Multi-layer rotationally molded articles

The multi-layer rotationally molded container with a crosslinked polyethylene outer layer and polyoxymethylene polymer lining addresses fuel permeation and bonding issues, providing superior fuel resistance and mechanical strength for diverse applications.

WO2026236054A1PCT designated stage Publication Date: 2026-11-12CELANESE INTERNATIONAL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/026253
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-06
Filing Date
2026-05-01
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing fuel tanks, particularly those with a nylon-based inner barrier layer and cross-linked polyethylene outer layer, face issues with fuel permeation sensitivity to chemical composition changes, degradation, and interlayer bonding challenges, leading to increased hydrocarbon permeation and delamination.

Method used

A multi-layer rotationally molded container with a crosslinked polyethylene outer layer and a polyoxymethylene polymer lining layer, combined with impact modifiers, exhibits improved fuel permeation resistance, mechanical strength, and strong adhesion, using a thickness ratio of 1.5:1 to 5:1 and a total wall thickness of 6-8 mm.

Benefits of technology

The container achieves fuel permeation of less than 2.5 g/m² per day at 40°C and multiaxial impact strength greater than 40 ft-lb-f, with excellent adhesion and durability, suitable for various fuel types and applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026026253_12112026_PF_FP_ABST
    Figure US2026026253_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Multi-layered, seamless and rotationally molded containers are disclosed. The containers include at least two polymer layers. In one aspect, the container includes an outer layer made from a high impact strength polymer such as a crosslinked polyethylene polymer. The inside layer is made from a polyoxymethylene polymer composition not only having good impact strength resistance but also possessing extremely low permeability characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

Attorney Docket No.: CICT-1562-PCT (2025P0008)MULTI-LAYER ROTATIONALLY MOLDED ARTICLESCROSS REFERENCE TO RELATED APPLICATIONS

[0001] This application claims priority to the benefit of U.S. Provisional Application No. 63 / 800,674, filed May 6, 2025, which is expressly incorporated herein by reference in its entirety.BACKGROUND

[0002] Fuel storage systems, particularly for use in automotive, marine, and industrial applications, are subject to increasingly stringent environmental regulations governing the emission of volatile organic compounds (VOCs), including fuel vapor permeation. Traditional single-layer polyethylene fuel tanks, while cost-effective and durable, exhibit unacceptably high levels of hydrocarbon permeation, making them unsuitable for modem regulatory requirements such as those imposed by the U.S. Environmental Protection Agency (EPA) and the California Air Resources Board (CARB).

[0003] To address these concerns, two-layer rotationally molded tanks have been developed, typically comprising an inner barrier layer of nylon (e.g., Nylon 6 or Nylon 12) and an outer structural layer of cross-linked polyethylene (XLPE). While this configuration offers improved fuel permeation resistance compared to single-layer XLPE tanks, it still suffers from several significant limitations.

[0004] First, the permeation performance of nylon-based barriers, although superior to polyethylene alone, remains sensitive to the chemical composition of the stored fuel. Ethanol-blended fuels (e.g., E10-E85), biodiesel, and other oxygenated or reformulated fuel types have been observed to degrade or swell nylon materials over time. This degradation can reduce barrier effectiveness and ultimately result in increased hydrocarbon permeation.

[0005] Second, the chemical dissimilarity between nylon and XLPE presents considerable challenges in achieving a strong and stable interlayer bond. The lack of inherent compatibility between these polymers frequently leads to delamination, blistering, or separation under thermal cycling, mechanical stress, or prolonged fuel exposure. To mitigate this, manufacturers often rely on mechanical interlocking or the use of adhesion-promoting additives, which add complexity, increase manufacturing cost, and still may not ensure long-term durability.Attorney Docket No.: CICT-1562-PCT (2025P0008)

[0006] Accordingly, there remains a need for an improved multi-layer fuel tank design that maintains low fuel permeation across a wide range of fuel types, while also addressing the material compatibility and bonding issues that currently limit the performance and reliability of existing solutions.SUMMARY

[0007] The present disclosure is directed to a multi-layer article, particularly a seamless rotationally molded container, having improved resistance to fuel permeation, high mechanical strength, and excellent interlayer adhesion. The container comprises a container wall formed from an outer layer and a lining layer that is adjacent to and in contact with the outer layer. The outer layer is made from a polyethylene polymer, which may be crosslinked, and the lining layer comprises a polymer composition containing a polyoxymethylene polymer having a melt flow rate of less than about 12 g / 10 min. The polymer composition optionally includes one or more impact modifiers comprising an elastomer.

[0008] In one aspect, the outer layer and lining layer have a thickness ratio from about 1.5:1 to about 5:1. In some embodiments, the thickness ratio may be from about 1.75: 1 to about 4.25: 1. The total wall thickness of the container may range from about 6 mm to about 8 mm, and the lining layer may have a thickness of less than about 2.75 mm, such as less than about 1.75 mm.

[0009] The multi-layer container exhibits high durability and strength, with a multiaxial impact of greater than 40 ftlb-f at 23°C, and in some embodiments, greater than 80 ftlb-f at 23°C. The wall of the container also demonstrates superior barrier properties, with a fuel permeation of less than 2.5 g / m2per day at 40°C, as determined in accordance with SAE Test J2665, and in certain embodiments, less than 1.4 g / m2per day.

[0010] The polyoxymethylene polymer of the lining layer may have a melt flow rate of from about 1.5 g / 10 min to about 9 g / 10 min. In certain embodiments, the polymer composition contains a blend of the polyoxymethylene polymer with impact modifiers comprising thermoplastic polyurethane elastomers and optionally thermoplastic copolyester elastomers. The polymer composition may include a thermoplastic elastomer impact modifier in an amount of from about 4% by weight to about 27% by weight, with the polyoxymethylene polymer present in an amount of at least about 55% by weight. The polymer composition may further include aAttorney Docket No.: CICT-1562-PCT (2025P0008)nucleant, such as a terpolymer, and an antioxidant.

[0011] In some embodiments, the polymer composition additionally comprises an acid scavenger, which may include a carboxylic acid salt, such as calcium citrate, calcium propionate, or mixtures thereof. The acid scavenger may be present in an amount from about 0.001 % by weight to about 1 % by weight.

[0012] The lining and outer layers are configured to display strong adhesion, with an adhesive shear force as measured by ASTM D903 of greater than about 120 lbs, such as greater than about 300 lbs, greater than about 400 lbs, or greater than about 450 lbs.

[0013] The container may be configured for use as a fuel tank, hydraulic oil tank, compressed gas tank, water tank, or diesel exhaust fluid tank, and may have a volume ranging from about 4 gallons to about 500 gallons, such as from about 10 gallons to about 110 gallons. In some embodiments, the lining layer has a density according to ISO Test 1183 of greater than 1 g / cc, such as greater than about 1.1 g / cc, about 1.2 g / cc, or about 1.3 g / cc, and less than about 1.6 g / cc.

[0014] In another aspect, a multi-layer article is provided comprising a seamless rotationally molded container wherein the outer layer comprises a crosslinked polyethylene polymer and the lining layer comprises a polymer composition including a polyoxymethylene polymer having a melt flow rate of less than about 12 g / 10 min, blended with impact modifiers comprising a thermoplastic polyurethane elastomer in combination with a thermoplastic copolyester elastomer. The container may have a volume of from about 4 gallons to about 500 gallons.

[0015] The outer layer and lining layer may have a thickness ratio from about 1.5:1 to about 5:1 , and the total wall thickness may range from about 5 mm to about 8 mm. The container may exhibit a multiaxial impact of greater than 40 ftlb-f at 23°C and a wall permeation of less than 2.5 g / m2per day at 40°C according to SAE Test J2665.

[0016] Other features and aspects of the present disclosure are discussed in greater detail below.BRIEF DESCRIPTION OF THE DRAWINGS

[0017] A full and enabling disclosure of the present disclosure is set forth more particularly in the remainder of the specification, including reference to the accompanying figures, in which:Attorney Docket No.: CICT-1562-PCT (2025P0008)Figure 1 is a perspective view of one embodiment of a container made in accordance with the present disclosure;Figure 2 is a perspective view of another embodiment of a container made in accordance with the present disclosure; andFigure 3 is a cross-sectional view of the container illustrated in Figure 2.

[0018] Repeat use of reference characters in the present specification and drawings is intended to represent the same or analogous features or elements of the present invention.DETAILED DESCRIPTION

[0019] It is to be understood by one of ordinary skill in the art that the present discussion is a description of exemplary embodiments only and is not intended as limiting the broader aspects of the present disclosure.

[0020] The present disclosure is generally directed to multi-layer and seamless rotationally molded containers. The containers can be used in all different types of applications. For instance, containers made according to the present disclosure can comprise bulk material storage containers, chemical tanks, transport bins, water and feed tanks, fertilizer storage tanks, floating docks and pontoons, rainwater collection tanks, trash and recycling bins, septic tanks and wastewater containers, insulated food and beverage coolers, food storage totes or bins, and the like. In one embodiment, the container made according to the present disclosure can be a fuel tank designed to hold a liquid or gas fuel. Containers made according to the present disclosure, for instance, not only display excellent permeability properties but also display very high impact strength properties.

[0021] In the past, rotationally molded containers were made utilizing a crosslinked polyethylene polymer as the outer layer and combined with an inner layer made from a polyamide, ethylene vinyl alcohol, or a fluoropolymer.Fluoropolymers, however, are subject to governmental scrutiny and their continued use is being discouraged. In addition, fluoropolymers and ethylene vinyl alcohol provide no structural benefit to the container. Polyamide inner layers can provide some structural benefit but do suffer from specific fuel permeation issues and can lead to defects in the product due to moisture absorption and viscosity control issues.

[0022] The present disclosure is directed to rotationally molded containers inAttorney Docket No.: CICT-1562-PCT (2025P0008)which an outer polymer layer with good impact strength is combined with a polyoxymethylene polymer as the inner layer of the container. The polyoxymethylene polymer composition has extremely low permeability characteristics in combination with excellent impact resistance, especially when combined with the outer layer. In one aspect, the polyoxymethylene polymer can be combined with one or more impact modifiers in order to optimize properties for rotationally molded articles.

