Foldable shield
A foldable shield made of polyvinyl alcohol-melanin composite tiles, connected by flexible joints and magnets, addresses the impracticality of military armor by offering lightweight, portable protection against shrapnel and projectiles, meeting NIJ Level IIIA specifications.
Patent Information
- Application Number
- PCT/US2026/026467
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-05
- Filing Date
- 2026-05-04
- Publication Date
- 2026-11-12
AI Technical Summary
Current armor and shielding designed for police and military personnel are inconveniently heavy and large, making them impractical for civilian use, and civilians lack effective protection against shrapnel and projectiles during attacks.
A foldable shield composed of polyvinyl alcohol-melanin composite tiles, connected by flexible joints and magnetic or hook-and-loop strips, which can be assembled into a compact, portable structure for personal protection.
The foldable shield provides lightweight, effective protection against shrapnel and projectiles, allowing civilians to assemble it quickly and carry it easily, meeting NIJ Level IIIA specifications.
Smart Images

Figure US2026026467_12112026_PF_FP_ABST
Abstract
Description
4774-0071W001FOLDABLE SHIELDCROSS-REFERENCE APPLICATION
[0001] This application claims the benefit of U.S. Serial No. 63 / 799,948, filed May 05. 2025, the entirety of which is incorporated herein by reference.FIELD
[0002] The present disclosure relates to a foldable shield. More specifically, the present disclosure relates to a foldable shield for protecting people against shrapnel, explosive materials, and projectiles.DESCRIPTION OF RELATED ART
[0003] The current routine use of explosive devices and projectiles, such as drone-fired projectiles and ballistic missiles, in attacks against civilian populations, for instance in Eastern Europe and the Middle East, by states, terrorists, or criminals, presents a serious and persistent threat to civilian safety. In some areas in which such attacks are frequent, systems have been implemented to issue warning sirens when a threat of attacks against civilians is detected. However, today, most civilians have no protective covering at all if a siren sounds and they are not near a building to hide. For example, in such situations, the official advice from the Israeli government to civilians when a siren sounds and they are in a car or walking and not near a building, is simply to lie flat in a prone position and cover their head with their hands, which is an inadequate position for protection.
[0004] Additionally, while armor and shielding exists for police and military personnel, most current types of armor and shielding designed for police and military personnel are inconveniently heavy and large, so much so that they are not practical for civilian use.SUMMARY
[0005] This Summary is provided to introduce a selection of concepts in a simplified form that are further described below in the Detailed Description. This Summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used as an aid in determining the scope of the claimed subject matter.14929-7619-2059, v. 14774-0071W001
[0006] In one general aspect, a foldable shield can include one or more foldable tile sheets. Each of the one or more foldable tile sheets can include a plurality of tiles connected in series. Adjacent tiles among the plurality of tiles can be connected to each other at flexible joints.
[0007] In some embodiments, the plurality of tiles can be constructed of a polyvinyl alcohol- melanin composite.
[0008] In some embodiments, the polyvinyl alcohol-melanin composite can be about 10% melanin by weight.
[0009] In some embodiments, the polyvinyl alcohol-melanin composite can be about 10% melanin to about 60% melanin by weight.
[0010] In some embodiments, each tile among the plurality of tiles can have a length of approximately 4 inches, a width of approximately 4 inches, and a thickness of approximately 8 millimeters.
[0011] In some embodiments, each of the foldable tile sheets can be configured to be folded into a folded configuration in which the plurality of tiles of each of the foldable tile sheets are vertically stacked.
[0012] In some embodiments, the plurality of tiles of each of the one or more tiles sheets can include three tiles. The one or more foldable tile sheets can each have a length of approximately 4 inches, a width of approximately 4 inches, and a thickness of approximately 24 millimeters in the folded configuration.
[0013] In some embodiments, the one or more foldable tile sheets can each further include tape strips connecting the adjacent tiles to each other at the joints.
[0014] In some embodiments, the one or more foldable tile sheets can include at least two foldable tile sheets. Adjacent foldable tile sheets, among the at least two foldable tile sheets, can be connected to each other at least one joint formed between respective adjacent edge portions of the adjacent foldable tile sheets.
[0015] In some embodiments, the least one joint can be formed by ferromagnetic regions disposed at the respective adjacent edge portions of the adjacent foldable tile sheets, and at least one magnetic strip attached to the ferromagnetic regions.
[0016] In some embodiments, the ferromagnetic regions can include ferromagnetic strips attached to the plurality of tiles of each of the adjacent foldable tile sheets.24929-7619-2059, v. 14774-0071W001
[0017] In some embodiments, the ferromagnetic regions can include ferromagnetic particles embedded in the plurality of tiles of each of the adjacent foldable tile sheets.
[0018] In some embodiments, the at least one joint can be formed by first hook-and-loop strips attached to the respective adjacent edge portions of the adjacent foldable tile sheets, and at least one second hook-and-loop strip attached to the first hook-and-loop strips.
[0019] In some embodiments, the one or more foldable tile sheets can include three foldable tile sheets. Adjacent foldable tile sheets, among the at least one or more foldable tile sheets, can be connected to each other at a joint formed along respective adjacent edge portions of the adjacent foldable tile sheets.
[0020] In some embodiments, the foldable shield can have a length of approximately 12 inches, a width of approximately 12 inches, and a thickness of approximately 24 millimeters in an assembled configuration in which the three foldable tile sheets are unfolded.
[0021] In some embodiments, each tile among the plurality of tiles can have a length of approximately 4 inches, a width of approximately 4 inches, and a thickness of approximately 8 millimeters.
[0022] In another general aspect, a shield can include a substantially flat plate including a plurality of tiles that are connected to each other. The plurality of tiles can be composed of a polyvinyl alcohol-melanin composite.
[0023] In some embodiments, the polyvinyl alcohol-melanin composite can be about 10% melanin by weight.
[0024] In some embodiments, the polyvinyl alcohol-melanin composite can be about 10% melanin to about 60% melanin by weight.
[0025] Other features and aspects will be apparent from the following detailed description, the drawings, and the claims.BRIEF DESCRIPTION OF THE DRAWINGS
[0026] FIG. 1 is a front view of a foldable shield, according to an embodiment.
[0027] FIGS. 2A and 2B are front and bottom side views, respectively, of a tile of a foldable tile sheet of the foldable shield, according to an embodiment.34929-7619-2059, v. 14774-0071W001
[0028] FIG. 3 is a front view of tiles arranged in a row for forming the foldable tile sheet, according to an embodiment.
[0029] FIG. 4A is a front view of the foldable tile sheet in an unfolded configuration, according to an embodiment.
[0030] FIG. 4B is a rear view of the foldable tile sheet of FIG. 4A in the unfolded configuration.
[0031] FIG. 5 is a bottom side view of the foldable tile sheet of FIGS. 4A and 4B in a folded configuration.
[0032] Throughout the drawings and the detailed description, the same reference numerals refer to the same elements. The drawings may not be to scale, and the relative size, proportions, and depiction of elements in the drawings may be exaggerated for clarity, illustration, and convenience.DETAILED DESCRIPTION
[0033] The following detailed description is provided to assist the reader in gaining a comprehensive understanding of the methods, apparatuses, and / or systems described herein. However, various changes, modifications, and equivalents of the methods, apparatuses, and / or systems described herein will be apparent after an understanding of the disclosure of this application. For example, the sequences of operations described herein are merely examples, and are not limited to those set forth herein, but may be changed as will be apparent after an understanding of the disclosure of this application, with the exception of operations necessarily occurring in a certain order. Also, descriptions of features that are known in the art may be omitted for increased clarity and conciseness.
[0034] The features described herein may be embodied in different forms, and are not to be construed as being limited to the examples described herein. Rather, the examples described herein have been provided merely to illustrate some of the many possible ways of implementing the methods, apparatuses, and / or systems described herein that will be apparent after an understanding of the disclosure of this application.
[0035] Throughout the specification, when an element, such as a layer, region, or substrate, is described as being "on," "connected to," or "coupled to" another element, it may be directly "on," "connected to," or "coupled to" the other element, or there may be one or more other44929-7619-2059, v. 14774-0071W001 elements intervening therebetween. In contrast, when an element is described as being "directly on," "directly connected to," or "directly coupled to" another element, there can be no other elements intervening therebetween.
[0036] As used herein, the term "and / or" includes any one and any combination of any two or more of the associated listed items.
[0037] Although terms such as "first," "second," and "third" may be used herein to describe various members, components, regions, layers, or sections, these members, components, regions, layers, or sections are not to be limited by these terms. Rather, these terms are only used to distinguish one member, component, region, layer, or section from another member, component, region, layer, or section. Thus, a first member, component, region, layer, or section referred to in examples described herein may also be referred to as a second member, component, region, layer, or section without departing from the teachings of the examples.
