Variable density isocyanate-based polymer material
By forming variable density isocyanate-based polymer materials through controlled bubble formation in spray applications, the challenges of complex equipment and skilled labor in polyurea coating are addressed, enhancing application efficiency and structural performance.
Patent Information
- Application Number
- PCT/US2026/026515
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-05-04
- Publication Date
- 2026-11-12
AI Technical Summary
Polyurea coatings require complex equipment and skilled technicians due to rapid cure time, limiting efficient application in multi-layered materials.
A method of forming variable density isocyanate-based polymer materials by combining an isocyanate component with a co-reactant and an aqueous solution to create layers with controlled density variations, using spray techniques to form layers with different densities through controlled bubble formation.
Enables efficient application of polyurea coatings with varying densities, improving flexibility and structural integrity while reducing equipment complexity and technician requirements.
Smart Images

Figure US2026026515_12112026_PF_FP_ABST
Abstract
Description
VARIABLE DENSITY ISOCYANATE-BASED POLYMER MATERIALCROSS REFERENCE TO RELATED APPLICATIONS
[0001] This application claims priority to and the benefit of United States Provisional Application No. 63 / 801,315, filed on May 7, 2025, which is incorporated herein by reference in its entirety.BACKGROUND
[0002] Polyurea coatings and materials can be formed by the reaction of an isocyanate with a polyamine. Polyurea exhibits a rapid cure time and can set within seconds to minutes. In a multi-layered material with multiple polyurca layers, the rapid cure time allows for fast application and limited downtime between application of each layer.
[0003] Polyurea can be applied via spray methods such as by using multi-line pump systems. However, manufacturing polyurea materials may require relatively complex pump / spray equipment and well-trained technicians for effective application due to the rapid cure time.SUMMARY
[0004] A method of manufacturing a variable density isocyanate-based polymer material comprises spraying a first portion of an uncured mixture over a substrate. The uncured mixture includes an isocyanate component and a co-reactant component. The method further comprises spraying a second portion of the uncured mixture over the first layer. Forming the first layer and / or the second layer comprises combining an aqueous solution with the first and / or second portion of the uncured mixture. The aqueous solution is formulated to react with the uncured mixture to form bubbles. Combining the aqueous solution with the uncured mixture comprises (i) directing a stream of the aqueous solution into a stream of the uncured mixture, and / or (ii) mixing the aqueous solution with the co-reactant component and combining a first stream that includes the isocyanate component with a second stream that includes the co-reactant component and the aqueous solution. One layer is formed without addition of the aqueous solution to the uncured mixture, or different proportional amounts of the aqueous solution (relative to the uncured mixture) are used to form the first layer as compared to the secondlayer. As a result, the density of the first layer is different from the density of the second layer. The isocyanate-based polymer material can include, for example, polyurea, polyurethane, polyisocyanurate, polyimide, or a combination / hybrid thereof such as a polyurea-urethane hybrid and / or a polyurethane-imide hybrid
[0005] Also disclosed herein is a variable density isocyanate-based polymer material comprising a first layer, second layer, and third layer, wherein the second layer is disposed between the first layer and the third layer and has a density that is lower than the first layer and lower than the third layer.
[0006] Also disclosed herein is a variable density isocyanate-based polymer material, comprising: a first layer comprising an isocyanate-based polymer of a first density, the structural layer defining a plurality of voids; and a second layer disposed within the voids, the second layer comprising an isocyanate -based polymer of a second density that is lower than the first density.
[0007] Also disclosed herein is an isocyanate -based polymer material comprising a first structural layer comprising an isocyanate-based polymer, a second structural layer comprising an isocyanate-based polymer, and an adhesive scrim disposed between the first and second structural layers, wherein the adhesive scrim has a density of 0.005 g / cm2to 0.1 g / cm2.
[0008] This summary is provided to introduce a selection of concepts in a simplified form that are further described below in the detailed description. This summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used as an indication of the scope of the claimed subject matter.BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Various features and advantages of this disclosure will become apparent and more readily appreciated from the following description, taken in conjunction with the accompanying drawings and the appended claims, all of which form a part of this specification.
[0010] Figures 1A and IB illustrate example configurations of a variable density isocyanate-based polymer material.
[0011] Figure 2 illustrates an example application system that can be utilized to carry out the disclosed method and / or to form the disclosed variable density isocyanate-based polymer material.
[0012] Figure 3 illustrates an example configuration of a variable density isocyanate -based polymer material comprising a grid pattern structural layer with voids filled by a lower density isocyanate-based polymer material.
[0013] Figure 4 illustrates an example configuration of an isocyanate-based polymer material comprising an adhesive scrim disposed between structural layers.
[0014] Figures 5A-5C illustrate the setup and results of a finite element analysis (FEA) simulation comparing polyurea materials of different patterned structural layers filled with lower density polyurea.DETAILED DESCRIPTIONIsocyanate-Based Polymer
[0015] The term “isocyanate-based polymer” refers to a polymer that can be formed from an isocyanate component and a co-reactant component. The isocyanate -based polymer can include, for example, polyurea, polyurethane, polyisocyanurate, polyimide, or a combination / hybrid thereof such as a polyurea-urethane hybrid and / or a polyurethane-imide hybrid. The co-reactant component can include, for example, a polyamine, polyol, polyanhydride, or combination thereof.
[0016] The co-reactant component and / or the isocyanate component can include a catalyst. While the reaction between an isocyanate and a polyamine is relatively fast and can be carried out without a catalyst, a catalyst can be included to accelerate the reaction between the isocyanate component and another type of co-reactant such as a polyol. The catalyst can include, for example, a tertiary amine catalyst such as triethylenediamine (TED A, also known as DABCO), N,N-dimethylcyclohexylamine (DMCHA), and / or N,N-dimethylbenzylamine (DMBA), and / or a metal-based catalyst such as an organotin compound, bismuth carboxylate, and / or zinc-based compound.Isocyanate Component
[0017] The isocyanate component can include monofunctional isocyanate (containing one isocyanate functional group (NCO)) and / or polyfunctional isocyanate (containing two or more isocyanate functional groups (NCOs)). The isocyanate component can include a blocked isocyanate. The isocyanate component can include isocyanate monomers, isocyanateoligomers (including dimers, trimers, and / or higher molecular weight structures), and / or isocyanate prepolymers. An isocyanate prepolymer can be formed by partially reacting an isocyanate with a reactive compound, such as a hydroxy 1-terminated polyol, leaving free NCO groups available for further reaction. The isocyanate component can include C2-C20 linear, branched, cyclic, aromatic, or aliphatic isocyanates, or combinations thereof.
[0018] The isocyanate component can additionally or alternatively include an aliphatic isocyanate such as a cycloaliphatic diisocyanate such as isophorone diisocyanate (IPDI) (3,3,5-trimethyl-5-isocyanato-methyl-cyclohexyl isocyanate); cyclohexylene diisocyanate; 4,4’-methylenedicyclohexyl diisocyanate (H12MDI); and / or a polymethylene isocyanate such as 1.4-tetramethylene diisocyanate, 1,5 -pentamethylene diisocyanate, 1,6-hexamethylene diisocyanate (HDI), 1,7-heptamethylene diisocyanate, 2,2,4- and / or 2,4,4-trimethylhexamethylene diisocyanate, 1,10-decamethylene diisocyanate, 2-methyl-l,5-pentamethylene diisocyanate; or combination thereof.
[0019] The isocyanate component can additionally or alternatively include an aralkyl diisocyanate such as tetramethylxylyl diisocyanate (TMXDI) and / or 1,3-bis(isocyanatomethyl)benzene (m-TMXDI).
[0020] The isocyanate component can additionally or alternatively include an aromatic isocyanate such as phenylene diisocyanate; toluene diisocyanate (TDI); xylene diisocyanate; 1.5 -naphthalene diisocyanate; chlorophenylene 2,4-diisocyanate; bitoluene diisocyanate; dianisidine diisocyanate; tolidine diisocyanate; an alkylated benzene diisocyanate: a methylene-interrupted aromatic diisocyanate, such as a methylenediphenyl diisocyanate, such as the 4,4’ -isomer (MDI) and / or 2,4’ -isomer, including alkylated analogs such as 3,3’-dimethyl-4,4’ -diphenylmethane diisocyanate; or combination thereof.
