Lithium tantalate electro-optic modulator

TFLT modulators with separate DC and RF electrode sections address the instability and power consumption issues of TFLN modulators, achieving stable DC operation and high RF bandwidth with low loss and error rates across varying temperatures.

WO2026236454A1PCT designated stage Publication Date: 2026-11-12PRESIDENT & FELLOWS OF HARVARD COLLEGE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/027050
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-05-07
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing thin-film lithium niobate (TFLN) electro-optic modulators suffer from slow relaxation of the electro-optic response, instability at elevated optical powers, and increased power consumption due to the need for active EO control or thermo-optic based biasing, while lithium tantalate (LT) modulators have not been widely adopted despite their superior properties.

Method used

Design and fabrication of thin-film lithium tantalate (TFLT) electro-optic modulators with separate DC and RF electrode sections, utilizing a path-length balanced Mach-Zehnder modulator structure to achieve superior DC stability and maintain low optical loss, RF bandwidth, and drive voltage, without the need for external bias-tees.

Benefits of technology

TFLT modulators exhibit less than 1 dB output power fluctuation over 46 hours, maintain low optical loss of 0.35 dB, and achieve flat RF electro-optic response from 3-50 GHz, with bit error rates below soft-division forward error correction thresholds over a wide temperature range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026027050_12112026_PF_FP_ABST
    Figure US2026027050_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The device comprises a monolithic substrate having a first side and a second side; an etched layer of electrooptical material disposed on the first side, the etched layer comprising a pair of ridge waveguides and a slab, the ridge waveguides extending from the slab; a first electrode section disposed on the slab at a first position with respect to the ridge waveguides, the first electrode section comprising a first plurality of electrodes configured to apply a DC bias to a first portion of each of the ridge waveguides; and a second electrode section disposed on the slab at a second position with respect to the ridge waveguides, the second position being spaced apart from the first position, the second electrode section comprising a second plurality of electrodes, the second plurality of electrodes configured to apply an RF signal to a second portion of each of the ridge waveguides.
Need to check novelty before this filing date? Find Prior Art

Description

HCU-08225 (HU 10197)LITHIUM TANT ALATE ELECTRO-OPTIC MODULATORCROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims the benefit of priority to U.S. Provisional App. No. 63 / 801,422, filed on May 7, 2025, and U.S. Provisional App. No. 63 / 802,206, filed on May 8, 2025. The entire contents of each application are hereby incorporated by reference.BACKGROUND

[0002] Embodiments of the present disclosure relate to electro-optic modulators, and more specifically to DC-stable electro-optic modulators using thin-film lithium tantalate.BRIEF SUMMARY

[0003] In a first example embodiment, the present invention is a device, comprising a monolithic substrate having a first side and a second side; an etched layer of electrooptical material disposed on the first side of the monolithic substrate, the etched layer comprising a pair of ridge waveguides and a slab, the pair of ridge waveguides extending from the slab; a first electrode section disposed on the slab of the etched layer of electrooptical material at a first position with respect to the pair of ridge waveguides, the first electrode section comprising a first plurality of electrodes, the first plurality of electrodes configured to apply a DC bias to a first portion of each of the ridge waveguides; and a second electrode section disposed on the slab of the etched layer of electrooptical material at a second position with respect to the pair of ridge waveguides, the second position being spaced apart from the first position, the second electrode section comprising a second plurality of electrodes, the second plurality of electrodes configured to apply an RF signal to a second portion of each of the ridge waveguides.

[0004] In another example embodiment, the present invention is a method of manufacturing a device, comprising providing a monolithic substrate having a first side and a second side, the first side having a layer of electrooptical material disposed thereon; patterning the layer of electrooptical material; etching the layer of electrooptical material to define a pair of ridge waveguides and a slab, the pair of ridge waveguides extending from the slab; forming a first electrode section on the etched layer of electrooptical material at a first position with respect to the pair of ridge waveguides, the first electrode section comprising a first plurality of electrodes; and forming a second electrode section on the etched layer of electrooptical material at a second position with respect to the pair of ridge waveguides, theHCU-08225 (HU 10197)second position being spaced apart from the first position, the second electrode section comprising a second plurality of electrodes.BRIEF DESCRIPTION OF THE SEVERAL VIEWS OF THE DRAWINGS

[0005] Figs. 1A-1E depict integrated thin-film lithium tantalate-on-insulator electro-optics according to one or more embodiments of the present disclosure.

[0006] Figs. 2A-2D depict simulations for thin-film lithium tantalate modulators according to one or more embodiments of the present disclosure.

[0007] Figs. 3A-3B depict DC electro-optic characterization measurements according to one or more embodiments of the present disclosure.

[0008] Figs. 4A-4B depict RF electro-optic characterization measurements according to one or more embodiments of the present disclosure.

[0009] Figs. 5A-5C depict optical resonator measurements according to one or more embodiments of the present disclosure.

[0010] Fig. 6 depicts a topology of a lithium tantalate electro-optic modulator with separate DC bias and RF electrodes according to one or more embodiments of the present disclosure.

[0011] Fig. 7 depicts a topology of a lithium tantalate IQ modulator with separate DC bias and RF electrodes according to one or more embodiments of the present disclosure.

[0012] Figs. 8A-8B depict a cross-sectional view and a top view of a device according to one or more embodiments of the present disclosure.

[0013] Fig. 9 depicts cross-sectional electrode configurations for Z-cut lithium tantalate ridge waveguide modulators according to one or more embodiments of the present disclosure.

[0014] Fig. 10 depicts cross-sectional electrode configurations for X-cut lithium tantalate ridge waveguide modulators according to one or more embodiments of the present disclosure.DETAILED DESCRIPTION

[0015] Tel ecommuni cation-wavelength Pockels electro-optic modulators in thin-film lithium tantalate (TFLT) with superior DC stability compared to equivalent thin-film lithium niobate (TFLN) modulators are demonstrated. Less than 1 dB output power fluctuation for quadrature-biased TFLT is measured compared to 5 dB with TFLN over 46 hours with 12.1 dBm input power. TFLT modulators as described herein maintain properties similar to those in TFLN: 3.4 Vcm half-wave voltage length product, 39 dB extinction ratio, flat RF electrooptic response from 3-50 GHz, and 0.35 dB on-chip loss. Low error-rate data modulation over 0-70°C with TFLT modulators and optical loss of 9 dB / m are shown.HCU-08225 (HU 10197)

[0016] Thin-film lithium niobate (TFLN) integrated electro-optic (EO) circuits have bolstered many advancements in optical science and technology over the last several years . The most seminal EO device-the Mach-Zehnder modulator (MZM)- benefits a host of technologies in optical communications, sensing and computing. TFLN MZMs at telecommunication wavelengths have shown low half-wave voltage length products (V_7tL), e.g. 2.3 Vcm, and EO bandwidths beyond 100 GHz . Optical loss of TFLN was recently measured to be as low as 1.3 dB / m . An unresolved issue with TFLN modulators is slow (<kHz) relaxation of the EO response. As a result, active EO control of the modulator is employed, or alternatively thermo-optic based control and biasing is utilized to maintain bias point . The former, however, introduces additional complexities related to the stability of the low-frequency EO response, while the latter results in increased steady-state power consumption, thermal cross talk and is not compatible with cryogenic operation. Furthermore, at elevated optical powers the photorefractive effect in TFLN can introduce additional relaxation dynamics and instabilities, that can be exacerbated in thin films, and thus many demonstrations use low input power and / or power-consuming amplifiers at the chip output to compensate this effect .