[0038] Spatially relative terms such as "above," "upper," "below," and "lower" may be used herein for ease of description to describe one element’s relationship to another element as shown in the figures. Such spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. For example, if the device in the figures is turned over, an element described as being "above" or "upper" relative to another element will then be "below" or "lower" relative to the other element. Thus, the term "above" encompasses both the above and below orientations depending on the spatial orientation of the device. The device may also be oriented in other ways (for example, rotated 90 degrees or at other orientations), and the spatially relative terms used herein are to be interpreted accordingly.
[0039] The terminology used herein is for describing various examples only, and is not to be used to limit the disclosure. The articles "a," "an," and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise. The terms "comprises," "includes," and "has" specify the presence of stated features, numbers, operations, members, elements, and / or combinations thereof, but do not preclude the presence or addition of one or more other features, numbers, operations, members, elements, and / or combinations thereof.
[0040] Due to manufacturing techniques and / or tolerances, variations of the shapes shown in the drawings may occur. Thus, the examples described herein are not limited to the specific54929-7619-2059, v. 14774-0071W001 shapes shown in the drawings, but include changes in shape that occur during manufacturing.
[0041] The features of the examples described herein may be combined in various ways as will be apparent after an understanding of the disclosure of this application. Further, although the examples described herein have a variety of configurations, other configurations are possible as will be apparent after an understanding of the disclosure of this application.
[0042] The present inventor has recognized a need for devices for protecting people, and particularly civilians, against shrapnel, explosive materials, and projectiles encountered in attacks against civilian populations. Accordingly, the present inventor has developed a foldable shield, as disclosed herein, that is portable, practical for civilian use, and effective to protect people against shrapnel, explosive materials, and projectiles.
[0043] According to recent reports of civilian attacks, a large number of injuries are suffered by people in the perimeter of a hit rather than in the exact location of the hit. Therefore, the foldable shield disclosed herein employs new families of materials that are light and effective against shrapnel and explosive materials that civilians under attack may encounter in the perimeter of a hit.
[0044] Additionally, current siren warning systems that warn civilians of detected attack threats typically give civilians 60 to 90 seconds of warning before a hit. The disclosed foldable shield is configured to be carried in a disassembled state, and can be assembled in substantially less than 60 seconds. Therefore, upon receiving a warning of an attack threat, a civilian would have ample time to assemble the foldable shield.
[0045] Additionally, the disclosed foldable shield employs new structural configurations and shielding materials, such that the foldable shield is light, compact, and portable for average people. For instance, in some embodiments, the foldable shield, when assembled, can have a length of approximately 12 inches, a width of approximately 12 inches, and a thickness of approximately 8 millimeters (0.314 Inches), can weigh about 2 lbs (or about 1 kilogram), and can be assembled in about 10 seconds. Thus, in such embodiments, the foldable shield could be carried in a school bag, a purse, or a briefcase on a routine daily basis.
[0046] Example embodiments of a foldable shield according to the inventive concept are described below.64929-7619-2059, v. 14774-0071W001
[0047] FIG. 1 is a front view of a foldable shield 10, according to an embodiment. In FIG. 1, the foldable shield 10 is shown in an unfolded, assembled configuration. The foldable shield 10 can include a plurality of foldable tile sheets that are connected to each other to form a plate-like structure. For example, as shown in FIG. 1, the foldable shield 10 can include a first tile sheet 100, a second tile sheet 200, and third tile sheet 300 connected in sequence from top to bottom.
[0048] The first foldable tile sheet 100, the second foldable tile sheet 200, and the third foldable tile sheet 300 can each include a plurality of tiles connected in series. For example, the first foldable tile sheet 100 can include a first tile 100a, a second tile 100b, and a third tile 100c connected in series from left to right. Similarly, the second foldable tile sheet 200 can include a first tile 200a, a second tile 200b, and a third tile 200c connected in series from left to right, and the third foldable tile sheet 300 can include a first tile 300a, a second tile 300b, and a third tile 300c connected in series from left to right.
[0049] As will be discussed below in more detail, in some implementations, each of the tiles 100a- 100c, 200a-200c, and 300a-300c can be constructed of a polyvinyl alcohol-melanin (PVA- melanin) composite manufactured by a heat compression method, or a bismuth-melanin composite manufactured by a heat compression method. In some embodiments, the PVA- melanin composite can be about 10% melanin by weight. In some embodiments, the PVA- melanin composite can be about 11% to about 60% melanin by weight. In some embodiments, the PVA-melanin composite can be about 45% melanin by weight. The tiles 100a-100c, 200a-200c, and 300a-300c constructed of the aforementioned composites can meet or exceed NIJ Level IllA.or NIJ Level III specifications, and thus are effective against shrapnel and other projectiles. However, the tiles 100a-100c, 200a-200c, and 300a-300c can be constructed of other materials and can be constructed by other methods.
[0050] An example configuration of the tiles 100a-100c, 200a-200c, and 300a-300c is described below with reference to FIGS. 2A and 2B.
[0051] FIGS. 2A and 2B are front and bottom side views, respectively, of the first tile 100a of the first foldable tile sheet 100, according to an embodiment. Although FIGS. 2A and 2B specifically depict the first tile 100a of the first foldable tile sheet 100, it is to be understood that the illustrations in FIGS. 2A and 2B and the corresponding descriptions thereof apply to all of the tiles 100a-100c, 200a-200c, and 300a-300c.74929-7619-2059, v. 14774-0071W001
[0052] As shown in FIGS. 2A and 2B, the tiles 100a-100c, 200a-200c, and 300a-300c can each have a substantially square shape, and can have a front surface SF, a rear surface SR, a top edge E1, a bottom edge E2, a left edge E3, and a right edge E4. In some embodiments, each of the tiles 100a-100c, 200a-200c, and 300a-300c can have a width WT of about 4 inches, a length LT of about 4 inches, and a thickness TT of about 8 millimeters. However, the tiles 100a-100c, 200a-200c, and 300a-300c are not limited to a specific width, length, and thickness, and any width, length, and thickness are possible. Additionally, other shapes, including but not limited to rectangular shapes, triangular shapes, circular shapes, and oval shapes, are possible for the tiles 100a-100c, 200a-200c, and 300a-300c.
[0053] Example configurations of the foldable tile sheets 100, 200, and 300 are described below with reference to FIGS. 3-4B. Although FIGS. 3-4B specifically depict the first foldable tile sheet 100, it is to be understood that the illustrations in FIGS. 3-4B and the corresponding descriptions thereof apply to all of the foldable tile sheets 100, 200, and 300 and the corresponding tiles 100a-100c, 200-a-200c, and 300a-300c thereof.
[0054] FIG. 3 is a front view of tiles arranged in a row for forming the foldable tile sheet 100, according to an embodiment. As shown in FIG. 3, the foldable tile sheet 100 includes the first to third tiles 100a- 100c arranged such that the top edges E1 of the first to third tiles 100a- 100c are aligned to be substantially colinear, the bottom edges E2 of the first to third tiles 100a-100c are aligned to be substantially colinear, the right edge E4 of the first tile 100a and the left edge E3 of the second tile 100b are adjacent to each other, and the right edge E4 of the second tile 100b and the left edge E3 of the third tile 100c are adjacent to each other. Thus, as is described in more detail below with respect to FIGS. 4A-4B, flexible joints can be formed between the first and second tiles 100a and 100b and between the second and third tiles 100b and 100c, to enable the foldable tile sheet 100 to unfolded to place the foldable shield 10 in its assembled configuration, and folded to place the foldable tile sheet 100 in a compact, folded configuration for storage and / or transportation by a person when the foldable shield 10 is disassembled.
[0055] FIG. 4A is a front view of the foldable tile sheet 100 in an unfolded configuration, according to an embodiment. FIG. 4B is a rear view of the foldable tile sheet 100 the unfolded configuration. The configuration of the foldable tile sheet 100 in FIGS. 4A and 4B corresponds to its configuration in the foldable shield 10 when the foldable shield 10 is84929-7619-2059, v. 14774-0071W001 assembled. As shown in FIGS. 4A and 4B, the foldable tile sheet 100 can include flexible tape strips 20 forming flexible joints between adjacent tiles. In some embodiments, a first flexible tape strip 20 can be attached to the first and second tiles 100a and 100b to form a first flexible joint therebetween, and a second flexible tape strip 20 can be attached to the second and third tiles 100b and 100c to form a second flexible joint therebetween.
[0056] For example, the first flexible tape strip 20 can be attached to an edge portion of the first tile 100a near / including the right edge E4 of the first tile 100a, and an edge portion of the second tile 100a near / including the left edge E3 of the second tile 100b. The second flexible tape strip 20 can be attached to an edge portion of the second tile 100a near / including the right edge E4 of the second tile 100b, and an edge portion of the third tile 100c near / including the left edge E3 of the third tile 100c. As an example, the first flexible tape strip 20 can be attached to the rear surfaces SR of the first and second tiles 100a and 100b, and the second flexible tape strip 20 can be attached to the front surfaces SF of the second and third tiles 100b and 100c. Thus, as described later in more detail, when the foldable shield 10 is disassembled, the foldable tile sheet 100 can be folded at the first and second flexible joints to place the foldable tile sheet 100 in the compact, folded configuration that is practical for storage and transportation of the disassembled foldable shield 10.