[0021] The isocyanate component can additionally or alternatively include a modified isocyanate, such as carbodiimide and / or uretone-imine modified isocyanate. Commercially available isocyanate examples include those sold under the DESMODUR name (Covestro LLC, Pittsburgh, PA) such as DESMODUR N 3200, DESMODUR N 3300, DESMODUR N 3400, DESMODUR XP 2410 and DESMODUR XP 2580.Co-Reactant Component
[0022] The co-reactant component can include a polyamine. The polyamine can include an aliphatic amine such as ethylene diamine; 1,2-diaminopropane; 1,4-diaminobutane; 1,3-diaminopentane; 1,6-diaminohexane (hexamethylene diamine (HMDA)); 2-methyl-l,5-pentane diamine: 2,5-diamino-2,5-dimethylhexane; 2,2,4- and / or 2,4,4-trimethyl-l,6-diamino-hexane; 1,11 -diaminoundecane; 1,12-diaminododecane; 1,3- and / or 1,4-cyclohexane diamine; l-amino-3,3,5-trimethyl-5-aminomethyl-cyclohexane (isophorone diamine (IPDA)); 2,4-and / or 2,6-hcxahydrotoluoylcnc diamine; 2,4’- and / or 4,4’ -diaminodicyclohcxyl methane and / or alkylated analogs thereof (e.g., methyl and / or ethyl) such as 3,3’-dialkyl-4,4’-diaminodicyclohexyl methane; a triamine such as dipropylene triamine (DPTA) and / or bis hexamethylene triamine (BHMT), or combination thereof.
[0023] The polyamine can additionally or alternatively include an aromatic diamine, such as 2,4- and / or 2,6-diaminotoluene; diethyltoluenediamine (DETDA) (also known as diethylmethylbenzenediamine) such as 3,5-diethyltoluene-2,4-diamine and / or 3,5-diethyltoluene-2,6-diamine; 3,5-dimethylthio-2,4-toluenediamine and / or 3,5-dimethylthio-2,6-toluenediamine; 2,4’- and / or 4,4’ -di aminodiphenyl methane; ethylenedianiline (EDA) (e.g., the 2,2’ -ethylene and / or 4,4’ -ethylene isomers); methylenedi aniline (MDA); or combination thereof.
[0024] The polyamine can additionally or alternatively include an amine -terminated polyether (i.e., polyoxyalkyleneamine) comprising two or more primary or secondary amino groups attached to a polyether backbone that includes, for example, propylene oxide, ethylene oxide, butylene oxide or combination thereof. Commercially available examples include JEFFAMINE products (Huntsman Corporalion) such as JEFFAMINE D-series (diamines with two reactive amine groups) and JEFFAMINE T-series (triamines with three reactive amine groups). Such amines may have an approximate molecular weight ranging from 200 to 7500.
[0025] The polyamine can additionally or alternatively include an amine-terminated polyurea. The polyamine can additionally or alternatively include a secondary amine that comprises the reaction products of a primary amine, such as those disclosed herein, with acrylonitrile.
[0026] The co-reactant component can additionally or alternatively include a polyol. The polyol can include, for example: a polyether polyol such as polypropylene glycol (PPG), polyethylene glycol (PEG), and / or polytetramethylene ether glycol (PTMEG); a polyester polyol such as a polyol formed from adipic acid and / or polycaprolactone; a polycarbonate polyol; and / or a poly(meth)acrylate polyol.
[0027] The co-reactant component can additionally or alternatively include a polyanhydride. The polyanhydride can include, for example: an aromatic polyanhydride such as pyromellitic dianhydride (PMDA), benzophenone tetracarboxylic dianhydride (BTDA), and / or oxy diphthalic anhydride (ODPA); and / or an aliphatic poly anhydride such as hcxafluoroisopropylidcnc bis(phthalic anhydride) (6FDA) and cyclohexane tetracarboxylic dianhydride (CHTDA).Aqueous Solution
[0028] The aqueous solution can include a foam stabilizer and / or an isocyanate-water reaction catalyst. The foam stabilizer can include a copolymer of a siloxane (e.g., dimethyl siloxane) and a polyoxyalkylene (i.e., a silicone polyether copolymer). Examples include commercially available products sold under the names TEGOSTAB and SILSTAB (e.g., 2100, 2550, 2580, and / or 2760). The inclusion of a foam stabilizer can stabilize and promote uniformity of bubbles generated when forming foam layers, which can minimize or prevent bubble collapse before the material solidifies, thereby helping to achieve target densities.
[0029] The isocyanate-water reaction catalyst can include a tertiary amine catalyst, such as triethylenediamine (TEDA, also known as DABCO), N,N-dimethylcyclohexylamine (DMCHA), and / or N,N-dimethylbenzylamine (DMBA). The isocyanate-water reaction catalyst can additionally or alternatively include a mctal-bascd catalyst such as an organotin compound, bismuth carboxylate, and / or zinc -based compound.
[0030] The isocyanate-water reaction catalyst can promote efficiency of the isocyanate-water reaction when the isocyanate component and the aqueous solution are mixed, resulting in effective generation of carbon dioxide (CO2) bubbles. As described herein, controlling the rate of addition of the aqueous solution to the isocyanate component can control bubble formation and enables the manufacture of a composite material with polyurea layers of varying density, including discrete or gradient changes in polyurea density along the thickness of the composite material.
[0031] An “aqueous solution’’ comprises at least 50% water, based on the total weight of the liquid portion of the solution. The aqueous solution can comprise at least 60% water, or at least 70% water, or at least 80% water, or at least 90% water, or at least 95% water, based on the total weight of the liquid portion of the solution. If present, other solvents that make up less than 50% of the liquid portion of the aqueous solution can include organic solvents such aspolar organic solvents (e.g., protic organic solvents such as glycols, glycol ether alcohols, alcohols, and volatile ketones, glycol diethers, esters, and diesters), and / or hydrocarbons (aromatic and / or aliphatic).Variable Density Isocyanate- Based Polymer Material
[0032] Figures 1A and IB illustrate example configurations of a variable density isocyanate-based polymer material 100. With reference to Figure 1A, a method of manufacturing the variable density isocyanate-based polymer material 100 can include applying multiple layers of material over a substrate. The substrate can include a mold 112, for example, such as shown in Figure 1A. As used herein, to apply (e.g., spray) a composition “over” or “on” a substrate (or previously applied layer of the material) means to direct the composition toward a surface of the substrate (or previously applied layer of the material) such that the composition covers at least a portion of the surface to which it was directed, with or without intervening layer(s).
[0033] The mold 112 can be coated with a release agent, and a gelcoat layer 108 can be applied on the mold 112 prior to forming subsequent layers. The gelcoat layer 108 can comprise polyurea, polyester, vinyl, and / or epoxy, for example. A “gelcoat layer” refers to an outer layer that is primarily included for aesthetic and / or protective purposes as opposed to structural purposes. The “gelcoat layer” can makes up less than 20% of the total thickness of the isocyanate-based polymer material 100 and / or has a layer thickness that is 45 mils (1.14 mm) or less, such as 30 mils (0.76 mm) or less.
[0034] The illustrated mold 112 is shown with a flat shape, but the shape of the mold 112 can vary. For example, the mold can be configured according to the component to be formed from the process. Examples include tank and pipe coatings; floor coatings; roof coatings; liners for truck beds, railcars, trailers, and other vehicles; boat hulls and decks; bathtubs, water containing structures such as pools, water treatment equipment, and other water contacting structures; and oil / gas industrial equipment. The mold 112 can have a cylindrical shape, and the layer-by-layer spraying process can be carried out on the outside surface or inside surface of the cylindrical mold. For example, the mold 112 can be used to form utility poles and / or pipes.
[0035] The method includes spraying a first portion of an uncurcd mixture over the mold 112 (and over the gelcoat layer 108, if present). The uncured mixture can include an isocyanatecomponent and a co-reactant component. As a result of reaction between the isocyanate component and the co-reactant component, the uncured mixture can cure to form a first layer 102. The method can further include spraying a second portion of the uncured mixture over the first layer 102. As a result of reaction between the isocyanate component and the co-reactant component, the uncurcd mixture can cure to form a second layer 104 with a density that is different than the density of the first layer 102.
[0036] The density of the first layer 102 and second layer 104 can be controlled by varying the amount of an aqueous solution combined with the respective portions of the uncured mixture when forming the layers. The aqueous solution can be formulated to react with the first portion and / or second portion of the uncured mixture to form bubbles. That is, water in the aqueous solution can react with the isocyanate component of the uncured mixture to generate CO2 bubbles. The generated bubbles, when maintained long enough for the mixture to cure, lower the density of the resulting isocyanate-based polymer material relative to the (otherwise) same material without bubbles.
