of the mandrels, thereby forming the plurality of spacers. The resulting structure produces a plurality of free-standing spacers that serve as a mask for patterning underlying layers such as the etch stop layer. Removal of the mandrels is performed by exposing the substrate to an etch chemistry that selective etches the mandrel material (mandrel pull chemistry). Thus, the ratio of the etch rate of the metal oxide mandrel material to the etch rate of the spacer material is greater than 1, and is more preferably greater than 1.5. Furthermore, the etch chemistry should, in some embodiments, selectively etch the metal oxide mandrel material relative to the etch stop layer material. In some implementations, the metal oxide mandrels are removed using a hydrogen-based etch. For example, in some embodiments, the substrate is contacted with a plasma- activated hydrogen-containing gas, such as a gas including H2, HBr, NH3, a hydrocarbon, H2O, or a combination thereof. The etch chemistry may have a high selectivity to the spacer material, such as a spacer material of W, WN, WO3, Mo, M0O2, M0O3, MoN, M02N, TiO2, AI2O3, ZrO2, or HfO2. By way of an example, a hydrogen-based chemistry such as H2 can have high selectivity to remove the metal oxide mandrels without removing the spacer material. Without being limited by any theory, the hydrogen-containing etch chemistry can form a volatile tin hydride, which can be easily removed from a process chamber.

[0074] Though not shown in the process flow 300, the etch stop layer may be etched in the presence of the plurality of spacers to form a patterned etch stop layer. This may also be referred to as a pattern transfer etch step. The pattern defined by the plurality of spacers is transferred to one or more underlying layers. The one or more underlying layers may include the etch stop layer. In some implementations, the one or more underlying layers may include the etch stop layer and the target layer, where the pattern transfer etch is performed to etch the etch stop layer and the target layer. The etch stop layer may be etched using an etch stop layer etch chemistry. The etch stop layer etch chemistry that is used in this step, in some embodiments, selectively etches the etch stop layer material in the presence of the plurality of spacers. In other words, in some embodiments, the ratio of the etch rate of the etch stop layer material to the etch rate of the spacer material is greater than 1, and is more preferably greater than 1.5 for the etch stop layer etch chemistry. In someimplementations, the etch stop layer etch chemistry includes a fluorine-based etch chemistry such as a fluorocarbon plasma etch chemistry.

[0075] The steps of spacer etch using a spacer etch chemistry, mandrel pull using a mandrel pull chemistry, and pattern transfer etch using an etch stop layer etch chemistry may be processed in-situ in an etch chamber or without a vacuum break in between operations.

[0076] Though not shown in the process flow 300, the plurality of spacers may be removed after the etch stop layer is etched to form a patterned etch stop layer.

[0077] Though not shown in the process flow 300, a gapfill material may be deposited in gaps between patterned features of the patterned etch stop layer.

[0078] In a multiple patterning process, a second organo-metal oxide EUV-sensitive resist material may be deposited over the gapfill material and patterned etch stop features. The second organo-metal oxide EUV-sensitive resist material may be configured to be exposed to EUV radiation to form a second photopatterned organo-metal oxide resist layer. In some implementations, the second organo-metal oxide EUV-sensitive resist material is dry deposited. After deposition, the second photopatterned organo-metal oxide resist layer is developed (e.g., dry developed) to form a second resist mask of second metal oxide mandrels. The second resist mask of second metal oxide mandrels may include two or more layers of varying composition / cross-linking. The second resist mask of second metal oxide mandrels may undergo reactive chemical treatment for hardening and / or reactive ion beam exposure for roughness reduction. A second layer of second spacer material may be deposited on horizontal surfaces and sidewalls of the second metal oxide mandrels. A portion of the second spacer material may be removed from at least the horizontal surfaces of the second metal oxide mandrels. The second metal oxide mandrels may be removed to form a plurality of second spacers used as a mask to etch an underlying layer such as a target layer.

[0079] Figures 4A-4P show cross-sectional schematic illustrations of various stages of an example multiple patterning scheme according to some implementations, using metal oxide mandrels in a patterning process.

[0080] Figure 4A shows a semiconductor substrate having protruding features (first mandrels) 401 residing over a first layer 405 (e.g., etch stop layer). A number of layers 407, 409, 411, 413, 415 underlie the first layer 405. These underlying layers may include the target layer that needs to be patterned and / or one or more hardmasks. By way of an example, the first layer 405 may include a silicon-containing material such as amorphous silicon,silicon oxide, silicon nitride, silicon carbide, silicon oxynitride, etc. In some implementations, the second layer 407 may include a dielectric layer such as an SiCb layer. In some implementations, the third layer 409 may include a hardmask layer such as an ashable hardmask layer. In some implementations, the fourth layer 411 may include a hardmask layer such as an oxide hardmask layer.

[0081] In the depicted embodiment, the first mandrels 401 are made of photoresist and an optional underlayer 403 is disposed between the first mandrels 401 and the first layer 405. The underlayer 403 may be deposited over the first layer 405 of the semiconductor substrate using any suitable deposition technique. In some implementations, the underlayer 403 may include an amorphous hydrogenated carbon film. The underlayer 403 may or may not be doped. The underlayer 403 may serve to improve adhesion of the first mandrels 401 and reduce radiation dose for effective patterning exposure of the photoresist.

[0082] The first mandrels 401 may be formed by deposition of an organo-metal oxide resist material, photopatteming the organo-metal oxide resist material by exposure to patterning radiation (e.g., EUV radiation), and developing the photopattemed organo-metal oxide resist material to form a resist mask of the first mandrels 401. Deposition of the organo-metal oxide resist material may be performed using a dry deposition process. In some implementations, the organo-metal oxide material may be deposited with two or more layers of varying composition / cross-linking. For instance, a bottom layer of the organo-metal oxide resist material may have a greater amount of pre-existing cross-linking than a top layer of the organo-metal oxide resist material. After exposure and PEB treatment, the organo-metal oxide resist material may be developed to form a first resist mask of the first mandrels 401. In some implementations, the organo-metal oxide resist material may be developed using a dry development process, where the dry development process can include exposure to one or more halogen-containing gases. The dry development process can involve a thermal development process, plasma development process, or a combination of thermal and plasma development processes. In some implementations, the first mandrels 401 may be exposed to a reactive chemical treatment to increase hardness and increase cross -linking. In some implementations, the first mandrels 401 may be exposed to a reactive ion beam to trim line CD to a desired target and smoothen the first mandrels 401 to reduce roughness. The first mandrels 401 may be developed to form the first resist mask in a first direction / orientation.

[0083] Figure 4B shows the semiconductor substrate after selective etching of the underlayer 403 using the first resist mask of the first mandrels 401. The underlayer etch canbe selective to the underlayer 403 without substantially etching the first layer 405. After the underlayer etch, the semiconductor substrate includes the first mandrels 401 and the patterned underlayer 403 to define the first resist mask for patterning the first layer 405.

[0084] Figure 4C shows the semiconductor substrate after a conformal layer of first spacer material 417 is deposited over the first resist mask. The conformal layer of first spacer material 417 is deposited over the first mandrels 401, the underlayer 403, and the first layer 405, where the conformal layer of the first spacer material 417 covers both the horizontal surfaces of the semiconductor substrate and the sidewalls of the first mandrels 401 and the underlayer 403. In some implementations, the first spacer material 417 can include W, WN, WO3, Mo, M0O2, M0O3, MoN, M02N, TiCh, AI2O3, Z1O2, or HfCF In some other implementations, the first spacer material 417 can include SiCh, SisN4, TiCh, or any of SiC, SiOC, SiNO, SiCNO, and SiCN. Conformal films generally follow the contour of the semiconductor substrate. The thickness of the conformal film in some embodiments is about the same (with a fluctuation of less than 50%) on all (horizontal and vertical) surfaces. In some embodiments the fluctuation of thickness in the deposited conformal film is less than 15%. In other embodiments the thickness of the conformal film can be significantly greater on horizontal surfaces than on the sidewalls. In some embodiments the conformal layer of the first spacer material 417 is deposited to a thickness of between about 5 - 30 nm, such as between about 10 - 20 nm. Generally, the conformal layer of the first spacer material layer 417 is deposited by any suitable method such as by CVD (including PECVD), ALD (including PEALD), sputtering, etc.

[0085] Figure 4D shows the semiconductor substrate after partial removal of the conformal layer of the first spacer material 417. The conformal layer of the first spacer material 417 is removed from horizontal surfaces without being fully removed from the sidewalls of the first mandrels 401 (and underlayer 403), providing the structure shown in Figure 4D. The first spacer material 417 can be selectively removed relative to the first mandrels 401, the underlayer 403, and the first layer 405 using any of the methods described herein. The first spacer material 417 can be selectively etched with a high selectivity relative to the first mandrels 401 using a suitable etch chemistry such as a fluorine-based chemistry or chlorine-based chemistry. Fluorine-based chemistries may include, for example, NF3, SHs, or a fluorocarbon. Chlorine-based chemistries may include, for example, Ch or BCI3. In some implementations, fluorine-based chemistry or chlorine-based chemistry is plasma-activated.

[0086] Figure 4E shows the semiconductor substrate after removal of the first mandrels 401 using a mandrel pull chemistry. The mandrel pull chemistry may also selectively remove the underlayer 403. The first mandrels 401 comprising the organo-metal oxide resist material may be selectively removed using any of the methods that were described herein. In some implementations, the first mandrels 401 and underlayer 403 can be selectively etched from horizontal surfaces using methods that involve hydrogen-based etching at least during a portion of the selective etch. The first mandrels 401 and underlayer 403 are selectively removed without fully removing the spacer material 417. The spacer material 417 that previously resided at the sidewalls of the first mandrels 401 are substantially retained. After removal of the first mandrels 401 and underlayer 403, the remaining spacer material 417 forms a plurality of free-standing spacers. The number of free-standing spacers 417 is twice the number of first mandrels 401. In some implementations, the first mandrels 401 are selectively removed using a hydrogen-based etchant such as H2, HBr, NH3, a hydrocarbon, H2O, or a combination thereof. In some implementations, the hydrogen-based etchant is plasma- activated. In some implementations, the first mandrels 401 are selectively removed using a combination of a hydrogen-based chemistry and an oxygen-based chemistry, delivered simultaneously or sequentially.

[0087] Figure 4F shows the semiconductor substrate after a pattern transfer etch to result in the formation of a patterned first layer 405. After the first mandrels 401 are removed, the free-standing spacers 417 form a mask in the first direction / orientation that can be used in a pattern transfer etch step. The pattern transfer etch can be applied to one or more underlying layers using the mask. In some implementations, the pattern transfer etch can be applied to both the first layer 405 and the second layer 407 to form a patterned first layer 405 and a patterned second layer 407. The pattern transfer etch chemistry can be used to etch portions of the first layer 405 and optionally portions of the second layer 407 defined by the mask of the free-standing spacers 417. By way of an example, the first layer 405 may include a silicon-containing material (e.g., amorphous silicon), where portions of the first layer 405 may be removed using a fluorine-based chemistry (e.g., fluorocarbon) to form the patterned first layer 405 in the first direction / orientation.

[0088] Figure 4G shows the semiconductor substrate after removal of the free-standing spacers 417 in a spacer strip step. The free-standing spacers 417 can be selectively etched relative to the patterned first layer 405. For example, if free-standing spacers 417 includes a material such as TiCh, the free-standing spacers 417 may be removed by a chlorine-based chemistry. In some implementations, the free-standing spacers 417 can be removed withpatterning the second layer 407 using the same chemistry. In some implementations, the free-standing spacers 417 are removed using a first chemistry and the second layer 407 is patterned using a second chemistry different than the first chemistry.

[0089] Figure 4H shows the semiconductor substrate after deposition of gapfill material 419 in gaps between features of the patterned first layer 405. The gapfill material 419 may be any suitable dielectric material different than a material of the patterned first layer 405. In some implementations, the gapfill material 419 includes a carbon-containing material. Gapfill material 419 may include, for example, amorphous carbon. The gapfill material 419 may be deposited (and optionally planarized) form a planar or substantially planar surface with the patterned first layer 405.