[0057] Although FIGS. 4A and 4B illustrate a particular example including the flexible tape strips 220 forming the first and second flexible joints, the first and second flexible joints are not limited to this particular example. For example, in some embodiments, the first flexible tape strip 20 can be attached to the front surfaces SF of the first and second tiles 100a and 100b, and the second flexible tape strip 20 can be attached to the rear surfaces SR of the second and third tiles 100b and 100c. Additionally, in some embodiments, matching hook-and-loop members can be provided to form the first and second flexible joints. Further, in some embodiments, the first and second flexible joints flexible joints can be replaced with first and second pivot assemblies.
[0058] Referring back to FIG. 1, when the foldable shield 10 is in its assembled configuration, the first to third foldable tile sheets 100-300 can be unfolded and configured as described above in the description of FIG. 4 with respect to the first foldable tile sheet 100. In the assembled foldable shield 10, a bottom edge of the first foldable tile sheet 100 (formed by the bottom edges E2 of the first to third tiles 100a- 100c) and a top edge of the second foldable tile sheet 200 (formed by the top edges E1 of the first to third tiles 200a-200c) can 94929-7619-2059, v. 14774-0071W001 be disposed adjacent to each other, and a bottom edge of the second foldable tile sheet 200 (formed by the bottom edges E2 of the first to third tiles 200a-200c) and a top edge of the third foldable tile sheet 300 (formed by the top edges E1 of the first to third tiles 300a-300c) can be disposed adjacent to each other.
[0059] Still referring to FIG. 1, adjacent foldable tile sheets among the first to third foldable tile sheets 100-300 can be connected to each other at shield joints formed between respective adjacent edge portions of the adjacent foldable tile sheets. More specifically, one or more first shield joints can be formed between a bottom edge portion of the first foldable tile sheet 100 (near / including the bottom edge of the first foldable tile sheet 100) and a top edge portion of the second foldable tile sheet 200 (near / including the top edge of the second foldable tile sheet 200), and one or more second shield joints can be formed between a bottom edge portion of the second foldable tile sheet 200 (near / including the bottom edge of the second foldable tile sheet 200) and a top edge portion of the third foldable tile sheet 300 (near / including the top edge of the third foldable tile sheet 300).
[0060] The first shield joint(s) can be formed by lower ferromagnetic regions 50 disposed at lower edge portions of the first to third tiles 100a-100c (near / including the lower edges E2 of the first to third tiles 100a-100c), upper ferromagnetic regions 52 disposed at upper edge portions of the first to third tiles 200a-200c (near / including the upper edges E1 of the first to third tiles 200a-200c), and two magnetic strips 30 attached to the lower and upper ferromagnetic regions 50 and 52 to securely attach connect the first and second foldable tile sheets 100 and 200 to each other. The second shield joints can be formed by lower ferromagnetic regions 50 disposed at lower edge portions of the first to third tiles 200a- 200c (near / including the lower edges E2 of the first to third tiles 200a-200c), upper ferromagnetic regions 52 disposed at upper edge portions of the first to third tiles 300a- 300c (near / including the upper edges E1 of the first to third tiles 300a-300c), and two magnetic strips 30 attached to the lower and upper ferromagnetic regions 50 and 52 to securely attach connect the second and third foldable tile sheets 200 and 300 to each other. In some embodiments, each of the two magneticstrips 30 can have a width of about 0.5 inches, length of about 4 inches, and a thickness of about 2 millimeters. Although two magnetic strips 30 are shown in each of the first and second shield joints, in alternate embodiments, a longer single magnetic strip 30 can be provided in each of the first and second shield joints, or three or more shorter magnetic strips 30 can be provided in each of the first and second shield joints.104929-7619-2059, v. 14774-0071WG01
[0061] The lower and upper ferromagnetic regions 50 and 52 can be formed of iron, for example.However, other materials can be used for the lower and upper ferromagnetic regions 50 and 52. In the illustrated embodiment of FIG. 1, the lower and upper ferromagnetic regions 50 and 52 can be ferromagnetic strips (e.g., iron strips) attached to the tiles 100a-100c, 200a-200c, and 300a-300c. In some implementations, the ferromagnetic strips can have a width of about 0.10 millimeters to about 0.25 millimeters.
[0062] In alternate embodiments, the lower and upper ferromagnetic regions 50 and 52 can be formed by ferromagnetic particles (e.g., iron particles) embedded in the tiles 100a-100c, 200a-200c, and 300a-300c.
[0063] Additionally, in other embodiments, the first shield joint can be formed by lower hook-and- loop strips attached to the lower edge portions of the first to third tiles 100a-100c, upper hook-and-loop strips attached to the upper edge portions of the first to third tiles 200a- 200c, and one or more hook-and-loop strips attached to the lower and upper hook-and- loop strips. Further, in such other embodiments, the second shield joint can be formed by lower hook-and-loop strips attached to the lower edge portions of the first to third tiles 200a-200c, upper hook-and-loop strips attached to the upper edge portions of the first to third tiles 300a-300c, and one or more hook-and-loop strips attached to the lower and upper hook-and-loop strips.
[0064] As a result of the construction described above, the foldable shield 10 can be quickly assembled to have a rigid plate-like structure effective to protect a person from explosive and projectile attacks. For example, the foldable shield 10 can be held over a person’s head to protect the person’s head.
[0065] In embodiments in which the foldable shield 10 includes the first to third tiles sheets 100- 300 each including three tiles 100a-100c, 200a-200c, and 300a-300c, respectively, and each of the tiles 100a- 100c, 200a-200c, and 300a-300c have the width WTof about 4 inches, the length l_Tof about 4 inches, and the thickness TTof about 8 millimeters, the assembled foldable shield 10 can have a width W of about 12 inches, a length L of about 12 inches, and the thickness TT of about 8 millimeters. However, it should be understood that these dimensions are not limiting and can vary based on the number and dimensions of the tiles and the number of foldable tile sheets.
[0066] Although the embodiment of FIG. 1 is shown and described as including three foldable tile sheets 100, 200, and 300 each including three tiles 100a- 100c, 200a-200c, and 300a-114929-7619-2059, v. 14774-0071W001 300c, respectively, a foldable shield according to the inventive concept is not limited to any particular number of foldable tile sheets or any particular number of tiles in each foldable tile sheet. Additionally, while the foldable shield 10 is shown and described herein as a substantially flat plate, in other embodiments, the tiles and / or the foldable tile sheets can have different shapes such that a foldable shield can have a different overall shape, including but not limited to a curved plate shape.
[0067] The foldable shield 10 can be disassembled by detaching the first to third foldable tile sheets 100-300 from each other. For example, in the embodiment illustrated in FIG. 1 , the magnetic strips 30 can be detached from the respective lower and upper ferromagnetic regions 50 and 52 to detach the foldable tile sheets 100-300 from each other. In other embodiments that employ first hook-and-loop strips disposed on the tiles 100a-100c, 200a-200c, and 300a-300c, and second hook-and-loop strips attached to the respective first hook-and-loop strips, the second hook-and-loop strips can be detached from the respective first hook-and-loop strips to detach the foldable tile sheets 100-300 from each other. Once the foldable shield 10 is disassembled, the foldable tile sheets 100-300 can each be folded into the compact, folded configuration illustrated for the first foldable tile sheet 100 in FIG. 5. Thus, the disassembled foldable shield 10, including the folded foldable tile sheets 100-300 and the detached magnetic strips 30 (or the detached second hook-and-loop strips) can be placed in a bag or case for storage or transportation by a person. FIG. 5 is described in greater detail below, with the understanding that the description of the folded configuration of the first foldable tile sheet 100 in FIG. 5 also applies to the folded configurations of the second and third foldable tile sheets 200 and 300.
[0068] Referring to FIG. 5, when the first foldable tile sheet 100 is in the compact, folded configuration, the first foldable tile sheet 100 is folded at the first and second flexible joints (e.g., at portions of the first and second flexible tape strips 20 between the adjacent tiles such that the first to third tiles 100a- 100c are vertically stacked. Due to the configuration of the first and second flexible tape strips 20 described above with respect to FIGS. 4A and 4B, the first foldable tile sheet 100 can be folded such that the second tile 100b is disposed on top of the first tile 100a and the third tile 10oc is disposed on top of the second tile 100b. Thus, the rear surface SR of the second tile 100b can be disposed on top of and in contact with the rear surface SR of the first tile 100a, and the front surface SF of the third tile 100c can be disposed on top of and in contact with the front surface SF of the second124929-7619-2059, v. 14774-0071W001 tile 100b. The left edge E3 of the second tile 100b and the right edges E4 of the first and third tiles 100a and 100c can be substantially aligned with each other on a left side of the stack. The right edge E4 of the second tile 100b and the left edges E3 of the first and third tiles 100a and 100c can be substantially aligned with each other on a right side of the stack. The top edges E1 of the first to third tiles 100a-100c can be substantially aligned with each other at a top side of the stack, and the bottom edges E2 of the first to third tiles 100a- 100c can be substantially aligned with each other at a bottom side of the stack. Therefore, the first to third tiles 100a-100c can be stacked in the folded configuration of the foldable tile sheet 100 such that there is minimal protrusion of any edges of any of the first to third tiles 100a-100c with respect to the corresponding edges of the other tiles among the first to third tiles 100a-100c.