[0037] Different proportional amounts of the aqueous solution can be used to form the first layer 102 as compared to the second layer 104. As a result, the density of the first layer can be different from the density of the second layer. For example, the density of the first layer 102 can be greater than the density of the second layer 104. The second layer 104 can have a density that is 5% to 65% the density of the first layer 102, such as 10% to 50% the density of the first layer 102, or 15% to 45% the density of the first layer 102, or a density within a range with endpoints selected from any two of the foregoing values. Alternatively, the density of the second layer 104 can be higher than the density of the first layer 102. For example, the first layer 102 can have a density that is 5% to 65% the density of the second layer 104, such as 10% to 50% the density of the second layer 104, or 15% to 45% the density of the second layer 104, or a density within a range with endpoints selected from any two of the foregoing values. The “proportional amount’’ of the aqueous solution refers to the wt. % of the aqueous solution based on the total weight of the uncured mixture and aqueous solution combined.
[0038] The first layer 102 and / or second layer 104 can include substantially uniform (but different) densities. For example, Figure 1 A shows a first layer 102 with a substantially uniform density and a second layer 104 with a substantially uniform density, with a discrete transition between the layers. A “discrete transition” refers to a transition that forms a distinct boundary between the first layer 102 and second layer 104 where a distinct change in density can bereadily seen in a cross section of the resulting isocyanate -based polymer material 100. The first layer 102 may be allowed to cure before applying the second layer 104.
[0039] The first layer 102, the second layer 104, or both can include a density gradient extending through at least a part of the thickness of the layer. For example, the uncured mixture may be continually applied as the delivery rate of the aqueous solution is ramped up or down relative to the delivery rates of the isocyanate and co-reactant components, causing a gradient change in density as the thickness of the material is increased. For example, Figure IB shows a density gradient that extends across both the first layer 102 and the second layer 104. In the context of such a continuous transition, the boundary between the first layer 102 and the second layer 104 can be considered as the halfway depth between the beginning of the first layer 102 and the end of the second layer.
[0040] In the example of Figure 1A, a discrete transition is shown between higher density first layer 102 and lower density second layer 104. A discrete transition can be formed by applying the first layer 102 at a set, first proportional amount of the aqueous solution, then adjusting to a set, second proportional amount of the aqueous solution that is different from the first proportional amount during or before applying the second layer 104. In the example of Figure 1A, the first proportional amount is lower than the second proportional amount. The first proportional amount of the aqueous solution can be zero, for example.
[0041] In the example of Figure IB, a continuous transition is shown as a higher density portion beginning at the bottom (i.e., side formed closer to the mold) of first layer 102 that transitions through a gradient to a lower density portion at the top (i.e., side formed farther from the mold) of second layer 104. The “bottom” and “top” indicators used herein are included for convenience in describing the illustrated isocyanate-based polymer material 100, and do not necessitate a particular orientation of the isocyanate-based polymer material 100 either during or after manufacture. A continuous transition can be formed by adjusting the proportional amount of the aqueous solution combined with the uncured mixture while the uncured mixture is continuously applied (e.g., via multiple passes) over the mold 112 (and / or other substrate). For example, while continuously applying the uncured mixture and increasing the thickness of the applied material, the delivery rate of the aqueous solution can be ramped up or down over time relative to the delivery rates for the isocyanate and co-reactant components.
[0042] In the isocyanate-based polymer materials 100 shown in Figures 1A and IB, the first layer 102 has a greater density than the second layer 104. That is, a greater proportional amount of the aqueous solution is used to form the second layer 104 as compared to the first layer 102. As discussed above, this could be reversed, such that the first layer 102 has a lower density than the second layer 104.
[0043] The isocyanate-based polymer of the first layer 102 and second layer 104 can be chemically equivalent. As used herein, “chemically equivalent” means that the isocyanatebased polymer is formed from the same isocyanate and co-reactant components with the same isocyanate / co-reactant component ratios. The isocyanate-based polymer of the layers may therefore be “chemically equivalent” even though certain physical properties (such as density) and / or relative amounts of other components (such as foam stabilizer and / or isocyanate-water reaction catalyst) are different in the respective layers, due to the inclusion of different amounts of the aqueous solution. For example, multiple layers of different density may be formed using the same spray system and the same batches of the isocyanate component and co-reactant component, without adjusting the mixing proportions of the isocyanate component and coreactant component. As disclosed herein, the variable density of different layers can be achieved by varying the proportional amount of the aqueous solution combined with the isocyanate and co-reactant components.
[0044] As illustrated in Figure 1A, the method can include spraying a third portion of the uncured mixture over the second layer 104 to form a third layer 106. The third layer 106 can have a density that is different from the density of the first layer 102 and / or the second layer 104. Both the first layer 102 and the third layer 106 can have densities that are greater than the density of second layer 104 such that the second layer 104 is “sandwiched” between layers of higher density. The density of the first layer 102 and third layer 106 can be the same. For example, the first layer and the third layer can be configured as relatively more rigid structural layers that arc formed without addition of the aqueous solution to the uncurcd mixture, and the second layer can be configured as a relatively less rigid and less dense foam layer formed by combining the aqueous solution with the uncured mixture.
[0045] A ratio of the thickness of the second layer 104 to the combined thickness of the first layer 102 and third layer 106 can be 0.2 to 5, such as 0.35 to 3.5 or 0.5 to 2, or can be within a range with endpoints selected from any two of the foregoing values. The thickness of the second layer 104 can be equal to or greater than the thickness of the first layer 102 and / orequal to or greater than the thickness of the third layer 106. The isocyanate-based polymer of the first layer 102, second layer 104, and third layer 106 can be chemically equivalent.
[0046] As demonstrated in the working examples, a variable density isocyanate-based polymer material comprising a second layer 104 of lower density disposed between a first layer 102 and third layer 106 of higher density can exhibit (1) a flexural rigidity that is equal to or greater than a flexural rigidity of a material of same thickness and formed entirely of the first layer; and / or (2) a flexural strength that is equal to or greater than a flexural strength of a material of same thickness and formed entirely of the first layer.
[0047] The method can include forming a bottom / inner layer 110 over the second layer 104 (and the third layer 106 when the third layer 106 is present). The bottom / inner layer 110 can comprise an elastomeric material, such as an elastomeric polyurea. An “elastomeric material” has higher elongation and lower hardness as compared to the other layers. For example, an elastomeric material can have a hardness measured on the Shore A or low Shore D scale (e.g., Shore D 40 or less), and can exhibit an elongation at break of 200% or more. As demonstrated in the working examples, the inclusion of a bottom / inner layer 110 can reduce bottom surface abrasion loss (e.g., according to ASTM D4060-19) as compared to the same material without the bottom / inner layer 110. The bottom / inner layer 110 can be included at a thickness of, for example, 25 mil (0.64 mm) to 75 mil (1.91 mm), such as 35 mil (0.89 mm) to 65 mil (1.65 mm), such as 50 mil (1.27 mm), or within a range with endpoints selected from any two of the foregoing values.
[0048] Combining the aqueous solution with the uncured mixture can include (i) directing a stream of the aqueous solution into a stream of the uncured mixture, and / or (ii) mixing the aqueous solution with the co-reactant component and combining a first stream that includes the isocyanate component with a second stream that includes the co-reactant component and the aqueous solution. In the first option, the uncured mixture can be formed (by mixing the isocyanate component and co-reactant component) immediately prior to directing the stream of the aqueous solution into the uncured mixture, before the uncured mixture is able to cure. In the second option, the uncured mixture includes the aqueous solution upon formation once the isocyanate component and co-reactant component are mixed to form the uncured mixture.
[0049] Combining the aqueous solution with the uncured mixture can be carried out using a spray system such as those including a plural component proportioner, hose system (e.g., heated), spray gun (e.g., mechanical purge, air purge, and / or impingement mixing), and / orother equipment such as drams and transfer pumps. The system can include separate lines for each of the isocyanate component, co-reactant component, and aqueous solution.
[0050] Figure 2 illustrates an example application system 200 that can be utilized to carry out the disclosed method and / or to form the disclosed variable density isocyanate -based polymer material 100. The application system 200 can include a first nozzle 202 configured to combine an isocyanate line 204 and a co-reactant line 206 to form an uncured mixture stream 208, which can be directed to an application target 220 (e.g., a mold). A second nozzle 212 can be connected to an aqueous solution line 214 and can be configured to direct an aqueous solution stream 218 into the uncured mixture stream 208. Alternatively, the second nozzle 212 can be omitted and the aqueous solution can be pre-mixed with the co-reactant component, and both directed through the co-reactant line 206.Patterned Structural Layer Integrated with Foam Layer
[0051] Figure 3 illustrates another example configuration of a variable density isocyanatebased polymer material 300. The variable density isocyanate -based polymer material 300 can include or be utilized with any of the features disclosed elsewhere herein with respect to variable density isocyanate -based polymer material 100, including any of the other layers described with respect to Figures 1A and IB, such as a gelcoat layer 108, bottom / inner layer 110, and / or additional structural and / or foam layers (e.g., corresponding to layers 102, 104, and / or 106 as disclosed herein).