[0090] Figure 41 shows the semiconductor substrate after formation of a second resist mask of second mandrels 421 over a second layer 407. The second layer 407 may include a dielectric layer such as a SiCF layer. The second resist mask of second mandrels 421 are formed in a second direction / orientation different than the first direction / orientation. In some implementations, the second direction / orientation may be perpendicular to the first direction / orientation.

[0091] In the depicted embodiment, the second mandrels 421 are made of a photoresist and an optional second underlayer 423 is disposed between the second mandrels 421 and the second layer 407. The second underlayer 423 may be deposited over the second layer 407 of the semiconductor substrate using any suitable deposition technique. In some implementations, the second underlayer 423 may include an amorphous hydrogenated carbon film. The second underlayer 423 may or may not be doped.

[0092] The second mandrels 421 may be formed by deposition of a second organo-metal oxide resist material, photopatteming the second organo-metal oxide resist material by exposure to patterning radiation (e.g., EUV radiation), and developing the second photopatterned organo-metal oxide resist material to form the second resist mask of the second mandrels 421. Deposition of the second organo-metal oxide resist material may be performed using a dry deposition process. In some implementations, the second organo-metal oxide material may be deposited with two or more layers of varying composition / cross-linking. For instance, a bottom layer of the second organo-metal oxide resist material may have a greater amount of pre-existing cross-linking than a top layer of the second organo-meta oxide resist material. After exposure and PEB treatment, the second organo-metal oxide resist material may be developed to form the second resist mask of the second mandrels 421. In some implementations, the second organo-metal oxide resistmaterial may be developed using a dry development process, where the dry development process can include exposure to one or more halogen-containing gases. In some implementations, the second mandrels 421 may be exposed to a reactive chemical treatment to increase hardness and increase cross -linking. In some implementations, the second mandrels 421 may be exposed to a reactive ion beam to trim line CD to a desired target and smoothen the second mandrels 421 to reduce roughness. The second mandrels 421 may be developed to form the second resist mask in the second direction / orientation. In some implementations with the second underlayer 423 between the second layer 407 and the second mandrels 421, the second underlayer 423 may be selectively etched using the second resist mask of the second mandrels 421 to define the pattern of the second underlayer 423. After the underlayer etch, the semiconductor substrate includes the second mandrels 421 and the second patterned underlayer 423 to define the second resist mask for patterning the second layer 407.

[0093] Figure 4J shows the semiconductor substrate after a second conformal layer of second spacer material 425 is deposited over the second resist mask. The second conformal layer of second spacer material 425 is deposited over the second mandrels 421, the second underlayer 423, and the second layer 407, where the second conformal layer of the second spacer material 425 covers both the horizontal surfaces of the semiconductor substrate and the sidewalls of the second mandrels 421 and the second underlayer 423. In some implementations, the second spacer material 425 can include W, WN, WO3, Mo, M0O2, M0O3, MoN, M02N, TiCh, AI2O3, ZrO2, or HfCb In some other implementations, the second spacer material 425 can include SiCh, SisN4, TiCh, or any of SiC, SiOC, SiNO, SiCNO, and SiCN. Conformal films generally follow the contour of the semiconductor substrate. The thickness of the conformal film in some embodiments is about the same (with a fluctuation of less than 50%) on all (horizontal and vertical) surfaces. In some embodiments the fluctuation of thickness in the deposited conformal film is less than 15%. In other embodiments the thickness of the conformal film can be significantly greater on horizontal surfaces than on the sidewalls. In some embodiments the conformal layer of the second spacer material 425 is deposited to a thickness of between about 5 - 30 nm, such as between about 10 - 20 nm. Generally, the second conformal layer of the second spacer material layer 425 is deposited by any suitable method such as by CVD (including PECVD), ALD (including PEALD), sputtering, etc.

[0094] Figure 4K shows the semiconductor substrate after partial removal of the second conformal layer of the second spacer material 425. The second conformal layer of thesecond spacer material 425 is removed from horizontal surfaces without being fully removed from the sidewalls of the second mandrels 421 (and second underlayer 423), providing the structure shown in Figure 4K. The second spacer material 425 can be selectively removed relative to the second mandrels 421, the second underlayer 423, and the second layer 407 using any of the methods described herein. The second spacer material 425 can be selectively etched with a high selectivity relative to the second mandrels 421 using a suitable etch chemistry such as a fluorine-based chemistry or chlorine-based chemistry. Fluorine-based chemistries may include, for example, NF3, SFe, or a fluorocarbon. Chlorine-based chemistries may include, for example, Ch or BCI3. In some implementations, fluorine-based chemistry or chlorine-based chemistry is plasma- activated.

[0095] Figure 4L shows the semiconductor substrate after removal of the second mandrels 421 using a mandrel pull chemistry. The mandrel pull chemistry may also selectively remove the second underlayer 423. In some implementations, the mandrel pull chemistry may selectively remove both the second mandrels 421 and the gap fill material 419 defined by the second spacer material 425. The second mandrels 421 comprising the second organo-metal oxide resist material may be selectively removed using any of the methods that were described herein. In some implementations, the second mandrels 421 and second underlayer 423 can be selectively etched from horizontal surfaces using methods that involve hydrogenbased etching at least during a portion of the selective etch. The second mandrels 421 and second underlayer 423 are selectively removed without fully removing the second spacer material 425. The second spacer material 425 that previously resided at the sidewalls of the second mandrels 421 are substantially retained. After removal of the second mandrels 421 and second underlayer 423, the remaining spacer material 425 forms a plurality of freestanding spacers. The number of free-standing spacers 425 is twice the number of second mandrels 421. In some implementations, the second mandrels 421 are selectively removed using a hydrogen-based etchant such as H2, HBr, NH3, a hydrocarbon, H2O, or a combination thereof. In some implementations, the hydrogen-based etchant is plasma-activated. In some implementations, the second mandrels 421 are selectively removed using a combination of a hydrogen-based chemistry and an oxygen-based chemistry, delivered simultaneously or sequentially. According to some embodiments, portions of the gapfill material 419 may be selectively removed using a gapfill etch chemistry defined by the freestanding spacers 425. The gapfill etch chemistry may be different than the mandrel pull chemistry. The free-standing spacers 425 may serve as a mask in the second direction / orientation to define removal of the gapfill material 419. The gapfill etchchemistry may selectively etch the gapfill material 419 without substantially removing the patterned first layer 405. The free-standing spacers 425 serve as a mask in the second direction / orientation that can be used to selectively remove portions of the gapfill material 419 defined by the mask, and the gapfill etch chemistry selectively removes the gapfill material 419 while preserving the patterned first layer 405 defined by the mask. This retains the patterned first layer 405 in both the first direction / orientation and the second direction / orientation.

[0096] Figure 4M shows the semiconductor substrate after a pattern transfer etch to result in the formation of a patterned second layer 407. After the second mandrels 421 are removed and some of the gapfill material 419 are removed according to the mask defined by the free-standing spacers 425, the free-standing spacers 425 may be removed in a spacer strip step. The free-standing spacers 425 can be selectively etched relative to the patterned first layer 405 and the remaining gapfill material 419. In some implementations, the freestanding spacers 425 are retained during a subsequent pattern transfer etch step. During the pattern transfer etch step, portions of the second layer 407 are removed to form the patterned second layer 407. The remaining gapfill material 419 and the remaining patterned first layer 405 serve as a mask that can be used in the pattern transfer etch step. The mask may include the patterned first layer 405 in the first direction / orientation and alternating gapfill material 419 and patterned first layer 405 in the second direction / orientation. The pattern transfer etch can be applied to one or more underlying layers using the mask. By way of an example, the second layer 407 may include an SiCF layer, where portions of the second layer 407 may be removed using the mask to form the patterned second layer 407.

[0097] Figure 4N shows the semiconductor substrate after a pattern transfer etch step to result in the formation of a patterned third layer 409. In some implementations, the mask including the remaining gapfill material 419 and the patterned first layer 405 can be selectively removed. Next, the patterned second layer 407 may serve as a mask for defining the pattern for the patterned third layer 409. The pattern transfer etch chemistry can be selective to third layer 409 without removing or substantially removing the patterned second layer 407. Alternatively, the pattern transfer etch chemistry can be selective to the third layer 409 and to the mask including the remaining gapfill material 419 and the patterned first layer 405 without removing or substantially removing the patterned second layer 407. That way, the pattern transfer etch can remove the mask including the remaining gapfill material 419 and the patterned first layer 405 as well as portions of the third layer 409 defined by the patterned second layer 407 simultaneously. By way of an example, the thirdlayer 409 may include an ashable hardmask, where portions of the third layer 409 may be removed using the patterned second layer 407 as the mask to form the patterned third layer 409.

[0098] Figure 40 shows the semiconductor substrate after an oxide etch to result in the formation of a patterned fourth layer 411. As discussed above, the fourth layer 411 may include an oxide hardmask. Using the patterned third layer 409 and / or the patterned second layer 407 as the mask, an oxide etch chemistry can be applied to selectively remove portions of the fourth layer 411 relative to the patterned third layer 409 and the patterned second layer 407. The oxide etch chemistry can be selective to the fourth layer 411 without removing or without substantially removing the patterned third layer 409 and the patterned second layer 407.

[0099] Figure 4P shows the semiconductor substrate after a strip step to result in removal of the patterned second layer 407 and the patterned third layer 409. One or more strip chemistries can be applied that selectively removes the patterned second layer 407 and the patterned third layer 409. In some implementations, a single strip chemistry can remove both the patterned second layer 407 and the patterned third layer 409 without removing or substantially removing the patterned fourth layer 411. In some implementations, a first chemistry can be applied to remove the patterned second layer 407 and a second chemistry can be applied to remove the patterned third layer 409 without removing or substantially removing the patterned fourth layer 411. In some implementations, the one or more strip chemistries may partially remove the fifth layer 413. Or, the one or more strip chemistries may selectively remove the patterned second layer 407 and the patterned third layer 409 without removing or substantially removing the patterned fourth layer 411 and the fifth layer 413.

[0100] Figures 5A-5C show schematic isometric views of a semiconductor substrate undergoing a multiple patterning process using conventional techniques. The conventional techniques utilize materials such as amorphous carbon or amorphous silicon as mandrels in a self-aligned double patterning (SADP) scheme. Such mandrels are more prone to sidewall oxidation and can lead to line CD loss.

[0101] In Figure 5A, a semiconductor substrate includes a first layer that comprises silicon oxynitride (SiON), a second layer that comprises amorphous carbon (a-C), a third layer that comprises silicon oxynitride (SiON), a fourth layer that comprises amorphous carbon (a-C), and a fifth layer that comprises an oxide-based etch stop layer (OX ESL). A patterned mask can be formed by a resist deposition and patterning radiation exposure step, followed by aresist trim and opening the first layer (SiON ARL open) and etching the second layer of amorphous carbon (a-C core etch). Spacer deposition can be performed to deposit an oxide spacer (Ox spacer) along sidewalls and top surfaces of the patterned mask. The oxide spacer can be etched (Ox spacer etch) from top surfaces of the patterned mask and top surfaces of the third layer, where the second layer of amorphous carbon (a-C core pull) can be removed, leaving free-standing oxide spacers.

[0102] In Figure 5B, the third layer that comprises the silicon oxynitride (SiON) undergoes pattern transfer etch using the free-standing oxide spacers as a mask, and the freestanding oxide spacers are subsequently removed. An additional layer of spin-on carbon (SOC) is deposited over the patterned third layer that comprises silicon oxynitride (SiON) followed by a capping layer of silicon oxynitride (SiON). Resist deposition and patterning radiation exposure step are performed. After a resist trim, an oxide spacer deposition step is performed to deposit an oxide spacer (Ox spacer). An oxide spacer etch is performed to remove the oxide spacer from top surfaces of the resist and top surfaces of the capping layer of silicon oxynitride (SiON), and the resist core is pulled, leaving free-standing oxide spacers. Pattern transfer etch is performed using the free-standing oxide spacers as a mask to etch portions of the capping layer of silicon oxynitride (SiON) and the additional layer of spin-on carbon (SOC). The SOC etch can etch partially into the patterned third layer of silicon oxynitride.