[0069] As illustrated in FIG. 5, in embodiments in which the first to third tiles 100a-100b each have the width WT of about 4 inches, the length LT of about 4 inches, and the thickness TT of about 8 millimeters, the first foldable tile sheet 100 can have the width WT of about 4 inches, the length LTof about 4 inches and a thickness Tsof about 24 millimeters. However, it should be understood that these dimensions are not limiting and can vary based on the number and dimensions of the tiles in the first foldable tile sheet 100.
[0070] In addition to the foldable shield 10, an added layer of protection against shock waves can be provided. For example, a folded plastic bag with an air valve can be unfolded. In some implementations, the plastic bag can be about 5 millimeters thick. The folded plastic bag can be expanded to a one inch thick cushion by blowing into the folded plastic bag or flowing gas into the folded plastic bag with an optional gas cartridge. Then, the expanded plastic bag can be placed between a person’s head and the foldable shield 10.
[0071] Manufacturing Melanin Composites for Shield Tiles
[0072] The melanins comprise a family of biopolymer pigments. A frequently used chemical description of melanin is that it is comprised of “heteropolymers of 5-6-dihydroxyindole and 5- 6-dihydroxyindole-2-carboxylic acid” (Bettingeret al., 2009). Melanins are polymers produced by polymerization of reactive intermediates. The polymerization mechanisms include, but are not limited to, autoxidation, enzyme-catalyzed polymerization and free radical initiated polymerization. The reactive intermediates are produced chemically, electrochemically, or enzymatically from precursors. Suitable enzymes include, but are not limited to, peroxidases, catalases, polyphenol oxidases, tyrosinase, tyrosine134929-7619-2059, v. 14774-0071W001 hydroxylases, and laccases. The precursors that are connected to the reactive intermediates are hydroxylated aromatic compounds. Suitable hydroxylated aromatic compounds include, but are not limited to 1) phenols, polyphenols, aminophenols and thiophenols of aromatic or polycyclicaromatic hydrocarbons, including, but not limited to, phenol, tyrosine, pyrogallol, 3-aminotyrosine, thiophenol and a-naphthol; 2) phenols, polyphenols, aminophenols, and thiophenols of aromatic heterocyclic or heteropoly cyclic hydrocarbons such as, but not limited to, 2-hydroxypyrrole,4-hydroxy-l,2-pyrazole, 4- hydroxypyridine, 8-hydroxyquinoline, and 4,5-dihydroxybenzothiazole.
[0073] The term melanin includes naturally occurring melanin polymers as well as melanin analogs as defined below. Naturally occurring melanins include eumelanins, phaeomelanins, neuromelanins and allomelanins.
[0074] As used here, the term “melanin” refers to melanins, melanin precursors, melanin analogs, melanin variants, melanin derivatives, melanin-like pigments, and / or melanosomes, unless the context dictates otherwise. The term “melanin-like” also refers to hydrogels with melanin-like pigmentation and quinoid electrophilicity. This electrophilicity can be exploited for facile coupling with biomolecules.
[0075] As used herein, the term “melanin analog” refers to a melanin in which a structural feature that occurs in naturally-occurring or enzymatically-produced melanins is replaced by a substituent divergent from substituents traditionally present in melanin. An example of such a substituent is a selenium, such as selenocysteine, in place of sulfur.
[0076] As used herein, the term “melanin derivative” refers to any derivative of melanin which is capable of being converted to either melanin or a substance having melanin activity. An example of a melanin derivative is melanin attached to a dihydrotrigonelline carrier such as described in Bodor, N., Ann. N.Y. Acad. Sci. 507, 289 (1987), which enables the melanin to cross the blood-brain barrier. The term melanin derivatives is also intended to include chemical derivatives of melanin, such as an esterified melanin.
[0077] As used herein, the term “melanin variant” refers to various subsets of melanin substances that occur as families of related materials. Included in these subsets, but not limited thereto, are:
[0078] (1) Naturally occurring melanins produced by whole cells that vary in their chemical and physical characteristics;144929-7619-2059, v. 14774-0071W001
[0079] (2) Enzymatically produced melanins prepared from a variety of precursor substrates under diverse reaction conditions;
[0080] (3) Melanin analogs in which a structural feature that occurs in (1) or (2) above is replaced by an unusual substituent divergent from the traditional; and
[0081] (4) Melanin derivatives in which a substituent in a melanin produced in (1), (2) or (3) above is further altered by chemical or enzymatic means.
[0082] As used herein, the term “Melanin-like substances” refers to heteropolymers of 5-6- dihydroxyindole and 5-6-dihydroxyindole-2-carboxylic acid which have one or more properties usually associated with natural melanins, such as UV absorption or semiconductor behavior.
[0083] Melanin Sources
[0084] Melanin and Melanin-like compounds can be obtained:
[0085] -by extraction and purification from natural sources, e.g. cephalopods such as cuttlefish (e.g. Sepia) or squid (e.g. Loligo), bird feathers (e.g. from species with black strains such as Silkie chickens);
[0086] -by chemical synthesis, whether water or non-water based e.g. (Deziderio, 2004) (daSilva et al., 2004; Lawrie et al., 2008; Pezzella et al., 2006);
[0087] -by electrochemical synthesis, e.g. (Meredith et al., 2005); -by bioreactors created by utilization of natural or genetically altered bacteria, fungi, lichens, or viruses e.g.(della- Cioppa , 1998).
[0088] Cephalopod inks are natural composites of melanin with other materials, including peptidoglycans, amino acids, proteins, metals, and chemicals and enzymes (such as tyrosinase) which are involved in the synthesis of melanin, and other materials. Cephalopod inks include cuttlefish (such as Sepia), squid, and octopus inks. There is some variation among different species of the percentages of these components. Reports of cephalopod ink components include: Derby, C.D. 2014 Cephalopod Ink: Production, Chemistry, Functions and Applications Marine Drugs 12, 2700-2730; doi:10.3390 / md12052700, and Magarelli M, Passamonti P, Renieri C. 2010. Purification, characterization and analysis of sepia melanin from commercial sepia ink (Sepia Officinalis) . Rev CES Med Vet Zootec; Vol 5 (2): 18-28.154929-7619-2059, v. 14774-0071W001
[0089] Melanin Manufacturing and Fabrication
[0090] Melanin and melanin-like compounds can be manufactured as particles, nanoparticles, dust, beads, or fibers that are woven or non-woven e.g. by methods as described by (Greiner and Wendorff, 2007), sheets e.g. (Meredith et al., 2005), films (daSilva et al., 2004), plates, bricks, chars, spheres, nodules, balls, graphite-like sheets and shards, liquids, gels, or solids (e.g. thermoplastic or thermoset), and by common chemical engineering molding and fabrication methods or custom methods. Sheets can range from one molecular layer to several millimeters. Fibers can range from nanometers to several millimeters.
[0091] The melanin material may be natural or synthetic, with natural pigments being extracted from plant and animal sources, such as squid, octopus, mushrooms, cuttlefish, and the like. In some cases, it may be desirable to genetically modify or enhance the plant or animal melanin source to increase the melanin production. Melanins are also available commercially from suppliers.
[0092] The following procedure describes an exemplary technique for the extraction of melanin from cuttlefish (Sepia Officinalis). 100 gm of crude melanin are dissected from the ink sac of 10 cuttlefish and washed with distilled water (3*100 ml). The melanin is collected after each wash by centrifugation (200*g for 30 minutes). The melanin granules are then stirred in 800 ml of 8 M Urea for 24 hours to disassemble the melanosomes. The melanin suspension is spun down at 22,000*g for 100 minutes and then washed with distilled water (5*400 ml). The pellet is washed with 50% aqueous DMF (5*400 ml) until a constant UV baseline is achieved from the washes. Finally, the pellet is washed with acetone (3*400 ml) and allowed to air dry. Synthetic melanins may be produced by enzymatic conversion of suitable starting materials, as described in more detail hereinbelow. The melanins may be formed in situ within the porous particles or may be preformed with subsequent absorption into the porous particles.
[0093] Suitable melanin precursors include but are not limited to tyrosine, 3,4-dihydroxy phenylalanine (dopa), D-dopa, catechol, 5-hydroxyindole, tyramine, dopamine, m- aminophenol, oaminophenol, p-aminophenol, 4-aminocatechol, 2-hydroxyl-1,4- naphthaquinone (henna), 4-methyl catechol, 3,4-dihydroxybenzylamine, 3,4- dihydroxybenzoic acid, 1,2-dihydroxynaphthalene, gallic acid, resorcinol, 2-chloroaniline, p-chloroanisole, 2-amino-p-cresol, 4,5-dihydroxynaphthalene2,7-disulfonicacid, o-cresol,164929-7619-2059, v. 14774-0071W001 m-cresol, p-cresol, and other related substances which are capable of being oxidized to tan, brown, or black melanin-like compounds capable of absorbing ultraviolet radiation when incorporated in the polymeric particle matrix of the present disclosure. Combinations of precursors can also be used.