[0017] Lithium tantalate (LT) is known to have slower and a smaller magnitude of EO relaxation than LN, while featuring comparable, or better, properties : EO coefficient (r_33~30 pm / V), bandgap 3.93 eV , 23* lower birefringence than LN at 633 nm , 5* lower photorefraction than LN at visible wavelengths , 2500* higher optical damage threshold than LN for green light , and 10x lower RF loss tangent than LN . Yet, optical modulators using waveguides in bulk LT have not been as widely adopted as those in LN , whereas LT and TFLT have had extensive use in acoustic filters . This is partially due to the low Curie temperature of LT, which restricts the creation of low-loss optical waveguides in LT via doping or ion exchange, in combination with instability issues . Recently, the first optical devices on TFLT have appeared: microdisks , strip-loaded waveguides , as well as dry-etched microrings , and MZMs . Nevertheless, it is still unclear as to what extent the desirable properties of bulk LT map to thin-film LT electro-optic modulators, e.g. weak EO relaxation, without sacrificing other metrics such as drive voltage, optical loss, and so on.

[0018] TFLT EO MZMs operating at 1550 nm with superior DC stability, in both amplitude and timescale, compared to equivalent TFLN MZMs are designed, fabricated, and demonstrated. Specifically, less than 1 dB output power fluctuation for quadrature-biased TFLT compared to 5 dB with TFLN over 46 hours with 12.1 dBm input power was measured. Importantly, TFLT MZMs as described herein do not sacrifice important deviceHCU-08225 (HU 10197)figures-of-merit including optical loss (0.35 dB), RF bandwidth (flat from 3-50 GHz), extinction ratio (39 dB), and drive voltage (3.4 Vcm half-wave voltage), compared to TFLT MZMs. Benefiting from the DC stability, a path-length balanced modulator was designed, which is insensitive to temperature fluctuations. This is demonstrated by measured bit error rates below soft-division forward error correction threshold over a temperature range from 0°C to 70°C. Open eye diagrams for 30 GBaud non-return-to-zero pseudorandom bit sequence modulation using high 28 dBm optical power were measured. Furthermore, to validate the quality of one or more etch processes described herein, TFLT racetrack resonators are fabricated, low single-mode optical loss of 9 dB / m was measured, and a thermo-optic coefficient of TFLT (dn / dT=3*10A(-6) KA(-1)) was measured.

[0019] Figs. 1A-1E depict integrated thin-film lithium tantalate-on-insulator electro-optics.Fig. 1A is a micrograph of a balanced Mach-Zehnder modulator 100 with an independent DC electrode section 102 and an RF electrode section 104 (e.g., 50 Ohm-terminated RF electrode section). An optical microscope image of a fabricated TFLT MZM 100 is shown in Fig. 1A.The device 100 can be fabricated on a 500 nm-thick x-cut TFLT-on-SiO_2 wafer from NanoLN.

[0020] Fabrication

[0021] Fig. IB depicts a device fabrication process with multiple steps (i) through (vii). Waveguides can be patterned using ma-N 2405 resist and 150 keV electron-beam lithography, then etched by 300 nm using ArA+ inductively coupled plasma dry etching to define ridge waveguides 112 extending from a slab 114. At step (i), a layer of electrooptical material 106 is disposed on a first side of a monolithic substrate 108, which may be further supported by a support 110 disposed on the second side of the monolithic substrate 108. For example, an x-cut thin-film lithium tantalate layer disposed on the monolithic substrate 108 can be coated with ma-N 2405 resist and exposed using 150 kV electron-beam lithography (EBL). The monolithic substrate 108 can include a SiO_2 layer that is 2 pm-thick and is thermally grown on a Si support. At step (ii), the layer of electrooptical material 106 can be etched to define a pair of ridge waveguides 112 and a slab 114, the ridge waveguides extending from the slab. For example, ArA+ etching can be used to define a pair of ridge waveguides 112.

[0022] Re-deposition from the etch and removal of the remaining ma-N 2405 is achieved using KOH and SC-1 solutions each heated to 65 °C. The devices are annealed in an 0 2 atmosphere at 520°C for 2 h to restore damage in the crystal, thus reducing optical loss and photo-refractive effects. The MZMs are left uncladded to measure the DC electro-optic driftHCU-08225 (HU 10197)without effects of oxide impurities, so as to fairly compare TFLT crystal properties to TFLN. For high frequency electro-optic measurements and optical resonator measurements, an 800 nm-thick SiO_2 cladding layer can subsequently be deposited by plasma-enhanced chemical vapor deposition. In various aspects, this can reduce the effects of sidewall scattering due to high index contrast between TFLT and air for loss characterization and achieves optimal RF phase and optical group velocity matching. At step (iii), a cladding layer 116 (e.g., an SiO_2 cladding layer) may be disposed over the ridge waveguides 112. For example, plasma-enhanced chemical vapor deposition (PECVD) of the cladding layer 116 can be performed.

[0023] A first electrode section and second electrode section can be formed on the etched layer of electrooptical material. The electrode sections can each have a plurality of electrodes and can be positioned with respect to the pair of ridge waveguides such that the first electrode section is spaced apart from the second electrode section. At step (iv), an electrode mask can be defined using 375 nm-photolithography and SPR700-1.0 resist. Electrodes can be patterned by photolithography at 375 nm with SPR700-1.0 resist.

[0024] For cladded devices, trenches can be dry etched using C_3F_8 and ArA+ gases. At step (v), the cladding 116 can be selectively removed using inductively coupled plasma etching. At step (vi), metal deposition of electrodes (e.g., Ti / Au electrodes) can be performed by electron-beam evaporation. At step (vii), lift-off can be used to define a plurality of electrodes 118a, 118b. Each of the electrodes can consist of a 15 nm-thick Ti adhesion layer and 800 nm-thick Au.

[0025] A termination resistor (20 nm-thick Ti, 5 nm-thick Pt) for the MZM can be defined by another round of photolithography, etching, electron-beam deposition, and liftoff. Electrodes for uncladded MZMs can also be similarly defined by photolithography, electron-beam deposition, and liftoff. As a final step, all devices can be hotplate-heated at 300°C for 5 h to remove trapped charges induced by the electron-beam metal deposition which can negatively impact DC drift effects. To unambiguously compare the DC drift of the TFLT MZM with a TFLN MZM, a TFLN MZM was fabricated using the same process, and with the same waveguide and electrode geometries.