[0103] In Figure 5C, the fourth layer of amorphous carbon (a-C) undergoes pattern transfer etch. Hard mask holes can be generated using the patterned fourth layer of amorphous carbon (a-C) by performing a pattern transfer etch of the fifth layer of the oxidebased etch stop layer (OX ESL). A sixth layer of amorphous silicon (a-Si) and a seventh layer of silicon nitride (SiN) can be etched. Holes can be manufactured in the sixth layer of amorphous silicon (a-Si) and the seventh layer of silicon nitride (SiN). Using conventional techniques for multiple patterning, the holes may have different diameters between the top of the hole and the bottom of the hole.

[0104] An apparatus of the present disclosure is configured for multiple patterning processes. The apparatus may be configured for photoresist deposition, photoresist development, reactive chemical treatment, reactive ion beam exposure, spacer material deposition, spacer etch, mandrel pull, strip etch, pattern transfer etch, and other processes described herein. In some implementations, the apparatus is configured to perform all dryoperations. In some implementations, the apparatus is configured to perform a combination of wet and dry operations. The apparatus may include a single wafer chamber or multiple stations in the same process chamber. With multiple stations in the same process chamber, various processing operations such as those described in the present disclosure may be performed in different stations in the same process chamber. In one example, reactive chemical treatment may be performed in one station and reactive ion beam exposure in another station.

[0105] Figure 6 schematically shows a cross-sectional view of a plasma apparatus 600 appropriate for implementing certain aspects of the present disclosure such as dry development and / or etch. The plasma apparatus 600 may be an inductively-coupled plasma (ICP) apparatus or transformer-coupled plasma (TCP) apparatus. An example of the plasma apparatus 600 is a Kiyo® reactor, produced by Lam Research Corporation of Fremont, CA. In other implementations, other tools or tool types having the functionality to conduct dry development and / or etch processes may be used for implementation.

[0106] The plasma apparatus 600 includes an overall process chamber 624 structurally defined by chamber walls 601 and a window 611. The chamber walls 601 may be fabricated from stainless steel or aluminum. The window 611 may be fabricated from quartz or other dielectric material. An optional internal plasma grid 650 can divide the overall process chamber 624 into an upper sub-chamber 602 and a lower sub-chamber 603. In most implementations, plasma grid 650 may be removed, thereby utilizing a chamber space made of sub-chambers 602 and 603. A chuck 617 is positioned within the lower sub-chamber 603 near the bottom inner surface. The chuck 617 is configured to receive and hold a semiconductor wafer 619 upon which etching and deposition processes are performed. The chuck 617 can be an electrostatic chuck for supporting the semiconductor wafer 619 when present. In some implementations, an edge ring (not shown) surrounds the chuck 617, which has an upper surface that is approximately planar with a top surface of the semiconductor wafer 619, when present over the chuck 617. The chuck 617 also includes electrostatic electrodes for chucking and dechucking the semiconductor wafer 619. A filter and DC clamp power supply (not shown) may be provided for this purpose. Other control systems for lifting the semiconductor wafer 619 off the chuck 617 can also be provided. The chuck 617 can be electrically charged using an RF power supply 623. The RF power supply 623 is connected to matching circuitry 621 through a connection 627. The matching circuitry 621 is connected to the chuck 617 through a connection 625. In this manner, the RF power supply 623 is connected to the chuck 617. In various implementations, a bias power of theelectrostatic chuck may be set at about 50 V or may be set at a different bias power depending on the process performed in accordance with the disclosed implementations. For example, the bias power may be between about 20 V and about 100 V, or between about 30 V and about 150 V.

[0107] Elements for plasma generation include a coil 633 positioned above window 611. In some implementations, a coil is not used in the disclosed implementations. The coil 633 is fabricated from an electrically conductive material and includes at least one complete turn. The example of a coil 633 shown in Figure 6 includes three turns. The cross sections of coil 633 are shown with symbols, and coils having an “X” extend rotationally into the page, while coils having aextend rotationally out of the page. Elements for plasma generation also include an RF power supply 641 configured to supply RF power to the coil 633. In general, the RF power supply 641 is connected to matching circuitry 639 through a connection 645. The matching circuitry 639 is connected to the coil 633 through a connection 643. In this manner, the RF power supply 641 is connected to the coil 633. An optional Faraday shield 649a is positioned between the coil 633 and the window 611. The Faraday shield 649a may be maintained in a spaced apart relationship relative to the coil 633. In some implementations, the Faraday shield 649a is disposed immediately above the window 611. In some implementations, the Faraday shield 649b is between the window 611 and the chuck 617. In some implementations, the Faraday shield 649b is not maintained in a spaced apart relationship relative to the coil 633. For example, the Faraday shield 649b may be directly below the window 611 without a gap. The coil 633, the Faraday shield 649a, and the window 611 are each configured to be substantially parallel to one another. The Faraday shield 649a may prevent metal or other species from depositing on the window 611 of the process chamber 624.

[0108] Process gases may be flowed into the process chamber through one or more main gas flow inlets 660 positioned in the upper sub-chamber 602 and / or through one or more side gas flow inlets 670. Eikewise, though not explicitly shown, similar gas flow inlets may be used to supply process gases to a capacitively-coupled plasma processing chamber. A vacuum pump, e.g., a one or two stage mechanical dry pump and / or turbomolecular pump 640, may be used to draw process gases out of the process chamber 624 and to maintain a pressure within the process chamber 624. For example, the vacuum pump may be used to evacuate the lower sub-chamber 603 during a purge operation. A valve-controlled conduit may be used to fluidically connect the vacuum pump to the process chamber 624 so as to selectively control application of the vacuum environment provided by the vacuum pump.This may be done employing a closed loop-controlled flow restriction device, such as a throttle valve (not shown) or a pendulum valve (not shown), during operational plasma processing. Likewise, a vacuum pump and valve controlled fluidic connection to the capacitively-coupled plasma processing chamber may also be employed.

[0109] During operation of the plasma apparatus 600, one or more process gases may be supplied through the gas flow inlets 660 and / or 670. In certain implementations, process gas may be supplied only through the main gas flow inlet 660, or only through the side gas flow inlet 670. In some cases, the gas flow inlets shown in the figure may be replaced by more complex gas flow inlets, one or more showerheads, for example. The Faraday shield 649a and / or optional grid 650 may include internal channels and holes that allow delivery of process gases to the process chamber 624. Either or both of the Faraday shield 649a and optional grid 650 may serve as a showerhead for delivery of process gases. In some implementations, a flow-over-vapor (FOV) delivery system may be situated upstream of the process chamber 624, such that a reactant or precursor is delivered in a gas mixture with a carrier gas and is introduced into the process chamber 624 via the gas flow inlet 660 and / or 670. A concentration of the reactant or precursor may be monitored and controlled by a vapor delivery system according to the present disclosure so that a desired amount of the reactant or precursor is introduced into the process chamber 624. In other implementations, a liquid vaporization and delivery system may be situated upstream of the process chamber 624, such that once a liquid reactant or precursor is vaporized, the vaporized reactant or precursor is introduced into the process chamber 624 via the gas flow inlet 660 and / or 670.

[0110] Radio frequency power is supplied from the RF power supply 641 to the coil 633 to cause an RF current to flow through the coil 633. The RF current flowing through the coil 633 generates an electromagnetic field about the coil 633. The electromagnetic field generates an inductive current within the upper sub-chamber 602. The physical and chemical interactions of various generated ions and radicals with the semiconductor wafer 619 can etch features of the semiconductor wafer 619 or selectively deposit layers on the semiconductor wafer 619.

[0111] If the plasma grid 650 is used such that there is both an upper sub-chamber 602 and a lower sub-chamber 603, the inductive current acts on the gas present in the upper subchamber 602 to generate an electron-ion plasma in the upper sub-chamber 602. The optional internal plasma grid 650 limits the amount of hot electrons in the lower sub-chamber 603. In some implementations, the plasma apparatus 600 is designed and operated such that the plasma present in the lower sub-chamber 603 is an ion-ion plasma.

[0112] Both the upper electron-ion plasma and the lower ion-ion plasma may contain positive and negative ions, though the ion-ion plasma will have a greater ratio of negative ions to positive ions. Volatile etching and / or deposition byproducts may be removed from the lower sub-chamber 603 through port 622. The chuck 617 disclosed herein may operate at elevated temperatures ranging between about 10°C and about 250°C. The temperature will depend on the process operation and specific recipe.

[0113] The plasma apparatus 600 may be coupled to facilities (not shown) when installed in a clean room or a fabrication facility. Facilities include plumbing that provide the processing gases, vacuum temperature control, and environmental particle control. These facilities are coupled to the plasma apparatus 600, when installed in the target fabrication facility. Additionally, the plasma apparatus 600 may be coupled to a transfer chamber that allows robotics to transfer semiconductor wafers into and out of the plasma apparatus 600 using automation.

[0114] In some implementations, a system controller 630 (which may include one or more physical or logical controllers) controls some or all of the operations of a process chamber 624. The system controller 630 may include one or more memory devices and one or more processors. In some implementations, the plasma apparatus 600 includes a switching system for controlling flow rates and durations when disclosed implementations are performed. In some implementations, the plasma apparatus 600 may have a switching time of up to about 500 ms, or up to about 750 ms. Switching time may depend on the flow chemistry, recipe chosen, reactor architecture, and other factors.

[0115] In some implementations, the system controller 630 is part of a system, which may be part of the above-described examples. Such systems can include semiconductor processing equipment, including a processing tool or tools, chamber or chambers, a platform or platforms for processing, and / or specific processing components (a wafer pedestal, a gas flow system, etc.). These systems may be integrated with electronics for controlling their operation before, during, and after processing of a semiconductor wafer or substrate. The electronics may be integrated into the system controller 630, which may control various components or subparts of the system or systems. The system controller 630, depending on the processing parameters and / or the type of system, may be programmed to control any of the processes disclosed herein, including the delivery of processing gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings, RF matching circuit settings, frequency settings, flow rate settings, fluid delivery settings, positional and operation settings, wafer transfersinto and out of a tool and other transfer tools and / or load locks connected to or interfaced with a specific system.

[0116] Figure 7 schematically shows a cross-sectional view of an apparatus 700 appropriate for implementing certain aspects of the present disclosure such as bake and / or treatment. The apparatus 700 may include a process chamber 702 that has an internal volume that houses a showerhead 706 and a pedestal 704. A stem of the pedestal 704 may extend through an aperture in the bottom of the process chamber 702 and may, in some instances, be connected with a vertical lift mechanism 709. The vertical lift mechanism 709 may be controlled so as to raise and / or lower the pedestal 704 relative to the process chamber 702. The process chamber 702 may, for example, include lift pins 721 that extend upwards through lift pin holes in the pedestal 704. The lift pins 721 may act to support a semiconductor wafer 723 when the pedestal 704 is in a lowered position, thereby providing a gap between the semiconductor wafer 723 and the pedestal 704 into which an end effector of a wafer handling robot (not shown) can be inserted in order to place or retrieve the semiconductor wafer 723 from the process chamber 702. When the pedestal 704 is in a raised position, the semiconductor wafer 723 may instead rest directly on a first side 714 of a main body 712 of the pedestal 704. One or more process gases may then be flowed across the semiconductor wafer 723 via the showerhead 706. For example, the showerhead 706 may have a plurality of small gas distribution ports distributed across its underside that act to deliver such process gases across the semiconductor wafer 723 during wafer processing operations. In some implementations, the showerhead 706 and / or the pedestal 704 may serve as electrodes that are used to deliver radio-frequency power to gases that may be in the gap between the showerhead 706 and the pedestal 704, thereby allowing a plasma to be generated and used during wafer processing operations.