[0094] The melanin precursor is dissolved in an aqueous solution, typically at an elevated temperature to achieve complete solution. A suitable amount of the enzyme tyrosinase (EC 1.14.18.1) is added to the solution, either before or after the melanin precursor. The concentration of tyrosinase is not critical, typically being present in the range from about 50 to about 5000 U / ml. The solution is buffered with an acetate, phosphate, or other suitable buffer, to a pH in the range from about 3 to 10, usually in the range from about 5 to 8, more usually being about 7. Melanin like pigments can be obtained using suitable precursors even in the absence of an enzyme just by bubbling oxygen through a solution of a precursor for an adequate period of time. Melanin material may be obtained by treatment of, e.g, cuttlefish ink or squid ink in a microwave, optionally with mixing. The inventor has found that microwaving can be used for the preparation of melanin formulations. The compositions and methods as disclosed herein may be produced and practiced using a variety of heating techniques, such as, for example, infrared heating, microwave heating, convection heating, laser heating, sonic heating, or optical heating. For example, it was found that drying melanin in a microwave oven made possible the preparation of large amount of melanin from cuttlefish ink in a very short period of time. In an exemplary embodiment, cuttlefish ink was placed at 40°C in a conventional oven and required 18 days to reduce the material to 40% of its original weight. In a 900 watt microwave oven, the same degree of drying was achieved in 12 minutes.
[0095] The disclosure provides a method for formulation of melanin by applying a hydraulic press to melanin partially dried in a microwave oven. In exemplary embodiments, hydraulic presses for this use may range in capacity from, for example, about 1 ton / sq. in. to about 500 tons / in2 approximately. The disclosure provides a method wherein the hydraulic press applies compression of approximately 500 tons / in2. In an exemplary embodiment, commercial cuttlefish ink was dried in a 900 watt microwave oven so that the product was 30% or 35% of the initial weight. A blender was used to mix and grind the melanin. A variety of formulations were made. In one formulation, the 30% preparation was mixed with 7% iron filings, and then the blender was used to mix again. In another formulation, 35% slabs were alternated with 30% slabs to create a layered composite. Each174929-7619-2059, v. 14774-0071W001 formulation was subjected to compression in a 20 ton / in2 hydraulic press for about 20 minutes. Because the platen was approximately 3.5 in2, it is estimated that a force of approximately 3265 pounds / sq. in. was exerted on each sample formulation.
[0096] The disclosure provides for the use of formulations of melanin produced by, for example, microwaving and hydraulic press compression to reduce penetration of bullets and other projectiles. The melanin produced by the methods of the disclosure proved effective in reducing the penetration of a bullet. In an exemplary embodiment, two slabs of melanin were produced by placing cuttlefish ink at 40°C in a conventional oven and dried for 18 days to reduce the material to 40% of its original weight. In an alternative embodiment, cuttlefish ink was placed in a 900 watt microwave oven, and dried for 12 minutes to form two slabs. Each slab was approximately 3.5 in square. One slab was 1 inch thick and 1 slab was 0.5 in. thick. Both slabs were placed together in a wood frame to create a 1.5 inch thick sample of melanin. Several blocks of ballistic clay, approximately 3.5 in. square were placed behind the melanin sample. A control was created separately where the melanin sample was replaced by a (dummy) ballistic clay block. 9 mm bullets were fired at approximately 1200 ft / sec.
[0097] In the experimental setup, the bullet penetrated the melanin and then went a depth of approximately 6 cm into the clay. In the control setup the bullet penetrated the initial (dummy) clay block, and then penetrated 12 cm into the clay. This demonstrated that the melanin formulation showed effectiveness in reducing the bullet's penetration compared to the clay control.
[0098] The disclosure provides for the use of elemental metals mixed with melanin to create new formulations of melanin with novel properties. The metals may be, for example, iron, copper, zinc, magnesium, manganese, bismuth, calcium, enamel, cesium, radium, strontium, thorium, uranium, or combinations thereof. In an exemplary embodiment, elemental iron was mixed with melanin in the form of dried cuttlefish ink resulted in unexpected hardness of the material while it remains somewhat flexible. This is an entirely novel finding since, although metal ions are known to bind to the melanin, it does not appear that anyone has experimented with or reported that elemental iron can bind. This new disclosure is based on the finding that iron and other elemental metals including, for example, copper, zinc, magnesium, manganese, bismuth, calcium, enamel, cesium, radium, strontium, thorium, or uranium, can bind to melanin and organize it in novel ways which confer upon it new properties. For instance, the new properties conferred will 184929-7619-2059, v. 14774-0071W001 include enhanced hardness, stiffness, impact resistance, electrical conductivity, capacitance, semiconductor properties, and enhanced ability to absorb radiation including x-ray and gamma ray.
[0099] In an exemplary embodiment, cuttlefish ink was dried using a microwave oven to 40% of its original weight. Iron filings were added so that they comprised 0.5% of the final formulation. The material felt harder than a similar sample without the 0.5% iron filings.
[0100] In some embodiments, melanins are incorporated into other materials and used for many useful applications, such as:
[0101] 1. Melanin and melanin-like compounds can be incorporated into: polymers, metals, salts, ceramics of many types, clothing, construction materials, existing armor materials including Kevlar and ceramics, other natural materials or their synthetic mimics, materials for implantation into human or mammalian living beings.
[0102] 2. A small percentage of melanin confers new or improved properties on resultant material: Another aspect of the present disclosure is that small amounts of melanin and of melanin like substances will impart to a mixture of melanin with other substances, such as a matrix or polymer, properties which are unexpected. Generally, 1 to 5% of melanin will impart desired properties to a mixture or composite, whereas small incremental improvement in properties will be gained by increasing up to 35%. In exemplary embodies as disclosed herein, melanin may be present at about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, at a range of about 1% to about 10%, at a range of about 2% to about 8%, at a range of about 3% to about 7%, at a range of about 1% to about 4%, at a range of about 2% to about 5%.
[0103] Examples of such unexpected properties are resistance to impact, ultraviolet light, radiation, heat, flame, chemical agents and toxins, biological agents and toxins, and to abrasion.
[0104] 3. Hydration effects and control: It is another aspect of the present disclosure that the control and maintenance of hydration of melanin and melanin like substances (or nonwater solvent or matrix concentration for melanins made from organic solvents) is critical for the applications described herein, including armor and shielding. Published research describes the effect of hydration on electrical conductivity, and on the ability to absorb radiation from the electromagnetic spectrum. The present disclosure includes the aspect194929-7619-2059, v. 14774-0071W001 that when melanin or melanin-like substances are extracted or synthesized, manufactured or fabricated, incorporated in any way with other substances, whether by mixtures, impregnation, layering, compositing, that control and maintenance of desired levels of hydration (and non-water solvent concentration for melanins made from organic solvents) may be critical to achieving and preserving the desired combination of properties. Much of the published research on melanin in the biological, chemical, physics, and electronics literature reports work done using commercially available melanin from Sigma-Aldrich Corp. (St. Louis, Missouri) which is prepared using lyophilization, thus dehydrating it. The present disclosure includes recognition that for the purposes set forth in this disclosure, such as armor and shielding, hydration and control of hydration may be critical for the properties desired in the final material, and the use of highly desiccated or lyophilized melanin may in many instances be undesirable. However, in certain aspects of the disclosure, desiccated or lyophilized melanin may be appropriate.[00105J 4. Oxygenation effects and control: It is another aspect of the present disclosure that the control and maintenance of oxygenation, or of lack of access to oxygen, by incorporating melanin into materials that control this factor, or by restricting use to environments that control or restrict this factor, may be critical for certain characteristics to be achieved for shielding, armor, flame retardancy, heat resistance, and cold resistance.
[0106] 5. Incorporation methods for melanin into other materials includes, for example:mixtures, covalent or non-covalent binding, printing, stamping, electrochemical deposition, metallic salt binding, adhering, and layering in composites. In certain embodiments, the compositions and methods of the disclosure may be produced or practiced using molding techniques such as transfer molding, resin film infusion, resin transfer molding, and structural reaction injection molding (SRIM). In certain embodiments, the compositions and methods of the disclosure may be produced or practiced using molding techniques such as a vacuum assisted resin transfer molding process (VARTM).[00107J Composites
[0108] Process aids and modifiers are materials commonly used to facilitate polymer fabrication, to help compatibilize the mixture of polymers, ceramics, and other additives, and the like, to increase fire resistance, or to modify other properties, other than primary ballistic protection properties. Any of these materials that are desirable for fabricating or204929-7619-2059, v. 14774-0071W001 using the new lightweight ballistic protection materials may be incorporated into the current disclosure, including but not limited to materials such as silicones, phthalates, bromides, and the like.