[0052] The first layer 302 of the variable density isocyanate-based polymer material 300 can be configured in a pattern that defines a plurality of voids, and the second layer 304 can be disposed within the voids. In this configuration, the first layer 302 can comprise an isocyanatebased polymer of a higher density than the isocyanate-based polymer of the second layer 304. The higher density first layer 302 can thereby form a “patterned structural layer” in which the lower density isocyanate -based polymer of the second layer 304 can be disposed. For example, the isocyanate-based polymer of the first layer 302 can be formed into a pattern without combining the aqueous solution with the uncured mixture (or by using relatively less of the aqueous solution), and the isocyanate -based polymer of the second layer 304 can applied to the voids while combining relatively more aqueous solution to form an isocyanate-based polymer of lower density relative to the first layer 302.
[0053] The first layer 302 can be arranged with a lattice structure, such as a grid pattern. The first layer 302 can include, for example, lines that form “ribs” extending longitudinally, laterally, diagonally, and / or in a random pattern. The grid can include various angles at which the ribs intersect and / or various spacing of the ribs to allow for a range of geometric configurations for the voids between the ribs. The grid pattern can include, for example, perpendicular lines forming square and / or rectangular shaped voids; diagonal lines that intersect at different angles (e.g., 15°, 30°, 45°, 60°, 75°, or a range with endpoints selected from any two of the foregoing values). The resulting voids can form triangles, parallelograms, hexagons, and / or irregular polygons, for example.
[0054] The second layer 304 can completely fill the voids formed by the first layer 302. For example, the second layer 304 can fill the voids such that the uppermost surfaces of the first layer 302 and the second layer 304 are flush. Alternatively, the second layer 304 can partially fill the volume of the voids, such as by filling 50%, 60%, 70%, 80%, 90%, or 95% of the volume of the voids, or within a range with endpoints selected from any combination of the foregoing values.
[0055] A patterned structural layer configuration in which the first layer 302 (of higher relative density) forms a pattern that defines a plurality of voids, with the second layer 304 (of lower relative density) disposed within the voids, can exhibit effective stiffness while minimizing the total amount of isocyanate-based polymer needed to form the material. For example, a structure comprising a patterned structural layer configuration such as shown in Figure 3 can exhibit greater flexural rigidity than a structure that uses the same amount of isocyanate-based polymer but does not include a patterned structural layer. When the isocyanate-based polymer material 300 is placed under stress, the patterned structural layer can undertake a greater portion of the load than the lower density portions in the voids, thus avoiding failure in the lower density portions for the same level of load.Isocyanate-Based Polymer Material Incorporating Adhesive Scrim
[0056] Figure 4 illustrates another example configuration of a isocyanate-based polymer material 400. The isocyanate -based polymer material 400 can include or be utilized with any of the features disclosed elsewhere herein with respect to variable density isocyanate-based polymer material 100 and / or variable density isocyanate-based polymer material 300, including any of the other layers described with respect to those materials, such as a gelcoatlayer 108, bottom / inner layer 110, additional structural and / or foam layers (e.g., corresponding to layers 102, 104, and / or 106 as disclosed herein), and / or a patterned structural layer forming voids filled with lower density material.
[0057] As illustrated, the isocyanate-based polymer material 400 can be manufactured by forming a first layer 402, then applying a scrim 405 to the first layer 402, and then applying a second layer 404 to the scrim 405. The process can be repeated to apply additional scrim and polyurea layers (e.g., in an alternating fashion). Multiple layers of scrim 405 can be inserted between each successive isocyanate-based polymer layer.
[0058] The scrim 405 can include an open mesh pattern of cross-direction yarns (e.g., fiberglass, polyester, carbon, and / or aramid), optionally coated with an adhesive binder. Suitable commercially available scrims include those sold under the trade name ADFORS Laid Scrim (Saint-Gobain), such as Laid Scrim 150 ± 10 g / m2(0.015 ± 0.001 g / cm2).
[0059] The scrim 405 can have a density of 0.005 g / cm2to 0.1 g / cm2, such as 0.010 g / cm2to 0.08 g / cm2, or 0.012 g / cm2to 0.7 g / cm2, such as 0.015 g / cm2, or can be within a range with endpoints selected from any two of the foregoing values. As demonstrated in the working examples, materials with scrim layers can exhibit material properties (e.g., flexural rigidity and strength) that are equal to or better than materials that instead include the same or similar mass of chopped fibers (e.g., glass, carbon, flax, jute) but are otherwise the same.Example Aspects
[0060] The following clauses represent a non-exhaustive list of example isocyanate-based polymer materials and related methods.
[0061] Clause 1. A variable density isocyanate -based polymer material, comprising: a first layer; a second layer; and a third layer, wherein the second layer is disposed between the first layer and the third layer and has a density that is lower than the first layer and lower than the third layer.
[0062] Clause 2. The variable density isocyanate-based polymer material of clause 1, wherein: (a) the variable density isocyanate-based polymer material exhibits a flexural rigidity that is equal to or greater than a flexural rigidity of a material of same thickness and formed entirely of the first layer; and / or (b) the variable density isocyanate -based polymer material exhibits a flexural strength that is equal to or greater than a flexural strength of a material of same thickness and formed entirely of the first layer.
[0063] Clause 3. The variable density isocyanate -based polymer material of any one of preceding clauses, wherein the density of the first layer and the density of the third layer are substantially the same.
[0064] Clause 4. The variable density isocyanate-based polymer material of any one of preceding clauses, wherein the second layer has a density that is 5% to 65% the density of the first layer, such as 10% to 50% the density of the first layer.
[0065] Clause 5. The variable density isocyanate-based polymer material of any one of the preceding clauses, wherein the thickness of the second layer is equal to or greater than the thickness of the first layer and equal to or greater than the thickness of the third layer.
[0066] Clause 6. The variable density isocyanate-based polymer material of any one of the preceding clauses, wherein the isocyanate-based polymer of the first layer, isocyanate-based polymer of the second layer, and isocyanate-based polymer of the third layer are chemically equivalent.
[0067] Clause 7. The variable density isocyanate-based polymer material of any one of the preceding clauses, wherein the isocyanate -based polymer of the second layer has a Shore D hardness of at least 60, or at least 65, measured according to ASTM D2240-15.
[0068] Clause 8. The variable density isocyanate -based polymer material of any one of the preceding clauses, wherein the variable density isocyanate-based polymer material does not include an elastomeric layer between the first layer and the third layer.
[0069] Clause 9. The variable density isocyanate-based polymer material of any one of the preceding clauses, further comprising an elastomeric layer disposed over the third layer on a side opposite the second layer, wherein the elastomer layer optionally comprises a polyurea elastomer.
[0070] Clause 10. The variable density isocyanate-based polymer material of any one of the preceding clauses, further comprising a gelcoat layer disposed over the first layer on a side opposite the second layer, wherein the gelcoat layer optionally comprises polyurea.
[0071] Clause 11. A variable density isocyanate-based polymer material, comprising: (a) a first layer comprising isocyanate-based polymer of a first density, the structural layer defining a plurality of voids; and (b) a second layer disposed within the voids, the second layer comprising an isocyanate-based polymer of a second density that is lower than the first density.
[0072] Clause 12. The variable density isocyanate-based polymer material of clause 11, wherein the second layer has a density that is 5% to 65% the density of the first layer, such as 10% to 50% the density of the first layer.
[0073] Clause 13. The variable density isocyanate-based polymer material of any one of clauses 11-12, wherein the second layer completely fills the voids of the structural layer.
[0074] Clause 14. The variable density isocyanate-based polymer material of any one of clauses 11-13, wherein the isocyanate-based polymer of the first layer and the isocyanate-based polymer of the second layer are chemically the same.
[0075] Clause 15. The variable density isocyanate-based polymer material of any one of clauses 11-14, wherein the first layer is configured as a lattice structure, such as a grid pattern.
[0076] Clause 16. A method of manufacturing a variable density isocyanate -based polymer material (such as in any one of clauses 1-15), the method comprising: spraying a first portion of an uncured mixture over a substrate to form a first layer, the uncured mixture comprising an isocyanate component and a co-reactant component; and spraying a second portion of the uncured mixture over the first layer to form a second layer, wherein forming the first layer and / or second layer comprises combining an aqueous solution with the first portion and / or second portion of the uncured mixture, the aqueous solution being formulated to react with the uncured mixture to form bubbles therein, wherein combining the aqueous solution with the uncured mixture comprises (i) directing a stream of the aqueous solution into a stream of the uncured mixture, and / or (ii) mixing the aqueous solution with the co-reactant component and combining a first stream that includes the isocyanate component with a second stream that includes the co-reactant component and the aqueous solution, wherein (a) one of the first layer or second layer is formed without addition of the aqueous solution to the uncured mixture, or (b) different proportional amounts of the aqueous solution are used to form the first layer as compared to the second layer, such that (because of (a) or (b)) a density of the first layer is different from a density of the second layer.