[0117] In some implementations, one or more gases flowed through the showerhead 706 includes a gas selected from the group consisting of: water, hydrogen, oxygen, ozone, nitrogen, hydrogen peroxide, carbon monoxide, carbon dioxide, ammonia, nitrous oxide, nitric oxide, an alcohol, acetyl acetone, formic acid, oxalyl chloride, pyridine, a carboxylic acid, an amine, and combinations thereof. In some cases, the gas may include water. In these or other cases, the gas may include hydrogen. In these or other cases, the gas may include oxygen. In these or other cases, the gas may include ozone. In some implementations, the one or more gases include water, oxygen, and / or nitrogen. Gases that are introduced into the process chamber 702 through the showerhead 706 may be used in abake operation, such as a post-exposure bake (PEB) or post-application (PAB) bake operation.

[0118] Gases that are introduced into the process chamber 702 during wafer processing operations may be evacuated from the process chamber 702 via an exhaust system. For example, the process chamber 702 may have an annular exhaust plenum 703 underneath the pedestal 704 that is connected with a vacuum pump 705, thereby allowing gases to be drawn out of the process chamber 702 in a more or less azimuthally uniform manner.

[0119] As noted above, the pedestal 704 may be configured to move up and down vertically relative to the process chamber 702. A bellows seal 711 may be provided to seal between the process chamber 702 and the stem 710 (or a component connected therewith). In this example, the stem 710 is connected with a baseplate that caps off the stem 710, thereby sealing the interior volume of the stem 710 such that non-reactive gas provided by a non-reactive gas source 707 and introduced into the interior of the stem 710 must flow up through the stem 710 and out of the pedestal 704 via gas ports in the first side 714 of the main body 712 of the pedestal 704. However, in other implementations, e.g., in which there is not a non-reactive gas supplied to the main body 712 or in which the non-reactive gas is supplied to the main body 712 but via a gas feed line that extends to the main body 712, the stem 710 may be open on the bottom, e.g., in equilibrium with the surrounding atmosphere.

[0120] An inlet passage 746 and an outlet passage 748 may be fluidically connected with a coolant reservoir 715 (which may incorporate a heat exchanger). A coolant pump 713 may be connected with one of the inlet passage 746 and the outlet passage 748 and used to circulate coolant from the coolant reservoir 715 through the one or more cooling passage segments 734 in the pedestal 704.

[0121] Somewhat similarly, heating element power cables 744 may be electrically connected with a power source 719. A relay or other power-regulating device may be included to allow the amount of power directed to one or more heating element segments 722 to be controlled by a controller 701. The controller 701 may also be communicatively connected with the coolant pump 713 to allow the controller 701 to control the flow of coolant through the one or more cooling passage segments 734. One or more thermocouples, if present, may also be communicatively coupled with the controller 701 as well. The controller 701, for example, may control the coolant pump 713 and the power delivery to the one or more heating element segments 722 in order to cool, heat, or maintain the pedestal 704 at or to a particular temperature. This may be useful for controlling atemperature of the semiconductor wafer 723 during bake and / or other wafer processing operations.

[0122] In some implementations, e.g., atomic layer etch tools, the main body 712 and / or the stem 710 may be coated with an anti-corrosion coating to reduce the potential for metal contamination on the wafers being processed due to the material of the main body 712 and / or the stem 710 being etched away. Such coatings may, for example, include anodized coatings, such as hard anodized coatings, platings, coatings of materials applied via atomic layer deposition, e.g., in another chamber or in the same chamber as the wafer is processed within. In some instances, such coatings may include silicon oxide coatings, aluminum oxide coatings, or other ceramic coatings. In yet other instances, such coatings may include plating, such as nickel plating.

[0123] The controller 701, depending on the processing requirements and / or type of system, may be programmed to control any of the processes disclosed herein, such as processes for controlling the pedestal 704, as well as other processes or parameters not discussed herein, such as the delivery of processing gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, RF generator settings, RF matching circuit settings, frequency settings, flow rate settings, fluid delivery settings, positional and operation settings, wafer transfers into and out of a chamber and other transfer tools and / or load locks connected to or interfaced with a specific system.

[0124] For example, the controller 701 may be configured to maintain the pedestal temperature at a setpoint temperature or range of temperatures (referred to hereinafter simply as a setpoint temperature, which will be understood to refer to both a single desired temperature or a desired range of temperatures), within a range between about 20°C and about 500°C or between about 50°C and about 350°C. The setpoint temperature may, for example, be a temperature, or a temperature range, that is within 50°C-55°C, within 55°C-60°C, within 60°C-65°C , within 65°C-70°C, within 70°C-75°C, within 75°C-80°C, within 80°C-85°C, within 85°C-90°C, within 90°C-95°C, within 95°C-100°C, within 100°C-105°C, within 105°C-110°C, within 110°C-115°C, within 115°C-120°C, within 120°C-125°C, within 125°C-130°C, within 130°C-135°C, within 135°C-140°C, within 140°C-145°C, within 145°C-150°C, within 150°C-155°C, within 155°C-160°C, within 160°C-165°C, within 165°C-170°C, within 170°C-175°C, within 175°C-180°C, within 180°C-185°C, within 185°C-190°C, within 190°C-195°C, within 195°C-200°C, within 200°C-205°C, within 205°C-210°C, or within 210°C-215°C, for example.

[0125] In order to do so, the controller 701 may cause one or more heat exchangers, one or more heaters, and / or one or more chillers (forming, for example, a temperature control system) in, or connected with, the reservoir 715 to heat and / or cool the coolant that is in the reservoir 715 to a temperature that is 50°C or less below the setpoint temperature or temperature range, e.g., within 40°C of and below the setpoint temperature or temperature range, within 30°C of and below the setpoint temperature or temperature range, within 20°C of and below the setpoint temperature or temperature range, within 15 °C of and below the setpoint temperature or temperature range, within 14°C of and below the setpoint temperature or temperature range, within 13 °C of and below the setpoint temperature or temperature range, within 12°C of and below the setpoint temperature or temperature range, within 11 °C of and below the setpoint temperature or temperature range, within 10°C of and below the setpoint temperature or temperature range, within 9°C of and below the setpoint temperature or temperature range, within 8 °C of and below the setpoint temperature or temperature range, within 7 °C of and below the setpoint temperature or temperature range, within 6°C of and below the setpoint temperature or temperature range, or within 5°C of and below the setpoint temperature or temperature range (with regard to the coolant being heated and / or cooled to a temperature of within X°C and below a temperature range, it will be understood that this is inclusive of heating or cooling the coolant to X°C below the setpoint temperature or the bottom end of the setpoint temperature range, as well as to temperatures in between X°C and the setpoint temperature or the bottom end of the setpoint temperature range). In particular implementations, the controller 701 may cause the heat exchanger and / or the heater in, or connected with, the reservoir 715 to heat and / or cool the coolant that is in the reservoir to a temperature that is 20°C or less below the setpoint temperature or temperature range, e.g., 10°C below the setpoint temperature or temperature range.

[0126] The controller 701 may also control the power source 719 to control the application of power to the one or more heating element segments 722 that are within the pedestal 704. The controller 701, for example, may control the application of power to the one or more heating element segments 722 such that when a measured temperature of the pedestal 704, e.g., as measured by the thermocouple or similar temperature measurement sensor(s), falls below a specified first threshold temperature, e.g., a temperature higher than the temperature that the coolant is controlled to be at but lower than the setpoint temperature or temperature range, power is caused to be applied to the one or more heating element segments 722 until the temperature sensor(s) indicate that a second threshold temperature is reached, e.g., thesetpoint temperature or a temperature associated with the setpoint temperature range. In some instances, the first threshold temperature may be the bottom end of the setpoint temperature range (if a range is used), while the second threshold temperature may be at the top end of the setpoint temperature range. In other implementations, the first and / or second threshold temperatures may be set above the bottom end and below the top end, respectively, of the setpoint temperature range.

[0127] Figure 8 schematically shows a cross-sectional view of a thermal apparatus 800 appropriate for implementing certain aspects of the present disclosure such as dry development and / or etch. The thermal apparatus 800 may be used to conduct thermal dry development, thermal etch, or thermal treatment operations. In other implementations, other tools or tool types having the functionality to conduct dry development and / or etch processes may be used for implementation.

[0128] The thermal apparatus 800 includes a process chamber 802 defined by chamber walls 801 and a chamber window 803. The chamber walls 801 may be fabricated from stainless steel or aluminum. In some implementations, the chamber walls 801 may be coated with corrosion-resistant films / liners or halogen-resistant films / liners. One such coating is anodized alumina. Another such coating is yttrium oxide (Y2O3). Another such coating is polytetrafluoroethylene (PTFE), e.g., Teflon IM. The chamber window 803 may be fabricated from quartz or other dielectric material.

[0129] A gas delivery system 810 is fluidically connected to the process chamber 802 via a showerhead 806. The gas delivery system 810 includes one or more gas sources 812. The one or more gas sources 812 are connected by valves 814 and mass flow controllers 816 to a manifold 818. The manifold 818 may be connected to a gas injector for delivery of one or more gases to the showerhead 806. The showerhead 806 distributes gases toward a substrate 820. In some implementations, the substrate 820 is located beneath the showerhead 806 and is supported on a pedestal 830. The showerhead 806 may have any suitable shape, and may have any suitable number and arrangement of ports / holes for distributing gases to the substrate 820. In some implementations, the one or more gas sources 812 of the gas delivery system 810 may provide a flow of dry development chemistries to the process chamber 802, where the dry development chemistries may include a halogen-containing gas such as hydrogen fluoride (HF), hydrogen chloride (HC1), hydrogen bromide (HBr), hydrogen iodide (HI), fluorine (F2), chlorine (CI2), bromine (B^), iodine (I2), or boron tetrachloride (BCI3). In some implementations, the one or more gassources 812 of the gas delivery system 810 may provide a flow of inert / carrier gas such as helium (He), neon (Ne), argon (Ar), xenon (Xe), or nitrogen (N2).

[0130] The pedestal 830 may be raised or lowered to expose the substrate 820 to a volume between the substrate 820 and the showerhead 806. A vertical lift mechanism may be used to control the height of the pedestal 830 relative to the process chamber 802. The pedestal height may be adjusted programmatically by a suitable controller (not shown).

[0131] The pedestal 830 may include an electrostatic chuck configured to receive and hold the substrate 820 upon which the dry development and / or etch processes are performed. The electrostatic chuck may include electrostatic electrodes for chucking and dechucking the substrate 820. The electrostatic electrodes may be embedded in the pedestal 830 and may be connected to a power supply (not shown). In some implementations, an edge ring (not shown) surrounds the electrostatic chuck, which has an upper surface that is approximately planar with a top surface of the substrate 820, when present over the electrostatic chuck.

[0132] In some implementations, the pedestal 830 may be temperature-controlled via one or more heaters 840. In some implementations, the pedestal 830 may be heated to a temperature greater than -60°C and up to 500°C, between about 0°C and about 300°C, between about 20°C and about 200°C, or between about 30°C and about 150°C. The pedestal 830 may be heated using the one or more heaters 840 during non-plasma thermal dry development of a photoresist such as a metal-containing photoresist. In some implementations, the one or more heaters 840 may be arranged in the pedestal 830 in a plurality of independently controllable temperature control zones. This allows the one or more heaters 840 in the pedestal 830 to more precisely and locally control temperature. The temperature control zones may be arranged in a defined pattern such as a rectangular grid, hexagonal grid, or other suitable pattern for generating a temperature profile as desired. In some implementations, the temperature control zones may be spatially arranged in the electrostatic chuck to correct azimuthal non-uniformity or localized CD non-uniformity. Though Figure 8 depicts one or more heaters 840 in the pedestal 830, it will be understood that other heating elements such as radiation sources (e.g., lamps, infrared lights, ultraviolet lights, or light-emitting diodes (LEDs)) may be used alternatively or in conjunction with the one or more heaters 840.

[0133] The thermal apparatus 800 may be equipped with one or more temperature sensors for monitoring the temperature of the substrate and / or substrate support during thermal dry development and / or etch operations. In one example, a controller may control applicationof power to the one or more heaters 840 according to a desired temperature setpoint or desired temperature range. When a measured temperature of the pedestal 830 falls below or above the desired temperature setpoint or desired temperature range, e.g., as measured by a thermocouple or similar temperature sensor, power is controlled to the one or more heaters 840 accordingly until the thermocouple or similar temperature sensor indicates that the desired temperature setpoint or desired temperature range is reached. As such, temperature measurements from the thermocouple or other similar temperature sensor may be used as feedback to actively control the temperature of the substrate 820 during substrate processing operations.