[0026] Fig. 1C is a cross-sectional schematic of a Mach-Zehnder modulator showing a monolithic substrate 122 disposed on a support 124, an etched layer of electrooptical material 126 disposed on the monolithic substrate 122, a pair of ridge waveguides 128a, 128b extending from a slab 132, an electrode section having a plurality of electrodes 134a, 134b, 134c and a layer of cladding 140, with crystal axes, relevant dimensions, and materials noted.HCU-08225 (HU 10197)

[0027] Fig. ID is a scanning electron-micrograph (SEM) of a cross section of an etched lithium tantalate ridge waveguide, wherein a sidewall angle of 61° is observed. Fig. IE depicts SEMs of fabricated grating couplers and waveguides showing smooth sidewalls.

[0028] Modulator Simulations

[0029] The optical mode supported by a ridge waveguide fabricated in the 500 nm TFLT-on-2 pm oxide stack is shown in Fig. 2A, and featured an effective index of 1.9 and group index of 2.25. Next, a microwave simulation was performed with electrodes to check the overlap between optical and microwave electric fields for the 300 nm etch depth used. As shown in Fig. 2B, most of the microwave field is in the surrounding oxide and slab due to the high permittivity contrast between lithium tantalate (~43) and SiO_2 (~4) at these frequencies. By using the same mesh in the waveguide region for both optical and RF simulations, an accurate field overlap over an entire cross-section and an estimate of the DC V_7tL may be obtained by calculating the RF-induced index change of optical mode. With this process, along with considerations for metal-induced optical loss and fabrication alignment accuracy, the gap between electrodes was chosen to be 5 pm, giving a simulated DC V_7tL of 3.1 Vcm.

[0030] To achieve high-bandwidth performance of the modulator, the required matching of optical group velocity to microwave phase velocity at high frequencies may be addressed. Given a stack as described herein, matching can be achieved by choosing the correct width for the signal electrode (Fig. 2C), which is 50 pm. Matching the impedance of the modulator, which is essentially a co-planar transmission line in ground-signal-ground configuration, to the 50Q RF loading port may be addressed. It was found that for a given stack and limiting tuning parameters, the best impedance achieved while maintaining velocity matching is 39Q (Fig. 2D). This was inferred from measurements of the electro-optic response of the modulator. It is expected that this will lead to a sharp roll-off at frequencies from hundreds of megahertz to a few gigahertz where the electrical modulation speed enters RF regime and reflections begin to happen. This problem can be alleviated by increasing the thickness of the bottom oxide from the current 2 pm to at least 4.7 pm. It is also worth noting that a segmented electrode design can help increase the impedance, but may strongly raise the RF index (to above 3 with one or more stacks described herein). Combining the segmented design with thicker bottom oxide may overcome this problem and further improve the bandwidth. Note that independent ellipsometry measurements were used to determine the refractive indices of TFLT, n_e~n_o~2.12 at 1550 nm, for simulations and calculations.

[0031] Figs. 2A-2D depict simulations for TFLT modulators. Fig. 2A depicts a simulated optical electric field profile (Comsol). The group velocity of the fundamental TE modeHCU-08225 (HU 10197)(shown) is 2.25. Fig. 2B depicts a simulated RF electric field profile (Comsol). The field overlap is calculated and V_7tL at DC is estimated to be 3.1 Vcm. Lines are used to define material boundaries and to guide the eye. Fig. 2C depicts the simulated RF effective index "neff (Lumerical HFSS). By design it matches the group index of light "optical ng" at high frequency. Fig. 2D depicts the simulated (Lumerical HFSS), ideal (50 Q), and measured (inferred from electro-optic measurements, 39 Q) RF impedance.

[0032] Modulator Chip Details

[0033] A path length-balanced MZM may be used to mitigate temperature and laser wavelength fluctuations. One or more designs described herein are based on directional couplers instead of Y-splitters and hence have two input and two output ports. Separate 7.5 mm-long ground-signal-ground DC and 50 Q-terminated RF electrodes avoids an external bias-tee, thereby providing excellent isolation between DC and RF signals while enabling low RF insertion loss, flat RF response, and avoids terminator damage under high DC bias. The MZM cross-section (Fig. 1C schematic) can be optimized for low optical loss with strong optical and RF field overlap. A scanning-electron microscope cross-section of the etched waveguide (Fig. ID) is used to determine the etched sidewall angle of 61° which is limited by the etch bias power and rate of re-deposition. The sidewall angle is used to design and simulate grating couplers. A loss of 7.9 dB per grating coupler for coupling light between optical fibers and the chips was measured. This differs from the simulated efficiency of ~3 dB due to fabrication imperfections. Fig. IE shows a scanning-electron microscope image of the etched grating couplers and waveguides, indicating successful removal of re-deposition and low sidewall roughness.

[0034] DC Electro-Optic Measurements

[0035] Low V_7tL of 3.4 Vcm at near-DC (Fig. 3A) was measured, which is close to that predicted by simulation. The V_7tL was measured by monitoring the output power of each MZM port and slowly varying the input voltage, which matches simulations described herein and is limited mainly by device geometry in various embodiments described herein, including gap width, etch depth, etc. Optimized stack and design may achieve a lower V_7tL. Notably, an exceptionally high extinction ratio of approximately 39 dB was measured at one of the ports. The second port had a lower extinction ratio of 16 dB due to asymmetric directional couplers (53:47 ratio) as well as etch-induced error and, as observed using a microscope, loss difference between the two arms induced by misalignment of the electrode (0.7 dB). The above effects of the directional coupler ratio and electrode-induced loss were estimated using simulation. Scattering in the MZM waveguides accounted for 0.13 dB loss, with the metalHCU-08225 (HU 10197)loss together leading to a total on-chip loss of 0.35 dB. Next, the TFLT MZM was biased at quadrature and EO relaxation was measured over 46 hours using 20 dBm off- (12.1 dBm on-) chip input optical power (Fig. 3B). Less than 1 dB of laser intensity variation was found in the first two hours, likely due to charge migration at the electrical contact, settling to 0.2 dB drift over the final 44 hours. On the other hand, the TFLN MZM exhibited 5 dB laser intensity variation when measured under the same conditions, that is, input power and measurement duration. Furthermore, EO relaxation of TFLN reported in literature varies from 3 dB in ~15 minutes to 8 dB over ~30 mins . Also note that optical powers unstated in both works. Note that temperature fluctuations of the room (less than 2°C) and mechanical disturbances, including fiber-to-chip coupling drift, were carefully monitored to ensure they do not play a role in DC drift measurements.

[0036] Figs. 3A-3B depict DC electro-optic characterization measurements. Fig. 3A depicts the measured transfer function at each output port of a modulator as a function of slowly varied bias voltage. A high extinction ratio of 38.8 dB was measured at output port OUT. A lower extinction ratio of 15.9 dB was measured at the complement port ("OUT" ) due to fabrication imperfections. Fig. 3B depicts the dynamics of optical output intensity relative to quadrature when bias is initially set to quadrature. The TFLT (TFLN) MZM exhibited less than 1 dB (5 dB) power drift over 46 hours. The first 30 minutes are shown in the left plot of Fig. 3B For reference, a curve (annotated “LiNbO_3 *” in the figure) is included showing the drift of a TFLN MZM from literature .