[0023] The use of a polyoxymethylene polymer for rotational molding processes can offer various advantages and benefits. Polyoxymethylene copolymers, for instance, possess a linear structure with a highly crystalline quality that provides a variety of characteristics including outstanding wear, long-term fatigue, toughness and creep resistance as well as excellent resistance to moisture, solvents, and strong alkalis. The chemical structure of polyoxymethylene polymers provides a higher stability to thermal and oxidative degradation compared to many different polymers. The use of a polyoxymethylene copolymer is, in fact, more thermally stable and resistant to degradation than a polyoxymethylene homopolymer. The polyoxymethylene polymer is formulated to increase the impact resistance while maintaining excellent permeability characteristics. The polymer composition of the present disclosure, for instance, can be used to produce containers or hollow vessels for containing all different types of fluids, including compressed gases and fuels. The containers have excellent impact resistance while also being relatively impermeable to fuel vapors and other gases.

[0024] Containers made according to the present disclosure are particularly well suited for producing fuel tanks that are designed to contain liquid or gaseous fuels. The fuels can include, for example, gasoline, diesel fuel, marine fuel, and compressed gases such as hydrogen, and the like.

[0025] Referring to FIG. 1, one embodiment of a fuel tank 10 made in accordance with the present disclosure is shown. The fuel tank 10 is made from at least two different layers of material in which one of the layers is comprised of a polyoxymethylene polymer composition. The polyoxymethylene polymer composition, for instance, can contain a polyoxymethylene polymer in combination with at least one thermoplastic elastomer. The fuel tank 10 is formed through a rotational molding process. During rotational molding, a pre-measured amount ofAttorney Docket No.: CICT-1562-PCT (2025P0008)a polymer resin is placed inside a hollow mold. The mold can be made of aluminum or steel and can be in the shape of the tank 10 as shown in FIG. 1. The mold is closed and moved into an oven. While inside an oven, the mold rotates slowly on two perpendicular axis (bi-axial rotation). As it rotates, the polymer resin melts and sticks evenly to the walls of the mold forming a consistent layer. In accordance with the present disclosure, after an outer layer is formed on the mold, another charge of polymer resin is then deposited in the mold for forming a second layer. After the polymer compositions have melted and coated the mold interior, the mold is cooled, such as with air, mist, or water spray, while still rotating. Once cooled, the mold is opened and the finished hollow part is removed. Of particular advantage, containers, such as fuel tank 10, can be made that are seamless meaning that different parts of the container are not welded together. Rotational molding is particularly well suited for producing large containers and tanks.

[0026] As shown in FIG. 1, the fuel tank 10 can include a spout 14 for receiving a fluid. The spout 14 can be threaded for receiving a fuel cap 12. The fuel tank 10 further includes at least one wall 16. In accordance with the present disclosure, the wall 16 is multi-layered and includes at least two layers of different polymer compositions. In the embodiment illustrated in FIG. 1, the fuel tank 10 includes a top, a bottom, and four side walls.

[0027] The fuel tank 10, as shown in FIG. 1, is designed for vehicle or automotive applications. Referring to FIG. 2, another fuel tank 20 made in accordance with the present disclosure is shown. The fuel tank 20 in FIG. 2 is particularly well suited for marine applications. For instance, the fuel tank 20 can be incorporated into a boat or shipping vessel.

[0028] The fuel tank 20, similar to FIG. 1, includes a spout 24 covered by a removable cap 22. The fuel tank 20 is made from at least one wall 26. For instance, the fuel tank 20 can include a top, a bottom, and four side walls.

[0029] Referring to FIG. 3, a cross-sectional view of the fuel tank 20 as shown in FIG. 2 is illustrated. The fuel tank 20 includes walls 26 made from two layers of polymeric materials. In particular, the wall 26 includes an exterior polymer layer 30 that is adjacent to an interior polymer layer 32. In accordance with the present disclosure, the exterior layer 30 is made from a polymer composition having high impact strength resistance. For instance, the exterior layer 30 can comprise aAttorney Docket No.: CICT-1562-PCT (2025P0008)crosslinked polyethylene polymer.

[0030] The interior layer 32, on the other hand, is comprised of a polyoxymethylene polymer composition. The polyoxymethylene polymer composition can comprise a polyoxymethylene polymer combined with an impact modifier and possibly other components. The interior layer 32 can further bolster the impact resistance of the fuel tank 20 while providing extremely low permeability properties and chemical resistance.

[0031] In the embodiment illustrated in FIG. 3, the fuel tank 20 is made from the two layers 30 and 32. In alternative embodiments, however, the fuel tank 20 or container can contain three layers, four layers, five layers, or six layers. For instance, in one embodiment, the container can contain multiple layers of the crosslinked polyethylene polymer and / or multiple layers of the polyoxymethylene polymer composition. In still another embodiment, the container can include an interior layer in which the polyoxymethylene polymer layer is positioned between the exterior layer and the interior layer.

[0032] Although fuel tanks are illustrated in FIGS. 1 and 2, all different types of containers can be made in accordance with the present disclosure. The containers can comprise hydraulic tanks, water tanks, compressed gas tanks, thermal coolers, diesel exhaust fluid tanks, and the like. Multi-layer containers made in accordance with the present disclosure generally have a volume of greater than about two gallons. For instance, the containers or tanks can have a volume of greater than about 5 gallons, such as greater than about 15 gallons, such as greater than about 20 gallons, such as greater than about 25 gallons, such as greater than about 30 gallons, such as greater than about 35 gallons, such as greater than about 40 gallons, such as greater than about 45 gallons, such as greater than about 50 gallons, such as greater than about 55 gallons, such as greater than about 60 gallons, and generally less than about 500 gallons, such as less than about 200 gallons, such as less than about 150 gallons, such as less than about 100 gallons.

[0033] Even when constructing large volume tanks, the thickness of the wall of the tank is relatively thin. For instance, the wall can have a thickness of less than about 14 mm, such as less than about 12 mm, such as less than about 10 mm, such as less than about 8 mm, and greater than about 3 mm, such as greater thanAttorney Docket No.: CICT-1562-PCT (2025P0008)about 4 mm, such as greater than about 5 mm, such as greater than about 6 mm. For example, in one embodiment, the wall thickness can be from about 6 mm to about 9 mm, such as from about 6 mm to about 8 mm.

[0034] Containers made according to the present disclosure can have excellent permeability characteristics in combination with excellent impact resistance. The permeability of the container or of the container wall can be tested according to SAE Test J2665 (latest version as of 2021 ). The SAE Test J2665 tests the permeability of the material with a test fuel comprising 10% ethanol, 45% toluene, and 45% iso-octane. Determination of the steady state flux is reported in gmm / m2per day and is carried out per SAE Test J2665, Section 10. Containers made according to the present disclosure can have a permeation of less than about 2.5 g / m2per day at 40°C, such as less than about 2 g / m2per day, such as less than about 1.8 g / m2per day, such as less than about 1.6 g / m2per day, such as less than about 1.4 g / m2per day, and can be as low as 0 g / m2per day at 40°C.

[0035] The wall can also be tested according to Test Method US EPA 40 CFR Part 1060.520 and can display a permeation of less than about 1.1 g / m2 / day, such as less than about 0.9 g / m2 / day, such as less than about 0.7 g / m2 / day, such as less than about 0.5 g / m2 / day, such as less than about 0.3 g / m2 / day (and generally greater than about 0.01 g / m2 / day).

[0036] Containers made according to the present disclosure can be tested for multiaxial impact strength according to ARM low temperature impact test (V4) at 23°C (t=3mm). The multiaxial impact strength can be greater than about 20 ft-lbs, such as greater than about 30 ft-lbs, such as greater than about 40 ft-lbs, such as greater than about 50 ft-lbs, such as greater than about 60 ft-lbs, such as greater than about 70 ft-lbs, such as greater than about 80 ft-lbs, such as greater than about 85 ft-lbs, such as greater than about 90 ft-lbs, such as greater than about 95 ft-lbs, such as greater than about 100 ft-lbs, such as greater than about 110 ft-lbs, such as greater than about 120 ft-lbs, such as greater than about 130 ft-lbs, such as greater than about 140 ft-lbs, and generally less than about 500 ft-lbs.

[0037] The polyoxymethylene polymer composition can also display a Charpy notched impact strength at 23°C of greater than about 12 kJ / m2, such as greater than about 14 kJ / m2, such as greater than about 16 kJ / m2, such as greater thanAttorney Docket No.: CICT-1562-PCT (2025P0008)about 18 kJ / m2, such as greater than about 20 kJ / m2, such as greater than about 22 kJ / m2, such as greater than about 24 kJ / m2, and generally less than about 200 kJ / m2. Charpy notched impact strength can be measured according to ISO Test 179 using an injection molded specimen.

[0038] The polyoxymethylene polymer composition of the present disclosure is particularly well suited for use in rotational molding applications. For instance, the polyoxymethylene polymer composition can form a layer of the tank or container with low voids. The polyoxymethylene polymer layer, for instance, can have a relatively high density. For instance, the density can be greater than about 1.2 g / cm3, such as greater than about 1.25 g / cm3, such as greater than about 1.3 g / cm3. The density is generally less than about 2 g / cm3, such as less than about 1.6 g / cm3.

[0039] As described above, at least one layer of the container or tank of the present disclosure is formed from a polyoxymethylene polymer composition. The polyoxymethylene polymer composition generally contains a polyoxymethylene polymer combined with one or more impact modifiers in addition to various other components. The polyoxymethylene polymer can be a polyoxymethylene copolymer.

[0040] The preparation of the polyoxymethylene polymer can be carried out by polymerization of polyoxymethylene-forming monomers, such as trioxane or a mixture of trioxane and a cyclic acetal such as dioxolane in the presence of a molecular weight regulator, such as a glycol. According to one embodiment, the polyoxymethylene is a homo- or copolymer which comprises at least 50 mol.%, such as at least 75 mol.%, such as at least 90 mol.% and such as even at least 97 mol.% of -CH2O-repeat units.