[0077] Clause 17. The method of clause 16, wherein the first layer includes a substantially uniform density and / or the second layer includes a substantially uniform density, optionally wherein a transition from the first layer to the second layer is discrete, such as wherein the first layer is cured before application of the second layer.
[0078] Clause 18. The method of clause 16, wherein the first layer, the second layer, or both include a density gradient extending through at least a part of a thickness of the layer, suchas wherein a transition from the first layer to the second layer is continuous, such as wherein the uncured mixture is continuously applied to form both the first layer and the second layer while a delivery rate of the aqueous solution is ramped up or down relative to a delivery rate of the uncured mixture.
[0079] Clause 19. The method of any one of clauses 16-18, wherein the substrate comprises a mold, the mold optionally being coated with a release agent.
[0080] Clause 20. The method of any one of clauses 16-19, further comprising forming a gelcoat layer on the substrate prior to forming the first layer and the second layer, wherein optionally the gelcoat comprises polyurea.
[0081] Clause 21. The method of any one of clauses 16-20, wherein the aqueous solution comprises (1) a foam stabilizer, such as a copolymer of a siloxane and a poly oxy alkylene, and / or (2) an isocyanate-water reaction catalyst, such as a tertiary amine.
[0082] Clause 22. The method of any one of clauses 16-21, wherein the isocyanate-based polymer of the first layer and the isocyanate-based polymer of the second layer are chemically equivalent.
[0083] Clause 23. The method of any one of clauses 16-22, wherein the density of the first layer is greater than the density of the second layer.
[0084] Clause 24. The method of clause 23, wherein the second layer has a density that is 5% to 65% the density of the first layer, such as 10% to 50% the density of the first layer, or 15% to 45% the density of the first layer, or a density within a range with endpoints selected from any two of the foregoing values.
[0085] Clause 25. The method of any one of clause 23 or clause 24, wherein the second layer has a Shore D hardness of at least 60, or at least 65, measured according to ASTM D2240-15.
[0086] Clause 26. The method of any one of clauses 16-25, further comprising spraying a third portion of the uncured mixture over the second layer, the uncured mixture curing to form a third layer, wherein both the first layer and the third layer have densities greater than the density of second layer.
[0087] Clause 27. The method of clause 26, wherein the first layer and the third layer are configured as structural layers that are formed without addition of the aqueous solution to theuncured mixture, and the second layer is configured as a foam layer and forming the second layer comprises combining the aqueous solution with the uncured mixture.
[0088] Clause 28. The method of any one of clause 26 or clause 27, wherein the density of the first layer and the density of the third layer are the same.
[0089] Clause 29. The method of any one of clauses 26-28, wherein the thickness of the second layer is equal to or greater than the thickness of the first layer and is equal to or greater than the thickness of the third layer.
[0090] Clause 30. The method of any one of clauses 26-29, wherein the isocyanate-based polymer of the first layer, second layer, and third layer are chemically equivalent.
[0091] Clause 31. The method of any one of clauses 26-30, wherein the variable density isocyanate-based polymer material does not include an elastomeric layer between the first layer and the second layer.
[0092] Clause 32. The method of any one of clauses 26-31, further comprising forming a bottom / inner layer over the third layer, the bottom / inner layer comprising an elastomeric material, such as an elastomeric polyurea.
[0093] Clause 33. The method of any one of clauses 26-32, wherein the variable density isocyanate-based polymer material manufactured by the method exhibits: a flexural rigidity that is equal to or greater than a flexural rigidity of a material of same thickness and formed entirely of the first layer; and / or a flexural strength that is equal to or greater than a flexural strength of a material of same thickness and formed entirely of the first layer.
[0094] Clause 34. The method of any one of clauses 23-25, wherein the first layer is configured in a pattern that defines a plurality of voids; and the second layer is disposed within the voids.
[0095] Clause 35. The method of clause 34, wherein the first layer is configured as a structural layer formed without addition of the aqueous solution to the uncured mixture, and the second layer is configured as a foam layer and forming the second layer comprises combining the aqueous solution with the uncured mixture.
[0096] Clause 36. The method of any one of clause 34 or clause 35, wherein the second layer completely fills the voids of the first layer.
[0097] Clause 37. The method of any one of clauses 34-36, wherein the first layer is arranged in a lattice structure, such as a grid pattern.
[0098] Clause 38. An isocyanate-based polymer material, comprising: a first structural layer comprising an isocyanate-based polymer: a second structural layer comprising an isocyanate-based polymer; and an adhesive scrim disposed between the first and second structural layers, wherein the adhesive scrim has a per layer density of 0.005 g / cm2to 0.1 g / cm2.
[0099] Clause 39. The isocyanate-based polymer material of clause 38, wherein the isocyanate -based polymer of the first structural layer and the isocyanate -based polymer of the second structural layer are chemically equivalent.
[0100] Clause 40: The method of any one of clauses 16-37, wherein the aqueous solution is combined with the uncured mixture for the first layer in an amount of 0.1 to 5 wt.%, 0.2 to 3 wt.%, 0.25 to 2.5 wt.%, or 0.3 to 2 wt.%, based on the total weight of the uncured mixture used to form the first layer, or in an amount within a range using any combination of the foregoing values as endpoints.
[0101] Clause 41: The method of any one of clauses 16-37 and 40, wherein the aqueous solution is combined with the uncured mixture for the second layer in an amount of 0.1 to 5 wt.%, 0.2 to 3 wt.%, 0.25 to 2.5 wt.%, or 0.3 to 2 wt.%, based on the total weight of the uncured mixture used to form the second layer, or in an amount within a range using any combination of the foregoing values as endpoints.
[0102] Clause 42: The method of any one of clauses 16-37 and 40-41, wherein the density of the second layer is 50 to 700 kg / m3, or 100 to 600 kg / m3, or 150 to 550 kg / m3, or 200 to 500 kg / m3, or is within a range using any combination of the foregoing values as endpoints.
[0103] Clause 43: The method of any one of clauses 16-37 and 40-42, wherein the density of the first layer and / or third layer is 750 to 2000 kg / m3, or 800 to 1800 kg / m3, or 900 to 1500 kg / m3, or 950 to 1300 kg / m3, or is within a range using any combination of the foregoing values as endpoints.Additional Terms & Definitions
[0104] While certain aspects of the present disclosure have been described in detail, with reference to specific components and / or features, the descriptions are illustrative and are not to be construed as limiting the scope of the claimed coating composition or related methods.
[0105] For any given component of a described example, any of the possible alternatives listed for that component may generally be used individually or in combination with oneanother, unless implicitly or explicitly stated otherwise. The various features of a given example can be combined with and / or incorporated into other examples disclosed herein. Thus, disclosure of certain features relative to a specific example should not be construed as limiting application or inclusion of said features to the specific example. Rather, it will be appreciated that other examples can also include such features.
[0106] Any headings and subheadings used herein are for organizational purposes only and are not meant to be used to limit the scope of the description or the claims.
[0107] Any standard testing method discussed herein (e.g., ASTM) will be understood to refer to the most recent version of the testing method available at the time of filing of this disclosure, unless specified otherwise.
[0108] It will also be noted that, as used in this specification and the appended claims, the singular forms “a,” “an” and “the” do not exclude plural referents unless the context clearly dictates otherwise. Thus, for example, an embodiment referencing a singular referent may also include two or more such referents.
[0109] The examples disclosed herein should be understood as comprising / including disclosed components, and may therefore include additional components not specifically described. Optionally, the examples disclosed herein are essentially free or completely free of components that are not specifically described. For example, isocyanate components, polyamine components, and composite material layers not specifically disclosed herein may optionally be completely omitted or essentially omitted from the disclosed multilayer polyurea materials.
[0110] A composition that “essentially omits” or is “essentially free of’ a component may include trace amounts and / or non-functional amounts of the component. For example, an “essentially omitted” component may be included in an amount no more than 1%, no more than 0.1%, no more than 0.05%, no more than 0.01%, or no more than 0.005% by total weight of the composition.