[0134] In some implementations, pressure control for the process chamber 802 may be controlled using a vacuum pump 850. The vacuum pump 850 may include a one-stage or two-stage mechanical dry pump and / or turbomolecular pump, which may be used to draw gases out of the process chamber 802. For example, the vacuum pump 850 may be used to evacuate reactive gases, carrier gases, inert gases, and / or volatile byproducts from the process chamber 802 during or after a thermal dry development and / or etch operation. In some implementations, the vacuum pump 850 may be fluidically connected with a valve-controlled conduit such as a throttle valve (e.g., butterfly valve) or pendulum valve. The valve-controlled conduit may throttle a vacuum provided by the downstream vacuum pump 850 to control pressure. However, in some implementations, pressure control of the process chamber 802 may be adjusted by varying a flow rate of one or more gases into the process chamber 802.

[0135] In some implementations, a chamber baffle 860 may be provided in the process chamber 802. The chamber baffle 860 may serve to manage gas flow, enhance process uniformity, and improve cleanliness by redirecting gas flow in the process chamber 802. The chamber baffle 860 may serve to prevent contaminants from escaping into exhaust lines and into the vacuum pump 850. The chamber baffle 860 may redirect gas flow from a direct line to a controlled path so that the gas flow is more evenly distributed about the circumference of the pedestal 830, thereby reducing the chances of flow non-uniformities developing in reactants flowed across the substrate 820.

[0136] In some implementations, the thermal apparatus 800 further includes a chamber port 808 that can be used for endpoint detection or monitoring a progress of a substrate processing operation. The chamber port 808 may be equipped for optical emission spectroscopy (OES) to monitor an emission intensity of light at a pre-specified wavelength in time. The identified wavelength corresponds to a chemical species present in thesemiconductor process, such as a volatile byproduct, and the intensity can be used to correlate with the completion of a semiconductor process such as thermal dry development and / or etch. The chamber port 808 may alternatively or additionally be equipped for infrared (IR) spectroscopy, which measures the absorbance by a chemical species in the IR spectrum. In some implementations, the chamber port 808 may alternatively or additionally be equipped for interferometric endpoint (IEP) detection, where a light beam is directed onto the substrate 820 and a reflected light beam emanates from the substrate 820. The reflected light beam is detected by a detector that generates an interference signal to determine an endpoint of the semiconductor process such as thermal dry development and / or etch. However, it will be understood that the process chamber 802 may be equipped with non-optical sensors to perform endpoint detection or monitor a progress of a substrate processing operation. Examples of non-optical techniques or non-optical sensors are described in International Patent Publication No. WO 2024 / 123632, entitled “ENDPOINT DETECTION AND TRACKING OF PHOTORESIST PROCESSES,” which is incorporated herein by reference in its entirety and for all purposes.

[0137] A controller 870 may control all of the activities of the thermal apparatus 800. The controller 870 may include one or more memory devices and one or more processors configured to execute the instructions so that the thermal apparatus 800 will perform a method in accordance with the present disclosure. In some implementations, instructions for the controller 870 may be provided via input / output control (IOC) sequencing operations. In one example, the instructions for setting conditions for a process phase may be included in a corresponding recipe phase of a process recipe. In some cases, process recipe phases may be sequentially arranged, so that all instructions for a process phase are executed concurrently with that process phase. Examples of programs or sections of programs for this purpose include a substrate positioning program, a process gas control program, a pressure control program, and a temperature control program. In some implementations, the controller 870 may be employed for setting a flow rate of a dry development chemistry reactant gas, such as a hydrogen halide (e.g., HBr or HC1), and time delay instructions for the recipe phase. In some implementations, the controller 870 may be employed for setting a temperature of the pedestal 830 to control substrate temperature during exposure to the dry development chemistry reactant gas.

[0138] Figure 9 schematically shows a cross-sectional view of an apparatus 900 appropriate for implementing certain aspects of the present disclosure such as deposition, etching, dry development, and / or cleaning. The apparatus 900 may be an inductively-coupled plasma (ICP) apparatus. An example of the apparatus 900 is a Selis® reactor, produced by Lam Research Corporation of Fremont, CA. In other implementations, other tools or tool types having the functionality to conduct deposition, etching, dry development, and / or cleaning processes may be used for implementation. It will be understood that one or more features described in connection with the apparatus 900 may be omitted. For example, such features may include, but are not limited to, hardware for generating plasma. While plasma may be used in some implementations, other implementations may occur without any use of plasma.

[0139] In some implementations, the apparatus 900 includes a lower chamber region 902 and an upper chamber region 904. The lower chamber region 902 may be defined by chamber sidewall surfaces 908, a chamber bottom surface 910, and a lower surface of a gas distribution device 914. In some implementations, the upper chamber region 904 is defined by an upper surface of the gas distribution device 914 and an inner surface of a dome 918. In some implementations, the dome 918 rests on a first annular support 921. The first annular support 921 includes one or more spaced holes 923 for delivering process gas to the upper chamber region 904. In some implementations, the process gas is delivered by the one or more spaced holes 923 in an upward direction at an acute angle relative to a plane including the gas distribution device 914, although other angles / directions may be used. In some implementations, a gas flow channel 934 in the first annular support 921 supplies gas to the one or more spaced holes 923.

[0140] In some implementations, the first annular support 921 may rest on a second annular support 925 that defines one or more spaced holes 927 for delivering process gas from a gas flow channel 929 to the lower chamber region 902. In some implementations, holes 931 in the gas distribution device 914 align with the spaced holes 927. In other implementations, the gas distribution device 914 has a smaller diameter and the holes 931 are not needed. IN some implementations, the process gas is delivered by the one or more spaced holes 927 in a downward direction towards a substrate 926 at an acute angle relative to the plane including the gas distribution device 914, although other angles / directions may be used. In some implementations, the upper chamber region 904 is cylindrical with a flat top surface and one or more flat inductive coils may be used. In still other examples, a single chamber may be used with a spacer located between a showerhead and a substrate support.

[0141] In some implementations, a substrate support 922 is arranged in the lower chamber region 902. In some implementations, the substrate support 922 includes an electrostaticchuck, although other types of substrate supports may be used. In some implementations, a substrate 926 is arranged on an upper surface of the substrate support 922 during substrate processing (e.g., deposition, development, etching, cleaning, etc.). In some implementations, the temperature of the substrate 926 may be controlled by a heater plate 917, an optional cooling plate with fluid channels, and one or more temperature sensors, although other suitable substrate support temperature control systems may be used.

[0142] In some implementations, the gas distribution device 914 includes a showerhead, e.g., a plate 933 having a plurality of spaced holes 935. The plurality of spaced holes 935 may extend from the upper surface of the plate 933 to the lower surface of the plate 933. In some implementations, the spaced holes 935 may have a diameter in a range from about 0.1 inches to about 0.75 inches. In some implementations, the showerhead is made of a conducting material such as aluminum or a non-conductive material such as ceramic with an embedded electrode made of a conducting material.

[0143] In some implementations, one or more inductive coils 940 are arranged around an outer portion of the dome 918. When energized, the one or more inductive coils 940 create an electromagnetic field inside of the dome 918. In some implementations, an upper coil and a lower coil are used. In some implementations, a gas injector 942 injects one or more gas mixtures from a gas delivery system 950-1. The gas delivery system 950-1 may include one or more gas sources 952, one or more valves 954, one or more mass flow controllers (MFCs) 956, and a mixing manifold 958, although other types of delivery systems may be used. In some implementations, the mixing manifold 958 may be omitted, and the gases may be independently provided to the gas injector 942. The vapor delivery system 959 may deliver vapor including a carrier gas and another gas to a process chamber of the apparatus 900. In some cases, the vapor delivery system 959 may deliver vapor to the mixing manifold 958 of the gas delivery system 950-1.

[0144] In some implementations, a gas splitter (not shown) may be used to vary flow rates of a gas mixture. In some implementations, another gas delivery system 950-2 may be used to supply other gas mixtures such as an etch gas or etch gas mixture to the gas flow channels 929 and / or 934 (in addition to or instead of etch gas from the gas injector 942). A process gas may include at least a halogen-containing gas. The halogen-containing gas (e.g., HBr) may be co-flowed with another halogen-containing gas, hydrogen gas, oxidizing gas, hydrocarbon gas, or inert / carrier gas. The halogen-containing gas may be flowed into the apparatus 900 using any combination of the gas delivery system 950-1, the gas delivery system 950-2, and / or the vapor delivery system 959. Suitable single or dual gas injectorsand other gas injection locations are shown and described in U.S. Patent No. 10,825,659, entitled “SUBSTRATE PROCESSING CHAMBER INCLUDING MULTIPLE GAS INJECTION POINTS AND DUAL INJECTOR,” which is hereby incorporated by reference in its entirety and for all purposes.

[0145] The gas injector 942 may include a center injection location that directs gas in a downward direction and one or more side injection locations that inject gas at an angle with respect to the downward direction. In some implementations, the gas delivery system 950-1 delivers a first portion of the gas mixture at a first flow rate to the center injection location and a second portion of the gas mixture at a second flow rate to the side injection location(s) of the gas injector 942. In some implementations, different gas mixtures are delivered by the gas injector 942. The gas delivery system 950-1 may deliver one or more processing gases to the gas flow channels 929 and 934 and / or to other locations in the processing chamber.

[0146] The plasma generator 970 may be used to generate RF power that is output to the one or more inductive coils 940. In some implementations, the plasma 990 is generated in the upper chamber region 904. In some implementations, the plasma generator 970 includes an RF source 972 and a matching network 974. In some implementations, the matching network 974 matches an impedance of the RF source 972 to the impedance of the one or more inductive coils 940. The gas distribution device 914 may be connected to a reference potential such as ground. In some implementations, a valve 978 and a pump 980 may be used to control pressure inside of the lower chamber region 902 and the upper chamber region 904 and to evacuate reactants / gases.

[0147] A controller 976 may control various components of the apparatus 900. In some implementations, the controller 976 communicates with the gas delivery system 950-1, the gas delivery system 950-2, the valve 978, the pump 980, and / or the plasma generator 970 to control flow of process gas, purge gas, RF plasma, and chamber pressure. In some implementations, plasma is sustained inside the dome 918 by the one or more inductive coils 940. One or more gas mixtures may be introduced from a top portion of the processing chamber using the gas injector 942 (and / or spaced holes 923) and the plasma may be confined within the dome 918 using the gas distribution device 914. In some implementations, the controller 976 may control various activities associated with the apparatus 900 to perform deposition, etch, dry development, and / or clean processes.

[0148] In some implementations, an RF bias 984 is provided and includes an RF source 986 and an optional matching network 988. The RF bias power can be used to create plasmabetween the gas distribution device 914 and the substrate support 922 or to create a self-bias on the substrate 926 to attract ions. In some implementations, the controller 976 may be used to control the RF bias power.

[0149] Figure 10 schematically shows a cross-sectional view of an apparatus 1000 appropriate for implementing certain aspects of the present disclosure such as deposition and / or etching. In some instances, the apparatus 1000 may be employed as a deposition chamber such as vapor-based deposition of a film. An example of the apparatus 1000 is an Argos® reactor, produced by Lam Research Corporation of Fremont, CA. In other implementations, other tools or tool types having the functionality to conduct deposition and / or etching processes may be used for implementation.

[0150] As can be seen, an apparatus 1000 is depicted that has a processing chamber 1002 that includes a lid 1008. The processing chamber 1002 may include a wafer transfer passage 1004 through one of the walls of the processing chamber 1002 that is sized to allow a substrate 1022 to be passed therethrough and into the interior of the processing chamber 1002, where the substrate 1022 may be placed on a wafer support 1024. The wafer transfer passage 1004 may have a gate valve 1006 or similar door mechanism that may be operated to seal or unseal the wafer transfer passage 1004, thereby allowing the environment within the processing chamber 1002 to be isolated from the environment on the other side of the gate valve 1006. For example, the processing chamber 1002 may be provided with substrate 1022 via a wafer handling robot that is located in an adjoining transfer chamber. Such a transfer chamber may, for example, have multiple processing chambers 1002 arranged around its periphery, with each such processing chamber 1002 connected with the transfer chamber via a corresponding gate valve 1006.