[0041] In one embodiment, a polyoxymethylene copolymer is used. The copolymer can contain from about 0.1 mol.% to about 20 mol.% and in particular from about 0.5 mol.% to about 10 mol.% of repeat units that comprise a saturated or ethylenically unsaturated alkylene group having at least 2 carbon atoms, or a cycloalkylene group, which has sulfur atoms or oxygen atoms in the chain and may include one or more substituents selected from the group consisting of alkyl cycloalkyl, aryl, aralkyl, heteroaryl, halogen or alkoxy. In one embodiment, a cyclic ether or acetal is used that can be introduced into the copolymer via a ring-openingAttorney Docket No.: CICT-1562-PCT (2025P0008)reaction.

[0042] Preferred cyclic ethers or acetals are those of the formula:in which x is 0 or 1 and R2is a C2 -C4 -alkylene group which, if appropriate, has one or more substituents which are Ci-C4-akyl groups, or are Ci-C4-alkoxy groups, and / or are halogen atoms, preferably chlorine atoms. Merely by way of example, mention may be made of ethylene oxide, propylene 1 ,2-oxide, butylene 1 ,2-oxide, butylene 1,3-oxide, 1,3-dioxane, 1 ,3-dioxolane, and 1,3-dioxepan as cyclic ethers, and also of linear oligo- or polyformals, such as polydioxolane or polydioxepan, as comonomers. It is particularly advantageous to use copolymers composed of from 99.5 to 95 mol.% of trioxane and of from 0.5 to 5 mol.%, such as from 0.5 to 4 mol.%, of one of the above-mentioned comonomers.

[0043] In one particular aspect of the present disclosure, the polyoxymethylene copolymer incorporated into the powder composition contains a relatively low amount of comonomer. For example, the polyoxymethylene copolymer can contain a comonomer, such as dioxolane, in an amount less than about 5% by weight, such as in an amount less than about 2% by weight, such as in an amount less than about 1.5% by weight, such as in an amount less than about 1 % by weight, such as in an amount less than about 0.75% by weight, such as in an amount less than about 0.7% by weight. The comonomer content is generally greater than about 0.3% by weight, such as greater than about 0.5% by weight.

[0044] The polymerization can be effected as precipitation polymerization or in the melt. By a suitable choice of the polymerization parameters, such as duration of polymerization or amount of molecular weight regulator, the molecular weight and hence the MVR value of the resulting polymer can be adjusted.

[0045] The polyoxymethylene polymer incorporated into the polymer composition can have various different terminal groups or end groups depending upon the particular application and the other components contained in the composition. In one aspect, the polyoxymethylene polymer is relatively thermally stable. For instance, the polyoxymethylene polymer can contain hemiformal groups in an amount less than about 2 mol%, such as in an amount less thanAttorney Docket No.: CICT-1562-PCT (2025P0008)about 1.5 mol%, such as in an amount less than about 1 mol%, such as in an amount less than about 0.8 mol%, such as in an amount less than about 0.6 mol%.

[0046] The amount of hydroxyl end groups on the polyoxymethylene polymer can depend on whether a polyisocyanate coupling agent is present in the composition. When a polyisocyanate coupling agent is not present, for instance, the polyoxymethylene polymer can have a terminal hydroxyl group content of less than about 10 mmol / kg, such as less than about 8 mmol / kg, such as less than about 6 mmol / kg, such as less than about 4 mmol / kg.

[0047] Alternatively, the polyoxymethylene polymer can contain greater amounts of terminal hydroxyl groups. In one embodiment, the polyoxymethylene polymer has a content of terminal hydroxyl groups of at least 15 mmol / kg, such as at least 18 mmol / kg, such as at least 20 mmol / kg, such as greater than about 25 mmol / kg, such as greater than about 30 mmol / kg, such as greater than about 40 mmol / kg, such as greater than about 50 mmol / kg. The terminal hydroxyl content is generally less than about 300 mmol / kg, such as less than about 200 mmol / kg, such as less than about 100 mmol / kg. In one embodiment, the terminal hydroxyl group content ranges from 18 to 50 mmol / kg. The quantification of the hydroxyl group content in the polyoxymethylene polymer may be conducted by the method described in JP-A-2001-11143.

[0048] In addition to the terminal hydroxyl groups, the polyoxymethylene polymer may also have other terminal groups usual for these polymers. Examples of these are alkoxy groups, formate groups, acetate groups or aldehyde groups. In one aspect, the polyoxymethylene polymer can also contain terminal-NH2 groups. According to one embodiment, the polyoxymethylene is a copolymer which comprises at least 50 mol-%, such as at least 75 mol-%, such as at least 90 mol-% and such as even at least 95 mol-% of -CF -repeat units.

[0049] The polyoxymethylene polymer can have any suitable molecular weight. The molecular weight of the polymer, for instance, can be from about 4,000 grams per mole to about 100,000 g / mol. The polyoxymethylene polymer, for instance, can have a molecular weight of greater than about 10,000 g / mol, such as greater than about 15,000 g / mol, such as greater than about 20,000 g / mol, such as greater than about 30,000 g / mol, such as greater than about 40,000 g / mol, and generally less than about 90,000 g / mol.Attorney Docket No.: CICT-1562-PCT (2025P0008)

[0050] The polyoxymethylene polymer present in the composition can generally have a melt flow index (MFI) ranging from about 0.1 to about 200 g / 10 min, as determined according to ISO 1133 at 190°C and 2.16 kg. In one aspect, however, the polyoxymethylene polymer has a relatively low melt flow index. The lower melt flow index has been found to result in a polymer composition having a larger operating window when used in rotational molding processes. In addition, the lower melt flow rate can lead to better physical properties. For instance, the polyoxymethylene polymer can have a melt flow rate of less than about 12 g / 10 min, such as less than about 10 g / 10 min, such as less than about 8 g / 10 min, such as less than about 7 g / 10 min, such as less than about 5 g / 10 min, such as less than about 4 g / 10 min, such as less than about 3 g / 10 min, such as less than about 2 g / 10 min, such as less than about 1 g / 10 min, and generally greater than about 0.5 g / 10 min, such as greater than about 1 g / 10 min, such as greater than about 2 g / 10 min, such as greater than about 3 g / 10 min, such as greater than about 4 g / 10 min.

[0051] The polyoxymethylene polymer may be present in the polyoxymethylene polymer composition in an amount of at least 40 wt.%, such as at least 45 wt.%, such as at least 55 wt.%, such as at least 60 wt.%, such as at least 70 wt.%, such as at least 80 wt.%. The polyoxymethylene polymer can be present in an amount less than about 96% by weight, such as in an amount less than about 85% by weight, such as in an amount less than about 80% by weight, such as in an amount less than about 75% by weight.

[0052] In accordance with the present disclosure, the polyoxymethylene polymer is combined with one or more impact modifiers. Examples of impact modifiers that may be incorporated into the composition include thermoplastic elastomers, a methacrylate butadiene styrene, a styrene acrylonitrile, and mixtures thereof. In one aspect, the impact modifier can be a core and shell impact modifier. Combinations of different impact modifiers may be used in order to enhance various properties of the polymer composition or of articles made from the composition. For example, the polymer composition can contain two or more thermoplastic elastomers.

[0053] Various different thermoplastic elastomers may be used as the impact modifier. Thermoplastic elastomers well suited for use in the present disclosureAttorney Docket No.: CICT-1562-PCT (2025P0008)are polyester elastomers (TPE-E), thermoplastic polyamide elastomers (TPE-A) and in particular thermoplastic polyurethane elastomers (TPE-ll). The above thermoplastic elastomers have active hydrogen atoms which can be reacted with a coupling reagent and / or the polyoxymethylene polymer. Examples of such groups are urethane groups, amido groups, amino groups or hydroxyl groups. For instance, terminal polyester diol flexible segments of thermoplastic polyurethane elastomers have hydrogen atoms which can react, for example, with isocyanate groups.

[0054] In one particular embodiment, a thermoplastic polyurethane elastomer is used as the impact modifier either alone or in combination with other impact modifiers. The thermoplastic polyurethane elastomer, for instance, may have a soft segment of a long-chain dial and a hard segment derived from a diisocyanate and a chain extender. In one embodiment, the polyurethane elastomer is a polyester type prepared by reacting a long-chain diol with a diisocyanate to produce a polyurethane prepolymer having isocyanate end groups, followed by chain extension of the prepolymer with a diol chain extender. Representative long-chain diols are polyester diols such as poly(butylene adipate)diol, polyethylene adipate)diol and poly(E-caprolactone)diol; and polyether diols such as poly(tetramethylene ether)glycol, polypropylene oxide)glycol and poly(ethylene oxide)glycol. Suitable diisocyanates include 4,4'-methylenebis(phenyl isocyanate), 2,4-toluene diisocyanate, 1 ,6-hexamethylene diisocyanate and 4,4'-methylenebis-(cycloxylisocyanate). Suitable chain extenders are C2-C6 aliphatic dials such as ethylene glycol, 1 ,4-butanediol, 1 ,6-hexanedial and neopentyl glycol. One example of a thermoplastic polyurethane is characterized as essentially poly(adipic acid-co-butylene glycol-co-diphenylmethane diisocyanate).

[0055] In one embodiment, the impact modifier can be a polyester-based thermoplastic polyurethane. The polyester-based thermoplastic polyurethane, for instance, can have a Shore A hardness of from about 80 to about 90, such as from about 83 to about 87. The thermoplastic polyurethane can have a Shore D hardness of from about 33 to about 43, such as from about 35 to about 39.

[0056] In an alternative embodiment, a carbonate-based thermoplastic polyurethane block copolymer can be used. The carbonate-based thermoplastic polyurethane elastomer can have the same Shore A and Shore D hardness rangesAttorney Docket No.: CICT-1562-PCT (2025P0008)as described above.