[0111] A composition that “completely omits” or is “completely free of’ a component does not include a detectable amount of the component (i.e., does not include an amount above any inherent background signal associated with the testing instrument) when analyzed using standard coating composition analysis techniques such as, for example, chromatographic techniques (e.g., thin-layer chromatography (TLC), gas chromatography (GC), liquidchromatography (LC)), or spectroscopy techniques (e.g., Fourier transform infrared (FTIR) spectroscopy).EXAMPLES
[0112] In the following description, the term “Example” refers to a specific test or process carried out as described, whereas the term “Example Material” refers to a specific composition formulated and arranged as described. While the following Examples relate primarily to polyurea-based materials, it will be understood that other isocyanate-based polymers, such as those disclosed herein, can be utilized to form other variable density isocyanate-based polymer materials, including variable density polyurethane materials and variable density polyureaurethane hybrid materials.Example 1
[0113] Variable-density polyurea materials were manufactured by preparing an A-side (isocyanate component), B-side (polyamine component), and aqueous solution (foam stabilizer and isocyanate-water reaction catalyst). The commercial product RESTORA-PIPE 202 XT HARDENER PART A (PPG Industries, Inc.) was used as the A-side. The composition of the product, as provided by the manufacturer’s safety data sheet, is shown in Table 1A.Table 1AIngredient Wt. % CAS number Isocyanic acid, polymethylenepolyphenylene ester >50 - <75 9016-87-9 4,4'-methylenediphenyl diisocyanate >20 - <45 101-68-8 o-(p-isocyanatobenzyl)phenyl isocyanate >5.0 - <9.6 5873-54-1
[0114] The commercial product RESTORA-PIPE 202 XT LIGHT GRAY PART B (PPG Industries, Inc.) was used as the B-side. The composition of the product, as provided by the manufacturer’s safety data sheet, is shown in Table IB.Table IBIngredient Wt. % CAS number Diethylmethylbenzenediamine >20 - <50 68479-98-1 Poly[oxy(methyl- 1 ,2-ethanediyl)], a-hydro-o-hydroxy-, >10 - <20 31568-06-6 ether with [[2-[(2-hydroxyethyl)(2- hydroxymethylethyl)amino]ethyl]imino]bis[propanol](4:1)polyoxypropylene triamine >10 - <20 N / APoly [oxy(methyl- 1 ,2-ethanediyl)], a- >10 - <20 9046-10-0 (2-aminomethylethyl)-or-(2-aminomethylethoxy)- (n > 6)Pentaerythritol, propoxylated >5.0 - <10 9051-49-4 titanium dioxide >1.0 - <5.0 13463-67-7 Propane- 1,2-diol, propoxylated >1.0 - <4.9 25322-69-4carbon black <1.0 1333-86-4
[0115] The aqueous solution was formulated by mixing the components of Table 1C in water. The SILSTAB products are commercially available from Siltech Corp. (Toronto, Ontario, Canada). The TEGOSTAB 8404 and POLYCAT 5 products arc commercially available from Evonik Industries AG (Essen, Germany). The SILSTAB and TEGOSTAB products are block copolymers of dimethyl-siloxane and a polyoxyalkylene, and function as surfactants and foam stabilizers that can promote uniformity and stability of the foam layer before solidifying. The POLYCAT 5 product is a pentamethyldiethylenetriamine (PMDETA) tertiary amine catalyst. Such a catalyst can promote the water-isocyanate reaction to generate CO2 bubbling to form the foam layer.Table 1CIngredient Wt. %TEGOSTAB 8404* 0-5POLYCAT 5 0.5Water Remainder* TEGOSTAB can be substituted with SILSTAB 2100, 2550, 2580, and / or 2760
[0116] The A-side and B-side formulations were loaded into a high-pressure pump (REACTOR E-10 HP, Graco Inc.). The A-side and B-side formulations were mixed immediately prior to passing through a sprayer nozzle. The aqueous solution was passedthrough a separate, adjustable flow rate nozzle and sprayed into the stream of the mixed A-side and B-side formulations. Adjusting the flow rate of the aqueous solution relative to mixed A-side and B-side streams enabled the formation of foam layers of various densities, as shown in Table ID. A default “structural” layer did not include spraying of the aqueous solution into the A-sidc and B-sidc mixture.Tabic IDAqueous solution 0 0.3 0.75 1 1.35 (wt. % in final product) (structurallayer)Density 74 30 15 12.5 10 (Ibs. / ft3)Density 1185 481 240 200 160(kg / m3)
[0117] As shown by the density values, even the densest foam layers use less than half the liquid material than the structural layer for a given thickness.Example 2
[0118] The Example Materials shown in Table 2 were prepared. The structural layers (“Structural 1” and “Structural 2”) were prepared according to the process of Example 1 (without the aqueous solution). For the Example Materials that included a foam layer (Example Materials 2-6), the foam layers were prepared according to the process of Example 1, with the aqueous solution applied with a flow rate to give 0.3 wt. % aqueous solution in the final product. The gelcoats were formed using BDL95663G1 (pigmented amine mixture) and CAT150 (aliphatic isocyanate), both available from PPG Industries, Inc. The gelcoat was kept constant for all Example Materials and did not contribute significantly to the tested properties.Table 2LayerEx. 1Thickness(1)Ex.2 Ex. 4 Ex.6(c Ex.3 Ex.5(mil / mm) omparative)Gelcoat(2)30 / 0.76 30 / 0.76 30 / 0.76 30 / 0.76 30 / 0.76 30 / 0.76 Structural 1 140 / 3.56 60 / 1.52 50 / 1.27 50 / 1.27 50 / 1.27 100 / 2.54Foam - 100 / 2.54 50 / 1.27 100 / 2.54 200 / 5.08 50 / 1.27 Structural 2 - - 50 / 1.27 50 / 1.27 50 / 1.27 100 / 2.54 Total(31140 / 3.56 160 / 4.06 150 / 3.81 200 / 5.08 300 / 7.62 250 / 6.35 ResultsFlexuralRigidity*411.23 0.20 1.32 1.89 3.53 1.94 (N-m2)FlexuralStrength 6950 / 1257 / 7699 / 3641 / 2354 / 3641 / 47.9 8.67 53.1 25.1 16.2 25.1 (psi / MPa)(1) Thicknesses have a variance of ± 10% as applied due to spray application tolerances.(2) Gelcoat used for decorative purposes; contribution to material properties was insignificant.(3) Reported total thickness does not include gelcoat.(4) Normalized to 50 mm width.
[0119] Throughout the Examples, flexural strength was measured according to ASTM D790-17. Normalized flexural rigidity was measured using the three-point bending test described in ASTM D790-17. Sample width and overall length were 0.5” and 5”, respectively. However, because some samples including foam layer had specimen dimension of 2” x 6”, flexural rigidity was normalized according to specimen width. Span was held constant for all samples. A test speed of 10 mm / min was applied to deform the sample.
[0120] Foam layers can weigh less and cost less than the structural layer. However, foam layers typically have lower flexural rigidity and flexural strength. Conventionally, for two materials of similar overall thickness, the higher density, heavier system generally has greater flexural rigidity and flexural strength. For example, Example Material 1 (no foam layer) has a higher density than Example Material 2 (includes foam layer). Example Material 1 has, as expected, greater flexural rigidity and strength than Example Material 2.
[0121] However, lighter weight, lower density materials can exhibit equivalent or better flexural rigidity and strength than higher density materials when formed according to the present disclosure. As demonstrated by Table 2, Example Material 3 contained a 50 mil foam layer, yet exhibited better normalized flexural rigidity and equivalent or better flexural strength than Example Formulation 1. The top and bottom layers (outer and inner layers) are generally deformed more significantly than the middle layer(s) during bending, and two separate samples can therefore exhibit similar strength and rigidity even if one includes a foam layer as a middle layer and the other does not.
[0122] Comparing Example Materials 3, 4, and 5 shows that increasing the thickness of the foam layer can further increase the flexural rigidity and strength. Considering Example Material 3 as a baseline and comparing Example Materials 4 and 6 shows that increasing the thickness of the foam layer (Example Material 4) has a greater positive effect on flexural rigidity and strength than increasing the thickness of the outer and inner structural layers (Example Material 6).