[0109] Other additives, present in amounts not exceeding 10% by weight, if any, may also be included. These materials may include, but are not limited to adhesion aides, colorants, fibers (carbon, polyaramid, polyethylene, etc.), fillers (talc, sand, microballoons) that further serve to modify the process-ability, stability, durability, or appearance of the objective ballistic protection materials.
[0110] Any suitable ceramic materials may be used in the composite composition in accordance with the current disclosure. In one embodiment the ceramic powders or particles may be selected from the group consisting of alumina, boron carbide, boron nitride, mullite, silica, silicon carbide, silicon nitride, magnesium boride, multi-walled carbon nanotubes, single walled carbon nanotubes, group IVB, VB and VIB metal sulfide nanotubes, titanium boride, titanium carbide, and diamond.
[0111] The current disclosure is also directed to methods of preparing impact protection materials. In one embodiment, the impact protection material is formed by a simple process of mixing the starting materials without melt processing prior to the final molding step. This simplifies the processing, as it is not necessary to undertake the possibly complicated step of melt processing with its accompanying difficulties in dispersion and equipment wear.
[0112] Although such a simple mixing process may be used, other processes for forming the ballistic protection material of the current disclosure can also be utilized. These include melt compounding, in which the ceramic and the polymer are intimately mixed while the polymer is in the molten state. In this embodiment the mixing can be done in any suitable standard machinery such as single and twin-screw extruders (both co- and counterrotating), Henschel mixers, cokneaders, etc. An additional technique that can be used is solvent mixing in which the ceramic and the polymer are mixed while the polymer is dissolved in the appropriate solvent. In such an embodiment any suitable solvent may be utilized.
[0113] The current disclosure is also directed to articles made with the impact resistant and / oror ballistic protection material in accordance with the above processes. Impact and / or ballistic protection materials of the present disclosure may be fabricated into any214929-7619-2059, v. 14774-0071W001 suitable article, including but not limited to sheets, slabs, disks, or more complex shapes, of varying thicknesses and sizes.
[0114] Using such construction techniques, the impact resistant and / or ballistic protection materials of the present disclosure may be used together with other ballistic materials, including but not limited to woven ballistic fabrics (such as but not limited to polyaramid or polyethylene fabrics), metals, ceramics, and the like to form ballistic protection articles, such as, for example, helmets, shields, sheets or panels, or body armor. In another example, a foldable shield using the inventive material may be fabricated by first forming a woven fiber vest containing pockets then sewing flat or curved panels or tiles comprising the composite into the pockets. The foldable shield or panels may also be incorporated into a number of blast or ballistic shields or armor, such as, for example, blast / ballistics shields or armor for personal use, vehicles, aircraft and watercraft like cars, trucks, vans, personnel carriers, limousines, trailers, helicopters, cargo planes, rail cars, boats and ships; armor or blast / ballistic protection for small buildings, especially military command posts and mobile headquarters; armor or blast / ballistic protection for cargo containers; armor or blast / ballistic protection for equipment housing, such as, for example, computers, communications equipment; and generally mobile or stationary blast or ballistic protection panels.
[0115] In an embodiment, a structure is provided. The structure includes bonded alternating layers of at least a melanin material and at least one of a for example, fibrous sheet, a plastic sheet, a plastic plate, a ceramic sheet, a ceramic plate, and a multilayer ply, the multilayer ply comprising multiple fibrous sheets bonded together.
[0116] In another embodiment, a structure is provided. The structure includes alternating layers of melanin material wherein said layers are bonded to each other. In another embodiment, a structure is provided. The structure includes alternating layers of melanin material wherein said layers are joined to each other by an array of oriented nanostructures.
[0117] In yet another embodiment, a method for fabricating a melanin composite is provided. The method includes providing a first layer, the layer comprising at least a fibrous sheet, metal and / or or a multilayer laminate; applying a second layer to the first layer, the layer comprising an melanin material; applying a third layer to the second layer, the layer comprising another fibrous sheet, metal and / or multilayer laminate; bonding or224929-7619-2059, v. 14774-0071W001 joining the first layer to the second layer; and bonding or joining the second layer to the third layer.
[0118] In another embodiment, a method for fabricating a melanin composite is provided.The method includes providing a first layer, the layer comprising at least a fibrous sheet, metal and / or a multilayer laminate; applying a second layer to the first layer, the layer comprising a liquid-phase gel precursor; applying a third layer to the second layer, the layer comprising another fibrous sheet, metal and / or or multilayer laminate; bonding or joining the first layer to the second layer; and bonding or joining the second layer to the third layer.
[0119] In yet another embodiment, a method for fabricating a melanin composite is provided. The method includes providing two layers of melanin material, and bonding the two layers together. In another embodiment, a method for fabricating a melanin composite is provided. The method includes providing a liquid-phase; forming a gel from the liquidphase precursor; and optionally forming a second gel in contact with the first gel.
[0120] In an embodiment, a composition is provided. The composition includes melanin and non-melanin material and embedding the melanin material within the non-melanin material.
[0121] Melanin Comprising Metal(s)
[0122] The disclosed method and materials takes advantage of the fact that melanin is rather unique among armor-like materials in the following respect. Melanin has multiple functional groups (e.g. potential chemical binding locations) which can bind metals (Hong, L. and Simon, J.D., 2004, Photochem. Photobiol., 80:477-481). Many melanins have been demonstrated to possess at least four functional groups with regard to binding of metals: carboxyl, hydroxyl, phenolic, and amine. Metals can be linked, either covalently or non- covalently, absorbed, adsorbed, or chelated to specific functional groups with multiple beneficial effects including: strengthening the bonds between the atoms in the melanin polymer, adding properties of each individual metal dopant, such as density, weight, resistance to penetration or abrasion or radiation, etc. Additionally, some metals can bind to more than one functional group, and conditions such as pH and temperature can determine the preference of a metal for one or the other functional group.234929-7619-2059, v. 14774-0071W001
[0123] It is known that once melanin and / or melanosomes are doped with a single metal, a second metal can be applied, in some instances, without dislodging the first metal (Hong, L. and Simon, J.D., 2007, J. Phys. Chem. B 111:7938-7947). As disclosed herein, more than one metal can simultaneously be used to dope melanin to enhance its impactresistance and other protective properties. For instance, the metals bismuth and / or zinc can be linked to, for example, melanin’s carboxyl group, and then copper could be linked to, for example, melanin’s hydroxyl group. Also, some of the sites of one specific functional group can be loaded with one metal, while other unoccupied sites of the same functional group can then be loaded with a another metal. These sorts of manufacturing methods for improving the melanin’s properties will lead to a variety of desirable properties regarding protective effect, which can be adjusted and tuned to particular applications.
[0124] Biological Polymers
[0125] The term “biological polymer” according to the disclosure, it is understood collagen and its derivatives, hyaluronic acid, its salts and its derivatives, alginates, synthetic polymers, elastin and biological polymers, and mixtures thereof. Preferably, the biological polymer may comprises compounds chosen from collagen, collagen of porcine origin, collagen of bovine origin, crosslinked collagens, hyaluronic acid, its salts and its derivatives, lactic acid polymers, methacrylate derivatives, calcium phosphate derivatives, polyacrylamides, polyurethanes, polyalkylimide gels, polyvinyl microspheres, silicones, silica (SiO2) polymers, and mixtures thereof.
[0126] Collagen is a fibrous protein, of approximately 300 kDa, which makes up the connective tissue in the animal kingdom. It may be of human or nonhuman origin, in particular of porcine or bovine origin. Collagen derivatives include, inter alia, crosslinked collagens.
[0127] The composites of the disclosure may be formed from a wide variety of polymers, including natural polymers such as carboxylmethylcellulose, cellulose acetate phthalate, ethylcellulose, methylcellulose, arabinogalactan, nitrocellulose, propylhydroxycellulose, and succinylated gelatin; and synthetic polymers such as polyvinyl alcohol, polyethylene, polypropylene, polystyrene, polyacrylamide, polyether, polyester, polyamide, polyurea, epoxy, ethylene vinyl acetate copolymer, polyvinylidene chloride, polyvinyl chloride, polyacrylate, polyacrylonitrile, chlorinated polyethylene, acetal copolymer, polyurethane,244929-7619-2059, v. 14774-0071W001 polyvinyl pyrrolidone, poly(p-xylene), polymethylmethacrylate, polyvinyl acetate, polyhydroxyethyl methacrylate, and combinations thereof.
[0128] Melanin Metal Composites
[0129] An example of a metal composite with both offensive and defensive properties enhanced by multiple metal bindings, would be the following. An outer melanin layer facing the environment, that is impregnated with radioactive substances, would be joined to an inner layer, impregnated with radiation absorbing or reflecting metals, which protects the person or tank wearing the composite from the radiation. This would have several applications, as described below.