[0057] In one embodiment, the thermoplastic elastomer may comprise a thermoplastic polyester elastomer. The thermoplastic polyester elastomer can be, for instance, a thermoplastic copolyester elastomer that comprises a thermoplastic ester ether elastomer. In one aspect, the thermoplastic polyester elastomer can be a thermoplastic copolyester elastomer that comprises a block copolymer of polybutylene terephthalate and polyether segments.

[0058] In one embodiment, the polymer composition may contain a segmented thermoplastic copolyester. The thermoplastic polyester elastomer, for example, may comprise a multi-block copolymer. Useful segmented thermoplastic copolyester elastomers include a multiplicity of recurring long chain ester units and short chain ester units joined head to tail through ester linkages. The long chain units can be represented by the formulaO O*‘OGO**CKC—and the short chain units can be represented by the formula? f"“ODO“"CRC’*“where G is a divalent radical remaining after the removal of the terminal hydroxyl groups from a long chain polymeric glycol having a number average molecular weight in the range from about 600 to 6,000 and a melting point below about 55°C., R is a hydrocarbon radical remaining after removal of the carboxyl groups from dicarboxylic acid having a molecular weight less than about 300, and D is a divalent radical remaining after removal of hydroxyl groups from low molecular weight diols having a molecular weight less than about 250.

[0059] The short chain ester units in the copolyetherester provide about 15 to 95% of the weight of the copolyetherester, and about 50 to 100% of the short chain ester units in the copolyetherester are identical.

[0060] The term "long chain ester units" refers to the reaction product of a long chain glycol with a dicarboxylic acid. The long chain glycols are polymeric glycolsAttorney Docket No.: CICT-1562-PCT (2025P0008)having terminal (or nearly terminal as possible) hydroxy groups, a molecular weight above about 600, such as from about 600-6000, a melting point less than about 55°C and a carbon to oxygen ratio about 2.0 or greater. The long chain glycols are generally poly(alkylene oxide) glycols or glycol esters of poly(alkylene oxide) dicarboxylic acids. Any substituent groups can be present which do not interfere with polymerization of the compound with glycol(s) or dicarboxylic acid(s), as the case may be. The hydroxy functional groups of the long chain glycols which react to form the copolyesters can be terminal groups to the extent possible. The terminal hydroxy groups can be placed on end capping glycol units different from the chain, i.e. , ethylene oxide end groups on polypropylene oxide glycol).

[0061] The term "short chain ester units" refers to low molecular weight compounds or polymer chain units having molecular weights less than about 550. They are made by reacting a low molecular weight diol (below about 250) with a dicarboxylic acid.

[0062] The dicarboxylic acids may include the condensation polymerization equivalents of dicarboxylic acids, that is, their esters or ester-forming derivatives such as acid chlorides and anhydrides, or other derivatives which behave substantially like dicarboxylic acids in a polymerization reaction with a glycol.

[0063] The dicarboxylic acid monomers for the elastomer have a molecular weight less than about 300. They can be aromatic, aliphatic or cycloaliphatic. The dicarboxylic acids can contain any substituent groups or combination thereof which do not interfere with the polymerization reaction. Representative dicarboxylic acids include terephthalic and isophthalic acids, bibenzoic acid, substituted dicarboxy compounds with benzene nuclei such as bis(p-carboxyphenyl) methane, p-oxy-(p-carboxyphenyl) benzoic acid, ethylene-bis(p-oxybenzoic acid), 1 ,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, 2,7-naphthalene dicarboxylic acid, phenanthralenedicarboxylic acid, anthralenedicarboxylic acid, 4, 4' -sulfonyl dibenzoic acid, etc. and Ci -C10 alkyl and other ring substitution derivatives thereof such as halo, alkoxy or aryl derivatives. Hydroxy acids such asp(P-hydroxyethoxy) benzoic acid can also be used providing an aromatic dicarboxylic acid is also present.

[0064] Representative aliphatic and cycloaliphatic acids are sebacic acid, 1,3-or 1 ,4-cyclohexane dicarboxylic acid, adipic acid, glutaric acid, succinic acid,Attorney Docket No.: CICT-1562-PCT (2025P0008)carbonic acid, oxalic acid, itaconic acid, azelaic acid, diethylmalonic acid, fumaric acid, citraconic acid, allylmalonate acid, 4-cyclohexene-1 ,2-dicarboxylate acid, pimelic acid, suberic acid, 2,5-diethyladipic acid, 2-ethylsuberic acid, 2, 2,3,3-tetramethylsuccinic acid, cyclopentanedicarboxylic acid, decahydro-1 ,5- (or 2,6-) naphthylenedicarboxylic acid, 4,4'-bicyclohexyl dicarboxylic acid, 4,4'-methylenebis(cyclohexyl carboxylic acid), 3,4-furan dicarboxylate, and 1,1-cyclobutane dicarboxylate.

[0065] The dicarboxylic acid may have a molecular weight less than about 300. In one embodiment, phenylene dicarboxylic acids are used such as terephthalic and isophthalic acid.

[0066] Included among the low molecular weight (less than about 250) diols which react to form short chain ester units of the copolyesters are acyclic, alicyclic and aromatic dihydroxy compounds. Included are diols with 2-15 carbon atoms such as ethylene, propylene, isobutylene, tetramethylene, pentamethylene, 2,2-dimethyltrimethylene, hexamethylene and decamethylene glycols, dihydroxy cyclohexane, cyclohexane dimethanol, resorcinol, hydroquinone, 1,5-dihydroxy naphthalene, etc. Also included are aliphatic diols containing 2-8 carbon atoms. Included among the bis-phenols which can be used are bis(p-hydroxy) diphenyl, bis(p-hydroxyphenyl) methane, and bis(p-hydroxyphenyl) propane. Equivalent ester-forming derivatives of diols are also useful (e.g., ethylene oxide or ethylene carbonate can be used in place of ethylene glycol). Low molecular weight diols also include such equivalent ester-forming derivatives.

[0067] Long chain glycols which can be used in preparing the polymers include the poly(alkylene oxide) glycols such as polyethylene glycol, poly(1 ,2- and 1,3-propylene oxide) glycol, poly(tetramethylene oxide) glycol, poly(pentamethylene oxide) glycol, poly(hexamethylene oxide) glycol, poly(heptamethylene oxide) glycol, poly(octamethylene oxide) glycol, poly(nonamethylene oxide) glycol and poly( 1 ,2-butylene oxide) glycol; random and block copolymers of ethylene oxide and 1 ,2-propylene oxide and poly-formals prepared by reacting formaldehyde with glycols, such as pentamethylene glycol, or mixtures of glycols, such as a mixture of tetramethylene and pentamethylene glycols.

[0068] In addition, the dicarboxym ethyl acids of poly(alkylene oxides) such as the one derived from polytetramethylene oxideAttorney Docket No.: CICT-1562-PCT (2025P0008)HOOCCH2(OCH2CH2CH2CH2)XOCH2COOH IV can be used to form long chain glycols in situ. Polythioether glycols and polyester glycols also provide useful products. In using polyester glycols, care must generally be exercised to control a tendency to interchange during melt polymerization, but certain sterically hindered polyesters, e.g., poly(2,2-dimethyl-1 ,3-propylene adipate), poly(2,2-dimethyl-1 ,3-propylene / 2-methyl-2-ethyl-1 ,3-propylene 2,5-dimethylterephthalate), poly(2,2-dimethyl-1 ,3-propylene / 2,2-diethyl-1 ,3-propylene, 1 ,4 cyclohexanedicarboxylate) and poly( 1 ,2-cyclohexylenedimethylene / 2,2-dimethyl-1 ,3-propylene 1 ,4-cyclohexanedicarboxylate) can be utilized under normal reaction conditions and other more reactive polyester glycols can be used if a short residence time is employed. Either polybutadiene or polyisoprene glycols, copolymers of these and saturated hydrogenation products of these materials are also satisfactory long chain polymeric glycols. In addition, the glycol esters of dicarboxylic acids formed by oxidation of polyisobutylenediene copolymers are useful raw materials.

[0069] Although the long chain dicarboxylic acids (IV) above can be added to the polymerization reaction mixture as acids, they react with the low molecular weight diols(s) present, these always being in excess, to form the corresponding poly(alkylene oxide) ester glycols which then polymerize to form the G units in the polymer chain, these particular G units having the structurewhen only one low molecular weight diol (corresponding to D) is employed. When more than one diol is used, there can be a different diol cap at each end of the polymer chain units. Such dicarboxylic acids may also react with long chain glycols if they are present, in which case a material is obtained having a formula the same as V above except the Ds are replaced with polymeric residues of the long chain glycols. The extent to which this reaction occurs is quite small, however, since the low molecular weight diol is present in considerable molar excess.

[0070] In place of a single low molecular weight diol, a mixture of such diols can be used. In place of a single long chain glycol or equivalent, a mixture of such compounds can be utilized, and in place of a single low molecular weight dicarboxylic acid or its equivalent, a mixture of two or more can be used inAttorney Docket No.: CICT-1562-PCT (2025P0008)preparing the thermoplastic copolyester elastomers which can be employed in the compositions of this invention. Thus, the letter "G" in Formula II above can represent the residue of a single long chain glycol or the residue of several different glycols, the letter D in Formula III can represent the residue of one or several low molecular weight diols and the letter R in Formulas II and III can represent the residue of one or several dicarboxylic acids. When an aliphatic acid is used which contains a mixture of geometric isomers, such as the cis-trans isomers of cyclohexane dicarboxylic acid, the different isomers should be considered as different compounds forming different short chain ester units with the same diol in the copolyesters. The copolyester elastomer can be made by conventional ester interchange reaction.

[0071] Copolyether esters with alternating, random-length sequences of either long chain or short chain oxyalkylene glycols can contain repeating high melting blocks that are capable of crystallization and substantially amorphous blocks with a relatively low glass transition temperature. In one embodiment, the hard segments can be composed of tetramethylene terephthalate units and the soft segments may be derived from aliphatic polyether and polyester glycols. Of particular advantage, the above materials resist deformation at surface temperatures because of the presence of a network of microcrystallites formed by partial crystallization of the hard segments. The ratio of hard to soft segments determines the characteristics of the material. Thus, another advantage to thermoplastic polyester elastomers is that soft elastomers and hard elastoplastics can be produced by changing the ratio of the hard and soft segments.