[0037] RF Electro-Optic Measurements

[0038] Figs. 4A-4B depict RF electro-optic characterization measurements. Fig. 4A depicts the normalized electro-optic conversion efficiency EO S_21, measured (simulated) shown using a solid (dashed) line, with the RF S_11 spectra shown below. The roll-off before 3 GHz is due to the low characteristic impedance of the transmission line electrode (39 Q), and can be mitigated with thicker underlying oxide and re-optimization of the modulator design. Insets depict an eye diagram for 30 GBaud non-return-to-zero pseudorandom bit sequence modulation using high 28 dBm optical power (left) and the associated setup (right), wherein EDFA denotes an erbium-doped fiber amplifier, BPF denotes a bandpass filter, AWG denotes an arbitrary waveform generator, PD denotes a photodetector, and OSC denotes an oscilloscope. Fig. 4B, top, depicts the measured bit error rate with 5.1 dBm power below soft-division forward error correction threshold under varied temperature. Fig. 4B, bottom, depicts eye diagrams at the measured temperatures.HCU-08225 (HU 10197)

[0039] The RF electro-optic response of an MZM described herein was measured by driving the modulator with a vector network analyzer at quadrature and measuring the variation in output optical power using a high-bandwidth photodiode which is plugged into the second port of the network analyzer. Matching the optical group and RF phase velocities in the modulator design described herein (Fig. 2C) produces a normalized electro-optic conversion efficiency (EO S_21, Fig. 4A) with a flat roll-off to 50 GHz after 3 GHz. A spectrum analyzer used was limited to a 50 GHz bandwidth. The roll-off before 3 GHz is due to the low characteristic impedance of the transmission line electrode (39 Q). This can straightforwardly be overcome using an optimized device geometry with a thicker bottom oxide. The RF EO response may be extrapolated with parameters obtained from simulations (optical and RF indices) and electrical measurements (RF loss and impedance). The result is shown in Fig. 4A with a dashed line, matching well with experiment. The electrode back-reflection is also monitored with the network analyzer (RF S_11, Fig. 4A). The RF back-reflection is primarily due to the aforementioned RF impedance mismatch, in addition to parasitic resonances.

[0040] To show the benefit of stable DC bias in conjunction with path length-balanced design for data modulation, the MZM may be biased at quadrature and driven using a non-return-to-zero (NRZ) pseudorandom binary sequence (PRBS) at 5 GBaud, over a 70°C temperature range. The temperature is controlled by mounting the chip onto a thermally controlled and monitored copper stage using clips. Eye diagrams are compiled from 20,000 shots and measured with 5.1 dBm on-chip input optical power (Fig. 4B, bottom). All measurements yield bit error rates (BERs) less than that required for soft-division forward error correction (SD-FEC), corresponding to signal-to-noise ratios of ~3 (Fig. 4B, top).Above 10°C a reduced error rate with increased temperature may be measured. This is due to thermal expansion-induced alignment improvement of the optical fiber with the grating couplers. Increased error is observed at 0°C, owing to misalignment induced by condensation. Proper packaging may be expected to reduce the temperature-induced misalignment of the gratings with the fibers.

[0041] Finally, at room temperature the on-chip optical power may be increased to 28 dBm and demonstrate data modulation (Fig. 4A, inset). The setup used to perform the measurement is also shown in the inset of Fig. 4A. Open eyes may be retained at up to 30 GBaud modulation rates and a signal-to-noise ratio of 3.3, limited by oscilloscope bandwidth. Instabilities of the optical amplifier prevented accurately testing the long-term DC stability at this power.HCU-08225 (HU 10197)

[0042] Optical Resonator Measurements

[0043] Figs. 5A-5C depict optical resonator measurements. Fig. 5A depicts the measured optical spectrum of a single-mode TFLT racetrack resonator. The resonance shown in Fig. 5B is indicated by the blue shaded area. Fig. 5B depicts a measured (x) and fit (red line) Lorentzian-shaped resonance used to determine linewidth, intrinsic quality factor, and loss coefficient indicated. The inset shows an optical micrograph of the corresponding fabricated racetrack resonator. Fig. 5C depicts measured and fitted temperature-dependent response extracted from the resonance shift of the racetrack resonator as a function of temperature.

[0044] For scalability of TFLT, it is pertinent to determine the optical loss induced by one or more etching processes described herein. To estimate this, an uncladded racetrack resonator of ~200 pm width and ~850 pm in the narrowest and widest parts, respectively, may be fabricated. The waveguide was etched by 300 nm, has a 1 pm top width in the coupler section, which corresponds to single mode behavior, and tapers to a maximum 4 pm top width. A bus waveguide has a 1 pm width, which ensures that only the fundamental mode is coupled in and out of the racetrack resonator. The gap width between the racetrack resonator and the bus waveguide is 1.4 pm, corresponding to undercoupled conditions. By varying the wavelength of the laser around 1530 nm, a single-mode spectrum with a free spectral range of 185 pm may be measured (Fig. 5A). By slowly varying the wavelength of the laser light through resonance at low optical power, a Lorentzian profile was measured and fit to extract a FWHM linewidth of 55.1 MHz. This corresponds to a loaded quality factor of Q_L=3.55 million (Fig. 5B). From this, and the transmission of the resonance T, an intrinsic quality factor of Q_i=2Q_L / (l+ T)=4.04 million may be calculated. This corresponds to a propagation loss of 9 dB / m, which includes bending loss from the racetrack design. Note that low-loss resonators may be created using a single-step ma-N-based lithography process, thereby avoiding an additional dry etching step and complexity associated with a hard-mask transfer.

[0045] The temperature dependence of the TFLT refractive index may be measured. This is performed by temperature tuning the chip similar to that for the eye diagram measurements, and monitoring the detuning of the resonance. The detuning is linear with temperature (Fig.5C). A fit suggests a thermo-optic coefficient of dn / dT=3xlOA(-6) KA(-1), including effects of resonator geometry and thermal expansion of LT only. This differs from 12><10A(-6) KA(-1) estimated from bulk LT due to the presence of the material stack, piezoelectricity, film properties, e.g. free charges or crystal structure differences due to etching or wafer cutting and bonding, or a combination of these effects.HCU-08225 (HU 10197)

[0046] Electro-Optic Modulator Topology

[0047] Fig. 6 depicts a topology of an electro-optic modulator 600 with separate DC bias and RF electrodes. The electro-optic modulator 600 includes optical waveguides 602a, 602b defined in thin-film lithium tantalate on an insulating substrate. The substrate has a lower refractive index than the lithium tantalate material such that an optical mode can be confined within the optical waveguides 602a, 602b. The electro-optic modulator 600 comprises an optical splitter 604 and an optical combiner 606, each of which may be formed using a directional coupler, a y-splitter, a multi-mode interference coupler, or other suitable coupler type that allows for the splitting of light into two substantially equal paths. The optical splitter 604 and the optical combiner 606 are joined by the optical waveguides 602a, 602b to create a Mach-Zehnder interferometer structure. The electro-optic modulator 600 further includes two distinct electrode sections: a first electrode section 608 (a DC bias electrode section) and a second electrode section 610 (an RF signal electrode section), each comprising at least three electrodes in a ground-signal-ground configuration. The first electrode section 608 and the second electrode section 610 are located between the optical splitter 604 and the optical combiner 606.