[0130] On the battlefield the radiation from this sort of composite would be harmful and perhaps lethal to the enemy soldiers. Even the knowledge that a soldier or tank wearing a melanin composite is radioactive would discourage close proximity attacks. In the context of an epidemic caused by a microbe, the composite suit would sterilize a zone around the wearer or tank in a short period of time. This would enhance the safety of the suit or tank against the epidemic dangerous organisms, for example when a researcher or rescuer needs to enter a contaminated zone.
[0131] Binder
[0132] Binders are useful in fabricating materials from non or loosely assembled matter.For example, binders enable two or more surfaces to become united. In certain embodiments, non-melanin material may be included in the compositions and methods of the disclosure and may be a binder. In exemplary embodiments, any adhesive material, such as phenolic resins, ureaformaldehyde resins, melamine formaldehyde resins, hyde glue, aminoplast resins, epoxy resins, acrylate resins, latexes, polyester resins, urethane resins, and mixtures thereof may be used as a binder. Suitable binders include glue, varnish, epoxy resins, phenolic resins, polyurethane resins. In exemplary embodiments, the binder may be, for example, glue, which may be selected from the group consisting of Clear Weld, LOCTITE® Heavy Duty Epoxy, LOCTITE® Epoxy Metal / Concrete, LOCTITE INSTANT-MIX®, LOCTITE®, LOCTITE® BULLDOG, LOCTITE® PL Marine Adhesive Sealant, E6000®, (E6000 STITCHLESS®, E6000 EXTREME TACK®, E6000 FABRI-FUSE®, PRO-POXY® 20, TITEBOND III®, TITEBOND III ULTIMATE WOOD GLUE®, FIBER FIX SUPER TAPE, ELMER’S SCHOOL GLUE NATURALS®, ELMER'S GLUE-ALL®, Elmer's Multi Purpose All Glue, KRAZY GLUE®, LIQUID NAILS®,254929-7619-2059, v. 14774-0071W001 PRODUTY ® HEAVY DUTY CONSTRUCTION ADHESIVE, Firmo Liquid, Welbond Universal Adhesive, and combinations thereof.
[0133] Thermally curable resins suitable for use in accordance with the compositions and methods of the disclosure are preferably selected from the group consisting of phenolic resins, urea formaldehyde resins, melamine-formaldehyde resins, epoxy resins, acrylate resins, urethane resins, melamine resins, alkyd resins, and polyimide resins, isocyanate, isocyanurate, and combinations thereof. Multifunctional acrylates are preferably selected from trimethylolpropane triacrylate, glycerol triacylate, pentaerythritol triacrylate and methacrylate, pentaerythritol tetraacrylate and methacrylate, di pentaerythritol pentaacrylate, sorbitol triacrylate, and sorbital hexaacrylate.
[0134] Thermoplastic binders comprise a variety of polymerized materials such as polyvinyl acetate, polyvinyl butyral, polyvinyl alcohol, and other polyvinyl resins; polystyrene resins; acrylic and methacrylic acid ester resins; cyanoacrylates; and various other synthetic resins such as polyisobutylene polyamides, courmarone-idene products, and silicones.
[0135] Suitable functionalized acrylics, alkyds, polyurethanes, polyesters, and epoxies can be obtained from a number of commercial sources. Useful acrylics are sold under the ACRYLOID™ trade name (Rohm & Haas, Co., Pennsylvania); useful epoxy resins are sold under the EPON™ trade name (Resolution Specialty Materials, LLC, Illinois); useful polyester resins are sold underthe CYPLEX® trade name (Cytec Industries, New Jersey); and useful vinyl resins are sold under the UCAR™ trade name (The Dow Chemical Company, Michigan).
[0136] Illustrative of useful high modulus or rigid binder materials are polycarbonates;polyphenylenesulfides; polyphenylene oxides; polyester carbonates; polyesterimides; polyimides; and thermoset resins such as epoxy resins, phenolic resins, modified phenolic resins, allylic resins, alkyd resins, unsaturated polyesters, aromatic vinylesters as for example the condensation produced of bisphenol A and methacrylic acid diluted in a vinyl aromatic monomer (e.g. styrene or vinyl toluene), urethane resins and amino (melamine and urea) resins. The major criterion is that such material holds the composition together and maintains the geometrical integrity of the composite underthe desired use conditions. The binder can be included in the composition in any suitable amount. For example, the binder can be included in an amount from about 5 wt. % to about 100 wt. % by weight (on264929-7619-2059, v. 14774-0071W001 a solids basis) of the wet composition, such as from about 20 wt. % to about 80 wt. %, from about 30 wt. % to about 70 wt. %, from about 40 wt. % to about 60 wt. %, etc.
[0137] As discussed above, in some embodiments, the tiles 100a-100c, 200a-200c, and 300a-300c can be constructed of a PVA-melanin composite or a bismuth-melanin composite. Melanin (e.g., 10% by weight) in PVA produced by a heat compression method can result in a generally uniform hard material with potential ballistic and stab resistance. It is noted that the heat compression method is well suited for rapid, mass production of uniform PVA-melanin material in different sizes and shapes, depending on the molds / dyes used.
[0138] In certain embodiments as disclosed herein the melanin material and the, for example PVA or bismuth, are present in a ratio selected form the group consisting of about 1 to about 15, about 15 to about 1, about 1 to about 10, about 10 to about 1, about 1 to about 5, about 5 to about 1, about 2 to about 98, about 5 to about 95, about 20 to about 80, about 30 to about 70, about 40 to about 60, about 50 to about 50, about 60 to about 40 about 70 to about 30 about 80 to about 20, about 95 to about 5, about 98 to about 2 (percent by weight). In certain embodiments as disclosed herein, melanin is present in the composite at a concentration selected from the group consisting of about 0.01%, about 0.02%, about 0.05%, about 0.1%, about 0.2%, about 0.3%, about 0.4%, about 0.5%, about 0.6%, about 0.7%, about 0.8%, about 0.9%, about 1%, about 1.5%, about 2%, about 2.5%, about 3%, about 3.5%, about 4%, about 4.5%, about 5%, about 5.5%, about 6%, about 6.5%, about 7%, about 7.5%, about 8%, about 8.5%, about 9%, about 9.5%, about 10%, about 11%, about 12%, about 13%, about 14%, about 15%, about 16%, about 17%, about 18%, about 19%, about 20%, about21%, about 22%, about 23%, about24%, about 25%, about 26%, about 27%, about 28%, about 29%, about 30%, about 35%, about 40%, about 45%, about 50%, about 55%, about 60%, about 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 75%, about 75%, about 80%, about 81 %, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 96%, about 97%, about 98%, about 99%, and about 99.5%.
[0139] Additionally, it is likely that PVA-Melanin composites with higher percentages of melanin (e.g. 11%-60% by weight) will have greater potential for ballistic and stab resistance.274929-7619-2059, v. 14774-0071W001
[0140] It is desirable for protective materials to be hard. However, in general, many materials become more brittle and thus susceptible to cracking as they become harder. The inventor has discovered a number of surprising methods for enhancing the hardness of melanin composites (e.g., with PVA or Bismuth) while decreasing the brittleness, yet maintaining a light overall weight. These methods, which can be implemented to manufacture tiles of a foldable shield according to the inventive concepts disclosed herein, include:1. Reducing the size of the particles of melanin by use of milling machines or manual particle size reduction processes before mixing melanin with PVA or Bismuth. The following would be close to optimal sizes for the melanin particles in a resulting batch:D10: 10% of the particles are smaller than about 0.4 micronsD50: 50% of the particles are smaller than about 4 micronsDOO: 90% of the particles are smaller than about 6 microns.2. Adding FeCh (about 1-15% by weight) to bismuth-melanin.3. Adding FeCh. (about 5% to 20% by weight) to PVA-melanin (e.g., 45% by weight melanin in PVA).4. Creating mixtures of PVA-melanin with silk solution (e.g., with 45% by weight melanin in PVA) in a 1:1 ratio of PVA-Melanin to Silk solution by weight. 5. Adding 1-5% by weight silk to PVA-melanin (e.g. 45% by weight melanin in PVA) by soaking the PVA-melanin in silk solution for several days.6. Forming composites of poly(acrylinitrile-co-butadiene) with melanin. This is accomplished by first dissolving the poly(acrylinitrile-co-butadiene) in dimethyl formamid (DMF) and then mixing with lyophilized purified melanin.7. Addition of ultra-high molecular weight polyethylene (UHMVPE) (e.g. 1-5% by weight) to PVA-melanin or bismuth-melanin8. Filling spaces in PVA-melanin composites and bismuth-melanin composites with materials with salutary ballistic protective properties to enhance the shielding material, while adding very little weight. (Melanin is known to have a large internal surface area (Meredith, 2006), and the inventor believes that there is some measure of porosity in PVA-melanin composites and bismuth- melanin composites.)9. Adding greater than 5% by weight FeCI3 to bismuth-melanin. (Bismuth- melanin with 5% by weight FeCI3 was brittle and broke with handling, whereas bismuth-melanin with 10% by weight FeCI3 was not brittle.)284929-7619-2059, v. 14774-0071W001 10. Manufacturing the melanin composite tile so that it has a core of wire, such as chicken wire or perforated stainless steel, to enhance the strength and reduce the tendency to crack when a bullet impacts the tile.