[0072] In one particular embodiment, the polyester thermoplastic elastomer has the following formula: -[4GT]x[BT]y, wherein 4G is butylene glycol, such as 1 ,4-butane diol, B is poly(tetramethylene ether glycol) and T is terephthalate, and wherein x is from about 0.60 to about 0.99 and y is from about 0.01 to about 0.40.

[0073] In one aspect, the thermoplastic polyester elastomer can be a block copolymer of polybutylene terephthalate and polyether segments and can have a structure as follows:Attorney Docket No.: CICT-1562-PCT (2025P0008)Ja L Jb Hard segment (PBT) Soft Segment (Polytetramethylene Ether Glycol Terephtalate)wherein a and b are integers and can vary from 2 to 10,000. The ratio between hard and soft segments in the block copolymer as described above can be varied in order to vary the properties of the elastomer. In one aspect, the density of the polyester elastomer as indicated above can be from about 1.05 g / cm3to about 1.15 g / cm3, such as from about 1.08 g / cm3to about 1.1 g / cm3.

[0074] In one embodiment, the polyoxymethylene polymer is combined with an impact modifier, such as a thermoplastic polyester elastomer, that has a melting temperature similar to the melting temperature of the polyoxymethylene polymer. For example, in one aspect, the impact modifier is selected such that the melting temperature of the impact modifier is within about 8°C, such as within about 5°C, such as within about 4°C, such as within about 3°C of the melting temperature of the polyoxymethylene polymer. For example, an impact modifier, such as a polyester elastomer, can be selected with a melting temperature of from about 150°C to about 185°C, such as from about 158°C to about 172°C, such as from about 163°C to about 169°C. Melting temperature can be determined according to ISO Test 11357-1 / -3 (10°C / min) or can be determined according to ASTM Test D3417 (DSC).

[0075] In one embodiment, an impact modifier, such as a thermoplastic polyester elastomer, can be selected that has a melting temperature that is less than the melting temperature of the polyoxymethylene polymer. For instance, the melting temperature of the impact modifier can be less than about 164°C, such as less than about 161 °C, such as less than about 158°C, such as less than about 155°C, such as less than about 153°C, and generally greater than about 140°C, such as greater than about 145°C, such as greater than about 148°C.

[0076] In an alternative embodiment, the impact modifier may comprise a nonaromatic polymer, which refers to a polymer that does not include any aromatic groups on the backbone of the polymer. Such polymers include acrylate polymersAttorney Docket No.: CICT-1562-PCT (2025P0008)and / or graft copolymers containing an olefin. For instance, an olefin polymer can serve as a graft base and can be grafted to at least one vinyl polymer or one ether polymer. In still another embodiment, the graft copolymer can have an elastomeric core based on polydienes and a hard or soft graft envelope composed of a (meth)acrylate and / or a (meth)acrylonitrile.

[0077] In general, one or more impact modifiers may be present in the polymer composition in an amount from about 2% by weight to about 45% by weight, such as from about 4% by weight to about 27% by weight, including all increments of 1 % by weight therebetween. For instance, one or more impact modifiers can be present in the polymer composition in an amount greater than about 6% by weight, such as in an amount greater than about 8% by weight, such as in an amount greater than about 10% by weight, such as in an amount greater than about 12% by weight, such as in an amount greater than about 14% by weight, such as in an amount greater than about 16% by weight, such as in an amount greater than about 20% by weight, such as in an amount greater than about 25% by weight, such as in an amount greater than about 30% by weight, such as in an amount greater than about 35% by weight, and generally in an amount less than about 50% by weight, such as less than about 40% by weight, such as less than about 25% by weight, such as in an amount less than about 23% by weight.

[0078] As described above, in various embodiments, the polymer composition can contain more than one impact modifier. For example, in one embodiment, the polymer composition can contain a thermoplastic polyurethane elastomer in combination with a thermoplastic polyester elastomer. For example, the thermoplastic polyester elastomer can be a thermoplastic ester ether elastomer. In one embodiment, a thermoplastic polyurethane elastomer can be combined with a thermoplastic copolyester elastomer that comprises a block copolymer of polybutylene terephthalate and polyether segments. Incorporating a block copolymer of a polybutylene terephthalate and polyether segments into the polymer composition can dramatically improve impact resistance, especially at lower temperatures. The weight ratio between the thermoplastic polyurethane elastomer and the thermoplastic copolyester elastomer can be from about 1 :5 to about 5: 1 , such as from about 1 :3 to about 3: 1 , such as from about 1.5:1 to about 1:1.5. In one aspect, for instance, a thermoplastic polyurethane elastomer can beAttorney Docket No.: CICT-1562-PCT (2025P0008)present in the polymer composition in an amount from about 5% to about 12% by weight and a thermoplastic copolyester elastomer can be present in the polymer composition in an amount from about 5% to about 12% by weight. In one embodiment, a thermoplastic polyurethane elastomer can be present in the polymer composition in an amount from about 8% to about 15% by weight, such as from about 9% to about 11% by weight, and a thermoplastic copolyester elastomer can be present in the polymer composition also in an amount from about 8% to about 15% by weight, such as from about 9% to about 11 % by weight.

[0079] In addition to a polyoxymethylene polymer and one or more impact modifiers, the polymer composition of the present disclosure can contain various other components. For instance, in one embodiment, a polyalkylene glycol can be incorporated into the polymer composition for providing various advantages and benefits. The polyalkylene glycol, for instance, can improve flow properties of the particles and / or can improve impact strength resistance.

[0080] Polyalkylene glycols particularly well suited for use in the polymer composition include polyethylene glycols, polypropylene glycols, and mixtures thereof.

[0081] The molecular weight of the polyalkylene glycol can vary depending upon various factors including the characteristics of the polyoxymethylene polymer and the process conditions for producing shaped articles. In one aspect, the polyalkylene glycol, such as the polyethylene glycol, can have a relatively low molecular weight. For example, the molecular weight can be less than about 10,000 g / mol, such as less than about 8,000 g / mol, such as less than about 6,000 g / mol, such as less than about 4,000 g / mol, and generally greater than about 1 ,000 g / mol, such as greater than about 2,000 g / mol. In one embodiment, a polyethylene glycol plasticizer is incorporated into the polymer composition that has a molecular weight of from about 2,000 g / mol to about 5,000 g / mol.

[0082] In another aspect, a polyalkylene glycol, such as the polyethylene glycol, can be selected that has a higher molecular weight. For example, the molecular weight of the polyalkylene glycol can be about 10,000 g / mol or greater, such as greater than about 20,000 g / mol, such as greater than about 30,000 g / mol, such as greater than about 35,000 g / mol, and generally less than about 100,000 g / mol, such as less than about 50,000 g / mol, such as less than about 45,000 g / mol, suchAttorney Docket No.: CICT-1562-PCT (2025P0008)as less than about 40,000 g / mol.

[0083] When present in the polymer composition, the polyalkylene glycol can be added in amounts greater than about 0.1% by weight, such as in an amount greater than about 0.3% by weight. The polyalkylene glycol can generally be present in the polymer composition in an amount less than about 5% by weight, such as in an amount less than about 3% by weight, such as in an amount less than about 1 % by weight.

[0084] In one embodiment, in addition to one or more impact modifiers, the polymer composition can contain a coupling agent. The coupling agent can be used to compatibilize the different components. For instance, the coupling agent can couple to the polyoxymethylene polymer and to the one or more impact modifiers. It should be understood, however, that in one embodiment the polymer composition is formulated so as not to contain any coupling agents.

[0085] In one embodiment, the coupling agent comprises a polyisocyanate, such as a diisocyanate, such as an aliphatic, cycloaliphatic and / or aromatic diisocyanate. The coupling agent may be in the form of an oligomer, such as a trimer or a dimer.