[0048] The phase of light is controlled in each waveguide path by the application of an external electric field. The electric field is induced across the optical waveguides 602a, 602b via a first plurality of metal electrodes 612a, 612b, 612c of the first electrode section 608 and a second plurality of metal electrodes 614a, 614b, 614c of the second electrode section 610.The electrodes can be located adjacent to the waveguides (e.g., for x-cut lithium tantalate) such that each of the ridge waveguides is disposed between a first pair of adjacent electrodes and a second pair of adjacent electrodes of each of the first plurality of electrodes and the second plurality of electrodes (e.g., as shown in Fig. 6). For z-cut lithium tantalate, the electrodes can be positioned on the top and bottom of the waveguides.

[0049] Application of voltage on the DC bias electrode section 608 allows for independent control of the optical phase, in addition to the time-varying phase induced by the RF signal electrode section 610. This configuration allows for control of the electro-optic modulator bias set point independently of the state of the RF signal, such that an RF bias tee is not required. This overcomes the bandwidth limitations of a bias tee while reducing the device footprint and improving efficiency by eliminating added loss from the bias tee. In addition to using separate DC bias and RF signal electrode sections, the design can be generalized for adding two signals together, either RF or DC, such that the device can perform a mathematical operation of addition.HCU-08225 (HU 10197)

[0050] The electro-optic modulator 600 may have a balanced path length configuration in which the path length difference between the two arms of the Mach-Zehnder interferometer is effectively zero. The electrode design described herein may be used with either balanced or unbalanced interferometer configurations. In various aspects, lithium tantalate enables the use of a balanced design, as compared to lithium niobate, owing to the superior stability of lithium tantalate when a DC voltage is applied.

[0051] Fig. 7 depicts a topology of an IQ modulator 700 with separate DC bias and RF electrodes. The IQ modulator 700 includes an input optical splitter 702 that divides optical power equally between a first electro-optic modulator 704 and a second electro-optic modulator 706. Each of the first electro-optic modulator 704 and the second electro-optic modulator 706 includes a respective pair of optical splitters forming a Mach-Zehnder interferometer structure as described with reference to Fig. 6. The first electro-optic modulator 704 includes in-phase RF electrodes 708a, 708b and in-phase DC electrodes 710a, 710b, which are separated as described above. The second electro-optic modulator 706 includes quadrature RF electrodes 712a, 712b and quadrature DC electrodes 714a, 714b. The in-phase DC electrodes 710a, 710b and the quadrature DC electrodes 714a, 714b may share a common ground electrode 716. The outputs from the first electro-optic modulator 704 and the second electro-optic modulator 706 feed a DC phase control section 718, which then enters an output optical combiner 720. The IQ modulator 700 configuration may be used for coherent communications, control of RF sideband amplitude ratio, and as an optical frequency shifter. The balanced path length design, as described with reference to Fig. 6, may be applied to all interferometers within the IQ modulator 700.

[0052] Thin-film lithium tantalate Mach-Zehnder modulators that have improved DC stability are demonstrated, both in timescale and magnitude, over equivalent Mach-Zehnder modulators in thin-film lithium niobate. Importantly, various embodiments do not sacrifice key figures-of-merit including RF bandwidth, drive voltage and optical loss, and fabricate the modulators with a scalable process using ma-N resist. One or more path-length balanced modulators as described herein mitigate against temperature and laser wavelength fluctuations, which has practical benefits in deployment. Furthermore, low-error data modulation at varied temperature and optical powers is also shown. Fabrication processes described herein yield low single-mode loss of 9 dB / m. Optimization of charge dynamics near surfaces, either by etching or metallization studies, may further improve the performance of thin-film lithium niobate electro-optics.HCU-08225 (HU 10197)

[0053] Referring to Figs. 8A-8B, a cross-sectional view and a top view, respectively, of a device 800 that can be used to practice the present invention is shown. As shown in Fig. 8A, the device 800 comprises a monolithic substrate 802 having a first side 804a and a second side 804b; and an etched layer 806 of electrooptical material disposed on the first side 804a of the monolithic substrate 802, said etched layer 806 comprising a pair of ridge waveguides 808a, 808b and a slab 810, the pair of ridge waveguides 808a, 808b extending from the slab 810. The device 800 further comprises a first electrode section disposed on the slab 810 of the etched layer 806 of electrooptical material at a first position with respect to the pair of ridge waveguides 808a, 808b, the first electrode section comprising a first plurality of electrodes 812a, 812b, 812c, the first plurality of electrodes configured to apply a DC bias to a first portion of each of the ridge waveguides. A support 814 may be disposed on the second side 804b of the monolithic substrate 802. A cladding 816 may be disposed over the pair of ridge waveguides 808a, 808b.

[0054] The device further comprises a second electrode section 818 (shown in Fig. 8B) disposed on the slab 810 of the etched layer 806 of electrooptical material at a second position 824 with respect to the pair of ridge waveguides. Fig. 8B shows the first electrode section 820 and the second electrode section 818. The second position 824 is spaced apart from the first position 826. The second electrode section 818 comprises a second plurality of electrodes 828a, 828b, 828c, the second plurality of electrodes configured to apply an RF signal to a second portion of each of the ridge waveguides. The first and the second pluralities of electrodes can each comprise at least three electrodes disposed adjacent to one another on the etched layer of electrooptical material. Each of the ridge waveguides 808a, 808b can be disposed between a first pair of adjacent electrodes and a second pair of adjacent electrodes of each of the first plurality of electrodes and the second plurality of electrodes. For example, the first ridge waveguide 808a can be disposed between a first pair of adjacent electrodes (e.g., electrodes 812a, 812b) of the first plurality of electrodes and a first pair of adjacent electrodes (e.g., electrodes 828a, 828b) of the second plurality of electrodes. The second ridge waveguide 808b can be disposed between a first pair of adjacent electrodes (e.g., electrodes 812b, 812c) of the first plurality of electrodes and a first pair of adjacent electrodes (e.g., electrodes 828b, 828c) of the second plurality of electrodes.

[0055] In some embodiments, the device further comprises an optical splitter 830 and an optical combiner 832, each disposed on the first side of the monolithic substrate 802, the optical splitter 830 and the optical combiner 832 each being in optical communication with each of the pair of ridge waveguides 808a, 808b, wherein the ridge waveguides form arms ofHCU-08225 (HU 10197)a Mach-Zehnder interferometer, and wherein the first electrode section 820 and the second electrode section 818 are disposed between the optical splitter 830 and the optical combiner 832. The first ridge waveguide 808a of the pair of ridge waveguides 808a, 808b can form a first arm of the Mach-Zehnder interferometer, and the second ridge waveguide 808b of the pair of ridge waveguides 808a, 808b forms a second arm of the Mach-Zehnder interferometer, and for each of the first plurality of electrodes 812a, 812b, 812c and the second plurality of electrodes 828a, 828b, 828c, the first arm is disposed between a first pair of adjacent electrodes and the second arm is disposed between a second pair of adjacent electrodes.