[0123] In sum, Example 2 demonstrates that use of a foam layer disposed between two structural layers can maintain or even improve flexural rigidity and strength as compared to the same (otherwise) material without a foam layer at reduced material usage and reduced weight.Example 3
[0124] Example Materials 7-9 were constructed using a softer (lower Shore D hardness) elastomeric polyurea layer in place of the foam layer of Example Materials 3-5 in Example 2. The elastomer polyurea layer was formed using the A and B packs of the commercial product FULL METAL JACKET® HYBRID POLYUREA (PPG Industries, Inc.). The composition of the product, as provided by the manufacturer’s safety data sheets, is shown in Table 3 A. Table 3B compares Example Materials 3-5 to Example Materials 7-9.Table 3AIngredient Wt. % CAS number A-PackPropane- 1,2-diol, propoxylatcd (MW<2000) >20 - <50 25322-69-4 4,4'-methylenediphenyl diisocyanate >20 - <34 101-68-8 methylenediphenyl diisocyanate >10 - <15 26447-40-5 Isocyanic acid, polymethylenepolyphenylene ester >5.0 - <10 9016-87-9 propylene carbonate >5.0 - <10 108-32-7 4-[[p-(p-isocyanatobenzyl)phenyl]imino]-2-oxo-l,3- >1.0 - <5.0 31107-36-5 di azetidine- 1 ,3-diylbis(pphenylenemethylene-p- phenylene) diisocyanateo-(p-isocyanatobenzyl)phenyl isocyanate >0.10 - <2.3 5873-54-1 2,2'-methylenediphenyl diisocyanate <1.0 2536-05-2B-PackOxirane, 2-methyl-, polymer with oxirane, ether with >20 - <50 9082-00-2 1,2,3-propanetriol (3:1)diethylmethylbenzenediamine >20 - <37 68479-98-1Propane- 1,2-diol, propoxylated (MW<2000) >1.0 - <5.0 25322-69-4 carbon black >1.0 - <5.0 1333-86-4bi s( 1 ,2,2,6, 6-pentamethyl-4-piperidyl) sebacate <1.0 41556-26-7Table 3BLayerEx.7Thickness*11Ex.3 Ex. 4 Ex.5 Ex. 8 Ex. 9(comparative) (comparative) (comparative) (mil / mm)Gelcoat*2130 / 0.76 30 / 0.76 30 / 0.76 30 / 0.76 30 / 0.76 30 / 0.76 Structural 1 50 / 1.27 50 / 1.27 50 / 1.27 50 / 1.27 50 / 1.27 50 / 1.27 Foam 50 / 1.27 100 / 2.54 200 / 5.08 - - - Elastomer- - - 50 / 1.27 100 / 2.54 200 / 5.08 middleStructural 2 50 / 1.27 50 / 1.27 50 / 1.27 50 / 1.27 50 / 1.27 50 / 1.27 Total*31150 / 3.81 200 / 5.08 300 / 7.62 150 / 3.81 200 / 5.08 300 / 7.62 ResultsFlexuralRigidity*4* 1.32 1.89 3.53 0.21 0.49 1.17(N-m2)Flexural 7699 / 3641 / 2354 / Strength 4278 / 29.5 4355 / 30.0 2926 / 20.253.1 25.1 16.2(psi / MPa)(1) Thicknesses have a variance of ± 10% as applied due to spray application tolerances.(2) Gelcoat used for decorative purposes; contribution to material properties was insignificant.(3) Reported total thickness does not include gelcoat.(4) Normalized to 50 mm width.
[0125] The normalized flexural rigidities of Example Materials 7-9 were significantly lower than for Example Materials 3-5, demonstrating that using a foam layer as a middle layer is more effective than using an elastomer layer as a middle layer.
[0126] Shore D surface hardness was measured according to ASTM D2240-15. The foam layer had a Shore D hardness of 65, and the elastomer layer had a Shore D hardness of 50. The results demonstrate that the middle layer’s resistance to external impact, such as due to shape change of the other layers, can affect the flexural rigidity of the overall material. Effective flexural rigidity can be exhibited when the Shore D hardness of the middle layer is 55 or more, such as 60 or more, such as 65 or more.Example 4
[0127] Example Materials 10 and 11 were the same as Example Materials 4 and 5, respectively, but further included 50 mils of an elastomer layer (the same elastomeric polyurea as used for the middle layer in Example Materials 7-9) added to the bottom (i.e., the side opposite the gelcoat). The bottom elastomer layer did not increase flexural rigidity, but did improve underside wear resistance. This can be beneficial for certain end uses, as the finished product may need to be dragged and / or contacted against other surfaces during transportation and installation. Table 4 shows the layer arrangements of Example Materials 4-5 and 10-11, also showing results of the bottom Hl 8 1000 cycle abrasion test according to ASTM D4060-1 . Example Materials 10 and 11 passed the cycle abrasion test by exhibiting a loss of less than 250 mg.Table 4Layer Thickness02Ex.4 Ex. 5 Ex. 10 Ex. 11(mil / mm)Gelcoat'230 / 0.76 30 / 0.76 30 / 0.76 30 / 0.76 Structural 1 50 / 1.27 50 / 1.27 50 / 1.27 50 / 1.27Foam 100 / 2.54 200 / 5.08 100 / 2.54 200 / 5.08 Structural 2 50 / 1.27 50 / 1.27 50 / 1.27 50 / 1.27 Elastomer bottom - - 50 / 1.27 50 / 1.27Totaf32200 / 5.08 300 / 7.62 250 / 6.35 350 / 8.89 ResultsFlexural Rigidity1421.89 3.53 1.82 3.10(Nm2)Flexural Strength3641 / 25.1 2354 / 16.2 2825 / 19.5 1925 / 13.3(psi / Mpa)Bottom surfaceNot pass Not pass Pass Passabrasion loss(5)(1 ) Thicknesses have a variance of ± 10% as applied due to spray application tolerances. (2) Gelcoat used for decorative purposes; contribution to material properties was insignificant. (3) Reported total thickness does not include gelcoat.(4) Normalized to 50 mm width.(5) Bottom surface abrasion H18 1000 cycle according to ASTM D4060-19; pass with loss less than 250 mg
[0128] The inclusion of a bottom side elastomer layer was also found to prevent other layers from falling apart or detaching after incurring damage. The elastomer layer was typically the last layer to break during severe impact testing and functioned to hold broken pieces of other layers together. Repairs can more readily be made when broken or damaged pieces remain substantially in their intended arrangements.Example 5
[0129] For many applications such as bathtubs or decorative accessories, the flexural strength (the maximum stress the material can withstand before breaking during a bending process) only needs to be high enough to cope with shipping and installation, as the back of the item will be filled or contacted against other building materials such as cement, concrete, and / or sand after installation. For such applications, a flexural strength of 1900 psi (13.1 MPa) or greater is typically sufficient. However, some applications, such as wall panels, may not involve ancillary construction materials directly behind the article, and the material can benefit from higher flexural strength to protect against unexpected high-impact events.
[0130] One conventional approach is to spray chopped glass fibers into the structural layer of the material to enhance flexural strength. The use of chopped fiberglass involves disadvantages such as skin irritation and other health hazards to the operator, fiberglass contamination in other areas of the production line, and product quality control issues caused by heat buildup and / or air trapped under the fiberglass.
[0131] Table 5 compared a conventional material that includes chopped fiberglass (Example Material 12) to examples that instead used an adhesive scrim (Example Materials 13-17). The adhesive scrim was an ADFORS Laid Scrim (Saint-Gobain) with density as shown in Table 5. The “Structural” layer was made in the same manner as the structural layers of Example 2 (without aqueous solution).Table 5LayerEx. 12Thickness(1)(comp.) Ex. 13 Ex. 14 Ex. 15 Ex. 16 Ex. 17 (mil / mm)Gelcoat'230 / 0.76 30 / 0.76 30 / 0.76 30 / 0.76 30 / 0.76 30 / 0.76 Structural 300 / 7.62 150 / 3.81 150 / 3.81 200 / 5.08 300 / 7.62 300 / 7.62Fiberglassadded toYes No No No No No structural(0.030 g / cm2)Adhesivescrim (no. oflayers) 0 1 1 2 3 4 (0.0156g / cm2)Total® 300 / 7.62 150 / 3.81 150 / 3.81 200 / 5.08 300 / 7.62 300 / 7.62 ResultsFlexuralRigidity11(N- 3.14 1.14 1.33 2.36 6.10 8.61 m2)Flexural 10209 / Strength (psi / 10908 / 8533 / 58.8 9466 / 65.3 9383 / 64.7 9818 / 67.7 75.2 70.4 MPa)(1) Thicknesses have a variance of ± 10% as applied due to spray application tolerances.(2) Gelcoat used for decorative purposes; contribution to material properties was insignificant.(3) Reported total thickness does not include gelcoat.(4) Normalized to 50 mm width.
[0132] Table 5 demonstrates that the performance of the conventional chopped glass fiber material can be achieved or exceeded by utilizing layers of adhesive scrim fibers. The adhesive scrims were able to effectively stick to the material surface and prevented air from entering under the scrim, even under high-pressure material spraying. The adhesive also allowed easily and efficient positioning of the scrim (i.e., in a matter of seconds).Example 6
[0133] Example Material 18 was formed as shown in Table 6 and was compared against Example Material 17. The structural layers (“Structural 1” and “Structural 2”) were formed in the same manner as the structural layers of Example 2 (without aqueous solution) and the “Elastomer middle” was formed in the same manner as the elastomer middle of Example 3.Table 6Layer Thickness® Ex. 17 Ex. 18(mil / mm) (comparative) Gelcoat® 30 / 0.76 30 / 0.76Structural 1 300 / 7.62 200 / 5.08Adhesive scrim(no. of layers) 4 0Elastomer middle - 200 / 5.08Structural 2 - 200 / 5.08Total'1300 / 7.62 600 / 15.24ResultsFlexural Rigidity(4)(Nm2) 8.61 8.87Flexural Strength 10209 / 70.4 1943 / 13.4(psi / Mpa)(1) Thicknesses have a variance of ± 10% as applied due to spray application tolerances. (2) Gelcoat used for decorative purposes; contribution to material properties was insignificant. (3) Reported total thickness does not include gelcoat.(4) Normalized to 50 mm width.