[0086] In one embodiment, the coupling agent comprises a diisocyanate or a triisocyanate which is selected from 2,2'-, 2,4'-, and 4,4'-diphenylmethane diisocyanate (MDI); 3,3'-dimethyl-4,4'-biphenylene diisocyanate (TODD; toluene diisocyanate (TDI); polymeric MDI; carbodiimide-modified liquid 4,4'-diphenylmethane diisocyanate; para-phenylene diisocyanate (PPDI); metaphenylene diisocyanate (MPDI); triphenyl methane-4,4'- and triphenyl methane-4,4"-triisocyanate; naphthylene-1,5-diisocyanate; 2,4'-, 4,4'-, and 2,2-biphenyl diisocyanate; polyphenylene polymethylene polyisocyanate (PMDI) (also known as polymeric PMDI); mixtures of MDI and PMDI; mixtures of PMDI and TDI; ethylene diisocyanate; propylene-1 ,2-diisocyanate; trimethylene diisocyanate; butylenes diisocyanate; bitolylene diisocyanate; tolidine diisocyanate; tetramethylene-1 , 2-diisocyanate; tetramethylene-1 ,3-diisocyanate; tetramethylene-1 ,4-diisocyanate; pentamethylene diisocyanate; 1 ,6-hexamethylene diisocyanate (HDI); octamethylene diisocyanate; decamethylene diisocyanate; 2,2,4-trimethylhexamethylene diisocyanate; 2,4,4-trimethylhexamethylene diisocyanate; dodecane-1 ,12-diisocyanate; dicyclohexylmethane diisocyanate; cyclobutane-1 , 3-Attorney Docket No.: CICT-1562-PCT (2025P0008)diisocyanate; cyclohexane-1 ,2-diisocyanate; cyclohexane-1 ,3-diisocyanate; cyclohexane-1 ,4-diisocyanate; diethylidene diisocyanate; methylcyclohexylene diisocyanate (HTDI); 2,4-methylcyclohexane diisocyanate; 2,6-methylcyclohexane diisocyanate; 4,4'-dicyclohexyl diisocyanate; 2, 4' -dicyclohexyl diisocyanate; 1,3,5-cyclohexane triisocyanate; isocyanatomethylcyclohexane isocyanate; 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane; isocyanatoethylcyclohexane isocyanate; bis(isocyanatomethyl)-cyclohexane diisocyanate; 4,4'-bis(isocyanatomethyl) dicyclohexane; 2,4'-bis(isocyanatomethyl) dicyclohexane; isophorone diisocyanate (IPDI); dimeryl diisocyanate, dodecane-1 ,12-diisocyanate, 1 ,10-decamethylene diisocyanate, cyclohexylene-1 , 2-diisocyanate, 1 ,10-decamethylene diisocyanate, 1-chlorobenzene-2, 4-diisocyanate, furfurylidene diisocyanate, 2,4,4-trimethy I hexamethylene diisocyanate, 2,2,4-trimethyl hexamethylene diisocyanate, dodecamethylene diisocyanate, 1 ,3-cyclopentane diisocyanate, 1 ,3-cyclohexane diisocyanate, 1, 3-cyclobutane diisocyanate, 1 ,4-cyclohexane diisocyanate, 4, 4'-methylenebis(cyclohexyl isocyanate), 4,4'-methylenebis(phenyl isocyanate), 1-methyl-2,4-cyclohexane diisocyanate, 1-methyl-2,6-cyclohexane diisocyanate, 1,3-bis (isocyanato-methyl)cyclohexane, 1 ,6-diisocyanato-2,2,4,4-tetra-methylhexane, 1 ,6-diisocyanato-2,4,4-tetra-trimethylhexane, trans-cyclohexane-1 ,4-diisocyanate, 3-isocyanato-methyl-3,5,5-trimethylcyclo-hexyl isocyanate, 1 -isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane, cyclo-hexyl isocyanate, dicyclohexylmethane 4,4'-diisocyanate, 1 ,4-bis(isocyanatomethyl)cyclohexane, m-phenylene diisocyanate, m-xylylene diisocyanate, m-tetramethylxylylene diisocyanate, p-phenylene diisocyanate, p,p'-biphenyl diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, 3,3'-dimethoxy-4,4'-biphenylene diisocyanate, 3,3'-diphenyl-4,4'-biphenylene diisocyanate, 4,4'-biphenylene diisocyanate, 3,3'-dichloro-4,4'-biphenylene diisocyanate, 1 ,5-naphthalene diisocyanate, 4-chloro-1 ,3-phenylene diisocyanate, 1 ,5-tetrahydronaphthalene diisocyanate, metaxylene diisocyanate, 2,4-toluene diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,4-chlorophenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, p,p'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 2,2-diphenylpropane-4,4'-diisocyanate, 4, 4' -toluidine diisocyanate, dianidine diisocyanate, 4,4'-diphenyl ether diisocyanate, 1,3-xylylene diisocyanate,Attorney Docket No.: CICT-1562-PCT (2025P0008)1 ,4-naphthylene di isocyanate, azobenzene-4,4'-diisocyanate, diphenyl sulfone-4,4'-diisocyanate, or mixtures thereof.

[0087] In one embodiment, an aromatic polyisocyanate is used, such as 4,4'-diphenylmethane diisocyanate (MDI).

[0088] When present, the coupling agent can be present in the composition in an amount generally from about 0.1 % to about 5% by weight. In one embodiment, for instance, the coupling agent can be present in an amount from about 0.1% to about 2% by weight, such as from about 0.2% to about 1 % by weight. In an alternative embodiment, the coupling agent can be added to the polymer composition in molar excess amounts when comparing the reactive groups on the coupling agent with the amount of functional groups on the polyoxymethylene polymer. As described above, in one embodiment, the polymer composition does not contain any coupling agents. For example, in one embodiment, the polymer composition can be polyisocyanate free. In fact, in one aspect, various advantages and benefits may be realized by not including any polyisocyanate compounds.

[0089] The polymer composition of the present disclosure can also optionally contain a stabilizer and / or various other additives. Such additives can include, for example, antioxidants, acid scavengers, UV stabilizers or heat stabilizers. In addition, the polymer composition may contain processing auxiliaries, for example adhesion promoters, or antistatic agents.

[0090] For instance, in one embodiment, an ultraviolet light stabilizer may be present. The ultraviolet light stabilizer may comprise a benzophenone, a benzotriazole, or a benzoate. Particular examples of ultraviolet light stabilizers include 2,4-dihydroxy benzophenone, 2-hydroxy-4-methoxybenzophenone, 2-(2'-hydroxy-3',5'-di-t-butylphenyl)benzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, and 5,5'-methylene bis(2-hydroxy-4-methoxybenzophenone); 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1 -phenylethyl) phenol; 2-(2'-hydroxyphenyl)benzotriazoles, e.g., 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-t-butylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-Attorney Docket No.: CICT-1562-PCT (2025P0008)methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-dicumylphenyl)benzotriazole, and 2,2'-methylene bis(4-t-octyl-6-benzotriazolyl)phenol, phenylsalicylate, resorcinol monobenzoate, 2,4-di-t-butylphenyl-3',5'-di-t-butyl-4'-hydroxybenzoate, and hexadecyl-3, 5-di-t-butyl-4-hydroxybenzoate; substituted oxanilides, e.g., 2-ethyl-2'-ethoxyoxanilide and 2-ethoxy-4'-dodecyloxanilide; cyanoacrylates, e.g., ethyl-.alpha.-cyano-.beta.,.beta.-diphenylacrylate and methyl-2-cyano-3-methyl-3-(p-methoxyphenyl)acrylate or mixtures thereof. A specific example of an ultraviolet light absorber that may be present is UV 234, which is a high molecular weight ultraviolet light absorber of the hydroxyl phenyl benzotriazole class. The UV light absorber, when present, can be present in the polymer composition in an amount ranging from about 0.1% by weight to about 2% by weight, such as in an amount ranging from about 0.25% by weight to about 1 % by weight based on the total weight of the polymer composition.

[0091] In one embodiment, the polymer composition may also include a formaldehyde scavenger, such as a nitrogen-containing compound. Mainly, of these are heterocyclic compounds having at least one nitrogen atom as hetero atom which is either adjacent to an amino-substituted carbon atom or to a carbonyl group, for example pyridine, pyrimidine, pyrazine, pyrrolidone, aminopyridine and compounds derived therefrom. Advantageous compounds of this nature are aminopyridine and compounds derived therefrom. Any of the aminopyridines is in principle suitable, for example 2,6-diaminopyridine, substituted and dimeric aminopyridines, and mixtures prepared from these compounds. Other advantageous materials are polyamides and dicyane diamide, urea and its derivatives and also pyrrolidone and compounds derived therefrom. Examples of suitable pyrrolidones are imidazolidinone and compounds derived therefrom, such as hydantoines, derivatives of which are particularly advantageous, and those particularly advantageous among these compounds are allantoin and its derivatives. Other particularly advantageous compounds are triamino-1 ,3,5-triazine(melamine) and its derivatives, such as melamine-formaldehyde condensates and methylol melamine. Oligomeric polyamides are also suitable in principle for use as formaldehyde scavengers. In one aspect, the formaldehyde scavenger can comprise melamine. In an alternative embodiment, the acidAttorney Docket No.: CICT-1562-PCT (2025P0008)scavenger can be a copolyamide. The copolyamide can be used alone or in combination with a melamine.

[0092] Further, the formaldehyde scavenger can be a guanidine compound which can include an aliphatic guanamine-based compound, an alicyclic guanamine-based compound, an aromatic guanamine-based compound, a hetero atom-containing guanamine-based compound, or the like. The formaldehyde scavenger can be present in the polymer composition in an amount ranging from about 0.005% by weight to about 2% by weight, such as in an amount ranging from about 0.0075% by weight to about 1 % by weight based on the total weight of the polymer composition.

[0093] In one embodiment, however, the polymer composition of the present disclosure can be formulated so as to be free of various formaldehyde scavengers that may, in some embodiments, have an adverse impact on rotationally molded articles made from the composition. For example, in one embodiment, the polymer composition can be formulated to be free of all formaldehyde scavengers, and particularly can be free of nitrogen-containing formaldehyde scavengers. Formaldehyde scavengers that can be excluded from the composition include guanamines, such as benzoguanamine, melamine, and melamine derivatives. In one embodiment, the only formaldehyde scavenger present in the polymer composition may be a copolyamide.

[0094] Still another additive that may be present in the composition is a sterically hindered phenol compound, which may serve as an antioxidant.Examples of such compounds, which are available commercially, are pentaerythrityl tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (IRGANOX® 1010, BASF), triethylene glycol bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate] (IRGANOX® 245, BASF), 3,3'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionohydrazide] (IRGANOX® MD 1024, BASF), hexamethylene glycol bis[3-(3,5-di-cert-butyl-4-hydroxyphenyl)propionate] (IRGANOX® 259, BASF), and 3,5-di-tert-butyl-4-hydroxytoluene (LOWINOX® BHT, Chemtura). The above compounds may be present in the polymer composition in an amount ranging from about 0.01 % by weight to about 1 % by weight based on the total weight of the polymer composition.

[0095] In one embodiment, the polymer composition of the present disclosureAttorney Docket No.: CICT-1562-PCT (2025P0008)contains significant amounts of antioxidant and other stabilizers. For example, the polymer composition can be formulated so as to contain one or more sterically hindered phenol compounds in an amount greater than about 0.2% by weight, such as in an amount greater than about 0.22% by weight, such as in an amount greater than about 0.3% by weight, and generally in an amount less than about 5% by weight, such as in an amount less than about 2% by weight. Including greater amounts of antioxidant can increase the thermal stability of the polymer composition.

[0096] Light stabilizers that may be present in addition to the ultraviolet light stabilizer in the composition include sterically hindered amines. Hindered amine light stabilizers that may be used include oligomeric compounds that are N-methylated. In one aspect, the light stabilizer can comprise bis(2, 2,6,6-tetramethyl-4-piperidyl)sebaceate. For instance, one example of a hindered amine light stabilizer comprises ADK STAB LA-63 light stabilizer available from Adeka Palmarole. The light stabilizers, when present, can be present in the polymer composition in an amount ranging from about 0.1% by weight to about 2% by weight, such as in an amount ranging from about 0.25% by weight to about 1% by weight based on the total weight of the polymer composition.