[0056] Materials

[0057] The electrooptical material used in the etched layer may comprise a material selected from LiTaCh, LiNbCh, SiC, GaAs, KNbCh, or KH2PO4. In some embodiments, the electrooptical material comprises LiTaCh, and each of the ridge waveguides is elongated in a direction perpendicular to a z-axis of the LiTaCh (Z-cut orientation). In other embodiments, the electrooptical material comprises LiTaCh, and each of the ridge waveguides is elongated in a direction perpendicular to an x-axis of the LiTaCh (X-cut orientation).

[0058] The monolithic substrate may be an insulator comprising a material selected from SiO?, AI2O3, TiCh, HfCh, ZnO, ITO, or CaF2, or another suitable electrical insulator having a lower refractive index than the electro-optic layer. The insulator has a refractive index less than that of the ridge waveguides so as to confine the optical mode. A support may be disposed on the second side of the monolithic substrate. The support may comprise a material selected from Si, AI2O3, or SiO2. The support may comprise an insulating bulk substrate or a non-insulating bulk substrate. The use of an insulating bulk substrate may serve to reduce RF propagation loss on the electrodes.

[0059] The first plurality of electrodes and the second plurality of electrodes each independently comprises a material selected from Au, Al, Ag, Cu, or other suitable electrically conductive material.

[0060] In some embodiments, the cladding disposed over the pair of ridge waveguides comprises an oxide material, such as a material selected from SiCh, AI2O3, TiCh, HfCh, ZnO, ITO, or CaF2. The cladding comprises a material having a refractive index lower than that of the ridge waveguides.

[0061] Electrode Configurations

[0062] Referring to Fig. 9, cross-sectional electrode configurations for Z-cut LiTaOs ridge waveguide modulators are shown. In a Z-cut orientation, the z-axis is oriented perpendicularHCU-08225 (HU 10197)to the substrate plane (vertical), and the dominant electro-optic coefficient is r_33. The electric field must be applied along the z-axis (vertically through the ridge waveguide). Three configurations are depicted. The figure depicts a monolithic substrate 902, a slab 904 of an etched layer of electrooptical material, a ridge waveguide 906 extending from the slab. As used herein, an electrode that is “transversely disposed” with respect to a ridge waveguide is disposed in a direction transverse to a longitudinal axis of the ridge waveguide.

[0063] In a first configuration (Z-Cut A), a signal electrode 908a is disposed on a top surface of the ridge waveguide, and ground electrodes 910a, 910b are disposed on the slab 904 such that the electric field is applied along the z-axis of the electrooptical material through the ridge waveguide. The ground electrodes 910a, 910b can be transversely disposed on the slab 904 on opposing lateral sides of the ridge waveguide 906 (e.g., being laterally spaced from the ridge waveguide 906), such that the ridge waveguide 906 is disposed between the ground electrodes 910a, 910b.

[0064] In a second configuration (Z-Cut B), a signal electrode 908b and a ground electrode 910c are disposed on the slab 904, such that a fringing electric field is applied along the z-axis through a lower portion of the ridge waveguide. The electrodes 908b, 910c can be transversely disposed on the slab 904 on opposing lateral sides of the ridge waveguide 906 (e.g., being laterally spaced from the ridge waveguide 906), such that the ridge waveguide 906 is disposed between the electrodes 908b, 910c.

[0065] In a third configuration (Z-Cut C), a signal electrode 908c is disposed on a top surface of the ridge waveguide 906, and a ground electrode 910d is embedded at or near the interface between the slab and the substrate beneath the ridge waveguide 906, such that the electric field is applied along the z-axis through the full thickness of the ridge waveguide.

[0066] Referring to Fig. 10, cross-sectional electrode configurations for X-cut LiTaCh ridge waveguide modulators are shown. In an X-cut orientation, the z-axis is oriented parallel to the substrate plane and perpendicular to the waveguide propagation direction (horizontal, inplane), and the dominant electro-optic coefficient is r_33. The electric field must be applied horizontally along the z-axis through the ridge waveguide. Three configurations are depicted. The figure depicts a monolithic substrate 1002, a slab 1004 of an etched layer of electrooptical material, and one or two ridge waveguides extending from the slab.

[0067] In a first configuration (X-Cut A), a signal electrode 1008a is transversely disposed on the slab 1004 on a first lateral side of the ridge waveguide 1006 (e.g., being laterally spaced from the ridge waveguide 1006), and a ground electrode 1010a is transversely disposed on the slab 1004 on an opposing second lateral side of the ridge waveguide 1006HCU-08225 (HU 10197)(e.g., being laterally spaced from the ridge waveguide 1006). In this way, the electric field is applied along the z-axis of the electrooptical material through the ridge waveguide.

[0068] In a second configuration (X-Cut B), for a pair of ridge waveguides 1006a, 1006b forming the arms of a Mach-Zehnder interferometer, a first ground electrode 1010b is transversely disposed on the slab 1004 on a lateral side of the first ridge waveguide 1006a (e.g., being in contact with the ridge waveguide 1006a), a signal electrode 1008b is disposed on the slab 1004 between the first and second ridge waveguides 1006a, 1006b, and a second ground electrode 1010c is transversely disposed on the slab 1004 on a lateral side of the second ridge waveguide 1006b (e.g., being in contact with the ridge waveguide 1006b). In this way, the opposing electric fields are applied along the z-axis through each of the ridge waveguides simultaneously (push-pull operation).

[0069] In a third configuration (X-Cut C), a signal electrode 1008c is disposed on a top surface of the ridge waveguide 1006, and a ground electrode lOlOd is transversely disposed on the slab 1004 on one lateral side of the ridge waveguide 1006 (e.g., being spaced apart from the ridge waveguide 1006), such that the electric field is applied along a direction having a component along the z-axis of the electrooptical material through the ridge waveguide.

[0070] The foregoing electrode configurations may be generalized for other electro-optic materials where the dominant electro-optic coefficient requires the electric field to be applied along a specific crystallographic axis. Applicable materials include, but are not limited to, LiNbCh, SiC, GaAs, KNbCh, and KH2PO4. In some embodiments, the electrodes may be laterally spaced from the ridge waveguides so as to reduce or substantially avoid metal-induced optical loss in the optical mode. It is contemplated, however, that in certain implementations, contact between the electrodes and the waveguide may be employed to exploit metal-optical interactions. In some embodiments, the electrodes may be disposed on or above a cladding layer, such as an SiCh cladding layer, overlying the etched layer of electrooptical material. Improved electro-optic modulation efficiency may be achieved when a mismatch in electric permittivity between the electrode material and the underlying electrooptical material is reduced. For electrooptical materials having a relatively high electric permittivity, such as LiTaCh or LiNbCh, it may be desirable to dispose at least a portion of one or more electrodes in contact with a remaining slab portion of the etched layer of electrooptical material, rather than on the sidewalls of the ridge waveguides, so as to enhance the electric field overlap with the optical mode while maintaining acceptable optical loss.HCU-08225 (HU 10197)

[0071] In a general lateral electrode pair configuration, at least one signal electrode and at least one ground electrode are disposed on the slab on opposing lateral sides of the ridge waveguide, such that the electric field is applied along a selected crystallographic axis of the electrooptical material through the ridge waveguide.