[0151] The wafer support 1024 may, for example, include an electrostatic chuck (ESC) 1026, which may be used to provide a wafer support surface for supporting the substrate 1022. The ESC 1026 may include, for example, a base plate 1034 that is bonded to a top plate 1028 that is placed atop the base plate 1034. The top plate 1028 may, for example, be made of a ceramic material and may have embedded within it several other components. In the depicted example, the top plate 1028 has two separate electrical systems embedded within it. One such system is an electrostatic clamping electrode system, which may have one or more clamping electrodes 1032 that may be used to generate an electric charge within the substrate 1022 that causes the substrate 1022 to be drawn against the wafer support surface of the top plate 1028. In the implementation of Figure 10, there are two clamping electrodes 1032 that provide a bi-polar electrostatic clamping system, although someimplementations may use only a single clamping electrode 1032 to provide a mono-polar electrostatic clamping system.

[0152] Another system is a thermal control system that may be used to control the temperature of the substrate 1022 during processing conditions. In Figure 10, the thermal control system is a multi-zone thermal control system featuring four annular resistance heater traces 1030a, 1030b, 1030c, and 1030d that are concentric with one another and positioned beneath the clamping electrodes 1032. The center resistance heater traces 1030a may, in some implementations, fill a generally circular area, and each resistance heater trace 1030a / b / c / d may follow a generally serpentine or otherwise meandering path within a corresponding annular region. Each resistance heater trace 1030a / b / c / d may be individually controlled to provide a variety of radial heating profiles in the top plate 1028; such a four-zone heating system may, for example, be controlled to maintain the substrate 1022 so as to have a temperature uniformity of ±0.5°C in some cases. While the apparatus 1000 of Figure 10 features a four-zone heating system in the ESC 1026, other implementations may use single-zone or multi-zone heating systems having more or fewer than four zones.

[0153] In some implementations, heat pumps may be used instead of resistance heating traces. For example, in some implementations, the resistance heater traces 1030a, 1030b, 1030c, and 1030d may be replaced by, or augmented by, Peltier junctions or other, similar devices that may be controlled to “pump” heat from one side thereof to another. Such mechanisms may be used, for example, to draw heat from the top plate 1028 (and thus the substrate 1022) and direct it into the baseplate 1034 and the heat exchange passages 1036, thereby allowing the substrate 1022 to be cooled more rapidly and more effectively, if desired.

[0154] The ESC 1026 may also include, for example, a base plate 1034 that may be used to provide structural support to the underside of the top plate 1028 and which may also act as a heat dispersion system. For example, the base plate 1034 may include one or more heat exchange passages 1036 that are arranged in a generally distributed fashion throughout the base plate 1034, e.g., the heat exchange passages 1036 may follow a serpentine, circular switchback, or spiral pattern around the center of the base plate 1034. A heat exchange medium, e.g., water or inert fluorinated liquid, may be circulated through the heat exchange passages 1036 during use. The flow rate and temperature of the heat exchange medium may be externally controlled so as to result in a particular heating or cooling behavior in the base plate 1034.

[0155] The ESC 1026 may, for example, be supported by a wafer support housing 1042 that is connected with, and supported by, a wafer support column 1044. The wafer support column 1044 may, for example, have a routing passage 1048 or other pass-throughs for routing cabling, fluid flow conduits, and other equipment to the underside of the base plate 1034 and / or the top plate 1028. For example, while not shown in Figure 10, cabling for providing electrical power to the resistance heater traces 1030a / b / c / d may be routed through the routing passage 1048, as may cabling for providing electrical power to the clamping electrodes 1032. Other cables, e.g., cables for temperature sensors, may also be routed through the routing passage 1048 to locations in the interior of the wafer support 1024. In implementations with a temperature-controllable base plate 1034, conduits for conveying heat exchange medium to and from the base plate 1034 may also be routed through the routing passage 1048. To avoid undue clutter, such cables and conduits are not depicted in Figure 10, but it is to be understood that they would, nonetheless, be present.

[0156] The apparatus 1000 of Figure 10 also includes a wafer support z-actuator 1046 that may provide movable support to the wafer support column 1044. The wafer support z-actuator 1046 may be actuated to cause the wafer support column 1044, and the wafer support 1024 supported thereby, to move up or down vertically, e.g., by up to several inches, within a reaction space 1020 of the processing chamber 1002. In doing so, a gap distance X between the substrate 1022 and the underside of the showerhead 1010 may be tuned depending on various process conditions.

[0157] The wafer support 1024 may also include, in some implementations, one or more edge rings that may be used to control and / or fine-tune various process conditions. In Figure 10, an upper edge ring 1038 is provided that lies on top of, for example, lower edge rings 1040a and 1040b, which, in turn, are supported by the wafer support housing 1042 and a third lower edge ring 1040c. The upper edge ring 1038 may, for example, be generally subjected to the same processing environment as the substrate 1022, whereas the lower edge rings 1040a / b / c may generally be shielded from the processing environment. Due to the increased exposure of the upper edge ring 1038, the upper edge ring 1038 may have a limited lifespan and may require more frequent replacement or cleaning as compared with the lower edge rings 1040a / b / c.

[0158] The apparatus 1000 may also include a system for removing process gases from the processing chamber 1002 during and after processing. For example, the processing chamber 1002 may include an annular plenum 1056 that encircles the wafer support column 1044. The annular plenum 1056 may, in turn, be fluidically connected with a vacuumforeline 1052 that may be connected with a vacuum pump, e.g., such as may be located beneath a subfloor below the apparatus 1000. A regulator valve 1054 may be provided in between the vacuum foreline 1052 and the processing chamber 1002 and actuated to control the flow into the vacuum foreline 1052. In some implementations, a baffle 1050, e.g., an annular plate or other structure that may serve to make the flow into the annular plenum 1056 more evenly distributed about the circumference of the wafer support column 1044, may be provided to reduce the chances of flow non-uniformities developing in reactants flowed across the substrate 1022.

[0159] The showerhead 1010 may be a dual-plenum showerhead 1010 and may include a first plenum 1012 that is provided to process gas via a first inlet 1016 and a second plenum 1014 that is provided to process gas via a second inlet 1018. Generally, two plenums can be employed to maintain separation between the precursor(s) and the counter-reactant(s) prior to release of the precursor and the counter-reactant. The showerhead 1010 may, in some implementations, have more than two plenums. In some instances, a single plenum is used to deliver the precursor(s) into the reaction space 1020 of the processing chamber 1002. Each plenum may have a corresponding set of gas distribution ports that fluidically connect the respective plenum with the reaction space 1020 through the faceplate of the showerhead 1010 (the faceplate being the portion of the showerhead 1010 that is interposed between the lowermost plenum and the reaction space 1020).

[0160] The first inlet 1016 and the second inlet 1018 of the showerhead 1010 may be provided processing gases via a gas supply system, which may be configured to provide one or more precursor(s) and / or counter-reactant(s), as discussed herein. The depicted apparatus 1000 is configured to provide multiple precursors and multiple counter-reactants. For example, a first valve manifold 1068a may be configured to provide precursor(s) to the first inlet 1016, while a second valve manifold 1068b may be configured to provide other precursor(s) or other counter-reactants to the second inlet 1018.

[0161] A first valve manifold 1068a may be configured to provide one or more precursor(s) to the first inlet 1016, while a second valve manifold 1068b may be configured to provide other precursor(s) or other reactant to the second inlet 1018. In this example, the first valve manifold 1068a, for example, includes multiple valves A1-A5. Valve A2 may, for example, be a three-way valve that has one port fluidically connected with a first vapor source 1072a, another port fluidically connected with a bypass line 1070a, and a third port fluidically connected with a port on another 3-way valve A3. Similarly, valve A4 may be another three-way valve that has one port fluidically connected with a second vapor source1072b, another port fluidically connected with the bypass line 1070a, and a third port fluidically connected with a port on another 3 -way valve A5. One of the other ports on valve A5 may be fluidically connected with the first inlet 1016 while the remaining port on valve A5 may be fluidically connected with one of the remaining ports on the valve A3. The remaining port on the valve A3 may, in turn, be fluidically connected with the valve Al which may be fluidically interposed between the valve A3 and a purge gas source 1074, e.g., nitrogen, argon, or other suitably inert gas (with respect to precursor(s) and / or counterreactants)). In some implementations, only the first valve manifold 1068a is employed.

[0162] For the purposes of this disclosure, the term “fluidically connected” is used with respect to volumes, plenums, holes, etc., that may be connected with one another in order to form a fluidic connection, similar to how the term “electrically connected” is used with respect to components that are connected together to form an electric connection. The term “fluidically interposed,” if used, may be used to refer to a component, volume, plenum, or hole that is fluidically connected with at least two other components, volumes, plenums, or holes such that fluid flowing from one of those other components, volumes, plenums, or holes to the other or another of those components, volumes, plenums, or holes would first flow through the “fluidically interposed” component before reaching that other or another of those components, volumes, plenums, or holes. For example, if a pump is fluidically interposed between a reservoir and an outlet, fluid that flowed from the reservoir to the outlet would first flow through the pump before reaching the outlet.

[0163] The first valve manifold 1068a may, for example, be controllable to cause vapors from one or both of the vapor sources 1072a and 1072b to be flowed either to the processing chamber 1002 or through the first bypass line 1070a and into the vacuum foreline 1052. The first valve manifold 1068a may also be controllable to cause a purge gas to be flowed from the purge gas source 1074 and into the first inlet 1016.

[0164] For example, to flow vapor from the first vapor source 1072a into the reaction space 1020, the valve A2 may be actuated to cause the vapor from the first vapor source 1072a to first flow into the first bypass line 1070a. This flow may be maintained for a period of time sufficient to allow the flow of the vapor to reach steady state flow conditions. After sufficient time has passed (or after a flow meter, if used, indicates that the flow rate is stable), valves A2, A3, and A5 may be actuated to cause the vapor flow from the first vapor source 1072a to be directed to the first inlet 1016. Similar operations with valves A4 and A5 may be performed to deliver vapor from the second vapor source 1072b to the first inlet 1016. In some instances, it may be desirable to purge one of the vapors from the first plenum1012 by actuating the valves Al, A3, and A5 so as to cause the purge gas from the purge gas source 1074 to be flowed into the first inlet 1016. In some additional implementations, it may be desirable to simultaneously flow vapor from one of the vapor sources 1072a or 1072b in tandem with flowing gas from the purge gas into the first inlet 1016. Such implementations may be used to dilute the concentration of the reactant(s) contained in such vapor(s).

[0165] It will be appreciated that the second valve manifold 1068b may be controlled in a similar manner, e.g., by controlling valves B1-B5, to provide vapors from vapor sources 1072c and 1072d to the second inlet 1018 or to the second bypass line 1070b. It will be further appreciated that different manifold arrangements may be utilized as well, including a single unitary manifold that includes valves for controlling flow of the precursor(s), counter-reactant(s), or other reactants to the first inlet 1016 and the second inlet 1018.

[0166] As mentioned earlier, some apparatuses 1000 may feature a lesser number of vapor sources, e.g., only two vapor sources 1072, in which case the valve manifold(s) 1068 may be modified to have a lesser number of valves, e.g., only valves A1-A3.

[0167] The vapor sources 1072 may be flow-over-vapor (FOV) sources. In an FOV source, a carrier gas may pass over a heated liquid compound containing a precursor or reactant to pick up and transport the precursor or reactant. The resulting gas mixture containing the carrier gas and the precursor or reactant is flowed through heated gas lines to prevent condensation of the precursor or reactant. The gas mixture is transported to valve manifold(s) 1068 to control the flow of the precursors and / or reactants passing through the first inlet 1016 and the second inlet 1018. In some implementations, concentrations of the precursors and / or reactants may be monitored to determine an amount of the precursors and / or reactants flowing through the valve manifolds 1068. Temperature-controlled mass flow controllers and / or dilution mass flow controllers may be used to control the flow rates of the precursors and / or reactants and adjust the concentrations of the precursors and / or reactants passing through the first inlet 1016 and the second inlet 1018. As such, a precise amount of precursors and / or reactants can be monitored and controlled through the showerhead 1010 and into the processing chamber 1002 during dry deposition of film on the substrate 1022.