[0097] In addition to the above components, the polymer composition may also contain an acid scavenger. The acid scavenger may comprise, for instance, an alkaline earth metal salt. For instance, the acid scavenger may comprise a calcium salt, such as a calcium citrate. In one aspect, the calcium citrate is a tricalcium citrate. Another acid scavenger well suited for use in the polymer composition is calcium propionate anhydrous. In one embodiment, the acid scavenger selected for use in the polymer composition is a calcium stearate.Calcium stearate has been found to provide various advantages and benefits with respect to properties obtained from molded articles made from the polymer composition. The calcium stearate, for instance, can be calcium 12-hydroxystearate. The acid scavenger may be present in an amount ranging from about 0.01% by weight to about 1% by weight based on the total weight of the polymer composition.

[0098] In one embodiment, a lubricant may be present. The lubricant can comprise a polymer wax composition. For example, a fatty acid amide may beAttorney Docket No.: CICT-1562-PCT (2025P0008)used. One example of a fatty acid amide is ethylene bis(stearamide).Alternatively, the lubricant can comprise a polyethylene wax. Lubricants may generally be present in the polymer composition in an amount from about 0.01% by weight to about 1 % by weight.

[0099] The polymer composition can also contain a nucleating agent that may increase the crystallinity of the polyoxymethylene polymer. The nucleating agent, for instance, can comprise an oxymethylene terpolymer, talc particles, or the like. Alternatively, the polymer composition can be formulated so as not to contain any nucleating agents. When present, the nucleating agent can be added to the polymer composition in an amount greater than about 0.1 % by weight, such as in an amount greater than about 0.2% by weight, and generally in an amount less than about 1.5% by weight, such as in an amount less than about 0.8% by weight.

[0100] In one embodiment, one or more coloring agents can also be added to the polymer composition. The coloring agent can be a pigment or a dye. In one aspect, the coloring agent can be added as a masterbatch in combination with a polyoxymethylene polymer. One or more coloring agents can be present in the polymer composition generally in an amount greater than about 0.1% by weight and generally in an amount less than about 2% by weight.

[0101] Any of the above additives can be added to the polymer composition alone or combined with other additives. In general, each additive is present in the polymer composition in an amount less than about 5% by weight, such as in an amount ranging from about 0.005% by weight to about 2% by weight, such as in an amount ranging from about 0.0075% by weight to about 1% by weight, such as from about 0.01 % by weight to about 0.5% by weight based on the total weight of the polymer composition.

[0102] In order to form a powder from the polyoxymethylene polymer composition, in one aspect, the components of the polymer composition can be mixed together and then melt blended. For instance, the components can be melt blended in an extruder. Processing temperatures can vary depending upon the type of polyoxymethylene polymer chosen for use in the application. In one embodiment, processing temperatures can be from about 165°C to about 200°C.

[0103] Extruded strands can be produced which are then pelletized. The pelletized compound can then be ground to a suitable particle size and to aAttorney Docket No.: CICT-1562-PCT (2025P0008)suitable particle size distribution to produce a powder that is well suited for use in rotational molding.

[0104] For example, any suitable hammermill or granulator may be used to produce the powder composition. In one embodiment, cryogenic grinding is used to produce particles having a relatively small size and a uniform particle size distribution. Cryogenic grinding, for instance, can produce a powder not only having a uniform size but also having particles that are approximately spherical in shape.

[0105] In one embodiment, in order to account for longer cycle times, the particle size distribution of the polymer composition includes relatively large particle sizes (although smaller sizes may be used depending on the application). For example, in one aspect, greater than 10% by weight of the particles can have a particle size of greater than about 625 microns, such as greater than about 630 microns, such as greater than about 635 microns, such as greater than about 640 microns. In particular applications, greater than 10% of the particles can have a particle size of greater than about 660 microns, such as greater than about 680 microns, such as greater than about 700 microns. The above 10% by weight of particles generally has an average particle size of less than about 1200 microns, such as less than about 1000 microns, such as less than about 900 microns, such as less than about 850 microns.

[0106] In addition to a D90 particle size, the particle size distribution of the polymer composition can also be described in terms of a D50 particle size, a D75 particle size, and a D10 particle size. For example, the powder composition can have a D50 particle size of generally greater than 150 microns, such as greater than about 160 microns, such as greater than about 175 microns, such as greater than about 200 microns, such as greater than about 225 microns, such as greater than about 250 microns, such as greater than about 275 microns, such as greater than about 290 microns. The D50 particle size is generally less than about 600 microns, such as less than about 550 microns, such as less than about 500 microns, such as less than about 450 microns.

[0107] The polymer composition in the form of a powder can have a D10 particle size (smallest particles) of generally greater than about 90 microns, such as greater than about 100 microns, such as greater than about 110 microns, suchAttorney Docket No.: CICT-1562-PCT (2025P0008)as greater than about 120 microns, such as greater than about 130 microns, and generally less than about 300 microns, such as less than about 250 microns, such as less than about 220 microns. The powder composition can have a D75 particle size of generally greater than about 380 microns, such as greater than about 400 microns, such as greater than about 420 microns, such as greater than about 440 microns, and generally less than about 700 microns, such as less than about 650 microns, such as less than about 625 microns, such as less than about 600 microns, such as less than about 590 microns. Particle size can be determined using a laser scattering particle size distribution analyzer, such as a Beckman Coulter LS 13320 particle size analyzer.

[0108] In an alternative embodiment, the particle size distribution of the polymer composition can include smaller particles than described above when using a particular type of polyoxymethylene polymer in combination with various impact modifiers. For example, in another embodiment, the polymer composition can have a particle size distribution such that 90% of the particles have a size of less than about 500 microns. 50% of the particles can have a particle size of from about 450 microns to about 250 microns, such as from about 420 microns to about 300 microns. From about 30% to about 50% of the particles by mass can have a particle size of from about 250 microns to about 500 microns.

[0109] In still another embodiment, the particle size distribution of the polymer composition can be such that 90% of the particles have a size less than about 420 microns, such as less than about 400 microns, such as less than about 380 microns. 50% of the particles by mass can have a particle size of from about 250 microns to about 177 microns. From about 45% to about 60% of the particles by mass can have a particle size of from about 420 microns to about 177 microns, such as from about 350 microns to about 170 microns, such as from about 280 microns to about 177 microns. In addition to using light scattering for determining particle size, in an alternative embodiment, a sieve test can be used. For example, particle size (based on mass) can be determined using a RO-TAP sieve shaker.

[0110] As described above, the polyoxymethylene polymer composition as described above is used to form at least one layer of the container. The polyoxymethylene polymer composition can form the interior layer or the exterior layer of the container or can form a middle layer that is sandwiched between twoAttorney Docket No.: CICT-1562-PCT (2025P0008)other layers. In one aspect, the polyoxymethylene polymer composition is used to form the interior layer of the tank due to its low permeability properties. The exterior layer of the tank, on the other hand, can comprise a polymer composition that displays a higher impact strength than the polyoxymethylene polymer layer.

[0111] In one aspect, the exterior layer of the tank is formed from a crosslinked polyethylene polymer resin.

[0112] The polyethylene material employed is preferably a low-density polyethylene (LDPE) or linear low-density polyethylene (LLDPE) with a melt flow index ranging from approximately 2 to 10 g / 10 min (ASTM D1238), providing appropriate flow and sintering behavior within the mold. The base resin may be in powder form, optimized for uniform distribution and surface adhesion during rotational molding processes.

[0113] To enable in-situ crosslinking during the molding cycle, the polyethylene resin is compounded with one or more free-radical generating initiators, typically selected from organic peroxides. Suitable initiators include, but are not limited to, dicumyl peroxide (DCP), 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane (DHBP), bis(t-butylperoxy)diisopropylbenzene, or t-butyl cumyl peroxide. These initiators decompose at elevated temperatures (generally in the range of 150°C to 190°C), producing free radicals that initiate covalent crosslinking reactions between polyethylene chains.

[0114] The initiator is typically incorporated at a concentration of about 0.5% to 3% by weight, relative to the polyethylene resin. The concentration and specific initiator are selected based on desired cure kinetics, processing temperatures, and the target degree of crosslinking (commonly expressed as gel content), which may range from approximately 60% to greater than 90%. Crosslinking is facilitated during the heating phase of the rotational molding cycle, wherein the mold temperature typically reaches 260°C to 300°C, enabling sufficient thermal activation of the initiator.

[0115] The resulting crosslinked polyethylene (XLPE) layer exhibits enhanced environmental stress crack resistance (ESCR), chemical resistance to hydrocarbon fuels including ethanol and biodiesel blends, improved thermal stability, and high impact strength. These attributes make XLPE particularly well-suited for inner or outer structural layers of multilayer fuel tank systems. AdditionalAttorney Docket No.: CICT-1562-PCT (2025P0008)additives such as antioxidants, UV stabilizers, carbon black, and barrier-enhancing agents may be included to further tailor performance properties.

[0116] In embodiments where the fuel tank comprises multiple layers, the XLPE layer may be co-molded or sequentially molded with one or more functional layers, such as an ethylene vinyl alcohol (EVOH) barrier layer, tie layers, or additional structural layers of high-density polyethylene (HDPE), to meet regulatory requirements for fuel permeation and structural integrity.

[0117] Once the polymer compositions are formulated and formed into a powder having a controlled particle size distribution, the polymer particles are loaded into a mold for producing molded articles. During rotational molding, the polymer particles are loaded into a mold and the mold is rotated at least about a first axis and a second axis while being heated. The polymer composition is heated to a molten temperature, causing the polymer composition to flow and coat the interior walls of the mold for producing hollow vessels.