[0141] Experimentation - Improved Manufacturing Process for PVA-Melanin Composites
[0142] An existing manufacturing process for composites of melanin and PVA provide a very good hardness (Shore D ~ 80) property. However, the existing process involves numerous steps and is time consuming. Accordingly, the inventor conducted the experiment described herein to develop an improved process for manufacturing composites of melanin and PVA that maintains the hardness of the product above Shore- D 80.
[0143] Supplies and Equipment
[0144] The following supplies were used in the experimental process:Melanin, Polyethylene (CAS 9002-88-4), Polyvinyl Alcohol 125 (CAS 9002-89-5), Isopropyl alcohol, PTFE Release Agent, 25 Ton Heated Platen Lab Hydraulic Press, 4 inch x 4 inch x 3.5mm mold, 2 12”x12” SS heavy plates, 2 Aluminum sheets 12”x 12”
[0145] Procedure
[0146] The following steps were performed in the experimental process:1. A sample A (polyethylene (PE) with 50% by weight melanin), and a sample B (polyvinyl alcohol (PVA) with 10% by weight melanin) were prepared.2. A heat press compressor was powered on.3. A temperature of both heat controlled upper and lower platens was adjusted up to 200°C and the heat press compressor was allowed to stand by for about 1 hour after it reached the set temperature.4. A mold of a desired size was selected and the mold was cleaned well with isopropyl alcohol (I PA) prior to use.5. An amount of sample was calculated as needed (~ 12g)6. The following steps were performed in order:a. A heavy stainless steel (SS) plate (12”X12”) was laid out.b. An aluminum sheet (12”x12”) was laid out.c. Arnold (4” x 4” x 3.5mm) was laid out.d. The PE + Melanin mixture was chargede. An aluminum sheet (12”x12”) was laid out.f. A SS heavy plate (12”X12”) wascovered on the top (PTFE294929-7619-2059, v. 14774-0071W001 release agent was sprayedbetween the layers)7. The entire set described above was inserted into a hot press compressor.8. A timer was set for 10 mins.9. The lower platen was raised up to clamp the sample (barely touching) for a first 5 mins.10. The platen was released and raised several times in the first 5 mins to eliminate any bubbles that might build up.11. The sample was allowed to slowly melt at the final raise with the pressure ~ 25 tons.12. After 10 mins, the sample was removed out and to a cool flat surface.
[0147] Results
[0148] Sample A (polyethylene-melanin) was watery during the process, and was then soft & brittle after cooling.
[0149] Sample B (PVA-melanin) was very hard to the touch, stuck to the mold and the aluminum sheet. Sample B was removed from the mold using the hydraulic press. The hardness of Sample B (Shore D) was an average of 83, with a tight range of 82-84.
[0150] Conclusions
[0151] 1.Melanin (10% by weight) in PVA produced by the experimental heat compression method resulted in a product that was a relatively uniform hard material with potential ballistic and stab resistance. It is likely that PVA-Melanin composites with higher percentages of melanin (e.g. 11%-60%) will have greater potential for ballistic and stab resistance. This heat compression method is well suited for rapid, mass production of uniform PVA-melanin material in different sizes and shapes, depending on the molds / dyes used.
[0152] 2. Polyethylene-melanin composite (1:1) did not result in a product with potential ballistic resistance because it was soft and brittle.
[0153] A foldable shield according to the disclosure herein provides effective protection against explosive materials, shrapnel, and projectiles. Additionally, the disclosed foldable shield is lightweight, can be quickly and easily disassembled, and includes foldable tile sheets that make the foldable shield practical and convenient for a person to carry when the foldable shield is disassembled. For example, the total volume of the foldable shield is not greater than the sum of its component parts, and the length and width dimensions of304929-7619-2059, v. 14774-0071W001 the foldable shield are not smaller than its largest component part. Additionally, fasteners (e.g., the flexible tape, magnetic strips, and hook-and-loop members) to affix the component parts of the foldable shield to each other and to permit folding, occupy minimal volumes. Furthermore, the manner in which the foldable tile sheets fold does not require folding on the depth (thickness) of the materials, nor does it stretch or require distance between component parts, such that the component parts are not adjacent and therefore do not afford complete covering protection.[00154J While this disclosure includes specific examples, it will be apparent after an understanding of the disclosure of this application that various changes in form and details may be made in these examples without departing from the spirit and scope of the claims and their equivalents. The examples described herein are to be considered in a descriptive sense only, and not for purposes of limitation. Descriptions of features or aspects in each example are to be considered as being applicable to similar features or aspects in other examples. Suitable results may be achieved if the described techniques are performed in a different order, and / or if components in a described system, architecture, device, or circuit are combined in a different manner, and / or replaced or supplemented by other components or their equivalents. Therefore, the scope of the disclosure is defined not by the detailed description, but by the claims and their equivalents, and all variations within the scope of the claims and their equivalents are to be construed as being included in the disclosure.314929-7619-2059, v. 1
Claims
4774-0071W001 WHAT IS CLAIMED IS:
1. A foldable shield, comprising:one or more foldable tile sheets, each of the one or more foldable tile sheets comprising a plurality of tiles connected in series, wherein adjacent tiles among the plurality of tiles are connected to each other at flexible joints.
2. The foldable shield of claim 1, wherein the plurality of tiles are constructed of a polyvinyl alcohol-melanin composite.
3. The foldable shield of claim 2, wherein the polyvinyl alcohol-melanin composite is about 10% melanin by weight.
4. The foldable shield of claim 2, wherein the polyvinyl alcohol-melanin composite is about 10% melanin to about 60% melanin by weight.
5. The foldable shield of claim 1, wherein each tile among the plurality of tiles has a length of approximately 4 inches, a width of approximately 4 inches, and a thickness of approximately 8 millimeters.
6. The foldable shield of claim 1 , wherein each of the foldable tile sheets is configured to be folded into a folded configuration in which the plurality of tiles of each of the foldable tile sheets are vertically stacked.
7. The foldable shield of claim 6, wherein the plurality of tiles of each of the one or more tiles sheets comprises three tiles, and wherein the one or more foldable tile sheets each have a length of approximately 4 inches, a width of approximately 4 inches, and a thickness of approximately 24 millimeters in the folded configuration.
8. The foldable shield of claim 1, wherein the one or more foldable tile sheets each further comprise tape strips connecting the adjacent tiles to each other at the joints.
9. The foldable shield of claim 1 , wherein:the one or more foldable tile sheets comprise at least two foldable tile sheets; and 324929-7619-2059, v. 14774-0071W001 adjacent foldable tile sheets, among the at least two foldable tile sheets, are connected to each other at least one joint formed between respective adjacent edge portions of the adjacent foldable tile sheets.
10. The foldable shield of claim 9, wherein the least one joint is formed by ferromagnetic regions disposed at the respective adjacent edge portions of the adjacent foldable tile sheets, and at least one magnetic strip attached to the ferromagnetic regions.
11. The foldable shield of claim 10, wherein the ferromagnetic regions comprise ferromagnetic strips attached to the plurality of tiles of each of the adjacent foldable tile sheets.
12. The foldable shield of claim 10, wherein the ferromagnetic regions comprise ferromagnetic particles embedded in the plurality of tiles of each of the adjacent foldable tile sheets.
13. The foldable shield of claim 9, wherein the at least one joint is formed by first hook-and-loop strips attached to the respective adjacent edge portions of the adjacent foldable tile sheets, and at least one second hook-and-loop strip attached to the first hook-and-loop strips.
14. The foldable shield of claim 1, wherein:the one or more foldable tile sheets comprise three foldable tile sheets;adjacent foldable tile sheets, among the at least one or more foldable tile sheets, are connected to each other at a joint formed along respective adjacent edge portions of the adjacent foldable tile sheets.
15. The foldable shield of claim 14, wherein the foldable shield has a length of approximately 12 inches, a width of approximately 12 inches, and a thickness of approximately 24 millimeters in an assembled configuration in which the three foldable tile sheets are unfolded.
16. The foldable shield of claim 15, wherein each tile among the plurality of tiles has a length of approximately 4 inches, a width of approximately 4 inches, and a thickness of approximately 8 millimeters.
17. A shield, comprising:a substantially flat plate comprising a plurality of tiles that are connected to each other,334929-7619-2059, v. 14774-0071W001 wherein the plurality of tiles are composed of a polyvinyl alcohol-melanin composite.
18. The shield of claim 17, wherein the polyvinyl alcohol-melanin composite is about 10% melanin by weight.
19. The shield of claim 17, wherein the polyvinyl alcohol-melanin composite is about 10% melanin to about 60% melanin by weight.344929-7619-2059, v. 1