[0168] As discussed above, apparatuses such as apparatus 1000, which may be used to provide for dry deposition of films, may be configured to maintain particular temperature profiles within the processing chamber 1002. In particular, such apparatuses 1000 may be configured to maintain the substrate 1022 at a lower temperature, e.g., at least 25°C to 50°Clower, than most of the equipment of the apparatus 1000 that comes into direct contact with the precursor(s) and / or counter-reactant(s). Additionally, the temperature of the equipment of the apparatus 1000 that comes into direct contact with the precursor(s) and / or counterreactants) may be kept to an elevated level that is sufficiently high that condensation of the vaporized reactants on the surfaces of such equipment is discouraged. At the same time, the temperature of the substrate 1022 may be controlled to a level that promotes condensation, or at least deposition, of the reactants on the substrate 1022.

[0169] To provide for such temperature control, various heating systems may be included in the apparatus 1000. For example, the processing chamber 1002 may have receptacles for receiving cartridge heaters 1058, e.g., for a processing chamber 1002 that has a generally cylindrical interior volume but a square or rectangular external shape, vertical holes for receiving cartridge heaters 1058 may be bored into the four comers of the processing chamber 1002 housing. In some implementations, the showerhead 1010 may be covered with heater blankets 1060, which may be used to apply heat across the exposed upper surface of the showerhead 1010 to keep the showerhead temperature elevated. It may also be beneficial to heat various gas lines that are used to conduct the vaporized reactants from the vapor sources 1072 to the showerhead 1010. For example, resistive heater tape may be wound around such gas lines and used to heat them to an elevated temperature. As shown in Figure 10, all of the gas lines that potentially have precursor(s) and / or counter-reactant(s) flowing through them are shown as being heated, including the bypass lines 1070. The only exceptions are the gas lines from the valve manifolds 1068 to the first inlet 1016 and the second inlet 1018, which may be quite short and may be indirectly heated by the showerhead 1010. Of course, even these gas lines may be actively heated, if desired. In some implementations, heaters may be provided proximate to the gate valve 1006 to provide heat to the gate valve as well.

[0170] The various operational systems of the apparatus 1000 may be controlled by a controller 1084, which may include one or more processors 1086 and one or more memory devices 1088 that are operatively connected with each other and that are communicatively connected with various systems and subsystems of the apparatus 1000 so as to provide for control functionality for those systems. For example, the controller 1084 may be configured to control the valves A1-A5 and B1-B5, the various heaters 1058, 1060, the vapor sources 1072, the regulator valve 1054, the gate valve 1006, the wafer support z-actuator, and so forth.

[0171] Once the film layer has been deposited on the substrate 1022, the substrate 1022 may, as noted above, be transferred to one or more subsequent processing chambers or tools for additional operations (e.g., any described herein). Further deposition apparatuses are described in International Patent Application No. PCT / US2020 / 038968, filed June 22, 2020, published as International Patent Publication No. WO 2020 / 263750, titled “APPARATUS FOR PHOTORESIST DRY DEPOSITION,” which is herein incorporated by reference in its entirety and for all purposes.

[0172] As described above, one or more process stations may be included in a multistation processing tool. Figure 11 shows a schematic view of an implementation of a multistation processing tool 1100, which can include an inbound load lock 1103 and an outbound load lock 1105, either or both of which may include a plasma source and / or an ultraviolet (UV) source. Robot 1137, at atmospheric pressure, is configured to move wafers from a cassette loaded through pod 1109 into inbound load lock 1103 via an atmospheric port 1111. Wafer 1107 is placed by robot 1137 on pedestal 1113 in inbound load lock 1103, atmospheric port 1111 is closed, and inbound load lock 1103 is pumped down. In instances in which inbound load lock 1103 includes a remote plasma source, wafer 1107 may be exposed to a remote plasma treatment in inbound load lock 1103 prior to being introduced into processing chamber 1115. Further, wafer 1107 may be heated in inbound load lock 1103 to, for example, remove moisture and / or adsorbed gases. Next, chamber transport port 1117 to processing chamber 1115 is opened, and another robot 1119 places wafer 1107 into the reactor on a pedestal of a first station shown in the reactor for processing. While the implementation depicted in Figure 11 includes load locks, it will be appreciated that, in some implementations, direct entry of wafer 1107 into a processing station may be provided.

[0173] As seen in Figure 11, processing chamber 1115 includes four process stations, numbered 1 to 4. Each process station may be considered a process module provided above. Each station has a temperature-controlled pedestal (such as temperature-controlled pedestal 1121 of station 1), and gas line inlets, one or more of which may include a corresponding flow adjuster configured to match (or substantially match) flow conditions (e.g., flow conductance, flow velocity, etc.) to the gas line inlets. It will be appreciated that, in some cases, each process station may have different or multiple purposes. For example, in some embodiments, a process station may be switchable between a CVD and PECVD process mode. In another example, deposition operations, e.g., PECVD operations, may be performed in one station, while exposure to radiation for curing may be performed in another station. In some cases, deposition and curing may be performed in the same station.Further, although processing chamber 1115 shown as including four stations, embodiments are not limited thereto. For example, processing chamber 1115 may have any suitable number of stations, such as five or more stations, or three or less stations

[0174] Figures 11 shows a the multi-station processing tool 1100 with a wafer handling system (e.g., robot 1119 including spider forks 1101) for transferring and / or positioning wafers within processing chamber 1115. In some implementations, the wafer handling system may transfer wafers between various process stations and / or between a process station and a load lock. It is contemplated, however, that any suitable wafer handling system may be employed, such as, for example, wafer carousels, other wafer handling robots, etc. Further, multi- station processing tool 1100 may include (or otherwise be coupled to) a system controller 1123 employed to control process conditions and hardware states of multistation processing tool 1100. The system controller 1123 may include one or more memory devices 1125, one or more mass storage devices 1127, and one or more processors 1129. Each processor 1129 may include a central processing unit (CPU) or computer, analog, and / or digital input / output connections, stepper motor controller boards, etc.

[0175] In some implementations, the system controller 1123 controls each of the activities of multi-station processing tool 1100. For instance, system controller 1123 may execute system control software 1131 stored in mass storage device 1127, loaded into memory device 1125, and executed by processor 1129. Alternatively, control logic may be hard coded in system controller 1123. Application specific integrated circuits (ASIC), programmable logic devices (e.g., field-programmable gate arrays (FPGAs)) and / or the like may be used for these purposes. In the following discussion, wherever “software” or “code” is used, functionally comparable hard coded logic may be used in its place. System control software 1131 may include instructions for controlling the timing, mixture of gases, gas flow rates, flow conductance, chamber and / or station pressure, chamber and / or station temperature, wafer temperature, target power levels, RF power levels, substrate pedestal, chuck and / or susceptor position, and other parameters of a particular process performed by multi-station processing tool 1100. Further, system control software 1131 may be configured in any suitable way. For example, various process tool component subroutines or control objects may be written to control operation of the process tool components used to carry out various process tool processes. System control software 1131 may be coded in any suitable computer readable programming language.

[0176] In some implementations, system control software 1131 may include input / output control (IOC) sequencing instructions for controlling the various parameters describedabove. Other computer software and / or programs stored on mass storage device 1127 and / or memory device 1125 associated with system controller 1123 may be employed in some implementations. Examples of programs or sections of programs for this purpose include a substrate positioning program, a process gas control program, a pressure control program, a heater control program, a cooler control program, and a plasma control program.

[0177] A substrate positioning program may include program code for process tool components that are used to load and orientate wafer 1107 on pedestal 1121 and to control the spacing between wafer 1107 and other parts of multi-station processing tool 1100.

[0178] A process gas control program may include code for controlling one or more precursors for forming a film on a substrate, for controlling a gas composition and flow rates of reactive gas(es) to treat a film on a substrate, for controlling a halogen-containing gas composition (e.g., HBr or HC1 gas as described herein) and flow rates and optionally for flowing gas into one or more process stations prior to deposition in order to stabilize the pressure in the process station. A cooling control program may include code for controlling a flow rate of conductive cooling fluid, e.g., clean dry air or CDA, through a cooling unit used to extract heat from a pedestal (e.g., pedestal 1121) and / or a showerhead of processing chamber 1115, and, thereby, transfer such thermal energy to, for instance, a waste heat capturing, storage, recycling, and / or disposing system. The flow of the cooling fluid through the cooling unit may also extract heat from wafer 1107. The tool, or system, 1100 also has a representational coolant source 1155 which may be a source of clean dry air (CDA) that is fluidically connected to each pedestal in stations 1-4. In some implementations, the coolant source 1155 may be a common source for multiple pedestals. A pressure control program may include code for controlling the pressure in the process station by regulating, for example, a throttle valve in the exhaust system of the process station, a gas flow into the process station, etc. A temperature control program may include code for controlling a temperature in the process station and / or a temperature of a pedestal by adjusting, for example, one or more heaters in the pedestal. Alternatively, the temperature control program may control delivery of a heat transfer gas (such as helium) to the substrate. A plasma control program may include code for setting RF power levels applied to the process electrodes in one or more process stations in accordance with the implementations herein.

[0179] In some implementations, there may be a user interface associated with system controller 1123. The user interface may include a display screen, graphical softwaredisplays of the apparatus and / or process conditions, and user input devices such as pointing devices, keyboards, touch screens, microphones, etc.

[0180] In some implementations, parameters adjusted by system controller 1123 may relate to process conditions. Non-limiting examples include process gas composition and flow rates, temperature, pressure, plasma conditions (such as RF bias power levels), etc. These parameters may be provided to the user in the form of a recipe, which may be entered utilizing the user interface.

[0181] Signals for monitoring the process may be provided by analog and / or digital input connections of system controller 1123 from various process tool sensors. The signals for controlling the process may be output on the analog and digital output connections of process tool 1100. Non-limiting examples of process tool sensors that may be monitored include mass flow controllers, pressure sensors (such as manometers), thermocouples, etc. Appropriately programmed feedback and control algorithms may be used with data from these sensors to maintain process conditions.

[0182] System controller 1123 may provide program instructions for implementing the above-described deposition processes. The program instructions may control a variety of process parameters, such as DC power level, RF bias power level, pressure, temperature, etc. The instructions may control the parameters to operate dry development and / or etch processes according to various implementations described herein. The system controller 1123 may also provide program instructions for implementing the above-described precursor concentration monitoring process. The program instructions may control the parameters, such as time, temperature, and / or IR power, visible light power, or UV power to provide IR radiation, visible light radiation, or UV radiation to one or more precursors, cause one or more IR sensors, visible light sensor, or UV sensors to receive and generate signals for absorption characteristics of one or more precursors, and monitor the concentrations of one or more precursors.

[0183] The system controller 1123 can include one or more memory devices and one or more processors configured to execute the instructions so that the apparatus will perform a method in accordance with disclosed implementations. Machine-readable media containing instructions for controlling process operations in accordance with disclosed implementations may be coupled to the system controller 1123.

[0184] In some implementations, the system controller 1123 is part of a system, which may be part of the above-described examples. Such systems can include semiconductor processing equipment, including a processing tool or tools, chamber or chambers, a platformor platforms for processing, and / or specific processing components (a wafer pedestal, a gas flow system, etc.). These systems may be integrated with electronics for controlling their operation before, during, and after processing of a semiconductor wafer or substrate. The electronics may be referred to as the “controller,” which may control various components or subparts of the system or systems. The system controller 1123, depending on the processing conditions and / or the type of system, may be programmed to control any of the processes disclosed herein, including the delivery of processing gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings, RF matching circuit settings, frequency settings, flow rate settings, fluid delivery settings, positional and operation settings, wafer transfers into and out of a tool and other transfer tools and / or load locks connected to or interfaced with a specific system.