[0118] When producing multi-layer articles in accordance with the present disclosure, the polyethylene resin particles are first loaded into the mold followed by the polyoxymethylene polymer composition. During rotational molding, the oven temperature can be generally from about 380°F to about 450°F. In one aspect, the temperature is from about 380°F to about 405°F. Temperature and cycle times can be controlled in order to control the properties of the resulting tank or container. Cycle times and temperatures can be based upon the thickness of the resulting product. Various different parameters can also be used to control the adhesion between the layers. If there is no adhesion between the different layers, the product tends to be unstable. Excessive adhesion between the layers has been found to be detrimental to the overall impact resistance properties of the product. In one aspect, the interior or lining layer and the exterior or outer layer can display an adhesive shear force according to ASTM Test D903 of greater than about 120 lbs., such as greater than about 300 lbs., such as greater than about 400 lbs., such as greater than about 450 lbs., and less than about 800 lbs., such as less than about 700 lbs., such as less than about 600 lbs., such as less than about 500 lbs.

[0119] As described above, the wall thickness can be generally from about 2 mm to about 12 mm. The ratio between the polyethylene layer or outer layer to theAttorney Docket No.: CICT-1562-PCT (2025P0008)polyoxymethylene polymer layer or lining layer can be from about 1.5:1 to about 5: 1 , such as from about 1.75: 1 to about 4.25: 1. In one aspect, the polyoxymethylene polymer layer or lining layer has a thickness of less than about 3.25 mm, such as less than about 2.75 mm, such as less than about 2.5 mm, such as less than about 2.25 mm, such as less than about 2 mm, such as less than about 1.75 mm, and greater than about 1 mm, such as greater than about 1.25 mm.

[0120] The present disclosure may be better understood with reference to the following example.Example

[0121] Two different polyoxymethylene polymer compositions were formulated. One composition contained a thermoplastic polyurethane elastomer. The second composition contained a thermoplastic polyurethane elastomer in combination with a thermoplastic polyester elastomer. In particular, the following polyoxymethylene polymer compositions were formulated:Weight % Material Sample No. 1A 2A Polyoxymethylene polymer (2.5 g / 10 min - 76.738% 73.288% low amount of hydroxyl groups)Thermoplastic polyurethane 18% 10% Thermoplastic polyester elastomer 10% Polyoxymethylene resin (carrier for additives) 3.502% 3.502% Polyethylene glycol 0.50% 0.50% Nucleant - (polyoxymethylene terpolymer) 0.50% Benzotriazole UV stabilizer 0.30% 0.30% Hindered amine light stabilizer 0.30% 0.30% Calcium propionate anhydrous 0.10% 0.10% Hindered phenolic antioxidant 0.23% 0.23% Melamine 0.03% 0.03% Ethylene bis(stearamide) 0.20% 0.20% Copolyamide 0.05% 0.05%Attorney Docket No.: CICT-1562-PCT (2025P0008)Tricalcium citrate 0.05% 0.05% |

[0122] The above polyoxymethylene polymer compositions were used to produce a rotationally molded two-layer container. The polyoxymethylene polymer composition was used to produce an inner layer while a crosslinked polyethylene polymer was used to produce an outer layer. The following polyethylene polymer products were used that contain a crosslinking agent that causes the polyethylene polymer to crosslink during the rotational molding process:Sample No. 1B: PAXON 7204 crosslinkable polyethylene polymer obtained from Exxon MobilSample No. 2B: SUPERLINK 120 obtained from Ingenia Polymers

[0123] Five different two-layer containers were produced as follows:PolymerContainer 1 Container 2 Container 3 Container 4 Container 5 Sample No.SpecificVariations of Cross-sectional thicknesses (mm)the MaterialA (inner layer) 2.54 mm 2.54 mmA (inner layer) 2.54 mm 1.524 mm 1.524 mm B (outer layer) 5.08 mm 5.08 mm 5.08 mmB (outer layer) 5.59 mm 5.59 mm

[0124] The above containers were then tested for impact strength. Containers No. 2 and 3 were also tested for adhesive shear force between the layers. The following results were obtained:Property Container 1 Container 2 Container 3 Container 4 Container 5Multiaxial ImpactMean Failure Energy80 112.5 112.5 90 150 (ARM method), 23C(ft-lbs)Attorney Docket No.: CICT-1562-PCT (2025P0008)Adhesive ShearForce between453 124layers, ASTM-D903(lbs)

[0125] Container No. 1 was also tested for fuel permeation according to SAE Test J2665 at 40°C. Two of the same containers were tested. In the first test, the fuel permeation was only 1.3 g / day-m2. During the second test, the container displayed a fuel permeation of only 1.0 g / day-m2.

[0126] These and other modifications and variations to the present invention may be practiced by those of ordinary skill in the art, without departing from the spirit and scope of the present invention, which is more particularly set forth in the appended claims. In addition, it should be understood that aspects of the various embodiments may be interchanged both in whole or in part. Furthermore, those of ordinary skill in the art will appreciate that the foregoing description is by way of example only and is not intended to limit the invention so further described in such appended claims.

Claims

Attorney Docket No.: CICT-1562-PCT (2025P0008)What Is Claimed:

1. A multi-layer article comprising:a seamless rotationally molded container defining an interior space, the container including a container wall comprised of an outer layer and a lining layer adjacent to and in contact with the outer layer, the outer layer comprising a polyethylene polymer, the lining layer being made from a polymer composition comprising a polyoxymethylene polymer having a melt flow rate of less than about 12 g / 10 min and optionally one or more impact modifiers comprising an elastomer, and wherein:the outer layer has a thickness ratio to the lining layer of from about 1.5:1 to about 5:1;the container has a multiaxial impact of greater than 40 ftlb-f at 23°C; and the wall of the container has a permeation of less than 2.5 g / m2per day at 40°C according to SAE Test J2665.

2. The multi-layer article as defined in claim 1 , wherein the polyoxymethylene polymer has a melt flow rate of from about 1.5 g / 10 min to about 9 g / 10 min.

3. The multi-layer article as defined in any of the preceding claims, wherein the outer layer has a thickness ratio to the lining layer of from about 1.75:1 to about 4.25:

14. The multi-layer article as defined in any of the preceding claims, wherein the container has a multiaxial impact of greater than 80 ftlb-f at 23°C.

5. The multi-layer article as defined in any of the preceding claims, wherein the wall of the container has a permeation of less than 1.4 g / m2per day at 40°C according to SAE Test J2665.

6. The multi-layer article as defined in any of the preceding claims, wherein the lining layer has a thickness of less than about 2.75 mm, such as less than about 1.75 mm.

7. The multi-layer article as defined in any of the preceding claims, wherein the wall has a thickness of from about 6 mm to about 8 mm.

8. The multi-layer article as defined in any of the preceding claims, wherein the lining layer and outer layer display an adhesive shear force according to ASTM D903 of greater than about 120 lbs, such as greater than about 300 lbs,Attorney Docket No.: CICT-1562-PCT (2025P0008)such as greater than about 400 lbs, such as greater than about 450 lbs.

9. The multi-layer article as defined in any of the preceding claims, wherein the polymer composition contains an impact modifier comprising a thermoplastic polyurethane elastomer.

10. The multi-layer article as defined in any of the preceding claims, wherein the polymer composition further comprises a thermoplastic polyurethane elastomer in combination with a thermoplastic copolyester elastomer.

11. The multi-layer article as defined in any of the preceding claims, wherein the container comprises a fuel tank, a hydraulic oil tank, a compressed gas tank, a water tank, or a diesel exhaust fluid tank.

12. The multi-layer article as defined in any of the preceding claims, wherein the container has a volume of from about 4 gallons to about 500 gallons, such as from about 10 gallons to about 110 gallons.

13. The multi-layer article as defined in any of the preceding claims, wherein the lining layer of the container has a density according to ISO Test 1183 of greater than 1 g / cc, such as greater than about 1.1 g / cc, such as greater than about 1.2 g / cc, such as greater than about 1.3 g / cc, and less than about 1.6 g / cc.

14. The multi-layer article as defined in claim 1, wherein the polymer composition comprises the polyoxymethylene polymer blended with the impact modifier, the impact modifier comprising a thermoplastic elastomer, the polyoxymethylene polymer having a melt flow rate of less than about 10 g / 10 min, the polyoxymethylene polymer being present in the polymer composition in an amount of at least about 55% by weight, the impact modifier being present in the polymer composition in an amount of from about 4% by weight to about 27% by weight, and wherein the polymer composition further comprise a nucleant and an antioxidant.

15. The multi-layer article as defined in claim 1, wherein the nucleant comprises a terpolymer.

16. The multi-layer article as defined in claim 1, wherein the polymer composition further contains an acid scavenger, the acid scavenger comprising a carboxylic acid salt.

17. The multi-layer article as defined in claim 16, wherein the acid scavenger comprises a calcium citrate, a calcium propionate, or mixtures thereof,Attorney Docket No.: CICT-1562-PCT (2025P0008)the acid scavenger being present in the polymer composition in an amount from about 0.001 % by weight to about 1 % by weight.

18. The multi-layer article as defined in any of the preceding claims, wherein the polyethylene polymer of the outer layer has been crosslinked.

19. A multi-layer article comprising:a seamless rotationally molded container defining an interior space, the container including a container wall comprised of an outer layer and a lining layer adjacent to and in contact with the outer layer, the outer layer comprising a crosslinked polyethylene polymer, the lining layer being made from a polymer composition comprising a polyoxymethylene polymer having a melt flow rate of less than about 12 g / 10 min blended with impact modifiers comprising a thermoplastic polyurethane elastomer in combination with a thermoplastic copolyester elastomer, and wherein the container has a volume of from about 4 gallons to about 500 gallons.

20. The multi-layer article as defined in claim 19, wherein:the outer layer has a thickness ratio to the lining layer of from about 1.5:1 to about 5:1 and the wall has a total thickness of from about 5 mm to about 8 mm;the container has a multiaxial impact of greater than 40 ftlb-f at 23°C; and the wall of the container has a permeation of less than 2.5 g / m2per day at 40°C according to SAE Test J2665.