[0134] Example Material 18 exhibited high rigidity due to the two 200 mil structural layers; however, the strength was 10 times lower than Example Material 17 despite having twice the thickness of Example Material 17. As with the example materials that include a foam layer, the example materials that include an adhesive scrim can achieve effective strength and rigidity while maintaining lighter weight and lower material requirements.Example 7
[0135] Finite element analysis (FEA) was conducted to analyze the flexural rigidity of multi-layer polyurea materials under 3-point bending. Simulated samples were tested using ABAQUS in a general, static nonlinear step. Figure 5A illustrates the simulated sample setup. Simulated samples had dimensions of 100 mm x 25 mm x 15 mm. The simulated loading rods had a radius of 2 mm, and the span between the 2 lower support rods was 72 mm. A deflection of 10 mm was applied for the simulation.
[0136] Figure 5B illustrates the FEA setup. The simulated samples included an uppermost gelcoat with 1.5 mm thickness. The next layer was a structural layer (corresponding to Table ID) with thickness of 2.0 mm. The next layer was a patterned structural layer with foam layer (corresponding to 1 wt. % aqueous solution of 'Table ID) filling the voids, with thickness of 10.0 mm. The bottom layer was an elastomer layer (corresponding to the elastomer bottom of Example Materials 10 and 11) with thickness of 1.5 mm.
[0137] Simulated materials with different patterned structural layers were tested, including box-shaped and C-shaped grids with 0 to 3 longitudinal “ribs” of structural material. Figure 5B illustrates, in cross sectional view, a C-shaped grid with 2 ribs (one rib on each side), a C-shaped grid with 1 rib (running down the center), a box-shaped grid with 2 ribs, and a boxshaped grid with a single rib. The shorter lateral ribs did not contribute significantly to the simulation results. An “empty area” sample including a box-shaped, 3-rib grid with empty voids (i.e., no foam filler) was also simulated.
[0138] Figure 5C shows stiffness (relative to a pure foam layer) of the grid pattern materials at different volumetric ratios of structural material to foam material. The simulations demonstrated that the increases in relative stiffness were greater than would be expected from a simple linear relationship based on volumetric amounts of structural material. That is, the grid pattern examples met or outperformed what would be expected from a straight line between the “Pure foam” and “Pure structural” data points. Configuring structural material in a pattern can therefore improve performance while minimizing raw materials and weight.
Claims
CLAIMS1. A method of manufacturing a variable density isocyanate-based polymer material, the method comprising:applying a first portion of an uncured mixture over a substrate to form a first layer, the uncured mixture comprising an isocyanate component and a co-reactant component; and applying a second portion of the uncured mixture over the first layer to form a second layer,wherein forming the first layer and / or second layer comprises combining an aqueous solution with the first portion and / or second portion of the uncured mixture, the aqueous solution being formulated to react with the uncured mixture to form bubbles therein, wherein combining the aqueous solution with the uncured mixture comprises(i) directing a stream of the aqueous solution into a stream of the uncured mixture, and / or(ii) mixing the aqueous solution with the co-reactant component and combining a first stream that includes the isocyanate component with a second stream that includes the co-reactant component and the aqueous solution,wherein(a) one of the first layer or second layer is formed without addition of the aqueous solution to the uncured mixture, or(b) different proportional amounts of the aqueous solution are used to form the first layer as compared to the second layer,such that a density of the first layer is different from a density of the second layer.
2. The method of claim 1, wherein the first layer includes a substantially uniform density and / or the second layer includes a substantially uniform density.
3. The method of any one of the preceding claims, wherein the first layer, the second layer, or both include a density gradient extending through at least a part of a thickness of the layer,such as wherein the uncured mixture is continuously applied while a delivery rate of the aqueous solution is ramped up or down relative to a delivery rate of the uncured mixture.
4. The method of any one of the preceding claims, wherein the substrate comprises a mold, the mold optionally being coated with a release agent.
5. The method of any one of the preceding claims, further comprising forming a gelcoat layer on the substrate prior to forming the first layer and the second layer, wherein optionally the gelcoat comprises polyurea.
6. The method of any one of the preceding claims, wherein the aqueous solution comprises (1) a foam stabilizer, such as a copolymer of a siloxane and a poly oxy alkylene, and / or (2) an isocyanate-water reaction catalyst, such as a tertiary amine.
7. The method of any one of the preceding claims, wherein the isocyanate -based polymer of the first layer and the isocyanate-based polymer of the second layer are chemically equivalent.
8. The method of any one of the preceding claims, wherein the density of the first layer is greater than the density of the second layer, optionally wherein:the density of the first layer is 750 to 2000 kg / m3, or 800 to 1800 kg / m3, or 900 to 1500 kg / m3, or 950 to 1300 kg / m3, or is within a range using any combination of the foregoing values as endpoints; and / orthe density of the second layer is 50 to 700 kg / m3, or 100 to 600 kg / m3, or 150 to 550 kg / m3, or 200 to 500 kg / m3, oris within a range using any combination of the foregoing values as endpoints.
9. The method of claim 8, wherein the second layer has a density that is 5% to 65% the density of the first layer, such as 10% to 50% the density of the first layer, or 15% to 45% the density of the first layer, or a density within a range with endpoints selected from any two of the foregoing values.
10. The method of claim 8 or claim 9, wherein the second layer has a Shore D hardness of at least 60, or at least 65.
11. The method of any one of the preceding claims, further comprising applying a third portion of the uncured mixture over the second layer, wherein both the first layer and the third layer have densities greater than the density of second layer, optionally wherein the density of the third layer is 750 to 2000 kg / m3, or 800 to 1800 kg / m3, or 900 to 1500 kg / m3, or 950 to 1300 kg / m3, or is within a range using any combination of the foregoing values as endpoints.
12. The method of claim 11, whereinthe first layer and / or the third layer are configured as structural layers that are formed without addition of the aqueous solution to the uncured mixture, andthe second layer is configured as a foam layer and forming the second layer comprises combining the aqueous solution with the uncured mixture.
13. The method of claim 11 or claim 12, wherein the density of the first layer and the density of the third layer are the same.
14. The method of any one of claims 11-13, wherein the thickness of the second layer is equal to or greater than the thickness of the first layer and is equal to or greater than the thickness of the third layer.
15. The method of any one of claims 11-14, wherein the isocyanate-based polymer of the first layer, second layer, and third layer are chemically equivalent.
16. The method of any one of claims 11-15, wherein the variable density isocyanate-based polymer material does not include an elastomeric layer between the first layer and the second layer.
17. The method of any one of claims 11-16, further comprising forming a bottom / inner layer over the third layer, the bottom / inner layer comprising an elastomeric material, such as an elastomeric polyurea.
18. The method of any one of claims 11-17, wherein the variable density isocyanate-based polymer material manufactured by the method exhibits:a flexural rigidity that is equal to or greater than a flexural rigidity of a material of same thickness and formed entirely of the first layer; and / ora flexural strength that is equal to or greater than a flexural strength of a material of same thickness and formed entirely of the first layer.
19. The method of any one of the preceding claims, whereinthe first layer is configured in a pattern that defines a plurality of voids; and the second layer is disposed within the voids.
20. The method of claim 1 , wherein the second layer completely fills the voids of the first layer.
21. The method of claim 19 or claim 20, wherein the first layer is arranged in a lattice structure, such as a grid pattern.
22. The method of any one of the preceding claims, wherein the co-reactant component comprises a polyamine and wherein the isocyanate-based polymer material comprises polyurea.
23. The method of any one of the preceding claims, wherein:forming the first layer comprises combining the aqueous solution with the uncured mixture in an amount of 0.1 to 5 wt.%, or 0.2 to 3 wt.%, or 0.25 to 2.5 wt.%, or 0.3 to 2 wt.%, based on total weight of the uncured mixture used to form the first layer; and / orforming the second layer comprises combining the aqueous solution with the uncured mixture in an amount of 0.1 to 5 wt.%, or 0.2 to 3 wt.%, or 0.25 to 2.5 wt.%, or 0.3 to 2 wt.%, based on total weight of the uncured mixture used to form the second layer.
24. A variable density isocyanate-based polymer material, manufactured according to the method of any of claims 1-23.