[0072] In a general vertical electrode pair configuration, at least one signal electrode is disposed above the ridge waveguide and at least one ground electrode is disposed on the slab or below the electrooptical layer, such that the electric field is applied perpendicular to the plane of the slab along a selected crystallographic axis of the electrooptical material through the ridge waveguide.

[0073] In a general ground-signal-ground dual waveguide push-pull configuration, a ground electrode is disposed on the slab laterally outboard of a first ridge waveguide, a signal electrode is disposed on the slab between the first and second ridge waveguides, and a ground electrode is disposed on the slab laterally outboard of the second ridge waveguide, such that opposing electric fields are applied along a selected crystallographic axis of the electrooptical material through each of the ridge waveguides.

[0074] In a general mixed or diagonal field configuration, at least one signal electrode and at least one ground electrode are positioned relative to the ridge waveguide such that the applied electric field has a component along a selected crystallographic axis of the electrooptical material that produces a desired change in refractive index through the electro-optic effect.

[0075] All electrode configurations described herein are described with reference to the cross-section of the waveguide perpendicular to the propagation direction. For Z-cut orientations, the z-axis is vertical (out-of-plane with respect to the substrate). For X-cut orientations, the z-axis is horizontal (in-plane, transverse to propagation). The X-Cut B ground-signal-ground push-pull configuration may map directly to the Mach-Zehnder interferometer structures described herein. The formulations encompass materials where the optimal axis may correspond to r_13 rather than r_33 (e.g., certain cuts of KNbCh or GaAs orientations). Electrode materials for all configurations may include Au, Al, Ag, Cu, or any suitable electrically conductive material.

[0001] In accordance with a 1stexample embodiment, the present invention is a device. In a 1staspect of the 1stexample embodiment, the device comprises a monolithic substrate having a first side and a second side; an etched layer of electrooptical material disposed on the first side of the monolithic substrate, the etched layer comprising a pair of ridge waveguides and a slab, the pair of ridge waveguides extending from the slab; a first electrode section disposed on the slab of the etched layer of electrooptical material at a first position with respect to theHCU-08225 (HU 10197)pair of ridge waveguides, the first electrode section comprising a first plurality of electrodes, the first plurality of electrodes configured to apply a DC bias to a first portion of each of the ridge waveguides; and a second electrode section disposed on the slab of the etched layer of electrooptical material at a second position with respect to the pair of ridge waveguides, the second position being spaced apart from the first position, the second electrode section comprising a second plurality of electrodes, the second plurality of electrodes configured to apply an RF signal to a second portion of each of the ridge waveguides.

[0076] As used herein, the term “monolithic” refers to a substrate formed as or from a single continuous piece of material, as distinguished from a substrate assembled from separate discrete pieces that are coupled to each other.

[0002] In a 2ndaspect of the 1stexample embodiment, the monolithic substrate is an insulator.

[0003] In a 3rdaspect of the 1stexample embodiment, the insulator comprises a material selected from SiCh or other suitable insulating material. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0004] In a 4thaspect of the 1stexample embodiment, the insulator has a refractive index less than that of the ridge waveguides. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0005] In a 5thaspect of the 1stexample embodiment, the device further comprises a support, the support disposed on the second side of the monolithic substrate. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0006] In a 6thaspect of the 1stexample embodiment, the support comprises a material selected from Si or other suitable support material. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0007] In a 7thaspect of the 1stexample embodiment, the electrooptical material comprises a material selected from LiTaCh, LiNbCh, SiC, GaAs, SiCh, KNbCh, or KH2PO4. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0008] In an 8thaspect of the 1stexample embodiment, the electrooptical material comprises LiTaCh, and each of the ridge waveguides is elongated in a direction perpendicular to a z-axis of the LiTaCh. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0009] In a 9thaspect of the 1stexample embodiment, the electrooptical material comprises LiTaCh, and each of the ridge waveguides is elongated in a direction perpendicular to an x-HCU-08225 (HU 10197)axis of the LiTaCh. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0010] In a 10thaspect of the 1stexample embodiment, the first plurality of electrodes and the second plurality of electrodes each comprises at least three electrodes disposed adjacent to one another on the electrooptical material. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0011] In an 11thaspect of the 1stexample embodiment, each of the ridge waveguides is disposed between a first pair of adjacent electrodes and a second pair of adjacent electrodes of each of the first plurality of electrodes and the second plurality of electrodes. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0012] In a 12thaspect of the 1stexample embodiment, the first plurality of electrodes and the second plurality of electrodes each independently comprises a material selected from Au or other suitable conductive material. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0013] In a 13thaspect of the 1stexample embodiment, the device further comprises a cladding disposed over the pair of ridge waveguides. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0014] In a 14thaspect of the 1stexample embodiment, the cladding comprises an oxide material. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0015] In a 15thaspect of the 1stexample embodiment, the cladding comprises a material selected from SiCh, AI2O3, TiCh, HfCh, ZnO, ITO, or CaF?. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0016] In a 16thaspect of the 1stexample embodiment, the cladding comprises a material having a refractive index lower than that of the ridge waveguides. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0017] In a 17thaspect of the 1stexample embodiment, a ratio of a thickness of each of the ridge waveguides to a thickness of the monolithic substrate is from 1 :20 to 1 :4. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0018] In an 18thaspect of the 1stexample embodiment, the device further comprises an optical splitter and an optical combiner, each disposed on the first side of the monolithic substrate, the optical splitter and the optical combiner each being in optical communicationHCU-08225 (HU 10197)with each of the pair of ridge waveguides, wherein the ridge waveguides form arms of a Mach-Zehnder interferometer, and wherein the first electrode section and the second electrode section are disposed between the optical splitter and the optical combiner. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0019] In a 19thaspect of the 1stexample embodiment, the first and the second pluralities of electrodes each comprises at least three electrodes disposed adjacent to one another on the electrooptical material; a first ridge waveguide of the pair of ridge waveguides forms a first arm of the Mach-Zehnder interferometer, and a second ridge waveguide of the pair of ridge waveguides forms a second arm of the Mach-Zehnder interferometer; and for each of the first plurality of electrodes and the second plurality of electrodes, the first arm is disposed between a first pair of adjacent electrodes and the second arm is disposed between a second pair of adjacent electrodes. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0020] In a 20thaspect of the 1stexample embodiment, the first plurality of electrodes and the second plurality of electrodes are in contact with the ridge waveguides. The remainder of the features and example features of the 1stexample embodiment are as described above.