[0185] Broadly speaking, the system controller 1123 may be defined as electronics having various integrated circuits, logic, memory, and / or software that receive instructions, issue instructions, control operation, enable cleaning operations, enable endpoint measurements, and the like. The integrated circuits may include chips in the form of firmware that store program instructions, digital signal processors (DSPs), chips defined as application specific integrated circuits (ASICs), and / or one or more microprocessors, or microcontrollers that execute program instructions (e.g., software). Program instructions may be instructions communicated to the system controller 1123 in the form of various individual settings (or program files), defining operational parameters for carrying out a particular process on or for a semiconductor wafer or to a system. The operational parameters may, in some implementations, be part of a recipe defined by process engineers to accomplish one or more processing steps during the fabrication of one or more layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits, and / or dies of a wafer.

[0186] The system controller 1123, in some implementations, may be a part of or coupled to a computer that is integrated with, coupled to the system, otherwise networked to the system, or a combination thereof. For example, the system controller 1123 may be in the “cloud” or all or a part of a fab host computer system, which can allow for remote access of the wafer processing. The computer may enable remote access to the system to monitor current progress of fabrication operations, examine a history of past fabrication operations, examine trends or performance metrics from a plurality of fabrication operations, to change parameters of current processing, to set processing steps to follow a current processing, or to start a new process. In some examples, a remote computer (e.g. a server) can provideprocess recipes to a system over a network, which may include a local network or the Internet. The remote computer may include a user interface that enables entry or programming of parameters and / or settings, which are then communicated to the system from the remote computer. In some examples, the system controller 1123 receives instructions in the form of data, which specify parameters for each of the processing steps to be performed during one or more operations. It should be understood that the parameters may be specific to the type of process to be performed and the type of tool that the system controller 1123 is configured to interface with or control. Thus, as described above, the system controller 1123 may be distributed, such as by including one or more discrete controllers that are networked together and working towards a common purpose, such as the processes and controls described herein. An example of a distributed controller for such purposes would be one or more integrated circuits on a chamber in communication with one or more integrated circuits located remotely (such as at the platform level or as part of a remote computer) that combine to control a process on the chamber.

[0187] Without limitation, example systems may include a plasma etch chamber or module, a deposition chamber or module, a spin-rinse chamber or module, a metal plating chamber or module, a clean chamber or module, a bevel edge etch chamber or module, a physical vapor deposition (PVD) chamber or module, a chemical vapor deposition (CVD) chamber or module, an ALD chamber or module, an atomic layer etch (ALE) chamber or module, an ion implantation chamber or module, a track chamber or module, an EUV lithography chamber (scanner) or module, a dry development chamber or module, and any other semiconductor processing systems that may be associated or used in the fabrication and / or manufacturing of semiconductor wafers.

[0188] As noted above, depending on the process step or steps to be performed by the tool, the system controller 1123 might communicate with one or more of other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, neighboring tools, tools located throughout a factory, a main computer, another controller, or tools used in material transport that bring containers of wafers to and from tool locations and / or load ports in a semiconductor manufacturing factory.

[0189] Aspects of the present disclosure may be implemented in a chamber which may be part of a substrate processing system. The substrate processing system may further include one or more additional substrate processing tools used to process substrates. Figure 12 illustrates a functional block diagram of an example of a substrate processing system including multiple substrate processing tools and a storage buffer according to someimplementations. A substrate processing system 1200 includes one or more substrate processing tools 1202 (substrate processing tools 1202a and 1202b are shown for illustration purposes) and substrate buffer 1230 or other substrate storage. Each of the substrate processing tools 1202a and 1202b includes a plurality of processing chambers 1204a, 1204b, 1204c, etc. (collectively processing chambers 1204). For example only, each of the processing chambers 1204 may be configured to perform a substrate treatment. In another example, each of the processing chambers 1204 may be configured to perform film deposition. In some examples, the substrates may be loaded into one of the processing chambers 1204, processed, and then moved to one or more other ones of the processing chambers 1204 and / or removed from the substrate processing tool 1200 (e.g., if all perform the same treatment).

[0190] Substrates to be processed are loaded into the substrate processing tools 1202a and 1202b via ports of a loading station of an atmosphere-to-vacuum (ATV) transfer module 1208. In some examples, the ATV transfer module 1208 includes an equipment front end module (EFEM). The substrates are then transferred into one or more of the processing chambers 1204. For example, a transfer robot 1212 is arranged to transfer substrates from loading stations 416 to load locks 1220. A vacuum transfer robot 1224 of a vacuum transfer module 428 is arranged to transfer substrates from the load locks 1220 to the various processing chambers 1204.

[0191] After processing in one or more of the substrate processing tools 1202a and 1202b, the substrates may be transported outside of a vacuum environment. For example, the substrates may be moved to a location for storage (such as the substrate buffer 1230). In other examples, the substrates may be moved directly from the substrate processing tool to another substrate processing tool for further processing or from the storage buffer 1230 to another substrate processing tool for further processing.

[0192] Exposure of the substrate to ambient conditions may cause defects or otherwise adversely impact downstream processing. A sacrificial protective layer can be added to the substrate prior to exposure to ambient conditions. In some examples, the sacrificial protective layer is applied in the substrate processing tool prior to transferring the substrate to the substrate buffer for storage or to another substrate processing tool. In other examples, the sacrificial protective layer is applied in another processing chamber (not associated with the substrate processing tool.

[0193] Prior to performing another treatment on the substrate, the sacrificial protective layer is removed. For example, the substrate may be transferred to the substrate processingtool 1202b after a period of storage in the storage buffer 1230 or after processing in the substrate processing tool 1202a. The sacrificial protective layer may be removed in one of the processing chambers in the substrate processing tool 1202b, or another processing chamber (not associated with the substrate processing tool 1202b). In some implementations, the sacrificial protective layer is removed in a load lock 1220.

[0194] In various implementations, a system controller is employed to control process conditions during processing. The controller will typically include one or more memory devices and one or more processors. A processor may include a CPU or computer, analog and / or digital input / output connections, stepper motor controller boards, etc.

[0195] The controller may control all the activities of a substrate processing apparatus. The system controller executes system control software, including sets of instructions for controlling the timing, mixture of gases, chamber pressure, chamber temperature, wafer temperature, wafer chuck or pedestal position, plasma power, and other parameters of a particular process. Other computer programs stored on memory devices associated with the controller may be employed in some implementations. Various aspects of the controller are discussed earlier herein and are not repeated for the sake of brevity.Conclusion

[0196] It is understood that the examples and implementations described herein are for illustrative purposes only and that various modifications or changes in light thereof will be suggested to persons skilled in the art. Although various details have been omitted for clarity’s sake, various design alternatives may be implemented. Therefore, the present examples are to be considered as illustrative and not restrictive, and the disclosure is not to be limited to the details given herein, but may be modified within the scope of the disclosure.

Claims

CLAIMS1. A method of processing a semiconductor substrate, the method comprising:providing a semiconductor substrate having a photopatterned organo-metal oxide resist layer over an etch stop layer;developing the photopattemed organo-metal oxide resist layer to form a resist mask of metal oxide mandrels;depositing a layer of a spacer material on horizontal surfaces and sidewalls of the metal oxide mandrels;removing a portion of the spacer material from at least the horizontal surfaces of the metal oxide mandrels; andremoving the metal oxide mandrels to form a plurality of spacers used as a mask to etch at least the etch stop layer.

2. The method of claim 1, further comprising:depositing an organo-metal oxide EUV-sensitive resist material on the semiconductor substrate, wherein the organo-metal oxide EUV-sensitive resist material is configured to be exposed to EUV radiation to form the photopattemed organo-metal oxide resist layer.

3. The method of claim 2, wherein depositing the organo-metal oxide EUV-sensitive resist material comprises vapor depositing the organo-metal oxide EUV-sensitive resist material.

4. The method of claim 2, wherein depositing the organo-metal oxide EUV-sensitive resist material comprises vapor depositing two or more layers of organo-metal oxide EUV-sensitive resist layers, wherein each of the two or more layers comprises varying amounts of cross -linking.

5. The method of claim 1, wherein the photopattemed organo-metal oxide resist layer has a thickness equal to or greater than about 30 nm.

6. The method of claim 1, wherein the layer of spacer material is selected from a group consisting of tungsten, tungsten nitride, tungsten oxide, molybdenum, molybdenum oxide, molybdenum nitride, aluminum oxide, zirconium oxide, and hafnium oxide.

7. The method of claim 1, wherein the layer of spacer material is selected from a group consisting of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, silicon oxycarbonitride, silicon carbonitride, and titanium oxide.

8. The method of claim 1, wherein the etch stop layer comprises a silicon-containing material.

9. The method of claim 1, wherein developing the photopattemed organo-metal oxide resist layer comprises dry developing the photopatterned organo-metal oxide resist layer.

10. The method of claim 1, further comprising:exposing the metal oxide mandrels to one or more halogen gases to harden the metal oxide mandrels.

11. The method of claim 1, further comprising:exposing the metal oxide mandrels to a reactive ion beam comprising at least one reactive gas to reduce sidewall roughness in the metal oxide mandrels.

12. The method of claim 11, wherein the reactive ion beam is an angled reactive ion beam that comprises hydrogen, a halogen-containing gas, a hydrocarbon gas, a nitrogencontaining gas, an oxygen-containing gas, or a combination thereof.

13. The method of claim 1, further comprising:etching the etch stop layer using the plurality of spacers as the mask.

14. The method of claim 1, wherein removing the portion of the spacer material comprises etching the portion of the spacer material using a halogen-based chemistry.

15. The method of claim 1, wherein removing the metal oxide mandrels comprises etching the metal oxide mandrels using a hydrogen-based chemistry.

16. A method of processing a semiconductor substrate, the method comprising:dry depositing a first organo-metal oxide EUV-sensitive resist material over an etch stop layer on the semiconductor substrate, wherein the first organo-metal oxide EUV-sensitive resist material is configured to be exposed to EUV radiation to form a first photopatterned organo-metal oxide resist layer;dry developing the first photopattemed organo-metal oxide resist layer to form first a resist mask of first metal oxide mandrels arranged in a first direction;conformally depositing a layer of first spacer material on horizontal surfaces and sidewalls of the first metal oxide mandrels;removing a portion of the first spacer material from at least the horizontal surfaces of the first metal oxide mandrels;removing the first metal oxide mandrels to form a plurality of first spacers; and etching the etch stop layer using the plurality of first spacers as the mask to form patterned etch stop features.

17. The method of claim 16, further comprising:removing the plurality of first spacers;depositing gapfill material in gaps between the patterned etch stop features; dry depositing a second organo-metal oxide EUV-sensitive resist material over the gapfill material and patterned etch stop features, wherein the second organo-metal oxide EUV-sensitive resist material is configured to be exposed to EUV radiation to form a second photopatterned organo-metal oxide resist layer;dry developing the second photopattemed organo-metal oxide resist layer to form a second resist mask of second metal oxide mandrels arranged in a second direction different from the first direction;conformally depositing a layer of second spacer material on horizontal surfaces and sidewalls of the second metal oxide mandrels;removing a portion of the second spacer material from at least the horizontal surfaces of the second metal oxide mandrels; andremoving the second metal oxide mandrels to form a plurality of second spacers used as a mask to etch an underlying layer.

18. The method of claim 17, wherein each of the first organo-metal oxide EUV-sensitive resist material and the second organo-metal oxide EUV- sensitive resist material has a thickness equal to or greater than about 30 nm.

19. The method of claim 16, further comprising:exposing the first metal oxide mandrels to one or more halogen gases to harden the first metal oxide mandrels.

20. The method of claim 16, further comprising:exposing the first metal oxide mandrels to a reactive ion beam comprising at least one reactive gas to reduce sidewall roughness in the first metal oxide mandrels.

21. The method of claim 16, wherein dry depositing a first organo-metal oxide EUV-sensitive resist material comprises vapor depositing two or more layers of first organo-metal oxide EUV-sensitive resist layers, wherein each of the two or more layers comprises varying amounts of cross-linking.