[0021] In a 2ndexample embodiment, the present invention is a method. The method comprises providing a monolithic substrate having a first side and a second side, the first side having a layer of electrooptical material disposed thereon; patterning the layer of electrooptical material; etching the layer of electrooptical material to define a pair of ridge waveguides and a slab, the pair of ridge waveguides extending from the slab; forming a first electrode section on the etched layer of electrooptical material at a first position with respect to the pair of ridge waveguides, the first electrode section comprising a first plurality of electrodes; and forming a second electrode section on the etched layer of electrooptical material at a second position with respect to the pair of ridge waveguides, the second position being spaced apart from the first position, the second electrode section comprising a second plurality of electrodes.

[0022] In a 2ndaspect of the 2ndexample embodiment, the method further comprises depositing a cladding over the ridge waveguides. The remainder of the features and example features of the 2ndexample embodiment are as described above.

[0023] The flowchart and block diagrams in the Figures illustrate the architecture, functionality, and operation of possible implementations of systems, methods, and computer program products according to various embodiments of the present disclosure. In this regard,HCU-08225 (HU 10197)each block in the flowchart or block diagrams may represent a module, segment, or portion of instructions, which comprises one or more executable instructions for implementing the specified logical function(s). In some alternative implementations, the functions noted in the block may occur out of the order noted in the figures. For example, two blocks shown in succession may, in fact, be executed substantially concurrently, or the blocks may sometimes be executed in the reverse order, depending upon the functionality involved. It will also be noted that each block of the block diagrams and / or flowchart illustration, and combinations of blocks in the block diagrams and / or flowchart illustration, can be implemented by special purpose hardware-based systems that perform the specified functions or acts or carry out combinations of special purpose hardware and computer instructions.

[0024] The descriptions of the various embodiments of the present disclosure have been presented for purposes of illustration, but are not intended to be exhaustive or limited to the embodiments disclosed. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The terminology used herein was chosen to best explain the principles of the embodiments, the practical application or technical improvement over technologies found in the marketplace, or to enable others of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

HCU-08225 (HU 10197)CLAIMS1. A device comprising:a monolithic substrate having a first side and a second side;an etched layer of electrooptical material disposed on the first side of the monolithic substrate, said etched layer comprising a pair of ridge waveguides and a slab, the pair of ridge waveguides extending from the slab;a first electrode section disposed on the etched layer of electrooptical material at a first position with respect to the pair of ridge waveguides, the first electrode section comprising a first plurality of electrodes, the first plurality of electrodes configured to apply a DC bias to a first portion of each of the ridge waveguides; and a second electrode section disposed on the etched layer of electrooptical material at a second position with respect to the pair of ridge waveguides, the second position being spaced apart from the first position, the second electrode section comprising a second plurality of electrodes, the second plurality of electrodes configured to apply an RF signal to a second portion of each of the ridge waveguides.

2. The device of claim 1, wherein the monolithic substrate is an insulator.

3. The device of claim 2, wherein the insulator comprises a material selected from SiO2, TiO2, HfO2, ZnO, ITO, or CaF2.

4. The device of claim 2, wherein the insulator has a refractive index less than that of the ridge waveguides.

5. The device of claim 1, further comprising a support, the support disposed on the second side of the monolithic substrate.

6. The device of claim 5, wherein the support comprises a material selected from Si, A12O3, SiO2.

7. The device of claim 1, wherein the electrooptical material comprises a material selected from LiTaO3, LiNbO3, SiC, GaAs, SiO2, KNbO3, or KH2PO4.

8. The device of claim 7, wherein the electrooptical material comprises LiTaO3, and whereinHCU-08225 (HU 10197)each of the ridge waveguides is elongated in a direction perpendicular to a z-axis of the LiTaOs.

9. The device of claim 7, wherein the electrooptical material comprises LiTaCh, and wherein each of the ridge waveguides is elongated in a direction perpendicular to an x-axis of the LiTaOs.

10. The device of claim 1, wherein the first plurality of electrodes and the second plurality of electrodes each comprises at least three electrodes disposed adjacent to one another on the electrooptical material.

11. The device of claim 10, wherein each of the ridge waveguides is disposed between a first pair of adjacent electrodes and a second pair of adjacent electrodes of each of the first plurality of electrodes and the second plurality of electrodes.

12. The device of claim 1, wherein the first plurality of electrodes and the second plurality of electrodes each independently comprises a material selected from Au, Al, Ag, or Cu.

13. The device of claim 1, further comprising a cladding disposed over the pair of ridge waveguides.

14. The device of claim 13, wherein the cladding comprises an oxide material.

15. The device of claim 13, wherein the cladding comprises a material selected from SiO2, AI2O3, TiO2, HfO2, ZnO, ITO, or CaF2.

16. The device of claim 13, wherein the cladding comprises a material having a refractive index lower than that of the ridge waveguides.

17. The device of claim 1, wherein a ratio of a thickness of each of the ridge waveguides to a thickness of the monolithic substrate is from 1:20 to 1:4.

18. The device of claim 1, further comprising an optical splitter and an optical combiner, each disposed on the first side of the monolithic substrate, the optical splitter and the opticalHCU-08225 (HU 10197)combiner each being in optical communication with each of the pair of ridge waveguides, wherein the ridge waveguides form arms of a Mach-Zehnder interferometer, and wherein the first electrode section and the second electrode section are disposed between the optical splitter and the optical combiner.

19. The device of claim 18, wherein:the first and the second pluralities of electrodes each comprises at least three electrodes disposed adjacent to one another on the electrooptical material;a first ridge waveguide of the pair of ridge waveguides forms a first arm of the Mach-Zehnder interferometer, and a second ridge waveguide of the pair of ridge waveguides forms a second arm of the Mach-Zehnder interferometer; andfor each of the first plurality of electrodes and the second plurality of electrodes, the first arm is disposed between a first pair of adjacent electrodes and the second arm is disposed between a second pair of adjacent electrodes.

20. The device of claim 1, wherein at least one electrode of each of the first plurality of electrodes and the second plurality of electrodes are in contact with the ridge waveguides.

21. The device of claim 1, wherein at least one electrode of each of the first plurality of electrodes and the second plurality of electrodes are disposed on the slab.

22. A method comprising:providing a monolithic substrate having a first side and a second side, the first side having a layer of electrooptical material disposed thereon;patterning the layer of electrooptical material;etching the layer of electrooptical material to define a pair of ridge waveguides and a slab, the pair of ridge waveguides extending from the slab;forming a first electrode section on the etched layer of electrooptical material at a first position with respect to the pair of ridge waveguides, the first electrode section comprising a first plurality of electrodes; andforming a second electrode section on the etched layer of electrooptical material at a second position with respect to the pair of ridge waveguides, the second position being spaced apart from the first position, the second electrode section comprising a second plurality of electrodes.HCU-08225 (HU 10197)23. The method of claim 22, further comprising depositing a cladding over the ridge waveguides.